Nail polish container

A polypropylene resin composition with specific antioxidants and light stabilizers addresses discoloration and thermal stability issues in nail polish containers, ensuring long-term stability and transparency.

JP7584228B2Active Publication Date: 2024-11-15KOSE CORPORATION +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020057681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-03-27
Publication Date
2024-11-15
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Polypropylene-based nail polish containers react with volatile components of the liquid inside, causing discoloration and lack long-term thermal stability, limiting design options to dark colors to hide discoloration.

Method used

A polypropylene resin composition is developed using specific antioxidants and light stabilizers, excluding hindered phenol, to enhance chemical resistance, moldability, barrier properties, and thermal stability, ensuring discoloration resistance.

Benefits of technology

The composition maintains product shape and appearance without discoloration, providing long-term thermal stability and transparency, suitable for nail polish containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584228000018
    Figure 0007584228000018
  • Figure 0007584228000019
    Figure 0007584228000019
  • Figure 0007584228000020
    Figure 0007584228000020
Patent Text Reader

Abstract

To provide a manicure container using a polypropylene resin composition excellent in chemical resistance, moldability, barrier properties, long-term thermal stability, physical property balance, and discoloration resistance.SOLUTION: A manicure container is composed of a container body 1 and a lid body 2 having a shaft body 3 with an application body 6 at the tip. At least part of the manicure container is a polypropylene resin composition having specific MFR, bending modulus, phosphorus-based antioxidation agent blending quantity, and hindered amine-based light stabilizer blending quantity, which substantially is not blended with hindered phenol.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nail polish container using a polypropylene resin composition which has excellent chemical resistance, moldability, barrier properties, long-term thermal stability, balance of physical properties and resistance to discoloration. [Background technology]

[0002] Propylene-based polymers are used in various applications, taking advantage of their excellent safety and hygiene, moldability, colorability, mechanical properties, chemical resistance, and barrier properties. In particular, they are used as cosmetic container materials because of their safety and hygiene, chemical resistance, and water vapor barrier properties. The cosmetics field includes makeup, skin care, and hair care, and one of the makeup applications is nail polish. Polypropylene and other materials are used as container materials for nail polish lids, but there is an issue that they react with the volatile components of the contents and discolor. For this reason, lids and other materials are currently colored in dark colors such as black so that discoloration is not noticeable. On the other hand, cosmetic containers are required to have high designability and high appearance, and there is also a demand for designs with light colors and transparency. Furthermore, although discoloration has been investigated in Patent Document 2, there was a problem in that long-term thermal stability could not be obtained unless a phenol-based antioxidant was used. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-175961 A [Patent Document 2] JP 2003-230427 A Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the above problems, the object of the present invention is to provide a nail polish container, and more specifically, to provide a nail polish container using a polypropylene resin composition which has excellent chemical resistance, moldability, barrier properties, long-term thermal stability, balance of physical properties, and discoloration resistance. [Means for solving the problem]

[0005] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that a polypropylene resin composition having specific properties and based on a propylene polymer, which contains specific antioxidants and light stabilizers in specific blend amounts, is an excellent material that does not discolor when used for nail polish containers, and is suitable as a nail polish container using a polypropylene resin composition having chemical resistance, moldability, barrier properties, long-term thermal stability, and an excellent balance of physical properties, thereby completing the present invention.

[0006] That is, the present invention provides a nail polish container using the following polypropylene resin composition, and in particular provides a nail polish container using a polypropylene resin composition having excellent resistance to discoloration.

[0007] [1] The nail polish container is composed of a container body and a lid body having a shaft body with an applicator body at the tip, and at least a part of the nail polish container is made of a polypropylene resin composition that is substantially free of hindered phenol and satisfies the following characteristics (i) to (iv). (i) The MFR measured in accordance with JIS K7210:1999, Appendix A, Table 1, Condition M, at a test temperature of 230°C and a nominal load of 2.16 kg is 0.5 to 120 g / 10 min. (ii) The flexural modulus in accordance with JIS K7171 is 150 MPa or more. (iii) 0.001 to 0.5 parts by weight of a phosphorus-based antioxidant is blended with 100 parts by weight of the polypropylene resin. (iv) 0.01 to 0.5 parts by weight of a hindered amine light stabilizer is blended with 100 parts by weight of polypropylene resin. [2] A nail polish container according to [1], wherein the polypropylene resin composition satisfies the following characteristic (v): (v) The polypropylene resin is a propylene homopolymer or a propylene-based copolymer consisting of propylene and an α-olefin content of 15% by weight or less. [3] The nail polish container according to [1] or [2], wherein the polypropylene resin composition has a haze of 50% or less at a wall thickness of 1 mm as measured in accordance with JIS K7136. [4] The nail polish container according to any one of [1] to [3], wherein the polypropylene resin composition further contains at least one nucleating agent selected from the group consisting of 0.10 to 0.50 parts by weight of a nucleating agent (a) represented by the following formula (1), 0.01 to 0.30 parts by weight of a nucleating agent (b) represented by the following formula (2), and 0.005 to 0.04 parts by weight of a nucleating agent (c) represented by the following formula (3), relative to 100 parts by weight of the polypropylene resin. [ka] (In the formula, n is an integer of 0 to 2, and R 1 ~R 5 are each independently the same or different and are hydrogen, halogen, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 20 carbon atoms, alkoxy having 1 to 20 carbon atoms, alkoxycarbonyl having 1 to 20 carbon atoms, or phenyl; R 6 is an alkyl group having 1 to 20 carbon atoms. [ka] (In the formula, R 1 is a direct bond, sulfur, an alkylene having 1 to 9 carbon atoms, or an alkylidene having 2 to 9 carbon atoms; R 2 and R 3are the same or different and each is hydrogen, an alkyl having 1 to 8 carbon atoms, or an alkylaryl having 7 to 9 carbon atoms; M is Li, Na, K, Mg, Ca, Zn, Al-OH, or Al; and n is the valence of M. When M is AlOH, n=2, and when M is Al, n=3. [ka] (In the formula, R 1 , R 2 and R 3 are, independently of each other, unsubstituted or substituted hydrocarbon radicals. [5] The nail polish container according to any one of [1] to [4], wherein the nail polish contains nitrocellulose as a component. Effect of the Invention

[0008] The nail polish container of the present invention is useful as a nail polish container that has the characteristics required of a nail polish container material, namely, the strength (rigidity) necessary to maintain the product shape, long-term thermal stability that does not cause problems such as deterioration or bleeding even when displayed on store shelves for long periods of time, barrier properties and chemical resistance to retain cosmetic solutions, moldability that allows for injection molding, excellent appearance that does not discolor, and in some cases transparency. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a partial cross-sectional view of an example of a nail polish container. [Diagram 2] FIG. 1 is a schematic diagram of a test using a sheet carried out for visual appearance evaluation in the examples (G). [Diagram 3] 1 is a flow sheet used to explain the production of a propylene-ethylene copolymer in the Examples. [Figure 4] FIG. 1 is a photograph of a test using a lid conducted for visual appearance evaluation in an embodiment (Comparative Example 1). [Diagram 5] 1 is a photograph of the sheet of Example 1 (control product) that was stored at room temperature during the test period. [Figure 6] 1 is a photograph of the sheet of Example 1 after testing. [Figure 7] 1 is a photograph of the lid (standard product) of Example 1 that was stored at room temperature during the test period. [Figure 8] 1 is a photograph of the lid of Example 1 after testing. [Figure 9] 1 is a photograph of the sheet of Example 2 (control product) that was stored at room temperature during the test period. [Figure 10] 1 is a photograph of the sheet after testing using the sheet of Example 2. [Figure 11] 1 is a photograph of the sheet of Example 3 (control product) that was stored at room temperature during the test period. [Figure 12] 1 is a photograph of the sheet after testing using the sheet of Example 3. [Figure 13] 1 is a photograph of the lid (standard product) of Example 3 that was stored at room temperature during the test period. [Figure 14] 1 is a photograph of the lid of Example 3 after testing. [Figure 15] 1 is a photograph of the sheet (standard product) of Comparative Example 1 that was stored at room temperature during the test period. [Figure 16] 1 is a photograph of the sheet after testing using the sheet of Comparative Example 1. [Figure 17] 1 is a photograph of the lid (standard product) of Comparative Example 1 that was stored at room temperature during the test period. [Figure 18] 1 is a photograph of the lid of Comparative Example 1 after testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The nail polish container of the present invention is characterized by having the properties required of a nail polish container material, namely, the strength (rigidity) necessary to maintain the product shape, long-term thermal stability that does not cause problems such as deterioration or bleeding even when displayed on store shelves for long periods of time, barrier properties and chemical resistance to retain cosmetic solutions, moldability that allows for injection molding, blow molding, etc., excellent appearance that does not discolor, and in some cases transparency. The nail polish container of the present invention will be described in detail below.

[0011] [1] Polypropylene resin composition for nail polish containers (1) Polypropylene resin used in polypropylene resin composition The polypropylene resin composition used in the nail polish container of the present invention has polypropylene resin as its main component, and the polypropylene resin is preferably a propylene-based polymer, such as a propylene homopolymer or a propylene-based copolymer consisting of propylene and an α-olefin having a content of 15% by weight or less, or may be a mixture thereof. From the viewpoint of rigidity, the propylene-based polymer is preferably a homopolymer, from the viewpoint of transparency related to color development, a random copolymer made of propylene and an α-olefin, and from the viewpoint of impact resistance against cracking due to dropping of the product, a block copolymer is preferable. The α-olefin used for copolymerization includes α-olefins having 2 to 20 carbon atoms other than propylene, such as ethylene, 1-butene, 1-hexene, and 1-octene. One or more types of α-olefins may be used to be copolymerized with propylene. Among these, ethylene and 1-butene are preferable. Ethylene is more preferable. In the case of a propylene-based copolymer containing ethylene, which is a more preferred α-olefin, the contents of propylene and ethylene are measured by the measurement method described in the examples below, i.e. 13 It is a value measured by infrared spectroscopy based on a calibration curve created by infrared spectroscopy using a reference material whose composition has been verified by C-NMR. Specific examples of the propylene polymer include propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, and propylene-1-butene-1-octene copolymer. These propylene polymers may be used in combination of two or more kinds. From the viewpoint of product rigidity, the α-olefin content of the propylene-based polymer is preferably 15% by weight or less, and when the propylene-based polymer is a random copolymer, the α-olefin content is more preferably 7% by weight or less, and even more preferably 5% by weight or less. The random copolymer may be a multi-stage polymer, and for example, in the case of a two-stage polymer, the first stage polymer is preferably a propylene homopolymer or a random copolymer comprising 5% by weight or less of an α-olefin, and the second stage polymer is preferably a random copolymer comprising 20% ​​by weight or less of an α-olefin. In addition, when the propylene-based polymer is a block copolymer, the content of α-olefin is more preferably 10% by weight or less from the viewpoint of product rigidity. In the case of a block copolymer, it is a multi-stage polymer, and for example, in the case of a two-stage polymer, the first stage polymer is preferably a propylene homopolymer or a random copolymer consisting of 2% by weight or less of α-olefin, and the second stage polymer is preferably a random copolymer consisting of 20% by weight to 80% by weight of α-olefin.

[0012] (2) Melt flow rate (MFR) according to JIS K7210 The melt flow rate (MFR) of the polypropylene resin composition used in the present invention is in the range of 0.5 to 120 g / 10 min, preferably 3 to 90 g / 10 min, more preferably 6 to 60 g / 10 min, as measured at a test temperature of 230° C. and a nominal load of 2.16 kg in accordance with JIS K7210:1999, Annex A, Table 1, Condition M. When the melt flow rate (MFR) is 0.5 g / 10 min or more, the molding processability is improved, and a product that is satisfactory can be obtained. When the melt flow rate (MFR) is 120 g / 10 min or less, the mechanical strength is improved and the appearance is improved due to sufficient kneading, and a product that is satisfactory can be obtained. The melt flow rate (MFR) of the propylene polymer to be incorporated in the polypropylene resin composition can also be measured by blending an appropriate amount of antioxidant in accordance with JIS K7210:1999, Annex A, Table 1, Condition M, at a test temperature of 230°C and a nominal load of 2.16 kg. The MFR of the propylene polymer is also preferably in the range of 0.5 to 120 g / 10 min. The melt flow rate (MFR) can be easily adjusted by adjusting the temperature and pressure, which are polymerization conditions when producing a propylene-based polymer, or by controlling the amount of hydrogen added in a method in which a chain transfer agent such as hydrogen is added during polymerization.

[0013] (3) Method for producing propylene polymer The method for producing a propylene-based polymer may be a method using a metallocene catalyst or a Ziegler catalyst, but it is preferable to use a metallocene catalyst in order to obtain bleeding resistance. When a Ziegler catalyst is used, bleeding may occur, especially when the random copolymer has a large amount of α-olefin and a high MFR. Examples of Ziegler catalysts include two-component catalysts consisting of a transition metal component, such as a titanium halide compound such as titanium trichloride, titanium tetrachloride or trichloroethoxytitanium, or a contact product of the titanium halide compound with a magnesium compound such as a magnesium halide, and an organometallic component, such as an alkylaluminum compound or its halide, hydride or alkoxide, and further three-component catalysts in which an electron donor compound containing nitrogen, carbon, phosphorus, sulfur, oxygen, silicon or the like is added to any of the above components. Examples of the metallocene catalyst include (r)-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4H-azulenyl}]zirconium, and more specifically, the catalyst is composed of (i) a transition metal compound of Group 4 of the periodic table containing a ligand having a cyclopentadienyl skeleton (so-called metallocene compound), (ii) a cocatalyst capable of reacting with the metallocene compound to activate it to a stable ionic state, and, if necessary, (iii) an organoaluminum compound, and any known catalyst can be used. The metallocene compound is preferably a bridged metallocene compound capable of stereoregular polymerization of propylene, and more preferably a bridged metallocene compound capable of isoregular polymerization of propylene. Metallocene compounds (i) are disclosed, for example, in JP-A-60-35007, JP-A-61-130314, JP-A-63-295607, JP-A-1-275609, JP-A-2-41303, JP-A-2-131488, JP-A-2-76887, JP-A-3-163088, JP-A-4-300887, JP-A-4-211694, JP-A-5-43616, JP-A-5-209013, JP-A-6-239914, JP-T-H7-504934, and JP-A-8-85708.

[0014] Examples of the polymerization method for producing a propylene-based polymer include a slurry polymerization method using an inert solvent in the presence of the above catalyst, a solution polymerization method, a gas phase polymerization method substantially without using a solvent, and a bulk polymerization method using a polymerization monomer as a solvent. For example, in the case of a slurry polymerization method, the polymerization can be carried out in an inert hydrocarbon such as n-butane, isobutane, n-pentane, isopentane, hexane, heptane, octane, cyclohexane, benzene, toluene, or xylene. In the case of a bulk polymerization method, the polymerization can be carried out in a liquid polymerizable monomer. The polymerization temperature is usually -80 to 150°C, and preferably 40 to 120°C. The polymerization pressure is preferably 1 to 60 atm (0.10 to 6.08 MPa), and the molecular weight of the resulting propylene-based polymer can be adjusted with hydrogen or other known molecular weight regulators. The polymerization is carried out by a continuous or batch reaction, and the conditions may be those usually used. Furthermore, the polymerization reaction may be carried out in one stage or multiple stages.

[0015] (4) Flexural modulus according to JIS K7171 The polypropylene resin composition used in the present invention has a flexural modulus in the range of 150 MPa or more, preferably 800 MPa or more, more preferably 1100 MPa or more, and even more preferably 1500 MPa or more, according to JIS K7171. When the flexural modulus is 150 MPa or more, molding is easy, and the product rigidity required for a nail polish container is obtained. The flexural modulus can be adjusted by the α-olefin content of the propylene polymer blended in the polypropylene resin composition, etc. The flexural modulus can be increased by reducing the α-olefin content.

[0016] (5) Haze according to JIS K7136 From the viewpoint of transparency related to color development, the polypropylene resin composition used in the present invention preferably has a haze at a thickness of 1 mm, measured in accordance with JIS K7136, in the range of 50% or less, more preferably 40% or less, and even more preferably 30% or less. The haze can be adjusted by the α-olefin content of the propylene polymer blended in the polypropylene resin composition, the nucleating agent, etc. The haze can be reduced by increasing the α-olefin content or blending a nucleating agent.

[0017] (6) Phosphorus-based antioxidants The polypropylene resin composition used in the present invention is prepared by blending 0.001 to 0.5 parts by weight of a phosphorus-based antioxidant with respect to 100 parts by weight of polypropylene resin, and the blending amount of the phosphorus-based antioxidant is preferably 0.01 to 0.20 parts by weight, more preferably 0.02 to 0.14 parts by weight. When the blending amount of the phosphorus-based antioxidant is 0.001 parts by weight or more, thermal stability during processing is sufficiently exhibited, and when it is 0.5 parts by weight or less, discoloration and burning can be suppressed. In addition, when the blending amount of the phosphorus-based antioxidant is 0.5 parts by weight or less, it is advantageous in terms of cost-effectiveness (cost performance) regarding thermal stability during processing. Specific examples of phosphorus-based antioxidants include bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, di-stearyl-pentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene diphosphonite, and tetrakis(2,4-di-t-butyl-5-methylphenyl)-4,4'-biphenylene diphosphonite. Of these phosphorus-based antioxidants, tris(2,4-di-t-butylphenyl)phosphite (BASF, trade name: Irgafos 168) is particularly preferred from the viewpoints of its performance as a processing stabilizer, its resistance to hydrolysis of the additive itself, and its resistance to scorching and discoloration.

[0018] (7) Hindered amine light stabilizers The polypropylene resin composition used in the present invention is obtained by blending 0.01 to 0.5 parts by weight of a hindered amine light stabilizer with respect to 100 parts by weight of polypropylene resin, and the blending amount of the hindered amine light stabilizer is preferably 0.02 to 0.20 parts by weight, more preferably 0.03 to 0.15 parts by weight. If the hindered amine light stabilizer is 0.01 parts by weight or more, long-term thermal stability is sufficiently exhibited, and if it is 0.5 parts by weight or less, the occurrence of bleeding can be prevented. In addition, if the blending amount of the hindered amine light stabilizer is 0.5 parts by weight or less, it is advantageous in terms of cost-effectiveness (cost performance) regarding long-term thermal stability. Representative examples of hindered amine light stabilizers include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, poly{[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino]}, N,N'-bis(3-aminopropyl)ethylenediamine-2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate, and dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate. Of these, it is preferable to incorporate a high molecular weight type such as dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate (manufactured by BASF, trade name: Tinuvin 622) from the viewpoint of preventing bleeding.

[0019] (8) Hindered phenols The polypropylene resin composition used in the present invention does not substantially contain hindered phenol. Specifically, the amount of hindered phenol must be less than 0.001 parts by weight, preferably less than 0.0005 parts by weight, and more preferably 0 parts by weight, per 100 parts by weight of polypropylene resin. Hindered phenol may cause discoloration due to reaction with components contained in nail polish and components contained in volatilized nitrocellulose. It may cause discoloration due to reaction with volatile components contained in nitrocellulose. Here, examples of the hindered phenol include phenol-based antioxidants used in polypropylene resins, and specific examples thereof include tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethane, and the like. tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 6-(4-hydroxy-3,5-di-t-butylanilino)-2,4-bis(n-octylthio)-1,3,5-triazine, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, and the like.

[0020] (9) Nucleating agents The polypropylene resin composition used in the present invention is preferably prepared by blending, relative to 100 parts by weight of the polypropylene resin, at least one nucleating agent selected from the group consisting of 0.10 to 0.50 parts by weight of a nucleating agent (a) represented by the following formula (1), 0.01 to 0.30 parts by weight of a nucleating agent (b) represented by the following formula (2), and 0.005 to 0.04 parts by weight of a nucleating agent (c) represented by the following formula (3):

[0021] [ka]

[0022] (In the formula, n is an integer of 0 to 2, and R 1 ~R 5 are each independently the same or different and are hydrogen, halogen, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 20 carbon atoms, alkoxy having 1 to 20 carbon atoms, alkoxycarbonyl having 1 to 20 carbon atoms, or phenyl; R 6 is an alkyl group having 1 to 20 carbon atoms.

[0023] Among the nucleating agents of formula (1), a representative commercially available product is Milad NX8000J (manufactured by Milliken & Company). Its chemical structure is as shown in formula (1-1) below. The molecular weight of this nucleating agent is 484. This substance is extremely stable thermally and chemically, and has the excellent characteristic of hardly decomposing thermally even at molding temperatures. This is very preferable because it does not cause the problem of decomposition products bleeding out onto the surface of the molded product and deteriorating its appearance.

[0024] [ka]

[0025] The amount of the nucleating agent (a) to be blended in the polypropylene resin composition used in the present invention is preferably 0.10 to 0.50 parts by weight, more preferably 0.10 to 0.40 parts by weight, and even more preferably 0.20 to 0.35 parts by weight, based on 100 parts by weight of the polypropylene resin. When the amount of the nucleating agent (a) is 0.10 parts by weight or more, it is expected that rigidity and transparency will be exhibited, and when it is 0.50 parts by weight or less, there is less concern about bleeding onto the surface of the molded article, which is advantageous in terms of cost-effectiveness (cost performance) and elution in terms of rigidity and transparency.

[0026] [ka]

[0027] (In the formula, R1 is a direct bond, sulfur, an alkylene having 1 to 9 carbon atoms, or an alkylidene having 2 to 9 carbon atoms; R 2 and R 3 are the same or different and each is hydrogen, an alkyl having 1 to 8 carbon atoms, or an alkylaryl having 7 to 9 carbon atoms; M is Li, Na, K, Mg, Ca, Zn, Al-OH, or Al; and n is the valence of M. When M is AlOH, n=2, and when M is Al, n=3.

[0028] Specifically, examples of the compound represented by formula (2) include hydroxyaluminum bis[2,2'-methylene-bis(4,6-dimethylphenyl)phosphate], hydroxyaluminum bis[2,2'-ethylidene-bis(4,6-dimethylphenyl)phosphate], hydroxyaluminum bis[2,2'-methylene-bis(4,6-diethylphenyl)phosphate], hydroxyaluminum bis[2,2'-ethylidene-bis(4,6-diethylphenyl)phosphate], hydroxyaluminum bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate], hydroxyaluminum bis[2,2' -methylene-bis(4-methyl-6-t-butylphenyl)phosphate], hydroxyaluminum-bis[2,2'-ethylidene-bis(4-methyl-6-t-butylphenyl)phosphate], hydroxyaluminum-bis[2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate], hydroxyaluminum-bis[2,2'-ethylidene-bis(4-ethyl-6-t-butylphenyl)phosphate], hydroxyaluminum-bis[2,2'-methylene-bis(4-i-propyl-6-t-butylphenyl)phosphate], hydroxyaluminum-bis[2,2'-ethylidene-bis(4-i-propyl-6-t-butylphenyl)phosphate], etc., and mixtures of two or more of these can be exemplified. It is effective to use these in combination with an organic alkali metal salt. Also, sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2'-butylidene-bis(4,6-dimethylphenyl) phosphate, sodium-2,2'-butylidene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2'-t-octylmethylene-bis(4,6-methylphenyl) phosphate, sodium-2,2'-t-octylmethylene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2' -methylene-bis(4-methyl-6-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate, sodium (4,4'-dimethyl-6,6'-di-t-butyl-2,2'-biphenyl)phosphate, sodium-2,2'-ethylidene-bis(4-s-butyl-6-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4,6-di-methylphenyl)phosphate, sodium-2,2'-methylene-bis(4,6-di-ethylphenyl)phosphate, etc. are also included as compounds represented by formula (2). Among these, sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate is particularly preferred. As such a nucleating agent, commercially available products can be used, specifically, a product name: "ADEKA STAB NA-11" manufactured by ADEKA CORPORATION can be mentioned. In addition, potassium 2,2'-ethylidene bis(4,6-di-t-butylphenyl) phosphate, calcium bis[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], magnesium bis[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], zinc bis[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], aluminum tris[2,2'-methylene bis(4,6-di-t-butylphenyl) phosphate], calcium bis[2,2'- methylene-bis-(4-methyl-6-t-butylphenyl) phosphate], calcium-bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate], calcium-bis[2,2'-thiobis(4-methyl-6-t-butylphenyl) phosphate], calcium-bis[2,2'-thiobis(4-ethyl-6-t-butylphenyl) phosphate], calcium-bis[2,2'-thiobis(4,6-di-t-butylphenyl) phosphate], magnesium-bis[2,2'-thiobis(4,6-di-t-bu t-butylphenyl) phosphate], magnesium bis[2,2'-thiobis(4-t-octylphenyl) phosphate], calcium bis[(4,4'-dimethyl-6,6'-di-t-butyl-2,2'-biphenyl) phosphate], magnesium bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate], aluminum tris[2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate], lithium 2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate Other examples of the compound represented by formula (2) include lithium 2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, lithium 2,2'-methylene-bis(4-cumyl-6-t-butylphenyl) phosphate, sodium 2,2'-ethylidene-bis(4-i-propyl-6-t-butylphenyl) phosphate, lithium 2,2'-methylene-bis(4-methyl-6-t-butylphenyl) phosphate, and lithium 2,2'-methylene-bis(4-ethyl-6-t-butylphenyl) phosphate.Among these, lithium 2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate is particularly preferred. As such a nucleating agent, commercially available products can be used, specifically, a product name: "ADEKA STAB NA-71" manufactured by ADEKA CORPORATION can be mentioned.

[0029] The amount of the nucleating agent (b) to be blended in the propylene resin composition used in the present invention is preferably 0.01 to 0.30 parts by weight, more preferably 0.05 to 0.20 parts by weight, and even more preferably 0.08 to 0.15 parts by weight, relative to 100 parts by weight of the polypropylene resin. When the amount of the nucleating agent (b) is 0.01 parts by weight or more, it is expected that rigidity and transparency will be exhibited, and when it is 0.30 parts by weight or less, there is less concern about bleeding onto the surface of the molded article, which is advantageous in terms of cost-effectiveness (cost performance) and elution in terms of rigidity and transparency.

[0030] [ka]

[0031] (In the formula, R 1 , R 2 and R 3 are, independently of each other, unsubstituted or substituted hydrocarbon radicals.

[0032] The compound having an unsubstituted or substituted hydrocarbon group is specifically exemplified by the various compounds shown below. The nucleating agent (c) used in the present invention has a performance that can be properly achieved as long as it has the form of the compound of the above formula (3). The various compounds having an unsubstituted or substituted hydrocarbon group depend on the reaction components selected when synthesizing the compound represented by formula (3) used in the present invention, and although they have a slight effect on the reaction yield of the compound of formula (3), they act equally as nucleating agents (c), and the following can be specifically exemplified. R 1 , R 2 and R 3is preferably a compound of formula (3), in which at least one of is represented by a branched alkyl group having 3 to 20 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms which is unsubstituted or substituted by one or more alkyl groups having 1 to 20 carbon atoms.

[0033] Also, R 1 , R 2 and R 3 are each independently an unsubstituted or at least one of 1-methylethyl, 2-methylpropyl, 1-methylpropyl, tert-butyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1,1-dimethylpropyl, 1-ethylpropyl, tert-butylmethyl, cyclopropyl, 3-methylcyclopropyl, 2,2,3,3-tetramethylcyclopropyl, cyclopentyl, cyclopentylmethyl, 2-cyclopentylethyl, cyclohexyl, cyclohexylmethyl, 2-cyclohexylethyl, 4-tert-butylcyclohexyl, (4-methylcyclohexyl)methyl, More preferred are compounds of formula (3) represented by the cyclic hydrocarbon groups represented by 3-1) to (3-3), α-cyclohexylbenzyl, 3-methylbenzyl, 3,4-dimethoxybenzyl, 4-biphenylmethyl, 2-naphthylmethyl, m-tolyl, m-methoxyphenyl, p-tolyl, 4-ethylphenyl, 4-isopropylphenyl, 4-tert-butylphenyl, 2,3-dimethylphenyl, 2,6-dimethylphenyl, 2,4-dimethylphenyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, 3,5-di-tert-butylphenyl or 2,4,6-trimethylphenyl.

[0034] [ka]

[0035] [ka]

[0036] [ka]

[0037] Specifically, the compound represented by formula (3) includes 1,3,5-tris[2,2-dimethylpropionylamino]benzene, 1,3,5-tris[cyclohexylcarbonylamino]benzene, 1,3,5-tris[4-methylbenzoylamino]benzene, 1,3,5-tris[3,4-dimethylbenzoylamino]benzene, 1,3,5-tris[3,5-dimethylbenzoylamino]benzene, 1,3,5-tris[cyclopentanecarbonylamino]benzene, 1,3,5-tris[1-adamantanecarbonylamino]benzene, 1,3,5 -Tris[2-methylpropionylamino]benzene, 1,3,5-tris[3,3-dimethylbutyrylamino]benzene, 1,3,5-tris[2-ethylbutyrylamino]benzene, 1,3,5-tris[2,2-dimethylbutyrylamino]benzene, 1,3,5-tris[2-cyclohexyl-acetylamino]benzene, 1,3,5-tris[3-cyclohexyl-propionylamino]benzene, 1,3,5-tris[4-cyclohexyl-butyrylamino]benzene, 1,3,5-tris[5-cyclohexyl-valeroylamino]benzene 1,3-bis[isobutyrylamino]-5-pivaloylaminobenzene, 1,3-bis[isobutyrylamino]-5-(2,2-dimethylbutyryl)aminobenzene, 1,3-bis[isobutyrylamino]-5-(3,3-dimethylbutyryl)aminobenzene, 1,3-bis[isobutyrylamino]-5-(3,3-dimethylbutyryl)aminobenzene, 1,3-bis[isobutyrylamino]-5-(3,3-dimethylbutyryl)aminobenzene, 1,3-bis[2,2-dimethylbutyryl 1,3-bis[2,2-dimethylbutyrylamino]-5-isobutyrylaminobenzene, 1,3-bis[2,2-dimethylbutyrylamino]-5-(3,3-dimethylbutyryl)-aminobenzene, 1,3-bis[3,3-dimethylbutyrylamino]-5-pivaloylamino-benzene, 1,3-bis[3,3-dimethylbutyrylamino]-5-isobutyryl-aminobenzene, 1,3-bis[3,3-dimethylbutyrylamino]-5-(2,2-dimethyl-butyrylamino)aminobenzene or 1,3,5-tris[3-(trimethylsilyl)propionylamino]benzene can be mentioned.

[0038] Such a compound can be produced, for example, by the method described in JP-A-2006-518402. Of these, R 1 , R 2 and R 3 In particular, the compound of formula (3) in which R 1 , R 2 and R 3 Particularly preferred is the compound of formula (3) in which is represented by tert-butyl, i.e. 1,3,5-tris[2,2-dimethylpropionylamino]benzene. As such a nucleating agent (c), a commercially available product can be used, specifically, a product name: "Irgaclear XT-386" manufactured by BASF Japan Ltd. can be mentioned.

[0039] The amount of the nucleating agent (c) to be blended in the polypropylene resin composition used in the present invention is preferably 0.005 to 0.04 parts by weight, more preferably 0.01 to 0.02 parts by weight, based on 100 parts by weight of the polypropylene resin. When the content of the nucleating agent (c) is 0.005 parts by weight or more, the expression of rigidity and transparency can be expected, and when it is 0.04 parts by weight or less, it is advantageous in terms of cost-effectiveness (cost performance) in terms of rigidity and transparency.

[0040] By using at least one nucleating agent selected from the group consisting of nucleating agent (a), nucleating agent (b), and nucleating agent (c), transparency is improved and cloudiness is reduced, improving color development and resulting in a nail polish container with a high-quality appearance.

[0041] (10) Other additives In the polypropylene resin composition used in the present invention, additives such as various antioxidants and neutralizing agents used as stabilizers for propylene polymers, except for hindered phenols, can be blended. Specifically, examples of the thio antioxidant include di-stearyl-β,β'-thio-di-propionate, di-myristyl-β,β'-thio-di-propionate, di-lauryl-β,β'-thio-di-propionate, and the like. Further, amine-based antioxidants such as those represented by the following formula (4) which have good resistance to discoloration due to NOx gas can be used.

[0042] [ka]

[0043] Examples of the neutralizing agent include fatty acid metal salts such as calcium stearate, zinc stearate, and magnesium stearate, hydrotalcite (trade name: DHT-4A, magnesium aluminum complex hydroxide salt manufactured by Kyowa Chemical Industry Co., Ltd.), and Mizukalac (trade name, lithium aluminum complex hydroxide salt manufactured by Mizusawa Chemical Industry Co., Ltd.), of which calcium stearate is the most preferred as it is economical and contributes to improving moldability. Furthermore, various known additives, for example, lubricants, dispersants such as fatty acid metal salts, dyes, pigments, etc., can be blended within the range that does not impair the object of the present invention. In addition, within the range that does not impair the properties and functions of the polypropylene resin composition used in the present invention, other polymers than the propylene polymer, for example, homopolymers such as polyethylene, ethylene-propylene copolymers, ethylene-propylene-diene copolymers, ethylene-1-butene copolymers, ethylene-vinyl acetate copolymers, ethylene-acrylate copolymers, and acrylate polymers, or binary or ternary copolymers, can be added arbitrarily in an amount of 0 to 30 parts by weight per 100 parts by weight of the polypropylene resin. Similarly, it is also possible to blend elastomers such as natural rubber, butyl rubber, diene rubber, EPM, EPDM, EBM, EHM, EOM, and PBM. Furthermore, it is also possible to use general-purpose inorganic fillers such as talc, calcium carbonate, silica, alumina, gypsum, and mica in combination.

[0044] [2] Method for producing polypropylene resin composition for use in nail polish containers The polypropylene resin composition used in the nail polish container of the present invention can be obtained by adding predetermined amounts of a phosphorus-based antioxidant, a hindered amine-based light stabilizer, and, if necessary, other additives to a polypropylene resin in a Henschel mixer (product name), a super mixer, a ribbon blender, or the like, mixing them, and then melt-kneading them in a temperature range of 190 to 260°C using a conventional single-screw extruder, twin-screw extruder, Banbury mixer, Brabender, rolls, or the like.

[0045] [3] Molded products In the nail polish container of the present invention, the molded product can be obtained by molding the polypropylene resin composition described in [1] above by a known method such as injection molding, extrusion molding, or blow molding. Examples of molded products of the nail polish container of the present invention include lids, containers, and other parts, but it is preferable that at least the lid, which is a part of the lid body, is molded from the polypropylene resin composition described in [1] above.

[0046] The nail polish container of the present invention is a nail polish container composed of a container (main body) and a lid body having a shaft body with an applicator at the tip, and is composed by combining the above-mentioned molded parts. FIG. 1 is a cross-sectional view of an example of the nail polish container of the present invention. The nail polish container of the illustrated example comprises a container body 1 that contains nail polish, and a lid body 2 that is detachably attached to open and close the container body 1. In the nail polish container of the illustrated example, the lid body 2 comprises a shaft body 3 and a lid 4. Here, the shaft body 3 comprises a shaft 7 that constitutes the center of the shaft body 3 and extends from the inside of the lid 4 to the inside of the container body 1, a fixing part 5 at the end on the lid 4 side that is configured to fix the shaft body 3 to the lid 4, and an applicator 6 at the end on the inside side of the container body 1 that is configured to apply the nail polish contained in the container body 1 to the nail. A brush is used as the applicator 6. The nail polish container of the present invention is at least partially made of the polypropylene resin composition described in [1] above, but as described above, it is preferable that the lid 4, which is at least a part of the lid body 2, is a molded part molded from the polypropylene resin composition described in [1] above.

[0047] In the case where the nail polish container of the present invention uses parts other than the molded parts molded from the polypropylene resin composition described in [1] above, for example, in the nail polish container shown in Figure 1, of the lid body 2, low-density polyethylene or the like can be used for the fixing part 5, a nylon brush or tip or the like can be used for the applicator body 6, low-density polyethylene, high-density polyethylene or the like can be used for the shaft 7, and glass, polyethylene naphthalate, nylon, or the like can be used for the container body 1.

[0048] The nail polish container of the present invention is suitable for use when the nail polish contained in the container contains nitrocellulose as a component constituting the nail polish (nail polish component). The polypropylene resin composition described in [1] above is substantially free of hindered phenol, and therefore can suppress discoloration due to reaction with volatile matters contained in the nail polish, particularly volatile matters contained in nitrocellulose. Table 1 below shows an example of a nail polish containing nitrocellulose as a nail polish component, but the nail polish contained in the nail polish container of the present invention is not limited to the example shown below.

[0049] [Table 1] EXAMPLES

[0050] EXAMPLES The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The methods for measuring physical properties, propylene-based polymers, and polypropylene resin compositions used in the examples and comparative examples are as follows.

[0051] 1.Measurement method (A) Ethylene content 13 The ethylene-propylene random copolymer, the composition of which was verified by the C-NMR method, was used as the standard substance. -1 The ethylene content in the random copolymer was measured by infrared spectroscopy using the characteristic absorption band of (calibration curve preparation). Based on the calibration curve, the ethylene content was measured by infrared spectroscopy using a film of about 500 μm thickness made by press molding a sample of the propylene-based polymer. Here, the contents of propylene and ethylene in the reference materials for creating the calibration curve are as follows: 13 This is a value measured by the C-NMR method. 13 Analysis of the C-NMR spectrum was carried out according to the analysis method described in JP-A-2006-307120, and the contents of propylene and ethylene were calculated. Equipment: JEOL-GSX270 manufactured by JEOL Co., Ltd. Concentration: 300mg / 2mL Solvent: orthodichlorobenzene (a) MFR Measurements were performed in accordance with JIS K7210:1999, Annex A, Table 1, Condition M, at a test temperature of 230°C and a nominal load of 2.16 kg. (c) Flexural modulus Measurements were performed at 23°C in accordance with JIS K7171. (d) Charpy impact strength Measurements were performed at 23°C in accordance with JIS K7111. (O) Hayes Measurements were performed in accordance with JIS K7136 using a sheet piece with a thickness of 1 mm. (K) Oven Life A 0.5 mm thick piece of the sheet was placed in an oven at 130°C and the time until deterioration was confirmed visually. (g) Visual appearance evaluation - Sheet test A 1mm thick (1mm x 20mm x 80mm) sheet piece and a 5ml open container containing an appropriate amount of cosmetic nitrocellulose raw material were placed in a 200ml beaker, sealed with three sheets of commercially available food wrap, and left to stand at 50°C for about a week, after which each sheet piece was removed and visually inspected for discoloration and bleeding in comparison with a standard product (stored at room temperature during the test period). The evaluation results are as follows. Figure 2 is an overview of the test using sheets. The standard specimen is used as a reference for observing the color change and bleeding of the test specimen (the test piece described below), and is stored without being exposed to cosmetic nitrocellulose. ◎: Very good (no change at all) ○: Good (There is a slight difference compared to the standard product, but it is hardly noticeable when used alone.) ×: Poor (changes are observed and the difference from the standard product is clearly visible) Lid test A glass nail polish bottle was filled with a sample of one of the nail polishes shown in Table 1, and a nail polish cap with a stem made of each material was attached and stored at 50°C. The cap was visually inspected for discoloration after 5 weeks in comparison with a standard product (stored at room temperature during the test period). The results are as follows. Figure 4 is a photograph of the cap of Comparative Example 1 after the test with the cap (5 weeks after storage). The standard product is used as a reference for observing the color change of the test product (the test piece described below), and is stored without being filled with nail polish. ◎: Very good (no change at all) ○: Good (There is a slight difference compared to the standard product, but it is hardly noticeable when used alone.) ×: Poor (changes are observed and the difference from the standard product is clearly visible)

[0052] 2. Additives, resins 2-1.Additives (IF168) Phosphorus-based antioxidant. Tris(2,4-di-t-butylphenyl)phosphite. BASF Japan Ltd. Product name: "Irgafos168" (TNV622) Hindered amine light (ultraviolet) stabilizer (weather resistance agent). Dimethyl succinate 2-(4-hydroxy-2,2,6,6-tetramethylpiperidine) ethanol condensate. Manufactured by BASF Japan Ltd. Product name: "TINUVIN622LD" (IR1010) Phenol-based antioxidant (hindered phenol). Tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane. Manufactured by BASF Japan Ltd. Product name: "IRGANOX 1010" (CAST) Calcium stearate. Manufactured by NOF Corporation (DHT4A) Hydrotalcite. Manufactured by Kyowa Chemical Industry Co., Ltd. Product name: "DHT-4A" (NA11) Equivalent to nucleating agent (b). Sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate. Manufactured by ADEKA Corporation. Product name: "ADEKA STAB NA-11" (NX8000J) Equivalent to nucleating agent (a). 1,2,3-trideoxy-4,6:5,7-O-bis[(4-propylphenyl)methylene]nonitol. Manufactured by Milliken & Company. Product name: "Milad NX8000J" (XT386) Equivalent to nucleating agent (c). 1,3,5-tris[2,2-dimethylpropionylamino]benzene. Manufactured by BASF Japan Ltd. Product name: "Irgaclear XT-386" (OA) Lubricant. Oleic acid amide. Manufactured by Nippon Kasei Co., Ltd. Product name: "Diamid O-200" (PHA25B) 2,5-dimethyl-2,5-di(t-butylperoxy)hexane. Product name: "Perhexa 25B" manufactured by NOF Corporation.

[0053] 2-2.Resin (I) Production Example 1 (Production of PP1) <Production of solid catalyst component> 20 L of dehydrated and deoxygenated n-heptane was introduced into a 50 liter (L) tank equipped with a stirrer and thoroughly purged with nitrogen, followed by 10 moles of magnesium chloride (MgCl2) and 20 moles of tetrabutoxytitanium [Ti(On-C4H9)4], and the reaction was carried out at 95°C for 2 hours. After the reaction was completed, the temperature was lowered to 40°C, and methylhydropolysiloxane [kinetic viscosity: 20 centistokes (cSt) = 2 x 10 -5 m 2 12 L of 1,2-dichloroethane (1000 mL / s) was introduced and reacted for 3 hours. The resulting solid component was washed with n-heptane. Next, 5 L of n-heptane purified in the same manner as above was introduced into the tank equipped with the stirrer, and 3 moles of the solid component synthesized above were introduced in terms of Mg atom. Next, 5 moles of tetrachlorosilane (SiCl4) were mixed with 2.5 L of n-heptane, introduced into the flask at 30°C for 30 minutes, and reacted at 70°C for 3 hours. After the reaction was completed, the mixture was washed with n-heptane. Next, 2.5 L of n-heptane was introduced into the tank equipped with the stirrer, and 0.3 moles of phthalic acid chloride was mixed and introduced at 70°C for 30 minutes, and reacted at 90°C for 1 hour. After the reaction was completed, the reaction mixture was washed with n-heptane. Then, 2 L of titanium tetrachloride (TiCl4) was introduced and reacted at 110°C for 3 hours. After the reaction was completed, the reaction mixture was washed with n-heptane to obtain a solid component (a1) for producing a solid catalyst component (a). When analyzed, the titanium content of this solid component was 2.0% by weight. Then, 8 L of n-heptane, 400 g of the solid component (a1) synthesized above, and 0.6 L of SiCl4 as component (a2) were introduced into the nitrogen-purged agitator-equipped tank, and the reaction was carried out for 2 hours at 90° C. After the reaction was completed, 0.54 mol of vinyltrimethylsilane [(CH2=CH)Si(CH3)3] as component (a3), 0.27 mol of t-butylmethyldimethoxysilane [(t-C4H9)(CH3)Si(OCH3)2] as component (a4), and 1.5 mol of triethylaluminum [Al(C2H5)3] as component (a5) were sequentially introduced, and the reaction was carried out for 2 hours at 30° C. After the contact, the mixture was thoroughly washed with n-heptane to obtain 390 g of a solid catalyst component (a) mainly composed of magnesium chloride. Analysis revealed that the titanium content of this solid catalyst component (a) was 1.8% by weight.

[0054] <Production of propylene homopolymer> Polymerization was carried out using a fluidized bed reactor with an internal volume of 230 L as a continuous reactor. The reactor was continuously fed with hydrogen as a molecular weight regulator at a polymerization temperature of 85°C, a propylene partial pressure of 1.8 MPa (absolute pressure), and a hydrogen / propylene molar ratio of 0.010. Furthermore, 5.25 g / hour of triethylaluminum and the above-described catalyst as the solid catalyst component (a) were fed so that the polymer polymerization rate was 20 kg / hour to produce a propylene homopolymer. The powder polymerized in the reactor was continuously discharged into a vessel so that the amount of powder held in the reactor was 60 kg. The reaction was stopped by supplying nitrogen gas containing moisture, and a propylene homopolymer was obtained. The MFR of this propylene homopolymer was 11 g / 10 min, and was designated PP1.

[0055] (II) Production Example 2 (Production of PP2) <Production of solid titanium catalyst component> 700g of anhydrous magnesium chloride is heated at 130°C for 2 hours with 3.7L of decane and 3.5L of 2-ethylhexyl alcohol to obtain a homogeneous solution, and then 165g of phthalic anhydride is added to the solution, and the mixture is stirred and mixed at 130°C for another hour to dissolve the phthalic anhydride in the homogeneous solution. The homogeneous solution thus obtained is cooled to room temperature, and then the entire amount is dropped into titanium tetrachloride kept at -20°C over 1 hour. After the addition, the temperature of the mixture is raised to 110°C over 4 hours, and when it reaches 110°C, 0.4L of diisobutyl phthalate is added, and the mixture is kept at the same temperature for 2 hours under stirring. After the reaction for 2 hours is completed, the solid portion is collected by hot filtration and thoroughly washed with 110°C decane and hexane until no free titanium compounds are detected in the washings. The titanium catalyst component synthesized by the above manufacturing method is dried with a dryer. Analysis revealed that the composition (main components) of the titanium catalyst component thus obtained was 2.3% by weight of titanium, 58.0% by weight of chlorine, 18.0% by weight of magnesium, and 14.0% by weight of diisobutyl phthalate.

[0056] <Prepolymerized titanium catalyst component> 200 ml of purified hexane was placed in a nitrogen-purged 400 ml glass reactor, and 20 mmol of triethylaluminum, 4 mmol of dicyclopentyldimethoxysilane, and 2 mmol of the titanium catalyst component, calculated as titanium atom, were added. Propylene was then supplied at a rate of 5.9 Nl / hour for 1 hour to polymerize 2.8 g of propylene per gram of the Ti catalyst component. After the preliminary polymerization was completed, the liquid phase was removed by filtration, and the separated solid portion (preliminary polymerization catalyst) was dispersed again in decane.

[0057] <Production of propylene-ethylene copolymer> After the inside of a 200-liter stirred autoclave was fully replaced with propylene, 45 kg of liquefied propylene was introduced. 0.44 kg of ethylene, 500 ml of triethylaluminum-n-heptane solution (triethylaluminum concentration: 50 g / l), and 1.9 g of cyclohexylmethyldimethoxysilane were added, and the internal temperature was maintained at 30°C. Next, 300 L of hydrogen (as standard volume) and 3.8 g of the above prepolymerization catalyst were pressed in with argon to start polymerization, and the temperature was raised to 70°C over 40 minutes. After 1.0 hour had elapsed while maintaining the polymerization temperature at 70°C, 100 ml of ethanol was added to stop the reaction, and the remaining gas was purged. The yield of the obtained polymer per 1 g of solid catalyst was 27 kg, the MFR was 30.0 g / 10 min, and the ethylene content was 2.3 wt%. This was named PP2.

[0058] (III) Production Example 3 (Production of PP3) <Production of solid titanium catalyst component> A 10L autoclave equipped with a stirrer was fully replaced with nitrogen, and 2L of purified toluene was introduced. 200g of Mg(OEt)2 and 1L of TiCl4 were added at room temperature. The temperature was raised to 90°C, and 50ml of di-n-butyl phthalate was introduced. Then, the temperature was raised to 110°C and the reaction was carried out for 3 hours. The reaction product was thoroughly washed with purified toluene. Next, purified toluene was introduced to adjust the total liquid volume to 2L. 1L of TiCl4 was added at room temperature, and the temperature was raised to 110°C and the reaction was carried out for 2 hours. The reaction product was thoroughly washed with purified toluene. Next, purified toluene was introduced to adjust the total liquid volume to 2L. 1L of TiCl4 was added at room temperature, and the temperature was raised to 110°C and the reaction was carried out for 2 hours. The reaction product was thoroughly washed with purified toluene. Furthermore, toluene was replaced with n-heptane using purified n-heptane, and a slurry of solid components was obtained. A portion of this slurry was sampled and analyzed, and the Ti content of the solid component was found to be 2.7% by weight. Next, a 20 L autoclave equipped with a stirrer was fully purged with nitrogen, and 100 g of the above solid component slurry was introduced as a solid component. Purified n-heptane was introduced to adjust the concentration of the solid component to 25 g / L. 50 ml of SiCl4 was added, and the reaction was carried out at 90°C for 1 hour. The reaction product was thoroughly washed with purified n-heptane. After that, refined n-heptane was introduced to adjust the liquid level to 4 L. 30 ml of dimethyldivinylsilane, 30 ml of (i-Pr)2Si(OMe)2, and 80 g of n-heptane diluted Et3Al (as Et3Al) were added to the flask, and the reaction was carried out at 40°C for 2 hours. The reaction product was thoroughly washed with refined n-heptane, and a portion of the resulting slurry was sampled, dried, and analyzed. The solid components contained 1.2 wt% Ti and 8.8 wt% (i-Pr)2Si(OMe)2. Further, the solid component obtained above was used to carry out preliminary polymerization according to the following procedure. Purified n-heptane was introduced into the above slurry to adjust the concentration of the solid component to 20 g / L. Next, the slurry was cooled to 10°C, and 10 g of n-heptane diluted solution of Et3Al was added as Et3Al, and 280 g of propylene was fed over 4 hours. After the propylene feed was completed, the reaction was continued for another 30 minutes. Next, the gas phase was fully replaced with nitrogen, and the reaction product was thoroughly washed with purified n-heptane. The obtained slurry was extracted from the autoclave and vacuum dried to obtain a solid catalyst component (c). This solid catalyst component contained 2.5 g of polypropylene per 1 g of the solid component. In addition, when analyzed, the part of this solid catalyst component (c) excluding polypropylene contained 1.0 wt% Ti and 8.2 wt% (i-Pr)2Si(OMe)2.

[0059] <Production of propylene-ethylene copolymer> The production of a propylene-ethylene copolymer will be described with reference to the flow sheet shown in FIG. 3. A gas phase polymerization reactor using two polymerization vessels was used. The two polymerization vessels 1 and 10 had an inner diameter D of 2100 mm, a length L of 11000 mm, and an internal volume of 40 m. 3The reactor is a continuous horizontal gas-phase polymerization reactor (length / diameter = 5.2) equipped with an agitator. After the inside of the polymerization vessel 1 was fully replaced with nitrogen, polypropylene powder from which polymer particles with a particle size of 500 μm or less had been removed was charged, and 120 g / hour of solid catalyst component (c) and 15 wt% hexane solution of triethylaluminum were continuously fed so that the molar ratio per mole of Ti atom in the catalyst component (c) was 350. In addition, hydrogen was fed into the polymerization vessel 1 so that the ratio of hydrogen concentration to propylene concentration in the polymerization vessel 1 was 0.095, ethylene was fed into the polymerization vessel 1 so that the ratio of ethylene concentration to propylene concentration in the polymerization vessel 1 was 0.020, and propylene monomer was fed into the polymerization vessel 1 so that the pressure in the polymerization vessel 1 was 2.10 MPa and the temperature was 61°C. The reaction heat was removed by the vaporization heat of the raw material liquefied propylene fed from the raw material mixed gas supply pipe 3. The unreacted gas discharged from the polymerization vessel 1 was extracted outside the reactor system through the unreacted gas extraction pipe 4, cooled and condensed, and refluxed to the polymerization vessel 1 through the recycle gas pipe 2. The propylene-ethylene copolymer (first stage) produced in the polymerization reactor 1 was continuously withdrawn from the polymerization reactor 1 through the polymer withdrawal pipe 5 so that the polymer retention level was 45% by volume of the reaction volume, and was supplied to the polymerization reactor 10 for the second polymerization step. In the polymerization vessel 10, the polymer from the first polymerization step, hydrogen so that the ratio of the hydrogen concentration to the propylene concentration in the polymerization vessel 10 was 0.021, ethylene so that the ratio of the ethylene concentration to the propylene concentration in the polymerization vessel 10 was 0.068, and propylene monomer so that the pressure in the polymerization vessel 10 was kept at 2.05 MPa and the temperature at 70°C were respectively supplied into the polymerization vessel 10. A polymerization activity inhibitor for adjusting the polymerization amount of the propylene-ethylene copolymer (second stage) was supplied from a polymerization activity inhibitor addition pipe 11. The reaction heat was removed by the vaporization heat of the raw material liquefied propylene supplied from the raw material mixed gas supply pipe 6. The unreacted gas discharged from the polymerization vessel 10 was extracted to the outside of the reactor system through an unreacted gas extraction pipe 8, cooled and condensed, and refluxed to the polymerization vessel 10 through a recycle gas pipe 7. The propylene polymer produced in the second polymerization step was continuously withdrawn from the polymerization vessel 10 through the polymer withdrawal pipe 9 so that the polymer retention level was 50% by volume of the reaction volume. The withdrawn powder was separated from gases by a gas recovery device 12, and the powder portion was withdrawn to a recovery system and granulated in a granulation system. The production rate of the propylene polymer was 9.6 T / hour, the average residence time in the polymerization reactor 1 was 1.9 hours, and the average residence time in the polymerization reactor 10 was 1.3 hours. The catalyst efficiency was calculated by dividing the production rate by the supply rate of the solid catalyst component (c), and was found to be 88,900 g-PP / g-catalyst. The propylene polymer thus obtained was analyzed, and found to have an MFR of 38.9 g / 10 min and an ethylene content of 5.0 wt%. The PP component (first stage) had an MFR of 71.9 g / 10 min and an ethylene content of 2.5 wt%. The index of the PP component (second stage) was calculated to be MFR=8.0 g / 10 min and an ethylene content of 11.3 wt%. Here, the MFR of the PP component (second stage) was calculated from the MFR of the PP component (first stage), the MFR of the propylene polymer, and the weight ratio of the PP components (first stage) and (second stage) according to an empirical formula called the logarithmic additivity rule of viscosity. The ethylene content was calculated from the ethylene content of the PP component (first stage), the ethylene content of the propylene polymer, and the weight ratio of the PP components (first stage) and (second stage). Here, the weight ratio of the PP components (first stage) and (second stage) was calculated from the production amount of each stage from the amount of liquefied propylene supplied to the polymerization tank, and the production amount of the PP component (second stage) was 28% of the total weight. This was designated PP3.

[0060] 2-3. Examples and Comparative Examples The propylene-based polymers PP1 to PP3 were prepared with additives in the blending ratios (parts by weight) shown in Tables 2 and 3, and then dry-blended in a super mixer. The mixture was melt-kneaded at a die outlet temperature of 220°C using a TEM-35B twin-screw extruder manufactured by Toshiba Machine Co., Ltd., and pelletized. The pellets of the polypropylene resin composition obtained were injection-molded at a resin temperature of 200°C and a mold temperature of 40°C using an EC100SX injection molding machine manufactured by Toshiba Machine Co., Ltd., to prepare test pieces (sheet pieces). In addition, the pellets of the polypropylene resin composition obtained were similarly injection-molded using an EC220C-6A injection molding machine manufactured by Toshiba Machine Co., Ltd., to prepare a lid, which was fitted with a commercially available applicator (brush)-attached shaft to prepare a test piece (shaft-attached lid). The obtained pellets or test pieces were used to measure the above-mentioned physical properties. The evaluation results are shown in Tables 2 and 3.

[0061] Regarding (g) visual appearance evaluation, photographs of the sheet after the test with the sheet and photographs of the lid before and after the test with the lid are shown in Figs. 5 to 18. FIG. 5 is a photograph of the sheet of Example 1 (standard product) stored at room temperature during the test period, FIG. 6 is a photograph of the sheet after the test using the sheet of Example 1, FIG. 7 is a photograph of the lid of Example 1 (standard product) stored at room temperature during the test period, and FIG. 8 is a photograph of the lid of Example 1 after the test using the lid. Fig. 9 is a photograph of the sheet of Example 2 (standard product) that was stored at room temperature during the test period, and Fig. 10 is a photograph of the sheet after the test using the sheet of Example 2. Note that the test using a lid was not performed for Example 2. FIG. 11 is a photograph of the sheet of Example 3 (standard product) stored at room temperature during the test period, FIG. 12 is a photograph of the sheet after the test using the sheet of Example 3, FIG. 13 is a photograph of the lid of Example 3 (standard product) stored at room temperature during the test period, and FIG. 14 is a photograph of the lid of Example 3 after the test. FIG. 15 is a photograph of the sheet (standard product) of Comparative Example 1 that was stored at room temperature during the test period, FIG. 16 is a photograph of the sheet after testing with the sheet of Comparative Example 1, FIG. 17 is a photograph of the lid (standard product) of Comparative Example 1 that was stored at room temperature during the test period, and FIG. 18 is a photograph of the lid after testing with the lid of Comparative Example 1. In the test using the lid, discoloration of the lid was checked every week. In Comparative Example 1, yellowing was confirmed one week after the start of storage at 50°C.

[0062] [Table 2]

[0063] [Table 3]

[0064] From Table 2, it can be confirmed that in Examples 1 to 3, no significant discoloration is observed even in an atmosphere where the volatile content of the nitrocellulose contained in the nail polish is present. On the other hand, it can be confirmed that in Comparative Example 1, the color significantly turns yellow in an atmosphere where the volatile content of the nitrocellulose contained in the nail polish is present, and bleeding was also observed. In Example 2, the color turns slightly yellow, but this is because the amount of the phosphorus-based antioxidant was slightly too high. In Example 3, slight bleeding is observed, but this is due to the high ethylene content and high MFR of the second-stage polymer component due to the Ziegler catalyst of PP3. In addition, the peroxide blended in Example 1 plays a role as a molecular weight regulator (degrader), and can change a propylene-based polymer with an MFR of 11 g / 10 min to 17 g / 10 min. Generally, polypropylene is given long-term thermal stability (oven life) by blending it with a phenolic antioxidant (hindered phenol). However, the volatile components of nail polish react with the phenolic antioxidant, causing the phenolic antioxidant to discolor. Therefore, polypropylene cannot be used for nail polish containers unless it is a color that can hide discoloration, such as black. From the oven life test results of Example 2 and Comparative Example 1, it can be confirmed that the present invention can obtain long-term thermal stability similar to that of polypropylene using a conventional phenol-based antioxidant, even without using a phenol-based antioxidant. Furthermore, from Table 3, Comparative Example 2 has an oven life of 50 hours using only a phosphorus-based antioxidant as the antioxidant, Comparative Example 3 has an oven life of 230 hours using only a hindered amine-based light (ultraviolet) stabilizer as the antioxidant, and Comparative Example 4 has an oven life of 42 hours without adding an antioxidant. It is found that Comparative Examples 2 to 4 have inferior oven lives compared to Example 4 of the present invention, and Example 4 is a combination of the antioxidants of Comparative Example 2 and Comparative Example 3, but the oven life of Example 4 is longer than the oven life of Comparative Examples 2 and 3 combined, and it can be seen that a synergistic effect is obtained. The time of the oven life test at 130°C can be used to estimate long-term thermal stability at room temperature using the Arrhenius equation. [Industrial Applicability]

[0065] The present invention can be applied to nail polish containers using a polypropylene resin composition which is excellent in chemical resistance, moldability, barrier properties, long-term thermal stability, and balance of physical properties, particularly in discoloration resistance. [Explanation of symbols]

[0066] Figure 1 1. Container body 2. Lid 3. Axial body 4. Lid 5.Fixed part 6. Application body (brush) 7. Axis

[0067] Figure 2 1. 200ml beaker 2. Nitrocellulose container 3. Sheets 4. Rap

[0068] Figure 3 1.Polymerization vessel (first polymerization step) 2.Recycled gas piping 3. Raw material mixed gas supply piping 4. Unreacted gas extraction piping 5. Polymer withdrawal piping 6. Raw material mixed gas supply piping 7.Recycled gas piping 8. Unreacted gas extraction piping 9. Polymer withdrawal piping 10.Polymerization vessel (second polymerization step) 11. Polymerization inhibitor addition pipe 12.Gas recovery machine

Claims

1. The nail polish container is composed of a container body and a lid body having a shaft body with an applicator body at the tip, and at least a part of the nail polish container is made of a polypropylene resin composition that is substantially free of hindered phenol and satisfies the following characteristics (i) to (iv). (i) The MFR measured in accordance with JIS K7210:1999, Annex A, Table 1, Condition M at a test temperature of 230° C. and a nominal load of 2.16 kg is 0.5 to 120 g / 10 min. (ii) The flexural modulus in accordance with JIS K7171 is 150 MPa or more. (iii) 0.001 to 0.5 parts by weight of a phosphorus-based antioxidant is blended with respect to 100 parts by weight of the polypropylene resin. (iv) 0.01 to 0.5 parts by weight of dimethyl succinate 2-(4-hydroxy-2,2,6,6-tetramethylpiperidine) ethanol condensate is blended as a hindered amine-based light stabilizer relative to 100 parts by weight of polypropylene resin.

2. 2. The nail polish container according to claim 1, wherein the polypropylene resin composition satisfies the following characteristic (v): (v) The polypropylene resin is a propylene homopolymer or a propylene-based copolymer comprising propylene and an α-olefin having a content of 15% by weight or less.

3. 3. The nail polish container according to claim 1, wherein the polypropylene resin composition has a haze of 50% or less at a wall thickness of 1 mm as measured in accordance with JIS K7136.

4. The nail polish container according to any one of claims 1 to 3, wherein the polypropylene resin composition further comprises at least one nucleating agent selected from the group consisting of 0.10 to 0.50 parts by weight of a nucleating agent (a) represented by the following formula (1), 0.01 to 0.30 parts by weight of a nucleating agent (b) represented by the following formula (2), and 0.005 to 0.04 parts by weight of a nucleating agent (c) represented by the following formula (3), relative to 100 parts by weight of the polypropylene resin. [Formula 1] (wherein n is an integer from 0 to 2; R 1 ~R 5 are each independently the same or different and are hydrogen, halogen, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 20 carbon atoms, alkoxy having 1 to 20 carbon atoms, alkoxycarbonyl having 1 to 20 carbon atoms, or phenyl; R 6 is an alkyl group having 1 to 20 carbon atoms. [chemical 2] (In the formula, R 1 is a direct bond, sulfur, an alkylene having 1 to 9 carbon atoms, or an alkylidene having 2 to 9 carbon atoms; R 2 and R 3 are the same or different and each is hydrogen, an alkyl having 1 to 8 carbon atoms, or an alkylaryl having 7 to 9 carbon atoms; M is Li, Na, K, Mg, Ca, Zn, Al-OH, or Al; and n is the valence of M. When M is AlOH, n=2, and when M is Al, n=3. [C3] (In the formula, R 1 , R 2 and R 3 are each independently an unsubstituted or substituted hydrocarbon group.

5. 5. The nail polish container according to claim 1, wherein the nail polish contains nitrocellulose as a component.

Citation Information

Patent Citations

  • Low-color processing, heat and light stabilizer system for polypropylene fibers

    JP1996509031A

  • Polypropylene composition and use thereof

    JP1997296085A

  • Manicure container having cap with applying member

    JP2003175961A

  • Bottle for liquid cosmetic

    JP2003230427A

  • Gravure ink composition for front printing

    JP2012012597A