Rubber composition for tires and tires
The rubber composition with isoprene rubber, styrene-butadiene rubber, silica, and a specific silane coupling agent addresses uneven silica distribution, enhancing fuel efficiency and TGC resistance by promoting uniform silica dispersion.
Patent Information
- Application Number
- JP2020120632
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-14
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-07-14
AI Technical Summary
The use of isoprene rubber and styrene-butadiene rubber with minimized silica content leads to uneven silica distribution, resulting in tread groove cracks (TGC) and inadequate TGC resistance performance.
A rubber composition containing isoprene rubber, styrene-butadiene rubber, silica, and a silane coupling agent with an alkoxysilyl group and sulfur atom, where the organosilicon compound has six or more carbon atoms connecting the alkoxysilyl group and sulfur atom, enhancing silica dispersion and improving TGC resistance.
The composition achieves improved fuel efficiency and TGC resistance by ensuring uniform silica distribution, reducing tread groove cracks.
Smart Images

Figure 0007581681000001 
Figure 0007581681000002 
Figure 0007581681000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]
[0002] In recent years, in order to reduce rolling resistance, a method has been proposed in which isoprene rubber and styrene-butadiene rubber are used as rubber components, and silica is used as a reinforcing agent, while the amount of silica blended is minimized. However, when the amount of silica is small, it is difficult to apply shear to the silica, making it difficult to disperse it sufficiently, and it is unevenly distributed in the isoprene rubber, which causes Tread Groove Cracks (TGCs) to occur at the bottom of the main grooves of the tread, resulting in a decrease in the performance of suppressing the progression of cracks at the bottom of the grooves (TGC resistance). Summary of the Invention [Problem to be solved by the invention]
[0003] The present invention has an object to provide a rubber composition for tires and a tire that solves the above problems and improves the overall performance of fuel efficiency and the performance of inhibiting the progression of cracks at the groove bottom (TGC resistance). [Means for solving the problem]
[0004] The present invention relates to a rubber composition for tires, which comprises a rubber component containing an isoprene-based rubber and a styrene-butadiene rubber, a filler containing silica, and a silane coupling agent, wherein the silane coupling agent contains an organosilicon compound that contains an alkoxysilyl group and a sulfur atom and has 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom.
[0005] The rubber composition preferably has an acetone extractable amount (AE amount) of 15.0 mass % or less.
[0006] It is preferable that the silica content and the amount of acetone extraction (AE amount) in the rubber composition satisfy the following formulas (1) and (2). (1) Silica content ≦30.0% by mass (2) Silica content / AE amount ≧ 2.0
[0007] The amount of the filler per 100 parts by mass of the rubber component is preferably 65 parts by mass or less.
[0008] The amount of silica per 100 parts by mass of the rubber component is preferably 60 parts by mass or less.
[0009] Nitrogen adsorption specific surface area 180m 2 It is preferable that the silica content is at least 1 / g.
[0010] The amount of the plasticizer per 100 parts by mass of the rubber component is preferably 20 parts by mass or less.
[0011] The total content of silica and plasticizer is preferably 80 parts by mass or less based on 100 parts by mass of the rubber component.
[0012] It is preferable that the resin contains at least one selected from the group consisting of terpene resins, C5 resins, C9 resins, C5 / C9 resins, and hydrogenated dicyclopentadiene resins.
[0013] The present invention also relates to a tire having a tire component made of the rubber composition.
[0014] Preferably, the tire component is a tread. Effect of the Invention
[0015] According to the present invention, the rubber composition for tires includes a rubber component containing an isoprene-based rubber and a styrene-butadiene rubber, a filler containing silica, and a silane coupling agent, and the silane coupling agent includes an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom, so that the overall performance of fuel efficiency and the performance of inhibiting the progression of cracks at the groove bottom (TGC resistance) can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention relates to a rubber composition for tires, which comprises a rubber component containing isoprene-based rubber and styrene-butadiene rubber, a filler containing silica, and a silane coupling agent, the silane coupling agent containing an organosilicon compound containing an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. The rubber composition can improve the overall performance of fuel economy and the performance of suppressing the progression of cracks at the bottom of the grooves (TGC resistance).
[0017] The reason why the above-mentioned effects are obtained is not entirely clear, but it is presumed that they are due to the following mechanism. As mentioned above, when isoprene-based rubber and styrene-butadiene rubber are used as rubber components and silica is used as a filler for the purpose of reducing rolling resistance, it is difficult to disperse silica sufficiently, and the silica is unevenly distributed on the isoprene-based rubber side, which causes cracks to progress at the bottom of the grooves and reduces TGC resistance. In this regard, by using an organic silicon compound containing an alkoxysilyl group and a sulfur atom as a silane coupling agent and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom, that is, a long-chain silane coupling agent, silica becomes easy to disperse in both the isoprene-based rubber and the styrene-butadiene rubber, the progress of cracks at the bottom of the grooves is suppressed, and good TGC resistance is obtained. Therefore, it is presumed that the rubber composition significantly improves the overall performance of fuel efficiency and the performance of suppressing the progress of cracks at the bottom of the grooves (TGC resistance).
[0018] (Rubber component) The rubber composition contains an isoprene-based rubber and a styrene-butadiene rubber (SBR) as rubber components.
[0019] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.
[0020] When the rubber composition contains an isoprene-based rubber, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, and particularly preferably 50% by mass or less. By keeping it within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0021] The SBR is not particularly limited, and for example, emulsion polymerized styrene butadiene rubber (E-SBR), solution polymerized styrene butadiene rubber (S-SBR), etc. can be used. These may be used alone or in combination of two or more kinds.
[0022] The styrene content of the SBR is preferably 5% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. The styrene content is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 28% by mass or less. By keeping the styrene content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.
[0023] The vinyl bond content of SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 12% by mass or more. The vinyl bond content is preferably 35% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. By keeping it within the above range, the overall performance of fuel economy and TGC resistance tends to be improved. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.
[0024] The SBR may be unmodified or modified. In addition, hydrogenated styrene-butadiene copolymer (hydrogenated SBR) may also be used as the SBR.
[0025] The modified SBR may be any SBR having a functional group that interacts with a filler such as silica, and examples thereof include terminal-modified SBR in which at least one end of SBR has been modified with a compound (modifying agent) having the above-mentioned functional group (terminal-modified SBR having the above-mentioned functional group at the end), main-chain-modified SBR having the above-mentioned functional group in the main chain, main-chain terminal-modified SBR having the above-mentioned functional group in the main chain and at least one end (for example, main-chain terminal-modified SBR having the above-mentioned functional group in the main chain and at least one end modified with the above-mentioned modifier), and terminal-modified SBR modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.
[0026] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0027] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.
[0028] The content of SBR in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more. The upper limit is preferably 95% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less. By keeping it within the above range, the overall performance of fuel economy performance and TGC resistance performance tends to be improved.
[0029] As a rubber component that can be used other than isoprene-based rubber and SBR, for example, other diene-based rubbers can be used. Examples of other diene-based rubbers include butadiene rubber (BR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), acrylonitrile butadiene rubber (NBR), etc. In addition, butyl-based rubber, fluororubber, etc. can also be used. These may be used alone or in combination of two or more.
[0030] (silica) Silica is blended as a filler in the rubber composition. Usable silica includes dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.
[0031] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 150m 2 / g or more, more preferably 160m 2 / g or more, particularly preferably 180m 2 / g or more, 210m 2 The upper limit of the N2SA of the silica is not particularly limited, but is preferably 600 m 2 / g or less, more preferably 350m 2 / g or less, more preferably 260m 2 By keeping the content within the above range, there is a tendency for the overall performance of fuel efficiency and TGC resistance to improve. 2 By using silica having a silica content of 100 / g or more, it is possible to obtain good reinforcing properties even with a small amount of silica blended. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.
[0032] In the rubber composition, the content of silica is preferably 5 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 35 parts by mass or more, and particularly preferably 45 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0033] (Silane coupling agent) The silane coupling agent used in the rubber composition contains an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more. Such organosilicon compounds may be used alone or in combination of two or more. Among the organosilicon compounds, an organosilicon compound represented by the following average composition formula (I) is preferred. [ka] (In the formula, x represents the average number of sulfur atoms and is 3.5 or more. m represents an integer of 6 or more. 1 ~R 6 are the same or different and each represents an alkyl group or an alkoxy group having 1 to 6 carbon atoms; R 1 ~R 3 At least one of and R 4 ~R 6 At least one of R is the alkoxy group. 1 ~R 6 may be a ring structure formed by bonding the alkyl group or the alkoxy group.
[0034] x represents the average number of sulfur atoms in the organosilicon compound, and is preferably 3.5 or more and 12 or less. Here, the average number of sulfur atoms and the number of silicon atoms are values calculated from the molecular weights of the sulfur and silicon atoms in the composition measured by fluorescent X-rays.
[0035] m represents an integer of 6 or more, and preferably 6 or more and 14 or less.
[0036] Alkyl group (R 1 ~R 6 The number of carbon atoms in the alkyl group is preferably 1 to 5. The alkyl group may be linear, branched, or cyclic. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.
[0037] Alkoxy group (R 1 ~R6 ) preferably has 1 to 5 carbon atoms. The hydrocarbon group in the alkoxy group may be linear, branched, or cyclic. Specific examples include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, and an n-butoxy group.
[0038] R 1 ~R 3 At least one of and R 4 ~R 6 At least one of R is an alkoxy group having 1 to 6 carbon atoms, and preferably R 1 ~R 3 , R 4 ~R 6 At least two of each of these are alkoxy groups having 1 to 6 carbon atoms.
[0039] In addition, R 1 ~R 6 may be a ring structure formed by bonding an alkyl group or an alkoxy group having 1 to 6 carbon atoms. For example, (i) R 1 is an ethoxy group, R 2 (ii) R 1 is an ethyl group, R 2 When R forms a ring structure with a methyl group bonded thereto, 1 and R 2 Examples of structures in which divalent groups such as "-O-C2H4-CH2-" and "-C2H4-CH2-" are formed and bonded to Si include
[0040] The organosilicon compound can be prepared, for example, by the manufacturing method described in JP 2018-65954 A. Specifically, the organosilicon compound can be produced by reacting a halogen-containing organosilicon compound of formula (I-1) described in JP 2018-65954 A, anhydrous sodium sulfide represented by Na2S, and sulfur as necessary. When carrying out the above reaction, the addition of sulfur is optional for adjusting the sulfide chain, and may be determined from the blending amount of the compound of the average composition formula (I-1), anhydrous sodium sulfide, and sulfur as necessary, so as to obtain a compound of the desired average composition formula (I). For example, if you want to make the x of the compound of the average composition formula (I) 3.5, you can react 1.0 mol of anhydrous sodium sulfide, 2.5 mol of sulfur, and 2.0 mol of the compound of formula (I-1).
[0041] And, when an organic silicon compound containing an alkoxysilyl group and a sulfur atom and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom is used as a silane coupling agent, that is, a long-chain silane coupling agent, the alkoxy group in the compound reacts with the hydroxyl group on the silica surface to hydrophobize the silica surface, and the effect of hydrophobization is greater than that of conventional silane coupling agents due to the long carbon chain of the compound, so that the dispersibility of silica can be significantly improved. Therefore, even in a compounding that reduces rolling resistance by using isoprene-based rubber and styrene-butadiene rubber as the rubber component and silica as the filler, silica can be uniformly dispersed in both the isoprene-based rubber and the styrene-butadiene rubber, the progression of cracks at the bottom of the grooves is suppressed, and good TGC resistance performance can be obtained. Therefore, by using such a long-chain silane coupling agent, it is possible to significantly improve the overall performance of fuel efficiency and TGC resistance.
[0042] In the rubber composition, the content of the organosilicon compound is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, the overall performance of fuel economy and TGC resistance tends to be improved. The content of the organosilicon compound represented by the average composition formula (I) is also preferably within the same range.
[0043] The rubber composition may contain a silane coupling agent other than the organosilicon compound that contains an alkoxysilyl group and a sulfur atom and has 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom. The other silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide ...3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(2-trimethoxysilylpropyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysil Examples of such silanes include sulfide-based silanes such as rubamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.
[0044] In the rubber composition, the content of the silane coupling agent (the total amount of the organic silicon compound and other silane coupling agents) is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. By keeping it within the above range, the overall performance of fuel efficiency and TGC resistance tends to be improved.
[0045] (Other filling materials) The filler other than silica is not particularly limited, and materials known in the rubber field can be used, such as inorganic fillers such as carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, and mica. Of these, carbon black is preferred.
[0046] In the rubber composition, the content of the filler (total content of the fillers) is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 40 parts by mass or more, and particularly preferably 50 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 85 parts by mass or less, and particularly preferably 65 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0047] The carbon black that can be used in the rubber composition is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shinnikka Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0048] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m 2 / g or more is preferable, and 70m 2 / g or more is more preferable, and 90m 2 / g or more is more preferable. 2 / g or less is preferable, and 150m 2 / g or less is more preferable, and 130m 2 By setting the content within the above range, there is a tendency for the overall performance of fuel economy and TGC resistance to be improved. The nitrogen adsorption specific surface area of carbon black can be determined in accordance with JIS K6217-2:2001.
[0049] In the rubber composition, the carbon black content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0050] (Plasticizer) The rubber composition may contain a plasticizer. A plasticizer is a material that imparts plasticity to a rubber component, and examples of the plasticizer include liquid plasticizers (plasticizers that are in a liquid state at room temperature (25° C.)) and resins (resins that are in a solid state at room temperature (25° C.)).
[0051] In the rubber composition, the content of the plasticizer (total amount of the plasticizer) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 12 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 15 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0052] In particular, when the amount of filler is small, the silica is not easily subjected to shear during mixing, and tends to be poorly dispersed or dispersed only in the isoprene-based rubber phase, but when the organic silicon compound is used with a reduced amount of plasticizer, shear is easily applied, and the effect of the silane coupling agent promotes dispersion even in a compounding system with a low amount of filler. As a result, it is presumed that sufficient reinforcing properties are obtained even with a small amount of filler, and the overall performance of fuel efficiency and TGC resistance is significantly improved.
[0053] The liquid plasticizer (a plasticizer in a liquid state at room temperature (25° C.)) that can be used in the rubber composition is not particularly limited, and examples thereof include oil, liquid polymer (liquid resin, liquid diene-based polymer, liquid farnesene-based polymer, etc.), etc. These may be used alone or in combination of two or more kinds.
[0054] In the rubber composition, the content of the liquid plasticizer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel efficiency and TGC resistance tends to be improved.
[0055] Examples of the oil include process oil, vegetable oil, or a mixture thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Co., Ltd. Among these, process oils (paraffin-based process oils, aromatic process oils, naphthenic process oils, etc.) and vegetable oils are preferred.
[0056] In the rubber composition, the content of the oil is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved. The oil content includes the oil contained in the extender oil.
[0057] Examples of liquid resins include terpene resins (including terpene phenol resins and aromatic modified terpene resins) that are liquid at 25° C., rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, dicyclopentadiene (DCPD) resins, coumarone-indene resins (including coumarone and indene simple resins), phenol resins, olefin resins, polyurethane resins, acrylic resins, etc. Hydrogenated versions of these resins can also be used.
[0058] In the rubber composition, the content of the liquid resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0059] Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, and liquid farnesene butadiene copolymers that are in a liquid state at 25°C. The ends or main chains of these may be modified with polar groups. Hydrogenated versions of these may also be used.
[0060] In the rubber composition, the content of the liquid diene polymer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping it within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0061] Liquid farnesene polymers are polymers obtained by polymerizing farnesene and have structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), but (E)-β-farnesene, which has the following structure, is preferred. [ka]
[0062] The liquid farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer).
[0063] Examples of vinyl monomers include aromatic vinyl compounds such as styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinyltoluene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene, as well as conjugated diene compounds such as butadiene and isoprene. These may be used alone or in combination of two or more. Among these, butadiene is preferred. That is, the farnesene-vinyl monomer copolymer is preferably a copolymer of farnesene and butadiene (farnesene-butadiene copolymer).
[0064] In the farnesene-vinyl monomer copolymer, the copolymerization ratio by mass of farnesene and vinyl monomer (farnesene / vinyl monomer) is preferably 40 / 60 to 90 / 10.
[0065] The liquid farnesene-based polymer that can be suitably used has a weight average molecular weight (Mw) of 3000 to 300,000. The Mw of the liquid farnesene-based polymer is preferably 8000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 50,000 or less.
[0066] In the rubber composition, the content of the liquid farnesene polymer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 20 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0067] Examples of the resins (resins in a solid state at room temperature (25°C)) that can be used in the rubber composition include aromatic vinyl polymers in a solid state at room temperature (25°C), coumarone-indene resins, coumarone resins, indene resins, phenolic resins, rosin resins, petroleum resins, terpene resins, and acrylic resins. The resins may be hydrogenated. These may be used alone or in combination of two or more. Among these, from the viewpoint of durability of the overall performance of fuel economy and TGC resistance, aromatic vinyl polymers, petroleum resins, and terpene resins are preferred, and petroleum resins and terpene resins are more preferred.
[0068] When the rubber composition contains the above resin (a resin in a solid state at room temperature (25°C)), the content thereof is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, there is a tendency for the overall performance of fuel economy and TGC resistance to be improved.
[0069] The softening point of the resin is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher. The upper limit is preferably 160° C. or lower, more preferably 130° C. or lower, and even more preferably 115° C. or lower. By keeping the softening point within the above range, good overall performance in terms of fuel economy and TGC resistance tends to be obtained. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.
[0070] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a structural unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.
[0071] When the rubber composition contains the aromatic vinyl polymer, the content thereof is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0072] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc. The content of the coumarone-indene resin is preferably 1 to 100 parts by mass based on 100 parts by mass of the rubber component.
[0073] The coumarone resin is a resin containing coumarone as a main monomer component constituting the skeleton (main chain) of the resin. The content of the coumarone is preferably 1 to 100 parts by mass based on 100 parts by mass of the rubber component.
[0074] The indene resin is a resin containing indene as a main monomer component constituting the resin skeleton (main chain). The content of the indene resin is preferably 1 to 100 parts by mass based on 100 parts by mass of the rubber component.
[0075] The phenolic resin may be a known polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural in the presence of an acid or alkali catalyst. Of these, a polymer obtained by reacting with an acid catalyst (such as a novolac-type phenolic resin) is preferred. The content of the phenolic resin is preferably 1 to 100 parts by mass per 100 parts by mass of the rubber component.
[0076] The rosin resin may be a rosin-based resin such as natural rosin, polymerized rosin, modified rosin, their ester compounds, their hydrogenated products, etc. The content of the rosin resin is preferably 1 to 100 parts by mass based on 100 parts by mass of the rubber component.
[0077] Examples of the petroleum resin include C5 resin, C9 resin, C5 / C9 resin, dicyclopentadiene (DCPD) resin, and hydrogenated products thereof. Among them, from the viewpoint of the overall performance of fuel economy and TGC resistance, C5 resin, C9 resin, C5 / C9 resin, and hydrogenated DCPD resin are preferred. These resins are highly compatible with either or both of isoprene rubber and SBR, and enable the entire composition to be homogenized, so that it is presumed that the overall performance is significantly improved.
[0078] When the rubber composition contains the petroleum resin, the content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0079] The terpene resin is a polymer containing terpene as a structural unit, and examples thereof include polyterpene resin obtained by polymerizing a terpene compound, and aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound. Hydrogenated products of these resins can also be used. Terpene resins are highly compatible with either or both of isoprene rubber and SBR, and the entire composition can be homogenized, so that it is presumed that the overall performance of fuel economy and TGC resistance is significantly improved.
[0080] The polyterpene resin is a resin obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.
[0081] Examples of the polyterpene resin include pinene resin, limonene resin, dipentene resin, pinene / limonene resin, etc., which are made from the above-mentioned terpene compounds. Among them, pinene resin is preferable. Pinene resin usually contains both α-pinene and β-pinene, which are isomers, but depending on the components contained, it is classified into β-pinene resin mainly composed of β-pinene and α-pinene resin mainly composed of α-pinene.
[0082] Examples of the aromatic modified terpene resin include terpene phenol resins made from the above terpene compounds and phenolic compounds, and terpene styrene resins made from the above terpene compounds and styrene compounds. Terpene phenol styrene resins made from the above terpene compounds, phenolic compounds, and styrene compounds can also be used. Examples of the phenolic compounds include phenol, bisphenol A, cresol, and xylenol. Examples of the styrene compounds include styrene and α-methylstyrene.
[0083] When the rubber composition contains the terpene resin, the content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and may be 10 parts by mass or less. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0084] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.
[0085] The solvent-free carboxyl group-containing styrene-acrylic resin is a (meth)acrylic resin (polymer) synthesized by a high-temperature continuous polymerization method (high-temperature continuous bulk polymerization method) (methods described in U.S. Pat. No. 4,414,370, JP-A-59-6207, JP-B-5-58005, JP-A-1-313522, U.S. Pat. No. 5,010,166, Toa Gosei Kenkyuu Nenpo TREND 2000 Vol. 3, p. 42-45, etc.) with minimal use of auxiliary raw materials such as polymerization initiators, chain transfer agents, and organic solvents. In this specification, (meth)acrylic means methacryl and acrylic.
[0086] Examples of the acrylic monomer components constituting the acrylic resin include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters such as 2-ethylhexyl acrylate, aryl esters, aralkyl esters, etc.), (meth)acrylamide, (meth)acrylic acid derivatives such as (meth)acrylamide derivatives, etc. (Meth)acrylic acid is a general term for acrylic acid and methacrylic acid.
[0087] Examples of the aromatic vinyl monomer component constituting the acrylic resin include aromatic vinyls such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene.
[0088] As the monomer components constituting the acrylic resin, other monomer components may be used in addition to the (meth)acrylic acid, (meth)acrylic acid derivative, and aromatic vinyl. The content of the acrylic resin is preferably 1 to 100 parts by mass based on 100 parts by mass of the rubber component.
[0089] Examples of the plasticizer that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0090] In the rubber composition, the total content of the filler and the plasticizer is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the total content is preferably 160 parts by mass or less, more preferably 110 parts by mass or less, even more preferably 95 parts by mass or less, particularly preferably 85 parts by mass or less, and may be 75 parts by mass or less. By keeping the total content within the above range, there is a tendency that the overall performance of fuel economy and TGC resistance is improved.
[0091] In the rubber composition, the total content of the silica and the plasticizer is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the total content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 90 parts by mass or less, particularly preferably 80 parts by mass or less, and may be 70 parts by mass or less. By keeping the total content within the above range, there is a tendency that the overall performance of fuel economy and TGC resistance is improved.
[0092] In the rubber composition, the total content of the silica and the liquid plasticizer is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the total content is preferably 130 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 80 parts by mass or less, particularly preferably 70 parts by mass or less, and may be 60 parts by mass or less. By keeping the total content within the above range, there is a tendency that the overall performance of fuel economy and TGC resistance is improved.
[0093] (Processing aids) From the viewpoint of overall performance of fuel economy and TGC resistance, it is preferable to compound a processing aid in the rubber composition. Examples of processing aids include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, fatty acid esters, mixtures of fatty acid metal salts and amide esters, mixtures of fatty acid metal salts and fatty acid amides, etc. These may be used alone or in combination of two or more. Among them, at least one selected from the group consisting of fatty acid metal salts, amide esters, and mixtures of fatty acid metal salts and amide esters or fatty acid amides is preferred, and fatty acid metal salts are more preferred. It is presumed that the incorporation of fatty acid metal salts further enhances the dispersion of silica, improving TGC resistance.
[0094] The fatty acid constituting the fatty acid metal salt is not particularly limited, but examples thereof include saturated or unsaturated fatty acids (preferably saturated or unsaturated fatty acids having 6 to 28 carbon atoms (more preferably 10 to 25 carbon atoms, and even more preferably 14 to 20 carbon atoms)), such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, arachidic acid, behenic acid, and nervonic acid. These may be used alone or in combination of two or more. Of these, saturated fatty acids are preferred, and saturated fatty acids having 14 to 20 carbon atoms are more preferred.
[0095] Examples of metals constituting fatty acid metal salts include alkali metals such as potassium and sodium, alkaline earth metals such as magnesium, calcium and barium, zinc, nickel, molybdenum, etc. These may be used alone or in combination of two or more. Among these, zinc and calcium are preferred, and zinc is more preferred.
[0096] Examples of the amide ester include fatty acid amide esters having the above-mentioned saturated or unsaturated fatty acids as constituents, etc. These may be used alone or in combination of two or more kinds.
[0097] The fatty acid amide may be a saturated fatty acid amide or an unsaturated fatty acid amide. These may be used alone or in combination of two or more. Examples of the saturated fatty acid amide include N-(1-oxooctadecyl)sarcosinamide, stearic acid amide, and behenic acid amide. Examples of the unsaturated fatty acid amide include oleic acid amide and erucic acid amide.
[0098] A specific example of the mixture of a fatty acid metal salt and an amide ester is Aflux 16 manufactured by Rhein Chemie, which is a mixture of a fatty acid calcium salt and an amide ester.
[0099] A specific example of the mixture of a fatty acid metal salt and a fatty acid amide is WB16 manufactured by Struktol, which is a mixture of fatty acid calcium salt and a fatty acid amide.
[0100] As the processing aid, for example, products available from Rhein Chemie, Struktol, etc. can be used.
[0101] In the rubber composition, the content of the processing aid is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 5 parts by mass or less, based on 100 parts by mass of the rubber component. By keeping the content within the above range, the overall performance of fuel economy and TGC resistance tends to be improved.
[0102] (Other materials) From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition preferably contains an antioxidant.
[0103] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.
[0104] In the rubber composition, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, more preferably 4.0 parts by mass or less.
[0105] The rubber composition preferably contains stearic acid. The content of stearic acid in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0106] As the stearic acid, any known stearic acid can be used, for example, products available from NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0107] The rubber composition preferably contains zinc oxide. The content of zinc oxide in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0108] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.
[0109] The rubber composition may contain wax. The content of the wax in the rubber composition is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the rubber component.
[0110] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.
[0111] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.
[0112] It is preferable to compound sulfur in the rubber composition, in order to form an appropriate amount of crosslinked chains in the polymer chains and to impart good performance.
[0113] In the rubber composition, the amount of sulfur is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and even more preferably 0.5 part by mass or more, based on 100 parts by mass of the rubber component. The amount is preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.
[0114] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0115] The rubber composition preferably contains a vulcanization accelerator. In the rubber composition, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.
[0116] The type of vulcanization accelerator is not particularly limited, and any commonly used accelerator can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.
[0117] In addition to the above-mentioned components, the rubber composition may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.
[0118] The rubber composition can be produced by a known method, for example, by kneading the components using a rubber kneading device such as an open roll or a Banbury mixer, followed by vulcanization.
[0119] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 50 to 200°C, preferably 80 to 190°C, and the kneading time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100°C or lower, preferably room temperature to 80°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 120 to 200°C, preferably 140 to 180°C.
[0120] From the viewpoint of overall performance of fuel economy and TGC resistance, it is preferable that the rubber composition has a silica content (mass %) in the rubber composition (100 mass %) that satisfies the following formula: Silica content ≦40.0% by mass The silica content is more preferably 35.0% by mass or less, even more preferably 30.0% by mass or less, and particularly preferably 29.0% by mass or less. Although there is no particular lower limit, it is preferably 10.0% by mass or more, more preferably 20.0% by mass or more, and even more preferably 25.0% by mass or more.
[0121] From the viewpoint of the overall performance of fuel economy and TGC resistance, the rubber composition (rubber composition after vulcanization) preferably has an acetone extractable amount (AE amount) of 20.0 mass% or less in the rubber composition (100 mass%). The acetone extractable amount is preferably 17.0 mass% or less, more preferably 15.0 mass% or less, and particularly preferably 13.0 mass% or less. There is no particular restriction on the lower limit, but it is preferably 5.0 mass% or more, more preferably 7.0 mass% or more, and even more preferably 9.0 mass% or more. It is presumed that by reducing the amount of acetone extractable, migration to adjacent parts is prevented, and TGC resistance is improved. The amount of acetone extractables (AE amount) is a value measured by the method described in the Examples.
[0122] From the viewpoint of the overall performance of fuel economy and TGC resistance, it is preferable that the rubber composition (rubber composition after vulcanization) has a silica content (mass%) and an acetone extractable amount (AE amount (mass%)) in the rubber composition (100 mass%) that satisfy the following formulas. Silica content / AE amount ≧ 1.6 The silica content / AE amount is more preferably 2.0 or more, even more preferably 2.1 or more, and particularly preferably 2.2 or more. Although there is no particular upper limit, the silica content / AE amount is preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.0 or less, and particularly preferably 2.8 or less.
[0123] Regarding the silica content and silica content / AE amount, good dispersion cannot be obtained simply when the silica amount is low. However, by reducing the plasticizer, i.e., by reducing the AE amount, it becomes possible to sufficiently disperse the silica, which improves reinforcement and is presumably a significant improvement in the overall performance of fuel economy and TGC resistance.
[0124] The rubber composition can be preferably used for each component of a pneumatic tire such as a tread (cap tread), a sidewall, a base tread, a bead apex, a clinch apex, an inner liner, an under tread, a breaker topping, a braid topping, a tread, etc. Among them, the rubber composition can be preferably used for a tread (cap tread).
[0125] A tire is manufactured by a conventional method using a rubber composition. That is, the rubber composition containing the above-mentioned components is extruded in an unvulcanized state to match the shape of a tread, etc., and molded together with other tire components in a conventional manner on a tire building machine to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in the vulcanizer to obtain a tire.
[0126] Examples of the tire include pneumatic tires and non-pneumatic tires. Among them, pneumatic tires are preferred. The tire can be used as a passenger car tire, a large passenger car tire, a large SUV tire, a heavy load tire such as a truck or a bus tire, a light truck tire, a two-wheeled vehicle tire, a racing tire (high performance tire), etc. Among them, the tire can be preferably used as a passenger car tire, a large passenger car tire, and a light truck tire. EXAMPLES
[0127] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0128] Various chemicals used in the examples and comparative examples will be collectively described below. NR:RSS3 SBR: SBR1502 (non-oil extended, styrene content 25% by mass) manufactured by Zeon Corporation Carbon black: Show Black N220 (N2SA111m) manufactured by Cabot Japan Co., Ltd. 2 / g) Silica 1: Ultrasil VN3 (N2SA175m) manufactured by Evonik Degussa 2 / g) Silica 2: Ultrasil 9100GR (N2SA235m) manufactured by Evonik Degussa 2 / g) Organosilicon compound 1: Silane coupling agent synthesized in Production Example 1 below Organosilicon compound 2: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Oil: NH-60 manufactured by Idemitsu Kosan Co., Ltd. Resin 1: YS Resin PX1150 (polyterpene (β-pinene resin), softening point 115°C) manufactured by Yasuhara Chemical Co., Ltd. Resin 2: SYLVARES SA85 manufactured by Arizona Chemical (copolymer of α-methylstyrene and styrene, Tg 43°C, softening point 85°C) Resin 3: ExxonMobil PR120 (hydrogenated DCPD resin, softening point 120°C) Wax: Ozoace 0355 by Nippon Seiro Co., Ltd. Anti-aging agent: Antigen 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Sumitomo Chemical Co., Ltd. Processing aid: EF44 (zinc salt of saturated fatty acid) manufactured by Struktol Stearic acid: NOF Corporation's "Tsubaki" stearic acid Zinc oxide: Ginrei R manufactured by Toho Zinc Co., Ltd. Sulfur: HK-200-5 (powdered sulfur containing 5% oil) manufactured by Hosoi Chemical Industries Co., Ltd. Vulcanization accelerator CZ: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator DPG: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0129] (Production Example 1: Synthesis of Organosilicon Compound 1) A 2L separable flask equipped with a stirrer, reflux condenser, dropping funnel and thermometer was charged with 78.0g (1.0 mol) of anhydrous sodium sulfide, 80.3g (2.5 mol) of sulfur and 480g of ethanol, and heated to 80°C. 566g (2.0 mol) of 6-chlorohexyltriethoxysilane was added dropwise thereto, and the mixture was heated and stirred at 80°C for 10 hours. The reaction liquid was filtered under pressure using a filter plate to obtain a filtrate from which the salt generated as the reaction proceeded was removed. The obtained filtrate was heated to 100°C, and ethanol was distilled off under a reduced pressure of 10mmHg or less to obtain an organosilicon compound 1 (silane coupling agent) as a reaction product. The obtained organosilicon compound 1 had a sulfur content of 18.5% by mass, the average number of sulfur atoms X contained in one molecule of the organosilicon compound was 3.5, and the value of m was 6.
[0130] <Examples and Comparative Examples> According to the compounding recipes shown in each table, chemicals other than sulfur and vulcanization accelerator were kneaded using a Banbury mixer to obtain a kneaded product. Next, sulfur and vulcanization accelerator were kneaded into the obtained kneaded product using an open roll to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was molded into a tread shape, and laminated together with other tire components to form an unvulcanized tire, which was press-vulcanized for 10 minutes under the condition of 170°C to produce a test tire (size 195 / 65R15, passenger car tire). The following tests were performed using the obtained test tire.
[0131] The obtained test tires were subjected to the following evaluations. The evaluation results are shown in the tables. In Tables 1 and 2, Comparative Examples 1-1 and 2-1 were used as reference comparative examples, respectively.
[0132] <Acetone extractable amount (AE amount)> For rubber test pieces cut out from the tread of the test tire, the amount of substance contained in the test piece that was extractable by acetone was measured according to the method for measuring acetone extractable amount in accordance with JIS K 6229. Acetone extractable amount (%) = (mass of sample before extraction - mass of sample after extraction) / mass of sample before extraction x 100
[0133] <Rolling resistance (low fuel consumption performance)> Each test tire was fitted to all wheels of a vehicle (domestic FF vehicle, 2000cc displacement) and filled with air to the standard internal pressure (250kPa), then the vehicle was driven on a test course with a dry road surface at a speed of 80km / h for 15 minutes, after which the accelerator was released and the distance from when the accelerator was turned off until the vehicle came to a stop was measured as rolling resistance, which was then indexed using the following formula.The higher the value, the longer the distance from when the accelerator was turned off until the vehicle came to a stop, the lower the rolling resistance, and the better the fuel economy. Rolling resistance = [(Test tire measurement result) / (Standard comparison example measurement result)] x 100
[0134] <TGC resistance performance> The test tires were heat-treated at 80°C for two weeks while irradiating the tread with 30 pphm of ozone, then mounted on a domestically produced FF vehicle and driven around on an asphalt road surface, after which the occurrence of cracks at the bottom of the grooves was observed. The length of the cracks that occurred at the bottom of the grooves was measured and indexed using the following formula. The higher the index, the better the resistance to cracks at the bottom of the grooves. (Crack length of the standard comparative tire) / (Crack length of each tire specification) x 100
[0135] [Table 1]
[0136] [Table 2]
[0137] From each table, it can be seen that the examples containing a rubber component containing isoprene-based rubber and styrene-butadiene rubber, a filler containing silica, and a silane coupling agent containing an organosilicon compound containing an alkoxysilyl group and a sulfur atom and having 6 or more carbon atoms connecting the alkoxysilyl group and the sulfur atom were excellent in overall fuel efficiency and TGC resistance (expressed as the sum of two indices, rolling resistance and TGC resistance).
Claims
1. The rubber composition includes a rubber component including an isoprene-based rubber and a styrene-butadiene rubber, a filler including silica, and a silane coupling agent, The silane coupling agent includes an organosilicon compound that contains an alkoxysilyl group and a sulfur atom, and the number of carbon atoms connecting the alkoxysilyl group and the sulfur atom is 6 or more, The vulcanized rubber composition for tires, wherein the organosilicon compound is an organosilicon compound represented by the following average composition formula (I): [Case 1] (In the formula, x represents the average number of sulfur atoms and is 3.5 or more. m represents an integer of 6 or more. R 1 ~R 6 are the same or different and each represents an alkyl group or an alkoxy group having 1 to 6 carbon atoms; R 1 ~R 3 and R 4 ~R 6 At least one of R is the alkoxy group. 1 ~R 6 may be a ring structure formed by bonding the alkyl group or the alkoxy group.
2. A vulcanized rubber composition for tires as described in claim 1, wherein the amount of acetone extractable (AE amount) in the vulcanized rubber composition is 15.0 mass% or less.
3. A vulcanized rubber composition for tires according to claim 1 or 2, wherein the silica content and the amount of acetone extraction (AE amount) in the vulcanized rubber composition satisfy the following formulas (1) and (2). (1) Silica content ≦30.0% by mass (2) Silica content / AE amount ≧2.0
4. 4. The vulcanized rubber composition for tires according to claim 1, wherein the content of the filler per 100 parts by mass of the rubber component is 65 parts by mass or less.
5. 5. The vulcanized rubber composition for tires according to claim 1, wherein the content of silica per 100 parts by mass of the rubber component is 60 parts by mass or less.
6. Nitrogen adsorption specific surface area 180m 2 The vulcanized rubber composition for tires according to any one of claims 1 to 5, comprising at least one silica.
7. A composition comprising a plasticizer, 7. The vulcanized rubber composition for tires according to claim 1, wherein the content of the plasticizer is 20 parts by mass or less per 100 parts by mass of the rubber component.
8. A composition comprising a plasticizer, 8. The vulcanized rubber composition for tires according to claim 1, wherein the total content of silica and plasticizer is 80 parts by mass or less based on 100 parts by mass of the rubber component.
9. The vulcanized rubber composition for tires according to any one of claims 1 to 8, comprising at least one resin selected from the group consisting of terpene resins, C5 resins, C9 resins, C5 / C9 resins and hydrogenated dicyclopentadiene resins.
10. A tire having a tire member made of the vulcanized rubber composition according to any one of claims 1 to 9.
11. 11. The tire of claim 10, wherein the tire component is a tread.
Citation Information
Patent Citations
Tire tread rubber composition and tire
JP2010090203A
Free-flowing filler composition and rubber composition containing the same
JP2015071763A
Rubber composition for tire, and pneumatic tire
JP2018123260A