Rubber composition for tires and tires
By adding aminoguanidine weak acid salts to silica-containing tire rubber compositions, the issues of vulcanization delay and moldability are addressed, resulting in improved fuel efficiency, breaking strength, and abrasion resistance.
Patent Information
- Application Number
- JP2018012967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-01-29
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2038-01-29
AI Technical Summary
The addition of silica to tire rubber compositions improves fuel efficiency but causes issues such as vulcanization delay and silica dispersibility, leading to reduced moldability and increased scorch time.
Incorporating aminoguanidine weak acid salts, such as aminoguanidine bicarbonate or aminoguanidine phosphate, into a rubber composition containing fine particle silica, along with specific amounts of styrene-butadiene rubber and plasticizers, to enhance silica dispersion and improve vulcanization speed while maintaining moldability.
The rubber composition achieves balanced performance in fuel efficiency, breaking strength, and abrasion resistance with improved moldability and vulcanization speed.
Smart Images

Figure 0007587338000001 
Figure 0007587338000002 
Figure 0007587338000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tires and a tire having tire components formed from the rubber composition for tires. [Background technology]
[0002] In recent years, the characteristics required for automobile tires have become more diverse. In particular, there is an increasing demand for low fuel consumption in order to reduce automobile fuel consumption in response to societal demands for energy conservation.
[0003] In order to improve fuel economy, a technique of compounding silica or the like in a rubber composition for tires is known, but compounding silica causes problems such as a decrease in vulcanization speed (vulcanization retardation) and deterioration of dispersibility of silica. In particular, when fine silica is used, there is an advantage that a large specific surface area can be obtained and high reinforcing properties can be obtained, but on the other hand, the above problems become more serious.
[0004] In order to suppress vulcanization delay, it is known to add a specific amine addition salt or the like (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-139727 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the addition of an amine addition salt or the like as described in Patent Document 1 has the problem that the scorch time is shortened, resulting in a decrease in moldability.
[0007] The present invention aims to provide a rubber composition for tires containing silica, which is excellent in fuel economy, breaking strength and abrasion resistance, and further satisfies both molding processability (ensuring molding time) and vulcanization speed (shortening vulcanization time), and to provide a tire having tire components constituted by this rubber composition. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors discovered that the above problem can be solved by further adding an aminoguanidine weak acid salt to a rubber composition containing a specified amount of a specified particulate silica, and after further research, they completed the present invention.
[0009] That is, the present invention provides [1] Per 100 parts by mass of the rubber component The BET nitrogen adsorption specific surface area is 200m 2 / g or more of silica, and Aminoguanidine weak acid salt A rubber composition for tires comprising: [2] The rubber composition for tires according to the above [1], wherein the aminoguanidine weak acid salt is at least one selected from the group consisting of aminoguanidine bicarbonate and aminoguanidine phosphate. [3] The rubber composition for tires according to the above [1] or [2], wherein the content of the aminoguanidine weak acid salt is 0.01 to 10 parts by mass. [4] The rubber composition for tires according to any one of the above [1] to [3], further comprising 30 parts by mass or more of a plasticizer, the plasticizer having a resin content of 5 parts by mass or more. [5] The rubber composition for tires according to any one of the above [1] to [4], wherein the rubber component contains 50% by mass or more of styrene-butadiene rubber. [6] A tire having a tire member formed from the rubber composition for tires according to any one of [1] to [5] above. Regarding. Effect of the Invention
[0010] According to the present invention, it is possible to provide a rubber composition for tires which is excellent in fuel efficiency, breaking strength and abrasion resistance, and which further satisfies both molding processability (ensuring molding time) and vulcanization speed (shortening vulcanization time), and to provide a tire having tire components made of this rubber composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In one embodiment, the nitrogen adsorption specific surface area by the BET method is 200 m per 100 parts by mass of the rubber component. 2 The rubber composition for tires comprises 60 parts by mass or more of silica having a silica content of 60 parts by mass or more and an aminoguanidine weak acid salt.
[0012] Another embodiment of the present invention is a tire having a tire component made of the above-mentioned rubber composition for tires.
[0013] Although it is not intended to be bound by theory, the following is considered to be the mechanism by which the desired effect is obtained in this embodiment. That is, since fine particle silica has a large specific surface area and high reinforcing properties, it can improve fracture strength and abrasion resistance, but on the other hand, its silanol group adsorbs vulcanization accelerator, so that the vulcanization time tends to be too long. However, when aminoguanidine weak acid salt (carbonate, phosphate) is added, the increase in vulcanization time is suppressed even when fine particle silica is highly blended, and as a result, it is considered that fuel efficiency, fracture strength, abrasion resistance, moldability (ensuring molding time), and vulcanization speed (shortening vulcanization time) are improved in a balanced manner. In addition, because of its strong polarity, aminoguanidine not only helps the dispersion of silica, but also helps the hydrolysis reaction of the coupling agent, and as a result, the reactivity between silica and polymer is also increased, and it is presumed that through these, the dispersibility of silica is improved and fuel efficiency is realized.
[0014] <Rubber component> In this embodiment, the rubber component is not particularly limited, and any rubber conventionally used in the tire industry can be suitably used. Examples of the rubber component include isoprene-based rubbers including natural rubber (NR) and polyisoprene rubber (IR), diene-based rubbers such as butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene rubber (SIR), styrene isoprene butadiene rubber (SIBR), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR), and butyl-based rubbers such as halogenated butyl rubbers including butyl rubber (IIR), brominated butyl rubber (Br-IIR), chlorinated butyl rubber (Cl-IIR), and fluorinated butyl rubber (F-IIR). These rubber components may be used alone or in combination of two or more. Among them, those containing NR, SBR, and BR are preferable because the effect of this embodiment can be more satisfactorily exhibited, and those consisting of only NR, SBR, and BR are more preferable.
[0015] (Natural rubber) The NR is not particularly limited, and examples of the NR that can be used include those (unmodified NR) that are common in the tire industry, such as SIR20, RSS#3, and TSR20, as well as modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), grafted natural rubber, deproteinized natural rubber (DPNR), and highly purified natural rubber.
[0016] When NR is contained, the content in the rubber component is preferably 1% by mass or more, more preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more from the viewpoints of molding processability, reinforcement, and fuel economy. Also, from the viewpoint of fuel economy, the content is preferably 35% by mass or less, more preferably 30% by mass or less, more preferably 28% by mass or less, and even more preferably 25% by mass or less.
[0017] (Styrene butadiene rubber) The SBR is not particularly limited, and examples thereof include unmodified emulsion-polymerized styrene butadiene rubber (E-SBR) and solution-polymerized styrene butadiene rubber (S-SBR), and modified SBRs such as modified emulsion-polymerized styrene butadiene rubber (modified E-SBR) and modified solution-polymerized styrene butadiene rubber (modified S-SBR) obtained by modifying these. Modified SBRs include modified SBRs whose terminals and / or main chains are modified, and modified SBRs (condensates, those having a branched structure, etc.) coupled with tin or silicon compounds. In addition, there are oil-extended SBRs in which flexibility is adjusted by adding an extender oil, and non-oil-extended SBRs in which no extender oil is added, and either of these can be used. For example, those manufactured by JSR Corporation, Asahi Kasei Chemicals Corporation, and Nippon Zeon Corporation can be used.
[0018] The styrene content of SBR is preferably 15.0% by mass to 40.0% by mass. From the viewpoint of rubber strength and grip performance, the styrene content is preferably 20.0% by mass or more, more preferably 25.0% by mass or more, even more preferably 30.0% by mass or more, and even more preferably 35.0% by mass or more. From the viewpoint of fuel economy, the styrene content of SBR is preferably 39.0% by mass or less. The styrene content of SBR is preferably, 1 This value is calculated by H-NMR measurement.
[0019] The vinyl content of SBR (amount of 1,2-bonded butadiene units) is preferably 10.0 to 30.0%. From the viewpoints of rubber strength and grip performance, the vinyl content is preferably 13.0% or more, and more preferably 15.0% or more. From the viewpoint of fuel economy, the vinyl content is preferably 25.0% or less, and more preferably 20.0% or less. The vinyl content of SBR is a value measured by infrared absorption spectroscopy.
[0020] When SBR is contained, the content in the rubber component is preferably 35% by mass or more, more preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, because the effects of this embodiment can be better exhibited. The content of SBR is preferably 95% by mass or less, preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. When oil-extended SBR is used as SBR, the content of SBR itself as a solid content contained in the oil-extended SBR is defined as the content of SBR in the rubber component.
[0021] (Butadiene rubber) The BR is not particularly limited, and any of those generally used in this field can be suitably used. For example, various BRs such as high cis-1,4-polybutadiene rubber (high cis BR), rare earth butadiene rubber (rare earth BR) synthesized using a rare earth catalyst, butadiene rubber containing 1,2-syndiotactic polybutadiene crystals (SPB-containing BR), and modified butadiene rubber (modified BR) can be used. As such BR, for example, those manufactured by Ube Industries, Ltd., Zeon Corporation, and Lanxess AG can be suitably used.
[0022] High-cis BR is a butadiene rubber having a cis-1,4 bond content of 90% by mass or more. Among them, a cis-1,4 bond content of 95% by mass or more is preferable, a cis-1,4 bond content of 96% by mass or more is more preferable, a cis-1,4 bond content of 97% by mass or more is even more preferable, and a cis-1,4 bond content of 98% by mass or more is even more preferable. By including high-cis BR, it is possible to improve low-temperature properties and abrasion resistance. The cis-1,4 bond content in BR is a value calculated by infrared absorption spectrum analysis.
[0023] The rare earth BR can be preferably one that is synthesized using a rare earth catalyst and has a vinyl content (amount of 1,2-bonded butadiene units) of 1.8% by mass or less, preferably 1.0% by mass or less, more preferably 0.8% by mass or less, and a cis content (cis-1,4 bond content) of 90% by mass or more, preferably 93% by mass or more, more preferably 95% by mass or more. When the vinyl content and cis-1,4 bond content are within the above ranges, the rubber composition obtained has excellent elongation at break and abrasion resistance. The vinyl content and cis content of the rare earth BR are values measured by infrared absorption spectroscopy.
[0024] As the rare earth element-based catalyst used in the synthesis of the rare earth BR, known catalysts can be used, and examples of such catalysts include lanthanum series rare earth element compounds, organoaluminum compounds, aluminoxanes, halogen-containing compounds, and catalysts containing a Lewis base as necessary.
[0025] In the case of SPB-containing BR, 1,2-syndiotactic polybutadiene crystals are not simply dispersed in the BR, but are dispersed after being chemically bonded to the BR. The complex modulus tends to be improved by dispersing the crystals after being chemically bonded to the rubber component.
[0026] Examples of modified BR include modified BR whose terminals and / or main chain are modified, modified BR coupled with tin, silicon compounds, etc. (condensates, those having a branched structure, etc.), modified BR whose terminals and / or main chain are modified with a functional group that interacts with silica, and in particular modified BR having at least one selected from the group consisting of silyl groups, amino groups, amide groups, hydroxyl groups, and epoxy groups. The use of modified BR provides the effect of strengthening the interaction with fillers and providing excellent fuel economy.
[0027] When BR is contained, the content in the rubber component is preferably 1% by mass or more, more preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more from the viewpoint of abrasion resistance. Also, the content of BR is preferably 35% by mass or less, more preferably 30% by mass or less, more preferably 28% by mass or less, and even more preferably 25% by mass or less from the viewpoint of molding processability.
[0028] <Silica> The rubber composition for tires according to the present embodiment contains a filler having a nitrogen adsorption specific surface area (N2SA) of 200 m2 by the BET method. 2 / g or more of silica (also referred to as "fine particle silica" in this specification). By containing fine particle silica, the effect of improving fuel efficiency can be suitably obtained and high reinforcing properties can be obtained.
[0029] Although it is generally very difficult to disperse finely divided silica in a rubber composition, the rubber composition containing the aminoguanidine weak acid salt of the present embodiment can disperse the finely divided silica well, making it possible to achieve a well-balanced expression of excellent rubber performance.
[0030] The silica is not particularly limited, and can be, for example, silica prepared by a dry method (anhydrous silica) or silica prepared by a wet method (hydrated silica), which is commonly used in the tire industry. Among them, hydrated silica prepared by a wet method is preferred because it has a large number of silanol groups. Silica can be used alone or in combination of two or more types.
[0031] Silica's N2SA is 200m 2 / g or more, 202m 2 / g or more is preferable, and 206m 2 / g or more is more preferable, and 208m 2 / g or more is more preferable, and 210m 2 / g or more is more preferable, and 214m 2 / g or more is more preferable, and 217m 2The upper limit of N2SA is not particularly limited, but from the viewpoint of ease of handling, it is preferably, for example, 500 m 2 / g or less is preferable, and 400m 2 / g or less is more preferable, and 300m 2 / g or less is more preferable, and 280m 2 / g or less is more preferable, and 250m 2 / g or less is more preferable, and 230m 2 / g or less is more preferable. By using silica having an N2SA within the above range, it is possible to improve abrasion resistance, fuel efficiency, and moldability in a well-balanced manner. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-81.
[0032] The content of silica per 100 parts by mass of the rubber component is 60 parts by mass or more, more preferably 65 parts by mass or more, more preferably 70 parts by mass or more, more preferably 75 parts by mass or more, and even more preferably 80 parts by mass or more, from the viewpoint of fuel economy. Also, the content of silica is preferably 150 parts by mass or less, more preferably 140 parts by mass or less, more preferably 130 parts by mass or less, and even more preferably 120 parts by mass or less, from the viewpoints of dispersibility of silica, moldability, and fuel economy.
[0033] <Other fillers> As the filler, other fillers may be used in addition to silica. Such fillers are not particularly limited, and any fillers generally used in this field, such as carbon black, aluminum hydroxide, alumina (aluminum oxide), calcium carbonate, talc, clay, etc., may be used. These fillers may be used alone or in combination of two or more. When a filler other than silica is used as the filler, carbon black is preferred from the viewpoint of rubber strength. That is, the filler preferably contains silica and carbon black, or is preferably composed of only silica and carbon black.
[0034] (Carbon Black) The carbon black is not particularly limited, and any carbon black commonly used in the tire industry, such as GPF, FEF, HAF, ISAF, or SAF, can be used.
[0035] Carbon black N2SA provides sufficient reinforcement and abrasion resistance, and is therefore recommended for use at 50m 2 / g or more is preferable, and 70m 2 / g or more is more preferable, and 90m 2 / g or more is more preferable. In addition, N2SA carbon black has excellent dispersibility and is less likely to generate heat, and is therefore preferred to have a particle size of 500 m 2 / g or less is preferable, and 450m 2 / g or less is more preferable, and 300m 2 / g or less is more preferable, and 250m 2 The N2SA of carbon black is a value measured in accordance with JIS K 6217-2:2001.
[0036] From the viewpoint of wear resistance, the DBP oil absorption of carbon black is preferably 50 ml / 100 g or more, more preferably 100 ml / 100 g or more. From the viewpoint of grip performance, the DBP oil absorption of carbon black is preferably 250 ml / 100 g or less, more preferably 200 ml / 100 g or less, and more preferably 150 ml / 100 g or less. The DBP oil absorption of carbon black is a value measured in accordance with JIS K 6217-4:2008.
[0037] When carbon black is contained, the content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 7 parts by mass or more, from the viewpoint of obtaining sufficient reinforcement and abrasion resistance. Also, the content of carbon black is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, from the viewpoints of molding processability, fuel economy, and abrasion resistance.
[0038] <Silane coupling agent> Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and any silane coupling agent that has been conventionally used in combination with silica in the rubber industry can be used. Examples of such silane coupling agents include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(4-trimethoxysilylbutyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-triethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)trisulfide, silane coupling agents having a sulfide group such as bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-trimethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazole tetrasulfide, and 3-trimethoxysilylpropyl methacrylate monosulfide;Silane coupling agents having a mercapto group, such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT-Z100, NXT-Z45, and NXT; silane coupling agents having a vinyl group, such as vinyltriethoxysilane and vinyltrimethoxysilane; amino groups, such as 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane; Silane coupling agents having a group; glycidoxy-based silane coupling agents such as γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and γ-glycidoxypropylmethyldimethoxysilane; nitro-based silane coupling agents such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; chloro-based silane coupling agents such as 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 2-chloroethyltrimethoxysilane, and 2-chloroethyltriethoxysilane; and the like. These silane coupling agents may be used alone or in combination of two or more. Among them, sulfide-based and mercapto-based agents are preferred because they have a strong bond with silica and are excellent in fuel economy characteristics. In addition, the use of mercapto-based agents is also preferred because it can suitably improve fuel economy characteristics and wear resistance.;
[0039] When containing silane coupling agent, the content relative to 100 parts by mass of silica is preferably 1.0 parts by mass or more, more preferably 2.0 parts by mass or more, more preferably 4.0 parts by mass or more, and even more preferably 6.0 parts by mass or more, because it can obtain sufficient silica dispersibility and viscosity reduction effects. Also, because it can obtain sufficient coupling effect and silica dispersion effect efficiently and ensure reinforcement, the content of silane coupling agent is preferably 20.0 parts by mass or less, more preferably 18.0 parts by mass or less, and even more preferably 15.0 parts by mass or less.
[0040] <Aminoguanidine weak acid salt> The rubber composition for tires according to this embodiment is characterized by containing an aminoguanidine weak acid salt.
[0041] In the present embodiment, the aminoguanidine weak acid salt is a salt of aminoguanidine and a weak acid, in which the guanidine moiety of aminoguanidine forms a salt with the weak acid. The aminoguanidine weak acid salt may be a salt of one molecule of the weak acid and one molecule of aminoguanidine, or a salt of one molecule of the weak acid and two molecules of aminoguanidine.
[0042] The aminoguanidine weak acid salt is not particularly limited as long as it can exhibit the effects of the present embodiment. The weak acid used in the aminoguanidine weak acid salt can be any organic acid or inorganic acid, but is preferably an inorganic acid. Specific examples of the aminoguanidine weak acid salt include, for example, aminoguanidine bicarbonate (aminoguanidine bicarbonate) consisting of aminoguanidine and carbonic acid, and aminoguanidine phosphate consisting of aminoguanidine and phosphoric acid. Such aminoguanidine weak acid salts may be used alone or in combination of two or more. Among them, from the viewpoint of better exhibiting the effects of the present embodiment by containing an aminoguanidine weak acid salt, being excellent in fuel efficiency, breaking strength and abrasion resistance, and further achieving both moldability and vulcanization speed, it is preferable to contain at least one selected from the group consisting of aminoguanidine bicarbonate and aminoguanidine phosphate. In addition, the aminoguanidine weak acid salt is preferably aminoguanidine bicarbonate, or preferably aminoguanidine phosphate, or preferably composed of aminoguanidine bicarbonate and aminoguanidine phosphate.
[0043] The aminoguanidine weak acid salt of the present embodiment can be obtained by a known method, for example, a method of mixing aminoguanidine bicarbonate and a weak acid. Note that, as the aminoguanidine bicarbonate and the weak acid, commercially available products can be used. For example, products manufactured by Tokyo Chemical Industry Co., Ltd. can be used.
[0044] The content of the aminoguanidine weak acid salt is preferably 0.01 to 10 parts by mass based on 100 parts by mass of the rubber component. The content of the aminoguanidine weak acid salt is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, more preferably 0.30 parts by mass or more, and even more preferably 0.50 parts by mass or more. The content of the aminoguanidine weak acid salt is preferably 9 parts by mass or less, more preferably 7 parts by mass or less, more preferably 5 parts by mass or less, more preferably 3 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less. By setting it in such a range, the effect of the present embodiment can be more satisfactorily exhibited.
[0045] <Plasticizer> The rubber composition for a tire according to the present embodiment preferably further contains a plasticizer.
[0046] The plasticizer is not particularly limited, and may be a plasticizer commonly used in the rubber industry or a softener, including any known plasticizer, such as resin, oil, liquid polymer, or low-temperature plasticizer. The plasticizer may be used alone or in combination of two or more. Among them, resin, oil, and liquid polymer are preferred, resin and oil are more preferred, and it is more preferred to use only resin and oil, because the effects of the present embodiment can be more effectively exhibited.
[0047] (resin) The resin is not particularly limited, and any resin commonly used in the rubber industry can be suitably used, such as terpene resins, hydrogenated terpene resins, C5-C9 resins, styrene / α-methylstyrene copolymer resins, adhesive resins, crosslinkable resins, and compatibilizing resins.
[0048] The softening point of these resins is preferably within the range of -20 to 180°C from the viewpoint of favorably exerting the function as a plasticizer. The upper limit of the softening point is preferably 170°C or lower, more preferably 150°C or lower, and even more preferably 130°C or lower. The lower limit of the softening point is preferably -10°C or higher, and more preferably -5°C or higher. In this specification, the softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K 6220-1 is measured using a ring and ball softening point measuring device.
[0049] The weight average molecular weight (Mw) of these resins is preferably within a predetermined range from the viewpoint of obtaining good moldability and ensuring rubber hardness. Specifically, Mw is preferably 120,000 or less, more preferably 10,000 or less, and even more preferably 5,000 or less. Mw is preferably 200 or more, more preferably 250 or more, even more preferably 300 or more, and even more preferably 350 or more. In this specification, Mw of a resin is a value calculated by converting it into standard polystyrene based on a measurement value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMALTPORE HZ-M manufactured by Tosoh Corporation).
[0050] <Styrene / α-methylstyrene copolymer resin> The styrene / α-methylstyrene copolymer resin is a resin obtained by polymerizing styrene and α-methylstyrene.
[0051] <Hydrogenated terpene resin> The hydrogenated terpene resin is obtained by hydrogenating a terpene resin. The hydrogenation treatment of the terpene resin can be carried out by a known method.
[0052] The hydrogenated terpene resin is not particularly limited, and examples thereof include polyterpene resins made of at least one terpene raw material selected from α-pinene, β-pinene, limonene, dipentene, etc., aromatic modified terpene resins made from terpene compounds and aromatic compounds, and terpene phenolic resins made from terpene compounds and phenolic compounds. Examples of aromatic compounds that are raw materials for aromatic modified terpene resins include styrene, α-methylstyrene, vinyltoluene, divinyltoluene, etc., and examples of phenolic compounds that are raw materials for terpene phenolic resins include phenol, bisphenol A, cresol, xylenol, etc.
[0053] <Adhesive resin> The adhesive resin is usually an oligomer having a molecular weight of several hundred to several tens of thousands, which has a property of being compatible or at least semi-compatible with the rubber component. By blending the adhesive resin, the adhesiveness (molding processability) of the unvulcanized material during tire molding is improved. Here, the adhesive resin is not particularly limited, and any resin other than those mentioned above that is usually used in the rubber industry can be suitably used, for example, phenolic resin, coumarone-indene resin, terpene resin, styrene resin, acrylic resin, rosin resin, dicyclopentadiene resin (DCPD resin), etc. can be mentioned. As the phenolic resin, for example, those manufactured by BASF and Taoka Chemical Co., Ltd. can be used, as the coumarone-indene resin, for example, those manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. and JXTG Energy Co., Ltd. can be used, as the styrene resin, for example, those manufactured by Arizona Chemical Co., Ltd. can be used. As the terpene resin, for example, those manufactured by Arizona Chemical Co., Ltd. and Yasuhara Chemical Co., Ltd. can be used. Examples of rosin-based resins that can be used include those manufactured by Harima Chemical Industries Co., Ltd. and Arakawa Chemical Industries Co., Ltd. Among them, it is preferable to use phenol-based resins, coumarone-indene resins, terpene-based resins, and acrylic resins because they have excellent grip performance.
[0054] <Liquid resin> As the resin, a liquid resin (liquid resin) can be preferably used from the viewpoint of exerting a good effect as a plasticizer. Here, the liquid resin refers to a resin that is not hardened at room temperature (25° C.).
[0055] As the liquid resin, for example, liquid coumarone-indene resin, liquid terpene resin, etc. can be suitably used. Among them, liquid coumarone-indene resin is preferable.
[0056] The liquid coumarone-indene resin contains coumarone and indene as monomer components constituting the skeleton (main chain) of the resin. In addition, examples of monomer components contained in the skeleton other than coumarone and indene include styrene, α-methylstyrene, methylindene, and vinyltoluene. The softening point of the liquid coumarone-indene resin is preferably -20 to 45°C. The upper limit is preferably 40°C or lower, more preferably 35°C or lower. The lower limit is preferably -10°C or higher, more preferably -5°C or higher. As the liquid coumarone-indene resin, for example, a product manufactured by Rutgers Chemicals can be suitably used.
[0057] (oil) The oil is not particularly limited, and any oil commonly used in the rubber industry can be suitably used, such as process oil, vegetable oil, and animal oil. Examples of process oil include paraffinic process oil, naphthenic process oil, and aromatic process oil. Examples of vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, safflower oil, and tung oil. Examples of animal oil include oleyl alcohol, fish oil, and beef tallow. Among them, process oil is preferred because it is advantageous in terms of processability, and process oil with a low content of polycyclic aromatic compounds (PCA) (low PCA content process oil) is preferred because of the reduction of the burden on the environment.
[0058] Examples of low PCA content process oils include Treated Distillate Aromatic Extract (TDAE), which is a re-extraction of aromatic process oil, aroma substitute oils which are mixtures of asphalt and naphthenic oil, mild extraction solvates (MES), and heavy naphthenic oil.
[0059] (Liquid Polymer) The liquid polymer has a weight average molecular weight of 1.0×10 in terms of polystyrene measured by gel permeation chromatography (GPC). 3 ~2.0×10 5 By setting the content in this range, it is possible to obtain a good balance between fracture properties, durability, and moldability.
[0060] The liquid polymer is not particularly limited, and any of those commonly used in the rubber industry can be suitably used, such as liquid SBR, liquid BR, liquid IR, liquid SIR, etc. Among them, it is preferable to use liquid SBR, since it can improve durability and grip performance in a well-balanced manner.
[0061] (Low temperature plasticizer) The low-temperature plasticizer is not particularly limited, and any of those commonly used in the rubber industry can be suitably used. Examples of the low-temperature plasticizer include ester-based plasticizers such as dibutyl adipate (DBA), diisobutyl adipate (DIBA), dioctyl adipate (DOA), di-2-ethylhexyl azelate (DOZ), dibutyl sebacate (DBS), diisononyl adipate (DINA), diethyl phthalate (DEP), dioctyl phthalate (DOP), diundecyl phthalate (DUP), dibutyl phthalate (DBP), dioctyl sebacate (DOS), tributyl phosphate (TBP), trioctyl phosphate (TOP), triethyl phosphate (TEP), trimethyl phosphate (TMP), thymidine triphosphate (TTP), tricresyl phosphate (TCP), and trixylenyl phosphate (TXP). Among these, DOS and TOP are preferred from the viewpoint of the balance between the plasticizing effect and the wear resistance at low temperatures, and DOS is preferred from the viewpoint of excellent fuel economy.
[0062] From the viewpoint of a sufficient grip improving effect, the freezing point of the low-temperature plasticizer is preferably −50° C. or lower, and more preferably −70° C. or lower. The lower limit of the freezing point of the low-temperature plasticizer is not particularly limited.
[0063] From the viewpoint of a sufficient grip improving effect, the viscosity of the low-temperature plasticizer at 25° C. is preferably 30 mPa·s or less, and more preferably 20 mPa·s or less. The lower limit of the viscosity of the low-temperature plasticizer is not particularly limited.
[0064] (Content) The content of the plasticizer per 100 parts by mass of the rubber component is preferably within a predetermined range from the viewpoints of fuel economy and abrasion resistance. That is, the content of the plasticizer is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, preferably 35 parts by mass or more, and even more preferably 40 parts by mass or more. The content of the plasticizer is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less. The content of the plasticizer includes not only the oil components contained in the oil-extended rubber and insoluble sulfur, but also the later-added oil (oil blended separately from the oil components contained in the oil-extended rubber and insoluble sulfur).
[0065] The content of the resin among the plasticizers is preferably 1 part by mass or more, more preferably 2 parts by mass or more, more preferably 3 parts by mass or more, more preferably 4 parts by mass or more, and even more preferably 5 parts by mass or more. The content of the resin is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less.
[0066] When only oil and resin are used as plasticizers, the oil content per 100 parts by mass of the rubber component is determined by subtracting the resin content from the plasticizer content.
[0067] <Other compounding agents> In addition to the above-mentioned components, the rubber composition according to the present embodiment may contain, as appropriate, compounding agents that are generally used in the manufacture of rubber compositions, such as zinc oxide, stearic acid, antioxidants, waxes, vulcanizing agents, and vulcanization accelerators.
[0068] (Anti-aging agent) The antiaging agent is not particularly limited, and any of those commonly used in the rubber industry can be suitably used, such as amine-ketone antiaging agents, imidazole antiaging agents, amine antiaging agents, phenol antiaging agents, sulfur antiaging agents, phosphorus antiaging agents, etc. Antiaging agents may be used alone or in combination of two or more.
[0069] When an antioxidant is contained, the content thereof is preferably 0.5 parts by mass or more, and more preferably 1.0 parts by mass or more, based on 100 parts by mass of the rubber component. The content of the antioxidant is preferably 7 parts by mass or less, and more preferably 5 parts by mass or less. By setting the content within such a range, the effect of the present embodiment can be more satisfactorily exhibited.
[0070] (wax) The wax is not particularly limited, and any wax commonly used in the rubber industry can be suitably used, such as paraffin wax manufactured by Nippon Seiro Co., Ltd. and Paramelt Co., Ltd. The wax may be used alone or in combination of two or more kinds.
[0071] When the wax is contained, the content thereof per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.2 parts by mass or more. Also, the content is preferably 3.0 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less. By setting the content within such a range, the effect of the present embodiment can be more satisfactorily exhibited.
[0072] (Vulcanizing agent) The vulcanizing agent is not particularly limited, and known vulcanizing agents can be used, such as sulfur, organic peroxides, resin vulcanizing agents, and metal oxides such as magnesium oxide. Of these, it is preferable to use sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur, and insoluble sulfur, and any of these can be suitably used. The vulcanizing agent may be used alone or in combination of two or more.
[0073] When sulfur is contained as a vulcanizing agent, the content thereof is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, based on 100 parts by mass of the rubber component. The content of sulfur is preferably 7 parts by mass or less, more preferably 5 parts by mass or less. By setting the content within such a range, the effect of the present embodiment can be more satisfactorily exhibited.
[0074] (Vulcanization accelerator) The vulcanization accelerator is not particularly limited, and known vulcanization aids can be used, such as sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based or aldehyde-ammonia-based, imidazoline-based, or xanthate-based vulcanization accelerators. Among them, sulfenamide-based and guanidine-based are preferred because they can achieve a good balance between scorch time and vulcanization time. The vulcanization accelerator may be used alone or in combination of two or more.
[0075] Examples of sulfenamide vulcanization accelerators include N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), N,N'-dicyclohexyl-2-benzothiazolylsulfenamide (DZ), etc. Among them, N-cyclohexyl-2-benzothiazolylsulfenamide (CBS) is preferred.
[0076] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine (DPG), di-orthotolylguanidine, orthotolylbiguanidine, etc. Among them, 1,3-diphenylguanidine (DPG) is preferred from the viewpoint of shortening the vulcanization time.
[0077] In this embodiment, it is more preferable to use only N-cyclohexyl-2-benzothiazolylsulfenamide (CBS) and 1,3-diphenylguanidine (DPG) as the vulcanization accelerator, because this allows the effects of this embodiment to be exhibited more satisfactorily.
[0078] When a vulcanization accelerator is contained, the content thereof is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 2.0 parts by mass or more, based on 100 parts by mass of the rubber component. The content of the vulcanization accelerator is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 3.5 parts by mass or less. By setting the content within such a range, the effect of the present embodiment can be more satisfactorily exhibited.
[0079] <Production of Rubber Composition for Tires> The rubber composition for tires of this embodiment is produced by a known method. For example, it can be produced by kneading the above-mentioned components with a Banbury mixer, a kneader, an open roll, etc., and then vulcanizing the components. When kneading, the components other than the vulcanizing agent and the vulcanization accelerator are first kneaded, and then the vulcanizing agent and the vulcanization accelerator are added to the kneaded mixture and kneaded. The method of compounding the aminoguanidine weak acid salt is not particularly limited, and it can be directly compounded as a powder, but other than such a compounding method, it can also be compounded by, for example, dissolving it in a solvent and compounding it as a solution, or compounding it as an emulsion solution.
[0080] <Rubber composition for tires> The rubber composition for tires of the present embodiment can be used for each tire component such as the tread, undertread, carcass, sidewall, bead, etc. In particular, it is preferable to form a tire having a tread composed of the rubber composition for tires of the present embodiment, since it is excellent in fuel economy, breaking strength, and abrasion resistance.
[0081] <Tire manufacturing> The tire of this embodiment can be manufactured by a normal method using the rubber composition for tires. That is, the rubber composition for tires is extruded in an unvulcanized state to match the shape of a tire component such as a tire tread, molded in a tire molding machine by a normal method, and laminated together with other tire components to form an unvulcanized tire. The tire of this embodiment can be manufactured by heating and pressurizing this unvulcanized tire in a vulcanizer. The vulcanization temperature is not particularly limited as long as it is a general vulcanization temperature in the tire industry, and is, for example, 120°C or higher and 200°C or lower, preferably 140°C or higher and 180°C or lower.
[0082] <Tires> The tire of the present embodiment may be either a pneumatic tire or a non-pneumatic tire, but is preferably a pneumatic tire. In addition, the pneumatic tire can be used for various tires such as passenger car tires, truck and bus tires, motorcycle tires, high performance tires such as racing tires, and run-flat tires.
[0083] <Other> In this specification, when a numerical range is expressed as "10 to 100," the numerical range includes both ends of the range unless otherwise specified. EXAMPLES
[0084] The present embodiment will be described based on examples, but the present embodiment is not limited to only the examples.
[0085] The various chemicals used in the examples and comparative examples are listed below. Natural rubber (NR): TSR20 Styrene butadiene rubber (SBR): Buna VSL2525-0 manufactured by LANXESS Butadiene rubber (BR): UBEPOL 150B manufactured by Ube Industries, Ltd. Carbon black (CB): Diaplac I manufactured by Mitsubishi Chemical Corporation Silica 1: Solvay's ZHRS 1200MP (N2SA (BET): 200m 2 / g) Silica 2: Zeosil Premium 200 MP (N2SA (BET): 220m) manufactured by Solvay 2 / g) Silica 3: Evonik Ultrasil VN3 (N2SA (BET): 175 m 2 / g) Silane coupling agent (coupling agent): Si69 (bis(3-triethoxysilylpropyl)tetrasulfide) manufactured by Evonik Liquid resin: NOVARES C10 (liquid coumarone-indene resin, softening point: 5 to 15°C) manufactured by Ruetgers Chemicals Oil: Process X-140 manufactured by Japan Energy Co., Ltd. Anti-aging agent: Crack 6C manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Stearic acid Zinc oxide sulfur Accelerator 1: N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS) Vulcanization accelerator 2: 1,3-diphenylguanidine (DPG) Aminoguanidine weak acid salt 1 (AG weak acid salt 1): Aminoguanidine phosphate Aminoguanidine Weak Acid Salt 2 (AG Weak Acid Salt 2): Aminoguanidine bicarbonate Aminoguanidine hydrochloride (AG hydrochloride)
[0086] Examples 1 to 4 and Comparative Examples 1 to 6 Among the ingredients shown in Table 1, various chemicals (except sulfur and vulcanization accelerators 1 and 2) are kneaded in a Banbury mixer to obtain a kneaded product. Next, sulfur and vulcanization accelerators 1 and 2 are added to the kneaded product obtained using an open roll and kneaded to obtain an unvulcanized rubber composition.
[0087] A vulcanized rubber composition is produced by molding the unvulcanized rubber composition into a desired shape and press-vulcanizing it under the condition of 170° C. The vulcanization time is set to twice the vulcanization characteristic t90 at 170° C. determined below.
[0088] The unvulcanized rubber composition is extruded using an extruder equipped with a nozzle in the shape of a tread, and then laminated together with other tire components to form an unvulcanized tire. A test tire (size: 195 / 65R15) is manufactured by press-vulcanizing the tire under a condition of 170°C.
[0089] <Moldability> For the unvulcanized rubber composition, a vulcanization test is carried out at a measurement temperature of 130°C using a vibration vulcanization tester (curelastometer) described in JIS K 6300, and a vulcanization rate curve is obtained by plotting time and torque. The minimum torque value of the vulcanization rate curve is ML, the maximum torque value is MH, and the difference (MH-ML) is ME. The time t10 (scorch time) (minutes) at which ML+0.1ME is reached is read. The scorch time of the reference comparative example is set to 100, and the results are expressed as an index according to the following formula. The larger the value, the longer the scorch time and the better the moldability. (Moldability index)= {(Scorch time of each formulation) / (Scorch time of standard comparison example)} x 100
[0090] <Vulcanization speed> For the unvulcanized rubber composition, a viscoelasticity measuring device (manufactured by Alpha Technologies, product name: RPA2000) was used to determine the vulcanization characteristic t90 at 170°C, which was taken as the vulcanization time. The vulcanization time of the reference comparative example was set to 100, and the value was expressed as an index using the following calculation formula. The larger the value, the shorter the vulcanization time. (Vulcanization speed index) = {(Vulcanization time of the reference comparative example) / (Vulcanization time of each compound)} x 100
[0091] <Breaking strength> Using a No. 6 dumbbell-shaped test piece made of a vulcanized rubber composition, a tensile test is carried out in an atmosphere of 25°C in accordance with JIS K 6251:2010 "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties" to measure the breaking strength TB (MPa) and the elongation at break EB (%). Then, the value of TB x EB / 2 (MPa%) is calculated. The calculated value is converted into an index using the following formula, with the reference comparative example being set at 100. The larger the value, the better the breaking strength. (Breaking strength index) = {(value for each compound) / (value for the reference comparison example)} x 100
[0092] <Wear resistance> For the vulcanized rubber composition, the Lambourn abrasion amount is measured using a Lambourn abrasion tester under the conditions of a temperature of 20°C, a slip rate of 20%, and a test time of 2 minutes. Furthermore, the volume loss amount is calculated from the measured Lambourn abrasion amount, and the abrasion resistance index of the reference comparative example is set to 100, and the abrasion resistance of each compound is expressed as an index according to the following calculation formula. The larger the value, the more excellent the abrasion resistance. (Wear resistance index) = {(Volume loss of the reference comparative example) / (Volume loss of each formulation)}×100
[0093] <Fuel-efficient> The loss tangent (tanδ) of each compound was measured using a viscoelasticity spectrometer VES (manufactured by Iwamoto Seisakusho Co., Ltd.) under the conditions of a temperature of 50°C, an initial strain of 10%, a dynamic strain of 2%, and a frequency of 10 Hz. 50℃ The fuel economy of each compound is expressed as an index using the following formula, with the fuel economy index of the standard comparative example being set at 100. The larger the value, the smaller the rolling resistance and the better the fuel economy. (Fuel Efficiency Index) = {(tan δ of the reference comparison example 50℃ ) / (tan δ of each compound 50℃ )}×100
[0094] By conducting the above tests based on the composition in Table 1, each index or a value close to it can be obtained.
[0095] [Table 1]
[0096] In this embodiment, the target values of the moldability index and the vulcanization rate index are not less than 100. The breaking strength index, the abrasion resistance index and the fuel economy index are each preferably greater than 100, and the higher the index the more desirable it is.
Claims
1. Relative to 100 parts by mass of the rubber component, BET nitrogen adsorption specific surface area is 200m 2 / g or more of silica, and Aminoguanidine weak acid salt A rubber composition for tires comprising: The rubber component of the rubber composition for tires comprises at least one of a styrene butadiene rubber and a butadiene rubber. (However, the following rubber compositions for tires (a) and (b) are excluded: (A) a rubber composition for tires containing zinc phosphate; (b) A rubber composition for tires, comprising a compound represented by the following formula (1): 【Chemistry 1】 (n is 1 or 2.)
2. 2. The rubber composition for tires according to claim 1, wherein the rubber component comprises a styrene-butadiene rubber, a natural rubber and a butadiene rubber.
3. Relative to 100 parts by mass of the rubber component, BET nitrogen adsorption specific surface area is 200m 2 / g or more of silica, Carbon black: more than 0 parts by mass and not more than 30 parts by mass; Plasticizers, and Aminoguanidine weak acid salt A rubber composition for tires comprising: the rubber component contains more than 0 mass% and 35 mass% or less of natural rubber, 50 mass% or more of styrene-butadiene rubber, and butadiene rubber, The plasticizer comprises a resin, and the resin comprises a liquid resin. (However, the following rubber compositions for tires (a) and (b) are excluded: (A) a rubber composition for tires containing zinc phosphate; (b) A rubber composition for tires, comprising a compound represented by the following formula (1): 【Chemistry 2】 (n is 1 or 2.)
4. The rubber composition for tires according to any one of claims 1 to 3, wherein the content of the butadiene rubber in the rubber component is 28 mass % or less.
5. 3. The rubber composition for tires according to claim 1, wherein the aminoguanidine weak acid salt comprises aminoguanidine bicarbonate.
6. 4. The rubber composition for tires according to claim 3, wherein the aminoguanidine weak acid salt is aminoguanidine bicarbonate.
7. The rubber composition for tires according to any one of claims 1 to 6, wherein the content of the aminoguanidine weak acid salt is 0.01 to 10 parts by mass.
8. The rubber composition for tires according to any one of claims 1 to 7, comprising 30 parts by mass or more of a plasticizer, the plasticizer containing a resin in an amount of 5 parts by mass or more.
9. 9. The rubber composition for tires according to claim 8, wherein the resin is a liquid resin.
10. The BET nitrogen adsorption specific surface area of silica is 208 m 2 The rubber composition for tires according to any one of claims 1 to 9, wherein the viscosity is 100% or more.
11. The BET nitrogen adsorption specific surface area of silica is 230m 2 The rubber composition for tires according to any one of claims 1 to 10, wherein the viscosity is 100 / g or less.
12. The rubber composition for tires according to any one of claims 1 to 11, wherein the content of silica is 70 parts by mass or more per 100 parts by mass of the rubber component.
13. A tire having a tire member formed from the rubber composition for tires according to any one of claims 1 to 12.
14. 14. The tire of claim 13, wherein the tire component is a tread.
Citation Information
Patent Citations
Bottom structure of vessel made of plastic
JP1987028335A
Rubber composition
JP2001139727A
Rubber composition for tire and pneumatic tire
JP2013053296A
Modified rubber for tyre, rubber composition for tyre using said modified rubber and tyre
WO2015190519A1
Rubber composition and tire
WO2017038474A1