Method for manufacturing a patterned liquid crystal display element

The method of using a radical-generating film and controlled light exposure allows for the creation of liquid crystal display elements with multiple alignment regions, addressing the complexity and cost issues of current alignment techniques.

JP7586094B2Active Publication Date: 2024-11-19NISSAN CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021565681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-18
Filing Date
2020-12-18
Publication Date
2024-11-19
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing liquid crystal display elements struggle to simultaneously achieve in-plane uniaxial alignment, out-of-plane alignment, and tilted alignment regions within the same device, as current methods are complex and costly, and there is a challenge in creating regions with different anchoring forces without precise alignment techniques.

Method used

A method involving the use of a radical-generating film on a substrate, where a liquid crystal composition containing a radically polymerizable compound is exposed to light of 240 to 400 nm, inducing polymerization and alignment, allowing for the creation of multiple alignment regions through controlled chemical reactions at the interface.

Benefits of technology

This method enables the production of liquid crystal display elements with two or three distinct alignment regions using a simple and cost-effective process, improving alignment control and reducing manufacturing complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586094000058
    Figure 0007586094000058
  • Figure 0007586094000059
    Figure 0007586094000059
  • Figure 0007586094000060
    Figure 0007586094000060
Patent Text Reader

Abstract

Provided is a method for manufacturing, in a simple, low-cost manner, a liquid crystal display element that includes two or three different orientation regions (an in-plane (uniaxial) orientation region, an out-of-plane orientation region, and an inclined orientation region) in the same element. The present invention provides a method for manufacturing a liquid crystal display element in which at least two regions of an in-plane orientation region, an out-of-plane orientation region, and an inclined orientation region are used as patterns therein. The method includes: a step (A) for forming, on a substrate, a radical generation film that could generate radicals as a result of being irradiated with light; and a step (B) for bringing a liquid crystal composition, which contains liquid crystals and a radical-polymerizable compound, into contact with the radical generation film and for irradiating, while maintaining said state, the liquid crystal composition with light having a peak at 240-400 nm, which is sufficient to cause a polymerization reaction of the radical-polymerizable compound. The radical-polymerizable compound has a function of vertically orienting the liquid crystals as a result of being polymerized. Furthermore, the method includes at least one of requirements (Z1) and (Z2). Requirement (Z1): a step (c) for deactivating the radical generation ability of the radical generation film by irradiating the radical generation film obtained in the step (A) with the light having a peak at 240-400 nm is additionally included between the step (A) and the step (B). Requirement (Z2): the step for irradiating the liquid crystal composition with the light having a peak at 240-400 nm in the step (B) is performed via a photomask.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a liquid crystal display element in which at least two of an in-plane alignment region, an out-of-plane alignment region, and an inclined alignment region are patterned, using a method that is inexpensive and does not involve complicated processes. [Background technology]

[0002] In recent years, liquid crystal display elements are widely used in displays for mobile phones, computers, and televisions. Liquid crystal display elements have characteristics such as thinness, light weight, and low power consumption, and are expected to be applied to further content in the future, such as VR (Virtual Reality) and ultra-high resolution displays. Various display modes have been proposed for liquid crystal displays, such as TN (Twisted Nematic), IPS (In-Plane Switching), and VA (Vertical Alignment), and all modes use a film (liquid crystal alignment film) that guides the liquid crystal into a desired alignment state.

[0003] In particular, for products equipped with touch panels such as tablet PCs, smartphones, and smart TVs, the IPS mode is preferred because it is less likely to distort the display when touched. In recent years, LCD display elements using FFS (Frindge Field Switching) and non-contact technology using optical alignment have come to be used to improve contrast and viewing angle characteristics.

[0004] However, FFS has a higher manufacturing cost for the substrate compared to IPS, and there is an issue of display defects specific to the FFS mode called Vcom shift. Photo-alignment has the advantage of being able to manufacture larger elements and greatly improve display characteristics compared to the rubbing method, but there are issues inherent in the photo-alignment principle (display defects due to decomposition products in the case of decomposition type, burn-in due to insufficient alignment force in the case of isomerization type, etc.). At present, LCD element manufacturers and LCD alignment film manufacturers are trying various ideas to solve these issues.

[0005] On the other hand, in recent years, an IPS mode that utilizes something called zero plane anchoring (also known as weak anchoring) has been proposed, and it has been reported that the use of this technique enables improved contrast and significantly lower voltage operation compared to conventional IPS modes (see, for example, Patent Document 1).

[0006] Specifically, a liquid crystal alignment film with strong anchoring energy is used on one of the substrates, and the other substrate equipped with the electrode that generates a lateral electric field is treated so that it has no liquid crystal alignment control power whatsoever, and using these, an IPS mode liquid crystal display element is produced.

[0007] In recent years, a zero-plane anchoring IPS mode technology has been proposed, in which a zero-plane state is created using dense polymer brushes, etc. (See, for example, Patent Document 2.) This technology has achieved a significant improvement in contrast ratio and a significant reduction in driving voltage. On the other hand, there is an issue of a significant drop in response speed, especially when the voltage is turned off. This is due to the effect of the response being made at a weaker electric field compared to normal driving methods due to the lower driving voltage, and because the anchoring strength of the alignment film is extremely weak, so it takes a long time for the liquid crystal to return to its original state. As a method for solving this problem, a method of zero anchoring only on the pixel electrode has been proposed (see, for example, Patent Document 3). It has been reported that this makes it possible to achieve both improved luminance and improved response speed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 4053530 [Patent Document 2] JP 2013-231757 A [Patent Document 3] JP 2017-211566 A Summary of the Invention [Problem to be solved by the invention]

[0009] By using an alignment film that is appropriately designed for each application, it is possible to control the alignment state of various liquid crystals. In particular, by using an alignment film that has an anchoring force in the in-plane uniaxial direction, in-plane uniaxial alignment is obtained, and by using an alignment film that has an anchoring force in the out-of-plane direction, out-of-plane alignment is obtained. On the other hand, it is very difficult to fabricate a liquid crystal element that simultaneously has an in-plane uniaxial alignment region and an out-of-plane alignment region within the same element. This is because it is necessary to create regions with significantly different anchoring strengths within the same element, and to achieve this, it is necessary to change the anchoring strength of an arbitrary region after fabricating the liquid crystal element, or to paint alignment films with different anchoring strengths on the substrates that make up the element in advance. There have been no reports of the former, and the latter also requires the preparation of a technology to paint extremely small regions accurately and perform alignment treatment, which is a major challenge for industrialization. If these technical challenges could be overcome, it would be possible to form liquid crystal elements having any desired alignment state in any desired region, which is expected to lead to applications in optical films, optical property modulation elements, and the like. The present invention has been made to solve the above-mentioned problems, and aims to provide a method for manufacturing a liquid crystal display element by inducing a chemical reaction at the contact interface between an alignment film and a liquid crystal, and by inducing this in any region in the in-plane direction of the alignment film, controlling the surface energy and anchoring energy of the interfacial reaction region to any state, thereby manufacturing a liquid crystal display element having two or three different alignment regions (an in-plane (uniaxial) alignment region, an out-of-plane alignment region, and an inclined alignment region) within the same element in a simple and inexpensive manner. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.

[0011] The present invention includes the following aspects. [1] Step (A): forming a radical generating film capable of generating radicals upon irradiation with light on a substrate; and Step (B): contacting a liquid crystal composition containing liquid crystal and a radical-polymerizable compound with the radical-generating film, and irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm, which is sufficient to polymerize the radical-polymerizable compound while maintaining the contact state; the radical polymerizable compound has a function of vertically aligning the liquid crystal by polymerization, Further, the method for manufacturing a liquid crystal display element includes at least one of the following requirements (Z1) and (Z2), and is characterized in that a liquid crystal display element is manufactured in which at least two regions among an in-plane alignment region, an out-of-plane alignment region, and an inclined alignment region are patterned. Requirement (Z1): Between the steps (A) and (B), the method further includes a step (C) of irradiating the radical-generating film obtained in the step (A) with light having a peak at 240 to 400 nm to inactivate the radical-generating ability of the radical-generating film. Requirement (Z2): The step (B) of irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm is carried out through a photomask. [2] The method for producing a liquid crystal display element according to [1], wherein the radical generating film is a film that has been subjected to uniaxial alignment treatment. [3] The method for producing a liquid crystal display element according to [1] or [2], wherein the step (B) of irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm is carried out without applying an electric field. [4] The method for producing a liquid crystal display element according to any one of [1] to [3], wherein the radical-generating film has a polymer containing an organic group that induces radical polymerization. [5] The method for producing a liquid crystal display element according to [4], wherein the polymer containing an organic group capable of inducing radical polymerization has a structural unit represented by the following formula (1) in its main chain: [ka] (In formula (1), A represents an organic group that induces radical polymerization.) [6] The method for producing a liquid crystal display element according to [4] or [5], wherein the polymer is at least one selected from a polyimide precursor obtained by using a diamine component including a diamine containing an organic group that induces radical polymerization, a polyimide, a polyurea, and a polyamide. [7] The method for producing a liquid crystal display element according to [5], wherein the organic group capable of inducing radical polymerization is a group represented by the following formula (3): [ka] (In formula (3), the dashed line represents a bond to the benzene ring, and R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH3)-, -CON(CH3)-, or -N(CH3)CO-, R 7 represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted by a fluorine atom, and one or more of any -CH2- or -CF2- in the alkylene group may be independently replaced by a group selected from -CH=CH-, a divalent carbocycle, and a divalent heterocycle, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: R 8 represents an organic group capable of inducing radical polymerization, represented by a formula selected from the formulae [X-1] to [X-18], [W], [Y], and [Z]; [ka] In formulas [X-1] to [X-18], * represents R 7each of S1 and S2 independently represents -O-, -NR-, or -S-; R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; each of R1 and R2 independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms; [ka] In the formula [W], [Y], and [Z], * is R 7 represents the bond with S 3 represents a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH)-, -CON(CH)-, or -N(CH)CO-; Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent; R 9 and R 10 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms. In the case of an alkyl group or an alkoxy group, R 9 and R 10 may form a ring, Q represents one of the following structures: [ka] In the formula, R 11 represents -CH2-, -NR-, -O-, or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, * represents a bond, R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. [8] The method for producing a liquid crystal display element according to [6], wherein the diamine containing an organic group capable of inducing radical polymerization is a diamine having a structure represented by the following formula (2): [ka] (In formula (2), A 1 and A2 each represents a hydrogen atom or a group represented by the following formula (3), 1 and A 2 At least one of the groups represented by the following formula (3) is represented: E is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m represents a divalent organic group consisting of -, -SO2-, or any combination thereof, and m represents an integer of 1 to 8. p represents an integer from 0 to 2. When p is 2, multiple A 2 and E each independently have the same definition as above. 1 is a group represented by the following formula (3): [ka] (In formula (3), the dashed line represents a bond to a benzene ring, and R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH3)-, -CON(CH3)-, or -N(CH3)CO-, R 7 represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted by a fluorine atom, and one or more of any -CH2- or -CF2- in the alkylene group may be independently replaced by a group selected from -CH=CH-, a divalent carbocycle, and a divalent heterocycle, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: R 8 represents an organic group capable of inducing radical polymerization, represented by a formula selected from the formulae [X-1] to [X-18], [W], [Y], and [Z]; [ka] In formulas [X-1] to [X-18], * represents R 7each of S1 and S2 independently represents -O-, -NR-, or -S-; R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; each of R1 and R2 independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms; [ka] In the formula [W], [Y], and [Z], * is R 7 represents the bond with S 3 represents a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH)-, -CON(CH)-, or -N(CH)CO-; Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent; R 9 and R 10 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms. In the case of an alkyl group or an alkoxy group, R 9 and R 10 may form a ring, Q represents one of the following structures: [ka] In the formula, R 11 represents -CH2-, -NR-, -O-, or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, * represents a bond, R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. [9] The method for producing a liquid crystal display element according to any one of [1] to [8], wherein at least one of the radical polymerizable compounds is a compound having compatibility with liquid crystal and one polymerizable unsaturated bond in one molecule.

[10] The method for producing a liquid crystal display element according to [9], wherein the polymerization reactive group of the radical polymerizable compound is selected from the following structures: [ka] (In the formula, * indicates a bonding site with a part of the compound molecule other than the polymerizable unsaturated bond. R b represents an alkyl group having 3 to 20 carbon atoms, and E represents a single bond, -O-, or -NR c R represents a linking group selected from -, -S-, an ester bond, and an amide bond. c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R b The alkyl group represents a linear, branched, or cyclic alkyl group.

[11] The method for producing a liquid crystal display element according to any one of [1] to

[10] , wherein the liquid crystal composition containing the liquid crystal and a radically polymerizable compound contains a radically polymerizable compound that allows the polymer obtained by polymerizing the radically polymerizable compound to have a Tg of 100° C. or less.

[12] A first substrate having a radical generating film and a second substrate are provided; The radical generating film on the first substrate is disposed so as to face the second substrate; The method further comprises a step of filling a liquid crystal composition containing liquid crystal and a radical polymerizable compound between the first substrate and the second substrate to prepare a liquid crystal cell. The method for producing a liquid crystal display element according to any one of [1] to

[11] .

[13] The method for producing a liquid crystal display element according to

[12] , wherein the second substrate has a radical-generating film.

[14] The method for producing a liquid crystal display element according to

[12] , wherein the second substrate is a substrate coated with a liquid crystal alignment film having uniaxial alignment properties.

[15] The method for producing a liquid crystal display element according to

[14] , wherein the liquid crystal alignment film having uniaxial alignment properties is a liquid crystal alignment film for horizontal alignment.

[16] The method for producing a liquid crystal display element according to any one of

[12] to

[15] , wherein the first substrate having the radical generating film is a substrate having a comb-shaped electrode. Effect of the Invention

[0012] According to the present invention, it is possible to provide a method for manufacturing a liquid crystal display element, which is a simple and inexpensive method for manufacturing a liquid crystal display element having two or three different alignment regions (an in-plane (uniaxial) alignment region, an out-of-plane alignment region, and an inclined alignment region) within the same element. [Brief description of the drawings]

[0013] [Figure 1A] FIG. 1A is a photograph of the liquid crystal display element obtained in Example 5. [Figure 1B] FIG. 1B is a schematic photograph of the liquid crystal display element of FIG. 1A. [Figure 2A] FIG. 2A is a photograph of the liquid crystal display element obtained in Comparative Example 4. [Figure 2B] FIG. 2B is a schematic photograph of the liquid crystal display element of FIG. 2A. [Figure 3A] FIG. 3A is a photograph of the liquid crystal display element obtained in Example 1. [Figure 3B] FIG. 3B is a schematic photograph of the liquid crystal display element of FIG. 3A. [Figure 4A] FIG. 4A is a photograph of the liquid crystal display element obtained in Example 23. [Figure 4B] FIG. 4B is a schematic photograph of the liquid crystal display element of FIG. 4A. [Figure 5A] FIG. 5A is a photograph of the liquid crystal display element obtained in Example 24. [Figure 5B] FIG. 5B is a schematic photograph of the liquid crystal display element of FIG. 5A. [Figure 6] FIG. 6 is a photograph of the liquid crystal display elements obtained in Examples 25 and 26. [Figure 7] FIG. 7 is a photograph of the liquid crystal display device obtained in Example 27. [Figure 8] FIG. 8 is a photograph of the liquid crystal display element obtained in Example 30. [Figure 9A] FIG. 9A is a photograph of the liquid crystal display element obtained in Example 32. [Figure 9B] FIG. 9B is a schematic photograph of the liquid crystal display element of FIG. 9A. [Figure 10] 1 is a schematic cross-sectional view showing an example of a liquid crystal display element according to the present invention. [Figure 11] FIG. 4 is a schematic cross-sectional view showing another example of a liquid crystal display element according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The method for producing a liquid crystal display element of the present invention will be described in detail below. However, the explanation of the constituent elements described below is an example of one embodiment of the present invention, and the present invention is not limited to these contents.

[0015] (Method of manufacturing liquid crystal display element) The method for producing a liquid crystal display element of the present invention includes the following steps (A) and (B). Step (A): A step of forming a radical generating film capable of generating radicals upon irradiation with light on a substrate. Step (B): A step of contacting a liquid crystal composition containing liquid crystal and a radically polymerizable compound with a radical-generating film, and irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm, which is sufficient to polymerize the radically polymerizable compound, while maintaining that state. The radically polymerizable compound in the above step (B) is a compound that has the function of vertically aligning liquid crystals by polymerization. Furthermore, the method for producing a liquid crystal display element of the present invention includes at least one of the following requirements (Z1) and (Z2). Requirement (Z1): Between steps (A) and (B), a step (C) is further included in which the radical-generating film obtained in step (A) is irradiated with light having a peak at 240 to 400 nm to inactivate the radical-generating ability of the radical-generating film. Requirement (Z2): The step (B) of irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm is carried out through a photomask. The present invention, which includes the above-mentioned steps (A) and (B) and further satisfies at least one of requirements (Z1) and (Z2), can produce a liquid crystal display element in which at least two regions among an in-plane alignment region, an out-of-plane alignment region, and an inclined alignment region are patterned.

[0016] <Radical generating film> In the present invention, a radical generating film is formed on a substrate. Here, the radical-generating film refers to a film capable of generating radicals. The radical-generating film is formed, for example, from a radical-generating film-forming composition.

[0017] <<Radical-generating film-forming composition>> The radical-generating film-forming composition contains a polymer and a group capable of generating radicals as components. In this case, the radical-generating film-forming composition may be a composition containing a polymer having a group capable of generating radicals bonded thereto, or may be a composition of a compound having a group capable of generating radicals and a polymer serving as a base resin. By applying such a radical-generating film-forming composition onto a substrate and curing the applied film, a radical-generating film in which a group capable of generating radicals is fixed can be obtained. The group capable of generating radicals is preferably an organic group that induces radical polymerization.

[0018] When the radical-generating film is made of a polymer containing an organic group that induces radical polymerization, an example of the polymer containing an organic group that induces radical polymerization is a polymer having a structural unit represented by the following formula (1) in its main chain. [ka] In formula (1), A represents an organic group that induces radical polymerization.

[0019] When using a polymer containing an organic group that induces radical polymerization, in order to obtain a polymer having a group capable of generating radicals, it is preferable to produce the polymer using, as a monomer component, a monomer having a photoreactive side chain containing at least one selected from a methacryl group, an acrylic group, a vinyl group, an allyl group, a coumarin group, a styryl group, and a cinnamoyl group, or a monomer having a site in a side chain that decomposes upon irradiation with light to generate radicals. On the other hand, the monomer that generates radicals has a problem that it spontaneously polymerizes itself, and there is a risk of it becoming an unstable compound. For this reason, from the viewpoint of ease of synthesis, polymers derived from diamines having a radical generating site are preferred, and more preferred are polyimide precursors such as polyamic acids and polyamic acid esters, polyimides, polyureas, polyamides, and the like.

[0020] An example of the organic group that induces radical polymerization is a group represented by the following formula (3). [ka] In formula (3), the dashed line represents a bond to the benzene ring, and R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH3)-, -CON(CH3)-, or -N(CH3)CO-, R 7 represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted by a fluorine atom, and one or more of any -CH2- or -CF2- in the alkylene group may be independently replaced by a group selected from -CH=CH-, a divalent carbocycle, and a divalent heterocycle, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: R 8 represents an organic group capable of inducing radical polymerization, represented by a formula selected from the formulae [X-1] to [X-18], [W], [Y], and [Z]; [ka] In formulas [X-1] to [X-18], * represents R 7 each of S1 and S2 independently represents -O-, -NR-, or -S-; R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; each of R1 and R2 independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms;

[0021] [ka] In the formula [W], [Y], and [Z], * is R 7 represents the bond with S 3 represents a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH)-, -CON(CH)-, or -N(CH)CO-; Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent; R 9 and R 10 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms. In the case of an alkyl group or an alkoxy group, R 9 and R 10 may form a ring, Q represents one of the following structures: [ka] In the formula, R 11 represents -CH2-, -NR-, -O-, or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, * represents a bond, R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.

[0022] Specifically, the organic group represented by the formula selected from the above [W], [Y] and [Z] is preferably the following: In particular, from the viewpoint of the reliability of the resulting liquid crystal display device, (b) and (c) are more preferable. [ka]

[0023] A preferred embodiment of the polymer containing an organic group capable of inducing radical polymerization is a diamine having an organic group capable of inducing radical polymerization. Specifically, such a diamine having a radical generating site is a diamine having a side chain capable of generating radicals and polymerizing, and an example thereof is a diamine represented by the following formula (2), but is not limited thereto.

[0024] [ka] In formula (2), A 1 and A 2 each represents a hydrogen atom or a group represented by the above formula (3), provided that A 1 and A 2 At least one of the groups represented by formula (3) is E is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m represents a divalent organic group consisting of -, -SO2-, or any combination thereof, and m represents an integer of 1 to 8. "Any combination thereof" includes -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO-, -COO-(CH2) m Examples of the alkyl group include, but are not limited to, -OCO-. p represents an integer from 0 to 2. When p is 2, multiple A2 and E each independently have the same definition as above. 1 is a group represented by the following formula (3).

[0025] In the above formula (2), when p=0, the bonding positions of the two amino groups (-NH2) are not limited. Specifically, the bonding positions on the benzene ring relative to the bonding group of the side chain include the 2,3 position, the 2,4 position, the 2,5 position, the 2,6 position, the 3,4 position, and the 3,5 position. Among them, the 2,4 position, the 2,5 position, or the 3,5 position is preferable from the viewpoint of reactivity in synthesizing a polyamic acid. Taking into account the ease of synthesizing a diamine, the 2,4 position or the 3,5 position is more preferable.

[0026] Specific examples of diamines having a photoreactive group containing at least one selected from the group consisting of a methacryl group, an acrylic group, a vinyl group, an allyl group, a coumarin group, a styryl group, and a cinnamoyl group include, but are not limited to, the following compounds. [ka]

[0027] [ka] (In the formula, J 1 is a single bond, -O-, -COO-, -NHCO-, or -NH- linking group, J 2 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms.

[0028] As the diamine having an organic group represented by the formula selected from the above [W], [Y], and [Z], in consideration of ease of synthesis, high versatility, properties, etc., the structure represented by the following formula is most preferable, but is not limited thereto. [ka] (In the formula, n is an integer of 2 to 8, and E is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO- or -COO-(CH2) m -OCO-, and m is an integer of 1 to 8. [ka] (In the formula, n is an integer of 2 to 8.)

[0029] The above diamines can be used alone or in combination of two or more depending on the properties such as liquid crystal alignment properties, sensitivity in the polymerization reaction, voltage retention properties, and stored charge when formed into a radical generating film.

[0030] The diamine having such a site where radical polymerization occurs is preferably used in an amount of 5 to 50 mol %, more preferably 10 to 40 mol %, and particularly preferably 15 to 30 mol %, of the total diamine components used in the synthesis of the polymer contained in the radical-generating film-forming composition.

[0031] When the polymer used in the radical generating film of the present invention is obtained from a diamine, other diamines than the diamines having the radical generating sites can be used as the diamine component. Specifically, p-phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, m-phenylenediamine, 2,4-dimethyl-m-phenylenediamine, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,5-diaminophenol, 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, 4,4'-diaminobenzyl alcohol, 4,5-diaminobenzyl alcohol, 4,6-diaminoresorcinol, 4,5-diaminobenzyl alcohol ... Aminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 3,3'-dicarboxy-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,2'-diaminobiphenyl, 2,3'-diaminobiphenyl Aminobiphenyl, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2'-diaminodiphenylmethane, 2,3'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 2,3'-diaminodiphenyl ether, 4,4'-sulfonyldianiline, 3,3'-sulfonyldianiline, biphenyl Bis(4-aminophenyl)silane, bis(3-aminophenyl)silane, dimethyl-bis(4-aminophenyl)silane, dimethyl-bis(3-aminophenyl)silane, 4,4'-thiodianiline, 3,3'-thiodianiline, 4,4'-diaminodiphenylamine, 3,3'-diaminodiphenylamine, 3,4'-diaminodiphenylamine, 2,2'-diaminodiphenylamine, 2,3'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, N-methyl(3,3'-diaminodiphenyl)amine, N-methyl(3,4'-diaminodiphenyl)amine, N-methyl(2,2'-diaminodiphenyl)amine, N-methyl(2,3'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 2,2'-diaminobenzophenone, 2,3'-diaminobenzophenone, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, 1,6-diaminonaphthalene, 1,7-diaminonaphthalene, 1,8- Diaminonaphthalene, 2,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 1,2-bis(4-aminophenyl)ethane, 1,2-bis(3-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,3-bis(3-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(3-aminophenyl)butane, bis(3,5-diethyl-4-aminophenyl)methane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4- aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]dianiline, 4,4'-[1,3-phenylenebis(methylene)]dianiline, 3,4'-[1,4-phenylenebis(methylene)]dianiline, 3,4'-[1,3-phenylenebis(methylene)]dianiline, 3,3'-[1,4-phenylene bis(methylene)]dianiline, 3,3'-[1,3-phenylenebis(methylene)]dianiline, 1,4-phenylenebis[(4-aminophenyl)methanone], 1,4-phenylenebis[(3-aminophenyl)methanone], 1,3-phenylenebis[(4-aminophenyl)methanone], 1,3-phenylenebis[(3-aminophenyl)methanone], 1,4-phenylenebis(4-aminobenzoate), 1,4-phenylenebis(3-aminobenzoate), 1,3-phenylenebis(4-aminobenzoate), 1,3-phenylenebis(3-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(3-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate, bis(3-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-(1,3-phenylene)bis(4-aminobenzamide), N,N'-(1,4-phenylene)bis(3-aminobenzamide), N,N'-(1,3-phenylene)bis(3-aminobenzamide), N,N'-bis(4-amino N,N'-bis(3-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, N,N'-bis(3-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 4,4'-bis(4-aminophenoxy)diphenylsulfone, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)hexafluoropropane propane, 2,2'-bis(3-aminophenyl)hexafluoropropane, 2,2'-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2'-bis(4-aminophenyl)propane, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(3-amino-4-methylphenyl)propane, trans-1,4-bis(4-aminophenyl)cyclohexane, 3,5-diaminobenzoic acid, 2,5-diaminobenzoic acid, bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis (4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(3-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,5-bis(3-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,6-bis(3-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, 1,7-bis(3-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,Aromatic diamines such as 8-bis(3-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,9-bis(3-aminophenoxy)nonane, 1,10-bis(4-aminophenoxy)decane, 1,10-bis(3-aminophenoxy)decane, 1,11-bis(4-aminophenoxy)undecane, 1,11-bis(3-aminophenoxy)undecane, 1,12-bis(4-aminophenoxy)dodecane, and 1,12-bis(3-aminophenoxy)dodecane; alicyclic diamines such as bis(4-aminocyclohexyl)methane and bis(4-amino-3-methylcyclohexyl)methane; 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, and 1,7-diaminoheptane. aliphatic diamines such as 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, and 1,12-diaminododecane; diamines having a urea structure such as 1,3-bis[2-(p-aminophenyl)ethyl]urea and 1,3-bis[2-(p-aminophenyl)ethyl]-1-tert-butoxycarbonylurea; diamines having a nitrogen-containing unsaturated heterocyclic structure such as Np-aminophenyl-4-p-aminophenyl(tert-butoxycarbonyl)aminomethylpiperidine; and diamines having an N-Boc group (Boc represents a tert-butoxycarbonyl group) such as N-tert-butoxycarbonyl-N-(2-(4-aminophenyl)ethyl)-N-(4-aminobenzyl)amine.

[0032] The above other diamines can be used alone or in combination of two or more depending on the properties such as liquid crystal alignment properties, sensitivity in the polymerization reaction, voltage retention properties, and stored charge when formed into a radical generating film.

[0033] In the synthesis of a polymer in the form of a polyamic acid, the tetracarboxylic dianhydride to be reacted with the diamine component is not particularly limited. Specifically, pyromellitic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 1,2,5,6-naphthalenetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 2,3,6,7-anthracenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether ... 2,2-bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)methane, 2,2-bis(3,4-dicarboxyphenyl)propane, 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane, bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,3',4,4'-diphenylsulfone Tetracarboxylic acids, 3,4,9,10-perylenetetracarboxylic acid, 1,3-diphenyl-1,2,3,4-cyclobutanetetracarboxylic acid, oxydiphthaltetracarboxylic acid, 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,3-dimethyl-1 ,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cycloheptanetetracarboxylic acid, 2,3,4,5-tetrahydrofurantetracarboxylic acid, 3,4-dicarboxy-1-cyclohexylsuccinic acid, 2,3,5-tricarboxycyclopentylacetic acid, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalenesuccinic acid, bicyclo[3.3.0]octane-2,4,6,8-tetracarboxylic acid, bicyclo[4.3.0]nonane-2,4,7,9-tetracarboxylic acid, bicyclo[4.4.0]decane-2,4,7,9-tetracarboxylic acid, bicyclo[4.4.0]decane-2,4,8,10-tetracarboxylic acid, tricyclo[6.3.0.0<2,6>]undecane-3,5,9,11-tetracarboxylic acid, 1,2,3,4-butanetetracarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydrinaphthalene-1,2-dicarboxylic acid, bicyclo[2.2.2]oct-7-ene Examples of dianhydrides of tetracarboxylic acids include norbornane-2,3,5,6-tetracarboxylic acid, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexane-1,2-dicarboxylic acid, tetracyclo[6.2.1.1<3,6>.0<2,7>]dodeca-4,5,9,10-tetracarboxylic acid, 3,5,6-tricarboxynorbornane-2:3,5:6 dicarboxylic acid, and 1,2,4,5-cyclohexanetetracarboxylic acid.

[0034] Of course, one or more kinds of tetracarboxylic dianhydrides may be used in combination depending on the properties such as liquid crystal alignment properties, sensitivity in polymerization reaction, voltage retention properties, and accumulated charge when used as a radical generating film.

[0035] In the synthesis of a polyamic acid ester polymer, the structure of the tetracarboxylic acid dialkyl ester reacted with the above diamine component is not particularly limited, but specific examples are given below. Specific examples of the aliphatic tetracarboxylic acid diester include 1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2-dimethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2,3,4-cyclopentane tetracarboxylic acid dialkyl ester, 2,3,4,5-tetrahydrofuran tetracarboxylic acid dialkyl ester, 1,2,4,5-cyclohexane tetracarboxylic acid dialkyl ester, 3,4-dicarboxy-1-cyclohexyl succinic acid dialkyl ester, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic acid dialkyl ester, 1,2,3,4-butane tetracarboxylic acid dialkyl ester, esters, bicyclo[3.3.0]octane-2,4,6,8-tetracarboxylic acid dialkyl esters, 3,3',4,4'-dicyclohexyl tetracarboxylic acid dialkyl esters, 2,3,5-tricarboxycyclopentyl acetate dialkyl esters, cis-3,7-dibutylcycloocta-1,5-diene-1,2,5,6-tetracarboxylic acid dialkyl esters, tricyclo[4.2.1.0<2,5>]nonane-3,4, Examples of such alkyl esters include 7,8-tetracarboxylic acid-3,4:7,8-dialkyl esters, hexacyclo[6.6.0.1<2,7>.0<3,6>.1<9,14>.0<10,13>]hexadecane-4,5,11,12-tetracarboxylic acid-4,5:11,12-dialkyl esters, and 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid dialkyl esters.

[0036] Examples of aromatic tetracarboxylic acid dialkyl esters include pyromellitic acid dialkyl esters, 3,3',4,4'-biphenyl tetracarboxylic acid dialkyl esters, 2,2',3,3'-biphenyl tetracarboxylic acid dialkyl esters, 2,3,3',4-biphenyl tetracarboxylic acid dialkyl esters, 3,3',4,4'-benzophenone tetracarboxylic acid dialkyl esters, 2,3,3',4'-benzophenone tetracarboxylic acid dialkyl esters, bis(3,4-dicarboxyphenyl)ether dialkyl esters, bis(3,4-dicarboxyphenyl)sulfone dialkyl esters, 1,2,5,6-naphthalene tetracarboxylic acid dialkyl esters, and 2,3,6,7-naphthalene tetracarboxylic acid dialkyl esters.

[0037] In the synthesis of a polyurea polymer, the diisocyanate to be reacted with the diamine component is not particularly limited, and can be used depending on availability, etc. Specific structures of diisocyanates are shown below. [ka] In the formula, R2 and R3 represent an aliphatic hydrocarbon having 1 to 10 carbon atoms.

[0038] Aliphatic diisocyanates shown in K-1 to K-5 have the advantage of being inferior in reactivity but improving solvent solubility, while aromatic diisocyanates shown in K-6 to K-7 are highly reactive and have the effect of improving heat resistance, but have the disadvantage of reducing solvent solubility. In terms of versatility and properties, K-1, K-7, K-8, K-9, and K-10 are preferred, while K-12 is preferred from the viewpoint of electrical properties, and K-13 is preferred from the viewpoint of liquid crystal alignment. Diisocyanates can be used in combination of one or more types, and it is preferable to apply them in various ways depending on the properties you want to obtain. In addition, a part of the diisocyanate can be replaced with the above-described tetracarboxylic dianhydride, and the polyimide may be used in the form of a copolymer of polyamic acid and polyurea, or in the form of a copolymer of polyimide and polyurea obtained by chemical imidization.

[0039] In the synthesis of a polyamide polymer, the structure of the dicarboxylic acid to be reacted is not particularly limited, but specific examples are as follows: Specific examples of aliphatic dicarboxylic acids include dicarboxylic acids such as malonic acid, oxalic acid, dimethylmalonic acid, succinic acid, fumaric acid, glutaric acid, adipic acid, muconic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, 2,2-dimethylglutaric acid, 3,3-diethylsuccinic acid, azelaic acid, sebacic acid, and suberic acid.

[0040] Examples of alicyclic dicarboxylic acids include 1,1-cyclopropanedicarboxylic acid, 1,2-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, 1,2-cyclobutanedicarboxylic acid, 1,3-cyclobutanedicarboxylic acid, 3,4-diphenyl-1,2-cyclobutanedicarboxylic acid, 2,4-diphenyl-1,3-cyclobutanedicarboxylic acid, 1-cyclobutene-1,2-dicarboxylic acid, 1-cyclobutene-3,4-dicarboxylic acid, 1,1-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexanedicarboxylic acid, 1,2-cyclopentane ...3-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopent Examples of suitable amines include norbornene dicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,4-(2-norbornene)dicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, bicyclo[2.2.2]octane-2,3-dicarboxylic acid, 2,5-dioxo-1,4-bicyclo[2.2.2]octanedicarboxylic acid, 1,3-adamantanedicarboxylic acid, 4,8-dioxo-1,3-adamantanedicarboxylic acid, 2,6-spiro[3.3]heptanedicarboxylic acid, 1,3-adamantanediacetic acid, and camphoric acid.

[0041] Examples of aromatic dicarboxylic acids include o-phthalic acid, isophthalic acid, terephthalic acid, 5-methylisophthalic acid, 5-tert-butylisophthalic acid, 5-aminoisophthalic acid, 5-hydroxyisophthalic acid, 2,5-dimethylterephthalic acid, tetramethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-anthracenedicarboxylic acid, 1,4-anthraquinonedicarboxylic acid, 2,5-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,5-biphenylenedicarboxylic acid, 4,4"-terphenyldicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylethanedicarboxylic acid, 4,4'-diphenylpropanedicarboxylic acid, 4,4'-diphenyl Examples of dicarboxylic acids include hexafluoropropane dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-bibenzyl dicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 4,4'-trans dicarboxylic acid, 4,4'-carbonyl dibenzoic acid, 4,4'-sulfonyl dibenzoic acid, 4,4'-dithio dibenzoic acid, p-phenylene diacetic acid, 3,3'-p-phenylene dipropionic acid, 4-carboxycinnamic acid, p-phenylene diacrylic acid, 3,3'-[4,4'-(methylene di-p-phenylene)] dipropionic acid, 4,4'-[4,4'-(oxydi-p-phenylene)] dipropionic acid, 4,4'-[4,4'-(oxydi-p-phenylene)] dibutyric acid, (isopropylidenedi-p-phenylenedioxy) dibutyric acid, and bis(p-carboxyphenyl) dimethylsilane.

[0042] Examples of dicarboxylic acids containing a heterocycle include 1,5-(9-oxofluorene)dicarboxylic acid, 3,4-furandicarboxylic acid, 4,5-thiazoledicarboxylic acid, 2-phenyl-4,5-thiazoledicarboxylic acid, 1,2,5-thiadiazole-3,4-dicarboxylic acid, 1,2,5-oxadiazole-3,4-dicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 3,4-pyridinedicarboxylic acid, and 3,5-pyridinedicarboxylic acid.

[0043] The above-mentioned various dicarboxylic acids may have an acid dihalide or anhydride structure. It is preferable that these dicarboxylic acids are capable of giving a polyamide having a linear structure, in order to maintain the alignment of liquid crystal molecules. Among these, terephthalic acid, isoterephthalic acid, 1,4-cyclohexanedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylethanedicarboxylic acid, 4,4'-diphenylpropanedicarboxylic acid, 4,4'-diphenylhexafluoropropanedicarboxylic acid, 2,2-bis(phenyl)propanedicarboxylic acid, 4,4"-terphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,5-pyridinedicarboxylic acid, or acid dihalides thereof are preferably used. Some of these compounds have isomers, and mixtures containing them may be used. Two or more compounds may be used in combination. The dicarboxylic acids used in the present invention are not limited to the above-mentioned exemplary compounds.

[0044] A known synthesis method can be used to obtain polyamic acid, polyamic acid ester, polyurea, or polyamide by reacting a raw material diamine (also referred to as a "diamine component") with a raw material tetracarboxylic dianhydride (also referred to as a "tetracarboxylic dianhydride component"), a tetracarboxylic diester, a diisocyanate, and a dicarboxylic acid. Generally, the method involves reacting a diamine component with one or more components selected from a tetracarboxylic dianhydride component, a tetracarboxylic diester, a diisocyanate, and a dicarboxylic acid in an organic solvent.

[0045] The reaction between the diamine component and the tetracarboxylic dianhydride component is advantageous in that it proceeds relatively easily in an organic solvent and does not produce by-products.

[0046] The organic solvent used in the reaction is not particularly limited as long as the polymer produced is soluble in the organic solvent. Furthermore, even if the polymer is not soluble in the organic solvent, it may be mixed with the above-mentioned solvent to the extent that the polymer produced does not precipitate. Note that, since the moisture in the organic solvent inhibits the polymerization reaction and further causes the polymer produced to be hydrolyzed, it is preferable to use the organic solvent that has been dehydrated and dried.

[0047] Examples of the organic solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, N-methylcaprolactam, dimethylsulfoxide, tetramethylurea, pyridine, dimethylsulfone, hexamethylphosphoric triamide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, diphenylmethane, ethylhexyl ether, butyl ether, isopropyl alcohol ... ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, methyl cellosolve acetate, butyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethacrylate ethyl ether, propylene glycol monobutyl ether, propylene glycol-tert-butyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, dioxane, n-hexane, n-pentane, n-octane,Examples of the organic solvent include diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diglyme, 4-hydroxy-4-methyl-2-pentanone, and 2-ethyl-1-hexanol. These organic solvents may be used alone or in combination.

[0048] When the diamine component and the tetracarboxylic dianhydride component are reacted in an organic solvent, any of the following methods may be used: a solution in which the diamine component is dispersed or dissolved in an organic solvent is stirred, and the tetracarboxylic dianhydride component is added as is or after being dispersed or dissolved in an organic solvent; a method in which the diamine component is added to a solution in which the tetracarboxylic dianhydride component is dispersed or dissolved in an organic solvent; a method in which the tetracarboxylic dianhydride component and the diamine component are added alternately; etc. In addition, when the diamine component or the tetracarboxylic dianhydride component is composed of a plurality of kinds of compounds, they may be reacted in a premixed state, or may be reacted individually in sequence, and low molecular weight compounds that have been reacted individually may be mixed and reacted to form a high molecular weight compound.

[0049] The temperature at which the diamine component and the tetracarboxylic dianhydride component are reacted can be selected arbitrarily, for example, within the range of −20 to 100° C., and preferably −5 to 80° C. The reaction can be carried out at an arbitrary concentration, and for example, the total amount of the diamine component and the tetracarboxylic dianhydride component relative to the reaction liquid is 1 to 50% by mass, and preferably 5 to 30% by mass.

[0050] In the above polymerization reaction, the ratio of the total number of moles of the tetracarboxylic dianhydride components to the total number of moles of the diamine components can be selected at any value depending on the molecular weight of the polyamic acid to be obtained. As in the case of a normal polycondensation reaction, the closer this molar ratio is to 1.0, the larger the molecular weight of the polyamic acid to be produced. The preferred range is 0.8 to 1.2.

[0051] The method for synthesizing the polymer used in the present invention is not limited to the above-mentioned method. When synthesizing a polyamic acid, a tetracarboxylic acid derivative such as a tetracarboxylic acid or a tetracarboxylic acid dihalide having a corresponding structure can be used instead of the above-mentioned tetracarboxylic acid dianhydride in the same manner as in the general polyamic acid synthesis method, and the corresponding polyamic acid can be obtained by reacting the tetracarboxylic acid derivative by a known method. When synthesizing a polyurea, a diamine can be reacted with a diisocyanate. When producing a polyamic acid ester or polyamide, a diamine, a component selected from a tetracarboxylic acid diester, and a dicarboxylic acid can be reacted with a diamine in the presence of a known condensing agent or after being derived into an acid halide by a known method.

[0052] The method of imidizing the above-mentioned polyamic acid to obtain a polyimide includes thermal imidization in which a solution of polyamic acid is heated as is, and catalytic imidization in which a catalyst is added to a solution of polyamic acid. The imidization rate from polyamic acid to polyimide is preferably 30% or more, more preferably 30 to 99%, because it can increase the voltage retention rate. On the other hand, from the viewpoint of whitening characteristics, that is, suppressing precipitation of polymers in the varnish, it is preferably 70% or less. Taking both characteristics into consideration, it is more preferably 40 to 80%.

[0053] The temperature when thermally imidizing the polyamic acid in a solution is usually 100 to 400° C., preferably 120 to 250° C., and it is preferable to carry out the imidization while removing water generated by the imidization reaction from the system.

[0054] The catalytic imidization of polyamic acid can be carried out by adding a basic catalyst and an acid anhydride to a solution of polyamic acid and stirring the mixture at -20 to 250°C, preferably 0 to 180°C. The amount of the basic catalyst is usually 0.5 to 30 times by mol, preferably 2 to 20 times by mol, the amount of the acid anhydride is usually 1 to 50 times by mol, preferably 3 to 30 times by mol, the amount of the amic acid group. Examples of the basic catalyst include pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc., among which pyridine is preferred because it has a suitable basicity for promoting the reaction. Examples of the acid anhydride include acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc., among which acetic anhydride is preferred because it facilitates purification after the reaction. The imidization rate by catalytic imidization can be controlled by adjusting the amount of the catalyst, the reaction temperature, the reaction time, etc.

[0055] When recovering the polymer generated from the reaction solution of the polymer, the reaction solution may be poured into a poor solvent to cause precipitation. Examples of poor solvents used for precipitation include methanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, and water. The polymer precipitated by pouring into the poor solvent can be recovered by filtration, and then dried at room temperature or by heating under normal or reduced pressure. In addition, the polymer precipitated and recovered can be redissolved in an organic solvent and the reprecipitation and recovery operation can be repeated 2 to 10 times to reduce impurities in the polymer. Examples of poor solvents in this case include alcohols, ketones, and hydrocarbons, and it is preferable to use three or more poor solvents selected from these because the efficiency of purification is further improved.

[0056] In addition, when the radical-generating film is made of a polymer containing an organic group that induces radical polymerization, the radical-generating film-forming composition used in the present invention may contain a polymer other than the polymer containing an organic group that induces radical polymerization. In this case, the content of the other polymer in the total polymer components is preferably 5 to 95 mass %, more preferably 30 to 70 mass %.

[0057] The molecular weight of the polymer contained in the radical-generating film-forming composition is preferably 5,000 to 1,000,000, and more preferably 10,000 to 150,000, in terms of weight-average molecular weight measured by GPC (Gel Permeation Chromatography), taking into consideration the strength of the radical-generating film obtained by applying the radical-generating film-forming composition, the workability during film formation, the uniformity of the film, and the like.

[0058] When the radical-generating film used in the present invention is obtained by applying a composition of a compound having a radical-generating group and a polymer, curing the composition to form a film and fixing the polymer in the film, the polymer may be at least one polymer selected from the group consisting of a polyimide precursor produced according to the above-mentioned production method, and polyimide, polyurea, polyamide, polyacrylate, polymethacrylate, etc., and the diamine having a site where radical polymerization occurs is 0 mol% of the total diamine components used to synthesize the polymer to be contained in the radical-generating film-forming composition. Examples of the compound having a radical-generating group to be added at this time include the following.

[0059] The compound that generates radicals by light is not particularly limited as long as it is a compound that initiates radical polymerization by irradiation with light. Examples of such radical photopolymerization initiators include benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexylphenyl ketone, isopropyl benzoin ether, isobutyl benzoin ether ... ,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, camphorquinone, benzanthrone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 4-dimethylaminobenzoic acid ethyl ester, 4-dimethylaminobenzoic acid isoamyl ester, 4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(tert-butylperoxycarbonyl)benzophenone, dicarbonyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2'-methoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-pentyloxy) p-Dimethylaminostyryl)-4,6-bis(trichloromethyl)-s-triazine, 4-[pN,N-di(ethoxycarbonylmethyl)]-2,6-di(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4'-methoxyphenyl)-s-triazine, 2-(p-Dimethylaminostyryl)benzoxazole, 2-(p-Dimethylaminostyryl)benzthiazole, 2-Mercaptobenzothiazole, 3,3'-Carbonylbis(7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetrakis(4-ethoxycarbonylphenyl)-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinopropionyl)-9-n-dodecylcarbazole, 1-hydroxycyclohexyl phenyl ketone, bis(5-2,4-cyclohexyl)phenyl (2,6-difluoro-3-(1H-pyrrol-1-yl)-cyclopentadien-1-yl)-phenyl titanium, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4'-di(methoxy Examples of the tert-butylperoxycarbonyl)benzophenone include 4,4'-di(methoxycarbonyl)-3,3'-di(tert-butylperoxycarbonyl)benzophenone, 2-(3-methyl-3H-benzothiazol-2-ylidene)-1-naphthalen-2-yl-ethanone, and 2-(3-methyl-1,3-benzothiazol-2(3H)-ylidene)-1-(2-benzoyl)ethanone. These compounds may be used alone or in combination of two or more.

[0060] Even when the radical-generating film is made of a polymer containing an organic group that induces radical polymerization, it may contain a compound having a group that generates the radicals in order to promote radical polymerization upon irradiation with light.

[0061] The radical-generating film-forming composition may contain an organic solvent that dissolves or disperses the polymer component, and if necessary, the radical generator and other components. There is no particular limitation on such organic solvent, and examples thereof include the organic solvents exemplified in the synthesis of the polyamic acid described above. Among them, N-methyl-2-pyrrolidone, γ-butyrolactone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, etc. are preferred from the viewpoint of solubility. In particular, N-methyl-2-pyrrolidone or N-ethyl-2-pyrrolidone is preferred, but a mixed solvent of two or more kinds may be used.

[0062] In addition, it is preferable to use a solvent that improves the uniformity and smoothness of the coating film by mixing it with an organic solvent in which the components contained in the radical-generating film-forming composition are highly soluble.

[0063] Examples of solvents that improve the uniformity and smoothness of the coating film include isopropyl alcohol, methoxymethyl pentanol, methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, butyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethyl carbitol acetate, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol-tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, n-hexa , n-pentane, n-octane, diethyl ether, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, 1-methoxy-2-propanol,Examples of the solvent include 1-ethoxy-2-propanol, 1-butoxy-2-propanol, 1-phenoxy-2-propanol, propylene glycol monoacetate, propylene glycol diacetate, propylene glycol-1-monomethyl ether-2-acetate, propylene glycol-1-monoethyl ether-2-acetate, dipropylene glycol, 2-(2-ethoxypropoxy)propanol, and 2-ethyl-1-hexanol. A plurality of these solvents may be mixed. When using these solvents, the amount is preferably 5 to 80% by mass, more preferably 20 to 60% by mass, of the total solvent contained in the liquid crystal alignment agent.

[0064] The radical-generating film-forming composition may contain components other than those mentioned above. Examples of such components include compounds that improve the film thickness uniformity and surface smoothness when the radical-generating film-forming composition is applied, compounds that improve the adhesion between the radical-generating film-forming composition and a substrate, and compounds that further improve the film strength of the radical-generating film-forming composition.

[0065] Compounds that improve the uniformity of the film thickness and the surface smoothness include fluorine-based surfactants, silicone-based surfactants, and nonionic surfactants. More specifically, for example, EFTOP EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronics Co., Ltd.), Megafac F171, F173, and R-30 (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by 3M), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by AGC Corporation) can be mentioned. When using these surfactants, the proportion of the surfactant used is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, based on 100 parts by mass of the total amount of the polymer contained in the radical-generating film-forming composition.

[0066] Specific examples of compounds that improve the adhesion between the radical-generating film-forming composition and the substrate include functional silane-containing compounds and epoxy group-containing compounds.For example, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane silane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyltrimethoxysilane, N-benzyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N- Phenyl-3-aminopropyltriethoxysilane, N-bis(oxyethylene)-3-aminopropyltrimethoxysilane, N-bis(oxyethylene)-3-aminopropyltriethoxysilane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, Examples of suitable glycidyl ethers include serine diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, 3-(N-allyl-N-glycidyl)aminopropyltrimethoxysilane, and 3-(N,N-diglycidyl)aminopropyltrimethoxysilane.

[0067] In order to further increase the film strength of the radical-generating film, a phenol compound such as 2,2'-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane, tetra(methoxymethyl)bisphenol, etc. may be added. When using these compounds, the amount is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, per 100 parts by mass of the total amount of the polymer contained in the radical-generating film-forming composition.

[0068] Furthermore, in addition to the above, the radical-generating film-forming composition may contain a dielectric or conductive substance for the purpose of changing the electrical properties, such as the dielectric constant and conductivity, of the radical-generating film, as long as the effects of the present invention are not impaired.

[0069] <<How to prepare a radical generating film>> The radical-generating film according to the present invention can be obtained by using the radical-generating film-forming composition. For example, the radical-generating film-forming composition used in the present invention can be applied to a substrate, and then dried and baked to obtain a cured film, which can be used as it is as a radical-generating film. In addition, the cured film can be rubbed, irradiated with polarized light or light of a specific wavelength, or treated with an ion beam, or irradiated with UV light on a liquid crystal display element filled with liquid crystal as an alignment film for PSA.

[0070] The irradiation light used when producing the radical generating film is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include light having a peak at 240 to 400 nm. Light having a peak at 250 to 365 nm is more preferable, and light having a peak at 250 to 360 nm is even more preferable. More specifically, examples thereof include light having a peak near 254 nm or near 313 nm. If necessary, light of a specific wavelength or light having a wavelength equal to or greater than a specific wavelength may be cut using a known cut filter.

[0071] The substrate to which the radical-generating film-forming composition is applied is not particularly limited as long as it is a highly transparent substrate, and is not limited to an electrode. For example, a preferred embodiment is a substrate on which a transparent electrode for driving liquid crystal is formed. Specific examples include substrates on which a transparent electrode is formed, such as a glass plate, or a plastic plate such as polycarbonate, poly(meth)acrylate, polyethersulfone, polyarylate, polyurethane, polysulfone, polyether, polyetherketone, trimethylpentene, polyolefin, polyethylene terephthalate, (meth)acrylonitrile, triacetyl cellulose, diacetyl cellulose, or acetate butyrate cellulose.

[0072] Substrates that can be used for IPS-type liquid crystal display elements can have electrode patterns such as standard IPS comb electrodes and PSA fishbone electrodes, as well as protrusion patterns such as MVA. Moreover, in highly functional elements such as TFT type elements, elements such as transistors are formed between electrodes for driving liquid crystal and a substrate. When a transmissive liquid crystal display element is intended, the above-mentioned substrates are generally used, but when a reflective liquid crystal display element is intended, an opaque substrate such as a silicon wafer can be used for only one of the substrates. In that case, a material such as aluminum that reflects light can be used for the electrodes formed on the substrate.

[0073] Examples of methods for applying the radical-generating film-forming composition include spin coating, printing, inkjet, spraying, and roll coating. From the viewpoint of productivity, the transfer printing method is widely used industrially and is also preferably used in the present invention.

[0074] The drying step after coating the radical-generating film-forming composition is not necessarily required, but when the time from coating to baking is not constant for each substrate, or baking is not performed immediately after coating, it is preferable to include a drying step. This drying is sufficient as long as the solvent is removed to an extent that the coating film shape is not deformed by transportation of the substrate, and the drying method is not particularly limited. For example, a method of drying on a hot plate at a temperature of 40 to 150°C, preferably 60 to 100°C, for 0.5 to 30 minutes, preferably 1 to 5 minutes, can be mentioned.

[0075] The coating formed by applying the radical-generating film-forming composition by the above method, that is, the radical-generating film, can be baked to form a cured film. In this case, the baking temperature can be any temperature between 100 and 350°C, preferably between 140 and 300°C, more preferably between 150 and 230°C, and even more preferably between 160 and 220°C. The baking time can be any time between 5 and 240 minutes, preferably between 10 and 90 minutes, and more preferably between 20 and 90 minutes. Heating can be performed by a commonly known method, such as a hot plate, a hot air circulation oven, an IR (infrared) oven, or a belt furnace.

[0076] The thickness of the radical generating film after curing can be selected as necessary, but it is preferably 5 nm or more, more preferably 10 nm or more, since the reliability of the liquid crystal display element is easily obtained. Also, it is preferable that the thickness of the cured film is 300 nm or less, more preferably 150 nm or less, since the power consumption of the liquid crystal display element does not become extremely large.

[0077] The first substrate having the radical generating film can be obtained in the above manner, and the radical generating film can be subjected to a uniaxial alignment treatment. Methods for performing the uniaxial alignment treatment include photoalignment, oblique deposition, rubbing, and uniaxial alignment treatment using a magnetic field.

[0078] When performing alignment treatment by unidirectional rubbing, for example, a rubbing roller wrapped with a rubbing cloth is rotated while the substrate is moved so that the rubbing cloth comes into contact with the film. In the case of the first substrate of the present invention having a comb-tooth electrode formed thereon, the direction is selected depending on the electrical properties of the liquid crystal, but when a liquid crystal having positive dielectric anisotropy is used, it is preferable that the rubbing direction is substantially the same as the direction in which the comb-tooth electrode extends.

[0079] <Liquid crystal composition containing liquid crystal and radically polymerizable compound> The liquid crystal display element according to the present invention is produced using a liquid crystal composition containing a liquid crystal and a radically polymerizable compound. The polymerizable compound used together with the liquid crystal is not particularly limited as long as it is a radically polymerizable compound, but for example, it is preferable that it is a compound having one or more polymerizable unsaturated bonds in one molecule. It is preferable that it is a compound having one polymerizable unsaturated bond in one molecule (hereinafter, it may be referred to as "a compound having a monofunctional polymerizable reactive group" or "a compound having a monofunctional polymerizable reactive group"). The polymerizable unsaturated bond is preferably a radically polymerizable unsaturated bond, for example, a vinyl bond.

[0080] At least one of the radically polymerizable compounds is preferably a compound having one polymerizable unsaturated bond in one molecule, which is compatible with the liquid crystal, that is, a compound having a monofunctional radically polymerizable group.

[0081] The polymerization reactive group of the radically polymerizable compound is preferably a polymerizable group selected from the following structures. [ka] (In the formula, * indicates a bonding site with a part of the compound molecule other than the polymerizable unsaturated bond. R b represents an alkyl group having 3 to 20 carbon atoms, and E represents a single bond, -O-, or -NR c R represents a linking group selected from -, -S-, an ester bond, and an amide bond. c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; Rb The alkyl group represents a linear, branched, or cyclic alkyl group.

[0082] In addition, in a liquid crystal composition containing liquid crystal and a radically polymerizable compound, it is preferable to contain a radically polymerizable compound that can polymerize the polymer to have a Tg of 100° C. or less.

[0083] The compound having a monofunctional radical polymerization reactive group has an unsaturated bond capable of undergoing radical polymerization in the presence of an organic radical, and examples of the compound include methacrylate monomers such as tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, lauryl methacrylate, and n-octyl methacrylate; acrylate monomers such as tert-butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, benzyl acrylate, lauryl acrylate, and n-octyl acrylate; styrene and styrene derivatives (e.g., o-, m-, and p-methoxystyrene, o-, m-, and p-tert-butoxy ... -chloromethylstyrene, etc.), vinyl esters (e.g., vinyl acetate, vinyl propionate, vinyl benzoate, vinyl acetate, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl hexyl ketone, methyl isopropenyl ketone, etc.), N-vinyl compounds (e.g., N-vinyl pyrrolidone, N-vinyl pyrrole, N-vinyl carbazole, N-vinyl indole, etc.), (meth)acrylic acid derivatives (e.g., acrylonitrile, methacrylonitrile, acrylamide, isopropyl acrylamide, methacrylamide, etc.), vinyl halides (e.g., vinyl chloride, vinylidene chloride, tetrachloroethylene, hexachloropropene, vinyl fluoride, etc.), etc., but are not limited thereto. These various radical polymerizable monomers may be used alone or in combination of two or more. In addition, it is preferable that these have compatibility with the liquid crystal.

[0084] Furthermore, as the radical polymerizable compound, a compound represented by the following formula (A) is also preferred. [ka] In formula (A), R a and R b each independently represents an alkyl group having 3 to 20 carbon atoms, and E represents a single bond, -O-, or -NR c represents a bond selected from -, -S-, an ester bond, and an amide bond; R c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R a or R b The alkyl group represents a linear, branched or cyclic alkyl group.

[0085] As the radical polymerizable compound represented by formula (A), one in which E is an ester bond (a bond represented by -C(=O)-O- or -OC(=O)-) is preferred from the viewpoints of ease of synthesis, compatibility with liquid crystal, and polymerization reactivity. Specifically, a compound having the following structure is preferred, but there is no particular limitation thereon. [ka] In formulas (A-1) and (A-2), R a and R b each independently represents an alkyl group having 3 to 20 carbon atoms; R a and R b The alkyl groups each independently represent a linear, branched or cyclic alkyl group.

[0086] The radical polymerizable compound according to the present invention may have a vertical alignment group. Examples of the vertical alignment group contained in the radically polymerizable compound used in the present invention include a group represented by the following formula [S1]. [ka] In formula [S1], X 1 and X 2 are independently a single bond, -(CH2) a-(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO-, or -((CH2) a1 -A1) m1 - (each of the multiple a1 independently represents an integer of 1 to 15, each of the multiple A1 independently represents an oxygen atom or -COO-, and m1 is 1 or 2). Among them, from the viewpoint of availability of raw materials and ease of synthesis, a single bond, -(CH2) a -(a is an integer of 1 to 15), -O-, -CH2O- or -COO- are preferred. A single bond, -(CH2) a -(a is an integer of 1 to 10), -O-, -CH2O- or -COO-. G 1 and G 2 are independently a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms, any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom, m and n are independently integers of 0 to 3, and the sum of these is 0 to 4, R 1 is an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms, in which any hydrogen atom may be replaced by a fluorine atom, provided that when the sum of m and n is 0, R 1 may be a group having a steroid skeleton. Examples of the divalent aromatic group having 6 to 12 carbon atoms include phenylene, biphenylene, naphthalene, etc. Examples of the divalent alicyclic group having 3 to 8 carbon atoms include cyclopropylene, cyclohexylene, etc.

[0087] Preferred specific examples of the formula [S1] include structures of the following formulae [S1-x1] to [S1-x7]. [ka] In formulas [S1-x1]~[S1-x7], R 1 is an alkyl group having 1 to 20 carbon atoms, and X p is -(CH2) a A1 represents an oxygen atom or -COO-* (wherein the bond marked with "*" is (CH2) a2 A2 is an oxygen atom or *-COO- (where the bond marked with "*" is (CH2) a2 wherein a1 and a3 each independently represent an integer of 0 or 1, a2 represents an integer of 2 to 10, and Cy represents a 1,4-cyclohexylene group or a 1,4-phenylene group.

[0088] Preferred specific examples of the group having a steroid skeleton include those represented by the following formula [S3-x]. [ka] In formula [S3-x], Col represents any one of the above formulae [Col1] to [Col4], and G represents any one of the above formulae [G1] to [G2]. * indicates a bonding position. A preferred embodiment of the radical polymerizable compound according to the present invention is, for example, a radical polymerizable compound having a vertical alignment group in which any of the above radical polymerizable groups is bonded to the above vertical alignment group [S1].

[0089] These various radical polymerizable monomers may be used alone or in combination of two or more kinds. In addition, it is preferable that these have compatibility with the liquid crystal.

[0090] The content of the radically polymerizable compound in the liquid crystal composition is preferably 3 mass % or more, more preferably 5 mass % or more, and preferably 50 mass % or less, more preferably 20 mass % or less, relative to the total mass of the liquid crystal and the radically polymerizable compound.

[0091] Liquid crystal generally refers to a substance that exhibits both solid and liquid properties, and representative liquid crystal phases include nematic liquid crystal and smectic liquid crystal, but the liquid crystal that can be used in the present invention is not particularly limited. One example is 4-pentyl-4'-cyanobiphenyl.

[0092] <Liquid crystal cell> The liquid crystal display element according to the present invention may have, for example, the following cell structure. After forming a radical-generating film on a substrate by the above-mentioned method, a first substrate having the radical-generating film and a second substrate are arranged so that the radical-generating film on the first substrate faces the second substrate, and a liquid crystal composition containing liquid crystal and a radically polymerizable compound is filled between the first substrate and the second substrate to prepare a liquid crystal cell. The liquid crystal display device produced in the present invention can use the liquid crystal cell thus obtained.

[0093] To explain the method for producing the above liquid crystal cell in more detail, the radical generating film on the first substrate is disposed so as to face the second substrate, and then the two substrates are fixed with a sealant via a spacer therebetween, and a liquid crystal composition containing a liquid crystal and a radically polymerizable compound is injected between the first and second substrates and sealed to obtain a liquid crystal cell. In this case, the size of the spacer used is usually 1 to 30 μm, and preferably 2 to 10 μm. The method for injecting the liquid crystal composition containing the liquid crystal and the radical polymerizable compound is not particularly limited, and examples thereof include a vacuum method in which the pressure inside the prepared liquid crystal cell is reduced and then a mixture containing the liquid crystal and the polymerizable compound is injected, and a dropping method in which a mixture containing the liquid crystal and the polymerizable compound is dropped and then sealed.

[0094] It is preferable that an alignment film for aligning liquid crystal is formed on the second substrate. The alignment film may be either a known liquid crystal alignment film or the radical generating film according to the present invention, and can be appropriately selected depending on the purpose. The alignment film formed on the second substrate can be subjected to a uniaxial alignment treatment. As described later, for example, when an out-of-plane alignment region is to be formed in a liquid crystal display element, it is preferable to form a radical generating film on the second substrate. Furthermore, for example, when an in-plane alignment region or an inclined alignment region is to be formed in a liquid crystal display element, it is preferable to form a liquid crystal alignment film for horizontal alignment that has been subjected to uniaxial alignment treatment on the second substrate.

[0095] <Formation of in-plane alignment, out-of-plane alignment, and tilt alignment regions> Using substrates on which a radical-generating film is formed, a liquid crystal cell in which a mixture (liquid crystal composition) containing liquid crystal and a radically polymerizable compound is placed between the substrates is irradiated with light sufficient to cause a polymerization reaction of the radically polymerizable compound. In this way, the present invention forms a radical generating film having an anchoring power on a substrate, and in a state where the radical generating film is in contact with a liquid crystal containing a specific polymerizable compound, light is irradiated onto the radical generating film in an area where the anchoring power is to be maintained. The liquid crystal is vertically oriented by polymerization of the polymerizable compound, and as a result, an out-of-plane oriented (vertical oriented) area is formed in the area irradiated with light.

[0096] The light to be irradiated here may have a peak at 240 to 400 nm. It is preferable to irradiate light having a wavelength that increases the absorbance of the portion corresponding to the photoradical generation site, and the light is more preferably light having a peak at 250 to 365 nm, and even more preferably light having a peak at 250 to 360 nm. More specifically, for example, light having a peak near 313 nm can be used. If necessary, light of a specific wavelength or light having a wavelength equal to or greater than a specific wavelength can be cut using a known cut filter. The amount of light irradiation is usually 0.01 to 30 J, but is preferably 10 J or less. A smaller amount of light irradiation is preferable because it can suppress deterioration in reliability due to damage to members constituting the liquid crystal display element, and also because it can reduce the light irradiation time, thereby improving the tact time in manufacturing.

[0097] The heating temperature during light irradiation is preferably within a temperature range where the introduced liquid crystal exhibits liquid crystallinity, and is usually 40° C. or higher, and is preferably below the temperature at which the liquid crystal changes to an isotropic phase.

[0098] In addition, it is preferable that the light irradiation for polymerizing the radical polymerizable compound is performed in a state without applying a voltage and without applying an electric field.

[0099] On the other hand, when irradiating a liquid crystal cell with light, if a photomask is placed on the outside of the liquid crystal cell and light is irradiated through the photomask, an in-plane alignment (horizontal alignment) region will be formed in the unexposed area (= area where radicals are not generated), and an out-of-plane alignment (vertical alignment) region will be formed in the exposed area, as described above. The pattern shape and pattern size of the photomask to be used are not particularly limited and can be appropriately selected according to the purpose. The pattern shape can be, for example, a line pattern shape, a line / space (L / S) pattern shape, a dot shape, etc. The pattern size can be a micrometer size pattern, and for example, when a photomask having an L / S pattern shape with a 5 μm pitch is used, an orientation pattern with a 5 μm pitch can be formed.

[0100] Furthermore, an in-plane alignment (horizontal alignment) region can also be formed by irradiating the radical generating film with light before assembling the liquid crystal cell to inactivate the radical generating ability of the radical generating film. By irradiating the radical generating film with light in advance, the radical generating ability can be eliminated, and the anchoring strength in the in-plane direction can be maintained throughout. In other words, even if a liquid crystal cell is produced using a radical generating film whose radical generating ability has been inactivated and the liquid crystal cell is irradiated with light, an in-plane alignment (horizontal alignment) region is formed in the region where the radical generating ability has been inactivated. The light used to deactivate the radical generating ability of the radical generating film may be light having a peak at 240 to 400 nm. The light is more preferably light having a peak at 250 to 365 nm, and even more preferably light having a peak at 250 to 360 nm. More specifically, for example, light having a peak near 313 nm may be used. If necessary, a known cut filter may be used to cut off light of a specific wavelength or light above or below a specific wavelength. The amount of light irradiation is usually 0.01 to 30 J, but is preferably 10 J or less.

[0101] In order to obtain good in-plane alignment of the liquid crystal in the unexposed area and the area where the radical generating ability has been deactivated, it is preferable that the radical generating film has been subjected to a uniaxial alignment treatment. In order to obtain good in-plane alignment of the liquid crystal in the unexposed area or the area where the radical generating ability has been deactivated, it is preferable that the polymer contained in the radical generating film-forming composition in the radical generating film does not contain a moiety having vertical alignment function.

[0102] As described above, when forming an out-of-plane alignment region using a radical generating film, a cell is prepared using both first and second substrates on which a radical generating film is formed, a liquid crystal composition containing a predetermined radical polymerizable compound is injected, and then light is irradiated from outside the cell to polymerize the polymerizable compound and vertically align the liquid crystal. On the other hand, when a radical generating film is used to form an in-plane alignment region, the first and second substrates on which the radical generating film is formed may be irradiated with light before cell assembly to inactivate the radical generating ability, and then the cell may be assembled, so that the interfacial reaction can be suppressed even if the liquid crystal cell after formation is irradiated with light. Alternatively, a liquid crystal cell prepared without inactivating the radical generating ability can be provided with a photomask on the outside of the liquid crystal cell and irradiated with light through the photomask, thereby preventing radicals from being generated in the unexposed areas and preventing the interfacial reaction from being induced.

[0103] In a liquid crystal display element, In-plane and out-of-plane orientation By fabricating a liquid crystal cell so that the two molecules face each other, a tilted alignment region can be formed. For example, when the radical generating film is used for both the first substrate and the second substrate, Methods for forming out-of-plane alignment and methods for forming in-plane alignment By appropriately combining these, a tilted alignment region can be created. More specifically, for example, a radical generating film is used on one of the first substrate and the second substrate, Forming an out-of-plane orientation, The other substrate is a radical generating film whose radical generating ability has been deactivated. Formation of in-plane orientation By this, a tilted alignment region can be formed.

[0104] Alternatively, a radical generating film may be used on one of the first and second substrates, and a liquid crystal alignment film without radical generating ability may be used on the other substrate. When a liquid crystal alignment film without radical generating ability is used on the other substrate, either an in-plane alignment film or an out-of-plane alignment film may be used as the liquid crystal alignment film. In-plane and out-of-plane orientation By combining with the production method, a variety of patterns can be formed consisting of various combinations of in-plane alignment regions, tilted alignment regions, and out-of-plane alignment regions. The liquid crystal alignment film is preferably subjected to uniaxial alignment treatment.

[0105] In addition, in the manufacturing method of the liquid crystal display element of the present invention, by adjusting the content of the radical polymerizable compound contained in the liquid crystal composition and the amount of irradiation when irradiating the liquid crystal cell with light, the liquid crystal can be aligned at an angle rather than vertically, thereby forming an inclined alignment region. As described above, according to the method for manufacturing a liquid crystal display element of the present invention, it is possible to manufacture a liquid crystal display element having a radical-generating film, in which at least two regions among the in-plane alignment region, the out-of-plane alignment region, and the tilt alignment region are patterned.

[0106] <Liquid crystal display element> According to the manufacturing method of the present invention, a liquid crystal display element having at least two patterned regions selected from an in-plane alignment region, an out-of-plane alignment region, and an inclined alignment region can be industrially produced with a high yield. Therefore, the liquid crystal display element manufactured by the manufacturing method of the present invention can be widely used in practical applications. For example, by providing a reflective electrode, a transparent electrode, a λ / 4 plate, a polarizing film, a color filter layer, etc., in the liquid crystal cell according to a conventional method, it can be used as a reflective liquid crystal display element. Furthermore, by providing the liquid crystal cell with a backlight, a polarizing plate, a λ / 4 plate, a transparent electrode, a polarizing film, a color filter layer, etc., according to a conventional method, the liquid crystal cell can be used as a transmission type liquid crystal display element. FIG. 10 is a schematic cross-sectional view showing an example of a liquid crystal display element according to the present invention, which is an example of an IPS mode liquid crystal display element. In a liquid crystal display element 101 illustrated in Fig. 10, a liquid crystal composition 103 is sandwiched between a comb-tooth electrode substrate 102 having a radical-generating film 102c and a counter substrate 104 having a liquid crystal alignment film 104a. The comb-tooth electrode substrate 102 has a base material 102a, a plurality of linear electrodes 102b formed on the base material 102a and arranged in a comb-tooth shape, and a radical-generating film 102c formed on the base material 102a so as to cover the linear electrodes 102b. The counter substrate 104 has a base material 104b and a liquid crystal alignment film 104a formed on the base material 104b. In this liquid crystal display element 101, when a voltage is applied to the linear electrodes 102b, an electric field is generated between the linear electrodes 102b as indicated by electric force lines L. FIG. 11 is a schematic cross-sectional view showing another example of the liquid crystal display element according to the present invention, which is an example of an FFS mode liquid crystal display element. In the liquid crystal display element 101 illustrated in Fig. 11, a liquid crystal composition 103 is sandwiched between a comb-tooth electrode substrate 102 having a radical-generating film 102h and a counter substrate 104 having a liquid crystal alignment film 104a. The comb-tooth electrode substrate 102 has a base material 102d, a plane electrode 102e formed on the base material 102d, an insulating film 102f formed on the plane electrode 102e, a plurality of linear electrodes 102g formed on the insulating film 102f and arranged in a comb-tooth shape, and a radical-generating film 102h formed on the insulating film 102f so as to cover the linear electrodes 102g. The counter substrate 104 has a base material 104b and a liquid crystal alignment film 104a formed on the base material 104b. In this liquid crystal display element 101, when a voltage is applied to the surface electrodes 102e and the linear electrodes 102g, an electric field is generated between the surface electrodes 102e and the linear electrodes 102g, as indicated by electric force lines L. EXAMPLES

[0107] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0108] In the examples, the abbreviations and property evaluation methods of the compounds used in the polymerization of the polymers and the preparation of the radical-generating film-forming compositions are as follows.

[0109] [ka] [ka]

[0110] NMP: N-methyl-2-pyrrolidone, BCS: Butyl cellosolve

[0111] <Viscosity measurement> The viscosity of the polyamic acid solution at 25° C. was measured using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample amount of 1.1 mL and a cone rotor TE-1 (1°34′, R24).

[0112] <Molecular weight measurement> The molecular weight was measured by a room temperature GPC (gel permeation chromatography) device, and the number average molecular weight (Mn) and weight average molecular weight (Mw) were calculated as polyethylene glycol and polyethylene oxide equivalent values. GPC apparatus: GPC-101 (Showa Denko K.K.), column: GPC KD-803, GPC KD-805 (Showa Denko K.K.) in series, column temperature: 50℃, eluent: N,N-dimethylformamide (additives: lithium bromide monohydrate (LiBr·H2O) 30mmol / L, phosphoric acid·anhydrous crystal (o-phosphoric acid) 30mmol / L, tetrahydrofuran (THF) 10mL / L), flow rate: 1.0mL / min. Standard samples for preparing a calibration curve: TSK standard polyethylene oxide (molecular weight: approximately 900,000, 150,000, 100,000, and 30,000) (manufactured by Tosoh Corporation) and polyethylene glycol (molecular weight: approximately 12,000, 4,000, and 1,000) (manufactured by Polymer Laboratory Co., Ltd.).

[0113] <Measurement of imidization rate> 20 mg of polyimide powder was placed in an NMR sample tube (Kusano Scientific NMR Sampling Tube Standard φ5), 0.53 mL of deuterated dimethyl sulfoxide (DMSO-d6, 0.05 mass% TMS (tetramethylsilane) mixture) was added, and the mixture was sonicated to completely dissolve. The 500 MHz proton NMR of this solution was measured using a measuring device (JNW-ECA500, manufactured by JEOL Datum Co., Ltd.). The imidization rate was determined by determining a proton derived from a structure that does not change before and after imidization as a reference proton, and using the peak integrated value of this proton and the peak integrated value of a proton derived from the NH of an amide group appearing in the vicinity of 9.5 to 10.0 ppm, according to the following formula. Imidization rate (%) = (1-α·x / y) × 100 In the formula, x is the integrated value of the proton peak derived from the NH of the amide group, y is the integrated value of the peak of the reference proton, and α is the ratio of the number of reference protons to one NH proton of the amide group in the case of polyamic acid (imidization rate 0%).

[0114] (Synthesis of compound DA-4) Compound DA-4 was obtained by the following method. [ka] <1st process> 4,4'-dinitro-[1,1'-biphenyl]-2,2'-dicarboxylic acid (20.0g, 60.2mmol) was charged with tetrahydrofuran (120g), 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (28.4g, 126mmol), 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (28.0g, 181mmol), and N,N-dimethylaminopyridine (0.735g, 6.02mmol), and stirred at room temperature overnight. After the reaction was completed, the mixture was extracted twice with water / chloroform, and the obtained organic phase was concentrated to obtain a syrup-like brown oil. This was purified by column chromatography using a mixed solvent of ethyl acetate / hexane = 3 / 1 (volume ratio). When the obtained fraction was concentrated, it became a yellow transparent oil, and when it was left to stand, white crystals precipitated from the oil. The precipitated crystals were slurry washed with a mixed solvent of ethyl acetate / hexane=3 / 1 (volume ratio), filtered, and the crystals were dried to obtain compound (DA-4-1) (yield: 29.8 g, 40.0 mmol, 67% yield). 1 H-NMR(500MHz) in DMSO-d6:8.57(d,J=2.5Hz,2H),8.37(dd,J=8.5Hz,2.5Hz,2H),8.18(d,J=9.0Hz,4H),7.55(d,J=8.5Hz,2H), 6.85(d,J=9.0Hz,4H),5.631(s,2H),4.39-4.35(m,4H),4.02-3.99(m,2H),3.96-3.94(m,2H),1.40(s,12H).

[0115] <Second process> To the compound (DA-4-1) (29.8g, 40.0mmol) obtained in the first step, tetrahydrofuran (240g) was added, and the atmosphere was replaced with nitrogen. Then, 3% platinum carbon (wet product) (2.38g) was added, and the mixture was further replaced with nitrogen. A hydrogen Tedlar bag was attached and the mixture was stirred at room temperature for about 17 hours. After the reaction was completed, the mixture was passed through a membrane filter to remove the platinum carbon, and then concentrated and dried to obtain compound (DA-4) (yield: 27.4g, 40.0mmol, quant). 1 H-NMR(500MHz) in DMSO-d6:8.20(dd,J=7.1Hz,1.9Hz,4H),6.99(d,J=2.5Hz,2H),6.92(dd,J=7.3Hz,1.9Hz,4H),6 .80(d,J=8.2Hz,2H),6.67(dd,J=8.2Hz,2.5Hz,2H),5.64(s,2H),5.24(s,4H),4.22(t,J=4.5Hz, 4H),4.00(br,4H),1.39(s,12H).

[0116] (Polymerization of Polymers and Preparation of Radical-Generating Film-Forming Compositions) <Synthesis Example 1> Synthesis of TC-1(50)TC-2(50) / DA-1(70)DA-2(30) polyimides In a 100mL four-neck flask equipped with a nitrogen inlet tube, an air-cooled tube, and a mechanical stirrer, 3.78g (35.0mmol) of DA-1 and 4.96g (15.0mmol) of DA-2 were weighed out, 35.0g of NMP was added, and the mixture was stirred under a nitrogen atmosphere to completely dissolve. After confirming dissolution, 6.26g (25.0mmol) of TC-2 and 25.0g of NMP were added, and the mixture was heated and stirred at 60°C for 3 hours under a nitrogen atmosphere. Then, 4.12g (21.0mmol) of TC-1 and 16.5g of NMP were added, and the mixture was stirred at room temperature for 12 hours. The polymerization viscosity was confirmed, and further TC-1 was added so that the polymerization viscosity was 1000mPa·s, and a polymerization liquid with a polyamic acid concentration of 20% by mass was obtained. 50.0 g of the polyamic acid solution obtained above was weighed out into a 200 mL Erlenmeyer flask equipped with a magnetic stirrer, 92.9 g of NMP was added to prepare a solution with a solid concentration of 7 mass%, and 10.6 g (103 mmol) of acetic anhydride and 3.28 g (41.4 mmol) of pyridine were added while stirring, and after stirring at room temperature for 30 minutes, the solution was heated and stirred at 60 ° C for 3 hours. After that, the solution was returned to room temperature and poured into 500 mL of methanol while stirring to precipitate a solid. This operation was repeated twice, and then air-dried and dried in a vacuum oven set at 60 ° C to obtain a polyimide powder (PI-1) with Mn of 11,453, Mw of 27,655, and an imidization rate of 67.0%.

[0117] <Synthesis Example 2> Synthesis of TC-1(50)TC-2(50) / DA-1(50)DA-2(50) polyimides A polyimide powder (PI-2) was obtained in the same manner as in Synthesis Example 1, except that the amount of the monomer used was changed as shown in Table 1. The Mn of this polyimide powder was 21,959, the Mw was 67,088, and the imidization rate was 62.2%.

[0118] <Synthesis Example 3> Synthesis of TC-1(50)TC-2(50) / DA-2(100) polyimides A polyimide powder (PI-3) was obtained in the same manner as in Synthesis Example 1, except that the amount of the monomer used was changed as shown in Table 1. The polyimide powder had an Mn of 21,959, an Mw of 67,088, and an imidization rate of 72.0%.

[0119] <Synthesis Example 4> Polymerization of TC-3(100) / DA-3(50) / DA-4(50) polyamic acid 2.44g (10.00mmol) of DA-3 and 6.85g (10.00mmol) of DA-4 were weighed out into a 100mL four-neck flask equipped with a nitrogen inlet tube, an air-cooled tube, and a mechanical stirrer, and 52.6g of NMP was added and stirred under a nitrogen atmosphere to completely dissolve. After confirming dissolution, 4.21g (18.80mmol) of TC-3 and 23.9g of NMP were added and heated and stirred at 40°C for 12 hours under a nitrogen atmosphere. The polymerization viscosity was confirmed, and further TC-3 was added so that the polymerization viscosity became 400mPa·s, and a polymerization liquid (PAA-1) with a polyamic acid concentration of 15% by mass was obtained. The Mn of this polyamic acid was 16,331 and the Mw was 42,999.

[0120] <Synthesis Example 5> Synthesis of AC-1(40) and AC-2(60) polymethacrylates In a 100mL four-neck flask equipped with a nitrogen inlet tube, an air-cooled tube, and a mechanical stirrer, 5.00g (15.0mmol) of AC-1, 6.91g (22.6mmol) of AC-2, and 0.185g (1.13mmol) of AIBN were weighed out, 67.5g of NMP was added, and the mixture was stirred under a nitrogen atmosphere to completely dissolve. After vacuum degassing, the solution was heated and stirred at 60°C under a nitrogen atmosphere for 12 hours. The solution was then returned to room temperature and poured into 300mL of methanol with stirring to precipitate a solid. This operation was repeated twice, and then the mixture was air-dried and dried in a vacuum oven set at 60°C to obtain a polymethacrylate powder (PMA-1) with Mn of 37,197 and Mw of 116,919.

[0121] <Preparation of radical-generating film-forming composition: AL-1> 0.90 g of the polyimide powder (PI-1) obtained in Synthesis Example 1 was weighed out into a 15 mL vial equipped with a magnetic stirrer, 5.10 g of NMP was added, and the mixture was heated and stirred at 50° C. to obtain a polymer solution with a solid content concentration of 15% by mass. 6.00 g of NMP and 3.00 g of BCS were added thereto, and the mixture was further stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-1 (solid content: 6.0% by mass, NMP: 74% by mass, BCS: 20% by mass).

[0122] <Preparation of radical-generating film-forming composition: AL-2> Using the polyimide powder (PI-2) obtained in Synthesis Example 2, a radical-generating film-forming composition according to the present invention: AL-2 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%) was obtained in the same manner as in the preparation of AL-1.

[0123] <Preparation of radical-generating film-forming composition: AL-3> Using the polyimide powder (PI-3) obtained in Synthesis Example 3, a radical-generating film-forming composition according to the present invention: AL-3 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%) was obtained in the same manner as in the preparation of AL-1.

[0124] <Preparation of radical-generating film-forming composition: AL-4> 6.00 g of the polyamic acid (PAA-1) obtained in Synthesis Example 4 was weighed out into a 15 mL vial equipped with a magnetic stirrer, 6.00 g of NMP and 3.00 g of BCS were added, and the mixture was stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-4 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%).

[0125] <Preparation of radical-generating film-forming composition: AL-5> 0.27 g of the polymethacrylate powder (PMA-1) obtained in Synthesis Example 5 and 0.63 g of the polyimide powder (PI-3) obtained in Synthesis Example 3 were weighed out into a 15 mL vial equipped with a magnetic stirrer, 5.10 g of NMP was added, and the mixture was heated and stirred at 60° C. to obtain a polymer solution with a solid content concentration of 15% by mass. 6.00 g of NMP and 3.00 g of BCS were added thereto and further stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-5 (solid content: 6.0% by mass, NMP: 74% by mass, BCS: 20% by mass).

[0126] <Preparation of radical-generating film-forming composition: AL-6> 0.45 g of the polymethacrylate powder (PMA-1) obtained in Synthesis Example 5 and 0.45 g of the polyimide powder (PI-3) obtained in Synthesis Example 3 were weighed out into a 15 mL vial equipped with a magnetic stirrer, 5.10 g of NMP was added, and the mixture was heated and stirred at 60° C. to obtain a polymer solution with a solid content concentration of 15% by mass. 6.00 g of NMP and 3.00 g of BCS were added to the mixture, and the mixture was further stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-6 (solid content: 6.0% by mass, NMP: 74% by mass, BCS: 20% by mass).

[0127] <Preparation of non-radical generating film-forming composition: AL-7> Using the polymethacrylate powder (PMA-1) obtained in Synthesis Example 5, a non-radical-generating film-forming composition for comparison of the present invention: AL-7 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%) was obtained in the same manner as in the preparation of AL-1.

[0128] The compositions of the polyamic acid and polyimide are shown in Table 1 below. [Table 1]

[0129] The composition of the polymethacrylate is shown in Table 2 below. [Table 2]

[0130] The compositions of the radical-generating film-forming composition and the non-radical-generating film-forming composition are shown in Table 3 below. [Table 3]

[0131] The composition of the liquid crystal species is shown in Table 4 below. [Table 4]

[0132] (polymerizable compound) The polymerizable compounds (additives) shown in Table 4 were obtained as follows. <Polymerizable compound synthesis example 1> Synthesis of didodecyl itaconate (IC-12) [ka] 30.0 g (231 mmol) of itaconic acid and 81.6 g (438 mmol) of 1-dodecanol were weighed into a four-neck flask equipped with a Dean-Stark tube and completely dissolved in cyclohexane (700 mL). After confirming that the solution had dissolved, 1.13 g (11.5 mmol) of concentrated sulfuric acid and 0.51 g (2.31 mmol) of dibutylhydroxytoluene (BHT) were added and the mixture was heated and stirred at 120°C for 24 hours under a nitrogen atmosphere. Nuclear magnetic resonance spectrum ( 1 After confirming the completion of the reaction using H-NMR spectrum, 100 mL of n-hexane was added to the reaction solution, which was then washed three times with 100 g of 10% aqueous sodium carbonate solution and three times with 100 mL of pure water, and dried over anhydrous magnesium sulfate. After filtration and concentration, the mixture was dried in vacuum to obtain 78.0 g (167 mmol: yield 76.3%) of a white solid. The structure is 1 The H-NMR spectrum confirmed that the product was the desired product. The measurement data are shown below. 1 H-NMR(400MHz,CDCl3)δ:6.30(1H), 5.65(1H), 4.20-4.00(4H), 3.32(2H), 1.64-1.58(4H), 1.40-1.25(36H), 0.96-0.83(6H)

[0133] <Polymerizable compound synthesis example 2> Synthesis of dihexylacrylamide (AAA-C6C6) [ka] 33.3g (180mmol) of dihexylamine and 27.3g (270mmol) of triethylamine were weighed out into a four-neck flask, and 500mL of THF was added and completely dissolved at room temperature. After confirming dissolution, the reaction vessel was cooled with ice to keep the system at 0°C, and 17.9g (198mmol) of acrylic acid chloride was gently added dropwise. Nuclear magnetic resonance spectrum ( 1 After confirming the completion of the reaction using H-NMR spectrum, 100 mL of ethyl acetate was added to the reaction solution, which was then washed three times with 100 g of 10% aqueous sodium carbonate solution and three times with 100 mL of pure water, and dried over anhydrous magnesium sulfate. After filtration and concentration, the mixture was dried in vacuum to obtain 33.6 g (140 mmol: yield 78.1%) of a transparent oily liquid. The structure is 1 The H-NMR spectrum confirmed that the product was the desired product. The measurement data are shown below. 1 H-NMR(400MHz,DMSO-d6)δ:6.62(1H), 6.04(1H), 5.58(1H), 3.20-4.00(4H), 3.35-3.25(4H), 1.64-1.58(4H), 1.30-1.25(12H), 0.96-0.83(6H)

[0134] <Polymerizable compound synthesis example 3> Synthesis of 4-amylcyclohexyl methacrylate (MACH-C5) [ka] 25.0 g (147 mmol) of 4-amylcyclohexanol and 22.3 g (220 mmol) of triethylamine were weighed out in a four-neck flask, and 400 mL of THF was added and completely dissolved at room temperature. After confirming dissolution, the system was kept at 0°C in an ice bath, and 18.4 g (176 mmol) of methacrylic acid chloride was gently added dropwise. Nuclear magnetic resonance spectrum ( 1 After confirming the completion of the reaction using H-NMR spectrum, 100 mL of hexane was added to the reaction solution, which was then washed three times with 100 g of 10% aqueous sodium carbonate solution and three times with 100 mL of pure water, and dried over anhydrous magnesium sulfate. After filtration and concentration, the mixture was dried in vacuum to obtain 20.3 g (86.2 mmol: yield 58.0%) of a transparent oily liquid. The structure is1 It was confirmed that it was the target substance by the 1H-NMR spectrum. The measurement data are shown below. 1 1H-NMR (400 MHz, DMSO-d6) δ: 6.15 - 5.95 (1H), 5.65 - 5.60 (1H), 4.95 - 4.90 (0.60H), 4.65 - 4.57 (0.40H), 1.89 - 1.86 (3H), 1.79 - 1.74 (2H), 1.56 - 1.50 (2H), 1.36 - 1.15 (11H), 0.87 - 0.84 (3H)

[0135] <Purchase of polymerizable compound> The polymerizable compound DMA was used as purchased from Tokyo Chemical Industry Co., Ltd. (TCI).

[0136] (Fabrication of liquid crystal display element) Using AL-1 to AL-7 obtained above and SE-6414 and NRB-U438 (manufactured by Nissan Chemical Industries, Ltd.), which are liquid crystal alignment agents for horizontal alignment, a liquid crystal cell was fabricated, and a liquid crystal display element having the configuration shown in Table 5 below was fabricated.

[0137] The configuration of the liquid crystal cell is shown in Table 5 below.

Table 5

[0138] <First and second substrates> The first and second substrates are non-alkali glass substrates with a size of 30 mm × 40 mm and a thickness of 1.1 mm. An ITO (Indium-Tin-Oxide) electrode with a thickness of 10 μm is formed on the substrate. The first substrate and the second substrate are the same substrate, and the names are separated for convenience.

[0139] <Surface treatment process of AL-1, AL-2, AL-3, SE-6414> AL-1, AL-2, AL-3, and SE-6414 were filtered through a filter with a pore size of 1.0 μm, then applied to the electrode-forming surfaces of the first and second substrates by spin coating, and dried on a hot plate at 80°C for 2 minutes. Subsequently, they were baked in a thermal circulation heating furnace with an internal temperature of 230°C for 30 minutes to obtain a coating film with a thickness of 100 nm. The first and second substrates with the obtained coating films were subjected to rubbing treatment. The first substrate was rubbed with the rubbing direction from the longitudinal direction, and the second substrate was rubbed with the rubbing direction from the short-side direction so that the rubbing directions would be anti-parallel after lamination. As the rubbing cloth type, a rayon cloth: YA-20R manufactured by Yoshikawa Chemical Industry Co., Ltd. with a roll diameter of 120 mm was used. The rubbing treatment of AL-1, AL-2, and AL-3 was carried out under the conditions of a rotation speed of 500 rpm, a moving speed of 30 mm / sec, and a pressing amount of 0.3 mm. Also, the rubbing treatment of SE-6414 was carried out under the conditions of a rotation speed of 1000 rpm, a moving speed of 20 mm / sec, and a pressing amount of 0.4 mm. After the rubbing treatment, ultrasonic cleaning was performed in pure water for 1 minute and dried at 80°C for 15 minutes.

[0140] <Surface treatment process of AL-4, AL-5, AL-6, AL-7, NRB-U438> AL-5, AL-6, and AL-7 were filtered through a filter with a pore size of 1.0 μm, then applied to the electrode-forming surfaces of the first and second substrates by spin coating, and dried on a hot plate at 70°C for 90 seconds. After that, using a high-pressure mercury lamp (313 nm band-pass filter manufactured by Thermo Precision Co., Ltd.), linearly polarized light with a wavelength of 313 nm was irradiated at 0.005 J / cm 2 and then baked on a hot plate at 150°C for 30 minutes. AL-4 and NRB-U438 were filtered through a filter with a pore size of 1.0 μm, then applied to the electrode-forming surfaces of the first and second substrates by spin coating, dried on a hot plate at 80°C for 2 minutes, and baked in a thermal circulation heating furnace with an internal temperature of 230°C for 30 minutes. After that, using a low-pressure mercury lamp (240 nm or less short-wavelength cut filter manufactured by Ushio Electric Inc.), linearly polarized light with a wavelength of 254 nm was irradiated at 0.3 J / cm 2After exposure, the film was baked in a heat circulation oven at an internal temperature of 230° C. for 30 minutes.

[0141] <First exposure> After the surface treatment process, two types of substrates (first and second substrates) with liquid crystal alignment films were irradiated with light of 313 nm wavelength at 10 J / cm using a high-pressure mercury lamp (thermoprecision 300 nm or less short wavelength cut filter). 2 When selective light irradiation was required, a photomask (100, 50, 30, and 5 μm L / S with chrome wiring, manufactured by Mitani Micronics) was placed on the substrate and pattern exposure was performed. Hereafter, this operation is referred to as the primary exposure. The primary exposure was performed for the purpose of intentionally deactivating groups capable of generating radicals contained in the alignment film, and was applied only to Examples 23, 24, 27, 28, 29, 30, and 32.

[0142] <Preparation of liquid crystal cell> For Examples 23, 24, 27, 28, 29, 30, and 32, two types of substrates (first and second substrates) with liquid crystal alignment films that had been subjected to the first exposure process were used, and the periphery was sealed except for a liquid crystal injection port to prepare empty cells with a cell gap of approximately 4 μm. For those that included a rubbing treatment in the surface treatment process, the empty cells were prepared so that the rubbing directions of the first substrate and the second substrate were anti-parallel. Liquid crystal (as shown in Table 4, Merck's positive liquid crystal for IPS MLC-3019 or Merck's negative liquid crystal for IPS MLC-7026 with the specified amount of additives added to the liquid crystal) was injected into this empty cell under vacuum at room temperature, and the injection port was then sealed to form a liquid crystal cell. The obtained liquid crystal cell constitutes an IPS mode liquid crystal display element. The obtained liquid crystal cell was then subjected to a heat treatment at 120°C for 10 minutes.

[0143] <Secondary exposure> The prepared liquid crystal cell was irradiated with light of 313 nm wavelength using a high pressure mercury lamp (Therma Precision, 300 nm or less short wavelength cut filter). The irradiation amount is as shown in Table 5. When it was desired to selectively irradiate light, a photomask (Mitani Micronics, 100, 50, 30, 5 μm L / S with chrome wiring) was placed on the liquid crystal cell and pattern exposure was performed. Hereinafter, this operation is referred to as secondary exposure. The purpose of the secondary exposure is to promote the reaction between the radical-generating groups contained in the alignment film and the polymerizable compound (additive) in the liquid crystal.

[0144] (Results of visual evaluation of liquid crystal alignment after secondary exposure) The alignment state of the liquid crystal cell after the secondary exposure was confirmed using polarizing plates arranged in a crossed Nicol configuration. The angle between the uniaxial alignment direction of the liquid crystal and the polarization direction was set to 45 degrees. At this time, if the liquid crystal is uniaxially aligned, light is transmitted, and if it is out-of-plane aligned, light is not transmitted. As an example, since the cell 7 (Example 5) was capable of controlling the out-of-plane orientation, the exposed area became a dark field (FIGS. 1A and 1B). FIG. 1A shows a photograph of a liquid crystal display element, and FIG. 1B shows a schematic diagram of the photograph of the liquid crystal display element of FIG. 1A (hereinafter, in the same manner as in FIG. 2 to FIG. 5 and FIG. 9, a photograph of the liquid crystal display element is shown in FIG. A, and a schematic diagram of the photograph is shown in FIG. B). In FIG. 1 (FIGS. 1A and 1B are also collectively referred to as FIG. 1), the exposed area indicated by reference numeral 1 represents a dark field (black), and the unexposed area indicated by reference numeral 2 represents a bright field (white). In Cell 27 (Comparative Example 4), the out-of-plane orientation could not be controlled, and the exposed area was a bright field (FIGS. 2A and 2B). In FIG. 2 (FIG. 2A and FIG. 2B are also collectively referred to as FIG. 2), both the exposed and unexposed areas showed bright fields (white). Cell 1 (Example 1) had a tilted alignment (partially out-of-plane alignment), and therefore the exposed area showed reduced coloring (partially dark field) and showed a neutral gray color (FIGS. 3A and 3B). In Figure 3 (Figures 3A and 3B are also collectively referred to as Figure 3), the exposed area indicated by reference number 1 was a mixture of dark field (black) b area and intermediate color (gray) a area. The non-exposed area indicated by reference number 2 showed bright field (white).

[0145] The liquid crystal display elements of the examples and comparative examples shown in Tables 6 to 8 below were also evaluated in the same manner as shown in FIGS. In Tables 6 to 8, the secondary exposure area was marked with a dark field (black) and was marked with an ◯ for which out-of-plane orientation control was possible, a × for which out-of-plane orientation control was not possible and a △ for which the secondary exposure area was marked with an intermediate color (gray) and was marked with a uniaxial orientation with a tilt angle or a non-uniform orientation.

[0146] The results of the visual evaluation of the liquid crystal alignment after the secondary exposure are shown in Table 6 below. [Table 6] In order to induce out-of-plane alignment from an in-plane uniaxial alignment state, it is necessary to (i) include radical-generating groups in the alignment film, (ii) include a polymerizable compound (additive) in the liquid crystal, and (iii) irradiate light. In this case, in order to form a good out-of-plane alignment state, it is effective to take into consideration the content of radical-generating groups, the content of polymerizable compounds, the amount of light irradiation, etc.

[0147] The results of the visual evaluation of the liquid crystal alignment after the secondary exposure are shown in Table 7 below. [Table 7] The polymerizable compound (additive) required for out-of-plane alignment control is not limited to DMA. Any additive with an appropriate structure can control out-of-plane alignment. In addition, the liquid crystal type is not limited to MLC-7026, which is a liquid crystal with a negative dielectric constant, and out-of-plane alignment control is possible even with MLC-3019, which is a liquid crystal with a positive dielectric constant.

[0148] The results of the visual evaluation of the liquid crystal alignment property after the secondary exposure are shown in Table 8 below. [Table 8] When a photo-alignment film that has been photo-aligned is used, out-of-plane alignment control is possible, and does not depend on the type of polymer constituting the alignment film or the exposure wavelength required for photo-alignment. Furthermore, as shown in the liquid crystal cells 22 and 23 used in Examples 19 and 20, when an alignment film material that does not have a radical-generating group is used, out-of-plane alignment control is possible by mixing a polymer material that has a radical-generating group. In this case, out-of-plane alignment control is possible if an appropriate amount of radical-generating groups is introduced. In addition, out-of-plane alignment control may be possible even when a photo-alignment film having radical generating ability is applied only to the first substrate as in Examples 21 and 22. This depends on the type of photo-alignment film used, and is seen, for example, when the alignment regulating force of the liquid crystal is small or when the alignment regulating force of the liquid crystal is reduced by irradiation with light.

[0149] (Results of visual evaluation of liquid crystal alignment when applying primary exposure) The alignment state of the liquid crystal cell after the secondary exposure was confirmed using polarizing plates arranged in a crossed Nicol position. The angle between the uniaxial alignment direction of the liquid crystal cell and the polarization direction was set to 45 degrees. The results are shown in Table 9 below.

[0150] [Table 9] When the entire surface of only the first substrate was exposed as the primary exposure, a tilted alignment was formed (FIGS. 4A and 4B). In Figure 4 (Figures 4A and 4B are also collectively referred to as Figure 4), the part indicated by the symbol 3 is a region where only the first substrate was exposed in the primary exposure and the entire surface was exposed in the secondary exposure. The part indicated by the symbol 3 shows an intermediate gray color, and a tilted alignment was formed. The part indicated by the symbol 4 is a non-exposed region where only the first substrate was exposed in the primary exposure and was not exposed in the secondary exposure. The part indicated by the symbol 4 shows a bright field (white color), and an in-plane alignment was formed. When the first and second substrates were blanket exposed in a first exposure, in-plane alignment was formed (FIGS. 5A and 5B). In FIG. 5 (FIG. 5A and FIG. 5B are collectively referred to as FIG. 5), the portion indicated by the symbol 5 is the region in which the first and second substrates were exposed in the primary exposure and then fully exposed in the secondary exposure. The portion indicated by the symbol 6 is the non-exposed region in which the first and second substrates were exposed in the primary exposure and not exposed in the secondary exposure. Both the portions indicated by the symbols 5 and 6 showed bright fields (white), and in-plane alignment was formed. In this way, it was confirmed that by irradiating the substrate before cell formation with light and deactivating the groups that can generate radicals contained in the alignment film, a reaction with the polymerizable compound (additive) is not induced during the secondary exposure, and out-of-plane alignment is not formed.

[0151] (Evaluation of Orientation Patterning) The alignment state of the pattern-exposed liquid crystal display element was confirmed using polarizing plates arranged in crossed Nicols. The angle between the uniaxial alignment direction of the liquid crystal cell and the polarization direction was 45 degrees. The alignment pattern was evaluated by visual observation from the viewpoints of whether alignment control by light irradiation was possible, the uniformity of alignment, and the clarity of the alignment control surface (the boundary surface between the in-plane uniaxial alignment and the out-of-plane alignment). The results are shown in Table 10 below.

[0152] [Table 10] The change in orientation from in-plane (uniaxial) to out-of-plane orientation by light irradiation could be uniformly controlled, and the boundary between the different orientations was clear (Fig. 6). As shown in Fig. 6, it was confirmed that clean patterning was possible in the in-plane orientation region in the bright field (white) and the out-of-plane orientation region in the dark field (black). This does not depend on the type of polymer constituting the alignment film or the alignment treatment method. Since alignment patterns could be produced using materials of significantly different types, it can be inferred that alignment patterning is possible in all of the examples in which out-of-plane alignment control was possible in Tables 6 to 8.

[0153] (Evaluation of fine alignment patterning) The alignment state of the pattern-exposed liquid crystal display element was confirmed using polarizing plates arranged in crossed Nicols. The angle between the uniaxial alignment direction of the liquid crystal cell and the polarization direction was 45 degrees. The alignment pattern was evaluated by visual observation from the viewpoints of whether alignment control by light irradiation was possible, the uniformity of alignment, and the clarity of the alignment control surface (the boundary surface between the in-plane uniaxial alignment and the out-of-plane alignment). The results are shown in Table 11 below.

[0154] [Table 11] The liquid crystal display device fabricated using the substrate pattern-exposed as the first exposure had a uniform and clear fine alignment pattern regardless of the L / S width of the photomask. For example, a photograph of the liquid crystal display element obtained in Example 27 is shown in Fig. 7. At this time, since the pattern exposure was performed only on the first substrate as the primary exposure, a tilted alignment state was formed in the intermediate color (gray) portion indicated by reference number 7 in Fig. 7. An out-of-plane alignment state was formed in the dark field (black) portion indicated by reference number 8 in Fig. 7. 8 shows the results of Example 30, in which the L / S width of the photomask of Example 27 was changed. In FIG. 8, the difference between the intermediate color (gray) portion and the dark field (black) portion is as described in FIG. If it is desired to give intermediate color (gray) parts an in-plane uniaxial orientation, the second substrate can be exposed to the same pattern as the first substrate, and the exposed parts can be bonded together to produce a liquid crystal cell, after which a secondary exposure can be performed. It was confirmed that the liquid crystal display element that was not subjected to the primary exposure but was subjected to the pattern exposure as the secondary exposure could be patterned with an L / S width of the photomask of 100 μm, as shown in Example 31. The liquid crystal display element of Example 31 also had a clear patterning of the in-plane alignment region in the bright field (white) and the out-of-plane alignment region in the dark field (black). Furthermore, as shown in Example 32, it was confirmed that by subjecting both the first and second substrates to pattern exposure, laminating them with the pattern direction perpendicular to each other to produce a liquid crystal cell, and then subjecting them to secondary exposure, it was possible to produce three types of alignment states, i.e., in-plane uniaxial alignment, out-of-plane alignment, and tilted alignment, within a single liquid crystal display element. The results of the liquid crystal display element obtained in Example 32 are shown (FIGS. 9A and 9B). FIG 9A shows a photograph of the liquid crystal display element, and FIG 9B shows a schematic diagram of the photograph of the liquid crystal display element in FIG 9A. As shown in Figure 9 (Figures 9A and 9B are also collectively referred to as Figure 9), an out-of-plane alignment state is formed in the dark field (black) portion designated by reference numeral 9. An in-plane alignment state is formed in the bright field (white) portion designated by reference numeral 10. A tilt alignment state is formed in the intermediate color (gray) portion designated by reference numeral 11 (represented by a diagonal line pattern in Figure 9B). [Industrial Applicability]

[0155] According to the present invention, a liquid crystal display element in which at least two regions among an in-plane alignment region, an out-of-plane alignment region, and an inclined alignment region are patterned can be produced industrially with a high yield. [Explanation of symbols]

[0156] 101 Liquid crystal display element 102 Comb-tooth electrode substrate 102a Base material 102b Linear electrode 102c Radical generating membrane 102d base material 102e surface electrode 102f Insulating film 102g linear electrode 102h Radical generating membrane 103 Liquid crystal composition 104 Opposing substrate 104a Liquid crystal alignment film 104b Base material

Claims

1. Step (A): A step of forming a radical generating film capable of generating radicals upon irradiation with light on one substrate, and a step of forming a radical generating film capable of generating radicals upon irradiation with light on the other substrate; and step (B): contacting a liquid crystal composition containing liquid crystal and a radical polymerizable compound with the radical generating film, and irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm, which is sufficient to polymerize the radical polymerizable compound while maintaining the contact state; the one substrate and the other substrate form a pair of substrates; the radical polymerizable compound has a function of vertically aligning the liquid crystal by polymerization, the radical generating film formed on the one substrate and the radical generating film formed on the other substrate are uniaxially oriented films and have a function of forming in-plane orientation; Further, the method includes a step of the following requirement (Z1) for at least one of the pair of substrates, In the step of the requirement (Z1), when the radical generating film is irradiated with light, the following step (a) is included in the case of performing pattern exposure, and the following step (b) is included in the case of performing full-surface exposure, The present invention is characterized by manufacturing a liquid crystal display element having at least two different types of patterned regions, each of which is composed of any combination of (i) a combination of an inclined alignment region and an in-plane alignment region, (ii) a combination of an inclined alignment region and an out-of-plane alignment region, and (iii) a combination of an inclined alignment region, an in-plane alignment region, and an out-of-plane alignment region; Here, the inclined orientation region is a region formed by arranging one of the pair of substrates, which is in-plane oriented, facing the other substrate, which is out-of-plane oriented, or by arranging one of the substrates, which is out-of-plane oriented, facing the other substrate, which is in-plane oriented, The in-plane alignment region is a region formed by disposing one of the pair of substrates, which has an in-plane alignment, facing the other substrate, which has an in-plane alignment; A method for manufacturing a liquid crystal display element, wherein the out-of-plane orientation region is a region formed by arranging one of the pair of substrates, which has an out-of-plane orientation, facing the other substrate, which has an out-of-plane orientation. Requirement (Z1): Between the steps (A) and (B), a step (C) is included in which the radical-generating film obtained in the step (A) is irradiated with light having a peak at 240 to 400 nm, thereby deactivating the radical-generating ability of the radical-generating film. Step (a): By the pattern exposure, a portion in which the radical generating ability of the radical generating film is deactivated and a portion in which the radical generating ability is not deactivated are formed. Step (b): In the case where the radical generating ability of the radical generating film is inactivated by the overall exposure, the following requirement (Z2) is further included. Requirement (Z2): The step (B) of irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm is carried out through a photomask.

2. 2. The method for producing a liquid crystal display element according to claim 1, wherein the step (B) of irradiating the liquid crystal composition with light having a peak in the range of 240 to 400 nm is carried out in the absence of an electric field.

3. A method for manufacturing a liquid crystal display element as described in claim 1 or 2, wherein at least one of the radical generating films formed on the one substrate and the radical generating film formed on the other substrate has a polymer containing an organic group that induces radical polymerization.

4. 4. The method for producing a liquid crystal display element according to claim 3, wherein the polymer containing an organic group capable of inducing radical polymerization has a structural unit represented by the following formula (1) in its main chain: 【Chemistry 1】 (In formula (1), A represents an organic group that induces radical polymerization.)

5. 5. The method for producing a liquid crystal display element according to claim 3, wherein the polymer is at least one selected from the group consisting of a polyimide precursor obtained by using a diamine component containing a diamine having an organic group that induces radical polymerization, a polyimide, a polyurea, and a polyamide.

6. The method for producing a liquid crystal display element according to claim 4 , wherein the organic group capable of inducing radical polymerization is a group represented by the following formula (3): 【Chemistry 2】 (In formula (3), the dashed line represents a bond to a benzene ring, and R 6 is a single bond, -CH 2 -, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 ) CO-, R 7 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, 2 -or-CF 2 one or more - may be independently replaced by a group selected from -CH=CH-, a divalent carbocyclic ring, and a divalent heterocyclic ring, and may be further replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: R 8 represents an organic group capable of inducing radical polymerization, represented by a formula selected from the formulae [X-1] to [X-18], [W], [Y], and [Z]; 【Chemistry 3】 In formulas [X-1] to [X-18], * represents R 7 indicates the bonding site with S 1 and S 2 each independently represents -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, R 1 and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms, 【Chemistry 4】 In the formulas [W], [Y], and [Z], * represents R 7 represents the bonding site with 3 is a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 )CO—, Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent, R 9 and R 10 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms. In the case of an alkyl group or an alkoxy group, R 9 and R 10 may form a ring, Q represents any one of the following structures: 【Chemistry 5】 In the formula, R 11 Ha-CH 2 represents -, -NR-, -O-, or -S-, where R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a bond; R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.

7. 6. The method for producing a liquid crystal display element according to claim 5, wherein the diamine containing an organic group capable of inducing radical polymerization is a diamine represented by the following formula (2): 【Chemistry 6】 (In formula (2), A 1 and A 2 Each represents a hydrogen atom or a group represented by the following formula (3), 1 and A 2 At least one of the groups represented by the following formula (3) is represented: E is a single bond, —O—, —C(CH 3 ) 2 -, -NH-, -CO-, -NHCO-, -COO-, -(CH 2 ) m -, -SO 2 -, or any combination thereof, and m is an integer of 1 to 8. p represents an integer of 0 to 2. When p is 2, a plurality of A 2 and E each independently have the same definition as above. 1 is a group represented by the following formula (3): 【Chemistry 7】 (In formula (3), the dashed line represents a bond to a benzene ring, and R 6 is a single bond, -CH 2 -, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 ) CO-, R 7 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, 2 -or-CF 2 one or more - may be independently replaced by a group selected from -CH=CH-, a divalent carbocyclic ring, and a divalent heterocyclic ring, and may be further replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: R 8 represents an organic group capable of inducing radical polymerization, represented by a formula selected from the formulae [X-1] to [X-18], [W], [Y], and [Z]; 【Chemistry 8】 In formulas [X-1] to [X-18], * represents R 7 indicates the bonding site with S 1 and S 2 each independently represents -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, R 1 and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms, 【Chemistry 9】 In the formulas [W], [Y], and [Z], * represents R 7 represents the bonding site with 3 is a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 )CO—, Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent, R 9 and R 10 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms. In the case of an alkyl group or an alkoxy group, R 9 and R 10 may form a ring, Q represents any one of the following structures: 【Chemistry 10】 In the formula, R 11 Ha-CH 2 represents -, -NR-, -O-, or -S-, where R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a bond; R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.

8. The method for producing a liquid crystal display element according to any one of claims 1 to 7, wherein at least one of the radical polymerizable compounds is a compound having compatibility with liquid crystal and having one polymerizable unsaturated bond in one molecule.

9. 9. The method for producing a liquid crystal display element according to claim 8, wherein the polymerization reactive group of the radical polymerizable compound is selected from the following structures: 【Chemistry 11】 (In the formula, * indicates a bonding site with a part of the compound molecule other than the polymerizable unsaturated bond. R b represents an alkyl group having 3 to 20 carbon atoms, and E represents a single bond, -O-, or -NR c R represents a linking group selected from -, -S-, an ester bond, and an amide bond. c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R b The alkyl group represents a linear, branched, or cyclic alkyl group.

10. The method for producing a liquid crystal display element according to any one of claims 1 to 9, wherein the liquid crystal composition containing the liquid crystal and a radical polymerizable compound contains a radical polymerizable compound that causes a polymer obtained by polymerizing the radical polymerizable compound to have a Tg of 100°C or less.

11. A method for manufacturing a liquid crystal display element as described in claim 1, wherein one of the substrates is a substrate having a comb-tooth electrode.

Citation Information

Patent Citations

  • Liquid crystal display device and its manufacture method

    JP1998206834A

  • Liquid crystal display device, its manufacture, substrate and its manufacture

    JP2000122099A

  • Method of aligning liquid crystal having no anchoring in plane and non-contact liquid crystal aligning method using the same, and liquid crystal display device

    JP2013231757A

  • Liquid crystal display and method for manufacturing liquid crystal display

    JP2017211566A

  • Zero plane anchoring liquid crystal alignment method and its liquid crystal device

    JP4053530B2