Functionalized hydrogenated interpolymers containing non-hydrogenated polymer segments
Functionalized polymers with hydrogenated and non-hydrogenated segments address compatibility and cure rate issues in H-SBR blends, improving tire performance by enhancing filler interaction and mechanical properties.
Patent Information
- Application Number
- JP2023539090
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-31
- Filing Date
- 2021-12-29
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-12-29
AI Technical Summary
Hydrogenated styrene-butadiene rubber (H-SBR) compositions face limitations in compatibility and cure rates when blended with other rubbers, and high hydrogenation levels reduce crosslinking sites, affecting miscibility and mechanical properties.
Development of functionalized polymers comprising a hydrogenated interpolymer portion, a non-hydrogenated polymer portion, and a functional coupling agent covalently bonded to both, enhancing interaction with silica fillers.
Improves miscibility with bulk rubbers and maintains or exceeds mechanical properties, reducing rolling resistance and enhancing tire performance.
Smart Images

Figure 0007580611000001 
Figure 0007580611000002 
Figure 0007580611000003
Abstract
Description
[Technical Field]
[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS) This international application claims the benefit of U.S. Provisional Patent Application No. 63 / 132,592, filed December 31, 2020, which is incorporated herein by reference in its entirety. [Background technology]
[0002] Rubber products such as tire components (e.g., treads, sidewalls, etc.) are often made from elastomeric compositions that include one or more reinforcing materials, such as particulate carbon black and silica; see, e.g., The Vanderbilt Rubber Handbook, 13th ed. (1990), pp. 603-04. Some of the most commonly used synthetic elastomeric materials used in the manufacture of vulcanizates, such as tire components, include high cis polybutadiene (BR), often produced by a process that uses a catalyst, and substantially random styrene / butadiene interpolymers (SBR), often produced by a process that uses an anionic initiator.
[0003] While good traction and wear resistance are primary considerations for tire treads, automotive fuel efficiency considerations dictate minimal rolling resistance, which correlates with reduced hysteresis and heat buildup during tire operation. To a large extent, these considerations are in conflict and somewhat at odds: treads made from compositions designed to provide good road traction typically exhibit increased rolling resistance, and vice versa.
[0004] Fillers, polymers, and additives are typically selected to provide an acceptable compromise or balance of desired properties. Ensuring that the reinforcing filler is well dispersed throughout the elastomeric material acts to enhance processability and improve physical properties. Filler particle dispersion can be improved by increasing their interaction with the elastomer and / or decreasing their interaction with each other. Examples of this type of approach include high-temperature mixing in the presence of selective reactivity promoters, surface oxidation of the compounded material, and surface grafting.
[0005] The portion of the polymer chain from the last crosslink site to the end cannot participate in an efficient elastic recovery process because it is not connected to the polymer network. As a result, energy transferred to this portion of the polymer (and vulcanizates incorporating such polymers) is lost as heat. Ensuring that these ends are bonded to or otherwise interact sufficiently with the reinforcing particulate filler is important for many vulcanizate physical properties, such as reduced hysteresis.
[0006] Chemically modifying a polymer, typically at its terminal, is one of the most effective ways to increase the interaction between fillers and polymers.End-chemical modification is often carried out by reacting a living polymer with a functional terminating agent, see, for example, U.S. Patent Nos. 3,109,871, 4,647,625, 4,677,153, 5,109,907, 6,977,281, etc., and the references cited therein and subsequent publications citing these patents.Post-polymerization end-functionalization, which can be carried out on anionically initiated polymers, is often not possible on coordination catalyst polymers, and vice versa, to a lesser extent.
[0007] Interest in hydrogenated polymers as components in rubber compositions continues to grow. These include hydrogenated BR (H-BR) and hydrogenated SBR (H-SBR). The latter typically exhibit improved tensile properties compared to otherwise equivalent SBR, especially when the degree of hydrogenation is greater than about 90%. (However, the degree of hydrogenation cannot be 100%, since some residual unsaturation must remain to participate in the crosslinking reaction (vulcanization).) Summary of the Invention [Problem to be solved by the invention]
[0008] However, it has become clear that there are limitations to the use of H-SBR. At hydrogenation levels above approximately 90%, few potential crosslinking sites remain, and H-SBR may exhibit a different cure rate than the bulk rubbers (e.g., SBR, BR, NR, etc.) with which it is sometimes blended. Hydrogenation also affects the polymer's solubility parameter, which can lead to incompatibility with other unsaturated polymers in a given rubber composition.
[0009] What remains desirable is an H-SBR that, when blended with one or more bulk rubbers, exhibits satisfactory compatibility and acceptable equivalent cure rates. Preferably, compositions containing the H-SBR can impart equivalent or superior tensile properties to vulcanizates compared to vulcanizates made from otherwise equivalent compositions that do not contain the H-SBR.
[0010] Provided herein is a functionalized polymer comprising a hydrogenated interpolymer segment, a non-hydrogenated polymer segment, and a functional coupling agent radical covalently attached to each of the segments, wherein the functional group resulting from the coupling agent attachment exhibits silica interactivity.
[0011] The interpolymer may advantageously comprise vinyl aromatic mers and conjugated diene mers, at least a portion of which has been hydrogenated, i.e., the polymer has been subjected to conditions under which H2 can add to some of its double bonds, resulting in the loss of some of the residual unsaturation resulting from the incorporation of such mers. Compared to the total number of conjugated diene mers incorporated into the interpolymer, the hydrogenated conjugated diene mers, i.e., no longer containing ethylenic unsaturation, typically constitute at least 50 mol %, preferably significantly higher, e.g., at least about 80 mol %.
[0012] In some embodiments, the interpolymer may contain 10 to 45 mole percent vinyl aromatic mers. In these and other embodiments, the interpolymer may incorporate a significant percentage of its conjugated diene mers in the 1,2-vinyl configuration, e.g., at least 30 mole percent.
[0013] The unhydrogenated polymeric portion of the polymer comprises, and in some embodiments consists of, conjugated diene mers. In embodiments where the unhydrogenated polymeric portion consists of conjugated diene mers, that portion has a number average molecular weight (M) of up to about 50 kg / mol, often from 10 to 40 kg / mol. n ).
[0014] The radicals covalently bonded to both polymer moieties may be the residue of a coupling agent, which comprises a functional group reactive with carbanions, comprises a functional group capable of interacting with silica, and does not react or decompose when exposed to hydrogenation conditions. In some embodiments, the functional coupling agent may comprise an epoxy group and a siloxy group.
[0015] Also provided is a method for producing the aforementioned functionalized polymer. An interpolymer containing a vinyl aromatic mer, a conjugated diene mer, and terminal functional groups derived from the incorporated coupling agent is subjected to conditions that hydrogenate a portion, preferably at least half, of the conjugated diene mer. The interpolymer is then infused with or incorporated into a carbanionic polymer containing the conjugated diene mer, and the carbanionic polymer reacts with the radicals of the coupling agent that were previously covalently bonded only to the interpolymer. Between 0.5 and 10 equivalents of the second type of polymer can be used per equivalent of interpolymer. This results in a polymer containing portions derived from both polymers.
[0016] Regardless of how characterized, the polymer is capable of interacting with the particulate filler, particularly silica. Compositions comprising the particulate filler and the functionalized polymer are also provided, as are methods of providing and using such compositions.
[0017] The composition can include other elastomers. Advantageously, the functionalized polymer can exhibit improved miscibility with certain bulk rubbers commonly used in rubber compositions, particularly BR, as well as desirable tensile properties in vulcanizates obtained therefrom.
[0018] Other aspects of the present invention will become apparent to those skilled in the art from the following detailed description. To aid in understanding that description, certain definitions are provided below, which are intended to apply throughout unless the surrounding text expressly indicates a contrary intention. "Polymer" means the polymerization product of one or more monomers, and is inclusive of homopolymers, copolymers, terpolymers, tetrapolymers, and the like. "Mer" or "mer unit" means a portion of a polymer derived from a single reactant molecule (e.g., an ethylene mer has the general formula -CH2CH2-). "Copolymer" means a polymer containing mer units derived from two reactants, typically monomers, and includes random copolymers, block copolymers, segmented copolymers, graft copolymers, and the like. "Interpolymer" means a polymer that includes mer units derived from at least two reactants, typically monomers, and is inclusive of copolymers, terpolymers, tetrapolymers, and the like. "Random interpolymer" means an interpolymer having mer units derived from each type of constituent monomer incorporated essentially non-repeatedly, and substantially free of blocks, i.e., segments of three or more of the same mer. "Gum Mooney viscosity" is the Mooney viscosity of the uncured polymer before the addition of any fillers. "Substituted" means containing heteroatoms or functional groups (eg, hydrocarbyl groups) that do not interfere with the intended purpose of the group. "Direct bond" means a covalent bond without any intervening atoms or groups. "Polyene" means a molecule having at least two double bonds in its longest segment or chain, and specifically includes dienes, trienes, and the like. "Polydiene" means a polymer containing one or more diene mer units. "Microstructure" refers to the individual properties of how polyenes are incorporated into polymer chains, or the sum of all such properties, including 1,4-content, 1,2-(vinyl) content, cis content, and trans content. "phr" means parts per hundred weight of rubber (pbw). "Radical" or "residue" means the portion of a molecule that remains after it reacts with another molecule, regardless of whether atoms are gained or lost as a result of the reaction. "Terminal" means the end of a polymer chain. "Terminal moiety" means a group or functional group located at a terminal end; By "reactive polymer" is meant a polymer having at least one site that readily reacts with other molecules due to the presence of an active end, and the term includes, among others, carbanionic polymers.
[0019] Throughout this specification, all values given in terms of percentages are percentages by weight (w / w) unless the surrounding text expressly indicates a contrary intention.
[0020] Unless otherwise indicated in the surrounding text, all numbers expressing quantities of ingredients, process conditions (e.g., time and temperature), and the like, are to be understood in all instances as being modified by the term "about." The recited numerical limitations include an appropriate degree of precision based on the number of significant digits used; for example, "up to 5.0" can be construed as setting an absolute upper limit that is lower than "up to 5."
[0021] All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety, as if fully set forth herein. DETAILED DESCRIPTION OF THE INVENTION
[0022] The interpolymer portion of the polymer is described first, followed by a description of the second polymer portion, and then a description of the coupling of the two polymer portions to form the polymer.
[0023] Interpolymers contain unsaturation resulting from the incorporation of polyenes, particularly dienes and trienes (e.g., myrcene), C4 to C6, such as, but not limited to, 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, and 1,3-hexadiene. 12 Conjugated dienes are preferred.
[0024] Polyenes can be incorporated into polymer chains in several ways. In some embodiments, polymer chains having an overall 1,2-(vinyl) microstructure of about 10 to about 80%, or about 25 to about 65%, expressed as a numerical percentage based on the total polyene content, may be desirable. Substantially linear polymers have an overall 1,2-microstructure of about 50% or less, preferably about 45% or less, more preferably about 40% or less, even more preferably about 35% or less, and most preferably about 30% or less, based on the total polyene content. For certain end uses, it may be desirable to maintain an even lower 1,2-linkage content, e.g., less than about 7%, less than 5%, less than 2%, or less than 1%. Controlling the initial vinyl content can maintain the amorphous nature of the interpolymer, thereby reducing crystallinity, which can degrade the performance of vulcanizates made from rubber compounds containing the polymer. (Vinyl content and other microstructural details can be determined, for example, by proton NMR.)
[0025] The pendant aromatic groups are vinyl aromatic mer units, particularly C-C such as styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, and vinylnaphthalene. 20 When used with one or more polyenes, the mer units having pendant aromaticity can constitute up to about 60%, from about 1 to about 50%, from about 10 to about 45%, from about 20 to about 35%, or from about 25 to about 30% of the total number of mer units in the polymer chain.
[0026] The various types of mers in the interpolymer are preferably incorporated randomly, meaning that each type of mer does not form blocks but instead is incorporated substantially non-repeatedly. Random microstructure can provide certain benefits in some end uses, such as, for example, rubber compositions used in making tire treads.
[0027] Exemplary interpolymers include those having one or more polyenes and mers derived from styrene, such as poly(styrene-co-butadiene), also known as SBR.
[0028] Such interpolymers, particularly those made according to anionic techniques (described below), generally have M up to about 500,000 daltons. n In certain embodiments, M n Advantageously, M may be at least about 10,000 daltons, or may range from about 50,000 to about 250,000 daltons, or from about 75,000 to about 150,000 daltons. Preferred ranges are from about 75,000 to about 225,000 daltons, and especially from about 100,000 to about 200,000 daltons. In many cases, M n is such that the quenched sample exhibits a gum Mooney viscosity (ML4 / 100°C) of from about 2 to about 150, more typically from about 2.5 to about 125, even more typically from about 5 to about 100, and most typically from about 10 to about 75.
[0029] Interpolymers can be produced by any of a variety of polymerization techniques. Solution polymerization generally allows for greater control over properties such as randomness and microstructure, although other techniques, such as emulsion polymerization, can also be used. Solution polymerization has been practiced since roughly the mid-20th century, so its general aspects are known to those skilled in the art. Useful polymerization solvents include various C5-C 12 Included are cyclic and acyclic alkanes and their alkylated derivatives, certain liquid aromatic compounds, and mixtures thereof; one skilled in the art will recognize other useful solvent options and combinations.
[0030] Anionic (living) polymerization requires an initiator rather than a catalyst. Exemplary initiators include organolithium compounds, particularly alkyllithium compounds. Examples of organolithium initiators include N-lithio-hexamethyleneimine; n-butyllithium; tributyltinlithium; dialkylaminolithium compounds such as dimethylaminolithium, diethylaminolithium, dipropylaminolithium, and dibutylaminolithium; dialkylaminoalkyllithium compounds such as diethylaminopropyllithium; and C1-C 12 Preferably, trialkylstannyllithium compounds having a C1-C4 alkyl group are mentioned.
[0031] Multifunctional initiators, i.e., initiators capable of forming polymers with two or more living ends, can also be used. Examples of multifunctional initiators include, but are not limited to, 1,4-dilithiobutane, 1,10-dilithiodecane, 1,20-dilithioeicosane, 1,4-dilithiobenzene, 1,4-dilithionaphthalene, 1,10-dilithioanthracene, 1,2-dilithio-1,2-diphenylethane, 1,3,5-tirithiopentane, 1,5,15-tirithioeicosane, 1,3,5-tirithiocyclohexane, 1,3,5,8-tetralithiodecane, 1,5,10,20-tetralithioeicosane, 1,2,4,6-tetralithiocyclohexane, and 4,4'-dilithiobiphenyl.
[0032] In addition to organolithium initiators, so-called functionalized initiators may also be useful. These are incorporated into the polymer chain, thus providing a functional group at the initiating end of the chain. Examples of such materials include lithiated arylthioacetals (see, e.g., U.S. Pat. No. 7,153,919), and reaction products of organolithium compounds with N-containing organic compounds, such as substituted aldimines, ketimines, and secondary amines, optionally pre-reacted with compounds such as diisopropenylbenzene (see, e.g., U.S. Pat. Nos. 5,153,159 and 5,567,815). The use of N-atom-containing initiators, such as lithiated HMI, can further enhance the interaction between the polymer chain and the carbon black particles. See, e.g., U.S. Pat. Nos. 8,227,562, 8,871,871, 9,365,660, 10,277,425, and 10,815,328.
[0033] In solution polymerizations, both randomization and vinyl content (i.e., 1,2-microstructure) can be increased by including a modifier, usually a polar compound, among the polymerization ingredients. Up to 90 or more equivalents of modifier per equivalent of initiator can be used, the amount depending, for example, on the desired vinyl content, the level of non-polyene monomer used, the reaction temperature, and the nature of the specific modifier used. Compounds useful as modifiers include organic compounds containing heteroatoms (e.g., O or N) with non-bonding electron pairs. Examples include dialkyl ethers of mono- and oligo-alkylene glycols; crown ethers; tertiary amines such as tetramethylethylenediamine; THF; THF oligomers; and linear and cyclic oligomeric oxolanyl alkanes such as 2,2-bis(2'-tetrahydrofuryl)propane, dipiperidylethane, hexamethylphosphoramide, N,N'-dimethylpiperazine, diazabicyclooctane, diethyl ether, and tributylamine (see, e.g., U.S. Pat. No. 4,429,091).
[0034] Those skilled in the art will understand the conditions typically used in anionically initiated polymerizations, but for convenience a representative description is provided. The following is based on a batch process, but can be extended to semi-batch, continuous, or other techniques.
[0035] The blend of monomers and solvent can be placed in a suitable reaction vessel, followed by the addition of modifiers (if used) and initiator, which are often added as part of a solution or blend, or the monomers and modifiers can be added to the initiator. The reactants can be heated (typically up to about 150° C.) and stirred.
[0036] After introduction of the initiator compound, polymerization is allowed to proceed under anhydrous, oxygen-free conditions for a time sufficient to form the desired polymer, usually from about 0.01 hours to about 100 hours, more usually from about 0.08 hours to about 48 hours, and typically from about 0.15 hours to about 2 hours.
[0037] After the desired degree of conversion is reached, the heat source (if used) can be removed and the reaction mixture can be transferred to a post-polymerization vessel for functionalization if the reaction vessel is reserved for polymerization only.
[0038] Interpolymers prepared according to anionic techniques have an active end (or at least two active ends if a multifunctional initiator is used). If a polymerization technique is used that does not provide at least one active end, it is necessary to render at least a portion of the polymer chain reactive so that functionalization can occur.
[0039] Functionalization of the active end can provide a terminal moiety, preferably a terminal moiety directly attached to the interpolymer. The provided terminal moiety must be reactive to (or contain a functional group reactive to) carbanions and must be capable of interacting with silica (or contain a functional group capable of interacting with silica). Preferably, the terminal moiety also does not react or decompose when the interpolymer to which it is attached is subjected to hydrogenation conditions.
[0040] Using the terminally activated interpolymer as an exemplary material, functionalization can be easily achieved by reaction with a compound capable of providing the aforementioned terminal moieties. A non-limiting example of such a compound is a compound containing both an epoxy group and a siloxy group. In some embodiments, the siloxy group can be a trialkoxysilane in which the alkyl portion contains 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms. Trimethoxysilane is preferred. An exemplary functionalizing compound is 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (ECETMOS).
[0041] If desired, the cement containing the functionalized interpolymer can be quenched in a suitable solvent containing active hydrogen atoms. Furthermore, if the polymer cement itself is not hydrogenated, it can be processed (dried, sheeted, etc.) and stored.
[0042] The functionalized interpolymer is mixed with a hydrogenation catalyst, often based on Ni (e.g., nickel octoate) alone or in combination with an Al-containing compound (e.g., an organoaluminum compound such as trialkylaluminum), in a suitable organic liquid and / or with additional organic liquid in the presence of a H stream. The solvent can include one or more of the aforementioned organic liquids. When the catalyst contains both Ni and Al, the Al / Ni molar ratio can be 1:1 to 5:1, preferably 2:1 to 4:1, and most preferably 3:1±20% (i.e., 2.4:1 to 3.6:1).
[0043] Pressurized H2 can be introduced at about 0.1 to about 10 MPa (1 to 100 atmospheres), generally about 0.25 to about 7.5 MPa (2.5 to 74 atmospheres), typically about 0.5 to about 5 MPa (5 to 50 atmospheres).
[0044] Degree of hydrogenation refers to the mole percent of polyene double bonds lost after the interpolymer is subjected to a hydrogenation process such as those described above; TThe hydrogenation degree can range from about 50% to nearly 100%, as measured by H NMR spectroscopy. A degree of hydrogenation of at least 80%, 84%, 88%, 92%, or 96% may be desirable in view of certain mechanical properties of vulcanizates made from rubber compounds containing the interpolymer.
[0045] Hydrogenation reduces the number of double bonds in both the main chain and the side chains of each polymer. The degree of hydrogenation of each type of unsaturation tends to be roughly equal.
[0046] If desired, the cement containing the hydrogenated functionalized interpolymer can be processed (dried, sheeted, etc.) and stored if the interpolymer cement itself will not be used in a reaction with a second type of polymer.
[0047] The second type of polymer has terminal functional groups and is therefore provided by anionically initiated polymerization, the general conditions of which are described above.
[0048] The second type of polymer contains unsaturation resulting from the incorporation of polyenes, particularly dienes and trienes (e.g., myrcene). 12 Conjugated dienes, such as 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, and 1,3-hexadiene, are preferred. Other types of mers that can be incorporated include monoolefin monomers, such as those derived from the above vinyl aromatic compounds and α-olefins (e.g., ethylene and propylene), as well as mixtures of the foregoing. The amount of monoolefin mers is generally kept below 20%, usually below 15%, typically below 10%, and most typically below 5%. Preferred embodiments are those in which the polymer comprises only polyenes, particularly conjugated diene mers, with homopolymers being particularly preferred.
[0049] The second polymer is typically synthesized to have a molecular weight substantially lower than that of the (hydrogenated) interpolymer.n Typically, the M is less than 75,000 daltons, typically about 5000 to about 50,000 daltons. n is about 10,000 to about 20,000 daltons, particularly about 12,000 to about 15,000 daltons, and M n is about 30,000 to about 40,000 daltons.
[0050] The microstructure of the second polymer can vary widely without significantly adversely affecting the process.
[0051] The second polymer has not been hydrogenated, functionalized, or (intentionally) quenched, so that the terminal activity is retained.
[0052] Once the two types of polymers are introduced, the latter reacts with the terminal functional groups of the former. This reaction can proceed at temperatures ranging from about 0°C to about 150°C, generally from about 10°C to about 100°C, and typically from about 20°C to about 80°C, for 10 to 600 minutes, typically 30 to 300 minutes. While catalysis is not required, maintaining oxygen-free, anhydrous conditions is preferred to maintain activity of the carbanionic polymer chains.
[0053] As will be appreciated by those skilled in the art, the amount of chains and the ratio of the two types of polymers can be used to control the coupling reaction. Assuming the interpolymer is prepared using an anionic (e.g., n-BuLi) initiator and all or nearly all of its chains are functionalized, the ratio of Li used in the two polymerizations can be used as a proxy for adjusting the amounts of the two types of polymers involved in the coupling reaction. The ratio of the second polymer to the first polymer can range from 1:2 to 10:1, with ratios of 1:1 to 5:1, or even about 3:1, being more common.
[0054] Upon completion of this coupling reaction, a polymer is obtained, which thus contains a hydrogenated interpolymer portion, a non-hydrogenated polymer portion, and a functional group covalently bonded between the two polymer portions, the functional group being interactive with the silica filler.
[0055] The polymer typically has an M of about 250,000 to about 600,000 daltons, often about 350,000 to about 550,000 daltons. n It has.
[0056] The majority of the conjugated diene mers throughout the polymer are preferably incorporated in the 1,2- (ie, vinyl) configuration.
[0057] The polymer can be used as a component in vulcanizable compositions containing a wide variety of other polymers, including, but not limited to, natural or synthetic polyisoprene and homopolymers and interpolymers of polyenes, particularly dienes, most particularly conjugated dienes. It has been found to be particularly useful when used with BR having a 1,2-vinyl content of 3% or less and a cis-1,4 content of at least 96%. (In this paragraph, all percentages are molar, and such percentages are measured by spectroscopic techniques.) When used with one or more polymers of this type, the polymer can be used in a ratio of 2:3 to 3:2, preferably 3:4 to 4:3, more preferably 4:5 to 5:4, and most preferably 1:1 to 9:8.
[0058] Any other polymers can be used in suitable amounts that do not interfere with the ability of the resulting rubber composition to provide a vulcanizate with the desired physical properties. Non-limiting examples include butyl rubber, neoprene, EPR, acrylonitrile / butadiene rubber, silicone rubber, fluoroelastomers, ethylene / acrylic rubber, EVA, epichlorohydrin rubber, chlorinated polyethylene rubber, chlorosulfonated polyethylene rubber, hydrogenated nitrile rubber, tetrafluoroethylene / propylene rubber, and the like.
[0059] Polymers of the types described above can be compounded with, among other things, reinforcing fillers. Elastomeric compounds are typically filled to a volume fraction (often about 25%) of the total volume of added fillers divided by the total volume of the elastomer stock, with typical (combined) amounts of reinforcing filler ranging from about 30 to about 100 phr, the upper end of this range being determined primarily by how effectively the processing equipment can handle the viscosity increase that occurs when such fillers are used.
[0060] Useful fillers include various forms of carbon black, including, but not limited to, furnace black, channel black, and lamp black. More specifically, examples of carbon black include ultra-abrasion resistant furnace black, high-abrasion resistant furnace black, high-speed extrudable furnace black, fine furnace black, medium-grade ultra-abrasion resistant furnace black, semi-reinforced furnace black, medium-grade processable channel black, difficult-to-process channel black, conductive channel black, and acetylene black, and mixtures of two or more of these may also be used. At least 20 m 2 / g, preferably at least about 35m 2 Carbon blacks having a surface area (EMSA) of 1000 psi / g are preferred, see ASTM D-1765 for methods of measuring carbon black surface area. The carbon black may be in pelletized or non-pelletized floc form, although non-pelletized carbon black may be preferred for use in certain mixers.
[0061] The amount of carbon black can be up to about 50 phr, with 5 to 40 phr being typical.
[0062] Amorphous silica (SiO2) can also be utilized as a filler. Silica is generally classified as a wet-process hydrated silica because it is produced by a chemical reaction in water, from which it precipitates as ultrafine spherical particles. These primary particles strongly associate into aggregates, which then more weakly join together into clumps. "Highly dispersible silica" is any silica that has a very high ability to disaggregate and disperse in an elastomeric matrix, as can be observed by thin-section microscopy.
[0063] Surface area is a reliable indicator of the reinforcing properties of various silicas, and the Brunauer, Emmett, and Teller ("BET") method (described in J. Am. Chem. Soc., vol. 60, p. 309 et seq.) is an accepted method for measuring surface area. The BET surface area of silica is approximately 450 m 2 / g or less, usually about 32 to about 400m 2 / g, or about 100 to about 250 m 2 / g, or about 150 to about 220 m 2 / g.
[0064] The pH of the silica filler (if used) is generally about 5 to about 7 or slightly higher, preferably about 5.5 to about 6.8.
[0065] When silica is used, a coupling agent such as a silane is often added to ensure good mixing and interaction with the elastomer. Typically, the amount of silane added ranges from about 4 to 20 weight percent, based on the weight of silica filler present in the elastomer compound. The coupling agent can have the general formula α-TG, where A represents a functional group capable of physically and / or chemically bonding with groups on the surface of the silica filler (e.g., surface silanol groups). T represents a hydrocarbon group bond, and G represents a functional group capable of bonding with the elastomer (e.g., via a sulfur-containing bond). Such coupling agents include organosilanes, particularly polysulfide alkoxysilanes (see, for example, U.S. Pat. Nos. 3,873,489, 3,978,103, 3,997,581, 4,002,594, 5,580,919, 5,583,245, 5,663,396, 5,684,171, 5,684,172, and 5,696,197), or polyorganosiloxanes having the G and A functional groups described above. The addition of processing aids can reduce the amount of silane used; see, for example, U.S. Pat. No. 6,525,118 for a description of fatty acid esters of sugars used as processing aids. Additional fillers useful as processing aids include, but are not limited to, mineral fillers such as clay (hydrous aluminum silicate), talc (hydrous magnesium silicate), and mica, as well as non-mineral fillers such as urea and Na2SO4. Exemplary mica contains primarily alumina, silica, and potash, although other variations can also be used. Additional fillers can be used in amounts up to about 40 phr, typically up to about 20 phr.
[0066] Silica is generally used in amounts up to about 100 phr, typically from about 5 to about 80 phr. If carbon black is also present, the amount of silica can be reduced to as little as 1 phr; this reduces the amount of processing aid and silane (if present) that can be used.
[0067] Relatively high interfacial free energy, i.e., the surface free energy value in water (γp1 ) can be used in conjunction with or in place of carbon black and / or silica. The term "relatively high" refers to, for example, at least about 300, at least about 400, at least about 500, at least about 600, at least about 700, at least about 750, at least about 1000, at least about 1500, and at least about 2000 mJ / m 2 For example, the γ of amorphous silica is greater than the value at the water-air interface, preferably several times (e.g., at least two times, at least three times, or at least four times) that value. p1 Interfacial free energy can be defined or characterized in various ways, such as by being at least several times (e.g., at least 2 times, at least 3 times, at least 4 times, at least 5 times, at least 6 times, at least 7 times, at least 8 times, at least 9 times, or at least 10 times) higher than the value of
[0001] . Non-limiting examples of naturally occurring materials with relatively high interfacial free energy include F-apatite, goethite, hematite, zincite, tenorite, gibbsite, quartz, kaolinite, all forms of pyrite, and the like. Certain synthetic complex oxides can also exhibit this type of high interfacial free energy.
[0068] The foregoing types of materials are typically denser than carbon black or amorphous silica, and therefore, replacing a particular mass of carbon black or silica with an equal mass of unconventional filler typically results in a much smaller total volume of filler being present in a given compound. Thus, the replacement is typically made on an equal volume basis rather than an equal weight basis.
[0069] Other conventional rubber additives may also be added, including, for example, processing oils, plasticizers, antidegradants such as antioxidants and antiozonants, curatives, and the like.
[0070] All ingredients can be mixed in standard equipment such as a Banbury or Brabender mixer. Typically, mixing is done in two or more stages. During the first stage (often called the masterbatch stage), mixing typically begins at a temperature of about 120 to about 130°C and increases until a so-called letdown temperature (typically about 165°C) is reached.
[0071] When the formulation contains fillers other than or in addition to carbon black, a separate regrind stage is often used to add the silane component separately. This stage is often carried out at temperatures similar to those used in the masterbatch stage, but often slightly lower, i.e., from about 90°C to a dump temperature of about 150°C.
[0072] Reinforced rubber compounds are conventionally cured with about 0.2 to about 5 phr of one or more known vulcanizing agents, such as sulfur- or peroxide-based cure systems. For a general disclosure of suitable vulcanizing agents, the interested reader is referred to overviews such as those provided in Kirk-Othmer, Encyclopedia of Chem. Tech., 3rd ed., (Wiley Interscience, New York, 1982), vol. 20, pp. 365-468. Vulcanizing agents, accelerators, and the like are added in the final mixing stage. To reduce the possibility of undesirable scorching and / or premature initiation of vulcanization, this mixing step is often carried out at lower temperatures, e.g., starting at about 60°C to about 65°C and not exceeding about 105°C to about 110°C.
[0073] The compounded mixture is then processed (e.g., milled) into sheets and molded into any of the various components, and then vulcanized, which typically occurs at a temperature about 5°C to about 15°C higher than the highest temperature used during the mixing stage, most commonly about 170°C.
[0074] As is apparent from the foregoing, it is contemplated that the general preferences regarding features, ranges, numerical limitations, and embodiments may be combined, to the extent feasible, with other such generally preferred features, ranges, and numerical limitations, unless they interfere or are incompatible. To assist in envisioning some of such combinations, the following numbered embodiments are provided.
[0075] Process Embodiments P1. A process for providing a functionalized polymer comprising a hydrogenated interpolymer portion and a non-hydrogenated polymer portion, comprising: a) providing a terminally functionalized interpolymer comprising a vinyl aromatic mer, a conjugated diene mer, a hydride of the conjugated diene mer, and a terminal functional group comprising a functional group reactive to carbanions and capable of interacting with silica; b) incorporating the interpolymer into a carbanionic polymer comprising a conjugated diene mer, or incorporating a carbanionic polymer into the interpolymer; c) reacting the carbanionic polymer with the terminal functional group to provide the functionalized macromolecule. P2. The process of P1, wherein the interpolymer is provided by exposing an end-functionalized polymer comprising a vinyl aromatic mer and a conjugated diene mer to hydrogenation conditions to hydrogenate at least 50 mole percent of the conjugated diene mer. P3. The process of P2, wherein the end-functionalized polymer is provided by reacting a carbanionic interpolymer comprising a vinyl aromatic mer and a conjugated diene mer with a compound capable of coupling polymer chains, wherein the compound comprises a silica-interactive functional group and is non-reactive and resistant to decomposition when exposed to hydrogenation conditions. P4. The process of P3, wherein the compound comprises an epoxy group and a siloxy group. P5. The process of P4, wherein the compound is 2-(3,4-epoxycyclohexyl)ethyltrialkoxysilane. P6. The process of P5, wherein the alkoxy moiety of said compound is a methoxy moiety. P7. The process of P1 wherein at least 80 mole percent of the conjugated diene mers in said interpolymer are hydrogenated. P8. The process of P7, wherein at least 90 mole percent of the conjugated diene mers in said interpolymer are hydrogenated. P9. The process of any one of P1-P8, wherein the interpolymer comprises 10-45 mole % styrene mers. P10. The process of any one of P1-P9, wherein the majority of the conjugated diene mers are incorporated in a 1,2-vinyl configuration. P11. The process of any one of P1-P10, wherein the carbanionic polymer comprises a conjugated diene mer. P12. The process of any one of P1-P11, wherein 0.5 to 10 equivalents of the carbanionic polymer are reacted per equivalent of the interpolymer. P13. The process of any one of P1 to P12, wherein the carbanionic polymer has a number average molecular weight of 5 to 50 kg / mol. P14. The process of P13, wherein the carbanionic polymer has a number average molecular weight of 10 to 20 kg / mol. P15. The process of P13, wherein the carbanionic polymer has a number average molecular weight of 30 to 40 kg / mol.
[0076] Polymeric Embodiments M1. A functionalized polymer comprising a hydrogenated interpolymer portion, a non-hydrogenated polymer portion, and a functional group covalently bonded to each of said portions, said functional group exhibiting silica interactivity. M2. A functionalized polymer according to M1, wherein the functional group is a radical of a compound containing an epoxy group and a siloxy group. M3. The functionalized polymer according to M1, wherein said compound is 2-(3,4-epoxy-cyclohexyl)ethylytrialkoxysilane. M4. A functionalized polymer according to M1, wherein the alkoxy moieties of said compound are methoxy moieties. M5. The functionalized polymer of any one of M1-M4, wherein the interpolymer comprises a vinyl aromatic mer and a conjugated diene mer. M6. The functionalized polymer according to M5, wherein said interpolymer consists of a vinyl aromatic mer and a conjugated diene mer. M7. The functionalized polymer according to M5 or M6, wherein at least 80 mole percent of the conjugated diene mers in said interpolymer are hydrogenated. M8. The functionalized polymer according to M7, wherein at least 90 mole percent of said conjugated diene mers in said interpolymer are hydrogenated. M9. The functionalized polymer of any one of M5-M8, wherein the interpolymer comprises 10-45 mole % styrene. M10. The functionalized polymer of any one of M5-M9, wherein the majority of the conjugated diene mers are incorporated in a 1,2-vinyl configuration. M11. The functionalized polymer of any one of M1-M10, wherein the unhydrogenated polymer portion comprises a conjugated diene mer. M12. A functionalized polymer according to M11, wherein said unhydrogenated polymeric portion comprises a conjugated diene mer. M13. The functionalized polymer of any one of M1-M12, wherein said polymer comprises a plurality of unhydrogenated polymeric segments. M14. The functionalized polymer according to any one of M1 to M12, wherein the unhydrogenated polymer portion is obtained from a conjugated diene homopolymer having a number average molecular weight of 5 to 50 kg / mol. M15. The functionalized polymer according to M14, wherein the conjugated diene homopolymer has a number average molecular weight of 10 to 20 kg / mol or 30 to 40 kg / mol.
[0077] Rubber Compound Embodiments R1. A composition comprising the functionalized polymer of any one of M1-M15 and at least one bulk rubber. R2. The composition of R1, wherein said at least one bulk rubber comprises polybutadiene. R3. The composition according to R2, wherein said at least one bulk rubber is polybutadiene. R4. The composition according to R2 or R3, wherein the polybutadiene has at least 90% of its mers in the cis configuration. R5. The composition of any one of R1-R4, further comprising a particulate filler comprising silica. R6. A composition according to any one of R1-R5, further comprising a heat-activated crosslinking agent, and a vulcanizate obtained from such a composition.
[0078] The following non-limiting illustrative examples provide detailed conditions and materials that may be useful in the practice of the present invention. These examples use 1,3-butadiene as an exemplary polyene and styrene as an exemplary vinyl aromatic compound due to various factors, including cost, availability, handling ability, and, most importantly, the ability to perform internal comparisons and comparisons with previously reported polymers. Those skilled in the art can extend these examples to various homopolymers and interpolymers. [Example]
[0079] In the following examples, the n-butyllithium (n-BuLi) solution is 2.5 M (1.6 M in Example 9), and the 2,2-bis(2'-tetrahydrofuryl)propane (BTHFP) solution is 1.6 M, both in hexane.
[0080] Example 1: Functionalized SBR To a 5 gallon (19 L) N2-purged reactor equipped with a stirrer was added 3.99 kg of hexane, 1.98 kg of styrene solution (30.3% (w / w) in hexane), and 5.41 kg of 1,3-butadiene solution (20.6% (w / w) in hexane). The reactor was then charged with 5.72 mL of n-BuLi solution, followed by 2.23 mL of BTHFP solution, and the reactor jacket was then heated to 50°C.
[0081] The batch temperature peaked at about 80°C after about 39 minutes.
[0082] After about an additional 40 minutes, 3.31 mL of ECETMOS was added to the reactor to functionalize the carbanionic polymer chains, and after about 30 minutes, 1.31 mL of isopropanol was added to terminate the polymerization.
[0083] A sample of the polymer cement was collected approximately 10 minutes after shutdown, and the remaining cement was transferred to a storage container. The properties of the collected functionalized SBR intermediate are summarized in Table 2 below.
[0084] Example 2: Hydrogenation To an approximately 44 L (11.7 gallon) stirred reactor under a N atmosphere was charged 11.43 kg of the functionalized polymer (in hexane) from Example 1, followed by 5.315 kg of hexane to give a 10.0% (w / w) solution. The reactor was purged three times with 138 kPa (20 psi) of H, and then the reactor jacket was heated to 50°C.
[0085] To a dry N2-purged bottle was added 400 mL of hexane and 21.97 mL of 1.03 M triethylaluminum, followed by 3.99 mL of nickel octoate solution (10.1% (w / w) in hexane) to obtain a hydrogenation catalyst system (Al / Ni=3.3:1).
[0086] The catalyst system was placed in the reactor, which was then immediately pressurized to 517 kPa (75 psi) with H2.
[0087] After approximately 90 minutes, the H2 was vented from the reactor and the polymer cement was transferred to a storage container. Approximately equal amounts of this polymer cement were transferred to previously collected 750 mL N2-purged glass bottles.
[0088] The percentage of hydrogenation of the butadiene mer was determined (by NMR) to be 92%.
[0089] Example 3: Low Molecular Weight BR To a 7.6 L (2 gallon) N2-purged reactor equipped with a stirrer was added 1.23 kg of hexane and 3.255 kg of 1,3-butadiene solution (20.9% w / w in hexane). The reactor was charged with 13.61 mL of n-BuLi solution, followed by 0.53 mL of BTHFP solution.
[0090] The reactor jacket was heated to 57° C. and the batch temperature peaked after 38 minutes at about 82° C. After a total reaction time of about 60 minutes, the reaction mixture was cooled to room temperature.
[0091] Examples 4 to 8: Coupling The polymer products of Examples 2 and 3 were coupled in various ratios as shown in the table below (ratios were determined based on the amount of Li in the 0.00125 mM / g polymer cement from Example 2 and the 0.0075 mM / g polymer cement from Example 3).
[0092] [Table 1]
[0093] The bottle was placed in a 50°C water bath and stirred for approximately 90 minutes. The sample was then agglomerated in a mixture of isopropanol and butylated hydroxytoluene (BHT). The agglomerated polymer sample was drum dried at 120°C.
[0094] Properties of the polymers from the foregoing examples are shown in the table below. Molecular weight values (all in kg / mol) of the polymer samples were determined by GPC, calibrated with a series of polystyrene standards, using THF as the solvent. The styrene and 1,2-bond (vinyl) content of the polymer samples was determined by NMR spectroscopy, and the glass transition temperatures (T g ) values were measured by DSC.
[0095] [Table 2]
[0096] Example 9: Low Molecular Weight BR To a 3.8 L (1 gallon) N2-purged reactor equipped with a stirrer was added 0.806 kg of hexane and 1.071 kg of 1,3-butadiene solution (24.1% w / w in hexane). The reactor was charged with 26.58 mL of n-BuLi solution, followed by 5.32 mL of BTHFP solution.
[0097] The reactor jacket was heated to 57° C. and the reaction was allowed to proceed for 30 minutes.
[0098] Example 10: Coupling To 500 mL of the polymer cement from Example 2 was added 12 mL of the product of Example 9. This resulted in an equivalence ratio of 2:1 (Examples 2-9) based on the amount of Li in each of the 0.00125 mM / g polymer cement from Example 2 and the 0.01875 mM / g polymer cement from Example 9.
[0099] The bottle was placed in a 50°C water bath and stirred for approximately 90 minutes. The sample was then agglomerated in a mixture of isopropanol and BHT. The agglomerated polymer sample was drum dried at 120°C.
[0100] The properties of the products of the coupling reaction are shown in the table below, where the units are as above and the properties were measured as above.
[0101] [Table 3]
[0102] Examples 11-13: Rubber Compounds and Vulcanizates Using an unfilled rubber composition formulation containing wax, antioxidants, accelerators, curatives, etc., three rubber compounds were prepared (Example 11 is a comparative example) that differed only in the nature and amount of polymers included. Example 11, 50 pbw of high cis BR and 50 pbw of the polymer of Example 2 Example 12, 45 pbw high cis BR and 55 pbw polymer of Example 10 Example 13, 45 pbw high cis BR, 49.5 pbw polymer of Example 2 and 5.5 pbw polymer of Example 10
[0103] Each formulation included a masterbatch and a final mix stage, and each compound was subjected to a standard cure time and temperature combination.
[0104] The stress at break and toughness of the resulting vulcanizates were evaluated at both room temperature (RT, approximately 22°C) and 100°C, and the results are summarized in the table below.
[0105] [Table 4]
[0106] From the above, it can be seen that the use of a polymer of the type of Example 10 as an additive (e.g., at 5 phr) improves tensile properties, but its use as a direct replacement for functionalized H-SBR gives essentially equivalent properties.
[0107] Tan 6 was plotted against temperature over the range of −120° C. to −100° C. for the vulcanizates of Examples 11 and 12. Comparing the peaks of the two vulcanizates over the range of about −80° C. to −100° C. shows that the peaks of the vulcanizate of Example 12 are both reduced and shifted by about +3° C., both of which indicate that the miscibility between high-cis BR and H-SBR is improved when the latter contains grafted BR segments.
[0108] The improved miscibility was confirmed by transmission electron microscopy, where images showed that the vulcanizate of Example 12 had less discrete domains than the vulcanizate of Example 11, and also showed better overall polymer mixing. [1] A functionalized polymer comprising a hydrogenated interpolymer portion, a non-hydrogenated polymer portion, and a functional group covalently bonded to each of said portions, said functional group exhibiting an interactive property with silica. [2] The functionalized polymer according to [1] above, wherein the functional group is a radical of a compound containing both an epoxy group and a siloxy group. [3] The functionalized polymer of [2] above, wherein the compound is 2-(3,4-epoxy-cyclohexyl)ethyltrialkoxysilane, and the alkoxy group is optionally a methoxy moiety. [4] The functionalized polymer according to any one of [1] to [3] above, wherein the interpolymer comprises a vinyl aromatic mer and a conjugated diene mer. [5] [4] The functionalized polymer according to [4], wherein at least 80 mole percent of the conjugated diene mers in the interpolymer are hydrogenated. [6] [5] The functionalized polymer according to [5], wherein at least 90 mole percent of the conjugated diene mers in the interpolymer are hydrogenated. [7] The functionalized polymer according to [4] above, wherein the interpolymer contains 10 to 45 mol % of styrene mers. [8] The functionalized polymer according to [4] above, wherein the majority of the conjugated diene mers are incorporated in a 1,2-vinyl configuration. [9] The functionalized polymer according to any one of [1] to [3] above, wherein the non-hydrogenated polymer portion comprises a conjugated diene mer.
[10] The functionalized polymer according to any one of [1] to [3] above, wherein the polymer comprises a plurality of non-hydrogenated polymer segments.
[11] The functionalized polymer according to any one of [1] to [3] above, wherein the non-hydrogenated polymer portion is obtained from a conjugated diene homopolymer having a number average molecular weight of 5 to 50 kg / mol.
[12] The functionalized polymer according to
[11] above, wherein the conjugated diene homopolymer has a number average molecular weight of 10 to 20 kg / mol.
[13] The functionalized polymer according to
[11] above, wherein the conjugated diene homopolymer has a number average molecular weight of 30 to 40 kg / mol.
[14] A composition comprising the functionalized polymer according to any one of the above [1] to [3], at least one bulk rubber optionally containing polybutadiene, and optionally silica.
[15] The composition according to
[14] , wherein the composition comprises at least one polybutadiene, at least 90% of whose mers are in a cis configuration.
[16] 1. A method for providing a functionalized polymer comprising a hydrogenated interpolymer portion and a non-hydrogenated polymer portion, comprising: a) 1) a vinyl aromatic mer; 2) conjugated dienes and 3) a hydrogenated conjugated diene mer; 4) providing a terminally functionalized interpolymer comprising a terminal functional group that is reactive to carbanions and that comprises a functional group capable of interacting with silica; b) incorporating the interpolymer into a carbanionic polymer comprising a conjugated diene mer, or incorporating the carbanionic polymer into the interpolymer, wherein the carbanionic polymer optionally has a number average molecular weight of 5 to 50 kg / mol; c) reacting the carbanionic polymer with the terminal functional group to provide the functionalized macromolecule.
[17] 17. The method of claim 16, wherein the interpolymer is provided by subjecting an end-functionalized polymer comprising a vinyl aromatic mer and a conjugated diene mer to hydrogenation conditions to hydrogenate at least 50 mole percent of the conjugated diene mer.
[18] The method of claim 17, wherein at least 80 mol % of the conjugated diene mers are hydrogenated.
[19] The method according to any one of
[16] to
[18] above, wherein at least one of the following is true: the interpolymer contains 10 to 45 mol% of styrene mers; and the majority of the conjugated diene mers are incorporated in a 1,2-vinyl configuration.
[20] The method according to any one of
[16] to
[18] above, wherein 0.5 to 10 equivalents of the carbanionic polymer are reacted per equivalent of the interpolymer.
Claims
1. A polymeric composition comprising: a random hydrogenated interpolymer portion; a non-hydrogenated polymer portion; and a functional group covalently bonded to each of said portions, said functional group exhibiting an interactive property with silica; the random hydrogenated interpolymer portion is a random hydrogenated interpolymer comprising vinyl aromatic mer units and conjugated diene mer units which are at least partially, but less than 100%, hydrogenated; A functionalized polymer, wherein the unhydrogenated polymer portion comprises conjugated diene mer units.
2. 2. The functionalized polymer of claim 1, wherein the functional group is a radical of a compound that contains both an epoxy group and a siloxy group.
3. 3. The functionalized polymer of claim 2, wherein the compound is 2-(3,4-epoxy-cyclohexyl)ethyltrialkoxysilane.
4. The functionalized polymer of claim 1, wherein the non-hydrogenated polymer portion is formed from a carbanionic polymer containing conjugated diene mer units.
5. A composition comprising the functionalized polymer of any one of claims 1 to 3, at least one bulk rubber optionally comprising polybutadiene, and optionally silica.
6. 1. A method for providing a functionalized polymer comprising a hydrogenated interpolymer portion and a non-hydrogenated interpolymer portion, comprising: a) 1) a vinyl aromatic mer; 2) a conjugated diene mer; 3) a hydrogenated conjugated diene mer; and 4) providing a terminal functionalized interpolymer comprising a terminal functional group, the terminal functional group comprising a functional group reactive to carbanions and capable of interacting with silica; b) introducing said interpolymer into a carbanionic polymer comprising a conjugated diene mer, or introducing said carbanionic polymer into said interpolymer, said carbanionic polymer optionally having a number average molecular weight of 5 to 50 kg / mol; and c) reacting the carbanionic polymer with the terminal functional group to provide the functionalized macromolecule.
Citation Information
Patent Citations
Asymmetric radial or star block copolymer with different arms and for adhesive and sealant
JP1995188361A
Conjugated polymer products, methods of making and compositions
JP2020510111A
Method for producing hydrogenated conjugated diene polymer, hydrogenated conjugated diene polymer, polymer composition, cross-linked polymer, and tire