Method for producing a hydrophilic surface on PS / DVB copolymer particles

The described process enhances polymeric support materials by oxidative treatment and reaction with polyfunctional compounds, addressing mechanical instability and capacity issues in ion exchange chromatography, achieving stable and efficient ion separation with linear pressure profiles and improved retention times.

JP7584436B2Active Publication Date: 2024-11-15METROHM AG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021559918
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-10
Filing Date
2020-04-07
Publication Date
2024-11-15
Estimated Expiration
2040-04-07

AI Technical Summary

Technical Problem

Existing methods for modifying polymeric substrates for ion exchange chromatography fail to independently tune hydrophilicity and capacity, resulting in mechanically unstable particles with insufficient mechanical stability and theoretical plate numbers, leading to undesirable pressure increases during high-flow rate separations.

Method used

A process involving oxidative treatment and reduction or hydrolysis of polymeric support materials, followed by reaction with polyfunctional compounds, introduces hydroxyl groups and ion exchange groups, forming covalent bonds that enhance mechanical stability and allow independent adjustment of hydrophilicity and capacity.

Benefits of technology

The process produces mechanically stable particles with linear pressure increase under high flow rates, enabling efficient separation of ions with high signal symmetry and baseline separation, reducing secondary interactions and maintaining capacity and selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584436000001
    Figure 0007584436000001
  • Figure 0007584436000002
    Figure 0007584436000002
  • Figure 0007584436000003
    Figure 0007584436000003
Patent Text Reader

Abstract

The present invention relates to a method for modifying a polymeric support material for use as a stationary phase in an analytical or preparative separation method, the method comprising the steps of: providing a polymeric support material formed at least in part from an aromatic hydrocarbon compound containing at least two vinyl or allylic substituents; generating hydroxy groups on / in the polymeric support material by a process comprising an oxidation treatment of the polymeric support material and a subsequent reduction or hydrolysis treatment of the reaction product; and reacting the product from the previous step with a polyfunctional compound. The present invention also relates to a polymeric support material produced according to the method according to the invention for use as a stationary phase in an analytical or preparative separation method, particularly a chromatographic method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for modifying a polymeric support material for use as a stationary phase in an analytical or preparative separation process, comprising the steps of providing a polymeric support material at least partially formed from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents, generating hydroxy groups on / in the polymeric support material by a process comprising an oxidation treatment of the polymeric support material and a subsequent reduction or hydrolysis treatment of the reaction product, and reacting the product of the preceding step with a polyfunctional compound. The present invention further relates to a polymeric support material prepared by the process according to the invention for use as a stationary phase in an analytical or preparative separation process, in particular a chromatographic process. [Background technology]

[0002] Ion exchangers are usually composed of particulate materials that carry a charge on their surface so that they can retain ions. In the case of anion exchangers, these are often cationic ammonium compounds, but phosphonium and arsonium ions are also known. The exchange groups are monocationic. For purely electrostatic interactions, the retention time is determined by Coulomb's law. According to this, only the charge of the retarded anion will affect its retention time.

[0003] However, in ion chromatography in aqueous solutions, other factors that influence the retention behavior can be identified, such as the hydration of the anions and the hydration of the exchange groups. In addition, the polarizability of the ions involved, as well as weaker secondary interactions between the analyte and the exchanger substrate, also play a role. The retention behavior of an ion exchanger can be altered by modifying the support material for the exchange groups, since the hydrophilicity of the base polymer carrying the exchange groups also influences their hydration. Direct substitution of cationic groups also influences the retention behavior.

[0004] The art already contains approaches to tailor the hydrophilicity of particles for ion exchange chromatography, selectively accounting for other desirable parameters such as balanced capacity, high theoretical plate count, or chemical inertness of the ion exchange material.

[0005] In US20050181224, a crosslinked layer containing exchange groups is deposited on a sulfonated hydrophilic support particle by cyclic reactions of diepoxides and amines. With each cycle, the capacity of the ion exchanger increases. Hydrophilicity is essentially guaranteed. However, due to the alternating epoxy / amine chemical reactions, further hydrophilicity cannot be obtained independently of the capacity.

[0006] In EP3248678, porous divinylbenzene particles are coated with modified polysaccharides (agarose reacted with glycidyl phenyl ether), which are then crosslinked with a polyfunctional crosslinker (e.g. ethylene glycol diglycidyl ether) to form a polymer with hydroxyl groups on the surface. The substrate is then set with diethylaminoethyl chloride hydrochloride to obtain the actual ion exchange groups. The application also explores hydrophilic ion exchange particles with improved stability (breaking strength). It is also found that the substrate is unstable due to purely adsorptive forces acting between the particle and the initially gel-like coating.

[0007] In EP1217012, one starts with a hydrophobic vinyl alcohol ester polymer. First, the esters present are hydrolyzed, liberating the alcohol groups. The polymer becomes hydrophilic. The OH groups react with diepoxides and then with amines to coat the substrate. The hydrophilicity can be further increased by subjecting the base polymer to more extensive hydrolysis in a first step. However, this causes a loss of mechanical stability of the particles. Undesirable swelling behavior can occur.

[0008] In a publication by Caglayan et al. (J Sep Sci 2006, Vol. 29, 940), an attempt is made to optimize some of the mentioned parameters, such as theoretical soil number, pore size and surface expansion, by using poly(vinyl acetate-co-divinylbenzene) particle substrates of different compositions. According to the publication, an increase in the amount of vinyl acetate (and therefore an increase in the amount of OH groups in the hydrolyzed particles) leads to a sharp increase in reflux pressure when a column packed with the substrate is subjected to an increased flow rate. This undesirable back pressure is due to the lack of mechanical stability of the particles, which become deformed during the separation process.

[0009] US5503933 discloses hydrophilic coatings covalently bonded to hydrophobic surfaces and their preparation methods. Compounds are provided with hydrophobic and hydrophilic domains containing unsaturated groups to form coated surfaces. Hydrophobic surfaces with unsaturated groups are also provided. Molecules of the compound are adsorbed onto the hydrophobic surface, and the unsaturated groups of the hydrophobic domains of the molecules of the compound are then covalently bonded to the unsaturated groups of the hydrophobic surface by free radical reactions. In one embodiment, the hydrophilic coating can be covalently bonded to divinylbenzene cross-linked polystyrene. However, the resulting particles are only suitable for the separation of macromolecules. For use in other chromatographic techniques, especially ion chromatography, the theoretical plate number of the particles is insufficient due to the large diameter of the particles. As the particle size decreases, the mechanical load-bearing capacity of macroporous materials is not sufficient for the pressures generated in such chromatographic processes. Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention is to overcome the above-mentioned disadvantages in the prior art. Currently, there is a lack of a method that allows the hydrophilicity of the polymer substrate surface to be adjusted independently of the oxygen content of the polymer core substrate, and allows the polymer substrate to be coated in such a way that mechanically stable and robust particles are obtained. At the same time, the ion exchange substrate based thereon should be largely chemically inert and it should be possible to configure the hydrophilicity and capacity, or the selectivity and capacity, independently of each other. [Means for solving the problem]

[0011] This problem is solved by a process having the features of claim 1. It relates to a process for modifying a polymeric support material for use as a stationary phase in an analytical or preparative separation process. The invention further relates to a polymeric support material prepared according to the method according to the invention for use as a stationary phase in an analytical or preparative separation process, in particular a chromatographic process. The invention relates to a chromatography column filled with the polymeric support material according to the invention, to a method for separating analytes using the polymeric support material according to the invention, and to the use of the polymeric support material according to the invention for analytical and preparative separation of analytes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The method comprises the steps of providing a polymeric support material (step a), at least partially formed from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents, preferably at least partially formed from a divinylbenzene monomer; generating hydroxy groups on / in the polymeric support material by a process comprising oxidatively treating the polymeric support material (step b.1) followed by reducing or hydrolyzing the reaction product of step b.1 (step b.2); and optionally reacting the product of step b.2 with a multifunctional compound, in particular a compound having at least one first functional group reactive with hydroxy groups, preferably a halogen group, and at least one second functional group reactive with amine and / or hydroxy groups, preferably an epoxide group (step c).

[0013] Needless to say, functional groups that react with amines may react or be reacted simultaneously with other organoelement compounds of the fifth main group, i.e., arsines or phosphines.

[0014] As will be further explained below, particularly with respect to the process according to the invention, the steps according to the invention affect the oxygen content of the polymeric support material surface, and therefore the hydrophilicity of the polymeric support material surface is independent of the oxygen content in the polymeric support core substrate.

[0015] The polymeric support material provided in step a is typically provided as particles, preferably as spherical particles, particularly preferably as spherical particles having an average particle size (median) of 1 to 50 μm, even more preferably as spherical particles having an average particle size of 2 to 25 μm, particularly preferably as spherical particles having an average particle size of 3 to 9 μm. However, other polymeric support materials are also contemplated, in particular polymeric support materials in the form of membranes or monoliths.

[0016] The oxygen content of the surface of the polymeric support material is increased by initial oxidation and reduction or hydrolysis. Modifications can also generate oxygen atoms on / in the core polymeric support material that have no detectable oxygen content. The increased oxygen content affects the nature and expression of secondary interactions, particularly the hydrophilicity of the resulting polymeric support material. Furthermore, through a series of steps following the initial oxidation and reduction / hydrolysis, the capacity can be tuned independently of the surface oxygen content.

[0017] By surface of a polymeric carrier material or surface of a polymeric carrier material is meant in this context in particular the solution-accessible outer surface of a polymeric carrier material structure, as well as a layer of 1 to 30 nm directly adjacent to this outer surface, which may for example be arranged partially on the microstructure of a porous structure, and in particular the solution-accessible outer surface of a polymeric carrier material particle of porous or non-porous structure.

[0018] The first contribution to chemical and mechanical stability is made by the covalent bond between the polymeric support material and the coating. This is in contrast to the situation with latex-based ion exchangers, where the latex particles, and therefore the exchange groups, are held to the substrate by pure electrostatic interactions. The covalent bond also ensures high chemical inertness. The second contribution to mechanical stability is made by the fact that the core polymeric support material is formed at least in part from aromatic hydrocarbon compounds having at least two vinyl or allyl substituents, preferably at least in part from divinylbenzene monomers. The stability of this core polymeric support material is not affected by steps b.1 and b.2. The core polymeric support material is preferably monodisperse.

[0019] Step c, i.e. the reaction of the product of step b.2 with a polyfunctional compound, in particular a compound having at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with amine and / or hydroxy groups, is optional. If this step is omitted, the particles are suitable for use, for example, in size exclusion chromatography.

[0020] In particular, the preparation of ion exchange materials for use in anion exchange chromatography or cation exchange chromatography based on the polymer support material modified according to the present invention is described below. However, the use of the particles is in no way limited thereto. The particles can also be used in other analytical and preparative separation methods, such as other adsorption chromatography methods, HILIC chromatography (hydrophilic interaction liquid chromatography), reversed phase chromatography, solid phase extraction, etc.

[0021] In a preferred embodiment, the method comprises the above steps a, b and c, as well as further steps following step c, namely carrying out several coating cycles (step d). One coating cycle of step d comprises the steps of introducing or generating a hydroxy group by reacting a second functional group, preferably an epoxide group, introduced in step c, with a polyfunctional compound having a hydroxy group, in particular a polyol, or by hydrolysis or a combination thereof (step d.1); and reacting the product of step d.1 with a polyfunctional compound, in particular a compound having at least one first functional group, preferably a halogen group, reacting with a hydroxy group, and at least one second functional group, preferably an epoxide group, reacting with an amine and / or hydroxy group (step d.2). The number of coating cycles is between 0 and 20.

[0022] If the number of coating cycles is at least two, the introduction or generation of hydroxyl groups from the first iteration onwards obviously does not relate anymore, or at least not exclusively, to the functional groups introduced in step c, but mainly to the corresponding functional groups introduced in step d.2. This is especially true if the conditions are chosen such that, when the first coating cycle is carried out in step d.1, the second functional groups from step c are substantially completely reacted.

[0023] By increasing the number of coating cycles, the oxygen content on the surface of the polymeric support material can be further increased, and the hydrophilicity of the ion exchange material based on the polymeric support material can be increased. By choosing the appropriate degree of hydrophilicity, the interaction of the ion exchange material with highly hydrated ions (such as fluoride) can be increased and with very weakly hydrated ions (such as bromate, nitrate, chlorate, etc.) can be reduced. In this way, for example, the retention order of bromate and chloride can be influenced, so that bromate appears quantitatively before chloride in the chromatogram. Furthermore, it can be ensured that fluoride is separated from the injection peak, especially when using carbonate eluents.

[0024] Moreover, the method according to the invention allows obtaining ion exchange materials with high signal symmetry (asymmetry <1.5) and a theoretical plate count of >50,000 TP / m per column meter for seven standard anions (fluoride, chloride, nitrite, bromide, nitrate, phosphate and sulfate), all of which appear baseline separated from one another in the chromatograms, with an overall short total chromatography time.

[0025] The advantage of the high robustness of the particles is particularly evident when a column packed with the polymeric support material obtained by the above method is subjected to a pressure flow test. In such a pressure test, the pressure generation in the column is determined as a function of the continuously increasing flow rate. In the column according to the invention, the pressure depends linearly on the flow rate. This is in contrast to the results obtained with a conventional column packed with a hydrophilic pDVB substrate with a high vinyl acetate content. In the conventional column, the pressure increases more than linearly as a function of the flow rate. For example, a hyperbolic slope of the function can occur. This comes, for example, from the publication by Caglayan et al. (J Sep Sci 2006, Vol. 29, 940) cited at the beginning.

[0026] The performance of the column according to the invention after pressure testing is also better than that of conventional columns. On the one hand, compared to conventional columns, the column shows only a small increase in the pressure drop across the column after pressure testing. Moreover, the number of theoretical bottoms decreases in the course of the loading test of the column according to the invention to a much lesser extent than in the case of conventional columns (Caglayan et al., J Sep Sci 2006, Vol. 29, 940). Maintaining the pressure ratio and number of stages even when using high flow rates allows for an efficient high-performance separation process.

[0027] The method may then further comprise step e of introducing ion exchange groups into the reaction product of step c or d.2. Step e produces an ion exchange material from the polymeric support material that realizes the advantages associated with the polymeric support material. Hydrophilicity and capacity, or selectivity and capacity, can be independently adjusted in this ion exchange material according to the invention. The ion exchange material according to the invention also has a high number of theoretical soil.

[0028] Ion exchange groups are understood to be charged groups, in particular charged amine, arsine or phosphine groups, on the surface of the polymeric support material.

[0029] By a polymeric support material at least partially formed from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents, it is understood in the context of the present invention that the polymeric support material can be prepared by a polymerization reaction involving at least an aromatic hydrocarbon compound having at least two vinyl or allyl substituents. Preferably, the polymeric support material is formed by a polymerization reaction with divinylbenzene. However, reactions with trivinylbenzene and divinylnaphthalene and equivalent compounds known to those skilled in the art are also contemplated.

[0030] The process can be characterized in that the polymeric support material of step a, at least partially formed from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents, is further partially formed from a monomer selected from the group consisting of ethylvinylbenzene, vinyl acetate, styrene, and combinations thereof. In this regard, the proportion of aromatic hydrocarbon compounds having at least two vinyl or allyl substituents is preferably at least 50% by weight. For example, the polymeric support material of step a may comprise at least 50% by weight of divinylbenzene units. Such polymeric support materials have advantageous properties in terms of pore structure, in particular a large number of double bonds available for subsequent surface modification.

[0031] The process can be characterized in that the oxidation treatment in step b.1 is a treatment with a peracid, preferably selected from the group consisting of metachloroperbenzoic acid (m-CPBA), peroxyformic acid, peroxyacetic acid, peroxytrifluoroacetic acid, treatment with KMnO4, treatment with oxygen plasma or a combination thereof. Exposing the polymer to a peracid oxidizes any double bonds present and makes them available for subsequent reduction or hydrolysis. Needless to say, this effect can in principle also be achieved by other oxidation processes known to those skilled in the art, for example ozonolysis.

[0032] It is particularly preferred if peracid is used in step b.1. The advantage of peracid is that a higher oxygen content can be achieved than, for example, plasma treatment. With oxygen plasma, an oxygen content of 2.0% can be achieved, whereas with mCPBA, for example, an oxygen content of 3.2% can be achieved, measurable by elemental analysis. If peracid is used, it can be added to the polymer in suspension or formed in situ from acid and hydrogen peroxide. Preferably, m-CPBA is added to the suspended core polymeric support material, for example PS / DVB polymeric support material, as it is less complicated to handle as a solid.

[0033] In a preferred embodiment, the reduction treatment of the reaction product from the oxidation step b.1 is carried out in step b.2 with a reagent for reducing polar bonds, preferably a metal hydride. This can be for example NaBH4, BH3, LAH, NaH, CaH. The use of a hydride has the advantage that the dissolved reagent can penetrate into the pores of the particles. This is not possible for example with palladium on activated carbon. Compared to hydrolysis with hydrochloric acid (see example 3), which can convert epoxides to hydroxylenes, the reduction with a metal hydride can also convert carbonyls and carboxyls to hydroxylenes. The reduction converts the formed oxidation products into alcohols. Preferably, lithium aluminum hydride in diethyl ether is used. In one embodiment, a 1-20% w / v suspension of the polymer in dry diethyl ether is presented, to which 5-100% w / w of the polymer dry weight of lithium aluminum hydride is added. Particularly preferred is a 5-15% w / v polymer suspension in dry diethyl ether to which lithium aluminum hydride is added in an amount of 5-20% w / w of the polymer dry weight. Temperatures of 25-70°C, particularly preferred the boiling temperature of diethyl ether, and reaction times of 1 min-72 h, particularly preferred 3 h-48 h, can be selected.

[0034] The OH groups generated on the polymer support surface by the above process are now available in sufficient numbers for modification in step c.As an alternative to reducing conditions, hydrolytic conditions can also be selected.

[0035] The reaction product of step b.2 is reacted with a polyfunctional compound, in particular a compound having at least one first functional group, preferably a halogen group, that reacts with hydroxy groups, and at least one second functional group, preferably an epoxide group, that reacts with amine and / or hydroxy groups.

[0036] The first functional group reacting with the hydroxy group can be a structure capable of nucleophilic attack by an OH group or an amine group, for example a halocarbon, an epoxide, a tosylate, a methyl sulfide, or a mixture thereof. The second functional group reacting with the amine and / or hydroxy group can be, for example, an epoxide. Preferably, the polyfunctional compound of step c is epichlorohydrin (ECH). For example, the substrate can be suspended in epichlorohydrin (preferably 5-30% w / v solids in ECH, more preferably 10-20% w / v solids in ECH). It can then be reacted with bases such as aqueous alkali and alkaline earth metal hydroxides. For this purpose, aqueous solutions of NaOH and KOH have proven suitable, particularly preferably 10-50% w / w NaOH in a ratio of ECH:NaOH(aq)=1:(0.1-10). Particularly preferably, the reaction is carried out using a quaternary ammonium salt as phase transfer catalyst. Alternatively, the substrate suspended in ECH can be reacted with a quaternary ammonium hydroxide. Tetramethylammonium hydroxide has been found to be suitable for this purpose. Preferably, the same amount of dimethylsulfoxide (DMSO) as ECH is added to the suspension of polymer in ECH prepared as above, preferably between 1 and 10 mmol of tetramethylammonium hydroxide in concentrated aqueous solution is added per gram of polymer used, more preferably between 2 and 5 mmol of tetramethylammonium hydroxide (aq).

[0037] However, the polyfunctional compound used in step c, which comprises at least one first functional group that reacts with hydroxy groups and at least one second functional group that reacts with amine and / or hydroxy groups, can also be a spacer molecule.

[0038] In the context of the present application, spacer molecules (spacers for short) mean molecules with at least two functional groups as described above, which ensure a spacing of at least 3 atoms, preferably 3 to 20 atoms, between the surface of the modified polymeric support material and the ion exchange groups to be introduced. The spacer molecules are attached in the finished ion exchange material on the one hand to the modified polymeric support material and on the other hand to the exchange groups. The functional groups of the spacer molecules may be structures that can be nucleophilically attacked by OH or amine groups, e.g. halohydrocarbons, epoxides, tosylates, methylsulfides or mixtures thereof. The spacer atoms may be carbon chains, but may also contain heteroatoms, e.g. ether groups or thioethers. The spacer molecules provide spacing between the substrate and the ion exchange groups. The function of the spacer is to prevent ions from interacting with the substrate. This counteracts unwanted peak broadening of the chromatogram. Spaced carbon chains with ether groups are preferred due to their higher hydrophilicity. Particularly preferably, the spacer has glycidyl groups that can react with amines, phosphines, arsines and / or hydroxy groups. Particularly preferred is the spacer molecule 1,4-butanediol diglycidyl ether.

[0039] If in step d.1 the hydroxyl group is introduced by reaction of the second functional group introduced in step c (or optionally in step d.2) by reaction with a polyfunctional compound containing a hydroxyl group, the use of a diol is preferred. Butanediol is particularly preferred. A diol can be used as solvent and reactant, the reaction being carried out under base catalysis at elevated temperature. Particularly preferred is 0.1-1 mol / L KOH at 60-160 °C for 1-48 hours. Most preferably the temperature is 100-130 °C and the reaction time is 3-36 hours. By the addition of such a compound, the epoxide previously bonded to the substrate is converted into a chain containing OH groups.

[0040] In one embodiment, the polyfunctional compound used in step d.2 having at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with amine and / or hydroxy groups is an epihalohydrin, preferably epichlorohydrin. In this regard, the carrier polymer particles can first be suspended in epichlorohydrin (preferably at a solids content of 5-30% w / v in ECH, more preferably at a solids content of 10-30% w / v in ECH). The suspension can then be reacted with a base, such as an aqueous solution of an alkali or alkaline earth metal hydroxide. For this purpose, aqueous solutions of NaOH and KOH have proven suitable, particularly preferably 10-50% w / w NaOH in a ratio of ECH:NaOH(aq)=1:(0.1-10). Particularly preferably, the reaction is carried out using a quaternary ammonium salt as phase transfer catalyst.

[0041] However, spacer molecules may alternatively be used in step d.2. It is particularly preferred if spacer molecules are used at least in the last run of the coating cycle of step d.2.

[0042] A preferred feature of the present invention is that steps d.1 and d.2, both also called coating cycles, can be repeated. The number of coating cycles can be between 0 and 20, preferably between 0 and 10. However, it is preferred that the number of coating cycles is between 0 and 5, more preferably between 1 and 3.

[0043] The hydrophilicity of the polymeric support material increases with each cycle. By choosing the appropriate number of cycles, the hydrophilicity can be optimally adjusted to the mixture to be separated. In particular, by choosing the appropriate degree of hydrophilicity, the hydrophilic interaction of the substrate with strongly hydrated ions (such as fluoride) can be increased and the interaction with weakly hydrated ions (such as bromate, nitrate, chlorate). This can affect the retention order. The generation of each layer also reduces secondary interactions between polarizable ions such as chlorate or bromate on the one hand and the substrate on the other. The tailing of the signal peaks observed due to such secondary interactions is greatly reduced, so that even polarizable ions elute symmetrically. The total capacity of the exchange material is reduced.

[0044] In a preferred embodiment, a spacer molecule, in particular a diepoxide, preferably butanediol diglycidyl ether, is used as polyfunctional compound in step d.2 in the final run of the coating cycle d. The advantages of the spacer molecule have been described above in connection with step c. The reaction of the spacer molecule is preferably carried out by adding a polar solvent to the reaction mixture, in particular DMSO, preferably in a volume ratio of 1:(0.1-5) to the diglycidyl ether, more preferably in a ratio of 1:(0.5-1.5). Also preferred is the use of quaternary ammonium salts as phase transfer catalysts, particularly preferred is tetrabutylammonium bromide, preferably in a concentration range of 1-100 mmol / L, particularly preferred in a concentration range of 10-50 mmol / L, based on the total volume of the reaction mixture. Alkali and alkaline earth metal hydroxides and carbonates can be used as bases, preferably aqueous solutions of NaOH and aqueous solutions of KOH, particularly preferred is NaOH in a concentration range of 0.1-5 mol / L, most preferred in a concentration range of 0.1-1 mol / L. The volume ratio to the diglycidyl ether is 1:(0.1-5), preferably 1:(0.5-1.5). The preferred reaction temperature is 0-50° C., particularly preferably 20-30° C., and the preferred reaction time is 2-40 hours, particularly preferably 15-25 hours.

[0045] In a preferred embodiment, the ion exchange groups are introduced by reacting the compound of step c or d.2 with an organoelement compound of the fifth main group, preferably an amine, particularly preferably a tertiary amine. However, the ion exchange groups may also comprise phosphines or arsines instead of amines. Compounds containing amines with 1-3 organic radicals of 1-10 C atoms per radical, including cyclic compounds, have proven particularly suitable. The cyclic compounds may carry substituents. Examples of suitable compounds include nitrogen-containing heterocycles, such as pyridine, monosubstituted alkylpyrrolidines, monosubstituted alkylpiperidines or disubstituted alkylpiperazines, with or without hydrocarbon or hydroxy substituents. The hydrocarbon radicals of the amine compounds may also carry heteroatoms, such as oxygen or sulfur atoms, or other substituents.

[0046] However, it is also conceivable to introduce compounds suitable for cation exchange chromatography or HILIC methods. Suitable cationic functional groups include sulfonic acid, carboxylic acid, or combinations thereof. Preferably, the introduced compound may also have multiple functional groups, for example when an amino acid is introduced.

[0047] For example, to generate the cation exchange centers, the polymer epoxidized in the previous step can be suspended in a mixture of water and a polar solvent, preferably DMSO, and the preferred amine can be added. The preferred reaction time is between 0.5 and 48 hours at a preferred temperature of 20-70°C.

[0048] The step e of introducing ion exchange groups is preferably followed by a further step f, which comprises heating the polymeric support material provided with ion exchange groups in an alkaline solution. This allows adjusting the selectivity and capacity of the ion exchange material from the preceding step. This treatment is hereinafter referred to as removal. This treatment in particular consists in heating the particles provided with exchange groups in an aqueous alkaline solution, particularly preferably in an aqueous solution of an alkali metal or alkaline earth metal hydroxide or carbonate, for example in a sodium hydroxide solution. The preferred concentration of NaOH is in the range of 0.1 to 5 mol / L of base, with 0.2 to 2 mol / L of base being particularly preferred. The reaction temperature can be 20 to 100 ° C, particularly preferably 90 to 100 ° C, and the treatment time is 0.1 to 150 h, particularly preferably 2 to 6 h.

[0049] The stripping step changes the relative strength of interactions between the substrate and individual ions. In particular, secondary interactions with polarizable analytes can be reduced. The tailing of the signal peaks observed due to such secondary interactions is reduced, so that polarizable ions are also eluted symmetrically. At the same time, the electrostatic interaction capacity of the column is also reduced after stripping, reducing the total capacity of the ion exchange material.

[0050] Another aspect of the invention relates to a polymeric support material for use as a stationary phase in analytical or preparative separation processes, in particular chromatographic processes, obtainable by a process comprising the steps described above, at least steps a, b and c.

[0051] Another aspect of the invention relates to a polymeric support material for use as stationary phase in an analytical or preparative separation process, a chromatographic process, in particular obtained by a process comprising the steps described above, at least steps a and b, preferably at least steps a and b and c, in which the polymeric support material provided in step a is hydrophobic and microporous or mesoporous. By hydrophobic it is understood herein that the polymeric support material is non-polar, i.e. that it does not have monomeric units with a dipole moment >0.2D. By microporous or mesoporous it is understood herein that the polymeric support material has an average pore size of at most 50 nm.

[0052] Another aspect of the invention relates to a modified polymeric support material for use as a stationary phase in ion exchange chromatography, wherein the method comprises at least steps a, b, c and e.

[0053] The modified polymer support material thus obtained is - starting from the value of the maximum O content in each case, a difference of at least 20%, preferably a difference of at least 50%, particularly preferably a difference of 100%, is detectable in a cross section through the polymer support material by X-ray photoelectron spectroscopy XPS, - the oxygen-containing group is covalently attached to a core polymer support material; - the polymer support material is mechanically stable, so that the pressure drop across a column packed with the polymer support material increases only linearly as a function of increased flow rate; - the polymeric support material is uncharged at neutral pH; The polymeric carrier material is characterized in that it has a nitrogen content of less than 2%.

[0054] In particular, the modified polymeric support material has a higher oxygen content at the surface than in the core. The modified polymeric support material obtained by this process is also largely chemically inert. The polymeric support material thus obtained is tunable in that it can have a more or less oxygen-containing surface. Due to its structure and surface properties, this material is particularly suitable for use as a stationary phase in analytical or preparative separation processes. In particular, the substrate is suitable for further processing into particulate ion exchange materials prepared by the above method, which is also part of the present invention. However, the polymeric support material can also be further processed for use in other adsorption chromatography methods, HILIC methods, reversed-phase chromatography, solid-phase extraction, etc. Thanks to the microporous or mesoporous nature, the modified polymeric support material is suitable for the manufacture of columns with high theoretical plate numbers with corresponding good separation performance, since microporous and mesoporous particles are mechanically stable even at small diameters and therefore shorter diffusion paths can be set up.

[0055] Another aspect of the invention relates to a polymeric support material obtained by a process comprising the steps described above and modified according to the invention for use as a stationary phase in ion exchange chromatography, wherein ion exchange groups are further introduced into the polymeric support material according to step e.

[0056] The ion exchange material thus obtained is - starting from the value of the maximum O content in each case, a difference of at least 20%, preferably a difference of at least 50% and particularly preferably a difference of 100% is detectable in a cross section through the polymer support material by X-ray photoelectron spectroscopy XPS, - the oxygen-containing group is covalently attached to a core polymer support material; - the pressure drop in a column packed with a polymeric support material increases only linearly as a function of increasing flow rate, since the ion exchange material is mechanically stable; - apart from the introduced ion exchange groups, the ion exchange material is not based on a modification by epoxide-amine reaction that may be detectable by Hoffmann elimination; - optionally, the ion exchange material has a plate number of >50,000 TP / m; - optionally characterized in that the selectivity and capacity are further adjustable in a removal step f.

[0057] In particular, the ion exchange material has a higher oxygen content at the surface than in the core, for example the surface of the modified polymeric support material produced according to the process according to the invention up to and including step c has an oxygen content detectable by XPS measurement that is 50% higher, preferably 60% higher, based on the value of the maximum O content, than the interior particle region.

[0058] The advantage of the ion exchange material according to the invention is that hydrophilicity and capacity or selectivity and capacity can be configured in separate steps, i.e. independently of each other. The ion exchange material prepared by the method according to the invention shows only weak secondary interactions with polarizable ions and increases the retention time of strongly hydrated ions. Columns packed with hydrophilized ion exchange substrates show the desired selectivity. The material does not swell and shows advantageous properties in pressure tests. Particularly efficient columns can be packed with ion exchange materials.

[0059] The above polymeric support materials are suitable for use as stationary phases in ion chromatography processes, in particular for separating the standard ions fluoride, chloride, nitrite, bromide, nitrate, phosphate and sulfate. A high ion exchange capacity of the column is particularly necessary for separating small, monovalent or divalent ions. In contrast, convective or perfusion mass transfer of the analyte solution, achieved by macroporous structures, is undesirable. Macroporous structures are also often associated with poor mechanical load-bearing capacity.

[0060] The present invention relates to a polymeric carrier material provided in step a. - monomer units derived from aromatic hydrocarbon compounds having at least two vinyl or allyl substituents, preferably derived from divinylbenzene, - monomer units derived from ethylvinylbenzene, - monomer units derived from styrene, - A combination of these The present invention further relates to the above modified polymeric carrier material, which is substantially completely composed of monomer units selected from the group consisting of:

[0061] By "substantially completely constructed" it is understood herein that the total proportion of the recited monomer units in the polymeric carrier material provided in step a is at least 95% by weight, preferably at least 98% by weight, particularly preferably at least 99% by weight. In other words, the monomer units can be substantially completely derived from compounds that do not contain oxygen atoms, resulting in a hydrophobic particle core.

[0062] Another aspect of the present invention relates to a modified polymeric support material as described above, wherein the polymeric support material provided in step a has an average pore radius of 1-50 nm, preferably 2-25 nm, more preferably 2-10 nm, measurable by nitrogen adsorption of the BJH model, the measurement being carried out as described in Example 5 below.

[0063] Another aspect of the present invention is that the polymeric support material provided in step a has a nitrogen adsorption capacity of 80 to 1000 m as measured by BET model nitrogen adsorption. 2 / g, preferably 100 to 800m 2 / g, and more preferably 200 to 600m 2 The above modified polymer support material has a specific surface area of ​​1000 nm / g. The measurement is carried out as described in Example 5 below. The high specific surface area increases the capacity and resolution of the column, especially when separating small ions, such as standard ions.

[0064] Another aspect of the present invention relates to the above modified polymeric support material, wherein the polymeric support material provided in step a has a pressure stability of up to 220 bar, preferably up to 250 bar. By pressure stability, it is understood herein that the increase in pressure as a function of flow rate behaves only linearly. The measurement is carried out as described in Example 6 below. The high pressure stability is due to the small particle size and the micro / mesoporous nature of the particle structure.

[0065] Preferably, the modified polymeric carrier material is present as particles, preferably as spherical particles, more preferably as spherical particles with an average particle size (median) of 1 to 50 μm. Particularly preferably, the particles are present in the diameter range of 2 to 25 μm, very particularly preferably in the diameter range of 3 to 9 μm. The particle size in this case is the average value between the longest and shortest straight lines passing through the center of the particle and can be determined by scanning electron microscopy (SEM) and automated image evaluation.

[0066] The particle size can be adjusted by suitable stirring speed, choice of solvent, concentration of polymer in the solvent, etc. The methods are known to those skilled in the art. The carrier polymer of this shape and size has a volume / surface ratio that has been found to be particularly favorable for exchange capacity. It shows high diffusivity into the pores and is easily filled.

[0067] One aspect of the present invention relates to a modified polymeric support material as described above which is stable in the pH range of 0 to 14. By pH stability it is understood herein that the retention time of sulfate salt in a column packed with the modified polymeric support material after rinsing with 1M NaOH solution and / or after rinsing with 1M HCl solution does not deviate by more than 8%, preferably more than 5%, more preferably more than 3% from the retention time of sulfate salt in a column packed with a modified polymeric support material that has not been previously exposed to pH values ​​of 0 and / or 14. The method for measuring pH stability is taken from Example Embodiment 8 below.

[0068] Another aspect of the invention relates to an ion exchange chromatography column packed with a modified polymeric support material, preferably a particulate modified polymeric support material, producible by the method according to the invention.

[0069] Furthermore, the present invention relates to a process for the chromatographic separation of analytes, characterized in that a solution containing the analytes is contacted with a modified polymeric support material according to the invention and in particular passed through an ion exchange chromatography column according to the invention.

[0070] The present invention therefore relates to the use of the polymeric support material obtainable by the process according to the invention for the analytical or preparative separation of analytes, in particular in anion exchange chromatography, cation exchange chromatography and / or HILIC chromatography (hydrophilic interaction liquid chromatography).

[0071] In order to further illustrate the present invention, exemplary embodiments are described below, which do not have a limiting effect on the disclosure and claims of the present invention.

[0072] The following diagram is shown. [Brief description of the drawings]

[0073] [Figure 1] FIG. 1 is a schematic diagram of an exemplary modification sequence on a polymeric support material. [Diagram 2] FIG. 1 is a schematic diagram of modification steps b.1 and b.2. [Diagram 3] FIG. 1 is a schematic diagram of modification steps b.1 and b.2 followed by exemplary modification steps c and d.1. [Figure 4] FIG. 1 is a schematic diagram of alternative modification steps c or d.2. [Diagram 5] FIG. 1 is a schematic diagram of the result of modification step d.1 and subsequent reaction with BDGE (butanediol diglycidyl ether). [Figure 6]FIG. 2 is a schematic diagram of an example of a modification step e, which introduces ion-exchange groups, following step c or d.2. [Figure 7] FIG. 1 shows a chromatogram obtained on a chromatography column according to embodiment 1 or 4. [Figure 8] FIG. 2 shows chromatograms obtained on a chromatography column according to embodiment 1 or 4 with increasing repetitions of modification step d. [Figure 9] FIG. 2 shows the pressure-flow profile measured on a chromatography column according to the present invention. [Figure 10] FIG. 2 shows chromatograms obtained on a chromatography column according to embodiment examples 1 or 4 with increasing duration of step f. [Figure 11] FIG. 2 shows the pressure-flow profile measured on a chromatography column packed with the polymeric support material according to the present invention from process step b.2. [Figure 12] FIG. 1 shows the results of particle size analysis by SEM (number relative to diameter [μm]). EXAMPLES

[0074] Example 1 All materials used were classified as “pure” or “pa” (except hydrogen peroxide and formic acid), and the solvent was separated from less volatile components by distillation on a rotary evaporator.

[0075] Oxidation with potassium permanganate 10.0 g of PS / DVB (55% DVB in EVB) was placed in a 350 mL sulfation flask and suspended in 100 mL of acetonitrile. 5.0 g of KMnO4 dissolved in 100 mL of water was then added over 20 min. The reaction solution was adjusted to acidic pH with a small amount of acid. The suspension was stirred at 25 °C for 120 h. The particles were treated with semi-concentrated hydrochloric acid and then washed with ultrapure water. The product was dried to constant weight in a vacuum drying oven. The final weight was 9.7 g.

[0076] Reduction with lithium aluminum hydride 8.6 g of dried oxide particles were placed in a 500 mL reactor and mixed with 150 mL of THF. After external cooling to 5 °C under argon atmosphere, 1.5 g of lithium aluminum hydride was slowly added and mixed with another 50 mL of THF. The reactor was warmed to room temperature and stirred for 17 hours. The reaction was stopped by slow addition of water. It was then worked up with water / acetone, acidified with dilute sulfuric acid and washed neutral with water. After a final wash with acetone, the resulting solid was dried in a vacuum drying oven. 8.35 g of particles were obtained.

[0077] Reaction with epichlorohydrin (ECH) 7.6 g of reduced dried particles were placed in a 250 mL three-neck flask. 35 mL of epichlorohydrin was added and the mixture was evacuated three times and aerated with argon. The solution was heated to 45° C. Subsequently, 7 mL of phase transfer catalyst solution (3 g of tetrabutylammonium hydroxide in 10 mL of water) was added, followed by 140 mL of sodium hydroxide solution. The reaction was stirred for 3.5 hours and then stopped by the addition of water / ethanol. Workup was performed with water / ethanol or water / acetone. The product was used directly in the next step without drying.

[0078] Reaction with butanediol The above polymer was then suspended in 70 mL of butanediol with 1.98 g of KOH at room temperature and then stirred at 130° C. for 18 hours. The reaction mixture was then allowed to react for a few minutes. After completion of the reaction time, water was added to the reaction mixture and filtered. The polymer was washed several times with water and acetone. The filter cake was dried overnight in a vacuum drying oven. 7 g of polymer was obtained.

[0079] Installing the spacer 6.6 g of the above polymer was suspended in 16.5 mL DMSO and 16.5 mL butanediol diglycidyl ether, evacuated three times and then aerated. Then 1.4 mL of 1 M tetrabutylammonium bromide solution and 16.5 mL of 0.6 M NaOH(aq) were added and mechanically stirred for 22 h. The reaction was stopped by adding solvent. The reaction was stopped by adding a 1:1 mixture of water and ethanol. Repeated washing was performed with a water / ethanol mixture. Finally the product was filtered and dried. The polymer was used directly in the next step.

[0080] Introduction of anion exchange groups The above polymer was then suspended in 45 mL of DMSO without a transfer step, followed by the addition of 45 mL of water. The suspension was heated to 70° C. and 45 mL of N-methylpyrrolidine was added. After completion of the 2-hour reaction time, the reaction was stopped by the addition of acetic acid. The polymer was filtered off and washed several times with water. The wet polymer was used directly in the next step.

[0081] Removal The above polymer was suspended in 50 mL of water and 7.5 mL of 40% NaOH(aq) was added. The suspension was then stirred at 100° C. for 4 h. The reaction was stopped by filtration. The filter cake was washed several times with ultrapure water and then packed into a 4×100 mm PEEK column following known high pressure packing procedures.

[0082] Example 2 Oxidation by low pressure oxygen plasma 40 g of PS / DVB (55% DVB in EVB) was oxidized in a plasma powder plant using oxygen plasma. The particles can be directly further processed after treatment.

[0083] Reduction with lithium aluminum hydride (LAH) 30 g of the oxidized dry polymer was suspended in 250 mL of dry diethyl ether in a pressure-equalized 1000 mL reactor. Adjusted to 25° C., 6 g of lithium aluminum hydride was added slowly under argon atmosphere, heated to 30° C. with stirring for 6 h and stirred at room temperature for another 20 h. The reaction mixture was cooled to 0° C. and quenched by slowly adding 15 mL of ethyl acetate. Workup was performed with water, dilute sulfuric acid, water, NaOH solution 5 w%, ultrapure water and dilute hydrochloric acid.

[0084] The polymer was washed neutrally with ultrapure water, filtered and dried with acetone. The product was dried in a vacuum drying oven. 30 g of polymer was obtained.

[0085] Reaction with epichlorohydrin 5.0 g of the reduced dried particles were placed in a 250 mL three-neck flask and 25 mL of epichlorohydrin was added. The suspension was evacuated three times and aerated with argon. Subsequently, 1.75 mL of 1 M phase transfer catalyst solution (tetrabutylammonium bromide in water) and 25 mL of 30% sodium hydroxide solution were added, heated to 45 °C and stirred for 3.5 h. The reaction was stopped by the addition of water / ethanol. Purification of the product was performed by washing several times with water / ethanol or water / acetone. The product was used directly in the next step without drying.

[0086] Reaction with butanediol The above polymer was then suspended in 50 mL of butanediol with 1.3 g of KOH at room temperature and heated to 130° C. for 18 hours. The reaction mixture was then allowed to settle. After the reaction time was completed, 200 mL of water was added to the reaction mixture and filtered.

[0087] The filter cake was washed with water and acetone. The product was dried in a vacuum drying oven to give 4.2 g of dry product.

[0088] Installing the spacer 3.8 g of the above polymer was suspended in 10 mL DMSO and 10 mL butanediol diglycidyl ether, subjected to three pressure cycles, and the reaction vessel was backfilled with argon. Then, 0.8 mL of 1 M tetrabutylammonium bromide solution and 10 mL of 0.6 M NaOH(aq) were added and stirred for 22 h. The reaction mixture was then subjected to three pressure changes. Subsequently, 200 mL of a 1:1 mixture of water and ethanol was added to the reaction mixture and filtered. This washing procedure was repeated several times, and the product was filtered and dried and used directly in the next step.

[0089] Introduction of ion exchange groups The above polymer was suspended in 30 mL of DMSO, 30 mL of water was added, and the suspension was heated to 70°C. After reaching the reaction temperature, 30 mL of N-methylpyrrolidine was added and stirred at 70°C for 2 hours. After the reaction time was completed, 60 mL of concentrated acetic acid was added and the product was filtered off. The filter cake was washed with neutral water and used for removal.

[0090] Removal The above polymer was suspended in 100 mL of water, mixed with 20 mL of 30% NaOH(aq) and stirred for 28 hours at 100° C. After completion of the reaction time, the reaction was quenched by addition of hydrochloric acid, the suspension was filtered, the filter cake was washed several times with neutral water and then packed into a 4×100 mm PEEK column following known high pressure packing procedures.

[0091] Example 3 Oxidation with metachloroperbenzoic acid 20 g of PS / DVB (55% DVB in EVB) was placed in a 250 mL glass bottle with a screw cap and suspended in 93 g of dichloromethane. 5.5 g of metachloroperbenzoic acid was then added as a solid and the reaction mixture was mixed on a shaker at room temperature for 18 hours. The product was washed several times with ethanol and water and dried in a vacuum drying oven to constant weight. The final weight was 19.0 g.

[0092] Hydrolysis with hydrochloric acid 19 g of the oxidatively dried polymer was placed in a 250 mL glass bottle with a screw cap and suspended in 52 g of acetone and 13 g of 37% hydrochloric acid. The reaction mixture was mixed for 21 hours at 40° C. with a circulating air heated shaker. The mixture was then removed from the bottle. The product was washed with neutral water, then washed several times with water and acetone, and dried to constant weight in a vacuum drying oven. The final weight was 18.5 g.

[0093] Reaction with epichlorohydrin 11.8 g of the hydrolyzed dry polymer was suspended in a 250 mL three-neck flask containing 60 mL of epichlorohydrin. The reaction vessel was subjected to three vacuum / argon cycles. The reaction mixture was heated to 45° C. with stirring, then 3 mL of 1 M (aq) tetrabutylammonium bromide solution was added. This was followed by 60 mL of 30% (aq) sodium hydroxide solution, with vigorous stirring. After 22 hours of reaction, the reaction mixture was diluted with 200 mL of water and 200 mL of ethanol, then the polymer was filtered off. The polymer was washed with acetone, water, and then acetone again.

[0094] Reaction with butanediol 5 g of the above product was suspended in a 100 mL three-neck flask with 1.4 g of potassium hydroxide and 50 mL of 1,4-butanediol and mixed at 130° C. for 19 hours. The reaction mixture was then cooled and mixed with 45 mL of water. The product was filtered off, washed with water until neutral, and then dried in a vacuum drying oven to a constant weight. The final weight was 4.0 g.

[0095] Reaction with 1,4-butanediol diglycidyl ether 3.1 g of the above product was suspended in a 100 mL three-neck flask containing 8 mL of dimethyl sulfoxide and 8 mL of 1,4-butanediol diglycidyl ether. The reaction vessel was subjected to three vacuum / argon cycles. With stirring, 0.8 mL of 1 M (aq) tetrabutylammonium bromide solution and 8 mL of 0.6 M sodium hydroxide solution were added to the reaction. After 22 hours of reaction, 25 mL of water and 25 mL of ethanol were added to the reaction mixture, which was then filtered off. The product was washed once with water and ethanol.

[0096] Introduction of ion exchange groups The above product was suspended in a 100 mL three-neck flask with 15 mL of dimethyl sulfoxide, 15 mL of water, and 15 mL of N-methylpyrrolidine. The reaction mixture was stirred at 70° C. for 1 hour, then cooled and 30 mL of acetic acid was added. The polymer was filtered off and washed with water.

[0097] Removal The above product was suspended in 50 mL of water and 7.5 mL of 40% (aq) sodium hydroxide solution in a 100 mL round bottom flask and heated to 100° C. After 4 hours of reaction, the reaction mixture was cooled and filtered off. The product was washed twice with water and then packed into a 4×100 mm PEEK column following known high pressure packing procedures.

[0098] Example 4 Oxidation with formic acid 25.0 g of PS / DVB (55% DVB in EVB) was suspended in 188 mL of formic acid in a pressure-equalized 500 mL three-neck flask. 54 mL of 35% hydrogen peroxide was added slowly via a dropping funnel to externally cool the reaction solution. After the reaction heat dissipated, stirring was carried out at room temperature for 65 hours. After completion of the second reaction, the reaction mixture was washed acid-free with ultrapure water and then dried to constant weight in a vacuum drying oven. The final weight was 27.78 g.

[0099] Reduction with lithium aluminum hydride 27.64 g of the oxidized dried polymer was suspended in 270 mL of dry diethyl ether in a 500 mL three-necked pressure flask, cooled to 0° C. in an ice bath, and 8.8 g of lithium aluminum hydride was carefully added with stirring. After the addition was complete, the ice bath was removed and the reaction mixture was refluxed with stirring for 10 h and stirred at room temperature for an additional 24 h. The reaction was quenched by external cooling and the addition of diethyl ether, ethyl acetate, and ultrapure water.

[0100] After the remaining hydride was reacted, the reaction mixture was placed on ice and diluted cold sulfuric acid was added with stirring. The reaction mixture was washed with the following solutions: water, 5% NaOH solution, water, dilute acetic acid, water and acetone. The filter cake was filtered to dryness and dried in a drying oven. The yield was 26.20 g.

[0101] Reaction with epichlorohydrin 4.00 g of the polymer was suspended in 20 mL each of ECH and DMSO, sonicated in an ultrasonic bath for 15 min, then subjected to two pressure changes and the reaction vessel was backfilled with argon. After adding 4.30 mL of a 25% solution of tetramethylammonium hydroxide in water, stirring was carried out for 2 h at room temperature. The reaction mixture was filtered and washed with a 1:1 mixture of water and 2-propanol and acetone. The filter cake was filtered and dried.

[0102] Reaction with butanediol The above polymer was then suspended in 40 mL of butanediol with 1.12 g of KOH at room temperature and then stirred at 120° C. for 20 hours. The reaction mixture was washed several times with water and acetone. After completion of the reaction time, the reaction mixture was washed several times with water and acetone. The product was filtered and dried. The wet mass was 13.36 g.

[0103] Coating cycle: Reaction with epichlorohydrin (ECH) The still wet polymer from the above step was made up to 13.50 g with water and 1 mL of 1M tetrabutylammonium bromide and 20 mL of ECH were added. Subsequently, 10.5 mL of 50% NaOH(aq) was added and stirred for 5.5 hours. The reaction mixture was then washed with a 1:1 mixture of water and 2-propanol, and acetone. The filter cake was filtered to dryness.

[0104] Coating cycle: Reaction with butanediol The above polymer was suspended in 40 mL of butanediol with 1.12 g of KOH at room temperature and then stirred at 120° C. for 18 hours. The reaction mixture was washed several times with water and acetone. After completion of the reaction time, the reaction mixture was washed several times with water and acetone. The product was filtered and dried. The polymer was finally dried before further reaction. The yield was 5.66 g.

[0105] Installing the spacer 2.30 g of the above polymer was suspended in 6 mL DMSO and 6 mL butanediol diglycidyl ether, subjected to three pressure cycles, and the reaction vessel was backfilled with argon. With stirring, 0.5 mL of 1 M tetrabutylammonium bromide solution and 6 mL of 0.6 M NaOH(aq) were added and stirred for 22 hours. The reaction mixture was then subjected to three pressure changes. The reaction mixture was then washed with a 1:1 mixture of water and 2-propanol, filtered, and dried.

[0106] Introduction of anion exchange groups The above polymer was suspended in 5 mL of DMSO and mixed with 5 mL of water and 5 mL of N-methylpyrrolidine. The reaction mixture was then stirred at 70° C. for 1 hour. The reaction was quenched by adding water and dilute acetic acid. The filter cake was then washed with dilute hydrochloric acid, water and acetone. The resulting polymer was dried in a drying oven at 60° C. The yield was 2.54 g.

[0107] Removal The above polymer was suspended in 50 mL of water, 5 mL of 30% NaOH(aq) was added and stirred at 100° C. for 2 hours. The reaction was quenched by filtration followed by washing with water, dilute HCl, water and acetone. The filter cake was filtered to dryness and the polymer was subsequently dried in a drying oven at 60° C. No significant weight loss was observed.

[0108] FIG. 1 is a schematic diagram showing different exemplary modification sequences of the core polymeric support material (pDVB). After initial oxidation (b.1) and subsequent reduction (alternatively, subsequent hydrolysis, b.2), a polymeric support material with hydroxy groups on the surface (pDVB-OH) is available. The polymeric support material with OH groups (pDVB-OH) can then be reacted with epichlorohydrin (ECH). This gives the compound according to step c. Alternatively, the polymeric support material with OH groups (pDVB-OH) can be reacted with butanediol diglycidyl ether (BDGE) in step c.

[0109] According to the invention, the polymeric support material can be reacted after step b.2 with ECH, diol and subsequently again with ECH or BDGE in one or more coating cycles (steps c, d.1, d.2). The polymeric support material can also be reacted directly with BDGE, for example, after step b.2. As a result, a modified polymeric support material is obtained with suitable reactive functional groups on the surface. In the example shown, these are epoxy groups.

[0110] In principle, any combination of ECH / BDGE modifications in steps c and d.2, respectively, and any combination of diol conversion / hydrolysis in step d.1 is also conceivable, however, as mentioned above, it is preferred if a spacer molecule is inserted during the last coating cycle in d.2.

[0111] The modified polymeric support material shown in Figure 1 is suitable for the subsequent introduction of ion exchange groups. The oxygen content of the surface of the modified polymeric support material increases in the order of the variations listed in the preceding section (variations from top to bottom in the figure). The introduction of ion exchange groups to each product results in an ion exchange material with increasing hydrophilicity in the order of the variations listed. Increased hydrophilicity manifests itself, for example, in a decrease in the selectivity σ from NO3 to Cl.

[0112] Figures 2 to 6 are diagrams intended to illustrate the process steps according to the invention and to show the reaction sequences in a very simplified form. They do not claim to be complete. The focus is on the respective modifications of the polymeric support material surface. The parts of the polymeric support material that are not modified in the respective steps are shown in simplified form as spherical particles.

[0113] FIG. 2 is a schematic diagram showing modification steps b.1 and b.2. After oxidation and reduction (alternatively hydrolysis), a polymeric support material with OH groups on the surface is provided. It is known to those skilled in the art that not only ketones can be formed in the oxidation step. Depending on the treatment, especially during treatment with KMnO4, in addition to ketones, diols, diketones, or dicarboxylic acids may be formed as cleavage products. Such processes and intermediates are included in the claimed process and are not intended to be excluded by the examples shown in the figures.

[0114] 3 is a schematic diagram showing modification steps b.1 and b.2 followed by exemplary modification steps c and d.1. In the variant shown, the compound used in step c, having at least one first functional group that reacts with hydroxy groups and at least one second functional group that reacts with amine and / or hydroxy groups, is epichlorohydrin. In the embodiment shown, the polyfunctional compound containing hydroxy groups used in step d.1 is butanediol. The coating sequence consisting of alternating reactions with epichlorohydrin and butanediol can be repeated as d.1 and d.2. The resulting particles are shown again abstracted after the double arrow.

[0115] 4 shows a schematic diagram of the alternative modification step c or d.2. The compound used in step c or d.2, which has at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with ion exchange groups and / or hydroxy groups, is BDGE.

[0116] As shown in Figure 3, the conversion with BDGE can also complete one or more coating cycles. Figure 5 shows the result of the modification step d.1 in a schematic and exemplary manner. After the use of ECH in step c, a coating cycle is carried out using ECH in step d.2. After reaction with butanediol, the final step d.2 is then carried out using BDGE as a spacer. The result is a modified polymer support material with a higher surface oxygen content, other things being equal, than the support material obtained from the scheme of Figure 3 / Figure 4.

[0117] Figure 6 is a schematic diagram showing an example of a modification step e, which follows step c or d.2, to introduce ion exchange groups. In the example shown, the ion exchange groups are formed by quaternization of 1-methylpyrrolidine. After carrying out the modification according to the invention, a polymeric support material is obtained with side chains on the surface as shown in the examples.

[0118] FIG. 7 shows chromatograms obtained with a chromatography column according to example 1 or 4. The x-axis shows the run time in minutes. The y-axis shows the conductivity in μS / cm. For this purpose, the dry substrate was packed into a column of 150x4 mm. The eluents used were 6.0 mmol / L Na2CO3 and 1.0 mmol / L NaHCO3. The analytes of the standard solution are present with baseline separation from one another and the elution order from left to right is fluoride, bromate, chloride, nitrite, bromide, chlorate, nitrate, azide, phosphate, sulfate. Bromate is quantitatively present before chloride (peak at 5.2, 5.7 min run time) and the chromatogram shows high signal symmetry. The total run time of the column is short, 15 min. The chromatography column prepared under the conditions of example 1 gives comparable chromatograms.

[0119] FIG. 8 shows three chromatograms obtained with a chromatographic column according to Example 4. Example 1 provides very similar chromatograms. The x-axis shows the run time in minutes. The y-axis shows the conductivity in μS / cm. The curves show chromatograms of the same standard solution, with the elution order from left to right being fluoride, chloride, nitrite, bromide, nitrate, phosphate and sulfate. The number of repetitions of the modification step d.1 / d.2 was increased (from top to bottom). For the plotted curve A, the step sequence d.1 / d.2 was carried out once. For the dotted curve B, the step sequence d.1 / d.2 was carried out twice. For the dashed curve C, the step sequence d.1 / d.2 was carried out three times. Thus, specifically, for the depicted curve A, a polymer substrate was used that had undergone an oxidation / reduction treatment, was treated once with ECH and then once with 1,4-butanediol and was subsequently reacted with BDGE. Curve B used a polymer substrate that had been subjected to an oxidation / reduction treatment, treated with ECH, then 1,4-butanediol, then again with ECH, then 1,4-butanediol, and then reacted with BDGE. Curve C shows a polymer substrate that had undergone an oxidation / reduction treatment. The following sequence of steps was then performed: ECH, 1,4-butanediol, ECH, 1,4-butanediol, ECH, 1,4-butanediol, reaction with BDGE. In all three cases, the modified substrate was then reacted with methylpyrrolidine. From the chromatograms it is clear that the signals of the anions affected by tailing (nitrite, bromide, nitrate) acquire symmetry with increasing number of plating cycles. The selectivity σ from NO3 to Cl decreases with increasing number of plating cycles. The total capacity decreases.

[0120] FIG. 9 shows the pressure-flow profile measured on a chromatography column according to the invention, prepared according to Example 4, measured at room temperature. The y-axis shows the system pressure in MPa. The x-axis shows the flow rate in mL / min. Seventeen intervals of 20 min each were measured while gradually increasing the flow rate from 1 mL / min to 2.6 mL / min. The pressure depends linearly on the flow rate. This is in contrast to the results obtained with a conventional column packed with a hydrophilic pDVB matrix, where the pressure increases more than linearly as a function of the flow rate. For example, a hyperbolic slope of the function may result.

[0121] FIG. 10 shows chromatograms obtained with a chromatography column according to the invention, in particular a chromatography column packed with modified polymeric support material according to example 1 or 4. The x-axis shows the run time in minutes. The y-axis shows the conductivity in μS / cm. The duration of step f was varied. The dry substrate was packed into a 100x4 mm column. In each case the curves show the chromatograms of the same standard solution, with the elution order from left to right being fluoride, chloride, nitrite, bromide, nitrate, phosphate and sulfate. From top to bottom, the curves show the chromatograms available after removing the column substrate in step f during 0 min (A), 60 min (B), 120 min (C), 180 min (D), 240 min (E) and 300 min (F). If step f is omitted (0 min), the nitrate and phosphate peaks overlap. The total capacity decreases with increasing removal time. The analytes are baseline separated from one another and the chromatogram provides high signal symmetry. Total column run times are short, approximately 14-20 minutes.

[0122] Example 5 Determination of the average pore radius and specific surface area of ​​the polymeric support material provided in step a.

[0123] In Example 1, the modification according to the invention is carried out in PS / DVB (55% DVB in EVB), thereby providing a starting polymeric support material that is both hydrophobic and microporous or mesoporous. The starting polymeric support material provided is obtained as follows:

[0124] Preparation of polystyrene seed particles stabilized with polyvinylpyrrolidone and initiated with azobisisobutyronitrile in dispersion polymerization of styrene in ethanol.

[0125] Diameter 1.5 μm and M N = 15 kg / mol, M W = 55 kg / mol of polystyrene particles are obtained. The resulting polystyrene particles are swollen with an emulsion of 55% divinylbenzene (DVB) / 45% ethylvinylbenzene (EVB) and toluene in water / isoamyl alcohol, stabilized with polyvinyl alcohol, and subsequently polymerized with azobisisobutyronitrile. The radius is 5 μm and the porosity is 1 cm. 3 / g of porous, highly crosslinked poly(DVB-co-EVB) particles are obtained.

[0126] The average pore radius of the starting polymer support material was determined by nitrogen adsorption in the BJH (Barret, Joyner, Halenda) model. The specific surface area was determined by nitrogen adsorption in the BET model (Brunauer, Emmett, Teller). A sample of 0.0945 g of PS / DVB polymer support material was used for both analyses. The density of the sample material was 1.05 g / cc. The measurements were performed on an Autosorb iQ S / N: 14713051301 instrument with a 9 mm cell. The bath temperature was 77.35 K. The final outgassing temperature was 60 °C. The measurements were evaluated with Quantachrome ASiQwin version 3.01. Two measurements were performed, one with an absorption time of 80 min and the other with an absorption time of 40 min. The outgassing rates were 1.0 °C / min and 20.0 °C / min, respectively. The average pore radius obtained from the BJH method based on the pore volume was 5.060 nm. The specific surface area obtained from the multipoint BET plot was 815.0 m 2 / g.

[0127] Example 6 Determination of the compressive stability of the polymer support material according to step b.2 In Example 4, the modification according to the invention is carried out in PS / DVB (55% DVB in EVB). The prepared starting polymeric support material is obtained as described in Example 5. Oxidation with hydrogen peroxide and reduction with lithium aluminum hydride are carried out on the starting polymeric support material according to the results of step b.2, both as described in Example 4. The obtained particles are subjected to a compression test. For the pressure test, a column of 250x4 mm is filled with the obtained particles and water is passed through the column at increasing flow rates. Figure 11 shows the pressure flow profile measured at room temperature. The y-axis shows the system pressure in bar. The x-axis shows the flow rate in mL / min. Eight intervals of 30 seconds each were measured while the flow rate was gradually increased from 0.2 mL / min to 1.6 mL / min. As can be seen, the pressure is linearly dependent on the flow rate up to a pressure of 400 bar or 40 MPa.

[0128] Example 7 Measurement of average particle size The circularity and average particle size were determined for a sample of the starting polymer support material prepared in step a. The sample was sputtered in a single particle layer onto a scanning electron microscope slide. For this purpose, the sample was deposited in a single particle layer onto a scanning electron microscope slide and coated with gold using a LOT AutomaticSputterCoater MSC1 sputter coater connected to a Vacubrand RZ6 vacuum pump. A series of 27 images was acquired using a scanning electron microscope (Phenom ProX) and individual particles were identified and measured using an Olympus Imaging Solutions Scandium. The identified particles were analyzed for sphericity and circularity. All images were analyzed in a batch process using identical threshold and measurement settings. A total of 6039 particles were measured and their circularity was always ≧0.8. The measurement results are shown in FIG. 12. The y-axis shows the number of particles and the x-axis shows the diameter in μm. The smallest radius measured was 0.8 μm and the largest radius was up to 10 μm. The average diameter (median) was 4.59 μm with a relative standard deviation of 6.23%. The polydispersity index PDI (Mw / Mn) was 1.044.

[0129] Example 8 pH stability measurements The pH stability was determined on a sample of the particulate polymeric support material according to Example 5, modified according to Example 4, i.e. corresponding to the polymeric material obtained according to steps a-f. For this purpose, the sample was packed into a chromatographic column (250x4 mm) and the retention time of sulfate was determined from 10 measurements with an eluent of 6 mmol / L Na2CO3 and 1 mmol / L NaHCO3. The column was subsequently rinsed for 14 hours at 0.8 mL / min with an eluent of 6 mmol / L Na2CO3 and 1 mol / L NaOH (pH 14). Then, 10 measurements of the sulfate retention time were carried out again with an eluent of 6 mmol / L Na2CO3 and 1 mmol / L NaHCO3. The column was subsequently rinsed for 14 hours at 0.8 mL / min with an eluent consisting of 6 mmol / L Na2CO3 and 1 mol / L HNO3 (pH 0). Ten determinations of sulfate retention time were then performed again using eluents of 6 mmol / L Na2CO3 and 1 mmol / L NaHCO3. At each eluent change, a 1-h water rinse was performed to prevent precipitation. Based on the sulfate retention time and plate number, possible changes were investigated, and both parameters deviated by up to 3% from the original determinations after both basic and acidic treatments.

Claims

1. 1. A method for modifying a polymeric support material for use as a stationary phase in an analytical or preparative separation process, comprising the steps of: a. providing a polymeric support material formed at least in part from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents; b. b.

1. Oxidation of the polymeric support material, followed by b.2 Reduction or hydrolysis treatment step of the reaction product of step b.1 generating hydroxy groups on / in a polymeric support material by a process comprising: c. The product of step b.2 is at least one first functional group which reacts with a hydroxy group, and at least one second functional group which reacts with amine and / or hydroxy groups; and reacting the compound with a polyfunctional compound comprising The method includes:

2. comprising steps a, b and c, where step c is followed by step d: Step d is d.1 - reaction with polyfunctional compounds containing hydroxy groups, or - Hydrolysis, or - combinations of these introducing or generating a hydroxy group by reaction of the second functional group introduced in step c) with d.2 The product of step d.1 is at least one first functional group which reacts with a hydroxy group, and at least one second functional group which reacts with amine and / or hydroxy groups; and reacting the compound with a polyfunctional compound comprising performing several coating cycles including The method of claim 1, wherein the number of coating cycles is between 1 and 20.

3. 3. The method of claim 1 or claim 2, comprising steps a, b and c, e. Introducing ion exchange groups into the reaction product from step c or d.2 The method further comprising:

4. The polymeric support material in step a, at least in part formed from an aromatic hydrocarbon compound having at least two vinyl or allyl substituents, further comprises - ethylvinylbenzene, - vinyl acetate, - styrene, and - combinations of these formed in part from a monomer selected from the group consisting of:

4. The process according to claim 1, wherein the proportion of aromatic hydrocarbon compounds having at least two vinyl or allyl substituents is at least 50% by weight.

5. The oxidation treatment in step b.1 may be treatment with peracid, KMnO 4 5. The method according to claim 1, characterized in that the treatment is with oxygen plasma, with oxygen plasma, or a combination thereof.

6. 6. The process according to claim 1, characterized in that the polyfunctional compound used in step c) comprising at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with amine and / or hydroxy groups is an epihalohydrin.

7. 6. The method according to claim 1, wherein the polyfunctional compound used in step c) comprising at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with amine and / or hydroxy groups is a spacer molecule.

8. 3. The method of claim 2, wherein the polyfunctional compound used in step d.2, comprising at least one first functional group reactive with hydroxy groups and at least one second functional group reactive with amine and / or hydroxy groups, is an epihalohydrin or a spacer molecule.

9. 3. The method of claim 2, characterized in that the number of coating cycles is between 1 and 10.

10. 4. The method of claim 3, characterized in that the ion-exchange groups are introduced by reacting the compound of step c or d.2 with an organoelement compound of main group 5.

11. 11. The method according to claim 3 or 10, characterized in that step e is followed by a step f, which comprises heating the polymeric support material provided with ion exchange groups in an alkaline solution.

12. A modified polymeric support material for use as a stationary phase in an analytical or preparative separation process, obtainable by the method according to any one of claims 1 to 11, wherein the polymeric support material provided in step a has an average pore radius of 1 to 50 nm, measurable by nitrogen adsorption according to the BJH model.

13. A modified polymeric support material for use as a stationary phase in an analytical or preparative separation process, obtainable by the method according to any one of claims 1 to 11, A modified polymeric support material, wherein the polymeric carrier material provided in step a is hydrophobic and either microporous or mesoporous.

14. The polymeric carrier material provided in step a) - monomer units derived from aromatic hydrocarbon compounds having at least two vinyl or allyl substituents, - monomer units derived from ethylvinylbenzene, - monomer units derived from styrene, - combinations of these 14. The modified polymeric support material of claim 12 or 13, which is substantially completely composed of monomer units selected from the group consisting of:

15. The polymeric support material provided in step a) has a nitrogen adsorption viscosity of 80 to 1000 m as measured by BET model nitrogen adsorption. 2 The modified polymeric support material of claim 12 having a specific surface area of ​​100 / g.

16. 13. The modified polymeric support material of claim 12, wherein the polymeric support material provided according to step b.2 is pressure stable at pressures up to 220 bar.

17. The modified polymeric support material of claim 12 in the form of particles.

18. 13. The modified polymeric support material of claim 12, which is stable in the pH range of 0 to 14.

19. A chromatography column packed with a modified polymeric support material according to any one of claims 12 to 18.

20. 19. A method for the chromatographic separation of an analyte, characterized in that a solution containing the analyte is contacted with a modified polymeric support material according to any one of claims 12 to 18.

21. Use of the polymeric support material according to any one of claims 12 to 18 or obtainable by the method according to any one of claims 1 to 11 for the analytical or preparative separation of analytes.

Citation Information

Patent Citations

  • Production process of anion exchange membrane

    JP1977006386A

  • Chromatography for coated media

    JP1992505968A

  • Weakly acidic exchange resin for liquid chromatography

    JP1994023280A

  • Porous polymer particle, alkali-resistant anion exchanger, production method thereof, ion chromatography column, and anion measurement method

    JP2002249517A