Heavy Duty Tires

A heavy-duty tire with a tread composed of isoprene and butadiene rubber, tailored to specific viscoelastic properties, enhances starting performance on ice by reducing ice melting and increasing contact area.

JP7581665B2Active Publication Date: 2024-11-13SUMITOMO RUBBER INDUSTRIES LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020102392
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-12
Publication Date
2024-11-13
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

Existing heavy-duty tires lack excellent starting performance on icy roads, necessitating improved drive performance on icy surfaces.

Method used

A heavy-duty tire tread made of a rubber composition containing isoprene-based rubber and butadiene rubber, with specific viscoelastic properties defined by a tan δ range of 0.38 to 0.48 at -10°C under shear mode conditions, incorporating silica, carbon black, and a surface roughening material to enhance grip on ice.

Benefits of technology

The tire achieves superior starting performance on ice by optimizing viscoelastic properties to reduce ice melting and increase contact area, thereby improving traction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581665000001
    Figure 0007581665000001
  • Figure 0007581665000002
    Figure 0007581665000002
Patent Text Reader

Abstract

To provide a tire for heavy load excellent in an on-ice start performance.SOLUTION: There is provided a tire for heavy load having a tread composed of a rubber composition which includes an isoprene rubber and a butadiene rubber and in which tanδ at -10°C under a condition in a following shear mode satisfies a following formula (1). The formula (1) is: tanδ≤0.48 at 0.38≤-10°C, and in the (shear mode), stress is 0.5 MPa, a frequency is 10 Hz, and a measured temperature of tanδ is -10°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heavy duty tire. [Background technology]

[0002] In recent years, performance on snow and ice has become an important requirement for tires for heavy loads such as trucks and buses, and in particular, there is a demand for improvement in driving performance on icy roads (starting performance on ice) (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-168427 A Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE PRESENT EMBODIMENTS The present invention has an object to solve the above problems and to provide a heavy-duty tire that is excellent in starting performance on ice. [Means for solving the problem]

[0005] The inventors have discovered that by clarifying the frequency that is input to the tread rubber from an icy road surface when starting on an icy road from the relationship between the shape of the icy road surface and the speed at the time of starting, and by reflecting these conditions in the viscoelasticity measurement conditions, it is possible to accurately predict (estimate) starting performance on ice, and have completed this invention.

[0006] The present invention relates to a heavy-duty tire having a tread made of a rubber composition containing an isoprene-based rubber and a butadiene rubber, and having a tan δ at −10° C. under the following shear mode condition that satisfies the following formula (1): 0.38≦tan δ at -10℃≦0.48 (1) [Shear mode] Stress: 0.5MPa Frequency: 10Hz Measurement temperature of tan δ: -10℃

[0007] The rubber composition preferably contains 14 parts by mass or more of silica per 100 parts by mass of the rubber component.

[0008] The rubber composition preferably contains a surface roughening material having an average particle size of 50 μm or more.

[0009] The rubber composition has an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of ​​130 m 2 It is preferable that the carbon black contains at least 100% by mass of carbon black.

[0010] The rubber composition preferably contains 10 to 35 parts by mass of the plasticizer relative to 100 parts by mass of the rubber component.

[0011] The rubber composition preferably contains 5 to 20 parts by mass of the liquid plasticizer per 100 parts by mass of the rubber component.

[0012] The rubber composition preferably contains 1.0 to 15 parts by mass of resin per 100 parts by mass of the rubber component. Effect of the Invention

[0013] According to the present invention, a heavy-duty tire having a tread made of a rubber composition that contains an isoprene-based rubber and a butadiene rubber and has a tan δ at −10° C. under the shear mode condition that satisfies the formula (1) can be provided, so that a heavy-duty tire with excellent starting performance on ice can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention provides a heavy-duty tire having a tread made of a rubber composition that contains an isoprene-based rubber and a butadiene rubber and has a tan δ at −10° C. under the shear mode condition that satisfies the formula (1). This provides excellent starting performance on ice.

[0015] The mechanism by which such an effect is obtained is not clear, but is presumed to be as follows. As described above, the present invention clarifies the frequency input from the icy road surface to the tread rubber when starting on the icy road surface from the relationship between the icy road surface shape and the starting speed, and reflects the condition in the viscoelasticity measurement condition to derive the parameters of the above formula (1). Specifically, for the above formula (1), the viscoelasticity measurement is performed at a temperature and frequency determined based on the principles of friction, and the measurement stress is performed using the tire's contact pressure, and "-10°C tan δ" is specified as the physical property parameter as the potential of hysteresis loss friction in shear deformation mode. It is considered that by determining the optimal range of "-10°C tan δ", it is possible to suppress the ice on the icy road surface melting and generating water, which reduces the contact area between the rubber and the road surface, due to the potential of hysteresis loss friction (tan δ) being too high. Therefore, it is presumed that excellent starting performance on ice can be imparted by satisfying the above formula (1).

[0016] In this way, the present invention solves the problem (objective) of improving starting performance on ice by configuring a heavy-duty tire having a tread made of a rubber composition that contains isoprene rubber and butadiene rubber and satisfies formula (1) "tan δ at 0.38≦-10°C≦0.48." In other words, the parameter of formula (1) does not define the problem (objective); the problem of the present application is to improve starting performance on ice, and the invention is configured to satisfy the parameter as a means to achieve this.

[0017] The rubber composition (vulcanized rubber composition) constituting the tread satisfies the following formula (1) in tan δ at −10° C. under the following shear mode conditions. In other words, tan(−10° C.) satisfies the following formula (1) not in a state where a specified strain is applied but in a state where a specified stress of 0.5 MPa is applied. 0.38≦tan δ at -10℃≦0.48 (1) [Shear mode] Stress: 0.5MPa Frequency: 10Hz Measurement temperature of tan δ: -10℃

[0018] In the formula (1), the tan δ at -10°C is preferably 0.39 or more, more preferably 0.40 or more, and even more preferably 0.41 or more. The tan δ at -10°C is preferably 0.47 or less, more preferably 0.46 or less, and even more preferably 0.45 or less. By keeping it within the above range, good starting performance on ice tends to be obtained.

[0019] The "tan δ at -10°C under the shear mode conditions" can be measured by a viscoelasticity test, specifically, by the method described in the Examples below.

[0020] The value of "tan δ at -10°C under the shear mode conditions" can be adjusted by using a method that can adjust tan δ at low temperatures. For example, the value of "tan δ at -10°C under the shear mode conditions" tends to be larger when using methods such as increasing the total amount of isoprene-based rubber and butadiene rubber, increasing the amount of butadiene rubber, increasing the amount of filler, using a filler with a high surface area, blending an appropriate amount of resin, blending an appropriate amount of liquid plasticizer (oil, liquid resin, etc.), and blending a material that imparts a scratching friction effect on ice road surfaces, such as eggshell powder.

[0021] By adjusting "tan δ at -10°C under the shear mode conditions" using these techniques, the formula (1) can be adjusted, and a rubber composition that satisfies this parameter can be produced.

[0022] (Rubber component) The rubber composition includes isoprene rubber and butadiene rubber (BR).

[0023] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.

[0024] In the rubber composition, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. By keeping it within the above range, good starting performance on ice tends to be obtained.

[0025] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. Among them, high cis BR with a cis content of 90% by mass or more is preferred because it improves wear resistance.

[0026] The BR may be either unmodified or modified. The modified BR may be any BR having a functional group that interacts with a filler such as silica, and examples of the modified BR include terminal-modified BR (terminal-modified BR having the functional group at the terminal) in which at least one terminal of the BR is modified with a compound (modifier) ​​having the functional group, main-chain-modified BR having the functional group in the main chain, main-chain-terminal-modified BR having the functional group in the main chain and at least one terminal (for example, main-chain-terminal-modified BR having the functional group in the main chain and modified with the modifier at least one terminal), and terminal-modified BR modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or an epoxy group introduced therein.

[0027] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.

[0028] As the BR, for example, products from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used.

[0029] In the rubber composition, the BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. By keeping it within the above range, good starting performance on ice tends to be obtained.

[0030] In the rubber composition, the total content of the isoprene-based rubber and the BR in 100% by mass of the rubber component is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of starting performance on ice. The upper limit is not particularly limited, and may be 100% by mass, or may be 90% by mass or less, or 80% by mass or less.

[0031] In the rubber composition, other diene rubbers can be used as rubber components other than isoprene rubber and BR. Examples of other diene rubbers include styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Other examples include butyl rubber and fluororubber. Among these, SBR is preferred. The isoprene rubber, BR, SBR, and other rubber components may be used alone or in combination of two or more.

[0032] The SBR is not particularly limited, and for example, emulsion polymerized styrene butadiene rubber (E-SBR), solution polymerized styrene butadiene rubber (S-SBR), etc. can be used. These may be used alone or in combination of two or more kinds.

[0033] The styrene content of the SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The styrene content is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. By keeping the styrene content within the above range, good starting performance on ice tends to be obtained. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.

[0034] The vinyl bond content of the SBR is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. The vinyl bond content is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less. By keeping it within the above range, good starting performance on ice tends to be obtained. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.

[0035] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.

[0036] The SBR may be unmodified SBR or modified SBR, and the modified SBR may be modified SBR having the same functional group as the modified BR introduced therein.

[0037] When the rubber composition contains SBR, the content of SBR in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The upper limit is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less. By keeping it within the above range, good starting performance on ice tends to be obtained. In addition, by using SBR, it becomes possible to increase the amount of silica blended, and tan δ tends to be efficiently increased.

[0038] (Filler) From the viewpoint of starting performance on ice, the rubber composition preferably contains a filler. The filler is not particularly limited, and materials known in the rubber field can be used, such as silica, carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, mica, etc. Among them, carbon black and silica are preferred.

[0039] In the rubber composition, the content of the filler (total content of the fillers) is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 40 parts by mass or more, and particularly preferably 45 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, even more preferably 100 parts by mass or less, and particularly preferably 85 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0040] From the viewpoint of starting performance on ice, the rubber composition is made of a material having an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 130 m 2 It is preferable that the composition contains carbon black (also referred to as carbon black (A)) having a molecular weight of at least 1000 mol / g.

[0041] The average particle size of the carbon black (A) is preferably 20 nm or less, more preferably 17 nm or less, and even more preferably 16 nm or less. The lower limit is not particularly limited, but is preferably 5 nm or more, more preferably 10 nm or more. By keeping it within the above range, good starting performance on ice tends to be obtained. The average particle size of carbon black is a number average particle size, and is measured by a transmission electron microscope.

[0042] The CTAB of carbon black (A) is preferably 130m 2 / g or more, more preferably 140m 2 / g or more, more preferably 145m 2 / g or more, particularly preferably 150m 2 / g or more. The upper limit is not particularly limited, but is preferably 250 m 2 / g or less, more preferably 200m 2 / g or less, more preferably 180m 2 By keeping the value within the above range, good starting performance on ice tends to be obtained. In this specification, the CTAB of carbon black is a value measured in accordance with JIS K6217-3:2001.

[0043] The nitrogen adsorption specific surface area (N2SA) of the carbon black (A) is preferably 125 m 2 / g or more, more preferably 145m 2 / g or more, more preferably 150m 2 / g or more, particularly preferably 155m 2 / g or more. The upper limit is not particularly limited, but is preferably 250 m 2 / g or less, more preferably 200m 2 / g or less, more preferably 180m 2 By keeping the value within the above range, good starting performance on ice tends to be obtained. The N2SA of carbon black is determined in accordance with JIS K 6217-2:2001.

[0044] The iodine adsorption amount (IA) (mg / g) of the carbon black (A) is preferably 120 mg / g or more, more preferably 125 mg / g or more, even more preferably 130 mg / g or more, and particularly preferably 140 mg / g or more. There is no particular upper limit, but it is preferably 200 mg / g or less, more preferably 180 mg / g or less, and even more preferably 160 mg / g or less. By keeping it within the above range, good starting performance on ice tends to be obtained. In this specification, the iodine adsorption amount (IA) of carbon black is a value measured in accordance with JIS K6217-1:2001.

[0045] The ratio (CTAB / IA) of the cetyltrimethylammonium bromide adsorption specific surface area (CTAB) to the iodine adsorption amount (IA) (mg / g) of the carbon black (A) is preferably 0.85 m 2 / mg or more, more preferably 0.92m 2 / mg or more, more preferably 1.00m 2 The upper limit is not particularly limited, but is preferably 1.35 m 2 / mg or less, more preferably 1.30m 2 / mg or less, more preferably 1.25m 2By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0046] The dibutyl phthalate absorption (DBP) of the carbon black (A) is preferably 120 cm 3 / 100g or more, preferably 125cm 3 / 100g or more, more preferably 135cm 3 / 100g or more. The upper limit is not particularly limited, but is preferably 180 cm 3 / 100g or less, more preferably 170cm 3 / 100g or less, more preferably 160cm 3 By keeping the value within the above range, good starting performance on ice tends to be obtained. The DBP of carbon black is measured in accordance with JIS K 6217-4:2001.

[0047] Examples of carbon black (A) include SAF. These carbon blacks may be used alone or in combination of two or more. Carbon black (A) can also be produced by the production methods described in JP-A-2000-319539 and JP-T-8-507555.

[0048] In the rubber composition, the content of carbon black (A) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0049] The rubber composition may further contain carbon black other than the carbon black (A) (also referred to as carbon black (B)).

[0050] The carbon black (B) may, for example, have an average particle size of more than 20 nm and not more than 25 nm and / or a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 100 m 2 / g or more 130m 2 Carbon black having a molecular weight of less than 1000 kJ / g (also referred to as carbon black (B)) can be suitably used.

[0051] The average particle size of the carbon black (B) is more than 20 nm and not more than 25 nm (greater than 20 nm and not more than 25 nm), but the lower limit is preferably 21 nm or more. The upper limit is preferably 24 nm or less, more preferably 23 nm or less. By keeping the average particle size within the above range, good starting performance on ice tends to be obtained.

[0052] The CTAB of carbon black (B) is preferably 105m 2 / g or more, more preferably 110m 2 The upper limit is not particularly limited, but is preferably 125 m 2 / g or less, more preferably 120m 2 By keeping the value within the above range, good starting performance on ice tends to be obtained.

[0053] The average particle size, CTAB, of carbon black (B) (other carbon black) can be measured by the same method as described above.

[0054] In the rubber composition, the content of carbon black (B) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0055] Carbon black (B) (other carbon black) is not particularly limited, but includes N220, N234, N219, N339, N330, N326, N351, N550, N762, etc. For example, products of Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. From the viewpoints of wear resistance and cost, N220 is particularly preferred.

[0056] In the rubber composition, the carbon black content (total content of carbon black (A) and carbon black (B)) is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 35 parts by mass or more, per 100 parts by mass of the rubber component. The content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 70 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0057] The content of carbon black (A) in 100% by mass of carbon black is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more, from the viewpoint of starting performance on ice. The upper limit of the content is not particularly limited, and may be 100% by mass.

[0058] Examples of silica include dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.

[0059] In the rubber composition, the content of silica is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, even more preferably 10 parts by mass or more, and particularly preferably 14 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0060] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 250m 2 / g or less, more preferably 200m 2 By keeping the value within the above range, good starting performance on ice tends to be obtained. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.

[0061] (Silane coupling agent) When the rubber composition contains silica, it is preferable that the rubber composition further contains a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, Examples of such silanes include sulfide-based silanes such as bamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.

[0062] In the rubber composition, the content of the silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, based on 100 parts by mass of silica. The content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0063] (Surface roughening material) The rubber composition may be blended with a surface roughening material. Examples of the surface roughening material include, but are not limited to, eggshell powder, short fibers, zinc oxide whiskers, shelled powder, granular whitebait, crushed walnuts, volcanic ash, and fine iron particles. These may be used alone or in combination of two or more. Among these, eggshell powder is preferred. Eggshell powder is obtained by crushing eggshells, and its main component is calcium carbonate. When a surface roughening material such as eggshell powder is blended, the surface roughening material protruding from the tread surface has a scratching friction effect on the ice road surface, which improves grip performance, and the edge effect (wiping effect) of the voids (holes) formed by the surface roughening material falling off the tread surface increases the contact area with the ice road surface, improving grip performance and improving starting performance on ice.

[0064] The average particle size of the surface roughening material (preferably eggshell powder) is preferably 50 μm or more, more preferably 70 μm or more, and even more preferably 90 μm or more, and although there is no particular upper limit, it is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, and particularly preferably 120 μm or less. By keeping it within the above range, good starting performance on ice tends to be obtained. The average particle size of the surface roughening material (eggshell powder) is measured using a particle size distribution measuring device.

[0065] As the surface roughening material such as eggshell powder, for example, products available from Green Techno 21 Co., Ltd., Kewpie Corporation, etc. can be used.

[0066] In the rubber composition, the content of the surface roughening material is preferably 0.5 parts by mass or more, more preferably 2 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained. The content of the eggshell powder is also preferably within the same range.

[0067] (Plasticizer) The rubber composition may contain a plasticizer. A plasticizer is a material that imparts plasticity to a rubber component, and examples of the plasticizer include liquid plasticizers (plasticizers that are in a liquid state at room temperature (25° C.)) and resins (resins that are in a solid state at room temperature (25° C.)).

[0068] When the rubber composition contains a plasticizer, the content thereof (total amount of plasticizer) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 35 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0069] The liquid plasticizer (a plasticizer that is in a liquid state at room temperature (25° C.)) is not particularly limited, and examples thereof include oil, liquid resin, liquid diene-based polymer, liquid farnesene-based polymer, etc. These may be used alone or in combination of two or more kinds.

[0070] When the rubber composition contains a liquid plasticizer, the content thereof is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 7 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0071] Examples of the oil include process oil, vegetable oil, or a mixture thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Co., Ltd. Among these, process oils (paraffin-based process oils, aromatic process oils, naphthenic process oils, etc.) and vegetable oils are preferred.

[0072] When the rubber composition contains oil, the content thereof is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0073] Examples of liquid resins include terpene resins (including terpene phenol resins and aromatic modified terpene resins) that are liquid at 25°C, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, dicyclopentadiene (DCPD) resins, coumarone-indene resins (including coumarone and indene simple resins), phenol resins, olefin resins, polyurethane resins, and acrylic resins.

[0074] When the rubber composition contains a liquid resin, the content thereof is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0075] Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, liquid farnesene butadiene copolymers, etc., which may be modified at the ends or main chains with polar groups.

[0076] When the rubber composition contains a liquid diene polymer, the content thereof is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0077] Liquid farnesene polymers are polymers obtained by polymerizing farnesene and have structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), but (E)-β-farnesene, which has the following structure, is preferred. [ka]

[0078] The liquid farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer).

[0079] Examples of vinyl monomers include aromatic vinyl compounds such as styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinyltoluene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene, as well as conjugated diene compounds such as butadiene and isoprene. These may be used alone or in combination of two or more. Among these, butadiene is preferred. That is, the farnesene-vinyl monomer copolymer is preferably a copolymer of farnesene and butadiene (farnesene-butadiene copolymer).

[0080] In the farnesene-vinyl monomer copolymer, the copolymerization ratio by mass of farnesene and vinyl monomer (farnesene / vinyl monomer) is preferably 40 / 60 to 90 / 10.

[0081] The liquid farnesene-based polymer that can be suitably used has a weight average molecular weight (Mw) of 3000 to 300,000. The Mw of the liquid farnesene-based polymer is preferably 8000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 50,000 or less.

[0082] When the rubber composition contains a liquid farnesene polymer, the content thereof is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 35 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0083] Examples of the resin (resin in a solid state at room temperature (25°C)) include aromatic vinyl polymers in a solid state at room temperature (25°C), coumarone-indene resins, coumarone resins, indene resins, phenolic resins, rosin resins, petroleum resins, terpene resins, and acrylic resins. The resins may be hydrogenated. These may be used alone or in combination of two or more. Of these, terpene resins are preferred from the viewpoint of starting performance on ice.

[0084] In the rubber composition, the content of the resin per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more. The upper limit is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0085] The softening point of the resin is preferably 80° C. or higher, more preferably 90° C. or higher, and even more preferably 100° C. or higher. The upper limit is preferably 180° C. or lower, more preferably 160° C. or lower, and even more preferably 140° C. or lower. By keeping the softening point within the above range, good starting performance on ice tends to be obtained. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.

[0086] The terpene resin is a polymer containing terpene as a structural unit. For example, polyterpene resin obtained by polymerizing a terpene compound, aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be mentioned. Hydrogenated products of these can also be used.

[0087] The polyterpene resin is a resin obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.

[0088] Examples of the polyterpene resin include pinene resin, limonene resin, dipentene resin, pinene / limonene resin, etc., which are made from the above-mentioned terpene compounds. Among them, pinene resin is preferable. Pinene resin usually contains both α-pinene and β-pinene, which are isomers, but depending on the components contained, it is classified into β-pinene resin mainly composed of β-pinene and α-pinene resin mainly composed of α-pinene.

[0089] Examples of the aromatic modified terpene resin include terpene phenol resins made from the above terpene compounds and phenolic compounds, and terpene styrene resins made from the above terpene compounds and styrene compounds. Terpene phenol styrene resins made from the above terpene compounds, phenolic compounds, and styrene compounds can also be used. Examples of the phenolic compounds include phenol, bisphenol A, cresol, and xylenol. Examples of the styrene compounds include styrene and α-methylstyrene.

[0090] In the rubber composition, the content of the terpene resin per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more. The upper limit is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. By keeping the content within the above range, good starting performance on ice tends to be obtained.

[0091] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a constituent unit. For example, it may be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it may be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, or a copolymer of styrene and another monomer. In the rubber composition, the content of the aromatic vinyl polymer per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0092] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc. In the rubber composition, the content of the coumarone-indene resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0093] The coumarone resin is a resin containing coumarone as a main monomer component constituting the resin skeleton (main chain). In the rubber composition, the content of the coumarone resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0094] The indene resin is a resin containing indene as a main monomer component constituting the resin skeleton (main chain). In the rubber composition, the content of the indene resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0095] The phenolic resin may be a known one, such as a polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural using an acid or alkali catalyst. Among them, a polymer obtained by reacting with an acid catalyst (such as a novolac-type phenolic resin) is preferable. In the rubber composition, the content of the phenolic resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0096] The rosin resin may be a rosin-based resin such as natural rosin, polymerized rosin, modified rosin, their ester compounds, or their hydrogenated products. In the rubber composition, the content of the rosin resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0097] The petroleum resin may be a C5 resin, a C9 resin, a C5 / C9 resin, a dicyclopentadiene (DCPD) resin, etc. Among them, a DCPD resin is preferable. In the rubber composition, the content of the petroleum resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0098] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.

[0099] The solvent-free carboxyl group-containing styrene-acrylic resin is a (meth)acrylic resin (polymer) synthesized by a high-temperature continuous polymerization method (high-temperature continuous bulk polymerization method) (methods described in U.S. Pat. No. 4,414,370, JP-A-59-6207, JP-B-5-58005, JP-A-1-313522, U.S. Pat. No. 5,010,166, Toa Gosei Kenkyuu Nenpo TREND 2000 Vol. 3, p. 42-45, etc.) with minimal use of auxiliary raw materials such as polymerization initiators, chain transfer agents, and organic solvents. In this specification, (meth)acrylic means methacryl and acrylic.

[0100] Examples of the acrylic monomer components constituting the acrylic resin include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters such as 2-ethylhexyl acrylate, aryl esters, aralkyl esters, etc.), (meth)acrylamide, (meth)acrylic acid derivatives such as (meth)acrylamide derivatives, etc. (Meth)acrylic acid is a general term for acrylic acid and methacrylic acid.

[0101] Examples of the aromatic vinyl monomer component constituting the acrylic resin include aromatic vinyls such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene.

[0102] In addition, as a monomer component constituting the acrylic resin, other monomer components may be used together with (meth)acrylic acid, (meth)acrylic acid derivatives, and aromatic vinyl. In the rubber composition, the content of the acrylic resin per 100 parts by mass of the rubber component is preferably 1 to 30 parts by mass.

[0103] Examples of the plasticizer that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.

[0104] (Other materials) From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition preferably contains an antioxidant.

[0105] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.

[0106] In the rubber composition, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, more preferably 4.0 parts by mass or less.

[0107] The rubber composition preferably contains stearic acid. The content of stearic acid in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0108] As the stearic acid, any known stearic acid can be used, for example, products available from NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.

[0109] The rubber composition preferably contains zinc oxide. The content of zinc oxide in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0110] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.

[0111] The rubber composition may contain wax. The content of the wax in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0112] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.

[0113] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.

[0114] It is preferable to compound sulfur into the rubber composition in that it forms an appropriate amount of crosslinked chains in the polymer chains and imparts good performance.

[0115] In the rubber composition, the sulfur content is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and even more preferably 0.5 part by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.

[0116] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0117] The rubber composition preferably contains a vulcanization accelerator. In the rubber composition, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 2.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 3.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.

[0118] The type of vulcanization accelerator is not particularly limited, and any commonly used accelerator can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.

[0119] In addition to the above components, the rubber composition may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.

[0120] The rubber composition can be produced by any known method, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, followed by vulcanization.

[0121] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 50 to 200°C, preferably 80 to 190°C, and the kneading time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100°C or lower, preferably room temperature to 80°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 120 to 200°C, preferably 140 to 180°C.

[0122] The rubber composition is used in a tread (cap tread), and the tread (cap tread) may be at least partially composed of the above-mentioned rubber composition, or may be entirely composed of the above-mentioned rubber composition.

[0123] Heavy-duty tires are manufactured by a conventional method using a rubber composition. That is, the rubber composition, which contains various additives as necessary, is extruded in an unvulcanized state to match the shape of the tread (cap tread), molded in a conventional method on a tire building machine, and laminated together with other tire components to form an unvulcanized tire. After that, the heavy-duty tire can be manufactured by heating and pressurizing in a vulcanizer.

[0124] In this specification, the heavy-duty tire is a tire that is particularly excellent in durability, and examples of such tires include tires for trucks and buses, industrial tires used for industrial vehicles such as heavy machinery, etc. Heavy-duty tires generally use all-steel tires in which the cords used in the case and breaker are both steel cords.

[0125] Heavy-duty tires have good starting performance on ice and can therefore be suitably used as heavy-duty winter tires (heavy-duty studless tires, heavy-duty snow tires, heavy-duty studded tires, etc.). EXAMPLES

[0126] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0127] (Production example) Carbon black A was produced using a carbon black reactor consisting of a combustion zone with an inner diameter of 800 mm and a length of 1600 mm equipped with an air inlet duct and a combustion burner, a raw material introduction zone consisting of a narrow-diameter section with an inner diameter of 145 mm and a length of 1000 mm connected to the combustion zone and having a raw material nozzle penetrating from the periphery, and a rear reaction zone with an inner diameter of 400 mm and a length of 3000 mm equipped with a quench device. Heavy oil C and creosote oil were used as the fuel and the raw material hydrocarbon, respectively, and the various conditions were set.

[0128] Various chemicals used in the examples and comparative examples will be collectively described below. NR:TSR20 BR: BR360 (cis 1,4 bond content 98% by mass) manufactured by Ube Industries, Ltd. SBR: Tufuden 1000 manufactured by Asahi Kasei Corporation (unmodified S-SBR, styrene content 18% by mass, vinyl bond content 10% by mass) Carbon black B: N220 (average particle size 22 nm, CTAB115m 2 / g, N2SA115m 2 / g, IA118mg / g, CTAB / IA0.97, DBP113cm 3 / 100g) Carbon black A: Manufacturing example (average particle size 16 nm, CTAB 158 m 2 / g, N2SA170m 2 / g, IA145mg / g, CTAB / IA1.09, DBP138cm 3 / 100g) Silica: Uratosil VN3 (N2SA172m) manufactured by Evonik Degussa 2 / g) Eggshell powder 1: Egg calcium (Calhope, average particle size 10 μm) manufactured by Kewpie Corporation Eggshell powder 2: Egg calcium (Calhope, average particle size 50 μm) manufactured by Kewpie Corporation Eggshell powder 3: Eggshell powder (average particle size 100 μm) manufactured by Green Techno 21 Co., Ltd. Oil: Diana Process NH-70S (aromatic process oil) manufactured by Idemitsu Kosan Co., Ltd. Resin: YS Resin PX1150N (β-pinene resin, softening point 115°C) manufactured by Yasuhara Chemical Co., Ltd. Liquid farnesene polymer: Kuraray's L-FBR-742 (liquid farnesene butadiene copolymer, SP value 8.1) Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Antioxidant 6C: Nocrac 6C (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: Paulownia wood produced by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: HK-200-5 (powdered sulfur containing 5% oil by mass) manufactured by Hosoi Chemical Industry Co., Ltd. Vulcanization accelerator CZ: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator DPG: Noccelaer D (N,N'-diphenylguanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0129] [Examples and Comparative Examples] According to the compounding recipe shown in Table 1, chemicals other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was molded into the shape of a cap tread, and laminated together with other tire components to produce an unvulcanized tire. The tire was press-vulcanized at 170°C for 10 minutes to obtain a test tire (heavy-duty winter tire, size: 11R22.5).

[0130] The rubber properties and tire performance of the produced test tires were evaluated by the following methods. The results are shown in Table 1. The reference comparative example in Table 1 is Comparative Example 1.

[0131] <Viscoelasticity test> For samples (rubber compositions after vulcanization) taken from the cap tread of the test tire, the loss tangent (tan δ at -10°C) was measured using a viscoelasticity tester (DMA+450) manufactured by Metravib under the following shear deformation mode conditions. [Shear mode] Stress: 0.5MPa Frequency: 10Hz Measurement temperature of tan δ: -10℃ Sample size: diameter 10mm, thickness 2mm

[0132] (Starting performance on ice) Test tires were fitted to all wheels of an actual vehicle (a large truck with a total vehicle weight of 20 tons and two passengers), and the acceleration distance from a standstill on an icy road to a speed of 10km / h was measured with the vehicle's designated air pressure and with a load of 50% of the maximum load, and an index was displayed using the following formula. The higher the index, the better the driving performance on icy roads (starting performance on ice). (Ice starting performance index) = (Acceleration distance of standard comparison example) / (Acceleration distance of each compound) x 100

[0133] [Table 1]

[0134] As can be seen from Table 1, the heavy-duty tires of the examples using rubber compositions containing isoprene-based rubber and butadiene rubber and having tan δ at -10°C under the shear mode conditions satisfying formula (1) above had excellent starting performance on ice.

Claims

1. Contains isoprene-based rubber and butadiene rubber, A heavy-duty tire having a tread made of a rubber composition (excluding a rubber composition containing highly purified natural rubber having a phosphorus content of 500 ppm or less and a rubber composition containing butadiene rubber synthesized using a rare earth element catalyst) having a tan δ at −10° C. under the following shear mode condition that satisfies the following formula (1): 0.38≦tan δ at −10° C.≦0.48 (1) [Shear mode] Stress: 0.5 MPa Frequency: 10Hz Measurement temperature of tan δ: -10°C The rubber composition comprises: The amount of carbon black per 100 parts by mass of the rubber component is 20 parts by mass or more and 150 parts by mass or less, The content of silica per 100 parts by mass of the rubber component is 5 parts by mass or more and 60 parts by mass or less, The content of the plasticizer per 100 parts by mass of the rubber component is 10 parts by mass or more, an amount of the resin in a solid state at 25° C. per 100 parts by mass of the rubber component is 1 part by mass or more and 30 parts by mass or less; a total content of the isoprene-based rubber and the butadiene rubber in 100% by mass of the rubber component is 60% by mass or more, The content of the isoprene-based rubber in 100% by mass of the rubber component is 30% by mass or more and 90% by mass or less, A heavy-duty tire, wherein the content of the butadiene rubber in 100% by mass of a rubber component is 5% by mass or more and 60% by mass or less.

2. The tire for heavy loads according to claim 1, wherein the rubber composition contains 14 parts by mass or more of silica per 100 parts by mass of the rubber component.

3. The heavy duty tire according to claim 1 or 2, wherein the rubber composition contains a surface roughening agent having an average particle size of 50 μm or more.

4. The rubber composition has an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of ​​130 m 2 4. The heavy duty tire according to claim 1, further comprising carbon black having a molecular weight of at least 100000 / g.

5. The tire for heavy loads according to any one of claims 1 to 4, wherein the rubber composition contains 10 to 35 parts by mass of a plasticizer per 100 parts by mass of a rubber component.

6. The tire for heavy loads according to any one of claims 1 to 5, wherein the rubber composition contains 5 to 20 parts by mass of a liquid plasticizer per 100 parts by mass of a rubber component.

7. The tire for heavy loads according to any one of claims 1 to 6, wherein the rubber composition contains the resin in an amount of 1.0 to 15 parts by mass per 100 parts by mass of a rubber component.

Citation Information

Patent Citations

  • Studless tire for truck-bus or for light truck

    JP2010059252A

  • Rubber composition and tire using the same

    JP2010168427A

  • Rubber composition for studless tire

    JP2018188601A

  • Winter tire

    WO2015076048A1