Charge Transporting Varnish
The charge transporting varnish with onium borate salt and polymer compound addresses the challenges of high refractive index and transparency in organic EL devices, enhancing brightness and efficiency through improved thin film properties.
Patent Information
- Application Number
- JP2020569495
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-31
- Filing Date
- 2020-01-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-01-16
AI Technical Summary
Existing organic electroluminescent (EL) devices face challenges in achieving high refractive index, transparency, and reproducibility in charge transporting thin films, particularly for large-area applications, which affect brightness and efficiency.
A charge transporting varnish containing an onium borate salt and a polymer compound with specific structural units is developed, enabling the formation of thin films with high refractive index, low extinction coefficient, and excellent charge transport properties, suitable for large-area applications using wet processes.
The varnish allows for the production of charge transporting thin films with enhanced brightness characteristics in organic EL devices, supporting large-area applications and improving light extraction efficiency.
Smart Images

Figure 0007586713000001 
Figure 0007586713000002 
Figure 0007586713000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a charge transporting varnish. [Background technology]
[0002] In organic electroluminescence (hereinafter referred to as organic EL) devices, charge transporting thin films made of organic compounds are used as the light emitting layer and charge injection layer. In particular, the hole injection layer is responsible for the exchange of charges between the anode and the hole transport layer or the light emitting layer, and plays an important role in achieving low voltage operation and high brightness of the organic EL device. The methods for forming the hole injection layer are roughly divided into dry processes, such as deposition, and wet processes, such as spin coating. Comparing these processes, wet processes can efficiently produce thin films with high flatness over a large area. Therefore, as organic EL displays are currently being made larger, there is a demand for hole injection layers that can be formed by wet processes.
[0003] In view of these circumstances, the present inventors have developed charge transport materials that are applicable to various wet processes and that, when applied to the hole injection layer of an organic EL element, give thin films that can realize excellent EL element characteristics, as well as compounds that have good solubility in organic solvents used therein (see, for example, Patent Documents 1 to 3). Meanwhile, various efforts have been made to improve the performance of organic EL elements, and efforts have been made to adjust the refractive index of the functional films used in order to improve light extraction efficiency, etc. Specifically, attempts have been made to improve the efficiency of elements by using hole injection layers and hole transport layers with relatively high or low refractive indices, taking into account the overall configuration of the element and the refractive indices of other adjacent members (see, for example, Patent Documents 4 and 5). Thus, the refractive index is an important factor in the design of an organic EL device, and is considered to be an important physical property that should be taken into consideration for materials for organic EL devices.
[0004] Furthermore, because coloration of a charge-transporting thin film used in an organic EL element reduces the color purity and color reproducibility of the organic EL element, in recent years, it has been desired that a charge-transporting thin film for an organic EL element has high transmittance in the visible region and high transparency (see, for example, Patent Document 6). In view of this, the present applicant has already found a material for wet processing that gives a charge transporting thin film with excellent transparency and suppressed coloration in the visible region (see, for example, Patent Documents 6 and 7). However, as the trend toward larger-area organic EL displays continues, vigorous development is being carried out toward the practical application of wet-processed organic EL displays, and there is a constant demand for wet-process materials that can provide highly transparent charge-transporting thin films. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2008 / 129947 [Patent Document 2] International Publication No. 2015 / 050253 [Patent Document 3] International Publication No. 2017 / 217457 [Patent Document 4] Special Publication No. 2007-536718 [Patent Document 5] Special Publication No. 2017-501585 [Patent Document 6] International Publication No. 2013 / 042623 [Patent Document 7] International Publication No. 2008 / 032616 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a charge-transporting varnish that has a high refractive index, very good transparency, and can reproducibly give a charge-transporting thin film with excellent charge transport properties. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted extensive research in order to achieve the above object, and as a result have found that a charge-transporting thin film having a high refractive index, very good transparency and excellent charge transport properties can be reproducibly obtained from a varnish obtained by dissolving a predetermined charge-transporting substance and a predetermined onium borate salt in an organic solvent, and that by using this thin film as a hole-injection layer, an organic EL device having excellent luminance characteristics can be obtained, thereby completing the present invention.
[0008] That is, the present invention provides the following charge transporting varnish. 1. A charge transporting material, an onium borate salt, and an organic solvent are included, The charge-transporting varnish is characterized in that the charge-transporting substance includes a polymeric compound containing a repeating unit represented by the following formula (1), and the onium borate salt includes an onium borate salt (which is an electrically neutral salt) consisting of a monovalent or divalent anion represented by formula (a1) and a counter cation represented by formulas (c1) to (c5). [ka] (In the formula, each R independently represents a hydrogen atom, an alkyl group, or an alkoxy group; Ar 1 and Ar 2 each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group; X represents an alkyl group having a polymerizable functional group, an alkoxy group having a polymerizable functional group, an aromatic hydrocarbon group having a polymerizable functional group, or an aromatic heterocyclic group having a polymerizable functional group; and a and b each independently represent an integer of 1 to 5. [ka] (In the formula, each Ar independently represents an aryl group which may have a substituent or a heteroaryl group which may have a substituent; L represents an alkylene group, -NH-, an oxygen atom, a sulfur atom, or -CN + - stands for [ka] 2. The charge transporting varnish of 1, wherein R is a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 3. The above Ar 1 and Ar 2 are each independently a group represented by any one of the following formulas (2-1) to (2-3): [ka] (In the formula, R 1 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and each c independently represents an integer of 1 to 3. 4. The charge-transporting varnish according to any one of 1 to 3, wherein the above Xs are each independently a group represented by any one of the following formulas (3-1) to (3-4): [ka] (In the formula, Y and Z each independently represent a single bond, an oxygen atom, a nitrogen atom, a sulfur atom, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent, and f represents an integer of 0 to 10.) 5. The charge transporting varnish according to 4, wherein the above X is a group represented by the following formula (4): [ka] (In the formula, Z represents a single bond or an oxygen atom, and g represents an integer of 0 to 10.) 6. The charge-transporting varnish according to any one of 1 to 5, wherein the charge-transporting substance comprises a polymer compound containing a repeating unit represented by the following formula (1-1): [ka] 7. The charge-transporting varnish according to any one of 1 to 6, wherein the Ar is an aryl group having one or more electron-withdrawing substituents. 8. The charge-transporting varnish of 7, wherein the electron-withdrawing substituent is a halogen atom. 9. A charge-transporting varnish according to any one of 1 to 8, wherein the anion is represented by formula (a2). [ka] 10. The charge transporting varnish according to claim 9, wherein the onium borate salt is represented by the following formula (P-1): [ka] 11. A charge-transporting thin film obtained from any one of the charge-transporting varnishes 1 to 10. 12. An organic electroluminescence device having the charge transporting thin film of 11. 13. A method for producing a charge-transporting thin film, comprising applying any one of the charge-transporting varnishes recited in 1 to 10 onto a substrate and evaporating the solvent. Effect of the Invention
[0009] By using the charge-transporting varnish of the present invention, it is possible to obtain a charge-transporting thin film that has a high refractive index (high n), excellent transparency (extremely low extinction coefficient k), and excellent charge transport properties. Moreover, the charge transporting thin film having such characteristics can be suitably used as a thin film for electronic devices such as organic EL devices. In particular, by applying this thin film to the hole injection layer of an organic EL device, an organic EL device having excellent luminance characteristics can be obtained. Furthermore, the charge-transporting varnish of the present invention can be used to reproducibly produce thin films with excellent charge-transporting properties even when various wet processes capable of forming films over large areas, such as spin coating and inkjet methods, and is therefore fully capable of responding to recent developments in the field of organic EL elements. Furthermore, a thin film obtained from the charge transport varnish of the present invention can also be suitably used in electronic devices such as organic photoelectric conversion devices, organic thin film solar cells, organic perovskite photoelectric conversion devices, organic integrated circuits, organic field effect transistors, organic thin film transistors, organic light-emitting transistors, organic optical inspectors, organic photoreceptors, organic field quenching devices, light-emitting electrochemical cells, quantum dot light-emitting diodes, quantum lasers, organic laser diodes, and organic plasmon light-emitting devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in further detail below. The charge transporting varnish according to the present invention comprises a charge transporting substance, an onium borate salt, and an organic solvent, wherein the charge transporting substance comprises a polymeric compound containing a repeating unit represented by formula (1), and the onium borate salt comprises an onium borate salt (which is an electrically neutral salt) consisting of a monovalent or divalent anion represented by formula (a1) and a counter cation represented by formulas (c1) to (c5). The charge transporting property is synonymous with electrical conductivity and hole transporting property. The charge transporting varnish of the present invention may have charge transporting property by itself, or may have charge transporting property in a solid film obtained by using the varnish.
[0011] [ka]
[0012] In the formula, each R independently represents a hydrogen atom, an alkyl group, or an alkoxy group.
[0013] Examples of the alkyl group include linear or branched alkyl groups having 1 to 15 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, t-butyl, n-pentyl, n-hexyl, n-octyl, n-decyl, 2-methylhexyl, 2-ethylhexyl, 2-n-propylhexyl, 2-n-butylhexyl, 2-ethyldecyl, and 3-ethylhexyl groups.
[0014] Examples of the alkoxy group include linear or branched alkoxy groups having 1 to 15 carbon atoms. Examples include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a t-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-octyloxy group, an n-decyloxy group, a 2-methylhexyloxy group, a 2-ethylhexyloxy group, a 2-n-propylhexyloxy group, a 2-n-butylhexyloxy group, a 2-ethyldecyloxy group, a 3-ethylhexyloxy group, and a phenoxy group.
[0015] The above R is preferably a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, more preferably a hydrogen atom, a methyl group, an ethyl group, an isopropyl group or a t-butyl group, still more preferably a hydrogen atom, a methyl group or an ethyl group, and further preferably a hydrogen atom or a methyl group.
[0016] Ar 1 and Ar 2 each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group.
[0017] Specific examples of the aromatic hydrocarbon group and aromatic heterocyclic group include n-valent groups derived from benzene, biphenyl, terphenyl, naphthalene, fluorene, furan, thiophene, pyridine, quinoline, isoquinoline, and carbazole. The term "n-valent group derived from" refers to a group in which n hydrogen atoms have been removed from a specific basic skeleton such as benzene.
[0018] Ar 1and Ar 2 Preferred embodiments of the above include groups represented by the following formulas (2-1) to (2-6).
[0019] [ka]
[0020] Wherein, R 1 and R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0021] As the alkyl group, among the above alkyl groups having 1 to 15 carbon atoms, an alkyl group having 1 to 10 carbon atoms can be mentioned.
[0022] c, d and e each independently represent an integer of 1 to 3.
[0023] Ar 1 and Ar 2 More preferred embodiments include groups represented by the following formulas (2-1') to (2-6').
[0024] [ka]
[0025] X represents an alkyl group having a polymerizable functional group, an alkoxy group having a polymerizable functional group, an aromatic hydrocarbon group having a polymerizable functional group, or an aromatic heterocyclic group having a polymerizable functional group. Examples of the alkyl group, alkoxy group, aromatic hydrocarbon group and aromatic heterocyclic group include the same groups as those exemplified above.
[0026] The polymerizable functional group is a group (polymerizable group) that can be crosslinked by light or heat regardless of the presence or absence of a catalyst, and specific examples thereof include vinyl group, trifluorovinyl group, acryloyl group, methacryloyl group, oxetane group, and epoxy group, etc. In the present invention, among these, vinyl group, acryloyl group, methacryloyl group, oxetane group, and epoxy group are preferred, and vinyl group is more preferred.
[0027] a and b each independently represent an integer of 1 to 5, preferably 1 to 3, and more preferably 1.
[0028] Preferred specific examples of X include groups represented by the following formulas (3-1) to (3-6).
[0029] [ka]
[0030] In the above formulas (3-1) to (3-6), Y and Z each independently represent a single bond, an oxygen atom, a nitrogen atom, a sulfur atom, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent; R 3 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; and f represents an integer of 0 to 10.
[0031] Examples of the alkyl group, aromatic hydrocarbon group and aromatic heterocyclic group include the same groups as those exemplified above.
[0032] Examples of the substituent that can be bonded to the aromatic hydrocarbon group and aromatic heterocyclic group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, a methoxy group, an ethoxy group, a phenyl group, a naphthyl group, a terphenyl group, a fluorenyl group, a benzyl group, a phenethyl group, a furanyl group, a thiophenyl group, a pyridinyl group, a quinolyl group, an isoquinolyl group, a carbazolyl group, a diphenylamino group, a triphenylamino group, and a styrenyl group.
[0033] A more preferred embodiment of X is a group represented by the following formula (4).
[0034] [ka]
[0035] In the above formula (4), Z represents a single bond or an oxygen atom, and g represents an integer of 0 to 10.
[0036] More preferred embodiments of X include, for example, groups represented by the following formulas (5-1) to (5-7).
[0037] [ka]
[0038] Examples of the polymer compound of the above formula (1) that can be suitably used in the present invention include polymer compounds containing repeating units represented by the following formulae (1-1) to (1-4).
[0039] [ka]
[0040] The weight average molecular weight (Mw) of the polymer compound is usually 10,000 to 500,000, and the dispersity (Mw / Mn) is usually 1 to 15. The values of the weight average molecular weight and the like are polystyrene-equivalent values measured by gel permeation chromatography.
[0041] The polymer compound can be synthesized by referring to known methods described in, for example, JP-A-2009-283509, assigned to Kanto Chemical Co., Ltd. When preparing the charge transporting varnish using the polymer compound, it may be used in the state of a solution after the reaction, or it may be used after removing the solvent and isolating it. When preparing the charge transporting varnish, if a solvent different from the solvent used in synthesizing the polymer compound is used, it may be replaced with the solvent to obtain the desired solvent system.
[0042] In the present invention, the polymer compound may contain repeating units other than the repeating units represented by formula (1). From the viewpoint of reproducibly obtaining a thin film having a high refractive index and high transparency, the content of the repeating units represented by formula (1) is preferably 80 to 100 mol % of all repeating units, more preferably 90 to 100 mol %, even more preferably 95 to 100 mol %, and most preferably 100 mol %, i.e., the repeating units represented by formula (1).
[0043] The charge transporting substance used in the present invention may further contain other charge transporting substances in addition to the polymer compound represented by the above formula (1).
[0044] [ka]
[0045] In the formula, each Ar independently represents an aryl group which may have a substituent or a heteroaryl group which may have a substituent; L represents an alkylene group, -NH-, an oxygen atom, a sulfur atom, or -CN + - represents.
[0046] The aryl group includes an aryl group having 6 to 20 carbon atoms, etc. Specific examples thereof include a phenyl group, a tolyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, a 9-phenanthryl group, etc., with the phenyl group, the tolyl group, and the naphthyl group being preferred.
[0047] Examples of the substituent include a halogen atom, a nitro group, a cyano group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, and an alkynyl group having 2 to 20 carbon atoms.
[0048] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom being preferred.
[0049] The alkyl group having 1 to 20 carbon atoms may be linear, branched, or cyclic. Specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-eicosanyl group. An alkyl group having 1 to 18 carbon atoms is preferred, and an alkyl group having 1 to 8 carbon atoms is more preferred.
[0050] Specific examples of alkenyl groups having 2 to 20 carbon atoms include ethenyl, n-1-propenyl, n-2-propenyl, 1-methylethenyl, n-1-butenyl, n-2-butenyl, n-3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, n-1-pentenyl, n-1-decenyl, and n-1-eicosenyl groups.
[0051] Specific examples of alkynyl groups having 2 to 20 carbon atoms include an ethynyl group, an n-1-propynyl group, an n-2-propynyl group, an n-1-butynyl group, an n-2-butynyl group, an n-3-butynyl group, a 1-methyl-2-propynyl group, an n-1-pentynyl group, an n-2-pentynyl group, an n-3-pentynyl group, an n-4-pentynyl group, a 1-methyl-n-butynyl group, a 2-methyl-n-butynyl group, a 3-methyl-n-butynyl group, a 1,1-dimethyl-n-propynyl group, an n-1-hexynyl group, an n-1-decynyl group, an n-1-pentadecinyl group, and an n-1-eicosynyl group.
[0052] Among the above-mentioned substituents, the aryl group preferably has one or more electron-withdrawing groups. Examples of the electron-withdrawing groups include a halogen atom, a nitro group, and a cyano group, and the like. A halogen atom is preferable, and a fluorine atom is particularly preferable.
[0053] The heteroaryl group preferably includes a heteroaryl group having 2 to 20 carbon atoms. Specific examples thereof include oxygen-containing heteroaryl groups such as a 2-thienyl group, a 3-thienyl group, a 2-furanyl group, a 3-furanyl group, a 2-oxazolyl group, a 4-oxazolyl group, a 5-oxazolyl group, a 3-isoxazolyl group, a 4-isoxazolyl group, and a 5-isoxazolyl group; sulfur-containing heteroaryl groups such as a 2-thiazolyl group, a 4-thiazolyl group, a 5-thiazolyl group, a 3-isothiazolyl group, a 4-isothiazolyl group, and a 5-isothiazolyl group; 2-imidazolyl group, aryl group, 4-imidazolyl group, 2-pyridyl group, 3-pyridyl group, 4-pyridyl group, 2-pyrazyl group, 3-pyrazyl group, 5-pyrazyl group, 6-pyrazyl group, 2-pyrimidyl group, 4-pyrimidyl group, 5-pyrimidyl group, 6-pyrimidyl group, 3-pyridazyl group, 4-pyridazyl group, 5-pyridazyl group, 6-pyridazyl group, 1,2,3-triazin-4-yl group, 1,2,3-triazin-5-yl group, 1,2,4-triazin-3-yl group, 1,2, 4-Triazin-5-yl group, 1,2,4-triazin-6-yl group, 1,3,5-triazin-2-yl group, 1,2,4,5-tetrazin-3-yl group, 1,2,3,4-tetrazin-5-yl group, 2-quinolinyl group, 3-quinolinyl group, 4-quinolinyl group, 5-quinolinyl group, 6-quinolinyl group, 7-quinolinyl group, 8-quinolinyl group, 1-isoquinolinyl group, 3-isoquinolinyl group, 4-isoquinolinyl group, 5-isoquinolinyl group, 6-isoquinolinyl group, and nitrogen-containing heteroaryl groups such as isoquinolinyl group, 7-isoquinolinyl group, 8-isoquinolinyl group, 2-quinoxanyl group, 5-quinoxanyl group, 6-quinoxanyl group, 2-quinazolinyl group, 4-quinazolinyl group, 5-quinazolinyl group, 6-quinazolinyl group, 7-quinazolinyl group, 8-quinazolinyl group, 3-cinnolinyl group, 4-cinnolinyl group, 5-cinnolinyl group, 6-cinnolinyl group, 7-cinnolinyl group, and 8-cinnolinyl group.
[0054] Examples of the substituent on the heteroaryl group include the same substituents as those exemplified for the aryl group.
[0055] L is an alkylene group, -NH-, an oxygen atom, a sulfur atom or -CN+ -, but -CN + - is preferred.
[0056] The alkylene group may be linear, branched, or cyclic, and includes an alkylene group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms. Specific examples thereof include a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a pentamethylene group, and a hexamethylene group.
[0057] An anion of the above formula (a1) that can be suitably used in the present invention includes, but is not limited to, an anion represented by formula (a2).
[0058] [ka]
[0059] On the other hand, examples of the counter cation include those represented by formulas (c1) to (c5). [ka]
[0060] A more preferred embodiment of the onium borate salt is, for example, one represented by the following formula (P-1).
[0061] [ka]
[0062] In the present invention, the above onium borate salts may be used alone or in combination of two or more. If necessary, other known onium borate salts may be used in combination. The onium borate salt can be synthesized by referring to known methods described in, for example, International Publication No. WO 2018 / 147204.
[0063] The onium borate salt may be dissolved in an organic solvent in advance in order to facilitate dissolution in the charge transporting varnish. Examples of such organic solvents include carbonates such as propylene carbonate, ethylene carbonate, 1,2-butylene carbonate, dimethyl carbonate, and diethyl carbonate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone, and 2-heptanone; polyhydric alcohols and derivatives thereof such as ethylene glycol, ethylene glycol monoacetate, diethylene glycol, diethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol, and the monomethyl ether, monoethyl ether, monopropyl ether, monobutyl ether, and monophenyl ether of dipropylene glycol monoacetate; cyclic ethers such as dioxane; and formic acid. Examples of the esters include ethyl, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl pyruvate, ethyl ethoxyacetate, methyl methoxypropionate, ethyl ethoxypropionate, methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, and 3-methyl-3-methoxybutyl acetate; and aromatic hydrocarbons such as toluene, xylene, 3-phenoxytoluene, 4-methoxytoluene, methyl benzoate, cyclohexylbenzene, tetralin, and isophorone. These may be used alone or in combination of two or more. When an organic solvent is used, the proportion of the organic solvent used is preferably 15 to 1,000 parts by mass, and more preferably 30 to 500 parts by mass, based on 100 parts by mass of the onium borate salt.
[0064] In the present invention, the ratio of the onium borate salt to the charge transporting substance can be about 1:0.1-10 (charge transporting substance:onium borate salt) in terms of substance amount (molar) ratio.
[0065] In the present invention, the ratio of the onium borate salt to the charge transporting substance can be within the range not exceeding the above molar ratio, that is, charge transporting substance:onium borate salt=about 1:0.01 to 20, preferably about 1:0.01 to 10, more preferably about 1:0.01 to 2, even more preferably about 1:0.1 to 2, and is optimally about 1:0.15 to 1.
[0066] As the organic solvent used in preparing the charge transporting varnish, a highly soluble solvent capable of dissolving the charge transporting substance and the onium borate salt well can be used. Examples of such highly soluble solvents include, but are not limited to, organic solvents such as cyclohexanone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, diethylene glycol monomethyl ether, 3-phenoxytoluene, 4-methoxytoluene, toluene, anisole, cyclohexylbenzene, methyl benzoate, tetralin, isophorone, etc. These solvents can be used alone or in combination of two or more, and the amount used can be 5 to 100 mass% based on the total solvent used in the varnish.
[0067] Furthermore, in the present invention, the varnish contains at least one high-viscosity organic solvent having a viscosity of 10 to 200 mPa s, particularly 35 to 150 mPa s at 25°C and a boiling point of 50 to 300°C, particularly 150 to 250°C, at normal pressure (atmospheric pressure). This makes it easy to adjust the viscosity of the varnish, and as a result, it becomes possible to prepare a varnish that reproducibly gives a thin film with high flatness and is suited to the application method. Examples of high-viscosity organic solvents include, but are not limited to, cyclohexanol, ethylene glycol, ethylene glycol diglycidyl ether, 1,3-octylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, 1,3-butanediol, 2,3-butanediol, 1,4-butanediol, propylene glycol, hexylene glycol, etc. These solvents may be used alone or in combination of two or more. The proportion of the high-viscosity organic solvent added to the entire solvent used in the varnish of the present invention is preferably within a range in which no solids precipitate, and as long as no solids precipitate, the proportion is preferably 5 to 90 mass %.
[0068] Furthermore, for the purpose of improving the wettability to the substrate, adjusting the surface tension of the solvent, adjusting the polarity, adjusting the boiling point, etc., other solvents can be mixed in an amount of 1 to 90 mass %, preferably 1 to 50 mass %, based on the total solvent used in the varnish. Examples of such solvents include, but are not limited to, propylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether, diacetone alcohol, γ-butyrolactone, ethyl lactate, n-hexyl acetate, etc. These solvents can be used alone or in combination of two or more.
[0069] The viscosity of the varnish of the present invention can be appropriately set depending on the thickness of the thin film to be produced and the solids concentration, but is usually 1 to 50 mPa s at 25°C, and the surface tension is usually 20 to 50 mN / m. The solids concentration of the charge-transporting varnish is appropriately set taking into consideration the viscosity and surface tension of the varnish and the thickness of the thin film to be produced, but is usually about 0.1 to 10.0 mass %, and in order to improve the coatability of the varnish, it is preferably about 0.5 to 5.0 mass %, and more preferably about 1.0 to 3.0 mass %.
[0070] The method for preparing the varnish is not particularly limited, but examples thereof include a method in which the onium borate salt is first dissolved in a solvent and then the charge transporting substance is added thereto in sequence, and a method in which a mixture of the onium borate salt and the charge transporting substance is dissolved in a solvent. In addition, when there are multiple organic solvents, for example, the onium borate salt and the charge transporting substance may be first dissolved in a solvent that dissolves them well, and then other solvents may be added thereto. Alternatively, the onium borate salt and the charge transporting substance may be dissolved in a mixed solvent of multiple organic solvents sequentially or simultaneously.
[0071] In the present invention, from the viewpoint of reproducibly obtaining a uniform thin film having a high refractive index and high transparency, the charge-transporting varnish is desirably prepared by dissolving the above-mentioned onium borate salt, charge-transporting substance, etc. in an organic solvent and then filtering the resultant solution using a filter of the submicrometer order.
[0072] The charge transporting thin film of the present invention can be formed on a substrate by applying the above-described charge transporting varnish onto the substrate and baking it. The method for applying the varnish is not particularly limited, and examples thereof include dipping, spin coating, transfer printing, roll coating, brush coating, inkjet coating, spraying, and slit coating. It is preferable to adjust the viscosity and surface tension of the varnish depending on the application method.
[0073] The firing atmosphere is not particularly limited, and a thin film having a uniform film surface and high charge transport properties can be obtained not only in air but also in an inert gas atmosphere such as nitrogen or in vacuum, but is usually fired in air.
[0074] The baking temperature is appropriately set within a range of about 100 to 260°C, taking into consideration the use of the resulting thin film, the degree of charge transport property to be imparted to the resulting thin film, the type and boiling point of the solvent, etc. However, when the resulting thin film is used as a hole injection layer of an organic EL device, the baking temperature is preferably about 140 to 250°C, and more preferably about 145 to 240°C. During firing, the temperature may be changed in two or more stages in order to achieve a more uniform film formation or to promote the reaction on the substrate. Heating may be performed using a suitable device such as a hot plate or an oven.
[0075] The thickness of the charge transporting thin film is not particularly limited, but is preferably 5 to 300 nm when used as a hole injection layer, a hole transport layer, or a hole injection transport layer of an organic EL device. Methods for changing the thickness include changing the solid concentration in the varnish, changing the amount of solution on the substrate during application, and the like.
[0076] The charge transporting thin film of the present invention described above usually has a refractive index (n) of 1.50 or more and a refractive index of 1.0×10 -2 In one embodiment, the refractive index is 1.60 or more, in another embodiment, the refractive index is 1.65 or more, and in one embodiment, the refractive index is 1.0×10 -3 The following extinction coefficient (k) is 2.0×10 in some other embodiments: -4 The following extinction coefficients (k) are shown:
[0077] The organic EL device of the present invention has a pair of electrodes and a charge transport layer made of the above-mentioned charge transport thin film of the present invention between the electrodes. Representative configurations of the organic EL element include, but are not limited to, the following (a) to (f). In the following configurations, an electron blocking layer or the like can be provided between the light-emitting layer and the anode, and a hole (positive hole) blocking layer or the like can be provided between the light-emitting layer and the cathode, if necessary. In addition, the hole injection layer, the hole transport layer, or the hole injection transport layer may also function as an electron blocking layer, etc., and the electron injection layer, the electron transport layer, or the electron injection transport layer may also function as a hole (positive hole) blocking layer, etc. Furthermore, an arbitrary functional layer can be provided between each layer, if necessary. (a) Anode / hole injection layer / hole transport layer / light emitting layer / electron transport layer / electron injection layer / cathode (b) Anode / hole injection layer / hole transport layer / light emitting layer / electron injection transport layer / cathode (c) Anode / hole injection transport layer / light emitting layer / electron transport layer / electron injection layer / cathode (d) Anode / hole injection transport layer / light emitting layer / electron injection transport layer / cathode (e) Anode / hole injection layer / hole transport layer / light emitting layer / cathode (f) Anode / hole injection transport layer / light emitting layer / cathode
[0078] The "hole injection layer", "hole transport layer" and "hole injection transport layer" are layers formed between the light-emitting layer and the anode, and have the function of transporting holes from the anode to the light-emitting layer. When only one layer of a hole transport material is provided between the light-emitting layer and the anode, it is the "hole injection transport layer". When two or more layers of a hole transport material are provided between the light-emitting layer and the anode, the layer closest to the anode is the "hole injection layer" and the other layers are the "hole transport layers". In particular, the hole injection (transport) layer is a thin film that is excellent not only in terms of hole acceptance from the anode but also in terms of hole injection into the hole transport (light-emitting) layer. An "electron injection layer," "electron transport layer," and "electron injection transport layer" are layers formed between a light-emitting layer and a cathode and have the function of transporting electrons from the cathode to the light-emitting layer. When only one layer of an electron transporting material is provided between the light-emitting layer and the cathode, it is the "electron injection transport layer." When two or more layers of an electron transporting material are provided between the light-emitting layer and the cathode, the layer closest to the cathode is the "electron injection layer," and the other layers are "electron transport layers." The "light-emitting layer" is an organic layer having a light-emitting function, and contains a host material and a dopant material when a doping system is adopted. In this case, the host material mainly has a function of promoting the recombination of electrons and holes and confining the excitons in the light-emitting layer, and the dopant material has a function of efficiently emitting the excitons obtained by the recombination. In the case of a phosphorescent element, the host material mainly has a function of confining the excitons generated by the dopant in the light-emitting layer.
[0079] A charge-transporting thin film prepared from the charge-transporting varnish of the present invention is suitable as a functional layer formed between an emitting layer and an anode in an organic EL element, but is more suitable as a hole injection layer, a hole transport layer, or a hole injection transport layer, and is even more suitable as a hole injection layer.
[0080] When an EL device is produced using the charge transporting varnish of the present invention, the materials to be used and the production method thereof are as follows, but are not limited thereto.
[0081] An example of a method for producing an OLED device having a hole injection layer made of a thin film obtained from the charge transporting varnish is as follows. Note that it is preferable to previously perform surface treatment of the electrodes, such as washing with alcohol, pure water, etc., or UV ozone treatment, oxygen plasma treatment, etc., within a range that does not adversely affect the electrodes. A hole injection layer is formed on an anode substrate by the above-mentioned method using the charge transport varnish. This is introduced into a vacuum deposition apparatus, and a hole transport layer, a light emitting layer, an electron transport layer / hole blocking layer, an electron injection layer, and a cathode metal are sequentially deposited. Alternatively, instead of forming a hole transport layer and a light emitting layer by deposition in the method, these layers are formed by a wet process using a hole transport layer forming composition containing a hole transport polymer and a light emitting layer forming composition containing a light emitting polymer. If necessary, an electron blocking layer may be provided between the light emitting layer and the hole transport layer.
[0082] Examples of anode materials include transparent electrodes such as indium tin oxide (ITO) and indium zinc oxide (IZO), metals such as aluminum, and metal anodes made of alloys thereof, and it is preferable to use those that have been subjected to planarization treatment. Polythiophene derivatives and polyaniline derivatives having high charge transport properties can also be used. Other metals constituting the metal anode include, but are not limited to, gold, silver, copper, indium, and alloys thereof.
[0083] Examples of materials for forming the hole transport layer include triarylamines such as (triphenylamine) dimer derivatives, [(triphenylamine) dimer] spiro dimer, N,N'-bis(naphthalen-1-yl)-N,N'-bis(phenyl)-benzidine (α-NPD), 4,4',4"-tris[3-methylphenyl(phenyl)amino]triphenylamine (m-MTDATA), and 4,4',4"-tris[1-naphthyl(phenyl)amino]triphenylamine (1-TNATA), and oligothiophenes such as 5,5"-bis-{4-[bis(4-methylphenyl)amino]phenyl}-2,2':5',2"-terthiophene (BMA-3T).
[0084] Materials for forming the light-emitting layer include, but are not limited to, low molecular weight light-emitting materials such as metal complexes such as aluminum complexes of 8-hydroxyquinoline, metal complexes of 10-hydroxybenzo[h]quinoline, bisstyrylbenzene derivatives, bisstyrylarylene derivatives, metal complexes of (2-hydroxyphenyl)benzothiazole, and silole derivatives; and systems in which a light-emitting material and an electron transfer material are mixed with a polymer compound such as poly(p-phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly(3-alkylthiophene), or polyvinylcarbazole. In addition, when forming a light-emitting layer by deposition, it may be co-deposited with a light-emitting dopant. The light-emitting dopant may be tris(2-phenylpyridine)iridium(III) (Ir(ppy) 3 ), naphthacene derivatives such as rubrene, quinacridone derivatives, condensed polycyclic aromatic rings such as perylene, but are not limited to these.
[0085] Examples of materials for forming the electron transport layer / hole block layer include, but are not limited to, oxydiazole derivatives, triazole derivatives, phenanthroline derivatives, phenylquinoxaline derivatives, benzimidazole derivatives, pyrimidine derivatives, and the like.
[0086] The material for forming the electron injection layer is lithium oxide (Li 2 O), magnesium oxide (MgO), alumina (Al 2 O 3 ), metal fluorides such as lithium fluoride (LiF) and sodium fluoride (NaF), but are not limited to these. Cathode materials include, but are not limited to, aluminum, magnesium-silver alloy, aluminum-lithium alloy, and the like. Examples of materials for forming the electron blocking layer include, but are not limited to, tris(phenylpyrazole)iridium.
[0087] The hole-transporting polymers include poly[(9,9-dihexylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,1'-biphenylene-4,4-diamine)], poly[(9,9-bis{1'-penten-5'-yl}fluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], and poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine]-endcapped with Examples thereof include polysilcisquinoxane and poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)].
[0088] Examples of the luminescent polymer include polyfluorene derivatives such as poly(9,9-dialkylfluorene) (PDAF), polyphenylenevinylene derivatives such as poly(2-methoxy-5-(2'-ethylhexoxy)-1,4-phenylenevinylene) (MEH-PPV), polythiophene derivatives such as poly(3-alkylthiophene) (PAT), and polyvinylcarbazole (PVCz).
[0089] The materials constituting the anode, cathode and layers formed therebetween differ depending on whether an element having a bottom emission structure or a top emission structure is manufactured, and therefore, the materials are appropriately selected taking this into consideration. Typically, in bottom emission elements, a transparent anode is used on the substrate side and light is extracted from the substrate side, whereas in top emission elements, a reflective anode made of metal is used and light is extracted from the transparent electrode (cathode) side opposite the substrate. In terms of anode material, for example, when manufacturing bottom emission elements, a transparent anode such as ITO is used, and when manufacturing top emission elements, a reflective anode such as Al / Nd is used.
[0090] The organic EL element of the present invention may be sealed, if necessary, with a moisture scavenger or the like in accordance with a standard method in order to prevent deterioration of the characteristics. EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The apparatus used is as follows. (1) Substrate cleaning: Substrate cleaning equipment (low pressure plasma method) manufactured by Choshu Sangyo Co., Ltd. (2) Varnish application: Spin coater MS-A100 manufactured by Mikasa Co., Ltd. (3) Film thickness measurement: Kosaka Laboratory Co., Ltd. Micro-shape measuring instrument Surfcorder ET-4000 (4) Observation of the membrane surface: Lasertec Corporation confocal laser microscope, real-time scanning laser microscope 1LM21D (5) Preparation of EL elements: Multi-function deposition system C-E2L1G1-N manufactured by Choshu Sangyo Co., Ltd. (6) Measurement of luminance of EL elements: Multi-channel IVL measurement device manufactured by EHC Corporation (7) EL element lifetime measurement (luminance half-life measurement): EHC Corporation, Organic EL luminance lifetime evaluation system PEL-105S (8) Measurement of refractive index (n) and extinction coefficient (k): Multi-angle spectroscopic ellipsometer VASE manufactured by J.A. Woollam Japan
[0092] [1] Synthesis of charge transport materials [Synthesis Example 1] Synthesis of polymer (1-1) According to the method described in Synthesis Example 15 of JP2009-283509A, 2,7-position-linked poly-N-[4-{N,N-bis(4'-(4-pentenyl)phenyl)amino}phenyl]-3,6-dimethylcarbazole consisting of repeating units represented by the following formula was synthesized. The weight average molecular weight Mw of the resulting polymer (1-1) was 285,682, and the polydispersity index Mw / Mn was 10.9. [ka]
[0093] [2] Synthesis of onium borate salts [Synthesis Example 2] Synthesis of onium borate salt (P-1) According to the method described in Synthesis Example 1 of WO 2018 / 147204, an onium borate salt (P-1) represented by the following formula was synthesized. [ka]
[0094] [Synthesis Example 3] Synthesis of onium borate salt (P-2) According to the method described in Synthesis Example 1 of WO 2017 / 150412, an onium borate salt (P-2) represented by the following formula was synthesized. [ka]
[0095] [3] Preparation of charge-transporting varnish [Example 1] To a mixture of 77 mg of polymer (1-1) and 77 mg of onium borate salt (P-1), 4.0 g of 3-phenoxytoluene and 1.0 g of 4-methoxytoluene were added and dissolved by stirring at room temperature. The resulting solution was filtered through a syringe filter having a pore size of 0.2 μm to obtain a charge-transporting varnish.
[0096] [Comparative Example 1] To a mixture of 51 mg of polymer (1-1) and 51 mg of onium borate salt (P-2), 4.0 g of cyclohexanone and 1.0 g of anisole were added and dissolved by stirring at room temperature. The resulting solution was filtered through a syringe filter having a pore size of 0.2 μm to obtain a charge transporting varnish.
[0097] [4] Evaluation of refractive index (n) and extinction coefficient (k) [Example 2] The varnish obtained in Example 1-1 was applied to a quartz substrate using a spin coater, and then baked in an air atmosphere at 200° C. for 30 minutes to form a uniform thin film of 50 nm on the quartz substrate. The n value and k value of the obtained quartz substrate were measured using a multi-angle spectroscopic ellipsometer. The results are shown in Table 1.
[0098] [Table 1]
[0099] As shown in Table 1, the charge transporting thin film of the present invention had a high refractive index and an extremely low extinction coefficient.
[0100] [5] Fabrication and characterization of organic electroluminescence devices [Example 3] The varnish obtained in Example 1 was applied to an ITO substrate using a spin coater, and then baked in an air atmosphere at 200°C for 30 minutes to form a 50 nm thin film on the ITO substrate. The ITO substrate was a 25 mm x 25 mm x 0.7 mm glass substrate with a 150 nm thick ITO patterned on the surface. 2 Impurities on the surface were removed using a plasma cleaning device (150 W, 30 seconds). Next, the ITO substrate on which the thin film was formed was placed in a deposition device (vacuum degree 1.0×10 -5 A 120 nm film of α-NPD was formed at 0.2 nm / sec using 1000 sapphire per square millimeter (Pa). Next, a 10 nm film of an electron blocking material HTEB-01 manufactured by Kanto Chemical Co., Ltd. was formed. Next, an emission layer host material NS60 and an emission layer dopant material Ir(ppy) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. were mixed and deposited on the substrate. 3 The co-evaporation was performed with Ir(ppy) 3 The deposition rate was controlled so that the concentration of Alq was 6%, and the film was deposited to a thickness of 40 nm. 3 Thin films of Alq, lithium fluoride and aluminum were successively deposited to obtain an organic EL device. 3The deposition rates for aluminum and lithium fluoride were 0.2 nm / sec and 0.02 nm / sec, respectively, and the film thicknesses were 20 nm, 0.5 nm, and 80 nm, respectively. In order to prevent deterioration of characteristics due to the influence of oxygen, water, etc. in the air, the organic EL element was sealed with a sealing substrate before evaluating its characteristics. Sealing was performed according to the following procedure. In a nitrogen atmosphere with an oxygen concentration of 2 ppm or less and a dew point of -76°C or less, the organic EL element was placed between the sealing substrates, and the sealing substrates were bonded together with an adhesive (MORESCO Moisture Cut WB90US(P) manufactured by MORESCO Corporation). At this time, a moisture scavenger (HD-071010W-40 manufactured by DYNIC Co., Ltd.) was placed inside the sealing substrate together with the organic EL element. The bonded sealing substrates were irradiated with UV light (wavelength: 365 nm, irradiation dose: 6,000 mJ / cm2). 2 ), and then annealed at 80°C for 1 hour to harden the adhesive.
[0101] [Comparative Example 2] An organic EL element was produced in the same manner as in Example 3, except that the varnish obtained in Comparative Example 1 was used instead of the varnish obtained in Example 1.
[0102] The obtained organic EL device had a luminance of 5,000 cd / m 2 The driving voltage, current density, current efficiency, luminous efficiency, external emission quantum yield (EQE), and luminance half-life (initial luminance 10,000cd / m 2 The time required for the luminance to reach half of the original value (the time required for the luminance to reach half of the original value) was measured. The results are shown in Table 2. Note that the EL element prepared in Comparative Example 2 had a luminance of 10 cd / m2 even when a voltage of 8 V was applied. 2 The results are not shown in the table because the results showed poor performance of less than 100%.
[0103] [Table 2]
[0104] As shown in Table 2, the EL device having the charge transporting thin film of the present invention was operated satisfactorily.
Claims
1. The charge transporting material includes an onium borate salt and an organic solvent. a charge-transporting varnish characterized in that the charge-transporting substance comprises a polymeric compound containing a repeating unit represented by the following formula (1), having a weight-average molecular weight (Mw) of 10,000 to 500,000 and a dispersity (Mw / Mn) of 1 to 15, and the onium borate salt comprises an onium borate salt (which is an electrically neutral salt) consisting of a monovalent or divalent anion represented by the following formula (a1) and a counter cation represented by the following formulas (c1) to (c5). 【Chemistry 1】 (In the formula, each R independently represents a hydrogen atom, an alkyl group, or an alkoxy group; Ar 1 and Ar 2 each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group; X represents an alkyl group having a polymerizable functional group, an alkoxy group having a polymerizable functional group, an aromatic hydrocarbon group having a polymerizable functional group, or an aromatic heterocyclic group having a polymerizable functional group; and a and b each independently represent an integer of 1 to 5. 【Chemistry 2】 (In the formula, each Ar independently represents an aryl group which may have a substituent or a heteroaryl group which may have a substituent; L represents an alkylene group, -NH-, an oxygen atom, a sulfur atom, or -CN + - represents.) 【Chemistry 3】
2. 2. The charge transporting varnish according to claim 1, wherein the R is a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.
3. The above Ar 1 and Ar 2 The charge transporting varnish according to claim 1 or 2, wherein each of the groups independently represents a group represented by any one of the following formulas (2-1) to (2-3): 【Chemistry 4】 (In the formula, R 1 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and each c independently represents an integer of 1 to 3.
4. The charge-transporting varnish according to any one of claims 1 to 3, wherein the X's are each independently a group represented by any one of the following formulas (3-1) to (3-4): 【Chemistry 5】 (In the formula, Y and Z each independently represent a single bond, an oxygen atom, a nitrogen atom, a sulfur atom, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent, and f represents an integer of 0 to 10.)
5. 5. The charge transporting varnish according to claim 4, wherein the X is a group represented by the following formula (4): 【Chemistry 6】 (In the formula, Z represents a single bond or an oxygen atom, and g represents an integer of 0 to 10.)
6. 6. The charge-transporting varnish according to claim 1, wherein the charge-transporting substance comprises a polymer compound containing a repeating unit represented by the following formula (1-1): 【Chemistry 7】
7. 7. The charge transporting varnish according to claim 1, wherein Ar is an aryl group having one or more electron-withdrawing substituents.
8. 8. The charge transporting varnish according to claim 7, wherein said electron-withdrawing substituent is a halogen atom.
9. 9. The charge-transporting varnish according to claim 1, wherein the anion is represented by formula (a2): 【Chemistry 8】
10. 10. The charge transporting varnish according to claim 9, wherein the onium borate salt is represented by the following formula (P-1): 【Chemistry 9】
11. 11. The charge transporting varnish according to claim 1, wherein the ratio of the onium borate salt to the charge transporting substance is, in mass ratio, charge transporting substance:onium borate salt=1:0.01-20.
12. A charge transporting thin film obtained from the charge transporting varnish according to any one of claims 1 to 11.
13. 13. An organic electroluminescence device comprising the charge transporting thin film according to claim 11 or 12.
14. A method for producing a charge-transporting thin film, comprising applying the charge-transporting varnish according to any one of claims 1 to 11 onto a substrate, and evaporating the solvent.
Citation Information
Patent Citations
Electronic devices containing organic semiconductors
JP2007536718A
Organic el element and organic el display
JP2009283509A
Organic Light Emitting Display Device and Top Emission Type OLED Device with Improved Viewing Angle Characteristics
JP2017501585A
Oligoaniline compounds
WO2008032616A1
Oligoaniline compound
WO2008129947A1