Propylene resin composition

The propylene resin composition, enriched with specific additives, addresses the need for improved tensile breaking strain in molded articles by enhancing their durability and reducing mold contamination.

JP7580651B1Active Publication Date: 2024-11-11SUMITOMO CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024104979
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-11-14
Filing Date
2024-06-28
Publication Date
2024-11-11
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Molded articles made from propylene resin compositions used in automobile, home appliance, and packaging materials require improved tensile breaking strain to enhance their durability and resistance to deformation.

Method used

A propylene resin composition containing a propylene polymer, a metal deactivator, and a hindered amine light stabilizer, with specific weight ratios and additives such as ethylene-α-olefin copolymers and inorganic fillers, to enhance tensile strain at break.

Benefits of technology

The composition results in molded articles with increased tensile strain at break, reducing the likelihood of sharp breakage and improving safety while minimizing mold contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580651000001
    Figure 0007580651000001
  • Figure 0007580651000002
    Figure 0007580651000002
Patent Text Reader

Abstract

To provide a propylene resin composition from which a molded article having a large tensile breaking strain can be produced. [Solution] A propylene resin composition containing a propylene polymer, a metal deactivator, and a hindered amine light stabilizer, wherein the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a propylene resin composition and a molded article thereof. [Background technology]

[0002] Molded articles containing (produced from) propylene resin compositions are used as automobile materials, home appliance materials, container and packaging materials, and the like. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-196379 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, molded articles used in automobile materials, home appliance materials, container and packaging materials, etc. are required to have a high tensile breaking strain.

[0005] Therefore, an object of the present invention is to provide a propylene resin composition from which a molded article having a large tensile breaking strain can be produced. Another object of the present invention is to provide a molded article having a large tensile breaking strain. [Means for solving the problem]

[0006] The present invention relates to, but is not limited to, the following: [Invention A1] A propylene resin composition comprising a propylene polymer, a metal deactivator, and a hindered amine light stabilizer, A propylene resin composition, wherein the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more. [Invention A2] The propylene resin composition according to Invention A1, wherein the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 50 or less. [Invention A3] The propylene resin composition according to Invention A1 or A2, wherein the propylene-based polymer comprises a heterophasic propylene polymer material. [Invention A4] The propylene resin composition according to any one of Inventions A1 to A3, wherein the weight ratio of the metal deactivator is 10 ppm by weight to 1000 ppm by weight with respect to 100 parts by weight of the total weight of the propylene resin composition. [Invention A5] The propylene resin composition according to any one of Inventions A1 to A4, wherein the weight ratio of the hindered amine light stabilizer is 200 ppm by weight to 10,000 ppm by weight based on 100 parts by weight of the total weight of the propylene resin composition. [Invention A6] The propylene resin composition according to any one of Inventions A1 to A5, wherein the weight ratio of the propylene polymer is 50 parts by weight or more based on 100 parts by weight of the total weight of the propylene resin composition. [Invention A7] The propylene resin composition according to any one of Inventions A1 to A6, wherein the propylene resin composition has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more. [Invention A8] The propylene resin composition according to any one of Inventions A1 to A7, wherein the propylene polymer has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more. [Invention A9] The propylene resin composition according to any one of Inventions A1 to A8, further comprising an ethylene-α-olefin copolymer. [Invention A10] The propylene resin composition according to Invention A9, wherein a weight ratio of the ethylene-α-olefin copolymer is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition. [Invention A11] The propylene resin composition according to any one of Inventions A1 to A10, further comprising an inorganic filler. [Invention A12] The propylene resin composition according to Invention A11, wherein a weight ratio of the inorganic filler is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition. [Invention A13] The propylene resin composition according to any one of Inventions A1 to A12, further comprising an ethylene-α-olefin copolymer and an inorganic filler. [Invention A14] A molded article comprising the propylene resin composition according to any one of Inventions A1 to A13.

[0007] Other aspects of the invention are set forth below. [Invention B1] A propylene resin composition comprising a propylene polymer, a metal deactivator having a triazole skeleton or a triazine skeleton, and a hindered amine light stabilizer having a 2,2,6,6-tetramethylpiperidine skeleton, the propylene-based polymer is a heterophasic propylene polymer material; the weight ratio of the metal deactivator is 10 ppm by weight to 1,000 ppm by weight, and the weight ratio of the hindered amine light stabilizer is 200 ppm by weight to 10,000 ppm by weight, relative to 100 parts by mass of the propylene polymer; the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more; Propylene resin composition. [Invention B2] The propylene resin composition according to Invention B1, wherein the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 50 or less. [Invention B3] The propylene resin composition according to Invention B1 or B2, wherein a weight ratio of the propylene-based polymer is 50 parts by weight or more based on 100 parts by weight of the total weight of the propylene resin composition. [Invention B4] The propylene resin composition according to any one of Inventions B1 to B3, wherein the propylene resin composition has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more. [Invention B5] The propylene resin composition according to any one of Inventions B1 to B4, wherein the propylene polymer has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more. [Invention B6] The propylene resin composition according to any one of Inventions B1 to B5, further comprising an ethylene-α-olefin copolymer. [Invention B7] The propylene resin composition according to Invention B6, wherein the weight ratio of the ethylene-α-olefin copolymer is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition. [Invention B8] The propylene resin composition according to any one of Inventions B1 to B7, further comprising an inorganic filler. [Invention B9] The propylene resin composition according to Invention B8, wherein a weight ratio of the inorganic filler is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition. [Invention B10] The propylene resin composition according to any one of Inventions B1 to B9, further comprising an ethylene-α-olefin copolymer and an inorganic filler. [Invention B11] A molded article comprising the propylene resin composition according to any one of Inventions B1 to B10. Effect of the Invention

[0008] According to the present invention, it is possible to provide a molded article having a large tensile breaking strain and a propylene resin composition which is a raw material thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to the specific embodiments described below.

[0010] Explanation of terms Before describing the embodiments of the present invention, commonly used terms will be described.

[0011] In this specification, the term "monomer unit" refers to a structural unit (residue) derived from a monomer contained in a polymer obtained by polymerizing a monomer.

[0012] As used herein, the term "α-olefin" refers to an olefin that includes a carbon atom chain of three or more carbon atoms having a terminal (α-position) carbon-carbon double bond.

[0013] In this specification, the term "intrinsic viscosity (unit: dL / g)" (also referred to as [η]) is a value measured at a temperature of 135° C. using tetralin as a solvent by the following method.

[0014] Specifically, the intrinsic viscosity can be determined by an "extrapolation method" in which the reduced viscosity is measured at a plurality of concentrations using an Ubbelohde viscometer, the reduced viscosity is plotted against the concentration, and the concentration is extrapolated to zero. For example, the measurement is performed according to the method described in the Examples.

[0015] In this specification, "melt flow rate (MFR)" means "melt mass flow rate" and is a melt flow rate measured in accordance with JIS K7210-1:2014 and K7210-2:2014 under conditions of a temperature of 230°C and a load of 2.16 kgf.

[0016] In this specification, unless otherwise specified, "%" means "% by weight" and "parts" means "parts by weight".

[0017] The description "lower limit to upper limit" expressing a numerical range means "lower limit or more, upper limit or less", and the description "upper limit to lower limit" expresses "upper limit or less, lower limit or more". That is, these descriptions express a numerical range including the lower limit and the upper limit, but in one embodiment, one or both of the upper limit and the lower limit may be excluded, that is, "lower limit to upper limit" may express "more than the lower limit and lower limit", "lower limit or more, less than the upper limit", or "more than the lower limit and less than the upper limit". Similarly, "xxx or more" may express "more than xxx", and "xxx or less" may express "less than xxx".

[0018] Propylene resin composition The propylene resin composition according to the present invention is a propylene resin composition containing a propylene polymer, a metal deactivator, and a hindered amine light stabilizer, and the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is not less than 10. In one embodiment, the weight ratio of the metal deactivator is 10 parts by weight to 1000 ppm by weight with respect to 100 parts by weight of the total weight of the propylene resin composition.

[0019] Hereinafter, components that may be contained in the propylene resin composition of the present embodiment will be described.

[0020] Propylene polymer (P) In this specification, a propylene-based polymer (also referred to as component P) is a polymer containing propylene units in an amount of more than 50% by weight based on the total constituent units (100% by weight). The amount of propylene units in a propylene-based polymer is usually 100% by weight or less.

[0021] Examples of propylene-based polymers include propylene homopolymers and propylene-based copolymers (copolymers obtained by polymerizing propylene and one or more other monomers copolymerizable with propylene in any combination in any ratio).

[0022] Propylene homopolymer The intrinsic viscosity [η] of the propylene homopolymer is preferably 0.1 dL / g to 5 dL / g, more preferably 0.5 dL / g to 4 dL / g, and even more preferably 0.6 dL / g to 3 dL / g, from the viewpoint of improving the fluidity of the propylene resin composition when melted and the toughness of a molded article obtained by molding the propylene resin composition.

[0023] Propylene-based copolymer The propylene copolymer may be a random copolymer or a block copolymer. Examples of other monomers that can be copolymerized with propylene include olefins other than propylene (e.g., ethylene, olefins having 4 or more carbon atoms). The number of carbon atoms of the olefin may be 12 or less.

[0024] The olefin having 4 or more carbon atoms may be a linear olefin or a branched olefin. The olefin having 4 or more carbon atoms may be an olefin having a cyclic structure, such as an α-olefin having a cyclic structure, such as vinylcyclopropane or vinylcyclobutane.

[0025] Examples of olefins other than propylene that can be copolymerized with propylene include α-olefins other than propylene (e.g., ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene). The olefins other than propylene that can be copolymerized with propylene are preferably ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and more preferably ethylene, 1-butene, 1-hexene, and 1-octene.

[0026] Propylene-based random copolymer Examples of propylene-based random copolymers include a random copolymer containing propylene units and ethylene units (hereinafter also referred to as random polymer (1)); a random copolymer containing propylene units and α-olefin units having 4 or more carbon atoms (hereinafter also referred to as random polymer (2)); and a random copolymer containing propylene units, ethylene units, and α-olefin units having 4 or more carbon atoms (hereinafter also referred to as random polymer (3)).

[0027] The α-olefin having 4 or more carbon atoms which can constitute the propylene-based random copolymer is preferably an α-olefin having 4 to 10 carbon atoms. Examples of the α-olefin having 4 to 10 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, and 1-octene.

[0028] Examples of the random copolymer (2) include propylene-1-butene random copolymer, propylene-1-hexene random copolymer, propylene-1-octene random copolymer, and propylene-1-decene random copolymer.

[0029] Examples of the random copolymer (3) include propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, and propylene-ethylene-1-decene copolymer.

[0030] The content of the ethylene unit in the random copolymer (1) is preferably 0.1% by weight to 40% by weight.

[0031] The content of α-olefin units having 4 or more carbon atoms in the random copolymer (2) is preferably 0.1 to 40% by weight, more preferably 0.1 to 30% by weight, and further preferably 2 to 15% by weight.

[0032] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in the random copolymer (3) is preferably 0.1% by weight to 40% by weight, more preferably 0.1% by weight to 30% by weight, and even more preferably 2% by weight to 15% by weight.

[0033] The content of propylene units in each of these random copolymers (1) to (3) is preferably 60% by weight to 99.9% by weight.

[0034] The propylene polymer (P) can be produced, for example, by the following polymerization method using a polymerization catalyst.

[0035] Examples of polymerization catalysts include Ziegler-type catalyst systems; Ziegler-Natta-type catalyst systems; catalyst systems containing a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane; catalyst systems containing a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with the transition metal compound to form an ionic complex, and an organoaluminum compound; and catalyst systems in which catalyst components (e.g., a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) are supported on inorganic particles (e.g., silica, clay minerals, etc.) and modified. In addition, a prepolymerization catalyst prepared by prepolymerizing a monomer such as ethylene or an α-olefin in the presence of such a catalyst system may be used. An example of a Ziegler-Natta-type catalyst system is a catalyst system that uses a combination of a titanium-containing solid transition metal component and an organometallic component.

[0036] Examples of such catalyst systems include those described in JP-A-61-218606, JP-A-5-194685, JP-A-7-216017, JP-A-9-316147, and JP-A-10-212319, and an example of a catalyst system used to produce a heterophasic propylene polymer material described later is the catalyst system described in JP-A-2004-182981.

[0037] Examples of polymerization methods include bulk polymerization, solution polymerization, and gas phase polymerization. Here, bulk polymerization refers to a method in which polymerization is carried out using an olefin that is liquid at the polymerization temperature as a medium. Solution polymerization refers to a method in which polymerization is carried out in an inert hydrocarbon solvent such as propane, butane, isobutane, pentane, hexane, heptane, or octane. Gas phase polymerization refers to a method in which a gaseous monomer is used as a medium and the gaseous monomer is polymerized in the medium.

[0038] In carrying out the polymerization method, examples of the polymerization system include a batch system, a continuous system, and a combination thereof. The polymerization system may be a multi-stage system in which a plurality of polymerization reaction vessels connected in series are used.

[0039] Various conditions in the polymerization method (polymerization temperature, polymerization pressure, monomer concentration, catalyst input amount, polymerization time, etc.) can be appropriately determined depending on the desired propylene-based polymer.

[0040] In the production of a propylene-based polymer, the resulting propylene-based polymer may be kept at a temperature at which impurities such as residual solvent and the oligomers can volatilize and which is lower than the temperature at which the propylene-based polymer melts, thereby removing the residual solvent contained in the resulting propylene-based polymer and the ultra-low molecular weight oligomers produced as by-products during the production. Examples of the method for removing impurities such as residual solvent and oligomers include the methods described in JP-A-55-75410 and JP-A-2565753.

[0041] The propylene resin composition of the present embodiment may contain two or more kinds of propylene polymers as the propylene polymer (P).

[0042] When two or more kinds of propylene-based polymers are contained, examples of the combination include a combination of two or more kinds of propylene homopolymers differing in weight average molecular weight, etc., and a heterophasic propylene polymer material.

[0043] Here, the term "heterophagic propylene polymer material" refers to a material containing two or more types of propylene polymers, in which the two or more types of propylene polymers are not compatible with each other and form separate phases.

[0044] Examples of heterophasic propylene polymer materials include materials containing a combination of polymer (I) and polymer (II) below.

[0045] Here, the polymer (I) is a polymer having propylene units in an amount of more than 80% by weight and not more than 100% by weight based on the amount of all constituent units. The polymer (I) may be a propylene homopolymer or a copolymer of propylene and other monomers. The total content of monomer units other than propylene units in the polymer (I) is usually 0% by weight or more and less than 20% by weight, and may be 0% by weight or more, or may be 0.01% by weight or more, when the weight of the polymer (I) is taken as 100% by weight. When the polymer (I) is a copolymer, the polymer (I) may be a random copolymer.

[0046] Examples of monomer units other than propylene units that the polymer (I) may have include ethylene units and α-olefin units having 4 or more carbon atoms.

[0047] The α-olefin having 4 or more carbon atoms which can constitute the polymer (I) is preferably an α-olefin having 4 to 10 carbon atoms, more preferably 1-butene, 1-hexene and 1-octene, and even more preferably 1-butene.

[0048] Examples of the polymer (I) include propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, and propylene-ethylene-1-octene copolymer.

[0049] Among these, as the polymer (I), propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, and propylene-ethylene-1-butene copolymer are preferred, and from the viewpoint of improving the rigidity of a molded body obtained by molding the propylene resin composition, propylene homopolymer is more preferred.

[0050] The polymer (II) is a copolymer of a propylene unit and at least one monomer unit selected from the group consisting of an ethylene unit and an α-olefin unit having 4 or more carbon atoms. The polymer (II) is preferably a polymer having propylene units in an amount of more than 0% by weight and not more than 90% by weight, more preferably more than 0% by weight and not more than 80% by weight, based on the amount of all constituent units. The polymer (II) may be a random copolymer or a block copolymer.

[0051] The total content of ethylene units and α-olefin units having 4 or more carbon atoms in polymer (II) is preferably 20% by weight to 80% by weight, and more preferably 20% by weight to 60% by weight, when the weight of polymer (II) is 100% by weight.

[0052] The α-olefin having 4 or more carbon atoms that can constitute polymer (II) is preferably an α-olefin having 4 to 10 carbon atoms, and examples thereof include the same as the examples of α-olefins that can constitute polymer (I) already described.

[0053] Examples of the polymer (II) include propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, propylene-ethylene-1-decene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, and propylene-1-decene copolymer. The polymer (II) is preferably a propylene-ethylene copolymer, a propylene-1-butene copolymer, and a propylene-ethylene-1-butene copolymer, and more preferably a propylene-ethylene copolymer.

[0054] The content of polymer (II) in the heterophasic propylene polymer material is preferably 1 wt% to 50 wt%, more preferably 1 wt% to 45 wt%, even more preferably 5 wt% to 40 wt%, and particularly preferably 7 wt% to 35 wt%, when the total weight of polymer (I) and polymer (II) is 100 wt%.

[0055] Each of the polymer (I) and the polymer (II) may consist of only one type of polymer, or may contain two or more types of polymers.

[0056] Examples of heterophasic propylene polymer materials include those in which the polymer (I) is a propylene homopolymer, a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-octene) copolymer, a combination of a propylene homopolymer and a (propylene-1-butene) copolymer, a combination of a propylene homopolymer and a (propylene-1-hexene) copolymer, a combination of a propylene homopolymer and a (propylene-1-octene) copolymer, and a combination of a propylene homopolymer and a (propylene-1-decene) copolymer.

[0057] The heterophasic propylene polymer material may be a combination in which the polymer (I) is a polymer containing a propylene unit and a monomer unit other than a propylene unit. If the type of the polymer (I) is described first and the type of the polymer (II) is described second, specific examples of such a heterophasic propylene polymer material include a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-hex ... -octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-decene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-hexene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-1-decene) copolymer combinations of (propylene-1-butene) copolymers and (propylene-ethylene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-ethylene-1-butene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-ethylene-1-hexene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-ethylene-1-octene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-ethylene-1-decene) copolymers combinations of (propylene-1-butene) copolymers and (propylene-1-butene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-1-hexene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-1-octene) copolymers; combinations of (propylene-1-butene) copolymers and (propylene-1-decene) copolymers; combinations of (propylene-1-hexene) copolymers and (propylene-1-hexene) copolymers;Examples of the combination include a combination of a (propylene-1-hexene) copolymer and a (propylene-1-octene) copolymer, a combination of a (propylene-1-hexene) copolymer and a (propylene-1-decene) copolymer, a combination of a (propylene-1-octene) copolymer and a (propylene-1-octene) copolymer, and a combination of a (propylene-1-octene) copolymer and a (propylene-1-decene) copolymer.

[0058] Preferred heterophasic propylene polymer materials that may be contained in the propylene resin composition of this embodiment include a combination of a propylene homopolymer and a (propylene-ethylene) copolymer, a combination of a propylene homopolymer and a (propylene-ethylene-1-butene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene) copolymer, a combination of a (propylene-ethylene) copolymer and a (propylene-ethylene-1-butene) copolymer, and a combination of a (propylene-1-butene) copolymer and a (propylene-1-butene) copolymer, with a combination of a propylene homopolymer and a (propylene-ethylene) copolymer being more preferred.

[0059] The heterophasic propylene polymer material can be produced by a multi-stage polymerization process having a first polymerization step of producing a polymer (I) and a second polymerization step of producing a polymer (II) in the presence of the polymer (I) produced in the first polymerization step. The polymerization can be carried out using the catalyst system exemplified as the catalyst system usable for producing the propylene polymer.

[0060] The propylene-based polymer (P) preferably contains one or more selected from the group consisting of propylene homopolymers and heterophasic propylene polymer materials, and is more preferably a heterophasic propylene polymer material.

[0061] The propylene polymer (P) is 13The isotactic pentad fraction (also called the [mmmm] fraction) measured by C-NMR is preferably 0.97 or more, more preferably 0.98 or more. The closer the isotactic pentad fraction of a propylene-based polymer is to 1, the higher the stereoregularity of the molecular structure of the propylene-based polymer, and the higher the crystallinity of the propylene-based polymer. When the propylene-based polymer is a copolymer, the isotactic pentad fraction can be measured for the chain of propylene units in the copolymer.

[0062] The melt flow rate (MFR) of the propylene polymer (P), measured under conditions of a temperature of 230°C and a load of 2.16 kgf, is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, preferably 500 g / 10 min or less, more preferably 400 g / 10 min or less, and preferably 0.1 g / 10 min to 500 g / 10 min, from the viewpoint of improving processability in molding of the propylene resin composition.

[0063] In addition, from the viewpoint of improving the fluidity and processability of the propylene resin composition, the intrinsic viscosity of the propylene polymer (P) of the present embodiment is usually less than 5 dL / g, 0.1 dL / g or more, preferably 0.5 dL / g or more, more preferably 0.7 dL / g or more and less than 4 dL / g, and even more preferably 0.8 dL / g or more and less than 3 dL / g.

[0064] In the present embodiment, the propylene polymer (P) has a polystyrene-equivalent weight average molecular weight of usually 100,000 to 1,000,000, and preferably 500,000 to 1,000,000, from the viewpoint of improving the appearance and elongation properties of the molded article.

[0065] The molecular weight distribution (Mw / Mn) of the propylene polymer (P) may be usually 10 or less, and preferably 3-8, from the viewpoint of improving moldability and mechanical properties.

[0066] In this specification, Mw represents the weight average molecular weight, Mn represents the number average molecular weight, and the molecular weight distribution can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment: Tosoh Corporation HLC-8121 GPC / HT Separation column: 3 GMHHR-H(S)HT, manufactured by Tosoh Corporation Measurement temperature: 140℃ Carrier: Orthodichlorobenzene Flow rate: 1.0mL / min Sample concentration: Approximately 1 mg / mL Sample injection volume: 400 μL Detector: Differential Refraction Calibration curve creation method: Standard polystyrene is used for conversion

[0067] When the propylene-based polymer is a heterophasic propylene polymer material substantially composed of polymer (I) and polymer (II) formed by multi-stage polymerization, a part of the polymer (I) prepared in the first polymerization stage is extracted from the polymerization reactor to determine its intrinsic viscosity (also referred to as [η]I), and the intrinsic viscosity (also referred to as [η]Total) of the polymer finally obtained by the multi-stage polymerization is determined. Using these intrinsic viscosity values ​​and the content ratio of each polymer, the intrinsic viscosity (also referred to as [η]II) of the polymer (II) formed in the second polymerization stage can be calculated. The calculation procedure is as follows. XI and XII can be determined from the material balance during polymerization. [η]II=([η]Total-[η]I × XI) / XII [η]Total: Intrinsic viscosity of the final polymer (unit: dL / g) [η]I: Intrinsic viscosity of polymer (I) (unit: dL / g) XI: Weight ratio of polymer (I) to final polymer XII: Weight ratio of polymer (II) to final polymer

[0068] The intrinsic viscosity [η]I of the polymer (I) is preferably 0.1 dL / g to 5 dL / g, more preferably 0.5 dL / g to 4 dL / g, and further preferably 0.6 dL / g to 3 dL / g.

[0069] The intrinsic viscosity [η]II of the polymer (II) is preferably 1 dL / g to 10 dL / g, more preferably 1.5 dL / g to 9 dL / g, and further preferably 2 dL / g to 8 dL / g.

[0070] The ratio of [η]II to [η]I ([η]II / [η]I) is preferably 1-20, and more preferably 1-10.

[0071] The weight ratio XII of the polymer (II) to the final polymer may be calculated from the following formula using the respective heats of crystal fusion of the polymer (I) and the final polymer. XII = 1 - (ΔHf)Total / (ΔHf)I (ΔHf)Total: Heat of fusion of the final polymer (polymer (I) and polymer (II)) (unit: cal / g) (ΔHf)I: Heat of fusion of polymer (I) (unit: cal / g)

[0072] The molecular weight distribution (Mw / Mn) of the polymer (I) is preferably 1 or more and less than 10, more preferably 2 or more and less than 7, and further preferably 3 or more and less than 5.

[0073] metal deactivator The propylene resin composition of the present invention contains a metal deactivator (also referred to as component D). A metal deactivator is a compound that has a function of chelating metal ions and prevents the progress of thermo-oxidative deterioration of a polymeric material caused by metals in an environment where the polymeric material comes into contact with the metal. As component D, a known metal deactivator can be used. For example, benzotriazole derivatives, compounds having one or more groups represented by -CO-NH- (e.g., oxalic acid derivatives, salicylic acid derivatives, hydrazide derivatives, hydroxybenzoic acid anilide derivatives), sulfur-containing phosphites, etc., disclosed in "New Developments in Polymer Additives" (Nikkan Kogyo Shimbun, pp. 76-85) or JP-A-8-302331, can be mentioned. These metal deactivators can be used alone, or two or more kinds of metal deactivators can be used in combination. Although overlapping with the above, other examples include compounds containing a nitrogen-containing heteromonocyclic ring in the molecule, compounds containing a nitrogen-containing condensed heterocyclic ring in the molecule, compounds containing a phenolic hydroxyl group in the molecule, compounds containing a salicyl group in the molecule, hydrazones and bishydrazones of aliphatic and aromatic aldehydes, hydrazides of aliphatic and aromatic mono- and dicarboxylic acids, and bisacylated hydrazine derivatives.

[0074] Metal deactivators having a triazole or triazine skeleton are preferred.

[0075] Specific preferred examples of the metal deactivator include unsubstituted or alkyl-substituted benzotriazole, 2,4,6-triamino-1,3,5-triazine, 3,9-bis[2-(3,5-diamino-2,4,6-triazaphenyl)ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, ethylenediamine-tetraacetic acid, alkali metal salts (Li, Na, K) of ethylenediamine-tetraacetic acid, N,N'-disalicylidene-ethylenediamine, N,N'-disalicylidene-ethylenediamine, Licylidene-1,2-propylenediamine, N,N''-disalicylidene-N'-methyl-dipropylenetriamine, 3-(N-salicyloyl)amino-1,2,4-triazole (Adekastab CDA-1M), decamethylenedicarboxylic acid-bis(N'-salicyloylhydrazide), nickel-bis(1-phenyl-3-methyl-4-decanoyl-5-pyrazolate), 2-ethoxy-2'-ethyloxanilide, 5-t-butyl-2-ethoxy-2'-ethyloxanilide, N,N- Diethyl-N',N'-diphenyloxamide, N,N'-diethyl-N,N'-diphenyloxamide, oxalic acid-bis(benzylidenehydrazide), thiodipropionic acid-bis(benzylidenehydrazide), isophthalic acid-bis(2-phenoxypropionylhydrazide), bis(salicylidenehydrazine), N-salicylidene-N'-salicylidenehydrazone, 2',3-bis[[3-[3,5-di-t-butyl-4-hydroxyphenyl]propionyl]]propionyl lopionohydrazide, trimethyl phosphate, tris[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butyl)phenyl-5-methyl]-phenyl phosphite, bis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-pentaerythritol-diphosphite, tetrakis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-1,6-Hexamethylene-bis(N-hydroxyethyl-N-methylsemicarbazide)-diphosphite, tetrakis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-1,10-decamethylene-dicarboxylic acid-dihydroxyethylcarbonylhydrazide-diphosphite, tetrakis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-1,10-decamethylene-dicarboxylic acid-di-salicyloylhydrazide-diphosphite, tetrakis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-1,10-decamethylene-dicarboxylic acid-di-salicyloylhydrazide-diphosphite Examples of such bis(hydroxyethyl) hydrazide include tetrakis[2-t-butyl-4-thio(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-5-methylphenyl]-N,N'-bis(hydroxyethyl)oxamide-diphosphite, 2,2'-oxamide bis[ethyl 3-(3,5-t-butyl-4-hydroxyphenyl)propionate], N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoyl]propanehydrazide, and melamine.

[0076] More preferred examples include 3-(N-salicyloyl)amino-1,2,4-triazole, trimethyl phosphate, N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide, melamine, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N'-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoyl]propanehydrazide.

[0077] Hindered amine light stabilizer (H) The propylene resin composition of the present invention contains a hindered amine stabilizer (also referred to as component H). The hindered amine stabilizer is a compound having a 2,2,6,6-tetramethylpiperidine skeleton in the molecule, and is a light stabilizer that captures radicals generated by light (ultraviolet rays) in organic materials, polymeric materials, etc., and prevents the organic materials and polymeric materials from decomposing due to hydroperoxide degradation. For example, low molecular weight or high molecular weight light stabilizers can be mentioned. The hindered amine light stabilizer (H) may be used alone or in combination of two or more kinds.

[0078] The low molecular weight light stabilizer is a light stabilizer having a molecular weight of less than 1000, and examples thereof include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (trade name: Tinuvin 770, molecular weight: 480), bis(N-methyl-2,2,6,6-tetramethyl-4-piperidyl)sebacate (trade name: Tinuvin 765, molecular weight: 508), tetrakis(2,2,6,6-tetra-methyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate (trade name: A Examples of such esters include DECASTAB LA-57, molecular weight: 792), tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate (trade name: ADK STAB LA-52, molecular weight: 847), decanedioic acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidyl)ester, and reaction product of 1,1-dimethylethyl hydroperoxide with octane (trade name: TINUVIN123, molecular weight: 737).

[0079] The high molecular weight light stabilizer is a light stabilizer having a molecular weight of 1000 or more, and examples thereof include sterically hindered amine oligomer "copolymer of N-(2,2,6,6-tetramethyl-4-piperidyl)maleimide and α-olefin (C20-24)" (product name: UVINUL [registered trademark] 5050H, molecular weight 3500), formaldehyde polycondensate, {2,4,6-trichloro-1,3,5-triazine·[N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexane-1,6-diyldiamine]·monomer, reaction product of sulfolin polymer and formic acid (trade name: CYASORB UV-3529, molecular weight: about 1700), polycondensation product of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol (trade name: TINUVIN 622LD, molecular weight: about 3100-4000), N,N',N'',N'''-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazin-2-yl)-4,7-diazadecane-1,10-diamine (molecular weight: 2286, 90%) and a mixture of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol polymer (molecular weight: approximately 3100 to 4000) (trade name: CHIMASORB119FL), mixed {1,2,2,6,6-pentamethyl-4-piperidyl / β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]dimethyl}-1,2,3,4 butanetetracarboxylate (ADEKA STAB LA-63, molecular weight: 2000), poly[{(6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl){(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}} (trade name: CHIMASORB944LD, molecular weight 2000-3100), dibutylamine·1,3,5-triazine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,Polycondensation product of 6-tetramethyl-4-piperidyl)butylamine (trade name: CHIMASORB2020FDL, molecular weight: about 2600 to 3400) and the like.

[0080] Ethylene-α-olefin copolymer (E) The propylene resin composition of the present embodiment may contain an ethylene-α-olefin copolymer (also referred to as component E).

[0081] In the ethylene-α-olefin copolymer (E), when the total weight of the ethylene-α-olefin copolymer is taken as 100% by weight, the sum of the content of monomer units derived from ethylene and the content of monomer units derived from an α-olefin having 4 or more carbon atoms may be 100% by weight.

[0082] Examples of α-olefins having 4 or more carbon atoms include α-olefins having 4 to 12 carbon atoms. Examples of α-olefins having 4 to 12 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. Among these, α-olefins having 4 or more carbon atoms are preferably 1-butene, 1-hexene, and 1-octene. The above α-olefins may be α-olefins having a cyclic structure, such as vinylcyclopropane and vinylcyclobutane.

[0083] Examples of the ethylene-α-olefin copolymer (E) include an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-1-decene copolymer, an ethylene-(3-methyl-1-butene) copolymer, and a copolymer of ethylene and an α-olefin having a cyclic structure.

[0084] In the ethylene-α-olefin copolymer (E), the content of monomer units derived from an α-olefin having 4 or more carbon atoms is preferably 1 wt% to 49 wt%, more preferably 5 wt% to 49 wt%, and even more preferably 24 wt% to 49 wt%, based on the total weight of the ethylene-α-olefin copolymer (100 wt%).

[0085] The ethylene-α-olefin copolymer (E) preferably has an MFR (measured at 190° C. under a load of 2.16 kgf) of 0.1 g / 10 min to 100 g / 10 min, more preferably 0.5 g / 10 min to 70 g / 10 min.

[0086] The density of the ethylene-α-olefin copolymer (E) is set to 0.850 g / cm from the viewpoint of improving the impact resistance of the molded product. 3 ~0.890g / cm 3 and preferably 0.850 g / cm 3 ~0.880g / cm 3 More preferably, it is 0.855 g / cm 3 ~0.870g / cm 3 It is even more preferable that:

[0087] The ethylene-α-olefin copolymer (E) can be produced by polymerizing ethylene and an α-olefin having 4 or more carbon atoms using a polymerization catalyst.

[0088] Examples of the polymerization catalyst used for the production include homogeneous catalysts such as metallocene catalysts, and Ziegler-Natta type catalysts.

[0089] Examples of homogeneous catalysts include catalysts consisting essentially of a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane; catalysts containing a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with the transition metal compound to form an ionic complex, and an organoaluminum compound; and catalysts modified by supporting a catalyst component (a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) on inorganic particles (silica, clay minerals, etc.).

[0090] An example of the Ziegler-Natta type catalyst is a catalyst that combines a titanium-containing solid transition metal component with an organometallic component.

[0091] The ethylene-α-olefin copolymer (E) may be a commercially available product. Examples of commercially available ethylene-α-olefin copolymers (E) include Engage (registered trademark) manufactured by Dow Chemical Japan, Tafmer (registered trademark) manufactured by Mitsui Chemicals, Neozex (registered trademark) and Ultzex ​​(registered trademark) manufactured by Prime Polymer Co., Ltd., Excellen FX (registered trademark), Sumikathene (registered trademark), and Esprene SPO (registered trademark) manufactured by Sumitomo Chemical Co., Ltd.

[0092] Inorganic filler (F) The propylene resin composition according to this embodiment may further contain an inorganic filler (also referred to as component F) from the viewpoint of improving mechanical properties, dimensional stability, and the like.

[0093] Examples of the inorganic filler (F) include (i) fibrous inorganic fillers and (ii) non-fibrous inorganic fillers. In this embodiment, the inorganic filler (F) may be used in combination of two or more kinds. The details are described below.

[0094] (i) Fibrous inorganic filler In this embodiment, the fibrous inorganic filler preferably has an average fiber diameter of 0.2 μm to 20 μm, an average fiber length of 5 μm to 200 μm, and an aspect ratio of 10 to 30. From the viewpoint of improving the rigidity and appearance of the molded article, it is more preferable that the average fiber diameter is 0.3 μm to 10 μm, the average fiber length is 7 μm to 150 μm, and the aspect ratio is 12 to 25.

[0095] The average fiber diameter and average fiber length of the fibrous inorganic filler are, for example, the average values ​​of the fiber diameter and fiber length measured by randomly selecting 50 or more fibers from an image of the fibrous inorganic filler obtained by an electron microscope, and the aspect ratio can be calculated using these average values.

[0096] Examples of fibrous inorganic fillers include fibrous magnesium oxysulfate, potassium titanate fiber, magnesium hydroxide fiber, aluminum borate fiber, calcium silicate fiber, calcium carbonate fiber, carbon fiber, glass fiber, and metal fiber. Of these, it is preferable to use fibrous magnesium oxysulfate and calcium silicate fiber.

[0097] The fibrous inorganic filler can be used as it is. From the viewpoint of improving the interfacial adhesion and further improving the dispersibility, the fibrous inorganic filler may be further surface-treated with, for example, a silane coupling agent or a metal salt of a higher fatty acid before use.

[0098] Examples of higher fatty acid metal salts that can be used for the surface treatment include calcium stearate, magnesium stearate, and zinc stearate.

[0099] In this embodiment, examples of the form of the fibrous inorganic filler include powder, flake, and granule. In this embodiment, any of the above-mentioned forms of the fibrous inorganic filler may be used. Since it is easy to handle, it is preferable to use a fibrous inorganic filler that is granular as the fibrous inorganic filler.

[0100] (ii) Non-fibrous inorganic fillers Examples of non-fibrous inorganic fillers include talc, mica, calcium carbonate, barium sulfate, magnesium carbonate, clay, alumina, calcium sulfate, silica sand, carbon black, titanium oxide, magnesium hydroxide, molybdenum, diatomaceous earth, sericite, shirasu, calcium hydroxide, calcium sulfite, sodium sulfate, bentonite, graphite, etc. From the viewpoints of improving the impact strength and improving the appearance of the molded body, it is preferable to use talc.

[0101] The average particle size of the non-fibrous inorganic filler is preferably 15 μm or less, more preferably 10 μm or less. Here, the average particle size of the non-fibrous inorganic filler is determined based on the volume-based particle size distribution measurement data measured by a laser diffraction method according to the method specified in JIS R1629, and means the particle size (50% equivalent particle size) when the cumulative number of particles from the small particle size side reaches 50% in the particle size distribution measurement data. The particle size defined in this way is generally called "50% equivalent particle size" and is represented by "D50".

[0102] The non-fibrous inorganic filler can be used as it is. From the viewpoint of improving the interfacial adhesion and dispersibility, the non-fibrous inorganic filler may be surface-treated with a silane coupling agent, a titanium coupling agent, or a surfactant.

[0103] Examples of surfactants that can be used for the surface treatment include higher fatty acids, higher fatty acid esters, higher fatty acid amides, and higher fatty acid salts.

[0104] The fibrous inorganic filler may be used as it is, or may be surface-treated with a silane coupling agent or a metal salt of a higher fatty acid in order to improve the interfacial adhesion and dispersibility.

[0105] Other Additives (A) In order to improve properties (for example, to improve rigidity, impact resistance, heat aging resistance, or water resistance, and / or to increase the tensile breaking strain), the propylene resin composition of the present embodiment may contain various other additives (also referred to as component A) as further optional components in addition to the above-mentioned components already described.

[0106] Examples of such optional additives include antioxidants, neutralizing agents, ultraviolet absorbers, lubricants, antistatic agents, colorants (e.g., inorganic pigments, organic pigments), flame retardants, elastomers, antiblocking agents, processing aids, organic peroxides, pigment dispersants, foaming agents, foam nucleating agents, plasticizers, crosslinking agents, crosslinking aids, brightness enhancers, antibacterial agents, light diffusing agents, and molecular weight adjusters.

[0107] The propylene resin composition of the present embodiment may contain one kind of these additives alone, or may contain two or more kinds of optional components in any combination at any ratio.

[0108] As the additive (A), an antioxidant, a neutralizing agent, an ultraviolet absorbing agent, and a coloring agent are preferably used. The specific description will be given below. The propylene resin composition of the present embodiment preferably includes a propylene resin composition further containing, in addition to the above components, at least one selected from the group consisting of an organic peroxide, a neutralizing agent, an antioxidant, an ultraviolet absorbing agent, and a coloring agent.

[0109] Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and hydroxylamine-based antioxidants, and preferably the phenol-based antioxidants, phosphorus-based antioxidants, or sulfur-based antioxidants.

[0110] Examples of phenolic antioxidants include 2,6-di-tert-butyl-4-methylphenol, tetrakis[methylene-3(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane (Irganox 1010), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox 1076), 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxo saspiro[5·5]undecane, 1,3,5-tris2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, pentaerythrityl-tetrakis[3-(3,5-di-te rt-butyl-4-hydroxyphenyl)propionate], triethylene glycol-N-bis-3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2-thiobis-diethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2'-methylene-bis-(4-methyl-6-tert-butylphenol), 2,2'-methylene-bis-(4- Ethyl-6-tert-butylphenol), 2,2'-methylene-bis-(4,6-di-tert-butylphenol), 2,2'-ethylidene-bis-(4,6-di-tert-butylphenol), 2,2'-butylidene-bis-(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-tert-amyl-6-(1-(3,5-di-tert-amyl-2-hydroxyphenyl)ethyl)phenyl acrylate, and tocopherols. Examples of tocopherols include vitamin E, which is α-tocopherol. Preferably, 2,6-di-tert-butyl-4-methylphenol, tetrakis[methylene-3(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane (Irganox1010), 2,6-di-tert-butyl-4-methylphenol, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox1076), 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}- 1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, or vitamin E, and more preferably tetrakis[methylene-3(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane (Irganox1010), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox1076), or vitamin E.

[0111] Examples of phosphorus antioxidants include tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite (Irgafos168), distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butyl-6-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-diphenylene diphosphonite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)2-ethylhexylphosphite, 2,2'-ethylidenebis(4,6-di-tert-butylphenyl)fluorophosphite, bis (2,4-di-tert-butyl-6-methylphenyl)ethyl phosphite, 2-(2,4,6-tri-tert-butylphenyl)-5-ethyl-5-butyl-1,3,2-oxaphosphorinane, 2,2',2''-nitrilo[triethyl-tris(3,3',5,5'-tetra-tert-butyl-1,1'-biphenyl-2,2'-diyl)phosphite, 2,4,8,10-tetra-tert-butyl-6-[3-(3-methyl-4-hi Examples of the tert-butyl-2,4-dihydroxy-5-tert-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine include tris(2,4-di-tert-butylphenyl)phosphite (Irgafos 168) and preferably 2,4,8,10-tetra-tert-butyl-6-[3-(3-methyl-4-hydroxy-5-tert-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine.

[0112] Examples of the sulfur-based antioxidant include dilauryl 3,3'-thiodipropionate, tridecyl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, laurylstearyl 3,3'-thiodipropionate, neopentanetetrayltetrakis(3-laurylthiopropionate), and bis[2-methyl-4-(3-n-alkyl(C12-C14)thiopropionyloxy)-5-tert-butylphenyl]sulfide, and preferably dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, or distearyl 3,3'-thiodipropionate.

[0113] The hydroxylamine compound is a compound represented by the following general formula, which forms nitroxyl radicals during the degradation reaction of polymeric materials due to heat and oxygen, thereby suppressing the thermal oxidative degradation of polymeric materials. [ka]

[0114] R of the hydroxylamine compound represented by the above general formula 4 and R 5 is a C12-30 alkyl group, and R 4 and R 5 The alkyl group is preferably a linear alkyl group or an alkyl group substituted with a cyclic alkyl group, more preferably an alkyl group having 12 to 22 carbon atoms, and further preferably a linear saturated alkyl group having 12 to 22 carbon atoms.

[0115] Examples of the linear saturated alkyl group include a linear saturated alkyl group such as a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an eicosyl group, a heneicosyl group, a docosyl group, a tricosyl group, and a tetracosyl group, and preferably a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, and a docosyl group.

[0116] Preferably, at least one selected from the group consisting of phenol-based antioxidants and phosphorus-based antioxidants is used. The above-mentioned various antioxidants may be used alone or in combination of two or more kinds.

[0117] Examples of the neutralizing agent include calcium stearate, hydrotalcite, alkaline earth metal oxides, alkaline earth metal hydroxides, etc. These neutralizing agents may be used alone or in combination of two or more kinds.

[0118] Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, tridiamine-based ultraviolet absorbers, anilide-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, etc. These neutralizing agents may be used alone or in combination of two or more kinds.

[0119] The colorant may be an inorganic pigment or an organic pigment. Examples of inorganic pigments include carbon black, iron oxide, titanium oxide, zinc oxide, red iron oxide, cadmium red, cadmium yellow, ultramarine, cobalt blue, titanium yellow, white lead, red lead, lead yellow, and Prussian blue. Examples of organic pigments include quinacridone, polyazo yellow, anthraquinone yellow, polyazo red, azo lake yellow, perylene, phthalocyanine green, phthalocyanine blue, and isoindolinone yellow.

[0120] The propylene resin composition may contain other additives such as resins and rubbers in addition to the additives already described.

[0121] Examples of other additives (A) include polystyrenes (e.g., polystyrene, poly(p-methylstyrene), poly(α-methylstyrene), AS (acrylonitrile / styrene copolymer) resin), ABS (acrylonitrile / butadiene / styrene copolymer) resin, AAS (special acrylic rubber / acrylonitrile / styrene copolymer) resin, ACS (acrylonitrile / chlorinated polyethylene / styrene copolymer) resin, polychloroprene, chlorinated rubber, polyvinyl chloride, polyvinylidene chloride, acrylic resin, ethylene / vinyl alcohol copolymer resin, fluororesin, polyacetal, grafted polyphenylene ether resin, and polyphenylene sulfide resin. Examples of suitable resins include thermoplastic resins such as polyurethane, polyamide, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate), polycarbonate, polysulfone, polyether ether ketone, polyether sulfone, and aromatic polyester resin, epoxy resin, diallyl phthalate prepolymer, silicone resin, silicone rubber, polybutadiene, 1,2-polybutadiene, polyisoprene, styrene / butadiene copolymer, butadiene / acrylonitrile copolymer, epichlorohydrin rubber, acrylic rubber, and natural rubber, as well as PLA resin (polylactic acid) produced by polymerizing plant-derived monomers extracted from biomaterials.

[0122] At least one of various components such as a propylene-based polymer, an ethylene-α-olefin copolymer, and an inorganic filler, which are used as raw materials in the production of the propylene resin composition, may be recycled.

[0123] Content of each ingredient In the propylene resin composition of the present invention, the content of each component is not particularly limited, provided that the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more. The ratio is preferably 13 or more, 15 or more, 18 or more, or 20 or more. The upper limit of the ratio is not particularly limited, and may be, for example, 200 or less, 150 or less, 100 or less, or 70 or less. All combinations of "any of the above lower limits to any of the above upper limits" are considered to be specified herein.

[0124] When the weight ratio of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more, the propylene resin composition of the present invention and the molded article containing the same (produced from the same) have a large tensile break strain and / or a small mold contamination. When the tensile break strain is large, the molded article is less likely to break sharply, improving safety. The tensile break strain is measured, for example, according to the method described in the Examples. When the metal contamination is small, the number of times the mold is washed can be reduced, and / or the number of molds can be reduced and the life (usage number) of the mold can be extended, reducing the burden on the environment. The mold contamination can be measured, for example, according to the method described in the Examples.

[0125] The content ratio of the propylene polymer (P) relative to 100 parts by weight of the propylene resin composition of the present invention is preferably 50 parts by weight or more, may be 60 parts by weight or more, may be 70 parts by weight or more, may be 80 parts by weight or more, may be 90 parts by weight or more, may be about 100 parts by weight or less, may be 99 parts by weight or less, may be 50 to 95 parts by weight, or may be 60 to 95 parts by weight. When the propylene resin composition of the present invention contains another polymer of component P, the content ratio of the total weight of component P and the other polymer relative to 100 parts by weight of the propylene resin composition may be as described above. The "other polymer" is preferably an ethylene-α-olefin copolymer (E).

[0126] When the propylene resin composition of the present invention contains an ethylene-α-olefin copolymer (E), the content of the ethylene-α-olefin copolymer (E) in the propylene resin composition is usually more than 0 parts by weight and not more than 40 parts by weight, preferably 1 part by weight or more and not more than 40 parts by weight, preferably 5 parts by weight or more and not more than 35 parts by weight, and more preferably 5 parts by weight or more and not more than 30 parts by weight, when the total amount of the propylene resin composition is 100 parts by weight. In one embodiment, the weight ratio of component E to the weight of component P is more than 0 parts by weight and not more than 40 parts by weight, preferably 1 part by weight or more and not more than 40 parts by weight, preferably 5 parts by weight or more and not more than 35 parts by weight, and more preferably 5 parts by weight or more and not more than 30 parts by weight. The above "more than 0 parts by weight" may be replaced with "0 parts by weight or more." In this specification, "0 parts by weight or more" used in relation to the content ratio of an optional component means both an embodiment in which the component is included and an embodiment in which the component is not included.

[0127] The content of the metal deactivator (D) relative to 100 parts by weight of the propylene polymer (P), 100 parts by weight of the total weight of the polymer components, or 100 parts by weight of the propylene resin composition is preferably 10 ppm by weight to 1000 ppm by weight, more preferably 50 ppm by weight to 800 ppm by weight, and even more preferably 80 ppm by weight to 500 ppm by weight. In order to exhibit the metal deactivation effect, the content of component D is preferably equal to or more than the above lower limit. In addition, in order not to adversely affect the hue of the propylene resin composition, the content of component D is preferably equal to or less than the above upper limit.

[0128] The content ratio of the hindered amine light stabilizer (H) relative to 100 parts by weight of the propylene polymer (P), 100 parts by weight of the total weight of the polymer components, or 100 parts by weight of the propylene resin composition is preferably 200 ppm by weight to 10,000 ppm by weight, more preferably 500 ppm by weight to 8,000 ppm by weight, and even more preferably 1,000 ppm by weight to 5,000 ppm by weight. In order for the resin composition of the present invention to have sufficient light resistance stability, the content of component H is preferably equal to or higher than the above lower limit. In addition, in order to prevent component H from bleeding out onto the surface of the molded product, causing whitening of the surface, fuming during molding, and causing mold contamination, the content of component H is preferably equal to or lower than the above upper limit.

[0129] When the polypropylene resin composition of the present invention contains an inorganic filler, the content of the inorganic filler (F) relative to 100 parts by weight of the propylene polymer (P), 100 parts by weight of the total weight of the polymer components, or 100 parts by weight of the propylene resin composition is usually more than 0 parts by weight and not more than 40 parts by weight, preferably 1 part by weight or more and not more than 40 parts by weight, more preferably 5 parts by weight or more and not more than 35 parts by weight, and more preferably 5 parts by weight or more and not more than 30 parts by weight. The above "more than 0 parts by weight" may be replaced with "0 parts by weight or more".

[0130] When the polypropylene resin composition of the present invention contains an antioxidant, the content ratio of the antioxidant relative to 100 parts by weight of the propylene polymer (P) or 100 parts by weight of the total weight of the polymer components is preferably more than 0 parts by weight and 5 parts by weight, preferably 0.001 to 5 parts by weight, more preferably 0.01 to 3 parts by weight, even more preferably 0.05 to 2 parts by weight, and even more preferably 0.1 to 1 part by weight. The above "more than 0 parts by weight" may be replaced with "0 parts by weight or more". In order to improve the rigidity, impact resistance, heat aging resistance, or water resistance, and / or to increase the tensile breaking strain, the content of the antioxidant is preferably not less than the above lower limit. In addition, in order to improve the appearance of the molded product, such as hue and gloss, the content of the antioxidant is preferably not more than the above upper limit. On the other hand, in order to reduce mold contamination, the content of the antioxidant may be 0 to 0.05 parts by weight, 0 to 0.01 parts by weight, 0 to 0.005 parts by weight, or 0 parts by weight (i.e., not included). The mold contamination is measured, for example, according to the method described in the Examples. The water resistance is measured, for example, according to the method described in the Examples.

[0131] Method for producing propylene resin composition The propylene resin composition of the present embodiment can be produced by melt-kneading the components described above. The temperature during melt-kneading may be 180° C. or higher, may be 180° C. to 300° C., or may be 180° C. to 250° C.

[0132] Examples of melt kneading apparatuses for melt kneading to produce the propylene resin composition of the present embodiment include any suitable conventionally known Banbury mixer, single screw extruder, co-rotating twin screw extruder, and counter-rotating twin screw extruder.

[0133] Specific examples of melt kneading apparatuses include ZSK (registered trademark) manufactured by Coperion, TEM (registered trademark) manufactured by Shibaura Machine Co., Ltd., TEX (registered trademark) manufactured by The Japan Steel Works, Ltd., KZW (registered trademark) manufactured by Technovel Co., Ltd., CMP (registered trademark) and TEX (registered trademark) manufactured by The Japan Steel Works, Ltd., and FCM (registered trademark), NCM (registered trademark), and LCM (registered trademark) manufactured by Kobe Steel, Ltd.

[0134] The order of kneading the raw materials is not particularly limited. For example, all the raw materials may be kneaded by being charged into a production device at once, or some of the selected components may be kneaded, and then the obtained kneaded product may be kneaded with other components.

[0135] The properties of the propylene resin composition of the present embodiment are not particularly limited. The propylene resin composition of the present embodiment can be in the form of, for example, a strand (filament), a sheet, a plate, or a pellet. The pellet shape can be produced, for example, by preparing a strand-shaped propylene resin composition and then cutting it to an appropriate length.

[0136] Molded body The present invention also relates to a molded article obtained by molding the propylene resin composition. That is, the propylene resin composition of the present embodiment can be suitably used as a material for forming a molded article. The molded article can be obtained by molding the propylene resin composition by various molding methods. The shape, size, etc. of the molded article may be appropriately determined.

[0137] The propylene resin composition of the present embodiment can be used as a material for molded articles such as, for example, automobile materials, home appliance materials, monitor materials, OA equipment materials, medical materials, drain pans, toiletry materials, food packaging containers, bottles, containers, sheets, films, etc. The propylene resin composition of the present embodiment is difficult to be charged, and can suppress, for example, the adhesion of dirt and the like, so that it can be preferably applied to materials for vehicle-related members, home appliance materials, and food packaging containers such as retort pouches and pouches that can be heated in a microwave oven.

[0138] The propylene resin composition of the present embodiment is particularly preferably used as a material for injection molding.

[0139] Hereinafter, an example of an injection molded article produced by using the propylene resin composition of the present embodiment as an injection molding material will be described.

[0140] The injection molded article is an article molded from the propylene resin composition of the present embodiment. Injection molded articles generally have excellent dimensional stability.

[0141] The injection molded article can be produced by any suitable injection molding method known in the art, such as injection foam molding, supercritical injection foam molding, ultra-high speed injection molding, injection compression molding, gas-assisted injection molding, sandwich molding, sandwich foam molding, and insert-outsert molding.

[0142] The molded article (such as an injection molded article) of this embodiment can be produced by the above-mentioned method in any suitable shape and size according to the application.

[0143] Examples of material applications for vehicle-related components that are injection molded articles include interior parts such as door trims, pillars, instrument panels, consoles, rocker panels, armrests, door panels, and spare tire covers, as well as exterior parts such as bumpers, spoilers, fenders, and side steps, as well as other parts such as air intake ducts, coolant reserve tanks, fender liners, fans, and under-deflectors, as well as integrally molded parts such as front-end panels.

[0144] Examples of home appliance materials include materials for washing machines (outer tubs, inner tubs, lids, pulsators, balancers, etc.), materials for dryers, materials for vacuum cleaners, materials for rice cookers, materials for pots, materials for warmers, materials for dishwashers, and materials for air purifiers. EXAMPLES

[0145] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0146] In the examples and comparative examples, the following raw materials were used.

[0147] Component P: Propylene-based polymer As the component P, the following propylene polymer P1 was prepared.

[0148] (P1) Heterophagic propylene polymer material The heterophasic propylene polymer material was produced by a gas phase polymerization method in the presence of a polymerization catalyst obtained by the method described in Example 1 of JP 2004-182981 A. The physical properties of the obtained component P1 are as follows:

[0149] Melt flow rate (MFR) (230℃, 2.16kg load): 27.5g / 10min (a) Propylene homopolymer component (Polymer I) Intrinsic viscosity: 1.06 dL / g (b) Propylene-ethylene random copolymer component (polymer II) Intrinsic viscosity: 2.8 dL / g Propylene-ethylene random copolymer component ratio: 21.0% by weight Ethylene content in polymer II: 39.0% by weight

[0150] In component P1, the "content of ethylene in polymer II" refers to the content of monomer units derived from ethylene based on the total weight of polymer II.

[0151] Ethylene content in polymer II The ethylene content in polymer II was determined based on the report by Kakugo et al. (Macromolecules, 15, 1150-1152 (1982)) from the 13C-NMR spectrum measured under the following conditions: 13C-NMR spectrum was measured under the following conditions using a sample prepared by uniformly dissolving about 200 mg of heterophasic propylene polymerization material in 3 mL of orthodichlorobenzene in a test tube with a diameter of 10 mm. Measurement temperature: 135℃ Pulse repetition time: 10 seconds Pulse width: 45° Number of times: 2500

[0152] Intrinsic viscosity (unit: dL / g) The intrinsic viscosity is a value measured at a temperature of 135° C. using tetralin as a solvent by the following method.

[0153] Using an Ubbelohde viscometer, the reduced viscosity is measured at three concentrations: 0.1 g / dL, 0.2 g / dL, and 0.5 g / dL. The reduced viscosity is plotted against the concentration, and the intrinsic viscosity is calculated by the extrapolation method in which the concentration is extrapolated to zero. The method for calculating the intrinsic viscosity by the extrapolation method is described, for example, in page 491 of "Polymer Solutions, Polymer Experiments 11" (published by Kyoritsu Publishing Co., Ltd. in 1982).

[0154] Component D: Metal deactivator As component D, the following metal deactivator was prepared.

[0155] (D1) ADEKA STAB CDA-1M: 3-(N-salicyloyl)amino-1,2,4-triazole, manufactured by ADEKA Corporation (D2) ADEKA Corporation ADK STAB CDA-1: 2-Hydroxy-N-1H-1,2,4-triazol-3-ylbenzamide (D3) ADEKA Corporation ADK STAB ZS-19: A composite of melamine resin ((1,3,5-triazine-2,4,6-triamine)H2C=O (formaldehyde)), phenolic compounds, and organic compounds

[0156] Component H: Hindered amine light stabilizer As component H, the following hindered amine light stabilizer was prepared.

[0157] (H1) Uvinul5050H manufactured by BASF Japan Ltd. (H2) ADEKA Corporation ADK STAB LA-52: Tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)=1,2,3,4-butanetetracarboxylate (H3) SABOSTAB UV 119 from SABO SpA: a mixture of: N,N',N'',N'''-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)triazin-2-yl)-4,7-diazadecane-1,10-diamine Polycondensation product of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine

[0158] Component A: Other additives As component A, which is another optional and suitable component, the following components were prepared.

[0159] (A1) Irganox1010 manufactured by BASF Japan Ltd. (A2) Irgfos168 manufactured by BASF Japan Ltd.

[0160] Examples 1 to 7 and Comparative Examples 1 to 4

[0161] Production of propylene resin composition The raw materials having the composition shown in Table 1 were uniformly premixed in a Henschel mixer or a tumbler, and then melt-kneaded using a twin-screw kneading extruder (TEX44αII-49BW-3V type manufactured by The Japan Steel Works, Ltd.) to obtain a pellet-shaped propylene resin composition. [Table 1]

[0162] The melt kneading conditions were a cylinder temperature of 210° C., a screw rotation speed of 200 rpm, a screen mesh of 40 mesh, 80 mesh, and 40 mesh, three sheets stacked together, and an extrusion rate of 50 kg / hr. The evaluation results are shown in Table 1.

[0163] Manufacturing of injection molded products for tensile breaking strain evaluation The pelletized propylene resin composition is mixed with the following materials in the range described in JIS K7152. An injection molded article for evaluating the tensile breaking strain was manufactured by injection molding under the following conditions. The propylene resin composition melted in the injection molding machine was fed from the gate into the mold cavity by the injection molding machine. The measurement results are shown in Table 1. Injection molding machine: Toyo Machinery & Metals Si30III (clamping force 30 tons, cylinder diameter 18 mm) Cylinder temperature: 200℃ Mold temperature: 50℃ Injection speed: 20mm / sec Cooling time: 30 seconds

[0164] Evaluation of mold contamination (mold contamination area) The pelletized propylene resin composition was dried at 100°C for 1 hour, and then injection molded continuously for 60 shots under the following conditions. The molded product was then removed, and a transparent heat-resistant polyester film was attached to the inside of the mold, the mold was clamped, and the mold was removed after being held for 5 seconds. The area of ​​the mold contamination transferred to the film (unit: mm 2 ) was measured using an image analyzer. The smaller the area of ​​the mold-contaminated portion, the less the mold-contamination. Injection molding machine: Toyo Machinery & Metals Si30III (clamping force 30 tons, cylinder diameter 18 mm) Cylinder temperature: 260℃ Mold temperature: 50℃ Injection speed: 40mm / sec Cooling time: 10 seconds

[0165] Color difference evaluation before and after water resistance test The pellet-like propylene resin composition was dried at 100° C. for 1 hour, and then injection molded under the following conditions to produce a plate-like molded product having a length of 80 mm, a width of 35 mm, and a thickness of 2.0 mm. Injection molding machine: Toyo Machinery & Metals Si30III (clamping force 30 tons, cylinder diameter 18 mm) Cylinder temperature: 220℃ Mold temperature: 50℃ Injection speed: 20mm / sec Cooling time: 30 seconds

[0166] One of the obtained flat plate-like molded bodies was placed in a 0.5 L glass bottle, which was then filled with water and sealed with a lid. The molded body was then submerged and fixed in a thermostatic water bath adjusted to 60° C. and left to stand for 1000 hours.

[0167] Then, the glass bottle was taken out of the thermostatic water bath, and the plate-like molded article was taken out and the water on the surface was wiped off.

[0168] The central part of the surface of the plate-shaped molded product was measured using a color difference meter (BYK-mac, manufactured by BYK) with a measurement area of ​​Φ23 mm, lighting of 45 degrees, and a measurement angle of 45 degrees. The value before the water resistance test was used as the standard, and the value after the water resistance test was measured to calculate the color difference ΔE*ab.

[0169] It can be seen from Table 1 that the molded articles according to the examples have a large tensile breaking strain. That is, it was confirmed that the propylene resin composition of the present invention can produce a molded article having a large tensile breaking strain, and that the molded article of the present invention has a large tensile breaking strain.

Claims

1. A propylene resin composition comprising a propylene polymer, a metal deactivator having a triazole skeleton or a triazine skeleton, and a hindered amine light stabilizer having a 2,2,6,6-tetramethylpiperidine skeleton, the propylene-based polymer is a heterophasic propylene polymer material; the metal deactivator is at least one selected from the group consisting of 3-(N-salicyloyl)amino-1,2,4-triazole, 2-hydroxy-N-1H-1,2,4-triazol-3-ylbenzamide, and a melamine resin; the hindered amine light stabilizer is at least one selected from the group consisting of N-(2,2,6,6-tetramethyl-4-piperidyl)maleimide and a copolymer of α-olefin (C20-24), tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)=1,2,3,4-butanetetracarboxylate, N,N',N'',N'''-tetrakis(4,6-bis(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)triazin-2-yl)-4,7-diazadecane-1,10-diamine, and dimethyl succinate / 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate; a weight ratio of the metal deactivator is 10 ppm by weight to 1,000 ppm by weight, and a weight ratio of the hindered amine light stabilizer is 200 ppm by weight to 10,000 ppm by weight, relative to 100 parts by mass of the propylene polymer; the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 10 or more; Propylene resin composition.

2. The propylene resin composition according to claim 1 , wherein the ratio of the weight of the hindered amine light stabilizer to the weight of the metal deactivator is 50 or less.

3. The propylene resin composition according to claim 1, wherein a weight ratio of the propylene-based polymer is 50 parts by weight or more based on 100 parts by weight of the total weight of the propylene resin composition.

4. The propylene resin composition according to claim 1, wherein the propylene resin composition has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more.

5. The propylene resin composition according to claim 1, wherein the propylene polymer has a melt flow rate (measured under conditions of a temperature of 230° C. and a load of 2.16 kgf) of 0.1 g / 10 min or more.

6. The propylene resin composition according to claim 1, further comprising an ethylene-α-olefin copolymer.

7. The propylene resin composition according to claim 6, wherein the weight ratio of the ethylene-α-olefin copolymer is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition.

8. The propylene resin composition of claim 1 further comprising an inorganic filler.

9. The propylene resin composition according to claim 8, wherein the weight ratio of the inorganic filler is 1 part by weight to 40 parts by weight based on 100 parts by weight of the total weight of the propylene resin composition.

10. The propylene resin composition according to claim 1, further comprising an ethylene-α-olefin copolymer and an inorganic filler.

11. A molded article comprising the propylene resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Polypropylene-based resin composition

    JP1991177447A

  • Polypropylene based resin composition

    JP2003105163A

  • Polyurethane elastic yarn and production method therefor

    JP2011144491A

  • Polypropylene resin composition

    JP2014196379A

  • Glass fiber-reinforced polypropylene-based resin composition and molded body of the same

    JP2014208807A