Composition for adhesive layer of non-aqueous secondary battery, battery member for non-aqueous secondary battery and method for producing same, method for producing laminate for non-aqueous secondary battery, and method for producing non-aqueous secondary battery

The use of a core-shell structured adhesive layer composition with specific viscosity and shear rate ratios addresses the low adhesive strength and battery resistance issues in non-aqueous secondary batteries, improving low-temperature output characteristics.

JP7583612B2Active Publication Date: 2024-11-14ZEON CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020539397
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-29
Filing Date
2019-08-22
Publication Date
2024-11-14
Estimated Expiration
2039-08-22

AI Technical Summary

Technical Problem

Conventional secondary battery adhesive layers formed using an inkjet method exhibit low adhesive strength, leading to increased battery resistance and impaired low-temperature output characteristics in non-aqueous secondary batteries.

Method used

A non-aqueous secondary battery adhesive layer composition containing organic particles with a core-shell structure, a thixotropic agent, and water, with specific viscosity and shear rate ratios, is used to form an adhesive layer on a porous membrane layer, ensuring firm adhesion and improved low-temperature output characteristics.

Benefits of technology

The composition allows for efficient formation of an adhesive layer that firmly bonds battery members, reducing battery resistance and enhancing low-temperature performance in non-aqueous secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583612000001
    Figure 0007583612000001
Patent Text Reader

Abstract

The organic particles have a core-shell structure including a core and a shell that at least partially covers the outer surface of the core, and the shear rate is 100 sec -1 Viscosity η0 is less than 10 mPa·s, shear rate is 10,000 sec -1 The present invention provides a non-aqueous secondary battery adhesive layer composition having a viscosity η1 of 0.5 mPa·s or more and 2.4 mPa·s or less, and a ratio of viscosity η0 to viscosity η1 (η0 / η1) of 1.2 or more and 10 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for a non-aqueous secondary battery adhesive layer, a battery member for a non-aqueous secondary battery and a method for producing the same, a method for producing a laminate for a non-aqueous secondary battery, and a method for producing a non-aqueous secondary battery. [Background technology]

[0002] Non-aqueous secondary batteries such as lithium ion secondary batteries (hereinafter sometimes abbreviated as "secondary batteries") are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Secondary batteries generally include battery components such as a positive electrode, a negative electrode, and a separator that isolates the positive electrode and the negative electrode to prevent a short circuit between the positive electrode and the negative electrode.

[0003] In manufacturing such a secondary battery, it has been conventional to bond battery components of the secondary battery, for example, an electrode and a separator, together to form a laminate for the secondary battery. Here, the bonding of the battery components together is performed, for example, by manufacturing a battery component having an adhesive layer on its surface and bonding the battery component to another battery component. The battery component having an adhesive layer on its surface can be produced by applying a composition for a secondary battery adhesive layer, which is made by dispersing and / or dissolving an adhesive polymer (binder) or the like in a solvent, to the surface of the battery component and then drying it.

[0004] In recent years, battery components equipped with a porous membrane layer that imparts desired performance such as heat resistance to the battery components have been used in secondary batteries. Specifically, for example, a separator with a porous membrane layer formed by forming a porous membrane layer on a separator substrate, or an electrode with a porous membrane layer formed by forming a porous membrane layer on an electrode substrate formed by providing an electrode mixture layer on a current collector, are used as battery components.

[0005] As the above-mentioned secondary battery adhesive layer composition, Patent Document 1 proposes a composition containing organic particles and a specific water-soluble polymer and having a predetermined viscosity. Patent Document 2 proposes a composition containing organic particles having a specific structure and a binder and having a predetermined viscosity. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2017 / 090242 [Patent Document 2] International Publication No. 2016 / 103559 Summary of the Invention [Problem to be solved by the invention]

[0007] Here, the present inventors have focused on an inkjet method in which a secondary battery adhesive layer composition for forming an adhesive layer is discharged as fine droplets from a nozzle and supplied to the surface of a battery component in order to firmly bond battery components together and to provide the secondary battery with excellent battery characteristics. The present inventors then applied the conventional secondary battery adhesive layer composition to the porous membrane layer of a separator with a porous membrane layer by an inkjet method to produce a separator with a porous membrane layer (substrate with a porous membrane layer) in which an adhesive layer is formed on the porous membrane layer, and bonded the separator with a porous membrane layer and an electrode (adhered member) via the adhesive layer to produce a secondary battery. However, it has become clear that the adhesive layer formed on the porous membrane layer by the inkjet method using the above-mentioned conventional secondary battery adhesive layer composition has low adhesive strength, and the obtained secondary battery has an increased battery resistance and impaired low-temperature output characteristics. Therefore, there has been a demand for a non-aqueous secondary battery adhesive layer composition (hereinafter sometimes abbreviated as "secondary battery adhesive layer composition") that can firmly bond a substrate with a porous membrane layer and an adherend using an inkjet method.

[0008] Therefore, the present invention aims to provide a composition for a secondary battery adhesive layer that can efficiently form an adhesive layer on the porous membrane layer of a substrate with a porous membrane layer even when an inkjet method is used, and can firmly bond the substrate with a porous membrane layer and an adherend member via the adhesive layer. Another object of the present invention is to provide a battery member for a non-aqueous secondary battery that can be firmly bonded to an adherend via an adhesive layer formed on the porous membrane layer of a substrate with a porous membrane layer, and a method for manufacturing such a battery member for a non-aqueous secondary battery. Furthermore, the present invention aims to provide a laminate for a non-aqueous secondary battery in which a substrate with a porous membrane layer and an adherend are firmly adhered to each other via an adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer by using an inkjet method, the laminate enabling the secondary battery to exhibit excellent low-temperature output characteristics, and a non-aqueous secondary battery using the laminate for a non-aqueous secondary battery obtained by the manufacturing method. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems. The present inventors have discovered a method for producing a viscoelastic composition comprising organic particles having a core-shell structure, a thixotropic agent, and water, and a shear rate of 100 sec -1 Viscosity η0 and shear rate 10000sec -1 It has been found that, by using a composition for a secondary battery adhesive layer having a viscosity η1 at a temperature within a predetermined range and a ratio of the viscosity η0 to the viscosity η1 within a predetermined range, an adhesive layer can be efficiently formed on the porous membrane layer of a substrate with a porous membrane layer even when an inkjet method is used, the substrate with a porous membrane layer and the adherend can be firmly adhered to each other via the adhesive layer, and further, the secondary battery can be made to exhibit excellent low-temperature output characteristics, thereby completing the present invention.

[0010] That is, the present invention has an object to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery adhesive layer composition of the present invention is a non-aqueous secondary battery adhesive layer composition containing organic particles, a thixotropic agent and water, the organic particles having a core part and a shell part at least partially covering the outer surface of the core part, and the composition is a non-aqueous secondary battery adhesive layer composition containing ... -1 The viscosity η0 at a shear rate of 10,000 sec is less than 10 mPa s. -1 The viscosity η1 at a shear rate of 100 sec is 0.5 mPa s or more and 2.4 mPa s or less, and the ratio of the viscosity η0 to the viscosity η1 (η0 / η1) is 1.2 or more and 10 or less. -1 Viscosity η0 at shear rate of 10000sec -1 If the composition for a secondary battery adhesive layer has a viscosity η1 at 1000° C. and a ratio of the viscosity η0 to η1 within a predetermined range, an adhesive layer can be efficiently formed on the porous membrane layer of the substrate with a porous membrane layer even when an inkjet method is used, and the substrate with a porous membrane layer and the adherend can be firmly adhered to each other via the adhesive layer, and further, the secondary battery can exhibit excellent low-temperature output characteristics.

[0011] Here, the non-aqueous secondary battery adhesive layer composition of the present invention preferably has a surface tension of 30 mN / m or more and 60 mN / m or less. If the surface tension of the secondary battery adhesive layer composition is equal to or more than the lower limit, the porous membrane layer-attached substrate and the adherend can be more firmly bonded via the adhesive layer formed on the porous membrane layer, and the increase in the battery resistance of the secondary battery can be suppressed to improve the low-temperature output characteristics. In addition, if the surface tension of the secondary battery adhesive layer composition is equal to or less than the upper limit, when the secondary battery adhesive layer composition is applied using the inkjet method, the droplets of the secondary battery adhesive layer composition discharged from the inkjet nozzle are stable. Therefore, the variation in discharge can be suppressed to maintain good dischargeability.

[0012] In addition, the non-aqueous secondary battery adhesive layer composition of the present invention preferably has a solid content concentration of 30 mass % or less. If the solid content concentration of the secondary battery adhesive layer composition is 30 mass % or less, the dischargeability of the secondary battery adhesive layer composition is improved when the secondary battery adhesive layer composition is applied by an inkjet method.

[0013] In the nonaqueous secondary battery adhesive layer composition of the present invention, the core part is preferably made of a polymer having a swelling degree in an electrolyte solution of 5 to 30 times, the shell part is preferably made of a polymer having a swelling degree in an electrolyte solution of more than 1 to 4 times, the polymer constituting the core part has a glass transition temperature of -50°C to 150°C, and the polymer constituting the shell part has a glass transition temperature that is 10°C or more lower than the glass transition temperature of the polymer constituting the core part. When the polymer constituting the core part and the polymer constituting the shell part each have a predetermined swelling degree in an electrolyte solution and a predetermined glass transition temperature, the secondary battery can exhibit excellent low-temperature output characteristics, and deterioration of the adhesive strength of the adhesive layer in an electrolyte solution and deterioration of high-temperature cycle characteristics can be suppressed.

[0014] The present invention also aims to advantageously solve the above problems, and the battery member for a non-aqueous secondary battery of the present invention comprises a substrate with a porous membrane layer formed on at least one side of the substrate, and a plurality of dot-shaped adhesive layers formed on the porous membrane layer, the substrate being a separator substrate or an electrode substrate, and the adhesive layer being a dried product of any of the above-mentioned compositions for a non-aqueous secondary battery adhesive layer. According to the present invention, the battery member for a non-aqueous secondary battery comprises a substrate with a porous membrane layer having a plurality of dot-shaped adhesive layers formed by drying any of the above-mentioned compositions for a secondary battery adhesive layer on the porous membrane layer, and therefore the battery member for a non-aqueous secondary battery is firmly bonded to the adherend member via the adhesive layer, and the secondary battery can exhibit excellent low-temperature output characteristics.

[0015] The present invention also aims to advantageously solve the above problems, and the manufacturing method of the battery member for non-aqueous secondary batteries of the present invention includes a coating step of applying any of the above-mentioned compositions for non-aqueous secondary battery adhesive layer on the porous membrane layer of a substrate with a porous membrane layer formed on at least one side of the substrate by an inkjet method, and a drying step of drying the composition for non-aqueous secondary battery adhesive layer applied on the porous membrane layer to form an adhesive layer, the substrate being a separator substrate or an electrode substrate. According to the manufacturing method of the battery member for non-aqueous secondary batteries of the present invention, a secondary battery battery member that can be firmly bonded to an adherend via the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer and can exhibit excellent low-temperature output characteristics in the secondary battery can be efficiently manufactured.

[0016] The present invention also aims to advantageously solve the above problems, and the method for producing a non-aqueous secondary battery laminate of the present invention includes a coating step of coating any of the above-mentioned non-aqueous secondary battery adhesive layer compositions by an inkjet method on the porous membrane layer of a substrate with a porous membrane layer formed on at least one side of the substrate, a drying step of drying the non-aqueous secondary battery adhesive layer composition coated on the porous membrane layer to form an adhesive layer, and an adhesion step of adhering the substrate with a porous membrane layer and an adherend member through the adhesive layer, wherein the substrate is a separator substrate or an electrode substrate. In this way, by forming an adhesive layer on the porous membrane layer of the substrate with a porous membrane layer using the above-mentioned secondary battery adhesive layer composition, and adhering the substrate with a porous membrane layer and the adherend member through the formed adhesive layer, a non-aqueous secondary battery laminate in which the substrate with a porous membrane layer and the adherend member are firmly adhered can be produced.

[0017] The present invention also aims to advantageously solve the above problems, and the method for producing a nonaqueous secondary battery of the present invention is characterized in that it uses a laminate for a nonaqueous secondary battery obtained by the above-mentioned method for producing a laminate for a nonaqueous secondary battery. In this way, by using the laminate for a nonaqueous secondary battery obtained by the above-mentioned method for producing a nonaqueous secondary battery of the present invention, a secondary battery having excellent low-temperature output characteristics can be efficiently produced. Effect of the Invention

[0018] According to the present invention, even when an inkjet method is used, an adhesive layer can be efficiently formed on the porous membrane layer of a substrate with a porous membrane layer, and a composition for a secondary battery adhesive layer can be provided that can firmly bond the substrate with a porous membrane layer and an adherend member via the adhesive layer. In addition, according to the present invention, it is possible to provide a battery member for a non-aqueous secondary battery that can be firmly bonded to an adherend via an adhesive layer formed on the porous membrane layer of a substrate with a porous membrane layer, and a method for manufacturing the same. Furthermore, according to the present invention, there can be provided a method for producing a laminate for a non-aqueous secondary battery, in which a substrate with a porous membrane layer and an adherend are firmly adhered to each other via an adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, and the laminate can cause the secondary battery to exhibit excellent low-temperature output characteristics. According to the present invention, a method for producing a nonaqueous secondary battery having excellent low-temperature output characteristics can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described in detail. Here, the non-aqueous secondary battery adhesive layer composition of the present invention can be used as an adhesive material when forming an adhesive layer on the porous membrane layer of a substrate with a porous membrane layer by using an inkjet method, and adhering the substrate with a porous membrane layer to an adherend via the adhesive layer. Specifically, the secondary battery adhesive layer composition of the present invention can be used in the manufacture of a battery member for a non-aqueous secondary battery, a laminate for a non-aqueous secondary battery, and a secondary battery.

[0020] (Non-aqueous secondary battery adhesive layer composition) The secondary battery adhesive layer composition of the present invention is a slurry composition containing organic particles, a thixotropic agent, and water, and may optionally contain other components. The secondary battery adhesive layer composition is a slurry composition in which the organic particles have a core-shell structure and the organic particles are melt-melted at a shear rate of 100 sec -1 Viscosity η0 at shear rate of 10000sec-1 and the ratio of viscosity η0 to viscosity η1 must be within a predetermined range.

[0021] <Organic particles> Here, the organic particles contained in the secondary battery adhesive layer composition are components that function as a binder in the adhesive layer that bonds battery components such as separators, electrodes, etc. By using organic particles having a core-shell structure as the binder, the battery components can be firmly bonded to each other via the adhesive layer.

[0022] <<Core-shell structure>> The organic particles have a core-shell structure including a core and a shell covering the outer surface of the core. The shell may cover the entire outer surface of the core, or may cover only a part of the outer surface of the core. Even if the outer surface of the core appears to be completely covered by the shell, the shell is a shell that partially covers the outer surface of the core if holes that communicate between the inside and outside of the shell are formed. Therefore, for example, an organic particle that includes a shell having pores that communicate from the outer surface of the shell (i.e., the circumferential surface of the organic particle) to the outer surface of the core corresponds to an organic particle in which the shell partially covers the outer surface of the core.

[0023] <<Core>> [Electrolyte swelling rate] The electrolyte swelling degree of the polymer constituting the core part is preferably 5 times or more, more preferably 7 times or more, even more preferably 9 times or more, preferably 30 times or less, more preferably 25 times or less, even more preferably 20 times or less, and particularly preferably 10 times or less. If the electrolyte swelling degree of the polymer constituting the core part is within the above range, even when the secondary battery adhesive layer composition of the present invention is used in the inkjet method, the adhesive strength of the formed adhesive layer can be suppressed from decreasing in the electrolyte, and the high-temperature cycle characteristics of the secondary battery can be suppressed from decreasing. Furthermore, if the electrolyte swelling degree of the polymer constituting the core part is equal to or more than the above lower limit, the low-temperature output characteristics of the secondary battery can be further improved. In the present invention, the "degree of swelling in an electrolyte solution" can be measured by the measurement method described in the Examples of this specification. The degree of swelling of the polymer constituting the core portion in an electrolyte solution can be adjusted, for example, by changing the types and ratios of monomers used in preparing the polymer constituting the core portion.

[0024] [Glass transition temperature (Tg)] Here, the glass transition temperature (Tg) of the polymer constituting the core part is preferably -50 ° C. or higher, more preferably -20 ° C. or higher, even more preferably 10 ° C. or higher, particularly preferably 50 ° C. or higher, preferably 150 ° C. or lower, more preferably 140 ° C. or lower, even more preferably 130 ° C. or lower, particularly preferably 100 ° C. or lower. If the glass transition temperature of the polymer constituting the core part is the above lower limit value or higher, even when the secondary battery adhesive layer composition of the present invention is used in the ink jet method, the battery components can be bonded more firmly through the formed adhesive layer, and the low-temperature output characteristics can be improved. On the other hand, if the glass transition temperature of the polymer constituting the core part is the above upper limit value or lower, the high-temperature cycle characteristics of the secondary battery can be improved, and the adhesive strength of the adhesive layer in the electrolyte can be prevented from decreasing. In the present invention, the "glass transition temperature" can be measured by the measurement method described in the Examples of this specification. The glass transition temperature of the polymer constituting the core portion can be adjusted, for example, by changing the types and ratio of monomers used in preparing the polymer constituting the core portion.

[0025] [composition] Examples of monomers used to prepare the polymer constituting the core portion include vinyl chloride monomers such as vinyl chloride and vinylidene chloride; vinyl acetate monomers such as vinyl acetate; aromatic vinyl monomers such as styrene, α-methylstyrene, styrenesulfonic acid, butoxystyrene, and vinylnaphthalene; vinylamine monomers such as vinylamine; vinylamide monomers such as N-vinylformamide and N-vinylacetamide; butyl acrylates such as methyl acrylate, ethyl acrylate, and n-butyl acrylate; 2-ethylhexyl acrylate; acrylate, (meth)acrylic acid ester monomers such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, cyclohexyl methacrylate, etc.; (meth)acrylamide monomers such as acrylamide, methacrylamide, etc.; (meth)acrylonitrile monomers such as acrylonitrile, methacrylonitrile, etc.; fluorine-containing (meth)acrylic acid ester monomers such as 2-(perfluorohexyl)ethyl methacrylate, 2-(perfluorobutyl)ethyl acrylate, etc.; maleimide; maleimide derivatives such as phenylmaleimide, etc. These may be used alone or in combination of two or more kinds in any ratio. In the present invention, (meth)acrylic means acrylic and / or methacrylic, and (meth)acrylonitrile means acrylonitrile and / or methacrylonitrile.

[0026] Among these monomers, as the monomer used for preparing the polymer constituting the core part, from the viewpoint of more firmly adhering the substrate with the porous membrane layer and the adherend member through the adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer, it is preferable to use at least one of aromatic vinyl monomer and (meth)acrylic acid ester monomer, and it is more preferable to use both aromatic vinyl monomer and (meth)acrylic acid ester monomer. That is, the polymer of the core part preferably contains at least one of aromatic vinyl monomer unit and (meth)acrylic acid ester monomer unit, and it is more preferable to contain both aromatic vinyl monomer unit and (meth)acrylic acid ester monomer unit. In the present invention, "containing a monomer unit" means that "a polymer obtained by using the monomer contains a repeating unit derived from the monomer".

[0027] From the viewpoint of further firmly adhering the substrate with a porous membrane layer and the adherend member via the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, the proportion of aromatic vinyl monomer units in the polymer constituting the core portion is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 75% by mass or more, preferably 95% by mass or less, and more preferably 90% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the core portion. In addition, from the viewpoint of more firmly adhering the substrate with a porous membrane layer and the adherend member via the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, the proportion of (meth)acrylic acid ester monomer units in the polymer constituting the core portion is preferably 2% by mass or more, more preferably 3% by mass or more, and even more preferably 4% by mass or more, preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the core portion. In the present invention, the "content ratio of each monomer unit" is 1 It can be measured using nuclear magnetic resonance (NMR) techniques such as H-NMR.

[0028] The polymer constituting the core portion may contain an acid group-containing monomer unit. Examples of the acid group-containing monomer capable of forming the acid group-containing monomer unit include a monomer having an acid group, such as a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, or a monomer having a phosphoric acid group.

[0029] Examples of the monomer having a carboxylic acid group include monocarboxylic acid and dicarboxylic acid. Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid. Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. Furthermore, examples of monomers having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In the present invention, (meth)allyl means allyl and / or methallyl, and (meth)acryloyl means acryloyl and / or methacryloyl. Among these, as the acid group-containing monomer, a monomer having a carboxylic acid group is preferable, among which a monocarboxylic acid is more preferable, and (meth)acrylic acid is further preferable. The acid group-containing monomer may be used alone or in combination of two or more kinds in any ratio.

[0030] The proportion of the acid group-containing unit in the polymer constituting the core part is preferably 0.1% by mass or more, more preferably 1% by mass or more, and preferably 15% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the core part. By keeping the proportion of the acid group-containing unit within the above range, the dispersibility of the polymer constituting the core part can be increased during preparation of the organic particles, and a shell part that partially covers the outer surface of the core part can be easily formed relative to the outer surface of the polymer constituting the core part.

[0031] The polymer constituting the core portion may contain a hydroxyl group-containing monomer unit. Examples of hydroxyl-containing monomers capable of forming hydroxyl-containing monomer units include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, etc. These may be used alone or in combination of two or more at any ratio. The ratio of the hydroxyl group-containing monomer units in the polymer constituting the core portion is preferably 0.1% by mass or more, more preferably 1% by mass or more, and preferably 15% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the core portion. By keeping the ratio of the hydroxyl group-containing monomer units within the above range, the dispersibility of the polymer constituting the core portion can be increased during preparation of the organic particles, and a shell portion that at least partially covers the outer surface of the core portion can be easily formed relative to the outer surface of the polymer constituting the core portion.

[0032] In addition, the polymer constituting the core part preferably contains a crosslinkable monomer unit in addition to the above-mentioned monomer unit. Here, the crosslinkable monomer capable of forming the crosslinkable monomer unit is a monomer capable of forming a crosslinked structure during or after polymerization by heating or irradiation with energy rays. By including the crosslinkable monomer unit in the polymer constituting the core part, the degree of swelling of the organic particles in an electrolyte can be easily kept within a suitable range.

[0033] Examples of the crosslinkable monomer include polyfunctional monomers having two or more polymerization reactive groups in the crosslinkable monomer. Examples of such polyfunctional monomers include divinyl monomers such as divinylbenzene, 1,3-butadiene, isoprene, and allyl methacrylate; di(meth)acrylic acid ester monomers such as ethylene dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester monomers such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate; and γ-methacryloxypropyltrimethoxysilane. Among these, di(meth)acrylic acid ester monomers are more preferable from the viewpoint of easily controlling the swelling degree of the organic particles in the electrolyte. In addition, these may be used alone or in combination of two or more at any ratio.

[0034] In addition, the ratio of the crosslinkable monomer unit in the polymer constituting the core part is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.5% by mass or more, and preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the core part. By keeping the ratio of the crosslinkable monomer unit within the above range, the porous membrane layer-attached substrate and the adherend are more firmly bonded via the adhesive layer formed on the porous membrane layer of the porous membrane layer-attached substrate, while controlling the electrolyte swelling degree of the organic particles, thereby further improving the low-temperature output characteristics of the secondary battery.

[0035] <<Shell section>> [Electrolyte swelling rate] In addition, the electrolyte swelling degree of the shell part is preferably more than 1, more preferably 1.1 times or more, even more preferably 1.3 times or more, preferably 4 times or less, more preferably 3.5 times or less, and even more preferably 3.0 times or less. If the electrolyte swelling degree of the shell part is within the above range, the adhesive strength of the adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer can be suppressed from decreasing in the electrolyte, and the high-temperature cycle characteristics of the secondary battery can be suppressed from decreasing. In addition, if the electrolyte swelling degree of the polymer constituting the shell part exceeds 1, the low-temperature output characteristics of the secondary battery can be further improved. The degree of swelling of the polymer constituting the shell portion in an electrolyte solution can be adjusted, for example, by changing the type and ratio of monomers used in preparing the polymer constituting the shell portion.

[0036] [Glass transition temperature (Tg)] In addition, the glass transition temperature (Tg) of the polymer constituting the shell part is preferably 10° C. or more lower than the glass transition temperature of the polymer constituting the core part described above, more preferably 30° C. or more lower, and even more preferably 50° C. or more lower, from the viewpoint of more firmly adhering the substrate with the porous membrane layer and the adherend member through the adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer. If the glass transition temperature of the polymer constituting the shell part is 10° C. or more lower than the glass transition temperature of the polymer constituting the core part, when an adhesive layer is formed on the porous membrane layer by the inkjet method using the composition for secondary battery adhesive layer of the present invention, the adhesive strength of the formed adhesive layer is suppressed from decreasing, and the secondary battery can exhibit even more excellent low-temperature strength characteristics.

[0037] [composition] Examples of the monomers used to prepare the polymer constituting the shell include the same monomers as those exemplified as the monomers that can be used to produce the polymer constituting the core. Such monomers may be used alone or in combination of two or more kinds in any ratio.

[0038] Among these monomers, as the monomer used for preparing the polymer constituting the shell portion, from the viewpoint of more firmly adhering the substrate with the porous membrane layer and the adherend member through the adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer, it is preferable to use at least one of (meth)acrylic acid ester monomer and aromatic vinyl monomer, and it is more preferable to use both (meth)acrylic acid ester monomer and aromatic vinyl monomer. That is, the polymer constituting the shell portion preferably contains at least one of (meth)acrylic acid ester monomer unit and aromatic vinyl monomer unit, and it is more preferable to contain both (meth)acrylic acid ester monomer unit and aromatic vinyl monomer unit.

[0039] From the viewpoint of more firmly adhering the substrate with a porous membrane layer and the adherend member via the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, the proportion of (meth)acrylic acid ester monomer units in the polymer constituting the shell portion is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more, preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on the total repeating units (total monomer units) contained in the polymer constituting the shell portion being 100% by mass. In addition, from the viewpoint of more firmly adhering the substrate with a porous membrane layer and the adherend member via the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, the proportion of aromatic vinyl monomer units in the polymer constituting the shell portion is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, based on the total repeating units (total monomer units) contained in the polymer constituting the shell portion being 100% by mass.

[0040] The polymer constituting the shell part may contain an acid group-containing monomer unit in addition to the (meth)acrylic acid ester monomer unit and the aromatic vinyl monomer unit. Here, the acid group-containing monomer capable of forming the acid group-containing monomer unit may be a monomer having an acid group, for example, a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, and a monomer having a phosphoric acid group. Specifically, the acid group-containing monomer may be the same monomer as the acid group-containing monomer that may be used to form the core part. Among these, as the acid group-containing monomer, a monomer having a carboxylic acid group is preferable, among which a monocarboxylic acid is more preferable, and (meth)acrylic acid is further preferable. The acid group-containing monomer may be used alone or in combination of two or more kinds in any ratio.

[0041] The proportion of the acid group-containing monomer units in the polymer constituting the shell portion is preferably 0.1% by mass or more, more preferably 0.4% by mass or more, and even more preferably 0.7% by mass or more, and preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer of the shell portion. By keeping the proportion of the acid group-containing monomer units within the above range, the dispersibility of the organic particles can be improved, and the battery components can be bonded together more firmly via the adhesive layer.

[0042] Here, the polymer constituting the shell portion may contain a hydroxyl group-containing monomer unit. Examples of hydroxyl-containing monomers capable of forming the hydroxyl-containing monomer units of the polymer constituting the shell portion include the same monomers as the hydroxyl-containing monomers usable in forming the core portion. The proportion of the hydroxyl group-containing monomer units in the polymer constituting the shell portion is preferably 0.1% by mass or more, more preferably 0.4% by mass or more, even more preferably 0.7% by mass or more, preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer constituting the shell portion. By keeping the proportion of the hydroxyl group-containing monomer units within the above range, the dispersibility of the organic particles can be improved, and the substrate with the porous membrane layer and the adherend can be bonded more firmly via the adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer.

[0043] The polymer constituting the shell part may contain a crosslinkable monomer unit. Here, examples of the crosslinkable monomer capable of forming the crosslinkable monomer unit include the same monomers as those exemplified as the crosslinkable monomer usable in the polymer constituting the core part. Among these, di(meth)acrylic acid ester monomers and divinyl monomers are preferred, and allyl methacrylate is preferred. The crosslinkable monomer may be used alone or in combination of two or more types at any ratio.

[0044] The proportion of crosslinkable monomer units in the polymer constituting the shell portion is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more, with all repeating units (all monomer units) contained in the polymer of the shell portion being 100% by mass, and is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less.

[0045] <Volume average particle size of organic particles (D50)> In addition, the volume average particle diameter (D50) of the organic particles is preferably 100 nm or more, more preferably 150 nm or more, even more preferably 180 nm or more, preferably 1000 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. If the volume average particle diameter of the organic particles is the above lower limit value or more, the porous membrane layer-attached substrate and the adherend member can be more firmly adhered via the adhesive layer formed on the porous membrane layer of the porous membrane layer-attached substrate. On the other hand, if the volume average particle diameter of the organic particles is the above upper limit value or less, when the secondary battery adhesive layer composition of the present invention is discharged using the ink jet method, nozzle clogging can be further suppressed, and an adhesive layer can be more efficiently formed on the porous membrane layer. In the present invention, the "volume average particle size of the organic particles" can be measured by the method described in the Examples of this specification. The volume average particle size of the organic particles can be adjusted, for example, by changing the type and amount of a polymerization initiator and an emulsifier used in the preparation of the organic particles.

[0046] <Core-shell ratio of organic particles> Furthermore, the shell part of the organic particles preferably has an average thickness within a predetermined range relative to the volume average particle diameter (D50) of the organic particles. Specifically, the core-shell ratio of the organic particles, which is the average thickness of the shell part relative to the volume average particle diameter (D50) of the organic particles, is preferably 1.5% or more, more preferably 3% or more, even more preferably 5% or more, and is preferably 40% or less, more preferably 30% or less, even more preferably 20% or less. If the core-shell ratio of the organic particles is the above lower limit or more, the adhesive strength of the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer can be suppressed from decreasing outside the electrolyte. In addition, if the core-shell ratio of the organic particles is the above upper limit or less, the adhesive strength of the adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer can be suppressed from decreasing in the electrolyte.

[0047] In the present invention, the "average thickness of the shell portion" can be measured using the method described in the examples of this specification.

[0048] <Coverage rate of organic particles> In addition, in the organic particles, the average ratio of the outer surface of the core part covered by the shell part is defined as the coverage of the organic particles. The coverage of the organic particles is preferably 20% or more, more preferably 40% or more, and even more preferably 55% or more, and is preferably 99% or less, more preferably 97% or less, and even more preferably 95% or less. If the coverage of the organic particles is the above lower limit or more, it is possible to suppress the adhesive strength of the adhesive layer from decreasing outside the electrolyte. If the coverage of the organic particles is the above upper limit or less, it is possible to further improve the low-temperature output characteristics of the secondary battery. In the present invention, the "coverage ratio of organic particles" can be measured by the method described in the examples of this specification. The coverage ratio Rc used to determine the coverage ratio of organic particles can be calculated manually from the cross-sectional structure of the organic particles, but can also be calculated using commercially available image analysis software. For example, "AnalySIS Pro" (manufactured by Olympus Corporation) can be used as the commercially available image analysis software.

[0049] <<How to prepare organic particles>> The organic particles having the above-mentioned core-shell structure can be prepared, for example, by using a monomer of a polymer constituting the core part and a monomer of a polymer constituting the shell part and polymerizing them stepwise while changing the ratio of the monomers over time. Specifically, the organic particles can be prepared by a continuous multi-stage emulsion polymerization method and a multi-stage suspension polymerization method in which the polymer of the previous stage is successively coated with the polymer of the later stage.

[0050] An example of obtaining organic particles having the above-mentioned core-shell structure by a multi-stage emulsion polymerization method will be described below.

[0051] In the polymerization, an anionic surfactant such as sodium dodecylbenzenesulfonate or sodium dodecylsulfate, a nonionic surfactant such as polyoxyethylene nonylphenyl ether or sorbitan monolaurate, or a cationic surfactant such as octadecylamine acetate can be used as an emulsifier in accordance with a conventional method. In addition, a peroxide such as t-butylperoxy-2-ethylhexanoate, potassium persulfate, or cumene peroxide, or an azo compound such as 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] or 2,2'-azobis(2-amidinopropane) hydrochloride can be used as a polymerization initiator.

[0052] The polymerization procedure is as follows: first, a monomer for forming the core portion and an emulsifier are mixed and emulsion-polymerized all at once to obtain a particulate polymer for forming the core portion. Then, a monomer for forming the shell portion is polymerized in the presence of the particulate polymer for forming the core portion to obtain organic particles having the above-mentioned core-shell structure.

[0053] In this case, when preparing organic particles in which the outer surface of the core part is at least partially covered with the shell part, it is preferable to feed the monomer forming the polymer constituting the shell part to the polymerization system in a divided manner or continuously. By feeding the monomer forming the polymer of the shell part to the polymerization system in a divided manner or continuously, the polymer constituting the shell part is formed in a particulate form, and this particle is bonded to the core part to form a shell part that at least partially covers the core part.

[0054] <Thixotropic agent> The thixotropic agent contained in the secondary battery adhesive layer composition is a component that imparts viscosity to the secondary battery adhesive layer composition. Furthermore, since the thixotropic agent has adhesiveness and electrolyte resistance, it can play a role in supporting adhesion between the components in the secondary battery adhesive layer composition and between battery members in the secondary battery.

[0055] The thixotropic agent may include, for example, a natural polymer, a semi-synthetic polymer, and a synthetic polymer.

[0056] [Natural polymer] Examples of natural polymers include polysaccharides and proteins derived from plants or animals, as well as fermentation products of these with microorganisms and heat treatment products of these. These natural polymers can be classified into plant-derived natural polymers, animal-derived natural polymers, and microbial-derived natural polymers. Examples of natural plant polymers include gum arabic, tragacanth gum, galactan, guar gum, carob gum, karaya gum, carrageenan, pectin, quince seed, alkecolloids (gasso extract), starch (derived from rice, corn, potato, wheat, etc.), and glycyrrhizin. Examples of natural animal polymers include collagen, casein, albumin, and gelatin. Examples of natural microbial polymers include xanthan gum, dextran, succinoglucan, and pullulan.

[0057] [Semi-synthetic polymer] The semi-synthetic polymer includes a cellulose-based semi-synthetic polymer, which can be classified into a nonionic cellulose-based semi-synthetic polymer, an anionic cellulose-based semi-synthetic polymer, and a cationic cellulose-based semi-synthetic polymer.

[0058] Examples of nonionic cellulose-based semi-synthetic polymers include alkyl celluloses such as methyl cellulose, methyl ethyl cellulose, ethyl cellulose, and microcrystalline cellulose; and hydroxyalkyl celluloses such as hydroxyethyl cellulose, hydroxybutyl methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose stearoxy ether, carboxymethyl hydroxyethyl cellulose, alkyl hydroxyethyl cellulose, and nonoxynyl hydroxyethyl cellulose.

[0059] Examples of anionic cellulose-based semisynthetic polymers include those obtained by substituting the above-mentioned nonionic cellulose-based semisynthetic polymers with various derivative groups and their salts (sodium salts, ammonium salts, etc.).Specific examples of such anionic cellulose-based semisynthetic polymers include sodium cellulose sulfate, methyl cellulose, methyl ethyl cellulose, ethyl cellulose, carboxymethyl cellulose (CMC), cellulose nanofiber (CNF), and their salts.

[0060] Examples of cationic cellulose-based semi-synthetic polymers include low-nitrogen hydroxyethyl cellulose dimethyldiallyl ammonium chloride (polyquaternium-4), O-[2-hydroxy-3-(trimethylammonio)propyl]hydroxyethyl cellulose chloride (polyquaternium-10), and O-[2-hydroxy-3-(lauryldimethylammonio)propyl]hydroxyethyl cellulose chloride (polyquaternium-24).

[0061] [Synthetic polymer] Examples of synthetic polymers include polyacrylates such as sodium polyacrylate, polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, copolymers of (meth)acrylic acid or acrylates and vinyl alcohol, copolymers of (meth)acrylic acid or acrylates and acrylic acid esters, fully or partially saponified products of maleic anhydride or copolymers of maleic acid or fumaric acid and vinyl acetate, modified polyvinyl alcohol, modified polyacrylic acid, polyethylene glycol, polycarboxylic acids, ethylene-vinyl alcohol copolymers, vinyl acetate polymers, and acrylamide polymers having carboxylic acid groups introduced therein.

[0062] Among these thixotropic agents, carboxymethyl cellulose and its salts, copolymers of (meth)acrylic acid or acrylates and acrylic esters, and cellulose nanofibers (CNF) are preferred, with cellulose nanofibers (CNF) being more preferred.

[0063] Here, from the viewpoint of ensuring good battery characteristics of the secondary battery, the content of the thixotropic agent in the composition for secondary battery adhesive layer is preferably 0.05 parts by mass or more, and preferably 5 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.4 parts by mass or less, per 100 parts by mass of the organic particles.

[0064] <Water> In addition, the water contained in the secondary battery adhesive layer composition functions as a solvent that dissolves or disperses each component contained in the secondary battery adhesive layer composition. The amount of water contained in the secondary battery adhesive layer composition is not particularly limited as long as it can dissolve or disperse each component in the secondary battery adhesive layer composition, but it is preferable to adjust the solid content concentration of the secondary battery adhesive layer composition to be preferably 0.5 mass% or more, more preferably 1 mass% or more, and even more preferably 3 mass% or more, and preferably 30 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less. If the solid content concentration of the secondary battery adhesive layer composition is the above lower limit value or more, the secondary battery adhesive layer composition can be applied using the inkjet method to efficiently form an adhesive layer, thereby improving the production speed of the secondary battery. In addition, if the solid content concentration of the secondary battery adhesive layer composition is the above upper limit value or less, the dischargeability of the secondary battery adhesive layer composition when applied using the inkjet method is further improved.

[0065] <Other ingredients> The other components that the secondary battery adhesive layer composition may contain, other than the organic particles having a core-shell structure, the thixotropic agent, and water, are not particularly limited. Examples of the other components include additives and other binders other than the organic particles having a core-shell structure.

[0066] <<Additives>> Here, the additives are not particularly limited, and examples thereof include surface tension modifiers, dispersants, viscosity modifiers, reinforcing materials, electrolyte additives, etc. These are not particularly limited as long as they do not affect the battery reaction, and known additives, such as those described in International Publication No. 2012 / 115096, can be used. Note that these additives may be used alone or in combination of two or more types in any ratio.

[0067] <<Other binders>> In addition, the other binder is not particularly limited as long as it is not an organic particle having a core-shell structure, and examples thereof include fluoropolymers such as polyvinylidene fluoride (PVdF) and polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymers; conjugated diene polymers such as styrene-butadiene copolymers (SBR) and acrylonitrile-butadiene copolymers (NBR); hydrogenated conjugated diene polymers; and polymers containing (meth)acrylic acid alkyl ester monomer units (acrylic polymers). These other binders may be used alone or in combination of two or more at any ratio.

[0068] Here, the glass transition temperature of the polymer constituting the other binder is preferably -60°C or higher, more preferably -40°C or higher, preferably 20°C or lower, more preferably 15°C or lower, and even more preferably 10°C or lower. If the glass transition temperature of the polymer constituting the other binder is equal to or higher than the lower limit, the low-temperature output characteristics of the secondary battery can be further improved. Also, if the glass transition temperature of the polymer constituting the other binder is equal to or lower than the upper limit, the powder-fall resistance of the adhesive layer can be improved.

[0069] In addition, the secondary battery adhesive layer composition preferably contains 1 part by mass or more of other binder per 100 parts by mass of the organic particles having the above-mentioned core-shell structure, more preferably 5 parts by mass or more, even more preferably 8 parts by mass or more, preferably 50 parts by mass or less, more preferably 35 parts by mass or less, and even more preferably 25 parts by mass or less. If the content of the other binder is equal to or more than the above lower limit, the powder-fall resistance of the adhesive layer can be further improved. If the content of the other binder is equal to or less than the above upper limit, the low-temperature output characteristics of the secondary battery can be further improved.

[0070] <Method for preparing non-aqueous secondary battery adhesive layer composition> The secondary battery adhesive layer composition of the present invention can be prepared by mixing, for example, organic particles having a core-shell structure, a thixotropic agent, water, and other components such as other optional binders. For mixing, a general stirring vessel, a ball mill, a sand mill, a bead mill, a pigment dispersing machine, an ultrasonic dispersing machine, a crushing machine, a homogenizer, a planetary mixer, a film mix, etc. can be used. The mixing conditions are not particularly limited, but the mixture can usually be mixed at room temperature to 80°C for 10 minutes to several hours.

[0071] <Properties of the composition for non-aqueous secondary battery adhesive layer> The secondary battery adhesive layer composition of the present invention is required to have specific properties from the standpoints of adhesion and resistance.

[0072] <<Viscosity>> The secondary battery adhesive layer composition of the present invention is subjected to a shear rate of 100 sec -1 The viscosity η0 at a shear rate of 100 sec must be less than 10 mPa·s, preferably 8 mPa·s or less, and more preferably 7 mPa·s or less. -1 If the viscosity η0 at is less than 10 mPa·s, nozzle clogging can be suppressed when the secondary battery adhesive layer composition is discharged from a nozzle using an inkjet method, and excellent dischargeability can be ensured.

[0073] In addition, the secondary battery adhesive layer composition of the present invention is -1 The viscosity η1 at 20°C must be 0.5 mPa·s or more and 2.4 mPa·s or less, preferably 0.6 mPa·s or more, more preferably 0.7 mPa·s or more, and preferably 2.0 mPa·s or less, and more preferably 1.5 mPa·s or less. Shear rate of secondary battery adhesive layer composition: 10,000 sec -1 When the viscosity η1 at 1000° C. is 0.5 mPa·s or more, when an adhesive layer is formed on a porous membrane layer by an ink-jet method using the composition for secondary battery adhesive layer of the present invention, the substrate with the porous membrane layer and the adherend can be firmly adhered via the formed adhesive layer, and an increase in the resistance of the secondary battery can be suppressed. In addition, the shear rate of the secondary battery adhesive layer composition was 10,000 sec -1 If the viscosity η1 at 2.4 mPa·s or less, nozzle clogging can be further suppressed when the secondary battery adhesive layer composition is ejected from a nozzle using an inkjet method, and better ejection properties can be ensured.

[0074] Furthermore, the composition for secondary battery adhesive layers of the present invention must have a ratio of viscosity η0 to viscosity η1 (η0 / η1) of 1.2 or more and 10 or less, preferably 1.6 or more, more preferably 2 or more, preferably 9 or less, and preferably 8 or less. When the ratio of viscosity η0 to viscosity η1 (η0 / η1) is equal to or greater than the lower limit, when an adhesive layer is formed on a porous membrane layer by an inkjet method using the composition for secondary battery adhesive layer of the present invention, the substrate with the porous membrane layer and the adherend can be firmly adhered via the formed adhesive layer, and an increase in the battery resistance of the secondary battery can be suppressed. Furthermore, if the ratio of viscosity η0 to viscosity η1 (η0 / η1) is equal to or less than the above upper limit, nozzle clogging can be further suppressed when ejecting the secondary battery adhesive layer composition from a nozzle using an inkjet method, ensuring even better ejection properties.

[0075] In addition, the shear rate is 100 sec -1Viscosity η0 at shear rate of 10000sec -1 The viscosity η1 at can be measured by the method described in the Examples of this specification.

[0076] In addition, the viscosity η0, the viscosity η1, and the ratio of the viscosity η0 to the viscosity η1 (η0 / η1) can be appropriately adjusted by adjusting the content of the organic particles and the thixotropic agent in the secondary battery contact layer composition, the solids concentration of the secondary battery adhesive layer composition, and the composition of the thixotropic agent, etc.

[0077] <<Surface tension>> The surface tension of the secondary battery adhesive layer composition is preferably 30 mN / m or more, more preferably 36 mN / m or more, even more preferably 42 mN / m or more, preferably 60 mN / m or less, more preferably 56 mN / m or less, and even more preferably 53 mN / m or less. If the surface tension of the secondary battery adhesive layer composition is the above lower limit or more, when an adhesive layer is formed on the porous membrane layer of the substrate with a porous membrane layer by the inkjet method, the substrate with a porous membrane layer and the adherend member can be more firmly adhered via the formed adhesive layer, and the increase in the battery resistance of the secondary battery can be further suppressed. In addition, if the surface tension of the secondary battery adhesive layer composition is the above upper limit or less, when the inkjet method is used, the droplets of the secondary battery adhesive layer composition discharged from the nozzle are stable, so that the variation in discharge can be suppressed and the dischargeability can be further improved.

[0078] (Battery materials for non-aqueous secondary batteries) The battery member for a non-aqueous secondary battery of the present invention (hereinafter sometimes abbreviated as "battery member for secondary battery" or "battery member") is a battery member with a porous membrane layer, which comprises a substrate with a porous membrane layer formed on at least one surface of the substrate, and a plurality of dot-shaped adhesive layers formed on the porous membrane layer. The substrate with a porous membrane layer is a separator substrate or an electrode substrate, and the adhesive layer is a dried product of the above-mentioned composition for secondary battery adhesive layer of the present invention. The battery member for a secondary battery of the present invention can be firmly bonded to an adherend member via the adhesive layer formed on the porous membrane layer, and can cause the secondary battery to exhibit excellent low-temperature output characteristics. The secondary battery member of the present invention can be used as a separator for a secondary battery when the substrate is a separator substrate, and can be used as an electrode for a secondary battery when the substrate is an electrode substrate.

[0079] <Substrate with porous membrane layer> The substrate with a porous membrane layer provided in the secondary battery member of the present invention is, as described above, a substrate having a porous membrane layer formed on at least one side thereof. Here, the porous membrane layer is a layer of a porous membrane formed on a separator substrate or an electrode substrate, and is intended to improve heat resistance, strength, etc. The porous membrane layer usually contains non-conductive inorganic particles, a binder for the porous membrane layer, and an optional additive, and can be formed on a separator substrate or an electrode substrate by, for example, a method described later.

[0080] <<Properties of the porous membrane layer>> [Surface roughness Ra] Here, the porous membrane layer usually has a surface roughness Ra of 0.1 μm or more and 5.0 μm or less. The surface roughness Ra of the porous membrane layer is preferably 0.15 μm or more, more preferably 0.2 μm or more, preferably 1.0 μm or less, and more preferably 0.6 μm or less. If the surface roughness Ra of the porous membrane layer is 0.1 μm or more, the contact area between the porous membrane layer and the adhesive layer formed on the porous membrane layer is increased, and in addition, the adhesion between the porous membrane layer and the adhesive layer can be increased via the adhesive layer formed on the porous membrane layer between the substrate with the porous membrane layer and the adherend. As a result, even when the secondary battery produced is repeatedly charged and discharged, good adhesion between the battery components can be maintained, and the expansion of the secondary battery can be suppressed. In addition, if the surface roughness Ra of the porous membrane layer is 5.0 μm or less, the organic particles contained in the adhesive layer formed on the porous membrane layer can be prevented from penetrating into the unevenness of the porous membrane layer surface. As a result, the adhesiveness of the organic particles can be fully exerted, and the adhesiveness between the substrate with the porous membrane layer and the adherend member via the adhesive layer can be enhanced. In addition, since the organic particles can be prevented from penetrating into the porous membrane layer and filling the voids in the porous membrane layer, the increase in the battery resistance of the secondary battery produced can be suppressed, and the secondary battery can exhibit good output characteristics.

[0081] <<Separator substrate and electrode substrate>> The separator substrate is not particularly limited, and any known separator substrate that can be used in the field of secondary batteries can be used. As the electrode substrate, an electrode substrate in which an electrode mixture layer is formed on a current collector is usually used. The current collector may be made of a metal material such as iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, or platinum. Among these, the current collector for the negative electrode is preferably made of copper. The current collector for the positive electrode is preferably made of aluminum. In addition, a layer containing an electrode active material and a binder (binder for electrode mixture layer) can be used as the electrode mixture layer. Specifically, the electrode mixture layer is not particularly limited, and for example, the electrode mixture layer described in JP 2013-145763 A can be used. Furthermore, a known method can be used to form the electrode mixture layer on the current collector.

[0082] <Adhesive layer> The adhesive layer of the battery member for secondary batteries of the present invention is a dried product of the above-mentioned composition for secondary battery adhesive layer of the present invention.The adhesive layer is formed in a dot shape on the porous membrane layer of the substrate with the porous membrane layer of the battery member.The dot-shaped adhesive layer is formed, for example, by ejecting the composition for secondary battery adhesive layer from a nozzle using an inkjet method.

[0083] Here, the dot-shaped adhesive layer may be formed uniformly over the entire surface of the surface of the porous membrane layer of the substrate with the porous membrane layer on which the adhesive layer is formed (hereinafter referred to as the "formation surface"), or a plurality of dot-shaped adhesive layers may be arranged in a predetermined pattern such as a stripe pattern, a dot pattern, or a lattice pattern in plan view. Among these, from the viewpoint of improving the electrolyte injection property when manufacturing a secondary battery using the battery member of the present invention, it is preferable that the dot-shaped adhesive layer is arranged in a stripe pattern. The cross-sectional shape of the adhesive layer is not particularly limited and may be a convex shape, a concave shape, or a concave shape, and among them, from the viewpoint of more firmly adhering the battery member for a secondary battery to the adherend member via the adhesive layer, a concave shape is preferable. Note that the cross-sectional shape of the adhesive layer can be changed, for example, by adjusting the drying conditions when forming the adhesive layer using the composition for secondary battery adhesive layer of the present invention.

[0084] The amount of the adhesive layer formed was 0.01 g / m 2 More than 10g / m 2 It is preferable that the content is 0.03 g / m or less. 2 More than 5g / m 2 More preferably, it is 0.05 g / m or less. 2 More than 0.5g / m 2 It is particularly preferable that the amount of the adhesive layer formed is 0.01 g / m or less. 2 If the amount of the adhesive layer formed is 10 g / m or more, the secondary battery member and the adherend member can be more firmly adhered to each other via the adhesive layer. 2If the temperature is equal to or lower than this, an increase in the battery resistance of the manufactured secondary battery can be suppressed, and the secondary battery can exhibit good output characteristics. In the present invention, the "amount of adhesive layer" refers to the amount of secondary battery adhesive layer composition required to form an adhesive layer per unit area of ​​the formation surface. The amount of adhesive layer can be calculated by dividing the mass of secondary battery adhesive layer composition required for the adhesive layer formed on the formation surface by the area of ​​the formation surface on which the adhesive layer is formed.

[0085] Here, when the dot-shaped adhesive layer is formed in two or more places on the formation surface, the size of one dot formed on the formation surface (hereinafter referred to as "formation area") is 25 μm 2 It is preferable that the thickness is 50 μm or more. 2 More preferably, it is 100 μm or more. 2 More preferably, it is 250,000 μm or more. 2 It is preferable that the thickness is less than 200,000 μm. 2 More preferably, it is 100,000 μm or less. 2 It is more preferable that the size of one dot is 25 μm or less. 2 If the size of each dot is 250,000 μm or more, the battery member for a secondary battery and the member to be bonded can be bonded more firmly via the adhesive layer. 2 If the above ratio is less than 1, the battery member for a secondary battery can be efficiently manufactured. The above-mentioned formation area can be adjusted by changing the amount, shape and range of the secondary battery adhesive layer composition of the present invention supplied to the formation surface. Specifically, for example, when forming an adhesive layer by an inkjet method using the secondary battery adhesive layer composition of the present invention, the formation area can be adjusted by changing the gradation of the discharge of the secondary battery adhesive layer composition from the nozzle of the inkjet head (the number of times discharged to the same point).

[0086] (Method of manufacturing battery components for non-aqueous secondary batteries) The method for producing a non-aqueous secondary battery member of the present invention (hereinafter sometimes abbreviated as "method for producing a secondary battery member") is a method for producing the above-mentioned secondary battery member of the present invention. Specifically, the method for producing a secondary battery member of the present invention includes a coating step of coating the composition for secondary battery adhesive layer of the present invention on the porous membrane layer of a substrate with a porous membrane layer formed on at least one surface of the substrate by an inkjet method, and a drying step of drying the composition for secondary battery adhesive layer coated on the porous membrane layer to form an adhesive layer. In addition, the method for producing a secondary battery member of the present invention may optionally include a substrate with a porous membrane layer production step of producing a substrate with a porous membrane layer before the coating step.

[0087] <Process for producing substrate with porous membrane layer> In the step of preparing a substrate with a porous membrane layer, a porous membrane layer is formed on at least one side of a substrate to prepare a substrate with a porous membrane layer. The substrate with a porous membrane layer can be obtained, for example, by applying a composition for a porous membrane layer to a substrate such as a separator substrate or an electrode substrate, and drying the applied composition for a porous membrane layer.

[0088] [Composition for porous membrane layer] Here, the composition for the porous membrane layer usually contains non-conductive inorganic particles, a polymer for the porous membrane layer, and a solvent such as an organic solvent and water, and may optionally contain other components.

[0089] -Non-conductive inorganic particles- As the non-conductive inorganic particles contained in the composition for the porous membrane layer, particles made of an inorganic material that is stable in the usage environment of the secondary battery and is electrochemically stable are preferred, and particles made of an inorganic compound are more preferred. From this viewpoint, preferred examples of non-conductive inorganic particles include inorganic oxide particles such as aluminum oxide (alumina), aluminum oxide hydrate (boehmite (AlOOH), gibbsite (Al(OH)3), silicon oxide, magnesium oxide (magnesia), magnesium hydroxide, calcium oxide, titanium oxide (titania), barium titanate (BaTiO3), ZrO, and alumina-silica composite oxide; nitride particles such as aluminum nitride and boron nitride; covalent crystal particles such as silicon and diamond; sparingly soluble ion crystal particles such as barium sulfate, calcium fluoride, and barium fluoride; and clay particles such as talc and montmorillonite. Among these, from the viewpoint of favorably adsorbing the polymer for the porous membrane layer and suppressing an increase in the internal resistance of the battery component having the porous membrane layer, inorganic oxide particles are preferred as the non-conductive inorganic particles, and alumina particles, boehmite particles, and titanium oxide particles are more preferred. In addition, these particles may be subjected to element substitution, surface treatment, solid solution treatment, etc., as necessary. In addition, these particles may be used alone or in combination of two or more kinds.

[0090] -density- Here, the density of the non-conductive inorganic particles is 3.0 g / cm 3 It is preferable that the content is 3.5 g / cm or more. 3 More preferably, it is 6.0 g / cm or more. 3 It is preferable that the density is 5.0 g / cm or less. 3 It is more preferable that the density of the non-conductive inorganic particles is equal to or higher than the lower limit. If the density of the non-conductive inorganic particles is equal to or lower than the upper limit, the density of the porous membrane layer can be sufficiently increased. Also, if the density of the non-conductive inorganic particles is equal to or lower than the upper limit, the low-temperature output characteristics of the secondary battery including the battery member having the porous membrane layer can be further improved. In the present invention, the "density of the non-conductive inorganic particles" refers to the true density measured at a temperature of 25°C using a gas phase displacement method.

[0091] -Volume average particle size- In addition, the volume average particle diameter of the non-conductive inorganic particles is preferably 0.1 μm or more, more preferably 0.2 μm or more, preferably 1.0 μm or less, and more preferably 0.8 μm or less. If the volume average particle diameter of the non-conductive inorganic particles is the above lower limit or more, the Gurley value of the porous membrane layer is prevented from increasing (i.e., the ion conductivity is reduced) and the low-temperature output characteristics of the secondary battery including the battery member having the porous membrane layer can be further improved. In addition, if the volume average particle diameter of the non-conductive inorganic particles is the above upper limit or less, when an electrode base material is used as a base material, the polymer for the porous membrane layer can be well adsorbed to the non-conductive inorganic particles, and the polymer for the porous membrane layer can be prevented from penetrating (seeping into) the electrode mixture layer during the formation of the porous membrane layer. In the present invention, the "volume average particle size of the non-conductive inorganic particles" refers to the particle size (D50) at which the cumulative volume calculated from the small diameter side is 50% in the particle size distribution (volume basis) measured by a laser diffraction method in accordance with JIS Z8825.

[0092] -Polymer for porous membrane layers- The polymer for the porous membrane layer contained in the composition for the porous membrane layer holds the components contained in the porous membrane layer so that they do not detach from the porous membrane layer. Here, for example, the polymer described in JP 2017-084589 A can be suitably used as the polymer for the porous membrane layer. In addition, the polymer for the porous membrane layer can be prepared by referring to the preparation method of the polymer described in the publication.

[0093] [Amount] The amount of the polymer for the porous membrane layer contained in the composition for the porous membrane layer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and more preferably 2.5 parts by mass or less per 100 parts by mass of non-conductive inorganic particles. If the content of the polymer for the porous membrane layer is within the above range, the viscosity of the composition for the porous membrane layer can be made moderate, and the dispersibility and coatability of the composition for the porous membrane layer can be further improved. In addition, if the content of the polymer for the porous membrane layer is equal to or more than the above lower limit, the powder-fall resistance of the porous membrane layer can be sufficiently improved. Furthermore, if the content of the polymer for the porous membrane layer is equal to or less than the above upper limit, when the electrode base material is used as the base material, the internal resistance of the battery member can be suppressed from increasing, and the low-temperature output characteristics of the secondary battery can be sufficiently improved.

[0094] - Organic solvents - The organic solvent contained in the composition for the porous membrane layer is not particularly limited, and examples thereof include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, and amyl alcohol, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, dioxane, and tetrahydrofuran, amide polar organic solvents such as N,N-dimethylformamide and N-methylpyrrolidone (NMP), and aromatic hydrocarbons such as toluene, xylene, chlorobenzene, orthodichlorobenzene, and paradichlorobenzene. These may be used alone or in combination of two or more. Among these, acetone and NMP are preferable as the organic solvent, and NMP is more preferable.

[0095] -Other ingredients- Furthermore, the composition for porous membrane layer may contain any other components other than the above-mentioned components. The other components are not particularly limited as long as they do not affect the battery reaction, and known ones can be used. In addition, these other components may be used alone or in combination of two or more. Examples of the other components include the above-mentioned additives that can be contained in the secondary battery adhesive layer composition of the present invention.

[0096] [Method of preparing composition for porous membrane layer] The method for preparing the composition for porous membrane layer is not particularly limited, but usually, the above-mentioned non-conductive inorganic particles, the polymer for porous membrane layer, organic solvent, and other components that are used as required are mixed to prepare the composition for porous membrane layer.The mixing method is not particularly limited, but in order to efficiently disperse and mix each component, usually, a dispersing machine is used as a mixing device to perform mixing. In addition, when preparing a composition for a porous membrane layer using a polymer prepared in water by an emulsion polymerization method or the like, the water used in preparing the polymer for a porous membrane layer may be removed before mixing with an organic solvent, or the water may be removed by evaporating the water after mixing an aqueous dispersion of the polymer for a porous membrane layer with an organic solvent.

[0097] <<Coating of the composition for the porous membrane layer>> The method for applying the above-mentioned composition for the porous membrane layer onto the substrate of the separator substrate or the electrode substrate is not particularly limited, and for example, a doctor blade method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, etc. can be used.

[0098] <<Drying of the composition for the porous membrane layer>> Furthermore, the method for drying the composition for porous membrane layer applied on the substrate is not particularly limited, and a known method can be used.Specifically, the drying method can be, for example, a drying method using warm air, hot air, or low humidity air, a vacuum drying method, or a drying method using infrared rays or electron beams.The drying conditions are not particularly limited, but the drying temperature is preferably 50 to 150°C, and the drying time is preferably 5 to 30 minutes.

[0099] [Thickness of porous membrane layer] The thickness of the porous membrane layer formed by drying the composition for the porous membrane layer is not particularly limited, but is preferably 0.3 μm or more and 10 μm or less. If the thickness of the porous membrane layer is 0.3 μm or more, the heat resistance and strength of the porous membrane layer can be further improved. In addition, if the thickness of the porous membrane layer is 10 μm or less, the secondary battery can exhibit excellent rate characteristics.

[0100] <Coating process> In the manufacturing method of the battery member for a secondary battery of the present invention, for example, the composition for a secondary battery adhesive layer of the present invention is applied by an inkjet method onto the porous membrane layer of the substrate with the porous membrane layer obtained as described above. The conditions for inkjet printing, etc. are not particularly limited as long as the secondary battery adhesive layer composition can be applied, and may be appropriately adjusted depending on the desired properties of the resulting adhesive layer (amount formed, area formed, etc.); however, it is preferable that the secondary battery adhesive layer composition can be applied in the form of dots.

[0101] <Drying process> In the method for producing a battery member for a secondary battery of the present invention, the composition for a secondary battery adhesive layer applied on the porous membrane layer is dried in the drying step, whereby a plurality of adhesive layers, for example in the form of dots, are formed on the porous membrane layer base material.

[0102] The drying of the secondary battery adhesive layer composition is not particularly limited, and can be performed using a heating device such as a heater, a dryer, or a heat roller. The temperature during drying of the porous membrane layer coated with the secondary battery adhesive layer composition is not particularly limited, but is preferably 0°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, preferably 200°C or lower, more preferably 150°C or lower, and even more preferably 100°C or lower. If the drying temperature is 0°C or higher, the drying speed can be sufficiently increased to efficiently manufacture the battery member for the secondary battery. In addition, if the drying temperature is 200°C or lower, the shape of the adhesive layer obtained after drying can be made good, and the battery member provided with the porous membrane layer can be well bonded to other battery members.

[0103] (Method of manufacturing laminate for non-aqueous secondary battery) The method for producing a laminate for a non-aqueous secondary battery of the present invention includes a coating step of coating the above-mentioned secondary battery adhesive layer composition of the present invention on a porous membrane layer of a substrate with a porous membrane layer formed on at least one surface of the substrate by an inkjet method, a drying step of drying the secondary battery adhesive layer composition coated on the porous membrane layer to form an adhesive layer, and an adhesion step of adhering the substrate with the porous membrane layer to an adherend via the adhesive layer, wherein the substrate is a separator substrate or an electrode substrate.

[0104] <Coating process> In the coating step, the above-mentioned secondary battery adhesive layer composition of the present invention is coated on the porous membrane layer of the substrate having a porous membrane layer formed on at least one surface of the substrate by an inkjet method. The substrate with a porous membrane layer is not particularly limited, and the substrate with a porous membrane layer listed in the section "Battery member for secondary battery" can be used. The conditions for inkjet printing, etc. can be the conditions listed in the section "Manufacturing method for battery member for secondary battery". Furthermore, the separator substrate or electrode substrate as the substrate can be the separator substrate or electrode substrate listed in the section "Battery member for secondary battery".

[0105] <Drying process> Then, in the drying step, the secondary battery adhesive layer composition coated on the porous membrane layer is dried to form an adhesive layer. The drying method and drying time of the secondary battery adhesive layer composition are not particularly limited, and can be adopted from the drying method and drying time mentioned in the section "Method of manufacturing battery member for secondary battery".

[0106] <Adhesion process> Furthermore, in the bonding step, the substrate with the porous membrane layer and the bonded member are bonded via an adhesive layer formed on the porous membrane layer of the substrate with the porous membrane layer. Here, the bonding method is not particularly limited, and can be performed, for example, by pressing the substrate with the porous membrane layer and the bonded member that are superimposed via the adhesive layer. In this case, if the substrate with the porous membrane layer is a separator substrate with a porous membrane layer, an electrode (positive electrode or negative electrode) can be used as the bonded member.

[0107] (Method of manufacturing non-aqueous secondary battery) The manufacturing method of the non-aqueous secondary battery of the present invention is characterized by using a non-aqueous secondary battery laminate manufactured by the manufacturing method of the non-aqueous secondary battery laminate described above. Specifically, the non-aqueous secondary battery obtained by the manufacturing method of the present invention includes, for example, a positive electrode, a negative electrode, a separator, and an electrolyte, and the positive electrode and the separator, and / or the negative electrode and the separator are bonded via an adhesive layer formed on the porous membrane layer by an inkjet method. The non-aqueous secondary battery of the present invention uses the above-mentioned non-aqueous secondary battery laminate as the positive electrode and the separator bonded via an adhesive layer on the porous membrane layer, and / or the negative electrode and the separator bonded via an adhesive layer on the porous membrane layer. The non-aqueous secondary battery of the present invention has excellent low-temperature output characteristics because the separator and the electrode (positive electrode or negative electrode) are firmly bonded via the adhesive layer formed on the porous membrane layer by using the non-aqueous secondary battery adhesive layer composition of the present invention.

[0108] In addition, in the case of using a positive electrode, a negative electrode, a separator, etc. in addition to the laminate for non-aqueous secondary batteries described above in the non-aqueous secondary battery (for example, when forming a secondary battery using a laminate formed by bonding a positive electrode substrate and a separator substrate via a porous membrane layer, and a negative electrode), the positive electrode, the negative electrode, and the separator can be a known positive electrode, a negative electrode, and a separator used in non-aqueous secondary batteries. In addition, the electrolyte can be a known electrolyte used in non-aqueous secondary batteries.

[0109] Also, as the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. For example, when the secondary battery is a lithium ion secondary battery, a lithium salt can be used as the supporting electrolyte. Examples of the lithium salt include LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. Among them, LiPF6, LiClO4, and CF3SO3Li are preferred, and LiPF6 is particularly preferred, since they are easily dissolved in a solvent and show a high degree of dissociation. Note that one type of electrolyte may be used alone, or two or more types may be used in combination at any ratio. Usually, the lithium ion conductivity tends to be higher as the supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0110] Furthermore, the organic solvent used in the electrolytic solution is not particularly limited as long as it can dissolve the supporting electrolyte, but for example, when the secondary battery is a lithium ion secondary battery, the organic solvent is preferably carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), etc.; esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as sulfolane and dimethyl sulfoxide; etc. Also, a mixture of these organic solvents may be used. Among them, it is preferable to use carbonates because they have a high dielectric constant and a wide stable potential range.

[0111] The method for producing the nonaqueous secondary battery of the present invention can be, for example, by stacking a nonaqueous secondary battery laminate produced by the above-mentioned production of a nonaqueous secondary battery laminate of the present invention, or a laminate of a nonaqueous secondary battery laminate and a positive electrode, a negative electrode, a separator, and the like other than the nonaqueous secondary battery laminate, rolling or folding the nonaqueous secondary battery laminate as necessary according to the shape of the battery, placing the laminate in a battery container, injecting an electrolyte into the battery container, and sealing the battery container. In addition, the secondary battery of the present invention may be provided with an overcurrent protection element such as a fuse or a PTC element, an expanded metal, a lead plate, etc., as necessary, in order to prevent an internal pressure rise, overcharging and overdischarging, etc. The shape of the secondary battery may be any type, such as a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc. EXAMPLES

[0112] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In addition, in a polymer produced by copolymerizing multiple types of monomers, the ratio of monomer units formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of that certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified.

[0113] In the examples and comparative examples, the electrolyte swelling degree of the polymers constituting the organic particles (core polymer, shell polymer), the glass transition temperature (Tg) of each polymer constituting the organic particles (core polymer, shell polymer) and other binders, the volume average particle diameter (D50) of the organic particles, the core-shell ratio, the coverage, the viscosity of the secondary battery adhesive layer composition, the surface tension, the dischargeability (nozzle clogging suppression), the adhesive strength A (dry adhesive strength between the separator and the electrode), the adhesive strength B (dry adhesive strength between the separator with the porous membrane layer and the electrode), and the low-temperature output characteristics of the secondary battery were measured and evaluated by the following methods.

[0114] <Electrolyte swelling rate> Using the monomers and various additives used in forming the core and shell parts of the organic particles, aqueous dispersions containing the polymers of the core and shell parts were prepared under the same polymerization conditions as those of the core and shell parts. The aqueous dispersions were placed in a polytetrafluoroethylene petri dish and dried at 25°C for 48 hours, and the powder obtained by drying was hot pressed at 200°C to obtain a film with a thickness of 0.5 mm. The obtained film was cut into 1 cm squares to obtain test pieces, and the weight W2 (g) of the test pieces was measured. Next, the test pieces were immersed in an electrolyte at 60°C for 72 hours. Thereafter, the test pieces were taken out of the electrolyte, the electrolyte on the surface was wiped off, and the weight W3 (g) of the test pieces was measured. Then, the electrolyte swelling degree (times) was calculated according to the following formula. Electrolyte swelling rate (times) = W3 / W2 The electrolyte used for the measurements was a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and vinylene carbonate (VC) in a volume ratio of EC / DEC / VC = 68.5 / 30 / 1.5, in which LiPF6 was dissolved as a supporting electrolyte at a concentration of 1 mol / L.

[0115] <Glass transition temperature (Tg)> Using the monomers and various additives used to form the core and shell parts of the organic particles, aqueous dispersions containing polymers (polymers for the core part and polymers for the shell part) were prepared under the same polymerization conditions as those for the core and shell parts, and were dried to obtain measurement sample (1). In addition, aqueous dispersions containing other binders were prepared and dried to obtain measurement sample (2). 10 mg of each measurement sample was weighed into an aluminum pan, and measurements were performed using a differential thermal analysis measuring device (SII NanoTechnology's "EXSTAR DSC6220") under the conditions specified in JIS Z 8703, with an empty aluminum pan as a reference, at a measurement temperature range of -100°C to 500°C, at a heating rate of 10°C / min, and a differential scanning calorimetry (DSC) curve was obtained. During this heating process, the glass transition temperature (°C) was determined as the intersection point between the baseline just before the endothermic peak of the DSC curve where the differential signal (DDSC) was 0.05 mW / min / mg or more and the tangent to the DSC curve at the first inflection point that appeared after the endothermic peak.

[0116] <Volume average particle size of organic particles (D50)> The particle size distribution (volume basis) of an aqueous dispersion of organic particles adjusted to a solid content concentration of 0.1% by mass was measured using a laser diffraction particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name "LS-230") The particle size at which the cumulative volume calculated from the small diameter side in the measured particle size distribution is 50% was defined as the volume average particle size (D50).

[0117] <Core-shell ratio of organic particles> The core-shell ratio of the organic particles was measured by the following procedure. The prepared organic particles were thoroughly dispersed in a visible light curable resin ("D-800" manufactured by JEOL Ltd.) and then embedded to obtain a block piece containing the organic particles. The obtained block piece was then cut into a thin piece having a thickness of 100 nm using a microtome equipped with a diamond blade to prepare a measurement sample. The measurement sample was then stained using ruthenium tetroxide. Next, the stained measurement sample was set in a transmission electron microscope (JEM-3100F manufactured by JEOL Ltd.), and the cross-sectional structure of the organic particles was photographed at an accelerating voltage of 80 kV. The magnification of the electron microscope was set so that the cross-section of one organic particle was included in the field of view. The photographed cross-sectional structure of the organic particles was then observed, and the average thickness of the shell part of the organic particles was measured according to the configuration of the shell part observed, using the following procedure. <<Measurement of the average thickness of the shell>> The average thickness of the shell part was obtained by observing the cross-sectional structure of the organic particles using a transmission electron microscope (TEM). Specifically, the maximum thickness of the shell part in the cross-sectional structure of the organic particles was measured using a TEM, and the average value of the maximum thickness of the shell part of 20 or more organic particles selected at random was taken as the average thickness of the shell part. However, when the shell part is composed of polymer particles and the particles constituting the shell part do not overlap each other in the radial direction of the organic particles and the polymer particles form a single layer of the shell part, the number-average particle diameter of the particles constituting the shell part was taken as the average thickness of the shell part. The core-shell ratio of the organic particles was then obtained by dividing the measured average thickness of the shell part by the volume-average particle diameter (D50) of the organic particles.

[0118] <Coverage rate of organic particles> The coverage of the organic particles was measured by the following procedure. In the same manner as in the method for measuring the core-shell ratio of the above organic particles, the cross-sectional structure of the organic particle was photographed, and in the photographed cross-sectional structure of the organic particle, the peripheral length D1 of the core portion and the length D2 of the portion where the outer surface of the core portion and the shell portion abutted were measured, and the proportion of the outer surface of the core portion of the organic particle that was covered by the shell portion [covering ratio Rc (%)] = (D2 / D1) × 100 was calculated. The covering ratio Rc was measured for 20 randomly selected organic particles, and the average value was taken as the average ratio of the outer surface of the core part of the organic particle covered by the shell part, and this average ratio was taken as the covering ratio of the organic particle.

[0119] <Viscosity of the composition for secondary battery adhesive layer> Using a rheometer (Anton Paar's "MCR502"), the temperature was 25°C and the shear rate was 100 sec -1 Viscosity η0 at shear rate of 10000sec -1 The viscosity η1 at each temperature was measured. The ratio of viscosity η0 to viscosity η1 (η0 / η1) was calculated using the obtained values ​​of viscosity η0 and viscosity η1.

[0120] <Surface tension of the composition for secondary battery adhesive layer> The prepared secondary battery adhesive layer composition was poured onto a glass petri dish. Then, the surface tension was measured by the plate method using a platinum plate. The measurement was performed twice using a fully automatic surface tensiometer "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd., and the average value of the surface tension was calculated from the measured values, and the average value was used as the surface tension of the secondary battery adhesive layer composition.

[0121] <Ejection performance (prevention of nozzle clogging)> Using an inkjet type slurry feeder equipped with an inkjet head (Konica Corporation's "KM1024 shear mode type"), the secondary battery adhesive layer composition was discharged under conditions of a flight speed of 6 to 10 m / sec. After the discharge was stopped, the composition was left to stand, and nozzle clogging was evaluated according to the following criteria based on whether or not the composition could be discharged again. The longer the time of leaving the composition, the better the dischargeability. A: Even if the ink was left for 30 minutes or more, it was possible to eject the ink again. B: When the standing time was less than 20 minutes, re-ejection was possible, but when the standing time was between 20 minutes and 30 minutes, re-ejection was not possible due to clogging of the nozzle. C: When the standing time was less than 10 minutes, re-ejection was possible, but when the standing time was 10 minutes or more but less than 20 minutes, re-ejection was not possible due to clogging of the nozzle. D: The standing time was less than 10 minutes, and re-ejection was not possible due to clogging of the nozzle.

[0122] <Evaluation of Adhesion A (Dry Adhesion between Separator and Electrode)> The obtained laminate A was placed with the collector side of the electrode (negative electrode) facing down, and cellophane tape was attached to the surface of the electrode (negative electrode). The cellophane tape used was specified in JIS Z1522. The cellophane tape was fixed to a horizontal test table. One end of the separator was pulled vertically upward at a pulling speed of 50 mm / min and peeled off, and the stress was measured. This measurement was performed a total of six times, and the average stress value was calculated as the peel strength, and the adhesion between the separator substrate and the electrode (negative electrode) via the adhesive layer was evaluated according to the following criteria: A higher peel strength indicates a higher adhesion between the separator and the electrode (negative electrode) via the adhesive layer. A: Peel strength is 1.5N / m or more B: Peel strength is 1.0N / m or more and less than 1.5N / m C: Peel strength is 0.5N / m or more and less than 1.0N / m D: Peel strength is less than 0.5N / m

[0123] <Evaluation of Adhesion B (Dry Adhesion between Separator with Porous Membrane Layer and Electrode)> The obtained laminate B was placed with the collector side of the electrode (negative electrode) facing down, and cellophane tape was attached to the surface of the electrode (negative electrode). The cellophane tape used was specified in JIS Z1522. The cellophane tape was fixed to a horizontal test table. Then, one end of the separator with the porous membrane layer was pulled vertically upward at a pulling speed of 50 mm / min and peeled off, and the stress was measured. This measurement was performed a total of six times, and the average stress value was calculated as the peel strength, and the adhesion between the separator with the porous membrane layer and the electrode (negative electrode) via the adhesive layer on the porous membrane layer was evaluated according to the following criteria: A higher peel strength indicates a higher adhesion between the separator with the porous membrane layer and the electrode (negative electrode) via the adhesive layer on the porous membrane layer. A: Peel strength is 1.5N / m or more B: Peel strength is 1.0N / m or more and less than 1.5N / m C: Peel strength is 0.5N / m or more and less than 1.0N / m D: Peel strength is less than 0.5N / m

[0124] <Low temperature output characteristics of secondary batteries> The secondary battery thus fabricated was charged at constant current and constant voltage (CCCV) up to 4.3 V in an atmosphere at 25° C. Then, the electric capacity was measured when the battery was discharged to 3.0 V at a constant current of 0.2 C in an atmosphere at −10° C., and the electric capacity was measured when the battery was discharged to 3.0 V at a constant current of 1 C. The capacity ratio [= (capacity at 1C / capacity at 0.2C) x 100 (%)] was then calculated. These measurements were performed on five secondary battery cells, and the average capacity ratio of each cell was taken as the discharge capacity retention rate and evaluated according to the following criteria. A higher discharge capacity retention rate indicates better low-temperature output characteristics. A: Discharge capacity retention rate is 80% or more B: Discharge capacity retention rate is 70% or more and less than 80% C: Discharge capacity retention rate is 60% or more and less than 70% D: Discharge capacity retention rate is less than 60%

[0125] Example 1 <Preparation of organic particles having a core-shell structure> First, in forming the core portion, 88 parts of styrene as an aromatic vinyl monomer, 6 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 5 parts of methacrylic acid as an acid group-containing monomer, 1 part of ethylene glycol dimethacrylate as a crosslinkable monomer, 1 part of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer, and after sufficient stirring, the mixture was heated to 60°C to initiate polymerization. When the polymerization conversion rate reached 96%, 80.7 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 1 part of methacrylic acid as an acid group-containing monomer, 18 parts of styrene as an aromatic vinyl monomer, and 0.3 parts of allyl methacrylate as a crosslinkable monomer were continuously added to form the shell portion, and the mixture was heated to 70°C to continue polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling to obtain an aqueous dispersion containing organic particles having a core-shell structure. The electrolyte swelling degree of the core and shell parts, the glass transition temperature of the core and shell parts, the volume average particle size, the core-shell ratio, and the coverage rate of the obtained organic particles are shown in Table 1.

[0126] <Preparation of other binders> To a reactor equipped with a stirrer, 70 parts of ion-exchanged water, 0.15 parts of sodium lauryl sulfate (manufactured by Kao Chemical Co., Ltd.: EMAL 2F) as an emulsifier, and 0.5 parts of ammonium persulfate were supplied, the gas phase was replaced with nitrogen gas, and the temperature was raised to 60°C. Meanwhile, in another container, 50 parts of ion-exchanged water, 0.5 parts of sodium dodecylbenzenesulfonate as an emulsifier, and 94 parts of n-butyl acrylate, 2 parts of acrylonitrile, 2 parts of methacrylic acid, 1 part of N-hydroxymethylacrylamide, and 1 part of allyl glycidyl ether as polymerizable monomers were mixed to obtain a monomer mixture. This monomer mixture was continuously added to the above-mentioned reactor over 4 hours to perform polymerization. During the addition, the reaction was carried out at 60°C. After the addition was completed, the reaction was terminated by stirring at 70°C for another 3 hours to produce an aqueous dispersion containing an acrylic polymer as another binder. Using this aqueous dispersion, the glass transition temperature of the other binder (acrylic polymer) was measured. The results are shown in Table 1.

[0127] <Preparation of Composition for Secondary Battery Adhesive Layer> 100 parts (solids equivalent) of the aqueous dispersion of organic particles having a core-shell structure obtained as described above and 15 parts (solids equivalent) of an aqueous dispersion of other binders (acrylic polymers) were mixed in a stirring vessel. 0.1 parts (solids equivalent) of an aqueous dispersion of cellulose nanofibers (manufactured by Sugino Machine Co., Ltd., "WFo-1002") as a thixotropic agent and 0.3 parts (solids equivalent) of an aqueous solution of a nonionic surfactant of a polyoxyalkylene derivative (manufactured by Kao Corporation, "LS-106") as a surface tension regulator were added to the resulting mixture, and ion-exchanged water was further added to obtain a secondary battery adhesive layer composition with a solids concentration of 4%. Using this secondary battery adhesive layer composition, a 100-sec shear rate was applied to the mixture. -1 Viscosity η0 at shear rate of 10000sec -1 The viscosity η1 and surface tension at 100° C. were measured, and the ratio of the viscosity η0 to the viscosity η1 was calculated. Then, the ejection performance (nozzle clogging) was evaluated. The results are shown in Table 1.

[0128] <Preparation of composition for porous membrane layer> 100 parts of alumina (Sumitomo Chemical Co., Ltd. "AKP3000", volume average particle size: 0.5 μm) as non-conductive particles, 1.0 part of ammonium polycarboxylate (Toa Gosei Co., Ltd. "Aron A-6114") as a dispersant, and water were mixed. The amount of water was adjusted so that the solid content concentration was 50%. The mixture was treated using a media-less dispersion device to disperse the alumina. 1.5 parts (solid content equivalent) of an aqueous solution in which carboxymethylcellulose (Daicel Chemical Co., Ltd. "Daicel 1220") as a thixotropic agent was dissolved was added to the obtained dispersion and mixed. The added thixotropic agent (carboxymethylcellulose) was dissolved in the mixture. Next, 3 parts (solid content equivalent) of an aqueous dispersion of an acrylic copolymer as a polymer for a porous membrane layer and 0.2 parts of an aliphatic polyether type nonionic surfactant as a surface tension adjuster were added, and water was further added so that the solid content concentration was 40% to obtain a composition for a porous membrane layer.

[0129] <Preparation of separator with porous membrane layer> The prepared composition for porous membrane layer was sealed in a polyethylene container and left to stand for 30 days. After that, a stirring blade was inserted into the polyethylene container and stirred at a rotation speed of 250 rpm. After the adhesion on the bottom of the container was no longer visually confirmed, stirring was continued for another 30 minutes to redisperse the non-conductive particles (alumina) in the composition for porous membrane layer. In addition, a single-layer polyethylene separator substrate (width 250 mm, length 1000 m, thickness 12 μm) manufactured by a wet method was prepared. The redispersed porous membrane layer composition was applied to one surface of the separator substrate using a gravure coater (application speed: 20 m / min) so that the thickness after drying was 2.5 μm. Next, the separator substrate to which the porous membrane layer composition was applied was dried in a drying oven at 50° C. and wound up to obtain a separator with a porous membrane layer formed on one surface of the separator substrate.

[0130] <Preparation of a separator with a porous membrane layer having an adhesive layer> The prepared secondary battery adhesive layer composition was discharged onto the porous membrane layer of the separator with a porous membrane layer obtained as described above using an inkjet type slurry feeder equipped with an inkjet head (Konica Corporation's "KM1024 (shear mode type)") under conditions of a flying speed of 6 to 10 m / sec, and the discharged secondary battery adhesive layer composition was dried. Then, a separator with a porous membrane layer was obtained in which a plurality of dot-shaped adhesive layers were formed on the porous membrane layer.

[0131] <Preparation of positive electrode> 100 parts of LiCoO2 [volume average particle diameter (D50): 12 μm] as a positive electrode active material, 2 parts of acetylene black ("HS-100" manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive material, 2 parts of polyvinylidene fluoride ("#7208" manufactured by Kureha Corporation) as a binder for the positive electrode composite layer in terms of solid content, and N-methylpyrrolidone were charged into a planetary mixer and mixed to give a total solid content concentration of 70%, to obtain a slurry composition for the positive electrode. The obtained positive electrode slurry composition was applied to a 20 μm thick aluminum foil as a current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried to obtain a positive electrode raw material. This drying was performed by conveying the aluminum foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Thereafter, the positive electrode raw material was rolled using a roll press to obtain a positive electrode with a positive electrode composite layer thickness of 95 μm.

[0132] <Preparation of negative electrode> In a 5MPa pressure vessel equipped with a stirrer, 33.5 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 62 parts of styrene, 1 part of 2-hydroxyethyl acrylate, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium peroxodisulfate as a polymerization initiator were added, and after thorough stirring, the mixture was heated to 50 ° C. to start polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to stop the reaction and obtain a mixture containing a binder (SBR) for the negative electrode composite layer. A 5% aqueous sodium hydroxide solution was added to the mixture containing the binder for the negative electrode composite layer to adjust the pH to 8, and then the unreacted monomer was removed by heating and vacuum distillation. Then, the mixture was cooled to 30 ° C. or less to obtain an aqueous dispersion containing a binder for the negative electrode composite layer. In addition, a mixture of 100 parts of artificial graphite [volume average particle diameter (D50): 15.6 μm] as a negative electrode active material and 1 part of a 2% aqueous solution of sodium salt of carboxymethylcellulose ("MAC350HC" manufactured by Nippon Paper Industries Co., Ltd.) as a thickener in terms of solid content was adjusted to a solid content concentration of 68% with ion-exchanged water, and then mixed at 25 ° C. for 60 minutes. After further adjusting the solid content concentration to 62% with ion-exchanged water, it was mixed at 25 ° C. for 15 minutes. The above-mentioned binder for the negative electrode mixture layer (SBR) was added in terms of solid content equivalent to 1.5 parts and ion-exchanged water, and the final solid content concentration was adjusted to 52%, and further mixed for 10 minutes. This was defoamed under reduced pressure to prepare a slurry composition for a negative electrode with good fluidity. The obtained negative electrode slurry composition was applied to a 20 μm-thick copper foil as a current collector using a comma coater so that the film thickness after drying was about 150 μm, and then dried to obtain a negative electrode raw sheet. This drying was performed by conveying the copper foil at a speed of 0.5 m / min in an oven at 60° C. for 2 minutes. Thereafter, the negative electrode raw sheet was rolled using a roll press to obtain a negative electrode with a negative electrode composite layer thickness of 100 μm.

[0133] <Preparation of Laminate A> Using an inkjet type slurry feeder equipped with an inkjet head (Konica Corporation's "KM1024 (shear mode type)"), the secondary battery adhesive layer composition was discharged onto the separator substrate under conditions of a flying speed of 6 to 10 m / s, and after drying, the coating amount, i.e., the amount of the adhesive layer formed, was 0.15 g / m 2 A plurality of dot-shaped adhesive layers were formed so that the size of each dot was 15,000 μm. 2 The adhesive layer was formed on the separator substrate, and the electrode (negative electrode) was laminated with the adhesive layer interposed therebetween, and the laminate was bonded together by holding the adhesive layer at a heating temperature of 80° C. and a pressure of 2.5 MPa for 10 seconds to obtain a laminate A. The adhesive strength A was evaluated using this laminate A. The results are shown in Table 1.

[0134] <Preparation of Laminate B> A composition for a secondary battery adhesive layer was discharged onto the porous membrane layer of the separator with a porous membrane layer using an inkjet type slurry supplying machine equipped with an inkjet head (Konica Corporation's "KM1024 (shear mode type)" under conditions of a flying speed of 6 to 10 m / sec, and after drying, a coating amount (formation amount) of 0.15 g / m was applied onto the separator with a porous membrane layer. 2 A plurality of dot-shaped adhesive layers were formed so that the size of each dot was 15,000 μm. 2 The result was as follows. The separator with a porous membrane layer, which is obtained by forming an adhesive layer on the porous membrane layer of the separator substrate with a porous membrane layer, and the electrode (negative electrode) were laminated together through the adhesive layer, and the laminate was bonded together by holding the laminate under pressure for 10 seconds under conditions of a heating temperature of 80°C and a pressure of 2.5 MPa, to obtain a laminate B. The adhesive strength B was evaluated using this laminate B. The results are shown in Table 1.

[0135] <Secondary battery manufacturing> An aluminum packaging exterior was prepared as the exterior of the battery. The positive electrode prepared as described above was cut into a square of 4.6 cm x 4.6 cm to be used as a positive electrode for a secondary battery. The separator with a porous membrane layer prepared as described above was cut into a square of 5.2 cm x 5.2 cm to be used as a separator for a secondary battery. The negative electrode was cut into a square of 5 cm x 5 cm to be used as a negative electrode for a secondary battery. The positive electrode for a secondary battery was placed in the aluminum packaging exterior so that the surface on the collector side was in contact with the aluminum packaging exterior. The separator for a secondary battery was placed on the surface of the positive electrode mixture layer of the positive electrode for a secondary battery so that the surface of the porous membrane layer on which the adhesive layer was formed was in contact with the positive electrode for a secondary battery. The negative electrode for a secondary battery was placed on the separator for a secondary battery so that the surface on the negative electrode mixture layer side faced the separator. Next, an electrolyte (solvent: ethylene carbonate / methyl ethyl carbonate / vinylene carbonate = 68.5 / 30 / 1.5 (volume ratio), electrolyte: LiPF6 with a concentration of 1 mol / L) was injected so that no air remained. Furthermore, in order to seal the opening of the aluminum packaging exterior, the aluminum packaging exterior was closed by heat sealing at 150°C, and a lithium ion secondary battery was manufactured as a secondary battery. The low-temperature output characteristics of this lithium-ion secondary battery were evaluated, and the results are shown in Table 1.

[0136] Example 2 In preparing the secondary battery adhesive layer composition, the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1, except that the monomers used to form the core and shell parts of the organic particles were changed as shown in Table 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0137] Example 3 In preparing the secondary battery adhesive layer composition, except that the cellulose nanofiber as a thixotropic agent was replaced with 0.3 parts of carboxymethyl cellulose, the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer on which adhesive layer was formed, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0138] Example 4 In preparing the secondary battery adhesive layer composition, the cellulose nanofibers as a thixotropic agent were replaced with 0.05 parts of (meth)acrylic acid copolymer (PMAA: Polymethacrylic acid), and the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer on which adhesive layer was formed, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0139] Example 5 In preparing the secondary battery adhesive layer composition, the content (solid content) of the acrylic polymer as another binder was changed as shown in Table 1, and the organic particles having a core-shell structure, the other binder, the secondary battery adhesive layer composition, the porous membrane layer composition, the separator with the porous membrane layer, the separator with the porous membrane layer on which the adhesive layer was formed, the positive electrode, the negative electrode, the laminate A, the laminate B, and the secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0140] Example 6 In preparing the secondary battery adhesive layer composition, the content (solid content) of the aqueous solution of the nonionic surfactant of the polyoxyalkylene derivative as a surface tension adjuster was changed as shown in Table 1, except that the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0141] Example 7 In preparing the secondary battery adhesive layer composition, the content (solid content) of cellulose nanofiber as a thixotropic agent and the content (solid content) of nonionic surfactant of polyoxyalkylene derivative as a surface tension adjuster were changed as shown in Table 1, respectively, except that the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0142] Example 8 In preparing the secondary battery adhesive layer composition, the content of cellulose nanofiber as a thixotropic agent was changed as shown in Table 1, and the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0143] Comparative Example 1 Except for using organic particles having a single-phase structure (non-core-shell) prepared as follows instead of organic particles having a core-shell structure, other binders, a composition for secondary battery adhesive layer, a composition for porous membrane layer, a separator with a porous membrane layer, a separator with a porous membrane layer formed with an adhesive layer, a positive electrode, a negative electrode, a laminate A, a laminate B, and a secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0144] <Preparation of organic particles with single-phase structure (non-core-shell)> To a reactor equipped with a stirrer, 70 parts of ion-exchanged water, 0.15 parts of sodium lauryl sulfate (manufactured by Kao Chemical Corporation, product name "EMAL 2F") as an emulsifier, and 0.5 parts of ammonium persulfate were supplied, the gas phase was replaced with nitrogen gas, and the temperature was raised to 60°C. Meanwhile, in another vessel, 50 parts of ion-exchanged water, 0.5 parts of sodium dodecylbenzenesulfonate as an emulsifier, and 40 parts of n-butyl acrylate, 1 part of methacrylic acid, 58 parts of styrene, and 1 part of ethylene glycol dimethacrylate as polymerizable monomers were mixed to obtain a monomer mixture. This monomer mixture was continuously added to the above-mentioned reactor over a period of 2 hours to carry out polymerization. During the addition, the reaction was carried out at 60°C. After the addition was completed, the mixture was stirred at 70°C for another 2 hours to terminate the reaction, and an aqueous dispersion containing organic particles with a single-phase structure (non-core-shell) was produced.

[0145] Comparative Example 2 In preparing the secondary battery adhesive layer composition, the content (solid content) of cellulose nanofiber as a thixotropic agent was changed as shown in Table 1, but in the same manner as in Example 1, the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0146] Comparative Example 3 In preparing the secondary battery adhesive layer composition, the content (solid content) of cellulose nanofiber as a thixotropic agent and the content (solid content) of other binders were changed as shown in Table 1, respectively, in the same manner as in Example 1. The organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer on which adhesive layer is formed, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0147] Comparative Example 4 In preparing the secondary battery adhesive layer composition, except that no thixotropic agent was used, the organic particles having a core-shell structure, other binders, secondary battery adhesive layer composition, porous membrane layer composition, separator with porous membrane layer, separator with porous membrane layer formed with adhesive layer, positive electrode, negative electrode, laminate A, laminate B, and secondary battery were prepared or produced in the same manner as in Example 1. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0148] In addition, in Table 1 shown below, "BA" indicates n-butyl acrylate units; "MAA" indicates a methacrylic acid unit, "ST" indicates a styrene unit, "AMA" indicates an allyl methacrylate unit; "EDMA" indicates ethylene glycol dimethacrylate units; "CNF" stands for cellulose nanofiber. "PMAA" stands for (meth)acrylic acid copolymer. "CMC" stands for carboxymethyl cellulose. "LS-106" refers to an aqueous solution of a nonionic surfactant of a polyoxyalkylene derivative. "ACL" refers to an acrylic polymer.

[0149] [Table 1]

[0150] From Table 1, the composition contains organic particles having a core-shell structure, a thixotropic agent and water, and is subjected to a shear rate of 100 sec -1 Viscosity η0 at shear rate of 10000sec -1 In Examples 1 to 8, which used compositions for secondary battery adhesive layers in which the viscosity η1 at and the ratio of the viscosity η0 to the viscosity η1 (η0 / η1) were within the specified ranges defined in the present invention, it was found that the separator with the porous membrane layer and the electrodes could be firmly bonded via the adhesive layer formed on the porous membrane layer. On the other hand, from Table 1, it can be seen that in Comparative Example 1, in which organic particles having a single structure, which is a non-core-shell structure, were used, the separator with the porous membrane layer and the electrodes could not be firmly bonded via the adhesive layer formed on the porous membrane layer, and the low-temperature output characteristics of the obtained secondary battery were deteriorated. Also, from Table 1, at a shear rate of 100 sec -1 Comparative Example 2, which used a secondary battery adhesive layer composition having a viscosity η0 at a shear rate of 10,000 sec outside the range specified in the present invention, and -1 It is clear that in Comparative Example 3, in which the viscosity η1 at 100° C. is outside the range specified by the present invention, the secondary battery adhesive layer composition cannot be discharged satisfactorily by the inkjet method. Furthermore, from Table 1, it can be seen that in Comparative Example 4, which uses a secondary battery adhesive layer composition that does not contain a thixotropic agent and has a ratio of viscosity η0 to viscosity η1 (η0 / η1) outside the specified range defined in the present invention, the separator with the porous membrane layer and the electrodes cannot be firmly bonded via the adhesive layer formed on the porous membrane layer, and the low-temperature output characteristics of the resulting secondary battery are deteriorated. [Industrial Applicability]

[0151] According to the present invention, even when an inkjet method is used, an adhesive layer can be efficiently formed on the porous membrane layer of a substrate with a porous membrane layer, and a composition for a secondary battery adhesive layer can be provided that can firmly bond the substrate with a porous membrane layer and an adherend member via the adhesive layer. In addition, according to the present invention, it is possible to provide a battery member for a non-aqueous secondary battery that can be firmly bonded to an adherend via an adhesive layer formed on the porous membrane layer of a substrate with a porous membrane layer, and a method for manufacturing the same. Furthermore, according to the present invention, a method for producing a laminate for a nonaqueous secondary battery can be provided, which can efficiently produce a laminate for a nonaqueous secondary battery in which a substrate with a porous membrane layer and an adherend are firmly adhered to each other via an adhesive layer formed on the porous membrane layer of the substrate with a porous membrane layer, and which can cause the secondary battery to exhibit excellent low-temperature output characteristics. According to the present invention, a nonaqueous secondary battery having excellent low-temperature output characteristics can be provided.

Claims

1. A non-aqueous secondary battery adhesive layer composition comprising organic particles, a thixotropic agent, and water, the organic particles have a core-shell structure including a core portion and a shell portion at least partially covering an outer surface of the core portion, Shear rate 100 sec -1 Viscosity at η 0 is less than 10 mPa·s and the shear rate is 10000 sec -1 Viscosity at η 1 is 0.5 mPa s or more and 2.4 mPa s or less, and the viscosity η 1 The viscosity η 0 The ratio of (η 0 / 1 ) is 1.2 or more and 9 or less.

2. The non-aqueous secondary battery adhesive layer composition according to claim 1 , having a surface tension of 30 mN / m or more and 60 mN / m or less.

3. The non-aqueous secondary battery adhesive layer composition according to claim 1 or 2, having a solids concentration of 30 mass % or less.

4. The composition for a nonaqueous secondary battery adhesive layer according to any one of claims 1 to 3, wherein the core portion is made of a polymer having a swelling degree in an electrolyte solution of 5 to 30 times, the shell portion is made of a polymer having a swelling degree in an electrolyte solution of more than 1 to 4 times, the polymer constituting the core portion has a glass transition temperature of -50°C or more and 150°C or less, and the glass transition temperature of the polymer constituting the shell portion is 10°C or more lower than the glass transition temperature of the polymer constituting the core portion.

5. A substrate having a porous membrane layer formed on at least one surface of the substrate; A plurality of dot-shaped adhesive layers formed on the porous membrane layer, the substrate is a separator substrate or an electrode substrate, A battery member for a non-aqueous secondary battery, wherein the adhesive layer is a dried product of the composition for a non-aqueous secondary battery adhesive layer according to any one of claims 1 to 4.

6. A coating step of coating the non-aqueous secondary battery adhesive layer composition according to any one of claims 1 to 4 on the porous membrane layer of a substrate having a porous membrane layer formed on at least one surface of the substrate by an inkjet method; A drying step of drying the non-aqueous secondary battery adhesive layer composition coated on the porous membrane layer to form an adhesive layer, The method for producing a battery member for a non-aqueous secondary battery, wherein the substrate is a separator substrate or an electrode substrate.

7. A coating step of coating the non-aqueous secondary battery adhesive layer composition according to any one of claims 1 to 4 on the porous membrane layer of a substrate having a porous membrane layer formed on at least one surface of the substrate by an inkjet method; A drying step of drying the non-aqueous secondary battery adhesive layer composition coated on the porous membrane layer to form an adhesive layer; and a bonding step of bonding the substrate with the porous membrane layer and an adherend member via the adhesive layer, The substrate is a separator substrate or an electrode substrate. A method for producing a laminate for a non-aqueous secondary battery.

8. A method for producing a nonaqueous secondary battery, comprising using a laminate for a nonaqueous secondary battery obtained by the method for producing a laminate for a nonaqueous secondary battery according to claim 7.

Citation Information

Patent Citations

  • Method for producing pressure-sensitive adhesive article

    JP2001181590A

  • Organic solvent-based thickening and thixotropy-imparting agent, coating composition, functional film and optical film

    JP2006096809A

  • Polyolefin microporous membrane

    JP2013203894A

  • Adhesive agent for lithium ion secondary batteries, lithium ion secondary battery separator, and lithium ion secondary battery

    JP2015088253A

  • Method for manufacturing secondary battery negative electrode

    JP2015141773A