Conductive carbon material dispersion for lithium ion batteries, slurry for lithium ion battery electrodes, electrodes for lithium ion batteries, and lithium ion batteries
A water-soluble poly(meth)acrylamide-based dispersant addresses the dispersion and electrolyte swelling issues of conductive carbon materials in lithium ion batteries, enhancing electrode adhesion and storage stability.
Patent Information
- Application Number
- JP2020188365
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-12
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-12
AI Technical Summary
Conductive carbon materials in lithium ion battery slurries often fail to disperse effectively, leading to inadequate conductivity and electrolyte swelling, which compromises the performance of lithium ion batteries.
A conductive carbon material dispersant for lithium ion batteries is developed, comprising 2 to 60 mol% of structural units derived from (meth)acrylamide group-containing compounds and 10 to 70 mol% of unsaturated sulfonic acid or its salt, with a weight average molecular weight of 10,000 to 300,000, formulated as a water-soluble poly(meth)acrylamide to enhance dispersion and reduce electrolyte swelling.
The dispersant effectively disperses conductive carbon materials, reduces electrolyte swelling, and improves electrode adhesion, resulting in enhanced storage stability and discharge capacity retention of lithium ion batteries.
Smart Images

Figure 0007581782000001 
Figure 0007581782000002 
Figure 0007581782000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a conductive carbon material dispersion for lithium ion batteries, a slurry for lithium ion battery electrodes, an electrode for lithium ion batteries, and a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been studied in order to further improve the performance of lithium-ion batteries.
[0003] Both the positive and negative electrodes of a lithium-ion battery are manufactured by dispersing an electrode active material and a binder resin in a solvent to form a slurry, which is applied to both sides of a current collector (e.g., a metal foil), drying and removing the solvent to form an electrode layer, and then compression molding this using a roll press or the like.
[0004] The lithium ion battery slurry may contain a conductive carbon material as a conductive assistant, such as carbon black. Summary of the Invention [Problem to be solved by the invention]
[0005] When a conductive carbon material is included in a slurry for lithium ion batteries, the conductive carbon material may not be dispersed in the slurry. In this case, the conductive carbon material cannot fully fulfill its role as a conductive assistant. Therefore, a dispersant is required to disperse the conductive carbon material. In addition, since the dispersant is used in a lithium ion battery, it is preferable that the dispersant has low swelling property and good resistance to the electrolyte of the lithium ion battery.
[0006] Therefore, the problem that the present invention aims to solve is to provide a conductive carbon material dispersant for lithium ion batteries that can satisfactorily disperse a conductive carbon material for lithium ion batteries, has low swelling properties in the electrolyte of a lithium ion battery, and has good electrolyte resistance. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above problems can be solved by using a specific component.
[0008] The present disclosure provides the following: (Item 1) 2 to 60 mol % of structural units derived from a (meth)acrylamide group-containing compound (a), and Contains 10 to 70 mol % of structural units derived from an unsaturated sulfonic acid or a salt thereof (b), The weight average molecular weight is 10,000 to 300,000. Water-soluble poly(meth)acrylamide (A-1) Including, Conductive carbon material dispersant for lithium-ion batteries. (Item 2) The water-soluble poly(meth)acrylamide (A-1) Contains 20 to 70 mol% of structural units derived from (meth)acrylic acid ester (c); The conductive carbon material dispersant for lithium ion batteries according to the above item. (Item 3) The conductive carbon material dispersant for a lithium ion battery according to any one of the above items, Polymer (A-2), Electrode active material (B-1), Conductive carbon material (B-2), and water. (Item 4) The polymer (A-2) is The slurry for lithium ion battery electrodes according to the above item, which is a water-soluble poly(meth)acrylamide (A-2A) containing a constituent unit derived from the (meth)acrylamide group-containing compound (a). (Item 5) An electrode for a lithium ion battery, obtained by applying the slurry for a lithium ion battery electrode according to any one of the preceding items to a current collector and drying the same. (Item 6) A lithium ion battery comprising the lithium ion battery electrode described in the above item.
[0009] In the present disclosure, one or more of the above-described features may be provided in further combinations in addition to the combinations explicitly stated. Effect of the Invention
[0010] The conductive carbon material dispersant for lithium ion batteries of the present invention satisfactorily disperses the conductive carbon material for lithium ion batteries. The conductive carbon material dispersant for lithium ion batteries has a low electrolyte swelling ratio and high electrolyte resistance. The lithium ion battery electrode slurry of the present invention has excellent storage stability. The electrode of the present invention has excellent electrode adhesion. The battery of the present invention has an excellent discharge capacity retention rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Throughout this disclosure, the range of the values of the physical properties, contents, etc. may be set as appropriate (for example, by selecting from the upper and lower limit values described in each item below). Specifically, when A4, A3, A2, A1 (where A4>A3>A2>A1) are exemplified as the upper and lower limits of the value α, the range of the value α is exemplified as A4 or less, A3 or less, A2 or less, A1 or more, A2 or more, A3 or more, A1 to A2, A1 to A3, A1 to A4, A2 to A3, A2 to A4, A3 to A4, etc.
[0012] [Dispersant for conductive carbon materials for lithium-ion batteries: also called dispersant] The present disclosure relates to a polymerizable composition comprising 2 to 60 mol % of a structural unit derived from a (meth)acrylamide group-containing compound (a), and Contains 10 to 70 mol % of structural units derived from an unsaturated sulfonic acid or a salt thereof (b), The weight average molecular weight is 10,000 to 300,000. Water-soluble poly(meth)acrylamide (A-1) Including, A conductive carbon material dispersant for lithium ion batteries is provided.
[0013] <Water-soluble poly(meth)acrylamide (A-1): Also called component (A-1).> The component (A-1) may be used alone or in combination of two or more types.
[0014] In this disclosure, "water-soluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble matter is less than 0.5% by mass (less than 2.5 mg).
[0015] In the present disclosure, "(meth)acrylic" means "at least one selected from the group consisting of acrylic and methacrylic". Similarly, "(meth)acrylate" means "at least one selected from the group consisting of acrylate and methacrylate". In addition, "(meth)acryloyl" means "at least one selected from the group consisting of acryloyl and methacryloyl".
[0016] <(Meth)acrylamide group-containing compound (a): also referred to as component (a)> In the present disclosure, the term "(meth)acrylamide group-containing compound" refers to a compound having a (meth)acrylamide group. As the (meth)acrylamide group-containing compound, various known compounds can be used without particular limitation, and they may be used alone or in combination of two or more kinds.
[0017] In one embodiment, the (meth)acrylamide group-containing compound has the following structural formula: [ka] (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 and R 3 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, or an acetyl group;2 and R 3 are groups that together form a ring structure, and R 4 and R 5 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a hydroxyl group, an amino group (-NR a R b (R a and R b are each independently a hydrogen atom or a substituted or unsubstituted alkyl group), and an acetyl group. Examples of the substituent of the substituted alkyl group include a hydroxy group, an amino group, and an acetyl group. 2 and R 3 Examples of the group that combines with each other to form a ring structure include a morpholyl group. It is expressed by:
[0018] Examples of the alkyl group include a straight-chain alkyl group, a branched alkyl group, and a cycloalkyl group.
[0019] A straight chain alkyl group is -C n H 2n+1 (n is an integer of 1 or more). Examples of the straight-chain alkyl group include a methyl group, an ethyl group, a propyl group, a n-butyl group, a n-pentyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, and a n-decamethyl group.
[0020] A branched alkyl group is a group in which at least one hydrogen atom of a linear alkyl group is replaced with an alkyl group. Examples of branched alkyl groups include an i-propyl group, an i-butyl group, an s-butyl group, a t-butyl group, a diethylpentyl group, a trimethylbutyl group, a trimethylpentyl group, and a trimethylhexyl group.
[0021] Examples of the cycloalkyl group include a monocyclic cycloalkyl group, a bridged ring cycloalkyl group, and a condensed ring cycloalkyl group.
[0022] In the present disclosure, a monocyclic ring refers to a ring structure formed by a carbon covalent bond and having no internal bridge structure. A fused ring refers to a ring structure in which two or more monocyclic rings share two atoms (i.e., each ring shares only one side (fused) with each other). A bridged ring refers to a ring structure in which two or more monocyclic rings share three or more atoms.
[0023] Examples of the monocyclic cycloalkyl group include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclodecyl group, and a 3,5,5-trimethylcyclohexyl group.
[0024] Examples of the bridged ring cycloalkyl group include a tricyclodecyl group, an adamantyl group, and a norbornyl group.
[0025] The condensed ring cycloalkyl group is exemplified by a bicyclodecyl group.
[0026] Examples of the (meth)acrylamide group-containing compound (a) include (meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-methylol(meth)acrylamide, diacetone(meth)acrylamide, maleic acid amide, (meth)acryloylmorpholine, hydroxyethyl(meth)acrylamide, and salts thereof, and examples of the salts include dimethylaminopropyl(meth)acrylamide methyl chloride quaternary salt, dimethylaminoethyl(meth)acrylate benzyl chloride quaternary salt, etc. Among these, when (meth)acrylamide, particularly acrylamide, is used, it is possible to produce a binder that not only reduces water absorption while maintaining water solubility, but also reduces irreversible capacity, has high interaction with electrode active materials, and has high dispersibility of the slurry and high binding between electrode active materials inside the electrode.
[0027] The upper and lower limits of the content of structural units derived from a (meth)acrylamide group-containing compound relative to 100 mol % of all structural units of the component (A-1) are, for example, 60, 59, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 5, 3, 2 mol %, etc. In one embodiment, the content is preferably 2 to 60 mol %.
[0028] The upper and lower limits of the content of the structural units derived from the (meth)acrylamide group-containing compound relative to 100 mass% of all structural units of the component (A-1) are, for example, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 5, 4, 2, 1 mass%, etc. In one embodiment, the content is preferably 1 to 70 mass%.
[0029] <Unsaturated sulfonic acid or its salt (b): Also referred to as component (b)> As the (b) component, various known substances can be used without particular limitation, and may be used alone or in combination of two or more. In the present disclosure, when compound A corresponds to both component (a) and component (b), said compound A is regarded as component (b).
[0030] Examples of unsaturated sulfonic acids include α,β-ethylenically unsaturated sulfonic acids such as vinyl sulfonic acid, styrene sulfonic acid, and (meth)allyl sulfonic acid; (meth)acrylamide t-butyl sulfonic acid, 2-(meth)acrylamide-2-methylpropane sulfonic acid, 2-(meth)acrylamide-2-hydroxypropane sulfonic acid, 3-sulfopropane (meth)acrylic acid ester, and bis-(3-sulfopropyl)itaconic acid ester.
[0031] The salt of the unsaturated sulfonic acid is exemplified by an inorganic salt of the unsaturated sulfonic acid. The inorganic salt of the unsaturated sulfonic acid is a salt in which the cation portion is a metal cation. Examples of the inorganic salt include a typical metal salt and a transition metal salt.
[0032] Examples of typical metal salts include alkali metal salts, alkaline earth metal salts, and Group 13 metal salts.
[0033] Examples of the alkali metal salt include lithium salts, sodium salts, and potassium salts.
[0034] Examples of the alkaline earth metal salt include magnesium salts and calcium salts.
[0035] Examples of Group 13 metal salts include aluminum salts.
[0036] The transition metal salt is exemplified by iron salts.
[0037] The upper and lower limits of the content of the structural units derived from the unsaturated sulfonic acid or a salt thereof (b) relative to 100 mol % of all structural units of the component (A-1) are, for example, 70, 69, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10 mol %, etc. In one embodiment, the content is preferably 10 to 70 mol %.
[0038] The upper and lower limits of the content of the structural units derived from unsaturated sulfonic acid or a salt thereof (b) relative to 100% by mass of all structural units of the component (A-1) are, for example, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5% by mass, etc. In one embodiment, the content is preferably 5 to 70% by mass.
[0039] <(Meth)acrylic acid ester (c): Also called component (c)> As the component (c), various known substances can be used without particular limitation, and they may be used alone or in combination of two or more kinds.
[0040] Examples of the (meth)acrylic acid ester include non-substituent-containing (meth)acrylic acid ester and substituent-containing (meth)acrylic acid ester.
[0041] In the present disclosure, the term "non-substituted (meth)acrylic acid ester" refers to a (meth)acrylic acid ester in which all atoms forming the compound are carbon atoms and hydrogen atoms, except for the oxygen atom forming the ester bond. The term "substituent-containing (meth)acrylic acid ester" refers to a (meth)acrylic acid ester that is not a non-substituted (meth)acrylic acid ester.
[0042] Examples of non-substituted (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate.
[0043] Examples of the substituent-containing (meth)acrylic ester include a hydroxyl group-containing (meth)acrylic ester and an alkoxy group-containing (meth)acrylic ester.
[0044] Hydroxyl group-containing (meth)acrylic acid esters include 1-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-1-methylethyl (meth)acrylate, 1-hydroxy-2-methylethyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1-hydroxy-1-methylpropyl (meth)acrylate, 2-hydroxy-1-methylpropyl (meth)acrylate, 3-hydroxy-1-methylpropyl (meth)acrylate, 1-ethyl-2-hydroxypropyl (meth)acrylate, Examples of the acrylates include hydroxyethyl, 1-hydroxy-2-methyl-propyl (meth)acrylate, 2-hydroxy-2-methyl-propyl (meth)acrylate, 3-hydroxy-2-methyl-propyl (meth)acrylate, 1,1-dimethyl-2-hydroxyethyl (meth)acrylate, 3-hydroxy-1-adamantyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerin mono(meth)acrylate, glycerin di(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol-mono(meth)acrylate, polypropylene glycol-mono(meth)acrylate, and polyethylene glycol-propylene glycol-mono(meth)acrylate.
[0045] Alkoxy group-containing (meth)acrylic acid esters include methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 1-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 1-methoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 1-methoxybutyl (meth)acrylate, Examples of the acrylate include tert-butyl acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 1-ethoxyethyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 1-ethoxypropyl (meth)acrylate, propoxymethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 1-propoxyethyl (meth)acrylate, butoxymethyl (meth)acrylate, etc. Methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, isobutyl acrylate, t-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate.
[0046] In one embodiment, the (meth)acrylic acid ester has the following structural formula: [ka] [In the formula, R α1 is a hydrogen atom or a methyl group, R α2 is an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or [ka] (In the formula, q is an integer of 1 to 3, and n is an integer of 0 to 100, preferably 0 to 10.) R is a polyoxyalkylene group represented by the formula: α3 and R α4 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a carboxyl group, a hydroxyl group, an amino group [-NRa R b (R a and R b are each independently a hydrogen atom or a substituted or unsubstituted alkyl group, and an acetyl group. Examples of the substituent of the substituted alkyl group include a hydroxy group, an alkoxy group, an amino group, and an acetyl group. It is expressed by:
[0047] A hydroxyalkyl group is an alkyl group in which at least one hydrogen atom has been replaced by a hydroxy group (hydroxyl group).
[0048] An alkoxyalkyl group is an alkyl group in which at least one hydrogen atom has been replaced by an alkoxy group.
[0049] An alkoxy group is a monovalent group in which an alkyl group is bonded to an oxygen atom.
[0050] The upper and lower limits of the content of the structural units derived from the (meth)acrylic acid ester (c) relative to 100 mol % of all structural units of the component (A-1) are, for example, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20 mol %, etc. In one embodiment, the content is preferably 20 to 70 mol %.
[0051] The upper and lower limits of the content of the structural units derived from the (meth)acrylic acid ester (c) relative to 100 mass% of all structural units of the component (A-1) are, for example, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20 mass%, etc. In one embodiment, the content is preferably 20 to 80 mass%.
[0052] <Monomers other than components (a), (b), and (c): Also called component (d)> All of the constituent units of component (A-1) may be derived from a monomer (component (d)) that does not fall under any of components (a), (b), or (c), as long as the desired effects of the present invention are not impaired. Component (d) may be used alone or in combination of two or more. Examples of component (d) include unsaturated carboxylic acids, unsaturated phosphoric acids, α,β-unsaturated nitriles, conjugated dienes, vinyl ethers, and aromatic vinyl compounds.
[0053] Examples of the unsaturated carboxylic acid include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid.
[0054] The content of structural units derived from unsaturated carboxylic acid relative to 100 mol % of all structural units of the component (A-1) is preferably less than 40 mol % (for example, 30, 25, 20, 19, 15, 10, 5, less than 1 mol %, or 0 mol %).
[0055] The content of structural units derived from unsaturated carboxylic acid relative to 100% by mass of all structural units of the component (A-1) is preferably less than 40% by mass (for example, 30, 25, 20, 19, 15, 10, 5, less than 1% by mass, or 0% by mass).
[0056] Examples of unsaturated phosphoric acids include vinylphosphonic acid, vinyl phosphate, bis((meth)acryloxyethyl)phosphate, diphenyl-2-(meth)acryloyloxyethyl phosphate, dibutyl-2-(meth)acryloyloxyethyl phosphate, dioctyl-2-(meth)acryloyloxyethyl phosphate, monomethyl-2-(meth)acryloyloxyethyl phosphate, and 3-(meth)acryloxy-2-hydroxypropane phosphoric acid.
[0057] The content of structural units derived from unsaturated phosphoric acid relative to 100 mol % of all structural units of the component (A-1) is preferably less than 40 mol % (for example, 30, 25, 20, 19, 15, 10, 5, less than 1 mol %, or 0 mol %).
[0058] The content of structural units derived from unsaturated phosphoric acid relative to 100% by mass of all structural units of the component (A-1) is preferably less than 40% by mass (for example, 30, 25, 20, 19, 15, 10, 5, less than 1% by mass, or 0% by mass).
[0059] The α,β-unsaturated nitrile can be suitably used for the purpose of imparting flexibility to the electrode. Examples of the α,β-unsaturated nitrile include (meth)acrylonitrile, α-chloro(meth)acrylonitrile, α-ethyl(meth)acrylonitrile, vinylidene cyanide, etc. Among these, (meth)acrylonitrile is preferred, and acrylonitrile is particularly preferred.
[0060] The content of structural units derived from an α,β-unsaturated nitrile is not particularly limited, but is preferably less than 40 mol % (for example, 30, 25, 20, 19, 15, 10, 5, less than 1 mol %, or 0 mol %) relative to 100 mol % of all structural units of the component (A-1).
[0061] In one embodiment, the content of structural units derived from an α,β-unsaturated nitrile relative to 100% by mass of all structural units of the component (A-1) is preferably less than 40% by mass (for example, 30, 25, 20, 19, 15, 10, 5, less than 1% by mass, or 0% by mass).
[0062] Examples of conjugated dienes include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, and substituted and side-chain conjugated hexadienes.
[0063] The content of the structural units derived from the conjugated diene is not particularly limited, but from the viewpoint of the springback resistance of the lithium ion battery according to the present invention, it is preferably less than 10 mol %, and more preferably 0 mol %, of 100 mol % of all structural units of the (A-1) component.
[0064] In one embodiment, the content of structural units derived from conjugated dienes relative to 100% by mass of all structural units of the component (A-1) is preferably less than 10% by mass, and more preferably 0% by mass.
[0065] Examples of vinyl ethers include hydroxyalkyl vinyl ethers and polyalkylene glycol monovinyl ethers.
[0066] Examples of the hydroxyalkyl vinyl ether include hydroxy linear alkyl vinyl ether, hydroxy branched alkyl vinyl ether, and hydroxycycloalkyl vinyl ether.
[0067] Examples of hydroxy linear alkyl vinyl ethers include 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 5-hydroxypentyl vinyl ether.
[0068] Examples of hydroxy branched alkyl vinyl ethers include 2-hydroxypropyl vinyl ether, 2-hydroxy-2-methylpropyl vinyl ether, and 4-hydroxy-2-methylbutyl vinyl ether.
[0069] Examples of hydroxycycloalkyl vinyl ethers include 4-hydroxycyclopentyl vinyl ether.
[0070] Examples of polyalkylene glycol monovinyl ethers include polymethylene glycol monovinyl ether, polyethylene glycol monovinyl ether, and polypropylene glycol monovinyl ether.
[0071] There are no particular limitations on the content of structural units derived from vinyl ether, but it is preferably less than 30 mol %, and more preferably 0 mol %, of 100 mol % of all structural units of the component (A-1).
[0072] In one embodiment, the content of structural units derived from vinyl ether relative to 100% by mass of all structural units of the component (A-1) is preferably less than 30% by mass, and more preferably 0% by mass.
[0073] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, and divinylbenzene.
[0074] There are no particular limitations on the content of structural units derived from aromatic vinyl compounds, but it is preferably less than 10 mol %, and more preferably 0 mol %, of 100 mol % of all structural units of the component (A-1).
[0075] In one embodiment, the content of structural units derived from an aromatic vinyl compound relative to 100% by mass of all structural units of the component (A-1) is preferably less than 10% by mass, and more preferably 0% by mass.
[0076] The proportion of structural units derived from component (d) other than the above unsaturated carboxylic acids, unsaturated phosphoric acids, α,β-unsaturated nitriles, conjugated dienes, vinyl ethers and aromatic vinyl compounds in all structural units of component (A-1) is less than 10 mol%, less than 5 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol%, or 0 mol%, relative to 100 mol% of all structural units of component (A-1); and less than 10 mass%, less than 5 mass%, less than 1 mass%, less than 0.5 mass%, less than 0.1 mass%, less than 0.01 mass%, or 0 mass%, relative to 100 mass% of all structural units of component (A-1).
[0077] The water-soluble poly(meth)acrylamide (A-1) can be synthesized by various known polymerization methods, preferably radical polymerization methods. The polymerization reaction may be carried out by adding a radical polymerization initiator and, if necessary, a chain transfer agent to a monomer mixture containing the components (a) and (b) and, if necessary, the components (c) and (d), and stirring the mixture at a reaction temperature of about 50 to 100°C. The reaction time is not particularly limited, and is preferably about 1 to 10 hours. In one embodiment, the component (A-1) is preferably produced by simultaneously dropping a solution containing a monomer and a solution containing an initiator to carry out a polymerization reaction.
[0078] The radical polymerization initiator may be any of various known initiators without any particular limitation. Examples of the radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; redox-based polymerization initiators that combine the above-mentioned persulfates with a reducing agent such as sodium hydrogen sulfite; and azo-based initiators such as 2,2'-azobis-2-amidinopropane dihydrochloride. The amount of the radical polymerization initiator used is not particularly limited, but is preferably 0.05 to 5.0% by mass, more preferably 0.1 to 3.0% by mass, based on 100% by mass of all the constituent units of the component (A-1) that gives the component (A-1).
[0079] For the purpose of improving production stability, before the radical polymerization reaction and / or when the obtained component (A-1) is dissolved in water, the pH of the reaction solution may be adjusted with a common neutralizing agent such as ammonia, organic amine, potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. In this case, the pH is preferably 2 to 11. For the same purpose, it is also possible to use a metal ion-sequestering agent such as EDTA or a salt thereof.
[0080] <Physical properties of water-soluble poly(meth)acrylamide (A-1)> The upper and lower limits of the glass transition temperature of the water-soluble poly(meth)acrylamide (A-1) are exemplified as 160, 155, 150, 145, 140, 135, 130, 125, 120, 115, 110, 105, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, and 0° C. In one embodiment, 0° C. or higher is preferable, and 30° C. or higher is more preferable from the viewpoint of mechanical strength and heat resistance.
[0081] The glass transition temperature of water-soluble poly(meth)acrylamide can be adjusted by the combination of monomers. In water-soluble poly(meth)acrylamide (A-1), the glass transition temperature can be calculated from the glass transition temperature (Tg) (absolute temperature: K) of the homopolymer of the monomers and their mass fractions based on the Fox formula shown below. 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+(W3 / Tg3)+···+(W n / Tgn ) [Wherein, Tg is the glass transition temperature (K) of the polymer to be determined, W1 to W n is the mass fraction of each monomer, Tg1 to Tg n indicates the glass transition temperature (K) of the homopolymer of each monomer.
[0082] For example, the glass transition temperature is 165°C for a homopolymer of acrylamide, 106°C for a homopolymer of acrylic acid, -15°C for a homopolymer of hydroxyethyl acrylate, and 105°C for a homopolymer of acrylonitrile. The monomer composition constituting the water-soluble poly(meth)acrylamide (A-1) can be determined so as to obtain a water-soluble poly(meth)acrylamide (A-1) having a desired glass transition temperature. The glass transition temperature of the homopolymer of the monomer can be measured, for example, under conditions of heating from -100°C to 300°C (heating rate 10°C / min.) using a DSC (differential scanning calorimeter), DTA (differential thermal analyzer), TMA (thermomechanical analyzer), or the like. Values described in literature can also be used. Examples of literature include "Chemical Handbook Basics II Edited by the Chemical Society of Japan (Revised 5th Edition)", p. 325, and the like.
[0083] Examples of the upper and lower limits of the weight average molecular weight (Mw) of the water-soluble poly(meth)acrylamide (A-1) are 300,000, 290,000, 250,000, 200,000, 150,000, 100,000, 90,000, 50,000, 40,000, 30,000, 20,000, 10,000, etc. In one embodiment, the weight average molecular weight (Mw) of the water-soluble poly(meth)acrylamide (A-1) is preferably 10,000 to 300,000, and more preferably 10,000 or more and less than 300,000, from the viewpoints of improving the dispersibility of the conductive carbon material and making it difficult to form aggregates.
[0084] The upper and lower limits of the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-1) are exemplified as 110,000, 100,000, 90,000, 70,000, 50,000, 30,000, 20,000, 10,000, 9,000, 7,000, and 5,000. In one embodiment, the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-1) is preferably 5,000 to 110,000.
[0085] The weight average molecular weight and number average molecular weight can be determined, for example, as a polyacrylic acid equivalent value measured in an appropriate solvent by gel permeation chromatography (GPC).
[0086] The upper and lower limits of the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-1) are exemplified as 15, 14, 13, 12, 11, 10, 9, 8, 7.5, 6, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-1) is preferably 1.1 to 15.
[0087] The upper and lower limits of the B-type viscosity of the conductive carbon material dispersant for lithium ion batteries containing the water-soluble poly(meth)acrylamide (A-1) are exemplified as 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, 25, 10 mPa·s, etc. In one embodiment, the B-type viscosity is preferably 10 to 500 mPa·s.
[0088] The Brookfield viscosity is measured using a Brookfield viscometer such as the "B-type Viscometer Model TVB-10M" manufactured by Toki Sangyo Co., Ltd.
[0089] The upper and lower limits of the pH of the conductive carbon material dispersant for lithium ion batteries are exemplified as 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, 5, etc. In one embodiment, the pH is preferably 5 to 7, and more preferably 5 or more and less than 7, from the viewpoint of solution stability.
[0090] The pH can be measured at 25° C. using a glass electrode pH meter (for example, product name "pH Meter D-52" manufactured by Horiba, Ltd.).
[0091] The upper and lower limits of the content of the water-soluble poly(meth)acrylamide (A-1) relative to 100% by mass of the conductive carbon material dispersant for lithium ion batteries are exemplified as 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 19, 17, 15, 13, 10, 9, 7, 5% by mass, etc. In one embodiment, the content is preferably 5 to 100% by mass.
[0092] In one embodiment, the conductive carbon material dispersion for lithium ion batteries may contain water. The upper and lower limits of the water content relative to 100% by mass of the conductive carbon material dispersion for lithium ion batteries are, for example, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, and 0% by mass. In one embodiment, the content is preferably 0 to 95% by mass.
[0093] The upper and lower limits of the mass ratio of water to the (A-1) component contained in the conductive carbon material dispersant for lithium ion batteries [mass of water / mass of the (A-1) component] are exemplified as 19, 17, 15, 13, 10, 9, 7, 5, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0, etc. In one embodiment, the mass ratio is preferably 0 to 19.
[0094] In one embodiment, the conductive carbon material dispersion for a lithium ion battery may include an organic solvent.
[0095] Examples of the organic solvent include ether solvents, ketone solvents, alcohol solvents, and amide solvents. Examples of the ether solvent include dioxane and tetrahydrofuran (THF). Examples of the ketone solvent include acetone and methyl ethyl ketone (MEK). Examples of the alcohol solvent include methanol, ethanol, 2-propanol, and isopropyl alcohol. Examples of the amide solvent include N-methyl-2-pyrrolidone (NMP).
[0096] The upper and lower limits of the content of the organic solvent relative to 100% by mass of the component (A-1) are, for example, 200, 175, 150, 125, 100, 75, 50, 25, 0% by mass, etc. In one embodiment, the content is preferably 0 to 200% by mass.
[0097] <Neutralizing agent> In one embodiment, the conductive carbon material dispersion for a lithium ion battery may include a neutralizing agent.
[0098] Examples of the neutralizing agent include alkali metal salts and alkaline earth metal salts.
[0099] Examples of the alkali metal salt include lithium salts, sodium salts, and potassium salts.
[0100] Examples of the lithium salt include lithium hydroxide, lithium chloride, lithium fluoride, lithium bromide, lithium acetate, lithium sulfate, lithium carbonate, lithium phosphate, and lithium hydrogen carbonate.
[0101] Examples of sodium salts include sodium hydroxide, sodium chloride, sodium fluoride, sodium bromide, sodium acetate, sodium sulfate, sodium carbonate, sodium phosphate, and sodium bicarbonate.
[0102] Examples of potassium salts include potassium hydroxide, potassium chloride, potassium fluoride, potassium bromide, potassium acetate, potassium sulfate, potassium carbonate, potassium phosphate, and potassium hydrogen carbonate.
[0103] Examples of the alkaline earth metal salt include calcium salts and magnesium salts.
[0104] Examples of magnesium salts include magnesium hydroxide, magnesium chloride, magnesium fluoride, magnesium bromide, magnesium acetate, magnesium sulfate, magnesium carbonate, magnesium phosphate, magnesium hydrogen carbonate, and the like.
[0105] Examples of calcium salts include calcium hydroxide, calcium chloride, calcium fluoride, calcium bromide, calcium acetate, calcium sulfate, calcium carbonate, calcium phosphate, calcium hydrogen carbonate, and the like.
[0106] The upper and lower limits of the content of the neutralizing agent relative to 100 mol % of the acidic groups contained in the component (A-1) are, for example, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 0 mol %, etc. In one embodiment, the content is preferably 0 to 100 mol %.
[0107] Examples of the acidic group contained in the component (A-1) include a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.
[0108] <Additives> The conductive carbon material dispersant for lithium ion batteries may contain an additive that does not fall under any of the (A-1) component, water, organic solvent, and neutralizing agent. Examples of additives include those described below. Examples of the content of the additive include 0 to 5 mass%, less than 1 mass%, less than 0.1 mass%, less than 0.01 mass%, 0 mass%, etc., relative to 100 mass% of the (A-1) component, and examples of the content of the additive include 0 to 5 mass%, less than 1 mass%, less than 0.1 mass%, less than 0.01 mass%, 0 mass%, etc., relative to 100 mass% of the conductive carbon material dispersant for lithium ion batteries.
[0109] The conductive carbon material dispersant for lithium ion batteries can be used as a conductive carbon material dispersant for lithium ion battery electrodes, a conductive carbon material dispersant for lithium ion battery negative electrodes, or a conductive carbon material dispersant for lithium ion battery positive electrodes.
[0110] Examples of the conductive carbon material include those described below.
[0111] [Lithium-ion battery electrode slurry: also called slurry] The present disclosure relates to the conductive carbon material dispersant for lithium ion batteries, Polymer (A-2), Electrode active material (B-1), Conductive carbon material (B-2), and water.
[0112] The upper and lower limits of the content of the conductive carbon material dispersant for lithium ion batteries relative to 100 mass% of the slurry are, for example, 40, 35, 30, 25, 20, 15, 10, 9, 5, 4, 2, 1, 0.9, 0.5, 0.4, 0.2, 0.1 mass%, etc. In one embodiment, the content is preferably 0.1 to 40 mass%.
[0113] The upper and lower limits of the content of the (A-1) component relative to 100% by mass of the slurry are, for example, 40, 35, 30, 25, 20, 15, 10, 9, 5, 4.5, 2, 1, 0.9, 0.5, 0.4, 0.2, 0.1% by mass, etc. In one embodiment, the content is preferably 0.1 to 40% by mass.
[0114] <Polymer (A-2): Also referred to as component (A-2)> The polymer may be used alone or in combination of two or more kinds. The polymer may be used as a binder or an aqueous binder. The polymer means a polymer solid synthesized in water or an organic solvent.
[0115] Examples of the polymer include a water-soluble polymer and a water-insoluble polymer.
[0116] Examples of the water-soluble polymer include cellulose compounds, starch, alginic acid, xanthan gum, chitosan, carrageenan, agar, dextrin, gelatin, polyvinyl alcohol, poly(meth)acrylamide, poly(meth)acrylic acid, polysulfonic acid, polyethyleneimine, polyethylene oxide, polyvinylpyrrolidone, polyethylene glycol, polystyrene sulfonic acid, ethylene-acrylic acid copolymer, ethylene-acrylamide-acrylic acid copolymer, polyamidine, polyvinylimidazoline, and derivatives or salts thereof. Examples include cellulose compounds, starch, alginic acid, xanthan gum, chitosan, carrageenan, agar, dextrin, gelatin, polyvinyl alcohol, poly(meth)acrylamide, poly(meth)acrylic acid, polysulfonic acid, polyethyleneimine, polyethylene oxide, polyvinylpyrrolidone, polyethylene glycol, polystyrene sulfonic acid, ethylene-acrylic acid copolymer, ethylene-acrylamide-acrylic acid copolymer, polyamidine, polyvinylimidazoline, and derivatives or salts thereof.
[0117] In the present disclosure, "water-insoluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble matter is 0.5% by mass or more.
[0118] The water-insoluble polymers are styrene-butadiene copolymer latex, polystyrene polymer latex, polybutadiene polymer latex, acrylonitrile-butadiene copolymer latex, polyurethane polymer latex, polymethyl methacrylate polymer latex, methyl methacrylate-butadiene copolymer latex, polyacrylate polymer latex, vinyl chloride polymer latex, vinyl acetate polymer emulsion, vinyl acetate-ethylene copolymer emulsion, polyethylene emulsion, carboxy-modified styrene butadiene, Examples of such polymers include ethylene copolymer resin emulsions, acrylic resin emulsions, polyethylene, polypropylene, polyethylene terephthalate, polyamide (PA), polyimide (PI), polyamideimide (PAI), aromatic polyamide, alginic acid and its salts, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and ethylene-tetrafluoroethylene copolymer (ETFE).
[0119] In one embodiment, the polymer (A-2) is a water-soluble poly(meth)acrylamide (A-2A) containing constitutional units derived from the (meth)acrylamide group-containing compound (a).
[0120] <Water-soluble poly(meth)acrylamide (A-2A): Also called component (A-2A)> The (A-2A) component contains a structural unit derived from a (meth)acrylamide group-containing compound (a). The (meth)acrylamide group-containing compound (a) may be used alone or in combination of two or more. From the viewpoint of electrode adhesion, it is preferable that the (A-1) component and the (A-2A) component are compatible with each other.
[0121] The upper and lower limits of the content of the structural units derived from the (meth)acrylamide group-containing compound relative to 100 mol % of all structural units of the component (A-2A) are exemplified as 100, 99.99, 99.9, 99.7, 99.5, 99, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 5, 3, 2, 1 mol %, etc. In one embodiment, the content is preferably 1 to 100 mol %.
[0122] Examples of upper and lower limits for the content of structural units derived from a (meth)acrylamide group-containing compound relative to 100 mass% of all structural units of the component (A-2A) include 100, 99.99, 99.9, 99.7, 99.5, 99, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 5, 3, 2, 1 mass%, etc. In one embodiment, the content is preferably 1 to 100 mass%.
[0123] In one embodiment, the component (A-2A) may contain a structural unit derived from an unsaturated organic acid or a salt thereof. The unsaturated organic acid or a salt thereof may be used alone or in combination of two or more kinds.
[0124] In the present disclosure, an unsaturated organic acid refers to a compound having an acidic group and a polymerizable unsaturated bond.
[0125] Examples of the unsaturated organic acid include unsaturated carboxylic acid, unsaturated sulfonic acid, and unsaturated phosphoric acid. Examples of the salt of the unsaturated organic acid include inorganic salts of the unsaturated organic acid. The inorganic salt of the unsaturated organic acid refers to a salt in which the cationic portion is a metal cation.
[0126] The upper and lower limits of the content of the structural units derived from an unsaturated organic acid or a salt thereof relative to 100 mol % of all structural units of the component (A-2A) are, for example, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0 mol %, etc. In one embodiment, the above content is preferably 0 to 50 mol %.
[0127] The upper and lower limits of the content of the structural units derived from an unsaturated organic acid or a salt thereof relative to 100% by mass of all structural units of the component (A-2A) are, for example, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0% by mass, etc. In one embodiment, the above content is preferably 0 to 70% by mass.
[0128] In one embodiment, the component (A-2A) may contain a structural unit derived from a (meth)acrylic acid ester (c). The (meth)acrylic acid ester may be used alone or in combination of two or more kinds.
[0129] The upper and lower limits of the content of the structural units derived from the (meth)acrylic acid ester (c) relative to 100 mol % of all structural units of the component (A-2A) are, for example, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0 mol %, etc. In one embodiment, the content is preferably 0 to 75 mol %.
[0130] The upper and lower limits of the content of the structural units derived from the (meth)acrylic acid ester (c) relative to 100 mass% of all structural units of the component (A-2A) are, for example, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0 mass%, etc. In one embodiment, the content is preferably 0 to 80 mass%.
[0131] In one embodiment, the component (A-2A) may contain a structural unit derived from an α,β-unsaturated nitrile. The α,β-unsaturated nitrile may be used alone or in combination of two or more kinds.
[0132] The upper and lower limits of the content of the structural units derived from α,β-unsaturated nitrile relative to 100 mol % of all structural units of the component (A-2A) are, for example, 45, 40, 35, 30, 25, 20, 15, 10, 5, 2, 1, 0 mol %, etc. In one embodiment, the above content is preferably 0 to 45 mol %.
[0133] The upper and lower limits of the content of structural units derived from α,β-unsaturated nitrile relative to 100% by mass of all structural units of the component (A-2A) are, for example, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0% by mass, etc. In one embodiment, the content is preferably 0 to 40% by mass.
[0134] In one embodiment, the (A-2A) component may contain a structural unit derived from a double bond-containing trihydroxysilyl compound having a vinyl group or a (meth)acryloxy group. The double bond-containing trihydroxysilyl compound having a vinyl group or a (meth)acryloxy group may be used alone or in combination of two or more kinds.
[0135] The upper and lower limits of the content of structural units derived from a double bond-containing trihydroxysilyl compound having a vinyl group or a (meth)acryloxy group relative to 100 mol % of all structural units of the component (A-2A) are, for example, 0.8, 0.7, 0.5, 0.3, 0.2, 0.1, 0.09, 0.07, 0.05, 0 mol %, etc. In one embodiment, the content is preferably 0 to 0.8 mol %.
[0136] The upper and lower limits of the content of structural units derived from a double bond-containing trihydroxysilyl compound having a vinyl group or a (meth)acryloxy group relative to 100% by mass of all structural units of the component (A-2A) are, for example, 10, 9, 7, 5, 3, 1, 0.9, 0.5, 0.3, 0.1, 0.09, 0.05, 0.01, 0.009, 0.005, 0.001, 0% by mass, etc. In one embodiment, the content is preferably 0 to 10% by mass.
[0137] In one embodiment, the component (A-2A) may contain a structural unit derived from a hydroxyl group-containing vinyl ether. The hydroxyl group-containing vinyl ether may be used alone or in combination of two or more kinds.
[0138] The upper and lower limits of the content of structural units derived from hydroxyl group-containing vinyl ether relative to 100 mol % of all structural units of the component (A-2A) are, for example, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0 mol %, etc. In one embodiment, the content is preferably 0 to 80 mol %.
[0139] The upper and lower limits of the content of structural units derived from hydroxyl group-containing vinyl ether relative to 100 mass% of all structural units of the component (A-2A) are, for example, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 2, 1, 0 mass%, etc. In one embodiment, the content is preferably 0 to 85 mass%.
[0140] The proportion of structural units derived from compounds not corresponding to any of the (meth)acrylamide group-containing compound (a), unsaturated organic acids or salts thereof, (meth)acrylic acid esters, α,β-unsaturated nitriles, double bond-containing trihydroxysilyl compounds having a vinyl group or a (meth)acryloxy group, and hydroxyl group-containing vinyl ethers in all structural units of the component (A-2A) is less than 10 mol%, less than 5 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol%, or 0 mol%, relative to 100 mol% of all structural units of the component (A-2A); and is less than 10 mass%, less than 5 mass%, less than 1 mass%, less than 0.5 mass%, less than 0.1 mass%, less than 0.01 mass%, or 0 mass%, relative to 100 mass% of all structural units of the component (A-2A).
[0141] The water-soluble poly(meth)acrylamide (A-2A) can be produced under the same conditions and by the same method as for the component (A-1).
[0142] Examples of upper and lower limits for the content of the neutralizing agent relative to 100 mol % of the acidic groups contained in the component (A-2A) are 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 0 mol %, etc. In one embodiment, the content is preferably 0 to 100 mol %.
[0143] <Physical properties of water-soluble poly(meth)acrylamide (A-2A)> Examples of the upper and lower limits of the glass transition temperature of the water-soluble poly(meth)acrylamide (A-2A) are 160, 155, 150, 145, 140, 135, 130, 125, 120, 115, 110, 105, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, and 0° C. In one embodiment, the glass transition temperature is preferably 0° C. or higher, and more preferably 30° C. or higher from the viewpoints of mechanical strength and heat resistance.
[0144] The upper and lower limits of the weight average molecular weight (Mw) of the water-soluble poly(meth)acrylamide (A-2A) are exemplified as 7 million, 6.5 million, 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 350,000, 300,000, 250,000, 200,000, 150,000, 100,000, etc. In one embodiment, the weight average molecular weight (Mw) is preferably 100,000 to 7 million, more preferably 500,000 to 1 million.
[0145] The upper and lower limits of the ratio of the weight average molecular weight of the (A-2A) component to the (A-1) component [weight average molecular weight of (A-2A) / weight average molecular weight of (A-1)] are exemplified as 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 75, 50, 25, 10, 5, 2, 1, etc. In one embodiment, the above ratio is preferably 1 to 600.
[0146] The upper and lower limits of the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-2A) are exemplified as 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 300,000, 200,000, 150,000, 100,000, 50,000, 10,000, etc. In one embodiment, the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-2A) is preferably 10,000 or more, more preferably 150,000 to 500,000.
[0147] The upper and lower limits of the ratio of the number average molecular weight of the (A-2A) component to the (A-1) component [number average molecular weight of (A-2A) / number average molecular weight of (A-1)] are exemplified as 100, 90, 75, 50, 25, 10, 5, 2, 1, 0.9, 0.5, 0.2, 0.1, 0.09, etc. In one embodiment, the ratio is preferably 0.09 to 100.
[0148] The upper and lower limits of the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-2A) are exemplified as 15, 14, 13, 11, 10, 9, 7.5, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) is preferably 1.1 to 15.
[0149] Examples of the upper and lower limits of the B-type viscosity of the slurry are 100,000, 90,000, 80,000, 70,000, 60,000, 50,000, 40,000, 30,000, 20,000, 10,000 mPa·s, etc. In one embodiment, the B-type viscosity is preferably 1,000 to 100,000 mPa·s.
[0150] Examples of the upper and lower limits of the pH of the slurry are 9, 8, 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, and 5. In one embodiment, the pH is preferably 5 to 9, more preferably 5 to 7, and even more preferably 5 or more and less than 7, from the viewpoint of solution stability.
[0151] The upper and lower limits of the content of the (A-2) component relative to 100% by mass of the slurry are, for example, 40, 35, 30, 25, 20, 15, 10, 9, 5, 4.5, 2% by mass, etc. In one embodiment, the content is preferably 2 to 40% by mass.
[0152] The upper and lower limits of the content of the (A-2A) component relative to 100% by mass of the slurry are, for example, 40, 35, 30, 25, 20, 15, 10, 9, 5, 4.5, 2, 0% by mass, etc. In one embodiment, the content is preferably 0 to 40% by mass.
[0153] The upper and lower limits of the mass ratio of the component (A-2A) to the component (A-1) in the slurry [mass of the component (A-2A) / mass of the component (A-1)] are, for example, 19, 17, 15, 13, 11, 10, 9, 7, 5, 4, 3, 2.5, 2.3, etc. In one embodiment, the mass ratio is preferably 2.3 to 19.
[0154] <Compatibility of polymers obtained by mixing components (A-1) and (A-2A)> From the viewpoint of electrode adhesion, it is preferable that the component (A-1) and the component (A-2A) are compatible (do not undergo microphase separation). An example of a method for confirming this phase separation structure is to measure the haze of the film. The film of the (A-1) component and the (A-2A) component is preferably obtained by mixing an aqueous solution containing the (A-1) component and the (A-2A) component in advance, applying the aqueous solution onto a flat glass plate, and preparing a film having a thickness of 5 to 30 μm in a circulating air dryer at 80° C. The haze of the prepared film can be measured using a turbidity meter "NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.)". The haze of the film is preferably 20% or less, and particularly preferably 10% or less. A film haze of less than 20% suggests that components (A-1) and (A-2A) are compatible with each other, whereas a film haze of more than 20% suggests that components (A-1) and (A-2A) are not compatible with each other (microphase separation).
[0155] <Electrode active material (B-1): Also called component (B-1)> Examples of the electrode active material include a negative electrode active material, a positive electrode active material, etc. The electrode active material may be used alone or in combination of two or more kinds.
[0156] <Negative electrode active material> The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium, and may be used alone or in combination of two or more. The negative electrode active material may be appropriately selected depending on the type of the target power storage device. Examples of the negative electrode active material include carbon materials, silicon materials, oxides containing lithium atoms, lead compounds, tin compounds, arsenic compounds, antimony compounds, and aluminum compounds that are alloyed with lithium. Carbon materials and materials that are alloyed with lithium have a large volume expansion rate during charging of the battery, so the effects of the present invention can be significantly exhibited.
[0157] Examples of the carbon material include highly crystalline carbon such as graphite (also called graphite, and examples of which include natural graphite and artificial graphite), low crystalline carbon (soft carbon, hard carbon), carbon black (ketjen black, acetylene black, channel black, lamp black, oil furnace black, thermal black, etc.), fullerene, carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon fibrils, mesocarbon microbeads (MCMB), and pitch-based carbon fibers.
[0158] The above silicon materials include silicon, silicon oxide, silicon alloys, as well as SiC, SiO x C y (0 <x≦3、0<y≦5)、Si3N4、Si2N2O、SiO xSilicon oxide composites represented by (0 < x ≤ 2) (such as materials described in JP-A-2004-185810 and JP-A-2005-259697), silicon materials described in JP-A-2004-185810, etc. are exemplified. Further, silicon materials described in Patent No. 5390336 and Patent No. 5903761 may also be used.
[0159] The above silicon oxide has a composition formula SiO x Silicon oxide represented by (0 < x < 2, preferably 0.1 ≤ x ≤ 1) is preferred.
[0160] The above silicon alloy is preferably an alloy of silicon and at least one transition metal selected from the group consisting of titanium, zirconium, nickel, copper, iron, and molybdenum. These transition metal silicon alloys are preferred because they have high electron conductivity and high strength. The silicon alloy is more preferably a silicon-nickel alloy or a silicon-titanium alloy, and particularly preferably a silicon-titanium alloy. The content ratio of silicon in the silicon alloy is preferably 10 mol% or more, more preferably 20 to 70 mol%, based on 100 mol% of the metal elements in the above silicon alloy. Note that the silicon material may be any of single crystal, polycrystal, and amorphous.
[0161] Further, when a silicon material is used as the negative electrode active material, a negative electrode active material other than the silicon material may be used in combination. Such negative electrode active materials include the above carbon materials; conductive polymers such as polyacene; A X B Y O Z (A is an alkali metal or a transition metal, B is at least one selected from transition metals such as cobalt, nickel, aluminum, tin, and manganese, O represents an oxygen atom, and X, Y, and Z are numbers in the ranges of 0.05 < X < 1.10, 0.85 < Y < 4.00, and 1.5 < Z < 5.00, respectively.) Composite metal oxides represented by, and other metal oxides, etc. are exemplified. When a silicon material is used as the negative electrode active material, it is preferable to use a carbon material in combination because the volume change accompanying the absorption and release of lithium is small.
[0162] The oxides containing lithium atoms include ternary lithium nickel cobalt manganese oxide, lithium-manganese composite oxide (LiMn2O4, etc.), lithium-nickel composite oxide (LiNiO2, etc.), lithium-cobalt composite oxide (LiCoO2, etc.), lithium-iron composite oxide (LiFeO2, etc.), lithium-nickel-manganese composite oxide (LiNi 0.5 Mn 0.5 O2, etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2 O2, etc.), lithium-transition metal phosphate compounds (LiFePO4, etc.), and lithium-transition metal sulfate compounds (Li x Fe2(SO4)3), lithium-titanium composite oxide (lithium titanate: Li4Ti5O 12 ) and other conventionally known negative electrode active materials.
[0163] The shape of the negative electrode active material is not particularly limited, and may be any shape such as fine particles or thin film, but fine particles are preferred. The average particle size of the negative electrode active material is not particularly limited, but the upper and lower limits are 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2.9, 2, 1, 0.5, 0.1 μm, etc. In one embodiment, from the viewpoint of forming a uniform and thin coating film, more specifically, if it is 0.1 μm or more, the handling property is good, and if it is 50 μm or less, the application of the electrode is easy, so that the average particle size of the negative electrode active material is preferably 0.1 to 50 μm, more preferably 0.1 to 45 μm, even more preferably 1 to 10 μm, and particularly preferably 5 μm.
[0164] In this disclosure, the term "particle size" refers to the maximum distance between any two points on the contour of a particle (hereinafter the same). In addition, in this disclosure, the term "average particle size" refers to a value calculated as the average particle size of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM) unless otherwise specified (hereinafter the same).
[0165] In order to prominently exhibit the effects of the present invention, the negative electrode active material contains a carbon material and / or a material that can be alloyed with lithium in an amount of preferably 50 mass % or more, more preferably 80 mass % or more, even more preferably 90 mass % or more, and particularly preferably 100 mass %.
[0166] In one embodiment, the content of silicon or silicon oxide covered with a carbon layer in the negative electrode active material is preferably 5% by mass or more (e.g., 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 100% by mass) relative to 100% by mass of the negative electrode active material, from the viewpoint of increasing the battery capacity of a lithium ion battery.
[0167] <Cathode active material> The positive electrode active material is exemplified by inorganic positive electrode active material and organic positive electrode active material. The inorganic positive electrode active material is exemplified by transition metal oxide, composite oxide of lithium and transition metal, transition metal sulfide, etc. The transition metal is exemplified by Fe, Co, Ni, Mn, Al, etc. Inorganic compounds used for the positive electrode active material are LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4, LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li [Li 0.1 Al 0.1 Mn 1.8 ]O4, LiFeVO4 and other lithium-containing composite metal oxides; TiS2, TiS3, amorphous MoS2 and other transition metal sulfides; Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, V6O 13Examples of the organic positive electrode active material include conductive polymers such as polyacetylene and poly-p-phenylene. Iron-based oxides, which have poor electrical conductivity, may be used as an electrode active material covered with a carbon material by making a carbon source material present during reduction and firing. Also, these compounds may be partially substituted with elements. Among these, in terms of practicality, electrical properties, and long life, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4, LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li [Li 0.1 Al 0.1 Mn 1.8 ]O4 is preferred.
[0168] The upper and lower limits of the content of the electrode active material (B-1) relative to 100% by mass of the above slurry are, for example, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20% by mass, etc. In one embodiment, the content is preferably 20 to 65% by mass.
[0169] <Conductive carbon material (B-2): Also called component (B-2)> Examples of the conductive carbon material include fibrous carbon and carbon black. The conductive carbon material may be used alone or in combination of two or more. The conductive carbon material may be used as a conductive assistant carbon material.
[0170] Examples of fibrous carbon include vapor grown carbon fiber (VGCF), carbon nanotube (CNT), and carbon nanofiber (CNF).
[0171] Examples of carbon black include graphite particles, acetylene black, ketjen black, furnace black, and the like.
[0172] The upper and lower limits of the content of the conductive carbon material (B-2) relative to 100 mass% of the slurry are, for example, 5, 4, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.07, 0.05, 0.03, 0.01 mass%, etc. In one embodiment, the content is preferably 0.01 to 5 mass%.
[0173] The upper and lower limits of the water content relative to 100% by mass of the slurry are, for example, 79, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20% by mass, etc. In one embodiment, the content is preferably 20 to 79% by mass.
[0174] <Slurry viscosity adjusting solvent> In one embodiment, the slurry may contain a slurry viscosity adjusting solvent. As the slurry viscosity adjusting solvent, various known ones can be used without particular limitation, and may be used alone or in combination of two or more kinds. Examples of the solvent include ether solvent, ketone solvent, alcohol solvent, amide solvent, water, etc.
[0175] The upper and lower limits of the content of the slurry viscosity adjusting solvent relative to 100% by mass of the slurry are, for example, 10, 9, 7, 5, 3, 2, 1, 0% by mass, etc. In one embodiment, the content is preferably 0 to 10% by mass.
[0176] <Hydroxysilyl compounds> In one embodiment, the slurry may contain a hydroxysilyl compound. In the present disclosure, the hydroxysilyl compound means a compound having a structure in which a hydroxy group (-OH) is directly bonded to a silicon atom, the trihydroxysilyl compound means a compound having a trihydroxysilyl group (-Si(OH)3), and the tetrahydroxysilyl compound means a compound represented by Si(OH)4.
[0177] In one embodiment, the trihydroxysilyl compound has the general formula: RSi(OH)3 (In the formula, R represents a substituted or unsubstituted alkyl group, vinyl group, or (meth)acryloxy group, and examples of the substituent include an amino group, a mercapto group, a glycidoxy group, a (meth)acryloxy group, and an epoxy group.) It is a compound represented by the formula:
[0178] The hydroxysilyl compound is preferably prepared by hydrolyzing a silane coupling agent or a tetraalkoxysilane. The hydroxysilyl compound may be partially polycondensed as long as it does not lose its water solubility. The silane coupling agent may be a silane coupling agent generally used in the technical field to which the present invention belongs.
[0179] The silane coupling agent is not particularly limited. The hydroxysilyl compound produced from the silane coupling agent may be used alone or in combination of two or more. In one embodiment, the hydroxysilyl compound includes trihydroxysilylpropylamine.
[0180] Examples of trialkoxysilanes include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and tetrahydroxysilane.
[0181] Examples of the tetraalkoxysilane include tetramethoxysilane, tetramethoxysilane oligomer, tetraethoxysilane, and tetraethoxysilane oligomer.
[0182] Examples of the upper and lower limits of the content of the hydroxysilyl compound relative to 100 mass% of the slurry are 15, 13, 10, 9, 7, 5, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.07, 0.05, 0.04, 0.02, 0.01, 0 mass%, etc. In one embodiment, the content is preferably 0 to 15 mass%.
[0183] <Crosslinking agent> In one embodiment, the slurry may contain a cross-linking agent. The cross-linking agents may be used alone or in combination of two or more kinds.
[0184] Examples of the crosslinking agent include water-soluble polyhydric alcohols, formaldehyde, glyoxal, hexamethylenetetramine, urea formaldehyde resins, and methylolmelamine resins. Formaldehyde, glyoxal, hexamethylenetetramine, urea formaldehyde resins, methylolmelamine resins, carbodiimides, polyfunctional epoxides, oxazolines, polyfunctional hydrazides, isocyanates, melamine, urea, and mixtures thereof.
[0185] The water-soluble polyhydric alcohol is a water-soluble alcohol having two or more hydroxyl groups.
[0186] Examples of the water-soluble polyhydric alcohol include methylene glycol, ethylene glycol, propylene glycol, isoprene glycol, 1,3-butylene glycol, 1,4-butylene glycol, diethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, glycerin, diglycerin, and polyglycerin. Among these, the general formula (B1): [ka] (wherein R is a methylene group, an ethylene group, or a propylene group, and n is an integer of 1 or more), particularly polyethylene glycol (n=1 to 6), is preferred.
[0187] Examples of the upper and lower limits of the content of the crosslinking agent relative to 100% by mass of the slurry are 20, 19, 17, 15, 13, 10, 9, 7, 5, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.05, 0.03, 0.01, 0.009, 0.005, 0.003, 0.001, 0% by mass, etc. In one embodiment, the content is preferably 0 to 20% by mass.
[0188] <Thickener> In one embodiment, the slurry may contain a thickener. The thickener may be used alone or in combination of two or more kinds.
[0189] Examples of thickeners include cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; (modified) poly(meth)acrylic acid and their ammonium salts and alkali metal salts; (modified) polyvinyl alcohols such as copolymers of acrylic acid or acrylates and vinyl alcohol, and copolymers of maleic anhydride or maleic acid or fumaric acid and vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, and hydrogenated acrylonitrile-butadiene copolymers.
[0190] Examples of the upper and lower limits of the content of the thickener relative to 100 mass% of the slurry are 20, 19, 17, 15, 13, 10, 9, 7, 5, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.05, 0.03, 0.01, 0.009, 0.005, 0.003, 0.001, 0 mass%, etc. In one embodiment, the content is preferably 0 to 20 mass%.
[0191] <Additives> The above slurry may contain, as an additive, an agent other than the conductive carbon material dispersant for lithium ion batteries, the water-soluble poly(meth)acrylamide (A-1), the polymer (A-2), the electrode active material (B-1), the conductive carbon material (B-2), water, a slurry viscosity adjusting solvent, a hydroxysilyl compound, a crosslinking agent, or a thickener.
[0192] The content of the additive is, for example, 0 to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, 0% by mass, etc., relative to 100% by mass of the slurry.
[0193] Examples of the additives include dispersants other than the above-mentioned conductive carbon material dispersants for lithium ion batteries, leveling agents, antioxidants, and the like.
[0194] Examples of dispersants other than the above-mentioned dispersant for conductive carbon material for lithium ion batteries include anionic dispersants, cationic dispersants, nonionic dispersants, polymer dispersants, and the like.
[0195] Examples of the leveling agent include surfactants such as alkyl surfactants, silicon surfactants, fluorine surfactants, and metal surfactants. By using a surfactant, it is possible to prevent repellency during coating and improve the smoothness of the slurry layer (coating layer).
[0196] Examples of the antioxidant include phenol compounds, hydroquinone compounds, organic phosphorus compounds, sulfur compounds, phenylenediamine compounds, and polymeric phenol compounds. The polymeric phenol compounds are polymers having a phenol structure in the molecule. The weight average molecular weight of the polymeric phenol compounds is preferably 200 to 1000, and more preferably 600 to 700.
[0197] Examples of additives other than those mentioned above include at least one compound selected from the group consisting of unsaturated carboxylic acids, unsaturated amides, and salts thereof.
[0198] The method for producing the slurry includes, for example, a method of mixing a conductive carbon material dispersant for lithium ion batteries, a polymer (A-2), an electrode active material (B-1), a conductive carbon material (B-2), and water, and a method of mixing a water-soluble poly(meth)acrylamide (A-1), a polymer (A-2), an electrode active material (B-1), a conductive carbon material (B-2), and water. Note that the order of mixing in the above methods is not particularly limited.
[0199] Examples of means for mixing the slurry include a ball mill, a sand mill, a pigment disperser, a crusher, an ultrasonic disperser, a homogenizer, a planetary mixer, and a Hobart mixer.
[0200] The lithium ion battery electrode slurry can be used as a lithium ion battery negative electrode slurry or a lithium ion battery positive electrode slurry.
[0201] [Electrodes for lithium-ion batteries] The present disclosure provides a lithium ion battery electrode obtained by applying the above-mentioned slurry for a lithium ion battery electrode to a current collector, drying and curing the slurry, The electrode has a cured product of the above-mentioned slurry for a lithium ion battery electrode on a current collector.
[0202] The coating means is not particularly limited, and examples thereof include conventionally known coating devices such as a comma coater, a gravure coater, a microgravure coater, a die coater, and a bar coater.
[0203] The drying means is not particularly limited, and the temperature is preferably about 80 to 200° C., more preferably about 90 to 180° C., and the atmosphere may be dry air or an inert atmosphere. From the viewpoint of improving the electrode adhesion, a drying means using far infrared rays may also be used.
[0204] The thickness of the electrode (cured coating film) is not particularly limited, but is preferably about 5 to 300 μm, and more preferably about 10 to 250 μm. By setting the thickness within the above range, it becomes easier to obtain a sufficient Li absorption / release function for a high-density current value.
[0205] The current collector may be any of various known current collectors without any particular limitation. The material of the current collector is not particularly limited, and examples thereof include metal materials such as copper, iron, aluminum, nickel, stainless steel, and nickel-plated steel, and carbon materials such as carbon cloth and carbon paper. The form of the current collector is also not particularly limited, and examples of metal materials include metal foil, metal cylinder, metal coil, and metal plate, and examples of carbon materials include carbon plate, carbon thin film, and carbon cylinder. Among them, when the electrode active material is used for the negative electrode, copper foil is preferred as the current collector because it is currently used in industrialized products.
[0206] The lithium ion battery electrode can be used as a negative electrode for a lithium ion battery or a positive electrode for a lithium ion battery.
[0207] [Lithium-ion battery] The present disclosure provides a lithium ion battery including the lithium ion battery electrode. In one embodiment, the battery includes an electrolyte, a separator, a positive electrode, and the like. These are not particularly limited.
[0208] The electrolyte solution may be, for example, a non-aqueous electrolyte solution in which a supporting electrolyte is dissolved in a non-aqueous solvent, etc. The non-aqueous electrolyte solution may also contain a film-forming agent.
[0209] As the non-aqueous solvent, various known solvents can be used without any particular limitation, and may be used alone or in combination of two or more. Examples of the non-aqueous solvent include chain carbonate solvents such as diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate; cyclic carbonate solvents such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain ether solvents such as 1,2-dimethoxyethane; cyclic ether solvents such as tetrahydrofuran, 2-methyltetrahydrofuran, sulfolane, and 1,3-dioxolane; chain ester solvents such as methyl formate, methyl acetate, and methyl propionate; cyclic ester solvents such as γ-butyrolactone and γ-valerolactone; and acetonitrile. Among these, a combination of a mixed solvent containing a cyclic carbonate and a chain carbonate is preferred.
[0210] The supporting electrolyte is a lithium salt. Various known lithium salts can be used without particular limitation, and may be used alone or in combination of two or more. Examples of the supporting electrolyte include LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. Among them, LiPF6, LiClO4, and CF3SO3Li, which are easily soluble in a solvent and show a high degree of dissociation, are preferred. The higher the degree of dissociation of the supporting electrolyte used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0211] The coating agent may be any of various known agents without particular limitation, and may be used alone or in combination of two or more. Examples of the coating agent include carbonate compounds such as vinylene carbonate, vinyl ethylene carbonate, vinyl ethyl carbonate, methyl phenyl carbonate, fluoroethylene carbonate, and difluoroethylene carbonate; alkene sulfides such as ethylene sulfide and propylene sulfide; sultone compounds such as 1,3-propane sultone and 1,4-butane sultone; and acid anhydrides such as maleic anhydride and succinic anhydride. The content of the coating agent in the electrolyte is not particularly limited, but is preferably 10% by mass or less, 8% by mass or less, 5% by mass or less, and 2% by mass or less in that order. By making the content 10% by mass or less, it becomes easier to obtain the advantages of the coating agent, such as suppression of initial irreversible capacity and improvement of low-temperature characteristics and rate characteristics.
[0212] The separator is an article interposed between the positive electrode and the negative electrode, and is used to prevent short circuit between the electrodes. Specifically, a porous separator such as a porous membrane or a nonwoven fabric can be preferably used, and is used by impregnating the nonaqueous electrolyte solution. The separator is made of a polyolefin such as polyethylene or polypropylene, or polyethersulfone, and is preferably made of polyolefin.
[0213] In addition, when a lithium ion battery is manufactured using a negative electrode manufactured using the above-mentioned slurry for lithium ion battery electrodes as a negative electrode and a positive electrode manufactured without using the above-mentioned slurry for lithium ion battery electrodes as a positive electrode, any of various known positive electrodes can be used without any particular limitation.
[0214] The positive electrode may be any of various known positive electrodes without any particular limitations. Examples of the positive electrode include a positive electrode obtained by mixing a positive electrode active material, a conductive assistant, and a positive electrode binder with an organic solvent to prepare a slurry, and applying the prepared slurry to a positive electrode current collector, drying, and pressing the slurry.
[0215] The positive electrode binder may be any of various known binders without particular limitation, and may be used alone or in combination of two or more. Examples of the positive electrode binder include fluorine-based resins (polyvinylidene fluoride, polytetrafluoroethylene, etc.), polyolefins (polyethylene, polypropylene, etc.), polymers having unsaturated bonds (styrene-butadiene rubber, isoprene rubber, butadiene rubber, etc.), and acrylic acid-based polymers (acrylic acid copolymers, methacrylic acid copolymers, etc.).
[0216] The positive electrode current collector is exemplified by an aluminum foil, a stainless steel foil, and the like.
[0217] The shape of the lithium ion battery is not particularly limited. Examples of the shape of the lithium ion battery include a cylinder type in which a sheet electrode and a separator are spirally wound, a cylinder type with an inside-out structure in which a pellet electrode and a separator are combined, and a coin type in which a pellet electrode and a separator are laminated. In addition, by housing a battery of these shapes in an arbitrary exterior case, it can be used in an arbitrary shape such as a coin type, a cylindrical type, or a square type.
[0218] The method for manufacturing the lithium ion battery is not particularly limited, and the battery may be assembled in an appropriate procedure according to the structure of the battery. The lithium ion battery may be manufactured, for example, by the method described in JP 2013-089437 A. The battery can be manufactured by placing a negative electrode on an exterior case, providing an electrolyte and a separator thereon, placing a positive electrode facing the negative electrode, and fixing them with a gasket and a sealing plate. EXAMPLES
[0219] The present invention will be specifically described below through examples and comparative examples. However, the above-mentioned description of the preferred embodiment and the following examples are provided for illustrative purposes only and are not provided for the purpose of limiting the present invention. Therefore, the scope of the present invention is not limited to the embodiments or examples specifically described in this specification, but is limited only by the claims. In each example and comparative example, unless otherwise specified, numerical values such as parts and % are based on mass.
[0220] Preparation of water-soluble poly(meth)acrylamide (A-1) Example 1-1 387 g of ion-exchanged water was placed in a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, and oxygen was removed from the reaction system by passing nitrogen gas through it, after which the temperature was raised to 80°C. 300 g (2.11 mol) of 50% acrylamide aqueous solution, 581 g (1.27 mol) of 50% acrylamide sodium t-butylsulfonate aqueous solution, 0.55 g (0.0035 mol) of sodium methallylsulfonate, 12.7 g (0.14 mol) of 80% acrylic acid, 8 g of ion-exchanged water, and 21 g of isopropyl alcohol were placed in a 2 L beaker and stirred for 30 minutes to obtain a homogeneous solution A. 4.1 g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 199 g of ion-exchanged water were placed in a 300 mL beaker and stirred for 30 minutes to obtain a homogeneous solution B. Solution A and solution B were simultaneously dropped into the reactor over a period of 3 hours to carry out a polymerization reaction. After that, 5.8 g (0.07 mol) of 48% sodium hydroxide aqueous solution was added as a neutralizing agent and stirred to obtain a conductive carbon material dispersant for lithium-ion batteries containing water-soluble poly(meth)acrylamide (A-1) with a solid content of 30 mass%. The B-type viscosity of this dispersant at 25°C was 350 mPa s and the pH was 5.2.
[0221] Example 1 other than Example 1-1 was carried out in the same manner as Example 1-1 above, except that the composition in Example 1-1 was changed to that shown in the table below.
[0222] Comparative Example 1-1 In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 1310g of ion-exchanged water, 80.0g (0.56mol) of 50% acrylamide aqueous solution, 5.8g (0.06mol) of 80% acrylic acid, 266.0g (0.58mol) of 50% acrylamide sodium t-butylsulfonate aqueous solution, 46.8g (0.40mol) of 2-hydroxyethyl acrylate, and 0.25g (0.0016mol) of sodium methallylsulfonate were placed, and oxygen in the reaction system was removed by passing nitrogen gas through the reaction system, and the temperature was raised to 50°C. 2.0g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 20g of ion-exchanged water were placed therein, and the temperature was raised to 80°C and the reaction was carried out for 3 hours. A dispersant containing water-soluble poly(meth)acrylamide with a solid content concentration of 13% by mass was obtained. The Brookfield viscosity of this dispersant at 25°C was 730 mPa·s and the pH was 5.1.
[0223] Comparative Example 1 other than the above Comparative Example 1-1 was carried out in the same manner as Example 1-1, except that the composition was changed to that shown in the following table. [Table 1] AM: Acrylamide (Mitsubishi Chemical Corporation "50% Acrylamide") ·DMAA: N,N-Dimethylacrylamide ("DMAA" manufactured by KJ Chemicals Co., Ltd.) ·ATBSNa: Sodium acrylamide t-butyl sulfonate ("ATBS-Na" manufactured by Toagosei Co., Ltd.) ·SMAS: Sodium methallyl sulfonate ·HEA: 2-Hydroxyethyl acrylate ("HEA" manufactured by Osaka Organic Chemical Industry Co., Ltd.) ·HEMA: 2-Hydroxyethyl methacrylate ·AN: Acrylonitrile ("Acrylonitrile" manufactured by Mitsubishi Chemical Corporation) ·AA: Acrylic acid ("80% Acrylic acid" manufactured by Osaka Organic Chemical Industry Co., Ltd.) ·NaOH: Sodium hydroxide ("48% Sodium hydroxide solution" manufactured by Kanto Chemical Co., Inc.)
[0224] <B-type viscosity> The viscosity of each dispersant was measured at 25°C under the following conditions using a B-type viscometer (product name "TVB-10M B-type viscometer" manufactured by Toki Sangyo Co., Ltd.). When the viscosity is less than 500 mPa·s: Use No. 2 rotor, rotation speed 60 rpm. When the viscosity is 500 to less than 1,000 mPa·s: Use No. 3 rotor, rotation speed 30 rpm. When the viscosity is 1,000 to less than 10,000 mPa·s: Use No. 3 rotor, rotation speed 12 rpm. When the viscosity is 10,000 mPa·s or more: Use No. 3 rotor, rotation speed 6 rpm.
[0225] <Weight average molecular weight> The weight average molecular weight was determined as the value in terms of polyacrylic acid measured by gel permeation chromatography (GPC) under a 0.2 M phosphate buffer / acetonitrile solution (90 / 10, pH 8.0). The GPC apparatus used was HLC-8220 (manufactured by Tosoh Corporation), and the column used was SB-806M-HQ (manufactured by SHODEX).
[0226] <ph> The pH of each dispersant was measured at 25° C. using a glass electrode pH meter (product name "Handy pH Meter D-52", manufactured by Horiba, Ltd.).
[0227] (A-2) Manufacture of component Manufacturing Example 1 In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 1007g of ion-exchanged water, 100g (0.70mol) of 50% acrylamide aqueous solution, 63.8g (0.70mol) of 80% acrylic acid, 69.8g (0.60mol) of 2-hydroxyethyl acrylate, and 0.32g (0.0020mol) of sodium methallylsulfonate were placed, and oxygen in the reaction system was removed by passing nitrogen gas through it, and the temperature was raised to 55°C. 1.6g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 16g of ion-exchanged water were placed therein, and the temperature was raised to 80°C and the reaction was carried out for 3 hours. Then, 52.7g (0.63mol) of 48% sodium hydroxide aqueous solution was added as a neutralizing agent and stirred, and ion-exchanged water was added so that the solid concentration was 13%, to obtain an aqueous solution containing water-soluble poly(meth)acrylamide. The aqueous solution had a Brookfield viscosity of 3000 mPa·s and a pH of 6.0 at 25°C.
[0228] The production examples other than Production Example 1 were carried out in the same manner as Production Example 1, except that the composition in Production Example 1 was changed to that shown in the table below.
[0229] [Table 2] *The amount of neutralizing agent is based on 100 mol % of the acidic groups (carboxyl groups) contained in component (A-2).
[0230] Conductive carbon paste evaluation, resin swelling rate and electrolyte resistance evaluation Example 2-1 Using a commercially available planetary centrifugal mixer (product name "Awatori Rentaro", manufactured by Thinky Corporation), 40 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1, calculated as solid content, and 60 parts by mass of a conductive carbon material ("Super C65", manufactured by Imerys GC Japan, Inc.) were charged into a container dedicated to the mixer. Ion-exchanged water was added thereto so that the solid content concentration was 13.5%, and the container was set in the planetary centrifugal mixer. Next, after kneading for 10 minutes at 2000 rpm, a conductive carbon material paste was obtained.
[0231] In Example 2 and Comparative Examples other than Example 2-1, conductive carbon material pastes were prepared in the same manner as in Example 2-1, except that the composition in Example 2-1 was changed to that shown in the table below.
[0232] <Initial dispersion test of conductive carbon paste> The median diameter (D50) of the conductive carbon material paste obtained in Example 2-1 was measured using a commercially available laser diffraction / scattering type particle size distribution measurement device (product name "LA-960", manufactured by HORIBA). The higher the measured median diameter value, the worse the initial dispersibility of the conductive additive and the more aggregated it is. The lower the median diameter value, the better the initial dispersibility of the conductive additive is. The median diameter (D50) was evaluated according to the following criteria. A: Less than 3.0 μm B:3.0μm or more
[0233] <Dispersion stability test of conductive carbon paste> The conductive carbon material paste obtained in Example 2-1 was left to stand at room temperature for 24 hours, and then the median diameter (D50) was measured. The greater the change in the measured median diameter, the worse the dispersion stability of the conductive assistant and the more aggregated it is. The smaller the change in the median diameter, the better the dispersion stability of the conductive assistant. The rate of change in the median diameter (D50) was calculated using the following formula and evaluated according to the following evaluation criteria. Rate of change (%) = [{(D50 of conductive carbon material paste after 24 hours) - (D50 of conductive carbon material paste after initial dispersion test)} / (D50 of conductive carbon material paste after initial dispersion test)] × 100 A: Less than ±20% B: ±20% or more
[0234] <Evaluation of electrolyte swelling rate and electrolyte resistance of water-soluble poly(meth)acrylamide (A-1)> The water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1 was poured into a petri dish and dried in a circulating dryer at 105°C for 3 hours to produce a solid resin. The mass α of the obtained solid resin was then measured. Next, the obtained solid resin was immersed in 50 mL of dimethyl carbonate solvent and stored in an environment of 25°C for 48 hours. After that, the immersed and stored solid resin was taken out of the dimethyl carbonate solvent, and the mass β was measured after the dimethyl carbonate attached to the surface of the solid resin was thoroughly wiped off. The mass γ of the wiped solid resin was then measured after drying in a circulating dryer at 105°C for 1 hour. Using the measured masses β and γ, the electrolyte swelling ratio of the polymer was calculated as (β / γ)×100(%). A lower electrolyte swelling ratio (closer to 100%) indicates a lower electrolyte swelling property of the polymer. A: Electrolyte swelling rate is less than 110% B: Electrolyte swelling rate is 110% or more and less than 120% C: Electrolyte swelling rate is 120% or more Similarly, the measured masses α and γ were used to calculate the electrolyte resistance rate of the polymer = (γ / α) × 100 (%). A lower electrolyte resistance rate (closer to 100%) indicates a lower solubility of the polymer in the electrolyte. A: Electrolyte resistance rate is 95% or more B: Electrolyte resistance rate is less than 95% [Table 3] CMC: Carboxymethyl cellulose PVP: Polyvinylpyrrolidone
[0235] Production of slurry for lithium-ion battery electrodes and cell fabrication and evaluation <Production of slurry for lithium-ion battery electrodes> Example 3-1 A slurry was prepared using a commercially available homodisper ("Homodisper 2.5 type" manufactured by Primix Corporation). 0.5 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1 in terms of solid content, 4.5 parts by mass of the binder (A-2) obtained in Production Example 1 in terms of solid content, 80 parts by mass of graphite having a D50 (median diameter) of 20 μm, 20 parts by mass of silicon monoxide particles ("CC powder" manufactured by Osaka Titanium Technologies Co., Ltd.) having a D50 (median diameter) of 5 μm, and 1 part by mass of a conductive carbon material ("Super C65" manufactured by Imerys GC Japan Co., Ltd.) were mixed in a mayonnaise bottle as a container. Ion-exchanged water was added thereto so that the solid content concentration was 47%, and the container was set in the homodisper. Then, the mixture was kneaded at 2000 rpm for 30 minutes. Thereafter, the mixture was defoamed for 1 minute using a planetary centrifugal mixer (Thinky Corporation's "Awatori Rentaro") to obtain a slurry for a lithium ion battery electrode.
[0236] Examples 3 and comparative examples other than Example 3-1 were carried out in the same manner as Example 3-1, except that the composition in Example 3-1 was changed to that shown in the table below.
[0237] Example 4-1 A slurry was prepared using a commercially available Homo Disper ("Homo Disper 2.5 type" manufactured by Primix Corporation). A mayonnaise bottle was used as a container, and 0.5 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-2, 4.5 parts by mass of the binder (A-2) obtained in Production Example 3, and lithium nickel manganese oxide (Li[Ni 1 / 2 Mn 3 / 2 ]O4, median diameter D50: 3.7μm) and 1 part by mass of conductive carbon material ("Super C65" manufactured by Imerys GC Japan Co., Ltd.) were mixed. Ion-exchanged water was added thereto so that the solid content concentration was 50%, and the container was set in the homodisper. Next, the mixture was kneaded at 2000 rpm for 30 minutes. After that, the mixture was degassed for 1 minute using a planetary centrifugal mixer ("Awatori Rentaro" manufactured by Thinky Corporation) to obtain a slurry for lithium-ion battery electrodes. In Comparative Example 4-1, a slurry was prepared in the same manner as in Example 4-1 above, except that the composition was changed to that shown in Table 4.
[0238] <Storage stability test of slurry for lithium-ion battery electrodes> The storage stability of the lithium ion battery electrode slurry was evaluated as follows. The viscosity (unit: mPa s) of the lithium-ion battery electrode slurry was measured using a Brookfield viscometer, and then it was stored in an oven heated to 40°C for 3 days. After storage, the viscosity was measured again using the Brookfield viscometer, and the change in viscosity was calculated using the following formula and evaluated according to the following criteria. Viscosity change (%) = {(viscosity of electrode slurry after storage) / (viscosity of electrode slurry before storage)} × 100 A: Less than 110% B: 110% or more but less than 120% C: 120% or more
[0239] <Production of negative electrodes> The above slurry was uniformly applied to the surface of a copper foil current collector by a doctor blade method so that the film thickness after drying would be 170 μm, and then dried at 150° C. for 30 minutes, followed by heat treatment at 150° C. / vacuum for 120 minutes. After that, the density of the film (electrode active material layer) was 1.5 g / cm 3 The electrode was obtained by pressing the electrode sheet with a roll press machine so that the electrode sheet had a thickness of 100 mm.
[0240] <Production of positive electrodes> The above slurry was uniformly applied to the surface of a current collector made of aluminum foil by a doctor blade method so that the film thickness after drying would be 110 μm, and after drying at 150° C. for 30 minutes, it was heat-treated at 150° C. / vacuum for 120 minutes. After that, the density of the film (electrode active material layer) was 3.0 g / cm 3 The electrode was obtained by pressing the electrode sheet with a roll press machine so that the electrode sheet had a thickness of 100 mm.
[0241] <Electrode Adhesion Evaluation> The electrode adhesion was evaluated as follows. A test piece measuring 2 cm wide x 10 cm long was cut out from the electrode and fixed with the coating surface facing up. Next, a 15 mm wide adhesive tape ("Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.) (specified in JIS Z1522) was applied to the surface of the active material layer of the test piece while pressing it, and then the stress was measured when the adhesive tape was peeled off from one end of the test piece in the 180° direction at a speed of 30 mm / min using a tensile tester ("Tensilon RTM-100" manufactured by A&D Co., Ltd.) under conditions of 25°C. The measurement was performed twice, and the average value was calculated as the peel strength. The higher the peel strength, the higher the adhesion strength between the current collector and the active material layer or the binding strength between the active materials, indicating that the active material layer or the active materials are less likely to peel off from the current collector.
[0242] <Assembling lithium half-cells> In an argon-substituted glove box, the above electrode was punched out to a diameter of 16 mm and placed inside the packing on the Al bottom cover of a test cell (manufactured by Nippon Tomcell Co., Ltd.). Next, a separator made of a polypropylene porous film punched out to a diameter of 24 mm (manufactured by CS TECH CO., LTD, product name "Selion P2010") was placed, and 500 μL of electrolyte was poured in to prevent air from entering, and then a commercially available metallic lithium foil punched out to a diameter of 16 mm was placed on the separator. The exterior body of the test cell was closed and sealed with screws to assemble a lithium half cell. The electrolyte used here was a solution in which LiPF6 was dissolved at a concentration of 1 mol / L in a solvent of ethylene carbonate / ethyl methyl carbonate = 1 / 1 (mass ratio).
[0243] <Charge / discharge measurement> The lithium half-cell was placed in a thermostatic chamber at 25° C., and charging was started at a constant current (0.1 C), and charging was completed (cut off) when the voltage reached 0.01 V. Next, discharging was started at a constant current (0.1 C), and charging and discharging was repeated 30 times, with discharging completed (cut off) when the voltage reached 1.0 V. In the above measurement conditions, "1C" refers to the current value at which a cell with a certain capacity is discharged at a constant current and the discharge is completed in 1 hour. For example, "0.1C" refers to the current value at which the discharge is completed in 10 hours, and "10C" refers to the current value at which the discharge is completed in 0.1 hour.
[0244] <Discharge capacity maintenance rate> The discharge capacity retention rate was calculated according to the following formula. Discharge capacity retention rate = {(discharge capacity at 30th cycle) / (discharge capacity at 1st cycle)} x 100 (%)
[0245] <haze> The aqueous solutions of Examples 3 and 4 and Comparative Examples 3 and 4 were applied onto a flat glass plate, and films were prepared to a thickness of 5 to 30 μm in a circulating air dryer at 80° C. The haze of the prepared films was measured using a turbidity meter "NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.)." As a result of the measurement, the haze of Examples 3-3, 3-8, and 3-9 was 3, 6, and 26, respectively. On the other hand, the haze of Examples 3 and 4 other than the above was 1 or less. [Table 4] SBR: Styrene-butadiene copolymer latex CMC: Carboxymethyl cellulose< / haze> < / ph>
Claims
1. Contains 2 to 60 mol % of structural units derived from a (meth)acrylamide group-containing compound (a) and 10 to 70 mol % of structural units derived from an unsaturated sulfonic acid or a salt thereof (b); The weight average molecular weight is 10,000 or more and less than 300,000. Water-soluble poly(meth)acrylamide (A-1) A compound which corresponds to both component (a) and component (b) is classified as component (b). Conductive carbon material dispersant for lithium-ion batteries.
2. The water-soluble poly(meth)acrylamide (A-1) is Contains 20 to 70 mol % of structural units derived from (meth)acrylic acid ester (c); The conductive carbon material dispersant for a lithium ion battery according to claim 1 .
3. The conductive carbon material dispersant for a lithium ion battery according to claim 1 or 2, Polymer (A-2), Electrode active material (B-1), Conductive carbon material (B-2), and water.
4. The polymer (A-2) is The slurry for lithium ion battery electrodes according to claim 3, which is a water-soluble poly(meth)acrylamide (A-2A) containing a structural unit derived from the (meth)acrylamide group-containing compound (a).
5. 5. An electrode for a lithium ion battery, obtained by applying the slurry for a lithium ion battery electrode according to claim 3 or 4 to a current collector and drying the same.
6. A lithium ion battery comprising the lithium ion battery electrode according to claim 5.
Citation Information
Patent Citations
Slurry for lithium ion battery negative electrode, method for manufacturing the same, negative electrode for lithium ion battery, and lithium ion battery
JP2018006334A
Binder aqueous solution for lithium ion battery, slurry for lithium ion battery, manufacturing methods thereof, electrode for lithium ion battery, separator for lithium ion battery, separator / electrode laminate for lithium ion battery and lithium ion battery
JP2019057486A
Binder composition for storage device, slurry for storage device, electrode for storage device, separator, and storage device
WO2015008626A1
Binder composition for non-aqueous secondary battery electrode, slurry composition for non-aqueous secondary battery electrode, electrode for non-aqueous secondary battery, and non-aqueous secondary battery
WO2019159706A1