Method for producing pigment composition for color filters, and method for producing colored composition for color filters
By dispersing quinacridone pigment and quinophthalone dye derivatives in a water-based medium and applying solvent salt milling, the method addresses dispersion stability and contrast ratio issues, resulting in improved red pixel formation in color filters.
Patent Information
- Application Number
- JP2021072235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-04-22
AI Technical Summary
Existing color filters using dispersed pigments face issues with dispersion stability and contrast ratio due to light scattering, leading to reduced brightness and contrast, particularly in red pixels, despite the use of quinacridone pigments and dye derivatives.
A method involving the dispersion of quinacridone pigment and quinophthalone dye derivatives in a water-based medium, followed by solvent salt milling and mixing under controlled temperatures, to enhance dispersion stability and form red pixels with a high contrast ratio.
The method produces a pigment composition with excellent dispersion stability and high contrast ratio, suitable for forming red pixels in color filters, enhancing brightness and contrast in devices like color liquid crystal displays and CCDs.
Smart Images

Figure 0007584349000001 
Figure 0007584349000002 
Figure 0007584349000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a pigment composition for color filters, a pigment composition for color filters, and a coloring composition for color filters. [Background technology]
[0002] In a typical color liquid crystal display device, a transparent electrode for driving the liquid crystal is formed on a color filter by vapor deposition or sputtering, and an alignment film for aligning the liquid crystal in a certain direction is further formed on top of the transparent electrode. In order to improve the performance of the transparent electrode and the alignment film, it is necessary to treat the color filter at a high temperature of 200°C or higher, preferably 230°C or higher, in the manufacturing process for forming the color filter. For this reason, it is mainstream to form color filters using a pigment with excellent light resistance and heat resistance, and using a colorant in which such a pigment is dispersed by a method called a pigment dispersion method.
[0003] However, color filters formed using dispersed pigments have problems such as the scattering of light by the pigments, which disrupts the degree of polarization controlled by the liquid crystals. In other words, when blocking light (OFF state), light leaks, and when transmitting light (ON state), the transmitted light is attenuated, which can reduce the brightness ratio (contrast ratio) on the display device in the ON and OFF states.
[0004] In recent years, in order to realize high brightness and high contrast of color filters, finely-processed pigments are often contained in filter segments. A typical pigment is a mixture of primary particles, which are obtained by pigmenting crude particles having a particle diameter of 10 to 100 μm obtained by chemical reaction, and secondary particles, which are aggregates of the primary particles. Even if such pigments are finely-processed by various fine processing methods, the finely-processed pigments generally tend to aggregate. Moreover, primary particles and secondary particles of pigments that are too fine tend to form huge lumpy pigment solids. Furthermore, even if finely-processed pigments are dispersed in a carrier containing a resin or the like and stabilized as close as possible to primary particles, it has been difficult to obtain pigment compositions or coloring compositions with good dispersion stability.
[0005] Pigment dispersions containing quinacridone pigments have been used in red coloring compositions for color filters, and have been attracting attention again in recent years from the viewpoint of high color reproducibility. However, since it has been difficult to ensure the dispersion stability, methods for improving the dispersion stability using dye derivatives, etc. have been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-38061 A [Patent Document 2] JP 2019-109487 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, even with the methods proposed in Patent Documents 1 and 2, the dispersion stability of the resulting colored composition is not necessarily excellent, and there is room for further improvement. In addition, the contrast ratio of a color filter formed using the resulting colored composition is also not necessarily sufficient, and further improvement is required.
[0008] The present invention has been made in consideration of the problems associated with the conventional techniques, and an object of the present invention is to provide a method for producing a pigment composition for color filters, which is capable of preparing a coloring composition for color filters that has excellent dispersion stability of a quinacridone pigment and is capable of forming red pixels with a high contrast ratio.
[0009] Another object of the present invention is to provide a pigment composition for color filters produced by the above-mentioned production method, which is capable of preparing a coloring composition for color filters that has excellent dispersion stability of quinacridone pigments and can form red pixels with a high contrast ratio.Furthermore, an object of the present invention is to provide a coloring composition for color filters obtained by using the above-mentioned pigment composition for color filters, which has excellent dispersion stability of quinacridone pigments and can form red pixels with a high contrast ratio. [Means for solving the problem]
[0010] That is, according to the present invention, there is provided a method for producing a pigment composition for color filters, which will be described below. [1] A method for producing a pigment composition for color filters, comprising a step of mixing a quinacridone pigment with at least one quinophthalone dye derivative selected from the group consisting of a sulfonated quinophthalone dye, a metal salt of a sulfonated quinophthalone dye, and an amine salt of a sulfonated quinophthalone dye in a dispersed state in a dispersion medium, wherein the dispersion medium is a liquid medium containing water as a main component. [2] The method for producing a pigment composition for color filters according to [1] above, comprising mixing the quinacridone pigment and the quinophthalone colorant derivative in a state of being dispersed in the dispersion medium at 0 to 100°C. [3] The method for producing a pigment composition for color filters according to [1] or [2] above, further comprising a step of subjecting the quinacridone pigment and the quinacridone pigment derivative to a solvent salt milling treatment, wherein the quinacridone pigment derivative is a phthalimide alkylated quinacridone. [4] The method for producing a pigment composition for color filters according to any one of [1] to [3] above, wherein the quinacridone pigment is at least one selected from the group consisting of CI Pigment Red 122, CI Pigment Red 202, CI Pigment Red 207, and CI Pigment Red 209.
[0011] According to the present invention, there is also provided a pigment composition for color filters as shown below. [5] A pigment composition for color filters, produced by the production method according to any one of [1] to [4] above.
[0012] Furthermore, according to the present invention, there is provided a coloring composition for color filters as shown below. [6] A coloring composition for color filters, comprising the pigment composition for color filters according to [5] above. Effect of the Invention
[0013] According to the present invention, it is possible to provide a method for producing a pigment composition for color filters, which is capable of preparing a coloring composition for color filters that has excellent dispersion stability of a quinacridone pigment and is capable of forming red pixels with a high contrast ratio.
[0014] Moreover, according to the present invention, it is possible to provide a pigment composition for color filters capable of preparing a color composition for color filters that is excellent in dispersion stability of quinacridone pigments and capable of forming red pixels with a high contrast ratio. Furthermore, according to the present invention, it is possible to provide a color composition for color filters that is excellent in dispersion stability of quinacridone pigments and capable of forming red pixels with a high contrast ratio. The color composition for color filters of the present invention is useful as a color composition for producing a color filter used in, for example, solid-state imaging devices such as color liquid crystal display devices, C-MOS (Complementary Metal Oxide Semiconductors), and CCDs (Charge Coupled Devices). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Method of manufacturing a pigment composition for color filters> Hereinafter, the embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. One embodiment of the manufacturing method of the pigment composition for color filters (hereinafter also referred to as "pigment composition for CF") of the present invention has a step of mixing a quinacridone pigment and a quinophthalone dye derivative in a state of being dispersed in a dispersion medium. And, as the quinophthalone dye derivative, at least one selected from the group consisting of a sulfonated quinophthalone dye, a metal salt of a sulfonated quinophthalone dye, and an amine salt of a sulfonated quinophthalone dye is used. Hereinafter, the manufacturing method of the CF pigment composition of this embodiment will be described in detail.
[0016] (Mixing process) The method for producing a pigment composition for CF according to the present embodiment (hereinafter, also simply referred to as the "production method") includes a step (mixing step) of mixing a quinacridone pigment and a quinophthalone colorant derivative in a state where they are dispersed in a dispersion medium. By mixing a quinacridone pigment and a quinophthalone colorant derivative in a state where they are dispersed in a dispersion medium, it is possible to obtain a pigment composition for color filters that has excellent dispersion stability of the quinacridone pigment and can prepare a coloring composition for color filters that can form red pixels with a high contrast ratio, although the reason is not necessarily clear.
[0017] As the dispersion medium, a liquid medium containing water as a main component is used. The liquid medium may contain liquid media other than water or various inorganic salts, etc., as necessary. As the liquid medium other than water, a water-soluble organic solvent can be used. However, the content of water in the dispersion medium is preferably 50% by mass or more, more preferably 80% by mass or more, and particularly preferably 95% by mass or more. Among them, it is most preferable to use water as the dispersion medium.
[0018] The quinacridone pigment and the quinophthalone colorant derivative dispersed in a dispersion medium are mixed preferably at 0 to 100° C., more preferably under heated conditions, and particularly preferably at 40 to 90° C. By mixing under heated conditions, the dispersion stability of the quinacridone pigment is further improved, and the contrast ratio of the formed color filter can be further increased.
[0019] After mixing the quinacridone pigment and the quinophthalone colorant derivative, the mixture is filtered and washed, and if necessary, dried and pulverized to obtain the desired pigment composition for CF. The drying method may be a method of heating to 80 to 120°C using a heat source installed in a dryer. The drying method may be either a batch method or a continuous method. As the dryer, a box dryer, a band dryer, a spray dryer, or the like may be used. As the pulverization method, a pulverization method using a mortar, a hammer mill, a disk mill, a pin mill, a jet mill, or the like may be used.
[0020] [Quinacridone pigments] Quinacridone pigments are components that function as colorants. Examples of quinacridone pigments include CI Pigment Violet 19 and 42; CI Pigment Red 122, 202, 206, 207, and 209; and CI Pigment Orange 48 and 49. Among these, CI Pigment Red 122, CI Pigment Red 202, CI Pigment Red 207, and CI Pigment Red 209 are preferred from the viewpoint of hue.
[0021] The average primary particle diameter of the quinacridone pigment is preferably 10 to 50 nm. By using a quinacridone pigment having an average primary particle diameter within the above range, the brightness and contrast of the obtained color filter can be further improved. In this specification, the "average primary particle diameter" refers to the median diameter (D 50) When the average primary particle size of the quinacridone pigment exceeds 50 nm, the brightness and contrast ratio of the color filter may be somewhat lower. On the other hand, when the average primary particle size of the quinacridone pigment is less than 10 nm, it may be somewhat difficult to disperse the pigment and to ensure the flowability of the colored composition, so that the brightness and contrast ratio of the color filter tend to be somewhat lower.
[0022] [Quinophthalone dye derivatives] The quinophthalone dye derivative is at least one selected from the group consisting of a sulfonated quinophthalone dye, a metal salt of a sulfonated quinophthalone dye, and an amine salt of a sulfonated quinophthalone dye. The quinophthalone dye derivative is represented, for example, by the following general formula (1).
[0023] TIFF0007584349000001.tif56170 (In the general formula (1), X's each independently represent a halogen atom, m1 and m2 each independently represent a number from 0 to 4, M represents a hydrogen atom, a metal atom, an amino group, an organic amino group, or a quaternary ammonium base, and n represents a number from 1 to 2.)
[0024] Examples of metals constituting the metal salt of sulfonated quinophthalone dye include sodium, potassium, calcium, barium, iron, magnesium, aluminum, nickel, cobalt, and strontium. Among them, aluminum salt of sulfonated quinophthalone dye is preferred. Aluminum salt of sulfonated quinophthalone dye has good dispersibility as a pigment dispersant and can improve isolation during production. Furthermore, it is possible to obtain a composition that has low viscosity and excellent flow characteristics and viscosity stability over time.
[0025] Examples of amines constituting the amine salt of the sulfonated quinophthalone colorant include lower amines such as ammonia, dimethylamine, trimethylamine, diethylamine, triethylamine, hydroxyethylamine, dihydroxyethylamine, 2-ethylhexylamine, N,N-dimethylaminopropylamine, N,N-diethylaminopropylamine, and N,N-dibutylaminopropylamine; long-chain alkylamines such as laurylamine, oleylamine, palmitylamine, stearylamine, and dimethyllaurylamine; and quaternary ammonium ions having a long-chain alkyl group such as laurylammonium, stearylammonium, lauryltrimethylammonium, dilauryldimethylammonium, stearyltrimethylammonium, and distearyldimethylammonium. Among these, when a salt with a quaternary ammonium ion having an alkyl group with 12 or more carbon atoms such as laurylammonium or stearylammonium is used, a coloring composition having excellent dispersion stability and particularly high storage stability can be obtained.
[0026] The content of the quinophthalone colorant derivative in the pigment composition for CF is preferably 1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the quinacridone pigment.
[0027] (Refining process) By subjecting the quinacridone pigment to a micronization treatment in advance to reduce the primary particle size, the brightness and contrast of the resulting color filter can be further improved. Micronization treatment methods include a method of mechanically pulverizing the pigment (grinding method), a method of dissolving the pigment in a good solvent and then putting it into a poor solvent to precipitate the pigment (precipitation method), and a method of producing a pigment with a desired primary particle size (synthetic precipitation method).
[0028] The grinding method is a method in which a pigment is mechanically kneaded (so-called "solvent salt milling process") together with a grinding agent such as a water-soluble inorganic salt and a water-soluble organic solvent that does not dissolve the grinding agent using a ball mill, sand mill, kneader, or the like, and then the grinding agent and the water-soluble organic solvent are washed away with water and dried. Note that, since the pigment may undergo crystal growth during the solvent salt milling, it is preferable to add a solid resin, a dispersing aid, or the like to the water-soluble organic solvent to suppress the crystal growth of the pigment.
[0029] The manufacturing method of this embodiment preferably further includes a step of subjecting the quinacridone pigment and the quinacridone pigment derivative to a solvent salt milling treatment (solvent salt milling treatment step) before the above-mentioned mixing step. The solvent salt milling treatment step is a step of kneading and grinding the quinacridone pigment, the quinacridone pigment derivative, a grinding agent, a water-soluble organic solvent, etc., in a kneading machine. As the kneading machine, a kneader, a mixer, etc. can be used. As the grinding agent, a water-soluble inorganic salt such as sodium chloride, potassium chloride, sodium sulfate, etc. can be used. The average particle size of the inorganic salt is preferably 0.3 to 70 μm.
[0030] Examples of the water-soluble organic solvent that can be used include diethylene glycol, glycerin, ethylene glycol, propylene glycol, liquid polyethylene glycol, liquid polypropylene glycol, 2-(methoxymethoxy)ethanol, 2-butoxyethanol, 2-isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol, etc. When performing the solvent salt milling treatment, organic pigments and pigment derivatives other than quinacridone pigments and quinacridone pigment derivatives may be further used for the purpose of color matching.
[0031] The inorganic salt and the water-soluble organic solvent may be charged in their entirety from the start of the solvent salt milling treatment, or may be charged in portions. The temperature during the solvent salt milling treatment is preferably 150° C. or lower, and more preferably 50 to 120° C. The time for the solvent salt milling treatment is preferably 3 to 36 hours, and more preferably 3 to 24 hours.
[0032] After the solvent salt milling process, the grinding agent such as inorganic salt and the water-soluble organic solvent are removed by washing with water or hot water. The obtained solid matter may then be dried and pulverized. The quinacridone pigment derivative may be added after removing the grinding agent and the water-soluble organic solvent. Considering that the product is to be used as a material for manufacturing pixel parts of color filters, it is preferable to wash the filtrate until the specific conductivity is 50 μS / cm or less, and more preferably 20 μS / cm or less.
[0033] [Quinacridone pigment derivatives] The quinacridone pigment derivative is a phthalimide alkylated quinacridone. The quinacridone pigment derivative is, for example, a pigment derivative represented by the following general formula (2).
[0034] TIFF0007584349000002.tif44170 (In the general formula (2), Y and Z each independently represent a hydrogen atom, a methyl group, or a chlorine atom, and s represents a number from 1 to 3.)
[0035] The content of the quinacridone pigment derivative in the pigment composition for CF is preferably 1 to 20 parts by mass, and more preferably 3 to 20 parts by mass, based on 100 parts by mass of the quinacridone pigment.
[0036] <Pigment composition for color filters> One embodiment of the pigment composition for color filters (pigment composition for CF) of the present invention is manufactured by the manufacturing method of the pigment composition for CF described above. Since the pigment composition for CF of this embodiment is manufactured by the manufacturing method described above, it is possible to prepare a coloring composition for color filters that has excellent dispersion stability of quinacridone pigment and can form red pixels with a high contrast ratio. It is presumed that, for example, the surface state and dispersion state of the quinacridone pigment in the obtained pigment composition for CF, and the interaction state of each component, etc. are changed by manufacturing by the manufacturing method described above, and a pigment composition for CF showing the expected characteristics is obtained. However, it is substantially difficult or impossible to analyze and confirm the surface state and dispersion state of the quinacridone pigment, and the interaction state of each component, etc.
[0037] <Coloring composition for color filters> One embodiment of the coloring composition for color filters (hereinafter also referred to as "coloring composition for CF") of the present invention contains the above-mentioned pigment composition for CF. Therefore, the coloring composition for CF of this embodiment has excellent dispersion stability of quinacridone pigment and can form red pixels with high contrast ratio.
[0038] The CF coloring composition can further contain various components contained in conventionally known coloring compositions for forming pixels for CF. Specifically, the CF coloring composition can contain a polymer dispersant for dispersing the pigment, a binder resin, various organic solvents, and the like.
[0039] [Polymer dispersant] As the polymer dispersant, a conventionally known polymer for dispersing quinacridone pigments can be used. Among them, an acrylic copolymer having a structural unit derived from monomer A that adsorbs to the surface of the pigment is preferred. As the monomer A, a (meth)acrylic acid ester monomer having a hydrocarbon ring structure such as benzyl (meth)acrylate, 1-naphthyl (meth)acrylate, 2-naphthyl (meth)acrylate, cyclopentyl (meth)acrylate, or cyclohexyl (meth)acrylate is preferred. In addition, the acrylic copolymer preferably further has a structural unit derived from monomer B that adsorbs to the surface of the pigment and exerts a dispersion stabilizing effect. As the monomer B, a (meth)acrylic acid monomer or a (meth)acrylic acid ester monomer such as glycidyl (meth)acrylate and acid phosphooxyethyl methacrylate is preferred.
[0040] The acrylic copolymer may further have a constituent unit derived from a monomer (other monomer) other than the monomer A and the monomer B. Examples of the other monomer include (meth)acrylic acid esters. The content of the polymer dispersant is preferably 0.5 to 10 parts by mass (as non-volatile content) relative to 100 parts by mass of the quinacridone pigment.
[0041] The quinacridone pigment is preferably coated with a polymer used as a polymeric dispersant. Methods for coating the quinacridone pigment with a polymer include, for example, a method of adding a polymer to a pigment composition for CF and precipitating it; a method of adding an emulsion of a polymer to a pigment composition for CF; and a method of kneading and grinding the quinacridone pigment together with a polymer. In addition, in order to effectively suppress the crystal growth of the quinacridone pigment during the above-mentioned solvent salt milling treatment, it is preferable to utilize the excellent crystal growth suppressing effect of the quinacridone pigment derivative. For this reason, it is preferable that the polymer used as the polymeric dispersant does not inhibit the adsorption of the quinacridone derivative to the quinacridone pigment. After the suppression of crystal growth is completed, the quinacridone pigment and the quinacridone pigment derivative may be coated with a polymer.
[0042] By using the coloring composition for CF of this embodiment, it is possible to form a pixel portion of a color filter, particularly a red pixel having a high contrast ratio, according to a conventionally known method such as a pigment dispersion method. EXAMPLES
[0043] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.
[0044] <Production of quinophthalone dye derivatives> (Production Example 1) 30 parts of CI Pigment Yellow 138 (trade name "Paliotol Yellow K0960HD", manufactured by BASF) was dissolved in 300 parts of 101% sulfuric acid, and the mixture was stirred at 70°C for 8 hours to carry out a sulfonation reaction. The reaction solution was poured into 3,000 parts of ice water, and a precipitate was obtained by filtration. The precipitate was washed with water and dried to obtain a sulfonated quinophthalone dye derivative.
[0045] <Production of Pigment Composition> (Production Example 2) 100 parts of CI Pigment Red 202 (trade name "Cinquasia Magenta K4535FP", manufactured by BASF), 5 parts of phthalimide methylated quinacridone, 1,000 parts of sodium chloride, and 250 parts of diethylene glycol were put into a stainless steel kneader (manufactured by Inoue Seisakusho, capacity 5 L) and kneaded at 60 ° C for 7 hours by salt milling treatment to obtain a kneaded product. The kneaded product obtained was put into 3 L of warm water, heated to 70 ° C and stirred for 1 hour to obtain a slurry. Filtration and washing with water were repeated to remove sodium chloride and diethylene glycol to obtain a press cake. The obtained press cake and 5 parts of a sulfonated quinophthalone dye derivative were peptized in 3 L of water and stirred for 1 hour while heating to 70 ° C. After repeated filtration and washing with water, the mixture was dried at 80 ° C for 24 hours to obtain 106 parts of a pigment composition (A-1).
[0046] (Production Example 3) Except for changing the amount of the sulfonated quinophthalone colorant derivative to 10 parts, the same procedure as in Production Example 2 was carried out to obtain 110 parts of a pigment composition (A-2).
[0047] (Production Example 4) Except for changing the amount of the sulfonated quinophthalone colorant derivative to 20 parts, the same procedure as in Production Example 2 was carried out to obtain 120 parts of a pigment composition (A-3).
[0048] (Production Example 4) A pigment composition (A-4) (101 parts) was obtained in the same manner as in Production Example 2 described above, except that no sulfonated quinophthalone dye derivative was used.
[0049] (Production Example 5) Quinacridone Microparticulate Pigment (A-5) 96 parts of a pigment composition (A-5) was obtained in the same manner as in the above-mentioned Production Example 2, except that the phthalimidomethylated quinacridone and sulfonated quinophthalone colorant derivatives were not used.
[0050] <Preparation of Coloring Composition (Pigment Dispersion)> Example 1 The components shown below were mixed and stirred until uniform, and then dispersed for 3 hours using a paint conditioner and zirconia beads with a diameter of 0.5 mm to obtain a dispersion. 24 parts of propylene glycol-1-monomethyl ether-2-acetate were added to 96 parts of the dispersion filtered through a filter. After dispersing for 3 hours using a paint conditioner and zirconia beads with a diameter of 0.1 mm, the mixture was filtered to obtain a colored composition (DA-1). Pigment composition (A-1): 15 parts Dispersant solution (product name "BYK LPN-6919", manufactured by BYK-Chemie): 10 parts Binder resin solution (product name "SPC-2000", manufactured by Showa Denko): 17.1 parts Propylene glycol-1-monomethyl ether-2-acetate: 57.9 parts
[0051] (Examples 2 and 3) Colored compositions (DA-2) and (DA-3) were obtained in the same manner as in Example 1 above, except that pigment compositions (A-2) and (A-3) were used instead of pigment composition (A-1), respectively.
[0052] Comparative Example 1 The components shown below were mixed and stirred until uniform, and then dispersed for 3 hours using a paint conditioner and zirconia beads with a diameter of 0.5 mm to obtain a dispersion. 24 parts of propylene glycol-1-monomethyl ether-2-acetate were added to 96 parts of the dispersion filtered through a filter. After dispersing for 3 hours using a paint conditioner and zirconia beads with a diameter of 0.1 mm, the mixture was filtered to obtain a colored composition (DA-4). Pigment composition (A-4): 14.3 parts Sulfonated quinophthalone dye derivative: 0.7 parts Dispersant solution (product name "BYK LPN-6919", manufactured by BYK-Chemie): 10 parts Binder resin solution (product name "SPC-2000", manufactured by Showa Denko): 17.1 parts Propylene glycol-1-monomethyl ether-2-acetate: 57.9 parts
[0053] Comparative Example 2 A colored composition (DA-5) was obtained in the same manner as in Comparative Example 1, except that the amount of pigment composition (A-4) was 13.7 parts and the amount of sulfonated quinophthalone colorant derivative was 1.3 parts.
[0054] Comparative Example 3 A colored composition (DA-6) was obtained in the same manner as in Comparative Example 1, except that the amount of the pigment composition (A-4) was 12.6 parts and the amount of the sulfonated quinophthalone dye derivative was 2.4 parts.
[0055] Comparative Example 4 A colored composition (DA-7) was obtained in the same manner as in Comparative Example 1, except that 13.6 parts of pigment composition (A-5) was used instead of pigment composition (A-4) and the amount of sulfonated quinophthalone dye derivative was 1.4 parts.
[0056] <Evaluation> (Contrast ratio) The coloring composition was applied to a glass substrate using a spinner, dried at 90°C for 2 minutes, and then heated at 230°C for 30 minutes to form a coating film. The brightness and darkness of three coating films formed by changing the spinner speed were measured using a contrast meter (manufactured by Tsubosaka Electric Co., Ltd.), and the contrast ratio (brightness / darkness) was calculated. In addition, the chromaticity x of the coating film was measured using a spectrophotometer (product name "U-3310", manufactured by Hitachi, Ltd.). The chromaticity x and the contrast ratio were plotted on a graph to create an approximate straight line, and the contrast ratio value at chromaticity x = 0.500 was read. Then, the relative values (%) were calculated, with the contrast ratio value of the coating film formed with the coloring composition of Comparative Example 1 taken as 100%. The results are shown in Table 1.
[0057] (Viscosity (dispersion stability)) Using an E-type viscometer, the viscosity (mPa s) of the colored composition immediately after preparation (initial) and after standing at 45°C for one week was measured. The measurement conditions were temperature: room temperature (25°C) and rotor rotation speed: 60 rpm. The results are shown in Table 1.
[0058] TIFF0007584349000003.tif63170 [Industrial Applicability]
[0059] The pigment composition for CF of the present invention is useful as a material for obtaining a coloring composition for producing a color filter used in color liquid crystal displays, solid-state imaging devices such as C-MOS and CCD, and the like.
Claims
1. The method includes a step of mixing a quinacridone pigment with at least one quinophthalone colorant derivative selected from the group consisting of a sulfonated quinophthalone colorant, a metal salt of a sulfonated quinophthalone colorant, and an amine salt of a sulfonated quinophthalone colorant in a dispersion medium, The method for producing a pigment composition for color filters, wherein the dispersion medium is a liquid medium having a water content of 50 mass % or more.
2. 2. The method for producing a pigment composition for color filters according to claim 1, wherein the quinacridone pigment and the quinophthalone colorant derivative dispersed in the dispersion medium are mixed at 0 to 100°C.
3. The method further comprises a step of subjecting the quinacridone pigment and the quinacridone pigment derivative to a solvent salt milling treatment, 3. The method for producing a pigment composition for color filters according to claim 1, wherein the quinacridone pigment derivative is a phthalimide alkylated quinacridone.
4. The method for producing a pigment composition for color filters according to any one of claims 1 to 3, wherein the quinacridone pigment is at least one selected from the group consisting of C.I. Pigment Red 122, C.I. Pigment Red 202, C.I. Pigment Red 207, and C.I. Pigment Red 209.
5. A method for producing a coloring composition for color filters, comprising a step of dispersing a mixture containing a pigment composition for color filters produced by the production method according to any one of claims 1 to 4, a polymer dispersant for dispersing the quinacridone pigment, a binder resin, and an organic solvent.
Citation Information
Patent Citations
Fuchsine-colored composition for color filter, and color filter to be set on color image pickup tube device using the composition
JP2008038061A
Pigment dispersant, pigment composition, and pigment dispersion
JP2008050420A
Pigment dispersant, pigment composition, and pigment coloring agent
JP2017125085A
Red coloring composition for color filter
JP2019086753A
Colored composition for color filter and color filter
JP2019109487A