Joining equipment for friction stir welding and resistance welding

The combined use of friction stir welding and resistance welding in a single device addresses the challenges of joining multiple metal plates with dissimilar materials, enhancing bonding strength and energy efficiency while reducing environmental impact and equipment complexity.

JP7579762B2Active Publication Date: 2024-11-08HONDA MOTOR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021118227
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-16
Publication Date
2024-11-08
Estimated Expiration
2041-07-16

AI Technical Summary

Technical Problem

Conventional methods for joining three or more metal plates with dissimilar materials face challenges such as increased production time, capital investment, and environmental impact due to the need for multiple joining techniques and equipment, leading to unstable bonding strength and difficulty in expanding the stirring range in friction stir welding.

Method used

A joining device that combines friction stir welding and resistance welding using an anvil and probe that serve as electrodes, allowing simultaneous performance of both methods to reduce equipment size and processing time, while minimizing gas generation and energy consumption.

Benefits of technology

The device achieves stable bonding strength, reduces environmental impact, and improves energy efficiency by simplifying equipment and processing, preventing intermetallic compound formation, and enhancing bonding strength through controlled current flow and frictional heat.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579762000001
    Figure 0007579762000001
  • Figure 0007579762000002
    Figure 0007579762000002
  • Figure 0007579762000003
    Figure 0007579762000003
Patent Text Reader

Abstract

To provide a joining device and a joining method with combination of friction stir joining and resistance welding, in which increase in a device size and increase in a processing time are reduced.SOLUTION: A laminate 2 includes a first component 3, an intermediate component 4 and a second component 5. A joining device 1 comprises: an anvil 11 which supports the laminate 2 from the first component 3 side; a rotatable probe 12 plunged into the laminate 2 from the second component 5 side; and a shoulder member 13 which encloses the probe 12, and allows electric current to flow between the anvil 11 and the probe 12 or the shoulder member 13. A surface of the anvil 11, which supports the laminate 2, includes an insulative area 113 and a conductive area 114. By plunging the probe 12 into the laminate 2 while rotating the same and causing electric current to flow between the anvil 11 and the probe 12 or the shoulder member 13, the first component 3 and the intermediate component 4 are resistance-welded to each other, and the second component 5 and the intermediate component 4 are friction stir-joined to each other.SELECTED DRAWING: Figure 13
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a joining device for friction stir welding and resistance welding. [Background technology]

[0002] Resistance welding and friction stir welding are examples of methods for joining multiple metal plates together that generate less gas than conventional welding methods, thereby reducing the negative environmental impact on air quality (SDGs 11.6). Furthermore, friction stir welding consumes less electricity than conventional welding methods, contributing to improved energy efficiency during manufacturing (SDGs 7.3).

[0003] When three or more metal plates including dissimilar materials are joined together by resistance welding, an adhesive is used to prevent electrolytic corrosion. This causes defects due to the adhesive, making it impossible to obtain a stable joint strength, and rivets must be used in combination to obtain the required strength. When three or more metal plates including dissimilar materials are joined together by friction stir welding, for example, one aluminum alloy plate and two steel (iron alloy) plates, the first and second layers (Al-Fe) can be joined, but it is difficult to join the second and third layers (Fe-Fe) because the stirring range cannot be expanded. Thus, it is difficult to join three or more metal plates including dissimilar materials using one joining method.

[0004] As a method for joining three or more metal members including dissimilar materials to each other by combining different joining methods, Patent Document 1 describes a method for joining an aluminum material, a steel material, and a clad material (a composite material in which dissimilar materials are rolled into one plate) including an aluminum material layer and a steel material layer. Patent Document 1 describes an embodiment in which an aluminum material and an aluminum material layer of a clad material are joined to each other by friction stir welding, and a steel material and a steel material layer of a clad material are joined to each other by a thermosetting adhesive using frictional heat generated by the friction stir welding, and an embodiment in which a steel material and a steel material layer of a clad material are joined to each other by resistance welding, and an aluminum material and an aluminum material layer of a clad material are joined to each other by a thermosetting adhesive using heat generated by the resistance welding. However, this method is lacking in versatility because it uses a clad material. Patent Document 2 describes that two members that are butted against each other are joined to each other by friction stir line welding, and then another member is fusion-welded or resistance-welded to the joint. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-111489 A [Patent Document 2] JP 2007-237253 A Summary of the Invention [Problem to be solved by the invention]

[0006] In order to join three or more metal components, including dissimilar materials, it is necessary to combine two or more joining methods. However, with conventional methods, the number of joining steps increases, more than two types of joining equipment must be prepared, and the production line must be lengthened, necessitating increased capital investment.

[0007] In view of the above background, the present invention has an objective of providing a joining device that combines friction stir welding and resistance welding, which contributes to reducing adverse environmental impacts on air quality (SDGs 11.6) and / or contributing to improving energy efficiency in manufacturing (SDG 7.3), and which reduces the increase in size of the device and the increase in processing time. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, one aspect of the present invention is a joining device (1, 51) for joining each member to each other in a laminate (2) including a first member (3), an intermediate member (4), and a second member (5) that are each conductive and extend along a predetermined main surface, stacked in this order, the joining device comprising: an anvil (111, 121) that includes an anvil abutment surface (112, 122) for supporting a first surface (6) that forms the surface of the laminate (2) that faces the first member, the anvil abutment surface (112, 122) including an insulating region (113, 123) and a conductive region (114, 124); the anvil (111, 121) and the probe (12, 41, 52) so as to face the anvil (111, 121) and be rotatable about an axis extending in a direction intersecting the main surface and capable of advancing and retracting along the axis relative to the second member (5), the probe (12, 41, 52 being at least partially conductive; a drive mechanism (14, 54) for rotating the probe (12, 41, 52) about the axis and advancing and retracting the probe (12, 41, 52) along the axis; a power source (15) electrically connected to the anvil (111, 121) and the probe (12, 41, 52) so as to pass a current between the anvil (111, 121) and the probe (12, 41, 52) via the laminate (2); and a control device (16) for controlling the operation of the drive mechanism (14, 54) and the power source (15). The probes (12, 41, 52) are rotated and advanced toward the stack (2) from the second surface (7) side until the tips of the probes (12, 41, 52) enter the intermediate member (4), and after the tips of the probes (12, 41, 52) reach the intermediate member (4), a current is passed between the probes (12, 41, 52) and the anvils (111, 121) through the pressurized stack (2). The joining device (1, 51) is for resistance welding the first member (3) and the intermediate member (4) together, and for friction stir joining the second member (5) and the intermediate member (4) together.

[0009] According to this embodiment, the anvil and probe used for friction stir welding also serve as electrodes for resistance welding, so that it is possible to suppress the enlargement and increase in size of the equipment and the lengthening of the manufacturing line, and therefore the capital investment can be suppressed. In addition, since friction stir welding and resistance welding can be performed simultaneously, it is possible to suppress the increase in processing time. Furthermore, this embodiment joins the laminated bodies by resistance welding, which generates less gas than general welding methods, and friction stir welding, which generates less gas than general welding methods and consumes less power than general welding methods, thereby reducing the adverse environmental impact on air quality (SDGs 11.6) and contributing to improving energy efficiency during manufacturing (SDG 7.3).

[0010] In order to solve the above-mentioned problems, one aspect of the present invention provides a joining device (101) for joining each member to each other in a laminate (2) including a first member (3), an intermediate member (4), and a second member (5) that are each electrically conductive and extend along a predetermined main surface, stacked in this order, the joining device comprising: an anvil (111, 121) including an anvil abutment surface (112, 122) for supporting a first surface (6) that forms a surface of the laminate (2) that faces the first member, the anvil abutment surface (112, 122) including an insulating region (113, 123) and a conductive region (114, 124); and an anvil (111, 121) that is rotatable about an axis extending in a direction intersecting the main surface and that is aligned along the axis so as to face a second surface (7) that forms a surface of the laminate (2) that faces the second member (5). A probe (12, 41) capable of advancing and retreating toward the second member (5), a through hole (20, 20a) through which the probe (12, 41) is inserted, and a shoulder abutment surface (24, 24a) to be pressed against the second surface (7), and a shoulder member (13, 13a, 61, 64, 68) having at least partial conductivity, and the probe (12, 41) are rotated around the axis and advanced and retreated along the axis. a power source (15) electrically connected to the anvil (111, 121) and the shoulder member (13, 13a, 61, 64, 68) so as to pass a current between the anvil (111, 121) and the shoulder member (13, 13a, 61, 64, 68) through the laminate (2); and a control device (16) for controlling the operation of the drive mechanism (14) and the power source (15). The probe (12, 41) is rotated and advanced toward the stack (2) from the second surface (7) side until the tip of the probe (12, 41) enters the intermediate member (4), and after the tip of the probe (12, 41) reaches the intermediate member (4), a current is passed between the shoulder member (13, 13a, 61, 64, 68) and the anvil (111, 121) via the pressurized stack (2). The joining device (101) is for resistance welding the first member (3) and the intermediate member (4) together, and for friction stir joining the second member (5) and the intermediate member (4) together.

[0011] According to this embodiment, the anvil and shoulder members used for friction stir welding also serve as electrodes for resistance welding, so that it is possible to suppress the enlargement and increase in size of the equipment and the lengthening of the manufacturing line, and to suppress capital investment. In addition, since friction stir welding and resistance welding can be performed simultaneously, it is possible to suppress an increase in processing time. Furthermore, this embodiment joins the laminated bodies by resistance welding, which generates less gas than general welding methods, and friction stir welding, which generates less gas than general welding methods and consumes less power than general welding methods, thereby reducing the adverse environmental impact on air quality (SDGs 11.6) and contributing to improving energy efficiency during manufacturing (SDG 7.3).

[0012] In the above aspect, the shoulder member (13, 13a, 61, 64, 68) may include a recess (25, 25a) recessed relative to the shoulder abutment surface (24, 24a) to define a bottom surface (26, 26a) that should face the second surface (7) and that receives a portion of the probe (12, 41).

[0013] According to this aspect, the presence of the recess positions the shoulder abutment surface radially outward, and the nugget is also formed radially outward, allowing resistance welding to be performed over a wide area, thereby increasing the joint strength.

[0014] In the above embodiment, the insulating region (113) may be disposed on the anvil contact surface (112) so as to intersect with an extension of the axis.

[0015] According to this aspect, by disposing the insulating region at the center, the nugget is formed on the radially outer side, so that the joining strength is increased and the stress applied to the joint is dispersed.

[0016] In the above embodiment, the conductive region (114) may be disposed in an annular shape on the anvil contact surface (112) so as to surround the insulating region (113).

[0017] According to this aspect, since the conductive region is annular, the nugget is formed in an annular shape, so that the joining strength is increased and the stress applied to the joint is dispersed.

[0018] In the above embodiment, the conductive region (124) of the anvil contact surface (122) may be divided into a plurality of isolated regions by the insulating region (123).

[0019] According to this aspect, since the conductive region is divided into a plurality of isolated regions, the nugget is formed in a plurality of isolated regions, so that the stress applied to the joint is dispersed. Effect of the Invention

[0020] According to the above aspects, it is possible to provide a joining apparatus and a joining method that combine friction stir welding and resistance welding, in which an increase in the size of the apparatus and an increase in processing time are reduced. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a joining device according to a first embodiment; [Diagram 2] FIG. 11 is a vertical cross-sectional view showing a modification of the joining device according to the first embodiment with respect to insulation. [Diagram 3] 4A and 4B are diagrams showing a shoulder member of the joining device according to the first embodiment (A: first embodiment, B: modified example, upper figure: cross-sectional view taken along line IV-IV in the lower figure, lower figure: bottom view). [Figure 4] FIG. 1 is an explanatory diagram of a bonding method using a bonding device according to a first embodiment; [Diagram 5] FIG. 11 is a vertical cross-sectional view showing a joining device according to a second embodiment. [Figure 6] FIG. 11 is a vertical cross-sectional view showing a joining device according to a third embodiment. [Figure 7] FIG. 13 is a vertical cross-sectional view showing a modified example of the probe of the bonding apparatus according to the third embodiment. [Figure 8] FIG. 13 is a diagram showing a modified example of an insulating portion of a shoulder member of the joining apparatus according to the third embodiment. [Figure 9]FIG. 13 is a diagram showing a modified example of the anvil of the joining apparatus according to the third embodiment. [Figure 10] FIG. 11 is an explanatory diagram of a bonding method using a bonding device according to a third embodiment. [Figure 11] FIG. 13 is an explanatory diagram of a modified example of the bonding method using the bonding device according to the third embodiment. [Figure 12] FIG. 11 is a plan view showing a modified example of the anvil of the joining device according to the first to third embodiments. [Figure 13] 1A and 1B are longitudinal sectional views showing modified examples of the anvil of the joining device according to the first and third embodiments (A: modified example of the first embodiment, B: modified example of the third embodiment). [Figure 14] 13A and 13B are views showing another modified example of the anvil of the joining device according to the first to third embodiments (A is a plan view of the anvil, and B is a cross-sectional view of a joint portion for resistance welding). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a cross-sectional view of a plane including an axis, showing a bonding device 1 according to a first embodiment and a state in the middle of bonding a laminate 2 bonded by the bonding device 1. Below, a case where the axis extends in the vertical direction will be described as an example, but the axis may be inclined with respect to the vertical direction, may extend in the horizontal direction, or may be upside down.

[0023] The laminate 2 includes a first member 3, an intermediate member 4, and a second member 5, each of which is electrically conductive and extends along a main surface perpendicular to the axis, stacked in this order. The axis may intersect with the main surface at an angle other than 90 degrees, instead of being perpendicular. The laminate 2 has a first surface 6 that forms the surface (lower surface) on the first member 3 side, and a second surface 7 that forms the surface (upper surface) on the second member side. The first member 3, the intermediate member 4, and the second member 5 are each formed into a plate shape. One or more other plate materials made of the same material as the first member 3 may be stacked below the first member 3.

[0024] The first member 3 and the intermediate member 4 are made of the same material, and the second member 5 is made of a different material from the first member 3 and the intermediate member 4. The material of the first member 3 and the intermediate member 4 has higher strength and higher electrical resistance than the material of the second member 5. For example, the first member 3 and the intermediate member 4 may be made of an iron alloy (steel) and the second member 5 may be made of an aluminum alloy, the first member 3 and the intermediate member 4 may be made of an iron alloy and the second member 5 may be made of a magnesium alloy, the first member 3 and the intermediate member 4 may be made of a titanium alloy and the second member 5 may be made of an aluminum alloy, the first member 3 and the intermediate member 4 may be made of a titanium alloy and the second member 5 may be made of a magnesium alloy, the first member 3 and the intermediate member 4 may be made of an iron alloy and the second member 5 may be made of a copper alloy, the first member 3 and the intermediate member 4 may be made of a titanium alloy and the second member 5 may be made of a copper alloy, or the first member 3 and the intermediate member 4 may be made of an aluminum alloy and the second member 5 may be made of a copper alloy.

[0025] The joining apparatus 1 comprises an anvil 11 for supporting the first surface 6 of the laminate 2, a probe 12 arranged above the anvil 11, a shoulder member 13 arranged above the anvil 11 and surrounding the probe 12, a drive mechanism 14 for driving the anvil 11, the probe 12 and the shoulder member 13, a power supply 15 for passing current between the probe 12 and the anvil 11 which sandwich the laminate 2, and a control device 16 for controlling the operation of the drive mechanism 14 and the power supply 15.

[0026] The anvil 11 is electrically conductive and has an anvil contact surface 17 that contacts the first surface 6 of the laminate 2 .

[0027] The probe 12 is a part of the rotor 18, and the entire rotor 18 is rotationally symmetrical about the axis and can rotate integrally about the axis. The probe 12 extends along the axis and preferably has a cylindrical shape that is thinner than the upper part 19 of the rotor 18. The tip (lower end) of the probe 12 is a free end so that it can enter the laminate 2. The probe 12 is made of a material such as a copper alloy (chromium copper, alumina-dispersed copper, tungsten copper alloy, etc.), conductive ceramic, or cemented carbide.

[0028] As shown in Fig. 1 and Fig. 3(A), the shoulder member 13 preferably has a rotational symmetric shape around the axis. The shoulder member 13 includes a probe support portion 21 having a through hole 20, a flange 22 extending radially outward from the probe support portion 21, and a side wall portion 23 extending downward from the lower surface of the probe support portion 21 and having a circular ring shape when viewed from below. The central axis of the through hole 20 coincides with the axis. The probe 12 is inserted into the through hole 20. The upper portion of the through hole 20 is expanded in diameter toward the upper portion so as to guide the probe 12 when the probe 12 is inserted. The inner diameter of the lower portion of the through hole 20 is slightly larger than the outer diameter of the probe 12, and when the probe 12 rotates around the axis, the inner peripheral surface of the through hole 20 slides against the outer peripheral surface of the probe 12 to support the probe 12. The inner diameter of the side wall portion 23 is larger than the outer diameter of the probe 12, and the inner peripheral surface of the side wall portion 23 is spaced from the outer peripheral surface of the probe 12. The inner peripheral surface of the side wall portion 23 is preferably inclined so as to be radially outward as it goes downward, but may be parallel to the axial direction. The lower surface of the side wall portion 23 forms a shoulder abutment surface 24 that abuts against the second surface 7 of the laminate 2. A recess 25 is provided on the lower surface of the shoulder member 13. The recess 25 is defined by a bottom surface 26 that is recessed with respect to the shoulder abutment surface 24 and faces the second surface 7 of the laminate 2, and the inner peripheral surface of the side wall portion 23, and receives the lower part of the probe 12. The bottom surface 26 forms the lower surface of the probe support portion 21. The shoulder member 13 is made of a material such as steel, ceramic, or cemented carbide.

[0029] As shown in FIG. 1, the drive mechanism 14 includes an anvil drive mechanism 27 that moves the anvil 11, a rotational drive mechanism 28 that rotates the rotor 18 including the probe 12 about an axis, an advance / retract drive mechanism 29 that moves the probe 12 forward and backward along the axis, and a shoulder drive mechanism 30 that moves the shoulder member 13.

[0030] The power source 15 is electrically connected to the first terminal 31 and the second terminal 32. The first terminal 31 is electrically connected to the anvil 11, and the second terminal 32 is electrically connected to the rotor 18. Even if the anvil 11 and the rotor 18 have partially non-conductive regions, the anvil 11 has electrical conductivity from the point where the first terminal 31 is electrically connected to the anvil abutment surface 17, and the rotor 18 has electrical conductivity from the point where the second terminal 32 is electrically connected to the tip of the probe 12.

[0031] FIG. 2(C) shows the flow of current when the tip of the probe 12 is inserted into the laminate 2 from the second surface 7, and a current is applied from the probe 12 to the anvil 11 through the laminate 2 by the power source 15 (see FIG. 1). The arrows shown in dot patterns indicate the direction of insertion of the probe 12, the thin black arrows indicate the direction of rotation of the probe 12, and the thick black arrows indicate the direction of the current. By applying a current, a nugget 33 (a portion in which the members to be joined are melted and solidified by resistance welding) is formed between the first member 3 and the intermediate member 4, and the first member 3 and the intermediate member 4 are joined to each other. However, the current not only flows straight from the probe 12 to the anvil 11, but also flows from the probe 12 to the shoulder member 13, which reduces the energy efficiency in performing resistance welding. Therefore, as shown in FIG. 2(A) or FIG. 2(B), it is preferable to partially insulate the probe 12 or the shoulder member 13.

[0032] In the description of the modified example of FIG. 2(A) and FIG. 2(B), the same reference numerals are used for the same configurations as those of the first embodiment, and the description thereof will be omitted. In the modified example shown in FIG. 2(A), the probe 41 includes a probe conductive portion 42 that extends along an axis, has a cylindrical shape, and is conductive, and an insulating probe insulating portion 43 that is provided along the outer circumferential surface of the probe conductive portion 42. The lower surface of the probe conductive portion 42 is not covered by the probe insulating portion 43. In the probe 41, it is the probe insulating portion 43 that slides against the inner circumferential surface of the through hole 20 of the shoulder member 13. Instead of the probe insulating portion 43 sliding against the inner circumferential surface of the through hole 20, a layer (not shown) that is highly wear-resistant and insulated from the probe conductive portion 42 by the probe insulating portion 43 may be provided along the outer circumferential surface of the probe insulating portion 43, and this layer may slide against the inner circumferential surface of the through hole 20. The probe insulating portion 43 can prevent a current from flowing from the probe 41 toward the shoulder member 13.

[0033] 2(B), the shoulder member 44 includes the probe support portion 21, the flange 22 (see FIG. 1), and the side wall portion 23, and also includes a conductive shoulder member main body 45, and a shoulder member insulating portion 46 having insulating properties provided along the shoulder abutment surface 24 and the region of the inner circumferential surface of the through hole 20 that comes into sliding contact with the probe 12. The shoulder member insulating portion 46 is preferably further provided along the inner circumferential surface of the side wall portion 23. The shoulder member insulating portion 46 can prevent or suppress a current from flowing from the probe 12 and the laminate 2 to the shoulder member 44.

[0034] In the above two modified examples, the probe conductive part 42 and the shoulder member main body 45 are made of, for example, a copper alloy (chromium copper, alumina-dispersed copper, tungsten copper alloy, etc.), conductive ceramic, cemented carbide, etc. The probe insulating part 43 and the shoulder member insulating part 46 are made of, for example, insulating ceramic, bakelite (phenolic resin), mica, etc.

[0035] The friction stir welding in the above-mentioned joining apparatus 1 is friction stir spot welding, and the appearance of the joint is improved by forming the shoulder abutment surface 24 in an annular shape. On the other hand, by changing the shape of the shoulder member 13 to that shown in Fig. 3(B), friction stir line welding can be achieved. In the shoulder member 13a shown in Fig. 3(B), configurations similar to those of the shoulder member 13 shown in Fig. 3(A) are designated by the same reference numerals with the suffix "a", and explanations of the common parts will be omitted, with only the differences being explained.

[0036] The shoulder member 13a shown in FIG. 3B includes a probe support portion 21a having a through hole 20a, a flange 22a, and a side wall portion 23a having a shoulder abutment portion 24a formed on the lower surface. When the shoulder member 13a is advanced along the second surface 7 while being pressed against the second surface 7, the side wall portion 23a is not provided on the rear side in the advancing direction of the shoulder member 13a, and the rear side in the advancing direction of the recess 25a is open so that the second member 5, which rises upward due to the insertion of the probe 12, is not caught. Therefore, the side wall portion 23a is U-shaped when viewed from below. Instead of the U-shaped shape, the side wall portion 23a may be formed by a pair of walls parallel to the advancing direction (not shown).

[0037] A method for bonding the laminate 2 using the bonding apparatus 1 will be described with reference to FIG.

[0038] As shown in Fig. 4(A), an operator places the laminate 2, in which the layers have not yet been joined, between the anvil 11 and the probe 12 and shoulder member 13. The operator sets and operates the joining apparatus 1 so that the control device 16 (see Fig. 1) moves the anvil 11, shoulder member 13, and probe 12 via the drive mechanism 14 (see Fig. 1) to perform friction stir spot joining and resistance spot joining.

[0039] 4(B), the anvil 11 presses the first surface 6 of the laminate 2 upward, and the shoulder member 13 presses the second surface 7 of the laminate 2 downward. With the laminate 2 pressed by the anvil 11 and the shoulder member 13, the probe 12 advances from the second surface 7 side toward the laminate 2 while rotating about its axis.

[0040] As shown in FIG. 4(C), the tip of the probe 12 penetrates into the second member 5. The second member 5 is deformed, and an amount equivalent to the portion pushed aside by the probe 12 is received in the recess 25 of the shoulder member 13. In the vicinity of the probe 12, the second member 5 undergoes plastic flow due to frictional heat caused by the rotation of the probe 12, and a flow region having an annular or circular shape as viewed from above is formed. After the tip of the probe 12 reaches the intermediate member 4, the control device 16 (see FIG. 1) applies a current between the probe 12 and the anvil 11. The position of the tip of the probe 12 is managed by the insertion depth of the probe 12, the plunge pressure (plunging load) of the probe 12 into the laminate 2, the rotation load of the probe 12, or the like.

[0041] As shown in FIG. 4(D), while a current flows between the probe 12 and the anvil 11, the probe 12 moves further downward while rotating, and the tip of the probe 12 penetrates the intermediate member 4. When a current flows between the probe 12 and the anvil 11, a molten part 34 is formed in the first member 3 and the intermediate member 4 by resistance heating of the first member 3 and the intermediate member 4 and frictional heat due to the rotation of the probe 12. In addition, in the vicinity of the probe 12, not only the second member 5 but also the intermediate member 4 undergoes plastic flow. Therefore, the part of the intermediate member 4 pushed aside by the probe 12 penetrates toward the second member 5 along the side of the probe 12. At this time, the temperature decreases and the fluidity decreases as the intermediate member 4 moves away from the probe 12, so that the part of the intermediate member 4 that penetrates into the second member 5 is pushed outward in the radial direction. Therefore, in the vicinity of the probe 12 of the intermediate member 4, a hook 35 is formed that extends outward in the radial direction toward the upper end.

[0042] As shown in Fig. 4(E), the control device 16 (see Fig. 1) stops the current flow between the probe 12 and the anvil 11, and the probe 12 retracts along the axis while rotating. Furthermore, the anvil 11 and the shoulder member 13 stop applying pressure to the laminate 2 and move away from the laminate 2. When the current is stopped and the probe 12 moves away, the molten part 34 (see Fig. 4(D)) solidifies to form a nugget 33, and the first member 3 and the intermediate member 4 are joined to each other. Furthermore, a hook 35 is formed by the second member 5 and the intermediate member 4 that have been plastically flowed by the rotation of the probe 12, and therefore the second member 5 and the intermediate member 4 are joined to each other.

[0043] The effects of the first embodiment will be described.

[0044] Since the anvil 11 and the probe 12 used for friction stir welding also serve as electrodes for resistance spot welding, the size and number of devices and the length of the production line can be suppressed, and capital investment can be suppressed, compared to the case where separate friction stir welding devices and resistance spot welding devices are prepared. Also, since friction stir welding and resistance spot welding can be performed simultaneously, an increase in processing time can be suppressed.

[0045] If dissimilar materials were resistance welded, brittle intermetallic compounds would be generated, which could reduce the joint strength. In this embodiment, the second member 5 and the intermediate member 4, which are dissimilar materials, are joined by friction stir welding, which can prevent the joint strength from being reduced by intermetallic compounds.

[0046] Not only the resistance heat generated by the current flow but also the frictional heat caused by the rotation of the probe 12 contributes to the melting of the first member 3 and the intermediate member 4, so that it is possible to reduce the amount of energy consumed for resistance welding. Furthermore, while the toughness of the nugget 33 decreases when the molten portion 34 is rapidly cooled, in this embodiment, after the current flow is stopped, the probe 12 is pulled out from the laminate 2 while being rotated, so that the frictional heat caused by the rotation of the probe 12 is transmitted to the molten portion 34, the molten portion 34 is prevented from being rapidly cooled, and the toughness of the nugget 33 is prevented from being reduced.

[0047] 2(A) or 2(B), in the modified example including the probe insulating portion 43 or the shoulder member insulating portion 46, the passage of electricity to the shoulder member 13 is suppressed or prevented, and the current path is limited. As a result, almost no current flows inside the second member 5, melting of the second member 5 is prevented, and the joining quality can be stabilized and improved. In addition, the electrical safety of the equipment can be improved.

[0048] 5 shows a joining device 51 according to the second embodiment. The same components as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted. The joining device 51 according to the second embodiment includes an anvil 11, a rotor 53 including a probe 52, a drive mechanism 54 including an anvil drive mechanism 27, a rotation drive mechanism 28, and an advance / retract drive mechanism 29, and a control device 16 that controls the operation of the advance / retract drive mechanism 29 and the power source 15.

[0049] The rotor 53 rotates around the axis as a whole. The rotor 53 includes a body 55 having a generally cylindrical shape centered on the axis, and a probe 52 extending downward along the axis from the lower surface of the body 55. The rotor 53 is conductive. The probe 52 preferably has a thread groove on its outer circumferential surface. The lower surface of the body 55 forms a shoulder 56 that is recessed upward from the radial outer edge toward the central portion from which the probe 52 extends. The probe 52 is made of, for example, a copper alloy (chromium copper, alumina-dispersed copper, tungsten copper alloy, etc.), conductive ceramic, or cemented carbide.

[0050] The method of joining the layers of the laminate 2 together using the joining device 51 according to the second embodiment is similar to that of the first embodiment, except that the shoulder member 13 (see FIG. 1) is not used. The concave shoulder 56 of the rotor 53 receives a part of the second member 5 pushed out by the insertion of the probe 52, similar to the concave portion 25 (see FIG. 1) of the shoulder member 13 in the first embodiment.

[0051] The third embodiment will be described with reference to Figs. 6 to 11. Configurations common to the first embodiment are given the same reference numerals and description thereof will be omitted. Fig. 6 is a cross-sectional view of a plane including an axis, showing a joining device 101 according to the third embodiment and a state in the middle of joining a laminate 2 joined by the joining device 101. In the first embodiment, the power source 15 is electrically connected to the anvil 11 and the probe 12 (see Fig. 1), whereas in the third embodiment, the power source 15 is electrically connected to the anvil 11 and the shoulder member 13.

[0052] The power source 15 is electrically connected to the first terminal 31 and the second terminal 32. The first terminal 31 is electrically connected to the anvil 11, and the second terminal 32 is electrically connected to the shoulder member 13. Even if the anvil 11 and the shoulder member 13 have a partially non-conductive region, the anvil 11 has conductivity from the point where the first terminal 31 is electrically connected to the anvil abutment surface 17, and the shoulder member 13 has conductivity from the point where the second terminal 32 is electrically connected to the shoulder abutment surface 24.

[0053] FIG. 7 shows a modified example of the probe 12. In the description of this modified example, the same components as those in the third embodiment are denoted by the same reference numerals, and the description thereof will be omitted. In the modified example shown in FIG. 7, the probe 41 includes a probe conductive portion 42 that extends along an axis, has a cylindrical shape, and is conductive, and an insulating probe insulating portion 43 that is provided along the outer circumferential surface of the probe conductive portion 42. In the probe 41, it is the probe insulating portion 43 that slides against the inner circumferential surface of the through hole 20 of the shoulder member 13. The probe insulating portion 43 can prevent a current from flowing from the shoulder member 13 to the probe 41. This can prevent a deterioration in energy efficiency when performing resistance welding.

[0054] FIG. 8(A) shows the same shoulder member 13 as shown in FIG. 6. FIGS. 8(B) to 8(D) show its modified examples. The shoulder member 13 shown in FIG. 8(A) is entirely conductive. A shoulder member 61 shown in FIG. 8(B) includes a shoulder member conductive portion 62 extending from the connection point of the second terminal 32 to the shoulder abutment surface 24, and a shoulder member insulating portion 63 provided in a region including a portion on the inner circumferential surface of the through hole 20 that slides against the probe 12. A shoulder member 64 shown in FIG. 8(C) includes an inner layer 65 including the inner circumferential surface of the through hole 20 and having conductivity, an outer layer 66 to which the second terminal 32 is connected and including the shoulder abutment surface 24 and having conductivity, and a shoulder member insulating portion 67 disposed between the inner layer 65 and the outer layer 66 to insulate the inner layer 65 from the outer layer 66. A shoulder member 68 shown in Fig. 8(D) includes an inner layer 65 having conductivity including the inner circumferential surface of the through hole 20, an outer layer 69 to which the second terminal 32 is connected and having conductivity including an outer portion of the shoulder abutting surface 24, and a shoulder member insulating portion 70 disposed between the inner layer 65 and the outer layer 69, including an inner portion of the shoulder abutting surface 24, and providing insulation between the inner layer 65 and the outer layer 69. In the shoulder members 61, 64, 68 shown in Figs. 8(B) to 8(D), the shoulder member insulating portions 63, 67, 70 prevent current from flowing from the shoulder members 61, 64, 68 to the probe 12 (see Fig. 6).

[0055] 7 and 8, the probe conductive part 42, the shoulder member conductive part 62, the inner layer 65 and the outer layers 66, 69 are made of, for example, a copper alloy (chromium copper, alumina-dispersed copper, tungsten-copper alloy, etc.), conductive ceramic, cemented carbide, etc. The probe insulating part 43 and the shoulder member insulating parts 63, 67, 70 are made of, for example, insulating ceramic, bakelite (phenolic resin), mica, etc.

[0056] The friction stir welding in the above-mentioned joining apparatus 101 is friction stir spot welding. By applying the shoulder member 13a shown in Fig. 3(B) according to the modified example of the first embodiment to the joining apparatus 101 of the third embodiment, friction stir line welding can be performed.

[0057] FIG. 9 shows the current flow that changes depending on the configuration of the anvil 11. The arrows superimposed on the laminate 2 indicate the current flow. The contour of the anvil 11 shown in FIG. 9(A) matches the contour of the probe 12 when viewed from the axial direction, or is located radially outward from the contour of the probe 12, and is located inside the inner contour of the shoulder abutment surface 24. The contact area of ​​the anvil 11 with the laminate 2 is relatively small, so that the pressure from the anvil 11 to the laminate 2 is stable. The contour of the anvil 11b shown in FIG. 9(B) matches the inner contour of the shoulder abutment surface 24, or is located radially outward from the inner contour of the shoulder abutment surface 24, and matches the outer contour of the shoulder abutment surface 24, or is located radially inward from the outer contour of the shoulder abutment surface 24. The anvil 11b has a relatively large contact area with the laminate 2 compared to the example shown in FIG. 9(A), and the current flows radially outward, so that the nugget 33 (see FIG. 6) is expanded radially. The anvil 11c shown in FIG. 9(C) has approximately the same size as the anvil 11b shown in FIG. 9(B), but the central portion 71 intersecting the axis is made of a material having higher rigidity than the outer peripheral portion 72 surrounding the central portion 71. Therefore, deformation of the anvil 11c when the anvil 11c is pressed against the laminate 2 is suppressed. The contour of the central portion 71 may be made larger than the inner contour of the shoulder abutment surface 24 when viewed from the axial direction, and in this case, deformation of the laminate 2 is suppressed. The anvil 11d shown in FIG. 9(D) has approximately the same size as the anvil 11b shown in FIG. 9(B), but the central portion 71 intersecting the axis is made of a material having lower rigidity than the outer peripheral portion 72 surrounding the central portion 71. When the anvil 11d is pressed against the laminate 2, pressure is applied to the outer peripheral portion 72 to ensure adhesion. Therefore, the current flows from the shoulder member 13 toward the outer peripheral portion 72. The anvils 11, 11b, 11c, and 11d are preferably circular when viewed in the axial direction.

[0058] With reference to FIG. 10, a method for bonding the laminate 2 using the bonding device 101 will be described.

[0059] As shown in Fig. 10(A), an operator places the laminate 2, in which each layer has not yet been joined, between the anvil 11 and the probe 12 and shoulder member 13. The operator sets and operates the joining device 101 so that the control device 16 (see Fig. 1) moves the anvil 11, shoulder member 13, and probe 12 via the drive mechanism 14 (see Fig. 1) to perform friction stir spot joining and resistance spot joining.

[0060] 10(B), the anvil 11 presses the first surface 6 of the laminate 2 upward, and the shoulder member 13 presses the second surface 7 of the laminate 2 downward. With the laminate 2 pressed by the anvil 11 and the shoulder member 13, the probe 12 advances from the second surface 7 side toward the laminate 2 while rotating about its axis.

[0061] As shown in FIG. 10(C), the tip of the probe 12 penetrates into the second member 5. The second member 5 is deformed, and an amount equivalent to the portion pushed aside by the probe 12 is received in the recess 25 of the shoulder member 13. In the vicinity of the probe 12, the second member 5 undergoes plastic flow due to frictional heat caused by the rotation of the probe 12, and a flow region having an annular or circular shape as viewed from above is formed. After the tip of the probe 12 reaches the intermediate member 4, the control device 16 (see FIG. 6) applies a current between the shoulder member 13 and the anvil 11. The position of the tip of the probe 12 is controlled by the insertion depth of the probe 12, the plunge pressure (plunging load) of the probe 12 into the laminate 2, the rotation load of the probe 12, or the like.

[0062] As shown in FIG. 10(D), while a current flows between the shoulder member 13 and the anvil 11, the probe 12 moves further downward while rotating, and the tip of the probe 12 penetrates the intermediate member 4. When a current flows between the shoulder member 13 and the anvil 11, a molten part 34 is formed in the first member 3 and the intermediate member 4 by resistance heating of the first member 3 and the intermediate member 4 and frictional heat due to the rotation of the probe 12. In addition, in the vicinity of the probe 12, not only the second member 5 but also the intermediate member 4 undergoes plastic flow. Therefore, the part of the intermediate member 4 pushed aside by the probe 12 penetrates toward the second member 5 along the side of the probe 12. At this time, the temperature decreases and the fluidity decreases as the intermediate member 4 moves away from the probe 12, so that the part of the intermediate member 4 that penetrates into the second member 5 is pushed outward in the radial direction. Therefore, in the vicinity of the probe 12 of the intermediate member 4, a hook 35 is formed that extends outward in the radial direction toward the upper end.

[0063] As shown in Fig. 10(E), the control device 16 (see Fig. 6) stops the current flow between the shoulder member 13 and the anvil 11, and the probe 12 retracts along the axis while rotating. Furthermore, the anvil 11 and the shoulder member 13 stop applying pressure to the laminate 2 and move away from the laminate 2. When the current is stopped and the probe 12 moves away, the molten part 34 (see Fig. 10(D)) solidifies to form a nugget 33, and the first member 3 and the intermediate member 4 are joined to each other. Furthermore, a hook 35 is formed by the second member 5 and the intermediate member 4 that have been plastically flowed by the rotation of the probe 12, and therefore the second member 5 and the intermediate member 4 are joined to each other.

[0064] With reference to FIG. 11, a case where the time when the current starts to flow between the shoulder member 13 and the anvil 11 is changed will be described. As shown in FIG. 11(A), if the current starts to flow before the tip of the probe 12 reaches the second surface 7 of the laminate 2 or at the same time, a wide range of the laminate 2 (such as the surface between the probe 12 and the shoulder abutment surface 24 in the second member 5) is softened by resistance heating due to the current flow, so that the probe 12 can easily penetrate into the laminate 2 and the penetration speed can be increased. The same is true when the current starts to flow before the tip of the probe 12 reaches the intermediate member 4 of the laminate 2. As shown in FIG. 11(B), if the current starts to flow when the tip of the probe 12 reaches the boundary surface between the second member 5 and the intermediate member 4, the second member 5 is softened from the outer peripheral surface of the probe 12, which is the starting point of the generation of the hook 35 (see FIG. 1), toward the shoulder abutment surface 24, and the tip of the hook 35 can be guided outward. Furthermore, since the intermediate member 4 also softens intensively directly above the anvil 11, the generation of hooks 35 is promoted and it is possible to suppress the inflow of material into the interface between the first member 3 and the intermediate member 4. As shown in Fig. 11(C), even if the current starts to flow after the tip of the probe 12 passes over the boundary surface between the second member 5 and the intermediate member 4, the same effect as that shown in Fig. 11(B) is achieved.

[0065] The effects of the third embodiment will be described.

[0066] Since the anvil 11 and the probe 12 used for friction stir welding also serve as electrodes for resistance spot welding, the size and number of devices and the length of the production line can be suppressed, and capital investment can be suppressed, compared to the case where separate friction stir welding devices and resistance spot welding devices are prepared. Also, since friction stir welding and resistance spot welding can be performed simultaneously, an increase in processing time can be suppressed.

[0067] If dissimilar materials were resistance welded, brittle intermetallic compounds would be generated, which could reduce the joint strength. In this embodiment, the second member 5 and the intermediate member 4, which are dissimilar materials, are joined by friction stir welding, which can prevent the joint strength from being reduced by intermetallic compounds.

[0068] Not only the resistance heat generated by the current flow but also the frictional heat caused by the rotation of the probe 12 contributes to the melting of the first member 3 and the intermediate member 4, so that it is possible to reduce the amount of energy consumed for resistance welding. Furthermore, while the toughness of the nugget 33 decreases when the molten portion 34 is rapidly cooled, in this embodiment, after the current flow is stopped, the probe 12 is pulled out from the laminate 2 while being rotated, so that the frictional heat caused by the rotation of the probe 12 is transmitted to the molten portion 34, the molten portion 34 is prevented from being rapidly cooled, and the toughness of the nugget 33 is prevented from being reduced.

[0069] As shown in Fig. 7 or Fig. 8, in the modified example including the probe insulating portion 43 or the shoulder member insulating portion 63, 67, 70, the passage of electricity to the probe 12 is suppressed or prevented, and the current path is limited. This improves the electrical safety of the equipment. Also, in the shoulder members 64, 68 shown in Fig. 8(C) and Fig. 8(D), a conductive material may be used for the portion that slides against the probe 12 in the through hole 20. This allows a material with high wear resistance to be placed in this portion, improving the durability of the shoulder members 64, 68.

[0070] In the above-mentioned first to third embodiments and their modified examples, the anvil 11 (see FIG. 1, etc.) may be changed to anvils 111, 121 shown in FIG. 12 or FIG.

[0071] The anvil 111 shown in FIG. 12 and FIG. 13 has a cylindrical shape and includes an anvil abutment surface 112 that supports the first surface 6 of the laminate 2. The anvil abutment surface 112 includes a circular insulating region 113 arranged so as to intersect with an extension of the axis of the probe 12, and a ring-shaped conductive region 114 arranged so as to surround the insulating region 113. The diameter of the insulating region 113 is preferably 2 mm or more. The shape of the conductive region 114 does not have to be a ring shape as long as it is a ring shape, and the shape of the insulating region 113 does not have to be a circle shape as long as it is arranged inside the ring-shaped conductive region. The portion of the anvil 111 from the conductive region 114 to the portion to which the first terminal 31 (see FIG. 1) is connected is conductive.

[0072] As shown in FIG. 13, the current flows from the probe 12 (FIG. A) or the shoulder member 13 (FIG. B) to the conductive region 114 of the anvil 111. Therefore, the nugget 115 is also formed in an annular shape. If the joining areas are equal to each other, the annular nugget 115 has a larger outer diameter than the circular nugget 33 (see FIG. 2), and therefore the joining strength, especially the joining strength against the load in the peeling direction, is increased. In addition, the anvil 111 including the circular insulating region 113 and the annular conductive region 114 can be manufactured at a lower cost than the anvil 121 shown in FIG. 14(A). In the mode in which the current flows between the anvil 11 and the shoulder member 13 as shown in FIG. 13(B), the current path is on the outside in the radial direction, and the outer diameter of the nugget 115 formed is larger than that in the mode in which the current flows between the anvil 11 and the probe 12 as shown in FIG. 13(A), and therefore the joining strength is increased.

[0073] The anvil 121 shown in FIG. 14(A) includes an anvil abutment surface 122 that supports the first surface 6 (see FIG. 13) of the laminate 2. The anvil abutment surface 122 includes a cross-shaped insulating region 123 and four conductive regions 124 that are separated from each other by the insulating region 123. The center of the cross shape of the insulating region 123 is on an extension of the axis of the probe 12. The insulating region 123 does not have to be cross-shaped if the conductive region 124 is divided into a plurality of regions. For example, the insulating region 123 may be composed of a plurality of bands extending radially from the center, or may be composed of a plurality of bands extending in the vertical and horizontal directions.

[0074] A current flows from the probe 12 or the shoulder member 13 to the conductive region 114 of the anvil 111. When the anvil 121 having the cross-shaped insulating region 123 is used, the current is divided and flows toward four mutually isolated conductive regions 124. Therefore, as shown in FIG. 14(B), four mutually isolated island-like nuggets 125 are formed. Since the nuggets 125 are formed in a dispersed island shape, the stress associated with the joint can be dispersed and received. In addition, compared to the case where the insulating region 123 is not present, the current density increases, so that the first member 3 and the intermediate member 4 are more likely to melt, and the nugget 125 is more likely to be formed.

[0075] Although the description of the specific embodiment is finished above, the present invention is not limited to the above embodiment and modified examples, and can be modified widely. The second member and the intermediate member may be joined by resistance welding other than spot welding. The insulating part shown in FIG. 3(A) and / or (B) may be applied to the modified example in which the shoulder member shown in FIG. 4(B) is applied. The current may flow from the anvil to the shoulder member. The timing at which the current flows between the shoulder member 13 and the anvil 11 in FIG. 10(D) may be when or after the probe 12 reaches the first member 3, which allows the ring-shaped nugget 33 to be stably produced and improves the joining strength. [Explanation of symbols]

[0076] 1,51,101:Joining equipment 2: Laminate 3: First member 4: Intermediate parts 5: Second member 6: 1st page 7:Second side 11, 11b, 11c, 11d, 111, 121: Anvil 12,41,52: Probe 13, 13a, 44, 61, 64, 68: Shoulder member 14,54: Drive mechanism 15: Power supply 16: Control device 17, 112, 122: Anvil contact surface 20:Through hole 24, 24a: Shoulder contact surface 25, 25a: recess 113, 123: Insulating area 114,124: Conductive areas

Claims

1. A joining device for joining each member to each other in a laminate including a first member, an intermediate member, and a second member stacked in this order, each of which is electrically conductive and extends along a predetermined main surface, comprising: an anvil including an anvil contact surface for supporting a first surface of the laminate that forms a surface on the first member side, the anvil contact surface including an insulating region and a conductive region; a probe that is at least partially conductive, the probe being rotatable about an axis extending in a direction intersecting the main surface and movable toward and away from the second member along the axis so as to face a second surface that forms a surface of the laminate on the second member side at a position corresponding to the anvil; a drive mechanism for rotating the probe about the axis and moving the probe forward and backward along the axis; a power source electrically connected to the anvil and the probe to pass an electrical current between the anvil and the probe through the stack; A control device that controls the operation of the drive mechanism and the power source; Equipped with A joining device for resistance welding the first member and the intermediate member to each other and friction stir welding the second member and the intermediate member to each other by rotating the probe and advancing the probe into the stack from the side of the second surface until the tip of the probe penetrates the intermediate member, and after the tip of the probe reaches the intermediate member, passing an electric current between the probe and the anvil through the pressurized stack.

2. A joining device for joining each member to each other in a laminate including a first member, an intermediate member, and a second member, each of which is electrically conductive and extends along a predetermined main surface, stacked in this order, comprising: an anvil including an anvil contact surface for supporting a first surface of the laminate that forms a surface on the first member side, the anvil contact surface including an insulating region and a conductive region; a probe that is rotatable about an axis extending in a direction intersecting the main surface and that is movable toward and away from the second member along the axis so as to face a second surface that forms a surface of the laminate on the second member side at a position corresponding to the anvil; a shoulder member including a through hole through which the probe is inserted and a shoulder contact surface to be pressed against the second surface, the shoulder member being at least partially conductive; a drive mechanism for rotating the probe about the axis and moving the probe forward and backward along the axis; a power source electrically connected to the anvil and the shoulder member for passing an electrical current between the anvil and the shoulder member through the laminate; A control device that controls the operation of the drive mechanism and the power source; Equipped with A joining device for resistance welding the first member and the intermediate member to each other and friction stir welding the second member and the intermediate member to each other by rotating the probe and advancing the probe into the stack from the side of the second surface until the tip of the probe penetrates the intermediate member, and after the tip of the probe reaches the intermediate member, passing an electric current between the shoulder member and the anvil through the pressurized stack.

3. The bonding device according to claim 2 , wherein the shoulder member includes a recess that is recessed relative to the shoulder abutment surface to define a bottom surface facing the second surface and that receives a portion of the probe.

4. 4. The joining device according to claim 1, wherein the insulating region is disposed on the anvil contact surface so as to intersect with an extension of the axis.

5. The joining device according to claim 4 , wherein the conductive region is arranged in an annular shape surrounding the insulating region.

6. 5. The joining device according to claim 1, wherein the conductive region on the anvil contact surface is divided into a plurality of isolated regions by the insulating region.

Citation Information

Patent Citations

  • Process for joining at least two metal workpieces lying against one another

    DE102016206759A1

  • Structure and method for joining dissimilar material

    JP2005111489A

  • Joining method

    JP2007237253A

  • Friction stir welding equipment

    JP2007268543A

  • Apparatus for spot welding

    KR1020090067434A