WIRE ELECTRODE FOR SPARK EROSION CUTTING AND METHOD FOR PRODUCING SAME - Patent application
The wire electrode with a core and agglomerated particle coating layer, separated by cracks and zinc oxide, addresses the limitations of existing electrodes by enhancing cutting performance and erosion resistance, ensuring improved surface quality and extended service life.
Patent Information
- Application Number
- JP2021566215
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-10
- Filing Date
- 2020-05-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-05-08
AI Technical Summary
Existing wire electrodes for spark erosion cutting face challenges in achieving high cutting performance while maintaining contour accuracy and surface quality, and are prone to interruptions due to wire wear debris, with limited service life and machine component wear.
A wire electrode with a core surrounded by a coating layer featuring agglomerated particles separated by cracks and a thin top layer of zinc oxide, produced through controlled diffusion annealing to enhance cutting performance and erosion resistance.
The electrode achieves significantly increased cutting performance, improved surface quality, and extended service life, with reduced machine disruptions and enhanced wear resistance, while maintaining contour accuracy.
Smart Images

Figure 0007581240000003 
Figure 0007581240000004 
Figure 0007581240000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a wire electrode for spark-erosion cutting and a method for its production. [Background technology]
[0002] Spark erosion (Electrical Discharge Machining (EDM)) is used to separate conductive workpieces, EDM being based on the removal of material by means of a spark discharge between the workpiece and a tool. For this purpose, a controlled spark discharge is produced between the respective workpiece and the tool in a dielectric liquid, e.g. deionized water or oil, the tool being placed at a short distance from the workpiece and acting as an electrode through the application of a voltage pulse. In this way, workpieces made of e.g. metals, conductive ceramics or composite materials can be machined virtually regardless of their hardness. The electrical energy for the spark discharge is provided by a pulse generator of the erosion machine.
[0003] A special spark erosion method in which the tool is constituted by a tensioned thin wire with a typical diameter in the range of about 0.02-0.4 mm is spark erosion cutting or wire erosion. Since the wire wears during the erosion process as a result of material removal, it has to be continuously stretched through the cutting or machining zone and can only be used once, i.e. the wire is continuously consumed. The desired cutting contour is first performed through a so-called main cut with a relatively high discharge energy. In order to improve the contour accuracy and surface roughness of the workpiece, the main cut can be followed by one or more so-called trimming cuts with successively reduced discharge energies. During these trimming cuts the wire electrode is engaged with only a part of its circumference.
[0004] In practice, both coated and uncoated wire electrodes are used, which are nowadays usually produced on the basis of brass or copper. Uncoated wire electrodes, also called bare wire, consist of a homogeneous material, while coated wire electrodes have a sheath or coated core. In the state of the art, coated wire electrodes are usually constructed such that the core of the wire electrode confers, for example, the necessary tensile strength for wire penetration and wire pretensioning, as well as the necessary electrical and thermal conductivity, while the sheath or sheath, which may consist of one sheath layer or several sheath layers arranged one on top of the other, is involved in the actual erosion process.
[0005] Bare wires typically consist of brass with a zinc proportion of 35-40% by weight, while most coated wires have a copper or brass core and one or more coating layers of zinc or copper-zinc alloy. As materials involved in the actual erosion process, zinc and brass with their low steaming temperature due to the presence of zinc offer the advantages of a relatively high removal rate and efficiency of the erosion process and the possibility of transferring very small pulse energies for fine finishing of the workpiece surface, i.e. machining that produces the smallest possible surface roughness. Against this background, for the purposes of fine finishing, wire electrodes with a coating layer consisting mainly or exclusively of zinc are often used.
[0006] It is known that the removal rate or cutting performance can be increased by using a wire with a coating of pure zinc or mainly pure zinc, compared to bare wire. Furthermore, it is known that a thin top layer, for example of zinc oxide or cadmium oxide, is advantageous for the cutting performance of the wire electrode (see US Pat. No. 4,977,303). Furthermore, it is known that a wire with a coating of brass containing β or β' phase then achieves a higher cutting performance than the aforementioned zinc-coated wire, since the zinc bonds in the β or β' brass alloy are vaporized more slowly compared to pure zinc, and are therefore available to promote removal for a sufficiently long time while the wire passes through the cutting or machining zone. Furthermore, the zinc content of the coating can be further increased using a wire with a coating of the γ and / or ε phase of brass, and in principle the same or higher cutting performance can be achieved compared to the aforementioned wire with a coating of β or β' brass.
[0007] To achieve high cutting performance, it has proven advantageous to produce a coating from a brittle alloy (such as brass in the gamma phase) at a diameter larger than the final diameter, for example through diffusion, and then stretch it to the final dimension by cold forming. As a result, the brittle and hard layer fractures open, resulting in pits and persistent cracks being formed in it and the material located directly below it emerging (see US 5,945,010, US 6,303,523). The cracks and pits increase the surface area of the wire. The latter is thereby better cooled by the surrounding dielectric, and the removal of particles removed from the gap is also facilitated. Apart from that, discharges are preferably formed at the edges produced by the cracks due to the excessive increase in the electric field. This promotes the ignition properties of the wire electrode and therefore the cutting performance.
[0008] This and further developments to increase the cutting performance are also based on the combination of different ones of the mentioned coating layers, optionally with further layers, in a coating construction multilayer. Often, inevitably due to diffusion processes that sometimes occur during the corresponding production process, jackets are also proposed here that have brass coating layers with phase mixtures, for example, of α and β phases, or β and γ phases.
[0009] In US 7,723,635 a wire electrode is proposed having a core and a first coating layer of a brass alloy with about 37-49.5% zinc by weight, in which uniformly distributed so-called agglomerates (spaced apart from one another and comprising a brass alloy with a zinc percentage of about 49.5-58% zinc by weight) are present embedded within the coating layer. With such a wire electrode the erosion properties are improved due to improved electrical conductivity and strength.
[0010] According to EP-A-2193876, at least one of the several coating layers has a fine-grained mixture of mainly β and γ brass. Through the incorporation of the γ brass into the matrix of the β brass, the γ brass will not be worn away as quickly during the erosion process, but will be released in small amounts into the erosion gap in an effective manner from the point of view of removal.
[0011] In EP-A-1846189 a wire electrode is proposed which comprises a first layer of β brass and a split layer of γ brass, within the pores of which the layer of β brass emerges.
[0012] EP-A-2517817 describes a wire electrode with two alloy layers formed by diffusion: the core wire material emerges along cracks in the second alloy layer, as a result of which a multi-grain structure forms on the surface.
[0013] However, in connection with coatings of brittle phases such as the gamma phase, it has been shown that on the one hand an increase in layer thickness does not necessarily lead to a further increase in performance (see EP-A-1295664) and, on the other hand, limits are set for the formability of thicker layers in terms of economic productivity (see US 5,945,010). Furthermore, gamma brass coatings have a higher spark erosive wear than beta brass coatings, as a result of which, in practice, the cutting performance is again frequently reduced.
[0014] Very high cutting performances can be achieved using coated wire electrodes consisting mainly (see EP-A-1295664) or entirely (see EP-A-1455981) of β-brass with a relatively thick layer thickness of, for example, 10-30% of the wire diameter, but only in combination with high-performance settings on the generator side. As a rule, however, this leads to a loss of contour accuracy on the machined components.
[0015] KR-A-10-2007-0075516 discloses, inter alia, a method for producing a wire electrode with a diffusion layer of a predetermined thickness. During the coating of the core wire of copper, copper alloy or copper-plated steel wire by hot dipping, the wire will be prevented from being stretched and therefore the thickness of the diffusion layer formation will be prevented from becoming uncontrollable. In a first step, the core wire of copper, copper alloy or steel is coated with a first metal, which has a lower water vaporization temperature than copper. In order to prevent the wire from stretching during coating, a dimension of 2-4 mm is preferably chosen instead of, for example, a dimension of the core wire of 0.90 mm. In a second step, the coated core wire is heat treated in order to produce an alloy layer due to diffusion. The heat treatment for producing the diffusion layer can alternatively be brought about in the course of coating. In a third step, the wire is drawn. In the fourth step, the wire is again heat treated to continue the diffusion and bring about recrystallization. In the fifth step, the wire is coated with a second metal, which has a lower water vaporization temperature than copper. In the sixth step, the second metal coated wire is drawn, and in the seventh step, the wire is heat treated to stabilize it.
[0016] Object of the Invention It is an object of the present invention to increase the economic viability of wire erosion techniques by further increasing cutting performance and erosion resistance.
[0017] It is a further object of the present invention to not adversely affect or even improve the contour accuracy and surface quality of the machined workpiece by spark erosion, in spite of the increased cutting performance, as compared to bare brass wire.
[0018] Additionally, it is an object of the present invention to provide a coated wire electrode for achieving high cutting performance with the result that the automated threading process can proceed unhindered on the erosion machine even under difficult conditions (e.g., tall workpieces, etc.) while remaining straight and with the greatest possible bending stiffness.
[0019] Furthermore, it is an object of the present invention to provide a coating that is as wear-resistant as possible, so that the erosion process carried out with the wire electrode according to the present invention does not suffer any disruption or impairment due to the deposition of wire wear debris.
[0020] Finally, it is an object of the present invention to provide a wire electrode for achieving high cutting performance with longer life of the wire guides and electrical contacts of the erosion machine as compared to wire electrodes with high cutting performance. [Prior art documents] [Patent documents]
[0021] [Patent Document 1] U.S. Patent No. 7,723,635 [Patent Document 2] European Patent Application Publication No. 2193876 [Patent Document 3] European Patent Application Publication No. 1846189 [Patent Document 4] European Patent Application Publication No. 2517817 [Patent Document 5] European Patent Application Publication No. 1295664 [Patent Document 6] European Patent Application Publication No. 1455981 [Patent Document 7] Korean Patent Publication No. 10-2007-0075516 Summary of the Invention [Means for solving the problem]
[0022] To achieve this object, a wire electrode is used with the features of claim 1. For producing a wire electrode according to the invention, a method is used with the features of claim 23. Advantageous embodiments of the wire electrode are the subject of the respective dependent claims. The present invention provides, for example, the following: (Item 1) 1. A wire electrode for spark erosive cutting, the wire electrode comprising: a core (2) comprising a metal or metal alloy; A coating material (3, 4, 6) surrounding the core (2); having said coating (3, 4, 6) comprising one or more coating layers (3, 4, 6), one of which comprises regions (3) whose morphology corresponds to agglomerated particles, said regions (3) being spatially separated, at least over a portion of their circumference, from each other, from the material of the layers comprising these regions, from the material of one or more further layers and / or from the core material by cracks, 1. A wire electrode, characterized in that, when viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire, more than 50% of the surface area of the region with the agglomerated particle morphology comprises a copper-zinc alloy with a zinc concentration of 38-49% by weight. (Item 2) Item 2. The wire electrode of item 1, wherein there is a thin overlayer on the aggregate particles consisting of greater than 50% by weight zinc oxide at a thickness of 0.05 to 2 μm, the overlayer having areas where the copper-zinc alloy contained within the aggregate particles breaks through onto the surface. (Item 3) 3. The wire electrode of claim 1 or 2, wherein the metal is copper and the metal alloy is a copper-zinc alloy. (Item 4) 4. A wire electrode according to any one of claims 1 to 3, wherein the material of the one or more coating layers and / or the material of the core occurs along the wire circumference between areas with the morphology of the agglomerated particles. (Item 5) 5. The wire electrode according to claim 1, wherein, when viewed in a wire cross section perpendicular or parallel to the wire axis, the portion of more than 50% of the region with lumpy grain morphology comprising a copper-zinc alloy with a zinc concentration of 38-49% by weight is within a portion of the region with lumpy grain morphology radially facing the core. (Item 6) 6. The wire electrode according to any one of claims 1 to 5, wherein, when viewed in a wire cross section perpendicular or parallel to the wire axis, more than 50% of the area with the morphology of agglomerated particles comprises a copper-zinc alloy with a zinc concentration of 40 to 48 wt.%. (Item 7) 7. The wire electrode according to any one of claims 1 to 6, wherein when viewed in a wire cross section perpendicular or parallel to the wire axis, less than 50% of the area with the morphology of agglomerated particles comprises a copper-zinc alloy with a zinc concentration of more than 49-68 wt.%. (Item 8) 8. A wire electrode according to any one of claims 5 to 7, wherein when viewed in a wire cross section perpendicular or parallel to the wire axis, the portion of the region with the morphology of agglomerated grains radially facing the core is more than 60%, in particular more than 80%. (Item 9) 9. The wire electrode according to any one of claims 1 to 8, wherein the regions with the morphology of agglomerated particles contain one or more metals from the group Mg, Al, Si, Mn, Fe, Sn, with a total proportion of 0.01 to 1% by weight relative to the alloy material in these regions. (Item 10) 9. The wire electrode according to any one of claims 1 to 8, wherein the region with the morphology of the agglomerated particles consists only of copper and zinc, excluding unavoidable impurities. (Item 11) 11. The wire electrode according to any one of claims 1 to 10, wherein the extent of the region with the morphology of the agglomerated particles is 1 to 30 μm, in particular 2 to 15 μm, measured in the radial direction of the wire cross section. (Item 12) 12. The wire electrode according to any one of claims 1-11, wherein the coating (3, 4) comprises an inner coating layer region (4), which comprises a copper-zinc alloy with a zinc proportion of 38-58% by weight. (Item 13) 13. The wire electrode according to any one of claims 1 to 12, wherein the coating (3, 4) comprises an inner coating layer region (4), which comprises a copper-zinc alloy with a zinc proportion of 38 to 51% by weight. (Item 14) 14. A wire electrode according to any one of claims 12-13, wherein the boundary between the inner coating layer region (4) of the layers (3, 4) comprising the region (3) whose morphology corresponds to agglomerated particles when viewed in a wire cross section perpendicular to the wire axis and the core (2) or the boundary between the inner coating layer region (4) and one or more further layers arranged between the core and the layers (3, 4) has an irregular, in particular substantially wavy, shape. (Item 15) 15. The wire electrode according to any one of claims 12-14, wherein the coating layer (3, 4) also has a break in the inner region through which the core material or an underlying further coating layer passes in the direction of the outer wire region. (Item 16) 16. The wire electrode according to any one of claims 1-15, wherein the coating (3, 4) has an outer coating layer (6), the outer coating layer (6) consisting of zinc, a zinc alloy, or zinc oxide in the range of at least 50% by weight. (Item 17) 17. A wire electrode according to any one of claims 1 to 16, wherein the regions with the morphology of agglomerated particles contain zinc oxide over part of their circumference, from each other, from the material of the layer comprising them, from the material of one or more further layers and / or along the cracks (7) that spatially separate them from the core material. (Item 18) 18. The wire electrode according to any one of claims 1-17, wherein the region (3) with the morphology of agglomerated particles has internal cracks (7'). (Item 19) Item 19. A wire electrode as described in item 18, wherein zinc oxide is present along the cracks (7'). (Item 20) 20. The wire electrode according to any one of claims 1-19, wherein the core (2) is formed from copper or a copper-zinc alloy with a zinc content of 2 to 40% by weight. (Item 21) 21. A wire electrode according to any one of claims 2 to 20, wherein the aggregated particles, when viewed perpendicular to the wire surface, have regions with a layered structure, in which lamellae formed from the upper layer consisting of zinc oxide in the range of more than 50% by weight and lamellae formed from the material of the aggregated particles are arranged next to each other in an alternating manner. (Item 22) 22. A wire electrode according to claim 21, wherein the width of the lamella formed from the material of the agglomerated particles is less than 5 μm, preferably less than 3 μm. (Item 23) A method for producing a wire electrode (1) according to any one of claims 1-22, in which a core (2) containing copper or brass is coated with zinc at a first diameter, and a wire with a brittle and hard coating layer consisting mainly of gamma brass is formed through a first diffusion annealing. and the wire is drawn to a second diameter, as a result of which the layer of gamma brass splits and regions (3) result with a morphology corresponding to agglomerated grains, said regions (3) being spatially separated by cracks, at least over a part of their circumference, from each other, from the material of the layer comprising them, from the material of one or more further layers and / or from the core material, and the wire is then subjected to a second diffusion annealing, as a result of which a major portion, i.e. a major portion of more than 50% of said regions with the morphology of agglomerated grains, has a zinc content of 38 to 49% by weight. (Item 24) 24. The method of producing a wire electrode (1) according to claim 23, wherein the wire is subjected to the second diffusion annealing in the presence of oxygen, whereby a top layer comprising zinc oxide in the range of more than 50% by weight arises on the agglomerated particles, and then the wire is optionally subjected to a multi-step drawing process, whereby the top layer of zinc oxide splits and the material of the agglomerated particles emerges in the pores. (Item 25) 24. The method for producing a wire electrode (1) according to item 23, wherein the first diffusion annealing is carried out at an annealing temperature of 180-300°C with an average heating rate of at least 80°C / h and an average cooling rate of at least 60°C / h for 2-8 hours, and the second diffusion annealing is carried out at an annealing temperature of 300-520°C with an average heating rate of at least 100°C / h and a cooling rate of at least 80°C / h for 4-24 hours. (Item 26) 25. A method for producing a wire electrode (1) according to claim 24, wherein a total cross-sectional reduction of the wire in the range of 60-85% is effected throughout the drawing process after the second diffusion annealing, and if a multi-step drawing process is performed, a cross-sectional reduction in the range of 8-12% is effected in each drawing step. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 shows, diagrammatically, not to scale, a cross section (perpendicular to the longitudinal axis) of a first embodiment of a wire electrode according to the invention. [Diagram 2] FIG. 2 shows a detailed cutaway view of a cross section of a first embodiment of a wire electrode 1 according to the invention according to FIG. [Diagram 3] FIG. 3 shows a detailed cutaway view of a cross section (perpendicular to the longitudinal axis) of a second embodiment of a wire electrode according to the present invention. [Figure 4]FIG. 4 shows a detailed cutaway view of a cross section (perpendicular to the longitudinal axis) of a third embodiment of a wire electrode according to the present invention. [Diagram 5] FIG. 5 shows a scanning electron microscopy (SEM) photograph of the surface of a first embodiment of a wire electrode according to the invention. [Figure 6] FIG. 6 shows a detailed cutaway view of a cross section (perpendicular to the longitudinal axis) of a fourth embodiment of a wire electrode according to the present invention. [Figure 7] FIG. 7 shows an SEM photograph (backscattered electrons 20 kV) of a peripheral cutout of a wire electrode according to the invention in a cross section perpendicular to the longitudinal axis of the wire. [Figure 8] FIG. 8 shows an SEM photograph (backscattered electrons 20 kV) of the surface of a further embodiment of a wire electrode according to the invention with a magnification of 300. [Figure 9] FIG. 9 shows an SEM photograph (backscattered electrons 5 kV) of the surface of a further embodiment of a wire electrode according to the invention with a magnification of 1,000. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] According to the invention, it is assumed that a wire electrode for spark erosive cutting has a core comprising a metal or metal alloy. The core preferably consists of one or more metals and / or one or more metal alloys to the extent of more than 50% by weight, more preferably completely or substantially completely. In particular, the core can therefore be formed completely of one metal or one metal alloy. The core can be formed homogeneously or, for example, in the form of several individual metal or metal alloy layers of different compositions arranged one on top of the other and have radially varying properties. As used herein, "substantially" means that the wire according to the invention, or its layers or its core, respectively, consists of the disclosed composition and / or has the disclosed properties, and production and measurement tolerances will take into account, for example, the presence of unavoidable impurities familiar to the expert.
[0025] The metal is in particular copper, and the metal alloy is in particular a copper-zinc alloy.
[0026] Surrounding the core is provided an outer jacket (hereinafter also called "cladding"), for example in the form of a coating, which comprises one or more layers of coating material. The coating material is provided such that it wears off during the wire erosion process and influences the erosion characteristics. In the case of several coating layers, the several coating layers are arranged radially one on top of the other, each coating material preferably extending around the core.
[0027] One of the coating layers of the wire electrode according to the invention comprises areas with a grain-like appearance (morphology), characterized in particular by irregular contours, including (when viewed in a wire cross section perpendicular or parallel to the wire longitudinal axis) sometimes sharp angles with a corner radius of less than 2 μm and lines with a straightness that deviates from an ideal straight line by less than 2 μm. These areas are therefore described as areas whose morphology corresponds to agglomerated or agglomerated particles. These areas are also referred to below as "areas with agglomerated morphology" or for short as "agglomerated particles" (or "agglomerated particles"). The material of adjacent layers and / or the core material adjacent or radially further inward may pass between the agglomerated particles. The agglomerated particles are additionally spatially separated from each other, from the material of the layer comprising these areas, from the material of the adjacent layers and / or from the core material by cracks over at least a part of their circumference. The agglomerated particles themselves may also contain cracks.
[0028] The cracks generally have a width of up to about 2 μm, mainly about 1 μm, as can be determined by analysis of images measured under normal conditions, for example, based on backscattered electrons (20 kV), using scanning electron microscopy. If larger crack widths appear along the course of the crack over short distances (for example, 1-2 μm), this structure is likewise considered a crack within the meaning of the present invention. By way of comparison, wider spaces between agglomerated particles (usually formed radially inwards from the outer surface of the wire) are called pits or gaps.
[0029] Along the cracks, but also along the depressions and gaps, zinc oxide can be formed depending on the mode of production of the wire according to the invention, which can reduce the width of the crack or sometimes completely fill its volume, but this likewise entails the consequence that it can be revealed by means of suitable scanning electron microscopy recording techniques, and that the morphology of the agglomerate-shaped particles determined by the crack formation can in this case also be recognized.
[0030] When viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire (also referred to herein as the "longitudinal wire axis" or simply "wire axis" for short), the major portion, i.e., more than 50% of the surface area of the aggregated particles, comprises a copper-zinc alloy with a zinc concentration of 38-49% by weight. According to the phase diagram for the CuZn system, the alloy is present in this portion of the surface area partly or mainly as β and / or β' phase. Less than 50% of the surface area of the aggregated particles comprises a copper(-zinc) alloy with a zinc concentration of 49-68% by weight or more. According to the phase diagram for the CuZn system, the alloy is present in this portion of the surface area as β+γ phase and / or as γ phase.
[0031] If an agglomerated particle is not completely separated from its surroundings by a crack, the surface area used to determine the composition of the particle is defined by taking as limit the shortest straight connecting line between the ends of the crack (partially) separating the particle from its surroundings, the end closest to the wire center in the radial direction (and therefore the radially innermost) being chosen. This is shown by way of example in Figures 6 and 7, which are referred to herein within the framework of this definition.
[0032] If a particle is separated from its surroundings not only by a crack but also by a cavity (gap), the connecting line between the crack end and the radially innermost point of the nearest cavity (gap) seen from one crack end is selected, which is likewise shown by way of example in FIG. 7, which is referred to here within the framework of this definition.
[0033] Preferably, at least some of the agglomerated particles according to the invention, when viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire (as defined above), are completely separated from their surroundings, i.e. from each other, from the material of the layer which comprises them, from the material of one or more layers and / or from the core material, by cracks.
[0034] With regard to the existence of the β / β' phase, it is noted that below a certain temperature the β' phase is stable and has an ordered lattice with defined lattice sites for copper and zinc, above which it transitions to the unordered β phase (atoms are statistically distributed on the lattice sites of a body-centered cubic lattice). Since, according to the prevailing opinion, the transformation between the β and β' phases cannot be suppressed and has only a minor effect on its mechanical and electrical properties, a general reference to the β phase always means also the β' phase within the framework of this application, unless a distinction is made explicitly.
[0035] Furthermore, it should be pointed out that the agglomerated particles may have multiple agglomerates in the metallurgical sense.
[0036] The agglomerated particles may contain zinc oxide over part of their circumference, along the cracks and gaps that spatially separate them from each other, from the material of the layer in which they are comprised, from the material of adjacent layers and / or from the (adjacent) core material, and along the cracks that the agglomerated particles themselves contain.
[0037] The copper-zinc alloy containing the agglomerated particles may contain, in addition to copper and zinc, one or more metals from the group Mg, Al, Si, Mn, Fe, Sn with a total proportion of 0.01 to 1% by weight.
[0038] The thickness of the agglomerated particles is preferably 1 to 30 μm when measured in the radial direction of the wire cross section.
[0039] The wire electrode may additionally have a thin overlayer, which consists essentially of Zn, a Zn alloy, or ZnO, for example, at a thickness of about 0.05 to 1 μm.
[0040] According to a further embodiment of the invention, there may additionally be a thin top layer on the agglomerated particles, e.g., about 0.05-2 μm thick, comprising predominantly zinc oxide, i.e. in the range of more than 50% by weight, said top layer having areas ("pores") within which the material of the agglomerated particles, i.e. one of the copper-zinc alloys contained within the agglomerated particles, emerges.
[0041] When viewed perpendicularly (radially) to the wire surface, these regions have a layered structure such that lamellae formed from a top layer containing zinc oxide and lamellae formed from the material of the agglomerated particles are arranged one after the other in an alternating manner. Such regions are represented by way of example in Figures 8 and 9.
[0042] By lamellar we mean a structure that is usually characterized by platelets or lamellae, which are located in a structure of this type of homogeneously arranged parallel or radial structural elements (platelets / lamellae). In this embodiment of the wire electrode according to the invention, the lamellar structure areas are not arranged strictly parallel, and the distance between the individual lamellae may also vary. Nevertheless, for an expert in this field, what is meant by lamellar is clear. In this respect a comparison can be made with the known lamellar graphite, which describes the most common type of cast iron in which the graphite is present in the form of thin irregularly shaped lamellae.
[0043] The layered structural elements appearing as whitish lighter areas in Figures 8 and 9 consist of agglomerated particulate material. The layered regions appearing as greyish darker areas consist of an upper layer of (mainly) zinc oxide.
[0044] The dimensions of the layered structures (hereinafter also called "lamellae" for short) are as follows:
[0045] The width of the lamellae formed from the agglomerated particulate material is less than 5 μm, preferably less than 3 μm, and even more preferably less than 2 μm. The length of the lamellae can be up to 50 μm. The width of the lamellae can vary over their length. These specifications relate to the lamellae formed from the agglomerated particulate material and appear as whitish lighter areas in Figures 8 and 9.
[0046] The lamellae formed from the agglomerated material can be partially connected to one another by strips, as a result of which a network made from the agglomerated material is formed on the wire surface.
[0047] 50×50 μm in SEM photographs (backscattered electrons 20 kV) in a top view on the wire along its longitudinal axis (i.e., in a view as shown in FIGS. 8 and 9). 2 For a unit area, the lamellae formed from the agglomerated particle material may account for up to 50%.
[0048] The metals contained within the core and coating may have unavoidable impurities.
[0049] According to the state of the art, it was expected that a wire electrode with a fractured and open layer consisting mainly of the γ-phase would lead to a higher cutting performance due to a higher zinc concentration compared to a layer with a comparable topography consisting mainly of the β-phase. However, it has surprisingly been shown that by using the wire electrode according to the invention, the cutting performance and the erosive wear resistance can be substantially increased at the same time compared to previously known wires.
[0050] The cracks that spatially separate the agglomerated particles, at least over part of their circumference, from each other, from the material of the layer containing them, from the material of the adjacent layers and / or from the (adjacent) core material, as well as the cracks that the agglomerated particles themselves may contain, promote a significant increase in the electric field and therefore the ignitability of the electrode. Through their high spark erosion wear resistance due to a zinc content of 38-49% by weight in their main part, the agglomerated particles can contribute to a higher ignitability over a longer duration. This effect is clearly noticeable, especially when the wire electrode according to the invention is used in the first two trimming cuts, because the agglomerated particles are effective from the point of view of removal for an even longer time due to the discharge energy that is continuously reduced compared to the main cut.
[0051] Cooling of the wire electrode is also generally improved due to the increased surface area caused by the cracked layer.
[0052] Zinc oxide on the surface formed by cracks and depressions (gaps) that spatially separate the agglomerated particles from each other, from the material of the layer containing them, from the material of adjacent layers and / or from the (adjacent) core material over part of their circumference, and zinc oxide on the surface formed by cracks contained in the agglomerated particles themselves, leads to a further increase in cutting performance.
[0053] In addition, the cutting performance is also increased by the zinc oxide top layer having pores through which the agglomerated material emerges. In particular, a layered surface structure as defined above in which lamellae formed from a top layer mainly comprising zinc oxide and lamellae formed from the agglomerated material are arranged adjacent to each other in an alternating manner has a beneficial effect on the cutting performance.
[0054] The thickness of the agglomerated particles, measured in the radial direction of the wire cross section perpendicular to the longitudinal axis, is advantageously in the range of 1 to 30 μm. In the case of thicker particles, there is a risk that the entire particle will break off due to insufficient bonding to the adjacent wire core or to the adjacent coating layer. This can lead to short circuits and thus to an impairment of the contour accuracy and surface quality of the eroded components. In the case of thicknesses below 1 μm, the positive effects of ignition and cooling action are no longer sufficiently given. The thickness of the agglomerated particles, measured in the radial direction of the wire cross section, is more preferably 2 to 15 μm, even more preferably 3 to 10 μm.
[0055] The coating layer can be applied to the core, for example, using a suitable coating method, optionally in combination with a heat treatment method. The application of the coating layer can be effected, for example, physically or electrochemically, and can optionally be followed by a step to reduce the wire diameter. Thus, for example, Cu, CuZn with a diameter of 1.20 mm. 20 , or CuZn 37 It is possible to proceed from an initial material in the form of a wire (coated with Zn, for example, by electrodeposition or by hot dipping) of (brass with 20 or 37% by weight zinc). The Zn-coated wire is then subjected to diffusion annealing, producing a coating layer, which at least in part has a continuous and homogeneous partial layer of, in particular, gamma brass. The zinc content in this part of the coating layer is therefore 58-68% by weight. In a next step, the wire is tapered to an intermediate or final dimension, preferably by cold forming. Here, the brittle and hard layer of brass in the gamma phase splits, as a result of which agglomerated particles are formed. The agglomerated particles are spatially separated from one another, as a result of which the material of adjacent layers and / or the (adjacent) core material can appear between the agglomerated particles. The agglomerated particles themselves can also contain cracks.
[0056] The wire is then subjected to a further diffusion annealing, so that the major portion, i.e. more than 50% of the agglomerated particles, has a zinc content of 38-49% by weight. The composition determination is carried out with reference to a wire cross section viewed perpendicularly or parallel to the wire axis. The particle surface area viewed is therefore as defined above.
[0057] The portion of the aggregate particle with the composition according to the invention is preferably in the region of the aggregate particle radially facing the core. Less than 50% of the aggregate particle portion comprises a copper alloy with a zinc concentration of more than 49-68% by weight. Due to the diffusion of zinc from the aggregate particle into the adjacent material, a diffusion layer with a zinc content of 38-58% by weight is formed. The size of the portion of the aggregate particle with a zinc content of 38-49% by weight can be influenced via the intensity of the annealing, i.e. temperature and duration.
[0058] The two diffusion annealings can be carried out in a stationary manner, for example in a hood-type furnace, and in a continuous process, for example by resistance heating. The first diffusion annealing can be carried out, for example in a hood-type furnace, under ambient atmosphere or protective gas, preferably in the range of 180-300 ° C for 4-12 hours, the average heating rate being preferably at least 80 ° C / h and the average cooling rate being preferably at least 60 ° C / h. It can alternatively be brought about in a continuous passage under ambient atmosphere or protective gas, for example by resistance heating, the average heating rate being preferably at least 10 ° C / s, the maximum wire temperature being preferably 600-800 ° C, the annealing time being preferably in the range of 10-200 seconds and the average cooling rate being preferably at least 10 ° C / s. The above annealing times relate to the period from leaving room temperature to reaching room temperature again. The second diffusion annealing can be carried out, for example, in a hood-type furnace, under ambient atmosphere or protective gas, preferably in the range of 300-520 ° C, for 4-24 hours, the average heating rate being preferably at least 100 ° C / h and the average cooling rate being preferably at least 80 ° C / h. Alternatively, it can be effected, for example, by resistive heating, in a continuous passage under ambient atmosphere or protective gas, the average heating rate being preferably at least 10 ° C / s, the maximum wire temperature being preferably 350-600 ° C, the annealing time being preferably in the range of 10-200 s and the average cooling rate being at least 10 ° C / s. The above annealing times relate to the period from the time of leaving room temperature to the time of reaching room temperature again. Due to the annealing under ambient atmosphere or in the presence of oxygen, a thin upper layer, mainly of zinc oxide, as defined above with a thickness of 0.05-2 μm can be produced on the wire surface and on the surface formed by cracks and gaps.
[0059] Optionally, another one or more further steps of coating with zinc and / or one or more further diffusion annealing processes can now follow before the wire is drawn to its final dimensions. The wire can be drawn before, during or after one of the cooling processes described above. The wire is preferably transformed to the desired final dimensions by cold drawing. As a result, further cracks can occur in the agglomerated particles and the surrounding coating layer.
[0060] Through appropriate selection of the total cross-sectional reduction during conventional multi-step cold drawing of the wire to the final dimension and through appropriate selection of the cross-sectional reduction at each drawing step, the formation of a layered or net-like surface structure can be achieved, in which lamellae formed mainly from the zinc oxide-containing top layer and lamellae formed from the agglomerated particulate material are arranged adjacent to each other in an alternating manner. The formation of such a surface structure is promoted by a total cross-sectional reduction of 60-85%. Moreover, the formation of such a surface structure is also promoted by a cross-sectional reduction of 8-12% at each drawing step.
[0061] Cold drawing can optionally be followed by a so-called stress relief annealing to ensure that the wire's straightness, tensile strength and elongation are affected. The stress relief annealing can be effected, for example, by resistive heating, inductively or by thermal radiation.
[0062] In a preferred embodiment, at least one coating layer is formed, which comprises agglomerated particles according to the invention, which are spatially separated, at least over a portion of their circumference, from each other, from the material of the adjacent coating layers and / or from the (adjacent) core material, such that, when viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire, the major portion, i.e. more than about 50% of the surface area (as defined above) of the agglomerated particles, preferably comprises a copper-zinc alloy with a zinc concentration of 38-49% by weight, more preferably 40-48% by weight, this portion of the surface area being in particular in the region of the agglomerated particles radially facing the core.
[0063] Preferably, this surface area fraction is greater than about 60%, more preferably, greater than about 80%, and even more preferably, about 100%.
[0064] In a further preferred embodiment, at least a portion of the amount of agglomerated particles are completely spatially separated (as defined herein, when viewed in a wire cross section) from each other, from the material of the layer comprising these particles, from the material of one or more further layers, and / or from the core material by cracks.
[0065] The copper-zinc alloy containing the lump particles preferably contains, in addition to Cu and Zn, one or more metals from the group Mg, Al, Si, Mn, Fe, Sn with a total proportion of 0.01-1 wt. %. More preferably, the copper-zinc alloy containing the lump particles consists only of copper and zinc and unavoidable impurities.
[0066] In a further preferred embodiment, the outer cladding layer comprises agglomerated particles, which are spatially separated from each other, from the material of the adjacent cladding layer and / or from the (adjacent) core material, at least over a part of their circumference. When viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire, the main part of this embodiment, i.e. the part of the surface area (as defined above) of the agglomerated particles amounting to more than 50%, comprises a copper-zinc alloy with a zinc concentration of 38-49% by weight, this part of the surface area being in particular in the region of the agglomerated particles radially facing the core. According to the phase diagram for the CuZn system, the alloy is present in this part of the surface area partly or mainly as β and / or β' phase ...γ phase. The adjacent inner cladding layer preferably comprises a copper alloy with a zinc percentage of 38-58% by weight. According to the phase diagram for the CuZn system, the alloy is present in this part partially or mainly as β-phase or as β+γ-phase. More preferably, the inner cladding layer comprises a copper-zinc alloy with a zinc percentage of 38-51% by weight. The adjacent layer differs from the outer cladding layer through its topography in that the outer cladding layer and its boundary to the core or to the further cladding layer located immediately below have a substantially wavy shape. The adjacent inner cladding layers are preferably continuous. However, they can also have breaks, through which the core material or the further cladding layer located immediately below passes.
[0067] In a further preferred embodiment, a further cladding layer, preferably of a copper-zinc alloy having a zinc concentration of 0.1-40% by weight, is arranged under said inner cladding layer.
[0068] In a further multi-layer design, the coating can have, for example, an outer coating layer, preferably in the form of an overlayer forming a part or the entire outer surface of the coating layer, the outer coating layer being formed, preferably completely or substantially completely, to the extent of at least 50% by weight, of zinc, zinc alloy or zinc oxide. The thickness of this overlayer can be 0.05 to 1 μm. Such an outer coating layer is advantageous for cutting performance with low discharge energy and in the framework of fine finishing processes, since zinc is then more rapidly available.
[0069] The layered or network structure described above has been found to be particularly suitable for increasing cutting performance as compared to an overlayer of zinc oxide which is continuous over a larger cross section.
[0070] A thin overlayer of zinc oxide is preferably formed through a second diffusion anneal, e.g., under ambient atmosphere, over a portion of their circumference, on the surfaces formed through the cracks that spatially separate the agglomerated particles from each other, from the material of adjacent layers, and / or from the (adjacent) core material, and on the surfaces formed by the cracks that the agglomerated particles themselves contain. Thus, in addition to the known overlayer of zinc oxide, further zinc oxide is available for the erosion process to increase removal.
[0071] The core is preferably formed mainly, preferably completely or substantially completely, from copper or a copper-zinc alloy with a zinc content of 2 to 40% by weight. Such a core is advantageously easily cold formable.
[0072] The structure and composition of the wire electrode according to the invention can be determined, for example, using scanning electron microscopy (SEM) investigations with energy dispersive X-ray spectroscopy (EDX). For this, the surface and cross-section polishing of the wire electrode are investigated. The production of the wire cross-section polishing can be brought about, for example, by the so-called ion beam oblique sectioning method, in which the wire is covered by a screen and irradiated with Ar +The wire is bombarded with ions and material is removed from the portion of the wire that protrudes beyond the screen by the ions. Through this method, samples can be prepared without mechanical deformation. The structure of the coating layer of the wire electrode according to the invention is therefore preserved through such preparation. The structure of the coating layer of the wire electrode according to the invention can therefore be represented by SEM images. Using point, line and surface EDX analysis, the composition of the wire electrode according to the invention can be determined.
[0073] The invention will now be explained in further detail with reference to the following drawings.
[0074] The wire electrode 1 shown in cross section in FIG. 1 has a wire core 2, which is completely surrounded by a coating 3, 4 formed on the outside of the wire electrode 1. In the illustrated exemplary embodiment, the core 2 is completely or substantially completely homogeneously formed from copper or a copper-zinc alloy, preferably with a zinc content of 2-40% by weight. The outer coating layer 3, 4 comprises agglomerated particles, which are spatially separated from each other or from the material 4, for example by cracks (not shown). In terms of the surface area of the agglomerated particles, the main part comprises a copper alloy with a zinc concentration of 38-49% by weight. According to the phase diagram for the CuZn system, the alloy is present in this part partially or mainly as β and / or β' phase.
[0075] The adjacent inner cladding layer regions 4 consist of a copper alloy with a zinc proportion of 38-51% by weight. According to the phase diagram for the CuZn system, the alloy is present in this region partly or mainly as β-phase. This adjacent layer region may have a border to the core or to a further cladding layer (not shown), which has an approximately wavy shape. The adjacent inner cladding layer regions are formed continuously around the circumference in this embodiment.
[0076] Figure 2 shows a detailed cutaway view of a cross section of a first embodiment of a wire electrode 1 according to the invention according to Figure 1, with the wire core 2 and the outer coating layers 3, 4. The more precise shape of the agglomerated or agglomerated particles, the fact that they are separated by cracks over part of their circumference or over their entire circumference (when viewed in this cross section) from each other or from the adjacent material 4 of the coating layer, and the approximately wavy boundary of the inner region 4 of the coating layer relative to the core 2 are discernible.
[0077] Figure 3 shows a detailed cutaway view of a cross section of a second embodiment of a wire electrode according to the invention, with a wire core 2 and outer coating layers 3, 4. Unlike the first embodiment according to Figure 2, the inner coating layer region 4 is interrupted at several points, whereby the core wire threads through at these points on the surface of the wire electrode.
[0078] FIG. 4 shows a detailed cutaway view of a cross section of a third embodiment of a wire electrode according to the invention, with a wire core 2 and outer coating layers 3, 4, 5. In terms of the surface area of the agglomerated particle, the main part consists of a copper-zinc alloy with a zinc concentration of 38-49% by weight, which part is in the region of the agglomerated particle radially facing the core in this embodiment. According to the phase diagram for the CuZn system, the alloy is present in this part partly or mainly as β and / or as β' phase. The outer region 5 of the agglomerated particle has a zinc content of 49-68% by weight or more. According to the phase diagram for the CuZn system, the alloy is present in this part as β+γ and / or as γ phase.
[0079] 5 shows a scanning electron microscopy photograph of the surface of a first embodiment of a wire electrode according to the invention. Agglomerated particles and cracks and pits (gaps) in the outer coating layer are visible.
[0080] All of the embodiments depicted in Figures 1-5 may have a thin top layer on the agglomerated particles (see Figure 6), which forms part or all of the outer surface of the coating layer 6. This layer is formed from or consists of zinc, zinc alloys, and zinc oxide in the range of at least 50% by weight or more. The thickness of this top layer is up to 0.05 to 1 µm or up to 2 µm. The top layer may have pores into which the material of the agglomerated particles emerge.
[0081] As depicted in Figure 6, the agglomerated particles may contain zinc oxide over at least a portion of their circumference, along the cracks and gaps (7) that spatially separate them from the material of the adjacent layers and / or from the adjacent core material, and along the cracks (7') that the agglomerated particles themselves contain. Based on scanning electron microscopy analysis, in a cross section parallel to the longitudinal axis or transverse to the wire, if the agglomerated particle is not completely separated from the material of the adjacent layers or from the core material by a crack, in order to define the surface area of the agglomerated particle, it must be separated by the shortest straight line connection between the end points (a, b) of the cracks (7) that surround it, located closest to the center of the wire in the radial direction (see Figure 6).
[0082] 7 is an SEM photograph (backscattered electrons 20 kV) of a cut-out of the circumference of a wire electrode according to the invention in a cross section perpendicular to the longitudinal axis of the wire. Lump-shaped particles separated from one another over at least a part of their circumference by cracks are visible. The straight connecting lines ab and a'-b' each illustrate how the surface area of particles comprising a copper alloy with a zinc concentration in the range of 38-49% by weight, in these cases more than 50%, is determined.
[0083] If the particle is not completely separated from its surroundings by a crack, the surface area is determined by choosing as the boundary the shortest straight line connecting the ends of the cracks that separate the particle from the surroundings that are radially inwards towards the wire center. For the particle that can be seen on the left side of Figure 7, this is the connecting line ab, according to the determination method already explained with reference to Figure 6. The straight line connection from one crack end to the "adjacent" (closest) crack end is therefore chosen.
[0084] The grain on the right side of the photograph is separated from its surroundings to the right by a dimple, in this case the connecting line between the crack end and the radially innermost point of the nearest dimple (gap) is selected.
[0085] Figures 8 and 9 show SEM photographs (backscattered electrons 20 kV and 5 kV, respectively) of the surface of a further embodiment of a wire electrode according to the invention with magnifications of 300 and 1,000, respectively. By means of color contrast, areas with layered structure (8) are discernible. The lamellae formed from the agglomerated particulate material appear as white lighter areas. In contrast, the lamellae formed mainly from the upper layer containing zinc oxide appear as grey darker areas. The black areas represent cracks and pits.
[0086] (Example) The advantages of the wire electrode according to the invention in comparison with different wire electrodes according to the state of the art are explained below with reference to two example embodiments: The production of wire samples was brought about according to the sequence depicted below.
[0087] Comparison sample V1: -Initial wire: CuZn37, d=1.20mm - Stretching to d=0.25mm and stress relief annealing
[0088] Comparison sample V2: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - Stretching up to d=0.50mm - Diffusion annealing in a hood furnace at 400°C for 12 hours under ambient air - Stretching to d=0.25mm and stress relief annealing
[0089] Comparison sample V3: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - Stretching up to d=0.50mm - Diffusion annealing in a hood furnace at 180°C for 6 hours under ambient air - Stretching to d=0.25mm and stress relief annealing
[0090] Comparison sample V4: -Initial wire: CuZn20, d=1.20mm Electrodeposition of zinc with -40μm - Stretching up to d=0.60mm - First diffusion annealing at 180°C for 6 hours under ambient atmosphere in a hood-type furnace - A second diffusion annealing under ambient air in continuous passes with a heating rate >10°C / s, maximum wire temperature 680°C, annealing time 15 seconds, and a cooling rate >10°C / s - Stretching to d=0.25mm and stress relief annealing
[0091] Sample E1 according to the invention: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - A first diffusion annealing in a hood-type furnace under ambient air at 180°C for 6 hours with an average heating rate of 100°C / h and an average cooling rate of 80°C / h. - Stretching up to d=0.50mm - A second diffusion annealing in a hood-type furnace under ambient air at 400°C for 12 hours with an average heating rate of 160°C / h and an average cooling rate of 140°C / h. - Stretching to d=0.25mm and stress relief annealing
[0092] Sample E2 according to the invention: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - A first diffusion annealing in a hood-type furnace under ambient air at 180°C for 6 hours with an average heating rate of 100°C / h and an average cooling rate of 80°C / h. - Stretching up to d=0.60mm - A second diffusion annealing in a hood-type furnace under ambient air at 400°C for 12 hours with an average heating rate of 160°C / h and an average cooling rate of 140°C / h. - Stretching to d=0.25mm and stress relief annealing
[0093] Sample E3 according to the invention: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - A first diffusion annealing in a hood-type furnace under ambient air at 180°C for 6 hours with an average heating rate of 100°C / h and an average cooling rate of 80°C / h. - Stretching up to d=0.70mm - A second diffusion annealing in a hood-type furnace under ambient air at 410°C for 12 hours with an average heating rate of 160°C / h and an average cooling rate of 140°C / h. - Stretching to d=0.25 mm with 18% cross-sectional reduction at each stretching step and subsequent stress relief annealing
[0094] Sample E4 according to the invention: -Initial wire: CuZn37, d=1.20mm Electrodeposition of zinc with -10μm - A first diffusion annealing in a hood-type furnace under ambient air at 180°C for 6 hours with an average heating rate of 100°C / h and an average cooling rate of 80°C / h. - Stretching up to d=0.40mm - A second diffusion annealing in a hood-type furnace under ambient air at 410°C for 12 hours with an average heating rate of 160°C / h and an average cooling rate of 140°C / h. - Stretching to d=0.25 mm with 10% cross-sectional reduction at each stretching step and subsequent stress relief annealing
[0095] The relative cutting performance achieved with each wire electrode in the case of spark erosion machining in the main cut and machining with the main cut and three trimming cuts is shown in Table 1. Spark erosion machining was effected on a commercial wire erosion system using deionized water as the dielectric. A 50 mm high workpiece of hardened cold work steel of type X155CrVMo12-1 was machined. A square with an edge length of 15 mm was selected as the cutting profile. The technique present on the machine side for bare brass wire with composition CuZn37 was selected as the machining technique. [Table 1]
[0096] The cutting performance achieved with comparative sample V1 in the main cut, the main cut and the three trimming cuts was set to 100% in each case. Comparative sample V2 has a continuous closed coating layer of β-brass. Compared to comparative sample V1, the cutting performance is increased by 8% and 10%, respectively. Comparative sample V3 has a coating layer consisting of agglomerated particles. The agglomerated particles consist mainly of γ-brass. In this comparative sample, the cutting performance is increased by 10% and 12%, respectively, compared to comparative sample V1. Comparative sample V4 has an inner coating layer of β-brass and an outer coating layer of a fine-grained agglomerated phase mixture of β-brass and γ-brass. The thickness of the zinc layer on the initial wire of comparative sample 4 is four times greater than the thickness of the zinc layer on the starting wire of comparative samples V2 and V3 and samples E1 and E2 according to the invention. In comparative sample V4, the cutting performance is increased by 19% and 24%, respectively, compared to comparative sample 1.
[0097] Sample E1 according to the invention has a coating layer with an inner continuous zone of brass with a zinc content of 39-43% by weight and outwardly directed agglomerated grains that are spatially separated from each other or from the material of the coating layer by cracks and pits (gaps) over at least a portion of their circumference, these grains having a zinc content of 43-48% by weight. The thickness of the agglomerated grains, measured radially on the wire cross section, is 5-11 μm. A portion of the coating layer is surrounded by an upper layer, which consists essentially entirely of zinc oxide. The thickness of this upper layer is 0.05-0.5 μm. Furthermore, the sample contains zinc oxide along the surface formed by the pits (gaps) and cracks and on the surface formed by the cracks contained in the agglomerated grains themselves. In sample E1 according to the invention, the cutting performance is increased by 43% and 26%, respectively, compared to comparative sample 1. Despite the same zinc layer thickness, after electrochemical coating on the starting material, the increase in cutting performance for this sample is much greater than for comparative samples V2 and V3. The cutting performance is even higher than for comparative sample V4, whose zinc layer is four times thicker than sample E1 according to the invention.
[0098] Sample E2 according to the invention has a coating layer with an inner continuous area of brass with a zinc content of 39-43% by weight and outwardly directed agglomerated grains that are spatially separated, partially or completely, from each other or from adjacent material of the coating layer by cracks and depressions (gaps), these grains having a zinc content of 43-48% by weight. A part of the outer surface of the coating layer is surrounded by an upper layer, which is formed substantially entirely of zinc oxide. The thickness of this upper layer is 0.05-0.5 μm. Furthermore, the sample contains zinc oxide along the surface formed by the gaps and cracks and on the surface formed by the cracks contained in the agglomerated grains themselves. Due to the larger intermediate dimension (d=0.60 mm) compared to sample E1 according to the invention, the first produced coating layer, mainly of gamma brass, is less significantly split and cracked. Since the gamma brass is transformed into beta brass in the second diffusion annealing process, the brittleness of the agglomerated particles is reduced, so that the surface structure of the sample E2 according to the invention is less cracked and the thickness of the agglomerated particles is more uniform, despite the larger deformation in the second drawing process. The thickness of the agglomerated particles is 9-11 μm, measured radially on the wire cross section. In the sample E2 according to the invention, the cutting performance is increased by 40% and 28%, respectively, compared to the comparative sample V1.
[0099] Sample E3 according to the invention has a coating layer with an inner continuous zone of brass with a zinc content of 39-43% by weight and outwardly directed agglomerated grains that are spatially separated from each other or from the material of the coating layer by cracks and pits (gaps) over at least a part of their circumference, these grains having a zinc content of 43-48% by weight. The thickness of the agglomerated grains, measured radially on the wire cross section, is 5-11 μm. A part of the coating layer is surrounded by an upper layer, which consists mainly of zinc oxide. The thickness of this upper layer is 0.05-2 μm. Furthermore, the sample contains zinc oxide along the surface formed by the pits (gaps) and cracks and on the surface formed by the cracks contained in the agglomerated grains themselves. In sample E3 according to the invention, the cutting performance is increased by 37% and 24%, respectively, compared to comparative sample 1.
[0100] Sample E4 according to the invention has a coating layer with an inner continuous area of brass with a zinc content of 39-43% by weight and outwardly directed agglomerated grains that are spatially separated from one another, partially or completely, or from the adjacent material of the coating layer, by cracks and recesses (gaps), these grains having a zinc content of 43-48% by weight. A part of the outer surface of the coating layer is surrounded by a top layer, which is formed substantially completely from zinc oxide. The thickness of this top layer is 0.05-2 μm.
[0101] Due to the smaller cross-sectional reduction during the final drawing process compared to sample E3, sample E4 has areas on the surface with a layered structure, such that lamellae formed from the top layer comprising zinc oxide and lamellae formed from the material of the aggregate particles comprising copper-zinc alloy are arranged adjacent to each other in an alternating manner.
[0102] Furthermore, sample E4 contains zinc oxide along the surface formed by the gaps and cracks and on the surface formed by the cracks contained in the agglomerated particles themselves. The thickness of the agglomerated particles, measured radially on the wire cross section, is 9-11 μm. In sample E4 according to the invention, the cutting performance is increased by 42% and 28%, respectively, compared to comparative sample V1.
[0103] Due to the more uniform surface structure and thickness of the agglomerated particles, a better surface roughness is achieved with samples E2 and E3 according to the invention compared to samples E1 and E4 (see Table 2). a The value is even smaller than for bare brass wire (V1). [Table 2]
[0104] Samples E1-E4 according to the invention have a much smaller total coating layer thickness than sample V4, which promotes the straightness and bending stiffness of the wire electrode, so that the automated threading process can proceed unhindered on the erosion machine, even under difficult conditions, e.g., with tall workpieces.
[0105] Overall, the coating layers of Samples E1-E4 according to the invention are more ductile and softer than Comparative Samples V3 and V4 due to the primary or complete conversion of gamma brass to beta brass, and therefore behave more wear resistant while proceeding on the wire erosion system, and as a result the process is less susceptible to disruption or impairment due to the accumulation of wire wear debris.
[0106] Additionally, longer life of the wire guides and electrical contacts of the erosion machine is achieved through the coating layer being overall more ductile and softer compared to comparative samples V3 and V4.
[0107] (Reference Number) 1: Wire electrode 2: Wire core 3: Agglomerated particles 4: Adjacent cladding layers 5: Outer region of the clumped particle 6: Upper layer 7: Cracks surrounding agglomerated particles 7': Internal cracks in agglomerated particles 8: Region with layered structure on the wire surface
[0108] (References) No. US4,977,303 No. US5,945,010 No. US6,303,523 No. US7,723,635 No. EP-A2193876 No. EP-A1846189 No. EP-A2517817 No. EP-A1295664 No. EP-A1455981 No. KR-A10-2007-0075516
Claims
1. 1. A wire electrode for spark erosive cutting, the wire electrode comprising: a core (2) comprising a metal or metal alloy; A coating material (3, 4, 6) surrounding the core (2); having the coating (3, 4, 6) comprises one or more coating layers (3, 4, 6), one of the one or more coating layers (3, 4, 6) comprising a plurality of regions (3), the morphology of which corresponds to a plurality of agglomerated particles, the agglomerated particles being spatially separated, at least over a portion of their circumference, from one another, from the material of the layer comprising these regions, from the material of one or more further layers and / or from the core material by a plurality of cracks, 1. A wire electrode, characterized in that, when viewed in a wire cross section perpendicular or parallel to the longitudinal axis of the wire, more than 50% of the surface area of a region having the morphology of agglomerated particles comprises a copper-zinc alloy having a zinc concentration of 38% to 49% by weight.
2. A wire electrode as described in claim 1, wherein a thin overlayer consisting of greater than 50 weight% zinc oxide in the range of 0.05 μm to 2 μm thick is present on said plurality of lumpy particles, said overlayer having a plurality of regions on a surface of said wire electrode through which the copper-zinc alloy contained within said plurality of lumpy particles has passed.
3. The wire electrode of claim 1 or 2, wherein the metal is copper and the metal alloy is a copper-zinc alloy.
4. A wire electrode as described in any one of claims 1 to 3, wherein the material of one or more coating layers and / or the core material appears along the circumference of the wire between a plurality of regions having the form of a plurality of agglomerated particles.
5. 5. A wire electrode as claimed in any one of claims 1 to 4, wherein, when viewed in a wire cross section perpendicular or parallel to the wire axis, more than 50% of the regions having the morphology of a plurality of agglomerated particles comprise a copper-zinc alloy having a zinc concentration of 40% to 48% by weight.
6. 6. A wire electrode as claimed in any one of claims 1 to 5, wherein when viewed in a wire cross section perpendicular or parallel to the wire axis, less than 50% of the regions having the morphology of a plurality of agglomerated particles comprise a copper-zinc alloy having a zinc concentration of from 49% to greater than 68% by weight.
7. 7. A wire electrode according to claim 1, wherein the regions having the form of a plurality of agglomerated particles comprise one or more metals from the group Mg, Al, Si, Mn, Fe, Sn, with a total proportion of 0.01% to 1% by weight relative to the alloy material in these regions.
8. The wire electrode according to any one of claims 1 to 6, wherein the regions having the form of a plurality of agglomerated particles consist only of copper and zinc, excluding unavoidable impurities.
9. 9. A wire electrode according to claim 1, wherein the extent of the regions having the form of agglomerated particles is between 1 μm and 30 μm, in particular between 2 μm and 15 μm, measured in the radial direction of the wire cross section.
10. A wire electrode as described in any one of claims 1 to 9, wherein the coating material (3, 4) of the wire electrode has an inner coating material layer region (4), the inner coating material layer region (4) comprising a copper-zinc alloy having a zinc proportion of 38% to 58% by weight.
11. A wire electrode as described in any one of claims 1 to 10, wherein the coating material (3, 4) of the wire electrode has an inner coating material layer region (4), the inner coating material layer region (4) comprising a copper-zinc alloy having a zinc proportion of 38% to 51% by weight.
12. 12. A wire electrode according to claim 10, wherein the boundary between the inner coating layer region (4) of the layer (3, 4) comprising the plurality of regions (3) whose morphology corresponds to a plurality of agglomerated particles when viewed in a wire cross section perpendicular to the wire axis and the core (2) or the boundary between the inner coating layer region (4) and one or more further layers arranged between the core and the layer (3, 4) has an irregular shape, in particular an approximately wavy shape.
13. 13. A wire electrode according to any one of claims 10 to 12, wherein the coating layers (3, 4) also have breaks in the inner region through which the core material or an underlying further coating layer passes in the radial direction of the wire cross section.
14. A wire electrode as described in any one of claims 1 to 13, wherein the coating material (3, 4) of the wire electrode has an outer coating material layer (6), the outer coating material layer (6) consisting of zinc, a zinc alloy or zinc oxide in an amount of at least 50% by weight.
15. 15. A wire electrode according to claim 1, wherein the regions having the form of agglomerated particles contain zinc oxide over part of their circumference, and along the cracks (7) which spatially separate them from one another, from the material of the layer comprising them, from the material of one or more further layers and / or from the core material.
16. A wire electrode according to any one of the preceding claims, wherein the regions (3) in the form of agglomerated particles have a plurality of internal cracks (7').
17. 17. A wire electrode as claimed in claim 16, wherein zinc oxide is present along said internal cracks (7').
18. The wire electrode according to any one of the preceding claims, wherein the core (2) is made of copper or the core (2) is made of a copper-zinc alloy having a zinc content of 2% to 40% by weight.
19. A wire electrode as described in any one of claims 2 to 18, wherein a scanning electron microscopy (SEM) photograph of the surface of the wire electrode shows (1) a plurality of regions that appear white in which the lamellae are formed from the top layer consisting of zinc oxide in the range of greater than 50% by weight, and (2) a plurality of regions that appear gray in which the lamellae are formed from the material of the plurality of agglomerated particles.
20. 20. A wire electrode as claimed in claim 19, wherein the width of the lamella formed from the material of the plurality of agglomerated particles is less than 5 μm, preferably less than 3 μm.
21. 21. A method for producing a wire electrode according to any one of claims 1 to 20, characterized in that a core (2) comprising copper or brass is coated with zinc in a first diameter, a wire having a brittle and hard coating layer mainly consisting of gamma brass is formed through a first diffusion annealing, this wire is drawn to a second diameter, as a result of which the layer of gamma brass splits and a plurality of regions (3) arise having a morphology corresponding to a plurality of agglomerated shaped particles, said plurality of regions (3) being spatially separated, at least over a portion of their circumference, from one another, from the material of the layer comprising them, from the material of one or more further layers and / or from the core material by a plurality of cracks, and the wire is then subjected to a second diffusion annealing, as a result of which a major portion, i.e. a major portion of more than 50% of said plurality of regions having the morphology of said agglomerated particles, has a zinc content of 38% to 49% by weight.
22. 22. The method of claim 21, wherein the wire is subjected to the second diffusion anneal in the presence of oxygen, whereby an overlayer comprising zinc oxide in the range of greater than 50% by weight occurs on the plurality of agglomerated particles, and the wire is then optionally subjected to a multi-step drawing process, whereby the overlayer of zinc oxide splits and material of the plurality of agglomerated particles emerges in a plurality of pores created by the multi-step drawing process.
23. 22. The method of claim 21, wherein the first diffusion annealing is effected at an annealing temperature of 180° C. to 300° C. for a period of 2 to 8 hours with an average heating rate of at least 80° C. / hr and an average cooling rate of at least 60° C. / hr, and the second diffusion annealing is effected at an annealing temperature of 300° C. to 520° C. for a period of 4 to 24 hours with an average heating rate of at least 100° C. / hr and a cooling rate of at least 80° C. / hr.
24. 23. The method of claim 22, wherein a total cross-section reduction of the wire in the range of 60% to 85% is effected throughout the drawing process after the second diffusion annealing, and if a multi-step drawing process is performed, a cross-section reduction in the range of 8% to 12% is effected at each drawing step.
Citation Information
Patent Citations
Wire electrode for electric-discharge machining
EP1295664A1
Wire for high-speed electrical discharge machining
EP1455981A2
Composite wire for electrical discharge machining
EP1846189A1
Motor spindle with a previous fixed bearing
EP2193876A1
Electrode wire for electro-discharge machining and method for manufacturing the same
EP2517817A2