Method and apparatus for manufacturing bonded laminated cores
By applying and actively drying curing accelerators for anaerobic and instant adhesives before press working oil, the method addresses productivity and adhesive strength issues in adhesive laminated core manufacturing, enabling efficient production of high-performance stators.
Patent Information
- Application Number
- JP2023514664
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-14
- Filing Date
- 2022-04-13
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2042-04-13
AI Technical Summary
Existing methods for manufacturing adhesive laminated cores, such as those used in rotating electric machines, face challenges in achieving high productivity while ensuring sufficient adhesive strength due to the interaction between press working oil and curing accelerators, which can affect punching workability and adhesive hardening.
The method involves applying a hardening accelerator for anaerobic adhesives and instant adhesives to the steel strip before press working oil, actively drying them to form a curing accelerator layer, and then laminating and bonding the steel plate parts to maintain high concentrations of the accelerators, ensuring early development of high adhesive strength.
This approach enhances productivity and ensures sufficient adhesive strength, allowing for the rapid manufacturing of high-performance stators for rotating electric machines with reduced manufacturing costs.
Smart Images

Figure 0007580580000003 
Figure 0007580580000004 
Figure 0007580580000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for manufacturing a bonded laminated core. This application claims priority based on Patent Application No. 2021-068134, filed in Japan on April 14, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] For example, a rotating electric machine used as an electric motor includes a laminated core. This laminated core is manufactured by punching a strip-shaped steel plate into a predetermined shape in several steps while intermittently feeding the strip-shaped steel plate, and stacking the obtained steel plate parts. The steel plate parts are fixed to each other by welding, bonding, crimping, etc., but among these, a fixing method by bonding has attracted attention from the viewpoint of effectively suppressing iron loss of the laminated core.
[0003] For example, Patent Document 1 listed below discloses a method for producing a metal sheet laminate by sequentially performing multiple press processes on a hoop material with press processing oil applied to one or both sides, applying an adhesive to one side of the hoop material, performing an outline punching process to obtain a metal sheet, and stacking and adhering a predetermined number of the metal sheets, in which a hardening accelerator is added to the press processing oil. According to this method for manufacturing a metal sheet laminate, by adding a hardening accelerator to the press processing oil, bonding between the metal sheets is achieved quickly and strongly without removing the press processing oil, and it is explained that this makes it possible to simplify the manufacturing process and reduce the size of the dies in the progressive die device, thereby improving product quality and productivity and reducing the size of the manufacturing equipment.
[0004] Furthermore, the following Patent Document 2 discloses a punching and laminating press method for punching steel plate parts of a predetermined shape from an intermittently fed strip steel plate and laminating the steel plate parts, the punching and laminating press method including a first application step of applying either an adhesive or a hardening accelerator for promoting hardening of the adhesive to the underside of the strip steel plate upstream of a press processing position where the steel plate parts are punched from the strip steel plate, and a second application step of applying the other of the adhesive and the hardening accelerator to the upper surface of the strip steel plate at the press processing position. It is explained that this punching and laminating press method makes it possible to significantly shorten the adhesive curing time by performing the first and second application processes, thereby increasing the productivity of cores manufactured by stacking multiple steel plate parts. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent No. 4648765 [Patent Document 2] Japanese Patent No. 6164029 Summary of the Invention [Problem to be solved by the invention]
[0006] According to the manufacturing method of the metal sheet laminate in the above-mentioned Patent Document 1, the adhesion between the metal sheets can be rapidly achieved by using a hardening accelerator. Since the hardening accelerator is applied in a diluted state by adding press processing oil, if a higher hardening acceleration effect is required, the content of the hardening accelerator needs to be increased to a considerable amount. However, in this case, the proportion of the press processing oil is reduced, which may affect the punching workability when punching the metal sheets. In addition, the punching lamination press method of Patent Document 2 claims to be able to significantly shorten the curing time of the adhesive. However, even in this case, no consideration is given at all to the effect of press oil, which is essential for punching, on the curing accelerator.
[0007] In this way, in order to further increase the productivity of bonded laminated cores, it is necessary to more effectively utilize the lubricating function of the press processing oil when punching the steel sheets and the hardening accelerator when bonding the steel sheets. However, in the past, sufficient consideration had not been given to the application form of the hardening accelerator.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a method and an apparatus for manufacturing bonded laminated cores that can achieve higher productivity while ensuring sufficient adhesive strength when manufacturing bonded laminated cores. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention employs the following means. (1) A method for producing a bonded laminated core according to one aspect of the present invention comprises the steps of: A method for manufacturing an adhesive laminated core, comprising the steps of: pressing a strip of steel plate coated with press processing oil on one or both sides; applying an anaerobic adhesive and an instant adhesive to one side of the strip of steel plate to obtain a plurality of steel plate parts; and laminating and bonding the steel plate parts together, the method comprising the steps of: Before applying the press processing oil, a hardening accelerator for anaerobic adhesives and a hardening accelerator for instant adhesives are applied to one or both sides of the strip-shaped steel sheet, and then dried to form a hardening accelerator layer. According to the method for manufacturing an adhesive laminated core described in (1) above, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are actively dried by applying heat or air, rather than natural drying. In this way, since the curing accelerator layer is formed by actively drying in advance, it is possible to suppress the curing accelerator from being mixed with the press processing oil applied in the post-processing and being diluted. Therefore, when the steel plate parts are laminated and bonded, the anaerobic adhesive curing accelerator mixes with the anaerobic adhesive while maintaining its high concentration, and the instant adhesive curing accelerator can also mix with the instant adhesive while maintaining its high concentration. Therefore, high adhesive strength can be developed early. Therefore, it is possible to obtain higher productivity while ensuring sufficient adhesive strength. Furthermore, by using an anaerobic adhesive that has high heat resistance and slow development of initial strength in combination with an instant adhesive that quickly develops initial strength, the steel plate parts can be handled immediately after being laminated and bonded. Therefore, the laminated and bonded adhesive laminated core can be transferred to the next process early or moved outside the work space, thereby freeing up the work space.
[0010] (2) In the method for producing an adhesive laminated core according to (1) above, The anaerobic adhesive curing accelerator and the instant adhesive curing accelerator may be arranged in a checkered pattern. According to the method for manufacturing an adhesive laminated core described in (2) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip, which makes it possible to make the adhesive strength along the coating surface uniform.
[0011] (3) In the method for producing an adhesive laminated core according to (1) above, The anaerobic adhesive curing accelerator and the instant adhesive curing accelerator may be mixed in advance and then applied to one or both sides of the strip steel plate and dried to form the curing accelerator layer. According to the method for manufacturing an adhesive laminated core described in (3) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip, which makes it possible to make the adhesive strength along the coating surface uniform.
[0012] (4) In the method for producing an adhesive laminated core according to (1) above, The curing accelerator for anaerobic adhesives and the curing accelerator for instantaneous adhesives may be arranged in a striped pattern to form the curing accelerator layer. According to the method for manufacturing an adhesive laminated core described in (4) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip, which makes it possible to make the adhesive strength along the coating surface uniform.
[0013] (5) In the method for producing an adhesive laminated core according to any one of the above (1) to (4), the following may be performed: The steel plate components include a first steel plate component and a second steel plate component, A first step of preparing the first steel plate part having a first surface, the hardening promotion layer formed on the first surface, and the press processing oil disposed on the hardening promotion layer; a second step of preparing the second steel plate component having a second surface and the anaerobic adhesive and the instant adhesive disposed on the second surface; A third step of overlapping and adhering the first steel plate part and the second steel plate part so that the first surface and the second surface face each other; has. According to the method for manufacturing an adhesive laminated core described in (5) above, in the first step, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are dried in advance to form a curing accelerator layer, and are in a state in which they are inhibited from mixing with the press processing oil. Therefore, when the first steel plate component and the second steel plate component are superimposed and bonded in the third step, the anaerobic adhesive curing accelerator can mix with the anaerobic adhesive while maintaining its high concentration, and the instant adhesive curing accelerator can also mix with the instant adhesive while maintaining its high concentration.
[0014] (6) In the method for producing an adhesive laminated core according to any one of the above (1) to (4), the following may be performed: The steel plate components include a first steel plate component and a second steel plate component, a fourth step of preparing the first steel plate component having a first surface, the hardening accelerating layer formed on the first surface, the press processing oil disposed on the hardening accelerating layer, and the anaerobic adhesive and the instant adhesive disposed on the press processing oil; A fifth step of providing the second steel plate component having a second surface; A sixth step of overlapping and adhering the first steel plate part and the second steel plate part so that the first surface and the second surface face each other; has. According to the method for manufacturing an adhesive laminated core described in (6) above, in the fourth step, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are dried in advance to form a curing accelerator layer, and are in a state in which they are inhibited from mixing with the press processing oil. Therefore, when the first steel plate component and the second steel plate component are superimposed and bonded in the sixth step, the anaerobic adhesive curing accelerator can mix with the anaerobic adhesive while maintaining its high concentration, and the instant adhesive curing accelerator can also mix with the instant adhesive while maintaining its high concentration.
[0015] (7) In the method for producing an adhesive laminated core according to any one of (1) to (6) above, The anaerobic adhesive curing accelerator may include an active ingredient that promotes anaerobic curing selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof. That is, the active ingredient that accelerates the curing of the anaerobic adhesive is selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof. Preferably, it may be selected from copper, iron, vanadium, cobalt, chromium, silver, and manganese, and combinations thereof. Desirably, it may be copper, iron, vanadium, cobalt, and chromium, and combinations thereof. Desirably, it is provided in the form of a metal oxide or salt. Preferably, it is one or a combination of two or more selected from vanadium acetylacetonate, vanadyl acetylacetonate, vanadyl stearate, vanadium propoxide, vanadium butoxide, vanadium pentoxide, cobalt naphthenate, manganese naphthenate, copper hexanoate, copper (II) bis(2-ethylhexanoate), and the like. According to the adhesive laminated core manufacturing method described in (7) above, the anaerobic adhesive hardens quickly and completely, which is particularly advantageous for manufacturing processes that require short manufacturing times and suppression of outgassing, thereby improving productivity.
[0016] (8) In the method for producing an adhesive laminated core according to any one of (1) to (7) above, The instant adhesive curing accelerator may contain an active ingredient that accelerates the curing of a 2-cyanoacrylate adhesive selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof. Specifically, specific examples of the active ingredient that accelerates the hardening of the instant adhesive include organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof. Preferably, one or a combination of two or more selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, N,N-diethylaniline, etc. may be used. According to the adhesive laminated core manufacturing method described in (8) above, the instant adhesive hardens quickly and completely, which is particularly advantageous for manufacturing processes that require short manufacturing times or suppression of outgassing, and thus provides the advantage of improving productivity.
[0017] (9) In the method for producing an adhesive laminated core according to any one of (1) to (8) above, At least one of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator may be diluted with a solvent such as a ketone-based solvent, an alcohol-based solvent, an ester-based solvent, a glycol ether-based solvent, a hydrocarbon-based solvent, a halogenated hydrocarbon-based solvent, an ether-based solvent, a glycol-based solvent, or an amine-based solvent. The solvent may be one or a combination of two or more selected from the above solvents. In terms of manufacturing an adhesive laminated core, preferred examples include one or a combination of two or more selected from ethyl acetate, acetone, ethanol, methanol, butanol, toluene, and heptane.
[0018] (10) In the method for producing an adhesive laminated core according to any one of (1) to (9) above, The bonded laminated core may be a stator for a rotating electrical machine. According to the adhesive laminated core manufacturing method described in (10) above, higher productivity can be achieved while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electric machines that have high performance but low manufacturing costs.
[0019] (11) An apparatus for manufacturing a bonded laminated core according to one aspect of the present invention comprises: An apparatus for manufacturing a bonded laminated core having a plurality of steel plate parts punched out from a strip-shaped steel plate, A press working oil application unit that applies press working oil to one side or both sides of the strip steel plate; a press working unit that applies press working to the strip steel plate; an adhesive application section that applies an anaerobic adhesive and an instant adhesive to one surface of the strip steel plate; a hardening accelerator layer forming section for forming a hardening accelerator layer by applying and drying an anaerobic adhesive hardening accelerator and an instant adhesive hardening accelerator on one or both sides of the strip steel plate before applying the press processing oil; Equipped with. According to the adhesive laminate core manufacturing device described in (11) above, the curing accelerator layer forming section actively dries both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator by applying heat or air, rather than natural drying. In this way, the curing accelerator layer is formed by actively drying in advance, so that the curing accelerator is prevented from being mixed with the press processing oil applied in the post-processing and being diluted. Therefore, when the steel plate parts are laminated and bonded, the anaerobic adhesive curing accelerator mixes with the anaerobic adhesive while maintaining its high concentration, and the instant adhesive curing accelerator also mixes with the instant adhesive while maintaining its high concentration. Therefore, high adhesive strength can be developed early. Therefore, it is possible to obtain higher productivity while ensuring sufficient adhesive strength.
[0020] (12) In the adhesive laminated core manufacturing apparatus described in (11) above, The curing accelerator layer forming section may include a nozzle that applies the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator in a checkered pattern. According to the adhesive laminated core manufacturing apparatus described in (12) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip by the nozzle, so that the adhesive strength along the coating surface can be made uniform.
[0021] (13) In the adhesive laminated core manufacturing apparatus described in (11) above, The curing accelerator layer forming section may include a curing accelerator supply flow path through which the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are mixed in advance and flow, and a nozzle communicating with the curing accelerator supply flow path. According to the adhesive laminated core manufacturing apparatus described in (13) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip by the nozzle, so that the adhesive strength along the coating surface can be made uniform.
[0022] (14) The adhesive laminated core manufacturing apparatus according to (11), The curing accelerator layer forming section may include a nozzle that applies the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator in stripes. According to the adhesive laminated core manufacturing apparatus described in (14) above, the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be evenly distributed along the coating surface of the steel strip by the nozzle, so that the adhesive strength along the coating surface can be made uniform.
[0023] (15) The adhesive laminated core manufacturing apparatus according to (11) above may be configured as follows: A first stage having the hardening acceleration layer forming section; A second stage having a conveying section that sends out the strip steel plate transferred from the first stage toward the press working oil application section; Equipped with In the second stage, the conveying section, the press working oil application section, the press working section and the adhesive application section are arranged in this order along the feed direction of the strip steel plate. According to the bonded laminated core manufacturing apparatus described in (15) above, strip steel sheets on which hardening accelerating layers have been formed in advance can be prepared in the first stage. Then, the required number of strip steel sheets can be taken out of these strip steel sheets and moved to the second stage, where press processing oil can be applied, anaerobic adhesive and instant adhesive can be applied, and each steel sheet component can be bonded. In this way, even if the bonded laminated core manufacturing apparatus is divided into the first stage and the second stage, it is possible to obtain higher productivity while ensuring sufficient adhesive strength.
[0024] (16) In the adhesive laminated core manufacturing apparatus according to any one of (11) to (15), The anaerobic adhesive curing accelerator may include an active ingredient that promotes anaerobic curing selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof. That is, in the adhesive laminated core manufacturing apparatus described in (16) above, the hardening accelerator for the anaerobic adhesive may include an active ingredient that accelerates the anaerobic hardening. The active ingredient for promoting anaerobic hardening is selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof. It may be preferably selected from copper, iron, vanadium, cobalt, chromium, silver, and manganese, and combinations thereof. It may be preferably copper, iron, vanadium, cobalt, and chromium, and combinations thereof. It is preferably provided in the form of a metal oxide or salt. It is preferably one or a combination of two or more selected from vanadium acetylacetonate, vanadyl acetylacetonate, vanadyl stearate, vanadium propoxide, vanadium butoxide, vanadium pentoxide, cobalt naphthenate, manganese naphthenate, copper hexanoate, copper(II) bis(2-ethylhexanoate), and the like. According to the adhesive laminated core manufacturing apparatus described in (16) above, the anaerobic adhesive hardens quickly and completely, which is particularly advantageous for production that requires short production times and suppression of outgassing, and thus provides the advantage of improving productivity.
[0025] (17) In the adhesive laminated core manufacturing apparatus according to any one of (11) to (16), The instant adhesive curing accelerator may contain an active ingredient that accelerates the curing of a 2-cyanoacrylate adhesive selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof. That is, in the adhesive laminated core manufacturing apparatus described in (17) above, the instant adhesive hardening accelerator may include one containing an active ingredient that accelerates the hardening of a 2-cyanoacrylate adhesive. Specific examples of the active ingredient that accelerates the curing of the 2-cyanoacrylate adhesive include organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof. Preferably, one or a combination of two or more selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, N,N-diethylaniline, etc. may be used. According to the adhesive laminated core manufacturing apparatus described in (17) above, the instant adhesive hardens quickly and completely, which is particularly advantageous for manufacturing processes that require short manufacturing times or suppression of outgassing, and thus provides the advantage of improving productivity.
[0026] (18) In the adhesive laminated core manufacturing apparatus according to any one of (11) to (17), The bonded laminated core may be a stator for a rotating electrical machine. According to the adhesive laminated core manufacturing apparatus described in (18) above, higher productivity can be achieved while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electric machines that have high performance but low manufacturing costs. Effect of the Invention
[0027] According to the above-mentioned aspects of the present invention, it is possible to provide a method and an apparatus for manufacturing a bonded laminated core, which can ensure sufficient adhesive strength and achieve higher productivity when manufacturing a bonded laminated core. [Brief description of the drawings]
[0028] [Figure 1] 1 is a cross-sectional view of a rotating electric machine including a stator adhesive laminated core manufactured in accordance with each embodiment of the present invention. [Diagram 2] FIG. 2 is a side view of the stator bonded laminated core. [Diagram 3] 1 is a side view of a bonded laminated core manufacturing apparatus according to a first embodiment of the present invention. [Figure 4] 4 is a flowchart for explaining a method for manufacturing a bonded laminated core according to the embodiment. [Diagram 5] 5A and 5B are diagrams illustrating a first embodiment of a bonded laminated core manufacturing method according to the present embodiment, in which (a) is a partial vertical cross-sectional view showing lamination and bonding steps, and (b) is a cross-sectional view taken along the line AA of (a). [Figure 6] 5A and 5B are diagrams illustrating a second embodiment of the bonded laminated core manufacturing method according to the same embodiment, in which (a) is a partial vertical sectional view showing lamination and bonding steps, and (b) is a BB sectional view of (a). [Figure 7] 11A and 11B are diagrams illustrating a third embodiment of the bonded laminated core manufacturing method according to the embodiment, in which (a) is a partial vertical sectional view showing lamination and bonding steps, and (b) is a CC sectional view of (a). [Figure 8]10 is a flowchart for explaining a modified example of the bonded laminated core manufacturing method according to the embodiment. [Figure 9] FIG. 5 is a side view of a bonded laminated core manufacturing apparatus according to a second embodiment of the present invention. [Figure 10] 4 is a flowchart for explaining a method for manufacturing a bonded laminated core according to the embodiment. [Figure 11] 4A and 4B are diagrams illustrating a first embodiment of a bonded laminated core manufacturing method according to the present embodiment, in which (a) is a partial vertical cross-sectional view showing lamination and bonding steps, and (b) is a DD cross-sectional view of (a). [Figure 12] 5A and 5B are diagrams illustrating a second embodiment of the bonded laminated core manufacturing method according to the same embodiment, in which (a) is a partial vertical cross-sectional view showing the lamination and bonding steps, and (b) is an E-E cross-sectional view of (a). [Figure 13] 10A and 10B are diagrams illustrating a third embodiment of the bonded laminated core manufacturing method according to the embodiment, in which (a) is a partial vertical sectional view showing lamination and bonding steps, and (b) is an FF sectional view of (a). [Figure 14] 10 is a flowchart for explaining a modified example of the bonded laminated core manufacturing method according to the embodiment. [Figure 15] FIG. 11 is a side view of a bonded laminated core manufacturing apparatus according to a third embodiment of the present invention. [Figure 16] 4 is a flowchart for explaining a method for manufacturing a bonded laminated core according to the embodiment. [Figure 17] 1A and 1B are diagrams illustrating a first embodiment of a bonded laminated core manufacturing method according to the present embodiment, in which (a) is a partial vertical cross-sectional view showing lamination and bonding steps, and (b) is a GG cross-sectional view of (a). [Figure 18] 5A and 5B are diagrams illustrating a second embodiment of the bonded laminated core manufacturing method according to the same embodiment, in which (a) is a partial vertical sectional view showing the lamination and bonding steps, and (b) is an HH sectional view of (a). [Figure 19] 11A and 11B are diagrams illustrating a third embodiment of the bonded laminated core manufacturing method according to the same embodiment, in which (a) is a partial vertical cross-sectional view showing the lamination and bonding steps, and (b) is a cross-sectional view taken along line II of (a). [Figure 20]10 is a flowchart for explaining a modified example of the bonded laminated core manufacturing method according to the embodiment. [Figure 21] FIG. 11 is a side view of a bonded laminated core manufacturing apparatus according to a fourth embodiment of the present invention. [Figure 22] 4 is a flowchart for explaining a method for manufacturing a bonded laminated core according to the embodiment. [Diagram 23] 5A and 5B are diagrams illustrating a first embodiment of a bonded laminated core manufacturing method according to the embodiment, in which (a) is a partial vertical sectional view showing lamination and bonding steps, and (b) is a JJ sectional view of (a). [Figure 24] 5A and 5B are diagrams illustrating a second embodiment of the bonded laminated core manufacturing method according to the same embodiment, in which (a) is a partial vertical sectional view showing lamination and bonding steps, and (b) is a KK sectional view of (a). [Diagram 25] 11A and 11B are diagrams illustrating a third embodiment of the bonded laminated core manufacturing method according to the embodiment, in which (a) is a partial vertical sectional view showing the lamination and bonding steps, and (b) is an LL sectional view of (a). [Figure 26] 10 is a flowchart for explaining a modified example of the bonded laminated core manufacturing method according to the embodiment. [Figure 27] FIG. 11 is a side view of a bonded laminated core manufacturing apparatus according to a fifth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, a method and an apparatus for manufacturing a bonded laminated core according to each embodiment of the present invention will be described with reference to the drawings. Before that, a bonded laminated core for a stator (bonded laminated core, a stator for a rotating electric machine) manufactured in each embodiment will be described with reference to Figs. 1 and 2.
[0030] [Adhesive laminated core for stator] Fig. 1 is a cross-sectional view of a rotating electrical machine 10 including a stator adhesive laminated core 21 manufactured in each embodiment. Fig. 2 is a side view of the stator adhesive laminated core 21. 1 is an electric motor, specifically an AC motor, more specifically a synchronous motor, and even more specifically a permanent magnet field type motor. This type of motor is preferably used in, for example, electric vehicles.
[0031] 1, the rotating electric machine 10 includes a stator 20, a rotor 30, a case 50, and a rotating shaft 60. The stator 20 and the rotor 30 are housed in the case 50. The stator 20 is fixed within the case 50. 1, the rotating electric machine 10 is an inner rotor type in which the rotor 30 is located radially inside the stator 20. However, the rotating electric machine 10 may be an outer rotor type in which the rotor 30 is located outside the stator 20. Also, here, the rotating electric machine 10 is illustrated as a 12-pole, 18-slot three-phase AC motor. However, the number of poles, the number of slots, the number of phases, etc. can be changed as appropriate. The rotating electric machine 10 can rotate at a rotation speed of 1000 rpm by applying an excitation current with an effective value of 10 A and a frequency of 100 Hz to each phase, for example.
[0032] The stator 20 includes a stator adhesive laminated core 21 and a winding (not shown). The stator adhesive laminated core 21 includes an annular core back portion 22 and a plurality of teeth portions 23. Hereinafter, the direction of the central axis O of the stator adhesive laminated core 21 (or the core back portion 22) will be referred to as the axial direction, the radial direction (direction perpendicular to the central axis O) of the stator adhesive laminated core 21 (or the core back portion 22) will be referred to as the radial direction, and the circumferential direction (direction going around the central axis O) of the stator adhesive laminated core 21 (or the core back portion 22) will be referred to as the circumferential direction.
[0033] The core back portion 22 is formed in an annular shape when viewed in a plan view of the stator 20 in the axial direction. The multiple teeth portions 23 protrude radially inward from the inner circumference of the core back portion 22. The multiple teeth portions 23 are arranged at equal angular intervals in the circumferential direction. In the example of FIG. 1, 18 teeth portions 23 are provided at central angle intervals of 20 degrees about the central axis O. The multiple teeth portions 23 are formed to have the same shape and size as one another. Therefore, the multiple teeth portions 23 have the same thickness dimension as one another. The winding is wound around the teeth portion 23. The winding may be a concentrated winding or a distributed winding.
[0034] The rotor 30 is disposed radially inside the stator 20 (the stator adhesive laminated core 21). The rotor 30 includes a rotor core 31 and a plurality of permanent magnets 32. The rotor core 31 is formed in an annular (circular) shape and is disposed coaxially with the stator 20. A rotating shaft 60 is disposed within the rotor core 31. The rotating shaft 60 is fixed to the rotor core 31. The multiple permanent magnets 32 are fixed to the rotor core 31. In the example of Fig. 1, a pair of the permanent magnets 32 forms one magnetic pole. The multiple pairs of permanent magnets 32 are arranged at equal angular intervals in the circumferential direction. In the example of Fig. 1, 12 pairs of permanent magnets 32 (24 in total) are provided at central angle intervals of 30 degrees around the central axis O.
[0035] In the example of FIG. 1, an embedded magnet type motor is used as the permanent magnet field type motor. A rotor core 31 is formed with a plurality of through holes 33 that pass through the rotor core 31 in the axial direction. The plurality of through holes 33 are provided corresponding to the arrangement of the plurality of permanent magnets 32. Each permanent magnet 32 is fixed to the rotor core 31 while being arranged in the corresponding through hole 33. Each permanent magnet 32 can be fixed to the rotor core 31 by, for example, bonding the outer surface of the permanent magnet 32 to the inner surface of the through hole 33 with an adhesive. Note that a surface magnet type motor may be used as the permanent magnet field type motor instead of the embedded magnet type.
[0036] Both the stator adhesive laminated core 21 and the rotor core 31 are laminated cores. For example, the stator adhesive laminated core 21 is formed by laminating a plurality of electromagnetic steel sheets 40 in a lamination direction, as shown in FIG. The lamination thickness (total length along the central axis O) of each of the stator adhesive laminated core 21 and the rotor core 31 is, for example, 50.0 mm. The outer diameter of the stator adhesive laminated core 21 is, for example, 250.0 mm. The inner diameter of the stator adhesive laminated core 21 is, for example, 165.0 mm. The outer diameter of the rotor core 31 is, for example, 163.0 mm. The inner diameter of the rotor core 31 is, for example, 30.0 mm. However, these values are merely examples, and the lamination thickness, outer diameter, and inner diameter of the stator adhesive laminated core 21 and the lamination thickness, outer diameter, and inner diameter of the rotor core 31 are not limited to these values. Here, the inner diameter of the stator adhesive laminated core 21 is based on the tip of the teeth portion 23 in the stator adhesive laminated core 21. In other words, the inner diameter of the stator adhesive laminated core 21 is the diameter of a virtual circle inscribed in the tip of all the teeth portions 23.
[0037] Each of the electromagnetic steel sheets 40 forming the stator adhesive laminated core 21 and the rotor core 31 is formed, for example, by punching a strip-shaped steel sheet as a base material. A known electromagnetic steel sheet can be used as the electromagnetic steel sheet 40. The chemical composition of the electromagnetic steel sheet 40 is shown below in mass %, and contains 2.5% to 3.9% Si by mass %. By setting the chemical composition within this range, the yield strength of each of the electromagnetic steel sheets 40 can be set to 380 MPa or more and 540 MPa or less.
[0038] Silicon: 2.5% to 3.9% Al: 0.001% to 3.0% Mn: 0.05% to 5.0% Remainder: Fe and impurities
[0039] In this embodiment, a non-oriented electromagnetic steel sheet is used as the electromagnetic steel sheet 40. As the non-oriented electromagnetic steel sheet, a non-oriented electrical steel strip according to JIS C2552:2014 can be used. However, a directional electromagnetic steel sheet may be used as the electromagnetic steel sheet 40 instead of the non-oriented electromagnetic steel sheet. In this case, as the directional electromagnetic steel sheet, a directional electrical steel strip according to JIS C2553:2012 can be used.
[0040] In order to improve the workability of the laminated core and the iron loss of the laminated core, both sides of the magnetic steel sheets 40 are coated with a phosphate-based insulating coating. Examples of the material that can be used to form the insulating coating include (1) inorganic compounds, (2) organic resins, and (3) mixtures of inorganic compounds and organic resins. Examples of inorganic compounds include (1) composites of dichromate and boric acid, and (2) composites of phosphate and silica. Examples of organic resins include epoxy resins, acrylic resins, acrylic styrene resins, polyester resins, silicone resins, and fluorine resins.
[0041] [First embodiment] The first embodiment of the present invention will be described below with reference to FIGS. First, a bonded laminated core manufacturing apparatus 100 according to this embodiment will be described with reference to the side view shown in Fig. 3. As shown in Fig. 3, the bonded laminated core manufacturing apparatus 100 includes a strip steel plate supply section 110, a hardening promotion layer forming section 120, a drive section (not shown), a press processing oil application section 130, a press processing section 140, an adhesive application section 150, and a lamination bonding section 160.
[0042] The strip steel sheet supplying section 110 supports a hoop material F wound with a strip steel sheet M, which is the raw material for the electromagnetic steel sheet (steel sheet component) 40, and feeds out the strip steel sheet M toward the right side of the paper in Fig. 3. In the following description, the right side of the paper, which is the feeding direction of the strip steel sheet M, may be referred to as the downstream side, and the left side of the paper, which is the opposite direction, may be referred to as the upstream side. The strip steel sheet M fed downstream from the strip steel sheet supplying section 110 is a steel sheet having the above-mentioned chemical composition, and both sides of the steel sheet are coated with the above-mentioned insulating coating.
[0043] The hardening accelerator layer forming section 120 includes a hardening accelerator tank 121 , a nozzle 122 , and a dryer 123 . The curing accelerator tank 121 has a first storage section for storing the anaerobic adhesive curing accelerator dissolved in a solvent, a second storage section for storing the instant adhesive curing accelerator dissolved in a solvent, and a curing accelerator mixing section (not shown). The first storage section and the second storage section are partitioned so that the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator do not mix with each other.
[0044] The curing accelerator for anaerobic adhesives contains an active ingredient that accelerates the curing of anaerobic adhesives. The curing accelerator for instant adhesives contains an active ingredient that accelerates the instant curing of 2-cyanoacrylate adhesives. The anaerobic adhesive and the curing accelerator for instant adhesives are each diluted to an appropriate concentration with a solvent such as a ketone solvent, an alcohol solvent, an ester solvent, a glycol ether solvent, a hydrocarbon solvent, a halogenated hydrocarbon solvent, an ether solvent, a glycol solvent, or an amine solvent. The solvent may be one or a combination of the above solvents. In terms of producing an adhesive laminated core, it is preferable to use, as the solvent type, one or a combination of two or more selected from ethyl acetate, acetone, ethanol, methanol, butanol, and toluene.
[0045] The active ingredient of the anaerobic adhesive curing accelerator is selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof. It may be preferably selected from copper, iron, vanadium, cobalt, chromium, silver, and manganese, and combinations thereof. It may be preferably copper, iron, vanadium, cobalt, and chromium, and combinations thereof. It is preferably provided in the form of a metal oxide or salt. It is preferably exemplified by one or a combination of two or more selected from vanadium acetylacetonate, vanadyl acetylacetonate, vanadyl stearate, vanadium propoxide, vanadium butoxide, vanadium pentoxide, cobalt naphthenate, manganese naphthenate, copper hexanoate, copper(II) bis(2-ethylhexanoate), and the like. The anaerobic adhesive curing accelerator promotes the instantaneous curing of the anaerobic adhesive by mixing with the anaerobic adhesive.
[0046] The instant adhesive curing accelerator contains an active ingredient that accelerates the curing of 2-cyanoacrylate adhesives selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof. Preferably, one or a combination of two or more selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline is used.
[0047] The nozzle 122 has a plurality of first nozzle holes for applying an anaerobic adhesive curing accelerator and a plurality of second nozzle holes for applying an instant adhesive curing accelerator (not shown). The first nozzle holes are directly connected to the first storage portion of the hardening accelerator tank 121 via first piping. The second nozzle holes are directly connected to the second storage portion of the hardening accelerator tank 121 via second piping. Furthermore, both of the first nozzle holes and the second nozzle holes are also connected to the curing accelerator mixing section via a third pipe. The curing accelerator mixing section is connected to both the first storage section and the second storage section via a fourth pipe. The curing accelerator mixing section can take in the anaerobic adhesive curing accelerator from the first storage section and the instant adhesive curing accelerator from the second storage section, and stir and mix them.
[0048] The first pipe, the second pipe, and the fourth pipe are connected to a switching valve (not shown). By operating this switching valve, the flow of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be switched to the following (1) or (2). (1) The anaerobic adhesive curing accelerator in the first storage section is caused to flow to the first nozzle hole through the first piping, and at the same time, the instant adhesive curing accelerator in the second storage section is caused to flow to the second nozzle hole through the second piping. As a result, the anaerobic adhesive curing accelerator is discharged from each of the first nozzle holes, and the instant adhesive curing accelerator is discharged from each of the second nozzle holes. (2) Both the anaerobic adhesive curing accelerator in the first storage section and the instant adhesive curing accelerator in the second storage section are taken into the curing accelerator mixing section via the fourth pipe and stirred and mixed. The mixed accelerator thus obtained by mixing the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator is caused to flow into both the first nozzle holes and the second nozzle holes via the third pipe. As a result, the mixed accelerator is discharged from both the first nozzle holes and the second nozzle holes.
[0049] The discharge outlets of each of the first nozzle holes are directed toward the upper surface of the strip-shaped steel plate M, and the anaerobic adhesive curing accelerator or the mixing accelerator can be applied to the upper surface in dots or lines. The outlets of each of the second nozzle holes are also directed toward the upper surface of the strip-shaped steel sheet M, and the instant adhesive hardening accelerator or the mixing accelerator can be applied to the upper surface in dots or lines. In the nozzle 122, the first nozzle holes and the second nozzle holes are arranged alternately, and the pitch is determined so that the hardening accelerators discharged from the respective holes are not mixed excessively on the coating surface of the strip-shaped steel sheet M. When the anaerobic adhesive hardening accelerator and the instant adhesive hardening accelerator are applied in a checkered pattern as described later with reference to Fig. 5, it is preferable that the pitch is the same as the pitch of the nozzle holes of the nozzle 153 described later, so that the application positions of these hardening accelerators relatively coincide with the application positions of the anaerobic adhesive and the instant adhesive in the subsequent process.
[0050] By switching between the above (1) and (2) by the switching valve, the application form of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the application surface of the strip-shaped steel sheet M is divided into a case where they are applied in an unmixed state and a case where they are applied in a mixed state. In the following explanation, the three types of curing accelerators, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators, may be collectively referred to simply as "curing accelerators." On the other hand, when it is necessary to distinguish between these, they will be explained separately as three types, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators.
[0051] The dryer 123 includes a pair of rollers 123a and a dryer 123b. The pair of rollers 123a are disposed downstream of the nozzle 122. The pair of rollers 123a hold the strip steel sheet M passing between them so that it is always kept horizontal. The dryer 123b is disposed at a position sandwiched between the pair of rollers 123a. The dryer 123b dries the hardening accelerator by blowing air onto the upper and lower surfaces of the strip steel plate M. As a result, the strip steel plate M receives air blowing when it passes the upstream side of the pair of rollers 123a, and the hardening accelerator starts to dry, and the drying is completed before it reaches the downstream side of the pair of rollers 123a. Therefore, on the upper surface of the strip steel plate M after passing the downstream side of the pair of rollers 123a, a hardening accelerator layer in which the solvent has dried is formed with an even thickness over the entire surface. The thickness of the hardening accelerator layer can be exemplified as 0.1 μm. On the other hand, the lower surface of the strip steel plate M is not coated with the hardening accelerator, so the insulating coating remains exposed. The hardening accelerating layer can be formed in a variety of patterns by operating the switching valve, etc. The patterns will be described later with reference to Figs.
[0052] The drive unit is disposed at a position DR between the hardening acceleration layer forming unit 120 and the press working oil application unit 130. The drive unit intermittently sends out the strip steel sheet M from the hardening acceleration layer forming unit 120 toward the press working oil application unit 130 toward the right side of the drawing. Note that, on the upper surface of the strip steel sheet M sent out from the hardening acceleration layer forming unit 120, a hardening acceleration layer where the hardening accelerator has dried has already been formed before entering the drive unit. On the other hand, on the lower surface of the strip steel sheet M before entering the drive unit, there is no hardening acceleration layer, and the insulating coating remains exposed.
[0053] The press working oil application section 130 includes an application roller 131 and an oil pan 132 . The oil pan 132 is disposed below the strip steel sheet M and directly below the application roller 131. The application roller 131 has an upper roller 131a and a lower roller 131b. The upper roller 131a is disposed directly above the strip steel sheet M, and by moving up and down, can be switched between a state in contact with and a state separated from the upper surface of the strip steel sheet M. The upper roller 131a can apply press processing oil to the upper surface of the strip steel sheet M by rolling while being in contact with the upper surface of the steel sheet M with press processing oil supplied from a press processing oil supply unit (not shown) permeating its outer circumferential surface. The lower roller 131b is disposed directly below the strip steel sheet M, and can be switched between a state in contact with and a state separated from the lower surface of the strip steel sheet M by moving up and down. The lower roller 131b can apply press processing oil to the underside of the strip steel sheet M by rolling while being in contact with the underside of the steel sheet M with the press processing oil supplied from the press processing oil supply unit permeating its outer circumferential surface. The oil pan 132 receives and collects excess press oil dripping from the upper roller 131a and the lower roller 131b, and returns it to the press oil supply section.
[0054] According to the press processing oil application section 130, by supplying press processing oil from the press processing oil supply section while the upper roller 131a is in contact with the upper surface of the strip steel plate M, a layer of press processing oil can be formed over the entire upper surface of the strip steel plate M, while the strip steel plate M is continuously or intermittently sent downstream. Similarly, by supplying press processing oil from the press processing oil supply section while the lower roller 131b is in contact with the underside of the strip steel plate M, a layer of press processing oil can be formed over the entire underside of the strip steel plate M, while the strip steel plate M is sent out downstream continuously or intermittently.
[0055] Alternatively, by sandwiching the strip steel sheet M between the upper roller 131a and the lower roller 131b, a layer of press processing oil can be formed over the entire surface of both the upper and lower surfaces of the strip steel sheet M, while the strip steel sheet M is continuously or intermittently sent downstream. In this way, by moving the positions of the upper roller 131a and the lower roller 131b up and down as needed, the press processing oil can be applied in three ways: only to the upper surface of the strip steel plate M, only to the lower surface of the strip steel plate M, or to both the upper and lower surfaces of the strip steel plate M.
[0056] In any of the above cases, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the upper surface of the strip steel sheet M are actively dried rather than naturally dried before the press processing oil is applied. In this way, the curing accelerator layer is formed by actively drying in advance, so that the curing accelerator is prevented from being mixed with the press processing oil and diluted. Therefore, the concentration of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator on the upper surface of the strip steel sheet M after the press processing oil is applied is maintained without change before and after the press processing oil is applied. Therefore, the strip steel sheet M after passing through the press processing oil application section 130 is sent to the press processing section 140 while maintaining the concentration of the curing accelerator on its upper surface.
[0057] The press processing section 140 includes a first stage punching section 141 and a second stage punching section 142 . The first-stage punching section 141 is disposed downstream of the press oil application section 130 and has a male die 141a and a female die 141b. The male die 141a and the female die 141b are disposed coaxially along the vertical direction, and the strip steel sheet M is inserted between them. Thus, the male die 141a faces the upper surface of the strip steel sheet M, and the female die 141b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is temporarily stopped, the male die 141a is moved downward by a hydraulic mechanism (not shown) to reach the female die 141b, thereby performing the first punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 141a is then moved upward and pulled out from the female die 141b, and the strip steel sheet M is again sent out toward the downstream side.
[0058] The second-stage punching section 142 is disposed downstream of the first-stage punching section 141 and has a male die 142a and a female die 142b. The male die 142a and the female die 142b are disposed coaxially along the vertical direction, and the strip steel sheet M after the first punching process is inserted between them. Thus, the male die 142a faces the upper surface of the strip steel sheet M, and the female die 142b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 142a is moved downward by a hydraulic mechanism (not shown) to reach the female die 142b, thereby performing the second punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 142a is then moved upward and pulled out from the female die 142b, and the strip steel sheet M is again sent out toward the downstream side.
[0059] The adhesive application section 150 is disposed downstream of the press processing section 140. The adhesive application section 150 includes an air compressor 151, a syringe 152, a nozzle 153, and a steel plate holder 154. The syringe 152 is a container having a space for storing an anaerobic adhesive and a space for storing an instantaneous adhesive (not shown). The space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive are partitioned so that the anaerobic adhesive and the instantaneous adhesive do not mix. Here, an example of the anaerobic adhesive is "Arontite" (registered trademark) manufactured by Toagosei Co., Ltd., and an example of the instantaneous adhesive (2-cyanoacrylate adhesive) is "Aron Alpha" (registered trademark) manufactured by Toagosei Co., Ltd. The syringe 152 and the air pump 151 are connected by a pipe that sends air from the air pump 151 to the syringe 152. The syringe 152 and the nozzle 153 are connected from the syringe 152 to the nozzle 153 via a fifth pipe that supplies the anaerobic adhesive and a sixth pipe that supplies the instantaneous adhesive.
[0060] The nozzle 153 is equipped with a plurality of needles (not shown) whose outlets face upward. These needles are arranged below the strip steel sheet M. Thus, the outlet of each of the needles faces the lower surface of the strip steel sheet M. Each of the needles includes a plurality of first needles for applying the anaerobic adhesive and a plurality of second needles for applying the instant adhesive (not shown). The outlets of the first and second needles are arranged alternately and evenly when the nozzle 153 is viewed from above.
[0061] Here, when the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in a checkered pattern as shown in FIG. 5 described later, it is preferable to make the position of the outlet of each of the first needles coincide with the position of each anaerobic adhesive curing accelerator applied and dried on the upper surface of the strip steel plate M. Similarly, it is preferable to make the position of the outlet of each of the second needles coincide with the position of each instant adhesive curing accelerator applied and dried on the upper surface of the strip steel plate M. In this case, when the feed of the strip steel plate M is temporarily stopped above the nozzle 153 via the press processing section 140, the relative positions of each anaerobic adhesive curing accelerator on the upper surface of the strip steel plate M and the outlet of each of the first needles coincide, and further, the relative positions of each instant adhesive curing accelerator and the outlet of each of the second needles coincide. This allows each adhesive to be applied in a correct combination with each curing accelerator.
[0062] Each of the first needles is directly connected to the space storing the anaerobic adhesive via the fifth pipe, while each of the second needles is directly connected to the space storing the instant adhesive via the sixth pipe. Then, each of the first needles and each of the second needles can apply the anaerobic adhesive and the instantaneous adhesive so as to form a checkered (grid) pattern on the lower surface of the strip steel plate M. As a result, square or circular patterns made of the anaerobic adhesive and square or circular patterns made of the instantaneous adhesive are alternately arranged on the lower surface side of the strip steel plate M along both the longitudinal direction and the width direction of the strip steel plate M. In other words, the anaerobic adhesive and the instantaneous adhesive can be arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M.
[0063] The steel plate holder 154 is disposed above the nozzle 153 (directly above the first and second needles). Thus, the steel plate holder 154 faces the upper surface of the strip steel plate M. The steel plate holder 154 is pressed downward by a hydraulic mechanism (not shown) while the delivery of the strip steel plate M is temporarily stopped. As a result, the lower surface of the steel plate holder 154 comes into contact with the upper surface of the strip steel plate M and presses the strip steel plate M downward. This allows the height position of the strip steel plate M to be pressed down to the adhesive application position by the nozzle 153 and positioned. In this positioned state, the lower surface of the strip steel plate M is close to the discharge ports of the first and second needles.
[0064] Furthermore, when air is pumped from the air pump 151 to the syringe 152 in this positioning state, the air is evenly supplied to both the space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive. Then, the anaerobic adhesive is supplied to each of the first needles via the fifth pipe, and the instantaneous adhesive is supplied to each of the second needles via the sixth pipe. Then, the anaerobic adhesive is discharged from the outlet of each of the first needles and applied to the lower surface of the strip steel plate M. Similarly, the instantaneous adhesive is discharged from the outlet of each of the second needles and applied to the lower surface of the strip steel plate M. Thereafter, the steel plate holder 154 is raised by the hydraulic mechanism, thereby returning the height position of the strip steel plate M to its original height.
[0065] The lamination bonding section 160 is disposed downstream of the adhesive application section 150. The lamination bonding section 160 includes a male outer periphery punching die 161, a female outer periphery punching die 162, a spring 163, and a heater 164. The outer periphery punching male die 161 is a cylindrical die with a circular bottom surface, and the upper end of the die is connected to the lower end of the spring 163. The outer periphery punching male die 161 is supported by the spring 163 and can move up and down together with the spring 163. The outer periphery punching male die 161 has an outer diameter substantially the same as that of the stator adhesive laminated core 21.
[0066] The outer periphery punching female die 162 is a die having a cylindrical internal space, and has an inner diameter dimension that is approximately the same as the outer diameter dimension of the stator bonded laminated core 21 . The heater 164 is integrally built into the outer periphery punching female die 162. The heater 164 heats the periphery of each of the electromagnetic steel sheets (steel sheet components) 40 stacked inside the outer periphery punching female die 162. When a heat-curing type adhesive is used as the adhesive, the adhesive cures when it receives heat from the heater 164. On the other hand, when a room temperature curing type adhesive is used as the adhesive, the adhesive cures at room temperature without the need for heating.
[0067] According to the laminated adhesive section 160, while the feeding of the strip-shaped steel sheet M is temporarily stopped, the outer periphery punching male die 161 is lowered to sandwich the strip-shaped steel sheet M between it and the outer periphery punching female die 162, and the outer periphery punching male die 161 is further pushed into the outer periphery punching female die 162, thereby obtaining an electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M. This punched out electromagnetic steel sheet 40 is stacked on the top surface of other electromagnetic steel sheets 40 that have been previously punched out and stacked and bonded inside the outer periphery punching female die 162, and is further subjected to a pressure from the outer periphery punching male die 161 and heat from a heater 164. At this time, the pressure applied to the electromagnetic steel sheet 40 from the outer periphery punching male die 161 is always kept constant by the biasing force of the spring 163. As a result, the currently punched electromagnetic steel sheet 40 is adhered and fixed to the upper surface of the previously punched electromagnetic steel sheet 40. By repeating these steps of outer periphery punching, pressurizing, and heating a number of times corresponding to the number of laminated electromagnetic steel sheets 40, an adhesive laminated core 21 for a stator is formed in the outer periphery punching female die 162.
[0068] 3, the female die 141b, the female die 142b, the nozzle 153, the outer periphery punching female die 162, and the heater 164 are fixed on a common fixed base 171. Therefore, the relative positions of the female die 141b, the female die 142b, the nozzle 153, the outer periphery punching female die 162, and the heater 164 are fixed in the horizontal and vertical directions. Similarly, the male die 141a, the male die 142a, the steel plate holder 154, and the outer periphery punching male die 161 are also fixed to the lower surface of a common movable base 172. Therefore, the relative positions of the male die 141a, the male die 142a, the steel plate holder 154, and the outer periphery punching male die 161 in the horizontal and vertical directions are fixed.
[0069] The drive unit sends out the strip steel sheet M downstream and, when it is temporarily stopped, lowers the movable base 172, thereby simultaneously punching out the outer periphery of the electromagnetic steel sheet 40, stacking and bonding, applying anaerobic adhesive and instant adhesive to the position of the electromagnetic steel sheet 40 where the outer periphery will next be punched in the strip steel sheet M, applying the second punching process to the position of the strip steel sheet M where the anaerobic adhesive and instant adhesive will next be applied, and the first punching process to the position of the strip steel sheet M where the second punching process will next be performed. Next, the movable base 172 is raised and retracted above the strip steel sheet M, and then the drive unit sends out the strip steel sheet M a predetermined distance downstream again and pauses again. In this state, the movable base 172 is lowered again and processing is continued at each position. In this way, the process of moving the movable base 172 up and down during pauses while intermittently sending the strip steel sheet M by the drive unit is repeated, thereby manufacturing the stator adhesive laminated core 21.
[0070] A bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 100 having the above-described configuration will be described below with reference to FIGS. Fig. 4 is a flow chart for explaining the bonded laminated core manufacturing method according to the present embodiment. Fig. 5 is a diagram for explaining a first embodiment of the bonded laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a cross-sectional view taken along line AA of (a). Fig. 6 is a diagram for explaining a second embodiment of the bonded laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a cross-sectional view taken along line BB of (a). Fig. 7 is a diagram for explaining a third embodiment of the bonded laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a cross-sectional view taken along line CC of (a). Fig. 8 is a flow chart for explaining a modified example of the bonded laminated core manufacturing method according to the present embodiment.
[0071] As shown in FIG. 4, the adhesive laminated core manufacturing method of this embodiment includes a steel plate feeding process S1, a hardening accelerator application process S2, a hardening accelerator drying process S3, a processing oil application process S4, a first punching process S5, a second punching process S6, an adhesive application process S7, a stacking and bonding process S8, a stack number confirmation process S9, and a removal process S10.
[0072] In the steel plate delivery process S1, a strip-shaped steel plate M is delivered downstream from the hoop material F. In the subsequent hardening accelerator application process S2, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are applied from the nozzle 122 to the entire upper surface of the strip-shaped steel plate M. At this point, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are both in liquid form.
[0073] Here, three application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are shown in Fig. 5 to Fig. 7. Fig. 5 to Fig. 7 are diagrams corresponding to the lamination and adhesion step S8, but the application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 formed in the curing accelerator application step S2 remain fixed after the curing accelerator drying step S3. Therefore, the application patterns will be explained using these drawings.
[0074] For example, in the application pattern of Fig. 5, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to form a checkered (lattice) pattern on the upper surface of the strip steel plate M (electromagnetic steel plate 40). More specifically, square or circular patterns made of the anaerobic adhesive curing accelerator a1 and square or circular patterns made of the instant adhesive curing accelerator a2 are arranged alternately along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the upper surface of the strip steel plate M. That is, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried in the subsequent curing accelerator drying step S3 to form a curing accelerator layer a having a constant thickness.
[0075] In the application pattern of FIG. 6, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are mixed in advance and placed on the upper surface of the strip steel plate M (electromagnetic steel plate 40). This mixing is obtained by taking both the anaerobic adhesive curing accelerator a1 in the first storage section and the instant adhesive curing accelerator a2 in the second storage section into the curing accelerator mixing section through the third pipe in the curing accelerator layer forming section 120 and stirring and mixing them. The mixing accelerator obtained in this manner is supplied to both the first nozzle holes and the second nozzle holes through the fourth pipe. As a result, the mixing accelerator is discharged from both the first nozzle holes and the second nozzle holes. The discharged mixing accelerator is then evenly arranged on the insulating coating formed on the upper surface of the strip steel plate M along both the longitudinal direction of the strip steel plate M and the width direction of the strip steel plate M. The mixed accelerator thus applied is dried in the subsequent hardening accelerator drying step S3 to form a hardening accelerator layer a having a certain thickness.
[0076] Alternatively, in the application pattern of FIG. 7, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged so as to form stripes (lines) on the upper surface of the strip-shaped steel sheet M (electromagnetic steel sheet 40). More specifically, a linear pattern consisting of the anaerobic adhesive curing accelerator a1 and a linear pattern consisting of the instant adhesive curing accelerator a2 are alternately arranged along the longitudinal direction of the strip-shaped steel sheet M on the insulating film formed on the upper surface of the strip-shaped steel sheet M. That is, when the right direction of the paper in FIG. 7(b) is the feed direction of the strip-shaped steel sheet M, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are each formed in a straight line so as to be parallel to the direction perpendicular to the feed direction. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged adjacent to each other when viewed along the feed direction of the strip-shaped steel sheet M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried in the subsequent curing accelerator drying step S3 to form a curing accelerator layer a having a constant thickness. In place of the above application form, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be formed in a straight line parallel to the feed direction of the strip steel plate M, with the downward direction of the paper in Figure 7(b) corresponding to the feed direction of the strip steel plate M.
[0077] Returning to Fig. 4, in the subsequent hardening accelerator drying step S3, air from the dryer 123b is blown onto the upper and lower surfaces of the strip-shaped steel plate M to dry the liquid hardening accelerator a1 for the anaerobic adhesive and the hardening accelerator a2 for the instant adhesive, thereby forming a hardening accelerator layer a. This hardening accelerator layer a is solid. In the subsequent processing oil application step S4, the upper roller 131a rolls in contact with the upper surface of the steel sheet M with the press processing oil b supplied from the press processing oil supply unit permeating its outer circumferential surface. As a result, the press processing oil b is applied to the entire surface only on the upper surface side of the strip-shaped steel sheet M. In other words, the press processing oil b is applied so as to cover the upper surface of the hardening-accelerating layer a. At this time, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are formed into a curing accelerator layer a that has been dried in advance, so that they are prevented from mixing with and being diluted by the press processing oil b that is applied to the upper surface. On the other hand, the lower roller 131b has been lowered and separated from the lower surface of the strip steel sheet M, so that the press working oil b is not applied to the lower surface of the strip steel sheet M, and the insulating coating remains exposed.
[0078] In the subsequent first punching process S5, the first punching of the strip steel sheet M is performed by the first-stage punching unit 141. At this time, since the press processing oil b has been applied in advance to the upper surface of the strip steel sheet M, defects in the press processing such as seizure between the male die 141a and the female die 141b do not occur. In the subsequent second punching process S6, the second punching of the strip steel sheet M is performed by the second-stage punching section 142. At this time as well, since the press processing oil b has been applied in advance to the upper surface of the strip steel sheet M, defects in the press processing such as seizure between the male die 142a and the female die 142b do not occur. By the above-mentioned first punching process S5 and second punching process S6, the core back portion 22 and the teeth portion 23 shown in FIG. 1 are formed in the strip-shaped steel plate M, except for the outer shape portion.
[0079] In the subsequent adhesive application process S7, as shown in Fig. 5 to Fig. 7, the anaerobic adhesive c1 and the instant adhesive c2 discharged from the nozzle 153 are applied directly to the lower surface of the strip-shaped steel plate M. At this time, the anaerobic adhesive c1 and the instant adhesive c2 are applied in dots having a predetermined thickness and a predetermined diameter. At this time, the anaerobic adhesive c1 and the instant adhesive c2 are in a liquid state because they have not yet been mixed with the hardening acceleration layer a. Furthermore, as shown in FIG. 5(b), when the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged in a checkered pattern, the anaerobic adhesive c1 and the instant adhesive c2 are also arranged in a checkered pattern in accordance with their relative positions.
[0080] In the subsequent lamination and bonding step S8, as shown in Figs. 5 to 7, the electromagnetic steel sheet 40, the periphery of which has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 161, is laminated on the upper surface of the other electromagnetic steel sheet 40 that has been previously punched out. At this time, a hardening accelerating layer a covered with press processing oil b is formed on the upper surface of the other electromagnetic steel sheet 40. The electromagnetic steel sheet 40 that has been punched out this time is laminated on top of this and heated while being pressurized. Then, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface of the electromagnetic steel sheet 40 that has been punched out this time push aside the press processing oil b on the upper surface side of the other electromagnetic steel sheet 40 that has been previously punched out and mix with the hardening accelerating layer a below it. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerating layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerating layer a.
[0081] By sequentially repeating the above steps, a predetermined number of electromagnetic steel sheets 40 are laminated and bonded together, and the bonded laminated core 21 for the stator is completed. That is, in the stacking number confirmation step S9, it is determined whether or not the number of stacked electromagnetic steel sheets 40 has reached a predetermined number. If the number has not reached the predetermined number (determination: NO), the flow returns to the steel sheet delivery step S1, and the steel sheet delivery step S1 to the stacking and bonding step S8 are repeated again. On the other hand, if the number has reached the predetermined number in the stacking number confirmation step S9 (determination: YES), the flow proceeds to the removal step S10. In the subsequent removal step S10, the completed bonded laminated core 21 for a stator is removed from the outer periphery punching female die 162, thereby completing all steps of the bonded laminated core manufacturing method.
[0082] The main points of the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 100 described above will be summarized below. The method for manufacturing a bonded laminated core in this embodiment is a method for manufacturing a bonded laminated core 21 for a stator (bonded laminated core) by applying an anaerobic adhesive a1 and an instant adhesive a2 to one side (upper side) of a strip-shaped steel plate M, on which a press processing oil b has been applied, pressing the strip-shaped steel plate M to obtain a plurality of electromagnetic steel plates 40 (steel plate components), and stacking and bonding the electromagnetic steel plates 40 together. In this embodiment, a hardening accelerator a1 for anaerobic adhesives and a hardening accelerator a2 for instant adhesives are applied to the upper surface of the strip steel plate M before the press processing oil b is applied, and then dried to form a hardening accelerator layer a. According to this method for manufacturing a bonded laminated core, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are actively dried instead of being naturally dried. In this way, since the curing accelerator layer a is formed by actively drying in advance, it is possible to suppress the mixture with the press processing oil b applied in the post-processing and dilution. Therefore, when laminating and bonding each of the electromagnetic steel sheets 40, the anaerobic adhesive curing accelerator a1 can be mixed with the anaerobic adhesive c1 while maintaining its high concentration, and the instant adhesive curing accelerator a2 can also be mixed with the instant adhesive c2 while maintaining its high concentration. Therefore, high adhesive strength can be developed early. Therefore, it is possible to obtain higher productivity while ensuring sufficient adhesive strength.
[0083] As shown in FIG. 5, in the above-mentioned method for producing an adhesive laminated core, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be arranged in a checkered pattern. Alternatively, as shown in Figure 6, in the above-mentioned adhesive laminated core manufacturing method, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be mixed in advance and then applied to the upper surface of the strip-shaped steel plate M and dried to form the curing accelerator layer a. Alternatively, as shown in FIG. 7, in the above adhesive laminated core manufacturing method, the curing accelerator a1 for anaerobic adhesives and the curing accelerator a2 for instant adhesives may be arranged in stripes to form the curing accelerator layer a. In any of the above cases, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 can be evenly distributed along the coating surface of the strip steel sheet M. Therefore, the adhesive strength along the coating surface can be made uniform.
[0084] More specifically, the method for manufacturing the bonded laminated core includes the following steps. That is, each electromagnetic steel sheet 40 includes an electromagnetic steel sheet (first steel sheet component) 40 that has been previously punched out and an electromagnetic steel sheet (second steel sheet component) 40 that has been subsequently punched out. This adhesive laminated core manufacturing method includes a first step of preparing an electromagnetic steel sheet (first steel sheet component) 40 having an upper surface (first surface), a hardening promotion layer a formed on the upper surface, and a press processing oil b arranged on the hardening promotion layer a; a second step of preparing an electromagnetic steel sheet (second steel sheet component) 40 that has been subsequently punched out and has a lower surface (second surface) and an anaerobic adhesive c1 and an instant adhesive c2 arranged on the lower surface; and a third step of overlapping and bonding the electromagnetic steel sheet (first steel sheet component) 40 that has been previously punched out and the electromagnetic steel sheet (second steel sheet component) 40 that has been subsequently punched out so that the upper surface and the lower surface face each other. According to this method for manufacturing an adhesive laminated core, in the first step, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are dried in advance to form the curing accelerator layer a, and are in a state in which they are inhibited from mixing with the press processing oil b. Therefore, when the electromagnetic steel sheet (first steel sheet component) 40 whose periphery has been punched first and the electromagnetic steel sheet (second steel sheet component) 40 whose periphery has been punched later are superimposed and bonded in the third step, the anaerobic adhesive curing accelerator a1 mixes with the anaerobic adhesive c1 while maintaining its high concentration, and the instant adhesive curing accelerator a2 also mixes with the instant adhesive c2 while maintaining its high concentration.
[0085] In the above-mentioned bonded laminated core manufacturing method, the bonded laminated core for a stator (bonded laminated core) 21 may be a stator for a rotating electric machine. This adhesive laminated core manufacturing method achieves higher productivity while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electrical machines that have high performance yet are low in manufacturing cost.
[0086] The bonded laminated core manufacturing apparatus 100 of this embodiment is an apparatus for manufacturing a stator bonded laminated core (bonded laminated core) 21 including a plurality of electromagnetic steel plates (steel plate components) 40 punched out from a strip-shaped steel plate M. The bonded laminated core manufacturing apparatus 100 of this embodiment is equipped with a press processing oil application section 130 that applies press processing oil b to the upper surface (one side) of the strip-shaped steel plate M; a press processing section 140 that applies press processing to the strip-shaped steel plate M; an adhesive application section 150 that applies anaerobic adhesive c1 and instant adhesive c2 to the lower surface of the strip-shaped steel plate M; and a hardening acceleration layer forming section 120 that forms a hardening acceleration layer a by applying and drying an anaerobic adhesive hardening accelerator a1 and an instant adhesive hardening accelerator a2 to the upper surface of the strip-shaped steel plate M before applying the press processing oil b.
[0087] According to the bonded laminated core manufacturing apparatus 100, the curing accelerator a1 for the anaerobic adhesive and the curing accelerator a2 for the instantaneous adhesive are both actively dried by the curing accelerator layer forming section 120 instead of being naturally dried. In this way, since the curing accelerator layer a is formed by actively drying in advance, it is possible to suppress the mixture with the press processing oil b applied in the post-processing and dilution. Therefore, when the magnetic steel sheets 40 are laminated and bonded, the curing accelerator a1 for the anaerobic adhesive is mixed with the anaerobic adhesive c1 while maintaining its high concentration, and the curing accelerator a2 for the instantaneous adhesive is also mixed with the instantaneous adhesive c2 while maintaining its high concentration. Therefore, high adhesive strength can be developed early. Therefore, it is possible to obtain higher productivity while ensuring sufficient adhesive strength.
[0088] In the above-mentioned adhesive laminated core manufacturing apparatus 100, the hardening acceleration layer forming section 120 may be equipped with a nozzle 122 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in a checkered pattern, as shown in FIG. Alternatively, in the above-mentioned adhesive laminated core manufacturing apparatus 100, the hardening acceleration layer forming section 120 may be equipped with a pipe (hardening accelerator supply flow path) through which the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are mixed in advance and flow, as shown in FIG. 6, and a nozzle 122 connected to this pipe. Alternatively, in the adhesive laminated core manufacturing apparatus 100, the hardening acceleration layer forming section 120 may be equipped with a nozzle 122 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in stripes, as shown in FIG. In any of the above cases, the nozzle 122 can uniformly distribute the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 along the coating surface of the strip steel sheet M. This makes it possible to make the adhesive strength along the coating surface uniform.
[0089] In this embodiment, the case where the press working oil b is applied only to the upper surface of the strip steel sheet M in the processing oil application step S4 shown in Fig. 4 has been described, but the present invention is not limited to this. For example, as shown in a modified example in Fig. 8, a processing oil application step S4A in which the press working oil b is applied only to the lower surface of the strip steel sheet M or to both the upper and lower surfaces of the strip steel sheet M may be adopted.
[0090] In this processing oil application step S4A, when the press processing oil b is applied only to the lower surface of the strip steel plate M, the upper roller 131a is retracted above the upper surface of the strip steel plate M to be out of contact with it, while the lower roller 131b is rolled against the lower surface of the strip steel plate M with the press processing oil b permeated into its outer circumferential surface. As a result, the press processing oil is applied to the entire lower surface of the strip steel plate M only. As a result, a hardening accelerator layer a consisting of the anaerobic adhesive hardening accelerator a1 and the instantaneous adhesive hardening accelerator a2 is formed in an exposed state on the upper surface of the strip steel plate M. On the other hand, the press processing oil b and the anaerobic adhesive c1 and instantaneous adhesive c2 applied on the press processing oil b are formed on the lower surface of the strip steel plate M.
[0091] In this case, in the lamination and bonding step S8A in FIG. 8, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 161 is laminated on the upper surface of the other electromagnetic steel sheet 40 whose periphery has been punched out earlier, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface of the electromagnetic steel sheet 40 whose periphery has been punched out later are pushed aside and applied to the lower surface of the electromagnetic steel sheet 40. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface of the electromagnetic steel sheet 40 whose periphery has been punched out later are mixed with the hardening accelerator layer a on the upper surface of the electromagnetic steel sheet 40 whose periphery has been punched out earlier. As a result, the anaerobic adhesive c1 is hardened while being mixed with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 is hardened instantly while being mixed with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described with reference to FIG. 4, so the same reference numerals are used and duplicated explanations are omitted.
[0092] Alternatively, for example, in the processing oil application step S4A shown in the modified example of FIG. In this case, in the processing oil application step S4A, the press processing oil b is permeated into both the upper roller 131a and the lower roller 131b, and then the upper roller 131a and the lower roller 131b are rolled while the strip steel plate M is sandwiched between them. As a result, a hardening acceleration layer a consisting of the anaerobic adhesive hardening accelerator a1 and the instantaneous adhesive hardening accelerator a2, and press processing oil b covering the upper surface of the hardening acceleration layer a are formed on the upper surface of the strip steel plate M. Meanwhile, the press processing oil b and the anaerobic adhesive c1 and instantaneous adhesive c2 applied on this press processing oil b are formed on the lower surface of the strip steel plate M.
[0093] Then, in the lamination and bonding process S8A of FIG. 8, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 161 is laminated on the upper surface of the other electromagnetic steel sheet 40 whose periphery has been punched out earlier, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface of the electromagnetic steel sheet 40 whose periphery has been punched out later are applied to the lower surface of the electromagnetic steel sheet 40, pushing aside the press processing oil b on them. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface of the electromagnetic steel sheet 40 whose periphery has been punched out later mix with the hardening accelerator layer a underneath, pushing aside the press processing oil b on the upper surface of the electromagnetic steel sheet 40 whose periphery has been punched out earlier. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described with reference to FIG. 4, so the same reference numerals are used and duplicated explanations are omitted.
[0094] [Second embodiment] A second embodiment of the present invention will be described below with reference to FIGS. First, a bonded laminated core manufacturing apparatus 200 according to this embodiment will be described with reference to the side view shown in Fig. 9. As shown in Fig. 9, the bonded laminated core manufacturing apparatus 200 includes a strip steel plate supply section 210, a hardening promotion layer forming section 220, a drive section (not shown), a press processing oil application section 230, a press processing section 240, an adhesive application section 250, and a lamination bonding section 260.
[0095] The strip steel sheet supplying section 210 supports a hoop material F wound with a strip steel sheet M, which is the raw material for the electromagnetic steel sheet (steel sheet component) 40, and sends out the strip steel sheet M toward the right side of the paper in Fig. 9. In the following description, the right side of the paper, which is the feeding direction of the strip steel sheet M, may be referred to as the downstream side, and the left side of the paper, which is the opposite direction, may be referred to as the upstream side. The strip steel sheet M sent downstream from the strip steel sheet supplying section 210 is a steel sheet having the above-mentioned chemical composition, and both sides thereof are coated with the above-mentioned insulating coating.
[0096] The hardening accelerator layer forming section 220 includes a hardening accelerator tank 221 , a nozzle 222 , a seal box 223 , and a wiping roller 224 . The curing accelerator tank 221 has a first storage section for storing the anaerobic adhesive curing accelerator dissolved in a solvent, a second storage section for storing the instant adhesive curing accelerator dissolved in a solvent, and a curing accelerator mixing section (not shown). The first storage section and the second storage section are partitioned so that the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator do not mix with each other. The anaerobic adhesive curing accelerator is a compound that promotes instantaneous curing of the anaerobic adhesive by mixing with the anaerobic adhesive, and the compounds exemplified in the first embodiment above can be used. Similarly, the instant adhesive curing accelerator is a compound that promotes instantaneous curing of the instant adhesive by mixing with the instant adhesive curing accelerator (2-cyanoacrylate adhesive), and the compounds exemplified in the first embodiment above can be used. The solvent type can also be the same as the solvent type exemplified in the first embodiment above.
[0097] The nozzle 222 has a plurality of first nozzle holes for applying an anaerobic adhesive curing accelerator and a plurality of second nozzle holes for applying an instant adhesive curing accelerator (not shown). The first nozzle holes are directly connected to the first storage portion of the hardening accelerator tank 221 via first piping. The second nozzle holes are directly connected to the second storage portion of the hardening accelerator tank 221 via second piping. Furthermore, both of the first nozzle holes and the second nozzle holes are also connected to the curing accelerator mixing section via a third pipe. The curing accelerator mixing section is connected to both the first storage section and the second storage section via a fourth pipe. The curing accelerator mixing section can take in the anaerobic adhesive curing accelerator from the first storage section and the instant adhesive curing accelerator from the second storage section, and stir and mix them.
[0098] The first pipe, the second pipe, and the fourth pipe are connected to a switching valve (not shown). By operating this switching valve, the flow of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be switched to the following (1) or (2). (1) The anaerobic adhesive curing accelerator in the first storage section is caused to flow to the first nozzle hole through the first piping, and at the same time, the instant adhesive curing accelerator in the second storage section is caused to flow to the second nozzle hole through the second piping. As a result, the anaerobic adhesive curing accelerator is discharged from each of the first nozzle holes, and the instant adhesive curing accelerator is discharged from each of the second nozzle holes. (2) Both the anaerobic adhesive curing accelerator in the first storage section and the instant adhesive curing accelerator in the second storage section are taken into the curing accelerator mixing section via the fourth pipe and stirred and mixed. The mixed accelerator thus obtained by mixing the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator is caused to flow into both the first nozzle holes and the second nozzle holes via the third pipe. As a result, the mixed accelerator is discharged from both the first nozzle holes and the second nozzle holes.
[0099] The discharge outlets of each of the first nozzle holes are directed toward the lower surface of the strip-shaped steel plate M, and the anaerobic adhesive curing accelerator or the mixing accelerator can be applied to the lower surface in dots or lines. The outlets of each of the second nozzle holes are also directed toward the lower surface of the strip-shaped steel sheet M, and the instant adhesive hardening accelerator or the mixing accelerator can be applied to the lower surface in dots or lines. In the nozzle 222, the first nozzle holes and the second nozzle holes are arranged alternately, and the pitch is determined so that the hardening accelerators discharged from the respective holes are not mixed excessively on the coating surface of the strip-shaped steel sheet M. When the anaerobic adhesive hardening accelerator and the instant adhesive hardening accelerator are applied in a checkered pattern as described later with reference to Fig. 11, it is preferable that the pitch is the same as the pitch of the nozzle holes of the nozzle 253 described later, so that the application positions of these hardening accelerators coincide relatively with the application positions of the anaerobic adhesive and the instant adhesive in the subsequent process.
[0100] By switching between the above (1) and (2) by the switching valve, the application form of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the application surface of the strip-shaped steel sheet M is divided into a case where they are applied in an unmixed state and a case where they are applied in a mixed state. In the following explanation, the three types of curing accelerators, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators, may be collectively referred to simply as "curing accelerators." On the other hand, when it is necessary to distinguish between these, they will be explained separately as three types, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators.
[0101] The seal box 223 is a box having an internal space, and has an entrance and an exit leading to the internal space. The strip steel sheet M is fed from the entrance into the internal space of the seal box 223 while maintaining its horizontal state, and then fed out of the seal box 223 from the exit. The nozzle 222 is disposed below the internal space of the seal box 223. As described above, the nozzle mouth of the nozzle 222 is directed to the lower surface of the portion of the strip steel sheet M that passes through the internal space. The hardening accelerator sprayed onto the lower surface of the strip steel sheet M from the nozzle 222 dries instantly because the solvent evaporates. As a result, a hardening accelerator layer with the solvent dried is formed on the lower surface of the strip steel sheet M with an even thickness and over the entire surface before the strip steel sheet M exits from the exit. The thickness of the hardening accelerator layer can be exemplified as 0.1 μm. Since the upper surface of the strip steel sheet M is hardly coated with the hardening accelerator, the insulating coating is almost exposed. The wiping roller 224 mainly wipes off excess hardening accelerator remaining on the upper surface of the strip steel sheet M. As a result, the upper surface of the strip steel sheet M after passing through the wiping roller 224 is in a state where the hardening accelerator has been completely wiped off and the insulating coating remains exposed. The hardening accelerating layer can be formed in a variety of patterns by operating the switching valve, which will be described later with reference to Figs.
[0102] The drive unit is disposed at a position DR between the hardening acceleration layer forming unit 220 and the press working oil application unit 230. The drive unit intermittently sends out the strip steel sheet M from the hardening acceleration layer forming unit 220 toward the press working oil application unit 230 toward the right side of the drawing. Note that a hardening acceleration layer formed by drying the hardening accelerator has already been formed on the lower surface of the strip steel sheet M sent out from the hardening acceleration layer forming unit 220 before entering the drive unit. On the other hand, the upper surface of the strip steel sheet M before entering the drive unit does not have a hardening acceleration layer, and the insulating coating remains exposed.
[0103] The press working oil application section 230 includes an application roller 231 and an oil pan 232 . The oil pan 232 is disposed below the strip steel sheet M and directly below the application roller 231. The application roller 231 has an upper roller 231a and a lower roller 231b. The upper roller 231a is disposed directly above the strip steel sheet M, and can be switched between a state in contact with and a state separated from the upper surface of the strip steel sheet M by moving up and down. The upper roller 231a can apply press processing oil to the upper surface of the strip steel sheet M by rolling while being in contact with the upper surface of the steel sheet M with press processing oil supplied from a press processing oil supply unit (not shown) permeating its outer circumferential surface. The lower roller 231b is disposed directly below the strip steel sheet M, and by moving up and down, can be switched between a state in contact with and a state separated from the lower surface of the strip steel sheet M. The lower roller 231b can apply press processing oil to the underside of the strip steel sheet M by rolling while in contact with the underside of the steel sheet M in a state in which the press processing oil supplied from the press processing oil supply unit has permeated its outer circumferential surface. The oil pan 232 receives and collects excess press oil dripping from the upper roller 231a and the lower roller 231b, and returns it to the press oil supply section.
[0104] According to the press processing oil application section 230, by supplying press processing oil from the press processing oil supply section while the upper roller 231a is in contact with the upper surface of the strip steel plate M, a layer of press processing oil can be formed over the entire upper surface of the strip steel plate M, while the strip steel plate M is continuously or intermittently sent downstream. Similarly, by supplying press processing oil from the press processing oil supply section while the lower roller 231b is in contact with the underside of the strip steel plate M, a layer of press processing oil can be formed over the entire underside of the strip steel plate M, while the strip steel plate M is continuously or intermittently sent downstream.
[0105] Alternatively, by sandwiching the strip steel sheet M between the upper roller 231a and the lower roller 231b, a layer of press processing oil can be formed over the entire surface of both the upper and lower surfaces of the strip steel sheet M, while the strip steel sheet M is continuously or intermittently sent downstream. In this way, by moving the positions of the upper roller 231a and the lower roller 231b up and down as needed, the press processing oil can be applied in three ways: only to the upper surface of the strip steel plate M, only to the lower surface of the strip steel plate M, or to both the upper and lower surfaces of the strip steel plate M.
[0106] Here, in any of the above cases, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the underside of the strip steel sheet M are actively dried rather than naturally dried before the press processing oil is applied. In this way, since the curing accelerator layer is formed by actively drying in advance, it is suppressed that they are mixed with the press processing oil and diluted. Therefore, the concentration of the anaerobic adhesive curing accelerator and the concentration of the instant adhesive curing accelerator on the underside of the strip steel sheet M after the press processing oil is applied are both maintained unchanged before and after the press processing oil is applied. Therefore, the strip steel sheet M after passing through the press processing oil application section 230 is sent to the press processing section 240 while maintaining the concentration of the curing accelerator on its underside.
[0107] The press processing section 240 includes a first stage punching section 241 , a second stage punching section 242 , and a third stage punching section 243 . The first-stage punching section 241 is disposed downstream of the press processing oil application section 230, and has a male die 241a and a female die 241b. The male die 241a and the female die 241b are disposed coaxially along the vertical direction, and the strip steel sheet M is inserted between them. Thus, the male die 241a faces the upper surface of the strip steel sheet M, and the female die 241b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is temporarily stopped, the male die 241a is moved downward by a hydraulic mechanism (not shown) to reach the female die 241b, thereby performing the first punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 241a is then moved upward and pulled out from the female die 241b, and the strip steel sheet M is again sent out toward the downstream side.
[0108] The second-stage punching section 242 is disposed downstream of the first-stage punching section 241 and has a male die 242a and a female die 242b. The male die 242a and the female die 242b are disposed coaxially along the vertical direction, and the strip steel sheet M after the first punching process is inserted between them. Thus, the male die 242a faces the upper surface of the strip steel sheet M, and the female die 242b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 242a is moved downward by a hydraulic mechanism (not shown) to reach the female die 242b, thereby performing the second punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 242a is then moved upward and pulled out from the female die 242b, and the strip steel sheet M is again sent out toward the downstream side.
[0109] The third-stage punching section 243 is disposed downstream of the second-stage punching section 242 and has a male die 243a and a female die 243b. The male die 243a and the female die 243b are disposed coaxially along the vertical direction, and the strip steel sheet M after the second punching process is inserted between them. Thus, the male die 243a faces the upper surface of the strip steel sheet M, and the female die 243b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 243a is moved downward by a hydraulic mechanism (not shown) to reach the female die 243b, thereby performing the third punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 243a is then moved upward and pulled out from the female die 243b, and the strip steel sheet M is again sent out toward the downstream side.
[0110] The adhesive applying section 250 is incorporated in the lamination bonding section 260 located downstream of the press processing section 240. The adhesive applying section 250 includes an air compressor 251, a syringe 252, and a nozzle 253. The syringe 252 is a container (not shown) having a space for storing an anaerobic adhesive and a space for storing an instant adhesive. The space for storing the anaerobic adhesive and the space for storing the instant adhesive are partitioned so that the anaerobic adhesive and the instant adhesive do not mix. Here, the anaerobic adhesive that can be used is one exemplified in the first embodiment. Similarly, the instant adhesive that can be used is one exemplified in the first embodiment. The syringe 252 and the air compressor 251 are connected by a pipe that sends air from the air compressor 251 to the syringe 252. The syringe 252 and the nozzle 253 are connected from the syringe 252 to the nozzle 253 by a fifth pipe that supplies an anaerobic adhesive and a sixth pipe that supplies an instant adhesive.
[0111] The nozzle 253 is equipped with a plurality of needles (not shown) whose outlets face downward. These needles are arranged above the strip steel sheet M. Thus, the outlets of the needles face the upper surface of the strip steel sheet M. The needles include a plurality of first needles for applying the anaerobic adhesive and a plurality of second needles for applying the instant adhesive (not shown). The outlets of the first and second needles are arranged alternately and evenly when the nozzle 253 is viewed from the bottom.
[0112] Here, when the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in a checkered pattern as shown in FIG. 11 described later, it is preferable to make the position of the outlet of each of the first needles coincide with the position of each anaerobic adhesive curing accelerator applied and dried on the lower surface of the strip steel plate M. Similarly, it is preferable to make the position of the outlet of each of the second needles coincide with the position of each instant adhesive curing accelerator applied and dried on the lower surface of the strip steel plate M. In this case, when the feed of the strip steel plate M is temporarily stopped above the nozzle 153 via the press processing section 140, the relative positions of each anaerobic adhesive curing accelerator on the lower surface of the strip steel plate M and the outlet of each of the first needles coincide, and further, the relative positions of each instant adhesive curing accelerator and the outlet of each of the second needles coincide. This allows each adhesive to be applied in a correct combination with each curing accelerator.
[0113] Each of the first needles is directly connected to the space storing the anaerobic adhesive via the fifth pipe, while each of the second needles is directly connected to the space storing the instant adhesive via the sixth pipe. The first needles and the second needles can apply the anaerobic adhesive and the instant adhesive so as to form a checkered (grid) pattern on the upper surface of the strip steel plate M. As a result, square or circular patterns made of the anaerobic adhesive and square or circular patterns made of the instant adhesive are alternately arranged along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the upper surface of the strip steel plate M. In other words, the anaerobic adhesive and the instant adhesive can be arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M.
[0114] Furthermore, in this positioned state, when air is pumped from the air pump 251 to the syringe 252, the air is evenly supplied to both the space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive. Then, the anaerobic adhesive is supplied to each of the first needles via the fifth pipe, and the instantaneous adhesive is supplied to each of the second needles via the sixth pipe. Then, the anaerobic adhesive is discharged from the outlet of each of the first needles and applied to the upper surface of the strip-shaped steel sheet M. Similarly, the instantaneous adhesive is discharged from the outlet of each of the second needles and applied to the upper surface of the strip-shaped steel sheet M.
[0115] The laminated adhesive section 260 includes a peripheral punching male die 261 , a peripheral punching female die 262 , a spring 263 , and a heater 264 . The outer periphery punching male die 261 is a cylindrical die having a circular bottom surface, and the upper end of the die is connected to the lower end of the spring 263. The outer periphery punching male die 261 is supported by the spring 263 and can move up and down together with the spring 263. The outer periphery punching male die 261 has an outer diameter substantially the same as that of the stator adhesive laminated core 21.
[0116] The outer periphery punching female die 262 is a die having a cylindrical internal space, and has an inner diameter dimension that is approximately the same as the outer diameter dimension of the stator bonded laminated core 21 . The heater 264 is integrally built into the outer periphery punching female die 262. The heater 264 heats the periphery of each of the electromagnetic steel sheets (steel sheet components) 40 stacked in the outer periphery punching female die 262. When a heat-curing type adhesive is used as the adhesive, the adhesive cures when it receives heat from the heater 264. On the other hand, when a room temperature curing type adhesive is used as the adhesive, the adhesive cures at room temperature without the need for heating.
[0117] According to the laminated adhesive section 260, while the feeding of the strip-shaped steel sheet M is temporarily stopped, the outer periphery punching male die 261 is lowered to sandwich the strip-shaped steel sheet M between it and the outer periphery punching female die 262, and the outer periphery punching male die 261 is further pushed into the outer periphery punching female die 262, thereby obtaining an electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M. This punched electromagnetic steel sheet 40 is stacked on the top surface of other electromagnetic steel sheets 40 that have been previously punched and stacked and bonded inside the outer periphery punching female die 262, and is further subjected to a pressure from the outer periphery punching male die 261 and heat from a heater 264. At this time, the pressure applied to the electromagnetic steel sheet 40 from the outer periphery punching male die 261 is always kept constant by the biasing force of the spring 263. As a result, the currently punched electromagnetic steel sheet 40 is adhered and fixed to the upper surface of the previously punched electromagnetic steel sheet 40. By repeating these steps of outer periphery punching, pressurizing, and heating a number of times corresponding to the number of laminated electromagnetic steel sheets 40, an adhesive laminated core 21 for a stator is formed in the outer periphery punching female die 262.
[0118] 9, the female die 241b, the female die 242b, the female die 243b, the outer periphery punching female die 262, and the heater 264 are fixed on a common fixed base 271. Therefore, the relative positions of the female die 241b, the female die 242b, the female die 243b, the outer periphery punching female die 262, and the heater 264 are fixed in the horizontal and vertical directions. Similarly, the male die 241a, the male die 242a, the male die 243a, the nozzle 253, and the outer periphery punching male die 261 are also fixed to the lower surface of a common movable base 272. Therefore, the relative positions of these male die 241a, male die 242a, male die 243a, nozzle 253, and outer periphery punching male die 261 are also fixed in the horizontal and vertical directions.
[0119] The drive unit sends out the strip steel plate M downstream and, when it is temporarily stopped, lowers the movable base 272, thereby simultaneously performing the following: outer periphery punching, stacking and bonding of the electromagnetic steel plate 40 and application of adhesive for the next process; the third punching process at the position on the strip steel plate M where the next outer periphery punching will be performed; the second punching process at the position on the strip steel plate M where the next third punching process will be performed; and the first punching process at the position on the strip steel plate M where the next second punching process will be performed. Next, the movable base 272 is raised and retracted above the strip steel sheet M, and then the drive unit sends out the strip steel sheet M a predetermined distance downstream again and pauses again. In this state, the movable base 272 is lowered again and processing is continued at each position. In this way, the process of moving the movable base 272 up and down during pauses while intermittently sending the strip steel sheet M by the drive unit is repeated, thereby manufacturing the stator adhesive laminated core 21.
[0120] A bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 200 having the above-described configuration will be described below with reference to FIGS. Fig. 10 is a flow chart for explaining the adhesive laminated core manufacturing method according to the present embodiment. Fig. 11 is a diagram for explaining a first embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a DD sectional view of (a). Fig. 12 is a diagram for explaining a second embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is an EE sectional view of (a). Fig. 13 is a diagram for explaining a third embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is an FF sectional view of (a). Fig. 14 is a flow chart for explaining a modified example of the adhesive laminated core manufacturing method according to the present embodiment.
[0121] As shown in FIG. 10, the adhesive laminated core manufacturing method of this embodiment includes a steel plate feeding process S11, a hardening accelerator application and drying process S12, an excess wiping off process S13, a processing oil application process S14, a first punching process S15, a second punching process S16, a third punching process S17, a stacking and bonding process S18, a stack number confirmation process S19, and a removal process S20.
[0122] In the steel plate delivery step S11, a strip-shaped steel plate M is delivered downstream from the hoop material F. In the subsequent curing accelerator application and drying process S12, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are applied from the nozzle 222 to the entire lower surface of the strip-shaped steel plate M and then dried. This forms a curing accelerator layer a consisting of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2. The curing accelerator layer a is solid.
[0123] Here, three application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are shown in Fig. 11 to Fig. 13. Fig. 11 to Fig. 13 correspond to the lamination and adhesion step S18, but the application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 formed in the curing accelerator application and drying step S12 remain fixed after the curing accelerator application and drying step S12. Therefore, the application patterns will be explained using these drawings.
[0124] For example, in the application pattern of Fig. 11, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to form a checkered (lattice) pattern on the lower surface of the strip steel plate M (electromagnetic steel plate 40). More specifically, square or circular patterns made of the anaerobic adhesive curing accelerator a1 and square or circular patterns made of the instant adhesive curing accelerator a2 are arranged alternately along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the lower surface of the strip steel plate M. That is, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried before leaving the sealed box 223, forming a curing accelerator layer a having a certain thickness. This curing accelerator layer a is solid.
[0125] In the application pattern of FIG. 12, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are mixed in advance and placed on the lower surface of the strip steel plate M (electromagnetic steel plate 40). This mixing is obtained by taking both the anaerobic adhesive curing accelerator a1 in the first storage section and the instant adhesive curing accelerator a2 in the second storage section into the curing accelerator mixing section through the third pipe in the curing accelerator layer forming section 220 and stirring and mixing them. The mixing accelerator thus obtained is supplied to both the first nozzle holes and the second nozzle holes through the fourth pipe. As a result, the mixing accelerator is discharged from both the first nozzle holes and the second nozzle holes. The discharged mixing accelerator is then evenly placed on the insulating coating formed on the lower surface of the strip steel plate M along both the longitudinal direction of the strip steel plate M and the width direction of the strip steel plate M. The mixed accelerator thus applied is dried before leaving the sealed box 223, and forms a hardening accelerator layer a having a certain thickness. This hardening accelerator layer a is solid.
[0126] Alternatively, in the application pattern of FIG. 13, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged so as to form stripes (lines) on the lower surface of the strip-shaped steel sheet M (electromagnetic steel sheet 40). More specifically, a linear pattern consisting of the anaerobic adhesive curing accelerator a1 and a linear pattern consisting of the instant adhesive curing accelerator a2 are alternately arranged along the longitudinal direction of the strip-shaped steel sheet M on the insulating film formed on the lower surface of the strip-shaped steel sheet M. That is, when the right direction of the paper in FIG. 13(b) is the feed direction of the strip-shaped steel sheet M, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are each formed in a linear shape so as to be parallel to the direction perpendicular to the feed direction. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged adjacent to each other when viewed along the feed direction of the strip-shaped steel sheet M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried before leaving the sealed box 223, forming a curing accelerator layer a having a certain thickness. This curing accelerator layer a is solid. In place of the above application form, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be formed in a straight line parallel to the feed direction of the strip steel plate M, with the downward direction of the paper in Figure 13(b) corresponding to the feed direction of the strip steel plate M.
[0127] Returning to Fig. 10, in the subsequent surplus wiping off process S13, the surplus hardening accelerator is wiped off on the upper surface of the strip steel sheet M. Therefore, no hardening accelerator layer a is formed on the upper surface of the strip steel sheet M. In the subsequent processing oil application step S14, the lower roller 131b rolls in contact with the lower surface of the steel sheet M with the press processing oil b supplied from the press processing oil supply unit permeating its outer circumferential surface. As a result, the press processing oil b is applied to the entire surface of only the lower surface of the strip-shaped steel sheet M. In other words, the press processing oil b is applied so as to cover the surface of the hardening-accelerating layer a. At this time, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are actively dried instead of being naturally dried. In this way, the curing accelerator layer a is formed by actively drying in advance, so that it is prevented from being mixed with and diluted by the press processing oil b applied to the surface. On the other hand, since the upper roller 131a has risen and is separated from the upper surface of the strip steel sheet M, the press working oil b is not applied to the upper surface of the strip steel sheet M, and the insulating coating remains exposed.
[0128] In the subsequent first punching process S15, the first punching of the strip steel sheet M is performed by the first-stage punching section 241. At this time, since the press processing oil b is applied in advance to the underside of the strip steel sheet M, defects in the press processing such as seizure between the male die 241a and the female die 241b do not occur. In the subsequent second punching process S16, the second punching of the strip steel sheet M is performed by the second-stage punching section 242. At this time, too, since the press processing oil b has been applied in advance to the underside of the strip steel sheet M, defects in the press processing such as seizure between the male die 242a and the female die 242b do not occur.
[0129] In the subsequent third punching process S17, the third punching of the strip steel sheet M is performed by the third-stage punching section 243. At this time, too, since the press processing oil b has been applied in advance to the underside of the strip steel sheet M, defects in the press processing such as seizure between the male die 243a and the female die 243b do not occur. By the above-mentioned first punching process S15 to third punching process S17, the core back portion 22 and the teeth portion 23 shown in FIG. 1 are formed in the strip-shaped steel plate M, except for the outer shape portion.
[0130] In the subsequent lamination and bonding process S18, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 261 is laminated on the upper surface of the other electromagnetic steel sheet 40 that was punched out earlier. At this time, adhesive c is applied to the upper surface of the other electromagnetic steel sheet 40. In addition, a hardening promotion layer a covered with press processing oil b is formed on the lower surface of the electromagnetic steel sheet 40 to be laminated thereon. In addition, as shown in FIG. 11(b), when the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged in a checkered pattern, the anaerobic adhesive c1 and the instant adhesive c2 are also arranged in a checkered pattern in accordance with their relative positions. Then, the electromagnetic steel sheets 40 are heated in a stacked and pressurized state. Then, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface of the electromagnetic steel sheet 40 that has been punched out first push aside the press processing oil b on the lower surface side of the electromagnetic steel sheet 40 that has been punched out later, and mix with the hardening accelerator layer a above it. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a.
[0131] By sequentially repeating the above steps, a predetermined number of electromagnetic steel sheets 40 are laminated and bonded together, and the bonded laminated core 21 for the stator is completed. That is, in the stacking number confirmation step S19, it is determined whether or not the number of stacked electromagnetic steel sheets 40 has reached a predetermined number. If the number has not reached the predetermined number (determination: NO), the flow returns to the steel sheet delivery step S11, and the steel sheet delivery step S11 to the stacking and bonding step S18 are repeated again. On the other hand, if the number has reached the predetermined number in the stacking number confirmation step S19 (determination: YES), the flow proceeds to the removal step S20. In the subsequent removal step S20, the completed bonded laminated core 21 for a stator is removed from the outer periphery punching female die 262, thereby completing all steps of the bonded laminated core manufacturing method.
[0132] The main points of the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 200 described above will be summarized below. The method for manufacturing a bonded laminated core in this embodiment is a method for manufacturing a bonded laminated core 21 for a stator (bonded laminated core) by applying an anaerobic adhesive a1 and an instant adhesive a2 to one side (lower side) of a strip-shaped steel plate M, on which a press processing oil b is further applied, performing a press processing on the strip-shaped steel plate M, obtaining a plurality of electromagnetic steel plates 40 (steel plate components), and stacking and bonding the electromagnetic steel plates 40 together. In this embodiment, a hardening accelerator layer a is formed by applying an anaerobic adhesive hardening accelerator a1 and an instant adhesive hardening accelerator a2 to the underside of the strip steel plate M before applying the press processing oil b, and then drying the applied hardening accelerator layer a. According to the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 100 described above, it is possible to obtain the same effects as those described in the first embodiment.
[0133] In addition, as shown in FIG. 11, in the above-mentioned adhesive laminated core manufacturing method, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be arranged in a checkered pattern. Alternatively, as shown in FIG. 12, in the above-mentioned adhesive laminated core manufacturing method, the curing accelerator a1 for anaerobic adhesives and the curing accelerator a2 for instant adhesives may be mixed in advance, and then applied and dried to form the curing accelerator layer a. Alternatively, as shown in FIG. 13, in the above adhesive laminated core manufacturing method, the curing accelerator a1 for anaerobic adhesives and the curing accelerator a2 for instant adhesives may be arranged in stripes to form the curing accelerator layer a. In any of the above cases, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 can be evenly distributed along the coating surface of the strip steel sheet M. Therefore, the adhesive strength along the coating surface can be made uniform.
[0134] More specifically, the method for manufacturing the bonded laminated core includes the following steps. That is, each electromagnetic steel sheet 40 includes an electromagnetic steel sheet (first steel sheet component) 40 whose periphery is subsequently punched out and an electromagnetic steel sheet (second steel sheet component) 40 whose periphery is previously punched out. The adhesive laminated core manufacturing method includes a first step of preparing an electromagnetic steel sheet (first steel sheet component) 40 whose periphery is subsequently punched out, the electromagnetic steel sheet (first steel sheet component) 40 having a lower surface (first surface), a hardening promotion layer a formed on the lower surface, and a press processing oil b arranged on the hardening promotion layer; a second step of preparing an electromagnetic steel sheet (second steel sheet component) 40 whose periphery is previously punched out, the electromagnetic steel sheet (second steel sheet component) 40 having an upper surface (second surface) and an anaerobic adhesive c1 and an instant adhesive c2 arranged on the upper surface; and a third step of overlapping and bonding the electromagnetic steel sheet (second steel sheet component) 40 whose periphery is previously punched out and the electromagnetic steel sheet (first steel sheet component) 40 whose periphery is subsequently punched out so that the upper surface and the lower surface face each other. According to this method for manufacturing a bonded laminated core, it is possible to obtain the same effects as those described in the first embodiment.
[0135] In the above-mentioned bonded laminated core manufacturing method, the bonded laminated core for a stator (bonded laminated core) 21 may be a stator for a rotating electric machine. This adhesive laminated core manufacturing method achieves higher productivity while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electrical machines that have high performance yet are low in manufacturing cost.
[0136] The bonded laminated core manufacturing apparatus 200 of this embodiment is an apparatus for manufacturing a stator bonded laminated core (bonded laminated core) 21 including a plurality of electromagnetic steel plates (steel plate components) 40 punched out from a strip-shaped steel plate M. The bonded laminated core manufacturing apparatus 200 of this embodiment is equipped with a press processing oil application section 230 that applies press processing oil b to the lower surface (one side) of the strip-shaped steel plate M; a press processing section 240 that applies press processing to the strip-shaped steel plate M; an adhesive application section 250 that applies anaerobic adhesive a1 and instant adhesive a2 to the upper surface of the strip-shaped steel plate M; and a hardening acceleration layer forming section 220 that forms a hardening acceleration layer a by applying and drying anaerobic adhesive hardening accelerator a1 and instant adhesive hardening accelerator a2 to the lower surface of the strip-shaped steel plate M before applying the press processing oil b. According to the bonded laminated core manufacturing apparatus 200, it is possible to obtain the same effects as those described in the first embodiment.
[0137] In the adhesive laminated core manufacturing apparatus 200, the hardening acceleration layer forming section 220 may be provided with a nozzle 222 for applying the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in a checkered pattern as shown in FIG. Alternatively, in the above-mentioned adhesive laminated core manufacturing apparatus 200, the hardening acceleration layer forming section 220 may be provided with a pipe (hardening accelerator supply flow path) through which the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are mixed in advance and flow, as shown in FIG. 12, and a nozzle 222 connected to this pipe. Alternatively, in the adhesive laminated core manufacturing apparatus 200, the hardening acceleration layer forming section 220 may be equipped with a nozzle 222 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in stripes, as shown in FIG. In any of the above cases, the nozzle 222 can uniformly distribute the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 along the coating surface of the strip steel sheet M. This makes it possible to make the adhesive strength along the coating surface uniform.
[0138] In this embodiment, the case where the press processing oil b is applied only to the lower surface side of the strip steel sheet M in the processing oil application step S14 shown in Fig. 10 has been described, but the present invention is not limited to this. For example, as shown in a modified example in Fig. 14, a processing oil application step S14A in which the press processing oil b is applied only to the upper surface of the strip steel sheet M or to both the upper and lower surfaces of the strip steel sheet M may be adopted.
[0139] In this processing oil application step S14A, when the press processing oil b is applied only to the upper surface of the strip steel plate M, the lower roller 131b is retracted below the lower surface of the strip steel plate M to be out of contact with it, while the upper roller 131a is rolled against the upper surface of the strip steel plate M with the press processing oil b permeated into its outer circumferential surface. As a result, the press processing oil is applied to the entire surface of only the upper surface of the strip steel plate M. Then, on the lower surface of the strip steel plate M, a hardening accelerator layer a consisting of the anaerobic adhesive hardening accelerator a1 and the instantaneous adhesive hardening accelerator a2 is formed in an exposed state. On the other hand, on the upper surface of the strip steel plate M, the press processing oil b and the anaerobic adhesive c1 and instantaneous adhesive c2 applied on the press processing oil b are formed.
[0140] In this case, in the lamination and bonding step S18A in FIG. 14, the electromagnetic steel sheet 40, the periphery of which has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 261, is laminated on the top surface of the other electromagnetic steel sheet 40, the periphery of which has been punched out first, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the top surface side of the electromagnetic steel sheet 40, the press processing oil b below them, are pushed aside and applied to the top surface of the electromagnetic steel sheet 40. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the top surface of the electromagnetic steel sheet 40, the periphery of which has been punched out first, are mixed with the hardening accelerator layer a on the bottom surface of the electromagnetic steel sheet 40, the periphery of which has been punched out later. As a result, the anaerobic adhesive c1 is hardened while being mixed with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 is hardened instantly while being mixed with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described with reference to FIG. 10, so the same reference numerals are used and duplicated explanations are omitted.
[0141] Alternatively, for example, in the processing oil application step S14A shown in the modified example of FIG. In this case, in the processing oil application step S14A, the press processing oil b is permeated into both the upper roller 131a and the lower roller 131b, and then the upper roller 131a and the lower roller 131b are rolled while the strip steel plate M is sandwiched between them. As a result, a hardening acceleration layer a consisting of the anaerobic adhesive hardening accelerator a1 and the instantaneous adhesive hardening accelerator a2, and press processing oil b covering the surface of the hardening acceleration layer a are formed on the lower surface of the strip steel plate M. Meanwhile, the press processing oil b and the anaerobic adhesive c1 and instantaneous adhesive c2 applied on this press processing oil b are formed on the upper surface of the strip steel plate M.
[0142] Then, in the lamination and bonding step S18A of FIG. 14, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 261 is laminated on the upper surface of the other electromagnetic steel sheet 40 whose periphery has been punched out earlier, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface side of the electromagnetic steel sheet 40 whose periphery has been punched out earlier are applied to the upper surface of the electromagnetic steel sheet 40, pushing aside the press processing oil b underneath them. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface of the electromagnetic steel sheet 40 whose periphery has been punched out earlier push aside the press processing oil b on the lower surface side of the electromagnetic steel sheet 40 whose periphery has been punched out later, and mix with the hardening accelerator layer a above it. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described with reference to FIG. 10, so the same reference numerals are used and duplicated explanations are omitted.
[0143] [Third embodiment] A third embodiment of the present invention will be described below with reference to FIGS. First, a bonded laminated core manufacturing apparatus 300 according to this embodiment will be described with reference to the side view shown in Fig. 15. As shown in Fig. 15, the bonded laminated core manufacturing apparatus 300 includes a strip steel plate supply section 310, a hardening promotion layer forming section 320, a drive section (not shown), a press processing oil application section 330, a press processing section 340, an adhesive application section 350, and a lamination bonding section 360.
[0144] The strip steel sheet supplying section 310 supports a hoop material F wound with a strip steel sheet M, which is the raw material for the electromagnetic steel sheet (steel sheet component) 40, and sends out the strip steel sheet M toward the right side of the paper in Fig. 15. In the following description, the right side of the paper, which is the feeding direction of the strip steel sheet M, may be referred to as the downstream side, and the left side of the paper, which is the opposite direction, may be referred to as the upstream side. The strip steel sheet M sent downstream from the strip steel sheet supplying section 310 is a steel sheet having the above-mentioned chemical composition, and both sides of the steel sheet are coated with the above-mentioned insulating coating.
[0145] The hardening accelerator layer forming section 320 includes a hardening accelerator tank 321 , a nozzle 322 , and a dryer 323 . The curing accelerator tank 321 has a first storage section for storing the anaerobic adhesive curing accelerator dissolved in a solvent, a second storage section for storing the instant adhesive curing accelerator dissolved in a solvent, and a curing accelerator mixing section (not shown). The first storage section and the second storage section are partitioned so that the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator do not mix with each other. The anaerobic adhesive curing accelerator is a compound that promotes instantaneous curing of the anaerobic adhesive by mixing with the anaerobic adhesive, and the compounds exemplified in the first embodiment above can be used. Similarly, the instant adhesive curing accelerator is a compound that promotes instantaneous curing of the instant adhesive by mixing with the instant adhesive curing accelerator (2-cyanoacrylate adhesive), and the compounds exemplified in the first embodiment above can be used. The solvent type can also be the same as the solvent type exemplified in the first embodiment above.
[0146] The nozzle 322 has a plurality of first nozzle holes for applying an anaerobic adhesive curing accelerator and a plurality of second nozzle holes for applying an instant adhesive curing accelerator (not shown). The first nozzle holes are directly connected to the first storage portion of the hardening accelerator tank 321 via first piping. The second nozzle holes are directly connected to the second reservoir of the hardening accelerator tank 321 via second piping. Furthermore, both of the first nozzle holes and the second nozzle holes are also connected to the curing accelerator mixing section via a third pipe. The curing accelerator mixing section is connected to both the first storage section and the second storage section via a fourth pipe. The curing accelerator mixing section can take in the anaerobic adhesive curing accelerator from the first storage section and the instant adhesive curing accelerator from the second storage section, and stir and mix them.
[0147] The first pipe, the second pipe, and the fourth pipe are connected to a switching valve (not shown). By operating this switching valve, the flow of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be switched to the following (1) or (2). (1) The anaerobic adhesive curing accelerator in the first storage section is caused to flow to the first nozzle hole through the first piping, and at the same time, the instant adhesive curing accelerator in the second storage section is caused to flow to the second nozzle hole through the second piping. As a result, the anaerobic adhesive curing accelerator is discharged from each of the first nozzle holes, and the instant adhesive curing accelerator is discharged from each of the second nozzle holes. (2) Both the anaerobic adhesive curing accelerator in the first storage section and the instant adhesive curing accelerator in the second storage section are taken into the curing accelerator mixing section via the fourth pipe and stirred and mixed. The mixed accelerator thus obtained by mixing the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator is caused to flow into both the first nozzle holes and the second nozzle holes via the third pipe. As a result, the mixed accelerator is discharged from both the first nozzle holes and the second nozzle holes.
[0148] The discharge outlets of each of the first nozzle holes are directed toward the upper surface of the strip-shaped steel plate M, and the anaerobic adhesive curing accelerator or the mixing accelerator can be applied to the upper surface in dots or lines. The outlets of each of the second nozzle holes are also directed toward the upper surface of the strip-shaped steel sheet M, and the instant adhesive hardening accelerator or the mixing accelerator can be applied to the upper surface in dots or lines. In the nozzle 322, the first nozzle holes and the second nozzle holes are arranged alternately, and the pitch is determined so that the hardening accelerators discharged from the respective holes are not mixed excessively on the coating surface of the strip-shaped steel sheet M. When the anaerobic adhesive hardening accelerator and the instant adhesive hardening accelerator are applied in a checkered pattern as described later with reference to FIG. 17, it is preferable that the pitch is the same as the pitch of the nozzle holes of the nozzle 353 described later, so that the application positions of these hardening accelerators coincide relatively with the application positions of the anaerobic adhesive and the instant adhesive in the subsequent process.
[0149] By switching between the above (1) and (2) by the switching valve, the application form of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the application surface of the strip-shaped steel sheet M is divided into a case where they are applied in an unmixed state and a case where they are applied in a mixed state. In the following explanation, the three types of curing accelerators, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators, may be collectively referred to simply as "curing accelerators." On the other hand, when it is necessary to distinguish between these, they will be explained separately as three types, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators.
[0150] The dryer 323 includes a pair of rollers 323a and a dryer 323b. The pair of rollers 323a are disposed downstream of the nozzle 322. The pair of rollers 323a hold the strip steel sheet M passing between them so that it is always kept horizontal. The dryer 323b is disposed at a position sandwiched between the pair of rollers 323a. The dryer 323b dries the hardening accelerator by blowing air onto the upper and lower surfaces of the strip steel plate M. As a result, the strip steel plate M receives the blowing of air at the point where it passes the upstream side of the pair of rollers 323a, and the hardening accelerator starts to dry, and the drying is completed before it reaches the downstream side of the pair of rollers 323a. Therefore, on the upper surface of the strip steel plate M after passing the downstream side of the pair of rollers 323a, a hardening accelerator layer in which the solvent has dried is formed with an even thickness over the entire surface. The thickness of the hardening accelerator layer can be exemplified as 0.1 μm. On the other hand, the lower surface of the strip steel plate M is not coated with the hardening accelerator, so the insulating coating remains exposed. The hardening accelerating layer can be formed in a variety of patterns by operating the switching valve, which will be described later with reference to Figs.
[0151] The drive unit is disposed at a position DR between the hardening acceleration layer forming unit 320 and the press working oil application unit 330. The drive unit intermittently sends out the strip steel sheet M from the hardening acceleration layer forming unit 320 toward the press working oil application unit 330 toward the right side of the drawing. Note that, on the upper surface of the strip steel sheet M sent out from the hardening acceleration layer forming unit 320, a hardening acceleration layer where the hardening accelerator has dried has already been formed before entering the drive unit. On the other hand, on the lower surface of the strip steel sheet M before entering the drive unit, there is no hardening acceleration layer, and the insulating coating remains exposed.
[0152] The press working oil application section 330 includes an application roller 331 and an oil pan 332 . The oil pan 332 is disposed below the strip steel sheet M and directly below the application roller 331. The application roller 331 has an upper roller 331a and a lower roller 331b. The upper roller 331a is disposed directly above the strip steel sheet M, and by moving up and down, can be switched between a state in contact with and a state separated from the upper surface of the strip steel sheet M. The upper roller 331a can apply press processing oil to the upper surface of the strip steel sheet M by rolling while in contact with the upper surface of the steel sheet M with press processing oil supplied from a press processing oil supply unit (not shown) permeating its outer circumferential surface. The lower roller 331b is disposed directly below the strip steel sheet M, and by moving up and down, can be switched between a state in contact with and a state separated from the lower surface of the strip steel sheet M. The lower roller 331b can apply press processing oil to the underside of the strip steel sheet M by rolling while in contact with the underside of the steel sheet M in a state in which the press processing oil supplied from the press processing oil supply unit has permeated its outer circumferential surface. The oil pan 332 receives and collects excess press oil dripping from the upper roller 331a and the lower roller 331b, and returns it to the press oil supply section.
[0153] According to the press processing oil application section 330, by supplying press processing oil from the press processing oil supply section while the upper roller 331a is in contact with the upper surface of the strip steel plate M, a layer of press processing oil can be formed over the entire upper surface of the strip steel plate M, while the strip steel plate M is continuously or intermittently sent downstream. Similarly, by supplying press processing oil from the press processing oil supply section while the lower roller 331b is in contact with the underside of the strip steel plate M, a layer of press processing oil can be formed over the entire underside of the strip steel plate M, while the strip steel plate M is sent out continuously or intermittently to the downstream side.
[0154] Alternatively, by sandwiching the strip steel sheet M between the upper roller 331a and the lower roller 331b, a layer of press processing oil can be formed over the entire surface of both the upper and lower surfaces of the strip steel sheet M, while the strip steel sheet M is continuously or intermittently sent downstream. In this way, by moving the positions of the upper roller 331a and the lower roller 331b up and down as needed, the press processing oil can be applied in three ways: only to the upper surface of the strip steel plate M, only to the lower surface of the strip steel plate M, or to both the upper and lower surfaces of the strip steel plate M.
[0155] Here, in any of the above cases, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the upper surface of the strip steel sheet M are actively dried rather than naturally dried before the press processing oil is applied. In this way, since the curing accelerator layer is formed by actively drying in advance, it is suppressed that they are mixed with the press processing oil and diluted. Therefore, the concentration of the anaerobic adhesive curing accelerator and the concentration of the instant adhesive curing accelerator on the upper surface of the strip steel sheet M after the press processing oil is applied are both maintained unchanged before and after the application of the press processing oil b. Therefore, the strip steel sheet M after passing through the press processing oil application section 330 is sent to the press processing section 340 while maintaining the concentration of the curing accelerator on its upper surface.
[0156] The press processing section 340 includes a first stage punching section 341 , a second stage punching section 342 , and a third stage punching section 343 . The first-stage punching section 341 is disposed downstream of the press oil application section 330 and has a male die 341a and a female die 341b. The male die 341a and the female die 341b are disposed coaxially along the vertical direction, and the strip steel sheet M is inserted between them. Thus, the male die 341a faces the upper surface of the strip steel sheet M, and the female die 341b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is temporarily stopped, the male die 341a is moved downward by a hydraulic mechanism (not shown) to reach the female die 341b, thereby performing the first punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press oil is applied to the strip steel sheet M, it can be punched without causing seizure or the like. After this punching process, the male die 341a is then moved upward and pulled out from the female die 341b, and the strip steel sheet M is again sent out toward the downstream side.
[0157] The second-stage punching section 342 is disposed downstream of the second-stage punching section 341 and has a male die 342a and a female die 342b. The male die 342a and the female die 342b are disposed coaxially along the vertical direction, and the strip steel sheet M after the first punching process is inserted between them. Thus, the male die 342a faces the upper surface of the strip steel sheet M, and the female die 342b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 342a is moved downward by a hydraulic mechanism (not shown) to reach the female die 342b, thereby performing the second punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 342a is then moved upward and pulled out from the female die 342b, and the strip steel sheet M is sent out again toward the downstream side.
[0158] The third-stage punching section 343 is disposed downstream of the second-stage punching section 342 and has a male die 343a and a female die 343b. The male die 343a and the female die 343b are disposed coaxially along the vertical direction, and the strip steel sheet M after the second punching process is inserted between them. Thus, the male die 343a faces the upper surface of the strip steel sheet M, and the female die 343b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 343a is moved downward by a hydraulic mechanism (not shown) to reach the female die 343b, thereby performing the third punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since press processing oil is applied to the upper surface of the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 343a is then moved upward and pulled out from the female die 343b, and the strip steel sheet M is again sent out toward the downstream side.
[0159] The adhesive applying section 350 is incorporated in a lamination bonding section 360 located downstream of the press processing section 340. The adhesive applying section 350 includes an air compressor 351, a syringe 352, and a nozzle 353. The syringe 352 is a container having a space for storing an anaerobic adhesive and a space for storing an instant adhesive (not shown). The space for storing the anaerobic adhesive and the space for storing the instant adhesive are partitioned so that the anaerobic adhesive and the instant adhesive do not mix. Here, the anaerobic adhesive that can be used is one exemplified in the first embodiment. Similarly, the instant adhesive that can be used is one exemplified in the first embodiment. Syringe 352 and air compressor 351 are connected by a pipe that sends air from air compressor 351 to syringe 352. Syringe 352 and nozzle 353 are connected from syringe 352 to nozzle 353 via a fifth pipe that supplies an anaerobic adhesive and a sixth pipe that supplies an instant adhesive.
[0160] The nozzle 353 is equipped with a plurality of needles (not shown) whose outlets face downward. These needles are arranged above the steel strip M. Thus, the outlets of the needles face the upper surface of the steel strip M. The needles include a plurality of first needles for applying the anaerobic adhesive and a plurality of second needles for applying the instant adhesive (not shown). The outlets of the first and second needles are arranged alternately and evenly when the nozzle 353 is viewed from the bottom.
[0161] Here, when the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in a checkered pattern as shown in FIG. 17 described later, it is preferable to make the position of the outlet of each of the first needles coincide with the position of each anaerobic adhesive curing accelerator applied and dried on the upper surface of the strip steel plate M. Similarly, it is preferable to make the position of the outlet of each of the second needles coincide with the position of each instant adhesive curing accelerator applied and dried on the upper surface of the strip steel plate M. In this case, when the feed of the strip steel plate M is temporarily stopped above the nozzle 153 via the press processing section 140, the relative positions of each anaerobic adhesive curing accelerator on the upper surface of the strip steel plate M and the outlet of each of the first needles coincide, and further, the relative positions of each instant adhesive curing accelerator and the outlet of each of the second needles coincide. This allows each adhesive to be applied in a correct combination with each curing accelerator.
[0162] Each of the first needles is directly connected to the space storing the anaerobic adhesive via the fifth pipe, while each of the second needles is directly connected to the space storing the instant adhesive via the sixth pipe. The first needles and the second needles can apply the anaerobic adhesive and the instant adhesive so as to form a checkered (grid) pattern on the upper surface of the strip steel plate M. As a result, square or circular patterns made of the anaerobic adhesive and square or circular patterns made of the instant adhesive are alternately arranged along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the upper surface of the strip steel plate M. In other words, the anaerobic adhesive and the instant adhesive can be arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M.
[0163] Furthermore, in this positioned state, when air is pressure-fed from the air pump 351 to the syringe 352, the air is evenly supplied to both the space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive. Then, the anaerobic adhesive is supplied to each of the first needles via the fifth pipe, and the instantaneous adhesive is supplied to each of the second needles via the sixth pipe. Then, the anaerobic adhesive is discharged from the outlet of each of the first needles and applied to the upper surface of the strip-shaped steel sheet M. Similarly, the instantaneous adhesive is discharged from the outlet of each of the second needles and applied to the upper surface of the strip-shaped steel sheet M.
[0164] The laminated adhesive section 360 includes a peripheral punching male die 361 , a peripheral punching female die 362 , a spring 363 , and a heater 364 . The outer periphery punching male die 361 is a cylindrical die having a circular bottom surface, and the upper end of the die is connected to the lower end of the spring 363. The outer periphery punching male die 361 is supported by the spring 363 and can move up and down together with the spring 363. The outer periphery punching male die 361 has approximately the same outer diameter as the outer diameter of the stator adhesive laminated core 21.
[0165] The outer periphery punching female die 362 is a die having a cylindrical internal space, and has an inner diameter dimension that is approximately the same as the outer diameter dimension of the stator bonded laminated core 21 . The heater 364 is integrally built into the outer periphery punching female die 362. The heater 364 heats the periphery of each of the electromagnetic steel sheets (steel sheet components) 40 stacked in the outer periphery punching female die 362. When a heat-curing type adhesive is used as the adhesive, the adhesive cures when it receives heat from the heater 364. On the other hand, when a room temperature curing type adhesive is used as the adhesive, the adhesive cures at room temperature without the need for heating.
[0166] According to the laminated adhesive section 360, while the feeding of the strip steel sheet M is temporarily stopped, the outer periphery punching male die 361 is lowered to sandwich the strip steel sheet M between it and the outer periphery punching female die 362, and the outer periphery punching male die 361 is further pushed into the outer periphery punching female die 362, thereby obtaining an electromagnetic steel sheet 40 whose periphery has been punched out from the strip steel sheet M. This punched out electromagnetic steel sheet 40 is stacked on the top surface of other electromagnetic steel sheets 40 that have been previously punched out and stacked and bonded inside outer periphery punching female die 362, and is further subjected to a pressure from outer periphery punching male die 361 and heat from heater 364. At this time, the pressure applied to electromagnetic steel sheet 40 from outer periphery punching male die 361 is always kept constant by the biasing force of spring 363. As a result, the currently punched electromagnetic steel sheet 40 is adhered and fixed to the upper surface of the previously punched electromagnetic steel sheet 40. By repeating these steps of outer periphery punching, pressurizing, and heating a number of times corresponding to the number of laminated electromagnetic steel sheets 40, an adhesive laminated core 21 for a stator is formed in the outer periphery punching female die 362.
[0167] 15, the female die 341b, the female die 342b, the female die 343b, the outer periphery punching female die 362, and the heater 364 are fixed on a common fixed base 371. Therefore, the relative positions of the female die 341b, the female die 342b, the female die 343b, the outer periphery punching female die 362, and the heater 364 are fixed in the horizontal and vertical directions. Similarly, the male die 341a, the male die 342a, the male die 343a, the nozzle 353, and the outer periphery punching male die 361 are also fixed to the lower surface of a common movable base 372. Therefore, the relative positions of the male die 341a, the male die 342a, the nozzle 353, and the outer periphery punching male die 361 are also fixed in the horizontal and vertical directions.
[0168] The drive unit sends out the strip steel plate M downstream and, when it is temporarily stopped, lowers the movable base 372, thereby simultaneously performing the following: outer periphery punching, stacking and bonding of the electromagnetic steel plate 40 and application of adhesive for the next process; the third punching process at the position on the strip steel plate M where the next outer periphery punching will be performed; the second punching process at the position on the strip steel plate M where the next third punching process will be performed; and the first punching process at the position on the strip steel plate M where the next second punching process will be performed. Next, the movable base 372 is raised and retracted above the strip steel sheet M, and the drive unit again sends out the strip steel sheet M a predetermined distance downstream and then pauses again. In this state, the movable base 372 is lowered again, and processing is continued at each position. In this way, the process of moving the movable base 372 up and down during pauses while intermittently sending the strip steel sheet M by the drive unit is repeated, thereby manufacturing the stator adhesive laminated core 21.
[0169] A bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 300 having the above-described configuration will be described below with reference to FIGS. Fig. 16 is a flow chart for explaining the method for manufacturing a bonded laminated core according to the present embodiment. Fig. 17 is a diagram for explaining a first embodiment of the method for manufacturing a bonded laminated core, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a GG sectional view of (a). Fig. 18 is a diagram for explaining a second embodiment of the method for manufacturing a bonded laminated core, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a HH sectional view of (a). Fig. 19 is a diagram for explaining a third embodiment of the method for manufacturing a bonded laminated core, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a II sectional view of (a). Fig. 20 is a flow chart for explaining a modified example of the method for manufacturing a bonded laminated core according to the present embodiment.
[0170] As shown in FIG. 16, the adhesive laminated core manufacturing method of this embodiment includes a steel plate feeding process S21, a hardening accelerator application process S22, a hardening accelerator drying process S23, a processing oil application process S24, a first punching process S25, a second punching process S26, a third punching process S27, a stacking and bonding process S28, a stack number confirmation process S29, and a removal process S30.
[0171] In the steel plate delivery step S21, a strip-shaped steel plate M is delivered downstream from the hoop material F. In the subsequent hardening accelerator application process S22, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are applied from the nozzle 322 to the entire upper surface of the strip-shaped steel plate M. At this point, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are both in liquid form.
[0172] Here, three application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are shown in Fig. 17 to Fig. 19. Fig. 17 to Fig. 19 correspond to the lamination and adhesion step S28, but the application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 formed in the curing accelerator application step S22 remain fixed after the curing accelerator drying step S23. Therefore, the application patterns will be explained using these drawings.
[0173] For example, in the application pattern of Fig. 17, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to form a checkered (lattice) pattern on the upper surface of the strip steel plate M (electromagnetic steel plate 40). More specifically, square or circular patterns made of the anaerobic adhesive curing accelerator a1 and square or circular patterns made of the instant adhesive curing accelerator a2 are arranged alternately along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the upper surface of the strip steel plate M. That is, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried in the subsequent curing accelerator drying step S23 to form a curing accelerator layer a having a constant thickness.
[0174] In the application pattern of FIG. 18, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are mixed in advance and placed on the upper surface of the strip steel plate M (electromagnetic steel plate 40). This mixing is obtained by taking both the anaerobic adhesive curing accelerator a1 in the first storage section and the instant adhesive curing accelerator a2 in the second storage section into the curing accelerator mixing section through the third pipe in the curing accelerator layer forming section 320 and stirring and mixing them. The mixing accelerator thus obtained is supplied to both the first nozzle holes and the second nozzle holes through the fourth pipe. As a result, the mixing accelerator is discharged from both the first nozzle holes and the second nozzle holes. The discharged mixing accelerator is then evenly arranged on the insulating coating formed on the upper surface of the strip steel plate M along both the longitudinal direction of the strip steel plate M and the width direction of the strip steel plate M. The mixed accelerator thus applied is dried in the subsequent hardening accelerator drying step S23 to form a hardening accelerator layer a having a certain thickness.
[0175] Alternatively, in the application pattern of FIG. 19, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged so as to form stripes (lines) on the upper surface of the strip-shaped steel sheet M (electromagnetic steel sheet 40). More specifically, a linear pattern consisting of the anaerobic adhesive curing accelerator a1 and a linear pattern consisting of the instant adhesive curing accelerator a2 are alternately arranged along the longitudinal direction of the strip-shaped steel sheet M on the insulating film formed on the upper surface of the strip-shaped steel sheet M. That is, when the right direction of the paper in FIG. 19(b) is the feed direction of the strip-shaped steel sheet M, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are each formed in a linear shape so as to be parallel to the direction perpendicular to the feed direction. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged adjacent to each other when viewed along the feed direction of the strip-shaped steel sheet M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried in the subsequent curing accelerator drying step S3 to form a curing accelerator layer a having a constant thickness. In addition, instead of the above-mentioned application form, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 may be formed in a straight line parallel to the feed direction of the strip steel plate M, so that the downward direction of the paper in Figure 19(b) corresponds to the feed direction of the strip steel plate M.
[0176] Returning to Fig. 16, in the subsequent hardening accelerator drying step S23, air from the dryer 323b is blown onto the upper and lower surfaces of the strip-shaped steel plate M to dry the liquid hardening accelerator a1 for the anaerobic adhesive and the hardening accelerator a2 for the instant adhesive, thereby forming a hardening accelerator layer a. This hardening accelerator layer a is solid. In the subsequent processing oil application step S24, the upper roller 331a rolls in contact with the upper surface of the steel sheet M with the press processing oil b supplied from the press processing oil supply unit permeating its outer circumferential surface. As a result, the press processing oil is applied to the entire surface of only the upper surface of the strip-shaped steel sheet M. In other words, the press processing oil b is applied so as to cover the upper surface of the hardening-accelerating layer a. At this time, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are actively dried instead of being naturally dried. In this way, the curing accelerator layer a is formed by actively drying in advance, so that it is prevented from being mixed with and diluted by the press processing oil b applied on the upper surface. On the other hand, the lower roller 331b has been lowered and separated from the lower surface of the strip steel sheet M, so that the press working oil b is not applied to the lower surface of the strip steel sheet M, and the insulating coating remains exposed.
[0177] In the subsequent first punching process S25, the first punching of the strip steel sheet M is performed by the first-stage punching unit 341. At this time, since the press processing oil b has been applied in advance to the upper surface of the strip steel sheet M, defects in the press processing such as seizure between the male die 341a and the female die 341b do not occur. In the subsequent second punching process S26, the second punching of the strip steel sheet M is performed by the second-stage punching unit 342. At this time, too, since the press processing oil b has been applied in advance to the upper surface of the strip steel sheet M, defects in the press processing such as seizure between the male die 342a and the female die 342b do not occur.
[0178] In the subsequent third punching process S27, the third punching of the strip steel sheet M is performed by the third-stage punching section 343. At this time, too, since the press processing oil b has been applied in advance to the upper surface of the strip steel sheet M, defects in the press processing such as seizure between the male die 343a and the female die 343b do not occur. By the above-mentioned first punching process S25 to third punching process S27, the core back portion 22 and the teeth portion 23 shown in FIG. 1 are formed in the strip-shaped steel plate M, except for the outer shape portion.
[0179] In the subsequent lamination and bonding step S28, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 361 is laminated on the upper surface of the other electromagnetic steel sheet 40 that was previously punched out. At this time, a hardening acceleration layer a, press processing oil b covering the upper surface of this hardening acceleration layer a, and anaerobic adhesive c1 and instant adhesive c2 applied on this press processing oil b are arranged on the upper surface of the other electromagnetic steel sheet 40. Meanwhile, the lower surface of the electromagnetic steel sheet 40 laminated on top of that leaves the insulating coating exposed. In addition, as shown in FIG. 17(b), when the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged in a checkered pattern, the anaerobic adhesive c1 and the instant adhesive c2 are also arranged in a checkered pattern in accordance with their relative positions. Then, the magnetic steel sheets 40 are heated in a stacked and pressurized state. Then, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface of the magnetic steel sheet 40 that has been punched out first are applied to the lower surface of the magnetic steel sheet 40 that has been punched out later. Furthermore, the anaerobic adhesive c1 and the instantaneous adhesive c2 push aside the press processing oil b underneath and mix with the hardening accelerator layer a underneath. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a.
[0180] By sequentially repeating the above steps, a predetermined number of electromagnetic steel sheets 40 are laminated and bonded together, and the bonded laminated core 21 for the stator is completed. That is, in the stacking number confirmation step S29, it is determined whether or not the number of stacked electromagnetic steel sheets 40 has reached a predetermined number. As a result, if it has not reached that number (determination: NO), the flow returns to the steel sheet delivery step S21, and the steel sheet delivery step S21 to the stacking and bonding step S28 are repeated again. On the other hand, if the predetermined number has been reached in the stacking number confirmation step S29 (determination: YES), the flow proceeds to the removal step S30. In the subsequent removal step S30, the completed bonded laminated core 21 for a stator is removed from the outer periphery punching female die 362, thereby completing all steps of the bonded laminated core manufacturing method.
[0181] The main points of the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 300 described above will be summarized below. The method for manufacturing a bonded laminated core in this embodiment is a method for manufacturing a bonded laminated core 21 for a stator (bonded laminated core) by applying an anaerobic adhesive a1 and an instant adhesive a2 to one side (upper side) of a strip-shaped steel plate M, on which a press processing oil b has been applied, pressing the strip to obtain a plurality of electromagnetic steel plates 40 (steel plate components), and stacking and bonding the electromagnetic steel plates 40 together. In this embodiment, a hardening accelerator layer a is formed by applying and drying an anaerobic adhesive hardening accelerator a1 and an instant adhesive hardening accelerator a2 to the upper surface of the strip-shaped steel plate M before applying the press processing oil b, and then the press processing oil b is applied to this hardening accelerator layer a, and the anaerobic adhesive c1 and instant adhesive c2 are applied to this press processing oil b. According to the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 300 described above, it is possible to obtain the same effects as those described in the first embodiment.
[0182] In addition, as shown in FIG. 17, in the above-mentioned adhesive laminated core manufacturing method, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 may be arranged in a checkered pattern. Alternatively, as shown in FIG. 18, in the above-mentioned adhesive laminated core manufacturing method, the curing accelerator a1 for anaerobic adhesives and the curing accelerator a2 for instant adhesives may be mixed in advance and then applied and dried to form the curing accelerator layer a. Alternatively, as shown in FIG. 19, in the above adhesive laminated core manufacturing method, the curing accelerator a1 for anaerobic adhesives and the curing accelerator a2 for instant adhesives may be arranged in stripes to form the curing accelerator layer a. In any of the above cases, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 can be evenly distributed along the coating surface of the strip steel sheet M. Therefore, the adhesive strength along the coating surface can be made uniform.
[0183] More specifically, the method for manufacturing the bonded laminated core includes the following steps. That is, each electromagnetic steel sheet 40 includes an electromagnetic steel sheet (second steel sheet component) 40 which has been circumferentially punched first and an electromagnetic steel sheet (first steel sheet component) 40 which has been circumferentially punched later. This adhesive laminated core manufacturing method includes a fourth step of preparing an electromagnetic steel sheet (second steel sheet component) 40 which has an upper surface (first surface), a hardening promotion layer a formed on this upper surface, press processing oil b placed on this hardening promotion layer a, and an anaerobic adhesive c1 and an instant adhesive c2 placed on the press processing oil b; a fifth step of preparing an electromagnetic steel sheet (first steel sheet component) 40 which has a lower surface (second surface) and which has been circumferentially punched later; and a sixth step of overlapping and adhering the electromagnetic steel sheet (second steel sheet component) 40 which has been circumferentially punched first and the electromagnetic steel sheet (first steel sheet component) 40 which has been circumferentially punched later so that the upper surface and the lower surface face each other. According to this method for manufacturing a bonded laminated core, it is possible to obtain the same effects as those described in the first embodiment.
[0184] In the above-mentioned bonded laminated core manufacturing method, the bonded laminated core for a stator (bonded laminated core) 21 may be a stator for a rotating electric machine. This adhesive laminated core manufacturing method achieves higher productivity while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electrical machines that have high performance yet are low in manufacturing cost.
[0185] The bonded laminated core manufacturing apparatus 300 of this embodiment is an apparatus for manufacturing a stator bonded laminated core (bonded laminated core) 21 including a plurality of electromagnetic steel plates (steel plate components) 40 punched out from a strip-shaped steel plate M. The bonded laminated core manufacturing apparatus 300 of this embodiment is equipped with a press processing oil application section 330 that applies press processing oil b to the upper surface (one side) of the strip-shaped steel plate M; a press processing section 340 that applies press processing to the strip-shaped steel plate M; an adhesive application section 350 that applies anaerobic adhesive a1 and instant adhesive a2 to the upper surface of the strip-shaped steel plate M; and a hardening acceleration layer forming section 320 that forms a hardening acceleration layer a by applying and drying anaerobic adhesive hardening accelerator a1 and instant adhesive hardening accelerator a2 to the upper surface of the strip-shaped steel plate M before applying the press processing oil b. According to the bonded laminated core manufacturing apparatus 300, it is possible to obtain the same effects as those described in the first embodiment.
[0186] In the adhesive laminated core manufacturing apparatus 300, the hardening acceleration layer forming section 320 may be equipped with a nozzle 322 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in a checkered pattern, as shown in FIG. Alternatively, in the above-mentioned adhesive laminated core manufacturing apparatus 300, the hardening acceleration layer forming section 320 may be provided with a pipe (hardening accelerator supply flow path) through which the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are mixed in advance and flow, as shown in FIG. 18, and a nozzle 322 connected to this pipe. Alternatively, in the adhesive laminated core manufacturing apparatus 300, the hardening acceleration layer forming section 320 may be equipped with a nozzle 322 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in stripes, as shown in FIG. In any of the above cases, the nozzle 322 can distribute the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 evenly along the coating surface of the strip-shaped steel sheet M. Therefore, the adhesive strength along the coating surface can be made uniform.
[0187] In this embodiment, the case where the press processing oil b is applied only to the upper surface of the strip steel plate M in the processing oil application step S24 shown in Fig. 16 has been described, but the present invention is not limited to this. For example, as shown in a modified example in Fig. 20, a processing oil application step S24A in which the press processing oil b is applied to both the upper and lower surfaces of the strip steel plate M may be adopted.
[0188] In this processing oil application step S24A, press processing oil b is applied to both the upper and lower surfaces of the strip steel plate M. That is, the press processing oil b is permeated into both the upper roller 331a and the lower roller 331b, and then the upper roller 331a and the lower roller 331b are rolled while the strip steel plate M is sandwiched between them. As a result, on the upper surface of the strip steel plate M, a hardening acceleration layer a consisting of an anaerobic adhesive hardening accelerator a1 and an instant adhesive hardening accelerator a2, press processing oil b covering the surface of the hardening acceleration layer a, and anaerobic adhesive c1 and instant adhesive c2 applied to the surface of the press processing oil b are formed. On the other hand, only the press processing oil b is formed on the lower surface of the strip steel plate M.
[0189] Then, in the lamination and bonding process S28A of FIG. 20, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 361 is laminated on the upper surface of the other electromagnetic steel sheet 40 whose periphery has been punched out earlier, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface side of the electromagnetic steel sheet 40 whose periphery has been punched out earlier are applied to the lower surface of the steel sheet part 40 whose periphery has been punched out later, pushing aside the press processing oil b applied to this lower surface. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the upper surface of the electromagnetic steel sheet 40 whose periphery has been punched out earlier push aside the press processing oil b that is underneath them and mix with the hardening accelerator layer a underneath. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described with reference to FIG. 16, so the same reference numerals are used and duplicated explanations are omitted.
[0190] [Fourth embodiment] The fourth embodiment of the present invention will be described below with reference to FIGS. First, a bonded laminated core manufacturing apparatus 400 according to this embodiment will be described with reference to a side view shown in Fig. 21. As shown in Fig. 21, the bonded laminated core manufacturing apparatus 400 includes a strip steel plate supply section 410, a hardening promotion layer forming section 420, a drive section (not shown), a press processing oil application section 430, a press processing section 440, an adhesive application section 450, and a lamination bonding section 460.
[0191] The strip steel sheet supplying section 410 supports a hoop material F wound with a strip steel sheet M, which is the raw material for the electromagnetic steel sheet (steel sheet component) 40, and sends out the strip steel sheet M toward the right side of the paper in Fig. 21. In the following description, the right side of the paper, which is the feeding direction of the strip steel sheet M, may be referred to as the downstream side, and the left side of the paper, which is the opposite direction, may be referred to as the upstream side. The strip steel sheet M sent downstream from the strip steel sheet supplying section 410 is a steel sheet having the above-mentioned chemical composition, and both sides of the steel sheet are coated with the above-mentioned insulating coating.
[0192] The hardening accelerator layer forming section 420 includes a hardening accelerator tank 421 , a nozzle 422 , a seal box 423 , and a wiping roller 424 . The curing accelerator tank 421 has a first storage section for storing the anaerobic adhesive curing accelerator dissolved in a solvent, a second storage section for storing the instant adhesive curing accelerator dissolved in a solvent, and a curing accelerator mixing section (not shown). The first storage section and the second storage section are partitioned so that the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator do not mix with each other. The anaerobic adhesive curing accelerator is a compound that promotes instantaneous curing of the anaerobic adhesive by mixing with the anaerobic adhesive, and the compounds exemplified in the first embodiment above can be used. Similarly, the instant adhesive curing accelerator is a compound that promotes instantaneous curing of the instant adhesive by mixing with the instant adhesive curing accelerator (2-cyanoacrylate adhesive), and the compounds exemplified in the first embodiment above can be used. The solvent type can also be the same as the solvent type exemplified in the first embodiment above.
[0193] The nozzle 422 has a plurality of first nozzle holes for applying an anaerobic adhesive curing accelerator and a plurality of second nozzle holes for applying an instant adhesive curing accelerator (not shown). The first nozzle holes are directly connected to the first storage portion of the hardening accelerator tank 421 via first piping. The second nozzle holes are directly connected to the second storage portion of the hardening accelerator tank 421 via second piping. Furthermore, both of the first nozzle holes and the second nozzle holes are also connected to the curing accelerator mixing section via a third pipe. The curing accelerator mixing section is connected to both the first storage section and the second storage section via a fourth pipe. The curing accelerator mixing section can take in the anaerobic adhesive curing accelerator from the first storage section and the instant adhesive curing accelerator from the second storage section, and stir and mix them.
[0194] The first pipe, the second pipe, and the fourth pipe are connected to a switching valve (not shown). By operating this switching valve, the flow of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator can be switched to the following (1) or (2). (1) The anaerobic adhesive curing accelerator in the first storage section is caused to flow to the first nozzle hole through the first piping, and at the same time, the instant adhesive curing accelerator in the second storage section is caused to flow to the second nozzle hole through the second piping. As a result, the anaerobic adhesive curing accelerator is discharged from each of the first nozzle holes, and the instant adhesive curing accelerator is discharged from each of the second nozzle holes. (2) Both the anaerobic adhesive curing accelerator in the first storage section and the instant adhesive curing accelerator in the second storage section are taken into the curing accelerator mixing section via the fourth pipe and stirred and mixed. The mixed accelerator thus obtained by mixing the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator is caused to flow into both the first nozzle holes and the second nozzle holes via the third pipe. As a result, the mixed accelerator is discharged from both the first nozzle holes and the second nozzle holes.
[0195] The discharge outlets of each of the first nozzle holes are directed toward the lower surface of the strip-shaped steel plate M, and the anaerobic adhesive curing accelerator or the mixing accelerator can be applied to the lower surface in dots or lines. The outlets of each of the second nozzle holes are also directed toward the lower surface of the strip-shaped steel sheet M, and the instant adhesive hardening accelerator or the mixing accelerator can be applied to the lower surface in dots or lines. In the nozzle 422, the first nozzle holes and the second nozzle holes are arranged alternately, and the pitch is determined so that the hardening accelerators discharged from the respective holes are not mixed excessively on the coating surface of the strip-shaped steel sheet M. When the anaerobic adhesive hardening accelerator and the instant adhesive hardening accelerator are applied in a checkered pattern as described later with reference to FIG. 23, it is preferable that the pitch is the same as the pitch of the nozzle holes of the nozzle 453 described later, so that the application positions of these hardening accelerators coincide relatively with the application positions of the anaerobic adhesive and the instant adhesive in the subsequent process.
[0196] By switching between the above (1) and (2) by the switching valve, the application form of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the application surface of the strip-shaped steel sheet M is divided into a case where they are applied in an unmixed state and a case where they are applied in a mixed state. In the following explanation, the three types of curing accelerators, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators, may be collectively referred to simply as "curing accelerators." On the other hand, when it is necessary to distinguish between these, they will be explained separately as three types, anaerobic adhesive curing accelerators, instant adhesive curing accelerators, and mixed accelerators.
[0197] The seal box 423 is a box having an internal space, and has an entrance and an exit leading to the internal space. The strip steel sheet M is fed from the entrance into the internal space of the seal box 423 while maintaining its horizontal state, and then fed out of the seal box 423 from the exit. The nozzle 422 is disposed below the internal space of the seal box 423. As described above, the nozzle mouth of the nozzle 422 is directed to the lower surface of the portion of the strip steel sheet M that passes through the internal space. The hardening accelerator sprayed onto the lower surface of the strip steel sheet M from the nozzle 422 dries instantly because the solvent evaporates. As a result, a hardening accelerator layer with the solvent dried is formed on the lower surface of the strip steel sheet M with an even thickness over the entire surface before the strip steel sheet M exits from the exit. The thickness of the hardening accelerator layer can be exemplified as 0.1 μm. Since the upper surface of the strip steel sheet M is hardly coated with the hardening accelerator, the insulating coating is almost exposed. The wiping roller 424 mainly wipes off excess hardening accelerator remaining on the upper surface of the strip steel sheet M. As a result, the upper surface of the strip steel sheet M after passing through the wiping roller 424 is in a state where the hardening accelerator has been completely wiped off and the insulating coating remains exposed. The hardening accelerating layer can be formed in a variety of patterns by operating the switching valve, which will be described later with reference to Figs.
[0198] The drive unit is disposed at a position DR between the hardening acceleration layer forming unit 420 and the press working oil application unit 430. The drive unit intermittently sends out the strip steel sheet M from the hardening acceleration layer forming unit 420 toward the press working oil application unit 430 toward the right side of the drawing. Note that, on the lower surface of the strip steel sheet M sent out from the hardening acceleration layer forming unit 420, a hardening acceleration layer where the hardening accelerator has dried has already been formed before entering the drive unit. On the other hand, on the upper surface of the strip steel sheet M before entering the drive unit, there is no hardening acceleration layer, and the insulating coating remains exposed.
[0199] The press working oil application section 430 includes an application roller 431 and an oil pan 432 . The oil pan 432 is disposed below the strip steel sheet M and directly below the application roller 431. The application roller 431 has an upper roller 431a and a lower roller 431b. The upper roller 431a is disposed directly above the strip steel sheet M, and by moving up and down, can be switched between a state in contact with and a state separated from the upper surface of the strip steel sheet M. The upper roller 431a can apply press processing oil to the upper surface of the strip steel sheet M by rolling while being in contact with the upper surface of the steel sheet M with press processing oil supplied from a press processing oil supply unit (not shown) permeating its outer circumferential surface. The lower roller 431b is disposed directly below the strip steel sheet M, and can be switched between a state in contact with and a state separated from the lower surface of the strip steel sheet M by moving up and down. The lower roller 431b can apply press processing oil to the underside of the strip steel sheet M by rolling while being in contact with the underside of the steel sheet M in a state in which the press processing oil supplied from the press processing oil supply unit has permeated its outer circumferential surface. The oil pan 432 receives and collects excess press oil dripping from the upper roller 431a and the lower roller 431b, and returns it to the press oil supply section.
[0200] According to the press processing oil application section 430, by supplying press processing oil from the press processing oil supply section while the upper roller 431a is in contact with the upper surface of the strip steel plate M, a layer of press processing oil can be formed over the entire upper surface of the strip steel plate M, while the strip steel plate M is continuously or intermittently sent downstream. Similarly, by supplying press processing oil from the press processing oil supply section while the lower roller 431b is in contact with the underside of the strip steel plate M, a layer of press processing oil can be formed over the entire underside of the strip steel plate M, while the strip steel plate M is sent out downstream continuously or intermittently.
[0201] Alternatively, by sandwiching the strip steel sheet M between the upper roller 431a and the lower roller 431b, a layer of press processing oil can be formed over the entire surface of both the upper and lower surfaces of the strip steel sheet M, while the strip steel sheet M is continuously or intermittently sent downstream. In this way, by moving the positions of the upper roller 431a and the lower roller 431b up and down as needed, the press processing oil can be applied in three ways: only to the upper surface of the strip steel plate M, only to the lower surface of the strip steel plate M, or to both the upper and lower surfaces of the strip steel plate M.
[0202] Here, in any of the above cases, both the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator applied to the underside of the strip steel plate M are actively dried rather than naturally dried before the press processing oil is applied. In this way, since the curing accelerator layer is formed by actively drying in advance, it is suppressed that they are mixed with the press processing oil and diluted. Therefore, the concentration of the anaerobic adhesive curing accelerator and the concentration of the instant adhesive curing accelerator on the underside of the strip steel plate M after the press processing oil is applied are both maintained unchanged before and after the application of the press processing oil b. Therefore, the strip steel plate M after passing through the press processing oil application section 430 is sent to the press processing section 440 while maintaining the concentration of the curing accelerator on its underside.
[0203] The press processing section 440 includes a first stage punching section 441 and a second stage punching section 442 . The first-stage punching section 441 is disposed downstream of the press processing oil application section 430, and has a male die 441a and a female die 441b. The male die 441a and the female die 441b are disposed coaxially along the vertical direction, and the strip steel sheet M is inserted between them. Thus, the male die 441a faces the upper surface of the strip steel sheet M, and the female die 441b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is temporarily stopped, the male die 441a is moved downward by a hydraulic mechanism (not shown) to reach the female die 441b, thereby performing the first punching process required to form the electromagnetic steel sheet 40 from the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it can be punched without causing seizure or the like. After this punching process, the male die 441a is then moved upward and pulled out from the female die 441b, and the strip steel sheet M is again sent out toward the downstream side.
[0204] The second-stage punching section 442 is disposed downstream of the first-stage punching section 441 and has a male die 442a and a female die 442b. The male die 442a and the female die 442b are disposed coaxially along the vertical direction, and the strip steel sheet M after the first punching process is inserted between them. Thus, the male die 442a faces the upper surface of the strip steel sheet M, and the female die 442b faces the lower surface of the strip steel sheet M. Then, in a state where the delivery of the strip steel sheet M is again temporarily stopped, the male die 442a is moved downward by a hydraulic mechanism (not shown) to reach the female die 442b, thereby performing the second punching process required to form the electromagnetic steel sheet 40 of the strip steel sheet M. At this time, since the press processing oil is applied to the strip steel sheet M, it is possible to punch without causing seizure or the like. After this punching process, the male die 442a is then moved upward and pulled out from the female die 442b, and the strip steel sheet M is again sent out toward the downstream side.
[0205] The adhesive application section 450 is disposed downstream of the press processing section 440. The adhesive application section 450 includes an air compressor 451, a syringe 452, a nozzle 453, and a steel plate holder 454. The syringe 452 is a container having a space for storing an anaerobic adhesive and a space for storing an instantaneous adhesive (not shown). The space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive are partitioned so that the anaerobic adhesive and the instantaneous adhesive do not mix. Here, an example of the anaerobic adhesive is "Arontite" (registered trademark) manufactured by Toagosei Co., Ltd., and an example of the instantaneous adhesive (2-cyanoacrylate adhesive) is "Aron Alpha" (registered trademark) manufactured by Toagosei Co., Ltd. The syringe 452 and the air pump 451 are connected by a pipe that sends air from the air pump 451 to the syringe 452. The syringe 452 and the nozzle 453 are connected from the syringe 452 to the nozzle 453 via a fifth pipe that supplies the anaerobic adhesive and a sixth pipe that supplies the instantaneous adhesive.
[0206] The nozzle 453 is equipped with a plurality of needles (not shown) whose outlets face upward. These needles are arranged below the strip steel sheet M. Thus, the outlet of each of the needles faces the lower surface of the strip steel sheet M. Each of the needles has a plurality of first needles for applying the anaerobic adhesive and a plurality of second needles for applying the instant adhesive (not shown). The outlets of the first and second needles are arranged alternately and evenly when the nozzle 453 is viewed from above.
[0207] Here, when the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in a checkered pattern as shown in FIG. 23 described later, it is preferable to make the position of the outlet of each of the first needles coincide with the position of each anaerobic adhesive curing accelerator applied and dried on the lower surface of the strip steel plate M. Similarly, it is preferable to make the position of the outlet of each of the second needles coincide with the position of each instant adhesive curing accelerator applied and dried on the lower surface of the strip steel plate M. In this case, when the feed of the strip steel plate M is temporarily stopped above the nozzle 453 via the press processing section 440, the relative positions of each anaerobic adhesive curing accelerator on the lower surface of the strip steel plate M and the outlet of each of the first needles coincide, and further, the relative positions of each instant adhesive curing accelerator and the outlet of each of the second needles coincide. This allows each adhesive to be applied in a correct combination with each curing accelerator.
[0208] Each of the first needles is directly connected to the space storing the anaerobic adhesive via the fifth pipe, while each of the second needles is directly connected to the space storing the instant adhesive via the sixth pipe. The first needles and the second needles can apply the anaerobic adhesive and the instant adhesive so as to form a checkered (grid) pattern on the underside of the strip steel plate M. As a result, square or circular patterns made of the anaerobic adhesive and square or circular patterns made of the instant adhesive are alternately arranged along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the underside of the strip steel plate M. In other words, the anaerobic adhesive and the instant adhesive can be arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M.
[0209] The steel plate holder 454 is disposed above the nozzle 453 (directly above the first and second needles). Thus, the steel plate holder 454 faces the upper surface of the strip steel plate M. The steel plate holder 454 is pressed downward by a hydraulic mechanism (not shown) while the delivery of the strip steel plate M is temporarily stopped. As a result, the lower surface of the steel plate holder 454 comes into contact with the upper surface of the strip steel plate M and presses the strip steel plate M downward. This allows the height position of the strip steel plate M to be pressed down to the adhesive application position by the nozzle 453 and positioned. In this positioned state, the lower surface of the strip steel plate M is close to the discharge ports of the first and second needles.
[0210] Furthermore, when air is pumped from the air pump 451 to the syringe 452 in this positioning state, the air is evenly supplied to both the space for storing the anaerobic adhesive and the space for storing the instantaneous adhesive. Then, the anaerobic adhesive is supplied to each of the first needles via the fifth pipe, and the instantaneous adhesive is supplied to each of the second needles via the sixth pipe. Then, the anaerobic adhesive is discharged from the outlet of each of the first needles and applied to the lower surface of the strip-shaped steel plate M. Similarly, the instantaneous adhesive is discharged from the outlet of each of the second needles and applied to the lower surface of the strip-shaped steel plate M. Thereafter, the steel plate holder 454 is raised by the hydraulic mechanism, thereby returning the height position of the strip-shaped steel plate M to its original height.
[0211] The lamination bonding section 460 is disposed downstream of the adhesive application section 450. The lamination bonding section 460 includes a male outer periphery punching die 461, a female outer periphery punching die 462, a spring 463, and a heater 464. The outer periphery punching male die 461 is a cylindrical die having a circular bottom surface, and the upper end of the die is connected to the lower end of the spring 463. The outer periphery punching male die 461 is supported by the spring 463 and can move up and down together with the spring 463. The outer periphery punching male die 461 has an outer diameter substantially the same as that of the stator adhesive laminated core 21.
[0212] The outer periphery punching female die 462 is a die having a cylindrical internal space, and has an inner diameter dimension that is approximately the same as the outer diameter dimension of the stator bonded laminated core 21 . The heater 464 is integrally built into the outer periphery punching female die 462. The heater 464 heats the periphery of each of the electromagnetic steel sheets (steel sheet components) 40 stacked in the outer periphery punching female die 462. When a heat-curing type adhesive is used as the adhesive, the adhesive cures by receiving heat from the heater 464. On the other hand, when a room temperature curing type adhesive is used as the adhesive, the adhesive cures at room temperature without the need for heating.
[0213] According to the laminated adhesive section 460, while the feeding of the strip-shaped steel sheet M is temporarily stopped, the outer periphery punching male die 461 is lowered to sandwich the strip-shaped steel sheet M between it and the outer periphery punching female die 462, and the outer periphery punching male die 461 is further pushed into the outer periphery punching female die 462, thereby obtaining an electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M. This punched electromagnetic steel sheet 40 is stacked on the top surface of other electromagnetic steel sheets 40 that have been previously punched and stacked and bonded inside the outer periphery punching female die 462, and is further subjected to a pressure from the outer periphery punching male die 461 and heat from a heater 464. At this time, the pressure applied to the electromagnetic steel sheet 40 from the outer periphery punching male die 461 is always kept constant by the biasing force of the spring 463. As a result, the currently punched electromagnetic steel sheet 40 is adhered and fixed to the upper surface of the previously punched electromagnetic steel sheet 40. By repeating these steps of outer periphery punching, pressurizing, and heating a number of times corresponding to the number of laminated electromagnetic steel sheets 40, an adhesive laminated core 21 for a stator is formed in the outer periphery punching female die 462.
[0214] 21, the female die 441b, the female die 442b, the nozzle 453, the outer periphery punching female die 462, and the heater 464 are fixed on a common fixed base 471. Therefore, the relative positions of the female die 441b, the female die 442b, the nozzle 453, the outer periphery punching female die 462, and the heater 464 are fixed in the horizontal and vertical directions. Similarly, the male die 441a, the male die 442a, the steel plate holder 454, and the outer periphery punching male die 461 are also fixed to the lower surface of a common movable base 472. Therefore, the relative positions of the male die 441a, the male die 442a, the steel plate holder 454, and the outer periphery punching male die 461 in the horizontal and vertical directions are fixed.
[0215] The drive unit sends out the strip steel sheet M downstream and, when it is temporarily stopped, lowers the movable base 472, thereby simultaneously punching out the outer periphery of the electromagnetic steel sheet 40, stacking and gluing, applying anaerobic adhesive and instant adhesive to the position of the electromagnetic steel sheet 40 where the outer periphery will next be punched in the strip steel sheet M, the second punching process at the position of the strip steel sheet M where the anaerobic adhesive and instant adhesive will next be applied, and the first punching process at the position of the strip steel sheet M where the second punching process will next be performed. Next, the movable base 472 is raised and retracted above the strip steel sheet M, and then the drive unit sends out the strip steel sheet M a predetermined distance downstream again and pauses again. In this state, the movable base 472 is lowered again and processing is continued at each position. In this manner, the process of moving the movable base 472 up and down during pauses while intermittently sending the strip steel sheet M by the drive unit is repeated, thereby manufacturing the stator adhesive laminated core 21.
[0216] A bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 400 having the above-described configuration will be described below with reference to FIGS. Fig. 22 is a flow chart for explaining the adhesive laminated core manufacturing method according to this embodiment. Fig. 23 is a diagram for explaining a first embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a JJ sectional view of (a). Fig. 24 is a diagram for explaining a second embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is a KK sectional view of (a). Fig. 25 is a diagram for explaining a third embodiment of the adhesive laminated core manufacturing method, where (a) is a partial vertical sectional view showing the lamination and bonding process, and (b) is an LL sectional view of (a). Fig. 26 is a flow chart for explaining a modified example of the adhesive laminated core manufacturing method according to this embodiment.
[0217] As shown in FIG. 22, the adhesive laminated core manufacturing method of this embodiment includes a steel plate feeding process S31, a hardening accelerator application and drying process S32, an excess wiping process S33, a processing oil application process S34, a first punching process S35, a second punching process S36, an adhesive application process S37, a stacking and bonding process S38, a stack number confirmation process S39, and a removal process S40.
[0218] In the steel plate delivery step S31, a strip-shaped steel plate M is delivered downstream from the hoop material F. In the subsequent hardening accelerator application and drying process S32, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are applied to the entire lower surface of the strip-shaped steel plate M from the nozzle 422 and dried. At this point, both the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 have dried and become solid.
[0219] Here, three application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are shown in Fig. 23 to Fig. 25. Fig. 23 to Fig. 25 are diagrams corresponding to the lamination and adhesion step S38, and the application patterns of the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 formed in the curing accelerator application and drying step S32 remain fixed after the curing accelerator application and drying step S32. Therefore, the application patterns will be explained using these drawings.
[0220] For example, in the application pattern of Fig. 23, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to form a checkered (lattice) pattern on the lower surface of the strip steel plate M (electromagnetic steel plate 40). More specifically, square or circular patterns made of the anaerobic adhesive curing accelerator a1 and square or circular patterns made of the instant adhesive curing accelerator a2 are arranged alternately along both the longitudinal direction and the width direction of the strip steel plate M on the insulating coating formed on the lower surface of the strip steel plate M. That is, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged so as to be adjacent to each other along both the longitudinal direction and the width direction of the strip steel plate M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried before leaving the sealed box 423, and form a curing accelerator layer a having a certain thickness. This curing accelerator layer a is solid.
[0221] In the application pattern of FIG. 24, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are mixed in advance and placed on the lower surface of the strip steel plate M (electromagnetic steel plate 40). This mixing is obtained by taking both the anaerobic adhesive curing accelerator a1 in the first storage section and the instant adhesive curing accelerator a2 in the second storage section into the curing accelerator mixing section through the third pipe in the curing accelerator layer forming section 420 and stirring and mixing them. The mixing accelerator obtained in this manner is supplied to both the first nozzle holes and the second nozzle holes through the fourth pipe. As a result, the mixing accelerator is discharged from both the first nozzle holes and the second nozzle holes. The discharged mixing accelerator is then evenly placed on the insulating coating formed on the lower surface of the strip steel plate M along both the longitudinal direction of the strip steel plate M and the width direction of the strip steel plate M. The mixed accelerator thus applied is dried before leaving the sealed box 223, and forms a hardening accelerator layer a having a certain thickness. This hardening accelerator layer a is solid.
[0222] Alternatively, in the application pattern of FIG. 25, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged so as to form stripes (lines) on the lower surface of the strip-shaped steel sheet M (electromagnetic steel sheet 40). More specifically, a linear pattern consisting of the anaerobic adhesive curing accelerator a1 and a linear pattern consisting of the instant adhesive curing accelerator a2 are alternately arranged along the longitudinal direction of the strip-shaped steel sheet M on the insulating film formed on the lower surface of the strip-shaped steel sheet M. That is, when the right direction of the paper in FIG. 25(b) is the feed direction of the strip-shaped steel sheet M, the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are each formed in a linear shape so as to be parallel to the direction perpendicular to the feed direction. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are alternately arranged adjacent to each other when viewed along the feed direction of the strip-shaped steel sheet M. The anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 thus applied are dried before leaving the sealed box 423, and form a curing accelerator layer a having a certain thickness. This curing accelerator layer a is solid. In addition, instead of the above-mentioned application form, the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 may be formed in a straight line parallel to the feed direction of the strip steel plate M, so that the downward direction of the paper in Figure 25 (b) corresponds to the feed direction of the strip steel plate M.
[0223] Returning to Fig. 22, in the subsequent surplus wiping off process S33, the surplus hardening accelerator is wiped off on the upper surface of the strip steel sheet M. Therefore, no hardening acceleration layer a is formed on the upper surface of the strip steel sheet M. In the subsequent processing oil application step S34, the lower roller 131b rolls in contact with the lower surface of the steel sheet M with the press processing oil b supplied from the press processing oil supply unit permeating its outer circumferential surface. As a result, the press processing oil b is applied to the entire surface of only the lower surface of the strip-shaped steel sheet M. In other words, the press processing oil b is applied so as to cover the surface of the hardening-accelerating layer a. At this time, both the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are actively dried instead of being naturally dried. In this way, the curing accelerator layer a is formed by actively drying in advance, so that it is prevented from being mixed with and diluted by the press processing oil b applied to the surface. On the other hand, since the upper roller 131a has risen and is separated from the upper surface of the strip steel sheet M, the press working oil b is not applied to the upper surface of the strip steel sheet M, and the insulating coating remains exposed.
[0224] In the subsequent first punching process S35, the first punching of the strip steel sheet M is performed by the first-stage punching unit 441. At this time, since the press processing oil b has been applied in advance to the underside of the strip steel sheet M, defects in the press processing such as seizure between the male die 441a and the female die 441b do not occur. In the subsequent second punching process S36, the second punching of the strip steel sheet M is performed by the second-stage punching section 442. At this time, too, since the press processing oil b has been applied in advance to the underside of the strip steel sheet M, defects in the press processing such as seizure between the male die 442a and the female die 442b do not occur. By the above-mentioned first punching process S35 and second punching process S36, the core back portion 22 and the teeth portion 23 shown in FIG. 1 are formed in the strip-shaped steel plate M, except for the outer shape portion.
[0225] In the subsequent adhesive application process S37, as shown in Fig. 23 to Fig. 25, the anaerobic adhesive c1 and the instant adhesive c2 discharged from the nozzle 453 are applied directly to the lower surface of the strip-shaped steel plate M. At this time, the anaerobic adhesive c1 and the instant adhesive c2 are applied in dots having a predetermined thickness and a predetermined diameter. At this time, the anaerobic adhesive c1 and the instant adhesive c2 are in a liquid state because they have not yet been mixed with the hardening acceleration layer a. In addition, as shown in FIG. 23(b), when the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 are arranged in a checkered pattern, the anaerobic adhesive c1 and the instant adhesive c2 are also arranged in a checkered pattern in accordance with their relative positions.
[0226] In the subsequent lamination and bonding step S38, as shown in Figs. 23 to 25, the electromagnetic steel sheet 40, the outer periphery of which has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 461, is laminated on the upper surface of the other electromagnetic steel sheet 40 that has been punched out previously. At this time, the insulating coating is exposed on the upper surface of the other electromagnetic steel sheet 40. The electromagnetic steel sheet 40 that has been punched out this time is laminated on top of this and heated while being pressed. Then, the anaerobic adhesive c1 and the instant adhesive c2 on the lower surface side of the electromagnetic steel sheet 40 that has been punched out this time are applied to the upper surface of the other electromagnetic steel sheet 40 that has been punched out previously. At the same time, the anaerobic adhesive c1 and the instant adhesive c2 on the lower surface side of the electromagnetic steel sheet 40 that has been punched out this time push aside the press processing oil b on top of them and mix with the hardening accelerator layer a on top of them. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instant adhesive c2 mixes with the instant adhesive curing accelerator a2 in the curing accelerator layer a and cures instantly.
[0227] By sequentially repeating the above steps, a predetermined number of electromagnetic steel sheets 40 are laminated and bonded together, and the bonded laminated core 21 for the stator is completed. That is, in the stacking number confirmation step S39, it is determined whether or not the number of stacked electromagnetic steel sheets 40 has reached a predetermined number. If the number has not reached the predetermined number (determination: NO), the flow returns to the steel sheet delivery step S31, and the steel sheet delivery step S31 to the stacking and bonding step S38 are repeated again. On the other hand, if the number has reached the predetermined number in the stacking number confirmation step S39 (determination: YES), the flow proceeds to the removal step S40. In the subsequent removal step S40, the completed bonded laminated core 21 for a stator is removed from the outer periphery punching female die 462, thereby completing all steps of the bonded laminated core manufacturing method.
[0228] The main points of the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 400 described above will be summarized below. The method for manufacturing a bonded laminated core in this embodiment is a method for manufacturing a bonded laminated core 21 for a stator (bonded laminated core) by applying an anaerobic adhesive a1 and an instant adhesive a2 to one side (lower side) of a strip-shaped steel plate M, on which a press processing oil b is further applied, performing a press processing on the strip-shaped steel plate M, obtaining a plurality of electromagnetic steel plates 40 (steel plate components), and stacking and bonding the electromagnetic steel plates 40 together. In this embodiment, a hardening accelerator layer a is formed by applying an anaerobic adhesive hardening accelerator a1 and an instant adhesive hardening accelerator a2 to the underside of the strip steel plate M before applying the press processing oil b, and then drying the applied hardening accelerator layer a. According to this method for manufacturing a bonded laminated core, it is possible to obtain the same effects as those described in the first embodiment.
[0229] In the above-mentioned bonded laminated core manufacturing method, the bonded laminated core for a stator (bonded laminated core) 21 may be a stator for a rotating electric machine. This adhesive laminated core manufacturing method achieves higher productivity while ensuring sufficient adhesive strength, making it possible to manufacture stators for rotating electrical machines that have high performance yet are low in manufacturing cost.
[0230] The bonded laminated core manufacturing apparatus 400 of this embodiment is an apparatus for manufacturing a stator bonded laminated core (bonded laminated core) 21 including a plurality of electromagnetic steel plates (steel plate components) 40 punched out from a strip-shaped steel plate M. The bonded laminated core manufacturing apparatus 400 of this embodiment includes a press processing oil application section 430 that applies press processing oil b to the underside (one side) of the strip-shaped steel plate M; a press processing section 440 that applies press processing to the strip-shaped steel plate M; an adhesive application section 450 that applies anaerobic adhesive a1 and instant adhesive a2 to the underside of the strip-shaped steel plate M; and a hardening acceleration layer forming section 420 that forms a hardening acceleration layer a by applying and drying anaerobic adhesive hardening accelerator a1 and instant adhesive hardening accelerator a2 to the underside of the strip-shaped steel plate M before the press processing oil b is applied. According to the bonded laminated core manufacturing apparatus 400, it is possible to obtain the same effects as those described in the first embodiment.
[0231] In the adhesive laminated core manufacturing apparatus 400, the hardening acceleration layer forming section 420 may be provided with a nozzle 422 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in a checkered pattern as shown in FIG. Alternatively, in the above-mentioned adhesive laminated core manufacturing apparatus 400, the hardening acceleration layer forming section 420 may be provided with a pipe (hardening accelerator supply flow path) through which the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 are mixed in advance and flow, as shown in FIG. 24, and a nozzle 422 connected to this pipe. Alternatively, in the adhesive laminated core manufacturing apparatus 400, the hardening acceleration layer forming section 420 may be equipped with a nozzle 422 that applies the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2 in stripes, as shown in FIG. In any of the above cases, the nozzle 422 can uniformly distribute the anaerobic adhesive curing accelerator a1 and the instant adhesive curing accelerator a2 along the coating surface of the strip-shaped steel sheet M. Therefore, the adhesive strength along the coating surface can be made uniform.
[0232] In this embodiment, the case where the press processing oil b is applied only to the lower surface of the strip steel plate M in the processing oil application step S34 shown in Fig. 22 has been described, but the present invention is not limited to this. For example, as shown in a modified example in Fig. 26, a processing oil application step S34A in which the press processing oil b is applied to both the upper and lower surfaces of the strip steel plate M may be adopted.
[0233] In this processing oil application step S34A, press processing oil b is applied to both the upper and lower surfaces of the strip steel plate M. That is, the press processing oil b is permeated into both the upper roller 431a and the lower roller 431b, and then the upper roller 431a and the lower roller 431b are rolled while the strip steel plate M is sandwiched between them. As a result, only the press processing oil b is formed on the upper surface of the strip steel plate M. On the other hand, a hardening acceleration layer a consisting of the anaerobic adhesive hardening accelerator a1 and the instant adhesive hardening accelerator a2, and the press processing oil b covering the surface of the hardening acceleration layer a are formed on the lower surface of the strip steel plate M.
[0234] Then, in the lamination and bonding process S38A of FIG. 26, the electromagnetic steel sheet 40 whose periphery has been punched out from the strip-shaped steel sheet M by the outer periphery punching male die 461 is laminated on the upper surface of the other electromagnetic steel sheet 40 whose periphery has been punched out earlier, and is heated while being pressed. At that time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface side of the electromagnetic steel sheet 40 whose periphery has been punched out later are applied to the upper surface of the steel sheet part 40 whose periphery has been punched out earlier, pushing aside the press processing oil b applied to this upper surface. At the same time, the anaerobic adhesive c1 and the instantaneous adhesive c2 on the lower surface side of the electromagnetic steel sheet 40 whose periphery has been punched out later push aside the press processing oil b on themselves and mix with the hardening accelerator layer a on top of them. As a result, the anaerobic adhesive c1 hardens while mixing with the anaerobic adhesive hardening accelerator a1 in the hardening accelerator layer a. Similarly, the instantaneous adhesive c2 hardens instantly while mixing with the instantaneous adhesive hardening accelerator a2 in the hardening accelerator layer a. The other steps are the same as those described in FIG. 22, so the same reference numerals are used and duplicated explanations are omitted.
[0235] [Fifth embodiment] A fifth embodiment of the present invention will be described below with reference to Fig. 27. Fig. 27 is a side view of a bonded laminated core manufacturing apparatus according to this embodiment. This embodiment corresponds to a modified example of the first embodiment with only one change, so in the following description, the same components as those in the first embodiment are designated by the same reference numerals and detailed description thereof will be omitted.
[0236] The bonded laminated core manufacturing apparatus 500 of this embodiment includes a first stage A having the hardening accelerating layer forming section 120, and a second stage B having a conveying section that sends out the strip steel sheet M transferred from the first stage A toward the press working oil application section 130. In the second stage B, the conveying section, the press working oil application section 130, the press working section 140, and the adhesive application section 150 are arranged in this order along the feed direction of the strip steel sheet M.
[0237] The first stage A has a conveying section that sends out the hoop material F, a hardening accelerating layer forming section 120, and a winding section that winds up the strip steel sheet M after the hardening accelerating layer a is formed to form a hoop material F1. The hoop material F1, which is an intermediate material produced in the first stage A, is removed from the winding section of stage A and moved to another location. By performing this multiple times, multiple hoop materials F1 can be prepared and stored. The second stage B includes another conveying section and the drive section (not shown) that receive the prepared hoop material F1 and send it out toward the press oil application section 130, the press working section 140, the adhesive application section 150, and the lamination bonding section 160. The strip steel sheet M sent out from the other conveying section is sent out toward the press oil application section 130 by the drive section. In the bonded laminated core manufacturing method using the bonded laminated core manufacturing apparatus 500 described above, it is possible to obtain the same effects as those in the first embodiment. Moreover, in the second to fourth embodiments other than the first embodiment, the stage may be divided into a first stage A and a second stage B in the same manner as in the fifth embodiment.
[0238] Although the embodiments of the present invention have been described above, the technical scope of the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention. For example, the shape of the stator adhesive laminated core 21 is not limited to the shapes shown in the respective embodiments. Specifically, the outer and inner diameters, lamination thickness, number of slots, circumferential and radial dimensional ratios of the teeth portion 23, and radial dimensional ratios of the teeth portion 23 and the core back portion 22 of the stator adhesive laminated core 21 can be designed as desired according to the characteristics of the desired rotating electric machine. In addition, in the rotor 30, a pair of permanent magnets 32 form one magnetic pole, but the manufacturing target of the present invention is not limited to this form. For example, one permanent magnet 32 may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole.
[0239] In addition, although a permanent magnet field type motor has been used as an example of the rotating motor 10, the structure of the rotating motor 10 is not limited to this, as exemplified below, and various known structures not exemplified below can also be adopted. Although a permanent magnet field type motor has been described as an example of the rotating electric machine 10, the present invention is not limited to this. For example, the rotating electric machine 10 may be a reluctance type motor or an electromagnetic field type motor (wound field type motor). Although a synchronous motor has been described as an example of an AC motor, the present invention is not limited to this. For example, the rotating electric machine 10 may be an induction motor. Further, although an AC motor has been described as an example of the rotating electric machine 10, the present invention is not limited to this. For example, the rotating electric machine 10 may be a DC motor. Further, although an electric motor has been given as an example of the rotating electric machine 10, the present invention is not limited to this. For example, the rotating electric machine 10 may be a generator.
[0240] In addition, within the scope of the present invention, the components in the above-mentioned embodiments may be replaced with known components as appropriate, and the above-mentioned modified examples may be combined as appropriate. For example, in the above-mentioned first to fifth embodiments, the hardening accelerating layer a is formed on only one surface (upper or lower surface), but it may be formed on both surfaces (upper and lower surfaces) as necessary. EXAMPLES
[0241] First, compounds that are hardening accelerator components shown in Table 1 below were prepared. That is, a compound that has the effect of accelerating the hardening of anaerobic adhesives and a compound that has the effect of accelerating the hardening of instant adhesives were prepared. Then, a hardening accelerator solution containing each of these compounds was prepared. Specifically, for each of the invention examples 1 to 5 and the comparative examples 1 to 4, a hardening accelerator solution was prepared with the contents shown in Table 1. In the comparative example 2, since the hardening accelerator solution was not used, the contents of all the compounds are zero.
[0242] [Table 1]
[0243] On the other hand, multiple non-oriented electrical steel sheets were prepared, each containing, by average mass%, 3.1% Si, 0.6% Al, and 0.1% Mn, with the remainder being Fe and impurities, with an average sheet thickness of 0.30 mm, and with average surface roughnesses Ra (center line average roughness) in the L direction and C direction of 0.28 μm each. Then, except for Comparative Example 5, the above-mentioned hardening accelerator solution was applied to the surface of each of these non-oriented electrical steel sheets in an amount of 0.5 μg / m 2 to 5.0 μg / m 2 The coating was performed in advance using a coating device so that the coating amount became The applied hardening accelerator solution is then dried with hot air at 50°C to form a hardening accelerator-coated area, and press processing oil is applied to the entire surface so as to cover the upper surface of the hardening accelerator-coated area after drying.
[0244] On the other hand, in Comparative Example 1, the applied hardening accelerator solution was not dried, but was left in a liquid state, and press processing oil was applied to the entire surface so as to cover the upper surface before the hardening accelerator solution was allowed to dry naturally. In addition, in Comparative Example 5, press processing oil was applied to the entire surface of the non-oriented electrical steel sheet, and then, a coating amount of 0.5 μg / m was applied on top of the press processing oil. 2 to 5.0 μg / m 2 The hardening accelerator solution was applied by an applicator so that the hardening accelerator solution overlapped the hardening accelerator solution. That is, in Comparative Example 5, the same hardening accelerator solution as in Invention Example 1 was used, but the hardening accelerator solution was made to float on the top surface of the press processing oil. Then, before this hardening accelerator solution was naturally dried, it was used to evaluate the initial adhesive strength and the final adhesive strength, which will be described later.
[0245] The curing accelerator compounds shown in Table 1 were used as curing accelerator solutions by dissolving the compounds in various solutions, dispersing them by microparticulation, emulsifying them, or dissolving them using a chelate. As the solvent, organic solvents such as dioxane, ethanol, acetone, and cellosolve were appropriately used in addition to pure water.
[0246] The hardening accelerator solutions shown in Table 1 were applied or sprayed on the surfaces of the non-oriented electrical steel sheets in a prescribed application pattern so that they remained thinly and uniformly, and then actively dried to obtain the prescribed amounts shown in Table 1. However, for Comparative Example 1, the hardening accelerator solution was not actively dried, and each item shown in Table 2 below was evaluated while the hardening accelerator solution under the press processing oil was in a liquid state and not naturally dried. For Comparative Example 5, each item shown in Table 2 below was also evaluated before the hardening accelerator solution on the press processing oil was naturally dried.
[0247] Next, the initial adhesive strength and final adhesive strength were examined for each of the combinations of adhesive and workpiece components for hardening acceleration in Invention Examples 1 to 5 and Comparative Examples 1 to 5. The results are shown in Table 2 below.
[0248] [Table 2]
[0249] In Table 2, in evaluating the initial adhesive strength and the final adhesive strength, first, multiple 30 mm × 60 mm sample pieces were prepared from the non-oriented electrical steel sheet that had been subjected to the above-mentioned treatment (hereinafter, these are referred to as "one sample piece"). In addition, multiple 30 mm × 60 mm sample pieces were prepared from another non-oriented electrical steel sheet that had not been subjected to the above-mentioned treatment (hereinafter, these are referred to as "the other sample piece"). Then, press processing oil was applied to the entire surface of one of the test pieces, except for Comparative Example 5, which had already been applied with press processing oil, and therefore no additional application of press processing oil was performed. Then, 5 μl of the anaerobic adhesive and instant adhesive were dropped onto the edge of the surface of one of the sample pieces in an area of 30 mm × 10 mm to form a bonding surface. Immediately after dropping the anaerobic adhesive and instant adhesive, the other sample piece was placed on the bonding surface of the one of the sample pieces and bonding was started. The adhesive strength measured after 20 seconds of lamination was defined as the initial adhesive strength, and the adhesive strength measured after 24 hours of lamination was defined as the final adhesive strength.
[0250] In addition to the evaluation of the initial adhesive strength and the final adhesive strength, as shown in Table 2, the removal time when 100 sheets were stacked was also evaluated. That is, for the "100-sheet stack core removal time" shown in Table 2, first, non-oriented electrical steel sheets having the compound components shown in Table 1 were processed into multiple ring-shaped test pieces with an outer diameter of 60 mm and an inner diameter of 40 mm using a die. Then, after applying press processing oil to each surface of these test pieces, 5 μl each of the anaerobic adhesive and instant adhesive were applied to four points on each surface. Then, immediately after applying the anaerobic adhesive and instant adhesive, these test pieces were stacked on top of other test pieces.
[0251] In this lamination, the hardening accelerator solution was not dried in Comparative Example 1, and the hardening accelerator solution under the press processing oil was layered while it was still in a liquid state and not naturally dried. Similarly, in Comparative Example 5, the hardening accelerator solution on the press processing oil was layered before it was naturally dried. This lamination was repeated at a lamination speed of 20 spm, resulting in a laminated core of 100 test pieces. The shortest time from the start of measurement when lamination was completed to the end of measurement when the laminated core obtained in this manner could be removed without slippage was defined as the "100-piece laminated core removal time." In addition, when slippage occurred and lamination was not completed, or when it took more than 300 seconds to laminate, it was indicated as 300 seconds in Table 2.
[0252] Based on the above evaluation results, a score of Good for all evaluation items was given an overall rating of Good, a score that included at least one Not Good was given an overall rating of Not Good, and a score that included at least one Bad was given an overall rating of Bad. As shown in Table 2, all of Examples 1 to 5 of the invention were given an overall rating of Good, whereas Comparative Examples 1, 2, 4, and 5 were given an overall rating of Bad, and Comparative Example 3 was given an overall rating of Not Good. From the above, it was confirmed that by applying an anaerobic adhesive curing accelerator and an instant adhesive curing accelerator to one or both sides of a strip steel sheet before applying press processing oil and then drying to form a curing accelerator layer, it is possible to obtain higher productivity while ensuring sufficient adhesive strength when manufacturing an adhesive laminated core.
[0253] In a general bonding process, either an anaerobic adhesive or an instantaneous adhesive is selected according to the application, and then bonding is performed. In contrast, in the present invention, an unusual bonding process is adopted in which four substances, an anaerobic adhesive, an instantaneous adhesive, an anaerobic adhesive curing accelerator, and an instantaneous adhesive curing accelerator, are used simultaneously. As a result, high handleability immediately after bonding, that is, prevention of slippage between the electromagnetic steel sheets when the laminated core immediately after bonding is lowered to another position, is ensured by the instantaneous adhesive force exerted by the combination of the instantaneous adhesive and the instantaneous adhesive curing accelerator. In addition, high durability required when the laminated core is incorporated as a part in a motor or the like is ensured by the strong adhesive force exerted by the combination of the anaerobic adhesive and the anaerobic adhesive. In this way, high handleability and high product durability can be achieved at the same time, and the high effect is as shown in the above example. [Industrial Applicability]
[0254] According to the above-mentioned aspects of the present invention, it is possible to provide a method and an apparatus for manufacturing a bonded laminated core, which can ensure sufficient adhesive strength and achieve higher productivity when manufacturing a bonded laminated core, and thus has high industrial applicability. [Explanation of symbols]
[0255] 21 Adhesive laminated core for stator (adhesive laminated core, stator for rotating electric machine) 40 Electromagnetic steel plate (steel plate parts, first steel plate parts, second steel plate parts) 100,200,300,400,500 Bonded laminated core manufacturing equipment 120,220,320,420 Hardening accelerating layer forming part 130,230,330,430 Press processing oil application section 140,240,340,440 Press processing section 150,250,350,450 Adhesive application section 153,253,353,453 Nozzles a Hardening accelerating layer a1 Anaerobic adhesive curing accelerator a2 Instant adhesive curing accelerator b. Press processing oil c1 Anaerobic adhesive (adhesive) c2 Instant adhesive (adhesive) M Steel strip
Claims
1. A method for manufacturing an adhesive laminated core, comprising the steps of: pressing a strip of steel plate coated with press processing oil on one or both sides; applying an anaerobic adhesive and an instant adhesive to one side of the strip of steel plate to obtain a plurality of steel plate parts; and laminating and bonding the steel plate parts together, the method comprising the steps of: A hardening accelerator for anaerobic adhesives and a hardening accelerator for instant adhesives are applied to one or both sides of the strip steel plate before the press processing oil is applied, and then dried to form a hardening accelerator layer. A method for manufacturing a bonded laminated core.
2. The anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in a checkered pattern to form the curing accelerator layer.
2. The method of claim 1, wherein the adhesive laminated core is made of a sintered material.
3. The anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are mixed in advance, and the mixture is applied to one or both sides of the strip steel plate and dried to form the curing accelerator layer.
2. The method of claim 1, wherein the adhesive laminated core is made of a sintered material.
4. The anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are arranged in stripes to form the curing accelerator layer.
2. The method of claim 1, wherein the adhesive laminated core is made of a sintered material.
5. The steel plate components include a first steel plate component and a second steel plate component, A first step of preparing the first steel plate part having a first surface, the hardening promotion layer formed on the first surface, and the press processing oil disposed on the hardening promotion layer; a second step of preparing the second steel plate component having a second surface and the anaerobic adhesive and the instant adhesive disposed on the second surface; a third step of overlapping and adhering the first steel plate part and the second steel plate part so that the first surface and the second surface face each other; The method for manufacturing an adhesive laminated core according to any one of claims 1 to 4, further comprising the steps of:
6. The steel plate components include a first steel plate component and a second steel plate component, a fourth step of preparing the first steel plate component having a first surface, the hardening accelerating layer formed on the first surface, the press processing oil disposed on the hardening accelerating layer, and the anaerobic adhesive and the instant adhesive disposed on the press processing oil; A fifth step of providing the second steel plate component having a second surface; A sixth step of overlapping and bonding the first steel plate part and the second steel plate part so that the first surface and the second surface face each other; The method for manufacturing an adhesive laminated core according to any one of claims 1 to 4, further comprising the steps of:
7. The adhesive laminated core manufacturing method according to any one of claims 1 to 4, characterized in that the anaerobic adhesive curing accelerator contains an active ingredient that promotes anaerobic curing and is selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin and combinations thereof.
8. The instant adhesive curing accelerator is selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof, and contains an active ingredient that accelerates the curing of 2-cyanoacrylate adhesives. The adhesive laminated core manufacturing method according to any one of claims 1 to 4.
9. At least one of the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator is diluted with a solvent such as a ketone-based solvent, an alcohol-based solvent, an ester-based solvent, a glycol ether-based solvent, a hydrocarbon-based solvent, a halogenated hydrocarbon-based solvent, an ether-based solvent, a glycol-based solvent, or an amine-based solvent.
5. The method for producing a bonded laminated core according to claim 1, wherein the adhesive laminated core is made of a fibrous material.
10. 5. The method for manufacturing a bonded laminated core according to claim 1, wherein the bonded laminated core is a stator for a rotating electric machine.
11. An apparatus for manufacturing a bonded laminated core having a plurality of steel plate parts punched out from a strip-shaped steel plate, A press working oil application unit that applies press working oil to one side or both sides of the strip steel plate; a press working unit that applies press working to the strip steel plate; an adhesive application section that applies an anaerobic adhesive and an instant adhesive to one surface of the strip steel plate; a hardening accelerator layer forming section for forming a hardening accelerator layer by applying and drying an anaerobic adhesive hardening accelerator and an instant adhesive hardening accelerator on one or both sides of the strip steel plate before applying the press processing oil; An apparatus for manufacturing a bonded laminated core, comprising:
12. The curing accelerator layer forming unit includes a nozzle for applying the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator in a checkered pattern.
12. An apparatus for manufacturing a bonded laminated core according to claim 11.
13. The curing accelerator layer forming section includes a curing accelerator supply flow path through which the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator are mixed in advance and flow, and a nozzle communicating with the curing accelerator supply flow path.
12. An apparatus for manufacturing a bonded laminated core according to claim 11.
14. The curing accelerator layer forming unit is provided with a nozzle for applying the anaerobic adhesive curing accelerator and the instant adhesive curing accelerator in stripes.
12. An apparatus for manufacturing a bonded laminated core according to claim 11.
15. A first stage having the hardening acceleration layer forming section; A second stage having a conveying section that sends out the strip steel plate transferred from the first stage toward the press working oil application section; Equipped with The second stage is provided with the conveying section, the press working oil application section, the press working section, and the adhesive application section, which are arranged in this order along the feed direction of the strip steel plate.
15. The apparatus for manufacturing a bonded laminated core according to claim 11,
16. The adhesive laminated core manufacturing apparatus according to any one of claims 11 to 14, characterized in that the anaerobic adhesive curing accelerator contains an active ingredient that promotes anaerobic curing selected from titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, vanadium, molybdenum, ruthenium, saccharin, and combinations thereof.
17. The instant adhesive curing accelerator is selected from organic amines such as dimethylaniline, diethylamine, o-phenylenediamine, dimethyl paratoluidine, diethyl paratoluidine, and N,N-diethylaniline, acid amides such as trichloroacetamide, organic imides such as succinimide, quaternary ammonium salts such as tetramethylammonium chloride and benzyltrimethylammonium chloride, and combinations thereof, and contains an active ingredient that promotes the curing of 2-cyanoacrylate adhesives. The adhesive laminated core manufacturing device according to any one of claims 11 to 14.
18. 15. The bonded laminated core manufacturing apparatus according to claim 11, wherein the bonded laminated core is a stator for a rotating electric machine.
Citation Information
Patent Citations
Conditioning unit of vacuum switch tube
JP1986064029A
Electromagnetic steel sheet laminated core which has good thermal conductivity, and method of manufacturing the same
JP2011023523A
Manufacturing method and manufacturing apparatus of laminate steel sheet
JP2018038119A
Laminated iron core manufacturing apparatus and laminated iron core manufacturing method
JP2019212756A
Manufacturing method for laminated metal sheets
JP4648765B2