Wavelength-selectively transparent polycarbonate resin composition

A polycarbonate resin composition with specific additives maintains optical stability during high-temperature molding, enabling cost-effective large-scale production of wavelength-selective articles for lidar applications.

JP7587405B2Active Publication Date: 2024-11-20SUMIKA POLYCARBONATE LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020200101
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-02
Publication Date
2024-11-20
Estimated Expiration
2040-12-02

AI Technical Summary

Technical Problem

Existing polycarbonate resin compositions for lidar applications are not suitable for large-scale production at low cost, and their optical properties change significantly during high-temperature molding, affecting their performance.

Method used

A polycarbonate resin composition containing an aromatic polycarbonate resin, a dye with a maximum absorption wavelength of less than 1200 nm, and a phosphoric acid or phosphoric acid ester compound, which maintains optical properties during high-temperature molding and provides wavelength-selective transmittance.

Benefits of technology

The composition allows for large-scale production of polycarbonate resin articles with stable optical properties, suitable for lidar applications by maintaining wavelength selectivity and preventing changes in transmittance during molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587405000001
    Figure 0007587405000001
  • Figure 0007587405000002
    Figure 0007587405000002
  • Figure 0007587405000003
    Figure 0007587405000003
Patent Text Reader

Abstract

To provide a polycarbonate resin composition having wavelength selective transmissivity without causing a substantial change in optical properties even when molded at high temperature, and a molding thereof.SOLUTION: A wavelength selective transmissive polycarbonate resin composition includes: an aromatic polycarbonate resin (A); a colorant (B) including dye having the maximum absorbance wavelength of less than 1200 nm; and a phosphoric ester based compound or phosphoric acid (C). The colorant (B) of 0.001-2.0 pts.mass and the phosphoric ester based compound (C1) of 0.005-0.3 pts.mass or the phosphoric acid (C2) of 0.0001-0.004 pts.mass in the phosphoric ester based compound or phosphoric acid (C) are included to 100 pts.mass of the aromatic polycarbonate resin (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wavelength-selectively transparent polycarbonate resin composition, and more particularly to a polycarbonate resin composition that is wavelength-selectively transparent and does not transmit visible light but transmits infrared light. [Background technology]

[0002] One of the optical remote sensing techniques is LIDAR (Light Detection and Ranging, Laser Imaging Detection and Ranging), which measures the scattered light from a pulsed laser to analyze the distance and properties of distant objects. This technique is similar to radar, but uses light instead of radio waves. The distance to an object is determined by the time it takes to receive the reflected light after emitting it. LIDAR uses electromagnetic waves with much shorter wavelengths than radar, typically ultraviolet, visible, or near infrared.

[0003] In recent years, autonomous driving technology for automobiles has been developing rapidly. To support level 3, which is conditional autonomous driving, and levels 4 to 5, which do not assume driving by a driver, a function for safe autonomous driving on highways and general roads is required. Therefore, in order to ensure sensing redundancy, in addition to cameras and millimeter-wave radar, Lidar is attracting attention. To support autonomous driving, it is necessary to further improve the accuracy of Lidar, and there is a demand to develop wavelength selection filters with superior performance.

[0004] Patent Document 1 discloses that an epoxy resin cured body containing an azoanthraquinone-based mixture or the like has an average transmittance of 0% in the wavelength range of 380 nm and an optical transmittance of 80% or more at a wavelength of 900 nm, and therefore can be suitably used when the laser light wavelength used in Lidar is in the range of 850 to 950 nm (see Patent Document 1, Examples 1 to 2,

[0050] , [Figure 1]). Furthermore, Patent Document 1 discloses that an epoxy resin cured body containing an azoanthraquinone-based mixture or the like has an average transmittance of 0% in the wavelength range of 380 nm and an optical transmittance of 80% or more at a wavelength of 1550 nm, and therefore can be suitably used when the laser light wavelength used in Lidar is in the range of 1500 to 1600 nm (see Patent Document 1, Examples 1 to 3,

[0050] , [Figure 1]). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-167484 A Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 discloses a cured epoxy resin, but the cured epoxy resin is not necessarily suitable for mass production at low cost. Considering the future development of Lidar, it is necessary to provide a composition and a molded product thereof that can be mass-produced at low cost.

[0007] The present inventors have focused on molded articles of polycarbonate, which has excellent transparency and mechanical strength, but have noticed that since polycarbonate has a high molding temperature, the transmittance may decrease and / or increase during molding of a polycarbonate resin composition at high temperatures, that is, the transmittance (optical properties) may change. The change in optical properties may cause malfunction. Therefore, an object of the present invention is to provide a polycarbonate resin composition and a molded article thereof, which have wavelength selective transmittance and do not substantially change in optical properties even when molded at high temperatures. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that a polycarbonate resin composition containing a colorant (e.g., an anthraquinone-based dye) having a maximum absorption wavelength of less than 1200 nm and a phosphoric acid or phosphoric acid ester-based compound does not cause substantial changes in optical properties even when molded at high temperatures and has wavelength selective transmittance, and a molded article thereof. Furthermore, it has been found that such a resin composition and molded article can be suitably used for Lidar applications, and the present invention has been completed.

[0009] The wavelength-selectively transparent polycarbonate resin molded article according to the present invention comprises an aromatic polycarbonate resin (A), a colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm, and Biri acid (C 2 ), The polymer component comprises an aromatic polycarbonate resin (A), The colorant (B) is contained in an amount of 0.001 to 2.0 parts by mass relative to 100 parts by mass of an aromatic polycarbonate resin (A). , Li Contains 0.0001 to 0.004 parts by mass of phosphoric acid (C2) or a polymer component comprising an aromatic polycarbonate resin (A), a colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm, and a phosphate ester compound or phosphoric acid (C), the polymer component being made of the aromatic polycarbonate resin (A), the colorant (B) containing an anthraquinone dye, and the phosphate ester compound or phosphoric acid (C) containing at least one selected from the group consisting of phosphate ester compounds or phosphoric acids represented by the following general formula (I): Formula (I): O=P(OH) n (OR) 3-n [In general formula (I), R is an alkyl group or an aryl group, and n is an integer of 2.] The composition contains 0.29 to 2.0 parts by mass of a colorant (B) relative to 100 parts by mass of an aromatic polycarbonate resin (A), and contains, with respect to the phosphate ester compound or phosphoric acid (C), 0.005 to 0.3 parts by mass of a phosphate ester compound (C1) or 0.0001 to 0.004 parts by mass of phosphoric acid (C2). .

[0010] The wavelength-selectively transmitting polycarbonate resin molded article according to the present invention contains the above-mentioned wavelength-selectively transmitting aromatic polycarbonate resin composition.

[0011] The method for producing a wavelength-selectively transmitting polycarbonate resin molded article according to the present invention comprises molding the above-mentioned resin composition. Effect of the Invention

[0012] The polycarbonate resin composition according to the embodiment of the present invention can be molded using a conventional device to produce a molded product, and the optical properties do not change substantially during the molding. Therefore, the polycarbonate resin composition according to the embodiment of the present invention can provide a molded product that has appropriate wavelength selectivity and does not substantially change in optical properties. The molded product can be suitably used for Lidar applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The wavelength-selective transparent polycarbonate resin composition according to an embodiment of the present invention comprises an aromatic polycarbonate resin (A), a colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm, and a phosphate ester compound or phosphoric acid (C), in which the colorant (B) is contained in an amount of 0.001 to 2.0 parts by mass relative to 100 parts by mass of the aromatic polycarbonate resin (A), and the phosphoric acid or phosphate ester compound (C) contains 0.005 to 0.3 parts by mass of a phosphate ester compound (C1) or 0.0001 to 0.004 parts by mass of phosphoric acid (C2).

[0014] In the embodiment of the present invention, the "aromatic polycarbonate resin (A)" is a polycarbonate resin based on an aromatic compound, and is not particularly limited as long as it can produce the aromatic polycarbonate resin composition of the present invention. Examples of such aromatic polycarbonate resins include polymers obtained by the phosgene method in which various dihydroxydiaryl compounds are reacted with phosgene, or the ester exchange method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate. A representative example includes a polycarbonate resin produced from 2,2-bis(4-hydroxyphenyl)propane (bisphenol A).

[0015] Examples of the dihydroxydiaryl compound include, in addition to bisphenol A, bis(hydroxyaryl)alkanes such as bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane; Examples of the cycloalkanes include bis(hydroxyaryl)cycloalkanes such as bis(4-hydroxyphenyl)cyclopentane and 1,1-bis(4-hydroxyphenyl)cyclohexane; dihydroxydiaryl ethers such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether; dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide; dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; and dihydroxydiaryl sulfones such as 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone. These can be used alone or in combination. In addition to these, piperazine, dipiperidyl hydroquinone, resorcin, 4,4'-dihydroxydiphenyl, etc. can be used in combination.

[0016] Furthermore, the dihydroxydiaryl compound may be used in combination with, for example, the following trivalent or higher aromatic compounds.

[0017] Examples of the trivalent or higher phenolic compounds include phloroglucin, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptene, 2,4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptane, 1,3,5-tri-(4-hydroxyphenyl)-benzene, 1,1,1-tri-(4-hydroxyphenyl)-ethane, and 2,2-bis-[4,4-(4,4'-dihydroxydiphenyl)-cyclohexyl]-propane.

[0018] The viscosity average molecular weight of the aromatic polycarbonate resin (A) is preferably 10,000 to 100,000, and more preferably 12,000 to 30,000. When producing such an aromatic polycarbonate resin (A), a molecular weight regulator, a catalyst, etc. can be used as necessary. As such an aromatic polycarbonate resin, a commercially available product can be used.

[0019] In the embodiment of the present invention, the colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm contains a dye having a maximum absorption wavelength of less than 1200 nm, and the dye can be selected from, for example, dyes (organic, inorganic), pigments (organic, inorganic), etc., and is not particularly limited as long as the aromatic polycarbonate resin composition of the present invention can be obtained. As such a dye, either a dye or a pigment can be used, but since dyes are usually less likely to diffusely reflect light on the surface of particles, it is more preferable to use a dye. These colorants (B) containing dyes can be used alone or in combination of two or more.

[0020] Examples of the dye-based dye include anthraquinone-based dyes, perinone-based dyes, perylene-based dyes, methine-based dyes, azo-based dyes, quinoline-based dyes, phthalocyanine-based dyes, and heterocyclic dyes. Oil-soluble dyes are preferred because they can be more easily and uniformly dispersed in the resin composition. Dyes are made of smaller particles than pigments, so they can be more uniformly mixed in the resin composition, making them preferable because they can reduce the cloudiness (haze value) of the molded body. Dyes are more preferred for Lidar.

[0021] Examples of the pigment-based coloring matter include organic coloring matter such as azo coloring matter (soluble azo coloring matter, insoluble azo coloring matter), condensation coloring matter, threne-based pigments, quinacridone coloring matter, dioxazine coloring matter, and isoindoline coloring matter; and inorganic coloring matter such as titanium oxide, iron oxide, chromium oxide, carbon black, ultramarine blue, barium sulfate, calcium carbonate, zinc oxide, lead sulfate, titanium black, and synthetic iron black.

[0022] The colorant (B) preferably contains a colorant (B1) containing a dye having a maximum absorption wavelength of less than 700 nm, and / or a colorant (B2) containing a dye having a maximum absorption wavelength of 700 nm or more and less than 1000 nm.

[0023] In an embodiment of the present invention, the colorant (B1) containing a dye having a maximum absorption wavelength of less than 700 nm preferably contains at least one selected from an anthraquinone dye, a perinone dye, a perylene dye, and a methine dye. The colorant (B1) preferably contains an anthraquinone dye.

[0024] The colorant (B1) may further contain at least one selected from the group consisting of phthalocyanine dyes and heterocyclic dyes.

[0025] In the resin composition of the embodiment of the present invention, in addition to the anthraquinone-based dye, a combination of multiple other dyes can be used as the colorant (B1). For example, a combination of a pigment and a pigment, a combination of a pigment and a dye, or a combination of a dye and a dye may be used, but it is preferable to use a combination of a dye and a dye. It is preferable to use a combination of an anthraquinone-based dye and another dye, because it can suppress or block light of various wavelengths and have good light transmittance in various wavelength regions.

[0026] The above-mentioned dye is not particularly limited as long as the composition according to the embodiment of the present invention can be obtained, but specifically, the following dyes can be used.

[0027] The anthraquinone dye preferably includes at least one selected from the group consisting of Solvent Yellow 163, Disperse Violet 28, Solvent Blue 97, Solvent Green 28, Solvent Green 3, and Disperse Blue 60.

[0028] Examples of perinone dyes include dyes commercially available with color indexes such as Solvent Orange 60, Solvent Orange 78, Solvent Orange 90, Solvent Violet 29, Solvent Red 135, Solvent Red 162, and Solvent Red 179.

[0029] Examples of perylene-based dyes include dyes commercially available with color indexes such as Solvent Green 3, Solvent Green 5, Solvent Orange 55, Vat Red 15, Vat Orange 7, F Orange 240, F Red 305, F Red 339, F Yellow 83, and Solvent Red 179.

[0030] Examples of methine dyes include dyes commercially available under the color indexes Solvent Orange 80, Solvent Yellow 93, Disperse Yellow 201, etc. Quinoline dyes include those commercially available with color indexes such as Solvent Yellow 33, Solvent Yellow 98, Solvent Yellow 157, Disperse Yellow 54, and Disperse Yellow 201.

[0031] In an embodiment of the present invention, the colorant (B2) containing a dye having a maximum absorption wavelength in the range of 700 nm or more and less than 1000 nm preferably contains at least one dye selected from the group consisting of phthalocyanine dyes, anthraquinone dyes, and heterocyclic dyes.

[0032] The colorant (B2) preferably contains a phthalocyanine dye, and examples of such phthalocyanine dyes include FDN-002, FDN-023, FDN-024, and the like, which are commercially available from Yamada Chemical Industry Co., Ltd.

[0033] The colorant (B2) preferably contains a heterocyclic dye, and examples of such heterocyclic dye include SDO-C8 available from Arimoto Chemical Industry Co., Ltd.

[0034] The colorant (B2) preferably contains an anthraquinone-based colorant, and examples of such an anthraquinone-based colorant include SDO-C33 commercially available from Arimoto Chemical Industry Co., Ltd.

[0035] The resin composition according to the embodiment of the present invention preferably contains 0.001 to 2.0 parts by mass, more preferably 0.005 to 1.5 parts by mass, and even more preferably 0.006 to 1.0 parts by mass of a colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm, relative to 100 parts by mass of an aromatic polycarbonate resin (A). The lower limit of the content of the colorant (B) may be 0.02 parts by mass or 0.025 parts by mass.

[0036] In an embodiment of the present invention, the phosphate ester compound or phosphoric acid (C) is not particularly limited as long as the resin composition of the embodiment of the present invention can be obtained, but it is preferable that the phosphate ester compound or phosphoric acid (C) contains at least one selected from the group consisting of phosphate ester compounds represented by the following general formula (I) and phosphoric acid.

[0037] Formula (I): O=P(OH) n (OR) 3-n [In formula (I), R is an alkyl group or an aryl group, each of which may be the same or different, and n is an integer of 0 to 3.]

[0038] In the above general formula (I), R is preferably an alkyl group having 1 to 30 carbon atoms or an aryl group having 6 to 30 carbon atoms, and more preferably an alkyl group having 2 to 25 carbon atoms. In addition, n is preferably 1 or 2.

[0039] Examples of the phosphate ester compound of formula (I) include mono- or di-stearyl acid phosphate, and a mixed stearyl phosphate ester (a mixture of about 50 mol % monostearyl phosphate and about 50 mol % distearyl phosphate (product name "AX-71" manufactured by Asahi Denka Co., Ltd.) is known.

[0040] Phosphoric acid is a non-volatile weak acid, and commercially available products can be used. Examples of the phosphoric acid include, but are not limited to, phosphoric acid manufactured by Nacalai Tesque and phosphoric acid manufactured by Wako Pure Chemical Industries.

[0041] The resin composition according to the embodiment of the present invention preferably contains 0.005 to 0.3 parts by mass of the phosphate ester compound (C1), more preferably 0.007 to 0.1 parts by mass, and even more preferably 0.009 to 0.08 parts by mass of the phosphoric acid (C), relative to 100 parts by mass of the aromatic polycarbonate resin (A). Alternatively, the resin composition preferably contains 0.0001 to 0.004 parts by mass of the phosphoric acid (C2), more preferably 0.0001 to 0.001 parts by mass, more preferably 0.0003 to 0.0008 parts by mass, and even more preferably 0.0004 to 0.0006 parts by mass of the phosphoric acid (C2).

[0042] The aromatic polycarbonate resin composition of the embodiment of the present invention may further contain a phosphorus-based antioxidant (D).

[0043] The phosphorus-based antioxidant is not particularly limited as long as it can provide the aromatic polycarbonate resin composition of the present invention, but it is preferable for the antioxidant to contain a phosphite compound having the following phosphite structure. [ka]

[0044] In the wavelength selectively transmitting polycarbonate resin composition according to an embodiment of the present invention, the phosphorus-based antioxidant (D) preferably contains at least one compound selected from a phosphite compound represented by the following formula (1), a phosphite compound represented by the following formula (2), a phosphite compound represented by the following formula (3), and a phosphite compound represented by the following formula (4):

[0045] The phosphorus-based antioxidant (D) preferably contains, for example, a compound represented by the following formula (1).

[0046] Formula (1): [ka] (In the formula, R 1represents an alkyl group having 1 to 20 carbon atoms, and a represents an integer of 0 to 3.

[0047] In the formula (1), R 1 is an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms.

[0048] Examples of the compound represented by formula (1) include triphenyl phosphite, tricresyl phosphite, tris(2,4-di-t-butylphenyl) phosphite, trisnonylphenyl phosphite, etc. Among these, tris(2,4-di-t-butylphenyl) phosphite is particularly suitable, and is commercially available as, for example, Irgafos 168 manufactured by BASF ("Irgafos" is a registered trademark of BASF Societas Europea).

[0049] The phosphorus-based antioxidant (D) preferably contains, for example, a compound represented by the following formula (2).

[0050] Formula (2): [ka] (In the formula, R 2 , R 3 , R 5 and R 6 R each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; X represents a single bond, a sulfur atom, or a group represented by the formula: -CHR 7 - (where R 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. A represents an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: *-COR 8 - (where R 8represents a single bond or an alkylene group having 1 to 8 carbon atoms, and * represents a bond on the oxygen side. Either Y or Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.

[0051] In formula (2), R 2 , R 3 , R 5 and R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group.

[0052] Here, examples of the alkyl group having 1 to 8 carbon atoms include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, t-butyl, t-pentyl, i-octyl, t-octyl, and 2-ethylhexyl groups. Examples of the cycloalkyl group having 5 to 8 carbon atoms include cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl groups. Examples of the alkylcycloalkyl group having 6 to 12 carbon atoms include 1-methylcyclopentyl, 1-methylcyclohexyl, and 1-methyl-4-i-propylcyclohexyl groups. Examples of the aralkyl group having 7 to 12 carbon atoms include benzyl, α-methylbenzyl, and α,α-dimethylbenzyl groups.

[0053] R 2 , R 3 and R 5 are each preferably independently an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms. 2 and R 5 are each preferably independently a t-alkyl group such as a t-butyl group, a t-pentyl group, or a t-octyl group, a cyclohexyl group, or a 1-methylcyclohexyl group. 3is preferably an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group, and more preferably a methyl group, a t-butyl group, or a t-pentyl group.

[0054] R 6 is preferably a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms, and more preferably a hydrogen atom, or an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group.

[0055] In formula (2), R 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms include the above-mentioned R 2 , R 3 , R 5 and R 6 In particular, R 4 is preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and more preferably a hydrogen atom or a methyl group.

[0056] In formula (2), X is a single bond, a sulfur atom or a group represented by the formula: -CHR 7 -, where the formula is -CHR 7 -R in 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms and the cycloalkyl group having 5 to 8 carbon atoms include the above-mentioned R 2 , R 3 , R 5 and R 6 In particular, X is preferably a single bond, a methylene group, or a methylene group substituted with a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a t-butyl group, or the like, and more preferably a single bond.

[0057] In formula (2), A is an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: 8 Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a 2,2-dimethyl-1,3-propylene group, and the like, with a propylene group being preferred. 8 -R in 8 R represents a single bond or an alkylene group having 1 to 8 carbon atoms. 8 Examples of the alkylene group having 1 to 8 carbon atoms represented by the formula (I) include the alkylene groups exemplified in the description of A above. 8 is preferably a single bond or an ethylene group. 8 The * in - is a bond on the oxygen side, indicating that the carbonyl group is bonded to the oxygen atom of the phosphite group.

[0058] In formula (2), one of Y and Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkoxy group having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a t-butoxy group, and a pentyloxy group. Examples of the aralkyloxy group having 7 to 12 carbon atoms include a benzyloxy group, an α-methylbenzyloxy group, and an α,α-dimethylbenzyloxy group. Examples of the alkyl group having 1 to 8 carbon atoms include the above-mentioned R 2 , R 3 , R 5 and R 6 Examples of the alkyl group include those exemplified in the explanation of the above.

[0059] Examples of the compound represented by formula (2) include 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine, 6 -[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, and the like. Among these, when the resulting aromatic polycarbonate resin composition is to be used in fields where optical properties are particularly required, 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine is suitable, and is commercially available, for example, as Sumilizer GP manufactured by Sumitomo Chemical Co., Ltd. ("Sumilizer" is a registered trademark).

[0060] The phosphorus-based antioxidant (D) preferably contains, for example, a compound represented by the following formula (3).

[0061] Formula (3): [ka] (In the formula, R 9 and R 10 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group which may be substituted with an alkyl group, and b and c each independently represent an integer of 0 to 3.

[0062] Examples of the compound represented by formula (3) include bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, etc. Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite is commercially available under the trade name "ADK STAB PEP-24G" manufactured by ADEKA CORPORATION. ADK STAB PEP-36 ("ADK STAB" is a registered trademark) manufactured by ADEKA CORPORATION is commercially available.

[0063] The phosphorus-based antioxidant (D) preferably contains, for example, a compound represented by the following formula (4).

[0064] Formula (4): [ka]

[0065] (In the formula, R 11 ~R 18 R each independently represents an alkyl group or an alkenyl group having 1 to 3 carbon atoms. 11 and R 12 , R 13 and R 14 , R 15 and R 16 , R 17 and R 18 may be bonded to each other to form a ring. 19 ~R 22 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. d to g each independently represents an integer of 0 to 5. X 1 ~X 4 Each of X independently represents a single bond or a carbon atom. 1 ~X 4 is a single bond, R 11 ~R 22 The functional group connected to the single bond is excluded from formula (4).

[0066] A specific example of the compound represented by formula (4) is bis(2,4-dicumylphenyl)pentaerythritol diphosphite, which is commercially available under the trade name "Doverphos (registered trademark) S-9228" manufactured by Dover Chemical Co., and under the trade name "ADEKA STAB PEP-45" manufactured by ADEKA Corporation (bis(2,4-dicumylphenyl)pentaerythritol diphosphite).

[0067] Further examples of the phosphorus-based antioxidant (D) include [1,1'-biphenyl]-4,4'-diylbis[bis(2,4-di-t-butylphenoxy)phosphine], and the like. For example, commercially available products include Irgafos P-EPQ (trade name) manufactured by BASF and HOSTANOX P-EPQ (trade name) manufactured by Clariant Chemicals.

[0068] The above-mentioned aromatic polycarbonate resin composition is preferably one that satisfies at least one selected from the following: The phosphite compound represented by the formula (1) contains tris(2,4-di-t-butylphenyl)phosphite; The phosphite compound represented by the formula (2) contains 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine; The phosphite compound represented by the formula (3) contains 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane; and The phosphite compound represented by the formula (4) contains bis(2,4-dicumylphenyl)pentaerythritol diphosphite.

[0069] The amount of the phosphorus-based antioxidant (D) is preferably up to 0.5 parts by mass, and more preferably from 0.02 to 0.2 parts by mass, based on 100 parts by mass of the aromatic polycarbonate resin (A).

[0070] The wavelength-selective polycarbonate resin composition according to the embodiment of the present invention may further contain a dye (E) containing a phthalocyanine compound having a maximum absorption wavelength in the range of 1000 nm to 1200 nm. When the wavelength-selective polycarbonate resin composition contains the dye (E), it absorbs light having a wavelength of 1000 to 1200 nm, and therefore the transmission wavelength range can be shifted to the long wavelength side.

[0071] The dye (E) preferably contains a compound represented by the following general formula (II). Formula (II): [ka] [In the formula, R 31 may be the same or different and represent a hydrogen atom or an alkyl group which may have a substituent. R 32 and R 33 may be the same or different, and each represents a halogen atom, OR 34 Base, SR 35 group or NR 36 or R 37 The group is shown. X 11 may be the same or different and represent an oxygen atom or a sulfur atom. R 34 and R 35 The groups may be the same or different and each represents an alkyl group which may have a substituent, an aryl group which may have a substituent, or a heteroaryl group which may have a substituent. R 36 and R 37 The groups may be the same or different and represent a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group. R 36 and R 37 may be bonded together with the nitrogen atom to which they are bonded, via or without another nitrogen atom, an oxygen atom, or a sulfur atom, to form a 5- to 10-membered saturated or unsaturated heterocycle. The 5- to 10-membered saturated or unsaturated heterocycle may have one or more substituents. M represents two monovalent metal atoms, a divalent metal atom, or a trivalent or tetravalent metal compound.

[0072] The phthalocyanine compound represented by the above general formula (II) is preferably a compound represented by the following general formula (III). Formula (III): [ka] [In the formula, R 31 may be the same or different and represent a hydrogen atom or an alkyl group which may have a substituent. X 11 , X 12 and X 13 may be the same or different and represent an oxygen atom or a sulfur atom. R 34 and R 35 The groups may be the same or different and each represents an alkyl group which may have a substituent, an aryl group which may have a substituent, or a heteroaryl group which may have a substituent. M represents two monovalent metal atoms, a divalent metal atom, or a trivalent or tetravalent metal compound.

[0073] Examples of the "halogen atom" include fluorine, chlorine, bromine and iodine.

[0074] Examples of the "alkyl group" include linear alkyl groups having 1 to 12 carbon atoms, branched alkyl groups having 3 to 12 carbon atoms, and cyclic alkyl groups having 3 to 12 carbon atoms. Specific examples include methyl groups, ethyl groups, n-propyl groups, isopropyl groups, n-butyl groups, isobutyl groups, s-butyl groups, t-butyl groups (hereinafter also referred to as t-Bu), n-pentyl groups, 2-methylbutyl groups, and the like. group, 1-methylbutyl group, neo-pentyl group, 1,2-dimethylpropyl group, 1,1-dimethylpropyl group, cyclopentyl group, n-hexyl group, 4-methylpentyl group, 3-methylpentyl group, 2-methylpentyl group, 1-methylpentyl group, 3,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1,3-dimethylbutyl group, 2,2-dimethylbutyl group, 1,2-dimethylbutyl group, 1,1-dimethylbutyl group, 2-ethylbutyl group, 1-ethylbutyl group, 1,1,2-trimethylpropyl group, 1-ethyl-2-methylpropyl group, cyclohexyl group, n-heptyl group, 2-methyl Examples of the alkyl group include an ethylhexyl group, a 3-methylhexyl group, a 4-methylhexyl group, a 5-methylhexyl group, a 2,4-dimethylpentyl group, an n-octyl group, a 2-ethylhexyl group, a 2,5-dimethylhexyl group, a 2,4,4-trimethylpentyl group, a 2,4-dimethylhexyl group, a 2,2,4-trimethylpentyl group, a t-octyl group, an n-nonyl group, a 3,5,5-trimethylhexyl group, an n-decyl group, a 4-ethyloctyl group, a 4-ethyl-4,5-dimethylhexyl group, an n-undecyl group, an n-dodecyl group, a 1,3,5,7-tetramethyloctyl group, and a 4-butyloctyl group. Preferred are linear alkyl groups having 1 to 8 carbon atoms, branched alkyl groups having 3 to 8 carbon atoms, or cyclic alkyl groups having 3 to 8 carbon atoms, and particularly preferred are a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an n-hexyl group, an n-octyl group, a 2-ethylhexyl group, and a t-octyl group.

[0075] Examples of the "aryl group" include monocyclic and polycyclic (e.g., bicyclic or tricyclic) aryl groups. Specific examples include phenyl, naphthyl, and anthryl groups. Monocyclic or bicyclic aryl groups are preferred, with phenyl and naphthyl groups being particularly preferred.

[0076] Examples of the "heteroaryl group" include monocyclic and polycyclic (e.g., bicyclic or tricyclic) heteroaryl groups. Specific examples include pyridyl, pyrimidine, indolyl, quinoline, benzimidazole, furanyl, thienyl, benzofuran, and 1,3,4-thiadiazole groups. Monocyclic or bicyclic heteroaryl groups are particularly preferred.

[0077] The substituents on the alkyl chain, aryl ring or heteroaryl ring of the above-mentioned alkyl group which may have a substituent, aryl group which may have a substituent, and heteroaryl group which may have a substituent (groups which may be substituted on the alkyl chain, aryl ring or heteroaryl ring) include, for example, an alkyl group, a haloalkyl group, a hydroxyalkyl group, an alkoxy group, an alkylthio group, an alkylamino group, a dialkylamino group, a cyclic amino group, a halogen atom, an acyl group, an alkoxycarbonyl group, a ureido group, a sulfamoyl group, a carbamoyl group, an alkylcarbamoyl group, an alkylsulfonyl group, an arylsulfonyl group, an alkoxysulfonyl group, an aryloxysulfonyl group, a cyano group, a nitro group, etc. The number of the substituents (groups which may be substituted on the alkyl chain, aryl ring or heteroaryl ring, hereinafter referred to as substituents) on the alkyl chain, aryl ring or heteroaryl ring may be 1 to 5.

[0078] For example, when the alkyl group which may have a substituent is an "alkyl group having a substituent", specific examples of the alkyl group having a substituent include a 2-chloroethyl group, a 2,2,2-trifluoroethyl group, a 2,2,3,3,3-pentafluoropropyl group, a benzyl group, a phenethyl group, a 2-phenylethyl group, a 3-phenylethyl group, a 4-hydroxybutyl group, a 2-methoxyethyl group, a 3-methoxypropyl group, a 2-isopropoxyethyl group, and an ethyl butanoate group.

[0079] When the aryl group which may have a substituent is an "aryl group having a substituent", specific examples of the aryl group having a substituent include a 2-chlorophenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 2,3-dichlorophenyl group, a 2,4-dichlorophenyl group, a 2,5-dichlorophenyl group, a 2,6-dichlorophenyl group, a 2,4,6-trichlorophenyl group, a 2-fluorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 2,3-difluorophenyl group, a 2,4-difluorophenyl group, a 2,5-difluorophenyl group, a 2,6-difluorophenyl group, a 2,4,6-trifluorophenyl group, Examples of the alkyl group include a phenyl group, a pentafluorophenyl group, an N,N-dimethylaminophenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2,6-dimethylphenyl group, a 2,4,6-trimethylphenyl group, a 4-ethylphenyl group, a 4-t-butylphenyl group, a 4-biphenyl group, a 4-hydroxyphenyl group, a 2-methoxyphenyl group, a 4-methylthiophenyl group, a 4-(trifluoromethyl)phenyl group, a 4-phenoxyphenyl group, a 4-acetylphenyl group, and a 4-methoxycarbonylphenyl group.

[0080] When the above-mentioned heteroaryl group which may have a substituent is a "heteroaryl group having a substituent", specific examples of the heteroaryl group having a substituent include a 2-methylpyridyl group, a 2-chloropyridyl group, a 6-fluorobenzothiazole group, a 6-chlorobenzothiazole group, a 6-methylbenzothiazole group, a 6-methoxybenzothiazole group, a 5-methyl-1,3,4-thiadiazole group, a 5-methylthio-1,3,4-thiadiazole group, and a 5-trifluoromethyl-1,3,4-thiadiazole group.

[0081] Examples of the divalent metal represented by M include metal atoms belonging to groups 3 to 15 of the periodic table, specifically Cu, Zn, Fe, Co, Ni, Ru, Pb, Rh, Pd, Pt, Mn, Sn, Pb, etc.

[0082] Examples of trivalent or tetravalent metal compounds represented by M include halides, hydroxides, and oxides of metals belonging to groups 3 to 15 of the periodic table. Specific examples include AlCl, AlOH, InCl, FeCl, MnOH, SiCl2, SnCl2, GeCl2, Si(OH)2, Si(OCH3)2, Si(OPh)2, Si(OSiCH3)2, Sn(OH)2, Ge(OH)2, VO, and TiO. In addition, Ph represents a phenyl group.

[0083] The phthalocyanine compound is preferably a phthalocyanine dye having a central metal selected from oxovanadium, copper, aluminum, cobalt and zinc.

[0084] The dye (E) preferably contains at least one of the phthalocyanine compounds represented by the following formulas. [ka]

[0085] The dye (E) containing a phthalocyanine compound having a maximum absorption wavelength of 1000 nm or more and 1200 nm or less is contained in an amount of preferably 0.001 to 0.2 parts by mass, more preferably 0.002 to 0.18 parts by mass, even more preferably 0.004 to 0.16 parts by mass, particularly preferably 0.005 to 0.15 parts by mass, and even more particularly preferably 0.01 to 0.1 parts by mass, relative to 100 parts by mass of the aromatic polycarbonate resin (A).

[0086] When the dye (E) containing a phthalocyanine compound having a maximum absorption wavelength of 1000 nm or more and 1200 nm or less is contained in an amount of 0.001 to 0.2 parts by mass per 100 parts by mass of the aromatic polycarbonate resin (A), the wavelength selectively transmitting polycarbonate resin composition and its molded article are more excellent because they can cut light of longer wavelengths.

[0087] The dye (E) containing a phthalocyanine compound having a maximum absorption wavelength in the range of 1000 nm to 1200 nm can be a commercially available product. For example, FDN-010 (product name) manufactured by Yamada Chemical Industry Co., Ltd. can be exemplified, and this can be used.

[0088] In addition to the above components, for example, an ultraviolet absorber, which is a component that further improves the weather resistance of the resulting aromatic polycarbonate resin composition, can be appropriately used in the aromatic polycarbonate resin composition according to the embodiment depending on the application of the molded article obtained by molding the aromatic polycarbonate resin composition.

[0089] As the ultraviolet absorbent, for example, ultraviolet absorbents that are usually blended with polycarbonate resins, such as benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, and anilide oxalate-based compounds, can be used alone or in combination of two or more kinds.

[0090] Examples of benzotriazole compounds include 2-(2-hydroxy-5-t-octylphenyl)benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-pentyl-2-hydroxyphenyl)-2H-benzotriazole, and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)benzotriazole. phenol, 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole, 2-[2'-hydroxy-3,5-di(1,1-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-Methylenbis[6-(2H-benzotriazol-2-yl)4-(1,1,3,3-tetramethylbutyl)phenol], etc. Among them, 2-(2-hydroxy-5-t-octylphenyl)benzotriazole, etc. are particularly suitable, and for example, TINUVIN 329 (TINUVIN is a registered trademark) manufactured by BASF, Seesorb 709 manufactured by Shipro Kasei Co., Ltd., Chemisorb 79 manufactured by Chemipro Kasei Co., Ltd., etc. are commercially available.

[0091] Examples of triazine compounds include 2,4-diphenyl-6-(2-hydroxyphenyl-4-hexyloxyphenyl)-1,3,5-triazine, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]phenol. For example, TINUVIN 1577 manufactured by BASF is commercially available.

[0092] As the oxalic acid anilide compound, for example, Sanduvor VSU manufactured by Clariant Japan K.K. and the like are commercially available.

[0093] Examples of benzophenone compounds include 2,4-dihydroxybenzophenone and 2-hydroxy-4-n-octoxybenzophenone.

[0094] The amount of the ultraviolet absorber is 0 to 1.0 part by mass, preferably 0 to 0.5 part by mass, relative to 100 parts by mass of the aromatic polycarbonate resin (A). If the amount of the ultraviolet absorber exceeds 1.0 part by mass, the initial hue of the resulting aromatic polycarbonate resin composition may be deteriorated. In addition, if the amount of the ultraviolet absorber is 0.1 part by mass or more, the effect of further improving the weather resistance of the aromatic polycarbonate resin composition is particularly great.

[0095] Furthermore, the aromatic polycarbonate resin composition according to the embodiment may appropriately contain various additives such as a heat stabilizer, other antioxidants, a release agent (e.g., Rikemal S-100A manufactured by Riken Vitamin Co., Ltd.), a softener, an antistatic agent, and an impact modifier, and a polymer other than the aromatic polycarbonate resin (A), within the scope that does not impair the effects of the present invention.

[0096] The aromatic polycarbonate resin composition of the embodiment of the present invention can be produced by mixing an aromatic polycarbonate resin (A), a colorant (B), and a phosphoric acid ester compound or phosphoric acid (C), and, if necessary, mixing a phosphorus-based antioxidant (D), a dye (E), the various additives, and a polymer other than the aromatic polycarbonate resin (A). As long as the aromatic polycarbonate resin composition of the present invention can be obtained, the production method is not particularly limited, and the type and amount of each component can be appropriately adjusted. The method of mixing the components is also not particularly limited, and examples thereof include a method of mixing using a known mixer such as a tumbler or a ribbon blender, and a method of melt kneading using an extruder. By these methods, pellets of the aromatic polycarbonate resin composition can be easily obtained.

[0097] The shape and size of the pellets of the aromatic polycarbonate resin composition obtained as described above are not particularly limited, and may be any shape and size that a typical resin pellet has. For example, the shape of the pellets may be an elliptical cylinder, a cylindrical shape, etc. The pellet size is preferably about 2 to 8 mm in length, and in the case of an elliptical cylinder, the major axis of the cross-sectional ellipse is preferably about 2 to 8 mm, and the minor axis is preferably about 1 to 4 mm, and in the case of a cylindrical shape, the diameter of the cross-sectional circle is preferably about 1 to 6 mm. Each of the obtained pellets may be of such a size, or all the pellets forming the pellet aggregate may be of such a size, or the average value of the pellet aggregate may be of such a size, and there is no particular limitation.

[0098] The thermal stability of the resin composition according to the embodiment of the present invention is preferably such that Δ after a molded article is left in the mold for 10 minutes is 200 nm or less, more preferably such that Δ after a molded article is left in the mold for 30 minutes is 200 nm or less, and even more preferably such that Δ after a molded article is left in the mold for 60 minutes is 200 nm or less. The thermal stability of the resin composition can be measured by the method described in the Examples.

[0099] The reliability of the resin composition according to the embodiment of the present invention is preferably such that the molecular weight of a molded article is 16,000 or more after standing for 240 hours under conditions of 85° C. and 95% RH, and more preferably such that the molecular weight of a molded article is 16,000 or more after standing for 240 hours under conditions of 120° C. The reliability of the resin composition can be measured by the method described in the Examples.

[0100] The molded article according to the embodiment of the present invention can be obtained by molding the aromatic polycarbonate resin composition described above, and can be suitably used for sensors, filters, and the like.

[0101] As long as the molded article intended by the present invention can be obtained, the method for producing the molded article is not particularly limited. For example, a method for molding an aromatic polycarbonate resin composition by a known injection molding method, compression molding method, or the like can be mentioned.

[0102] The molded article according to the embodiment of the present invention is suitable as, for example, a Lidar sensor cover.

[0103] As described above, the embodiments of the present invention have been described as examples of the present invention. However, the technology of the present invention is not limited to the above, and can be applied to embodiments in which appropriate changes, substitutions, additions, omissions, etc. are made. EXAMPLES

[0104] The present invention will be specifically and in detail explained below with reference to examples and comparative examples. However, these examples are merely one embodiment of the present invention, and the present invention is not limited to these examples in any way.

[0105] The components used in this example are shown below. (A) Aromatic polycarbonate resin (a1) Polycarbonate resin synthesized from bisphenol A and carbonyl chloride Viscosity average molecular weight: 18,800, SD Polyca 200-20 (product name) manufactured by Sumika Polycarbonate Co., Ltd., "SD Polyca" is a registered trademark of Sumika Polycarbonate Co., Ltd.

[0106] (B) Dye with maximum absorption wavelength less than 1200 nm (b1) Anthraquinone dye (Solvent Blue 97) Bayer AG Macrolex Blue RR (product name), maximum absorption wavelength: 630 nm [ka]

[0107] (b2) Anthraquinone dye (Solvent Green 28) Bayer AG Macrolex Green G (product name), maximum absorption wavelength: 690 nm [ka]

[0108] (b3) Anthraquinone dyes (SD-3, mixtures) Manufactured by Kenei Kogyo Co., Ltd., maximum absorption wavelength: 630 nm (b4) Anthraquinone dye (Solvent Green 3) Mitsui PS Green B (product name) manufactured by Mitsui Fine Chemicals Co., Ltd., maximum absorption wavelength: 640 nm [ka]

[0109] (b5) Methine dye (Disperse Yellow 201) Bayer AG Macrolex Yellow 6G (product name), maximum absorption wavelength: 440 nm [ka]

[0110] (b6) Perylene dye (Solvent Red 179) Bayer AG Macrolex Red E2G (product name), maximum absorption wavelength: 480 nm [ka]

[0111] (b7) Phthalocyanine dye (FDN-001 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 754 nm (b8) Phthalocyanine dye (FDN-002 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 807 nm (b9) Phthalocyanine dye (FDN-023 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 790 nm

[0112] (b10) Phthalocyanine dye (FDN-024 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 830 nm

[0113] (b11) Anthraquinone dye (SDO-C33 product name) Arimoto Chemical Industry Co., Ltd., Maximum absorption wavelength: 846 nm (b12) Heterocyclic dye (SDO-C8 product name) Manufactured by Arimoto Chemical Industry Co., Ltd., maximum absorption wavelength: 785 nm

[0114] (b13) Phthalocyanine dye (FDN-004 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 880 nm (b14) Phthalocyanine dye (FDN-006 product name) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 927 nm

[0115] (C) Phosphoric acid or phosphate ester compounds (c1) Phosphate ester compounds Mixed stearyl phosphate ester (a mixture of approximately 50 mol% monostearyl phosphate and approximately 50 mol% distearyl phosphate; ADEKA STAB "AX-71 (trade name)" manufactured by ADEKA Corporation) [ka] (c2) Phosphate Nacalai Tesque phosphoric acid (H3PO4)

[0116] (D) Phosphorus-based antioxidants (d1) Phosphorus-based antioxidants HOSTANOX P-EPQ (product name) manufactured by Clariant Chemicals [1,1'-biphenyl]-4,4'-diylbis[bis(2,4-di-t- Butylphenoxy)phosphine Additives

[0117] (E) A dye having a maximum absorption wavelength of 1000 nm or more and 1200 nm or less (e1) Phthalocyanine dye (product name: FDN-010) Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 1014 nm

[0118] (X) Release agent (x1) Riken Vitamin Co., Ltd. Rikemal S-100A (product name)

[0119] These components were mixed in the mass ratios shown in Tables 1 to 3 to produce polycarbonate compositions of Examples 1 to 18 and Comparative Examples 1 to 4.

[0120] Each of the polycarbonate compositions of Examples 1 to 18 and Comparative Examples 1 to 4 was evaluated by the following evaluation methods. (1) Thermal stability To evaluate the thermal stability, the polycarbonate resin composition was molded using a Japan Steel Works J100 E2P at a cylinder temperature of 320°C and a mold temperature of 100°C, and then allowed to remain in the cylinder (320°C) for 10, 30, and 60 minutes to obtain molded products (1 mm). The optical spectrum of the molded product was evaluated using a Hitachi High-Tech Science UH4150 transmission spectrum, and the change in optical properties was quantified as follows:

[0121] The transmittance was measured every 2 nm from 1200 nm to 500 nm, and the difference between the wavelength where the transmittance started to decrease (hereinafter referred to as the decrease start wavelength) and the wavelength where the transmittance had completely decreased (hereinafter referred to as the decrease complete wavelength) was measured. A product was deemed to be good when the decrease start wavelength - decrease complete wavelength (Δ) was 200 nm or less. A product was deemed to be defective when it was 200 nm or more. It is preferable that the optical spectrum of a specific wavelength selection filter is steep, and a large difference in wavelength, i.e., when the above Δ is 200 nm or more (when it is not steep), is not preferable because it may cause problems as a filter.

[0122] (2) Reliability Each of the polycarbonate resin compositions of Examples 1 to 18 and Comparative Examples 1 to 4 was evaluated by the following evaluation methods.

[0123] The polycarbonate resin composition was molded using a Japan Steel Works J100 E2P at a cylinder temperature of 320°C and a mold temperature of 100°C, and the molded product was left to stand for 240 hours under conditions of 85°C 95% RH and 120°C for heat aging evaluation to obtain a sample (for evaluation). The weight average molecular weight of the molded product was measured. A weight average molecular weight of 16,000 or more was considered to be a good product, and a weight average molecular weight of less than 16,000 was considered to be a bad product. The weight average molecular weight was measured using an Alliance HPLC system manufactured by Japan Waters as a GPC device. A PLgel 5μm MiniMIX-C manufactured by Agilent Technologies was used as a GPC column. A solution was prepared by dissolving the sample in dichloromethane as a solvent. The solution was passed through the column at 40°C and a flow rate of 0.3mL / min using THF as an eluent, and a measurement value was obtained. A calibration curve for gel permeation chromatography (GPC) was prepared using a sample (monodisperse polystyrene) with a known weight-average molecular weight, and the measured values ​​were calibrated to obtain the target weight-average molecular weight.

[0124] [Table 1]

[0125] [Table 2]

[0126] [Table 3]

[0127] [Table 4]

[0128] The polycarbonate resin compositions of Examples 1 to 18 contain an aromatic polycarbonate resin (A), a colorant (B) containing a dye having a maximum absorption wavelength of less than 1,200 nm, and a phosphate ester compound or phosphoric acid (C), and contain 0.001 to 2.0 parts by mass of the colorant (B) relative to 100 parts by mass of the aromatic polycarbonate resin (A), and the phosphoric acid or phosphate ester compound (C) contains 0.005 to 0.3 part by mass of a phosphate ester compound (C1) or 0.0001 to 0.04 part by mass of phosphoric acid (C2).

[0129] The polycarbonate resin compositions of Examples 1 to 18 are excellent in thermal stability and reliability, and are suitable as wavelength-selective transmissive polycarbonate resin compositions for filters.

[0130] The molded products of Comparative Examples 1 and 2 have a large wavelength range from the transmittance decrease start wavelength to the decrease completion wavelength, so they cannot properly transmit the 850-950 nm near infrared rays used in Lidar. Therefore, the detection ability of Lidar may be reduced. In contrast, in the case of Examples 1 to 18 using the phosphoric acid ester compound of the present invention or phosphoric acid, the transmittance decrease start wavelength and wavelength range do not change significantly even after a residence time of 60 minutes, and it is possible to properly transmit the 850 nm-950 nm near infrared rays, and it is clear that they are excellent as wavelength selection filters.

[0131] When an excessive amount of phosphate ester or phosphoric acid is blended as in Comparative Examples 3 and 4, the molecular weight is significantly reduced after the reliability test, and the impact resistance required for the polycarbonate resin is impaired. When used as a lidar cover, there is a risk of problems such as the cover being damaged when it collides with pebbles on the road. In contrast, when an appropriate amount of phosphate ester and phosphoric acid is added, no significant molecular weight reduction is observed, and it is clear that the properties of the polycarbonate resin can be maintained. [Industrial Applicability]

[0132] The polycarbonate resin composition according to the embodiment of the present invention can be molded using a conventional device to produce a molded product, and the optical properties do not change substantially during the molding process. Therefore, the polycarbonate resin composition according to the embodiment of the present invention can provide a molded product that has appropriate wavelength selectivity and does not substantially change in optical properties. The molded product can be suitably used for Lidar applications.

Claims

1. The present invention comprises an aromatic polycarbonate resin (A), a colorant (B) containing a dye having a maximum absorption wavelength of less than 1200 nm, and phosphoric acid (C2), The polymer component comprises an aromatic polycarbonate resin (A), Relative to 100 parts by mass of the aromatic polycarbonate resin (A), The colorant (B) is contained in an amount of 0.001 to 2.0 parts by mass, A wavelength selectively transmitting polycarbonate resin composition comprising the phosphoric acid (C2) in an amount of 0.0001 to 0.004 parts by mass.

2. 2. The wavelength-selective polycarbonate resin composition according to claim 1, wherein the colorant (B) comprises a colorant (B1) containing a dye having a maximum absorption wavelength of less than 700 nm, and / or a colorant (B2) containing a dye having a maximum absorption wavelength in the range of 700 nm or more and less than 1000 nm.

3. 3. The wavelength-selective transmitting polycarbonate resin composition according to claim 1 or 2, wherein the colorant (B) comprises at least one selected from the group consisting of anthraquinone-based dyes, perinone-based dyes, perylene-based dyes, methine-based dyes, azo-based dyes, quinoline-based dyes, phthalocyanine-based dyes, and heterocyclic dyes.

4. 3. The wavelength-selective transmissive polycarbonate resin composition according to claim 2, wherein the colorant (B1) containing a dye having a maximum absorption wavelength of less than 700 nm contains at least one dye selected from the group consisting of anthraquinone dyes, perinone dyes, perylene dyes, and methine dyes.

5. 5. The wavelength-selective polycarbonate resin composition according to claim 2, wherein the colorant (B1) containing a dye having a maximum absorption wavelength of less than 700 nm contains an anthraquinone dye.

6. 6. The wavelength-selective transmitting polycarbonate resin composition according to claim 5, wherein the anthraquinone dye comprises at least one selected from the group consisting of Solvent Yellow 163, Disperse Violet 28, Solvent Blue 97, Solvent Green 28, Solvent Green 3, and Disperse Blue 60.

7. The wavelength-selective transparent polycarbonate resin composition according to any one of claims 2 and 4 to 6, wherein the colorant (B2) containing a dye having a maximum absorption wavelength in the range of 700 nm or more and less than 1000 nm contains at least one dye selected from the group consisting of a phthalocyanine dye, an anthraquinone dye, and a heterocyclic dye.

8. A composition comprising an aromatic polycarbonate resin (A), a colorant (B) containing a pigment having a maximum absorption wavelength of less than 1200 nm, and a phosphate ester compound or phosphoric acid (C), The polymer component comprises an aromatic polycarbonate resin (A), The colorant (B) contains an anthraquinone colorant, The phosphate ester compound or phosphoric acid (C) includes at least one selected from the group consisting of phosphate ester compounds or phosphoric acids represented by the following general formula (I): Formula (I): O=P(OH) n (OR) 3-n [In general formula (I), R is an alkyl group or an aryl group, and n is an integer of 2.] Relative to 100 parts by mass of the aromatic polycarbonate resin (A), The colorant (B) is contained in an amount of 0.29 to 2.0 parts by mass, The wavelength selectively transmitting polycarbonate resin composition contains, with respect to the phosphate ester compound or phosphoric acid (C), 0.005 to 0.3 parts by mass of a phosphate ester compound (C1) or 0.0001 to 0.004 parts by mass of phosphoric acid (C2).

9. The wavelength-selective transparent polycarbonate resin composition according to claim 8, wherein the colorant (B) further comprises a colorant (B1) containing a pigment having a maximum absorption wavelength of less than 700 nm, and / or a colorant (B2) containing a pigment having a maximum absorption wavelength in the range of 700 nm or more and less than 1000 nm.

10. The wavelength-selective transparent polycarbonate resin composition according to claim 8 or 9, wherein the colorant (B) further comprises at least one selected from perinone dyes, perylene dyes, methine dyes, azo dyes, quinoline dyes, phthalocyanine dyes, and heterocyclic dyes.

11. The wavelength-selective transparent polycarbonate resin composition according to claim 9, wherein the colorant (B1) containing a pigment having a maximum absorption wavelength of less than 700 nm further contains at least one selected from a perinone pigment, a perylene pigment, and a methine pigment.

12. The wavelength-selective transparent polycarbonate resin composition according to any one of claims 8 to 11, wherein the anthraquinone dye comprises at least one selected from the group consisting of Solvent Yellow 163, Disperse Violet 28, Solvent Blue 97, Solvent Green 28, Solvent Green 3, and Disperse Blue 60.

13. The wavelength-selective transparent polycarbonate resin composition according to any one of claims 9, 11 and 12, wherein the colorant (B2) containing a dye having a maximum absorption wavelength in the range of 700 nm or more and less than 1000 nm further contains at least one dye selected from the group consisting of phthalocyanine dyes and heterocyclic dyes.

14. The wavelength-selective polycarbonate resin composition according to any one of claims 8 to 13, wherein the compound represented by the general formula (I) includes monostearyl acid phosphate.

15. The wavelength selectively transmitting polycarbonate resin composition according to any one of claims 8 to 14, wherein the compound represented by the general formula (I) comprises a mixture of monostearyl acid phosphate and distearyl acid phosphate.

16. The wavelength-selective polycarbonate resin composition according to any one of claims 1 to 15, further comprising a dye (E) containing a phthalocyanine compound having a maximum absorption wavelength in the range of 1000 nm to 1200 nm.

17. The wavelength-selective polycarbonate resin composition according to claim 16, wherein the dye (E) is represented by the following general formula (II): Formula (II): [C6] [In the formula, R 31 may be the same or different and represent a hydrogen atom or an alkyl group which may have a substituent. R 32 and R 33 may be the same or different, a halogen atom, OR 34 Base, SR 35 Group or NR 36 Or R 37 The group is shown. X 11 may be the same or different and represent an oxygen atom or a sulfur atom. R 34 and R 35 The groups may be the same or different and each represents an alkyl group which may have a substituent, an aryl group which may have a substituent, or a heteroaryl group which may have a substituent. R 36 and R 37 The groups may be the same or different and represent a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group. R 36 and R 37 may be bonded together with the nitrogen atom to which they are bonded, via or without another nitrogen atom, an oxygen atom, or a sulfur atom, to form a 5- to 10-membered saturated or unsaturated heterocyclic ring. The 5- to 10-membered saturated or unsaturated heterocyclic ring may have one or more substituents. M represents two monovalent metal atoms, a divalent metal atom, or a trivalent or tetravalent metal compound.

18. The wavelength-selective polycarbonate resin composition according to claim 16 , wherein the dye (E) is represented by the following general formula (III): Formula (III): [C7] [In the formula, R 31 may be the same or different and represent a hydrogen atom or an alkyl group which may have a substituent. X 11 , X 12 and X 13 may be the same or different and represent an oxygen atom or a sulfur atom. R 34 and R 35 The groups may be the same or different and each represents an alkyl group which may have a substituent, an aryl group which may have a substituent, or a heteroaryl group which may have a substituent. M represents two monovalent metal atoms, a divalent metal atom, or a trivalent or tetravalent metal compound.

19. The wavelength-selective transmitting polycarbonate resin composition according to any one of claims 16 to 18, wherein the phthalocyanine compound is a phthalocyanine dye having a central metal selected from oxovanadium, copper, aluminum, cobalt, and zinc.

20. The wavelength-selective polycarbonate resin composition according to any one of claims 1 to 19, further comprising at least one selected from the group consisting of a heat stabilizer, an antioxidant, a release agent, an ultraviolet absorber, a colorant, a softener, an antistatic agent, an impact modifier, and a spreading agent.

21. A wavelength-selectively transparent polycarbonate resin molded article comprising the wavelength-selectively transparent polycarbonate resin composition according to any one of claims 1 to 20.

22. The wavelength-selectively transmissive polycarbonate resin molded article according to claim 21, which is a Lidar cover.

23. A method for producing a wavelength selectively transmitting polycarbonate resin molded article, comprising molding the resin composition according to any one of claims 1 to 20.

Citation Information

Patent Citations

  • Polycarbonate resin composition and filter for infrared laser

    JP2008009238A

  • Electrophotographic seamless belt and electrophotographic image forming apparatus

    JP2008185945A

  • Black resin composition and resin-molded product

    JP2009035691A

  • One-way valve, and related apparatus, method, flexible pouch and valve assembly using the same

    JP2011088680A

  • Selected wavelength absorption resin composition for lidar and manufacturing method thereof

    JP2017167484A