Metallic film-formed nonwoven fabric and its manufacturing method

Dispersed metal film pieces on nonwoven fabrics address uneven electron movement and antibacterial inefficiencies, enhancing filter lifespan and reducing waste through cost-effective production.

JP7586437B2Active Publication Date: 2024-11-19SEIWA ELECTRIC MFG CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022006352
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-19
Publication Date
2024-11-19
Estimated Expiration
2042-01-19

AI Technical Summary

Technical Problem

Conventional methods for forming metal films on nonwoven fabrics result in uneven electron movement and antibacterial effects, leading to inefficient use and waste due to uneven dust capture and frequent replacement of sterilizing filters.

Method used

A method involving a metal precursor liquid with metal complexes, ammonia, and an organic reducing agent is used to form metal film pieces on nonwoven fabrics, ensuring dispersed formation with high electrical resistance, preventing electron movement inhibition and maintaining antibacterial efficacy.

Benefits of technology

The dispersed metal film pieces on nonwoven fabrics ensure even antibacterial action and reduce waste by extending the lifespan of filters, allowing for cost-effective production and efficient electron movement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586437000003
    Figure 0007586437000003
  • Figure 0007586437000004
    Figure 0007586437000004
  • Figure 0007586437000005
    Figure 0007586437000005
Patent Text Reader

Abstract

To provide a metal film piece formation nonwoven fabric capable of achieving preferable antibacterial effects even in the nonwoven fabric including incorporated filaments, and capable of being produced easily and inexpensively, and a production method of the same.SOLUTION: There is provided a metal film piece formation nonwoven fabric formed by forming in a dispersed state, metal film pieces, on a surface of each filament forming the nonwoven fabric, by immersing the nonwoven fabric in a metal formation composition which includes: a metal precursor liquid which has a reaction product being formed of at least one kind selected from, a metal complex, and a metal salt, and at least one kind selected from ammonia and amine, and an organic reductant, then drying the nonwoven fabric, in the metal film piece formation nonwoven fabric, electric resistance between two points on a plane and between two points on front and rear faces, is greater than or equal to 100 MΩ.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal film flake-formed nonwoven fabric obtained by providing a metal in a dispersed state to a nonwoven fabric, and to a method for producing the same. [Background technology]

[0002] In general, deodorizing fiber sheets and bactericidal filters are known that have deodorizing and sterilizing effects achieved by forming a film of a metal such as Cu on fibers such as nonwoven fabric (see, for example, Patent Documents 1 to 3).

[0003] Conventionally, a method for forming a metal film on fibers such as nonwoven fabrics has been to immerse the fibers in a special solution and then dry them, producing a film that has good electrical and thermal conductivity (see, for example, Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 52-44458 [Patent Document 2] Japanese Patent Application Publication No. 58-8530 [Patent Document 3] JP 2006-14965 A [Patent Document 4] Patent Publication No. 2021-70873 Summary of the Invention [Problem to be solved by the invention]

[0005] However, as in the above-mentioned conventional film-forming method, when the film is formed so that the electrical conductivity and thermal conductivity are good, electrons can freely move in a wide range of the metal film on the surface of the substrate. That is, in the metal film formed by the above-mentioned conventional film-forming method, electrons are released from the surface of the monovalent copper compound, react with oxygen in the air to generate superoxide, and the superoxide reacts with moisture in the air to generate active oxygen, which exerts antibacterial properties. However, since the entire bactericidal filter formed by the metal film is a conductor, if a potential difference occurs at a specific part of the metal film due to an external factor, the movement of free electrons is restricted, and the electron emission is easily biased, making it difficult for the entire metal film to exert an antibacterial effect evenly. In particular, when the substrate on which the metal film is formed has a thickness like a nonwoven fabric and the environment is completely different between the surface and the inside, this phenomenon becomes significant, and excellent antibacterial performance cannot be obtained.

[0006] In addition, when the bactericidal filter made of the metal film is used as a purification filter for various fluids, the bactericidal filter is used to capture dust in the fluid that has passed through the bactericidal filter to purify the fluid, but in this case, the dust is not captured evenly in the thickness direction of the bactericidal filter, but is usually captured from the upstream side surface through which the fluid passes. Therefore, even if the downstream side surface of the bactericidal filter is clean, the upstream side surface is clogged with dust, so a guideline for replacement is given for one to several months, and disposable types are usually used by replacing with a new one each time. Therefore, even if a dense metal film is formed to have good electrical conductivity, the bactericidal filter itself must be replaced with a new one before the antibacterial effect of the metal film is exhausted, and the manufacturing cost for forming a dense metal film that ensures electrical conductivity and the densely formed metal film itself are wasted.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a metal film piece-formed nonwoven fabric and a manufacturing method thereof that can obtain a good antibacterial effect even when a metal film is formed on a substrate having an intricate filament structure such as a nonwoven fabric, and that can be manufactured simply and inexpensively. [Means for solving the problem]

[0008] In order to solve the above problems, the metal film flake-forming nonwoven fabric of the present invention is obtained by immersing the nonwoven fabric in a composition for forming a metal film, the composition comprising a metal precursor liquid having a reaction product of at least one selected from the group consisting of metal complexes and metal salts with at least one selected from ammonia and amines, and an organic reducing agent, and then drying the nonwoven fabric, so that metal film flakes are formed on the surface of each filament constituting the nonwoven fabric. but Formed in a dispersed state Be Tenari, Plane all Between two points, front and back all The electrical resistance between the two points is 100MΩ or more. After cutting into 30 mm x 30 mm pieces and sterilizing, the pieces were placed in a sterilized petri dish, and 0.1 ml of a test bacterial solution containing NBRC3972 Escherichia coli in a phosphate buffer solution at a concentration of 9 x 105 to 3 x 106 cfu / ml was dropped onto the dish. After culturing for 24 hours at 35 ± 1°C, the dish was thoroughly washed out using 9.9 ml of SCDLP medium, and then serially diluted to 1:10,000 with diluted water. Each diluted bacterial solution was cultured for 48 hours at 35 ± 1°C using the agar plate culture method, and the resulting viable cell count was 0. This is what was done.

[0010] The metal of the metal film piece-formed nonwoven fabric may be Cu.

[0011] In the above-mentioned metal film piece-forming nonwoven fabric, the nonwoven fabric may be made of natural fibers or resin fibers.

[0012] The method for producing a metal piece-formed nonwoven fabric of the present invention that solves the above problems is as follows: A step of immersing a nonwoven fabric in a composition for forming a metal film piece, the composition comprising a metal precursor liquid having a reaction product of at least one selected from the group consisting of a metal complex and a metal salt with at least one selected from ammonia and an amine, and an organic reducing agent; and drying the nonwoven fabric after the immersion. The method for manufacturing a metal film-formed nonwoven fabric includes forming metal film pieces in a dispersed state on the surface of each filament constituting the nonwoven fabric, so that the electrical resistance between two points on the entire plane and between two points on the front and back is 100 MΩ or more. The nonwoven fabric is cut into a size of 30 mm x 30 mm, sterilized, and placed in a sterilized petri dish, and 0.1 ml of a test bacteria solution prepared by adjusting NBRC3972 Escherichia coli to a concentration of 9 x 105 to 3 x 106 cfu / ml in phosphate buffer is dropped onto the test bacteria solution. After culturing at 35 ± 1 ° C for 24 hours, the test bacteria solution is thoroughly washed out using 9.9 ml of SCDLP medium, and then diluted stepwise to 1:10000 diluted water. Each diluted bacteria solution is cultured by the agar plate culture method at 35 ± 1 ° C for 48 hours, and the immersion time, immersion pressure, and number of immersions and drying times are adjusted so that the viable bacteria count obtained is 0. It is something.

[0014] The method for producing the metal film piece-formed nonwoven fabric may involve one cycle of immersion and drying at atmospheric pressure for one day.

[0015] [Metal precursor liquid] The metal precursor liquid is obtained by reacting at least one selected from the group consisting of a metal complex and a metal salt with at least one selected from ammonia and an amine in a mixed liquid of at least one selected from the group consisting of a metal complex and a metal salt, at least one selected from ammonia and an amine, and a solvent.

[0016] [At least one selected from the group consisting of metal complexes and metal salts] The at least one selected from the group consisting of the above metal complexes and metal salts may be only one or more types of metal complexes, only one or more types of metal salts, or a mixture containing both one or more types of metal complexes and one or more types of metal salts.

[0017] The metal complex is preferably a reaction product of one or more compounds for forming a metal complex selected from compounds having a partial structure of a NH3 ligand, an RNH2 ligand (R represents an alkylene group), an OH2 ligand, and a ligand derived from a diamine such as ethylenediamine or hexamethylenediamine, which can generate a metal complex, and a metal ion. The metal complex may be a metal complex previously generated by the above reaction. As the metal in the metal complex, a metal according to the purpose of the metal film to be formed may be used. Examples of the metal include silver (Ag), copper (Cu), lithium (Li), nickel (Ni), manganese (Mn), zinc (Zn), and cobalt (Co). Specific examples of the metal complex include ethylenediaminetetraacetate copper, tetraammine copper, and the like, which contain copper (Cu) as a metal.

[0018] The metal salt is a metal compound having a function of dissociating in a solvent containing water to become metal ions and forming a metal complex. The metal salt refers to a metal salt that is soluble in water at 25°C. Soluble in water at 25°C means that the solubility in water at 25°C is 0.1% by mass or more, and the solubility is preferably 1% by mass or more. When the metal salt is soluble in water, the metal salt dissociates in a solvent containing water to become metal ions, and the metal ions react with amines contained in the solvent to obtain a metal complex. Furthermore, when a compound for forming a complex described later is optionally contained in the solvent, the metal ions may react with the compound for forming a complex to form a metal complex.

[0019] [At least one selected from ammonia and amines] The at least one selected from the above ammonia and amine may be only one or more types of ammonia, may be only one or more types of amine, or may be a mixture containing both one or more types of ammonia and one or more types of amine. These may be included as salt compounds. The amines include primary amines, secondary amines, and tertiary amines. Specific examples of amines include alkylamines. Instead of amines or in addition to amines, ammonia may be included. As ammonia, various substances having basicity similar to amines can be used.

[0020] [solvent] The solvent is not particularly limited as long as it can dissolve at least one selected from the group consisting of the above-mentioned metal complexes and metal salts, and at least one selected from the above-mentioned ammonia and amines, and for example, an aqueous solvent such as water or a mixture of water and alcohol can be used. It is preferable that the water contains a small amount of impurities, particularly ions other than metal ions, and from this viewpoint, it is preferable to use purified water, ion-exchanged water, pure water, etc. Examples of alcohol include monohydric alcohols having 1 to 10 carbon atoms, such as methanol, ethanol, isopropanol, n-propanol, isobutanol, and n-butanol, and polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, and glycerin.

[0021] From the viewpoint of solubility and handling, the aqueous solvent is preferably water or a mixture of water and a monohydric alcohol having 1 to 5 carbon atoms, more preferably water or a mixture of water and an alcohol selected from methanol, ethanol and propanol, and even more preferably water. When using a mixture of water and alcohol as a solvent, the mixing ratio is appropriately selected depending on the purpose. When using a mixture of water and alcohol as a solvent, the content of alcohol in the total amount of the mixture of water and alcohol is preferably 1% by mass to 60% by mass.

[0022] [Preparation of metal precursor liquid] The metal precursor liquid can be prepared by adding at least one selected from the group consisting of the above-mentioned metal complexes and metal salts, and at least one selected from the above-mentioned ammonia and amines in a solvent, and thoroughly stirring and mixing the mixture.

[0023] Mixing may be performed at room temperature, or for the purpose of promoting dissolution, the solvent may be heated to 40° C. to 60° C. The stirring method is not particularly limited, and any known stirring method can be used, such as a method of putting the mixed solution into a container and stirring it using a rotor such as a magnetic stirrer, a method of stirring with a stirring device equipped with a rotary stirring blade such as a paddle, a method of putting the solution into a sealable container and stirring by shaking the container, and a method of irradiating with ultrasound.

[0024] A simple method is to use a stirring device equipped with a stirring blade. The rotation speed of the rotor can be 300 rpm (revolutions / minute: the same below) to 800 rpm, and preferably 400 rpm to 600 rpm. The stirring is preferably performed until the reaction between at least one selected from the group consisting of the above-mentioned metal complexes and metal salts and at least one selected from the above-mentioned ammonia and amines proceeds sufficiently, and when stirring is performed at room temperature using the above-mentioned stirring device equipped with a rotor, stirring is preferably performed for about 30 minutes to 90 minutes, and more preferably for about 50 minutes to 80 minutes. For example, when preparing a metal precursor liquid containing a copper complex, the metal precursor liquid that has been thoroughly stirred exhibits a blue color due to copper ions.

[0025] The above-mentioned metal precursor liquid may be prepared by applying a known molecular precursor method. In addition, the preparation of the metal precursor liquid can be performed by applying a known precursor method as described above, but from the viewpoint of obtaining a metal precursor with higher purity, it is preferable to include the following electrolysis step. That is, this electrolysis step is a step of storing an amine-containing electrolytic solution in each of the pair of electrolytic solution tanks in a reaction apparatus equipped with a pair of electrolytic solution tanks connected via a flow path equipped with a filter that does not allow metal ions to pass through but can allow hydrogen ions to pass through, and arranging a pair of metal electrodes at a position where at least a part of the electrodes contacts the electrolytic solution, and connecting the pair of electrodes via a DC power source, and applying a voltage between the pair of electrodes by a DC power source, and reacting the metal ions derived from the metal that is the electrode with the electrolytic solution in the electrolytic solution tank in which the electrode that becomes the anode is immersed to obtain a metal precursor liquid.

[0026] [Organic reducing agents] The organic reducing agent preferably includes at least one selected from compounds having a carboxy group. The organic reducing agent is preferably appropriately selected from organic carboxylic acid compounds having a carboxy group in the molecule and functioning as a reducing agent.

[0027] Examples of the organic reducing agent include at least one selected from ascorbic acid, citric acid, oxalic acid, formic acid, and 3,4,5-trihydroxybenzoic acid, and from the viewpoint of better formability of the metal film pieces, at least one selected from ascorbic acid, citric acid, and 3,4,5-trihydroxybenzoic acid is preferable, and at least one selected from ascorbic acid and citric acid is more preferable. One of the preferred aspects of the composition for forming metal film pieces is to include ascorbic acid as the organic reducing agent.

[0028] The organic reducing agent is preferably used as an aqueous solution. The water used to prepare the aqueous solution does not contain metal ions or has a metal ion concentration as low as possible from the viewpoint of uniformity of the obtained metal film. Therefore, the water used to prepare the aqueous solution is preferably purified water, ion-exchanged water, pure water, etc., for example. When dissolving the organic reducing agent in water, the water as the solvent may be heated to 30°C to 60°C, preferably to 35°C to 45°C, for the purpose of improving solubility. The dissolution may be performed with stirring, and the stirring method mentioned in the above-mentioned section on the method for preparing the solution of the metal complex can be appropriately applied in the same manner. The content of the specific reducing agent in the aqueous solution of the organic reducing agent is preferably in the range of 10% by mass to 40% by mass, more preferably in the range of 10% by mass to 30% by mass. When the content of the organic reducing agent relative to the total amount of the aqueous solution is 10% by mass or more, the aqueous solution contains a sufficient amount of organic reducing agent for the reaction, and when the content is 40% by mass or less, the stability of the aqueous solution is better.

[0029] [Preparation of composition for forming metal film pieces] The metal film piece forming composition is obtained by mixing the metal precursor liquid and the organic reducing agent, and the mixing ratio of the metal precursor liquid and the organic reducing agent is not particularly limited and can be appropriately selected according to the target metal. The metal ion contained in the metal precursor liquid can be 50 parts by mass to 400 parts by mass relative to 100 parts by mass of the organic reducing agent contained in the metal film piece forming composition, and from the viewpoint of obtaining a better formability of the metal film piece of the metal film piece forming composition, it is preferable that the metal ion contained in the metal precursor liquid is 100 parts by mass to 350 parts by mass relative to 100 parts by mass of the organic reducing agent, and it is more preferable that the metal ion contained in the metal precursor liquid is 150 parts by mass to 350 parts by mass relative to 100 parts by mass of the organic reducing agent.

[0030] By setting the content of metal ions relative to the organic reducing agent within the above preferred range, metal film pieces can be formed more efficiently on the surface of each filament constituting the nonwoven fabric. If the mixing ratio of the metal precursor liquid to 100 parts by mass of the organic reducing agent is less than 50 parts by mass, the metal is difficult to precipitate quickly, and if it exceeds 400 parts by mass, the reducing power of the metal ions becomes insufficient. The content of the metal precursor liquid in the preparation of the composition for forming metal film pieces can be controlled by adjusting the type and content of the metal complex when preparing the metal precursor liquid, or the type of electrolyte, the concentration of the electrolyte, the applied energy of the direct current, the application time, etc. in the electrolysis process when preparing the above-mentioned metal precursor liquid.

[0031] In general, it is difficult to measure the content of a specific metal compound relative to the total amount of the composition for forming metal film pieces. However, the physical properties of the metal film pieces formed by the composition for forming metal film pieces depend on the metal content in the composition for forming metal film pieces. From the viewpoint of forming stable metal film pieces, the metal content relative to the total amount of the composition for forming metal film pieces is preferably in the range of 0.5% by mass to 10% by mass, and more preferably in the range of 1% by mass to 8% by mass. When the metal content is in the above range, the structure of the metal film pieces formed by the composition for forming metal film pieces becomes more uniform, and stable metal film pieces can be formed.

[0032] The metal content in the composition for forming metal film pieces can be measured, for example, by the method described in "Basics of Coordination Chemistry: Werner Complexes and Organometallic Complexes" (KS Chemistry Specialist Book: Kodansha, 1989).

[0033] The content of the specific reducing agent in the composition for forming metal film pieces can be measured, for example, by the following method. First, the composition for forming metal film pieces is dried to prepare a powder. The obtained powder is analyzed using a thermogravimeter-differential thermal analyzer (TG-DTA) to measure the content of the specific reducing agent.

[0034] The pH of the composition for forming metal film pieces at room temperature (25° C.) is preferably 6 to 8, and more preferably in the neutral range of about pH 7.5. The pH can be measured with a known pH meter.

[0035] [Nonwoven fabric] The nonwoven fabric is not particularly limited as long as it is formed in a sheet shape, and can be appropriately selected according to the purpose. The nonwoven fabric may be one using various natural fibers such as silk, cotton, cellulose, and hemp as filaments, or one using various resin fibers such as polyethylene such as PET, low density polyethylene (LDPE), and high density polyethylene (HDPE), polycarbonate (PC), polyvinyl chloride (PVC), polystyrene, acrylic resin such as polymethyl methacrylate (PMMA), polyamide such as nylon 6, phenol resin, melamine resin, and urethane resin as filaments, one using carbon fiber as filaments, one using glass fiber as filaments, or one or more types of filaments selected from these may be mixed. In addition, the length and thickness of each filament constituting the nonwoven fabric may be the same, or the nonwoven fabric may be composed of filaments of different lengths and thicknesses. In addition, the nonwoven fabric may be composed of a combination of multiple types of filaments of different lengths and thicknesses. The basis weight of the nonwoven fabric is not particularly limited, and may be 20 g / m 2 More than 200g / m 2 The following ranges are particularly preferred: The thickness of the nonwoven fabric is not particularly limited as long as it is in sheet form, but it is preferable to use one in the range of 50 μm to 5 mm, particularly 140 μm to 760 μm.

[0036] [Production of metal film-formed nonwoven fabric] The metal film piece-formed nonwoven fabric is manufactured by immersing the nonwoven fabric in the metal film piece-formed composition and drying it, so that the metal film pieces are dispersed and formed on the surface of each filament constituting the nonwoven fabric. In this case, the immersion time, immersion pressure, and number of immersions and drying are not particularly limited as long as the conditions are such that the metal film pieces can be formed in a dispersed state on the surface of each filament constituting the nonwoven fabric so that the electrical resistance between two points on the plane of the completed metal film piece-formed nonwoven fabric and between two points on the front and back is non-conductive to 100 MΩ or more. The immersion time, immersion pressure, and number of immersions and drying are each subjected to a batch test, and the immersion time, immersion pressure, and number of immersions and drying that satisfy the corresponding conditions can be adopted. The immersion time is preferably 6 hours or more at room temperature (25°C), for example, and more preferably 12 hours or more. When the membrane thickness is to be increased, the immersion time or storage time can be 24 hours or more.

[0037] There is no particular limit to the upper limit of the immersion time, but from the viewpoint of productivity, it can be 120 hours or less, and preferably 90 hours or less. In this case, by setting the temperature of the composition for forming metal film pieces to room temperature or higher, for example, 30°C or higher, preferably 40°C or higher, the reaction rate increases and metal film pieces can be formed in a shorter storage time. From the viewpoint of not affecting the composition for forming metal film pieces, the temperature is preferably 80°C or less. For example, when the atmospheric temperature is 35°C, the storage time is preferably 4 hours or more, and more preferably 8 hours or more. The upper limit of the storage time is the same as that at room temperature.

[0038] The immersion pressure may be normal atmospheric pressure, or may be reduced pressure or increased pressure. The immersion may be performed without degassing the air bubbles trapped between the filaments, or may be performed after degassing. When degassing, the nonwoven fabric surface may be physically pressed, or the immersion pressure may be changed.

[0039] Drying can be performed by a conventional method such as natural drying, heat drying, and blow drying, which are generally performed. In the case of natural drying, it is sufficient to leave it at room temperature for 60 minutes to 5 hours. In the case of heat drying, a known heating means can be appropriately selected and applied. Examples of the heating method include a method of contacting a heating means such as a plate-shaped heater or a heat roll from the back side of the substrate, a method of passing through a heating zone such as an electric furnace, a method of irradiating energy rays such as infrared rays or microwaves, and a method of blowing hot air. There is no particular limit to the heating temperature during heat drying. Considering the drying efficiency and suppression of the influence on the substrate, the heating temperature can be in the range of 30°C or more and less than 100°C, and is preferably in the range of 30°C to 60°C. From the viewpoint of productivity, the drying time during heat drying is preferably in the range of 10 seconds to 20 minutes. In the case of blow drying, it may be blown with air under the environmental atmosphere, or it may be blown with hot air as described above.

[0040] The amount of metal that constitutes the metal film piece by the metal film piece forming composition is not particularly limited, but in fact, when the metal film piece forming nonwoven fabric is used as a filter for fluid filtration, it has a lifespan set for the original purpose of the nonwoven fabric, so it is common to have a replacement period of one to several months, one to several years. Therefore, even if a dense metal film having a conductivity of less than 100 MΩ is formed, the filter itself has a lifespan, so the metal that constitutes the metal film is often wasted to the extent that it is formed densely. Therefore, it is most efficient for the metal film forming nonwoven fabric to form a metal film with as little metal adhesion as possible that can efficiently obtain antibacterial effect during the lifespan of the filter. Specifically, if the immersion time is short, the immersion pressure is close to normal pressure, and the number of immersing and drying is small, this condition (electrical resistance between two points on the plane of the metal film piece forming nonwoven fabric and between two points on the front and back is 100 MΩ or more) can be easily met, so in the case of the metal film piece forming composition according to the embodiment described later, it can be achieved by simply immersing and drying once.

[0041] The dispersion state of the metal film pieces formed on the surface of each filament constituting the nonwoven fabric can be confirmed by the electrical resistance between two points on the plane of the metal film piece-formed nonwoven fabric and between two points on the front and back being nonconductive at 100 MΩ or more, but ideally, it is preferable that the metal film pieces are formed in an evenly dispersed state on each filament constituting the nonwoven fabric from the surface to the inside of the nonwoven fabric. When the nonwoven fabric is immersed in the composition for forming metal film pieces, the composition for forming metal film pieces can be brought into contact evenly with the entire surface of each filament constituting the nonwoven fabric from the surface to the inside of the nonwoven fabric, so that the above-mentioned evenly dispersed state can be easily obtained.

[0042] For the antibacterial effect, it is important that the free electrons of the metal molecules that make up the formed metal film pieces can move freely. However, if the metal film b is formed over the entire nonwoven fabric c as in the case of metal film-formed nonwoven fabric a in which electrical conductivity is ensured and the fabric becomes a single conductor as in the case of metal film-formed nonwoven fabric a, as in FIG. 2(a), and the metal film b is formed over the entire nonwoven fabric c, when a part of the metal film-formed nonwoven fabric a is placed in an environment in which a potential difference is generated as in FIG. 2(b), the movement of the free electrons e around the metal molecules d that make up the metal film b will be hindered, raising concerns that the antibacterial effect will not be achieved. However, if the metal film pieces 3 are formed and dispersed on the surface of each filament that makes up the nonwoven fabric 2 as in the case of metal film piece-formed nonwoven fabric 1 shown in FIG. 1(a), the electrical conductivity is independent in the formation area of ​​each dispersed metal film piece 3, and the movement of the free electrons 32 around the metal molecules 31 that make up each metal film piece 3 is ensured. Therefore, as shown in FIG. 1(b), even if a part of the area of ​​the metal film piece-formed nonwoven fabric 1 where the metal film piece 3 is formed is placed in an environment where the movement of the free electrons 32 is inhibited by the potential difference, the movement of the free electrons 32 around the metal molecules 31 constituting the metal film piece 3 is not inhibited in the other areas where the metal film piece 3 is formed, and the antibacterial effect can be exhibited. Therefore, if the metal film piece 3 can be formed in a dispersed state on the surface of each filament constituting the nonwoven fabric 2, excellent antibacterial properties can be obtained. An example of an environment where a part of the area of ​​the metal film piece-formed nonwoven fabric 1 is subjected to a potential difference is when the housing to which the metal film piece-formed nonwoven fabric 1 is attached or the metal screw that fastens the housing is made of an electrical conductor having a different potential from the metal film piece-formed nonwoven fabric 1 and is in contact with a part of the metal film piece-formed nonwoven fabric 1.

[0043] Regarding the antibacterial effect, it has been confirmed that, in the case of the metal film piece forming composition according to the embodiment described later, a metal film piece-formed nonwoven fabric having a viable bacteria count of 0 in a specified antibacterial activity test can be formed even by performing a minimum treatment of ordinary immersion and drying once. Regarding the performance of this metal film piece-formed nonwoven fabric, a batch test is performed to determine the immersion time, immersion pressure, and number of immersion and drying cycles so that the viable bacteria count is 0 in the specified antibacterial activity test, and the manufacturing conditions for the metal film piece-formed nonwoven fabric having a viable bacteria count of 0 in the specified antibacterial activity test can be found. Therefore, from the immersion time, immersion pressure, number of immersion and drying cycles, etc. obtained from this batch test, a metal film piece-formed nonwoven fabric having a viable bacteria count of 0 in the specified antibacterial activity test can be manufactured.

[0044] The metal film piece-formed nonwoven fabric of the present invention constructed in this manner simply has metal film pieces formed in a dispersed state on the surface of each filament constituting the nonwoven fabric so that the electrical resistance between two points on the plane of the metal film piece-formed nonwoven fabric and between two points on the front and back is 100 MΩ or more. Therefore, it can be produced by a simple method, for example, by simply immersing the nonwoven fabric once in a composition for forming metal film pieces and drying it. Moreover, since only a single immersion and drying is required and the amount of metal used to form the metal film pieces is small, it can be produced inexpensively.

[0045] In addition, in the case of metal film-formed nonwoven fabric, metal film pieces are formed in a dispersed state on the surface of each filament that constitutes the nonwoven fabric, which ensures the movement of free electrons in metal molecules in the formation area of ​​each metal film piece, thereby achieving excellent antibacterial properties.

[0046] In addition, since the metal film piece-formed nonwoven fabric has metal film pieces formed in a dispersed state on the surface of each filament that constitutes the nonwoven fabric, it can be used without impairing the inherent properties of the nonwoven fabric material, such as softness and flexibility.

[0047] In the above description, the nonwoven fabric is immersed in the composition for forming metal film pieces, but the method for attaching the composition for forming metal film pieces to the nonwoven fabric is not limited to the immersion method, and the composition may be applied by roll coating, flow coating, spray coating, etc. However, in the case of these application methods, the composition is easily applied to the surface of the nonwoven fabric, but is difficult to apply to the inside, so there is a concern that it will be difficult to form metal film pieces in a dispersed state on the surface of each filament constituting the nonwoven fabric on both the surface and the inside of the nonwoven fabric. However, even if this happens, if it is confirmed that the electrical resistance between two points on the plane of the nonwoven fabric and between two points on the front and back is 100 MΩ or more, and a metal film piece-formed nonwoven fabric with a viable bacteria count of 0 is obtained in a predetermined antibacterial activity test, it can be determined that the metal film pieces are formed in a required dispersed state. Effect of the Invention

[0048] As described above, according to the present invention, a nonwoven fabric is immersed in a composition for forming metal film pieces, the composition comprising a metal precursor liquid having a reaction product of at least one selected from the group consisting of metal complexes and metal salts with at least one selected from ammonia and amines, and an organic reducing agent, and then dried, whereby metal film pieces are formed in a dispersed state on each filament constituting the nonwoven fabric. The electrical resistance between all two points on the flat surface and between all two points on the front and back was 100 MΩ or more. The specimen was cut into a size of 30 mm x 30 mm, sterilized, and then placed in a sterilized petri dish. 0.1 ml of a test bacterial solution prepared by adjusting the concentration of NBRC3972 Escherichia coli to 9 x 105 to 3 x 106 cfu / ml in phosphate buffer was dropped onto the specimen. After culturing for 24 hours at 35 ± 1 °C, the specimen was thoroughly washed out using 9.9 ml of SCDLP medium, and then serially diluted to 1:10,000 diluted water. Each diluted bacterial solution was cultured for 48 hours at 35 ± 1 °C using the agar plate culture method, and the resulting viable cell count was 0. Therefore, it is possible to prevent the metal molecules attached to each filament constituting the nonwoven fabric from forming a single electrically conductive film. Therefore, each metal molecule attached to each filament constituting the nonwoven fabric can exchange electrons individually in units of metal film pieces, so that the entire metal film piece-formed nonwoven fabric on which these metal film pieces are formed can exhibit an excellent antibacterial effect uniformly in any part of the metal film piece-formed nonwoven fabric. Moreover, since the metal film pieces formed on this metal film piece-formed nonwoven fabric are not dense metal films that ensure electrical conductivity, they can be manufactured easily and at low cost. [Brief description of the drawings]

[0049] [Figure 1]FIG. 2(a) is a partial cross-sectional view showing an outline of the overall configuration of a metal film flake-formed nonwoven fabric, and FIG. 2(b) is a partially enlarged view explaining the movement of electrons in the metal film flake-formed nonwoven fabric. [Diagram 2] FIG. 1(a) is a partial cross-sectional view showing an outline of the overall configuration of a conventional metal film-formed nonwoven fabric, and FIG. 1(b) is a partially enlarged view explaining the movement of electrons in the metal film-formed nonwoven fabric. [Diagram 3] 1 is a graph showing the relationship between the absorption coefficient measured by a photoelectric colorimeter and the bacterial concentration of NBRC3972 (Escherchia coli). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] [Examples 1 and 2] (1. Preparation of copper complex aqueous solution) 2.54 g of copper formate tetrahydrate (metal salt) and 4.56 g of 25% by mass ammonia water were added to 25 g of pure water, and the mixture was stirred at room temperature at 500 rpm for 1 hour to obtain a metal precursor liquid. The obtained metal precursor solution was deep blue when observed with the naked eye.

[0051] (2. Preparation of Aqueous Ascorbic Acid Solution) 72 g of pure water and 18 g of ascorbic acid as an organic reducing agent were mixed and stirred at a liquid temperature of 40° C. for 10 minutes to obtain a colorless and transparent aqueous solution of ascorbic acid.

[0052] (3. Preparation of composition for forming metal film pieces) The metal precursor liquid obtained in (1.) and the ascorbic acid aqueous solution obtained in (2.) were mixed in a ratio of 100 parts by mass of ascorbic acid to 300 parts by mass of copper in the metal precursor solution, and the mixture was stirred and mixed at room temperature for 20 minutes to obtain a composition for forming metal film pieces. Immediately after mixing, the mixture was dark green, but when mixing was continued, the obtained composition for forming metal film changed to yellow after 20 minutes. The pH of the obtained composition for forming metal film pieces was measured using a pH meter (PICCOLO+, manufactured by HANNA Instruments), and the pH of the composition for forming metal film pieces at 25°C was 7.5.

[0053] (4. Application of the composition for forming metal film pieces to a substrate) A polystyrene plastic petri dish (diameter 90 mm, depth 15 mm) was filled with a thoroughly washed polyethylene nonwoven fabric (length: 50 mm × width: 50 mm × thickness: 0.14 mm, basis weight 20.0 g / m 2 ) was placed. 30 g of the metal film piece forming composition obtained above was poured into a plastic petri dish, and the nonwoven fabric was immersed in the metal film piece forming composition and left to stand at room temperature for one day. After one day, the nonwoven fabric was removed from the plastic petri dish, washed five times with pure water, and then dried at room temperature to obtain a metal film piece-formed nonwoven fabric in which copper was attached to the surface of each filament constituting the nonwoven fabric.

[0054] [Copper evaluation] (1. Regarding adhesion status) The metal film piece-formed nonwoven fabric obtained above was cut, and the cut surface was observed with an electron microscope equipped with elemental analysis. The electron microscope was JSM-6010LA (manufactured by JEOL Ltd.), and the cross section was subjected to elemental analysis at an acceleration voltage of 15 V, a spot size of 60, and a magnification of 50 times to a size of 2500 x 1875 μm. As a result, Cu was qualitatively detected.

[0055] (2. Conductivity Evaluation) Using a digital multimeter (Keysight Technologies 34401A), the resistance between two points on the flat surface of the nonwoven fabric with metal film pieces and between two points on the front and back surfaces were measured. As a result, it was confirmed that the resistance was high, exceeding the measurement limit of 100 MΩ, and that no conductivity was obtained.

[0056] (3. Antibacterial Evaluation) The metal film piece-formed nonwoven fabric obtained in Example 1 above was subjected to the following antibacterial activity test. As a control, the same antibacterial activity test was carried out using the nonwoven fabric before copper was attached (Comparative Example 1). The test bacteria used in the antibacterial test were NBRC3972 (Escherchia coli) obtained from the National Institute of Technology and Evaluation. The concentration of the bacteria in the solution was 9 x 105 ~3×10 6 The concentration of bacteria was adjusted to 0.065 and 0.170 (9×10 7 ~3×10 8 cfu / ml), which is reduced to 1 / 100, resulting in 9 x 10 5 ~3×10 6 A bacterial solution containing cfu / ml was prepared. The nonwoven fabric with the metal film piece was cut into a size of 30 mm x 30 mm, and both sides were sterilized by ultraviolet irradiation. The sterilized test piece was placed in a sterilized petri dish, and the above 9 x 10 5 ~3×10 6 A test bacterial solution adjusted to a concentration of cfu / ml was dropped in 0.05 ml portions twice, a total of 0.1 ml. After culturing at 35±1° C. for 24 hours, the test specimen was placed in a sterilized stomacher bag and thoroughly washed out with 9.9 ml of SCDLP medium (manufactured by Nippon Pharmaceutical Co., Ltd.). The viable cell count was confirmed by agar plate culture method, and serial dilution was performed up to 1:10000 diluted water. 1 ml of each dilution was taken out into a 90 mm sterilized petri dish, and standard agar medium (manufactured by Nippon Pharmaceutical Co., Ltd.) prepared at about 48°C was poured over it, stirred, solidified, and then cultured in an incubator at a temperature of 35°C ± 1°C for 48 hours. From each dilution rate, a petri dish suitable for measurement (with the number of grown colonies being approximately 30 to 300 cfu) was selected, and the number of colonies was measured. The results are shown in Table 1.

[0057] [Examples 3 and 4, Comparative Example 1] The thickness of the polyethylene nonwoven fabric is 0.40 mm and the basis weight is 70.0 g / m 2 A metal film piece-formed nonwoven fabric was prepared in the same manner as in Example 1, except that the thickness of the polyethylene nonwoven fabric was changed to 0.40 mm and the basis weight was changed to 70.0 g / m2. 2A sample having no metal film piece formed thereon was used as Comparative Example 1, and the same test was carried out. The results are shown in Table 1.

[0058] [Table 1]

[0059] [Examples 5 to 10, Comparative Example 2] The polyethylene nonwoven fabric filter of Example 1 was used, which had a thickness of 0.17 mm and a basis weight of 20.0 g / m 2 Polypropylene nonwoven filter, thickness 0.51 mm, basis weight 100.0 g / m 2 Polypropylene nonwoven filter, thickness 0.76 mm, basis weight 200.0 g / m 2 A metal film piece-formed filter was fabricated in the same manner as in Example 1, except that the polypropylene nonwoven fabric filter was changed to the one having a thickness of 0.76 mm and a basis weight of 200.0 g / m2, and the same test was carried out. 2 The polypropylene nonwoven fabric filter having no metal film pieces formed thereon was used as Comparative Example 2, and the same test was carried out. The results are shown in Table 2.

[0060] [Table 2]

[0061] In Tables 1 and 2, the viable cell count and antibacterial activity value were calculated according to the following formulas. [Viable bacteria count] N=C×D×V N: number of live bacteria, C: number of colonies in the petri dish, D: dilution ratio, V: volume of SCDLP medium

[0062] From the above results, it was found that the copper-adhered metal film piece-formed filters according to the respective Examples had an extremely excellent antibacterial effect, with the viable bacteria count being 0 after 24 hours of culture.

[0063] The present invention can be embodied in various other forms without departing from its spirit or main features. Therefore, the above-described embodiments are merely illustrative in all respects and should not be interpreted as being limiting. The scope of the present invention is defined by the claims and is not limited to the text of the specification. Furthermore, all modifications and changes within the scope of the claims are within the scope of the present invention. [Explanation of symbols]

[0064] 1 Nonwoven fabric with metal film pieces 2. Nonwoven fabric 3 Metal film piece 31 Metal molecules 32 free electron

Claims

1. A nonwoven fabric is immersed in a composition for forming metal film pieces, the composition comprising a metal precursor liquid having a reaction product of at least one selected from the group consisting of a metal complex and a metal salt with at least one selected from ammonia and an amine, and an organic reducing agent, and then dried, whereby metal film pieces are formed in a dispersed state on the surface of each filament constituting the nonwoven fabric, The electrical resistance between any two points on the flat surface and between any two points on the front and back is 100 MΩ or more. A metal film piece-formed nonwoven fabric, characterized in that the fabric is cut into a size of 30 mm x 30 mm, sterilized, and then placed in a sterilized petri dish, and 0.1 ml of a test bacterial solution prepared by adjusting NBRC3972 Escherichia coli to a concentration of 9 x 105 to 3 x 106 cfu / ml with a phosphate buffer is dropped onto the test bacterial solution. After culturing at 35 ± 1°C for 24 hours, the test bacterial solution is thoroughly washed out using 9.9 ml of SCDLP medium, and then diluted stepwise to 1:10,000 diluted water. Each diluted bacterial solution is cultured at 35 ± 1°C for 48 hours using an agar plate culture method, and the resulting viable bacterial count is 0.

2. A metal film piece-formed nonwoven fabric as described in claim 1, wherein the metal is Cu.

3. The nonwoven fabric is a metal film piece-forming nonwoven fabric described in claim 1 or 2, which is made of natural fibers or resin fibers.

4. A method for forming a metal film piece, comprising: immersing a nonwoven fabric in a composition for forming a metal film piece, the composition comprising: a metal precursor liquid having a reaction product of at least one selected from the group consisting of a metal complex and a metal salt with at least one selected from ammonia and an amine; and an organic reducing agent; drying the nonwoven fabric after immersion; A method for producing a metal film-formed nonwoven fabric, in which metal film pieces are formed in a dispersed state on the surface of each filament constituting the nonwoven fabric, comprising: A method for producing a metal film piece-formed nonwoven fabric, comprising forming metal film pieces in a dispersed state on the surface of each filament constituting the nonwoven fabric so that the electrical resistance between any two points on the entire plane and between any two points on the front and back is 100 MΩ or more, cutting the filaments into pieces of 30 mm x 30 mm size, sterilizing the filaments, placing them in a sterilized petri dish, dropping 0.1 ml of a test bacteria solution prepared by adjusting NBRC3972 Escherichia coli to a concentration of 9 x 105 to 3 x 106 cfu / ml in a phosphate buffer, culturing the filaments at 35 ± 1°C for 24 hours, thoroughly washing the test bacteria out using 9.9 ml of SCDLP medium, and then diluting the test bacteria to 1:10,000 diluted water by stepwise dilution. Each diluted bacteria solution is cultured at 35 ± 1°C for 48 hours by an agar plate culture method, and adjusting the immersion time, immersion pressure, and number of immersion and drying times so that the resulting viable bacteria count is 0.

5. A method for producing a metal film flake-formed nonwoven fabric as described in claim 4, which comprises a single immersion and drying step under atmospheric pressure for one day.

Citation Information

Patent Citations

  • Suspended matter filter having sterilizing filter material and manufacturing method therefor

    JP1977044458A

  • Disinfectant air filter material

    JP1983008530A

  • Hydrogen storage alloy electrode for alkaline storage battery and core body of hydrogen storage alloy electrode for alkaline storage battery

    JP1996315811A

  • Deodorant fiber sheet

    JP2006014965A

  • Fiber sheet bonded with silver particles and method for producing the same

    JP2010001581A