How to get iodine
The pretreatment of brine with manganese oxide and chlorine-based activation enhances iodine yield from brine by reducing heavy metal and organic polymer interference, addressing equipment contamination issues in iodine extraction.
Patent Information
- Application Number
- JP2021009924
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-25
AI Technical Summary
Existing methods for extracting iodine from brine face challenges in achieving high yield while preventing contamination of equipment due to insolubilization of other components and equipment clogging, particularly with brines containing high levels of heavy metals and organic carbon.
A method involving a pretreatment step where brine is contacted with manganese oxide, followed by a chlorine-based activation treatment, and subsequent washing to remove residual activator, effectively reducing heavy metal and organic polymer interference, thereby enhancing iodine yield and preventing equipment contamination.
The method significantly improves iodine yield from brine by minimizing equipment contamination and reducing side reactions, achieving superior iodine acquisition efficiency.
Smart Images

Figure 0007586404000003 
Figure 0007586404000001 
Figure 0007586404000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for obtaining iodine from brine. [Background technology]
[0002] Iodine is a common element that is also found in seawater, but its presence as a resource on Earth is uneven; it is known to exist in high concentrations only in brines produced in association with natural gas and petroleum, and in saltpeter ore in Chile.
[0003] Apart from the method of separating iodine from saltpeter ore, iodine is mainly produced industrially by separating it from brine that is pumped up from permeable underground strata along with dissolved natural gas and contains iodide ions after the natural gas is separated.
[0004] As a method for producing molecular iodine (I2; hereinafter, sometimes simply referred to as iodine) using brine as a raw material, the blowing out method and the ion exchange resin method are industrially practiced (see Non-Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Non-Patent Document 1] Kaiho Tatsuo, "The Book of Iodine," published by Nikkan Kogyo Shimbun on June 25, 2015, p.16-23 Summary of the Invention [Problem to be solved by the invention]
[0006] In the industrial extraction of iodine from natural underground brine containing iodine atoms (hereinafter simply referred to as "brine"), it is necessary to efficiently extract the iodine component contained in the brine without loss. In particular, from the viewpoint of resource conservation, it is required to further improve the yield of iodine, which is a natural resource.
[0007] Furthermore, conventionally, when obtaining iodine, there was a problem that other components contained in the brine became insoluble and precipitated, thereby contaminating the equipment. [Means for solving the problem]
[0008] The present invention has been made to solve the above-mentioned problems, and can be realized by the following invention.
[0009] (1) A method for extracting iodine from brine, comprising the steps of: The above-mentioned irrigation Activated by contacting with a chlorine-based activating agent a pretreatment step of contacting the mixture with oxides of manganese; and an iodine obtaining step of obtaining iodine using the pretreated brine obtained through the pretreatment step.
[0010] (2) The manganese oxide to be subjected to the pretreatment step is one which has been contacted with the chlorine-based activation treatment agent and then washed with water not containing the chlorine-based activation treatment agent to remove the chlorine-based activation treatment agent remaining on the solid surface. The method for obtaining iodine described in (1) above.
[0012] ( 3 The total organic carbon (TOC) in the brackish water to be subjected to the pretreatment step is 10 mg / L or more. Or (2) The method for obtaining iodine described in the above.
[0013] ( 4 The iodine obtaining step is a step of obtaining iodine by a blowing out method, 3 ) A method for obtaining iodine according to any one of the above. Effect of the Invention
[0014] According to the present invention, it is possible to provide a method for obtaining iodine, which can prevent contamination of an iodine obtaining apparatus and can achieve a particularly excellent yield of iodine from brine. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram showing an example of a preferred embodiment of the method for obtaining iodine of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will now be described in detail. FIG. 1 is a diagram showing an example of a preferred embodiment of the method for obtaining iodine of the present invention.
[0017] The method for obtaining iodine of the present invention is a method for obtaining iodine from brine, and includes a pretreatment step of contacting the brine with manganese oxide, and an iodine obtaining step of obtaining iodine using the pretreated brine obtained through the pretreatment step.
[0018] This makes it possible to provide a method for obtaining iodine that can achieve a particularly excellent yield of iodine from brine while preventing contamination of the iodine obtaining apparatus.
[0019] In contrast, for example, if the pretreatment step of contacting the brine with manganese oxide is omitted and an oxidizing agent such as sodium hypochlorite is directly added to the brine to be used in the iodine extraction step, the iodine yield from the brine decreases, and furthermore, other components contained in the brine become insoluble and precipitate, contaminating the iodine extraction device.
[0020] [1] About irrigation The brine used in the present invention contains iodide ions (I - ). Economically preferable is the brine that remains after being pumped from an underground brine aquifer and having dissolved natural gas separated and extracted using a natural gas separation device. Furthermore, in the present invention, underground brines with variations in iodide ion concentration, oxidized matter concentration, and pH value, such as mixed brines collected from multiple wells at regular intervals, can also be used.
[0021] The content of iodide ions in the brine is not particularly limited, but is preferably 20 mg / L or more, more preferably 30 mg / L or more, and even more preferably 40 mg / L or more.
[0022] In the present invention, the mere mention of "iodine" means molecular iodine, which has the chemical formula I2.
[0023] Brine pumped from underground generally contains natural water-soluble polymers, such as polysaccharides having hydroxyl or carboxyl groups, humic substances such as humic acid and fulvic acid, and proteins.
[0024] The molecular weight of the water-soluble polymer contained in the brine is, for example, in the range of 500 or more and 2,000,000 or less.
[0025] [2] Water treatment Before the underground brine is subjected to each process described in detail below, it may be subjected to water treatment to remove impurities such as sand and suspended solids from the brine. Examples of water treatment include filtration and aeration.
[0026] By carrying out such water treatment, for example, insoluble matter contained in the brine and substances causing insoluble matter that may be generated in the process of obtaining iodine can be efficiently removed, the treatment efficiency in the pretreatment step described in detail later can be improved, and the iodine yield can be further increased and the time required for the method of obtaining iodine can be shortened, thereby further improving the productivity of iodine.
[0027] In particular, by carrying out the filtration treatment, it is possible to more suitably prevent the occurrence of contamination or clogging in the apparatus and piping used in the iodine obtaining step.
[0028] It is also preferable to aerate the brine with air or oxygen, for example, to precipitate iron ions contained in the brine as iron hydroxides or the like, and then filter and remove such precipitates (insoluble matter) using a filtering material.
[0029] This makes it possible to more effectively prevent contamination and clogging of the devices and piping used in the iodine obtaining step.
[0030] The filtration treatment can be carried out, for example, by subjecting the brine pumped from underground to a filtration treatment such as coagulation precipitation filtration, sand filtration, or porous membrane filtration, either alone or in combination.
[0031] The pore size of the porous filtration membrane is not particularly limited, but in view of the balance between removal performance and the amount of permeated water, the average pore size is preferably 0.01 μm or more and 1 μm or less.
[0032] Examples of the filtering material that can be used include particles of sand, coal, activated carbon, inorganic oxides or resins, and porous filtering membranes such as microfiltration membranes or ultrafiltration membranes.
[0033] For such water treatment, an insoluble matter removal device equipped with either or both of a filtration treatment device and an aeration treatment device is suitably used.
[0034] [3] Pretreatment process In the pretreatment step, the brine is brought into contact with manganese oxides.
[0035] It is believed that the pretreatment process causes the heavy metals contained in the brine to precipitate and be removed from the liquid phase, and also causes the water-soluble polymers to be modified, decreasing their reactivity with iodine.
[0036] Hereinafter, the brine after contact with manganese oxides, i.e., the brine that has been treated in the pretreatment step, will be referred to as "pretreated brine".
[0037] The brine subjected to the pretreatment process contains heavy metals even after water treatment; the total iron content is usually 0.10 mg / L or more, and the total manganese content is usually 0.05 mg / L or more.
[0038] In addition, even if the brine subjected to the pretreatment step has been subjected to water treatment, it contains water-soluble polymers, and the total organic carbon concentration (TOC), which is an indicator of water-soluble polymers, is usually 10 mg / L or more, and more specifically, for example, 20 mg / L or more and 200 mg / L or less.
[0039] As described above, when using brine having a relatively high heavy metal content and total organic carbon concentration, there have been problems in the past in that the iodine acquisition device is particularly susceptible to contamination and the yield of iodine from the brine is easily reduced, but according to the present invention, the yield of iodine from the brine can be particularly excellent while sufficiently preventing contamination of the iodine acquisition device. In other words, when using brine having a relatively high heavy metal content and total organic carbon concentration as described above, the effects of the present invention are more pronounced.
[0040] In the pretreatment process, manganese oxides oxidize heavy metal ions, such as iron ions and manganese ions, contained in the brine, producing metal oxides and metal hydroxides, etc. These can be adsorbed and removed as insoluble matter.
[0041] The manganese oxide used in the pretreatment step is, for example, MnO x (x is a number between 1 and 2), and more specifically, manganese oxide having an α-type, β-type, ε-type, γ-type, λ-type, δ-type or R-type crystal structure, or a combination of two or more selected from these, can be used. More specifically, for example, a composite of β-type manganese dioxide and γ-type manganese dioxide can be used.
[0042] Manganese ores containing manganese oxide can also be used. Additionally, complexes of manganese oxide containing metals other than manganese may also be used.
[0043] Furthermore, a support in which manganese oxide is supported on a support (for example, a powder-like, granular, honeycomb-like support) can be used.
[0044] As the carrier, for example, anthracite, zeolite, other ceramics, etc. Manganese oxide or a molded product of a manganese oxide carrier can also be used.
[0045] When powdered manganese oxide is used, the particle size of the manganese oxide is not particularly limited, but is preferably 0.2 mm or more and 5.0 mm or less, and more preferably 0.3 mm or more and 3.0 mm or less.
[0046] In addition, when a powdered manganese oxide is used, the bulk density of the manganese oxide is not particularly limited, but is preferably 1.0 g / cm 3 It is preferable that the content is 1.4 g / cm or more. 3 More preferably, it is equal to or greater than this.
[0047] Moreover, the manganese oxide may be a porous material. This makes it possible to increase the surface area per unit volume of the manganese oxide, and the above-mentioned effects are more pronounced.
[0048] The manganese oxide is preferably activated by contacting it with an activating agent.
[0049] This makes it possible to further enhance the oxidation activity against heavy metal ions and water-soluble polymers contained in the brine.
[0050] Examples of activation treatment agents used in the activation treatment of manganese oxide include chlorine, hypochlorite, chlorine dioxide, hydrogen peroxide, persulfate, ozone, etc., and from the standpoint of cost and oxidation activity, chlorine-based activation treatment agents such as sodium hypochlorite and chlorine are preferred, with sodium hypochlorite being particularly preferred.
[0051] The activation treatment agent may be mixed with the irrigation water before the pretreatment, in which case the activation treatment step or the activation frequency can be reduced.
[0052] This makes it possible to more significantly exert the effects described above. Furthermore, even if the activity of the manganese oxide used in the method for obtaining iodine of the present invention decreases, it can be suitably reactivated and reused.
[0053] The temperature at which the manganese oxide is brought into contact with the activation treatment agent is not particularly limited, but is preferably from 5°C to 40°C.
[0054] The time for which the manganese oxide is brought into contact with the activation treatment agent is not particularly limited, but is preferably 10 hours or less, and more preferably 0.1 to 3.5 hours.
[0055] After contacting the manganese oxide with the activating treatment agent, it is preferable to wash the manganese oxide with water that does not contain the activating treatment agent to remove any activating treatment agent remaining on the solid surface.
[0056] The pretreatment step can be carried out, for example, by passing brine through a pretreatment tank filled with oxides of manganese.
[0057] The flow rate of the brine to the pretreatment tank is not particularly limited, but is preferably at least 1 Hour in terms of spatial velocity. -1 More than 200 hours -1 It is preferable that the time is 5 hours or less. -1 More than 100 hours -1 It is more preferable that:
[0058] The pH of the brine to be subjected to the pretreatment step (for example, the brine passed through the pretreatment tank) is not particularly limited, but is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less. In addition, in order to adjust the pH of the brine, a pH adjuster such as hydrochloric acid or sulfuric acid may be added.
[0059] The temperature of the brine in the pretreatment step (for example, the temperature of the brine in the pretreatment tank) is not particularly limited, but is preferably 0°C or higher and 60°C or lower.
[0060] A plurality of pretreatment tanks may be arranged in series along the flow of irrigation water. This makes it easier to manage the pretreatment tank. A filtration device for filtering insoluble matters such as metal oxides and metal hydroxides may be provided downstream of the pretreatment tank.
[0061] In the pretreatment step, manganese oxide can be used continuously while passing brine. The activity of the manganese oxide gradually decreases as the water is passed through for a long period of time, but at that point, it can be reactivated and reused by carrying out an activation treatment in which the manganese oxide is brought into contact with an activating treatment agent.
[0062] A preferred embodiment of the present invention is a method in which a number of pretreatment tanks filled with manganese oxide are arranged in parallel, and the flow of brine is switched in sequence to the pretreatment tanks filled with active manganese oxide. That is, the flow of brine to the pretreatment tank in which the activity of the manganese oxide has decreased is stopped, and pretreatment is carried out using the other pretreatment tanks. Meanwhile, the pretreatment tank in which the activity has decreased is subjected to activation treatment by supplying an activating agent to reactivate the manganese oxide, in preparation for the flow of brine in the next switchover.
[0063] The pretreatment step reduces the concentrations of heavy metals contained in the brine. The heavy metal contents in the pretreated brine obtained by the pretreatment step are preferably less than 0.10 mg / L for total iron and less than 0.05 mg / L for total manganese. This makes it possible to more effectively prevent contamination of the iodine obtaining device.
[0064] As described above, the total iron content in the pretreated brackish water obtained in the pretreatment step is preferably less than 0.10 mg / L, and more preferably less than 0.05 mg / L. This makes the above-mentioned effects more pronounced.
[0065] As described above, the total manganese content in the pretreated brackish water obtained in the pretreatment step is preferably less than 0.05 mg / L, and more preferably less than 0.01 mg / L. This makes the above-mentioned effects more pronounced.
[0066] The pretreatment step does not necessarily oxidize the water-soluble polymers contained in the brine to the point where they are completely decomposed.
[0067] It is believed that in the pretreatment step, the water-soluble polymer is denatured by manganese oxide, which changes the structure and physical properties of the water-soluble polymer, thereby reducing the chemical or physical bonding strength between the water-soluble polymer and iodine.
[0068] [4] Iodine extraction process The pretreated brine that has been subjected to the pretreatment step is subjected to an iodine extraction step, in which iodine is separated and extracted from the pretreated brine.
[0069] More specifically, in the iodine acquisition process, the iodide ions contained in the brine are converted to molecular iodine (I2) by an oxidation reaction caused by an oxidizing agent such as chlorine or sodium hypochlorite. Hereinafter, the brine containing molecular iodine as a result of the iodide ions being oxidized by an oxidizing agent is referred to as "oxidized brine."
[0070] In the present invention, the pretreated brine obtained through the pretreatment step has a reduced heavy metal content and a reduced reactivity of the water-soluble polymer with iodine. Therefore, it is considered that the pretreated brine can effectively prevent undesirable side reactions of iodide ions (e.g., reactions with organic matter) from proceeding in the iodine obtaining step, and the iodine yield is excellent.
[0071] In the iodine acquisition step, iodine can be acquired from iodide ions contained in the pretreated brine by using an iodine acquisition method such as the blowing out method or the ion exchange resin method. An apparatus that performs the iodine acquisition step is called an iodine acquisition apparatus.
[0072] The present invention significantly improves the iodine yield in an iodine obtaining apparatus using the blowing out method and the ion exchange resin method.
[0073] In particular, by performing the iodine obtaining step by the blowing out method, iodine can be obtained by treating a large amount of water economically, as compared with the ion exchange resin method. Also, as compared with the case where the blowing out method is performed without carrying out a pretreatment step, the iodine yield from the brine can be particularly excellent while preventing contamination of the iodine stripper tower, which is an iodine obtaining device.
[0074] In addition, by carrying out the iodine obtaining step by the ion exchange resin method, iodine can be obtained economically by treating a small amount of water compared to the blowing out method. Also, compared to the case where the ion exchange resin method is carried out without carrying out the pretreatment step, it is possible to prevent contamination of the iodine adsorption tower, which is an iodine obtaining device, and to obtain a particularly excellent iodine yield from the brine.
[0075] The blowing-out method involves adding an oxidizing agent to pretreated brine, then blowing in air to volatilize the molecular iodine produced, which is then absorbed in an absorbing solution containing a reducing agent, and adding an oxidizing agent to the absorbing solution to reoxidize it and obtain iodine.
[0076] Specifically, the process for obtaining iodine by the blowing out method is a process for obtaining iodine from brine, which includes: an oxidation step in which a chlorine-based oxidizing agent such as chlorine or sodium hypochlorite is mixed with the pretreated brine to produce oxidized brine containing iodine; a stripping step in which the oxidized brine after the oxidation step is sent to a stripping tower equipped with a blower and a gas such as air is blown in to vaporize the iodine; an absorption step in which the iodine-containing gas released from the stripping tower in the stripping step is brought into contact with an aqueous solution containing a reducing agent such as sulfurous acid or sodium (bis)sulfite in an absorption tower to obtain an absorption liquid containing a high concentration of iodide ions; and a crystallization step in which an oxidizing agent such as chlorine or sodium hypochlorite is added to the obtained absorption liquid to produce and obtain solid iodine.
[0077] The oxidation step by mixing an oxidizing agent in the blowing out method is preferably carried out under conditions in which the pH of the oxidizing brine to which the oxidizing agent has been added is in the acidic or neutral range. More specifically, the pH of the oxidizing brine in the oxidation step is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less.
[0078] In the ion exchange resin method, an oxidizing agent is added to the pretreated brine, and then polyiodine ions are generated via the generated molecular iodine. In this method, the oxidized brine containing polyiodine ions is brought into contact with an ion exchange resin, the adsorbed polyiodine ions are eluted, and an oxidizing agent is added to the eluate to reoxidize it and obtain iodine.
[0079] The iodine extraction process using the ion exchange resin method involves mixing a chlorine-based oxidizing agent, such as chlorine or sodium hypochlorite, with the pretreated brine to extract I3 - the like; an adsorption step in which the polyiodine ion-containing brine after the oxidation step is sent to an adsorption tower filled with an anion exchange resin and the polyiodine ions are adsorbed onto the anion exchange resin; an elution step in which the anion exchange resin is sent to an elution tower and the adsorbed polyiodine ions are eluted by contacting it with an eluent such as sulfurous acid, sodium (bis)sulfite, etc.; and a crystallization step in which an oxidizing agent such as chlorine, sodium hypochlorite, etc. is added to the eluate to produce and obtain solid iodine.
[0080] The oxidation step using an oxidizing agent in the ion exchange resin method is preferably carried out under conditions in which the pH of the oxidizing brine to which the oxidizing agent has been added is in the acidic or neutral range. More specifically, the pH of the oxidizing brine in the oxidation step is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less.
[0081] In the iodine acquisition process, iodine that forms an organic compound by chemically or physically bonding with a water-soluble polymer contained in the brine (hereinafter referred to as "organic iodine") is generated. According to the study by the present inventors, the organic iodine in the oxidized brine is difficult to vaporize in the stripping step of the blowing out method and difficult to adsorb to the anion exchange resin in the adsorption step of the ion exchange resin method, and is discharged without being used. Therefore, the generation of organic iodine in the iodine acquisition process reduces the yield of iodine.
[0082] On the other hand, in the present invention, the generation of organic iodine is suppressed. The cause of this is presumably that the pretreatment process of the brine causes the molecular chains or functional groups of the water-soluble polymers in the brine to be oxidized by manganese oxides, and the primary or higher structure of at least some of the water-soluble polymers is changed or the polymers are degraded, making them inactive and no longer capable of forming stable chemical or physical bonds with iodine. Although the pretreatment process presumably causes the water-soluble polymers to be denatured, the color of the brine may not be removed.
[0083] In short, the treated brine that has been subjected to the pretreatment step of the present invention has a reduced organic iodine concentration and a significantly increased molecular iodine concentration in the iodine extraction step, compared to the brine that has not been subjected to the pretreatment step, which results in an improved yield of iodine from iodide ions contained in the brine in the iodine extraction step.
[0084] It is known that natural brine pumped from underground contains heavy metals and water-soluble polymers, but it was not known that this is related to the acquisition of iodine. Furthermore, it was not known that the yield of iodine in the iodine acquisition process can be improved by contacting the brine with manganese oxide.
[0085] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these. For example, modifications such as changing conditions or adding other steps may be made within the scope of the gist of the present invention. EXAMPLES
[0086] The present invention will be described in detail below based on examples, but the present invention is not limited thereto.
[0087] [5] Implementation of iodine acquisition method Example 1 First, manganese oxide A (manganese oxide (MnO x A pretreatment tank was prepared by filling the tank with 100 mL of ceramic particles (manufactured by Tokemi Corporation, product name Radical Light UC3) carrying 12% by mass sodium hypochlorite aqueous solution, and then washing the tank with 3 L of water mixed with 6.76 g of sodium hypochlorite aqueous solution at a space velocity of 10 H -1 The pretreatment tank was then backwashed with ion-exchanged water to prepare a pretreatment tank filled with activated manganese oxide.
[0088] Next, the brine A (iodide ion content 35 mg / L, TOC content 40 mg / L, total iron content 0.15 mg / L, total manganese content 0.10 mg / L) that had been aerated with air and filtered with anthracite was introduced into the pretreatment tank prepared as described above at a space velocity of 60 H -1 The pretreatment step was carried out by continuously passing water through the mixture at 25 to 30°C.
[0089] The pretreated brine discharged from the outlet of the pretreatment tank was collected for 60 minutes from 60 to 120 minutes after the start of irrigation.
[0090] Using the collected pretreated brine, a 12% by mass aqueous solution of sodium hypochlorite was added, and an oxidation reaction was carried out to generate molecular iodine, and iodine was obtained by the blowing-out method. The results are shown in Table 1. The TOC of the brine discharged after the iodine extraction process was 40 mg / L, the total iron content was 0.05 mg / L, and the total manganese content was 0.01 mg / L.
[0091] Example 2 The manganese oxide used in the pretreatment process was manganese oxide B (manganese oxide (MnO x Iodine was obtained by carrying out the same method as in Example 1, except that the ceramic particles (manufactured by Nihon Genryo Co., Ltd., product name New Color Cutter Light) carrying iodine (x is a number of 1 or more and 2 or less) were used. The results are shown in Table 1.
[0092] Example 3 Iodine was obtained by carrying out the same method as in Example 1, except that the brine before the pretreatment step was aerated with air and filtered with anthracite, and then sulfuric acid was added as an additive to adjust the pH to 6.0. The results are shown in Table 1.
[0093] Example 4 Iodine was obtained by carrying out the iodine extraction method in the same manner as in Example 1, except that brine B (iodide ion content 38 mg / L, TOC 50 mg / L, total iron content 0.35 mg / L, total manganese content 0.25 mg / L) was used as the brine passed through the pretreatment step. The results are shown in Table 2. The brine discharged after the iodine extraction step had a TOC of 50 mg / L, a total iron content of 0.10 mg / L, and a total manganese content of 0.01 mg / L.
[0094] Comparative Example 1 Iodine was obtained by carrying out the iodine obtaining method in the same manner as in Example 1, except that the pretreatment step was omitted.
[0095] That is, using the brine A that had been subjected to an aeration process using air and filtration using anthracite, a 12% by mass aqueous solution of sodium hypochlorite was added, and an oxidation reaction was carried out to generate molecular iodine, and iodine was obtained by the blowing-out method. The results are shown in Table 1. The TOC of the brine discharged after the iodine extraction process was 40 mg / L, the total iron content was 0.15 mg / L, and the total manganese content was 0.10 mg / L.
[0096] Comparative Example 2 Iodine was obtained by carrying out the iodine obtaining method in the same manner as in Example 1, except that anthracite (manufactured by Tokemi Corporation, product name Anthracite 0.6 mm) was used instead of manganese oxide in the pretreatment step. The results are shown in Table 1.
[0097] Comparative Example 3 Iodine was obtained by carrying out the iodine obtaining method in the same manner as in Example 4, except that the pretreatment step was omitted.
[0098] That is, using the brine B that had been subjected to an aeration process using air and filtration process using anthracite, a 12% by mass aqueous solution of sodium hypochlorite was added, and an oxidation reaction was carried out to generate molecular iodine, and iodine was obtained by the blowing-out method. The results are shown in Table 2. The TOC of the brine discharged after the iodine extraction process was 50 mg / L, the total iron content was 0.35 mg / L, and the total manganese content was 0.25 mg / L.
[0099] For each of the Examples and Comparative Examples, the treatment conditions for the iodine extraction method when brine A was used are summarized in Table 1, and the treatment conditions for the iodine extraction method when brine B was used are summarized in Table 2.
[0100] In addition, the molecular iodine (I2) concentration, organic iodine concentration, and total iodine concentration of the brine (oxidized brine) collected in the oxidation process are summarized in Tables 1 and 2.
[0101] In addition, the organic iodine concentration and total iodine concentration of the brine collected in the iodine extraction process (brine after iodine extraction) are summarized in Tables 1 and 2.
[0102] Tables 1 and 2 show the ratio of iodine (I2) finally obtained by carrying out the iodine obtaining method to the iodide ions contained in the brine A or B, respectively, and the presence or absence of visual contamination of the iodine obtaining device after carrying out the iodine obtaining method, respectively.
[0103] [Table 1]
[0104] [Table 2]
[0105] As is clear from Tables 1 and 2, excellent results were obtained in each of the Examples, whereas satisfactory results were not obtained in each of the Comparative Examples.
[0106] By carrying out the present invention, the generation of organic iodine is suppressed and the molecular iodine concentration is significantly increased in the iodine acquisition process, thereby improving the yield of iodine from iodide ions contained in the brine in the iodine acquisition process. [Industrial Applicability]
[0107] The method for obtaining iodine of the present invention is a method for obtaining iodine from brine, and includes a pretreatment step of contacting the brine with manganese oxide, and an iodine obtaining step of obtaining iodine using the pretreated brine obtained through the pretreatment step.
[0108] According to the method for obtaining iodine of the present invention, it is possible to provide a method for obtaining iodine that can prevent contamination of an iodine obtaining apparatus while achieving a particularly excellent yield of iodine from brine. Therefore, the method for obtaining iodine of the present invention has industrial applicability.
Claims
1. A method for obtaining iodine from brine, comprising the steps of: a pretreatment step of contacting the brine with manganese oxide activated by contacting the brine with a chlorine-based activation treatment agent; and an iodine obtaining step of obtaining iodine using the pretreated brine obtained through the pretreatment step.
2. The method for obtaining iodine described in Claim 1, wherein the manganese oxide to be subjected to the pretreatment step is one from which the chlorine-based activation treatment agent has been brought into contact with the manganese oxide and then washed with water not containing the chlorine-based activation treatment agent to remove the chlorine-based activation treatment agent remaining on the solid surface.
3. 3. The method for obtaining iodine according to claim 1, wherein the total organic carbon (TOC) in the brackish water subjected to the pretreatment step is 10 mg / L or more.
4. The method for obtaining iodine according to claim 1 , wherein the iodine obtaining step is a step of obtaining iodine by a blowing out method.
Citation Information
Patent Citations
JP1973018156B1
Preparation of filter mediom for water disposal
JP1984012794A
Filter material for purifying water
JP1985005215A
Method for removing manganese and equipment therefor
JP2003305485A
Manufacturing method of iodine from oil field brine
JP2005187306A