Rubber composition and tire

The rubber composition addresses the issue of silica-induced hardness by using a multicomponent copolymer and inorganic compound to improve wet grip and wear resistance in tires.

JP7581631B2Active Publication Date: 2024-11-13SUMITOMO RUBBER INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020030539
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-26
Publication Date
2024-11-13
Estimated Expiration
2040-02-26

AI Technical Summary

Technical Problem

High silica filling in rubber compositions leads to decreased dispersibility and increased hardness, compromising wet grip performance and wear resistance due to brittle fracture.

Method used

A rubber composition containing a multicomponent copolymer with conjugated diene, non-conjugated olefin, and aromatic vinyl units, combined with a specific inorganic compound and silica filler, optimized to maintain polymer flexibility and enhance interaction with silica.

Benefits of technology

Improves both wet grip performance and wear resistance by balancing silica content and polymer interaction, preventing hardening and enhancing abrasion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581631000001
    Figure 0007581631000001
Patent Text Reader

Abstract

To provide rubber compositions that can achieve general improvement in wet grip performance and wear resistance, and tires including the rubber compositions.SOLUTION: A rubber composition has a rubber component that has a multi-component copolymer including a conjugated diene unit, a non-conjugated olefin unit and an aromatic vinyl unit, and an inorganic filler that has an inorganic compound represented by the formula (1) and silica with a BET specific surface area of 150 m2 / g or more. In 100 mass% of the rubber component, the multi-component copolymer content is 30 mass% or more, and the inorganic filler content is 80-170 pts.mass with respect to 100 pts.mass of the rubber component, and the silica content>the inorganic compound content. mM xSiOy zH2O (1) (where M is at least one metal selected from the group consisting of Al, Mg, Ti, Ca and Zr, or an oxide or a hydroxide of the metal, m is an integer of 1-5, x is an integer of 0-10, y is an integer of 2-5, and z is an integer of 0-10).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and a tire. [Background technology]

[0002] Among tire performances, wet grip performance is particularly important because it is directly related to safety, and various studies have been conducted to improve wet grip performance. For example, Patent Document 1 discloses that wet grip performance is improved by using fine silica particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-140613 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a rubber composition is highly loaded with silica (particularly finely divided silica), the number of double bonds in the polymer bound by the silica increases, and the dispersibility of the silica in the rubber composition deteriorates, which may harden the rubber composition and cause brittle fracture, resulting in a decrease in abrasion resistance.

[0005] An object of the present invention is to provide a rubber composition that can solve the above problems and improve the overall performance of wet grip performance and abrasion resistance, and a tire using the same. [Means for solving the problem]

[0006] The present invention relates to a rubber component containing a multicomponent copolymer containing a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit, an inorganic compound represented by the following formula (1), and a rubber composition having a BET specific surface area of ​​150 m 2 / g or more of an inorganic filler containing silica, wherein a content of the multicomponent copolymer in 100% by mass of the rubber component is 30% by mass or more, a content of the inorganic filler is 80 to 170 parts by mass per 100 parts by mass of the rubber component, and a content of the silica>a content of the inorganic compound. mM xSiOy zH2O (1) (In the formula, M is at least one metal selected from the group consisting of Al, Mg, Ti, Ca and Zr, or an oxide or hydroxide of the metal, m is an integer of 1 to 5, x is an integer of 0 to 10, y is an integer of 2 to 5, and z is an integer of 0 to 10.)

[0007] The rubber composition preferably satisfies the relationship of the following formula (A). (Inorganic filler content) 2 / 3 / (Inorganic filler content + Carbon black content) 2 / 3 ≧0.90 (A)

[0008] The rubber composition preferably contains a silane coupling agent, and the content of the silane coupling agent is preferably 1 to 5 parts by mass per 100 parts by mass of the total content of the silica and other silica.

[0009] The multicomponent copolymer is preferably a hydrogenated styrene-butadiene rubber, and the hydrogenated styrene-butadiene rubber preferably has a hydrogenation rate of 50 mol % or more, a weight average molecular weight of 2000 or more, and a styrene content of 25 to 40 mass %.

[0010] The rubber composition preferably satisfies the relationship of the following formula (B). Resin content / Silane coupling agent content>2.0 (B)

[0011] The rubber composition preferably has a sulfur content of 0.8 mass % or less.

[0012] The rubber composition preferably satisfies the relationship of the following formula (C). (Oil content + resin content) / inorganic filler content≦1.0 (C)

[0013] The content of the multi-component copolymer in 100% by mass of the rubber component is preferably 30 to 60% by mass.

[0014] The inorganic compound is preferably aluminum hydroxide.

[0015] The present invention also relates to a tire having a tread using the above rubber composition. Effect of the Invention

[0016] The present invention relates to a rubber component containing a multi-component copolymer containing a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit, an inorganic compound represented by formula (1), and a rubber composition having a BET specific surface area of ​​150 m 2 / g or more of an inorganic filler containing silica, the content of the multicomponent copolymer is 30% by mass or more in 100% by mass of the rubber component, the content of the inorganic filler is 80 to 170 parts by mass per 100 parts by mass of the rubber component, and the content of the silica is greater than the content of the inorganic compound, so that the overall performance of wet grip performance and abrasion resistance can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The rubber composition of the present invention comprises a rubber component containing a multicomponent copolymer containing conjugated diene units, non-conjugated olefin units and aromatic vinyl units, an inorganic compound represented by formula (1) and a carboxylic acid having a BET specific surface area of ​​150 m 2 / g or more of an inorganic filler containing silica, a content of the multicomponent copolymer is 30% by mass or more in 100% by mass of the rubber component, a content of the inorganic filler is 80 to 170 parts by mass per 100 parts by mass of the rubber component, and the content of the silica is greater than the content of the inorganic compound.

[0018] The reason why the above rubber composition improves the overall performance of wet grip performance and abrasion resistance is not clear, but is presumed to be as follows.

[0019] As mentioned above, when a rubber composition is highly filled with silica (particularly fine silica), the rubber composition hardens, and there is concern that the wear resistance will decrease due to brittle fracture. However, in the rubber composition, the inorganic compound represented by formula (1) is contained in a smaller amount than the silica, so that the chemical bonds of the polymer are appropriately cut and the polymer is softened. In addition, the rubber composition contains the multi-component copolymer, which has little interaction with silica, in the rubber component, so that the hardening of the rubber composition is suppressed. Due to these actions, it is believed that the rubber composition can obtain good wear resistance while enjoying the effect of improving wet grip performance by highly filling inorganic fillers such as silica.

[0020] The rubber composition contains, as a rubber component, a multicomponent copolymer including conjugated diene units, non-conjugated olefin units and aromatic vinyl units.

[0021] The multicomponent copolymer may be in a solid state or a liquid state at room temperature (25° C.), but is preferably in a solid state.

[0022] In the multicomponent copolymer, the conjugated diene unit is a constituent unit derived from a conjugated diene compound, and examples of the conjugated diene compound include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethylbutadiene, 2-phenyl-1,3-butadiene, 1,3-hexadiene, etc. These may be used alone or in combination of two or more kinds, with 1,3-butadiene and isoprene being preferred, and 1,3-butadiene being more preferred.

[0023] In the multicomponent copolymer, the non-conjugated olefin unit is a structural unit derived from a non-conjugated olefin, and examples of the non-conjugated olefin include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, etc. These may be used alone or in combination of two or more kinds, with ethylene, propylene, and 1-butene being preferred, and ethylene being more preferred.

[0024] In the above multicomponent copolymer, the aromatic vinyl unit is a constituent unit derived from an aromatic vinyl compound, and examples of the aromatic vinyl compound include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene, 2,4,6-trimethylstyrene, etc. These may be used alone or in combination of two or more kinds, but styrene and α-methylstyrene are preferred, and styrene is more preferred.

[0025] The multicomponent copolymer can be prepared, for example, by a method of copolymerizing a conjugated diene compound, a non-conjugated olefin, and an aromatic vinyl compound, or by a method of copolymerizing a conjugated diene compound and an aromatic vinyl compound, or a conjugated diene compound, a non-conjugated olefin, and an aromatic vinyl compound, and then converting a part of the conjugated diene units to non-conjugated olefin units by hydrogenation. That is, the multicomponent copolymer may be a copolymer of a conjugated diene compound, a non-conjugated olefin, and an aromatic vinyl compound, or a copolymer of a conjugated diene compound, a non-conjugated olefin, and an aromatic vinyl compound, or a hydrogenated copolymer (hydrogenated copolymer) of a copolymer of a conjugated diene compound, a non-conjugated olefin, and an aromatic vinyl compound. These may be used alone or in combination of two or more. Among them, a hydrogenated copolymer of a conjugated diene compound and an aromatic vinyl compound is preferred, and a hydrogenated styrene-butadiene copolymer (hydrogenated SBR) is more preferred.

[0026] In preparing the multicomponent copolymer, the polymerization method is not particularly limited, and may be random polymerization or block polymerization, with random polymerization being preferred.

[0027] When the multicomponent copolymer is a hydrogenated copolymer such as hydrogenated SBR, the hydrogenation method and reaction conditions are not particularly limited, and hydrogenation may be performed by a known method and under known conditions. Usually, hydrogenation is performed at 20 to 150°C under a hydrogen pressure of 0.1 to 10 MPa in the presence of a hydrogenation catalyst. Other production methods and conditions are also not particularly limited, and for example, the contents described in the above-mentioned International Publication No. 2016 / 039005 can be applied.

[0028] When the multi-component copolymer is a hydrogenated copolymer, the hydrogenation rate is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 65 mol% or more, and is preferably 95 mol% or less, more preferably 85 mol% or less, and even more preferably 80 mol% or less, based on 100 mol% of the total conjugated diene units before hydrogenation. When it is within the above range, the effect tends to be better obtained. The hydrogenation rate is 1 It can be calculated from the spectral reduction rate of the unsaturated bond part of the spectrum obtained by measuring H-NMR.

[0029] In 100% by mass of the multicomponent copolymer, the content of the conjugated diene unit is preferably 4% by mass or more, more preferably 9% by mass or more, even more preferably 14% by mass or more, and is preferably 60% by mass or less, more preferably 45% by mass or less, even more preferably 30% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0030] In 100% by mass of the multicomponent copolymer, the content of the non-conjugated olefin unit is preferably 10% by mass or more, more preferably 25% by mass or more, even more preferably 35% by mass or more, particularly preferably 40% by mass or more, and is preferably 66% by mass or less, more preferably 61% by mass or less, and even more preferably 56% by mass or less. Within the above range, the effect tends to be better obtained.

[0031] In 100% by mass of the multicomponent copolymer, the content of aromatic vinyl units is preferably 25% by mass or more, more preferably 30% by mass or more, and is preferably 40% by mass or less, more preferably 35% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0032] The contents of the conjugated diene unit, the non-conjugated olefin unit, and the aromatic vinyl unit in the multicomponent copolymer are as follows: 1 H-NMR, 13 It can be measured by C-NMR, etc.

[0033] The weight average molecular weight (Mw) of the multicomponent copolymer is preferably 2000 or more, more preferably 10,000 or more, even more preferably 100,000 or more, and particularly preferably 200,000 or more, and is preferably 1,000,000 or less, more preferably 750,000 or less, and even more preferably 500,000 or less. Within the above ranges, the effect tends to be better obtained. The weight average molecular weight (Mw) can be determined by standard polystyrene conversion based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation). In the case of a copolymer having a modifying group, the modifying group interacts with the silica gel of the column, making it impossible to obtain an accurate Mw, so the Mw is measured before the modification treatment is carried out.

[0034] The content of the multicomponent copolymer in 100% by mass of the rubber component is 30% by mass or more, preferably 35% by mass or more, more preferably 40% by mass or more, and preferably 60% by mass or less, more preferably 50% by mass or less. When it is within the above range, the effect tends to be better obtained.

[0035] In the rubber composition, examples of rubber components that can be used other than the multi-component copolymer include diene rubbers such as natural rubber (NR), styrene butadiene rubber (SBR), butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), and styrene-isoprene-butadiene copolymer rubber (SIBR). These may be used alone or in combination of two or more. Among these, SBR is preferred.

[0036] The SBR is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. Commercially available products include those from Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc.

[0037] The styrene content of the SBR is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, and is preferably 60% by mass or less, and more preferably 50% by mass or less. Within the above ranges, the effect tends to be better obtained. The styrene content of SBR is: 1 It can be measured by H-NMR.

[0038] The vinyl content of the SBR is preferably 25% by mass or more, more preferably 35% by mass or more, and even more preferably 46% by mass or more, and is preferably 60% by mass or less, and more preferably 50% by mass or less. Within the above range, the effect tends to be better obtained. The vinyl content (amount of 1,2-bonded butadiene units) of SBR can be measured by infrared absorption spectroscopy.

[0039] The amount of SBR in 100% by mass of the rubber component is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and further preferably 60% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0040] The rubber component may be either a non-modified rubber or a modified rubber. The modified rubber may be any rubber having a functional group that interacts with a filler such as silica, and examples thereof include terminally modified rubber (terminally modified rubber having the above-mentioned functional group at the terminal) in which at least one terminal of the rubber has been modified with a compound (modifying agent) having the above-mentioned functional group, main chain modified rubber having the above-mentioned functional group in the main chain, main chain terminal modified rubber having the above-mentioned functional group in the main chain and at least one terminal (for example, main chain terminal modified rubber having the above-mentioned functional group in the main chain and at least one terminal modified with the above-mentioned modifier), and terminally modified rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.

[0041] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.

[0042] Specific examples of compounds (modifiers) having the above-mentioned functional groups include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and the like.

[0043] The rubber composition contains an inorganic compound represented by the following formula (1) as an inorganic filler. mM xSiOy zH2O (1) (In the formula, M is at least one metal selected from the group consisting of Al, Mg, Ti, Ca and Zr, or an oxide or hydroxide of the metal, m is an integer of 1 to 5, x is an integer of 0 to 10, y is an integer of 2 to 5, and z is an integer of 0 to 10.)

[0044] In formula (1), M is preferably Al, an oxide of Al, or a hydroxide of Al, and more preferably a hydroxide of Al. m is preferably 1 to 3, and more preferably 1. x is preferably 0 to 3, and more preferably 0. y is preferably 0 to 3, and more preferably 0.

[0045] Specific examples of the inorganic compound represented by formula (1) include alumina, alumina hydrate, aluminum hydroxide, magnesium hydroxide, talc, titanium white, titanium black, calcium oxide, calcium hydroxide, calcium aluminum oxide, clay, pyrophyllite, bentonite, aluminum silicate, calcium silicate, calcium aluminum silicate, magnesium silicate, zirconium, zirconium oxide, etc. These may be used alone or in combination of two or more. Among them, aluminum hydroxide is preferred.

[0046] The content of the inorganic compound represented by formula (1) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less. When it is within the above range, the effect tends to be better obtained.

[0047] The rubber composition contains an inorganic filler having a BET specific surface area of ​​150 m 2 Contains more than 1 / g of silica (fine particle silica). Examples of silica include dry silica (anhydrous silicic acid) and wet silica (hydrated silicic acid), but wet silica is preferred because it has a large number of silanol groups. Commercially available products include those from EVONIK, Tosoh Silica, SOLVAY, Tokuyama, OSC SIAM SILICA, etc. These may be used alone or in combination of two or more.

[0048] The BET specific surface area of ​​the fine silica particles is 150m 2 / g or more, but preferably 160m 2 / g or more, more preferably 170m 2 / g or more, more preferably 180m 2 / g or more, and preferably 220m 2 / g or less, more preferably 210m 2 / g or less, more preferably 200m 2 Within the above range, there is a tendency for the effect to be better obtained. The BET specific surface area of ​​silica is a value measured by the BET method in accordance with ASTM D3037-81.

[0049] The content of the fine particle silica is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 100 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 150 parts by mass or less, more preferably 130 parts by mass or less, and even more preferably 120 parts by mass or less. Within the above range, the effect tends to be better obtained.

[0050] In the rubber composition, the content of the fine particle silica (content (parts by mass) relative to 100 parts by mass of the rubber component) is greater than the content of the inorganic compound represented by formula (1) (content (parts by mass) relative to 100 parts by mass of the rubber component). This makes it possible to prevent the chemical bonds of the polymer from being excessively broken by the inorganic compound represented by formula (1).

[0051] The content of fine particle silica-content of inorganic compound is preferably 60 parts by mass or more, more preferably 90 parts by mass or more, even more preferably 105 parts by mass or more, and is preferably 145 parts by mass or less, more preferably 135 parts by mass or less. When it is within the above range, the effect tends to be better obtained.

[0052] The rubber composition contains, in addition to the fine silica particles, another silica (having a BET specific surface area of ​​150 m 2 The BET specific surface area of ​​the other silica is preferably 50 to 120 m 2 / g.

[0053] The content of the inorganic filler (total content of the inorganic compound represented by formula (1), fine silica particles, and other inorganic fillers) is 80 to 170 parts by mass, preferably 100 parts by mass or more, more preferably 125 parts by mass or more, still more preferably 135 parts by mass or more, and preferably 165 parts by mass or less, based on 100 parts by mass of the rubber component. When it is within the above range, the effect tends to be better obtained.

[0054] The rubber composition preferably contains a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, Examples of such silanes include sulfide-based silanes such as bamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those from EVONIK, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.

[0055] The content of silane coupling agent is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 4 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and particularly preferably 5 parts by mass or less, based on 100 parts by mass of silica content (total content of fine silica and other silica).When it is within the above range, the effect tends to be better obtained.

[0056] The rubber composition preferably contains carbon black. The carbon black is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.

[0057] The nitrogen adsorption specific surface area (N2SA) of the carbon black is preferably 50 m 2 / g or more, more preferably 75m 2 / g or more, and preferably 120m 2 / g or less, more preferably 100m 2 / g or less, more preferably 90m 2 Within the above range, there is a tendency for the effect to be better obtained. The nitrogen adsorption specific surface area of ​​carbon black is determined by Method A of JIS K6217.

[0058] The dibutyl phthalate (DBP) oil absorption of the carbon black is preferably 50 ml / 100 g or more, more preferably 80 ml / 100 g or more, even more preferably 102 ml / 100 g or more, and is preferably 200 ml / 100 g or less, more preferably 170 ml / 100 g or less, even more preferably 140 ml / 100 g or less. Within the above ranges, the effect tends to be better. The DBP oil absorption of carbon black is measured in accordance with JIS K6217-4:2001.

[0059] The amount of carbon black is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.

[0060] In the rubber composition, the contents (parts by mass) of the inorganic filler and carbon black per 100 parts by mass of the rubber component preferably satisfy the relationship of the following formula (A), which is believed to increase the probability of interaction between the inorganic filler and the polymer during compounding, thereby improving the effects of improving abrasion resistance and wet grip performance. (Inorganic filler content) 2 / 3 / (Inorganic filler content + Carbon black content) 2 / 3 ≧0.90 (A)

[0061] In formula (A), (content of inorganic filler) 2 / 3 / (Inorganic filler content + Carbon black content) 2 / 3 is not less than 0.90, and is preferably not less than 0.95. The upper limit is preferably not more than 1.50, and more preferably not more than 1.20.

[0062] The rubber composition preferably contains a resin. Examples of the resin include aromatic hydrocarbon resins such as phenolic resins, alkylphenolic resins, terpene resins, coumarone resins, indene resins, coumarone-indene resins, styrene resins, acrylic resins, rosin resins, and dicyclopentadiene resins (DCPD resins), aliphatic hydrocarbon resins such as C5 resins, C8 resins, C9 resins, and C5 / C9 resins, and hydrogenated products thereof, which are commonly used in the tire industry. Commercially available products include those from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Co., Ltd., Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Energy Corporation, Nippon Zeon Co., Ltd., Harima Chemical Co., Ltd., Toagosei Co., Ltd., Arakawa Chemical Industries Co., Ltd., and Taoka Chemical Co., Ltd. These may be used alone or in combination of two or more. Of these, C5 / C9 resins are preferred.

[0063] The C5 / C9 resin is a polymer mainly composed of structural units derived from a C5 fraction and a C9 fraction, and includes copolymers of a C5 fraction and a C9 fraction as well as copolymers of a C5 fraction and a C9 fraction with other monomers that can be copolymerized therewith. Among these, copolymers of a C5 fraction and a C9 fraction are preferred.

[0064] The softening point of the resin is preferably 50° C. or higher, more preferably 80° C. or higher, and even more preferably 96° C. or higher, and is preferably 150° C. or lower, more preferably 130° C. or lower, and even more preferably 115° C. or lower. Within the above ranges, the effect tends to be better obtained. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point tester.

[0065] The resin may be in a solid or liquid state at room temperature (25° C.), but is preferably in a solid state.

[0066] The resin content is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0067] In the above rubber composition, the contents (parts by mass) of the resin and the silane coupling agent per 100 parts by mass of the rubber component preferably satisfy the relationship of the following formula (B). This is believed to allow the resin, which is compatible with the polymer, and the silane coupling agent to be incorporated into the polymer while interacting with each other, thereby allowing the coupling reaction to proceed more efficiently. Resin content / Silane coupling agent content>2.0 (B)

[0068] In formula (B), the resin content / silane coupling agent content may be more than 2.0, but is preferably more than 2.5, and more preferably more than 3.5. The upper limit is preferably 5.0 or less, and more preferably 4.0 or less.

[0069] The rubber composition preferably contains oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, naphthenic process oil, and the like. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. In addition, ester-based plasticizers such as di(2-ethylhexyl) sebacate (DOS), tri(2-ethylhexyl) phosphate (TOP), di(2-ethylhexyl) adipate (DOA), and di-2-ethylhexyl phthalate (DOP) may be used as the oil. Commercially available products include those from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., JXTG Nippon Oil & Energy Corporation, Orisoi Co., Ltd., H&R Corporation, Toyokuni Oil Mills Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0070] The content of the oil is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0071] In the rubber composition, the contents (parts by mass) of the oil, resin, and inorganic filler per 100 parts by mass of the rubber component preferably satisfy the relationship of the following formula (C). This makes it difficult for the viscosity of the kneaded product to decrease during kneading, making it easier for the inorganic filler to be incorporated into the polymer, which is believed to result in easier severing of the chemical bonds of the polymer by the inorganic filler and easier obtaining the reinforcing effect of silica. (Oil content + resin content) / inorganic filler content≦1.0 (C)

[0072] In formula (C), the ratio (oil content + resin content) / inorganic filler content may be 1.0 or less, preferably 0.8 or less, more preferably 0.7 or less. The lower limit is preferably 0.1 or more, more preferably 0.2 or more.

[0073] The rubber composition may contain sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0074] The amount of sulfur is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 0.9 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.

[0075] In the above rubber composition, the sulfur content (amount of sulfur in 100% by mass of the rubber composition) is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 0.6 mass% or more, and is preferably 1.5 mass% or less, more preferably 1.2 mass% or less, even more preferably 0.8 mass% or less, even more preferably 0.7 mass% or less. The sulfur content includes not only the sulfur used as a vulcanizing agent, but also the sulfur contained in a silane coupling agent, etc. For example, the sulfur content in a silane coupling agent can be calculated by multiplying the value calculated by (number of sulfur atoms contained in the structure of the silane coupling agent * atomic weight of sulfur / molecular weight of the silane coupling agent) by the content of the silane coupling agent.

[0076] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and di-2-benzothiazolyl disulfide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-oxyethylene-2-benzothiazolesulfenamide, and N,N'-diisopropyl-2-benzothiazolesulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. Commercially available products include products from Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.

[0077] The content of the vulcanization accelerator is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.

[0078] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0079] The amount of zinc oxide is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.

[0080] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.

[0081] The content of the antioxidant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better.

[0082] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.

[0083] The content of stearic acid is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.

[0084] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0085] The amount of the wax is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above range, the effect tends to be better obtained.

[0086] In addition to the above components, the rubber composition may further contain additives commonly used in the rubber industry, such as fatty acid metal salts, short fibers (carbon fibers, aramid fibers, etc.), nanofibers (cellulose nanofibers, etc.), organic crosslinking agents (KA9188 manufactured by LANXESS AG, TACKIROL V200 manufactured by Taoka Chemical Co., Ltd., etc.), organic peroxides, etc. The content of these additives is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.

[0087] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.

[0088] As for the kneading conditions, in the base kneading step in which additives other than sulfur and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which sulfur and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with sulfur and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.

[0089] The rubber composition can be suitably used, for example, in a tire tread (cap tread).

[0090] The tire (pneumatic tire, etc.) of the present invention is manufactured by a normal method using the above rubber composition. That is, the above rubber composition is extruded in an unvulcanized state according to the shape of the tread, and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.

[0091] The above-mentioned tires can be used as tires for passenger cars, tires for large passenger cars, tires for large SUVs, tires for heavy loads such as trucks and buses, tires for light trucks, tires for two-wheeled vehicles, racing tires (high performance tires), etc. They can also be used as all-season tires, summer tires, studless tires (winter tires), etc. EXAMPLES

[0092] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0093] The various chemicals used in the examples and comparative examples will be described below.

[0094] SBR: Asahi Kasei Corporation's Tufuden 4850 (unmodified S-SBR, styrene content: 40% by mass, vinyl content: 46%, contains 50 parts by mass of oil per 100 parts by mass of rubber solids) Hydrogenated SBR (1): Production Example 1 below (solid at room temperature, Mw: 500,000, hydrogenation rate: 60 mol%, conjugated diene units: 28 mass%, non-conjugated olefin units: 42 mass%, aromatic vinyl units (styrene content): 30 mass%) Hydrogenated SBR (2): Production Example 2 below (liquid at room temperature, Mw: 10,000, hydrogenation rate: 60 mol%, conjugated diene units: 42 mass%, non-conjugated olefin units: 28 mass%, aromatic vinyl units (styrene content): 30 mass%) Hydrogenated SBR (3): Production Example 3 below (liquid at room temperature, Mw: 10,000, hydrogenation rate: 80 mol%, conjugated diene units: 56 mass%, non-conjugated olefin units: 14 mass%, aromatic vinyl units (styrene content): 30 mass%) Multicomponent copolymer (1): Production Example 4 below (solid at room temperature, Mw: 300,000, conjugated diene units: 16% by mass, non-conjugated olefin units: 64% by mass, aromatic vinyl units (styrene content): 20% by mass) Multicomponent copolymer (2): Production Example 5 below (solid at room temperature, Mw: 300,000, conjugated diene units: 6% by mass, non-conjugated olefin units: 59% by mass, aromatic vinyl units (styrene content): 35% by mass) Silica (1): ZEOSIL 115GR (BET specific surface area: 100-120 m) manufactured by SOLVAY 2 / g) Silica (2): ULTRASIL VN3 manufactured by EVONIK (BET specific surface area: 180 m 2 / g) Aluminum hydroxide: Apyral 200SM manufactured by Nabaltec Magnesium hydroxide: Fujifilm Wako Pure Chemical Industries, Ltd. Carbon black: Show Black N330 (N2SA: 75m) manufactured by Cabot Japan Co., Ltd. 2 / g, DBP oil absorption 102ml / 100g) Oil: H&R VIVATEC 500 Resin: Petrotac 100V manufactured by Tosoh Corporation (solid at room temperature, C5 / C9 resin, softening point: 96°C) Anti-aging agent: Antigen 6C (N-(1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine)) manufactured by Sumitomo Chemical Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Zinc oxide: Two types of zinc oxide manufactured by Mitsui Metals Co., Ltd. Silane coupling agent: Si69 (bis(3-triethoxysilylpropyl)tetrasulfide) manufactured by Evonik Sulfur: Powdered sulfur manufactured by Karuizawa Sulfur Co., Ltd. Vulcanization accelerator (1): Succinol DG (1,3-diphenylguanidine) manufactured by Sumitomo Chemical Co., Ltd. Vulcanization accelerator (2): Noccela CZ-G (N-cyclohexyl-2-benzothiazole sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0095] <Production Example 1: Production of Hydrogenated SBR (1)> n-Hexane, styrene, 1,3-butadiene, TMEDA (N,N,N',N'-tetramethylethylenediamine), and n-butyllithium were added to a heat-resistant reaction vessel that had been thoroughly substituted with nitrogen, and the mixture was stirred at 50°C for 5 hours to carry out a polymerization reaction. After that, the mixture was stirred for 20 minutes while supplying hydrogen gas at a pressure of 0.4 MPa-Gauge, and reacted with the unreacted lithium at the polymer end to produce lithium hydride. The hydrogen gas supply pressure was set to 0.7 MPa-Gauge, the reaction temperature was set to 90°C, and hydrogenation was carried out using a catalyst mainly composed of titanocene dichloride. When the absorption of hydrogen reached the cumulative amount that would result in the desired hydrogenation rate, the reaction temperature was set to room temperature, the hydrogen pressure was returned to normal pressure, and the mixture was removed from the reaction vessel. The reaction solution was stirred and poured into water, and the solvent was removed by steam stripping to obtain hydrogenated SBR (1). The polymerization conversion rate was nearly 100%.

[0096] <Production Example 2: Production of Hydrogenated SBR (2)> Except for changing the amounts of each chemical used, hydrogenated SBR (2) was obtained in the same manner as in Production Example 1. The polymerization conversion was nearly 100%.

[0097] <Production Example 3: Production of hydrogenated SBR (3)> Except for changing the amounts of each chemical used and the cumulative amount of hydrogen absorption, hydrogenated SBR (3) was obtained in the same manner as in Production Example 1. The polymerization conversion was nearly 100%.

[0098] <Production Example 4: Production of multicomponent copolymer (1)> Styrene as an aromatic vinyl compound and toluene were placed in a thoroughly dried 1500 mL pressure-resistant stainless steel reactor. Meanwhile, in a glove box under a nitrogen atmosphere, 1-benzyldimethylsilyl-3-methylindene, tris(bis(dimethylsilyl)amide)gadolinium complex, and triethylaluminum were charged into a glass vessel, toluene was added, and the mixture was reacted at 80° C. for 6 hours. After that, diisobutylaluminum hydride and toluene were added, followed by the addition of trityltetrakis(pentafluorophenyl)borate to obtain a catalyst solution. The obtained catalyst solution was added to the above-mentioned pressure-resistant stainless steel reactor and heated to 70°C. Next, ethylene as a non-conjugated olefin was added to the pressure-resistant stainless steel reactor at a pressure of 1 MPa, and a toluene solution containing 1,3-butadiene as a conjugated diene compound was further added over 3.5 hours, and a polymerization reaction was carried out at 70°C for a total of 4 hours. Thereafter, an isopropanol solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) was added to the pressure-resistant stainless steel reactor to terminate the reaction, and a large amount of methanol was used to separate the reaction product, which was then vacuum-dried at 50°C to obtain a multicomponent copolymer (1) (a copolymer of 1,3-butadiene, ethylene and styrene).

[0099] <Production Example 5: Production of multicomponent copolymer (2)> A multicomponent copolymer (2) (a copolymer of 1,3-butadiene, ethylene and styrene) was obtained in the same manner as in Production Example 4, except that the amounts of each chemical used were changed.

[0100] Examples and Comparative Examples According to the composition of Table 1, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized rubber composition. The unvulcanized rubber composition obtained was molded into a tread shape, and laminated together with other tire components on a tire building machine to form an unvulcanized tire, which was then vulcanized at 170°C for 12 minutes to produce a test tire (size: 195 / 65R15). In Table 1, the sulfur content (mass %) is calculated from the total amount of the sulfur content used as a vulcanizing agent, the sulfur content in the silane coupling agent, and the sulfur content in the vulcanization accelerator.

[0101] The following evaluations were carried out using the above test tires. The results are shown in Table 1.

[0102] (Wet grip performance) Each test tire was mounted on a vehicle, and the braking distance from an initial speed of 80 km / h on a wet asphalt road surface was determined, and expressed as an index with Comparative Example 1 being set at 100. A higher index indicates a shorter braking distance and better wet grip performance.

[0103] (Wear resistance) Each test tire was mounted on a vehicle, and the groove depth of the tread portion was measured after driving 50,000 km. The amount of wear of the tread portion was calculated from the measured values, and expressed as an index with Comparative Example 1 being set at 100. The larger the index, the smaller the amount of wear and the better the wear resistance.

[0104] [Table 1]

[0105] As can be seen from Table 1, the Examples had improved overall performance (total of all indexes) in terms of wet grip performance and abrasion resistance, compared to the Comparative Examples.

[0106] In addition, a comparison of Comparative Examples 1, 2, 3, and 7 with Example 1 shows that a multicomponent copolymer containing a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit, an inorganic compound represented by formula (1), and a polymer having a BET specific surface area of ​​150 m 2 It was confirmed that a synergistic improvement effect was obtained by using silica at a concentration of 0.1g or more in combination with SiO2.

Claims

1. a rubber component including a multicomponent copolymer including a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit; An inorganic compound represented by the following formula (1) and a BET specific surface area of ​​150 m 2 / g or more of an inorganic filler containing silica, The content of the multicomponent copolymer in 100% by mass of the rubber component is 30% by mass or more, The content of the inorganic filler is 80 to 170 parts by mass based on 100 parts by mass of the rubber component, A rubber composition in which the content of the silica is greater than the content of the inorganic compound, mM・xSiOy・zH 2 O (1) (In the formula, M is at least one metal selected from the group consisting of Al, Mg, Ti, Ca, and Zr, or an oxide or hydroxide of the metal, m is an integer of 1 to 5, x is an integer of 0 to 10, y is an integer of 2 to 5, and z is an integer of 0 to 10.) The multicomponent copolymer is a hydrogenated styrene butadiene rubber, The hydrogenated styrene butadiene rubber has a hydrogenation rate of 50 mol% or more, a weight average molecular weight of 2000 or more, and a styrene content of 25 to 40 mass%. The inorganic compound is at least one selected from the group consisting of aluminum hydroxide and magnesium hydroxide, A rubber composition in which the content (parts by mass) of the silica and the content (parts by mass) of the inorganic compound per 100 parts by mass of the rubber component satisfy the following formula: The content of the silica−the content of the inorganic compound≧60 parts by mass

2. The rubber composition according to claim 1 , which satisfies the following formula (A): (Inorganic filler content) 2/3 / (content of inorganic filler + content of carbon black) 2/3 ≧0.90 (A)

3. Contains a silane coupling agent, 3. The rubber composition according to claim 1, wherein the content of the silane coupling agent is 1 to 5 parts by mass per 100 parts by mass of the total content of the silica and the other silica.

4. The rubber composition according to any one of claims 1 to 3, which satisfies the following formula (B): Resin content / Silane coupling agent content>2.0 (B)

5. The rubber composition according to any one of claims 1 to 4, having a sulfur content of 0.8 mass % or less.

6. The rubber composition according to any one of claims 1 to 5, which satisfies the following formula (C): (Oil content + resin content) / inorganic filler content ≦ 1.0 (C)

7. 7. The rubber composition according to claim 1, wherein the content of the multi-component copolymer is 30 to 60 mass % based on 100 mass % of the rubber component.

8. The rubber composition according to any one of claims 1 to 7, wherein the inorganic compound is aluminum hydroxide.

9. A tire having a tread using the rubber composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Rubber composition for tire and pneumatic tire using the same

    JP2001214003A

  • Rubber composition for tire tread

    JP2010013551A

  • Rubber composition for tire and pneumatic tire

    JP2011140613A

  • Rubber composition for tire tread and pneumatic tire

    JP2012246429A

  • Rubber composition and pneumatic tire

    JP2015086315A