Rubber composition for tires and winter tires

The rubber composition for tires, using isoprene rubber, butadiene rubber, and a specific silane coupling agent with a long carbon chain, addresses silica dispersion issues, improving high-speed ice turning performance both initially and after aging.

JP7581679B2Active Publication Date: 2024-11-13SUMITOMO RUBBER INDUSTRIES LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020119397
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-10
Publication Date
2024-11-13
Estimated Expiration
2040-07-10

AI Technical Summary

Technical Problem

Tires, particularly winter tires, face challenges in maintaining high-speed turning performance on ice both initially and after aging, due to issues with silica dispersion and re-agglomeration, which affect followability and hydrophobicity.

Method used

A rubber composition incorporating isoprene rubber and butadiene rubber with silica filler and a silane coupling agent containing an alkoxysilyl group and sulfur atom, where the organosilicon compound has a carbon chain of 6 or more atoms, enhancing silica dispersibility and preventing re-agglomeration.

Benefits of technology

The composition improves high-speed turning performance on ice and maintains it after aging by ensuring good silica dispersion and hydrophobicity, thereby enhancing overall tire performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581679000001
    Figure 0007581679000001
  • Figure 0007581679000002
    Figure 0007581679000002
  • Figure 0007581679000003
    Figure 0007581679000003
Patent Text Reader

Abstract

To provide a tire rubber composition that achieves overall improvement in high-speed on-ice turning performance, as well as the high-speed on-ice turning performance after aging, and provide a winter tire.SOLUTION: A tire rubber composition contains a rubber component including isoprene rubber and butadiene rubber, a filler including silica, and a silane coupling agent. The silane coupling agent contains an organic silicon compound including alkoxysilyl groups and sulfur atoms, where, carbon atoms connecting the alkoxysilyl groups and sulfur atoms are 6 or more in number.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tires and a winter tire. [Background technology]

[0002] The demand for the market life of tires is increasing year by year, and it is expected that studless tires will be used for a long time. In addition, as roads are improved, it is not uncommon to drive long distances at high speeds with studless tires. Therefore, it is not uncommon for drivers to encounter black ice, where it is difficult to notice that the road surface is frozen by visual inspection, and there is a demand for improved cornering performance in such conditions. In addition, as tires have a longer lifespan, it is thought that good high-speed cornering performance on ice will be required even after aging. Summary of the Invention [Problem to be solved by the invention]

[0003] An object of the present invention is to solve the above problems and to provide a rubber composition for tires and a winter tire which are excellent in overall performance, including high-speed turning performance on ice and high-speed turning performance on ice after aging. [Means for solving the problem]

[0004] The present invention relates to a rubber composition for tires, which comprises a rubber component containing an isoprene-based rubber and a butadiene rubber, a filler containing silica, and a silane coupling agent, wherein the silane coupling agent contains an organosilicon compound that contains an alkoxysilyl group and a sulfur atom and has 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom.

[0005] It is preferable that the content of the silica is 15 to 120 parts by mass per 100 parts by mass of the rubber component, and the content of the organosilicon compound is 0.1 to 20 parts by mass per 100 parts by mass of the silica.

[0006] The silica content in 100% by mass of the filler is preferably 50% by mass or more.

[0007] The silica has a nitrogen adsorption specific surface area of ​​100 m 2 It is preferable that the molecular weight is 1 / g or more.

[0008] The butadiene rubber preferably contains a butadiene rubber having a cis content of 90% by mass or more.

[0009] It is preferable that the rubber composition further contains a resin, and the compounding ratio of the content of the silica to the content of the resin (silica content / resin content) is 2.5 to 10.0.

[0010] It is preferable that the rubber composition further contains short fibers and at least one surfactant selected from the group consisting of fatty acid polyhydric alcohol esters, nonionic ester type surfactants, alkanolamide type surfactants, and sulfonic acid type surfactants.

[0011] The rubber composition preferably further contains a compound represented by the following formula (1). [ka] (In the formula, R 31 R is a divalent hydrocarbon group having 1 to 20 carbon atoms. 32 and R 33 are the same or different and each is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. X is a hydrogen atom, R 34 -COO-, R 34 -CONH- or R 34 is a group represented by -O-, 34 is a hydrocarbon group having 1 to 20 carbon atoms.

[0012] The rubber composition preferably further contains a foaming agent.

[0013] The present invention also relates to a winter tire using the above rubber composition in the tread. Effect of the Invention

[0014] According to the present invention, a rubber composition for tires comprises a rubber component containing an isoprene-based rubber and a butadiene rubber, a filler containing silica, and a silane coupling agent, the silane coupling agent containing an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom, and therefore has excellent overall performance in terms of high-speed cornering performance on ice and high-speed cornering performance on ice after aging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention relates to a rubber composition for tires, which comprises a rubber component containing an isoprene-based rubber and a butadiene rubber, a filler containing silica, and a silane coupling agent, the silane coupling agent containing an alkoxysilyl group and a sulfur atom, and an organosilicon compound in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. The rubber composition is excellent in overall performance in terms of high-speed cornering performance on ice and high-speed cornering performance on ice after aging.

[0016] The reason why the above-mentioned effects are obtained is not entirely clear, but it is presumed that they are due to the following mechanism. In order to improve the performance on ice, isoprene-based rubber and butadiene rubber are preferably used as rubber components and silica is preferably used as a filler in order to obtain the rubber's low-temperature tracking ability, but in such a compounding, silica is easily dispersed in isoprene-based rubber. Therefore, only the isoprene-based rubber phase is reinforced, and hard domains are generated, which results in poor tracking ability and leaves room for improvement in high-speed turning performance on ice. To improve the dispersibility of silica, it is possible to use a silane coupling agent, but if the carbon chain in the silane coupling agent is short, the movement between the silica and the polymer becomes too small, so it is thought that good tracking ability cannot be obtained, as mentioned above. On the other hand, if an organic silicon compound containing an alkoxysilyl group and a sulfur atom and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom is used as the silane coupling agent, the alkoxy group in the compound reacts with the hydroxyl group on the silica surface to hydrophobize the silica surface, and the effect of hydrophobization is greater than that of conventional silane coupling agents due to the long carbon chain of the compound, so it is thought that the dispersibility of silica is significantly improved. Furthermore, since the carbon chain is long and flexible, it is believed that good tracking ability is obtained even on ice, and high-speed turning performance on ice is also improved. In addition, since the hydrophobicity is improved from the conventional one, it is possible to prevent re-aggregation of silica in the rubber over time, and it is believed that good high-speed turning performance on ice is obtained even after aging. It is presumed that the rubber composition exhibits the above-mentioned functions and functions, and thus the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging is significantly improved.

[0017] (Rubber component) The rubber composition contains an isoprene-based rubber and a butadiene rubber (BR) as rubber components.

[0018] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.

[0019] In the rubber composition, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0020] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. In particular, the BR preferably contains high cis BR with a cis content of 90% by mass or more. The cis content is more preferably 95% by mass or more. The cis content can be measured by infrared absorption spectroscopy.

[0021] In addition, the BR may be a non-modified BR or a modified BR. The modified BR may be any BR having a functional group that interacts with a filler such as silica, and examples thereof include terminal-modified BR (terminal-modified BR having the above-mentioned functional group at the terminal) in which at least one terminal of BR has been modified with a compound (modifying agent) having the above-mentioned functional group, main-chain-modified BR having the above-mentioned functional group in the main chain, main-chain terminal-modified BR having the above-mentioned functional group in the main chain and at least one terminal (for example, main-chain terminal-modified BR having the above-mentioned functional group in the main chain and at least one terminal modified with the above-mentioned modifying agent), and terminal-modified BR modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.

[0022] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.

[0023] As the BR, for example, products from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used.

[0024] In the rubber composition, the BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. By keeping the BR content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0025] In the rubber composition, the total content of the isoprene rubber and the BR in 100% by mass of the rubber component is preferably 10% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass. By keeping it within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0026] As a usable rubber component other than isoprene-based rubber and butadiene rubber, for example, other diene-based rubber can be used. Examples of other diene-based rubber include styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Other examples include butyl-based rubber and fluororubber. These may be used alone or in combination of two or more. Among them, SBR is preferred.

[0027] There are no particular limitations on the SBR, and examples of the SBR that can be used include emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. These may be used alone or in combination of two or more kinds.

[0028] The styrene content of the SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The styrene content is preferably 45% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less. By keeping the styrene content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.

[0029] The vinyl bond content of SBR is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. The vinyl bond content is preferably 25% by mass or less, more preferably 15% by mass or less, and even more preferably 13% by mass or less. By keeping it within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.

[0030] The SBR may be unmodified SBR or modified SBR, and the modified SBR may be modified SBR having the same functional group as the modified BR introduced therein.

[0031] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.

[0032] When the rubber composition contains SBR, the content of SBR in 100% by mass of the rubber component is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. The upper limit is preferably 90% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0033] (silica) Silica is blended as a filler in the rubber composition. Usable silica includes dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.

[0034] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 250m 2 / g or less, more preferably 200m 2 By keeping the value within the above range, there is a tendency for the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging to improve. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.

[0035] In the rubber composition, the content of silica is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 50 parts by mass or more, and particularly preferably 60 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, even more preferably 120 parts by mass or less, and particularly preferably 100 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0036] (Silane coupling agent) The silane coupling agent used in the rubber composition contains an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. Such organosilicon compounds may be used alone or in combination of two or more. Among the organosilicon compounds, an organosilicon compound represented by the following average composition formula (I) is preferred. [ka] (In the formula, x represents the average number of sulfur atoms and is 3.5 or more. m represents an integer of 6 or more. 1 ~R 6 are the same or different and each represents an alkyl group or an alkoxy group having 1 to 6 carbon atoms; R 1 ~R 3 At least one of and R4 ~R 6 At least one of R is the alkoxy group. 1 ~R 6 may be a ring structure formed by bonding the alkyl group or the alkoxy group.

[0037] x represents the average number of sulfur atoms in the organosilicon compound, and is preferably 3.5 or more and 12 or less. Here, the average number of sulfur atoms and the number of silicon atoms are values ​​calculated from the molecular weights of the sulfur and silicon atoms in the composition measured by fluorescent X-rays.

[0038] m represents an integer of 6 or more, and preferably 6 or more and 14 or less.

[0039] Alkyl group (R 1 ~R 6 The number of carbon atoms in the alkyl group is preferably 1 to 5. The alkyl group may be linear, branched, or cyclic. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.

[0040] Alkoxy group (R 1 ~R 6 ) preferably has 1 to 5 carbon atoms. The hydrocarbon group in the alkoxy group may be linear, branched, or cyclic. Specific examples include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, and an n-butoxy group.

[0041] R 1 ~R 3 At least one of and R 4 ~R 6 At least one of R is an alkoxy group having 1 to 6 carbon atoms, and preferably R 1 ~R 3 , R 4 ~R 6 At least two of each of these are alkoxy groups having 1 to 6 carbon atoms.

[0042] In addition, R 1 ~R6 may be a ring structure formed by bonding an alkyl group or an alkoxy group having 1 to 6 carbon atoms. For example, (i) R 1 is an ethoxy group, R 2 (ii) R 1 is an ethyl group, R 2 When R forms a ring structure with a methyl group bonded thereto, 1 and R 2 Examples of structures in which divalent groups such as "-O-C2H4-CH2-" and "-C2H4-CH2-" are formed and bonded to Si include

[0043] The organosilicon compound can be prepared, for example, by the manufacturing method described in JP 2018-65954 A. Specifically, the organosilicon compound can be produced by reacting a halogen-containing organosilicon compound of formula (I-1) described in JP 2018-65954 A, anhydrous sodium sulfide represented by Na2S, and sulfur as necessary. When carrying out the above reaction, the addition of sulfur is optional for adjusting the sulfide chain, and may be determined from the blending amount of the compound of the average composition formula (I-1), anhydrous sodium sulfide, and sulfur as necessary, so as to obtain a compound of the desired average composition formula (I). For example, if you want to make the x of the compound of the average composition formula (I) 3.5, you can react 1.0 mol of anhydrous sodium sulfide, 2.5 mol of sulfur, and 2.0 mol of the compound of formula (I-1).

[0044] And, when an organic silicon compound containing an alkoxysilyl group and a sulfur atom and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom is used as a silane coupling agent, that is, a long-chain silane coupling agent, the alkoxy group in the compound reacts with the hydroxyl group on the silica surface to hydrophobize the silica surface, and the effect of hydrophobization is greater than that of conventional silane coupling agents due to the long carbon chain of the compound, so that the dispersibility of silica is significantly improved. In addition, the long-chain structure makes it flexible, and good tracking ability is obtained even on ice, improving high-speed turning performance on ice. Furthermore, since the hydrophobicity is improved more than before, it is possible to prevent re-aggregation of silica in rubber over time, and good high-speed turning performance on ice can be obtained even after aging. Therefore, by using such a long-chain silane coupling agent, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging is significantly improved.

[0045] In the rubber composition, the content of the organosilicon compound is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, the overall performance of high-speed ice turning performance and high-speed ice turning performance after aging tends to improve. The content of the organosilicon compound represented by the average composition formula (I) is also preferably in the same range.

[0046] The rubber composition may contain a silane coupling agent other than the organosilicon compound that contains an alkoxysilyl group and a sulfur atom and has 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom. The other silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide ...3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(2-trimethoxysilylpropyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysil Examples of such silanes include sulfide-based silanes such as rubamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.

[0047] In the rubber composition, the content of the silane coupling agent (the total amount of the organosilicon compound and other silane coupling agents) is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0048] (Other filling materials) The filler other than silica is not particularly limited, and materials known in the rubber field can be used, such as inorganic fillers such as carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, and mica. Of these, carbon black is preferred.

[0049] In the rubber composition, the content of the filler (total content of the fillers) is preferably 5 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 60 parts by mass or more, and particularly preferably 65 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 130 parts by mass or less, even more preferably 120 parts by mass or less, and particularly preferably 100 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0050] In the rubber composition, the silica content in 100% by mass of the filler is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging. The upper limit is not particularly limited, but is preferably 98% by mass or less, and more preferably 95% by mass or less.

[0051] The carbon black that can be used in the rubber composition is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shinnikka Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.

[0052] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m 2 / g or more is preferable, and 70m 2 / g or more is more preferable, and 90m 2 / g or more is more preferable. 2 / g or less is preferable, and 150m 2 / g or less is more preferable, and 130m 2 By keeping the molecular weight within the above range, there is a tendency for the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging to improve. The nitrogen adsorption specific surface area of ​​carbon black can be determined in accordance with JIS K6217-2:2001.

[0053] In the rubber composition, the carbon black content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0054] (Plasticizer) The rubber composition may contain a plasticizer, which is a material that imparts plasticity to the rubber component, and examples of the plasticizer include liquid plasticizers (plasticizers that are in a liquid state at room temperature (25° C.)) and resins (resins that are in a solid state at room temperature (25° C.)).

[0055] In the rubber composition, the content of the plasticizer (total amount of the plasticizer) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 25 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 70 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0056] The liquid plasticizer (a plasticizer in a liquid state at room temperature (25° C.)) that can be used in the rubber composition is not particularly limited, and examples thereof include oil, liquid polymer (liquid resin, liquid diene-based polymer, liquid farnesene-based polymer, etc.), etc. These may be used alone or in combination of two or more kinds.

[0057] In the rubber composition, the content of the liquid plasticizer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0058] Examples of the oil include process oil, vegetable oil, or a mixture thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Co., Ltd. Among these, process oils (paraffin-based process oils, aromatic process oils, naphthenic process oils, etc.) and vegetable oils are preferred.

[0059] In the rubber composition, the oil content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve. The oil content includes the oil contained in the oil extension oil.

[0060] Examples of liquid resins include terpene resins (including terpene phenol resins and aromatic modified terpene resins), rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, dicyclopentadiene (DCPD) resins, coumarone-indene resins (including coumarone and indene simple resins), phenol resins, olefin resins, polyurethane resins, acrylic resins, etc. Hydrogenated products of these resins can also be used.

[0061] In the rubber composition, the content of the liquid resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0062] Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, and liquid farnesene butadiene copolymers that are in a liquid state at 25°C. The ends or main chains of these may be modified with polar groups. Hydrogenated versions of these may also be used.

[0063] In the rubber composition, the content of the liquid diene polymer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0064] Liquid farnesene polymers are polymers obtained by polymerizing farnesene and have structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), but (E)-β-farnesene, which has the following structure, is preferred. [ka]

[0065] The liquid farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer).

[0066] Examples of vinyl monomers include aromatic vinyl compounds such as styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinyltoluene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene, as well as conjugated diene compounds such as butadiene and isoprene. These may be used alone or in combination of two or more. Among these, butadiene is preferred. That is, the farnesene-vinyl monomer copolymer is preferably a copolymer of farnesene and butadiene (farnesene-butadiene copolymer).

[0067] In the farnesene-vinyl monomer copolymer, the copolymerization ratio by mass of farnesene and vinyl monomer (farnesene / vinyl monomer) is preferably 40 / 60 to 90 / 10.

[0068] The liquid farnesene-based polymer that can be suitably used has a weight average molecular weight (Mw) of 3000 to 300,000. The Mw of the liquid farnesene-based polymer is preferably 8000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 50,000 or less.

[0069] In the rubber composition, the content of the liquid farnesene polymer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0070] In the rubber composition, the compounding ratio of the silica content to the total content of liquid polymers (polymers in a liquid state at room temperature (25°C), such as liquid resins, liquid diene polymers, and liquid farnesene polymers) (silica content (parts by mass) per 100 parts by mass of rubber component / total content (parts by mass) of liquid polymers per 100 parts by mass of rubber component) is preferably 1.0 or more, more preferably 4.0 or more, even more preferably 6.0 or more, and particularly preferably 6.5 or more. The upper limit is preferably 15.0 or less, more preferably 10.0 or less, even more preferably 8.0 or less, and particularly preferably 7.5 or less. By keeping it within the above range, there is a tendency that the overall performance of high-speed ice turning performance and high-speed ice turning performance after aging is improved.

[0071] By blending the above resin (a resin that is in a solid state at room temperature (25° C.)) with the rubber composition, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging is improved.

[0072] The reason why such an effect is obtained is not entirely clear, but it is presumed that the effect is due to the following mechanism. By blending the above resin and adjusting the amount of resin to a predetermined range relative to silica as necessary, the resin is more likely to interact with the silica surface bonded to the long-chain silane coupling agent (an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom), and the dispersion of the silica can be further improved. In addition, the adhesive effect of the resin is also obtained, improving the high-speed turning performance on ice. At the same time, it is possible to prevent the resin from re-aggregating over time and creating domains in the polymer phase, so it is thought that it is possible to maintain high high-speed turning performance on ice even after aging. It is presumed that the above-mentioned functions significantly improve the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging.

[0073] Examples of the resins (resins in a solid state at room temperature (25° C.)) that can be used in the rubber composition include aromatic vinyl polymers in a solid state at room temperature (25° C.), coumarone-indene resins, coumarone resins, indene resins, phenolic resins, rosin resins, petroleum resins, terpene resins, and acrylic resins. The resins may be hydrogenated. These may be used alone or in combination of two or more. Of these, aromatic vinyl polymers, petroleum resins, and terpene resins are preferred from the viewpoint of durability of the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging.

[0074] In the rubber composition, the content of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0075] The softening point of the resin is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher. The upper limit is preferably 160° C. or lower, more preferably 130° C. or lower, and even more preferably 115° C. or lower. By keeping the softening point within the above range, good durability during high-speed running tends to be obtained. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.

[0076] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a structural unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.

[0077] In the rubber composition, the content of the aromatic vinyl polymer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0078] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc. The content of the coumarone-indene resin is preferably 1 to 200 parts by mass based on 100 parts by mass of the rubber component.

[0079] The coumarone resin is a resin containing coumarone as a main monomer component constituting the resin skeleton (main chain). The content of the coumarone is preferably 1 to 200 parts by mass based on 100 parts by mass of the rubber component.

[0080] The indene resin is a resin containing indene as a main monomer component constituting the resin skeleton (main chain). The content of the indene resin is preferably 1 to 200 parts by mass based on 100 parts by mass of the rubber component.

[0081] The phenolic resin may be a known one, such as a polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural in the presence of an acid or alkali catalyst. Of these, a polymer obtained by reacting with an acid catalyst (such as a novolac-type phenolic resin) is preferred. The content of the phenolic resin is preferably 1 to 200 parts by mass per 100 parts by mass of the rubber component.

[0082] The rosin resin may be a rosin-based resin such as natural rosin, polymerized rosin, modified rosin, their ester compounds, or their hydrogenated products, etc. The content of the rosin resin is preferably 1 to 200 parts by mass based on 100 parts by mass of the rubber component.

[0083] Examples of the petroleum resin include C5 resin, C9 resin, C5 / C9 resin, dicyclopentadiene (DCPD) resin, and hydrogenated versions of these resins. Of these, DCPD resin and hydrogenated DCPD resin are preferred.

[0084] In the rubber composition, the content of the petroleum resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0085] The terpene resin is a polymer containing terpene as a structural unit. For example, polyterpene resin obtained by polymerizing a terpene compound, aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be mentioned. Hydrogenated products of these can also be used.

[0086] The polyterpene resin is a resin obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.

[0087] Examples of the polyterpene resin include pinene resin, limonene resin, dipentene resin, pinene / limonene resin, etc., which are made from the above-mentioned terpene compounds. Among them, pinene resin is preferable. Pinene resin usually contains both α-pinene and β-pinene, which are isomers, but depending on the components contained, it is classified into β-pinene resin mainly composed of β-pinene and α-pinene resin mainly composed of α-pinene.

[0088] Examples of the aromatic modified terpene resin include terpene phenol resins made from the above terpene compounds and phenolic compounds, and terpene styrene resins made from the above terpene compounds and styrene compounds. Terpene phenol styrene resins made from the above terpene compounds, phenolic compounds, and styrene compounds can also be used. Examples of the phenolic compounds include phenol, bisphenol A, cresol, and xylenol. Examples of the styrene compounds include styrene and α-methylstyrene.

[0089] In the rubber composition, the content of the terpene resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0090] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.

[0091] The solvent-free carboxyl group-containing styrene-acrylic resin is a (meth)acrylic resin (polymer) synthesized by a high-temperature continuous polymerization method (high-temperature continuous bulk polymerization method) (methods described in U.S. Pat. No. 4,414,370, JP-A-59-6207, JP-B-5-58005, JP-A-1-313522, U.S. Pat. No. 5,010,166, Toa Gosei Kenkyuu Nenpo TREND 2000 Vol. 3, p. 42-45, etc.) with minimal use of auxiliary raw materials such as polymerization initiators, chain transfer agents, and organic solvents. In this specification, (meth)acrylic means methacryl and acrylic.

[0092] Examples of the acrylic monomer components constituting the acrylic resin include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters such as 2-ethylhexyl acrylate, aryl esters, aralkyl esters, etc.), (meth)acrylamide, (meth)acrylic acid derivatives such as (meth)acrylamide derivatives, etc. (Meth)acrylic acid is a general term for acrylic acid and methacrylic acid.

[0093] Examples of the aromatic vinyl monomer component constituting the acrylic resin include aromatic vinyls such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene.

[0094] As the monomer components constituting the acrylic resin, other monomer components may be used in addition to the (meth)acrylic acid, (meth)acrylic acid derivatives, and aromatic vinyl. The content of the acrylic resin is preferably 1 to 200 parts by mass based on 100 parts by mass of the rubber component.

[0095] In the rubber composition, the compounding ratio of the silica content to the total content of the above resins (resins in a solid state at room temperature (25°C), such as aromatic vinyl polymers and coumarone-indene resins) (the silica content (parts by mass) per 100 parts by mass of the rubber component / the total content (parts by mass) of the above resins per 100 parts by mass of the rubber component) is preferably 1.0 or more, more preferably 2.5 or more, even more preferably 3.5 or more, and particularly preferably 4.0 or more. The upper limit is preferably 30.0 or less, more preferably 15.0 or less, even more preferably 12.0 or less, and particularly preferably 10.0 or less. By keeping the upper limit within the above range, there is a tendency for the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging to improve.

[0096] Examples of the plasticizer that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.

[0097] The rubber composition may contain short fibers and at least one specific surfactant selected from the group consisting of fatty acid polyhydric alcohol esters, nonionic ester-type surfactants, alkanolamide-type surfactants, and sulfonic acid-type surfactants.

[0098] (Short Fiber) The material of the short fibers is not particularly limited, and short fibers made of ordinary synthetic resins can be appropriately used. Examples of the resin constituting the short fibers include polyethylene, polypropylene, ethylene-vinyl alcohol copolymer, vinyl alcohol homopolymer, poly(meth)acrylic acid or its ester, polyethylene glycol, carboxyvinyl copolymer, styrene-maleic acid copolymer, polyvinylpyrrolidone, vinylpyrrolidone-vinyl acetate copolymer, mercaptoethanol, etc. Among these, ethylene-vinyl alcohol copolymer, vinyl alcohol homopolymer, and poly(meth)acrylic acid are preferred, and ethylene-vinyl alcohol copolymer is more preferred.

[0099] The short fibers have an average length of preferably 0.1 to 500 mm, more preferably 0.1 to 7 mm, an average diameter of preferably 0.001 to 2 mm, more preferably 0.005 to 0.5 mm, and an aspect ratio of preferably 10 to 4,000, more preferably 50 to 2,000.

[0100] In the rubber composition, the content of the short fibers is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 50 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0101] (Surfactant) Examples of fatty acid polyhydric alcohol esters include glycerin monolaurate, glycerin monooleate, glycerin monostearate, glycerin dilaurate, glycerin dioleate, glycerin distearate, glycerin trilaurate, glycerin trioleate, glycerin tristearate, sorbitan monolaurate, sorbitan monooleate, sorbitan monostearate, sorbitan dilaurate, sorbitan dioleate, sorbitan distearate, sorbitan trilaurate, sorbitan trioleate, sorbitan stearate, castor oil, and hydrogenated castor oil.

[0102] Examples of nonionic ester surfactants include polyoxyalkylene glycerin monolaurate, polyoxyalkylene glycerin monooleate, polyoxyalkylene glycerin monostearate, polyoxyalkylene glycerin dilaurate, polyoxyalkylene glycerin dioleate, polyoxyalkylene glycerin distearate, polyoxyalkylene glycerin trilaurate, polyoxyalkylene glycerin trioleate, polyoxyalkylene glycerin tristearate, polyoxyalkylene sorbitan monolaurate, polyoxyalkylene sorbitan monooleate, polyoxyalkylene sorbitan monostearate, polyoxyalkylene sorbitan dilaurate, polyoxyalkylene sorbitan dioleate, polyoxyalkylene sorbitan distearate, polyoxyalkylene sorbitan trilaurate, polyoxyalkylene sorbitan trioleate ... Stearate, polyoxyalkylene castor oil monolaurate, polyoxyalkylene castor oil monooleate, polyoxyalkylene castor oil monostearate, polyoxyalkylene castor oil dilaurate, polyoxyalkylene castor oil dioleate, polyoxyalkylene castor oil distearate, polyoxyalkylene castor oil trilaurate, polyoxyalkylene castor oil trioleate, polyoxyalkylene castor oil tristearate, polyoxyalkylene Examples of the hydrogenated castor oil include polyoxyalkylene hydrogenated castor oil monolaurate, polyoxyalkylene hydrogenated castor oil monooleate, polyoxyalkylene hydrogenated castor oil monostearate, polyoxyalkylene hydrogenated castor oil dilaurate, polyoxyalkylene hydrogenated castor oil dioleate, polyoxyalkylene hydrogenated castor oil distearate, polyoxyalkylene hydrogenated castor oil trilaurate, polyoxyalkylene hydrogenated castor oil trioleate, and polyoxyalkylene hydrogenated castor oil tristearate.

[0103] Examples of alkanolamide type surfactants include lauric acid diethanolamide, coconut fatty acid diethanolamide, myristic acid diethanolamide, palmitic acid diethanolamide, stearic acid diethanolamide, oleic acid diethanolamide, polyoxyethylene octylamide, polyoxyethylene lauryl amide, polyoxyethylene stearyl amide, and polyoxyethylene oleyl amide. Examples of sulfonic acid surfactants include alkyl sulfonates such as sodium octyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, lithium tetradecyl sulfonate, and potassium hexadecylsulfonate; alkyl benzene sulfonates having an alkyl group such as potassium octylbenzene sulfonate and sodium dodecylbenzene sulfonate; sodium 1,2-bis(dibutyloxycarbonyl)-ethanesulfonate, potassium 1,2-bis(dipentyloxycarbonyl)-ethanesulfonate, and lithium 1,2-bis(dihexyloxycarbonyl)-ethanesulfonate. Examples of 1,2-bis(dialkyloxycarbonyl)-ethanesulfonates having an alkyl group include lithium, sodium 1,2-bis(diheptyloxycarbonyl)-ethanesulfonate, sodium 1,2-bis(dioctyloxycarbonyl)-ethanesulfonate, lithium 1,2-bis(dinonyloxycarbonyl)-ethanesulfonate, sodium 1,2-bis(didecyloxycarbonyl)-ethanesulfonate, sodium 1,2-bis(diundecyloxycarbonyl)-ethanesulfonate, and sodium 1,2-bis(didodecyloxycarbonyl)-ethanesulfonate.

[0104] In the rubber composition, the content of the specific surfactant is preferably 0.0003 parts by mass or more, more preferably 0.0005 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 15.0 parts by mass or less, more preferably 10.0 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0105] (Compound represented by the following formula (1)) The rubber composition may contain a compound represented by the following formula (1). [ka] (In the formula, R 31 R is a divalent hydrocarbon group having 1 to 20 carbon atoms. 32 and R 33 are the same or different and each is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. X is a hydrogen atom, R 34 -COO-, R 34 -CONH- or R 34 is a group represented by -O-, 34 is a hydrocarbon group having 1 to 20 carbon atoms.

[0106] R 31 preferably has 2 or more carbon atoms, and preferably has 18 or less carbon atoms, more preferably has 12 or less carbon atoms, further preferably has 8 or less carbon atoms, and particularly preferably has 6 or less carbon atoms. R 31 Examples of the divalent hydrocarbon group in R include an alkylene group, an alkenylene group, an alkylidene group, and an arylene group. 31 is preferably a linear or branched alkylene group or a linear or branched alkenylene group, more preferably a linear alkylene group or a linear alkenylene group.

[0107] R 32 and R 33 With respect to the hydrocarbon group having 1 to 6 carbon atoms in R, the number of carbon atoms in the hydrocarbon group is preferably 1 to 3, and more preferably 1 or 2. 32 and R 33 Examples of the hydrocarbon group having 1 to 6 carbon atoms in R include an alkyl group, an alkenyl group, an aryl group, and an aralkyl group. 32 and R 33 are each preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 32 is a methyl group and R 33 is preferably a hydrogen atom.

[0108] X is a hydrogen atom or R 34 R is preferably a group represented by -COO-. 34 It is more preferable that R is a group represented by -COO-. 34 R preferably has 2 or more carbon atoms, more preferably has 3 or more carbon atoms, and preferably has 18 or less carbon atoms, more preferably has 12 or less carbon atoms, further preferably has 8 or less carbon atoms, and particularly preferably has 6 or less carbon atoms. 34 Examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkyl group, an alkenyl group, an aryl group, and an aralkyl group.

[0109] In the rubber composition, the content of the compound represented by the formula (1) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to be improved.

[0110] (foaming agent) The rubber composition may contain a foaming agent. As the foaming agent, for example, a thermally expandable microcapsule can be used. The thermally expandable microcapsule has a structure in which a thermally expandable substance is encapsulated in a shell material formed of a thermoplastic resin.

[0111] The shell material of the thermally expandable microcapsule can be formed, for example, from a nitrile-based polymer. The thermally expandable substance contained in the shell material of the microcapsule has the property of vaporizing or expanding by heat, and is exemplified by at least one selected from the group consisting of hydrocarbons such as isoalkanes and normal alkanes. Examples of isoalkanes include isobutane, isopentane, 2-methylpentane, 2-methylhexane, and 2,2,4-trimethylpentane, and examples of normal alkanes include n-butane, n-propane, n-hexane, n-heptane, and n-octane. These hydrocarbons may be used alone or in combination. A preferred form of the thermally expandable substance is one in which a hydrocarbon that is gaseous at room temperature is dissolved in a hydrocarbon that is liquid at room temperature.

[0112] As commercially available thermally expandable microcapsules, "EXPANCEL 091DU-80" and "EXPANCEL 092DU-120" manufactured by Expancel, "Microsphere F-85D" and "Microsphere F-100D" manufactured by Matsumoto Yushi Seiyaku Co., Ltd. can be used.

[0113] Further, examples of the foaming agent include dinitrosopentamethylenetetramine (DPT), azodicarbonamide (ADCA), dinitrosopentastyrenetetramine, benzenesulfonyl hydrazide derivatives, oxybisbenzenesulfonyl hydrazide (OBSH), ammonium bicarbonate, sodium bicarbonate, ammonium carbonate which generate carbon dioxide, nitrososulfonyl azo compounds which generate nitrogen, N,N'-dimethyl-N,N'-dinitrosophthalamide, toluenesulfonyl hydrazide, P-toluenesulfonylsemicarbazide, P,P'-oxybis(benzenesulfonylsemicarbazide), and the like.

[0114] Further, the foaming agent may be a normal foaming agent or a foaming agent that kneads salt and dissolves it in water to generate bubbles later. Examples of such foaming agents include water-soluble inorganic salts and water-soluble organic substances. Examples of water-soluble inorganic salts include metal sulfates such as magnesium sulfate and potassium sulfate; metal chlorides such as potassium chloride, sodium chloride, calcium chloride, and magnesium chloride; metal hydroxides such as potassium hydroxide and sodium hydroxide; carbonates such as potassium carbonate and sodium carbonate; phosphates such as sodium hydrogen phosphate and sodium dihydrogen phosphate; and the like. Examples of water-soluble organic substances include lignin derivatives and sugars. Examples of lignin derivatives include lignin sulfonic acid and lignin sulfonate salts. The lignin derivative may be obtained by either the sulfite pulp method or the kraft pulp method.

[0115] In the rubber composition, the content of the foaming agent is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 15 parts by mass or less. By keeping the content within the above range, the overall performance of high-speed turning performance on ice and high-speed turning performance on ice after aging tends to improve.

[0116] (Other materials) From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition preferably contains an antioxidant.

[0117] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.

[0118] In the rubber composition, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, more preferably 4.0 parts by mass or less.

[0119] The rubber composition preferably contains stearic acid. The content of stearic acid in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0120] As the stearic acid, any known stearic acid can be used, for example, products available from NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.

[0121] The rubber composition preferably contains zinc oxide. The content of zinc oxide in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0122] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.

[0123] The rubber composition may contain wax. The content of the wax in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0124] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.

[0125] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.

[0126] It is preferable to compound sulfur in the rubber composition, in order to form an appropriate amount of crosslinked chains in the polymer chains and to impart good performance.

[0127] In the rubber composition, the amount of sulfur is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and even more preferably 0.5 part by mass or more, based on 100 parts by mass of the rubber component. The amount is preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.

[0128] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0129] The rubber composition preferably contains a vulcanization accelerator. In the rubber composition, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.

[0130] The type of vulcanization accelerator is not particularly limited, and any commonly used accelerator can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.

[0131] In addition to the above-mentioned components, the rubber composition may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.

[0132] The rubber composition can be produced by a known method, for example, by kneading the components using a rubber kneading device such as an open roll or a Banbury mixer, followed by vulcanization.

[0133] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 50 to 200°C, preferably 80 to 190°C, and the kneading time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100°C or lower, preferably room temperature to 80°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 120 to 200°C, preferably 140 to 180°C.

[0134] The rubber composition can be preferably used for each component of a pneumatic tire such as a tread (cap tread), a sidewall, a base tread, a bead apex, a clinch apex, an inner liner, an under tread, a breaker topping, a braid topping, a tread, etc. Among them, the rubber composition can be preferably used for a tread (cap tread).

[0135] A tire is manufactured by a conventional method using a rubber composition. That is, the rubber composition containing the above-mentioned components is extruded in an unvulcanized state to match the shape of a tread, etc., and molded together with other tire components in a conventional manner on a tire building machine to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.

[0136] Examples of the tire include pneumatic tires and non-pneumatic tires. Among them, pneumatic tires are preferred. The tire can be suitably used as a winter tire (studless tire, snow tire, studded tire, etc.). The tire can be suitably used as a passenger car tire, a large passenger car tire, a large SUV tire, a heavy load tire such as a truck or a bus, a light truck tire, a two-wheeled vehicle tire, a racing tire (high performance tire), etc. Among them, the tire can be suitably used as a passenger car tire. EXAMPLES

[0137] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0138] Various chemicals used in the examples and comparative examples will be collectively described below. NR:RSS#3 BR1: BR730 manufactured by JSR Corporation (rare earth BR synthesized using a Nd-based catalyst, cis content 97% by mass, vinyl content 0.9% by mass) BR2: N103 (vinyl content 12% by mass, cis content 38% by mass) manufactured by Asahi Kasei Chemicals Corporation Carbon black: Mitsubishi Chemical Corporation's Seast N220 (N2SA114m 2 / g) Silica: Ultrasil VN3 (N2SA175m) manufactured by Evonik Degussa 2 / g) Organosilicon compound 1: Silane coupling agent synthesized in Production Example 1 below Organosilicon compound 2: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Wax: Ozoace wax made by Nippon Seiro Co., Ltd. Anti-aging agent: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6PPD)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Oil: PS-32 (mineral oil) manufactured by Idemitsu Kosan Co., Ltd. Resin 1: SYLVARES SA85 manufactured by Arizona Chemical (copolymer of α-methylstyrene and styrene, Tg 43°C, softening point 85°C) Resin 2: YS Resin PX1150 (polyterpene (β-pinene resin), softening point 115°C) manufactured by Yasuhara Chemical Co., Ltd. Resin 3: ExxonMobil PR120 (hydrogenated DCPD resin, softening point 120°C) Liquid butadiene polymer: Sartomer's Licon 150 (Mn5200) Liquid farnesene polymer: Kuraray's L-FBR-742 (liquid farnesene butadiene copolymer, SP value 8.1) Short fiber: Polyethylene (PE) fiber with a fiber diameter of 10 μm Surfactant 1: Rheodol SP-L10 (fatty acid polyhydric alcohol ester) manufactured by Kao Corporation Surfactant 2: Rheodol TW-L120 (non-ionic ester type surfactant) manufactured by Kao Corporation Surfactant 3: Nimeen O-205 (alkanolamide surfactant) manufactured by NOF Corporation Surfactant 4: Newcol 211-MB (sulfonic acid surfactant) manufactured by Nippon Nyukazai Co., Ltd. Thermally expandable microcapsules: Matsumoto Yushi Pharmaceutical Co., Ltd. Microsphere F100 Magnesium sulfate: MN-00 (magnesium sulfate, median particle size: 75 μm) manufactured by Mai Chemical Industry Co., Ltd. Stearic acid: Paulownia wood produced by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccela NS (N-tert-butyl-2-benzothiazylsulfenamide (TBBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0139] (Production Example 1: Synthesis of Organosilicon Compound 1) A 2L separable flask equipped with a stirrer, reflux condenser, dropping funnel and thermometer was charged with 78.0g (1.0 mol) of anhydrous sodium sulfide, 80.3g (2.5 mol) of sulfur and 480g of ethanol, and heated to 80°C. 566g (2.0 mol) of 6-chlorohexyltriethoxysilane was added dropwise thereto, and the mixture was heated and stirred at 80°C for 10 hours. The reaction liquid was filtered under pressure using a filter plate to obtain a filtrate from which the salt generated as the reaction proceeded was removed. The obtained filtrate was heated to 100°C, and ethanol was distilled off under a reduced pressure of 10mmHg or less to obtain an organosilicon compound 1 (silane coupling agent) as a reaction product. The obtained organosilicon compound 1 had a sulfur content of 18.5% by mass, the average number of sulfur atoms X contained in one molecule of the organosilicon compound was 3.5, and the value of m was 6.

[0140] (Production Example 1: Synthesis of compound represented by formula (1)) In a 200mL four-neck flask equipped with a dropping funnel and a stirrer equipped with a borosilicate glass rod with a polytetrafluoroethylene (PTFE) stirring blade, 18.8g (0.150 mol) of 6-methylisocytosine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 130mL of dimethyl sulfoxide were charged under nitrogen flow and heated to 150°C while mixing. While maintaining the mixed liquid at 150°C, 25.6g (0.165 mol) of isocyanate ethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was dropped over 30 minutes and maintained at 150°C for 30 minutes. The resulting reaction liquid was cooled to room temperature, then mixed with 1300mL of methanol, and a white solid was precipitated and collected by filtration. The resulting white solid was a compound represented by the following formula. [ka]

[0141] <Examples and Comparative Examples> According to the compounding recipes shown in each table, polymers and compounding chemicals were added using a 1.7 L Banbury mixer, and the mixture was kneaded for 3 minutes at 150°C to obtain a kneaded product. Sulfur and a vulcanization accelerator were added, and the mixture was kneaded for 2 minutes at 100°C using an open roll to obtain an unvulcanized rubber composition. Each of the obtained unvulcanized rubber compositions was molded into the shape of a cap tread, laminated together with other tire components, and vulcanized at 170°C for 15 minutes to produce a winter test tire (tire size: 195 / 65R15).

[0142] The following evaluations were carried out on the obtained winter test tires. The evaluation results are shown in the tables. In addition, in Tables 1, 2, 3, and 4, Comparative Examples 1-8, 2-1, 3-2, and 4-2 were used as the reference comparative examples, respectively.

[0143] <High-speed turning performance on ice (when new)> A domestically manufactured 2000cc car was fitted with winter test tires on all wheels, and made to make a steady turn on an icy road surface while gradually increasing the speed from 10km / h, and the speed at which the driver felt slippage was indexed, with the standard comparison example being set at 100. The higher the index, the better the high-speed ice turning performance. (High-speed ice cornering performance) = (speed (km / h) at which the driver felt slippage for each winter test tire) / (speed (km / h) at which the driver felt slippage for the reference comparative example) x 100

[0144] <High-speed turning performance on ice (after aging)> The rim-mounted winter test tires were heat-treated at 80°C for two weeks, and then the aging performance on high-speed ice was evaluated using the same method as for "high-speed ice turning performance" above. The higher the index, the better the aging performance on high-speed ice.

[0145] [Table 1]

[0146] [Table 2]

[0147] [Table 3]

[0148] [Table 4]

[0149] As can be seen from each table, the example tires which contained a rubber component containing isoprene-based rubber and butadiene rubber, a filler containing silica, and a silane coupling agent, wherein the silane coupling agent contained an alkoxysilyl group and a sulfur atom and contained an organosilicon compound having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom, had excellent overall performance (expressed as the sum of two indices of high-speed turning performance on ice and high-speed turning performance on ice after aging) of high-speed turning performance on ice.

Claims

1. The rubber composition includes a rubber component including an isoprene-based rubber and a butadiene rubber, a filler including silica, and a silane coupling agent, The silane coupling agent is a rubber composition for tires, which contains an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, a content of the isoprene-based rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, and a content of the butadiene rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, The rubber composition for tires, wherein the organosilicon compound is a compound represented by the following average composition formula (I): 【Chemistry 1】 (In the formula, x represents the average number of sulfur atoms and is 3.5 or more. m represents an integer of 6 or more. R 1 ~R 6 are the same or different and each represents an alkyl group or an alkoxy group having 1 to 6 carbon atoms; R 1 ~R 3 and R 4 ~R 6 At least one of R is the alkoxy group. 1 ~R 6 may be a ring structure formed by bonding the alkyl group or the alkoxy group.

2. The rubber composition includes a rubber component including an isoprene-based rubber and a butadiene rubber, a filler including silica, and a silane coupling agent, The silane coupling agent is a rubber composition for tires, which contains an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, a content of the isoprene-based rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, and a content of the butadiene rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, The rubber composition for tires further comprises a compound represented by the following formula (1): 【Chemistry 2】 (In the formula, R 31 R is a divalent hydrocarbon group having 1 to 20 carbon atoms. 32 and R 33 are the same or different and each is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. X is a hydrogen atom, R 34 -COO-, R 34 -CONH- or R 34 is a group represented by —O—, and R 34 is a hydrocarbon group having 1 to 20 carbon atoms.

3. The rubber composition includes a rubber component including an isoprene-based rubber and a butadiene rubber, a filler including silica, a silane coupling agent, and a liquid polymer, The silane coupling agent is a rubber composition for tires, which contains an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and in which the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, a content of the isoprene-based rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, and a content of the butadiene rubber in 100% by mass of the rubber component is 5% by mass or more and 95% by mass or less, A rubber composition for tires, in which a compounding ratio of the content of the silica to the total content of the liquid polymers (the content of the silica (parts by mass) per 100 parts by mass of the rubber component / the total content of the liquid polymers (parts by mass) per 100 parts by mass of the rubber component) is 1.0 or more and 15.0 or less.

4. 3. The rubber composition for tires according to claim 1, wherein a compounding ratio of a content of silica to a total content of the liquid polymer (a content of silica (parts by mass) per 100 parts by mass of the rubber component / a total content of the liquid polymer (parts by mass) per 100 parts by mass of the rubber component) is 1.0 or more and 15.0 or less.

5. 5. The rubber composition for tires according to claim 1, wherein the content of the silica is 15 to 120 parts by mass per 100 parts by mass of the rubber component, and the content of the organosilicon compound is 0.1 to 20 parts by mass per 100 parts by mass of the silica.

6. The rubber composition for tires according to any one of claims 1 to 5, wherein the silica content in 100% by mass of the filler is 50% by mass or more.

7. The silica has a nitrogen adsorption specific surface area of ​​100 m 2 The rubber composition for tires according to any one of claims 1 to 6, wherein the viscosity is 1 / g or more.

8. The rubber composition for tires according to any one of claims 1 to 7, wherein the butadiene rubber contains a butadiene rubber having a cis content of 90% by mass or more.

9. The rubber composition for tires according to any one of claims 1 to 8, further comprising a resin, and a compounding ratio of the content of the silica to the content of the resin (silica content / resin content) is 2.5 to 10.

0.

10. The rubber composition for a tire according to any one of claims 1 to 9, further comprising short fibers and at least one surfactant selected from the group consisting of fatty acid polyhydric alcohol esters, nonionic ester type surfactants, alkanolamide type surfactants and sulfonic acid type surfactants.

11. The rubber composition for tires according to claim 1 or 3, further comprising a compound represented by the following formula (1): 【Chemistry 3】 (In the formula, R 31 R is a divalent hydrocarbon group having 1 to 20 carbon atoms. 32 and R 33 are the same or different and each is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. X is a hydrogen atom, R 34 -COO-, R 34 -CONH- or R 34 is a group represented by —O—, and R 34 is a hydrocarbon group having 1 to 20 carbon atoms.

12. The rubber composition for tires according to any one of claims 1 to 11, further comprising a foaming agent.

13. A winter tire having a tread made of the rubber composition according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Methods for synthesizing supramolecular materials

    JP2011522909A

  • Tire rubber composition and pneumatic tire

    JP2016151016A

  • Method for producing rubber composition, rubber composition, and tire

    JP2017128649A

  • Tire rubber composition and pneumatic tire

    JP2018065954A

  • Rubber composition for tire, and pneumatic tire

    JP2019108450A