Crystalline tantalum oxide particles and method for producing crystalline tantalum oxide particles
The chemical vapor phase reaction method produces nano-sized, spherical tantalum oxide particles with high crystallinity, addressing the challenges of conventional methods by ensuring dense coatings and enhanced catalytic performance.
Patent Information
- Application Number
- JP2021030636
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Conventional methods struggle to produce nano-sized, highly crystalline, and substantially spherical tantalum oxide particles, as high-temperature and long-time calcination treatments lead to grain growth and sintering, making it difficult to achieve a high specific surface area and dense coatings or films.
The production of tantalum oxide particles is achieved through a chemical vapor phase reaction method, controlling parameters such as temperature, pressure, and gas flow to generate particles with an average diameter of 20 nm to 500 nm and crystallite size of 10 nm or more, maintaining a spherical shape and high crystallinity.
This method yields nano-sized, substantially spherical tantalum oxide particles with excellent crystallinity and a high specific surface area, suitable for dense coatings and improved catalytic activity.
Smart Images

Figure 0007584091000003 
Figure 0007584091000004 
Figure 0007584091000005
Abstract
Description
[Technical field]
[0001] The present invention relates to crystalline tantalum oxide particles and a method for making crystalline tantalum oxide particles. [Background technology]
[0002] Tantalum oxide (Ta2O5) has the characteristics of a high dielectric constant and refractive index, which makes it useful as a material for capacitors and optical coatings. To apply it to these applications, an ink containing tantalum oxide nanoparticles and a binder is prepared, and this ink is applied to a substrate and heat-treated to produce a tantalum oxide film.
[0003] For example, Patent Document 1 discloses a method for producing an optical element, which comprises the steps of preparing tantalum oxide particles, dispersing the prepared tantalum oxide particles in an organic monomer, and curing the organic monomer (claim 7 of Patent Document 1). Patent Document 1 also discloses a method for producing tantalum oxide particles by hydrolyzing tantalum alkoxide so that the maximum temperature and maximum pressure in a container satisfy a specific relationship (claim 1 of Patent Document 1).
[0004] Tantalum oxide is also attracting attention as a material for photocatalysts for water splitting, which generate hydrogen from solar energy and water. If hydrogen can be efficiently produced from sunlight, a renewable natural energy source, and water, it will be possible to move away from a fossil fuel society and towards a hydrogen society, where hydrogen is the energy source. For this reason, tantalum oxide is a promising material for water splitting catalysts.
[0005] For example, Patent Document 2 discloses tantalum oxide particles having a primary particle size of 70 nm or less and an optical absorptance of 0.32 or less at a wavelength of 1800 nm measured by diffuse reflectance spectroscopy (claim 1 of Patent Document 2). Patent Document 1 also describes that the tantalum oxide particles have the characteristics of having both high crystallinity and a fine primary particle size, that they can be used as a photocatalyst for photodecomposition of water, and that they can also be used as a dielectric material for multilayer films and the like (
[0009] ,
[0021] , and
[0022] of Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-111684 A [Patent Document 2] JP 2014-004574 A Summary of the Invention [Problem to be solved by the invention]
[0007] Thus, it has been proposed to apply tantalum oxide particles to various applications including capacitors, optical coatings, and photocatalysts. In these applications, fine, highly crystalline, spherical tantalum oxide particles are sometimes desired. For example, when an ink containing tantalum oxide particles is applied and heat-treated to produce a tantalum oxide film for optical applications, fine, highly crystalline, and spherical tantalum oxide particles are desired. This is because the use of spherical particles makes the applied film dense. In addition, fine and highly crystalline tantalum oxide particles are desired for photocatalyst applications. This is because if the crystallinity of the particles is low, electrons and holes (positive holes) are recombined at lattice defects in the particles, which reduces the catalytic activity. In addition, fine particles have a high specific surface area, so there are many active sites and they have excellent catalytic performance.
[0008] However, with the techniques proposed in the past, it was difficult to obtain spherical tantalum oxide particles that are nano-level fine and highly crystalline. That is, with the conventional manufacturing methods, in order to obtain tantalum oxide particles with high crystallinity, high-temperature and long-term sintering treatment was required. Therefore, grain growth and sintering of the tantalum oxide particles progressed during the sintering treatment, resulting in coarsening of the particles, making it difficult to obtain particles with a high specific surface area.
[0009] The present inventors have conducted extensive research in light of these problems, and as a result have discovered that nano-sized, approximately spherical tantalum oxide particles with good crystallinity can be obtained by carrying out production under specific conditions using a chemical vapor reaction method.
[0010] The present invention was completed based on these findings, and an object of the present invention is to provide nano-sized, approximately spherical tantalum oxide particles with excellent crystallinity, and a method for producing the same. [Means for solving the problem]
[0011] The present invention includes the following aspects (1) to (8). In other words, "X~Y" is synonymous with "greater than or equal to X and less than or equal to Y."
[0012] (1) Approximately spherical crystalline tantalum oxide particles having an average particle size (Dm) of 20 nm or more and 500 nm or less and a crystallite size (CS) of 10 nm or more.
[0013] (2) The crystalline tantalum oxide particles according to (1) above, wherein the crystal form of the crystalline tantalum oxide particles is at least one of an orthorhombic β type and a hexagonal δ type.
[0014] (3) The crystalline tantalum oxide particles according to (1) or (2) above, wherein the carbon content of the crystalline tantalum oxide particles is 3.0 mass % or less.
[0015] (4) Crystalline tantalum oxide particles according to any one of (1) to (3) above, having a ratio of crystallite size (CS) to average particle size (Dm) of 0.05 or more.
[0016] (5) A method for producing crystalline tantalum oxide particles by a chemical vapor reaction method, comprising the steps of: providing a tantalum source; heating and vaporizing the tantalum source to generate a tantalum-containing gas; and a step of maintaining the tantalum-containing gas at a temperature of 600° C. or more and 1200° C. or less under a pressure of 500 Pa or more and 50,000 Pa or less to cause thermal decomposition and oxidation reaction, thereby producing substantially spherical crystalline tantalum oxide particles having an average particle size of 20 nm or more and 500 nm or less and a crystallite size of 10 nm or more; A method comprising:
[0017] (6) The method according to (5) above, wherein the tantalum source is at least one selected from the group consisting of tantalum pentamethoxide, tantalum pentaethoxide, tantalum penta-n-propoxide, tantalum pentaisopropoxide, tantalum penta-n-butoxide, tantalum chloride, and tantalum fluoride.
[0018] (7) The method according to (5) or (6) above, wherein the crystal form of the crystalline tantalum oxide particles is at least one of an orthorhombic β type and a hexagonal δ type.
[0019] (8) The method according to any one of (5) to (7) above, wherein the carbon content of the crystalline tantalum oxide particles is 2.0 mass % or less. Effect of the Invention
[0020] According to the present invention, there are provided nano-sized, approximately spherical tantalum oxide particles having good crystallinity, and a method for producing the same. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a schematic diagram of a powder production apparatus used for synthesis by a chemical vapor reaction method. [Diagram 2] 4 shows a TEM image of tantalum oxide particles (Example 2). [Diagram 3] 4 shows a TEM image of tantalum oxide particles (Example 5). [Figure 4] 1 shows an XRD chart of tantalum oxide particles (Example 2). [Diagram 5] 1 shows an XRD chart of tantalum oxide particles (Example 4). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.
[0023] 1. Tantalum oxide particles The tantalum oxide particles of this embodiment are crystalline. Whether or not the particles are crystalline can be determined by subjecting the particles to X-ray diffraction (XRD) analysis. If a sharp diffraction peak based on crystals is clearly observed in an X-ray diffraction chart, it can be determined that the particles are crystalline. In this specification, the term "particle" refers to an independent particle or an aggregate of multiple independent particles. When the particle is an aggregate of multiple particles, the particle is synonymous with powder.
[0024] The tantalum oxide particles of this embodiment are substantially spherical in shape. By making the particle shape substantially spherical, a dense coating film can be obtained using the tantalum oxide particles. That is, if the particle shape is amorphous, the number of contact points between the particles increases during coating. Furthermore, the particles physically interlock with each other, preventing their movement. As a result, many voids are generated in the coating film, inhibiting densification. In contrast, by using substantially spherical particles, the particles can move smoothly during coating, and as a result, a highly packed coating film can be obtained. In this specification, substantially spherical means particles with an average aspect ratio of 1.5 or less. The average aspect ratio is preferably 1.4 or less, more preferably 1.3 or less.
[0025] The tantalum oxide particles of this embodiment have an average particle diameter (Dm) of 20 nm or more and 500 nm or less. If the average particle diameter is less than 20 nm, even if an ink containing the particles is applied to prepare a fired film, the particles tend to aggregate during sintering and become islands in the sea. Therefore, it may be difficult to obtain a dense fired film. In addition, the crystallite diameter becomes excessively small, resulting in low crystallinity. From the viewpoint of obtaining a dense fired film and excellent crystallinity, the average particle diameter may be 50 nm or more, 100 nm or more, 150 nm or more, 200 nm or more, 250 nm or more, or 300 nm or more. On the other hand, if the average particle diameter exceeds 500 nm, the particles become too coarse, resulting in a small sintering driving force. Therefore, it may be difficult to obtain a dense fired film. In addition, the specific surface area becomes too small, which is unsuitable in terms of catalytic activity. The average particle size may be 450 nm or less, 400 nm or less, 350 nm or less, 300 nm or less, 250 nm or less, or 200 nm or less. The average particle size is determined by observing tantalum oxide particles using a transmission electron microscope (TEM), measuring the particle size from the TEM observation image by image processing, and calculating the average particle size of 100 particles.
[0026] The tantalum oxide particles of this embodiment have a crystallite size (CS) of 10 nm or more. The crystallite size is an index of the crystallinity of the particles, and it can be said that the larger the crystallite size, the fewer the lattice defects and the higher the crystallinity. If the crystallite size is less than 10 nm, the crystallinity may decrease and the catalytic activity of the particles may be insufficient. This is because particles with low crystallinity have lattice defects in the particles, and electrons and holes generated when used as a catalyst recombine at the defects, which adversely affects the catalytic activity. In particular, amorphous particles have crystallites that are so small that they cannot be measured, and catalytic activity cannot be expected. From the viewpoint of crystallinity, the crystallite size may be 40 nm or more, 45 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, or 100 nm or more. On the other hand, if the crystallite size is large, the particle size will inevitably be large. If the crystallite size is excessively large, the number of active sites will decrease with a decrease in the specific surface area, and even if a co-catalyst is supported, the catalytic performance may not be improved. From the viewpoint of the specific surface area, the crystallite diameter may be 300 nm or less, 200 nm or less, 100 nm or less, 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, or 50 nm or less. The crystallite diameter can be calculated by analyzing tantalum oxide particles by X-ray diffraction (XRD), determining the full width at half maximum (FWHM) of the (001) diffraction peak of tantalum oxide (Ta2O5) in the XRD chart, and introducing the obtained FWHM value into Scherrer's formula. Although the crystallite diameter is a guide to the size of the crystallites in the particles, the measurement method and calculation method are different from the average particle diameter. Therefore, the crystallite diameter is not necessarily equal to or less than the average particle diameter.
[0027] The tantalum oxide particles preferably have at least one of an orthorhombic β-type and a hexagonal δ-type crystal form. Tantalum oxide is known to have α-type, β-type, and δ-type crystal forms. The α-type is an unstable phase that forms at relatively high temperatures, whereas the β-type and δ-type are stable phases that form at low temperatures. The β-type tantalum oxide has an orthorhombic crystal form, and the δ-type tantalum oxide has a hexagonal crystal form.
[0028] The tantalum oxide particles preferably have a ratio (CS / Dm) of the crystallite size (CS) to the average particle size (Dm) of 0.05 or more. By increasing CS / Dm, the crystallinity of the particles can be further increased. From the viewpoint of crystallinity, CS / Dm may be 0.10 or more, 0.15 or more, 0.20 or more, 0.25 or more, 0.30 or more, or 0.35 or more. The higher CS / Dm is, the more preferable, but it is typically 1.50 or less.
[0029] The tantalum oxide particles may contain other components in addition to tantalum (Ta) and oxygen (O). However, in order to fully exert properties such as catalytic performance, it is preferable that the content of other components is small. The content of other components may be 10.0 mass% or less, 5.0 mass% or less, 2.0 mass% or less, 1.0 mass% or less, 0.5 mass% or less, or 0.1 mass% or less.
[0030] In particular, it is preferable that the tantalum oxide particles have a low carbon content. When tantalum oxide particles are synthesized using a carbon (C)-containing tantalum source, the synthesized tantalum oxide particles may contain carbon components (carbon, organic compounds) derived from the raw materials. If such carbon components are present on the particle surface, the number of active sites may decrease, and the catalytic performance may be reduced. From the viewpoint of catalytic performance, the carbon content may be 5.0 mass% or less, 3.0 mass% or less, 1.5 mass% or less, 1.0 mass% or less, 0.5 mass% or less, or 0.1 mass% or less. The carbon content can be determined by analyzing the particles using thermogravimetry-mass spectrometry or oxygen flow combustion-infrared absorption spectrometry.
[0031] 2. Method for producing tantalum oxide particles The tantalum oxide particles of this embodiment are not limited in the manufacturing method as long as they satisfy the above-mentioned requirements. However, it is preferable to synthesize them by a chemical vapor reaction method. The chemical vapor reaction method is a method in which a heated and vaporized raw material is introduced into a reaction chamber together with a carrier gas, and a reaction is caused to proceed by heating in the reaction chamber. The vaporized raw material particles are thermally decomposed in the reaction chamber to become tantalum oxide, and the tantalum oxide grows to become tantalum oxide particles.
[0032] FIG. 1 shows a schematic diagram of a powder manufacturing apparatus suitable for use in a chemical vapor reaction method. The powder manufacturing apparatus (100) includes a raw material chamber (10), a reaction chamber (20), and a connecting pipe (30) connecting the raw material chamber (10) and the reaction chamber (20). A raw material container (12) capable of storing a compound that is a raw material for tantalum oxide particles is disposed in the raw material chamber (10), and a raw material chamber heater (14) for vaporizing the raw material is disposed around the raw material chamber (10). Furthermore, a carrier gas inlet (16) is disposed in the raw material chamber (10), and a carrier gas is introduced through the carrier gas inlet (16). A reaction chamber connecting port (18) is disposed on the wall surface of the raw material chamber (10) facing the carrier gas inlet (16). The reaction chamber connecting port (18) is communicated with a raw material inlet (22) of the reaction chamber (20) via the connecting pipe (30). The connecting pipe (30) is equipped with a valve (32). In the reaction chamber (20), an exhaust port (26) equipped with a recovery filter (24) is provided on the wall surface opposite to the wall surface on which the raw material inlet (22) is provided. In addition, a reaction heater (28) is provided around the reaction chamber (20). The reaction in the reaction chamber (20) is carried out under a reduced pressure atmosphere. Therefore, it is preferable that the raw material chamber (10), the reaction chamber (20), and the connecting pipe (30) have a structure capable of withstanding a reduced pressure atmosphere.
[0033] The particularly preferred method for producing the tantalum oxide particles of this embodiment includes the following steps: a step of preparing a tantalum source (preparation step), a step of heating and vaporizing the prepared tantalum source to generate a tantalum-containing gas (gasification step), and a step of maintaining the tantalum-containing gas at a temperature of 600°C to 1200°C under a pressure of 500 Pa to 50,000 Pa to cause thermal decomposition and oxidation reaction, thereby generating substantially spherical crystalline tantalum oxide particles with an average particle size (Dm) of 20 nm to 500 nm and a crystallite size of 10 nm or more (reaction step).Details of each step are described below.
[0034] <Preparation process> In the preparation step, a tantalum (Ta) source is prepared. As the tantalum source, an organic tantalum compound such as tantalum alkoxide (tantalum pentamethoxide, tantalum pentaethoxide, tantalum penta-n-propoxide, tantalum pentaisopropoxide, tantalum penta-n-butoxide, etc.) can be used. Alternatively, an inorganic tantalum compound such as tantalum chloride or tantalum fluoride can be used. However, when the produced tantalum oxide particles are used for photocatalytic purposes, it is desirable to use a tantalum source that does not contain a halogen element. This is because if a halogen element remains in the tantalum oxide particles, the catalytic activity may be lost due to the halogen element.
[0035] <Gasification process> In the gasification process, the prepared tantalum source is heated and vaporized to generate a tantalum-containing gas. Specifically, the raw material chamber is heated using a raw material chamber heater, and the tantalum source loaded in the raw material container is vaporized. In this specification, vaporization is a concept that includes sublimation. Then, a carrier gas is introduced into the raw material chamber, and the generated tantalum-containing gas is introduced into the reaction chamber through a connecting tube. In the reaction chamber, the tantalum-containing gas is thermally decomposed into tantalum oxide in the subsequent reaction process, and the generated tantalum oxide grows into tantalum oxide particles.
[0036] Gasification parameters such as the raw material heating temperature, raw material chamber gas pressure, and carrier gas flow rate in the gasification process are controlled so that the average particle size of the tantalum oxide particles finally obtained is 20 nm or more and 500 nm or less. The optimal values of the gasification parameters depend on the size and structure of the equipment, so it is difficult to determine them in general. Therefore, the optimal values can be determined depending on the equipment.
[0037] The raw material heating temperature affects the vaporization or sublimation of the tantalum source. Therefore, by controlling the raw material heating temperature, the amount of tantalum-containing gas generated and the amount introduced into the reaction chamber can be adjusted. If the amount of tantalum-containing gas introduced is large, the average particle size of the obtained tantalum oxide particles becomes small, and if the amount of gas introduced is small, the average particle size becomes large. In the reaction chamber, the tantalum oxide particles grow by adsorbing and decomposing the tantalum-containing gas around the fine tantalum oxide particles as nuclei. If the amount of tantalum-containing gas introduced is small, the number of fine oxide particles that become nuclei decreases. Therefore, the average particle size becomes large. The lower the raw material heating temperature, the smaller the amount of tantalum-containing gas generated, and therefore the larger the average particle size of the tantalum oxide particles. On the other hand, the higher the raw material heating temperature, the greater the amount of tantalum-containing gas generated, and therefore the smaller the average particle size. The raw material heating temperature is preferably not less than the vaporization start temperature of the tantalum source and not more than the vaporization completion temperature. The vaporization start temperature is the temperature at which the mass loss begins when the tantalum source is thermally analyzed using a thermogravimetry (TG), and is close to its boiling point if the tantalum source is liquid. On the other hand, the vaporization completion temperature is the temperature at which the tantalum source disappears. The amount of tantalum-containing gas generated varies depending on the configuration of the device, but is preferably 1 g / hour or less.
[0038] The gas pressure in the raw material chamber also affects the vaporization or sublimation of the tantalum source. Therefore, the amount of tantalum-containing gas generated and the average particle size of tantalum oxide particles can be adjusted by controlling the gas pressure in the raw material chamber. That is, the lower the gas pressure in the raw material chamber, the longer the residence time of the tantalum-containing gas in the reaction chamber, and the higher the tantalum concentration at the time of nucleation. Therefore, the amount of nucleation increases and the average particle size decreases. The gas pressure in the raw material chamber is preferably 50,000 Pa or less. By maintaining the raw material chamber under a reduced pressure atmosphere, it becomes possible to easily control the vaporization or sublimation of the tantalum source.
[0039] The flow rate of the carrier gas also affects the average particle size of the tantalum oxide particles. When the flow rate is high, the residence time of the tantalum-containing gas in the reaction chamber is short, and as a result, the average particle size becomes large. On the other hand, when the flow rate is low, the average particle size becomes small. It is preferable to control the flow rate of the carrier gas so that the time required for the tantalum source to reach the reaction temperature after reaching the reaction chamber is 0.01 to 20 seconds, and the residence time in the reaction chamber is 0.1 to 30 seconds. In addition, a gas containing an inert gas such as argon (Ar) can be used as the carrier gas. The carrier gas is preferably argon (Ar) or a mixed gas of argon (Ar) and oxygen (O2), and is particularly preferably a mixed gas with an oxygen concentration of 1 to 20% by volume. By setting the oxygen concentration to 1% by volume or more, it is possible to promote the thermal decomposition of the tantalum source and prevent impurities such as carbon from remaining in the tantalum oxide particles. In addition, by setting the oxygen concentration to 20% by volume or less, a rapid oxidation reaction can be suppressed and coarsening of the tantalum oxide particles can be prevented.
[0040] <Reaction process> In the reaction process, the tantalum-containing gas is maintained at a temperature of 600°C to 1200°C under a pressure of 500 Pa to 50,000 Pa to cause thermal decomposition and oxidation. This produces roughly spherical crystalline tantalum oxide particles with an average particle size of 20 nm to 500 nm and a crystallite size of 10 nm or more. Specifically, the tantalum-containing gas introduced into the reaction chamber is heated using a reaction heater. As a result, thermal decomposition and oxidation reactions of the tantalum-containing gas occur, producing fine tantalum oxide particles that act as initial nuclei. When the tantalum-containing gas is continuously introduced, the tantalum-containing gas is adsorbed around the produced fine particles, and further thermal decomposition and oxidation reactions occur, causing the tantalum oxide particles to grow.
[0041] The pressure in the reaction process (reaction pressure) affects the shape and production rate of the reaction product. If the reaction pressure is less than 500 Pa, the reaction product will be in the form of a film, making it difficult to obtain tantalum oxide particles. From the viewpoint of particle properties, the reaction pressure may be 1000 Pa or more, 1500 Pa or more, or 2000 Pa or more. On the other hand, if the reaction pressure exceeds 50000 Pa, although tantalum oxide particles can be obtained, the production rate will be significantly slowed down, which may hinder productivity. From the viewpoint of productivity, the reaction pressure may be 10000 Pa or less, 7500 Pa or less, or 5000 Pa or less.
[0042] The holding temperature (reaction temperature) affects the particle size, crystallinity, and amount of residual impurities of the tantalum oxide particles. If the reaction temperature is less than 600°C, it is difficult to obtain tantalum oxide particles with excellent crystallinity. In addition, the decomposition reaction of the tantalum-containing gas does not proceed sufficiently, and unreacted carbon components as impurities may remain in the particles. From the viewpoint of crystallinity and impurities, the reaction temperature may be 650°C or more, 700°C or more, 750°C or more, 800°C or more, 850°C or more, 900°C or more, 950°C or more, or 1000°C or more. On the other hand, if the reaction temperature is more than 1200°C, the tantalum oxide particles become coarse. As a result, the average particle size may exceed 500 nm, or coarse particles with a particle size of 2 μm or more may be generated. From the standpoint of particle size, the reaction temperature may be 1100°C or less, 1050°C or less, 1000°C or less, 950°C or less, 900°C or less, 850°C or less, 800°C or less, 750°C or less, or 700°C or less.
[0043] In this manner, the tantalum oxide particles of the present embodiment can be produced. The obtained tantalum oxide particles are collected in a collection filter in the reaction chamber. The collected particles are collected from the filter to obtain tantalum oxide particles.
[0044] Although the manufacturing method by chemical vapor phase reaction method has been mainly described, the tantalum oxide particles of this embodiment are not limited to those manufactured by chemical vapor phase reaction method. For example, techniques such as aqueous solution thermal decomposition method, solid-phase reaction method, sol-gel method, complex polymerization method, and hydrothermal reaction method may be used. Among these, the aqueous solution thermal decomposition method is a technique in which a metal-containing precursor is used as a raw material, and the aqueous solution containing the metal-containing precursor is heated to evaporate the water as a solvent, thereby causing a dehydration polycondensation reaction of the metal-containing precursor. Any technique may be adopted as long as tantalum oxide particles that satisfy the requirements of this embodiment can be obtained. EXAMPLES
[0045] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0046] (1) Production of tantalum oxide particles [Example 1] In Example 1, tantalum ethoxide was used as the tantalum source, and tantalum oxide particles were synthesized by a chemical vapor reaction method using the powder production apparatus shown in Figure 1. This powder production apparatus had an internal volume of 400 cm 3 The raw material chamber and the internal volume are 200 cm 3 Specifically, the particles were produced in the following manner.
[0047] First, tantalum ethoxide (tantalum source) was charged into the raw material container in the raw material chamber. After evacuating the reaction chamber and the raw material chamber with the valve open, heating of the reaction chamber was started without flowing carrier gas, and it was waited for 1 to 2 hours until the reaction chamber reached the specified temperature. When the reaction chamber reached the specified temperature, carrier gas was flowed, and then heating of the raw material chamber was started. It was waited for 15 to 25 minutes until the raw material chamber reached the specified temperature. After the raw material chamber reached the specified temperature, it was maintained in that state for 1 hour. Precipitation of tantalum oxide particles began in the reaction chamber due to the heating of the raw material chamber. At that time, the temperatures of the raw material chamber (outside) and the reaction tube inlet (inside) were measured using a thermocouple, and were taken as the raw material heating temperature and the reaction temperature, respectively. The precipitated tantalum oxide particles were collected by the filter in the reaction chamber. After the precipitation reaction was completed, the tantalum oxide particles collected by the filter were recovered.
[0048] In Example 1, a mixed gas containing 90 vol% argon (Ar) and 10 vol% oxygen (O2) was used as the carrier gas, and the flow rate of the carrier gas was set to 280 SCCM. The raw material heating temperature was 220°C, the gas pressure in the reaction chamber was 5000 Pa, and the reaction temperature was 1025°C. Furthermore, the evaporation amount of tantalum ethoxide (tantalum source) was 1 g / hour.
[0049] [Example 2] In Example 2, the reaction temperature was set to 938° C. Other than that, tantalum oxide particles were produced in the same manner as in Example 1.
[0050] [Example 3] In Example 3, the reaction temperature was set to 830° C. Other than that, tantalum oxide particles were produced in the same manner as in Example 1.
[0051] [Example 4] In Example 4, the reaction temperature was set to 729° C. Except for this, tantalum oxide particles were produced in the same manner as in Example 1. In Example 4, the evaporation rate of tantalum ethoxide (tantalum source) in the raw material chamber was 0.54 g / hour.
[0052] [Example 5] In Example 5, argon (Ar) gas was used as the carrier gas. Also, the reaction temperature was set to 824 °C. Tantalum oxide particles were produced in the same manner as in Example 1 except for this.
[0053] [Example 6] In Example 6, the raw material heating temperature was 200 °C, the gas pressure in the reaction chamber was 2000 Pa, and the reaction temperature was 629 °C. Tantalum oxide particles were produced in the same manner as in Example 1 except for this. Note that the amount of tantalum oxide particles obtained in Example 6 was small, and thermal analysis described later could not be performed.
[0054] [Comparative Example 1] In Comparative Example 1, the raw material heating temperature was 200 °C, the gas pressure in the reaction chamber was 2000 Pa, and the reaction temperature was 580 °C. Tantalum oxide particles were produced in the same manner as in Example 1 except for this. Note that the tantalum oxide particles according to Comparative Example 1 were dark gray, and evaluations other than visual observation described later were not performed.
[0055]
Table 1
[0056] (2) Evaluation For the tantalum oxide particles obtained in Examples 1 to 6 and Comparative Example 1, evaluations of various properties were performed as follows.
[0057] <Visual Observation> The tantalum oxide particles were visually observed to examine their color tone.
[0058] <TEM Observation> The tantalum oxide particles were observed using a scanning transmission electron microscope (STEM; Hitachi High-Tech Corporation, HD2700). Then, the particle sizes of 100 particles were measured, and the average value was taken as the average particle size.
[0059] <xrd> X-ray diffraction (XRD) analysis of tantalum oxide particles was performed using a powder X-ray diffractometer (Spectris Co., Ltd., X’Pert PRO MRD), and the generated phase was identified and its crystallinity was evaluated based on the obtained results. CuKα radiation was used as the X-ray source for the analysis.
[0060] Also, based on the XRD analysis results, the crystallite size of the tantalum oxide particles was calculated. Specifically, the XRD chart obtained by the analysis was analyzed, and the full width at half maximum (FWHM) of the (001) diffraction peak of tantalum oxide (Ta2O5) existing near 2θ = 22.9° was determined. Then, the obtained FWHM value was introduced into Scherrer's formula to calculate the crystallite size.
[0061] <Thermal analysis> Thermogravimetric analysis (TG; Bruker - AXS, 2020SA) was performed on the tantalum oxide particles to examine the amount of unreacted substances in the particles. The thermal analysis was carried out under an N2 - 21% O2 gas atmosphere at a heating rate of 20 °C / min.
[0062] (3) Evaluation results
[0063] <Visual observation> The color tones of the tantalum oxide particles of Examples 1 to 6 are summarized in Table 2. White particles were obtained in Examples 1 to 4, while light gray particles were obtained in Examples 5 and 6. This was considered to be due to the residual organic matter. In Comparative Example 1, dark gray particles were obtained. This color was considered to be due to the higher carbon content compared to the examples. <TEM observation> TEM images of the tantalum oxide particles of Example 2 and Example 5 are shown in FIGS. 2 and 3, respectively. The obtained particles were substantially spherical in shape. Also, grain boundaries were observed inside the particles, confirming that they were polycrystalline particles. Most of the particles had not grown in a net-like manner and were not combined with other particles. It was considered that the characteristics of particles growing in the gas phase during transportation were exhibited. When the aspect ratios of 10 particles of Example 2 were measured, the average aspect ratio was 1.16 (minimum 1.01, maximum 1.61).
[0064] <xrd> The XRD chart of the tantalum oxide particles of Example 2 is shown in Figure 4. The diffraction peak angle of this sample was consistent with the value of the standard diffraction data (JCPDS card 01-89-2843) of orthorhombic β-type tantalum oxide (β-Ta2O3). In addition, the diffraction peak was sharp, and it was confirmed that the crystallinity was good. Similar results were obtained with the tantalum oxide particles of Example 1.
[0065] The XRD chart of the tantalum oxide particles obtained in Example 4 is shown in Figure 5. The diffraction peak angle of this sample was consistent with the standard diffraction data (JCPDS card 19-1299) of hexagonal δ-type tantalum oxide (δ-Ta2O3). Similar results were obtained for the tantalum oxide particles of Examples 3, 5, and 6.
[0066] The crystallite diameters of the tantalum oxide particles obtained in Examples 1 to 6 are summarized in Table 2. The tantalum oxide particles of Comparative Example 1 were amorphous (non-crystalline), so the crystallite diameter could not be calculated. All of the crystallite diameters of Examples 1 to 6 were large, at 40 nm or more. In particular, Example 1, in which the reaction temperature during production was as high as 1025°C, had a very large crystallite diameter of over 100 nm. This demonstrated that the tantalum oxide particles of the example samples had excellent crystallinity.
[0067] <Thermal analysis> The mass loss rates at 1200° C. for the tantalum oxide particles obtained in Examples 1 to 6 are summarized in Table 2. In addition, in Table 2, samples with a mass loss rate of 3.0 mass % or less were determined to have "no" unreacted substances.
[0068] The mass loss rate of all the example samples was small, at 3.0 mass% or less. In particular, the mass loss rate of Example 1 was 0.0 mass%. It is believed that the raw material undecomposed tantalum ethoxide and its intermediate products remain in the synthesized tantalum oxide as unreacted carbon components, and these residues are detected as mass loss by thermal analysis. It was confirmed that the example samples contained almost no unreacted carbon components derived from the raw materials.
[0069] [Table 2] [Explanation of symbols]
[0070] 10 Raw material room 12 Raw material container 14 Raw material chamber heater 16 Carrier gas inlet 18 Reaction chamber connection port 20 Reaction chamber 22 Raw material input port 24 Collection filter 26 Exhaust port 28 Reaction heater 30 Connecting Pipe 32 Valve 100 Powder manufacturing equipment< / xrd> < / xrd>
Claims
1. Approximately spherical crystalline tantalum oxide particles having an average particle size (Dm) of 20 nm or more and 500 nm or less, a crystallite size (CS) of 10 nm or more and 300 nm or less, and a ratio of the crystallite size (CS) to the average particle size (Dm) of 0.20 or more.
2. 2. The crystalline tantalum oxide particles according to claim 1, wherein the crystal form of the crystalline tantalum oxide particles is at least one of an orthorhombic β type and a hexagonal δ type.
3. 3. The crystalline tantalum oxide particles according to claim 1, wherein the carbon content of the crystalline tantalum oxide particles is 3.0 mass % or less.
4. A method for producing crystalline tantalum oxide particles by a chemical vapor reaction method, comprising the steps of: providing a tantalum source; heating and vaporizing the tantalum source to generate a tantalum-containing gas; and a step of maintaining the tantalum-containing gas at a temperature of 600° C. or more and 1200° C. or less under a pressure of 500 Pa or more and 50,000 Pa or less to cause thermal decomposition and oxidation reaction, thereby producing substantially spherical crystalline tantalum oxide particles having an average particle size of 20 nm or more and 500 nm or less and a crystallite size of 10 nm or more and 300 nm or less; A method comprising:
5. 5. The method of claim 4, wherein the tantalum source is at least one selected from the group consisting of tantalum pentamethoxide, tantalum pentaethoxide, tantalum penta-n-propoxide, tantalum pentaisopropoxide, tantalum penta-n-butoxide, tantalum chloride, and tantalum fluoride.
6. The method according to claim 4 or 5, wherein the crystal form of the crystalline tantalum oxide particles is at least one of an orthorhombic β type and a hexagonal δ type.
7. The method according to any one of claims 4 to 6, wherein the carbon content of the crystalline tantalum oxide particles is 3.0% by mass or less.
Citation Information
Patent Citations
Method for producing particle of highly crystalline metal or metal oxide
JP2010007105A
Fine particle dispersion liquid containing tantalum oxide fine particle, tantalum oxide fine particle-resin composite, and method of producing the fine particle dispersion liquid and the fine particle-resin composite
JP2011116966A
Method for manufacturing tantalum oxide particle
JP2012111684A
Tantalum oxide particle and method for producing the same
JP2014004574A