MRAM Devices Containing Hardened Gap-Fill Dielectric Materials

By introducing bond-breaking additives and curing the gap-fill dielectric material with UV and laser annealing, the MRAM device addresses the issue of non-uniformity and poor properties in existing materials, resulting in enhanced etch resistance and reduced via blowout for improved MRAM performance.

JP7586603B2Active Publication Date: 2024-11-19INTERNATIONAL BUSINESS MACHINE CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022517707
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-23
Filing Date
2020-09-22
Publication Date
2024-11-19
Estimated Expiration
2040-09-22

AI Technical Summary

Technical Problem

Current MRAM devices face challenges with wafer-to-wafer variations in the non-uniform height of MTJ pillars due to the use of gap-fill dielectric materials that lack self-planarizing properties and have insufficient chemical and physical properties, leading to issues like via blowout and poor etch resistance.

Method used

A method involving ion implantation of bond-breaking additives into the gap-fill dielectric material, followed by curing with UV and laser annealing, to create a hardened dielectric material with improved properties, ensuring uniformity and stability between MTJ pillars.

Benefits of technology

The hardened gap-fill dielectric material enhances etch resistance and reduces via blowout, providing better via profiles and improved chemical stability, allowing for higher memory density and reliable operation of MRAM devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586603000001
    Figure 0007586603000001
  • Figure 0007586603000002
    Figure 0007586603000002
  • Figure 0007586603000003
    Figure 0007586603000003
Patent Text Reader

Abstract

A cured gap-fill dielectric material having improved chemical and physical properties is formed laterally adjacent to a multilayer magnetic tunnel junction (MTJ) pillar and top electrode structure of a memory structure. The cured gap-fill dielectric material can be formed by introducing a bond-breaking additive into an as-deposited gap-fill dielectric material layer via ion implantation, and then curing the gap-fill dielectric material layer containing the bond-breaking additive. Curing includes UV curing alone or UV curing in combination with laser annealing. Curing as used in this application does not adversely affect the MTJ pillar or top electrode structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a memory structure and a method for forming the same, and more particularly, to a magnetoresistive random access memory (MRAM) structure including a hardened gap-filling dielectric material having improved chemical and physical properties, and a method for forming the same. [Background technology]

[0002] MRAM is a non-volatile random access memory technology in which data is stored by magnetic memory elements. These elements are typically formed from two ferromagnetic plates, each capable of holding a magnetization, separated by a thin dielectric layer (i.e., tunnel barrier). One of the two plates is a permanent magnet set to a specific polarity (i.e., magnetic reference layer), while the magnetization of the other plate can be changed to match that of an external magnetic field to store memory (i.e., magnetic free layer). Such a configuration is known as a magnetic tunnel junction (MTJ) pillar. In cutting-edge or neuromorphic computing systems, MTJ pillars are commonly embedded in structures at the back end of the line (BEOL).

[0003] In the fabrication of an MRAM device, blanket layers of MTJ pillar materials (i.e., magnetic reference material, tunnel barrier, magnetization free material, and MTJ cap material) and top electrode material are formed on a conductive landing pad, which forms the bottom electrode of the MRAM device. The blanket layers are then patterned by lithography and etching to provide a material stack of the multi-layer MTJ pillar (including the remaining portions of the magnetic reference material, tunnel barrier, magnetization free material, and MTJ cap material) and the top electrode located on the conductive landing pad. Immediately following the formation of this material stack, a dielectric passivation layer, for example, silicon nitride (SiN), is formed to passivate the tunnel barrier. A gap-filling dielectric material is then formed that fills the gaps between adjacent MTJ pillars.

[0004] In MRAM device arrays, the gap-fill dielectric material must have self-planarizing properties. Furthermore, in current MRAM device processing involving dep-etch-dep methods, the gap-fill dielectric material is subject to wafer-to-wafer variations ranging from non-uniform height of the MTJ pillars. Therefore, there is a need to provide an MRAM device array including a self-planarizing gap-fill dielectric between the MTJ pillars that also has improved chemical and physical properties. Summary of the Invention

[0005] In one aspect of the present application, a method for forming a memory structure is provided. In one embodiment, the method includes forming a patterned material stack on a surface of a bottom electrode, the patterned material stack including a multi-layer magnetic tunnel junction (MTJ) pillar and a top electrode structure. A gap-fill dielectric material layer is then formed laterally adjacent to and on top of the patterned material stack. A bond-breaking additive is then introduced into the gap-fill dielectric material layer by ion implantation to provide a modified gap-fill dielectric material layer. The modified gap-fill material layer is then cured to provide a cured gap-fill dielectric material layer.

[0006] In the present application, curing is performed using an energy source that provides electromagnetic radiation. In some embodiments, curing includes only UV curing. In other embodiments, curing includes UV curing and laser annealing. In such embodiments, laser annealing can occur before or after UV curing. In some embodiments, when laser annealing is used as part of the curing process, the laser annealing can be performed at a wavelength of 0.4 J / cm 2 The laser annealing can be performed for a duration of about 1 nanosecond to about 500 nanoseconds at an incident laser energy density of: In some embodiments, a sacrificial helplayer is formed on the modified gap-fill dielectric material layer prior to the laser annealing.

[0007] In some embodiments, the bond breaking additive used comprises a light element or molecule (i.e., an element or molecule having an atomic number equal to or less than that of argon) selected from hydrogen, helium, nitrogen, carbon, and neon. In one example, the bond breaking additive is nitrogen and the ion implantation is performed at a concentration of 1×10 with an implantation energy of 1 keV to 40 keV. 13 ions / cm 2 ~3×10 14 ions / cm 2 In another example, the bond-breaking additive is helium and the ion implantation is performed using an ion dose of 5 x 10 with an implantation energy of 1 keV to 10 keV. 13 ions / cm 2 ~1×10 15 ions / cm 2 In this application, the bond-breaking additive introduced into the as-deposited gap-fill dielectric material does not adversely affect the MTJ pillar or top electrode structure.

[0008] In another aspect of the present application, a memory structure is provided. In one embodiment, the memory structure includes a plurality of spaced apart patterned material stacks located on a surface of a bottom electrode, each patterned material stack including a multi-layer magnetic tunnel junction (MTJ) pillar and a top electrode structure. A cured gap-fill dielectric material having a dielectric constant less than 3 and a first carbon content is disposed laterally adjacent and between each patterned material stack. A via structure is located within the cured gap-fill dielectric material, and the cured gap-fill dielectric material adjacent a sidewall of the via structure has a carbon content of 90% or more of the first carbon content. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view of an exemplary structure that can be used in one embodiment of the present application, the exemplary structure including an interconnect level including at least one conductive structure embedded within an interconnect dielectric material layer, with a bottom electrode located on a surface of the at least one conductive structure. [Diagram 2]FIG. 2 is a cross-sectional view of the example structure of FIG. 1 after forming a multi-layer magnetic tunnel junction (MTJ) stack and a top electrode metal-containing layer. [Diagram 3] 3 is a cross-sectional view of the example structure of FIG. 2 after patterning the MTJ stack and top electrode metal-containing layers to provide an MTJ pillar and a top electrode structure, respectively, above the bottom electrode. [Figure 4] 4 is a cross-sectional view of the exemplary structure of FIG. 3 after forming an encapsulant layer. [Diagram 5] 5 is a cross-sectional view of the example structure of FIG. 4 after forming a gap-fill dielectric material layer having self-planarizing properties. [Figure 6] FIG. 6 is a cross-sectional view of the example structure of FIG. 5 after introducing a bond-breaking additive into the as-deposited gap-fill dielectric material layer by ion implantation to provide a modified gap-fill dielectric material layer. [Figure 7] FIG. 7 is a cross-sectional view of the example structure of FIG. 6 after laser annealing as a first step of a curing process in accordance with an embodiment of the present application. [Figure 8] FIG. 8 is a cross-sectional view of the example structure of FIG. 7 after a laser anneal followed by a UV cure to provide a hardened gap-fill dielectric material layer. [Figure 9] 9 is a cross-sectional view of the example structure of FIG. 8 after removal of the cured gap dielectric fill material layer and the encapsulant material layer from on top of the patterned material stack. [Figure 10] 10 is a cross-sectional view of the example structure of FIG. 9 after forming a via structure in the cured gap-fill dielectric material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present application will now be described in more detail by reference to the following discussion and the drawings attached hereto. It should be noted that the drawings in this application are provided for illustrative purposes only, and therefore the drawings are not drawn to scale. It should also be noted that like and corresponding elements are referred to by like reference numerals.

[0011] In the following description, numerous specific details are set forth, such as specific structures, components, materials, dimensions, processing steps and techniques, to provide an understanding of various embodiments of the present application. However, it will be understood by those skilled in the art that various embodiments of the present application may be practiced without these specific details. In other instances, well-known structures or processing steps have not been described in detail to avoid obscuring the present application.

[0012] When an element, such as a layer, region, or substrate, is referred to as being "on" or "over" another element, it will be understood that it may be directly on the element, or that intervening elements may be present. In contrast, when an element is referred to as being "directly on" or "directly over" another element, there are no intervening elements present. When an element is referred to as being "beneath" or "under" another element, it will be understood that it may be directly below or beneath the other element, or that intervening elements may be present. In contrast, when an element is referred to as being "directly beneath" or "directly under" another element, there are no intervening elements present.

[0013] In embodiments of the invention described below, a hardened gap-fill dielectric material having improved chemical and physical properties is formed laterally adjacent to a multilayer magnetic tunnel junction (MTJ) pillar and top electrode structure of a memory structure. The hardened gap-fill dielectric material can be formed by introducing a bond-breaking additive into an as-deposited gap-fill dielectric material layer via ion implantation, and then curing the gap-fill dielectric material layer containing the bond-breaking additive. Curing includes UV curing alone or UV curing in combination with laser annealing. Curing as used in this application does not adversely affect the MTJ pillar or top electrode structure.

[0014] The cured gap-fill dielectric material provided herein is more etch resistant than comparable prior art gap-fill dielectric materials that are not modified and cured as outlined herein. The presence of the cured gap-fill dielectric material in a memory structure including at least one MTJ pillar and top electrode structure can provide a better via profile with reduced or no via blowout at the bottom of the via in an integration flow with multiple interconnect levels.

[0015] It should be noted that the drawings of this application show memory device regions in which memory devices, such as MRAM devices, are formed, and that non-memory device regions may be located laterally adjacent to the memory device regions shown in the drawings of this application.

[0016] 1, an exemplary structure that may be used in one embodiment of the present application is shown. The exemplary structure of FIG. 1 includes an interconnect level L that includes at least one conductive structure 14 embedded within an interconnect dielectric material layer 10. n , with bottom electrodes 16 located on the surface of at least one of the conductive structures 14. In this application, the interconnect level L n "n" can be an integer starting from 1.

[0017] Although not shown in the drawing, metal level L n-1 is the interconnection level L n In some embodiments, when n is 1, the metal level L n-1 is a mid-line (MOL) level. In other embodiments, when n is 2, 3, 4, etc., the metal level L n-1 is the interconnection level L n In either embodiment, the metal level L is a lower interconnect level located below the metal level L. n-1The FEOL level includes a layer of dielectric material having embedded therein at least one metal level conductive structure that is directly or indirectly connected to an underlying CMOS device (not shown) present at a front end of line (FEOL) level (not shown). n-1 , and interconnection level L n can be formed utilizing processes well known to those skilled in the art.

[0018] When n is 1, the metal level L n-1 The dielectric material layer may be comprised of a MOL dielectric material such as, for example, silicon dioxide, undoped silicate glass (USG), fluorosilicate glass (FSG), borophosphosilicate glass (BPSG), spin-on low-k dielectric layers, chemical vapor deposition (CVD) low-k dielectric layers, or any combination thereof. The term "low-k" as used throughout this application means a dielectric material having a dielectric constant less than 4.0 (all dielectric constants expressed herein are measured in vacuum). Also, in such embodiments (i.e., where n is 1), the conductive structure of at least one metal level is a contact structure comprising a contact metal or contact metal alloy, such as, for example, tungsten (W), cobalt (Co), platinum (Pt), nickel (Ni), or alloys thereof.

[0019] If n is greater than 1, the metal level L n-1The dielectric material layer of may be comprised of an interconnect dielectric material having a dielectric constant less than 4.0. Exemplary interconnect dielectric materials that may be used include, but are not limited to, silsesquioxanes, C-doped oxides (i.e., organosilicates) containing atoms of Si, C, O, and H, thermosetting polyarylene ethers, or multilayers thereof. The term "polyarylene" is used in this application to denote aryl or inertly substituted aryl moieties linked together by bonds, fused rings, or inert linking groups, such as oxygen, sulfur, sulfone, sulfoxide, carbonyl, and the like. Also, in such embodiments (i.e., when n is greater than 1), the conductive structure of at least one metal level is comprised of a conductive metal or a conductive metal alloy. Examples of conductive materials that may be used in this application include copper (Cu), aluminum (Al), or tungsten (W), and examples of conductive metal alloys include Cu-Al alloys.

[0020] Interconnect Level L n The interconnect dielectric material layer 10 of the metal level L n-1 The interconnect dielectric material layer 10 may be comprised of one of the interconnect dielectric materials described above for the dielectric material layer 10. The interconnect dielectric material layer 10 may be formed by depositing an interconnect dielectric material and optionally curing it using known curing techniques that are compatible with back end (BEOL) processing.

[0021] The deposition of the interconnect dielectric material to provide the interconnect dielectric material layer 10 may include chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), or spin-on coating. The interconnect dielectric material layer 10 may have a thickness between 30 nm and 150 nm. Other thicknesses are possible and may be used as the thickness of the interconnect dielectric material layer 10.

[0022] Interconnect Level L nThe remaining components present in may be formed utilizing processes well known to those skilled in the art. In one embodiment, at least one opening may be formed in the interconnect dielectric material layer 10 by lithography and etching. Lithography involves forming a photoresist material over the material or material stack that needs to be patterned, exposing the photoresist material to a pattern of radiation, and then developing the exposed photoresist material.

[0023] The conductive structure 14 may be formed in at least one opening formed in the interconnect dielectric material layer 10. The conductive structure 14 comprises a conductive metal or metal alloy as defined above. In some embodiments (not shown), the conductive structure 14 has a top surface that is coplanar with the top surface of the interconnect dielectric material layer 10. In other embodiments, as shown in FIG. 1, the conductive structure 14 has a top surface that is located below the top surface of the interconnect dielectric material layer 10.

[0024] In some embodiments, a diffusion barrier liner 12 may be present along the sidewalls and bottom wall of at least one opening, as shown in FIG. 1. In some embodiments, no diffusion barrier liner is present. The diffusion barrier liner 12 is comprised of a diffusion barrier material (i.e., a material that acts as a barrier to prevent conductive materials, such as copper, from diffusing). Examples of diffusion barrier materials that may be used in providing the diffusion barrier liner include, but are not limited to, Ta, TaN, Ti, TiN, Ru, RuN, RuTa, RuTaN, W, or WN. In some embodiments, the diffusion barrier material may include a material stack of diffusion barrier materials. In one example, the diffusion barrier material may be comprised of a stack of Ta / TaN.

[0025] As shown in the present application, a bottom electrode 16 is present on a surface of each conductive structure 14. In some embodiments (as shown), the bottom electrodes 16 are located on recessed surfaces of the conductive structures 14. In other embodiments (not shown), the bottom electrodes 16 are formed on non-recessed surfaces of the conductive structures 14. In such embodiments, a dielectric capping layer (not shown) may be located on the top surface of the interconnect dielectric material layer 10, laterally adjacent to the bottom electrodes 16.

[0026] The bottom electrode 16 may be comprised of Ta, TaN, Ti, TiN, Ru, RuN, RuTa, RuTaN, Co, CoWP, CoN, W, WN, or any combination thereof. The bottom electrode 16 may have a thickness of 2 nm to 25 nm, although other thicknesses are possible and may be used as the thickness of the bottom electrode 16 in this application. The bottom electrode 16 may be formed by a deposition process, such as, for example, sputtering, atomic layer deposition (ALD), chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), or physical vapor deposition (PVD). An etch-back process, a planarization process (e.g., chemical mechanical polishing, etc.), or a patterning process (e.g., lithography and etching, etc.) may follow the deposition of the conductive material that provides the bottom electrode 16.

[0027] In some embodiments (not shown), bottom electrode 16 has a top surface that is coplanar with a top surface of a dielectric capping layer (not shown) that is laterally adjacent bottom electrode 16 and may be present on the top surface of interconnect dielectric material layer 10. In other embodiments (as shown in FIG. 1), bottom electrode 16 has a top surface that is coplanar with the top surface of interconnect dielectric material layer 10.

[0028] Referring now to FIG. 2, the exemplary structure of FIG. 1 is shown after forming a multi-layer magnetic tunnel junction (MTJ) stack 18 and a top electrode metal-containing layer 28. The MTJ material stack 18 includes at least a magnetic pinned layer, a tunnel barrier layer, and a magnetic free layer. In some embodiments, as shown in FIG. 2, the MTJ material stack 18 is a bottom-pinned MTJ material stack including, from bottom to top, a magnetic pinned layer 20, a tunnel barrier layer 22, and a magnetic free layer 24. An optional metal seed layer (not shown) may also be present in the bottom-pinned MTJ material stack. In a bottom-pinned MTJ material stack, the optional metal seed layer is formed below the magnetic pinned layer 20. The bottom-pinned MTJ material stack may also include a non-magnetic spacer layer (not shown) located on the magnetic free layer 24, a second magnetic free layer (not shown) located on the non-magnetic spacer layer, or an MTJ cap layer 26 located on the magnetic free layer 24 or on the second magnetic free layer, or a combination thereof.

[0029] In other embodiments (not shown), the MTJ material stack 18 is a top-pinned MTJ material stack including, from bottom to top, a magnetic free layer, a tunnel barrier layer, and a magnetic pinned layer, in which the order of elements 20 and 24 is reversed from that shown in Figure 2. In such embodiments, the top-pinned MTJ material stack can also include an optional metallic seed layer located below the magnetic free layer, a non-magnetic spacer layer located on the magnetic free layer, a second magnetic free layer located on the non-magnetic spacer layer, and / or an MTJ cap layer located on the magnetic pinned layer.

[0030] The various material layers of the MTJ material stack 18 may be formed by utilizing one or more deposition processes, such as, for example, sputtering, plasma enhanced atomic layer deposition (PEALD), plasma enhanced chemical vapor deposition (PECVD), or physical vapor deposition (PVD).

[0031] The optional metallic seed layer may be comprised of platinum (Pt), palladium (Pd), nickel (Ni), rhodium (Rh), iridium (Ir), rhenium (Re), or alloys and multilayers thereof. In one example, the optional metallic seed layer is comprised of platinum (Pt).

[0032] The magnetization pinned layer 20 has a fixed magnetization. The magnetization pinned layer 20 can be composed of a metal or metal alloy (or stacks) including one or more metals that exhibit high spin polarization. In alternative embodiments, exemplary metals for forming the magnetization pinned layer 20 include iron, nickel, cobalt, chromium, boron, or manganese. Exemplary metal alloys can include the metals listed above. In another embodiment, the magnetization pinned layer 20 can be a multi-layer configuration having (1) regions of high spin polarization formed from metals and / or metal alloys using the metals listed above, and (2) regions composed of materials that exhibit strong perpendicular magnetic anisotropy (strong PMA). Exemplary materials with strong PMA that can be used include metals such as cobalt, nickel, platinum, palladium, iridium, or ruthenium, and can be arranged as alternating layers. The strong PMA regions can also include alloys that exhibit strong PMA, with example alloys including cobalt-iron-terbium, cobalt-iron-gadolinium, cobalt-chromium-platinum, cobalt-platinum, cobalt-palladium, iron-platinum, or iron-palladium, or combinations thereof. The alloys can be arranged as alternating layers. In one embodiment, combinations of these materials and regions can also be used as the magnetization pinned layer 20.

[0033] The tunnel barrier layer 22 is made of an insulating material and is formed to a thickness to provide an adequate tunnel resistance. Exemplary materials for the tunnel barrier layer 22 include magnesium oxide, aluminum oxide, and titanium oxide, or materials with higher electrical tunnel conductance, such as semiconductors or low bandgap insulators.

[0034] The magnetic free layer 24 may be composed of a magnetic material (or a stack of magnetic materials) having a magnetization that can change orientation relative to the magnetization orientation of the magnetic pinned layer 20. Exemplary magnetic materials for the magnetic free layer 24 include alloys and / or multilayers of cobalt, iron, cobalt-iron alloys, nickel, nickel-iron alloys, and cobalt-iron-boron alloys.

[0035] If present, the non-magnetic metallic spacer layer is composed of a non-magnetic metal or metal alloy through which magnetic information can be transferred and through which the two magnetically free layers can be magnetically coupled, so that in equilibrium, the first and second magnetically free layers are always parallel. The non-magnetic metallic spacer layer enables spin torque switching between the first and second magnetically free layers.

[0036] If present, the second magnetic free layer can include one of the magnetic materials described above for the magnetic free layer 24. In one embodiment, the second magnetic free layer is composed of the same magnetic material as the magnetic free layer 24. In another embodiment, the second magnetic free layer is composed of a magnetic material that is compositionally different from the magnetic free layer 24.

[0037] If present, the MTJ cap layer 26 may be composed of Nb, NbN, W, WN, Ta, TaN, Ti, TiN, Ru, Mo, Cr, V, Pd, Pt, Rh, Sc, Al or other refractory metals or conductive metal nitrides. The MTJ cap layer 26 may have a thickness between 2 nm and 25 nm, although other thicknesses are possible and may be used as the thickness of the MTJ cap layer 26 in this application.

[0038] Top electrode metal-containing layer 28 may be comprised of a conductive material such as, for example, Ta, TaN, Ti, TiN, Ru, RuN, RuTa, RuTaN, Co, CoWP, CoN, W, WN, or any combination thereof. In one embodiment of the present application, top electrode metal-containing layer 28 is comprised of Ti / TiN. The conductive material providing top electrode metal-containing layer 28 may be compositionally the same as or compositionally different from the conductive material providing bottom electrode 16.

[0039] In the present application, top electrode metal-containing layer 28 can have a thickness of 100 nm to 500 nm, although other thicknesses are possible and can be used as the thickness of top electrode metal-containing layer 28. Top electrode metal-containing layer 28 can be formed by a deposition process such as, for example, sputtering, plasma enhanced atomic layer deposition (PEALD), plasma enhanced chemical vapor deposition (PECVD), or physical vapor deposition (PVD).

[0040] 3, the exemplary structure of FIG. 2 is shown after the MTJ stack 18 and the top electrode metal-containing layer 28 have been patterned to provide an MTJ pillar 18P and a top electrode structure 28S, respectively, located above the bottom electrode 16.

[0041] Patterning the top electrode metal-containing layer 28 and the MTJ stack 18 may include first forming a patterned mask (not shown) on the physically exposed surface of the top electrode metal-containing layer 28. In some embodiments, the patterned mask may be comprised of a photolithography resist stack. In one embodiment, the photolithography resist stack providing the patterned mask may include a bottom organic layer, a middle inorganic layer, and a top resist layer. The bottom organic layer of the photolithography resist stack may include an organic planarization layer (OPL). The bottom organic layer of the photolithography resist stack may include a spin-on organic layer such as, for example, Near Frictionless Carbon (NFC), diamond-like carbon, a thermoset polyarylene ether, or a polyimide. The intermediate inorganic layer of the photolithography resist stack can include any oxide layer, such as, for example, low temperature (e.g., below 250° C.) CVD oxide, oxide derived from TEOS (tetraethyl orthosilicate), silicon oxide, silane oxide, or Si-containing antireflective coating materials (SiARC). The top resist layer of the photolithography resist stack can be composed of a resist material that provides high-resolution lithography patterning. The photolithography resist stack can be formed by first utilizing a sequence of deposition processes that include a first spin-on coating of a bottom organic layer, a second spin-on coating of a middle inorganic layer, and a third spin-on coating of a top resist layer. After providing the photolithographic resist stack, the top resist layer is patterned by photolithography (i.e. exposing the top resist layer to a radiation pattern and then developing the exposed top resist layer), after which the pattern provided in the top resist layer is transferred to the underlying layers of the photolithographic resist stack to provide a patterned mask. The transfer may include one or more etching processes.

[0042] In some embodiments, the patterning may include first patterning the top electrode metal-containing layer 28 using a first etching process, such as a reactive ion etch using a patterned mask as an etch mask. The remaining, i.e., unpatterned, portion of the top electrode metal-containing layer 28 provides the top electrode structure 28S. The top electrode structure 28S may be cylindrical in shape, although other asymmetric shapes are possible and may be used as the shape of the top electrode structure 28S in the present application. The critical dimension (CD) of the top electrode structure 28S may vary and is not critical to the present application. The top electrode structure 28 typically has a width that is greater than the width of the top of the bottom electrode 16. In such a case, undesired redeposition of metal particles from the bottom electrode 16 onto the MTJ pillar 18P may be avoided.

[0043] After patterning the top electrode metal-containing layer 28, the patterned mask is removed from above the top electrode structure 28S, which is formed using conventional processes well known to those skilled in the art. The MTJ material stack 18 is then patterned using ion beam etching (IBE), with the top electrode structure 28S used as the patterned mask. The remaining, i.e., unpatterned, portions of the MTJ stack 18 provide the MTJ pillars 18P. In one example, as shown in FIG. 3, each MTJ pillar 18P is a bottom-pinned MTJ material structure including, from bottom to top, a magnetic pinning material layer portion 20P (i.e., the remaining unetched portion of the magnetic pinning material layer 20), a tunnel barrier layer portion 22P (i.e., the remaining unetched portion of the tunnel barrier layer 22), and a magnetic free layer portion 24P (i.e., the remaining unetched portion of the magnetic free layer 24).

[0044] In another example (not shown), the MTJ pillar 18P is a top-pinned MTJ structure including, from bottom to top, a magnetic free layer portion 24P, a tunnel barrier layer portion 22P, and a magnetic pinning material layer portion 20P. The MTJ pillar 18P can include remaining portions of any other layers present in the MTJ stack 18. For example, FIG. 3 shows the MTJ pillar 18P including the MTJ cap portion 26P (i.e., the unetched portion of the remaining portion of the MTJ cap layer 26). The MTJ pillar 18P can be cylindrical in shape, although other asymmetric shapes are also possible and can be used as the shape of the MTJ pillar 18P in this application, and the MTJ pillar 18P and the top electrode structure 28S have the same shape. The critical dimension (CD) of the MTJ pillar 18P can vary and is not critical to this application. The CD of the MTJ pillar 18P is typically the same as the CD of the top electrode structure 28S.

[0045] Collectively, the MTJ stack 18P and top electrode structure 28S form a high aspect structure with a total height of over 100 nm. As memory cells continue to be scaled to improve memory density, the spacing between adjacent MTJ pillars decreases, resulting in high aspect ratio gaps. The MTJ pillar 18P includes multiple functional layers as described above. Proper operation of MTJ-based devices is highly dependent on precise engineering of the various interfaces between these functional layers. The required spatial control of the interfaces should be better than one atomic layer or about 0.3 nm. Additionally, the structural material control (e.g., grain texture, material composition, etc.) of these functional layers within the MTJ pillar 18P is also paramount to achieving proper operation of MTJ-based devices. Thus, once the MTJ stack 18 is formed, great care must be taken to preserve the material properties of the MTJ stack. Generally, all high energy processing of the MTJ stack 18 and MTJ pillar 18P thus formed is avoided.

[0046] 4, the exemplary structure of FIG. 3 is shown after forming an encapsulation material layer 30. The encapsulation material layer 30 is located on the sidewalls of each MTJ pillar 18P, as well as on the sidewalls and top of each top electrode 28S. In some embodiments, the formation of the encapsulation material layer 30 can be omitted.

[0047] The encapsulation material layer 30 is composed of a dielectric material that is compositionally different from the interconnect dielectric material that provides the interconnect dielectric material layer 10. The dielectric material that provides the encapsulation material layer 30 can provide passivation to the top electrode structure 28S and the MTJ pillars 18P. In one embodiment, the encapsulation material layer 30 is composed of silicon nitride. In another embodiment, the encapsulation material layer 30 can be composed of a dielectric material that contains atoms of silicon, carbon, and hydrogen. In some embodiments, in addition to atoms of carbon and hydrogen, the dielectric material that provides the encapsulation material layer 30 can include atoms of at least one of nitrogen and oxygen. In other embodiments, in addition to atoms of silicon, nitrogen, carbon, and hydrogen, the dielectric material that provides the encapsulation material layer 30 can include atoms of boron. In one example, the encapsulation material layer 30 can be composed of an nBLOK dielectric material that contains atoms of silicon, carbon, hydrogen, nitrogen, and oxygen. In an alternative example, the encapsulation material layer 30 can be composed of a SiBCN dielectric material that contains atoms of silicon, boron, carbon, hydrogen, and nitrogen.

[0048] The encapsulation material layer 30 is a continuous conformal layer that can be formed by a deposition process such as, for example, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD), or atomic layer deposition (ALD). The term "conformal" indicates that the material layer has a vertical thickness along the horizontal plane that is substantially the same (i.e., within ±5%) as its lateral thickness along the vertical plane. The encapsulation material layer 30 can have a thickness between 10 nm and 200 nm. Other thicknesses are possible and can be used as the thickness of the encapsulation material layer 30. The presence of the encapsulation material layer 30 reduces the gap between adjacent MTJ pillars 18P, making the aspect ratio of the gap higher.

[0049] In some embodiments, the encapsulation material layer 30 is formed by a low temperature deposition process. The term "low temperature deposition process" refers to a deposition process that is performed at a temperature of 400° C. or less. In one embodiment, the deposition of the encapsulation material layer 30 is performed at a temperature between 200° C. and 400° C. In an alternative embodiment, the deposition of the encapsulation material layer 30 is performed at a temperature between 200° C. and 350° C. The low temperature deposition prevents surface diffusion of metal particles across the tunnel barrier layer of the multilayer MTJ pillar 18P, which may lead to shorting of the device. The metal particles are formed during etching of the blanket layers that provide the multilayer MTJ pillar 18P.

[0050] In some embodiments, the encapsulant layer 30 may be of low quality. In other words, the encapsulant layer 30 may have poor mechanical and chemical properties associated with it, which need to be improved before further processing of the MTJ device. By "low quality" we mean that the encapsulant layer 30 is defective (containing a high content of carbon and hydrogen impurities), has low hermeticity, a low Young's modulus, and has a relatively high amount of bond-terminating radicals, such as hydrogen, hydrocarbon groups, and amino groups, which break the backbone of the chemically strong -Si-O-, -Si-N-, -CN-, and -BN- bond chains. As a result, the encapsulant layer 30 may have low etch resistance and high etch or erosion rates.

[0051] Referring now to FIG. 5, the exemplary structure of FIG. 4 is shown after forming a gap-fill dielectric material layer 32L having self-planarizing properties. The gap-fill dielectric material layer is formed laterally adjacent to and on top of each patterned structure (i.e., the MTJ pillars 18P and the top electrode structure 28S). The gap-fill dielectric material layer 32L is void-free. As shown, the gap-fill dielectric material layer 32L is formed on the encapsulation material layer 30. The gap-fill dielectric material layer 32L is composed of a dielectric material that is compositionally different than the dielectric material of the encapsulation material layer 30. In one embodiment, the gap-fill dielectric material layer 32L is composed of a flowable CVD or spin-on dielectric material, such as, for example, a dielectric material containing atoms of Si, C, O, and H. In some embodiments, the flowable low-k dielectric is nanoporous. Nanopores may be created in the gap-fill dielectric material 32L in a later step by activating an organic porogen additive that may be present in the as-deposited gap-fill dielectric material. In some embodiments, the flowable deposition process mixes organic precursors to achieve the target flowability, sacrificial porogens (e.g., cyclohexene), and matrix precursors for siloxane-based backbone structures (e.g., decamethylcyclopentasiloxane, diethoxymethylsilane, dimethyldimethoxysilane, tetramethylcyclotetrasilane, octamethylcyclotetrasilane). The flowable CVD or spin-on dielectric material can flow and fill very small gaps between topographical structures without forming voids or seams. In some embodiments, flowability is achieved by using siloxane-based polymers in which two silicon bonds are terminated with radicals such as hydrogen and / or methyl, and two other bonds participate in the siloxane backbone chain. Flowability can be affected by the length of the siloxane-based polymer chain, as well as by the amount and type of organic additive or solvent. The longer the polymer chain and the higher the organic solvent content, the higher the flowability. The as-deposited flowable dielectric material is chemically weak, can have a relatively high dielectric constant (eg, about 4.0), and is typically devoid of nanopores.After deposition, the flowable dielectric material requires a curing process to convert the material to its low-k state (i.e., a dielectric constant less than 4.0), form nanopores, and improve its chemical strength. The gap-fill dielectric material layer 32L is formed by a CVD or spin-on coating process, and although no planarization process is used in forming the gap-fill dielectric material layer 32L shown in FIG. 5, an optional CMP process can be used to planarize the gap-fill dielectric material 32L prior to curing.

[0052] An exemplary curing process for the flowable dielectric material can include heating up to 400° C. in the presence of intense UV light with radiation wavelengths less than about 250 nm. The curing process can result in the formation of weakly bonded organic groups (e.g., CH 3 , C.H. 2 In some embodiments, the bridges are either hydrogen (H) or methyl (CH) and the free dangling bonds are crosslinked into a strong chemical backbone network (e.g., a crosslinked siloxane-based Si-O backbone) while forming a target amount of nanopores. 3 The process involves cleaving one of the organic radical groups from some of the Si atoms in the polymer chain, forming three Si-O bonds to those atoms, while maintaining a fourth silicon bond terminated by a radical group such as SiO 2 , SiO 3 , or both. It is understood that a certain amount of these organic radical groups is required to achieve a low dielectric constant k, while a certain amount of crosslinking is required to achieve a certain level of chemical and mechanical strength. The bond scission is driven primarily by photochemical reactions initiated by abundant energy UV photons, while the removal of the detached organic groups is driven primarily by diffusion processes that take place at high substrate temperatures. Conventionally cured gap-fill dielectric material layers can be of poor quality due to inefficiencies in the curing process.

[0053] The gap-fill dielectric material layer 32L of the present application may have insufficient mechanical and chemical properties associated therewith, which need to be improved prior to further processing of the MTJ device. "Low quality" refers to the gap-fill dielectric material layer 32L being defective (containing a high content of carbon and hydrogen impurities), having poor hermeticity, a low Young's modulus, and chemically strong -Si-O-, -Si-CH bridged by chemically strong bonds of the same type. 2 This refers to a relatively high amount of bond-terminating radicals, such as hydrogen, hydrocarbon, and amino groups, that break the backbone of - and -CO bond chains. In some embodiments, poor quality refers to the resistance of the gap-fill dielectric material layer 32L to oxygen-containing plasmas that are often used in RIE processes. Oxygen radicals and ions generated in such plasmas attack organic radical groups that are abundant in the gap-fill dielectric material layer 32L and replace them with hydroxyl (-OH) groups. This is the case for Si-CH 3 and a decrease in the amount of Si-H bonds and an increase in the amount of Si-OH bonds. As a result, the gap-fill dielectric material layer 32L exposed to an oxygen-containing plasma may have a lower etch resistance and a higher etch or erosion rate.

[0054]

[0023] Referring now to Figure 6, the example structure of Figure 5 is shown after introducing a bond-breaking additive into gap-fill dielectric material layer 32L via ion implantation to provide modified gap-fill dielectric material layer 32M. The introduction of the bond-breaking additive occurs prior to curing. In Figure 6, the arrows indicate the direction of the ion implantation process.

[0055] In the present application, modifying the gap-fill dielectric material 32L prior to curing includes ion-implanting a bond-breaking additive into the gap-fill dielectric material layer. The bond-breaking additive includes a light element or molecule. By "light element" is meant an element whose atomic number Z is equal to or less than the atomic number of argon (Z=18). Illustrative examples of light elements that can be used as bond-breaking additives include, but are not limited to, hydrogen (H), helium (He), nitrogen (N), carbon (C), or neon (Ne). Light molecules include hydrogen molecules (H 2) and molecular nitrogen (N 2 ) is a light element such as Cr. The as-deposited gap-fill dielectric material layer 32L is implanted through its entire thickness to provide a modified gap-fill dielectric material layer 32M. The implantation energy determines the depth of penetration into the gap-fill dielectric material layer 32L. Various penetration levels can be achieved by predetermining the ion implantation energy. Multiple implantation energies can be used to distribute the implanted ions uniformly throughout the gap-fill dielectric material layer 32L or to distribute the implantation damage uniformly throughout the gap-fill dielectric material layer 32L. The ion implantation dose is selected such that the implanted element does not exceed 0.5 atomic percent of the constituents of the gap-fill dielectric material.

[0056] In one embodiment, the modified bond-breaking light element is a nitrogen atom. In this embodiment, the ion implantation energy is 1 keV to 40 keV and the ion implantation energy is 1×10 13 ions / cm 2 ~3×10 14 ions / cm 2 Using the above-mentioned ion implantation conditions, the concentration of nitrogen added to gap-filling dielectric material layer 32L is between 0.01 atomic percent and 0.1 atomic percent (in other words, the concentration of nitrogen added to gap-filling dielectric material layer 32L is between 5×10 18 atoms / cm 3 ~5×10 19 atoms / cm 3 Also, using the above-mentioned ion implantation conditions, nitrogen penetrates into the gap-fill dielectric material layer 32L to a depth of 200 Å to 2000 Å. Ion implantation for using C and Ne is similar to that described above for nitrogen. Nitrogen is present in its molecular form (N 2 + ), in which case the implant energy range increases by a factor of two and the ion implant dose range decreases by a factor of two.

[0057] In another embodiment of the present invention, the modified bond breaking light element is a helium atom. In this embodiment, the ion implantation energy is 1 keV to 10 keV and the ion implantation energy is 5×10 13 ions / cm 2 ~1×10 15 ions / cm 2 Using the above-mentioned ion implantation conditions, the concentration of helium added to gap-fill dielectric material layer 32L is between 0.05 atomic percent and 0.5 atomic percent (in other words, the concentration of helium added to gap-fill dielectric material 32L is between 2.5×10 19 atoms / cm 3 ~2.5×10 20 atoms / cm 3 Also, using the above ion implantation conditions, helium penetrates into gap-fill dielectric material layer 32L to a depth of 200 Å to 2000 Å. + or H 2 + The ion implantation conditions for using are similar to those described above for helium.

[0058] The implantation step can be performed using a conventional beam-line ion implanter or a plasma immersion implanter. In the case of plasma immersion implantation, the implantation energy is controlled by the electrical bias of the substrate relative to the plasma potential. To achieve a uniform distribution of the implanted ions and / or a uniform distribution of the bond breakage (damage) caused by the implantation, the implantation step can be performed using multiple implant energies as described above.

[0059] The implant step does not adversely affect the MTJ pillars 18P or the top electrode structure 28S because it is a low dose implant that does not significantly modify the inorganic metal film of the electrode structure 28S and the MTJ pillars 18P. However, the low implant dose causes significant changes to the organic components of the gap-fill dielectric material layer 32L. Furthermore, the addition of the bond-breaking additive to the encapsulant liner 30L has little adverse effect on the inorganic encapsulant layer.

[0060] The modified gap-fill dielectric material layer 32M is then cured (as described in more detail herein below) with the aid of an energy source in the form of electromagnetic radiation. Curing can include UV curing alone or in combination with laser annealing. Laser annealing may be performed before or after UV curing. In a preferred embodiment, laser annealing is performed before UV curing, as shown in Figures 7 and 8. During the curing process of the present application, the modified gap-fill dielectric material layer 32M is maintained at an elevated temperature. Due to temperature sensitive structures present in the substrate at this step (e.g., MTJ pillars 18P), the substrate temperature is limited to 400°C for exposures longer than a few seconds, 800°C for exposures shorter than tens of milliseconds but longer than a few microseconds, and 1200°C for exposures shorter than a few microseconds.

[0061] Referring now to FIG. 7, there is shown the exemplary structure of FIG. 6 after laser annealing as a first step of a curing process according to one embodiment of the present application. In this case, the curing energy source is electromagnetic radiation ER of an incident laser beam. In some embodiments, the laser annealing is omitted and curing is performed using UV curing as defined herein below. In still other embodiments, curing may include UV curing followed by laser annealing. In FIG. 7, element 32C shows the modified gap-fill dielectric material layer that has been laser annealed.

[0062] In some embodiments, a sacrificial assist layer 34 can be deposited on the modified gap-fill dielectric material layer 32M prior to laser annealing. The purpose of the sacrificial assist layer 34 is to couple the electromagnetic radiation ER to the substrate and assist in heating the modified gap-fill dielectric material layer 32M to the target temperature. The sacrificial assist layer 34 is a continuous layer formed over the entire structure shown in FIG. 7. In one embodiment, the sacrificial assist layer 34 is an absorbing layer. The material of the absorbing layer is selected to absorb the electromagnetic radiation ER of the incident laser beam. In one embodiment, the absorbing layer is TaN, which has an extinction coefficient of 1.27 at 308 nm.

[0063] The sacrificial help-layer 34 can be formed utilizing a conventional deposition process, such as, for example, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or sputtering. The sacrificial help-layer 34 can have a thickness of 1 nm to 20 nm. Other thicknesses are possible for the sacrificial help-layer 34, as long as the thickness is sufficient to absorb most of the electromagnetic radiation ER. The laser annealing used in this step does not adversely affect the MTJ pillar 18P.

[0064] Laser annealing, as used as the first step of the curing process of the present application, is a short duration (in the nanosecond range) laser anneal, as defined herein. Such laser annealing can be used to improve the properties (chemical and mechanical) of a dielectric material, such as modified gap-fill dielectric material layer 32M. The laser annealing can harden modified gap-fill dielectric material layer 32M, resulting in a laser annealed modified gap-fill dielectric material layer 32C.

[0065] As used herein, the term "laser annealing" refers to an annealing method that uses a laser to induce heat in the surface being treated. A laser is an electro-optical device that emits coherent radiation. In some embodiments, a typical laser emits light having a defined wavelength in a narrow, low divergence beam. In some cases, the advantage of using a laser for the annealing process is that its light can be easily shaped and focused onto specific areas of the annealing surface to achieve very high radiation intensities with short exposure durations.

[0066] In some embodiments, the short exposure duration is achieved by raster scanning a focused laser beam over the surface of the substrate, including the as-deposited dielectric material, i.e., interconnect dielectric material, encapsulation material, or modified gap-fill dielectric material. In this case, the exposure duration measured at the incident intensity FWHM is the beam width in the scan direction divided by the scan speed. In an alternative embodiment, the short exposure duration is achieved by using a pulsed laser. In this case, the laser beam is shaped to achieve the required peak intensity over a selected substrate region, such as over the entire product die, and the laser is operated in a pulsed mode, as in the case of a Q-switched laser. The pulse duration of the Q-switched laser at the intensity FWHM (i.e., full width at half maximum) determines the substrate exposure time. The exposure process is repeated for the entire wafer surface in a step-and-repeat manner. In some embodiments, the exposure to light, i.e., laser annealing, e.g., by application of a laser beam, includes light exposure of 1 pulse to 100 pulses.

[0067] In some embodiments, the laser type used in the laser annealing method of the present application is selected from solid-state Nd:YAG lasers emitting at 1064 nm and frequency doubled or tripled to emit at 532 nm or 355 nm, respectively, or excimer lasers emitting below 400 nm. Excimer lasers can be driven by chemical reactions involving excited dimers or excimers, which are short-lived dimeric or heterodimeric molecules formed from two nuclear species (atoms) with at least one in an excited electronic state. Commonly used excimer molecules include F 2(fluorine, emitting at 157 nm), as well as rare gas compounds such as ArF (193 nm), KrCl (222 nm), KrF (248 nm), XeCl (308 nm), and XeF (351 nm). Excimer lasers are typically operated in a Q-switched, pulsed mode suitable for step-and-repeat pulsed wafer exposure. Solid-state Nd:YAG lasers offer an alternative to excimer lasers because of their stable, high-power output at 1064 nm, and can be efficiently frequency doubled or tripled to emit radiation at 532 nm or 355 nm. Solid-state lasers can be configured in continuous, pulsed, or Q-switched, pulsed modes suitable for both raster-scanned and step-and-repeat pulsed operation. The choice of laser wavelength is important to couple the laser radiation to the appropriate absorbing material. Typical dielectric materials either do not absorb or only slightly absorb (e.g., absorb less than 5% of the coupled radiation) at wavelengths as short as about 350 nm to about 250 nm, and the term "about" is used herein to indicate ±10 percent or less from the stated value. Metals and metal compounds, on the other hand, absorb radiation at wavelengths of about 600 nm or less, so shorter wavelength lasers are more preferred for structures with metal layers. In some embodiments, a XeCl laser (308 nm) can be used to couple about 35% of its incident radiation into the top electrode 28S and MTJ pillars 18P, thereby heating the adjacent modified gap-fill dielectric material layer 32M from below. In an alternative embodiment, a XeCl laser (308 nm) can be used to couple about 60% of its incident radiation into the sacrificial assist layer 34, thereby heating the underlying modified gap-fill dielectric material layer 32M from above.

[0068] When the substrate including the modified gap-fill dielectric material layer 32M is exposed to laser radiation, either by raster scanning or by laser pulsing, the temperature of the metal-containing structures present within the substrate begins to rise from a base value and then drops shortly thereafter. Increasing the temperature of the metal-containing structures at the metal level causes thermal energy or heat to flow into adjacent structures including the modified gap-fill dielectric material layer 32M, raising their temperature in lock step with the temperature of the metal-containing structures present within the substrate. A typical temperature-time trace of a nanosecond laser annealing process includes four distinct temperature regions: an initial or base substrate temperature, a heating portion, a temperature peak point, and a cooling portion. The initial or base substrate temperature is in the range of 23° C. (room temperature) to 400° C. This temperature is typically set by a hot plate on which the substrate resides. Alternative heating devices can also be used to maintain the substrate at the base temperature. Such alternative or additional heating devices can include backside or frontside lamp annealing, microwave heating, and a secondary millisecond scale preheating laser beam. A laser beam having a wavelength near 308 nm increases the surface temperature of the substrate, including the modified gap-fill dielectric material layer 32M, from a base temperature to a peak at a heating rate of about 1,000,000,000° C. / sec to about 100,000,000,000° C. / sec. After exposure to the laser radiation, the surface temperature, including the surface temperature of the modified gap-fill dielectric material layer 32M, is rapidly reduced to the base temperature at a heating rate of about 300,000,000° C. / sec to about 30,000,000,000° C. / sec. The anneal duration, measured near the temperature peak point, typically 50° C. below the peak point, ranges from about 1 nanosecond to about 500 nanoseconds, with about 10 to about 100 nanoseconds being more typical. Laser anneal process durations are customarily specified in terms of radiation exposure duration at FWHM, rather than anneal duration at a temperature level 50° C. below the peak temperature. These duration quantities are related to each other, and in some embodiments, the anneal duration is a fraction (e.g., about 1 / 3) of the radiation exposure duration.

[0069] The laser-induced surface temperature rise is set by the laser incident radiation intensity, the laser pulse or exposure duration, and the optical and thermal properties of the as-deposited interconnect dielectric material and the underlying substrate. A short front laser exposure causes non-uniform heating of the substrate including the modified gap-fill dielectric material layer 32M. Thermal penetration depths for nanosecond-scale laser pulses range from about 1 micron to about 5 microns for metal structures such as copper, and from about 100 nanometers to about 500 nanometers for typical interconnect dielectrics. Thus, a relatively thick substrate including the modified gap-fill dielectric material layer 32M can be heated relatively uniformly throughout its thickness with a small top-to-bottom temperature gradient of about 0.1-3° C. / nm. This also ensures that the modified gap-fill dielectric material layer 32M is heated to a similar temperature throughout its thickness of less than about 100 nm.

[0070] It will be appreciated that the radiation intensity required for a substrate containing as-deposited dielectric material to reach a target annealing temperature range of about 1000° C. to about 1300° C. will depend on the particular materials present in the substrate, the laser pulse duration, and the selected laser wavelength. However, the required incident radiation intensity can be determined experimentally for a particular set of substrates and annealing parameters containing modified gap-fill dielectric material layer 32M by incorporating copper material into the metal level and observing its melting point of about 1090° C. In some embodiments, the nanosecond laser wavelength is 308 nm, the substrate base temperature is 250° C., the pulse duration at FWHM is 160 nanoseconds, and the combined laser energy density at which the copper layer at the metal level begins to melt is 0.13 J / cm. 2 (This is the incident laser energy density of 0.2 J / cm 2 This calibration point can be converted to the incident laser energy density required for specific selection of metals present at the metallurgical level by appropriate normalization to the metal optical reflectance at 308 nm.

[0071] In some embodiments, the laser anneal of the substrate including the modified gap-fill dielectric material layer 32M is performed at a laser energy of 0.4 J / cm2 The laser annealing is performed with incident laser energy densities of 0.03 J / cm. In one example, laser annealing of a substrate containing as-deposited dielectric material is performed with incident laser energy densities of 0.03 J / cm. 2 ~0.38J / cm 2 In an alternative embodiment, the laser annealing is performed with an incident laser energy density of 0.03 J / cm 2 ~0.46J / cm 2 In some embodiments, a target annealing temperature range of about 1000 °C to about 1300 °C can be achieved with an incident laser energy density of 0.4 J / cm. 2 It is necessary that the

[0072] The substrate may include a metal-containing structure (including absorber layer 34) that has a relatively low melting point of less than about 1300° C. In this case, the desired annealing temperature range is from about 1000° C. to below the melting point of the metal-containing structure present in the substrate. The melting point of the metal-containing structure and the corresponding threshold incident laser energy density can be determined experimentally for a particular selection of materials and laser annealing parameters that provide a substrate including an as-deposited dielectric material by observing the electrical functionality of the metal-containing structure before and after laser annealing.

[0073] Referring now to FIG. 8, the exemplary structure of FIG. 7 is shown after performing a UV lamp cure (i.e., UV cure) as the second step of the curing process of the present application. In the step, the curing energy source is electromagnetic radiation ER' from a UV lamp. In some embodiments, the electromagnetic radiation wavelength is in the UV region of the spectrum, preferably shorter than 250 nm, the substrate temperature is between 200° C. and 400° C., and the process time is between 1 minute and 10 minutes. In some embodiments, the UV cure can be performed on the exemplary structure shown in FIG. 6 without performing a laser anneal as part of the curing process.

[0074] Electromagnetic radiation ER' passing through modified gap fill dielectric material layer 32M held at elevated temperature or laser annealed modified gap fill dielectric material layer 32C held at elevated temperature chemically converts the gap fill dielectric material into hardened gap fill dielectric material layer 33. Hardened gap fill dielectric material layer 33 is void free and has a dielectric constant of less than 3 and a first carbon content.

[0075] Upon this conversion, the cured gap-fill dielectric material layer 33 has unique material properties such that its dielectric constant is less than 3, typically in the range of 2.7-2.9, and the wet etch rate of the plasma-ion damaged material is improved (lower) by a factor of 2-4 than the wet etch rate of a flowable low-k film cured only by a conventional UV curing process. The cured gap-fill dielectric material layer 33 has a small (less than 5%) increase in dielectric constant compared to that of a conventionally cured gap-fill dielectric material. Importantly, the low-dose implant, nanosecond laser annealing, and conventional UV curing processes used in this step do not adversely affect the MTJ pillars 18P and top electrode structure 28S.

[0076] Although FIGS. 7 and 8 show a preferred order of curing (first laser annealing, then UV lamp curing), other curing orders are also viable and provide similar benefits. In one embodiment, the laser annealing can be omitted. In another embodiment, a conventional UV cure can be performed prior to the laser annealing. In yet another embodiment, the curing sequence shown in FIGS. 7 and 8 can be followed by an additional laser annealing step. In any of the above-described embodiments, after the laser annealing, the sacrificial assist layer 34 can be selectively removed utilizing any conventional material removal process, including, but not limited to, planarization or etching.

[0077] 9, the exemplary structure of FIG. 8 is shown after a planarization process is performed to remove the cured gap-fill dielectric material layer 33 and the encapsulant material layer 30 located above the top surface of the top electrode structure 28S. The cured gap-fill dielectric material 33 remains laterally adjacent to each MTJ pillar 18P and each top electrode structure 28S. Also, remaining portions of the encapsulant material layer 30, i.e., the encapsulant material liner 30L, remain on the sidewalls of each MTJ pillar 18P and each top electrode structure 28S. In some embodiments, the encapsulant liner 30L may remain on the top electrode structure 28S (not shown). The planarization process may include chemical-mechanical polishing and / or grinding.

[0078] The cured gap-fill dielectric material 33 has a top surface that is coplanar with the top surface of the encapsulant liner 30L and / or the top surface of the top electrode structure 28S. The cured gap-fill dielectric material 33 has improved chemical and physical properties. In some embodiments, the encapsulant liner 30L also has improved chemical and physical properties.

[0079] 10, the exemplary structure of FIG. 9 is shown after forming a via structure 14V in the cured gap-fill dielectric material 33 to provide an electrical connection to one of the bottom electrodes 16, or one of the conductive structures 14, or both. Note that in the drawing, the via structure 14V is formed in a portion of the cured gap-fill dielectric material 33 in front of the middle MTJ pillar 18P and top electrode structure 28S shown in FIG. 9. A number of such via structures 14V can be arranged in several geometric configurations, such as a checkerboard pattern relative to the MTJ pillar 18P and top electrode structure 28S, or at the edge of the MTJ pillar array, as shown in FIG. 10. The structure of FIG. 9 can be optionally capped with an ILD film 10T prior to forming the via structure 14V. The ILD film 10T is similar to the ILD film 10 and is formed using similar techniques. The via openings used in providing the corresponding via structures 14V are patterned at desired locations away from the MTJ pillars 18P and the top electrode structures 28S using suitable lithography techniques. The hardened gap-fill dielectric material 33 is removed through the via openings using reactive ion etching (RIE). The RIE chemistry can be switched to break through the encapsulating liner 30L after removing the hardened gap-fill dielectric material 33. All or a portion of the exposed bottom electrode 16 can also be removed. The exposed surfaces of the conductive structures 16 / 14 are cleaned and a conductive liner 12V is typically deposited within the via openings. The conductive liner 12V is similar to the liner 12 and is formed using similar techniques. The via openings including the conductive liner 12V are then filled with a metal conductor and planarized to form the via structures 14V. The metal conductors used in providing the via structures 14V are similar to those of the conductive structures 14 and are formed using similar techniques. The same via structure can be used to contact the top electrode structure 28S and wire the MTJ pillar 18P to the memory array. The RIE chemistry used to form the via structure may contain oxygen, creating damaged hardened gap-fill dielectric material regions 33D adjacent to the via sidewalls.In the damaged cured gap fill dielectric material regions 33D, oxygen radicals and ions attack the organic radical groups and replace them with hydroxyl (-OH) groups. The cured gap fill dielectric material 33 provides better resistance to these chemical processes, as compared to the cured gap fill dielectric material 33, where Si-CH. 3 Note that the depletion of Si-H bonds and the accumulation of -OH bonds are reduced. As a result, the via profile is more vertical and there is reduced or no via blowout, enabling higher density memory.

[0080] Without being limiting, the above implantation steps result in bond scission (i.e., bond breaking) of the gap-fill dielectric material. Moderate bond scission breaks long polymer chains into smaller pieces, separating bond-terminating radicals such as hydrogen, hydrocarbon, or amino groups, and freeing adjacent dangling bonds to participate in chemically strong bond chains and crosslinks formed during the subsequent curing step. It is understood that a certain amount of bond-terminating organic radical groups is required to achieve a low dielectric constant k. Thus, the implantation dose is selected to keep the resulting dielectric constant k below 3.

[0081] Without being limiting in any way, laser annealing of modified gap-fill dielectric and encapsulant materials, performed at temperatures of about 1000°C or higher, can separate bond-terminating radicals, such as hydrogen, hydrocarbon, or amino groups, and free adjacent dangling bonds to participate in chemically strong cross-linking bonds. Although the separated radicals may diffuse out of the film and desorb from the free surface well after the laser-induced temperature pulse, some of them may reattach back to similar bond-terminating sites, partially negating the positive effects of laser-induced dielectric film hardening. In addition, high-temperature laser annealing can increase the likelihood of joining adjacent dangling bonds caused by either ion implantation or the laser annealing itself. Longer annealing times also increase the likelihood of separating bond-terminating radicals and joining adjacent dangling bonds. Advantageously, multiple short-time laser anneals can be utilized in lieu of longer annealing times. Thus, 2-30 successive laser anneals can be utilized to increase the cumulative radiation exposure time, or equivalently, the cumulative annealing time, by a factor of 2-30 compared to a single laser anneal. It is understood that a certain amount of bond-terminating organic radical groups is required to achieve a low dielectric constant k. Thus, the peak temperature and duration of the laser anneal are selected to keep the resulting dielectric constant k below 3.

[0082] Without being limiting, conventional UV curing steps at high substrate temperatures for dielectric materials, i.e., gap-fill dielectric materials, result in the removal of isolated terminating radicals and converting dangling bonds to chemically tough -Si-O-, -Si-CH 2 -, -CO-, and -CN- crosslinking bonds and further crosslinking of chains. The resulting material is more resistant to oxygen-containing plasmas, as manifested by a reduced rate of replacement of remaining bond-terminating organic radical groups with hydroxyl groups.

[0083] In some embodiments, the conventionally cured gap fill dielectric material (i.e., the as-deposited gap fill dielectric material that has been UV cured) has a first resistance to plasma induced damage and the cured gap fill dielectric material 33 has a second resistance to plasma induced damage, the second resistance being greater than the first resistance. The plasma induced damage comprises exposure to an oxygen-containing plasma. The conventionally cured gap fill dielectric material exposed to an oxygen-containing plasma has a first hydroxyl content and the cured gap fill dielectric material 33 exposed to an oxygen-containing plasma has a second hydroxyl content, the first hydroxyl content being greater than the second hydroxyl content. The conventionally cured gap-fill dielectric material exposed to the oxygen-containing plasma has a first hydrogen content and a first carbon-hydrogen content, and the cured gap-fill dielectric material 33 exposed to the oxygen-containing plasma has a second hydrogen content and a second carbon-hydrogen content, the first hydrogen content being lower than the second hydrogen content and the first carbon-hydrogen content being lower than the second carbon-hydrogen content. The conventionally cured gap-fill dielectric material exposed to the oxygen-containing plasma has a first etch rate, and the cured gap-fill dielectric material 33 exposed to the oxygen-containing plasma has a second etch rate that is lower than the first etch rate.

[0084] In some embodiments, the Si-CH in the damaged cured gap-fill dielectric material region 33D 3 The amount of bonds, i.e., carbon content, is 90% or more of their respective amounts in the cured gap-fill dielectric material 33. In some embodiments, the Si-CH 3 The amount of bonds, i.e., the carbon content, is essentially the same as in the cured gap-fill dielectric material 33. In one embodiment, the carbon content in the damaged, cured gap-fill dielectric material regions 33D is greater than 10 atomic %, preferably about 12 atomic %. In some embodiments, the amount of Si-H bonds in the damaged, cured gap-fill dielectric material regions 33D is more than half of the amount in the cured gap-fill dielectric material 33.

[0085] In other embodiments, the conventionally cured gap fill dielectric material has a first Young's modulus and the cured gap fill dielectric material 33 has a second Young's modulus that is greater than the first Young's modulus. In some embodiments, the cured gap fill dielectric material 33 has improved chemical bonds, i.e., less amount of bond terminating radicals such as hydrogen, hydrocarbon groups, and amino groups, and less amount of -Si-O-, -Si-CH at a given low dielectric constant k less than 3. 2 This allows the backbone of the -, -CO-, and -CN- bonded chains to be stronger.

[0086] In some embodiments, the cured gap-fill dielectric material 33 is composed of a low-k dielectric material containing atoms of Si, C, O, and H. In other embodiments, the cured gap-fill dielectric material 33 is composed of a low-k dielectric material containing atoms of Si, C, O, N, and H.

[0087] In some embodiments, the as-deposited encapsulant material layer 30 has a first hydrogen content, a first nitrogen-hydrogen bond content, and a first carbon-hydrogen bond content, and the laser annealed encapsulant material liner 30L has a second hydrogen content less than the first hydrogen content, a second nitrogen-hydrogen bond content less than the first nitrogen-hydrogen bond content, and a second carbon-hydrogen bond content less than the first carbon-hydrogen bond content. The as-deposited encapsulant material layer 30 has a first etch rate, and the laser annealed encapsulant material liner 30L has a second etch rate less than the first etch rate.

[0088] In other embodiments, the as-deposited encapsulant material layer 30 has a first Young's modulus and the laser annealed encapsulant material liner 30L has a second Young's modulus greater than the first Young's modulus. In some embodiments, the laser annealed encapsulant material liner 30L has improved chemical bonds, i.e., less amount of bond terminating radicals such as hydrogen, hydrocarbon groups, and amino groups, allowing for stronger backbones of -Si-O-, -Si-N-, -CN-, and -BN- bond chains.

[0089] While the present application has been particularly shown and described with respect to its preferred embodiments, it will be understood by those skilled in the art that the foregoing and other changes in form and detail may be made therein without departing from the scope of the present application. It is therefore intended that the present application not be limited to the exact forms and details described and illustrated, but fall within the scope of the appended claims.

Claims

1. 1. A method of forming a memory structure, comprising: forming a patterned material stack on a surface of the bottom electrode, the patterned material stack including a multi-layer magnetic tunnel junction (MTJ) pillar and a top electrode structure; forming a gap-fill dielectric material layer laterally adjacent and on top of the patterned material stack; ion implanting a bond-breaking additive into the layer of gap-fill dielectric material to provide a modified layer of gap-fill dielectric material; curing the modified gap-fill dielectric material layer to provide a cured gap-fill dielectric material layer; A method comprising:

2. The method of claim 1 , wherein the curing is performed with an energy source providing electromagnetic radiation.

3. The method of claim 2 , wherein the curing comprises UV curing.

4. The method of claim 3 , wherein the curing further comprises laser annealing.

5. The method of claim 4 , wherein the laser annealing occurs before the UV curing.

6. The method of claim 4 , wherein the laser annealing occurs after the UV curing.

7. The laser annealing is performed at a dose of 0.4 J / cm 2 5. The method of claim 4, wherein the method is performed at an incident laser energy density of about 1 nanosecond to about 500 nanoseconds.

8. The method of claim 4 , further comprising forming a sacrificial helplayer on the modified gap-fill dielectric material layer prior to laser annealing.

9. The method of claim 1 , wherein a bond-breaking additive breaks bonds within the gap-fill dielectric material layer and does not adversely affect the MTJ pillars and the top electrode structure.

10. 10. The method of claim 9, wherein the bond-breaking additive comprises a light element or molecule selected from hydrogen, helium, nitrogen, carbon and neon.

11. The bond-breaking additive comprises nitrogen, and the ion implantation is performed at an implantation energy of 1 keV to 40 keV and a 1×10 13 ions / cm 2 ~3×10 14 ions / cm 2 The method of claim 9 , wherein the method is performed using an ion dose of

12. The bond-breaking additive comprises helium, and the ion implantation is performed at an implantation energy of 1 keV to 10 keV and a 5×10 13 ions / cm 2 ~1×10 15 ions / cm 2 The method of claim 9 , wherein the method is performed using an ion dose of

13. The method of claim 1 , wherein the bottom electrode is on a surface of a conductive structure embedded in an interconnect dielectric material layer.

14. The method of claim 1 , further comprising forming an encapsulation material layer between the patterned material stack and the gap-fill dielectric material layer.

15. The method of claim 1 , further comprising removing the cured gap-fill dielectric material layer and encapsulant material layer on top of the patterned material stack.

16. The method of claim 1 , further comprising forming a via structure in said hardened gap-fill dielectric material, said forming said via structure comprising reactive ion etching.

17. 17. The method of claim 16, wherein the reactive ion etch damages the hardened gap-fill dielectric material disposed laterally adjacent the via structure.

18. 20. The method of claim 17, wherein the damaged cured gap-fill dielectric material has a carbon content of 90% or greater of the cured gap-fill dielectric material.

19. 1. A memory structure comprising: a plurality of spaced apart patterned material stacks overlying a surface of a bottom electrode, each patterned material stack including a multi-layer magnetic tunnel junction (MTJ) pillar and a top electrode structure; a hardened gap-fill dielectric material having a dielectric constant less than 3 and a first carbon content located laterally adjacent and between each patterned material stack; a via structure located within the cured gap-fill dielectric material, the cured gap-fill dielectric material adjacent a sidewall of the via structure having a first carbon content of 90% or greater; and A memory structure comprising:

20. 20. The memory structure of claim 19, wherein said bottom electrode is on a surface of a conductive structure embedded in an interconnect dielectric material layer.

21. 20. The memory structure of claim 19 further comprising an encapsulant liner positioned between the patterned material stack and the cured gap-fill dielectric material.

22. 20. The memory structure of claim 19, wherein the MTJ pillar comprises a bottom-pinned MTJ material structure.

23. 20. The memory structure of claim 19, wherein the MTJ pillar comprises a top-pinned MTJ material structure.

24. 20. The memory structure of claim 19, wherein said hardened gap-fill dielectric material has a top surface that is coplanar with a top surface of said top electrode structure.

Citation Information

Patent Citations

  • Ultra-low dielectric constant film with controlled biaxial stress and its fabrication method

    JP2008527757A

  • Nonvolatile magnetic memory device

    JP2010165790A

  • Semiconductor device and manufacturing method thereof

    JP2013214697A

  • Advanced process flow for high quality fcvd film backgrounds

    JP2018503259A

  • Semiconductor structure and method of manufacturing the same

    US20180351081A1