Temporary fixing laminate and method for manufacturing semiconductor device
The use of incoherent light to irradiate a heat-generating temporary fixing material layer addresses thermal damage and inefficiencies in existing methods, enabling efficient and cost-effective separation of semiconductor members from support members in semiconductor device manufacturing.
Patent Information
- Application Number
- JP2022198692
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-12-01
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2038-11-29
AI Technical Summary
Existing methods for separating semiconductor members from support members in semiconductor device manufacturing cause thermal damage and are inefficient due to the use of coherent laser light, which requires complex processes and expensive equipment.
A method involving the use of incoherent light, such as a xenon lamp, to irradiate a temporary fixing material layer that absorbs light and generates heat, allowing easy separation of semiconductor members from support members without thermal damage, using a curable resin composition containing conductive particles that absorb light and generate heat.
The method enables efficient and damage-free separation of semiconductor members from support members, reducing process complexity and cost by utilizing incoherent light, which provides wider irradiation areas and faster processing times.
Smart Images

Figure 0007582288000009 
Figure 0007582288000010 
Figure 0007582288000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a semiconductor device, a curable resin composition for a temporary fixing material, a film for a temporary fixing material, and a laminate film for a temporary fixing material. [Background technology]
[0002] In the field of semiconductor devices, in recent years, there has been remarkable growth in technology relating to packages called SIPs (System in Packages) in which multiple semiconductor elements are stacked. In SIP-type packages, many semiconductor elements are stacked, so the semiconductor elements are required to be thin. In response to this requirement, after an integrated circuit is incorporated into a semiconductor member (e.g., a semiconductor wafer), the semiconductor element is subjected to processing such as thinning by grinding the back surface of the semiconductor member and individualization by dicing the semiconductor wafer. These processing processes of the semiconductor member are usually performed by temporarily fixing the semiconductor member to a support member with a temporary fixing material layer (see, for example, Patent Documents 1 to 3).
[0003] The processed semiconductor member is firmly fixed to the support member via the temporary fixing material layer. Therefore, in a manufacturing method of a semiconductor device, it is required to be able to separate the processed semiconductor member from the support member while preventing damage to the semiconductor member. Patent Document 1 discloses a method for physically separating such semiconductor members while heating the temporary fixing material layer. Patent Documents 2 and 3 disclose a method for separating the semiconductor members by irradiating the temporary fixing material layer with laser light (coherent light). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-126803 A [Patent Document 2] JP 2016-138182 A [Patent Document 3] JP 2013-033814 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the method disclosed in Patent Document 1 has a problem that damage due to thermal history occurs in the semiconductor wafer, resulting in a decrease in yield.On the other hand, the methods disclosed in Patent Documents 2 and 3 have problems that the laser light is a coherent light, so the irradiation area is narrow and it is necessary to repeatedly irradiate the entire semiconductor component many times, which takes time, the process is complicated because the focus of the laser light is controlled to perform scanning irradiation, and expensive equipment is required.
[0006] The present invention has been made in view of the above circumstances, and aims to provide a method for manufacturing a semiconductor device in which a temporarily fixed semiconductor member can be easily separated from a support member. Another aim of the present invention is to provide a curable resin composition for a temporary fixing material, a film for a temporary fixing material, and a laminate film for a temporary fixing material, which are useful as a temporary fixing material. [Means for solving the problem]
[0007] One aspect of the present invention provides a method for manufacturing a semiconductor device, comprising: a preparation step of preparing a laminate in which a support member, a temporary fixing material layer that absorbs light and generates heat, and a semiconductor member are laminated in this order; and a separation step of irradiating the temporary fixing material layer in the laminate with incoherent light to separate the semiconductor member from the support member.
[0008] The light source of the incoherent light in the separation step may be a xenon lamp. The incoherent light in the separation step may be light including at least infrared light.
[0009] The separation step may be a step of irradiating the temporary fixing material layer with incoherent light via a support member.
[0010] In one embodiment, the temporary fixing material layer may contain a cured product of a curable resin composition that contains conductive particles that absorb light and generate heat.
[0011] The content of the conductive particles may be 30 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles in the curable resin composition.
[0012] The curable resin composition may further include a thermoplastic resin. The curable resin composition may further include a polymerizable monomer and a polymerization initiator.
[0013] In another embodiment, the temporary fixing material layer may have a light absorbing layer that absorbs light and generates heat, and a resin cured product layer that contains a cured product of a curable resin component.
[0014] The light absorbing layer may be formed by sputtering or vacuum deposition.
[0015] In another aspect, the present invention provides a curable resin composition for a temporary fixing material for temporarily fixing a semiconductor member to a support member, the curable resin composition for a temporary fixing material including conductive particles that absorb light and generate heat.
[0016] The content of the conductive particles may be 30 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles in the curable resin composition for a temporary fixing material.
[0017] The curable resin composition for a temporary fixing material may further contain a thermoplastic resin. Also, the curable resin composition for a temporary fixing material may further contain a polymerizable monomer and a polymerization initiator.
[0018] The present invention may further relate to the application of the curable resin composition containing conductive particles that absorb light and generate heat as a temporary fixing material or for producing a temporary fixing material.
[0019] In another aspect, the present invention provides a film for a temporary fixing material for temporarily fixing a semiconductor member to a support member, the film for a temporary fixing material comprising the above-mentioned curable resin composition for a temporary fixing material.
[0020] In another aspect, the present invention provides a laminate film for a temporary fixing material for temporarily fixing a semiconductor member to a support member, the laminate film having a light absorbing layer that absorbs light and generates heat, and a resin layer that contains a curable resin component. Effect of the Invention
[0021] According to the present invention, a method for manufacturing a semiconductor device is provided that allows a temporarily fixed semiconductor member to be easily separated from a support member. Also, according to the present invention, a curable resin composition for a temporary fixing material, a film for a temporary fixing material, and a laminated film for a temporary fixing material that are useful as a temporary fixing material are provided. The curable resin composition for a temporary fixing material in some forms makes it possible to form a temporary fixing material layer that is excellent in heat resistance. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device of the present invention, and FIGS. 1(a) and 1(b) are schematic cross-sectional views showing each step. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one embodiment of the temporary fixing material precursor layer. [Diagram 3] 3(a), (b), (c), and (d) are schematic cross-sectional views showing an embodiment of a laminate formed using the temporary fixing material precursor layer shown in FIG. [Figure 4] FIG. 4 is a schematic cross-sectional view illustrating one embodiment of a method for manufacturing a semiconductor device of the present invention using the laminate shown in FIG. 3(d), and FIGS. 4(a) and (b) are schematic cross-sectional views showing each step. [Diagram 5] 5(a), (b), and (c) are schematic cross-sectional views showing other embodiments of the temporary fixing material precursor layer. [Figure 6]6(a), (b), (c), and (d) are schematic cross-sectional views showing an embodiment of a laminate formed using the temporary fixing material precursor layer shown in FIG. 5(a). [Figure 7] FIG. 7 is a schematic cross-sectional view illustrating one embodiment of a method for manufacturing a semiconductor device of the present invention using the laminate shown in FIG. 6(d), and FIGS. 7(a) and (b) are schematic cross-sectional views showing each step. [Figure 8] FIG. 8 is a schematic cross-sectional view for explaining another embodiment of the method for producing the laminate shown in FIG. 1(a), and FIGS. 8(a), (b), and (c) are schematic cross-sectional views showing each step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. However, the present invention is not limited to the following embodiment. In the following embodiment, the components (including steps, etc.) are not essential unless specifically stated. The size of the components in each figure is conceptual, and the relative relationship of the size between the components is not limited to that shown in each figure.
[0024] The same applies to the numerical values and their ranges in this specification, and the present invention is not limited thereto. In this specification, the numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit described in one numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples.
[0025] In this specification, (meth)acrylic acid means acrylic acid or its corresponding methacrylic acid, and the same applies to other similar expressions such as (meth)acrylate and (meth)acryloyl group.
[0026] [Method of manufacturing semiconductor device] The manufacturing method of the semiconductor device according to this embodiment includes a preparation step of preparing a laminate in which a support member, a temporary fixing material layer that absorbs light and generates heat (hereinafter, may be simply referred to as a "temporary fixing material layer"), and a semiconductor member are laminated in this order, and a separation step of irradiating the temporary fixing material layer in the laminate with incoherent light to separate the semiconductor member from the support member.
[0027] <Laminate preparation process> 1A and 1B are schematic cross-sectional views for explaining one embodiment of the method for manufacturing a semiconductor device of the present invention, and are schematic cross-sectional views showing each step. As shown in FIG. 1A, in the step of preparing a laminate, a laminate 100 is prepared in which a support member 10, a temporary fixing material layer 20c or 30c, and a semiconductor member 40 are laminated in this order.
[0028] The support member 10 is not particularly limited, and may be, for example, a glass substrate, a resin substrate, a silicon wafer, a metal thin film, etc. The support member 10 may be a substrate that does not prevent light transmission, and may be a glass substrate.
[0029] The thickness of the support member 10 may be, for example, 0.1 to 2.0 mm. If the thickness is 0.1 mm or more, handling tends to be easier, and if the thickness is 2.0 mm or less, material costs tend to be reduced.
[0030] The temporary fixing material layer 20c or 30c is a layer for temporarily fixing the support member 10 and the semiconductor member 40, and is a layer that absorbs light and generates heat when irradiated with light. The light to be absorbed in the temporary fixing material layer 20c or 30c may be light containing any of infrared light, visible light, and ultraviolet light. As described later, the temporary fixing material layer 20c or 30c may contain conductive particles (hereinafter, sometimes simply referred to as "conductive particles") that absorb light and generate heat, or may have a light absorbing layer (hereinafter, sometimes simply referred to as "light absorbing layer") that absorbs light and generates heat. Since the conductive particles and the light absorbing layer can efficiently generate heat, the light to be absorbed in the temporary fixing material layer 20c or 30c may be light that contains at least infrared light. In addition, the temporary fixing material layer 20c or 30c may be a layer that absorbs infrared light and generates heat when irradiated with light containing infrared light.
[0031] The laminate 100 shown in FIG. 1(a) can be produced, for example, by forming a temporary fixing material precursor layer containing a curable resin component on a support member, arranging a semiconductor member on the temporary fixing material precursor layer, curing the curable resin component in the temporary fixing material precursor layer, and forming a temporary fixing material layer containing a cured product of the curable resin component.
[0032] (Temporary Fixing Material Precursor Layer: First Embodiment) In one embodiment, the temporary fixing material precursor layer contains a curable resin composition containing conductive particles that absorb light and generate heat. FIG. 2 is a schematic cross-sectional view showing one embodiment of the temporary fixing material precursor layer. As shown in FIG. 2, the temporary fixing material precursor layer 20 may be composed of conductive particles 22 and a curable resin component 24. That is, the curable resin composition may contain conductive particles and a curable resin component. The curable resin component 24 may be a curable resin component that is cured by heat or light.
[0033] The conductive particles 22 are not particularly limited as long as they absorb light and generate heat, but may absorb infrared light and generate heat. The conductive particles 22 may be, for example, at least one selected from the group consisting of silver powder, copper powder, nickel powder, aluminum powder, chromium powder, iron powder, brass powder, tin powder, titanium alloy, gold powder, copper alloy powder, copper oxide powder, silver oxide powder, tin oxide powder, and conductive carbon powder. From the viewpoint of handling and safety, the conductive particles 22 may be at least one selected from the group consisting of silver powder, copper powder, silver oxide powder, copper oxide powder, and carbon powder. The conductive particles 22 may also be particles having a resin or metal core plated with a metal such as nickel, gold, or silver. Furthermore, from the viewpoint of dispersibility in a solvent, the conductive particles 22 may be particles whose surfaces are treated with a surface treatment agent.
[0034] The surface treatment agent may be, for example, a silane coupling agent. Examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyl Examples of the silane derivatives include propylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxypropyl)tetrasulfide, and 3-isocyanatopropyltriethoxysilane.
[0035] The shape of the conductive particles 22 is not particularly limited and may be granular, flat, etc. When the conductive particles 22 are carbon powder, they may be granular, tubular, wire-like, etc.
[0036] The average particle diameter of the conductive particles 22 may be, for example, 0.1 to 5.0 μm. Here, the average particle diameter is the particle diameter (D 50 ) The average particle size (D 50 ) can be obtained by measuring a suspension of the positive electrode active material in water by a laser scattering method using a laser scattering type particle size measuring device (for example, Microtrac).
[0037] The content of the conductive particles 22 may be 30 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The components other than the conductive particles of the curable resin composition do not include the solvent described below. The content of the conductive particles 22 may be 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more. When the content of the conductive particles 22 is 30 parts by mass or more relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition, the conductive particles tend to be separated from the support member by irradiation with incoherent light of lower energy. The content of the conductive particles 22 may be 80 parts by mass or less, 70 parts by mass or less, or 60 parts by mass or less. When the content of the conductive particles 22 is 90 parts by mass or less relative to 100 parts by mass of the total amount of the components other than the conductive particles of the temporary fixing material layer, the flatness of the temporary fixing material layer tends to be easily ensured.
[0038] The curable resin composition may contain a thermoplastic resin, a polymerizable monomer, and a polymerization initiator.
[0039] The thermoplastic resin may be a resin having thermoplasticity, or a resin having thermoplasticity at least in an uncured state and forming a crosslinked structure after heating. Examples of the thermoplastic resin include elastomer, polycarbonate, polyphenylene sulfide, polyethersulfone, polyetherimide, polyimide, petroleum resin, novolac resin, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of bump embedding property and low-temperature application property, the thermoplastic resin may be an elastomer.
[0040] Specific examples of elastomers include ethylene-propylene copolymer elastomers, ethylene-1-butene copolymer elastomers, ethylene-propylene-1-butene copolymer elastomers, ethylene-1-hexene copolymer elastomers, ethylene-1-octene copolymer elastomers, ethylene-styrene copolymer elastomers, ethylene-norbornene copolymer elastomers, propylene-1-butene copolymer elastomers, ethylene-propylene-non-conjugated diene copolymer elastomers, ethylene-1-butene-non-conjugated diene copolymer elastomers, ethylene-propylene-1-butene-non-conjugated diene copolymer elastomers, polyisoprene, polybutadiene, and carbene. Examples of the elastomer include carboxyl-terminated polybutadiene, hydroxyl-terminated polybutadiene, 1,2-polybutadiene, carboxyl-terminated 1,2-polybutadiene, hydroxyl-terminated 1,2-polybutadiene, acrylic rubber, styrene-butadiene rubber, hydroxyl-terminated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene rubber containing a carboxyl group, a hydroxyl group, a (meth)acryloyl group, or a morpholine group at the polymer end, carboxylated nitrile rubber, hydroxyl-terminated poly(oxypropylene), alkoxysilyl-terminated poly(oxypropylene), poly(oxytetramethylene) glycol, polyolefin glycol, and poly-ε-caprolactone. These elastomers may be hydrogenated. Among these, the elastomer may be an elastomer containing a monomer unit derived from styrene.
[0041] The Tg of the thermoplastic resin may be −100 to 500° C., −50 to 300° C., or −50 to 50° C. If the Tg of the thermoplastic resin is 500° C. or less, when a film-like temporary fixing material is formed, flexibility is easily ensured and low-temperature application tends to be improved. If the Tg of the thermoplastic resin is −100° C. or more, when a film-like temporary fixing material is formed, deterioration in handleability and peelability due to excessive flexibility tends to be suppressed.
[0042] The Tg of a thermoplastic resin is a midpoint glass transition temperature obtained by differential scanning calorimetry (DSC). Specifically, the Tg of a thermoplastic resin is a midpoint glass transition temperature calculated by a method in accordance with JIS K 7121, by measuring the change in heat quantity under conditions of a heating rate of 10°C / min and a measurement temperature of -80 to 80°C.
[0043] The weight-average molecular weight (Mw) of the thermoplastic resin may be 10,000 to 5,000,000 or 100,000 to 2,000,000. When the weight-average molecular weight is 10,000 or more, the heat resistance of the temporary fixing material layer formed tends to be easily ensured. When the weight-average molecular weight is 5,000,000 or less, when a film-like temporary fixing material layer is formed, the decrease in flow and the decrease in adhesion tend to be easily suppressed. The weight-average molecular weight is a polystyrene-equivalent value obtained by using a calibration curve of standard polystyrene in gel permeation chromatography (GPC).
[0044] The content of the thermoplastic resin may be 10 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The content of the thermoplastic resin may be 30 parts by mass or more, 50 parts by mass or more, or 70 parts by mass or more, and may be 88 parts by mass or less, 85 parts by mass or less, or 82 parts by mass or less. When the content of the thermoplastic resin is within the above range, the thin film formability and flatness of the temporary fixing material layer tend to be more excellent.
[0045] The polymerizable monomer is not particularly limited as long as it is polymerized by heating or irradiation with ultraviolet light or the like. From the viewpoint of material selectivity and availability, the polymerizable monomer may be, for example, a compound having a polymerizable functional group such as an ethylenically unsaturated group. Examples of the polymerizable monomer include (meth)acrylate, vinylidene halide, vinyl ether, vinyl ester, vinyl pyridine, vinyl amide, and arylated vinyl. Among these, the polymerizable monomer may be a (meth)acrylate. The (meth)acrylate may be monofunctional (monofunctional), bifunctional, or trifunctional or higher, but from the viewpoint of obtaining sufficient curability, it may be a bifunctional or higher (meth)acrylate.
[0046] Examples of monofunctional (meth)acrylates include (meth)acrylic acid; methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, butoxyethyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octylheptyl (meth)acrylate, nonyl (meth)acrylate, and decyl (Meth)acrylate 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, mono(2-(meth)acryloyloxyethyl) Aliphatic (meth)acrylates such as succinate; benzyl (meth)acrylate, phenyl (meth)acrylate, o-biphenyl (meth)acrylate, 1-naphthyl (meth)acrylate, 2-naphthyl (meth)acrylate, phenoxyethyl (meth)acrylate, p-cumylphenoxyethyl (meth)acrylate, o-phenylphenoxyethyl (meth)acrylate, 1-naphthoxyethyl (meth)acrylate, 2-naphthoxyethyl (meth)acrylate, phenoxypolyethylene glycol Examples of the aromatic (meth)acrylates include aromatic (meth)acrylates such as 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-3-(o-phenylphenoxy)propyl (meth)acrylate, 2-hydroxy-3-(1-naphthoxy)propyl (meth)acrylate, and 2-hydroxy-3-(2-naphthoxy)propyl (meth)acrylate.
[0047] Examples of bifunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3- Aliphatic (meth)acrylates such as propanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, glycerin di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, and ethoxylated 2-methyl-1,3-propanediol di(meth)acrylate; ethoxylated bisphenol A di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, eth ... and aromatic (meth)acrylates such as ethoxylated propoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, propoxylated bisphenol F di(meth)acrylate, ethoxylated propoxylated bisphenol F di(meth)acrylate, ethoxylated fluorene type di(meth)acrylate, propoxylated fluorene type di(meth)acrylate, and ethoxylated propoxylated fluorene type di(meth)acrylate.
[0048] Examples of the trifunctional or higher polyfunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, and ethoxylated propoxylated pentaerythritol tri(meth)acrylate. aliphatic (meth)acrylates such as pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated propoxylated pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetraacrylate, and dipentaerythritol hexa(meth)acrylate; and aromatic epoxy (meth)acrylates such as phenol novolac type epoxy (meth)acrylate and cresol novolac type epoxy (meth)acrylate.
[0049] These (meth)acrylates may be used alone or in combination of two or more thereof. Furthermore, these (meth)acrylates may be used in combination with other polymerizable monomers.
[0050] The content of the polymerizable monomer may be 10 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The content of the polymerizable monomer may be 12 parts by mass or more, 15 parts by mass or more, or 18 parts by mass or more. When the content of the polymerizable monomer is 10 parts by mass or more relative to 100 parts by mass of the total amount of the components other than the conductive particles of the temporary fixing material layer, the temporary fixing material layer tends to have excellent heat resistance. The content of the polymerizable monomer may be 70 parts by mass or less, 50 parts by mass or less, or 30 parts by mass or less. When the content of the polymerizable monomer is 90 parts by mass or less relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition, peeling, breakage, etc. during the process tend to be suppressed.
[0051] The polymerization initiator is not particularly limited as long as it initiates polymerization by heating or irradiation with ultraviolet light, etc. For example, when a compound having an ethylenically unsaturated group is used as the polymerizable monomer, the polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator.
[0052] Examples of the thermal radical polymerization initiator include diacyl peroxides such as octanoyl peroxide, lauroyl peroxide, stearyl peroxide, and benzoyl peroxide; t-butyl peroxypivalate, t-hexyl peroxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-hexylperoxyisopropyl monocarbonate, and t-butylperoxyisopropyl peroxide. peroxyesters such as t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-butylperoxybenzoate, t-hexylperoxybenzoate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, and t-butylperoxyacetate; and azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2'-dimethylvaleronitrile).
[0053] Examples of the photoradical polymerization initiator include benzoin ketals such as 2,2-dimethoxy-1,2-diphenylethan-1-one; α-hydroxyketones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one; and phosphine oxides such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0054] These thermal and photoradical polymerization initiators may be used alone or in combination of two or more.
[0055] The content of the polymerization initiator may be 0.01 to 5 parts by mass relative to 100 parts by mass of the total amount of the polymerizable monomers. The content of the polymerization initiator may be 0.03 parts by mass or more, or 0.05 parts by mass or more. When the content of the polymerization initiator is 0.01 parts by mass or more relative to 100 parts by mass of the total amount of the polymerizable monomers, the curability tends to be improved and the heat resistance tends to be better. The content of the polymerization initiator may be 3 parts by mass or less, 1 part by mass or less, or 0.1 parts by mass or less. When the content of the polymerization initiator is 5 parts by mass or less relative to 100 parts by mass of the total amount of the polymerizable monomers, the generation of gas during the process tends to be suppressed.
[0056] The curable resin composition may further contain a thermosetting resin, a curing accelerator, an insulating filler, a sensitizer, an antioxidant, and the like, as necessary.
[0057] The thermosetting resin is not particularly limited as long as it is a resin that is cured by heat. Examples of the thermosetting resin include epoxy resin, acrylic resin, silicone resin, phenol resin, thermosetting polyimide resin, polyurethane resin, melamine resin, urea resin, etc. These may be used alone or in combination of two or more. Among these, the thermosetting resin may be an epoxy resin because it is more excellent in heat resistance, workability, and reliability. When an epoxy resin is used as the thermosetting resin, it may be used in combination with an epoxy resin curing agent.
[0058] The epoxy resin is not particularly limited as long as it has heat resistance when cured. Examples of the epoxy resin include bifunctional epoxy resins such as bisphenol A type epoxy, phenol novolac type epoxy resins, cresol novolac type epoxy resins, and other novolac type epoxy resins. The epoxy resin may also be a multifunctional epoxy resin, a glycidylamine type epoxy resin, a heterocyclic epoxy resin, or an alicyclic epoxy resin.
[0059] The epoxy resin curing agent may be a commonly used known curing agent, such as amine, polyamide, acid anhydride, polysulfide, boron trifluoride, bisphenol having two or more phenolic hydroxyl groups in one molecule, such as bisphenol A, bisphenol F, and bisphenol S, and phenol resins, such as phenol novolac resin, bisphenol A novolac resin, and cresol novolac resin.
[0060] The content of the thermosetting resin and the curing agent may be 10 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. When the content of the thermosetting resin and the curing agent is within the above range, the heat resistance tends to be better.
[0061] Examples of the curing accelerator include imidazole derivatives, dicyandiamide derivatives, dicarboxylic acid dihydrazide, triphenylphosphine, tetraphenylphosphonium tetraphenylborate, 2-ethyl-4-methylimidazole-tetraphenylborate, 1,8-diazabicyclo[5,4,0]undecene-7-tetraphenylborate, etc. These may be used alone or in combination of two or more.
[0062] The content of the curing accelerator may be 0.01 to 5 parts by mass relative to 100 parts by mass of the total amount of the thermosetting resin and the curing agent. When the content of the curing accelerator is within the above range, the curability is improved and the heat resistance tends to be better.
[0063] The insulating filler is added for the purpose of imparting low thermal expansion and low moisture absorption to the resin composition. Examples of the insulating filler include nonmetallic inorganic fillers such as silica, alumina, boron nitride, titania, glass, and ceramic. These insulating fillers may be used alone or in combination of two or more. The insulating filler may be a particle whose surface is treated with a surface treatment agent from the viewpoint of dispersibility in a solvent. The surface treatment agent may be the same as the above-mentioned silane coupling agent.
[0064] The content of the insulating filler may be 5 to 20 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. When the content of the insulating filler is within the above range, the heat resistance tends to be further improved without impeding the light transmission. In addition, it may also contribute to easy peeling property.
[0065] Examples of the sensitizer include anthracene, phenanthrene, chrysene, benzopyrene, fluoranthene, rubrene, pyrene, xanthone, indanthrene, thioxanthene-9-one, 2-isopropyl-9H-thioxanthene-9-one, 4-isopropyl-9H-thioxanthene-9-one, and 1-chloro-4-propoxythioxanthone.
[0066] The content of the sensitizer may be 0.01 to 10 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles in the curable resin composition. When the content of the sensitizer is within the above range, the effect on the characteristics and thin film properties of the curable resin component tends to be small.
[0067] Examples of the antioxidant include quinone derivatives such as benzoquinone and hydroquinone, phenol derivatives such as 4-methoxyphenol and 4-t-butylcatechol, aminoxyl derivatives such as 2,2,6,6-tetramethylpiperidine-1-oxyl and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl, and hindered amine derivatives such as tetramethylpiperidyl methacrylate.
[0068] The content of the antioxidant may be 0.1 to 10 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. When the content of the antioxidant is within the above range, decomposition of the curable resin components is inhibited, and contamination tends to be prevented.
[0069] The temporary fixing material precursor layer 20 can be formed from a curable resin composition containing conductive particles 22 and a curable resin component 24 (thermoplastic resin, polymerizable monomer, polymerization initiator, etc.).
[0070] The curable resin composition may be used as a varnish of the curable resin composition diluted with a solvent. The solvent is not particularly limited as long as it can dissolve components other than the conductive particles 22 and the insulating filler. Examples of the solvent include aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-cymene; aliphatic hydrocarbons such as hexane and heptane; cyclic alkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; and amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These solvents may be used alone or in combination of two or more. Of these, the solvent may be toluene, xylene, heptane, or cyclohexane from the viewpoints of solubility and boiling point.
[0071] The solid content concentration in the varnish may be 10 to 80 mass % based on the total mass of the varnish.
[0072] The curable resin composition can be prepared by mixing and kneading the conductive particles 22 and the curable resin component 24 (thermoplastic resin, polymerizable monomer, polymerization initiator, etc.). The mixing and kneading can be performed by appropriately combining a dispersing machine such as a normal stirrer, a grinding machine, a triple roll, or a bead mill.
[0073] The curable resin composition may be formed into a film. The curable resin composition formed into a film (hereinafter, sometimes referred to as a "film for temporary fixing material") can be formed by applying the curable resin composition to a support film. When using a varnish of the curable resin composition diluted with a solvent, the curable resin composition can be formed by applying the curable resin composition to a support film and removing the solvent by heating and drying.
[0074] The thickness of the film for temporary fixing material can be adjusted according to the desired thickness of the temporary fixing material layer. From the viewpoint of stress relaxation, the thickness of the film for temporary fixing material may be 0.1 to 2000 μm (2 mm) or 10 to 500 μm.
[0075] The support film is not particularly limited, and examples thereof include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate; polyolefins such as polyethylene and polypropylene; polycarbonate, polyamide, polyimide, polyamideimide, polyetherimide, polyethersulfide, polyethersulfone, polyetherketone, polyphenylene ether, polyphenylene sulfide, poly(meth)acrylate, polysulfone, and liquid crystal polymer films. These may be subjected to a release treatment. The thickness of the support film may be, for example, 3 to 250 μm.
[0076] Examples of methods for applying the curable resin composition to a support film include spin coating, spraying, printing, film transfer, slit coating, scan coating, and inkjet methods.
[0077] The temporary fixing material film provided on the support film may be provided with a protective film as necessary. Examples of the protective film include polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; and polyolefins such as polyethylene and polypropylene. The thickness of the protective film may be, for example, 10 to 250 μm.
[0078] The film for temporary fixing material can be easily stored, for example, by winding it up in a roll. Also, the film for temporary fixing material in a roll shape can be cut into a suitable size and stored in a sheet shape.
[0079] The temporary fixing material precursor layer 20 can be formed by directly applying the curable resin composition to the supporting member 10. When using a varnish of the curable resin composition diluted with a solvent, the temporary fixing material precursor layer 20 can be formed by applying the curable resin composition to the supporting member 10 and removing the solvent by heating and drying.
[0080] The method of applying the curable resin composition directly to the support member 10 may be similar to the method of applying the curable resin composition to a support film.
[0081] The temporary fixing material precursor layer 20 can also be formed by laminating a previously prepared film for the temporary fixing material onto the support member 10. The lamination can be performed under predetermined conditions (for example, at room temperature (20° C.) or in a heated state) using a roll laminator, a vacuum laminator, or the like.
[0082] The thickness of the temporary fixing material precursor layer 20 may be 0.1 to 2000 μm (0.0001 to 2 mm) or 10 to 500 μm from the viewpoint of stress relaxation.
[0083] (Temporary Fixing Material Precursor Layer: Second Embodiment) As another embodiment, the temporary fixing material precursor layer has a light absorbing layer that absorbs light and generates heat, and a resin layer containing a curable resin component. Figures 5(a), (b), and (c) are schematic cross-sectional views showing other embodiments of the temporary fixing material precursor layer. The temporary fixing material precursor layer 30 is not particularly limited in its configuration as long as it has a light absorbing layer 32 and a resin layer 34. For example, the temporary fixing material precursor layer 30 may have a configuration having a light absorbing layer 32 and a resin layer 34 in this order from the support member 10 side (Figure 5(a)), a configuration having a resin layer 34 and a light absorbing layer 32 in this order from the support member 10 side (Figure 5(b)), and a configuration having a light absorbing layer 32, a resin layer 34, and a light absorbing layer 32 in this order (Figure 5(c)). Of these, the temporary fixing material precursor layer 30 may have a configuration having a light absorbing layer 32 and a resin layer 34 in this order from the support member 10 side (Figure 5(a)). In the following, an embodiment in which the temporary fixing material precursor layer 30 having the configuration shown in FIG. 5(a) is used will be described in detail.
[0084] One embodiment of the light absorbing layer 32 is a layer (hereinafter, sometimes referred to as a "conductor layer") made of a conductor (hereinafter, sometimes simply referred to as a "conductor") that absorbs light and generates heat. The conductor constituting such a conductor layer is not particularly limited as long as it is a conductor that absorbs light and generates heat, but may be a conductor that absorbs infrared light and generates heat. Examples of the conductor include metals such as chromium, copper, titanium, silver, platinum, and gold, alloys such as nickel-chromium, stainless steel, and copper-zinc, metal oxides such as indium tin oxide (ITO), zinc oxide, and niobium oxide, and carbon materials such as conductive carbon. These may be used alone or in combination of two or more. Of these, the conductor may be chromium, titanium, copper, aluminum, silver, gold, platinum, or carbon.
[0085] The light absorbing layer 32 may be composed of a plurality of conductive layers. Examples of such light absorbing layers include a light absorbing layer composed of a first conductive layer provided on the support member 10 and a second conductive layer provided on the surface of the first conductive layer opposite the support member 10. The conductor in the first conductive layer may be titanium from the viewpoints of adhesion to the support member (e.g., glass), film formability, thermal conductivity, low heat capacity, etc. The conductor in the second conductive layer may be copper, aluminum, silver, gold, or platinum from the viewpoints of high expansion coefficient, high thermal conductivity, etc., and among these, copper or aluminum is preferable.
[0086] The light absorbing layer 32 can be formed directly on the support member 10 by physical vapor deposition (PVD) such as vacuum deposition or sputtering, or chemical vapor deposition (CVD) such as electrolytic plating, electroless plating, or plasma-enhanced chemical vapor deposition. Of these, the conductive layer can be formed over a large area, so it may be formed by physical vapor deposition, or it may be formed by sputtering or vacuum deposition.
[0087] From the viewpoint of easy peelability, the thickness of one embodiment of the light absorbing layer 32 may be 1 to 5000 nm (0.001 to 5 μm) or 50 to 3000 nm (0.05 to 3 μm). When the light absorbing layer 32 is composed of a first conductive layer and a second conductive layer, the thickness of the first conductive layer may be 1 to 1000 nm, 5 to 500 nm, or 10 to 100 nm, and the thickness of the second conductive layer may be 1 to 5000 nm, 10 to 500 nm, or 50 to 200 nm.
[0088] Another aspect of the light absorbing layer 32 is a layer containing a cured product of a curable resin composition containing conductive particles that absorb light and generate heat. The curable resin composition may contain conductive particles and a curable resin component. The curable resin component may be a curable resin component that is cured by heat or light. The conductive particles may be the same as those exemplified as the conductive particles 22 described above. The curable resin component is not particularly limited, and examples thereof include those exemplified as the curable resin component in the first embodiment of the temporary fixing material precursor layer described above.
[0089] The content of the conductive particles may be 10 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The components other than the conductive particles of the curable resin composition do not include the organic solvent described below. The content of the conductive particles may be 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more. The content of the conductive particles may be 80 parts by mass or less, or 50 parts by mass or less.
[0090] The curable resin composition may contain a thermosetting resin, a curing agent, and a curing accelerator. The content of the thermosetting resin may be 10 to 90 parts by mass with respect to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The content of the curing agent and the curing accelerator may be 0.01 to 5 parts by mass with respect to 100 parts by mass of the total amount of the thermosetting resin.
[0091] The light absorbing layer 32 can be formed from a curable resin composition containing conductive particles that absorb light and generate heat. The curable resin composition may be used as a varnish of the curable resin composition diluted with an organic solvent. Examples of the organic solvent include acetone, ethyl acetate, butyl acetate, and methyl ethyl ketone (MEK). These organic solvents may be used alone or in combination of two or more. The solid component concentration in the varnish may be 10 to 80% by mass based on the total mass of the varnish.
[0092] The light absorbing layer 32 can be formed by directly applying the curable resin composition to the support member 10. When using a varnish of a curable resin composition diluted with an organic solvent, the light absorbing layer 32 can be formed by applying the curable resin composition to the support member 10 and removing the solvent by heating and drying.
[0093] The thickness of the light absorbing layer 32 in other embodiments may be 1 to 5000 nm (0.001 to 5 μm) or 50 to 3000 nm (0.05 to 3 μm) from the viewpoint of easy peelability.
[0094] Subsequently, a resin layer 34 is formed on the light absorbing layer 32 .
[0095] The resin layer 34 is a layer that does not contain conductive particles and contains a curable resin component that is cured by heat or light. The resin layer 34 may be a layer made of a curable resin component. The curable resin component is not particularly limited, and examples thereof include those exemplified as the curable resin component in the first embodiment of the temporary fixing material precursor layer described above. The resin layer 34 can be formed from a curable resin component (a curable resin composition that does not contain conductive particles). The curable resin component may be diluted with a solvent and used as a varnish of the curable resin component. The solid component concentration in the varnish may be 10 to 80 mass % based on the total mass of the varnish.
[0096] The resin layer 34 can be formed by directly applying the curable resin component to the light absorbing layer 32. When using a varnish of the curable resin component diluted with a solvent, the resin layer 34 can be formed by applying the curable resin component to the light absorbing layer 32 and removing the solvent by heating and drying. The resin layer 34 can also be formed by preparing a curable resin component film made of the curable resin component.
[0097] From the viewpoint of stress relaxation, the thickness of the resin layer 34 may be 0.1 to 2000 μm (0.0001 to 2 mm) or 10 to 150 μm.
[0098] The temporary fixing material precursor layer 30 can also be produced by preparing in advance a laminated film having a light absorbing layer 32 and a resin layer 34 (hereinafter, sometimes referred to as a "laminated film for temporary fixing material") and laminating it so that the light absorbing layer 32 and the support member 10 are in contact with each other.
[0099] The configuration of the light absorbing layer 32 and the resin layer 34 in the laminate film for temporary fixing material is not particularly limited as long as it has the light absorbing layer 32 and the resin layer 34, but examples thereof include a configuration having the light absorbing layer 32 and the resin layer 34, and a configuration having the light absorbing layer 32, the resin layer 34, and the light absorbing layer 32 in this order. Among these, the laminate film for temporary fixing material may have a configuration having the light absorbing layer 32 and the resin layer 34. The light absorbing layer 32 may be a layer made of a conductor (conductor layer) or a layer containing conductive particles. The laminate film for temporary fixing material may be provided on a support film, and a protective film may be provided on the surface opposite to the support film, as necessary.
[0100] The thickness of the light absorbing layer 32 in the laminated film for temporary fixing material may be 1 to 5000 nm (0.001 to 5 μm) or 50 to 3000 nm (0.05 to 3 μm) from the viewpoint of easy peelability.
[0101] The thickness of the resin layer 34 in the temporary fixing material laminated film may be 0.1 to 2000 μm (0.0001 to 2 mm) or 10 to 150 μm from the viewpoint of stress relaxation.
[0102] The thickness of the laminated film for temporary fixing material can be adjusted according to the desired thickness of the temporary fixing material layer. From the viewpoint of stress relaxation, the thickness of the laminated film for temporary fixing material may be 0.1 to 2000 μm (0.0001 to 2 mm) or 10 to 150 μm.
[0103] The temporary fixing material precursor layer 30 having the configuration shown in Fig. 5(b) can be produced, for example, by forming a resin layer 34 on a support member 10, and then forming a light absorbing layer 32. The temporary fixing material precursor layer 30 having the configuration shown in Fig. 5(c) can be produced, for example, by alternately forming a light absorbing layer 32, a resin layer 34, and a light absorbing layer 32 on a support member 10. These temporary fixing material precursor layers 30 may be produced by previously producing a laminated film for temporary fixing material having the above configuration and laminating it on the support member 10.
[0104] Next, a semiconductor member is placed on the prepared temporary fixing material precursor layer, and the curable resin component in the temporary fixing material precursor layer is cured to form a temporary fixing material layer containing a cured product of a curable resin composition containing conductive particles, or a temporary fixing material layer having a light absorbing layer and a resin cured product layer containing a cured product of a curable resin component, thereby preparing a laminate in which the support member 10, the temporary fixing material layer 20c or 30c, and the semiconductor member 40 are laminated in this order (FIG. 1(a)). FIGS. 3(a), (b), (c), and (d) are schematic cross-sectional views showing one embodiment of a laminate formed using the temporary fixing material precursor layer shown in FIG. 2. FIGS. 6(a), (b), (c), and (d) are schematic cross-sectional views showing one embodiment of a laminate formed using the temporary fixing material precursor layer shown in FIG. 5(a).
[0105] The semiconductor member 40 may be a semiconductor wafer or a semiconductor chip obtained by cutting a semiconductor wafer into a predetermined size and dividing it into individual chips. When a semiconductor chip is used as the semiconductor member 40, a plurality of semiconductor chips are usually used. The thickness of the semiconductor member 40 may be 1 to 1000 μm, 10 to 500 μm, or 20 to 200 μm from the viewpoint of miniaturizing and thinning the semiconductor device as well as suppressing cracks during transportation and processing steps. The semiconductor wafer or semiconductor chip may be provided with a rewiring layer, a pattern layer, or an external connection member having an external connection terminal.
[0106] The support member 10 provided with the prepared temporary fixing material precursor layer 20 or 30 is placed on a vacuum press or vacuum laminator, and the semiconductor member 40 can be arranged by being pressed with a press.
[0107] When using a vacuum press, the semiconductor member 40 is pressure-bonded to the temporary fixing material precursor layer 20 or 30 at an atmospheric pressure of 1 hPa or less, a pressure of 1 MPa, a pressure of 120 to 200° C., and a holding time of 100 to 300 seconds, for example.
[0108] When a vacuum laminator is used, the semiconductor member 40 is pressure-bonded to the temporary fixing material precursor layer 20 or 30, for example, at an atmospheric pressure of 1 hPa or less, a pressure-bonding temperature of 60 to 180°C or 80 to 150°C, a lamination pressure of 0.01 to 0.5 MPa or 0.1 to 0.5 MPa, and a holding time of 1 to 600 seconds or 30 to 300 seconds.
[0109] After the semiconductor member 40 is disposed on the support member 10 via the temporary fixing material precursor layer 20 or 30, the curable resin component in the temporary fixing material precursor layer 20 or 30 is thermally cured or photocured under predetermined conditions. The thermal curing conditions may be, for example, 300° C. or less or 100 to 200° C. and 1 to 180 minutes or 1 to 60 minutes. In this manner, a cured product of the curable resin component is formed, and the semiconductor member 40 is temporarily fixed to the support member 10 via the temporary fixing material layer 20c or 30c containing the cured product of the curable resin component, thereby obtaining the laminate 200 or 300. As shown in FIG. 3(a), the temporary fixing material layer 20c may be composed of the conductive particles 22 and the cured product 24c of the curable resin component. As shown in FIG. 6(a), the temporary fixing material layer 30c may be composed of the light absorbing layer 32 and the resin cured product layer 34c containing the cured product of the curable resin component.
[0110] The laminate can also be produced, for example, by forming a temporary fixing material layer and then arranging a semiconductor member. FIG. 8 is a schematic cross-sectional view for explaining another embodiment of the manufacturing method of the laminate shown in FIG. 1(a), and FIGS. 8(a), 8(b), and 8(c) are schematic cross-sectional views showing each step. Each step of FIG. 8 uses the temporary fixing material precursor layer shown in FIG. 5(a). The laminate can be produced by forming a temporary fixing material precursor layer 30 containing a curable resin component on a support member 10 (FIG. 8(a)), curing the curable resin component in the temporary fixing material precursor layer 30 to form a temporary fixing material layer 30c containing a cured product of the curable resin component (FIG. 8(b)), and arranging a semiconductor member 40 on the formed temporary fixing material layer 30c (FIG. 8(c)). In such a manufacturing method, a wiring layer 41 such as a rewiring layer or a pattern layer can be provided on the temporary fixing material layer 30c before arranging the semiconductor member 40, so that the semiconductor member 40 having the wiring layer 41 can be formed by arranging the semiconductor member 40 on the wiring layer 41.
[0111] The semiconductor member 40 in the laminate 100 (the semiconductor member 40 temporarily fixed to the support member 10) may be further processed. By processing the semiconductor member 40 in the laminate 200 shown in FIG. 3(a), laminates 210 (FIG. 3(b)), 220 (FIG. 3(c)), 230 (FIG. 3(d)), etc. are obtained. By processing the semiconductor member 40 in the laminate 300 shown in FIG. 6(a), laminates 310 (FIG. 6(b)), 320 (FIG. 6(c)), 330 (FIG. 6(d)), etc. are obtained. The processing of the semiconductor member is not particularly limited, and examples thereof include thinning the semiconductor member, fabricating a through electrode, forming a wiring layer such as a rewiring layer or a pattern layer, etching, plating reflow, sputtering, etc.
[0112] The semiconductor member can be thinned by grinding the surface of the semiconductor member 40 opposite to the surface in contact with the temporary fixing material layer 20c or 30c with a grinder or the like. The thickness of the thinned semiconductor member may be, for example, 100 μm or less.
[0113] The grinding conditions can be set arbitrarily depending on the desired thickness of the semiconductor member, the grinding state, and the like.
[0114] The through electrode can be produced by performing processing such as dry ion etching or the Bosch process on the surface of the thinned semiconductor member 40 opposite to the surface in contact with the temporary fixing material layer 20c or 30c to form a through hole, and then performing processing such as copper plating.
[0115] In this manner, the semiconductor member 40 is processed, for example, the semiconductor member 40 is thinned, and a laminate 210 (FIG. 3(b)) or a laminate 310 (FIG. 6(b)) having a through electrode 44 formed therein can be obtained.
[0116] The laminate 210 shown in FIG. 3(b) or the laminate 310 shown in FIG. 6(b) may be covered with a sealing layer 50 as shown in FIG. 3(c) and FIG. 6(c). The material of the sealing layer 50 is not particularly limited, but may be a thermosetting resin composition from the viewpoint of heat resistance and other reliability. Examples of the thermosetting resin used for the sealing layer 50 include epoxy resins such as cresol novolac epoxy resin, phenol novolac epoxy resin, biphenyl diepoxy resin, and naphthol novolac epoxy resin. The composition for forming the sealing layer 50 may contain additives such as a filler and / or a flame retardant substance such as a bromine compound.
[0117] The form in which the sealing layer 50 is supplied is not particularly limited, but may be a solid material, a liquid material, a granular material, a film material, or the like.
[0118] For example, a compression sealing molding machine, a vacuum laminating device, or the like is used to seal the processed semiconductor member 42 with the sealing layer 50 formed from the sealing film. Using the above-mentioned device, for example, the processed semiconductor member 42 is covered with a sealing film that is heat-melted under conditions of 40 to 180°C (or 60 to 150°C), 0.1 to 10 MPa (or 0.5 to 8 MPa), and 0.5 to 10 minutes, to form the sealing layer 50. The sealing film may be prepared in a state in which it is laminated on a release liner such as a polyethylene terephthalate (PET) film. In this case, the sealing film is placed on the processed semiconductor member 42, the processed semiconductor member 42 is embedded, and then the release liner is peeled off to form the sealing layer 50. In this manner, the laminate 220 shown in FIG. 3(c) or the laminate 320 shown in FIG. 6(c) can be obtained.
[0119] The thickness of the sealing film is adjusted so that the sealing layer 50 has a thickness equal to or greater than the thickness of the processed semiconductor member 42. The thickness of the sealing film may be 50 to 2000 μm, 70 to 1500 μm, or 100 to 1000 μm.
[0120] The processed semiconductor member 42 having the sealing layer 50 may be divided into individual pieces by dicing, as shown in Fig. 3(d) and Fig. 6(d). In this manner, the laminate 230 shown in Fig. 3(d) or the laminate 330 shown in Fig. 6(d) can be obtained. The division into individual pieces by dicing may be performed after the semiconductor member separation step described later.
[0121] <Separation process for semiconductor components> As shown in FIG. 1(b), in the step of separating the semiconductor member, the temporary fixing material layer 20c or 30c in the laminate 100 is irradiated with incoherent light to separate the semiconductor member 40 from the support member 10.
[0122] Fig. 4 is a schematic cross-sectional view for explaining one embodiment of the method for manufacturing a semiconductor device of the present invention using the laminate shown in Fig. 3(d), and Fig. 4(a) and (b) are schematic cross-sectional views showing each step. Fig. 7 is a schematic cross-sectional view for explaining one embodiment of the method for manufacturing a semiconductor device of the present invention using the laminate shown in Fig. 6(d), and Fig. 7(a) and (b) are schematic cross-sectional views showing each step.
[0123] When the temporary fixing material layer 20c or 30c is irradiated with incoherent light, the conductive particles 22 or the light absorbing layer 32 absorbs the light and instantaneously generates heat, which may cause melting of the cured product 24c of the curable resin component or the resin cured product layer 34c due to heat at the interface or bulk, stress between the support member 10 and the semiconductor member 40 (processed semiconductor member 42), scattering of the conductive particles 22 or the light absorbing layer 32, etc. The occurrence of such phenomena allows the temporarily fixed processed semiconductor member 42 to be easily separated (peeled off) from the support member 10. In addition, in the separation process, a slight stress may be applied to the processed semiconductor member 42 in a direction parallel to the main surface of the support member 10 along with the irradiation of the incoherent light.
[0124] Incoherent light is an electromagnetic wave that has properties such as no interference fringes, low coherence, and low directivity, and tends to attenuate more as the optical path length becomes longer. Incoherent light is light that is not coherent. Laser light is generally coherent light, whereas sunlight, fluorescent light, and other light are incoherent light. Incoherent light can also be said to be light excluding laser light. The irradiation area of incoherent light is overwhelmingly larger than that of coherent light (i.e., laser light), so it is possible to reduce the number of irradiations (for example, once).
[0125] The incoherent light in the separation process may be light including at least infrared light. The light source of the incoherent light in the separation process is not particularly limited, but may be a xenon lamp. A xenon lamp is a lamp that utilizes light emission by application and discharge in an arc tube filled with xenon gas. A xenon lamp discharges while repeating ionization and excitation, so it has a continuous wavelength from the ultraviolet light region to the infrared light region stably. Since a xenon lamp requires a short time to start up compared to lamps such as metal halide lamps, the time required for the process can be significantly reduced. In addition, since a high voltage needs to be applied to emit light, high heat is generated instantaneously, but the cooling time is short, and continuous work is possible. In addition, the irradiation area of a xenon lamp is overwhelmingly larger than that of a laser, so it is possible to reduce the number of irradiations (for example, once).
[0126] The irradiation conditions of the xenon lamp can be set arbitrarily, such as the applied voltage, pulse width, irradiation time, irradiation distance (distance between the light source and the temporary fixing material layer), irradiation energy, etc. The irradiation conditions of the xenon lamp may be set so that separation is possible with one irradiation, or may be set so that separation is possible with two or more irradiations, but from the viewpoint of reducing damage to the processed semiconductor member 42, the irradiation conditions of the xenon lamp may be set so that separation is possible with one irradiation.
[0127] The separation step may be a step of irradiating the temporary fixing material layer 20c or 30c with incoherent light via the support member 10 (direction A in Figs. 4(a) and 7(a)). That is, the temporary fixing material layer 20c or 30c may be irradiated with incoherent light from the support member 10 side. By irradiating the temporary fixing material layer 20c or 30c with incoherent light via the support member 10, it is possible to irradiate the entire temporary fixing material layer 20c or the entire temporary fixing material layer 30c.
[0128] When the semiconductor member 40 or the processed semiconductor member 42 is separated from the support member 10, if any residues 20c' (FIGS. 4(a) and (b)) or 30c' (FIGS. 7(a) and (b)) of the temporary fixing material layer are attached to the semiconductor member 40 or the processed semiconductor member 42, these can be washed with a solvent. The solvent is not particularly limited, and examples thereof include ethanol, methanol, toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, and hexane. These may be used alone or in combination of two or more. The semiconductor member 40 or the processed semiconductor member 42 may be immersed in the solvent, or ultrasonic cleaning may be performed. Furthermore, the semiconductor member 40 or the processed semiconductor member 42 may be heated to a temperature of 100° C. or less.
[0129] By separating the semiconductor member from the support member in this manner, a semiconductor element 60 including the semiconductor member 40 or the processed semiconductor member 42 is obtained (FIGS. 4(b) and 7(b)). A semiconductor device can be manufactured by connecting the obtained semiconductor element 60 to another semiconductor element or a semiconductor element mounting substrate.
[0130] [Curable resin composition for temporary fixing material] The above-mentioned curable resin composition containing conductive particles that absorb light and generate heat can be suitably used as a temporary fixing material for temporarily fixing a semiconductor member to a support member.
[0131] The content of the conductive particles may be 30 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The components other than the conductive particles of the curable resin composition do not include a solvent. The content of the conductive particles may be 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more. The content of the conductive particles may be 80 parts by mass or less, 70 parts by mass or less, or 60 parts by mass or less.
[0132] The curable resin composition may further contain a thermoplastic resin. The content of the thermoplastic resin may be 10 to 90 parts by mass relative to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The content of the thermoplastic resin may be 30 parts by mass or more, 50 parts by mass or more, or 70 parts by mass or more. The content of the thermoplastic resin may be 88 parts by mass or less, 85 parts by mass or less, or 82 parts by mass or less.
[0133] The curable resin composition may further include a polymerizable monomer and a polymerization initiator. The content of the polymerizable monomer may be 10 to 90 parts by mass with respect to 100 parts by mass of the total amount of the components other than the conductive particles of the curable resin composition. The content of the polymerizable monomer may be 12 parts by mass or more, 15 parts by mass or more, or 18 parts by mass or more. The content of the polymerizable monomer may be 70 parts by mass or less, 50 parts by mass or less, or 30 parts by mass or less. The content of the polymerization initiator may be 0.01 to 5 parts by mass with respect to 100 parts by mass of the total amount of the polymerizable monomer. The content of the polymerization initiator may be 0.03 parts by mass or more, or 0.05 parts by mass or more. The content of the polymerization initiator may be 3 parts by mass or less, 1 part by mass or less, or 0.1 parts by mass or less.
[0134] The curable resin composition may be formed into a film.
[0135] [Film for temporary fixing material] The film containing the above-mentioned curable resin composition for a temporary fixing material can be suitably used as a temporary fixing material for temporarily fixing a semiconductor member to a support member.
[0136] [Laminated film for temporary fixing] The laminate film having the above-mentioned light absorbing layer and the resin layer containing a curable resin component can be suitably used as a temporary fixing material for temporarily fixing a semiconductor member to a support member. EXAMPLES
[0137] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0138] [Examples 1-1 to 1-4 and Comparative Example 1-1] (Production Example 1-1) <Preparation of Curable Resin Composition for Temporary Fixing Material> 80 parts by mass of hydrogenated styrene-butadiene elastomer (product name: Dynaron 2324P, JSR Corporation, Tg: -50°C) was mixed as the thermoplastic resin, 20 parts by mass of 1,9-nonanediol diacrylate (product name: FA-129AS, Hitachi Chemical Co., Ltd.) was mixed as the polymerizable monomer, and 1 part by mass of peroxyester (product name: Perhexa 25O, NOF Corporation) was mixed as the polymerization initiator. The hydrogenated styrene-butadiene elastomer was diluted with toluene to a solid content of 40% by mass. Conductive particles A (copper powder, product name: 1300Y, Mitsui Mining & Smelting Co., Ltd., shape: granular, average particle size (D 50 ): 3.5μm, tap density: 5.0g / cm 3 50 parts by mass of toluene was added to the mixture obtained. The mixture obtained was stirred for 10 minutes at 2200 rpm using an automatic stirrer to obtain a varnish of a curable resin composition for temporary fixing material containing toluene as a solvent.
[0139] <Preparation of film for temporary fixing material> The obtained varnish of the curable resin composition for temporary fixing material was applied to a release-treated surface of a polyethylene terephthalate (PET) film (Purex A31, Teijin DuPont Films Co., Ltd., thickness: 38 μm) using a precision coater, and the solvent was removed by drying at 80° C. for 10 minutes to produce a film for temporary fixing material of Production Example 1-1 having a thickness of approximately 100 μm.
[0140] <Preparation of laminate (evaluation sample)> The film for temporary fixing material of Production Example 1-1 prepared above was cut into 5 mm x 5 mm. A slide glass (size: 15 mm x 20 mm, thickness: 1 mm) was used as a support member, and a silicon wafer (size: 8 mm x 10 mm, thickness: 750 μm) was used as a semiconductor member. The film for temporary fixing material of Production Example 1-1 was sandwiched between the silicon wafer and the slide glass, and temporary thermocompression bonding was performed using a thermocompression bonding machine under conditions of 90 ° C, 5 seconds, and 1 MPa. After that, the film was thermally cured in an explosion-proof dryer under conditions of 150 ° C, 1 hour to form a temporary fixing material layer, thereby producing a laminate of Production Example 1-1.
[0141] (Production Example 1-2) Conductive particles A were mixed with conductive particles B (silver powder, product name: K0082P, Metalor, shape: granular, average particle size (D 50 ): 1.5μm, tap density: 5.0g / cm 3 ), a film for a temporary fixing material and a laminate of Production Example 1-2 were produced in the same manner as in Production Example 1-1.
[0142] (Production Example 1-3) Conductive particles A were replaced with conductive particles C (silver powder, product name: AgC-239, Fukuda Metal Foil Powder Co., Ltd., shape: flat, average particle size (D 50 ): 2.0~3.4μm, tap density: 4.2~6.1g / cm 3 ), a film for a temporary fixing material and a laminate of Production Example 1-3 were produced in the same manner as in Production Example 1-1.
[0143] (Production Example 1-4) A film for a temporary fixing material and a laminate of Production Example 1-4 were prepared in the same manner as in Production Example 1-1, except that the conductive particles A were changed to conductive particles D (carbon powder, product name: MA600, manufactured by Mitsubishi Chemical Corporation, shape: granular).
[0144] (Production Example 1-5) A laminate of Production Example 1-5 was produced in the same manner as Production Example 1-1, except that the conductive particles A were not added.
[0145] (Examples 1-1 to 1-4 and Comparative Example 1-1) <Peeling test> A xenon lamp was used as a light source of incoherent light. Under the irradiation conditions shown in Table 1, the laminates of Production Examples 1-1 to 1-5 were irradiated with the xenon lamp, and the peelability from the support member was evaluated. The xenon lamp used was S2300 (wavelength range: 270 nm to near infrared region, irradiation energy per unit area: 17 J / cm) manufactured by Xenon. 2 ) was used to irradiate the temporary fixing material layer via the supporting member for the laminate (glass slide). The irradiation distance was the distance between the light source and the stage on which the glass slide was placed. The peelability test was evaluated as follows: if the silicon wafer naturally peeled off from the glass slide after irradiation with the xenon lamp, it was rated as "A"; if the silicon wafer could be separated without damage when tweezers were inserted between the silicon wafer and the glass slide, it was rated as "B"; and if it could not be separated, it was rated as "C". The results are shown in Table 1.
[0146] [Table 1]
[0147] <Heat resistance test> The laminates of Production Examples 1-1 to 1-5 were heated, and the adhesiveness between the support member and the semiconductor member and the peelability from the support member after the heat treatment were evaluated as heat resistance. Heating was performed by leaving the laminates of Production Examples 1-1 to 1-5 on a hot plate heated to 260°C for 1 hour. The adhesiveness after the heat treatment was evaluated as "A" when tweezers were inserted between the silicon wafer and the slide glass, and "B" when they were not separated. The peelability from the slide glass after the heat treatment was evaluated in the same manner as in the peelability test. The xenon lamp irradiation was performed using the same xenon lamp as in the peelability test, with an applied voltage of 3000V, a pulse width of 5000μs, an irradiation distance of 10mm, one irradiation, and an irradiation time of 5000μs. The results are shown in Table 2.
[0148] [Table 2]
[0149] Comparison of Examples 1-1 to 1-4 with Comparative Example 1-1 revealed that Examples 1-1 to 1-4 were superior to Comparative Example 1-1 in terms of releasability from a support member. In addition, it was revealed that the temporary fixing curable resin composition of the present invention can form a temporary fixing material layer having excellent heat resistance.
[0150] [Examples 2-1, 2-2 and Comparative Example 2-1] (Production Example 2-1) <Preparation of Curable Resin Component> 80 parts by mass of hydrogenated styrene-butadiene elastomer (product name: Dynaron 2324P, JSR Corporation) was mixed as the thermoplastic resin, 20 parts by mass of 1,9-nonanediol diacrylate (product name: FA-129AS, Hitachi Chemical Co., Ltd.) was mixed as the polymerizable monomer, and 1 part by mass of peroxyester (product name: Perhexa 25O, NOF Corporation) was mixed as the polymerization initiator. The hydrogenated styrene-butadiene elastomer was diluted with toluene to a solid content of 40% by mass before use. In this way, a varnish of the curable resin component containing toluene as a solvent was prepared.
[0151] <Preparation of Curable Resin Composition> A varnish of a curable resin composition was prepared by mixing 14 parts by mass of an epoxy resin (product name: EPICLON EXA-4816, DIC Corporation), 1 part by mass of a curing agent (product name: Curesol 1B2MZ, Shikoku Chemical Industry Co., Ltd.), 60 parts by mass of conductive particles E (silver-coated copper powder, product name: Ag1400YP, Mitsui Mining & Smelting Co., Ltd., shape: flat), and 25 parts by mass of an organic solvent (ethyl acetate).
[0152] <Preparation of laminated film for temporary fixing material> The obtained varnish of the curable resin component was applied to a release-treated surface of a polyethylene terephthalate (PET) film (Purex A31, Teijin DuPont Films Ltd., thickness: 38 μm) using a precision coater, and the solvent was removed by drying at 80°C for 10 minutes to produce a resin layer of approximately 100 μm.
[0153] Next, the varnish of the curable resin composition was applied onto the resin layer using a precision coater, and the organic solvent was dried and removed at 80° C. for 10 minutes to prepare a light absorbing layer of 1000 nm. As a result, a laminated film for temporary fixing material of Production Example 2-1 having a thickness of about 100 μm was obtained.
[0154] <Preparation of laminate (evaluation sample)> The laminated film for temporary fixing material of Production Example 2-1 prepared above was cut to 5 mm x 5 mm. A slide glass (size: 20 mm x 15 mm, thickness: 1 mm) was used as a support member, and a silicon wafer (size: 8 mm x 10 mm, thickness: 750 μm) was used as a semiconductor member. The laminated film for temporary fixing material of Production Example 2-1 was sandwiched between the silicon wafer and the slide glass so that the light absorbing layer was in contact with the slide glass (configuration shown in FIG. 5(a)), and temporary thermocompression bonding was performed using a thermocompression bonding machine under conditions of 90 ° C, 5 seconds, and 1 MPa. Thereafter, the laminated body of Production Example 2-1 was produced by thermally curing the laminated film in an explosion-proof dryer under conditions of 150 ° C, 1 hour.
[0155] (Production Example 2-2) A laminate film and a laminate for a temporary fixing material of Production Example 2-2 were obtained in the same manner as in Production Example 2-1, except that the light absorbing layer was changed to a layer composed of two conductive layers (first conductive layer: titanium, second conductive layer: copper). The light absorbing layer was pretreated by reverse sputtering (Ar flow rate: 1.2 × 10 -2 Pa·m 3 After that, RF sputtering was performed under the processing conditions shown in Table 3, resulting in a titanium (first conductive layer) / copper (second conductive layer) thickness of 50 nm / 200 nm.
[0156] [Table 3]
[0157] (Production Example 2-3) A laminate of Production Example 2-3 was produced in the same manner as Production Example 2-1, except that no light absorbing layer was provided (that is, only a resin layer was provided).
[0158] (Examples 2-1, 2-2 and Comparative Example 2-1) <Peeling test> A xenon lamp was used as a light source of incoherent light. Under the irradiation conditions shown in Table 4, the laminates of Production Examples 2-1 to 2-3 were irradiated with a xenon lamp, and the peelability from the support member was evaluated. The xenon lamp used was S2300 (wavelength range: 270 nm to near infrared region, irradiation energy per unit area: 17 J / cm) manufactured by Xenon. 2 ) was used to irradiate the temporary fixing material layer through the supporting member (glass slide) of the laminate. The irradiation distance was the distance between the light source and the stage on which the glass slide was placed. The peelability test was evaluated as follows: if the silicon wafer naturally peeled off from the glass slide after irradiation with the xenon lamp, it was rated as "A"; if the silicon wafer could be separated without damage when tweezers were inserted between the silicon wafer and the glass slide, it was rated as "B"; and if it could not be separated, it was rated as "C". The results are shown in Table 4.
[0159] [Table 4]
[0160] Comparing Examples 2-1 and 2-2 with Comparative Example 2-1, it was found that Examples 2-1 and 2-2 were superior to Comparative Example 2-1 in terms of releasability from the support member.
[0161] [Examples 3-1 to 3-3 and Comparative Examples 3-1 to 3-3] (Production Example 3-1) <Preparation of evaluation samples> The laminated film for temporary fixing material of Example 2-2 prepared above was cut to 5 mm x 5 mm. A slide glass (size: 20 mm x 15 mm, thickness: 1 mm) was used as a support member, and a silicon wafer (size: 8 mm x 10 mm, thickness: 750 μm) was used as a semiconductor member. The laminated film for temporary fixing material of Example 2-2 was sandwiched between the silicon wafer and the slide glass so that the light absorbing layer was in contact with the slide glass (so as to have the configuration shown in FIG. 5 (a)), and temporary thermocompression bonding was performed using a thermocompression bonding machine under conditions of 90 ° C, 5 seconds, and 1 MPa. Thereafter, the laminated body of Production Example 3-1 was produced by thermally curing the laminated film in an explosion-proof dryer under conditions of 150 ° C, 1 hour.
[0162] (Production Example 3-2) A laminate of Production Example 3-2 was produced in the same manner as in Production Example 3-1, except that the laminate film for temporary fixing material of Example 2-2 was sandwiched between a silicon wafer and a slide glass so that the light absorbing layer was in contact with the silicon wafer (so as to have the configuration shown in FIG. 5(b)).
[0163] (Production Example 3-3) A second light absorbing layer (copper) and a first light absorbing layer (titanium) were further laminated in this order on the surface of the laminated film for temporary fixing material of Example 2-2 on which the light absorbing layer was not provided, to prepare a laminated film for temporary fixing material. Note that, as in Example 2-2, the light absorbing layer was pretreated by reverse sputtering (Ar flow rate: 1.2×10 -2 Pa·m 3 After that, RF sputtering was performed under the treatment conditions shown in Table 3, and the thickness of titanium / copper was set to 50 nm / 200 nm. The laminate of Production Example 3-3 was produced in the same manner as Production Example 3-1, except that the laminate film for temporary fixing material produced in this manner was sandwiched between a silicon wafer and a slide glass so as to have the configuration shown in Fig. 5(c).
[0164] (Examples 3-1 to 3-3) <Peeling test> A xenon lamp was used as a light source of incoherent light. Under the irradiation conditions shown in Table 5, the laminates of Production Examples 3-1 to 3-3 were irradiated with a xenon lamp, and the peelability from the support member was evaluated. The xenon lamp used was S2300 (wavelength range: 270 nm to near infrared region, irradiation energy per unit area: 17 J / cm) manufactured by Xenon. 2 ) was used to irradiate the temporary fixing material layer through the supporting member (glass slide) of the laminate. The irradiation distance was the distance between the light source and the stage on which the glass slide was placed. The peelability test was evaluated as follows: if the silicon wafer naturally peeled off from the glass slide after irradiation with the xenon lamp, it was rated as "A"; if the silicon wafer could be separated without damage when tweezers were inserted between the silicon wafer and the glass slide, it was rated as "B"; and if it could not be separated, it was rated as "C". The results are shown in Table 5.
[0165] [Table 5]
[0166] (Comparative Examples 3-1 to 3-3) <Peeling test> A YAG laser was used as a light source of coherent light. The laminates of Manufacturing Examples 3-1 to 3-3 were irradiated with a YAG laser to evaluate the peelability from the support member. As the YAG laser, MD-H (wavelength: 1064 nm, output: 10 W, scanning speed: 1000 mm / s) manufactured by Keyence Corporation was used to irradiate the temporary fixing material layer through the support member (slide glass) of the laminate. In the evaluation of the peelability test, after irradiation with the YAG laser, the silicon wafer was naturally peeled off from the slide glass, which was evaluated as "A", the silicon wafer was not broken when tweezers were inserted between the silicon wafer and the slide glass, which could be separated, which was evaluated as "B", and the one that could not be separated was evaluated as "C". The results are shown in Table 6.
[0167] [Table 6]
[0168] Comparing Examples 3-1 to 3-3 with Comparative Examples 3-1 to 3-3, it was found that Examples 3-1 to 3-3, which used a xenon lamp that is incoherent light, were superior in terms of peelability to Comparative Examples 3-1 to 3-3, which used a YAG laser that is coherent light.
[0169] [Examples 4-1 to 4-6] (Manufacturing Examples 4-1 to 4-6) <Preparation of Curable Resin Component> As the thermoplastic resin, 70 parts by mass of hydrogenated styrene-based elastomer (product name: FG1924, Kraton Polymer Japan Co., Ltd.), as the epoxy resin, 30 parts by mass of dicyclopentadiene-type epoxy resin (product name: HP-7200H, DIC Corporation), and as the curing accelerator, 2 parts by mass of 1-cyanoethyl-2-phenylimidazole (product name: Curesol 2PZ-CN, Shikoku Kasei Co., Ltd.) were mixed. The hydrogenated styrene-based elastomer was diluted with toluene to a solid content of 25% by mass, and the epoxy resin was diluted with toluene to a solid content of 50% by mass. The mixture was mixed using a mix rotor and stirred at 50 rpm for 24 hours to prepare a varnish of the curable resin component containing toluene as a solvent.
[0170] <Preparation of Curable Resin Component Film> The obtained varnish of the curable resin component was applied to a release-treated surface of a polyethylene terephthalate (PET) film (Purex A31, Teijin DuPont Films Ltd., thickness: 38 μm) using a precision coater, and the solvent was removed by drying at 80°C for 10 minutes to produce a curable resin component film (resin layer) of approximately 20 μm.
[0171] <Preparation of laminate (evaluation sample)> A slide glass (size: 20 mm x 15 mm, thickness: 1 mm) was prepared as a support member, and a conductive layer was prepared with the metal type and thickness shown in Table 7 using a metal deposition device, and this was used as a light absorbing layer. In the light absorbing layer, the support member, the first conductive layer, and the second conductive layer were laminated in this order. Next, the above-mentioned curable resin component film was cut out to 50 mm x 50 mm, and a silicon wafer (size: 8 mm x 10 mm, thickness: 750 μm) was prepared as a semiconductor member. The cut-out curable resin component film was sandwiched between the light absorbing layer and the slide glass so as to have the configuration shown in FIG. 5(a), and a thermocompression machine was used to perform temporary thermocompression bonding under conditions of 90 ° C, 5 seconds, and 1 MPa. Thereafter, the laminates of Production Examples 4-1 to 4-6 were produced by thermally curing the laminates in an explosion-proof dryer under conditions of 150 ° C, 1 hour.
[0172] (Examples 4-1 to 4-6) <Peeling test> A xenon lamp was used as a light source of incoherent light. Under the irradiation conditions shown in Table 7, the laminates of Production Examples 4-1 to 4-6 were irradiated with a xenon lamp, and the peelability from the support member was evaluated. The xenon lamp used was S2300 (wavelength range: 270 nm to near infrared region, irradiation energy per unit area: 17 J / cm) manufactured by Xenon Corporation. 2 ) was used to irradiate the temporary fixing material layer through the supporting member (glass slide) of the laminate. The irradiation distance was the distance between the light source and the stage on which the glass slide was placed. The peelability test was evaluated as follows: if the silicon wafer naturally peeled off from the glass slide after irradiation with the xenon lamp, it was rated as "A"; if the silicon wafer could be separated without damage when tweezers were inserted between the silicon wafer and the glass slide, it was rated as "B"; and if it could not be separated, it was rated as "C". The results are shown in Table 7.
[0173] [Table 7]
[0174] It was found that all of Examples 4-1 to 4-6 were excellent in terms of releasability from the support member.
[0175] [Examples 5-1 to 5-7] (Manufacturing Examples 5-1 to 5-7) <Preparation of Curable Resin Component> As the thermoplastic resin, 70 parts by mass of hydrogenated styrene-based elastomer (product name: FG1924, Kraton Polymer Japan Co., Ltd.), as the epoxy resin, 30 parts by mass of dicyclopentadiene-type epoxy resin (product name: HP-7200H, DIC Corporation), and as the curing accelerator, 2 parts by mass of 1-cyanoethyl-2-phenylimidazole (product name: Curesol 2PZ-CN, Shikoku Kasei Co., Ltd.) were mixed. The hydrogenated styrene-based elastomer was diluted with toluene to a solid content of 25% by mass, and the epoxy resin was diluted with toluene to a solid content of 50% by mass. The mixture was mixed using a mix rotor and stirred at 50 rpm for 24 hours to prepare a varnish of the curable resin component containing toluene as a solvent.
[0176] <Preparation of Curable Resin Component Film> The obtained varnish of the curable resin component was applied to a release-treated surface of a polyethylene terephthalate (PET) film (Purex A31, Teijin DuPont Films Ltd., thickness: 38 μm) using a precision coater, and the solvent was removed by drying at 80°C for 10 minutes to produce a curable resin component film (resin layer) of approximately 20 μm.
[0177] <Preparation of laminate (evaluation sample)> A glass slide (size: 20 mm × 15 mm, thickness: 1 mm) was prepared as a support member, and a conductive layer was prepared by sputtering with the metal type and thickness shown in Table 8, which was used as a light absorbing layer. Note that the light absorbing layer was prepared by pretreatment by reverse sputtering (Ar flow rate: 1.2 × 10 -2 Pa·m 3After that, RF sputtering was performed under the treatment conditions shown in Table 3. In the light absorbing layer having two conductive layers, the support member, the first conductive layer, and the second conductive layer were laminated in this order. Next, the above-mentioned curable resin component film was cut into 50 mm x 50 mm, and a silicon wafer (size: 8 mm x 10 mm, thickness: 750 μm) was prepared as a semiconductor member. The cut-out curable resin component film was sandwiched between the light absorbing layer and a slide glass so as to have the configuration shown in FIG. 5(a), and a thermocompression machine was used to perform temporary thermocompression bonding under conditions of 90 ° C, 5 seconds, and 1 MPa. Then, the laminates of Examples 5-1 to 5-7 were produced by thermally curing the laminates in an explosion-proof dryer under conditions of 150 ° C, 1 hour.
[0178] (Examples 5-1 to 5-7) <Peeling test> A xenon lamp was used as a light source of incoherent light. Under the irradiation conditions shown in Table 8, the laminates of Production Examples 5-1 to 5-7 were irradiated with a xenon lamp, and the peelability from the support member was evaluated. The xenon lamp used was S2300 (wavelength range: 270 nm to near infrared region, irradiation energy per unit area: 17 J / cm) manufactured by Xenon. 2 ) was used to irradiate the temporary fixing material layer through the supporting member (glass slide) of the laminate. The irradiation distance was the distance between the light source and the stage on which the glass slide was placed. The peelability test was evaluated as follows: if the silicon wafer naturally peeled off from the glass slide after irradiation with the xenon lamp, it was rated as "A"; if the silicon wafer could be separated without damage when tweezers were inserted between the silicon wafer and the glass slide, it was rated as "B"; and if it could not be separated, it was rated as "C". The results are shown in Table 8.
[0179] [Table 8]
[0180] It was found that all of Examples 5-1 to 5-7 were excellent in terms of releasability from the supporting member.
[0181] From the above results, it was confirmed that the method for manufacturing a semiconductor device of the present invention makes it possible to easily separate a temporarily fixed semiconductor member from a supporting member. [Explanation of symbols]
[0182] DESCRIPTION OF THE PREFERRED EMBODIMENTS 10...support member, 20...temporary fixing material precursor layer, 20c...temporary fixing material layer, 20c'...residue of temporary fixing material layer, 22...conductive particles, 24...curable resin component, 24c...cured product of curable resin component, 30...temporary fixing material precursor layer, 30c...temporary fixing material layer, 30c'...residue of temporary fixing material layer, 32...light absorbing layer, 34...resin layer, 34c...cured resin layer, 40...semiconductor member, 41...wiring layer, 42...processed semiconductor member, 44...through electrode, 50...sealing layer, 60...semiconductor element, 100,200,210,220,230,300,310,320,330...laminate.
Claims
1. A support member and a conductive layer formed on the support member and made of a conductive material that absorbs light and generates heat, the support member is a glass substrate, the conductor contains at least one selected from the group consisting of titanium and copper, the conductive layer is composed of a first conductive layer made of a first conductive material provided on the support member, and a second conductive layer made of a second conductive material provided on a surface of the first conductive layer opposite to the support member; the first conductor comprises titanium; The second conductor comprises at least one metal selected from the group consisting of copper, aluminum, silver, gold, and platinum.
2. The temporary fixing laminate according to claim 1 , further comprising a resin layer containing a curable resin component provided on the conductive layer.
3. A step of preparing a temporary fixing laminate including a support member and a temporary fixing material precursor layer, the temporary fixing material precursor layer including, in this order from the support member side, a conductor layer made of a conductor that absorbs light and generates heat, and a resin layer including a curable resin component; A step of disposing a semiconductor member on the support member via the temporary fixing material precursor layer of the temporary fixing laminate; a step of curing the curable resin component in the temporary fixing material precursor layer to produce a laminate in which the supporting member, the conductor layer, a temporary fixing material layer having a resin cured material layer containing a cured product of the curable resin component, and the semiconductor member are laminated in this order; a step of irradiating the temporary fixing material layer in the laminate with incoherent light to separate the semiconductor member from the support member; Equipped with the support member is a glass substrate, the conductor contains at least one selected from the group consisting of titanium and copper, the conductive layer is composed of a first conductive layer made of a first conductive material provided on the support member, and a second conductive layer made of a second conductive material provided on a surface of the first conductive layer opposite to the support member; the first conductor comprises titanium; The method for manufacturing a semiconductor device, wherein the second conductor includes at least one selected from the group consisting of copper, aluminum, silver, gold, and platinum.
Citation Information
Patent Citations
Peeling method, semiconductor device, and manufacturing method therefor
JP2003174153A
Laminate including substrate to be ground, method of manufacturing the same, method of manufacturing ultrathin substrate using the laminate, and apparatus therefor
JP2004064040A
Manufacturing method of semiconductor chip
JP2005159155A
Laminate and method for separating the same
JP2012109538A
Temporary fixing agent, and method for processing base material
JP2012126803A