Rubber gloves and their manufacturing method

The rubber glove design with a polyethylene oxide inner layer addresses flowback and fingertip issues, enhancing comfort and texture by stabilizing the immersion liquid during manufacturing.

JP7581820B2Active Publication Date: 2024-11-13SUMITOMO RUBBER INDUSTRIES LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020204657
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-11-13
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Conventional rubber gloves suffer from issues such as flowback and fingertip formation due to uneven film thickness, which adversely affect wearing comfort, and the flocked texture can be improved for better user experience.

Method used

A rubber glove design comprising an outer layer made primarily of a rubber component and an inner layer containing polyethylene oxide, which suppresses flowback and fingertip formation by reducing the fluidity of the immersion liquid during manufacturing.

Benefits of technology

The design results in a rubber glove with an excellent flocked texture and improved wearing comfort by minimizing flowback and fingertip occurrences.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581820000001
    Figure 0007581820000001
  • Figure 0007581820000002
    Figure 0007581820000002
  • Figure 0007581820000003
    Figure 0007581820000003
Patent Text Reader

Abstract

To provide a rubber glove in which occurrence of flow back and finger tips is suppressed, which is excellent in pile flocking texture and excellent in wearing feeling.SOLUTION: A rubber glove includes: an outer layer including rubber components (A) as main components; and an inner layer including macromolecular components (B) as main components. The inner layer contains polyethylene oxide.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber glove. The present invention also relates to a method for producing the same. [Background technology]

[0002] Rubber gloves made of rubber film are used for a wide variety of purposes in various fields such as general households, industrial production, research, medicine, etc., because of their ease of use, low cost, etc. In recent years, it has become desirable to use aqueous materials as raw materials from the viewpoint of environmental protection, and latex rubber gloves have become widespread.

[0003] The performance and quality required for latex gloves vary depending on the application, but comfort is an important quality required for any application. One of the methods for improving comfort from the design aspect is known to be flocking the inner surface of the glove. Flocking is specifically a process in which pile (short fibers) of cotton, rayon, etc. are flocked to the inner surface of the glove by electrostatic action, etc. The denser the pile is, the better the texture of the flocking and the better the comfort.

[0004] Here, it is known that in order to plant the pile densely, a layer with enhanced adhesiveness by adding an acrylic resin is provided on the inside of the glove. For example, Patent Document 1 discloses that in a rubber glove having an outermost layer made of nitrile rubber and an innermost layer with flocking, an acrylic resin with a glass transition temperature of -35°C or more and 0°C or less is blended in the innermost layer.

[0005] In addition, the uniformity of the thickness of the rubber glove affects the comfort of wearing it, and if there is a region of the rubber glove with a locally large thickness, the comfort of wearing it becomes poor. Here, the salt coagulant immersion method is widely used industrially for manufacturing latex rubber gloves. For example, Patent Document 1 describes a method in which a hand mold corresponding to the three-dimensional shape of the glove is prepared, the surface of the hand mold is treated with a coagulant such as an aqueous calcium nitrate solution, the treated hand mold is then immersed in an immersion liquid for the outermost layer containing latex and then pulled out to attach the immersion liquid to the surface of the hand mold, and then, in a semi-dried state, the hand mold is immersed in an immersion liquid for the innermost layer containing acrylic latex and then pulled out, and before the immersion liquid dries, flocking is performed by electrostatic flocking or the like, and then the innermost layer is formed by heating, thereby manufacturing a rubber glove.

[0006] In this method, if the latex hardens slowly, dripping phenomena called flowback and fingertips may occur on the hand mold, making the rubber layer thicker than the surrounding area. Flowback occurs mainly on the fingers and between the fingers, while fingertips occur at the fingertips. Flowback and fingertips have a negative effect on the comfort of the product. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2020-12216 A Summary of the Invention [Problem to be solved by the invention]

[0008] As a result of intensive research, the present inventors have found that the conventional rubber gloves have room for improvement in terms of pile texture. Furthermore, the present inventors have found that the conventional rubber gloves have room for improvement in terms of flowback and fingertip occurrence. Therefore, the present inventors have found that the conventional rubber gloves have room for improvement in terms of comfort.

[0009] In view of the above circumstances, the present invention provides a rubber glove which is suppressed in occurrence of flowback and fingertips, has an excellent pile texture, and is comfortable to wear. [Means for solving the problem]

[0010] The present invention relates to a rubber glove comprising an outer layer containing a rubber component (A) as a main component and an inner layer containing a polymer component (B) as a main component, wherein the inner layer contains polyethylene oxide.

[0011] From another aspect, the present invention provides a method for manufacturing a rubber glove, comprising the steps of: treating a surface of a hand mold corresponding to a three-dimensional shape of a rubber glove with a coagulant; immersing the treated hand mold in an immersion liquid for forming an outer layer containing latex (C); and immersing the immersed hand mold in an immersion liquid for forming an inner layer containing latex (D), wherein the immersion liquid for forming the inner layer contains polyethylene oxide. Effect of the Invention

[0012] According to the present invention, it is possible to provide a rubber glove which is suppressed in occurrence of flowback and fingertips, has an excellent pile texture, and is comfortable to wear. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The rubber glove of the present invention comprises an outer layer containing a rubber component (A) as a main component and an inner layer containing a polymer component (B) as a main component. Here, the inner layer contains polyethylene oxide. In this specification, the "inner layer" means a layer on the side of the "outer layer" where the user's hand of the rubber glove is placed.

[0014] [Outer layer] The outer layer contains a rubber component (A) as a main component. Therefore, the outer layer is a rubber layer. In the rubber glove of the present invention, the outer layer may be the outermost layer. In this case, the outer layer becomes a surface rubber layer. In addition, another layer may be laminated on the outer layer (i.e., on the outer surface side of the rubber glove). In the rubber glove of the present invention, the outer layer is preferably the outermost layer.

[0015] In this specification, the phrase "the outer layer contains a rubber component (A) as a main component" means that the content of the rubber component (A) in the outer layer is 50% by mass or more. The content of the rubber component (A) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.

[0016] The rubber component (A) may be a rubber component used in known rubber gloves, and preferably a rubber component that can be converted into latex when not vulcanized. Examples of the rubber component include natural rubber (NR), deproteinized natural rubber, acrylonitrile-butadiene rubber (NBR), styrene-butadiene rubber (SBR), and chloroprene rubber (CR). The rubber component (A) may be composed of only one type of rubber component, or may be composed of two or more types of rubber components. The rubber component (A) contained in the outer layer is usually a vulcanized (crosslinked) rubber component.

[0017] The outer layer may contain components other than the rubber component (A). Examples of such components include various additives such as heat stabilizers, antiaging agents, fillers, anionic dispersion stabilizers, nonionic dispersion stabilizers, pH adjusters, surfactants, thickeners, defoamers, foaming agents, plasticizers, and colorants. The specific types and contents of these additives may be the same as those used in the rubber layer of known rubber gloves. In addition, the outer layer may contain residues of vulcanizing agents, vulcanization accelerators, vulcanization accelerator assistants (e.g., zinc oxide), crosslinking assistants, and the like.

[0018] [Inner layer] The inner layer contains the polymer component (B) as a main component and further contains polyethylene oxide. In the rubber glove of the present invention, the inner layer may be the innermost layer, or another layer may be laminated on the inner layer (i.e., on the inner surface side of the rubber glove). In the rubber glove of the present invention, the inner layer is preferably the innermost layer.

[0019] In this specification, the phrase "the inner layer contains the polymer component (B) as a main component" means that the content of the polymer component (B) in the inner layer is 50% by mass or more. The content of the polymer component (B) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.

[0020] As the polymer component (B), one that can be made into a latex is preferably used. In other words, one that can be dispersed as fine particles in water is preferably used. As the polymer component (B), a rubber component that can be used as the above-mentioned rubber component (A) (e.g., natural rubber (NR), deproteinized natural rubber, acrylonitrile-butadiene rubber (NBR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), etc.) can be used. In addition, as the polymer component (B), a resin (especially a thermoplastic resin) such as a (meth)acrylic resin, a vinyl chloride resin, or a urethane resin can be used. The polymer component (B) may be the same as or different from the rubber component (A).

[0021] The polymer component (B) is preferably a (meth)acrylic resin (i.e., a (meth)acrylic resin that can be made into a latex). In this case, when the inner layer is subjected to a flocking treatment, the adhesive strength between the pile and the inner layer is particularly high, so that the pile can be prevented from falling off and the flocking texture is particularly excellent. In this specification, "(meth)acrylic" is a term that includes "acrylic" and "methacrylic".

[0022] The (meth)acrylic resin may be a homopolymer containing only (meth)acrylic acid ester units as monomer units, or may be a copolymer containing other monomer units in addition to (meth)acrylic acid ester units, within a range that does not significantly impair the effects of the present invention. Suitable examples of other monomer units include styrene units, acrylonitrile units, (meth)acrylic acid units, maleic acid units, etc. The content of other monomer units is not particularly limited, but is preferably 50 mol% or less, more preferably 30 mol% or less, and more preferably 10 mol% or less of the total monomer units.

[0023] The inner layer contains polyethylene oxide (PEO). In the manufacture of rubber gloves by the coagulant immersion method, a hand mold is immersed in the immersion liquid with the fingertips facing down, and the hand mold is removed after a few to several tens of seconds. At this time, the immersion liquid that has not completely coagulated gathers on the fingertips of the hand mold. If this is left as it is, it will become a lump due to heating and drying, so the hand mold immediately after being removed from the immersion liquid is turned so that the fingertips are facing up. At this time, the immersion liquid that has not completely coagulated drips and collects locally on the fingers and between the fingers, causing a flow-back phenomenon. Furthermore, if the dripping liquid remains on the fingertips, the fingertip phenomenon occurs. In the present invention, the inner layer contains polyethylene oxide, so that the occurrence of this flow-back and fingertip can be suppressed. The reason for this is that polyethylene oxide has many ether oxygens with large dipole moments in its main chain, and the fluidity of the immersion liquid is reduced by the action of these many ether oxygens (especially the action of the ether oxygen coordinating with the cation of the coagulant to cause the immersion liquid containing latex to exhibit pseudo-salt coagulation properties).

[0024] The polyethylene oxide used is not particularly limited. The polyethylene oxide may be a homopolymer containing only ethylene oxide units (oxyethylene units) as monomer units, or may be a copolymer containing other monomer units within a range that does not significantly impair the effects of the present invention. The content of other monomer units in the total monomer units is preferably 30 mol% or less, more preferably 10 mol% or less.

[0025] The polyethylene oxide used may be one having a viscosity of 50 mPa·s or more and 7,000 mPa·s or less in a 5% by mass aqueous solution at 25°C, or one having a viscosity of 20 mPa·s or more and 1,000 mPa·s or less in a 0.5% by mass aqueous solution at 25°C.

[0026] From the viewpoint of further suppressing the occurrence of flowback and further improving the wearing comfort, it is preferable to use polyethylene oxide having a viscosity of 20 mPa·s or more and 500 mPa·s or less in a 0.5% by mass aqueous solution at 25°C. In other words, it is preferable that the viscosity of polyethylene oxide in a 0.5% by mass aqueous solution at 25°C is 20 mPa·s or more and 500 mPa·s or less. By using polyethylene oxide having a viscosity of 20 mPa·s or more, the fluidity of the immersion liquid for the inner layer can be more effectively suppressed. By having a viscosity of 500 mPa·s or less, the influence of the stringiness peculiar to polyethylene oxide can be effectively reduced.

[0027] The viscosity of the aqueous solution of polyethylene oxide at 25° C. can be measured using a B-type viscometer. As for the measurement conditions, the rotation speed is, for example, 12 rpm.

[0028] The viscosity average molecular weight (Mv) of the polyethylene oxide is not particularly limited, and is, for example, 150,000 or more and 10,000,000 or less. If the Mv of the polyethylene oxide is too small, the effect of suppressing the occurrence of flowback tends to be small. Therefore, the Mv of the polyethylene oxide is preferably 1,200,000 or more, more preferably 1,500,000 or more. On the other hand, if the Mv of the polyethylene oxide is too large, the effect of suppressing the occurrence of flowback and the effect of improving comfort tend to be small. Therefore, the Mv of the polyethylene oxide is preferably 5,800,000 or less, more preferably 5,000,000 or less.

[0029] The viscosity average molecular weight of polyethylene oxide can be calculated based on the intrinsic viscosity determined by measurement using an Ostwald viscometer, using the following formula: The viscosity measurement can be performed, for example, using pure water as a solvent at a measurement temperature of 35°C. [η] = K × M α ([η]=intrinsic viscosity, M=viscosity average molecular weight, K(constant)=6.4×10 -5 , α(constant)=0.82)

[0030] Polyethylene oxide can be obtained by synthesis according to known methods. It is also available as a commercial product. Examples of commercial polyethylene oxide products include PEO-1 (viscosity of 5% aqueous solution = 50 to 200 mPa·s; Mv = 150,000 to 400,000), PEO-3 (viscosity of 5% aqueous solution = 2,500 to 5,500 mPa·s; Mv = 600,000 to 1,100,000), and PEO-8 (viscosity of 0.5% aqueous solution = 20 to 70 mPa·s), all manufactured by Sumitomo Seika Chemicals Co., Ltd. s;Mv=1,700,000~2,200,000), PEO-15 (0.5% aqueous solution viscosity=130~250mPa·s;Mv=3,300,000~3,800,0 00), PEO-18 (0.5% aqueous solution viscosity = 250~430mPa·s; Mv=4,300,000~4,800,000), PEO-27 (0.5% aqueous solution viscosity = 60 0~800mPa·s; Mv=6,000,000~8,000,000), PEO-29 (0.5% aqueous solution viscosity=800~1,000mPa·s; Mv=8,000,000~10,000,000); Alcox E-45 (2% aqueous solution viscosity=150~600mPa·s; Mv=600,000~1,000,0 00), E-60 (2% aqueous solution viscosity = 1,000 to 4,000 mPa s; Mv = 1,000,000 to 1,500,000), E-100 (0.5% aqueous solution viscosity = 80 to 120 mPa s; Mv = approximately 3,000,000), and E-240 (0.5% aqueous solution viscosity = 180 to 280 mPa s; Mv = approximately 5,000,000).

[0031] The content of polyethylene oxide in the inner layer is not particularly limited. If the content of polyethylene oxide is small, the effect of suppressing the occurrence of flowback and fingertips and the effect of improving texture tend to be small. Therefore, the content of polyethylene oxide in the inner layer is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5% by mass or more, relative to 100 parts by mass of the polymer component (B). On the other hand, when the content of polyethylene oxide exceeds a certain amount, the effect is saturated. Therefore, from the viewpoint of cost, etc., the content of polyethylene oxide in the outer layer is preferably 3.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.0 parts by mass or less, relative to 100 parts by mass of the polymer component (B).

[0032] The inner layer may contain components other than the polymer component (B) and polyethylene oxide. Examples of such components include various additives such as heat stabilizers, antiaging agents, fillers, anionic dispersion stabilizers, nonionic dispersion stabilizers, pH adjusters, surfactants, thickeners, defoamers, foaming agents, plasticizers, and colorants. The specific types and contents of these additives may be the same as those used in the rubber layer of known rubber gloves. The inner layer may also contain residues of vulcanizing agents, vulcanization accelerators, vulcanization accelerator assistants (e.g., zinc oxide), crosslinking assistants, and the like.

[0033] [Hair transplantation] In a preferred embodiment of the rubber glove of the present invention, the inner layer is the innermost layer and has pile (short fibers) implanted therein. The pile is typically implanted by an electrostatic flocking method.

[0034] The pile to be implanted is not particularly limited, and piles similar to those used in known rubber gloves can be used. From the viewpoints of texture, cost, etc., piles made of cotton, nylon, or rayon are preferably used.

[0035] The length of the pile is not particularly limited, but is, for example, 0.3 mm to 0.7 mm, and the diameter of the pile is not particularly limited, but is, for example, 10 μm to 20 μm.

[0036] [Rubber gloves]

[0037] The dimensions of the rubber glove of the present invention (e.g., outer dimensions, thickness of the inner layer, thickness of the outer layer, etc.) are not particularly limited and may be the same as the dimensions of known rubber gloves.

[0038] The rubber glove of the present invention may contain layers other than the inner layer and the outer layer. For example, since the inner layer of the rubber glove of the present invention has excellent adhesiveness, the inner layer may be used as an adhesive intermediate layer, and another layer may be provided on the inner layer (i.e., on the inner surface side of the rubber glove) instead of flocking. This other layer may be a layer that improves comfort or a layer that imparts other functions. In the rubber glove of the present invention, another layer may be laminated on the outer layer (i.e., on the outer surface side of the rubber glove). One example of the rubber glove of the present invention is composed of only the inner layer and the outer layer, and pile may be flocked on the inner layer.

[0039] In the rubber glove of the present invention, the occurrence of flowback and finger tips is suppressed. In addition, when the rubber glove of the present invention is flocked, the flocked texture is excellent. Therefore, the rubber glove of the present invention is excellent in comfort. The rubber glove of the present invention can be used for a wide variety of purposes in various fields such as general households, industrial production, research, and medicine.

[0040] [Manufacturing method] The method for manufacturing the rubber glove of the present invention is not particularly limited. A suitable method for manufacturing the rubber glove of the present invention includes a process for treating the surface of a hand mold corresponding to the three-dimensional shape of the rubber glove with a coagulant (hereinafter also referred to as a "coagulant treatment process"), a process for immersing the treated hand mold in an immersion liquid for forming an outer layer containing latex (C) (hereinafter also referred to as a "first immersion process"), and a process for immersing the immersed hand mold in an immersion liquid for forming an inner layer containing latex (D) (hereinafter also referred to as a "second immersion process"). Here, the immersion liquid for forming the inner layer contains polyethylene oxide.

[0041] First, the coagulant treatment step will be described. The coagulant treatment step can be carried out in the same manner as known methods. Specifically, in the coagulant treatment step, a hand mold corresponding to the three-dimensional shape of the rubber glove is prepared. As the hand mold, a known hand mold used in the manufacture of rubber gloves, such as a ceramic hand mold, can be used.

[0042] As the coagulant, a known coagulant used in the production of rubber gloves can be used, and examples thereof include calcium nitrate, calcium chloride, etc. The coagulant is usually used as a coagulating liquid in the form of a solution (e.g., an aqueous solution, a methanol solution, etc.).

[0043] The treatment with the coagulant can be carried out, for example, by immersing the hand mold in a coagulant liquid (preferably an aqueous solution of the coagulant), removing it from the mold, and then drying it. In this way, a hand mold with the coagulant attached to its surface can be obtained.

[0044] Next, the first immersion step will be described. In the first immersion step, an immersion liquid for forming an outer layer is used.

[0045] The immersion liquid for forming the outer layer contains latex (C) (first latex). The latex (C) is not particularly limited, and latexes such as natural rubber (NR), deproteinized natural rubber, acrylonitrile-butadiene rubber (NBR), styrene-butadiene rubber (SBR), and chloroprene rubber (CR) can be used. Examples of natural rubber latexes include HA latex and LA latex. These latexes can be used alone or in combination of two or more. The rubber component contained in the latex (C) corresponds to the above-mentioned rubber component (A).

[0046] The immersion liquid for forming the outer layer usually contains a vulcanizing agent. Examples of the vulcanizing agent include sulfur and sulfur-containing organic compounds, and sulfur is preferred. The immersion liquid for forming the outer layer may contain a vulcanization accelerator, a vulcanization acceleration assistant (e.g., zinc oxide), a crosslinking assistant, and the like. The contents of the vulcanizing agent, the vulcanization accelerator, the vulcanization acceleration assistant (e.g., zinc oxide), and the crosslinking assistant may be the same as those in the immersion liquid used for forming the rubber layer of a known rubber glove. For example, the content of the vulcanizing agent is 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the rubber component contained in the latex (C).

[0047] The immersion liquid for forming the outer layer may contain various additives such as a heat stabilizer, an antiaging agent, a filler, an anionic dispersion stabilizer, a nonionic dispersion stabilizer, a pH adjuster, a surfactant, a thickener, an antifoaming agent, a foaming agent, a plasticizer, a colorant, etc. The content of these additives may be the same as the content in the immersion liquid used for forming the rubber layer of a known rubber glove.

[0048] The dipping liquid for forming the outer layer can be prepared by mixing the latex (C) and the above-mentioned components in accordance with a known method.

[0049] The first immersion step can be performed by immersing the hand mold treated with the coagulant in the immersion liquid for forming the outer layer. After immersion, the hand mold is removed from the immersion liquid for forming the outer layer. After immersion, it is preferable to dry the hand mold by heating or the like. It is preferable to form a non-crosslinked outer layer by this drying.

[0050] Next, the second immersion step will be described. In the second immersion step, an immersion liquid for forming an inner layer is used.

[0051] The immersion liquid for forming the inner layer contains latex (D) (second latex). As the latex (D), a rubber latex or a resin latex can be used.

[0052] The rubber latex used as latex (D) is the same as the latex used for latex (C). The rubber component of latex (D) and the rubber component of latex (C) may be the same or different.

[0053] As the resin latex, a (meth)acrylic latex, a vinyl chloride latex, a urethane latex, or the like can be used.

[0054] As the latex (D), a (meth)acrylic latex is preferred. When a (meth)acrylic latex is used to form the inner layer, the adhesion strength between the pile and the inner layer is particularly high when the inner layer is subjected to a flocking treatment, so that the pile can be prevented from falling off and the flocking texture is particularly excellent.

[0055] As the (meth)acrylic latex, commercially available products may be used. Examples of commercially available products include Nissensol TG-76 and TG-106 manufactured by Shin Nissen Co., Ltd., Ultrasol manufactured by Aica Kogyo Co., Ltd., and the like.

[0056] When the latex (D) is a rubber latex, the immersion liquid for forming the inner layer usually contains a vulcanizing agent, and may contain a vulcanization accelerator, a vulcanization accelerator assistant (e.g., zinc oxide), a crosslinking assistant, etc. When the latex (D) is a resin latex, the immersion liquid for forming the inner layer may contain a vulcanizing agent, a vulcanization accelerator, a vulcanization accelerator assistant (e.g., zinc oxide), and a crosslinking assistant. The contents of the vulcanizing agent, the vulcanization accelerator, and the crosslinking assistant may be the same as those in the immersion liquid used for forming the rubber layer of a known rubber glove. For example, the content of the vulcanizing agent is 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the rubber component or the resin component contained in the latex (D).

[0057] The immersion liquid for forming the inner layer contains polyethylene oxide. The specific content of the polyethylene oxide is as described above.

[0058] The content of polyethylene oxide in the immersion solution for forming the inner layer is not particularly limited. It is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5% by mass or more, based on 100 parts by mass of the rubber component or resin component contained in the latex (D). On the other hand, the content of polyethylene oxide is preferably 3.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.0 part by mass or less, based on 100 parts by mass of the rubber component or resin component contained in the latex (D). The rubber component or resin component contained in the latex (D) corresponds to the above-mentioned polymer component (B).

[0059] The immersion liquid for forming the inner layer may contain various additives such as a heat stabilizer, an antiaging agent, a filler, an anionic dispersion stabilizer, a nonionic dispersion stabilizer, a pH adjuster, a surfactant, a thickener, an antifoaming agent, a foaming agent, a plasticizer, a colorant, etc. The content of these additives may be the same as the content in the immersion liquid used for forming the rubber layer of a known rubber glove.

[0060] The dipping liquid for forming the inner layer can be prepared by mixing the latex (D), polyethylene oxide, and the above-mentioned components according to a known method.

[0061] The second immersion step can be performed by immersing the hand mold immersed in the immersion liquid for forming the outer layer into the immersion liquid for forming the inner layer. After immersion, the hand mold is removed from the immersion liquid for forming the inner layer.

[0062] In order to obtain a rubber glove having fibers implanted on the inner surface, a step of implanting pile fibers (hereinafter also referred to as a "fiber implantation step") is further carried out after the second dipping step. The fiber implantation step is typically carried out before the dipping solution for forming the inner layer is completely dried.

[0063] The pile used is as described above. The pile can be implanted by a known method (particularly, electrostatic implantation). In addition, when performing the second dipping step, the hand mold may be heated before dipping. In this case, the dipping liquid for forming the inner layer can form a partially dried coating film on the hand mold, which makes it easier to anchor the pile vertically in the implantation step.

[0064] Then, typically, a step of heating the hand mold is performed. This heating effectuates drying and vulcanization. The vulcanized product is inverted and demolded from the hand mold to obtain the rubber glove of the present invention. EXAMPLES

[0065] Examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "parts" refers to "parts by mass".

[0066] Example 1 [Preparation of immersion solution for forming outer layer] A mixture containing 100 parts of the rubber component of a commercially available HA latex, 0.5 parts of casein, 0.5 parts of potassium hydroxide, 0.5 parts of potassium oleate, 1 part of sulfur, 1 part of zinc oxide, 1 part of antioxidant, 1 part of vulcanization accelerator, and 0.03 parts of defoamer was prepared. This mixture was aged for 2 days to prepare immersion solution A for forming the outer layer.

[0067] [Preparation of immersion solution for forming inner layer] A mixture was prepared containing 100 parts of the rubber component of a commercially available HA latex, 0.5 parts of casein, 0.5 parts of potassium hydroxide, 0.5 parts of potassium oleate, 1 part of sulfur, 1 part of zinc oxide, 1 part of antioxidant, 1 part of vulcanization accelerator, 0.03 parts of defoamer, and 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd. The mixture was aged for 2 days to prepare immersion solution B1 for forming an inner layer.

[0068] [Making gloves] A ceramic hand mold corresponding to the three-dimensional shape of the glove was prepared. After heating this mold at 60°C for 20 minutes, it was immersed in a 25% calcium nitrate aqueous solution, and then removed and heated at 60°C for 1 minute to dry. This mold was immersed in the outer layer forming immersion liquid A for 10 seconds and then removed. This was placed in a dryer and dried at 100°C for 1 minute. Then, this was immersed in the inner layer forming immersion liquid B1 and then removed. Next, rayon pile was flocked using an electrostatic flocking device, and this was placed in a continuous dryer and heated at 100°C for 60 minutes. This was inverted and removed from the hand mold to obtain a rubber glove.

[0069] Comparative Example 1 A rubber glove was prepared in the same manner as in Example 1, except that 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd. was not mixed into the immersion solution B1 for forming the inner layer.

[0070] Comparative Example 2 A rubber glove was prepared in the same manner as in Example 1, except that 0.5 parts of polyacrylate was mixed into the inner layer forming immersion solution B1 instead of 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0071] Example 2 A mixed solution containing 0.5 parts of potassium hydroxide, 0.5 parts of potassium oleate, 1 part of sulfur, 2.5 parts of zinc oxide, 1 part of vulcanization accelerator, 0.03 parts of defoamer, and 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd. was prepared based on 100 parts of rubber component of commercially available NBR latex. The mixed solution was aged for 2 days to prepare an inner layer forming immersion solution B2. A rubber glove was produced in the same manner as in Example 1, except that the inner layer forming immersion solution B2 was used.

[0072] Comparative Example 3 A rubber glove was prepared in the same manner as in Example 2, except that 0.5 parts of polyacrylate was mixed into the inner layer forming immersion solution B2 instead of 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0073] Example 3 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed with 100 parts of the (meth)acrylic resin component of a commercially available acrylic latex to prepare an inner layer forming immersion solution B3. A rubber glove was produced in the same manner as in Example 1, except that this inner layer forming immersion solution B3 was used.

[0074] Example 4 A rubber glove was prepared in the same manner as in Example 3, except that the amount of PEO-1 (manufactured by Sumitomo Seika Chemicals Co., Ltd.) in the immersion solution B3 for forming an inner layer was changed from 0.5 parts to 1 part.

[0075] Example 5 A rubber glove was prepared in the same manner as in Example 3, except that 0.5 parts of PEO-3 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0076] Example 6 A rubber glove was prepared in the same manner as in Example 3, except that 0.1 part of PEO-8 manufactured by Sumitomo Seika Chemicals was mixed into the inner layer forming immersion solution B3 instead of 0.5 part of PEO-1 manufactured by Sumitomo Seika Chemicals.

[0077] Example 7 A rubber glove was prepared in the same manner as in Example 3, except that 0.5 parts of PEO-8 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0078] Example 8 A rubber glove was prepared in the same manner as in Example 3, except that 1 part of PEO-8 manufactured by Sumitomo Seika Chemicals was mixed into the inner layer forming immersion solution B3 instead of 0.5 part of PEO-1 manufactured by Sumitomo Seika Chemicals.

[0079] Example 9 A rubber glove was prepared in the same manner as in Example 3, except that 0.5 parts of PEO-18 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0080] Example 10 A rubber glove was prepared in the same manner as in Example 3, except that 0.5 parts of PEO-27 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0081] Example 11 A rubber glove was prepared in the same manner as in Example 3, except that 0.5 parts of PEO-29 manufactured by Sumitomo Seika Chemicals Co., Ltd. was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0082] Comparative Example 4 A rubber glove was prepared in the same manner as in Example 3, except that the immersion solution B3 for forming the inner layer did not contain 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0083] Comparative Example 5 A rubber glove was prepared in the same manner as in Example 3, except that 1.5 parts of polyacrylate was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0084] Comparative Example 6 A rubber glove was prepared in the same manner as in Example 3, except that 3 parts of polyacrylate was mixed into the inner layer forming immersion solution B3 instead of 0.5 parts of PEO-1 manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0085] [Evaluation of Viscosity of Immersion Liquid for Forming Inner Layer] An appropriate amount of the immersion liquid for forming the inner layer prepared in each Example and Comparative Example was taken and measured using a B-type viscometer at a rotor rotation speed of 60 rpm to read the value. This value was taken as the viscosity (mPa s) of the immersion liquid for forming the inner layer. The results are shown in Tables 1 to 3.

[0086] [Evaluation of flock texture] A sensory test was carried out on the inner surface of the rubber gloves produced in each Example and Comparative Example, and the gloves were evaluated according to the following criteria. The results are shown in Tables 1 to 3. A: Extremely good texture = No exposed rubber due to pile falling off B: Good texture = slight rubber exposure due to pile loss C: Poor texture = Rubber is exposed in many areas due to pile loss.

[0087] [Flowback evaluation] The inner surface of the rubber gloves produced in each Example and Comparative Example was inspected visually and by touch, and was evaluated according to the following criteria. The results are shown in Tables 1 to 3. A: There is no flow back at all and no protrusions are felt. B: Slight flow back is observed and a slight protrusion is felt C: Flow back is significant and the convex part is clearly felt

[0088] [Fingertip evaluation] The inner surface of the rubber gloves produced in each Example and Comparative Example was inspected visually and by touch, and was evaluated according to the following criteria. The results are shown in Tables 1 to 3. A: There are no fingertips and no protrusions are felt. B: Fingertips are slightly visible and protrusions are slightly felt C: Fingertips are prominent and convex parts are clearly felt

[0089] [Evaluation of wearing comfort] Ten subjects wore the rubber gloves and evaluated the comfort of wearing them according to the following criteria. The results are shown in Tables 1 to 3. A: Very comfortable to wear B: Comfortable to wear C: Not comfortable to wear

[0090] [Table 1]

[0091] [Table 2]

[0092] [Table 3]

[0093] In addition, in the above Tables 1 to 3, the amount (parts) of latex is the amount (parts) of the rubber component or resin component contained in the latex.

[0094] Comparisons between Example 1 and Comparative Examples 1 and 2, between Example 2 and Comparative Example 3, and between Examples 3 to 11 and Comparative Examples 4 to 6 show that blending polyethylene oxide into the inner layer improves the flocked texture, reduces flowback and fingertips, and improves comfort. Therefore, it is clear that the present invention can provide rubber gloves that suppress the occurrence of flowback and fingertips, and have an excellent flocked texture and comfort.

Claims

1. An outer layer containing a rubber component (A) as a main component; The rubber glove has an inner layer including a polymer component (B) containing a rubber component capable of being turned into a latex or a resin component capable of being turned into a latex as a main component, and polyethylene oxide.

2. 2. The rubber glove according to claim 1, wherein the polyethylene oxide has a viscosity of 20 mPa·s or more and 500 mPa·s or less at 25° C. when the polyethylene oxide is dissolved in an aqueous solution having a concentration of 0.5% by mass.

3. The rubber glove according to claim 1 or 2, wherein the content of the polyethylene oxide is 0.5 parts by mass or more and 1.0 parts by mass or less based on 100 parts by mass of the polymer component (B).

4. The rubber glove according to any one of claims 1 to 3, wherein the polymer component (B) is a (meth)acrylic resin which can be made into a latex.

5. The rubber glove according to any one of claims 1 to 4, wherein the inner layer is an innermost layer and has a pile flock.

6. A step of treating a surface of a hand mold corresponding to the three-dimensional shape of a rubber glove with a coagulant; immersing the treated hand mold in a dip liquid for forming an outer layer containing latex (C); immersing the immersed mold in an immersion liquid for forming an inner layer, the immersion liquid containing latex (D) containing a rubber component or a resin component and polyethylene oxide; The method for producing a rubber glove includes the steps of:

7. The method according to claim 6, wherein the polyethylene oxide has a viscosity of 20 mPa·s or more and 500 mPa·s or less at 25° C. when made into an aqueous solution with a concentration of 0.5% by mass.

8. A manufacturing method as described in claim 6 or 7, wherein the content of the polyethylene oxide in the immersion liquid for forming the inner layer is 0.5 parts by mass or more and 1.0 parts by mass or less per 100 parts by mass of the rubber component or resin component.

9. The method according to any one of claims 6 to 8, wherein the latex (D) is a (meth)acrylic latex.

10. The method according to any one of claims 6 to 9, further comprising a step of implanting pile fibers after the step of immersing in the immersion liquid for forming the inner layer.

Citation Information

Patent Citations

  • Antibacterial food-grade PVC glove

    CN209563514U

  • Method of molding from mixture of pre-vulcanized natural rubber latex and water-soluble polymer, and its molded article

    JP1999172042A

  • gloves

    JP2020012216A