Negative electrode active material, secondary battery, and method for producing artificial graphite particles

Artificial graphite particles with controlled porosity and oriented internal voids in lithium-ion batteries address the expansion issue, improving battery stability and capacity by absorbing volume changes during charging and discharging.

JP7583762B2Active Publication Date: 2024-11-14PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022072357
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-26
Publication Date
2024-11-14
Estimated Expiration
2042-04-26

AI Technical Summary

Technical Problem

Conventional methods fail to effectively suppress the expansion of negative electrodes in secondary batteries, particularly lithium-ion batteries, as they do not address the volume change of graphite particles during charging and discharging.

Method used

The use of artificial graphite particles with controlled porosity (0.7 to 15%) and internal voids with circularity of 0.1 to 0.6, oriented parallel to the graphite layer, achieved through rapid graphitization of graphite precursors with controlled sulfur content and high-frequency induction heating, which creates internal voids that absorb the expansion of the graphite crystals.

Benefits of technology

This configuration significantly reduces the expansion of the negative electrode, enhancing the battery's capacity and stability by effectively managing the volume changes during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583762000002
    Figure 0007583762000002
  • Figure 0007583762000003
    Figure 0007583762000003
  • Figure 0007583762000004
    Figure 0007583762000004
Patent Text Reader

Abstract

To provide a negative electrode active material capable of suppressing expansion of a negative electrode.SOLUTION: A negative electrode active material disclosed herein includes artificial graphite particles having a plurality of internal voids. The porosity of the artificial graphite particles is 0.7 to 15%. Binarization processing is performed on cross-sectional electron microscope images of 10 or more arbitrarily selected artificial graphite particles, circular approximation is performed for internal voids with a cross-sectional area of 1000nm2 or more, and when the circularity of 20 or more arbitrarily selected internal voids for each particle is obtained, the average value of the circularity of the internal voids is 0.1 to 0.6.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode active material containing artificial graphite particles. The present invention also relates to a secondary battery using the negative electrode active material. The present invention also relates to a method for producing the artificial graphite particles. [Background technology]

[0002] 2. Description of the Related Art In recent years, secondary batteries such as lithium-ion secondary batteries have been suitably used as portable power sources for personal computers, mobile terminals, and the like, and as power sources for driving vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), among others.

[0003] In the electrodes of secondary batteries, particularly lithium-ion secondary batteries, active materials capable of absorbing and releasing ions that serve as charge carriers are used. The active materials expand and contract as they absorb and release the ions, causing the volume of the electrodes to change during charging and discharging of the secondary batteries. In secondary batteries, suppressing the volume change of the electrodes has been a long-standing challenge. To address this challenge, Patent Document 1 proposes suppressing the expansion of the negative electrode in the thickness direction by orienting the graphite layer to a certain extent perpendicular to the negative electrode current collector. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6625336 specification Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques do not suppress the expansion of the graphite particles themselves, and therefore cannot fundamentally suppress the volume change of the negative electrode.

[0006] In view of the above circumstances, an object of the present invention is to provide a negative electrode active material capable of suppressing expansion of a negative electrode. [Means for solving the problem]

[0007] The negative electrode active material (1) disclosed herein contains artificial graphite particles having a plurality of internal voids. The porosity of the artificial graphite particles is 0.7 to 15%. Cross-sectional electron microscope images of arbitrarily selected 10 or more of the artificial graphite particles are binarized, and a 1000 nm 2 When the internal voids having the above cross-sectional area are approximated to a circle and the circularity of 20 or more internal voids selected arbitrarily for each particle is calculated, the average circularity of the internal voids is 0.1 to 0.6. With this configuration, it is possible to provide a negative electrode active material that can suppress expansion of the negative electrode.

[0008] The negative electrode active material (2) disclosed herein is the negative electrode active material (1) in which the porosity of the artificial graphite particles is 8 to 15%. With this configuration, the expansion of the negative electrode can be further suppressed.

[0009] The negative electrode active material (3) disclosed herein is the negative electrode active material (1) or (2), in which the internal voids have an average circularity of 0.3 to 0.6. With this configuration, the expansion of the negative electrode can be further suppressed.

[0010] The negative electrode active material (4) disclosed herein is any one of the negative electrode active materials (1) to (3), wherein the peak intensity (I D ) versus G-band peak intensity (I G ) ratio (I G / I D ) is 1.5 to 60. With this configuration, the internal voids are oriented parallel to the graphite layers, and the expansion of the negative electrode can be further suppressed. In addition, the capacity is increased.

[0011] The negative electrode active material (5) disclosed herein is any one of the negative electrode active materials (1) to (4), wherein the interplanar spacing d of the (002) plane of the graphite crystal of the artificial graphite particles is determined by powder X-ray diffraction measurement. 002is 3.36 Å to 3.38 Å. With this configuration, the internal voids are oriented parallel to the graphite layers, and the expansion of the negative electrode can be further suppressed.

[0012] From another aspect, a secondary battery (6) disclosed herein includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode includes any one of the negative electrode active materials (1) to (5). With this configuration, it is possible to provide a secondary battery in which expansion of the negative electrode is suppressed.

[0013] From another aspect, a method (7) for producing artificial graphite particles disclosed herein includes a step of graphitizing a graphite precursor by heating the graphite precursor from 1000°C to a temperature of 2600°C or higher within 5 hours. The graphite precursor has a sulfur concentration of 0.4% or more and 7% or less. With this configuration, a negative electrode active material capable of suppressing expansion of the negative electrode can be produced.

[0014] The method (8) for producing artificial graphite particles disclosed herein is the method (7) in which the graphite precursor is graphitized by heating from 1000° C. to a temperature of 2800° C. or higher within 5 hours. This configuration is more advantageous in producing a negative electrode active material capable of suppressing expansion of the negative electrode.

[0015] The method (9) for producing artificial graphite particles disclosed herein is the same as the method (7) or (8), except that the heating is performed by high-frequency induction heating. This configuration allows heating at a very high temperature rise rate. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a schematic cross-sectional view of an example of an artificial graphite particle contained in a negative electrode active material according to one embodiment of the present invention. [Diagram 2] 4A to 4C are explanatory diagrams of the mechanism of internal void generation in a manufacturing method according to one embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view showing a schematic configuration of a lithium ion secondary battery constructed using a negative electrode active material according to one embodiment of the present invention. [Figure 4] 4 is a schematic exploded view showing the configuration of a wound electrode body of the lithium ion secondary battery of FIG. 3. [Diagram 5] 1 is a scanning electron microscope image of a cross section of the artificial graphite particles obtained in Example 3. [Figure 6] 1 is a scanning electron microscope image of a cross section of an artificial graphite particle obtained in Comparative Example 2. [Figure 7] 6 is an image showing the result of performing binarization processing on the graphite portion and void portion of the image in FIG. 5. [Figure 8] This is an image showing the result of extracting internal voids having a cross-sectional area of ​​1000 nm2 or more from the image in FIG. 7 and performing circular approximation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Matters not mentioned in this specification but necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, members and parts having the same function are described with the same reference numerals. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B.

[0018] In this specification, the term "secondary battery" refers to an electricity storage device that can be repeatedly charged and discharged, and includes so-called storage batteries and electricity storage elements such as electric double layer capacitors. In addition, in this specification, the term "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as a charge carrier and realizes charging and discharging by the transfer of charge associated with the lithium ions between the positive and negative electrodes.

[0019] The negative electrode active material according to this embodiment contains artificial graphite particles having a plurality of internal voids. The void ratio of the artificial graphite particles is 0.7 to 15%. A binarization process is performed on cross-sectional electron microscope images of 10 or more arbitrarily selected artificial graphite particles, and a 1000 nm 2 When internal voids having the above cross-sectional area are approximated to a circle and the circularity of 20 or more arbitrarily selected internal voids of each particle is determined, the average circularity of the internal voids is 0.1 to 0.6.

[0020] Fig. 1 is a diagram for explaining the concept of the artificial graphite particles contained in the negative electrode active material according to this embodiment, and is a schematic cross-sectional view of one example of the artificial graphite particle. As shown in Fig. 1, an artificial graphite particle 10 has a graphite portion 12 and a plurality of internal voids 14. In the artificial graphite particle 10, the plurality of internal voids 14 exist as independent voids. As can be seen from the fact that the average circularity is calculated using 20 or more internal voids, the number of internal voids 14 in one artificial graphite particle 10 is 20 or more.

[0021] In Fig. 1, the internal void 14 has an elliptical shape. However, the shape of the internal void 14 is not limited to this. The internal void 14 may be, for example, substantially rectangular or irregular. In addition, the position, number, etc. of the internal void 14 are not limited to those shown in Fig. 1.

[0022] The porosity of the particle can be used as an index of the amount of internal voids 14. In this embodiment, the artificial graphite particles 10 have internal voids 14 in an amount such that the porosity is 0.7 to 15%. Note that artificial graphite obtained by graphitizing a graphite precursor generally does not have internal voids.

[0023] Regarding the shape of the internal void 14, the circularity of the figure can be used as an index. The circularity is expressed as 4πS / L 2 (where S is the area of ​​the shape, and L is the perimeter of the shape). The circularity of a perfect circle is 1, and as the circularity decreases, the shape is more distant from a perfect circle. In this embodiment, 2A circular approximation is performed on the internal voids 14 having the above cross-sectional area. In the above formula for the circularity, S is the area of ​​the circularly approximated internal voids 14, and L is the perimeter of the circularly approximated internal voids 14. Since the internal voids 14 are circularly approximated, a smaller circularity means that the internal voids 14 are flatter. In this embodiment, the average circularity is 0.1 to 0.6.

[0024] The artificial graphite particles 10 according to the present embodiment have a specific amount of internal voids 14 with a specific circularity, and thus can suppress expansion of a negative electrode using the artificial graphite particles 10. The reason for this is believed to be as follows.

[0025] When lithium ions are inserted between the graphite layers of the graphite particles by charging, the interplanar spacing of the graphite crystals expands, which causes the graphite particles to expand. The artificial graphite particles 10 have a specific amount of internal voids 14 with a specific degree of circularity, and are therefore able to absorb the expansion of the interplanar spacing of the graphite crystals. In particular, the circularity of the internal voids that are approximated to a circle is within a specific range (i.e., the internal voids are elongated), which makes it easier to absorb the expansion of the interplanar spacing of the graphite crystals. This makes it possible to effectively reduce the volume change of the artificial graphite particles 10. As a result, the expansion of the negative electrode using the artificial graphite particles 10 can be suppressed.

[0026] The porosity of the artificial graphite particles 10 is preferably 8 to 15% from the viewpoint of further suppressing the expansion of the negative electrode using the artificial graphite particles 10. The porosity can be determined by taking a cross-sectional electron microscope photograph of the artificial graphite particles 10 and expressing the ratio (%) of the total area of ​​internal voids to the area of ​​the entire particle.

[0027] Specifically, the porosity can be determined, for example, as follows. A cross section is taken of a material or member (e.g., a negative electrode active material layer of a negative electrode) containing artificial graphite particles by ion milling. A scanning electron microscope (SEM) image of this cross section is obtained, and the SEM image is subjected to image analysis software to clearly distinguish between graphite and voids, and binarized. The areas of the graphite and voids are determined, and [(total area of ​​voids) / {(area of ​​graphite)+(total area of ​​voids)}]×100 is calculated. This value is determined for 10 or more particles, and the average value is taken as the porosity.

[0028] From the viewpoint of further suppressing the expansion of the negative electrode using the artificial graphite particles 10, the circularity of the artificial graphite particles 10 is preferably 0.3 to 0.6, and more preferably 0.45 to 0.6. The circularity can be determined, for example, as follows. A cross section of a material or member (for example, a negative electrode active material layer of a negative electrode) containing the artificial graphite particles is taken by ion milling. An SEM image of the cross section is obtained, and the SEM image is subjected to image analysis software to clearly distinguish between graphite portions and void portions, and binarized. 1000 nm 2 Extract internal voids having a cross-sectional area of ​​100 mm or more, and perform a circular approximation on the extracted internal voids. Calculate the circularity of 20 or more arbitrarily selected internal voids. Perform this for 10 or more arbitrarily selected graphite particles, and calculate the average value.

[0029] As image analysis software for calculating the porosity and circularity, for example, "ImageJ" manufactured by the National Institutes of Health can be used.

[0030] In the example shown in Fig. 1, the internal voids 14 are oriented in a predetermined direction. However, the internal voids 14 do not have to be oriented in a predetermined direction. In order to efficiently absorb the expansion of the interplanar spacing of the graphite crystals in the artificial graphite particles 10, the internal voids 14 are preferably oriented parallel to the graphite layers (in other words, the graphene planes). Here, if the artificial graphite particles 10 have a high degree of crystallinity, the major axis of the internal voids 14 when approximated to a circle can be oriented parallel to the graphite layers.

[0031] The crystallinity of the artificial graphite particles 10 is determined by the peak intensity of the D band (I D ) versus G-band peak intensity (I G ) ratio (I G / I D ) can be evaluated by this ratio (I G / I D When the ratio (I) is 1.5 or more, the crystal growth in the artificial graphite particles 10 progresses sufficiently, the internal voids are sufficiently developed, and the internal voids are highly oriented in the elongation direction of the graphite layers, which is preferable. G / I D When the peak intensity (I D ) and G-band peak intensity (I G ) are the Raman spectra of the artificial graphite particles 10 measured using an argon ion laser at 1360 cm -1 Near and 1580cm -1 It can be calculated as the intensity of a peak that appears in the vicinity.

[0032] The crystallinity of the artificial graphite particles 10 is determined by the interplanar spacing d 002 The surface spacing d 002 In the case where the interplanar spacing d is in the range of 3.36 Å to 3.38 Å, the crystal growth in the artificial graphite particles 10 progresses sufficiently, the internal voids are sufficiently developed, and the internal voids are highly oriented in the elongation direction of the graphite layers, which is preferable. 002 can be determined by powder X-ray diffraction (XRD) measurement.

[0033] The average particle diameter (median diameter: D50) of the artificial graphite particles 10 is not particularly limited and is, for example, 0.1 μm or more and 50 μm or less. Since the artificial graphite particles 10 are used as a negative electrode active material, the average particle diameter (D50) of the artificial graphite particles 10 is preferably 1 μm or more and 30 μm or less, and more preferably 5 μm or more and 20 μm or less. The average particle diameter (D50) of the artificial graphite particles 10 can be determined, for example, by a laser diffraction scattering method.

[0034] Next, a method for producing the artificial graphite particles contained in the negative electrode active material according to this embodiment will be described. The artificial graphite particles contained in the negative electrode active material according to this embodiment can be suitably produced by the following method. Note that the artificial graphite particles contained in the negative electrode active material according to this embodiment are not limited to those produced by the following production method.

[0035] The method for producing the artificial graphite particles contained in the negative electrode active material according to the present embodiment includes a step of graphitizing a graphite precursor by heating the graphite precursor from 1000° C. to a temperature of 2600° C. or higher within 5 hours. The graphite precursor has a sulfur concentration of 0.4% or more and 7% or less.

[0036] As the graphite precursor, a carbon material that can be graphitized by heat treatment at 2600°C or higher can be used. Examples of the graphite precursor include coal (e.g., anthracite, bituminous coal, etc.), petroleum pitch, coal-based pitch, coal-based coke, petroleum-based coke, coal-based needle coke, petroleum-based needle coke, bulk mesophase, mesophase pitch carbon fiber, mesophase pitch, mesocarbon microbeads, coke refined from vacuum residual oil generated in a crude oil refining process, etc. These can be used alone or in combination of two or more. Among them, at least one selected from the group consisting of coal, petroleum pitch, coal-based pitch, coal-based coke, petroleum-based coke, coal-based needle coke, and petroleum-based needle coke is preferred, and at least one selected from the group consisting of coal, petroleum pitch, and petroleum coke is more preferred.

[0037] In this manufacturing method, a graphite precursor having a sulfur concentration of 0.4% to 7% is used, and this graphite precursor is graphitized by heating from 1000°C to a temperature of 2600°C or higher within 5 hours.

[0038] Graphite precursors start to transition to a graphite structure at temperatures of 1000°C or higher. It is known that graphite precursors undergo volume expansion called puffing during graphitization. This puffing leads to deterioration in the quality of artificial graphite, such as a decrease in strength and the generation of cracks. One of the causes of puffing is thought to be that the sulfur components contained in the graphite precursor expand the structure of the graphite precursor when they decompose at high temperatures and volatilize to the outside. For this reason, graphite precursors with a low sulfur content, specifically, graphite precursors with a sulfur content of 0.35% or less (particularly, graphite precursors with a sulfur content of less than 0.1% for secondary battery applications) are generally used.

[0039] On the other hand, graphitization by heat treatment causes thermal shrinkage, so that in order to reduce the degree of this thermal shrinkage, the temperature is generally raised over a long period of time (for example, in secondary battery applications, the temperature is raised over a period of several weeks).

[0040] In contrast, in the manufacturing method according to the present embodiment, a graphite precursor having a high sulfur content is used, and the temperature is raised in a short time. This makes it possible to efficiently obtain artificial graphite particles having a porosity of 0.7 to 15% and an average circularity of the internal voids of 0.1 to 0.6. The mechanism by which such internal voids are generated is presumed to be as follows. In FIG. 2 described below, the number of internal voids is set to 5 for convenience of explanation and ease of understanding. In reality, 20 or more internal voids are generated.

[0041] 2A shows a raw material graphite precursor particle 110. The graphite precursor particle contains optical texture 120 that serves as a nucleus for crystal growth and sulfur component 130 therein.

[0042] When the graphite precursor particle 110 is heated to 1500°C or higher, crystal growth of the optical texture 120 and desorption of the sulfur component 130 (i.e., desulfurization) occur simultaneously. During the crystal growth of the optical texture 120, contraction occurs toward the center of the optical texture 120 (see the arrow in FIG. 2(B)). As a result, as shown in FIG. 2(B), cracks 140 occur in the portions where the sulfur component 130 has been desorbed.

[0043] Thereafter, the optical texture 120 continues to grow as crystals such that the interplanar spacing of the graphite structure is reduced. In response to this, the cracks 140 widen to form internal voids 150. At this time, as shown in FIG. 2(C), the internal voids 150 are oriented parallel to the graphene plane, and the cross-sectional shape of the internal voids 150 becomes elongated. As described above, the elongated cross-sectional shape has a low circularity. In this way, a large number of voids are formed whose average circularity in the above-mentioned circular approximation is 0.1 to 0.6, and the porosity is as high as 0.7 to 15%.

[0044] Graphite precursors having a sulfur content of 0.4% or more and 7% or less are known and can be obtained according to known methods. The sulfur content in the graphite precursor can be determined by combustion ion chromatography. Combustion ion chromatography can be performed according to known methods. Specifically, for example, a graphite precursor sample is placed in a combustion decomposition unit and burned in a combustion gas stream containing oxygen. The generated gas is collected in an absorption liquid, and the sulfate ions collected in the absorption liquid are separated and quantified by ion chromatography. Based on this, the sulfur content of the graphite precursor is determined. In this specification, the unit of sulfur content "%" means "mass%" according to the usual meaning in the field of artificial graphite.

[0045] For the purpose of obtaining homogeneous artificial graphite particles, the graphite precursor may be subjected to a pulverization treatment, a classification treatment, etc. The pulverization treatment can be performed using a known pulverizing device (e.g., a jet mill, a hammer mill, a roller mill, a pin mill, a vibration mill, etc.). The classification treatment can be performed using a known classification device.

[0046] The graphite precursor alone may be subjected to heating. However, the graphite precursor may be mixed with other components and heated within a range that does not significantly impair the effects of the present invention. For example, binder pitch (e.g., pitch with a softening point of about 70 to 300°C) may be added in the production of an artificial graphite material, and in this embodiment, binder pitch may also be added to the graphite precursor. When binder pitch is added, it is preferable to appropriately select the type and amount thereof, taking into consideration the possibility of blocking voids in the resulting artificial graphite particles.

[0047] In the manufacturing method according to the present embodiment, the graphite precursor is graphitized by heating it from 1000° C. to a temperature of 2600° C. or higher within 5 hours. In order to realize such a rapid temperature rise, the heating is preferably performed by a high-frequency induction heating method or a direct current heating method.

[0048] The high-frequency induction heating method is a heating method in which a conductive object to be heated is placed inside a heating coil, a high-frequency current is passed through the heating coil to induce eddy currents in the object to be heated, and Joule heat is generated by the resistance of the object to be heated, causing the object to self-heat. For example, a graphite precursor can be added to a carbon crucible, container, or mold, and this can be used as the object to be heated by the high-frequency induction heating method.

[0049] The direct resistance heating method is a heating method in which an electric current is passed directly through a conductive object to be heated, and Joule heat is generated by the resistance of the object to be heated, causing the object to self-heat. For example, a graphite precursor is placed in a carbon crucible, container, or mold, and this is used as the object to be heated to perform heating by the direct resistance heating method.

[0050] It is more preferable that the heating be performed by high frequency induction heating, since this allows a higher temperature rise rate.

[0051] The heating is preferably carried out in an inert atmosphere (eg, an inert gas atmosphere such as argon gas) in order to avoid adverse effects due to the atmosphere, but the atmosphere is not limited thereto.

[0052] The heating rate is not particularly limited as long as heating can be performed from 1000° C. to a temperature of 2600° C. or higher within 5 hours. The heating rate is preferably 10° C. / min or higher, more preferably 20° C. / min or higher, and even more preferably 30° C. / min or higher.

[0053] From the viewpoint of further increasing the crystallinity of the resulting artificial graphite particles, the heating is preferably performed from 1000°C to a temperature of 2800°C or higher within 5 hours, and more preferably from 1000°C to a temperature of 2800°C or higher within 3 hours. If the heating temperature is too high, sublimation of the graphite may occur and the energy consumption for heating increases. Therefore, the maximum temperature during the heating is preferably 3500°C or lower, and more preferably 3200°C or lower.

[0054] The conditions for heating the graphite precursor to 1000° C. are not particularly limited. The graphite precursor may be subjected to a predetermined heat treatment at less than 1000° C. The heating rate from room temperature to 1000° C. and the heating rate from 1000° C. to 2600° C. or higher may be the same or different.

[0055] In order to promote sufficient graphitization, the material may be heated to a temperature of 2600° C. or higher and then held at that temperature for a predetermined time, for example, for 30 minutes or more, and may be held for 24 hours or less, 12 hours or less, 6 hours or less, or 3 hours or less.

[0056] This heating can graphitize the graphite precursor. After heating, the material may be left as it is to cool. That is, the material may be allowed to cool naturally (in other words, naturally cooled).

[0057] In the manner described above, the artificial graphite particles according to the present embodiment can be obtained. According to such a production method, the porosity of the artificial graphite particles and the average circularity of the internal voids can be controlled by adjusting the sulfur concentration of the graphite precursor and the temperature rise conditions.

[0058] The negative electrode active material according to the present embodiment can be used to construct a negative electrode according to a known method. Specifically, the negative electrode active material according to the present embodiment can be used as the negative electrode active material in a known negative electrode that uses a graphite-based negative electrode active material. Furthermore, a secondary battery can be constructed using the negative electrode according to a known method. In a negative electrode that includes the negative electrode active material according to the present embodiment, the expansion of the negative electrode is suppressed.

[0059] From another perspective, the secondary battery according to this embodiment includes a positive electrode, a negative electrode, and an electrolyte, and the negative electrode includes the negative electrode active material according to the above embodiment. Hereinafter, a configuration example of the secondary battery according to this embodiment will be described. The secondary battery of this configuration example is a flat prismatic lithium ion secondary battery having a flat wound electrode body and a flat battery case. However, the configuration of the secondary battery according to this embodiment is not limited to the example described below.

[0060] The lithium-ion secondary battery 100 shown in Fig. 3 is a sealed battery constructed by housing a flat wound electrode assembly 20 and a non-aqueous electrolyte (not shown) in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The positive and negative electrode terminals 42, 44 are electrically connected to the positive and negative electrode current collector plates 42a, 44a, respectively. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.

[0061] As shown in Fig. 3 and Fig. 4, the wound electrode body 20 has a configuration in which a positive electrode sheet 50 and a negative electrode sheet 60 are overlapped with two long separator sheets 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long positive electrode current collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long negative electrode current collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the wound electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are joined to the positive electrode current collector 42a and the negative electrode current collector 44a, respectively.

[0062] A known positive electrode current collector used in lithium ion secondary batteries may be used as the positive electrode current collector 52, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). As the positive electrode current collector 52, aluminum foil is preferred.

[0063] The dimensions of the positive electrode current collector 52 are not particularly limited and may be appropriately determined depending on the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.

[0064] The positive electrode active material layer 54 contains a positive electrode active material. Examples of the positive electrode active material include lithium nickel composite oxides (e.g., LiNiO2, etc.), lithium cobalt composite oxides (e.g., LiCoO2, etc.), and lithium nickel cobalt manganese composite oxides (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2, etc.), lithium nickel cobalt aluminum composite oxides (e.g., LiNi 0.8 Co 0.15 Al 0.5 O2, etc.), lithium manganese composite oxides (e.g., LiMn2O4, etc.), lithium nickel manganese composite oxides (e.g., LiNi 0.5 Mn 1.5 Lithium transition metal composite oxides (e.g., LiFePO4, etc.) and lithium transition metal phosphate compounds (e.g., LiFePO4, etc.).

[0065] The positive electrode active material layer 54 may contain components other than the positive electrode active material, such as trilithium phosphate, a conductive material, a binder, etc. As the conductive material, for example, carbon black such as acetylene black (AB) or other carbon materials (e.g., graphite, etc.) can be suitably used. As the binder, for example, polyvinylidene fluoride (PVDF) can be used.

[0066] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 85 mass% or more and 99 mass% or less. The content of the trilithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 15 mass% or less, and more preferably 0.2 mass% or more and 10 mass% or less. The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 20 mass% or less, and more preferably 0.3 mass% or more and 15 mass% or less. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.4 mass% or more and 15 mass% or less, and more preferably 0.5 mass% or more and 10 mass% or less.

[0067] The thickness of the positive electrode active material layer 54 is not particularly limited, but is, for example, from 10 μm to 300 μm, and preferably from 20 μm to 200 μm.

[0068] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.

[0069] The dimensions of the negative electrode current collector 62 are not particularly limited and may be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 6 μm or more and 20 μm or less.

[0070] The negative electrode active material layer 64 contains the negative electrode active material of the above-mentioned embodiment as the negative electrode active material. The negative electrode active material layer 64 may contain other negative electrode active materials in addition to the negative electrode active material of the above-mentioned embodiment, as long as the effects of the present invention are not significantly impaired.

[0071] The negative electrode active material layer 64 may contain components other than the active material, such as a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc. may be used. As the thickener, for example, carboxymethyl cellulose (CMC), etc. may be used.

[0072] The content of the negative electrode active material in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.

[0073] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 300 μm, and preferably not less than 20 μm and not more than 200 μm.

[0074] The separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) may be provided on the surface of the separator 70.

[0075] The thickness of the separator 70 is not particularly limited, but is, for example, from 5 μm to 50 μm, and preferably from 10 μm to 30 μm.

[0076] The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). As the non-aqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones that are used in general electrolytes of lithium ion secondary batteries can be used without any particular limitation. Among them, carbonates are preferable, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more.

[0077] As the supporting salt, for example, a lithium salt such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.

[0078] The nonaqueous electrolyte may contain various additives other than the above-mentioned components, such as film-forming agents such as vinylene carbonate (VC) and oxalate complexes; gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB); and thickeners, as long as the effects of the present invention are not significantly impaired.

[0079] The lithium ion secondary battery 100 can be used for various purposes. Suitable applications include a driving power source mounted on vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs). The lithium ion secondary battery 100 can also be used as a storage battery for small power storage devices and the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack typically consisting of a plurality of batteries connected in series and / or parallel.

[0080] The above describes a rectangular lithium ion secondary battery 100 including a flat wound electrode assembly 20 as an example. However, the lithium ion secondary battery can also be configured as a lithium ion secondary battery including a laminated electrode assembly (i.e., an electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately laminated). The lithium ion secondary battery can also be configured as a cylindrical lithium ion secondary battery, a laminated lithium ion secondary battery, or the like. It can also be configured as an all-solid-state lithium ion secondary battery using a solid electrolyte instead of a nonaqueous electrolyte according to a known method.

[0081] The negative electrode active material according to the above embodiment is suitable for the negative electrode active material of a lithium ion secondary battery, but can be used as the negative electrode active material of other secondary batteries. Other secondary batteries can be constructed according to known methods. Therefore, the secondary battery according to the present embodiment can be constructed as a secondary battery other than a lithium ion secondary battery according to known methods.

[0082] Examples of the present invention will be described in detail below, but it is not intended that the present invention be limited to those shown in these examples.

[0083] <Preparation of negative electrode active material> [Examples 1 to 6, Comparative Example 1] Petroleum cokes with different sulfur concentrations were prepared. The petroleum cokes were coarsely pulverized using a hammer mill until the particle size was 10 mm or less, and then further pulverized using a jet mill. The pulverized material obtained was classified using an airflow classifier to remove fine powder of submicron order generated by pulverization. In this manner, a graphite precursor was prepared. The sulfur concentrations contained in the graphite precursors are shown in Table 1. The sulfur concentrations were measured by the method described below.

[0084] About 20 g of graphite precursor was placed in a carbon crucible and placed in a high-frequency induction heating type sintering furnace. The atmosphere in this furnace was an argon atmosphere. The material was heated to 3000°C at a temperature increase rate of 50°C / min, and graphitized by holding at 3000°C for 1 hour. Thereafter, heating was stopped, and the graphitized material was allowed to cool in the furnace. In this way, artificial graphite particles (i.e., negative electrode active materials) of Examples 1 to 6 and Comparative Example 1 were obtained.

[0085] Comparative Example 2 The graphite precursor used was the same as that used in Example 3. Approximately 20 g of the graphite precursor was placed in a carbon crucible and placed in an Acheson furnace. The atmosphere in the furnace was an argon atmosphere. The graphite precursor was heated to 3000°C at a temperature increase rate of approximately 30°C / hour, and graphitized by holding at approximately 3000°C for four days. Thus, it took about four days for the temperature to reach 2800°C or higher. After that, the heating was stopped, and the graphitized material was allowed to cool in the furnace. In this manner, the artificial graphite particles (i.e., the negative electrode active material) of Comparative Example 2 were obtained.

[0086] <Measurement of sulfur concentration in graphite precursor> As a combustion apparatus for the graphite precursor, the total organic halogen analyzer "TOX-100" manufactured by Mitsubishi Chemical Corporation was used. A sample obtained by mixing 5 mg of the graphite precursor and 50 mg of the tungsten-based combustion aid used in each example and each comparative example was collected on a sample board (ceramic board). The sample was burned under an oxygen stream using the above apparatus. The heater temperature was 1100 °C and the heating time was 500 seconds. The sulfur content in the generated combustion gas was collected with 20 mL of an absorption liquid. The absorption liquid was prepared by adding hydrogen peroxide solution to ion-exchanged water so that the concentration of hydrogen peroxide became 5 μg / mL.

[0087] Quantitative analysis of the absorption liquid was performed using an ion chromatograph analyzer "ICS-5000" manufactured by Dionex Corporation, Japan, equipped with a column "AS15" and a suppressor "AERS-500" (2 mm) to determine the sulfur content concentration. A potassium hydroxide solution was used as the eluent and the regenerant.

[0088] <Measurement of average particle diameter> Using a commercially available laser diffraction particle size distribution measuring device, the average particle diameter (D50) of the artificial graphite particles (negative electrode active material) in each example and each comparative example was determined. The results are shown in Table 1.

[0089] <Raman spectroscopy measurement> Using a commercially available Raman spectrometer, the ratio of the peak intensity (I -1 ) of the D band near 1360 cm D to the peak intensity (I -1 ) of the G band near 1580 cm G for the artificial graphite particles (negative electrode active material) in each example and each comparative example was determined. The results are shown in Table 1.

[0090] <XRD measurement> Using a commercially available X-ray diffractometer, the interplanar spacing d 002 of the (002) plane of the graphite crystal of the artificial graphite particles (negative electrode active material) in each example and each comparative example was determined. The results are shown in Table 1.

[0091] <Fabrication of evaluation half cell> For each of the examples and comparative examples, the negative electrode active material (C), styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in an ion-exchanged water at a mass ratio of C:SBR:CMC = 99:0.5:0.5 to prepare a slurry for forming a negative electrode active material layer. This slurry was applied to the surface of a copper foil with a thickness of 10 μm, dried, and then roll-pressed to produce a negative electrode sheet. The thickness of the negative electrode sheet at this time was measured.

[0092] A metallic lithium foil was prepared as a lithium electrode. Also, a separator sheet was prepared in which a ceramic particle layer (HRL) with a thickness of 4 μm was formed on a porous polyolefin layer having a three-layer structure of PP / PE / PP with a thickness of 20 μm. A non-aqueous electrolyte was prepared by dissolving LiPF6 as a supporting salt at a concentration of 1.0 mol / L in a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:3:4.

[0093] The negative electrode sheet, the separator, and the metallic lithium foil were laminated. At this time, the HRL of the separator was opposed to the negative electrode sheet. The obtained laminate was sealed in a battery case together with the above non-aqueous electrolyte to produce a coin-type half cell.

[0094] <SEM Observation and Evaluation> The cross-section of the negative electrode active material layer of the negative electrode prepared above was taken by ion milling. This cross-section was observed using a commercially available scanning electron microscope (SEM) to obtain an SEM image. For reference, the cross-sectional SEM images of the artificial graphite particles of Example 3 and Comparative Example 2 are shown in FIGS. 5 and 6, respectively.

[0095] For this SEM image, the graphite part and the void part were distinguished using the image analysis software "ImageJ" and subjected to binarization processing. For 10 or more particles, the porosity was determined from the areas of the graphite part and the void part, and the average value was calculated. The results are shown in Table 1.

[0096] Furthermore, using the image analysis software "ImageJ", the binarized graphite and void areas were analyzed at 1000 nm 2 Internal voids having a cross-sectional area of ​​100 mm or more were extracted, and the extracted internal voids were subjected to circular approximation. The circularity of 20 or more internal voids for 10 or more particles was determined, and the average value was calculated. The results are shown in Table 1. For reference, the image after binarization processing and the image after circular approximation in Example 3 are shown in Figures 7 and 8, respectively.

[0097] <Discharge capacity measurement> Each evaluation half cell was charged at a constant current of 0.1C to 3V against the lithium electrode, and then charged at a constant voltage until the current value became 1 / 10C. Then, each evaluation half cell was discharged at a constant current of 0.1C to 1.6V against the lithium electrode, and then discharged at a constant voltage until the current value became 1 / 10C. This charge-discharge cycle was repeated for two cycles, and the discharge capacity (mAh) at the time of the second cycle discharge was calculated. The capacity density (mAh / g) of the negative electrode active material was calculated from this discharge capacity and the weight of the negative electrode active material. The results are shown in Table 1.

[0098] <Measurement of negative electrode expansion rate> The thickness measured above when the negative electrode sheet was prepared was taken as the initial thickness of the negative electrode. Each evaluation half-cell was charged to a capacity value of 80% of the discharge capacity measured above. Thereafter, each evaluation half-cell was disassembled, and the thickness of the negative electrode was measured, which was taken as the thickness of the negative electrode after charging. The expansion rate was calculated using the following formula. The results are shown in Table 1. Expansion rate (%) = (thickness of negative electrode after charging / initial thickness of negative electrode) x 100

[0099] [Table 1]

[0100] The results in Table 1 show that when the porosity of the artificial graphite particles is 0.7 to 15% and the average circularity of the internal voids is in the range of 0.1 to 0.6, the expansion of the negative electrode can be significantly reduced. Therefore, it is clear that the negative electrode expansion can be suppressed by the negative electrode active material disclosed herein.

[0101] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]

[0102] 10. Artificial graphite particles 12 Graphite Section 14 Internal void 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 Separator sheet (separator) 100 Lithium-ion secondary battery

Claims

1. A negative electrode active material comprising artificial graphite particles having a plurality of internal voids, The porosity of the artificial graphite particles is 10.4% to 15%, A cross-sectional electron microscope image of 10 or more arbitrarily selected artificial graphite particles is subjected to a binarization process, 2 When internal voids having a cross-sectional area of ​​the above or similar are approximated to a circle and the circularity of 20 or more internal voids arbitrarily selected for each particle is determined, the average circularity of the internal voids is 0.53 to 0.

6. Negative electrode active material.

2. The peak intensity of the D band of the artificial graphite particles obtained by Raman spectroscopy (I D ) versus G band peak intensity (I G ) ratio (I G / I D 2. The negative electrode active material according to claim 1, wherein the molecular weight of the negative electrode is 1.5 to 60.

3. The interplanar spacing d of the (002) plane of the graphite crystal of the artificial graphite particles is determined by powder X-ray diffraction measurement. 002 The negative electrode active material according to claim 1, wherein the surface roughness is 3.36 Å to 3.38 Å.

4. A secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, A secondary battery, wherein the negative electrode comprises the negative electrode active material according to claim 1 .

5. The graphite precursor is graphitized by heating the graphite precursor from 1000° C. to a temperature of 2600° C. or higher within 5 hours, The method for producing artificial graphite particles, wherein the graphite precursor has a sulfur concentration of 5.5% or more and 7% or less.

6. The method according to claim 5, wherein the graphite precursor is graphitized by heating from 1000°C to a temperature of 2800°C or higher within 5 hours.

7. The method according to claim 5, wherein the heating is performed by high-frequency induction heating.

Citation Information

Patent Citations

  • Method for producing graphite material for lithium ion battery electrode material

    JP2014053314A

  • Negative electrode active material, negative electrode, and lithium ion secondary battery

    JP2018139171A

  • Carbon material for negative electrode of non-aqueous secondary battery and non-aqueous secondary battery

    JP6625336B2