Method for circulating iron-based electroplating solution, method for producing iron-based electroplating solution, and method for producing galvannealed steel sheet
The described method for circulating and processing iron-based electroplating solution through a reduction tank and vertical centrifugal separator addresses inefficiencies in iron ion supply and sludge separation, enhancing electrolytic efficiency and reducing equipment needs, leading to stable and cost-effective production.
Patent Information
- Application Number
- JP2023522758
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Conventional methods for supplying iron ions in iron-based alloy electroplating face inefficiencies in electrolytic efficiency and sludge formation, leading to decreased productivity and equipment requirements, while sludge separation devices struggle with incomplete removal and large equipment needs.
A method involving a plating solution circulation system that includes a reduction tank and a vertical centrifugal solid-liquid separator, where iron-based electroplating solution is processed to adjust iron ion concentration and separate sludge effectively, maintaining pH and using nitrogen gas to prevent oxidation.
Achieves high electrolytic efficiency, complete sludge removal, and stable power-saving production without requiring large equipment, resulting in improved plating quality and reduced operational costs.
Smart Images

Figure 0007586310000002 
Figure 0007586310000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for circulating an iron-based electroplating solution, which circulates and adjusts an iron-based electroplating solution used in an electroplating cell, a method for producing an iron-based electroplating solution, and a method for producing a galvannealed steel sheet, which includes a step of performing an iron-based electroplating treatment. [Background technology]
[0002] In recent years, there has been an increasing demand for high-tensile steel sheets (high-tensile steel materials) that can be used to reduce the weight of structures in the fields of automobiles, home appliances, building materials, etc. It is known that high-tensile steel materials can be obtained, for example, by adding Si to the steel to give steel sheets with good hole expandability, and by adding Si, Al, and Mn to the steel to give steel sheets with good ductility because residual γ is easily formed.
[0003] However, when a high-tensile steel sheet containing a large amount of Si or Mn (particularly 0.2 mass% or more) is used as a base material to manufacture a galvannealed steel sheet, the following problems arise. A galvannealed steel sheet is manufactured by heating and annealing a base steel sheet at a temperature of about 600 to 900°C in a reducing atmosphere or a non-oxidizing atmosphere, subjecting the steel sheet to a hot-dip galvanizing process, and further heating and alloying the galvanized steel sheet. Here, Si and Mn in steel are easily oxidized elements, and are selectively oxidized even in a commonly used reducing atmosphere or a non-oxidizing atmosphere, and are concentrated on the surface of the steel sheet to form oxides. These oxides reduce the wettability with molten zinc during the plating process, causing bare spots. Therefore, as the Si and Mn concentrations in the steel increase, the wettability drops sharply, and bare spots occur frequently. In addition, even if bare spots do not occur, there is a problem that the plating adhesion is poor. Furthermore, when Si and Mn in the steel are selectively oxidized and concentrated on the surface of the steel sheet, there is a significant delay in alloying during the alloying process after hot-dip galvanizing, which causes a problem of significantly impairing productivity.
[0004] To address this issue, for example, Patent Document 1 describes a method for applying 0.2 to 2 g / m 2This method of manufacturing a high-tensile hot-dip galvanized steel sheet is disclosed in which the steel sheet is plated with Fe and then a direct-fired furnace (DFF) and a radiant heating furnace (RTF) are adjusted to predetermined conditions to prevent Si, Mn, or Al, which are difficult elements contained in the steel to be plated, from diffusing to the surface and forming oxides. By preventing Si, Mn, or Al from diffusing to the surface and forming oxides, it is possible to prevent the phenomenon of non-plating, ensure excellent plating surface quality and plating adhesion, ensure high strength, and also reduce manufacturing costs. However, in an iron-based plating solution, the Fe consumed in the electrodeposition of the plating film is 2+ There is no electrodeposition reaction with Fe 3+ There is Fe 3+ It is known that plating solutions with high content of sludge can cause problems such as reduced plating electrolysis efficiency, clogged pipes due to the generation of sludge (fine solid matter), adhesion of sludge to steel sheets, and restrictions on continuous operation due to the need for sludge removal maintenance.
[0005] Regarding this problem, Patent Document 2 describes Fe 3+ The tank's stirring mechanism efficiently supplies iron powder for reduction, ion supply and dissolution into the plating solution. 3+ A method for reducing the Patent Document 3 specifies the relationship between the diameter and height of the cylindrical iron chip packed bed in the iron chip dissolving tank, and the Fe in the plating solution on the inlet side of the iron chip dissolving tank. 3+ By setting the concentration at 5g / L or more and the relative flow rate between the iron chips being dissolved and the plating solution being injected at 3m / min or more, the Fe 3+ A method for supplying iron ions in iron-based alloy electroplating that reduces In Patent Document 4, the surface area Sm of iron powder filled in a stirring tank is 2 and the amount of plating solution circulating to the mixing tank Qm 3 By setting the ratio H (=S / Q) of S / hr to 1≦H≦5, 3+ A highly efficient method for reducing trivalent Fe ions in an iron-based electroplating solution is disclosed, which achieves highly efficient reduction.
[0006] Patent Document 5 discloses a sludge separation treatment device for a continuous electroplating apparatus, which efficiently removes sludge generated in an electroplating solution by adding a coagulant to a plating solution containing sludge that has been partially extracted from a plating solution circulation tank and transferred to a sludge settling tank, stirring and mixing the solution to cause the sludge to settle, and then separating and recovering the sludge. Although Patent Document 6 does not explicitly state that it is for electroplating, it discloses a horizontal centrifugal separator that is airtight, compact, and capable of continuous operation as a general-purpose centrifugal separator. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2013 / 100615 [Patent Document 2] Japanese Patent Application Publication No. 3-2399 [Patent Document 3] Japanese Patent Application Publication No. 3-243798 [Patent Document 4] Japanese Patent Application Publication No. 6-306697 [Patent Document 5] JP 2012-188715 A [Patent Document 6] International Publication No. 2009 / 072209 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the conventional iron ion supplying method in iron-based alloy electroplating shown in Patent Document 2 and Patent Document 3, the highly efficient reduction method of trivalent Fe ions in an iron-based electroplating solution shown in Patent Document 4, the sludge separation treatment device of a continuous electroplating apparatus shown in Patent Document 5, and the horizontal centrifugal separator shown in Patent Document 6 all have the following problems.
[0009] That is, the iron ion supplying method in iron-based alloy electroplating shown in Patent Document 2 and Patent Document 3, and the highly efficient reduction method of trivalent Fe ions in an iron-based electroplating solution shown in Patent Document 4 provide highly efficient Fe 3+ However, in these methods, the amount of iron powder or iron chips to be added is unknown. 3+ If the iron source is small, even if Fe 3+ Even if the reduction efficiency of Fe is high, 3+ The plating efficiency decreases and the Fe 3+ The iron oxide present in the plating solution turns into sludge, which adversely affects operation. 3+ If there is too much iron source, the excess iron source can cause increased damage to the piping, and the reduction reaction can increase the pH of the plating solution, promoting an increase in sludge, which can also have a negative impact on operations.
[0010] Furthermore, the sludge separation treatment device for continuous electroplating equipment shown in Patent Document 5 is a so-called precipitation method in which a coagulant is added to a plating solution containing sludge in a sludge settling tank, and the sludge is precipitated by stirring and mixing, and then separated and recovered. However, the sludge separation treatment device for continuous electroplating equipment shown in Patent Document 5 has a small treatment flow rate, so it requires huge equipment that can handle the continuous production of iron-based electroplating solution, and this causes problems in terms of cost and installation space. Furthermore, in the case of the horizontal centrifugal separator shown in Patent Document 6, although continuous operation is possible, there is a problem that the fine sludge contained in the iron-based electroplating solution cannot be completely removed, and the sludge separation rate that can be achieved is only about 70%.
[0011] Therefore, the present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a method for circulating an iron-based electroplating solution, a method for producing an iron-based electroplating solution, and a method for producing a galvannealed steel sheet, which can provide an iron-based electroplating solution that has high electrolysis efficiency, is free from sludge contamination, and is stable and energy-saving, without requiring huge equipment. [Means for solving the problem]
[0012] In order to solve the above problems, a method for circulating an iron-based electroplating solution according to one embodiment of the present invention is a method for circulating and adjusting an iron-based electroplating solution used in an electroplating cell for iron-based electroplating, in which the iron-based electroplating solution used in the electroplating cell is passed through at least a reduction tank and a vertical centrifugal separator in that order, and then introduced into the electroplating cell. In the reduction tank, Fe in the iron-based electroplating solution transferred to the reduction tank is 3+ The gist is that an iron source for reduction is added according to the (Fe trivalent ion) concentration.
[0013] A method for producing an iron-based electroplating solution according to another aspect of the present invention is characterized in that an iron-based electroplating solution is produced by circulating and adjusting the iron-based electroplating solution by the above-mentioned method for circulating the iron-based electroplating solution. Furthermore, a method for producing a galvannealed steel sheet according to another aspect of the present invention is summarized as including a step of performing an iron-based electroplating treatment on a steel sheet using the iron-based electroplating solution produced by the above-mentioned method for producing an iron-based electroplating solution. Effect of the Invention
[0014] According to the method for circulating an iron-based electroplating solution, the method for producing an iron-based electroplating solution, and the method for producing a galvannealed steel sheet of the present invention, it is possible to provide a method for circulating an iron-based electroplating solution, a method for producing an iron-based electroplating solution, and a method for producing a steel sheet, which can produce an iron-based electroplating solution that is stable and energy-saving, has high electrolysis efficiency, is free of sludge contamination, and does not require large-scale equipment. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic diagram of an electroplating facility to which a method for circulating an iron-based electroplating solution according to one embodiment of the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments shown below are merely examples of devices and methods for embodying the technical concept of the present invention, and the technical concept of the present invention is not limited to the following embodiments in terms of the materials, shapes, structures, arrangements, etc. of the components. In addition, the drawings are schematic, and therefore, it should be noted that the relationship between thickness and planar dimensions, ratios, etc. may differ from the actual relationship between thickness and planar dimensions, and the drawings may include parts in which the relationship between dimensions and ratios differ from one another.
[0017] FIG. 1 shows a schematic configuration of an electroplating facility to which a method for circulating an iron-based electroplating solution according to one embodiment of the present invention is applied. The electroplating equipment 1 shown in FIG. 1 includes an electroplating cell 10 for iron-based electroplating, which performs iron-based electroplating on a steel sheet S to be plated. The electroplating cell 10 is a horizontal plating cell, in which the steel sheet S is made to travel horizontally by a current-carrying roll 14, an iron-based electroplating solution P in a treatment tank 11 is supplied to a gap between the steel sheet S and a pair of anode electrodes 12, and an electric current is applied between the plating surface of the steel sheet S, which is a cathode, and the pair of anode electrodes 12 to perform iron-based electroplating on both sides of the steel sheet S. In FIG. 1, reference numeral 13 denotes a plating solution nozzle header. In this embodiment, the electroplating cell 10 is a horizontal plating cell, but it may be any type, such as a vertical plating cell or a radial cell. In addition, the electroplating cell 10 may be a plurality of such treatment equipment connected together, or an intermediate tank may be provided between the treatment equipment. Here, the term "iron-based electroplating solution" is defined as an electroplating solution in which the concentration of Fe ions among the metal ions contained in the plating solution is 60% or more.
[0018] The electroplating equipment 1 also includes a plating solution circulation tank 20 that supplies the iron-based electroplating solution P to the electroplating cell 10. The treatment tank 11 of the electroplating cell 10 and the plating solution circulation tank 20 are connected by a pipe 15 that transfers the iron-based electroplating solution P from the treatment tank 11 to the plating solution circulation tank 20 in order to circulate the iron-based electroplating solution P. The plating solution nozzle header 13 on one side of the electroplating cell 10 and the plating solution circulation tank 20 are also connected by a pipe 24 that supplies the iron-based electroplating solution P from the plating solution circulation tank 20 to the plating solution nozzle header 13 on one side by a pump 25 and a pipe 26 that branches off from the pipe 24. The plating solution nozzle header 13 on the other side of the electroplating cell 10 and the plating solution circulation tank 20 are also connected by a pipe 24 that supplies the iron-based electroplating solution P from the plating solution circulation tank 20 to the plating solution nozzle header 13 on the other side by a pump 25 and a pipe 27 that branches off from the pipe 24. It is desirable to fill the plating solution circulation tank 20 with nitrogen gas (N2 gas) so that the iron-based electroplating solution P is kept in a non-oxidizing state without coming into contact with air.
[0019] In addition, the electroplating equipment 1 is configured to circulate Fe in the iron-based electroplating solution P from the plating solution circulation tank 20. 3+ The plating solution circulating tank 20 and the reduction tank 30 are connected by a pipe 21 that supplies the iron-based electroplating solution P transferred from the treatment tank 11 to the plating solution circulating tank 20 to the reduction tank 30 by a pump 22. The pipe 21 is connected to a pump 22 that pumps out Fe contained in the iron-based electroplating solution P before the iron-based electroplating solution P is supplied to the reduction tank 30. 3+ (Fe trivalent ion) concentration measurement 3+ A total of 23 have been installed. 3+ The total is Fe 3+ Any method capable of measuring the (Fe trivalent ion) concentration may be used, for example, an absorptiometer may be used.
[0020] In the reduction tank 30, Fe 3+ Fe in iron-based electroplating solution P measured by a 3+ The iron source (iron powder or iron chips) for reduction is added according to the (Fe trivalent ion) concentration. The amount of iron source added can be adjusted appropriately depending on the reduction efficiency, but generally it is Fe3+ The concentration of the iron-based electroplating solution P is preferably 1.1 to 1.3 times the concentration of the iron-based trivalent ion (Fe trivalent ion). The reduction tank 30 is provided with an agitator 31 for agitating the iron-based electroplating solution P in the reduction tank 30. The reduction tank 30 is provided with a pH meter 32 for measuring the pH of the iron-based electroplating solution P in the reduction tank 30. Since the pH of the iron-based electroplating solution P during reduction may increase due to the addition of an iron source, and sludge may increase, sulfuric acid is added to maintain the pH at 2.3 or less. There is no lower limit for the pH of the iron-based electroplating solution P during reduction, but from the viewpoint of reducing the pH readjustment process in the final adjustment tank 50 described later and reducing the amount of chemical adjustment, the pH is preferably 1.0 or more, and more preferably 2.0 or more. Nitrogen gas (N2 gas) is sealed in the reduction tank 30 to prevent the iron-based electroplating solution P from coming into contact with air and to keep it in an unoxidized state.
[0021] The electroplating equipment 1 also includes a vertical centrifugal separator 40 that separates sludge in the iron-based electroplating solution P from the iron-based electroplating solution P. The reduction tank 30 and the solid-liquid separator 40 are connected by a pipe 33 that supplies the iron-based electroplating solution P reduced in the reduction tank 30 to the solid-liquid separator 40 by a pump 34. The solid-liquid separator 40 is a vertical centrifugal separator with a screw 43 arranged to extend vertically (up and down in FIG. 1 ), and includes a screw outer cylinder 42 that rotates differentially relative to each other so as to centrifuge the solid (sludge) and liquid in the iron-based electroplating solution P as the raw liquid due to the specific gravity difference, and a screw 43 disposed in the screw outer cylinder 42, in a centrifugal separator tube 41. The rotating shaft 44 of the screw 43 is formed in a cylindrical shape so that the iron-based electroplating solution P as the raw liquid is led from the screw 43 into the screw outer cylinder 42, and a diffusion opening 48 is formed on the side of the rotating shaft 44. The screw outer cylinder 42 and the screw 43 are mounted in a centrifugal separator 41. A raw solution supply port 45 is formed on a rotating shaft 44 of the screw 43 in the centrifugal separator 41, through which the iron-based electroplating solution P as the raw solution from the pipe 33 is supplied to a diffusion opening 48. A separated water discharge port 46 is provided on a side surface of the centrifugal separator 41, and a solid discharge port 47 for discharging solids (sludge) is provided on a bottom surface of the centrifugal separator 41. As the vertical centrifugal separator 40, for example, the solid-liquid separator described in JP 2007-38068 A can be used.
[0022] When such a vertical centrifugal separation type solid-liquid separator 40 is used, even sludge containing a wide range of particle sizes from 0.5 to 100 μm contained in the iron-based electroplating solution P can be separated and recovered at a recovery rate of 90% or more. However, even with this solid-liquid separator 40, if the centrifugal force is increased, fine sludge of 5 μm or less is not separated and accompanies the clean solution, reducing the separation efficiency, so it is preferable that the centrifugal force is 1000 to 1800 G and the differential speed between the screw 43 and the screw outer cylinder 42 is 1.0 to 2.0 rpm. If the centrifugal force is less than 1000 G, the centrifugal force is insufficient, resulting in a small separation effect and a decrease in separation performance. If the differential speed between the screw 43 and the screw outer cylinder 42 is 1.0 rpm or less, the scraping time by the screw 43 is short and the separation efficiency decreases. If the differential speed exceeds 2.0 rpm, the scraping time by the screw 43 is long, but the mixing of fine particles into the clean solution increases, resulting in a decrease in separation efficiency, which is not preferable. Below the solid-liquid separator 40, a solid receiving tank 49 for receiving solids (sludge) discharged from the solid discharge port 47 is provided.
[0023] The electroplating equipment 1 preferably includes a final adjustment tank 50 for adjusting the iron-based electroplating solution P from which solids (sludge) have been separated in the solid-liquid separation device 40 to a plating solution state suitable for efficient iron-based electroplating. The separated water outlet 46 of the solid-liquid separation device 40 and the final adjustment tank 50 are preferably connected by a pipe 55 for supplying the iron-based electroplating solution P from which solids (sludge) have been separated in the solid-liquid separation device 40 to the final adjustment tank 50. The final adjustment tank 50 is preferably provided with a pipe 55 for supplying the iron-based electroplating solution P from which solids (sludge) have been separated in the solid-liquid separation device 40 to the final adjustment tank 50. 3+ (Fe trivalent ion) concentration measurement 3+ The final adjustment tank 50 is also provided with a pH meter 51 for measuring the pH of the iron-based electroplating solution P in the final adjustment tank 50.
[0024] In the final adjustment tank 50, the iron-based electroplating solution P from which the solid (sludge) has been separated in the solid-liquid separator 40 is adjusted to a plating solution state suitable for efficient iron-based electroplating. 3+The iron-based electroplating solution P is adjusted with pure water, dilute sulfuric acid, and a heater so that the (Fe trivalent ion) concentration is 4.0 g / L or less, the pH of the iron-based electroplating solution P in the final adjustment tank 50 is 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution P is 40 to 55°C. By keeping the iron-based electroplating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and energy-saving production can be achieved. More preferably, the Fe trivalent ion concentration in the iron-based electroplating solution P is 4.0 g / L or less, the pH of the iron-based electroplating solution P in the final adjustment tank 50 is 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution P is 40 to 55°C. By keeping the iron-based electroplating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and energy-saving production can be achieved. 3+ By adjusting the (Fe trivalent ion) concentration to 2.0 g / L or less, the pH of the iron-based electroplating solution P in the final adjustment tank 50 to 2.2 to 2.3, and the liquid temperature of the iron-based electroplating solution P to 40 to 45°C, it is possible to achieve an electroplating efficiency of 80% or more. The final adjustment tank 50 and the plating solution circulation tank 20 are preferably connected by a pipe 53 that supplies the iron-based electroplating solution P that has been finalized in the final adjustment tank 50 to the plating solution circulation tank 20 by a pump 54.
[0025] Next, a method for circulating the iron-based electroplating solution in the electroplating equipment 1 will be described. The iron-based electroplating solution P is mainly a mixed solution of iron sulfate and sodium sulfate. 2+ (Fe divalent ions) are present, but the insoluble anode surface in the electroplating cell 10 undergoes the anodic oxidation phenomenon: Fe 2+ →Fe 3+ +e - In addition, when the iron-based electroplating solution P is mixed with air, the air oxidation phenomenon occurs: 2Fe 2+ +1 / 2O2+H2O→2Fe 3+ +2OH - Also, Fe in the iron-based electroplating solution P 3+ If this iron-based electroplating solution P is used without modification, the Fe (Fe trivalent ion) concentration will increase. 3+ (Fe trivalent ions) are excessive, which reduces the efficiency of plating. 3+ When the amount of (Fe trivalent ions) increases and the pH of the iron-based electroplating solution P becomes 2.4 or higher, 3Fe 3+ +7 / 2SO4 2-+2OH - +1 / 2Na2SO4+4H2O → NaFe3(SO4)2(OH)6(natrojarosite)+2H2SO4 This reaction is accelerated, and a fine sludge called natrojarosite is generated. If this sludge is left alone, it will grow larger and cause blockage of pipes or adhesion to steel sheets, resulting in poor appearance, so it is necessary to remove it while it is still fine. Therefore, as explained in the Background Art, it is necessary to reduce the iron-based electroplating solution P before such reactions progress.
[0026] Therefore, in the method for circulating an iron-based electroplating solution according to this embodiment, first, the iron-based electroplating solution P that has been used in the electroplating cell 10 and discharged from the electroplating cell 10 is transferred to the plating solution circulation tank 20 via piping 15. Next, the iron-based electroplating solution P is sucked out by a pump 22 from a pipe 21 installed in a position close to the iron-based electroplating solution P discharged from the electroplating cell 10 in the plating solution circulation tank 20, and transferred to a reduction tank 30. Here, before the iron-based electroplating solution P is supplied to the reduction tank 30, the Fe 3+ The total amount of Fe contained in the iron-based electroplating solution P was calculated by 23. 3+ Measure the (Fe3+ ion) concentration.
[0027] Next, the iron-based electroplating solution P is poured into the reduction tank 30, and the Fe 3+ The iron source for reduction (iron powder or iron chips) is added according to the (Fe trivalent ion) concentration. The amount of iron source added can be adjusted appropriately depending on the reduction efficiency, but as mentioned above, it is generally Fe 3+ It is desirable to set the concentration at 1.1 to 1.3 times the concentration of Fe(trivalent ions). For example, 3+When the (Fe trivalent ion) concentration is 4.0 g / L, it is desirable to add 4.4 to 5.2 g / L of the iron source. The iron-based electroplating solution P in the reduction tank 30 is constantly stirred by the stirrer 31, and at the same time, the pH of the iron-based electroplating solution P is constantly measured and monitored by the pH meter 32. As described above, the pH of the iron-based electroplating solution P during reduction may rise due to the addition of the iron source, which may increase sludge, so sulfuric acid is added to the reduction tank 30 so as to always maintain the pH at 2.3 or less. Here, the lower limit of the pH of the iron-based electroplating solution P during reduction is not limited, but as described above, from the viewpoint of reducing the pH readjustment process in the final adjustment tank 50 described later and reducing the amount of chemical adjustment, the pH is preferably 1.0 or more, and more preferably 2.0 or more. In addition, nitrogen gas (N2 gas) is sealed in the reduction tank 30 so that the iron-based electroplating solution P is not exposed to air and is in an unoxidized state.
[0028] Next, the iron-based electroplating solution P reduced in the reduction tank 30 is transferred to the solid-liquid separation device 40 by the pump 34 through the piping 33. The solid-liquid separation device 40 used in this embodiment is a vertical centrifugal separation device having the above-mentioned configuration. The iron-based electroplating solution P is introduced from the piping 33 into the raw solution supply port 45 formed on the rotating shaft 44 of the screw 43 and supplied to the diffusion opening 48. Then, the iron-based electroplating solution P is introduced from the diffusion opening 48 into the screw outer cylinder 42, where it is centrifuged into solids (sludge) and liquid due to the difference in specific gravity. Thereafter, the liquid is transferred from the separated water discharge port 46 through the piping 55 to the final adjustment tank 50. Meanwhile, the solids (sludge) are discharged from the solid discharge port 47 to the solid receiving tank 49.
[0029] Here, since the solid-liquid separator 40 is a vertical centrifugal separator, as described above, even if the sludge contained in the iron-based electroplating solution P contains a wide range of particle sizes from 0.5 to 100 μm, the sludge can be separated and collected at a collection rate of 90% or more. However, even with this solid-liquid separator 40, if the centrifugal force is increased, fine sludge of 5 μm or less is not separated and accompanies the clean liquid, decreasing the separation efficiency, so as described above, it is preferable that the centrifugal force is 1000 to 1800 G and the differential speed between the screw 43 and the screw outer cylinder 42 is 1.0 to 2.0 rpm. If the centrifugal force is less than 1000 G, the centrifugal force is insufficient, resulting in a small separation effect and a decrease in separation performance. If the differential speed between the screw 43 and the screw outer cylinder 42 is 1.0 rpm or less, the scraping time by the screw 43 is short, and the separation efficiency decreases. If the differential speed exceeds 2.0 rpm, the scraping time by the screw 43 is long, but the mixing of fine particles into the clean liquid increases, resulting in a decrease in separation efficiency, which is not desirable. Furthermore, since the solid-liquid separation device 40 does not require periodic cleaning of the inside of the device, it can be operated continuously for 24 hours, and there is no need for production adjustments or interruptions due to sludge.
[0030] Next, in the final adjustment tank 50 to which the iron-based electroplating solution P has been transferred, the iron-based electroplating solution P from which the solid (sludge) has been separated in the solid-liquid separator 40 is adjusted to a plating solution state suitable for efficient iron-based electroplating. 3+ It is preferable to adjust the iron-based electroplating solution P in the final adjustment tank 50 to a liquid state of 40 to 55°C using pure water, dilute sulfuric acid, and a heater so that the (Fe trivalent ion) concentration is 4.0 g / L or less, the pH of the iron-based electroplating solution P in the final adjustment tank 50 is 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution P is 40 to 55°C. By keeping the iron-based electroplating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and energy-saving production can be achieved. More preferably, the Fe in the iron-based electroplating solution P is 3+ By adjusting the (Fe trivalent ion) concentration to 2.0 g / L or less, the pH of the iron-based electroplating solution P in the final adjustment tank 50 to 2.2 to 2.3, and the liquid temperature of the iron-based electroplating solution P to 40 to 45°C, it is possible to achieve an electroplating efficiency of 80% or more.
[0031] The iron-based electroplating solution P that has been finalized in the final adjustment tank 50 is then transferred by a pump 54 via a pipe 53 to the plating solution circulation tank 20 . Finally, the iron-based electroplating solution P transferred to the plating solution circulation tank 20 is supplied by the pump 25 via pipes 24 and 26 to one plating solution nozzle header 13 of the electroplating cell 10, and then by the pump 25 via pipes 24 and 27 to the other plating solution nozzle header 13 of the electroplating cell 10, thereby completing the circulation of the iron-based electroplating solution P. In the method for producing an iron-based electroplating solution, the iron-based electroplating solution P is produced by regulating circulation using this circulation method for the iron-based electroplating solution.
[0032] In the electroplating cell 10, the iron-based electroplating treatment is performed on the steel sheet S using the iron-based electroplating solution P circulated and adjusted in this manner. Thereafter, in a post-process, the steel sheet S that has been subjected to the iron-based electroplating treatment is heat-annealed, the heat-annealed steel sheet S is subjected to a hot-dip galvanizing treatment, and the galvanized coating is further heat-alloyed to produce a galvannealed steel sheet. That is, the manufacturing method of a galvannealed steel sheet includes a step of electroplating a steel sheet S using an iron-based electroplating solution manufactured by the above-mentioned manufacturing method of an iron-based electroplating solution. Then, in a post-process, the steel sheet S that has been subjected to the iron-based electroplating treatment is heat-annealed, the heat-annealed steel sheet S is subjected to a hot-dip galvanizing treatment, and the galvanized coating is further heat-alloyed to manufacture a galvannealed steel sheet.
[0033] As described above, according to the method for circulating an iron-based electroplating solution, the method for producing an iron-based electroplating solution, and the method for producing a galvannealed steel sheet according to the present embodiment, the iron-based electroplating solution P used in the electroplating cell 10 is passed through at least the reduction tank 30, the vertical centrifugal separator 40, and the final adjustment tank 50 in this order, and then introduced into the electroplating solution. 3+ Add an iron source for reduction according to the (Fe trivalent ion) concentration. This makes it possible to provide an iron-based electroplating solution that does not require large-scale equipment, has high electrolysis efficiency, is free of sludge contamination, and is stable and energy-saving.
[0034] Furthermore, according to the method for circulating an iron-based electroplating solution, the method for producing an iron-based electroplating solution, and the method for producing a galvannealed steel sheet according to the present embodiment, sulfuric acid is added to the reduction tank 30 so as to maintain the pH of the iron-based electroplating solution P in the reduction tank 30 at 2.3 or less. This makes it possible to avoid the possibility of an increase in the pH of the iron-based electroplating solution P due to the addition of the iron source, which would lead to an increase in sludge. Moreover, according to the method for circulating an iron-based electroplating solution, the method for producing an iron-based electroplating solution, and the method for producing a galvannealed steel sheet according to the present embodiment, nitrogen gas is sealed inside the reduction tank 30. This prevents the iron-based electroplating solution P in the reduction tank 30 from coming into contact with air and keeps it in a non-oxidized state.
[0035] According to the circulation method of an iron-based electroplating solution, the manufacturing method of an iron-based electroplating solution, and the manufacturing method of a galvannealed steel sheet of the present embodiment, a vertical centrifugal separation device 40 includes a screw outer cylinder 42 which rotates differentially with respect to each other so as to separate the solid and liquid of the raw solution by centrifugal separation due to the difference in specific gravity, and a screw 43 disposed in the screw outer cylinder 42. The rotation shaft 44 of the screw 43 is formed in a cylindrical shape so as to lead the raw solution from the screw 43 into the screw outer cylinder 42, and a diffusion opening 48 is formed on the side of the rotation shaft 44. As a result, the iron-based electroplating solution P transferred to the solid-liquid separation device 40 is supplied from the rotation shaft 44 of the screw 43 to the diffusion opening 48, and is introduced from the diffusion opening 48 into the screw outer cylinder 42. In the screw outer cylinder 42, the raw solution is centrifuged into solids (sludge) and liquid due to the difference in specific gravity. Therefore, even if the sludge contained in the iron-based electroplating solution P contains a wide range of particle sizes from 0.5 to 100 μm, the sludge can be separated and recovered at a recovery rate of 90% or more.
[0036] In addition, according to the method for circulating an iron-based electroplating solution, the method for producing an iron-based electroplating solution, and the method for producing a galvannealed steel sheet according to the present embodiment, in the final adjustment tank 50, Fe in the iron-based electroplating solution P is 3+ Adjust the iron-based electroplating solution P with sulfuric acid and pure water so that the (Fe trivalent ion) concentration is 2.0 g / L or less, the pH of the iron-based electroplating solution P is 2.0 to 2.3, and the liquid temperature of the iron-based electroplating solution P is 40 to 55°C. By keeping the iron-based electroplating solution P in this liquid state, an electroplating efficiency of 70% or more can be achieved, and energy-saving production can be achieved. In addition, by carrying out an iron-based electroplating process using the iron-based electroplating solution P circulated and adjusted by the method for circulating an iron-based electroplating solution according to the present embodiment, the plating appearance of the produced galvannealed steel sheet is beautiful and free of sludge marks.
[0037] Although the embodiment of the present invention has been described above, the present invention is not limited to this and various modifications and improvements can be made. For example, it is not necessarily necessary to add sulfuric acid to the reduction tank 30 so as to maintain the pH of the iron-based electroplating solution P in the reduction tank 30 at 2.0 to 2.3. Furthermore, it is not necessarily required that the reduction chamber 30 be filled with nitrogen gas. In the final adjustment tank 50, Fe in the iron-based electroplating solution P is 3+ It is not necessarily necessary to adjust the (Fe trivalent ion) concentration to 2.0 g / L or less.
[0038] Furthermore, in the final adjustment tank 50, it is not necessarily necessary to adjust the pH of the iron-based electroplating solution P to 2.0 to 2.3. Furthermore, in the final adjustment tank 50, it is not always necessary to adjust the temperature of the iron-based electroplating solution P to 40 to 55°C. In addition, the iron-based electroplating solution P used in the electroplating cell 10 is passed through the plating solution circulation tank 20, the reduction tank 30, the vertical centrifugal separator 40, and the final adjustment tank 50 in that order, and then fed into the electroplating cell 10, but it is not necessarily required to pass through the plating solution circulation tank 20. EXAMPLES
[0039] In order to verify the effects of the present invention, the power consumption rate (kWh / T), electrolysis efficiency (%), and appearance of the product galvannealed steel sheet were investigated for Comparative Examples 1 to 3 and Examples 1 to 5. The galvannealed steel sheet is produced by subjecting a steel sheet to an iron-based electroplating treatment, then heat-annealing the steel sheet that has been subjected to the iron-based electroplating treatment in a post-process, subjecting the heat-annealed steel sheet to a hot-dip galvanizing treatment, and further heating and alloying the galvanized steel sheet.
[0040] In Examples 1 to 5, electroplating equipment similar to the electroplating equipment 1 having the configuration shown in FIG. 1 was used. In Comparative Examples 1 to 3, the electroplating cell, plating solution circulation tank, and final adjustment tank were the same as those in Examples 1 to 5, and the reduction tank was the one used in Patent Document 4 (the surface area of the iron powder filled in the reduction tank was Sm 2 and the amount of plating solution circulated to the reduction tank Qm 3 The ratio H (=S / Q) of the time periods S and Q per hour was set to 1≦H≦5. In Comparative Example 1, a solid-liquid separator similar to the sedimentation type sludge settling tank used in Patent Document 5 was used. In Comparative Examples 2 and 3, a solid-liquid separator similar to the horizontal centrifugal separator used in Patent Document 6 was used.
[0041] In the electroplating cells in Examples 1 to 5 and Comparative Examples 1 to 3, the longitudinal length of the electrode in each cell was 2 m, the distance between the steel sheet and the electrode was 30 mm on one side, and two cells were connected together. The iron-based electroplating solution (plating bath) was a sulfuric acid bath with iron content of 55 to 65 g / L and sodium content of 5 to 7 g / L. The survey results for the power consumption rate (kWh / T), electrolysis efficiency (%), and the appearance of the finished galvannealed steel sheet are shown in Table 1. "Appearance after plating" in Table 1 refers to the appearance of the finished galvannealed steel sheet.
[0042] [Table 1]
[0043] In Comparative Examples 1 to 3, Fe before being charged into the reduction tank was 3+ (Fe trivalent ion) The iron source was not added according to the concentration. 3+ (Fe trivalent ion) concentration could not be sufficiently reduced (in the final adjustment tanks of Comparative Examples 1 to 3, Fe 3+ (Fe trivalent ion) concentration could not be sufficiently reduced, so Fe 3+ The electrolysis efficiency (%) was low at 54% or less. The power consumption rate (kWh / T) was also high at 112kWh / T or more. Furthermore, because a settling or horizontal centrifugal separator was used as the solid-liquid separator, the sludge could not be completely removed, and sludge marks remained on the exterior of the finished galvannealed steel sheet.
[0044] On the other hand, in Examples 1 to 5, in the reduction tank, Fe before being charged into the reduction tank 3+ The iron source was added according to the Fe(3-valent ion) concentration. 3+ (Fe trivalent ion) concentration can be sufficiently reduced (in the final adjustment tanks of Examples 1 to 5, Fe 3+ (Fe trivalent ion) concentration was sufficiently reduced, so that Fe 3+ The electrolysis efficiency (%) was high at 71% or more. The power consumption rate (kWh / T) was also low at 66kWh / T or less. The vertical centrifugal separator was used as the solid-liquid separator, so the sludge could be sufficiently removed, and the appearance of the finished galvannealed steel sheet was beautiful.
[0045] Regarding the appearance of the products in Table 1 after plating, the product surface (surface area 10 m 2 ) and if 50 or more sludge marks were found it was rated as "many sludge marks", if 10 to 50 sludge marks were found it was rated as "few sludge marks", and if less than 10 marks were found it was rated as "beautiful". [Explanation of symbols]
[0046] 1. Electroplating equipment 10 Electroplating Cell 11 Treatment tank 12 Anode electrode 13 Plating solution nozzle header 14 Conductive roll 15 Piping 20 Plating solution circulation tank 21 Piping 22 Pump 23 Fe 3+ Total 24 Piping 25 Pump 26 Piping 27 Piping 30 Reduction tank 31 Stirrer 32 PH meter 33 Piping 34 Pump 40 Solid-liquid separator 41 Centrifuge tube 42 Screw outer cylinder 43 Screw 44 Rotational Axis 45 Stock solution supply port 46 Separated water outlet 47 Solids outlet 48 Diffusion Aperture 49 Solid Receptor 50 Final adjustment tank 51 PH meter 52 Fe 3+ Total 53 Piping 54 Pump 55 Piping P Iron-based electroplating solution
Claims
1. A method for circulating an iron-based electroplating solution, which circulates and adjusts an iron-based electroplating solution used in an electroplating cell for iron-based electroplating, comprising: The iron-based electroplating solution used in the electroplating cell is passed through at least a reduction tank and a vertical centrifugal separator in this order, and then introduced into the electroplating cell, In the reduction tank, Fe in the iron-based electroplating solution transferred to the reduction tank is 3+ Add an iron source for reduction according to the (Fe trivalent ion) concentration, The method for circulating an iron-based electroplating solution is characterized in that after the iron-based electroplating solution is treated in the vertical centrifugal separation type solid-liquid separation device, it is passed through a final adjustment tank, and in the final adjustment tank, the Fe3+ (Fe trivalent ion) concentration in the iron-based electroplating solution is adjusted to 4.0 g / L or less.
2. 2. The method for circulating an iron-based electroplating solution according to claim 1, wherein sulfuric acid is added to the reduction tank so as to maintain the pH of the iron-based electroplating solution in the reduction tank at 2.3 or less.
3. 2. The method for circulating an iron-based electroplating solution according to claim 1, wherein nitrogen gas is sealed inside the reduction chamber.
4. 2. The method for circulating an iron-based electroplating solution according to claim 1, wherein the vertical centrifugal separation type solid-liquid separation device comprises: an outer screw cylinder which rotates differentially relative to each other so as to centrifuge the solid and liquid of the raw solution based on the specific gravity difference; and a screw disposed in the outer screw cylinder, the rotation shaft of the screw being formed in a cylindrical shape so as to lead the raw solution from the screw into the outer screw cylinder, and a diffusion opening is formed on a side surface of the rotation shaft.
5. 2. The method for circulating an iron-based electroplating solution according to claim 1, wherein the pH of the iron-based electroplating solution is adjusted to 2.0 to 2.3 in the final adjustment tank.
6. 2. The method for circulating an iron-based electroplating solution according to claim 1, wherein the temperature of the iron-based electroplating solution in the final adjustment tank is adjusted to 40 to 55°C.
7. A method for circulating an iron-based electroplating solution as described in claim 5, characterized in that in the final adjustment tank, the liquid temperature of the iron-based electroplating solution is adjusted to 40 to 55°C.
8. A method for circulating and adjusting an iron-based electroplating solution used in an electroplating cell for iron-based electroplating, comprising the steps of: The iron-based electroplating solution used in the electroplating cell is passed through at least a reduction tank and a vertical centrifugal separator in this order, and then introduced into the electroplating cell, In the reduction tank, an iron source for reduction is introduced according to the Fe 3+ (Fe trivalent ion) concentration in the iron-based electroplating solution to be transferred to the reduction tank; After being treated in the vertical centrifugal separator, the iron-based electroplating solution is passed through a final adjustment tank. In the final adjustment tank, the Fe in the iron-based electroplating solution is 3+ A method for circulating an iron-based electroplating solution, comprising adjusting the iron-based electroplating solution with sulfuric acid and pure water so that the (Fe trivalent ion) concentration is 2.0 g / L or less, the pH of the iron-based electroplating solution is 2.0 to 2.3, and the temperature of the iron-based electroplating solution is 40 to 55°C.
9. A method for circulating an iron-based electroplating solution as described in claim 8, characterized in that sulfuric acid is added to the reduction tank so as to maintain the pH of the iron-based electroplating solution in the reduction tank at 2.3 or less.
10. A method for circulating an iron-based electroplating solution as described in claim 8, characterized in that nitrogen gas is sealed inside the reduction tank.
11. The vertical centrifugal separation type solid-liquid separation device is characterized in that it comprises a screw outer cylinder which rotates differentially relative to each other so as to centrifuge the solid and liquid of the raw solution based on the difference in specific gravity, and a screw disposed within the screw outer cylinder, the rotating shaft of the screw being formed into a cylindrical shape so as to guide the raw solution from the screw into the screw outer cylinder, and a diffusion opening being formed on the side of the rotating shaft.
12. A method for producing an iron-based electroplating solution, characterized in that the iron-based electroplating solution is produced by adjusting the circulation using the circulation method for iron-based electroplating solution described in any one of claims 1 to 11.
13. A method for producing an alloyed hot-dip galvanized steel sheet, comprising a step of performing an iron-based electroplating process on a steel sheet using an iron-based electroplating solution produced by the method for producing an iron-based electroplating solution described in claim 12.
Citation Information
Patent Citations
Senjoyokumatahametsukyokuno renzokutekiseijokanryuryohoho
JP1976109228A
Bath composition control method of composite plating bath dispersed with metal particle
JP1980065399A
Production of zn-fe alloy electroplated steel plate
JP1983110691A
Device for maintaining and controlling concentration of iron electroplating liquid and storing said liquid
JP1988125700A
Method for replenishing ion in iron or iron-based alloy electroplating
JP1991002399A