Concrete floor structure and its manufacturing method
By applying a primer with a resin and organosilicon compound to the self-leveling material slurry cured layer, the method enhances adhesive strength, addressing inconsistent bonding issues and resulting in a durable concrete floor structure.
Patent Information
- Application Number
- JP2021050158
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2041-03-24
AI Technical Summary
Existing methods for constructing concrete floor structures face challenges in achieving stable adhesive strength between the stretched flooring material and the hardened self-leveling material slurry due to variations in construction and curing conditions, leading to inconsistent bonding.
Applying a flooring primer containing a resin component and an organosilicon compound, such as alkoxysilanes, to the upper surface of the self-leveling material slurry cured layer under specific conditions to enhance penetration and reinforcement, thereby improving adhesive strength.
The method stabilizes the adhesive strength between the flooring material and the self-leveling material slurry cured layer, ensuring a durable and robust concrete floor structure with improved bonding properties.
Smart Images

Figure 0007579189000006 
Figure 0007579189000007 
Figure 0007579189000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a concrete floor structure and a method for manufacturing the same. [Background technology]
[0002] In buildings such as offices, hospitals, factories, and warehouses, various resin-based flooring materials are generally used to finish concrete floors. When these flooring materials are used as finishing materials for concrete floors, they tend to improve the dynamic load resistance, abrasion resistance, chemical resistance, antibacterial properties, antistatic properties, etc. of the floor surface. Known methods for constructing the base layer when installing these flooring materials include the direct concrete pressing method and joint construction methods using mortars, self-leveling materials, etc.
[0003] Patent Document 1 describes that by using a self-leveling material containing cement, aggregate, and a water-retaining agent as the main components of a floor base material and at least one of vinyl acetate resin, vinyl versatate resin, vinyl acetate-vinyl versatate copolymer, ethylene-vinyl acetate copolymer, acrylic resin, vinyl acetate-acrylic acid copolymer, vinyl acetate-vinyl versatate-acrylic acid ester copolymer, and SBR (styrene-butadiene rubber) as a synthetic resin, the synthetic resin gathers on the surface during drying after the application of the self-leveling material, and hardens in that state, thereby obtaining excellent self-leveling properties and a surface with a density close to a mirror finish, and obtaining a surface state similar to that of a synthetic resin. Furthermore, Patent Document 1 discloses that the self-leveling material is used to form a base on a base such as concrete, wood, or metal, and a flooring or the like is applied on the top surface and used, and the flooring can be easily removed when it deteriorates, which significantly improves the efficiency of the work of replacing adhesive-attached flooring during renovations, and also significantly reduces the work time.
[0004] Patent Document 2 also discloses that a concrete floor structure with a floor finish can be obtained that has excellent horizontal leveling, rapid hardening, and rapid drying properties and has excellent durability even in severe service environments, by a manufacturing method for a concrete floor structure that includes the steps of: providing a primer layer for a self-leveling material slurry on the upper surface of a concrete floor; pouring and hardening a slurry prepared by mixing a self-leveling material containing alumina cement and powdered resin with water on the upper surface of the primer layer for the self-leveling material; providing a primer layer for flooring on the upper surface of the hardened self-leveling material slurry layer; applying an adhesive for flooring on the upper surface of the primer layer for flooring to provide an adhesive layer for flooring; and laying and adhering a finishing material for flooring on the upper surface of the adhesive layer for flooring. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-20263 A [Patent Document 2] JP 2009-203790 A Summary of the Invention [Problem to be solved by the invention]
[0006] When applying a self-leveling material to the top surface of a concrete floor and then applying a floor covering on top of that to obtain a concrete floor structure, a floor covering primer may be applied to the surface of the self-leveling material slurry hardened body in order to improve the adhesive strength between the floor covering and the self-leveling material slurry hardened body. However, the quality of the surface layer of the self-leveling material slurry hardened body may change depending on the application or curing conditions of the self-leveling material, and sufficient adhesive strength between the floor covering layer and the self-leveling material slurry hardened body layer may not be consistently obtained even if a floor covering primer is applied.
[0007] Therefore, a main object of the present invention is to provide a method for manufacturing a concrete floor structure having excellent adhesive strength between a floor covering layer and a self-leveling material slurry hardened body layer. [Means for solving the problem]
[0008] The inventors conducted intensive research to solve the above problems and discovered that by applying a specified flooring primer containing a resin component and an organosilicon compound to the top surface of a self-leveling material slurry hardened body layer under specified conditions, the adhesive strength between the flooring layer and the self-leveling material slurry hardened body layer is excellent, which led to the completion of the present invention.
[0009] One aspect of the present invention relates to a method for manufacturing a concrete floor structure. The method for manufacturing the concrete floor structure includes the steps of applying a primer for a self-leveling material to the upper surface of a concrete floor to provide a primer layer for the self-leveling material, pouring a self-leveling material slurry prepared by kneading a self-leveling material and water on the upper surface of the primer layer for the self-leveling material to provide a self-leveling material slurry hardened body layer containing a hardened body of the self-leveling material slurry, applying a primer for flooring materials containing a resin component and an organosilicon compound to the upper surface of the hardened body layer of the self-leveling material slurry to provide a primer layer for flooring materials, applying an adhesive for flooring materials to the upper surface of the primer layer for flooring materials to provide an adhesive layer for flooring materials, and laying a finish material for flooring materials on the upper surface of the adhesive layer for flooring materials to bond the adhesive layer for flooring materials to the finish material for flooring materials. The content of the organosilicon compound in the primer for flooring is 15 to 30 mass % based on the total amount of the resin component and the organosilicon compound. The application amount of the resin component and the organosilicon compound in the primer for flooring is 130 to 400 g / m 2 It is.
[0010] According to this manufacturing method, a concrete floor structure having excellent adhesive strength between the flooring layer and the self-leveling material slurry hardened body layer can be stably manufactured. The inventors believe that the reason for this effect is as follows. By applying a flooring primer containing a predetermined amount of an organosilicon compound to the upper surface of the self-leveling material slurry hardened body layer, the flooring primer penetrates deeper into the self-leveling material slurry hardened body, and a layer reinforced by the flooring primer is generated deeper from the surface of the self-leveling material slurry hardened body. It is presumed that this action improves the adhesive strength between the flooring layer and the self-leveling material slurry hardened body layer.
[0011] Preferred embodiments of the method for manufacturing a concrete floor structure are shown below. A plurality of these preferred embodiments can be combined. 1) The self-leveling material must be a fast-hardening self-leveling material containing fast-hardening cement and / or gypsum. 2) The Shore hardness of the hardened surface of the self-leveling material slurry must be 50 or more 6 hours after the slurry is poured (constructed). 3) The moisture content on the surface of the hardened self-leveling material slurry must be less than 5% (D value = less than 690) 24 hours after the slurry is poured (constructed). 4) The expansion of the length change rate of the hardened body of the self-leveling material slurry is 0 to 0.08%, and the contraction of the length change rate is -0.08 to 0%. 5) The resin components contained in the primer for flooring materials are epoxy resin and epoxy resin hardener. 6) The organosilicon compounds contained in the primer for flooring materials are alkoxysilanes. 7) Finishing materials for flooring must be polyvinyl chloride-based finishing materials for flooring. 8) The thickness of the finishing material for flooring must be 1 to 10 mm.
[0012] Another aspect of the present invention relates to a concrete floor structure. The concrete floor structure comprises, in this order, a concrete floor, a primer layer for a self-leveling material, a hardened self-leveling material slurry layer, a primer layer for a floor material formed by applying a primer for a floor material containing a resin component and an organosilicon compound, an adhesive layer for the floor material, and a finishing material for the floor material. The content of the organosilicon compound in the primer for the floor material is 15 to 30 mass % based on the total amount of the resin component and the organosilicon compound. The application amount of the resin component and the organosilicon compound in the primer for the floor material is 130 to 400 g / m 2 It is. Effect of the Invention
[0013] According to the present invention, there is provided a method for manufacturing a concrete floor structure having excellent adhesive strength between a floor covering layer and a self-leveling material slurry hardened body layer. Also, according to the present invention, there is provided a concrete floor structure obtained by such a manufacturing method. [Brief description of the drawings]
[0014] [Figure 1] 1(a), 1(b), 1(c), 1(d), and 1(e) are cross-sectional views that typically show the process of manufacturing a concrete floor structure. [Diagram 2] 2(a) and 2(b) are cross-sectional views that typically show an apparatus for measuring the change in length of a hardened body of a self-leveling material slurry. [Diagram 3] 3(a), 3(b), and 3(c) are diagrams showing schematic examples of changes in the length of a sample during the process of hardening of a self-leveling material slurry. [Figure 4] FIG. 4 is a diagram showing a schematic example of a tensile load curve obtained in the measurement of peel adhesion strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. However, the present invention is not limited to the following embodiment.
[0016] In this specification, the term "flooring material" refers to a material that is composed of a primer for flooring material, an adhesive for flooring material, and a finish material for flooring material. In this specification, the term "flooring material layer" refers to a material that is composed of a primer layer for flooring material, an adhesive layer for flooring material, and a finish material for flooring material.
[0017] Figures 1(a), 1(b), 1(c), 1(d), and 1(e) are cross-sectional views that typically show the process of manufacturing a concrete floor structure. The concrete floor structure and the manufacturing method thereof of this embodiment will be described with reference to Figures 1(a) to 1(e).
[0018] First, as shown in FIG. 1(a), a concrete floor 30 is prepared. The concrete floor may be a concrete floor of a building. The upper surface 30a of the concrete floor 30 may have unevenness (small unevenness) 32 or a slope (subtle slope) 33. Next, as shown in FIG. 1(b), a primer for a self-leveling material is applied to the upper surface 30a of the concrete floor 30 to provide a primer layer 34 for the self-leveling material. Next, after the primer layer 34 for the self-leveling material is dried to form a film, a self-leveling material slurry 35 is poured as shown in FIG. 1(c).
[0019] The self-leveling material slurry can be prepared by transporting the self-leveling material in a bag to the construction site and mixing a predetermined amount of water with the self-leveling material using a mixer such as an on-site mixing and kneading device or a hand mixer near the construction site.
[0020] Next, the self-leveling material slurry 35 supplied and applied on the concrete floor 30 is hardened, and the moisture content of the surface of the hardened slurry is reduced to less than 5% (D value less than 690). This allows the formation of a hardened self-leveling material slurry layer containing the hardened self-leveling material slurry. Next, as shown in FIG. 1(d) and FIG. 1(e), a flooring primer containing a resin component and an organosilicon compound is applied to the upper surface of the hardened self-leveling material slurry layer 36 to provide a flooring primer layer 37, a flooring adhesive is applied to the upper surface of the flooring primer layer 37 to provide a flooring adhesive layer 38, and a flooring finish material 39 is laid on the upper surface of the flooring adhesive layer 38 and bonded to the flooring adhesive layer 38. This allows the formation of a concrete floor structure 100, 110 having a floor surface 39a with a flooring finish.
[0021] In this embodiment, a concrete floor base having good flatness can be efficiently formed by using a self-leveling material having excellent fast hardening properties. As a result, a concrete floor structure having a floor finish and excellent horizontal level without defects can be easily formed without forming a gap between the floor adhesive layer 38 and the floor finishing material 39, not only when the floor finishing material 39 is thin as shown in Fig. 1(d) but also when the floor finishing material 39 is thick as shown in Fig. 1(e) or when a hard floor finishing material is applied.
[0022] Next, the primer for the self-leveling material, the self-leveling material (self-leveling material slurry), and the flooring material used in this embodiment will be described.
[0023] The self-leveling material primer used in this embodiment is used to prevent the moisture in the self-leveling material slurry from penetrating into the concrete floor when the slurry is poured, and to firmly bond the concrete floor and the hardened layer of the self-leveling material slurry.
[0024] The primer for the self-leveling material may be, for example, a commercially available product whose main component is a resin component such as an acrylic-styrene copolymer resin or an ethylene vinyl acetate copolymer, regardless of the type. The resin component is preferably an acrylic-styrene copolymer resin. For example, when using a primer in which the resin component in the primer for the self-leveling material is 45% by mass, the coating amount of the primer is preferably 50 to 240 g / m from the viewpoint of stably obtaining good adhesive strength. 2 , more preferably 60 to 225 g / m 2 , and more preferably 70 to 200 g / m 2 , particularly preferably 80 to 180 g / m 2 The self-leveling primer can be used after diluting it with water as needed.
[0025] The drying time after application of the primer for the self-leveling material can be appropriately set according to the temperature conditions or ventilation conditions. The drying time after application of the primer for the self-leveling material is preferably 3 to 8 hours in summer and preferably 5 to 12 hours in winter.
[0026] The self-leveling material used in this embodiment may be, for example, a commercially available product such as a cement-based self-leveling material, a gypsum-based self-leveling material, etc. From the viewpoint of shortening the construction period, it is preferable to use a fast-hardening self-leveling material containing fast-hardening cement and / or gypsum as a hydraulic component.
[0027] As the fast-setting cement, any commercially available product containing calcium aluminate, calcium sulfoaluminate, calcium fluoroaluminate or the like as a main component can be used regardless of its type.
[0028] The CaO / Al2O3 molar ratio of calcium aluminate is preferably 1 or more, and it is particularly preferable to use an alumina cement whose main component is monocalcium aluminate, which has a CaO / Al2O3 molar ratio of 1, because this provides an appropriate pot life and rapid hardening properties.
[0029] The gypsum may be any of various types such as anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum, and may be used alone or in a mixture of two or more types, regardless of the type.
[0030] Self-leveling material can be mixed and stirred with water to produce self-leveling material slurry (mortar). By adjusting the amount of water added, it is possible to adjust the fluidity, pot life, material segregation properties, and strength of the hardened slurry (mortar) body.
[0031] The mass ratio (W / S) of the self-leveling material (S) to water (W) in the self-leveling material slurry is preferably 0.16 to 0.28, more preferably 0.17 to 0.27, further preferably 0.18 to 0.26, and particularly preferably 0.19 to 0.25.
[0032] The self-leveling material is preferably adjusted such that the flow value of the slurry (mortar) having self-leveling properties (self-fluidity) prepared by mixing with water is preferably 190 to 270 mm, more preferably 200 to 260 mm, and even more preferably 210 to 255 mm. If the flow value is within such a range, it tends to be easy to apply and to easily obtain a hardened body surface with high smoothness.
[0033] The thickness of the self-leveling material slurry applied varies depending on the unevenness of the concrete floor slab surface and the inclination of the slab surface, and can be set appropriately for each construction site. The thickness of the self-leveling material slurry applied is preferably 2 to 70 mm, more preferably 2 to 50 mm, even more preferably 2 to 40 mm, and particularly preferably 2 to 30 mm, based on the top surface of the most convex part of the floor slab surface.
[0034] When applying the self-leveling material slurry thinly to a height of 2 to 5 mm based on the top surface of the most convex part of the floor slab surface, it is preferable to pour the slurry and apply it while performing an operation to spread the slurry evenly using a spike roller, a dragonfly, a trowel, etc., to form a slurry with a thin layer and a high horizontal level over the entire floor slab. When applying the self-leveling material slurry thickly to a height of 5 to 70 mm based on the top surface of the most convex part of the floor slab surface, it is preferable to pour the slurry and apply it while performing an auxiliary operation to spread the slurry evenly using a dragonfly, etc., to form a slurry with a thick layer and a high horizontal level over the entire floor slab.
[0035] The Shore hardness of the surface of the hardened self-leveling material slurry is preferably 50 or more 6 hours after casting (applying) the slurry, more preferably 50 or more 4 hours, even more preferably 50 or more 3.5 hours, and particularly preferably 50 or more 3 hours. After casting (applying) of the slurry is completed, hardening proceeds quickly and casting (applying) of the self-leveling material slurry is completed.
[0036] Furthermore, the time (elapsed time from pouring the slurry) until the moisture content of the surface of the hardened self-leveling material slurry reaches less than 5% (D value less than 690), which is the moisture content suitable for application to flooring, is preferably 12 to 24 hours, more preferably 12 to 22 hours, even more preferably 12 to 20 hours, and particularly preferably 12 to 18 hours. By using such a self-leveling material, a good hardened state and surface dry state can be quickly obtained, allowing the next step of application of the flooring material to begin early.
[0037] The expansion of the length change rate of the hardened body of the self-leveling material slurry is preferably in the range of 0 to 0.08%, more preferably 0 to 0.06%, and even more preferably 0 to 0.05%, and the contraction of the length change rate is preferably in the range of -0.08 to 0%, more preferably -0.06 to 0%, and even more preferably -0.05 to 0%. By using a self-leveling material having such expansion or contraction characteristics, it is possible to prevent cracks from occurring in the hardened body itself, and it is also possible to maintain high adhesive strength between the concrete floor as the base and the flooring material applied on the top surface. If the length change rate is outside of this range, cracks may occur due to the hardening contraction of the hardened body of the self-leveling slurry, and the moisture released from the concrete floor as the base may diffuse through the cracks, causing swelling in the flooring material layer on the top surface.
[0038] The flooring layer used in this embodiment is composed of a flooring primer layer, a flooring adhesive layer, and a flooring finish. The flooring primer layer and the flooring adhesive layer can be formed from the flooring primer and flooring adhesive, respectively.
[0039] The flooring primer layer is a layer used to improve adhesion to a concrete floor base. The flooring primer for forming the flooring primer layer contains a resin component and an organosilicon compound. The flooring primer may be mainly composed of the resin component and the organosilicon compound.
[0040] The resin component may be composed of, for example, a curable resin and a curing agent for the curable resin. Examples of the curable resin include epoxy resins such as solvent-based epoxy resins, solventless epoxy resins, and water-based epoxy resins. The curable resin is preferably an epoxy resin. When the curable resin is an epoxy resin, the curing agent for the curable resin may be a curing agent for the epoxy resin. Examples of the curing agent for the epoxy resin include amines such as aliphatic amines, aromatic amines, and modified amines (ketimines (ketoimines)); imidazoles; and acid anhydrides. The resin component is preferably an epoxy resin and a curing agent for the epoxy resin. The primer for flooring materials is preferably one that has low viscosity and excellent impregnation. A commercially available product can be used as the primer for flooring materials containing a resin component (e.g., epoxy resin and epoxy resin curing agent).
[0041] The flooring primer contains an organosilicon compound in addition to the resin component. The flooring primer contains an organosilicon compound, which can improve the adhesive strength of the flooring layer to the self-leveling material slurry hardened body layer. The reason for this effect is believed to be that the flooring primer penetrates deeper into the hardened body of the self-leveling material slurry, and the layer reinforced by the flooring primer is generated deeper from the surface of the hardened body of the self-leveling material slurry.
[0042] The organosilicon compound is preferably an alkoxysilane. The alkoxysilane is preferably tetraethoxysilane.
[0043] The content of the organosilicon compound in the primer for flooring is 15 to 30 mass%, preferably 17 to 28 mass%, more preferably 18 to 26 mass%, and even more preferably 19 to 25 mass%, based on the total amount of the resin component and the organosilicon compound. By having the content of the organosilicon compound in the primer for flooring within such a range, the primer for flooring can penetrate deeper into the hardened body of the self-leveling material slurry, improving the adhesive strength between the flooring layer and the hardened body layer of the self-leveling material slurry.
[0044] The primer for flooring can be applied using a brush, roller, trowel, or other suitable tool.
[0045] The amount of resin component and organosilicon compound applied in the primer for flooring is 130 to 400 g / m2 from the viewpoints of improving the adhesive strength between the flooring layer and the hardened layer of the self-leveling material slurry and of economy. 2 and preferably 140 to 370 g / m 2 , more preferably 145 to 350 g / m 2 , and more preferably 150 to 300 g / m 2 It is.
[0046] The adhesive for flooring is used to bond a finishing material for flooring to a layer of a hardened self-leveling material slurry provided with a primer layer for flooring. Examples of the adhesive for flooring include epoxy resin-based adhesives for flooring, such as solvent-based epoxy resins, solventless epoxy resins, and water-based epoxy resins.
[0047] The application of flooring adhesives can be done in accordance with the application instructions of each flooring manufacturer, using a comb trowel, roller, brush, etc. as appropriate.
[0048] The finishing material for flooring can be appropriately selected and used according to the required characteristics. Examples of the finishing material for flooring include plastic floors, carpet floors, linoleum floors, rubber floors, wooden floors, stone floors, and ceramic floors. The finishing material for flooring is preferably a finishing material for plastic floors, carpet floors, linoleum floors, rubber floors, or wooden floors, and more preferably a finishing material for plastic floors. The finishing material for flooring may contain an antibacterial agent or may be antibacterial-treated.
[0049] Examples of plastic floors include homogeneous vinyl floor tiles, semi-rigid composition vinyl floor tiles, soft composition vinyl floor tiles, pure vinyl floor tiles, resin terrazzo tiles, vinyl floor sheets, woven vinyl floor sheets, nonwoven vinyl floor sheets, woven laminated vinyl floor sheets, nonwoven laminated vinyl floor sheets, laminated vinyl floor sheets, woven laminated expanded vinyl floor sheets, nonwoven laminated expanded vinyl floor sheets, laminated expanded vinyl floor sheets, nonwoven laminated printed expanded vinyl floor sheets, laminated printed expanded vinyl floor sheets, etc. Among these, plastic floors are preferably vinyl chloride-based flooring finishing materials because they have excellent dynamic load resistance, chemical resistance, and abrasion resistance. For example, vinyl chloride-based sheets or vinyl chloride tiles can be suitably used as vinyl chloride-based flooring finishing materials.
[0050] For carpet floors, carpet tiles, roll carpets, etc. can be used. For linoleum floors, linoleum floor tiles, linoleum floor sheets, etc. can be used. For rubber floors, rubber floor tiles, rubber floor sheets, etc. can be used. For wood floors, flooring boards, flooring blocks, etc. can be used.
[0051] The thickness of the floor finishing material is appropriately selected according to the function required for each application of the concrete floor and the material of the floor finishing material used. The thickness of the floor finishing material (layer) is preferably 1 to 10 mm, more preferably 1.2 to 8 mm, even more preferably 1.3 to 5 mm, and particularly preferably 1.5 to 3 mm. When the thickness of the floor finishing material is within such a range, it tends to be possible to obtain a floor finishing concrete structure with excellent durability performance to which the floor finishing material is firmly attached, taking advantage of the high flatness formed using the self-leveling material. If the thickness of the floor finishing material is smaller than the above range, it becomes difficult for the floor finishing concrete structure to obtain sufficient durability characteristics, and if it is larger than the above range, it is not possible to improve the durability performance, which is not preferable from the viewpoint of economic efficiency.
[0052] By such a manufacturing method, a concrete floor structure can be obtained which comprises, in this order, a concrete floor, a primer layer for self-leveling material, a hardened self-leveling material slurry layer, a primer layer for flooring material formed by applying a primer for flooring material containing a resin component and an organosilicon compound, an adhesive layer for flooring material, and a finishing material for flooring material. The content of the organosilicon compound in the primer for flooring material is 15-30 mass% based on the total amount of the resin component and the organosilicon compound. The coating amount of the resin component and the organosilicon compound in the primer for flooring material is 130-400 g / m 2 It is.
[0053] (Method of evaluating characteristics) (1) Fluidity evaluation of self-leveling material slurry: Flow value measurement method: Measurements are made in accordance with JASS·15M-103. A resin pipe (100mL capacity) with an inner diameter of 50mm and height of 51mm is placed on a polished glass plate 5mm thick, and the mixed self-leveling material slurry is filled up to the top of the resin pipe, after which the pipe is lifted vertically. After the slurry stops spreading, the diameters in two perpendicular directions are measured, and the average value is taken as the flow value to evaluate the fluidity of the slurry. The evaluation conditions are a temperature of 20°C and humidity of 65%.
[0054] (2) Evaluation of length change of hardened self-leveling material slurry: 2(a) and 2(b) are cross-sectional views showing a schematic diagram of an apparatus for measuring the change in length of hardened self-leveling material slurry. The apparatus shown in Fig. 2(a) and 2(b) is used to measure the rate of change in length. The rate of change in length is measured by pouring the slurry immediately after mixing up to the height of the formwork inside the mold, and starting to measure the change in length immediately after pouring. Measurements are taken at 5-minute intervals and for a material age of up to 28 days. Measurements are taken in air at 20°C and RH 65%.
[0055] The rate of change in length of the self-leveling material slurry when it hardens is determined by dividing the change in the distance (mm) between the SUS disc 75b shown in Figure 2(a) and the end of the displacement sensor 74 (the end on the SUS disc 75b side) by the distance (480 mm) between the SUS discs 75a and SUS discs 75c.
[0056] 3(a), 3(b), and 3(c) are diagrams showing an example of the change in length of a sample during the hardening process of a self-leveling material slurry. In FIG. 3(a), the measured sample has a base length of 0 days (point a), expands with hardening, expands most at point b, and then gradually shrinks to the length of 28 days (point c). In formulas (1) to (3), B is the length of the sample at point a, C is the length of the sample at point b, and A is the length of the sample at point c. In FIG. 3(b), the measured sample has a base length of 0 days (point a), expands without expanding with hardening, and gradually shrinks to the length of 28 days (point c). In formulas (1) to (3), B and C are the lengths of the sample at point a, and A is the length of the sample at point c. In Fig. 3(c), the length of the measured sample at 0 days (point a) is the base length, and as the sample hardens, it gradually expands without shrinking, reaching the length at 28 days (point c). In formulas (1) to (3), B is the length of the sample at point a, and A and C are the lengths of the sample at point c.
[0057] -Method of measuring the rate of change in length: Measurement is performed using the device shown in Figure 2(a) and Figure 2(b), and the rate of change in length is calculated according to the following formula (1). The measurement sample is filled with self-leveling material slurry and the age of the material is considered to be 0 days immediately after casting. The measurement is performed in air at 20℃ and RH 65%. A (-) in the rate of length change means contraction and a (+) means expansion.
[0058]
number
[0059] - Measurement method of contraction of length change rate: Using the equipment shown in Figure 2 (a) and Figure 2 (b), measurement is performed using the measurement sample prepared by the measurement method of length change rate. The expansion of length change rate is the length (C) of the sample when it is most expanded, and is calculated according to formula (2).
[0060]
number
[0061] - Measurement method of shrinkage of length change rate: Using the equipment shown in Figure 2 (a) and Figure 2 (b), measurements are made using the measurement sample prepared by the measurement method of length change rate. The shrinkage of length change rate is calculated according to formula (3), with the length of the sample at its most expanded state being the base length.
[0062]
number
[0063] (3) Evaluation of surface properties of hardened self-leveling material slurry: - Shore hardness measurement method: After a certain time has elapsed since pouring the self-leveling material slurry, a spring type D hardness tester (manufactured by Ueshima Seisakusho) is pressed vertically on the hardened surface at any 3 to 5 points. The average value of the gauge reading of the spring type D hardness tester at that time is taken as the Shore hardness at that time, and the surface hardness is evaluated. - Moisture content on the surface of the hardened body A specific amount of time has passed since the self-leveling material slurry was poured, and the moisture content (D value) of the hardened surface is measured using a concrete / mortar moisture meter (Kett Electric Laboratory). Based on the Japan Floor Construction Technology Research Council's "Methods for measuring and grading various qualities of the surface layer of concrete floor base," if the measured value D value (HI-500) is less than 690, it is determined that the moisture content is less than 5%.
[0064] (4) Evaluation of peel adhesion strength: Peel adhesion strength measurement method: Measured according to the adhesive peeling strength test method of JIS K 6854. A floor primer layer is laid on top of the hardened self-leveling slurry layer aged 14 days after pouring the self-leveling slurry, and floor adhesive is applied on the top of the primer layer. Five floor finishing materials with a width of 25 mm and a length of 200 mm are laid on the top of the applied layer of floor adhesive, and the 160 mm part from the end without the eyelet stud is glued to form a finishing material layer. After 7 days of age, cut the edges by making incisions along the periphery of the floor finishing material with a cutter knife or the like until it reaches the hardened self-leveling slurry layer. The eyelet stud part of the floor finishing material without the adhesive layer is attached to the jig of a digital force gauge (made by Imada), and a vertical tensile load is applied so that the floor finishing material peels off 100 mm per minute, and pulling is continued until the floor finishing material peels off 160 mm. Fig. 4 is a diagram showing a schematic example of a tensile load curve obtained in the measurement of peel adhesion strength. 1000 pieces of measurement data are recorded per second, and the tensile load curve shown in Fig. 4 is obtained. The tensile load data recorded from 25 mm to 140 mm, excluding the data from the first 25 mm and the last 20 mm, is averaged to obtain a single peel adhesion strength (N / 25 mm width), and the average value of five repeated measurements is evaluated as the peel adhesion strength. EXAMPLES
[0065] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.
[0066] (Materials used): The following materials were used. 1) Primer for self-leveling materials: A commercially available product whose main component is acrylic-styrene copolymer resin. 2) Self-leveling material: A commercially available fast-hardening self-leveling material that contains fast-hardening cement. 3) Primers for flooring: A stock solution of epoxy resin, epoxy resin hardener (ketimine), and organosilicon compound (tetraethoxysilane) (commercial product, one-liquid type, epoxy resin, epoxy resin hardener, and organosilicon compound total amount is 100 mass%, epoxy resin and epoxy resin hardener (ketimine) content: 92.5 mass%, organosilicon compound (tetraethoxysilane) content: 7.5 mass%), and a mixed solution of organosilicon compound (tetraethoxysilane) (commercial product, organosilicon compound content: 100 mass%) were prepared. These were mixed as is or in a specified ratio to prepare a primer for flooring materials. 4) Flooring adhesive: Tajima Cement EP30, epoxy type. 5) Finishing material for flooring: Tajima, polyvinyl chloride floor sheet, floor for moving loads, thickness = 2mm.
[0067] (Preparation of self-leveling material slurry) Under conditions of room temperature of 20°C and relative humidity of 65%, the self-leveling material (S) and water (W) were mixed so that the mass ratio (W / S) was 0.19, 0.22, and 0.25, respectively, and the mixture was kneaded for 3 minutes using a chemical stirrer at a rotation speed of 650 rpm to prepare a self-leveling material slurry.
[0068] (Preparation of primer for flooring materials) At room temperature of 20°C and relative humidity of 65%, the original solution of flooring primer and the mixed solution were mixed in the proportions shown in Table 1, and mixed for 3 minutes using a chemical stirrer at 650 rpm to prepare epoxy-based flooring primers A to C.
[0069] [Table 1]
[0070] (Preparation of adhesive for flooring materials) At room temperature of 20°C and relative humidity of 65%, 100 parts by mass of agent A of the epoxy adhesive for flooring was mixed with 100 parts by mass of agent B, and mixed for 3 minutes using a chemical stirrer at 650 rpm to prepare an epoxy adhesive for flooring.
[0071] (Preparation of finishing materials for floor coverings) Under conditions of room temperature of 20°C and relative humidity of 65%, the finishing material for flooring was cut into strips 25 mm wide and 200 mm long, and eyelets were attached 15 mm from one end in the longitudinal direction to prepare the finishing material for flooring.
[0072] A self-leveling material primer was applied to a JIS A5304 paving concrete slab and dried to form a layer of the self-leveling material primer. Self-leveling material slurry was poured to a thickness of 10 mm, allowed to harden, and cured for 14 days in accordance with the specifications for surface adhesion test specimens described in JASS 15 M-103 (quality standard for self-leveling materials) to obtain a hardened layer of self-leveling material slurry. Next, floor covering was applied on top of the hardened layer of self-leveling material slurry, and cured for 7 days to obtain a floor finishing concrete structure specimen for peel adhesion test.
[0073] The Tajima vinyl flooring was installed as follows.
[0074] [Reference examples 1~3] No flooring primer was applied, and flooring adhesive was applied at 360 g / m 2 The self-leveling material slurry hardened body layer was applied with a comb trowel so that the adhesive layer for flooring materials was laid on the self-leveling material slurry hardened body layer. The flooring finishing material was laid on the adhesive layer for flooring materials and adhered to the adhesive layer for flooring materials with a rolling roller.
[0075] [Examples 1 to 10 and Comparative Examples 1 to 9] The flooring primer type shown in Table 1 was applied to the self-leveling material slurry hardened layer using a brush in the amount shown in Table 2, and then dried to form a flooring primer layer. Then, 360 g / m of flooring adhesive was applied. 2 A flooring finish material was laid on the flooring adhesive layer and adhered to the flooring finish material using a rolling roller.
[0076] Table 2 shows the results of peel adhesion strength tests conducted on specimens of concrete structures with floor finishing.
[0077] [Table 2]
[0078] Reference Examples 1 to 3, in which no flooring primer was applied, showed a tendency for the adhesive strength to decrease as the parts by mass of water per 100 parts by mass of the self-leveling material increased.
[0079] On the other hand, the adhesive strength improves when a flooring primer is applied, and for example, as shown in Comparative Examples 1, 3, and 4, adhesive strength tends to improve when the content of the organosilicon compound in the flooring primer is higher, even if the amount of the primer is the same. This is presumably because the inclusion of the organosilicon compound improves the permeability of the flooring primer into the hardened layer of the self-leveling material slurry.
[0080] Furthermore, for example, as shown in Comparative Example 3 and Examples 1 and 2, even if the content of the organosilicon compound in the primer for flooring materials is the same, the adhesive strength showed a tendency to improve by increasing the amount of primer for flooring materials (resin component and organosilicon compound) applied.
[0081] In Examples 1 to 10, the content of the organosilicon compound in the primer for flooring materials and the application amount of the primer for flooring materials were within the appropriate range, and particularly excellent adhesive strength was obtained. [Industrial Applicability]
[0082] According to the present invention, there is provided a method for manufacturing a concrete floor structure having excellent adhesive strength between a floor covering layer and a self-leveling material slurry hardened body layer. Also, according to the present invention, there is provided a concrete floor structure obtained by such a manufacturing method. [Explanation of symbols]
[0083] 30...Concrete floor, 32...Unevenness (small unevenness), 33...Slope (subtle slope), 34...Primer layer for self-leveling material, 35...Self-leveling material slurry, 36...Hardened self-leveling material slurry layer, 37...Primer layer for flooring material, 38...Adhesive layer for flooring material, 39...Finishing material for flooring material, 71...Length change measuring device, 72...Formwork, 73...Cushioning material, 74...Eddy current displacement sensor, 75a, 75b, 75c...SUS disc, 76a, 76b...SUS rod, 77...Fluoropolymer sheet, 80...Tensile load curve, 81...Average tensile load (peel adhesion strength), 82...Evaluation range, 100, 110...Concrete floor structure.
Claims
1. A step of applying a primer for a self-leveling material to an upper surface of a concrete floor to provide a primer layer for a self-leveling material; A step of pouring a self-leveling material slurry prepared by kneading a self-leveling material and water onto an upper surface of the self-leveling material primer layer, and providing a self-leveling material slurry hardened body layer consisting of a hardened body of the self-leveling material slurry; A step of applying a primer for flooring materials containing a resin component and an organosilicon compound to an upper surface of the self-leveling material slurry hardened body layer to provide a primer layer for flooring materials; A step of applying an adhesive for flooring materials to an upper surface of the primer layer for flooring materials to provide an adhesive layer for flooring materials; A step of laying a floor finishing material on the upper surface of the floor adhesive layer and adhering the floor adhesive layer and the floor finishing material; Equipped with The moisture content of the hardened surface of the self-leveling material slurry hardened layer is less than 5%, The content of the organosilicon compound in the primer for flooring is 15 to 30 mass% based on the total amount of the resin component and the organosilicon compound, The coating amount of the resin component and the organosilicon compound in the primer for flooring is 130 to 400 g / m 2 A method for manufacturing a concrete floor structure.
2. 2. The method for manufacturing a concrete floor structure according to claim 1, wherein the resin components contained in the primer for flooring material are an epoxy resin and a hardener for the epoxy resin.
3. The method for manufacturing a concrete floor structure according to claim 1 or 2, wherein the organosilicon compound contained in the primer for flooring is an alkoxysilane.
4. The method for manufacturing a concrete floor structure according to any one of claims 1 to 3, wherein the self-leveling material is a rapid-hardening self-leveling material containing rapid-hardening cement and / or gypsum.
5. The method for manufacturing a concrete floor structure according to any one of claims 1 to 4, wherein the finishing material for flooring is a vinyl chloride-based finishing material for flooring.
6. The method for manufacturing a concrete floor structure according to any one of claims 1 to 5, wherein the finishing material for flooring has a thickness of 1 to 10 mm.
7. Concrete floor and A primer layer for a self-leveling material; A hardened layer of a self-leveling material slurry; A primer layer for flooring materials formed by applying a primer for flooring materials containing a resin component and an organosilicon compound; A flooring adhesive layer; Finishing materials for floor coverings; In this order, The moisture content of the hardened surface of the self-leveling material slurry hardened layer is less than 5%, The content of the organosilicon compound in the primer for flooring is 15 to 30 mass% based on the total amount of the resin component and the organosilicon compound, The coating amount of the resin component and the organosilicon compound in the primer for flooring is 130 to 400 g / m 2 That is, the concrete floor structure.
Citation Information
Patent Citations
Primer composition
JP1990227482A
Formation of moisture-permeable waterproof laminated coating film
JP1999290771A
Technique for laminating floor moisture-permeable coating film
JP2001340806A
Self-levelling plaster
JP2003020263A
Surface-treating material for concrete and unevenness- modifying material for concrete
JP2003213199A