Rubber composition for tires and tires
The rubber composition for tires, with specific styrene-butadiene rubber and carbon black formulations, enhances fuel efficiency and chipping resistance by optimizing interaction and dispersion, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2020148982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-04
AI Technical Summary
Existing rubber compositions for tires do not adequately address the need for improved fuel efficiency and chipping resistance.
A rubber composition containing styrene-butadiene rubber and carbon black, with specific ranges for styrene content, carbon black surface area, and carbon black content, along with optional additives like silica and dibenzylamine compounds, to enhance interaction and dispersion, thereby improving reinforcing properties.
The composition achieves better fuel efficiency and chipping resistance by promoting carbon black dispersion and reinforcing properties, resulting in improved overall tire performance.
Smart Images

Figure 0007585669000001 
Figure 0007585669000002 
Figure 0007585669000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]
[0002] Conventionally, various methods for improving fuel economy and chipping resistance have been investigated (for example, see Patent Documents 1 and 2). However, in recent years, further improvements in these overall performances have been required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-344955 A [Patent Document 2] JP 2014-012768 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition for tires and a tire that can solve the above problems and improve the overall performance of fuel economy and chipping resistance. [Means for solving the problem]
[0005] The present invention relates to a rubber composition comprising a rubber component containing styrene-butadiene rubber and carbon black, the total styrene content of the rubber component being 15 mass% or less, and the average cetyltrimethylammonium bromide specific surface area of the carbon black being 120 m 2 / g or more, and the cetyltrimethylammonium bromide specific surface area in 100% by mass of the carbon black is 115 m 2 / g or less is 50 mass % or more, and the amount of the carbon black per 100 mass parts of the rubber component is 20 mass parts or more.
[0006] It is preferable that the rubber component contains an isoprene-based rubber, and the content of the isoprene-based rubber is greater than the content of the styrene-butadiene rubber.
[0007] The total amount of styrene in the rubber component is preferably 10% by mass or less.
[0008] The rubber composition preferably contains silica.
[0009] The rubber composition preferably contains a styrene-based resin.
[0010] The rubber composition preferably contains a dibenzylamine compound.
[0011] The present invention also relates to a tire using the rubber composition. Effect of the Invention
[0012] The present invention relates to a rubber composition comprising a rubber component containing styrene-butadiene rubber and carbon black, the total styrene content of the rubber component being 15 mass% or less, and the average cetyltrimethylammonium bromide specific surface area of the carbon black being 120 m 2 / g or more, and the cetyltrimethylammonium bromide specific surface area in 100% by mass of the carbon black is 115 m 2 / g or less is 50 mass % or more, and the content of the carbon black per 100 mass parts of the rubber component is 20 mass parts or more, so that the overall performance of fuel economy and chipping resistance is good. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The rubber composition for tires of the present invention contains a rubber component containing styrene-butadiene rubber and carbon black, the total styrene content in the rubber component is 15 mass% or less, and the average cetyltrimethylammonium bromide specific surface area of the carbon black is 120 m 2 / g or more, and the cetyltrimethylammonium bromide specific surface area in 100% by mass of the carbon black is 115 m 2 / g or less is 50 mass % or more, and the amount of the carbon black per 100 mass parts of the rubber component is 20 mass parts or more.
[0014] The reason why the above-mentioned effects are obtained with the above-mentioned rubber composition is presumed to be as follows. In the above rubber composition, styrene-butadiene rubber and carbon black are blended, and the total amount of styrene in the rubber component and the amount of carbon black are adjusted to fall within a predetermined range, so that the carbon black is less susceptible to the steric hindrance caused by the styrene moiety, which facilitates the generation of an interaction between the rubber component and the carbon black, and promotes the dispersion of the carbon black. In addition, the average CTAB specific surface area of carbon black and the CTAB specific surface area of 115 m 2 By adjusting the ratio of those having a molecular weight of 1000 to 10000 / g or less to fall within a predetermined range, the dispersion of the carbon black is further promoted. It is believed that these actions facilitate the provision of reinforcing properties by carbon black, thereby significantly improving the overall performance of fuel economy and chipping resistance.
[0015] The rubber composition contains a rubber component. Here, the rubber component is a component that contributes to crosslinking, and generally has a weight average molecular weight (Mw) of 10,000 or more.
[0016] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.
[0017] In this specification, the weight average molecular weight (Mw) can be determined by converting it into standard polystyrene based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0018] The total amount of styrene in the rubber component may be 15% by mass or less, but is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, and is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more. Within the above ranges, the effect tends to be better obtained.
[0019] Here, the total amount of styrene in the rubber component is the total content of styrene parts contained in the total amount of rubber component (unit: mass%), and can be calculated by Σ(content of each rubber component × amount of styrene in each rubber component / 100). For example, in a case where 100% by mass of rubber component contains 85% by mass of SBR with styrene content: 40% by mass, 5% by mass of SBR with styrene content: 25% by mass, and 10% by mass of BR with styrene content: 0% by mass, the total amount of styrene in the rubber component is 35.25% by mass (=85×40 / 100+5×25 / 100+10×0 / 100).
[0020] The total vinyl content in the rubber component is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, and is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 12% by mass or more. Within the above ranges, the effect tends to be better obtained.
[0021] Here, the total vinyl content in the rubber component is the total content of vinyl parts contained in the entire rubber component (unit: mass%) and can be calculated by Σ (content of each rubber component × vinyl content in each rubber component / 100). For example, in a 100% rubber component, when the rubber component contains 85% by mass of SBR with a vinyl content of 30% by mass, 5% by mass of SBR with a vinyl content of 20% by mass, and 10% by mass of BR with a vinyl content of 10% by mass, the total vinyl content in the rubber component is 27.5% by mass (=85×30 / 100+5×20 / 100+10×10 / 100).
[0022] The ratio of the total vinyl content in the rubber component to the total styrene content in the rubber component is preferably 0.5 or more, more preferably 2 or more, even more preferably 3 or more, and particularly preferably 4 or more, and is preferably 8 or less, more preferably 6 or less, and even more preferably 5 or less. Within the above ranges, the effect tends to be better obtained.
[0023] The styrene amount and vinyl amount in each rubber component can be measured by a nuclear magnetic resonance (NMR) method. In addition, in the examples of this specification, the total styrene amount and the total vinyl amount in the rubber component are calculated according to the above-mentioned formula, but they may also be analyzed from the tire using, for example, a pyrolysis gas chromatograph mass spectrometer (Py-GC / MS) or the like.
[0024] The rubber composition contains styrene-butadiene rubber (SBR) as a rubber component. The SBR is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. Commercially available products include those from Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc.
[0025] The styrene content of the SBR is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, and is preferably 35% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0026] The vinyl content of the SBR is preferably 15% by mass or more, more preferably 25% by mass or more, and even more preferably 35% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0027] The above-mentioned styrene amount and vinyl amount of SBR mean the styrene amount and vinyl amount of the SBR when there is one type of SBR, and mean the average styrene amount and average vinyl amount when there are multiple types of SBR. The average styrene amount of SBR can be calculated by {Σ(content of each SBR × styrene amount of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a styrene amount of 40% by mass and 5% by mass of SBR with a styrene amount of 25% by mass, the average styrene amount of the SBR is 39.2% by mass (=(85×40+5×25) / (85+5)). Similarly, the average vinyl content of SBR can be calculated by {Σ(content of each SBR × vinyl content of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a vinyl content of 30% by mass and 5% by mass of SBR with a vinyl content of 20% by mass, the average vinyl content of the SBR is 29.4% by mass (=(85×30+5×20) / (85+5)).
[0028] In 100% by mass of the rubber component, the content of SBR is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0029] Examples of rubber components that can be used other than SBR include diene rubbers such as isoprene rubber, butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene-isoprene-butadiene copolymer rubber (SIBR). These may be used alone or in combination of two or more. Among these, isoprene rubber and BR are preferred.
[0030] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubbers that are common in the tire industry. Examples of IR include IR2200 and other rubbers that are common in the tire industry. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more. Among these, NR is preferred.
[0031] In 100% by mass of the rubber component, the content of the isoprene-based rubber is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, and is preferably 75% by mass or less, more preferably 65% by mass or less, and even more preferably 55% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0032] From the viewpoint of overall performance such as fuel economy and chipping resistance, it is preferable that the content of the isoprene-based rubber in the rubber composition is greater than the content of the SBR.
[0033] In the rubber composition, the ratio of the isoprene rubber content to the SBR content is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 1.8 or more, and is preferably 3.5 or less, more preferably 2.5 or less, and even more preferably 2.2 or less. Within the above ranges, the effect tends to be better obtained.
[0034] In these relationships, the content of isoprene-based rubber and the content of SBR are the contents in 100% by mass of the rubber component (unit: mass %).
[0035] The BR is not particularly limited, and can be high cis content BR, low cis content BR, BR containing syndiotactic polybutadiene crystals, etc. Commercially available products include those from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc.
[0036] The cis amount (cis content) of BR is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, and is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less. Within the above ranges, the effect tends to be better obtained. The cis content of BR can be measured by infrared absorption spectroscopy.
[0037] The above-mentioned cis amount of BR means the cis amount of the BR when there is one type of BR, and means the average cis amount when there are multiple types of BR. The average cis content of BR can be calculated by {Σ(content of each BR × cis content of each BR)} / total content of all BRs. For example, when 100% by mass of the rubber component contains 20% by mass of BR with a cis content of 90% by mass and 10% by mass of BR with a cis content of 40% by mass, the average cis content of BR is 73.3% by mass (=(20×90+10×40) / (20+10)).
[0038] In 100% by mass of the rubber component, the content of BR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0039] The rubber component may be modified to introduce a functional group that interacts with a filler such as silica. Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0040] Specific examples of compounds (modifiers) having the above-mentioned functional groups include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and the like.
[0041] The rubber composition contains carbon black. Carbon black is cetyltrimethylammonium bromide (CTAB) with an average specific surface area of 120m 2 / g or more, and the CTAB specific surface area is 115 m per 100 mass% of carbon black. 2 The ratio of carbon black having a particle size distribution of 0.1 to 1.0 μm / g or less is 50% by mass or more, but the method for satisfying this condition is not particularly limited, and for example, the particle size distribution during the production of carbon black may be adjusted, or two or more types of carbon black may be used in combination. Examples of carbon black that can be used in combination of two or more types include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shinnikka Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. The CTAB specific surface area of carbon black is a value measured in accordance with JIS K6217-3:2001.
[0042] The average CTAB specific surface area of carbon black is 120m 2 / g or more, but preferably 160m 2 / g or less, more preferably 140m 2 / g or less, more preferably 130m 2 Within the above range, there is a tendency for the effect to be better obtained. Here, the average value of the CTAB specific surface area of carbon black can be calculated by {Σ(content of each carbon black × CTAB specific surface area of each carbon black)} / total content of all carbon blacks. For example, when the rubber component is 100 parts by mass, the average value of the CTAB specific surface area of carbon black is 110 m. 2 / g of carbon black: 30 parts by mass, CTAB: 140m 2 When the amount of carbon black is 20 parts by mass / g, the average value of the CTAB specific surface area is 122 m 2 / g(=(30×110+20×140) / (30+20)).
[0043] As an example of a method to satisfy the above-mentioned carbon black conditions, a CTAB specific surface area of 115 m 2 / g or less (hereinafter referred to as first carbon black) and CTAB specific surface area of 125m 2 A method of using carbon black having a molecular weight of 1 / g or more (hereinafter also referred to as second carbon black) in combination with the carbon black having a molecular weight of 1 / g or more (hereinafter also referred to as second carbon black) is also exemplified.
[0044] The CTAB specific surface area of Daiichi Carbon Black is 115m 2 / g or less, but preferably 50m 2 / g or more, more preferably 70m 2 / g or more, more preferably 90m 2 Within the above range, there is a tendency for the effect to be better obtained.
[0045] The CTAB specific surface area of the secondary carbon black is 125m 2 / g or more, but preferably 130m 2 / g or more, and preferably 180m 2 / g or less, more preferably 170m 2 / g or less, more preferably 160m 2 Within the above range, there is a tendency for the effect to be better obtained.
[0046] In 100% by mass of carbon black, the content of the first carbon black may be 50% by mass or more, preferably 55% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less. When it is within the above range, the effect tends to be better obtained.
[0047] In 100% by mass of carbon black, the content of the second carbon black is preferably 20% by mass or more, preferably 30% by mass or more, preferably 40% by mass or more, and preferably 50% by mass or less, more preferably 45% by mass or less. Within the above range, the effect tends to be better obtained.
[0048] The carbon black content (total content) is not less than 20 parts by mass per 100 parts by mass of the rubber component, but is preferably not more than 55 parts by mass, more preferably not more than 40 parts by mass, and further preferably not more than 30 parts by mass. Within the above range, the effect tends to be better obtained.
[0049] The rubber composition preferably contains silica. Examples of silica include dry silica (silicic anhydride) and wet silica (silicic acid hydrate), but wet silica is preferred because it has a large number of silanol groups. Commercially available products include those from Rhodia, EVONIK, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.
[0050] The content of silica is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0051] Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl, mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Toray Dow Corning Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, mercapto-based products are preferred.
[0052] As the mercapto-based silane coupling agent, in addition to a compound having a mercapto group, a compound having a structure in which the mercapto group is protected by a protecting group (for example, a compound represented by the following formula (S1)) can also be used.
[0053] Particularly suitable mercapto-based silane coupling agents include silane coupling agents represented by the following formula (S1) and silane coupling agents containing a bond unit A represented by the following formula (I) and a bond unit B represented by the following formula (II). [ka] (In the formula, R 1001 -Cl, -Br, -OR 1006 , -O(O=)CR 1006 , -ON=CR 1006 R 1007 , -NR 1006 R 1007 and-(OSiR 1006 R 1007 ) h (OSiR 1006 R 1007 R 1008 ) a monovalent group (R 1006 , R 1007 and R 1008 may be the same or different, each is a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms, and h has an average value of 1 to 4; 1002 is R 1001 , a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms, R 1003 is -[O(R 1009 O) j ]-group(R 1009 is an alkylene group having 1 to 18 carbon atoms, and j is an integer of 1 to 4. 1004 is a divalent hydrocarbon group having 1 to 18 carbon atoms, R 1005 represents a monovalent hydrocarbon group having 1 to 18 carbon atoms, and x, y, and z are numbers that satisfy the relationship: x+y+2z=3, 0≦x≦3, 0≦y≦2, 0≦z≦1. [ka] [ka] (In the formula, v is an integer of 0 or more, and w is an integer of 1 or more. R 11 R represents hydrogen, halogen, a branched or unbranched alkyl group having 1 to 30 carbon atoms, a branched or unbranched alkenyl group having 2 to 30 carbon atoms, a branched or unbranched alkynyl group having 2 to 30 carbon atoms, or an alkyl group in which the terminal hydrogen atom has been substituted with a hydroxyl group or a carboxyl group. 12 R represents a branched or unbranched alkylene group having 1 to 30 carbon atoms, a branched or unbranched alkenylene group having 2 to 30 carbon atoms, or a branched or unbranched alkynylene group having 2 to 30 carbon atoms. 11 and R 12 may form a ring structure.)
[0054] In formula (S1), R 1005 , R 1006 , R 1007 and R 1008 are each preferably independently selected from the group consisting of a linear, cyclic or branched alkyl group, an alkenyl group, an aryl group and an aralkyl group having 1 to 18 carbon atoms. 1002 When R is a monovalent hydrocarbon group having 1 to 18 carbon atoms, it is preferably a group selected from the group consisting of linear, cyclic or branched alkyl groups, alkenyl groups, aryl groups and aralkyl groups. 1009 R is preferably a linear, cyclic or branched alkylene group, and particularly preferably a linear one. 1004 Examples of R include an alkylene group having 1 to 18 carbon atoms, an alkenylene group having 2 to 18 carbon atoms, a cycloalkylene group having 5 to 18 carbon atoms, a cycloalkylalkylene group having 6 to 18 carbon atoms, an arylene group having 6 to 18 carbon atoms, and an aralkylene group having 7 to 18 carbon atoms. The alkylene group and the alkenylene group may be either linear or branched, and the cycloalkylene group, the cycloalkylalkylene group, the arylene group, and the aralkylene group may have a functional group such as a lower alkyl group on the ring. This R 1004As the alkylene group, an alkylene group having 1 to 6 carbon atoms is preferable, and a linear alkylene group such as a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, or a hexamethylene group is particularly preferable.
[0055] R in formula (S1) 1002 , R 1005 , R 1006 , R 1007 and R 1008 Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, a cyclopentyl group, a cyclohexyl group, a vinyl group, a propenyl group, an allyl group, a hexenyl group, an octenyl group, a cyclopentenyl group, a cyclohexenyl group, a phenyl group, a tolyl group, a xylyl group, a naphthyl group, a benzyl group, a phenethyl group, and a naphthylmethyl group. R in formula (S1) 1009 Examples of the linear alkylene group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and a hexylene group, and examples of the branched alkylene group include an isopropylene group, an isobutylene group, and a 2-methylpropylene group.
[0056] Specific examples of the silane coupling agent represented by formula (S1) include 3-hexanoylthiopropyl triethoxysilane, 3-octanoylthiopropyl triethoxysilane, 3-decanoylthiopropyl triethoxysilane, 3-lauroylthiopropyl triethoxysilane, 2-hexanoylthioethyl triethoxysilane, 2-octanoylthioethyl triethoxysilane, 2-decanoylthioethyl triethoxysilane, 2-lauroylthioethyl triethoxysilane, 3-hexanoylthiopropyl trimethoxysilane, 3-octanoylthiopropyl trimethoxysilane, 3-decanoylthiopropyl trimethoxysilane, 3-lauroylthiopropyl trimethoxysilane, 2-hexanoylthioethyl trimethoxysilane, 2-octanoylthioethyl trimethoxysilane, 2-decanoylthioethyl trimethoxysilane, and 2-lauroylthioethyl trimethoxysilane. These may be used alone or in combination of two or more kinds. Among them, 3-octanoylthiopropyltriethoxysilane is particularly preferable.
[0057] In the silane coupling agent containing the bond unit A represented by formula (I) and the bond unit B represented by formula (II), the content of the bond unit A is preferably 30 mol% or more, more preferably 50 mol% or more, and preferably 99 mol% or less, more preferably 90 mol% or less. The content of the bond unit B is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 10 mol% or more, and preferably 70 mol% or less, more preferably 65 mol% or less, even more preferably 55 mol% or less. The total content of the bond units A and B is preferably 95 mol% or more, more preferably 98 mol% or more, and particularly preferably 100 mol%. The content of the bond units A and B includes the case where the bond units A and B are located at the terminals of the silane coupling agent. When the bond units A and B are located at the terminals of the silane coupling agent, the form is not particularly limited, and it is sufficient that they form units corresponding to the formulas (I) and (II) representing the bond units A and B.
[0058] R in formula (I) and (II)11 With respect to the above, examples of halogen include chlorine, bromine, and fluorine. Examples of branched or unbranched alkyl groups having 1 to 30 carbon atoms include methyl and ethyl groups. Examples of branched or unbranched alkenyl groups having 2 to 30 carbon atoms include vinyl and 1-propenyl groups. Examples of branched or unbranched alkynyl groups having 2 to 30 carbon atoms include ethynyl and propynyl groups.
[0059] R in formula (I) and (II) 12 Regarding the above, examples of the branched or unbranched alkylene group having 1 to 30 carbon atoms include an ethylene group, a propylene group, etc. Examples of the branched or unbranched alkenylene group having 2 to 30 carbon atoms include a vinylene group, a 1-propenylene group, etc. Examples of the branched or unbranched alkynylene group having 2 to 30 carbon atoms include an ethynylene group, a propynylene group, etc.
[0060] In a silane coupling agent containing a bonding unit A represented by formula (I) and a bonding unit B represented by formula (II), the total number of repetitions (v+w) of the bonding unit A and the bonding unit B is preferably in the range of 3 to 300.
[0061] The content of silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, even more preferably 8 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, based on 100 parts by mass of silica.When it is within the above range, the effect tends to be better obtained.
[0062] The rubber composition preferably contains a resin. The resin is not particularly limited, but a styrene-based resin can be preferably used. The styrene-based resin is a polymer containing a styrene-based monomer as a constituent monomer, and examples thereof include a homopolymer obtained by polymerizing one type of styrene-based monomer alone, a copolymer obtained by copolymerizing two or more types of styrene-based monomers, and a copolymer of a styrene-based monomer and another monomer that can be copolymerized therewith.
[0063] Examples of styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, and p-chlorostyrene. These may be used alone or in combination of two or more. Among them, styrene and α-methylstyrene are preferred.
[0064] Examples of other monomers include terpene compounds (terpene monomers) such as α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol, and non-conjugated olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. These may be used alone or in combination of two or more.
[0065] From the viewpoint of overall performance such as fuel economy and chipping resistance, the styrene-based resin that can be suitably used is a copolymer of a terpene compound and styrene, or a copolymer of styrene and ethylene.
[0066] Examples of commercially available resins that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JX Nippon Oil & Energy Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0067] The amount of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0068] In the rubber composition, the resin content / carbon black content is preferably 0.1 or more, more preferably 0.2 or more, and is preferably 0.8 or less, more preferably 0.6 or less, and even more preferably 0.4 or less. Within the above ranges, the effect tends to be better obtained. In this regard, the resin content and the carbon black content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0069] In the rubber composition, the resin content / silica content is preferably 0.1 or more, and is preferably 0.6 or less, more preferably 0.4 or less, and further preferably 0.3 or less. Within the above range, the effect tends to be better obtained. In this relationship, the resin content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0070] The rubber composition preferably contains a dibenzylamine compound. The dibenzylamine compound is a compound having at least one group (dibenzylamine group) represented by the following formula. [ka]
[0071] Specific examples of the dibenzylamine compound include dibenzylamine, tetrabenzylthiuram disulfide (TBzTD), zinc dibenzyldithiocarbamate, 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane, etc. Commercially available products include those from Sanshin Chemical Industry Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., LANXESS, etc. These may be used alone or in combination of two or more. Among them, compounds having two dibenzylamine groups are preferred, and 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane is more preferred.
[0072] The content of the dibenzylamine compound is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 2 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0073] The rubber composition may contain a processing aid. Examples of processing aids include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, fatty acid esters, mixtures of fatty acid metal salts and amide esters, mixtures of fatty acid metal salts and fatty acid amides, etc. Commercially available products include those from Rhein Chemie and Struktol. These may be used alone or in combination of two or more. Among these, fatty acid metal salts are preferred.
[0074] Examples of fatty acids constituting the fatty acid metal salt include saturated or unsaturated fatty acids (preferably saturated or unsaturated fatty acids having 6 to 28 carbon atoms (more preferably 10 to 25 carbon atoms, and even more preferably 14 to 20 carbon atoms)), such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, arachidic acid, behenic acid, and nervonic acid. These can be used alone or in combination of two or more. Of these, saturated fatty acids are preferred, and saturated fatty acids having 14 to 20 carbon atoms are more preferred.
[0075] Examples of metals constituting fatty acid metal salts include alkali metals such as potassium and sodium, alkaline earth metals such as magnesium, calcium and barium, zinc, nickel, molybdenum, etc. These may be used alone or in combination of two or more. Among these, zinc is preferred.
[0076] The content of the processing aid is preferably 1 part by mass or more, more preferably 1.5 parts by mass or more, and even more preferably 2 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 4 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0077] The rubber composition may contain oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., JXTG Nippon Oil & Energy Corporation, Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and the like. These may be used alone or in combination of two or more.
[0078] The content of the oil is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, and further preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0079] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.
[0080] The content of the antioxidant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 4 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better.
[0081] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0082] The amount of the wax is preferably 1 part by mass or more, more preferably 1.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0083] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.
[0084] The content of stearic acid is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0085] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0086] The amount of zinc oxide is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0087] The rubber composition may contain sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0088] The amount of sulfur is preferably 0.8 parts by mass or more, more preferably 1.2 parts by mass or more, and even more preferably 1.5 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.
[0089] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and di-2-benzothiazolyl disulfide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD) and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-oxyethylene-2-benzothiazolesulfenamide and N,N'-diisopropyl-2-benzothiazolesulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. Commercially available products include products from Sumitomo Chemical Co., Ltd. and Ouchi Shinko Chemical Co., Ltd. These may be used alone or in combination of two or more.
[0090] The content of the vulcanization accelerator is preferably 0.8 parts by mass or more, more preferably 1.2 parts by mass or more, and even more preferably 1.5 parts by mass or more, and is preferably 8 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.
[0091] In addition to the above components, the rubber composition may further contain additives commonly used in the tire industry, such as organic peroxides, fillers such as talc, alumina, clay, aluminum hydroxide, mica, etc. The content of these additives is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.
[0092] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0093] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.
[0094] The rubber composition can be used (as a rubber composition for tires) for tire components such as treads (cap treads), sidewalls, base treads, under treads, shoulders, clinches, bead apexes, breaker cushion rubbers, carcass cord covering rubbers, insulations, chafers, inner liners, and side reinforcing layers of run-flat tires. Among these, the rubber composition is particularly suitable for treads.
[0095] The tire of the present invention is produced by a conventional method using the above rubber composition. That is, the rubber composition is extruded in an unvulcanized state to match the shape of the tread, etc., and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is then heated and pressurized in a vulcanizer to obtain a tire.
[0096] The above tires (pneumatic tires, etc.) can be used for passenger car tires; truck and bus tires; motorcycle tires; high-performance tires; winter tires such as studless tires; run-flat tires with side reinforcing layers; tires with sound-absorbing material having a sound-absorbing material such as sponge in the tire cavity; tires with sealing material having a sealant inside or in the tire cavity that can seal in the event of a puncture; tires with electronic components having electronic components such as sensors and wireless tags inside or in the tire cavity, etc., and are suitable for passenger car tires.
[0097] The size of the tire is not particularly limited, and can be appropriately selected, for example, from a tire width in the range of 100 to 400 mm, an aspect ratio in the range of 25 to 85%, and a rim diameter in the range of 10 to 25 inches. Specific examples include 105 / 50R16, 115 / 50R17, 125 / 55R20, 135 / 45R21, 145 / 45R21, 155 / 45R18, 165 / 45R22, 175 / 45R23, 185 / 60R20, 195 / 55R14, 205 / 40R16, 215 / 40R16, 225 / 40R17, 235 / 40R17, 245 / 40R16, 255 / 40R17, 265 / 40R17, 275 / 35R18, 285 / 30R19, and 295 / 45R20.
[0098] It is preferable that the tire outer diameter Dt and the tire section width Wt of the tire satisfy the following relational expression.
number
[0099] Specific examples of tires that can satisfy the above formula include 145 / 60R18, 145 / 60R19, 155 / 55R18, 155 / 55R19, 155 / 70R17, 155 / 70R19, 165 / 55R20, 165 / 55R21, 165 / 60R19, 165 / 65R19, 165 / 70R18, 175 / 55R19, 175 / 55R20, 175 / 55R22, 175 / 60R18, 185 / 55R19, 185 / 60R20, 195 / 50R20, 195 / 55R20, and the like.
[0100] A tire satisfying the above formula is preferably applied to a pneumatic tire for a passenger vehicle, because a pneumatic tire for a passenger vehicle satisfying the above formula tends to be more suitable for solving the problem of the present invention. EXAMPLES
[0101] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0102] The various chemicals used in the examples and comparative examples will be described below.
[0103] (Rubber component) Natural rubber: TSR20 SBR1: Modified SBR synthesized in Production Example 1 below (styrene content: 10% by mass, vinyl content: 40% by mass, Mw: 300,000) SBR2: SBR1502 manufactured by JSR Corporation (styrene content: 24% by mass, vinyl content: 16% by mass) BR: BR710 manufactured by Ube Industries, Ltd. (cis content: 90% by mass or more, vinyl content: 1.2% by mass)
[0104] (Chemicals other than rubber components) Carbon black 1: N134 (CTAB: 135m 2 / g) Carbon black 2: N220 (CTAB: 111m 2 / g) Silica 1: Ultrasil VN3 (CTAB: 165 m) manufactured by Evonik Degussa 2 / g) Silica 2: Ultrasil 9100GR (CTAB: 200m) manufactured by Evonik Degussa 2 / g) Silane coupling agent 1: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Silane coupling agent 2: NXT (3-octanoylthiopropyltriethoxysilane) manufactured by Momentive Oil: A / O Mix manufactured by Sankyo Yuka Kogyo Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Resin 1: YS Resin TO125 (terpene styrene resin (copolymer of terpene compounds and styrene)) manufactured by Yasuhara Chemical Co., Ltd. Resin 2: Struktol 40MS (a copolymer of styrene and ethylene) manufactured by Struktol Antioxidant 1: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Antioxidant 2: Nocrac RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Processing aid: EF44 (zinc salt of saturated fatty acid) manufactured by Struktol Stearic acid: NOF Corporation's "Tsubaki" stearic acid Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Dibenzylamine compound: Vulcuren VP KA9188 (1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane) manufactured by LANXESS
[0105] (Production Example 1) Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyllithium was added to initiate polymerization. Polymerization was performed under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion reached 99%, butadiene was added, and polymerization was continued for another 5 minutes, after which 3-dimethylaminopropyltriethoxysilane was added as a modifier and the reaction was continued for 15 minutes. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR1.
[0106] Examples and Comparative Examples According to the formulation shown in Table 1, materials other than the dibenzylamine compound, sulfur, and vulcanization accelerator were kneaded for 5 minutes under the condition of 150 ° C using a 1.7 L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, the dibenzylamine compound, sulfur, and vulcanization accelerator were added to the obtained kneaded product, and the mixture was kneaded for 5 minutes under the condition of 80 ° C using an open roll to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was molded into a tread shape, and laminated together with other tire components to form an unvulcanized tire, which was press-vulcanized for 12 minutes under the condition of 150 ° C to produce a test tire (size: 175 / 60R18). The following evaluations were performed using the obtained test tire, and the results are shown in Table 1.
[0107] (Chipping resistance) After a vehicle equipped with the above test tires on all wheels was driven 8000 km, the number of chipping occurrences in the tread portion was counted and expressed as an index with Comparative Example 3 being set at 100. A higher index indicates fewer chipping occurrences and better chipping resistance.
[0108] (low fuel consumption) Using a rolling resistance tester, the rolling resistance was measured when the test tire was run at a speed (80 km / h), and the rolling resistance was expressed as an index with Comparative Example 2 being set at 100. A larger index indicates a smaller rolling resistance and better fuel economy.
[0109] [Table 1]
[0110] As can be seen from Table 1, the Examples were superior to the Comparative Examples in overall performance in terms of the desired fuel economy and chipping resistance.
Claims
1. The rubber component contains styrene-butadiene rubber, carbon black, and silica, The total styrene content in the rubber component is 15% by mass or less, The average cetyltrimethylammonium bromide specific surface area of the carbon black is 120 m 2 / g or more, The carbon black has a specific surface area of 115 m 2 / g or less is 50 mass% or more, A rubber composition for tires, wherein the amount of the carbon black per 100 parts by mass of the rubber component is 20 parts by mass or more, A rubber composition for tires, in which the ratio of resin content / silica content is 0.1 or more and 0.6 or less (excluding the rubber composition for tires described in (1) below). (1) 100 parts by mass of a rubber component containing 40 to 75% by mass of modified natural rubber having a nitrogen content of 0.40% by mass or less and 10 to 35% by mass of styrene-butadiene rubber; 20 to 60 parts by mass of carbon black having a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 120 m 2 / g or more; 0.5 to 3.0 parts by mass of a compound represented by the following formula (A): A rubber composition for tires comprising: R 1 -S-S-Y-S-S-R 2 (A) (In the formula, Y is an alkylene group having 2 to 10 carbon atoms, and R 1 and R 2 are the same or different and each represents a monovalent organic group containing a nitrogen atom.)
2. The rubber component contains an isoprene-based rubber, 2. The rubber composition for tires according to claim 1, wherein the content of said isoprene-based rubber is greater than the content of said styrene-butadiene rubber.
3. The rubber composition for tires according to claim 1 or 2, wherein the total amount of styrene in the rubber component is 10% by mass or less.
4. The rubber composition for tires according to any one of claims 1 to 3, which contains a styrene-based resin.
5. The rubber composition for tires according to any one of claims 1 to 4, which contains a dibenzylamine compound.
6. A tire using the rubber composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Tread rubber composition for heavy load tire or its retreaded tire
JP2000219778A
Modified diene-based rubber composition
JP2000344955A
Rubber composition for tire and tire for heavy load
JP2014012768A
Tire rubber composition and pneumatic tire
JP2018135461A
Rubber composition for tire, and pneumatic tire
JP2018150419A