Ethylene gas adsorbent
A porous metal complex or metal-supported inorganic porous body in a thermoplastic resin film addresses the inefficiencies of existing ethylene gas adsorption technologies by effectively removing ethylene gas, maintaining the freshness of perishable products.
Patent Information
- Application Number
- JP2020107251
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-06-22
AI Technical Summary
Existing ethylene gas adsorption technologies, such as those using zeolite-based films, do not effectively address the need to maintain freshness in perishable products by efficiently removing ethylene gas, leading to deterioration and decomposition of vegetables, fruits, and fresh flowers.
An ethylene gas adsorbent containing a porous metal complex or metal-supported inorganic porous body is used, which absorbs ethylene gas through its porous structure, characterized by specific metal ions and bridging ligands, dispersed in a thermoplastic resin film.
The ethylene gas adsorbent effectively removes ethylene gas, preventing deterioration and decomposition of fresh produce, ensuring prolonged freshness.
Smart Images

Figure 0007585631000002 
Figure 0007585631000003 
Figure 0007585631000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an ethylene gas adsorbent. [Background technology]
[0002] In the distribution process of fresh produce such as vegetables, fruits, and flowers, there is a need to maintain their freshness, and furthermore, there are requests from retailers and consumers to extend the shelf life, so there is a demand for technology to keep fresh produce fresh for a long period of time. The cause of loss of freshness is the accelerated ripening and aging caused by metabolic gases, especially ethylene gas, generated by fruits and flowers. Therefore, the biggest problem in maintaining freshness is how to suppress the generation of ethylene gas for a certain period of time or how to remove the gas generated by ethylene.
[0003] Various methods are used to maintain the freshness of fresh produce during transportation and storage. Among them, an ethylene gas adsorption film is known as one of the methods for maintaining the freshness of fresh produce such as vegetables, fruits, and flowers. The film is made by kneading an ethylene gas adsorbent made of inorganic porous particles such as zeolite into a resin component. The film is designed to suppress the maturation and aging of fresh produce by utilizing the characteristic of inorganic porous particles with many tiny pores that adsorb gas, thereby giving the film the ability to adsorb ethylene gas, which is said to be a plant aging hormone, generated as a result of the metabolic activity of fresh produce.
[0004] For example, Patent Document 1 proposes an ethylene gas adsorption sheet in which powder of zeolite, a porous material for adsorbing ethylene gas, is attached to the surface of a sheet of plastic or the like.
[0005] However, Patent Document 1 does not disclose an ethylene gas adsorption sheet using, as an ethylene gas adsorbent, a metal-supported inorganic porous body in which a metal is supported on a porous material such as zeolite, or a porous metal complex (Metal Organic Framework; MOF) in which a porous structure is formed by metal ions and organic ligands capable of bonding to the metal ions. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-337802 Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide an ethylene gas adsorbent that can remove ethylene gas and prevent deterioration, rot or spoilage of vegetables, fruits, flowers, and other items that particularly require freshness, thereby enabling them to be preserved for a long period of time. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems and have found that an ethylene gas adsorbent containing a specific ethylene gas adsorbent can achieve the above objects, thereby completing the present invention.
[0009] That is, the ethylene gas adsorbent of the present invention is characterized in that it absorbs at least ethylene gas and contains a porous metal complex or a metal-supported inorganic porous material. Effect of the Invention
[0010] According to the present invention, there is provided an ethylene gas adsorbent which removes ethylene gas and prevents deterioration, rotting or spoilage of vegetables, fruits, flowers and the like which particularly require freshness, thereby enabling them to be preserved for a long period of time. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the layer structure of a film containing the ethylene gas adsorbent of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of the layer structure of a film containing the ethylene gas absorbent of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The ethylene gas adsorbent of the present invention will be described below with reference to specific examples, but the present invention is not limited thereto.
[0013] 1 and 2 are schematic cross-sectional views showing an example of the layer structure of a film containing the ethylene gas adsorbent of the present invention. As shown in FIG. 1, a film 10 containing the ethylene gas adsorbent (hereinafter referred to as an ethylene gas adsorption film) is formed by mixing and dispersing the ethylene gas adsorbent in a thermoplastic resin 2 that is a film-forming material.
[0014] Moreover, a modified example of the ethylene gas adsorption film 10 is configured such that an ethylene gas adsorbent 1 that absorbs ethylene gas is attached to the surface of a base layer 4 via a binder layer 3, as shown in FIG.
[0015] Next, the ethylene gas adsorbent 1 contained in the ethylene gas adsorption film of the present invention adsorbs at least ethylene gas generated from fresh produce such as vegetables, fruits, and flowers.
[0016] The ethylene gas adsorbent preferably contains a porous metal complex or a metal-supported inorganic porous material.
[0017] The porous metal complex is a porous material composed of metal ions and a compound having a bridging ligand, and therefore has pores that can accommodate ethylene gas.
[0018] The size of the pores in the porous metal complex in this embodiment is not particularly limited, but is preferably, for example, 0.1 nm to 10 nm.
[0019] As the constituent metal ions, for example, ions of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, etc. are preferred, and from the viewpoint of ethylene gas adsorptivity and environmental aspects, copper and zinc are more preferred.
[0020] On the other hand, examples of the bridging ligand include 2-methylimidazole, terephthalic acid, trimesic acid, 1,4-naphthalenedicarboxylic acid, and compounds having functional groups such as amino groups, sulfonic acid groups, and hydroxyl groups attached thereto.
[0021] Specific examples of the porous metal complex that can be used include a porous metal complex composed of zinc ions and 2-methylimidazole (Basolite (registered trademark) Z1200 manufactured by BASF), a porous metal complex composed of aluminum ions and terephthalic acid (Basolite (registered trademark) A100 manufactured by BASF), a porous metal complex composed of copper ions and trimesic acid (Basolite (registered trademark) C300 manufactured by BASF), and a porous metal complex composed of iron ions and trimesic acid (Basolite (registered trademark) F300 manufactured by BASF).
[0022] The metal-supported inorganic porous body is an inorganic porous body that supports a metal element in the state of metal, metal ion, or metal oxide. The metal component in the metal-supported inorganic porous body is ionized, and can exhibit a catalytic effect that promotes the adsorption reaction of ethylene gas.
[0023] The metal species to be supported is preferably one or more selected from the group consisting of copper, zinc, silver, platinum, iron and cobalt, and from the viewpoints of ethylene gas adsorption and the environment, copper and zinc are more preferred.
[0024] The inorganic porous body is a porous material having a large number of micropores on its surface and carrying a metal compound on the surface, and it is preferable that the metal compound is supported in a dispersed state on the surface without blocking the micropores.
[0025] Here, the inorganic porous material refers to a substrate having a large number of micropores on the surface, and examples of the inorganic porous material that can be used include zeolite, silicon dioxide, silicates, activated carbon, titania, inorganic phosphates such as calcium phosphate, alumina, aluminum hydroxide, magnesium hydroxide, etc. At least one of these may be used in combination.
[0026] As such a porous material, it is particularly preferable to use aluminum hydroxide, zeolite, or silicate from the viewpoint of safety and of having a porous state with pores of an effective size relative to the molecular size of ethylene gas.
[0027] The external shape of the inorganic porous material may be any shape, such as a sphere, a rod, an ellipse, or the like, and may be in any form, such as a powder, a lump, or a particle. From the viewpoints of the above-mentioned film-forming properties, uniform dispersion, kneading properties, and the like, after the metal compound is supported to form a metal-supported inorganic porous material, the powder form is preferred.
[0028] The inorganic porous body can be appropriately selected from those with any average particle size depending on the application, but in order to achieve the above average particle size of the metal-supported inorganic porous body, the average particle size is preferably 1 μm to 100 μm, more preferably 5 μm to 50 μm. If the average particle size is smaller than the above range, the metal-supported inorganic porous body is likely to aggregate and the dispersibility tends to decrease. On the other hand, if the average particle size is larger than the above range, the film-forming property is poor, so it tends to be difficult to contain a large amount of the metal-supported inorganic porous body, and there is a risk that a sufficient ethylene gas adsorption effect cannot be obtained. Here, the average particle size is a value measured by a dynamic light scattering method.
[0029] As a specific example of a metal-supported inorganic porous material, for example, a copper oxide or zinc oxide-supported inorganic porous material (Dashlight (registered trademark) CZU manufactured by Sinanen Zeomic Co., Ltd.) can be used.
[0030] The thermoplastic resin 2 contained in the ethylene gas adsorption film preferably contains a polyolefin resin, taking into consideration the dispersibility and heat sealability of the ethylene gas adsorbent, and further, mixing with other heat sealable resins.
[0031] Specific examples of polyolefin resins include low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylic acid copolymer, ethylene-propylene copolymer, and mixtures of these resins.
[0032] Among the above polyolefin-based resins, polyethylene-based resins are preferred, and among the polyethylene-based resins, LDPE, LLDPE, general-purpose PE, PE-based copolymers, and the like are more preferred.
[0033] The ethylene gas adsorption film of the present embodiment can be provided with heat sealability and bag formability by further containing a heat sealable resin as necessary. The ethylene gas adsorption film can also have a support layer on one side to reinforce the rigidity of the film.
[0034] The heat-sealable resin contained in the ethylene gas adsorption film is not particularly limited as long as it can be melted and fused by heat, and examples thereof include polyolefin, olefin copolymer, copolymer of olefin and vinyl compound, copolymer of olefin and various (meth)acrylic compounds, copolymer of olefin and unsaturated carboxylic acid, ionomer resin, ternary copolymer resin of olefin, various (meth)acrylic compounds and various unsaturated carboxylic acid, polyethylene terephthalate (PET), polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more. Among the above, polyolefin and olefin copolymer are preferred from the viewpoint of heat-sealability, and olefin copolymer is more preferred.
[0035] The thickness of the ethylene gas adsorption film is preferably 30 μm or more and 150 μm or less, more preferably 30 μm or more and 100 μm or less. If the thickness of the ethylene gas adsorption film is too thin, it is difficult to increase the content of the porous metal complex or the metal-supported inorganic porous body, and the freshness preserving effect cannot be sufficiently exhibited, and the heat sealability may be insufficient. On the other hand, if the thickness is too thick, the rigidity may be too strong, and the usability as a packaging material or packaging material may be poor.
[0036] The support layer contained in the ethylene gas adsorption film is not particularly limited as long as it supplements the rigidity of the ethylene gas adsorption film. The support layer is disposed on the outer surface layer of the ethylene gas adsorption film, and is preferably non-adhesive in order to prevent blocking when the ethylene gas adsorption film is rolled or stacked. Among the above, the resin contained in the support layer is preferably, for example, LDPE or LLDPE.
[0037] The thickness of the support layer is not particularly limited, but is preferably 1 μm or more and 50 μm or less. If it is thinner than the above range, it is difficult to exert the effect of reinforcing the rigidity, and if it is thicker than the above range, the rigidity is too strong and it is likely to become difficult to use as a packaging material or packaging material. The support layer can contain a heat-sealable resin.
[0038] The base layer 4 for adhering the ethylene gas adsorbent to the base is not particularly limited as long as it is a film having rigidity, but for example, a polyolefin film, paper, polyamide film, or polyester film can be used. The thickness of the base layer 4 is not particularly limited, but is preferably 30 μm or more and 100 μm or less.
[0039] When it is desired to improve the gas barrier property of the ethylene gas adsorption film, it is preferable to use a silica-vapor-deposited film, an aluminum oxide-vapor-deposited film, or an aluminum foil, and the film can be produced by forming a silica-vapor-deposited film, an aluminum oxide-vapor-deposited film, or the like on at least one side of the above-mentioned resin film.
[0040] The ethylene gas adsorption film may further include a binder layer 3 formed on one side of the base film in order to adhere the ethylene gas adsorbent to the film. Examples of the binder layer 3 include, but are not limited to, room temperature curing, heat curing, ultraviolet curing, and electron beam curing adhesives or paints, pressure sensitive adhesives, hot melt adhesives or paints, etc.
[0041] Although there is no particular limitation on the thickness of the binder layer 3, it is preferably 1 μm or more and 10 μm or less. If it is thinner than the above range, it is difficult to support the ethylene gas adsorbent on the film, and if it is thicker than the above range, the adhesiveness is not improved.
[0042] Of the binder layer 3, the resin constituting the adhesive layer is preferably, for example, a grade having adhesive properties such as polyolefin-based resin, EVA, NBR rubber, SBR rubber, etc., more preferably a grade having adhesive properties of polyolefin-based resin, and even more preferably a grade having adhesive properties of linear low-density polyethylene.
[0043] The above-mentioned adhesive linear low-density polyethylene has a density of 0.88 g / cm 3 More than 0.915g / cm 3It is preferable that the density is less than the above range. If the density is less than the above range, the adhesiveness is too strong or the softening point is too low, making it difficult to maintain the layer structure. If the density is more than the above range, it is difficult to exhibit sufficient adhesiveness.
[0044] The ethylene gas adsorption film may be prepared by laminating previously prepared layers via an adhesive layer, by laminating a molten resin composition onto a previously prepared layer by extrusion, by simultaneously preparing a plurality of layers and laminating them by melt compression bonding, or by coating one or more resins onto another layer by applying and drying the resin.
[0045] In order to improve the adhesion between the layers constituting the ethylene gas adsorption film, the surfaces of the layers may be subjected to a desired surface treatment in advance, if necessary. For example, a corona-treated layer, an ozone-treated layer, a plasma-treated layer, an oxidation-treated layer, etc. can be formed by optionally carrying out pretreatment such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas or nitrogen gas, etc., glow discharge treatment, oxidation treatment using chemicals, etc. Furthermore, various coating layers such as a primer coating layer, an undercoat coating layer, an anchor coating layer, an adhesive layer, a vapor-deposited anchor coating layer, etc. can also be formed on the surface of each layer to form a surface treatment layer.
[0046] The ethylene gas adsorption film may contain various modifying resins, plastic compounding agents, additives, etc., for the purpose of improving or modifying the processability, heat resistance, weather resistance, mechanical properties, dimensional stability, antioxidant properties, slipperiness, release properties, flame retardancy, antifungal properties, electrical properties, strength, etc., of the odor adsorbing laminate. In this case, these additives may be optionally contained in the base layer in an amount ranging from a trace amount to several tens of mass % depending on the purpose. In this embodiment, general additives may be optionally contained, such as lubricants, crosslinking agents, antioxidants, ultraviolet absorbents, light stabilizers, fillers, antistatic agents, lubricants, antiblocking agents, colorants such as dyes and pigments, etc.
[0047] Next, a method for producing a film containing an ethylene gas adsorbent will be described.
[0048] Next, the ethylene gas adsorption film is not particularly limited, but for example, it can be produced by evenly scattering and adhering ethylene gas adsorbent powder onto the surface of the base layer 4, the surface of which is coated with an adhesive.
[0049] When the base layer 4 is a thermoplastic base, the powder of the ethylene gas adsorbent may be sprinkled on the base layer 4 immediately after the resin that forms the film is extruded, or may be sprinkled on the base layer 4 after it is first molded and then heated again. After that, the base layer 4 may be left as it is, or may be heated by thermocompression or in a hot air oven, etc., as necessary.
[0050] Next, a modified example of the method for producing the ethylene gas adsorption film of this embodiment will be described. For example, the ethylene gas adsorbent may be directly mixed with other components of the ethylene gas adsorption film and melt-kneaded, but the ethylene gas adsorbent may be mixed with a thermoplastic resin at a high concentration and then melt-kneaded to prepare a master batch, which is then mixed with other components of the ethylene gas adsorption film in a ratio corresponding to the target content and melt-kneaded to produce an ethylene gas adsorption film of the ethylene gas adsorbent by a so-called master batch method. By adopting the master batch method, even when an ethylene gas adsorbent that is prone to aggregation is used, the ethylene gas adsorbent can be efficiently and uniformly dispersed in the ethylene gas adsorption film.
[0051] The content of the ethylene gas adsorbent in the master batch is preferably 5% by mass to 50% by mass, and more preferably 7% by mass to 40% by mass. A content within this range facilitates melt-kneading with the ethylene gas adsorbent, facilitates dispersion of the ethylene gas adsorbent in the ethylene gas adsorption film, and enables the ethylene gas adsorbent to be sufficiently supported on the ethylene gas adsorption film.
[0052] The ethylene gas adsorption film can be produced by a conventional film-forming method such as (co)extrusion, cast molding, T-die method, cutting method, or inflation method.
[0053] Each layer of the ethylene gas adsorption film may be unstretched, but may also be stretched uniaxially or biaxially by, for example, a tenter system or a tubular system to improve strength, dimensional stability, and heat resistance.
[0054] A method for producing a packaging bag using the ethylene gas adsorption film of this embodiment will be described below.
[0055] First, the ethylene gas adsorbing film is folded or two sheets are overlapped so that the sealant layers containing the ethylene gas adsorbent face each other, and the peripheral edges are heat sealed to prepare the sealant film.
[0056] Examples of the shape of the packaging bag include side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, palm seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, and gusset type.
[0057] As the heat sealing method, for example, known methods such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc. can be used.
[0058] The ethylene gas adsorbent and ethylene gas adsorption film of the present invention can be applied not only to food packaging but also to all packaging objects which require ethylene gas absorption ability. EXAMPLES
[0059] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0060] [Ethylene gas adsorbent (test specimen)] Metal-supported inorganic porous material 1: Sinanen Zeomic Co., Ltd., Dashlight CZU, CuO, ZnO-supported zeolite Metal-supported inorganic porous material 2: Zeomic Ag10D, silver-supported zeolite, manufactured by Sinanen Zeomic Co., Ltd. Metal-supported inorganic porous material 3: Zeomic 4Ag1MH, manufactured by Sinanen Zeomic Co., Ltd., silver-supported zeolite Porous metal complex 1: BASF's Basolite C300, a porous metal complex composed of copper ions and trimesic acid Inorganic porous material 1: Mizusawa Chemical Industry Co., Ltd., Mizuka Sieves Y-420, hydrophobic zeolite, SiO2 / Al2O3 molar ratio = 3.8 / 1 Inorganic porous material 2: Mizusawa Chemical Industry Co., Ltd., Silton MT-100, hydrophobic zeolite, SiO2 / Al2O3 molar ratio = 100 / 1 Inorganic porous material 3: Mizusawa Chemical Industry Co., Ltd., Silton MT-400, hydrophobic zeolite, SiO2 / Al2O3 molar ratio = 400 / 1 Inorganic porous material 4: Shilton MT-2000, manufactured by Mizusawa Chemical Industry Co., Ltd., SiO2 / Al2O3 molar ratio = 2000 / 1
[0061] Example 1 1.0 g of powder of metal-supported inorganic porous material 1 (average particle size: 3 μm to 5 μm) was used. Example 2 1.0 g of powder of metal-supported inorganic porous material 2 (average particle size: 3 μm to 5 μm) was used. Example 3 1.0 g of powder (average particle size: 3 μm to 5 μm) of metal-supported inorganic porous material 3 was used. Example 4 1.0 g of powder of porous metal complex 1 (average particle size: 1 μm to 10 μm) was used. Comparative Example 1 No test specimen was used. Comparative Example 2 1.0 g of inorganic porous material 1 powder (average particle size: 5 μm) was used. Comparative Example 3 1.0 g of powder of inorganic porous body 2 (average particle size: 3 μm to 4.5 μm) was used. Comparative Example 4 1.0 g of powder of inorganic porous material 3 (average particle size: 5 μm to 7 μm) was used. Comparative Example 5 1.0 g of powder of inorganic porous material 4 (average particle size: 2 μm to 4 μm) was used.
[0062] [Ethylene gas adsorption test] The powder of each test specimen was placed in a gas sampling bag (GL Sciences, SMART BAG PA AKK-10, pouch 100mm x 160mm), which was then filled with 160ml of ethylene gas at 50ppm and sealed. The bag was then left to stand for 5 days in a room temperature environment filled with ethylene gas until it reached a saturated state. The concentration of the ethylene gas component was then measured. The measurement results are shown in Table 1.
[0063] [Table 1]
[0064] As shown in Table 1, it was found that the residual ethylene gas concentration was reduced and the ethylene gas removal performance was high in Examples 1 and 2. In contrast, the residual ethylene gas concentration was hardly reduced in Comparative Examples 1 to 5, and the ethylene gas removal performance was low.
[0065] 1. Ethylene gas adsorbent 2 Thermoplastic resin 3. Binder Layer 4 Base material layer 10 Ethylene gas adsorption film
Claims
1. An ethylene gas adsorbent that absorbs at least ethylene gas, The ethylene gas adsorbent includes a metal-supported inorganic porous material, The ethylene gas adsorbent is characterized in that the metal contains copper oxide and zinc oxide.
2. A film comprising the ethylene gas adsorbent of claim 1.
Citation Information
Patent Citations
Preparation of adsorbent for unsaturated hydrocarbon
JP1985147239A
Freshness retaining agent for packaging material
JP1989047337A
Ethylene adsorbent and method for keeping freshness of plant
JP1990052040A
Agent and method for retaining freshness of fruit, vegetable, flower or tree
JP1992211326A
Adsorbent of hydrocarbon in exhaust gas from internal combustion engine
JP1995096178A