Surface-functionalized carbonaceous particles, their preparation and application

Surface-functionalized carbonaceous particles, produced through mechanical force and controlled oxidation, address the issues of high surface area carbon additives by improving cycle stability and reducing oxidative corrosion in lead-acid batteries.

JP7587426B2Active Publication Date: 2024-11-20IMERTECH SAS
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020573473
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-27
Filing Date
2019-06-27
Publication Date
2024-11-20
Estimated Expiration
2039-06-27

AI Technical Summary

Technical Problem

Conductive carbon additives used in electrodes for batteries and electrochemical cells face issues such as adverse electrochemical and chemical reactions due to high surface area, leading to reduced cycle life, performance at high speeds, and safety concerns, particularly in lead-acid batteries.

Method used

The production of surface-functionalized carbonaceous particles involves applying mechanical force to non-graphitic carbonaceous materials in a sealed container followed by controlled oxidation, resulting in particles with specific properties like increased oxygen content and altered morphology, which are then dispersed to enhance electrochemical performance.

Benefits of technology

The method produces carbonaceous particles that improve cycle stability, charge acceptance, and reduce oxidative corrosion, enhancing the performance of lead-acid batteries and other electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587426000010
    Figure 0007587426000010
  • Figure 0007587426000011
    Figure 0007587426000011
  • Figure 0007587426000012
    Figure 0007587426000012
Patent Text Reader

Abstract

This disclosure relates to surface-functionalized carbonaceous particles in optionally aggregated forms, methods for producing such surface-functionalized carbonaceous particles, and their use, for example, as conductive additives in battery electrodes. Surface-functionalized carbonaceous particles can be obtained, for example, by a process of grinding a non-graphite carbon material, followed by a functionalization process by controlled oxidation. Surface-functionalized carbonaceous particles can be used as additives in battery electrodes. This disclosure also relates to dispersions of such carbonaceous materials in liquid media, and their use, in particular, as conductive coatings. Polymer compounds filled with surface-functionalized carbonaceous particles are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to surface-functionalized carbonaceous particles, methods for their preparation, and their use, for example, as conductive additives in various applications. [Background technology]

[0002] Generally, conductive carbon particles are used as fillers to enhance electrical conductivity in electrodes of polymers, ceramics, coatings and electrochemical systems.For example, carbon conductive additives are used in various primary and secondary batteries, such as alkaline zinc / manganese dioxide batteries, zinc carbon batteries, lithium primary and rechargeable batteries, nickel cadmium batteries, lead acid batteries, and nickel metal hydride batteries with metals such as zinc or iron, lithium sulfur batteries, lithium air batteries, metal air batteries, fuel cells and capacitor systems.

[0003] Conductive additives are applied in the electrodes of electrochemical cells to reduce the electrical electrode resistance. Carbonaceous powder materials are often chosen as conductive additives due to their small mass and inertness to acidic or alkaline electrolytes. The conductive additives do not contribute to the electrochemical process of the electrodes, which means that for high energy density cells, the amount of conductive additive applied is desirably minimized. Typical carbon conductive additives used are fine graphite powder and conductive carbon black (see, for example, MESpahr, Lithium-ion Batteries-Science and Technology, edited by M. Yoshio, RJ Brodd, A. Kozawa et al., Springer, New York, 2009, Chapter 5).

[0004] The addition of small amounts of conductive carbon to the negative electrode of a lead-acid battery results in improved cycle life when the battery is operated in a high rate partial state of charge (HRPSoC) mode, as applied, for example, in hybrid electric vehicle use (see, for example, K. Nakamura, M. Shiomi, K. Takahashi, M. Tsubota, Journal of Power Sources 59 (1996) 153; M. Shiomi, T. Funato, K. Nakamura, K. Takahashi, M. Tsubota, Journal of Power Sources 64 (1997) 147; and D. Pavlov, P. Nikolov, T. Rogachev, Journal of Power Sources 196 (2011) 5155-5167). When lead-acid batteries are operated at partial state of charge (PSoC), the irreversible formation of lead sulfate (the "sulfation effect") causes a significant decrease in the battery cycle life (see, for example, D. Pavlov, Lead-Acid Batteries-Science and Technology, Elsevier 2011, Chapter 1, pp. 23-26). In addition, it is known that the increased electrode surface provided by the insertion of carbon additives into the electrode structure results in increased charge acceptance of the lead-acid battery, which is required when the lead-acid battery is charged with electricity generated from the brake energy. The increased electrode surface area is thought to result in a supercapacitor effect, which explains the ability to charge the electrode at higher current rates. Therefore, what is required of the carbon is high electrical conductivity as well as high lead uptake when the carbon is immersed in a lead salt solution. During the first electrochemical charging process of a lead-acid electrochemical cell, the incorporated lead forms nuclei for lead deposition (D. Cericola, M. Spahr, Journal of Power Sources 324 (2016), 41-44).

[0005] In addition to using carbon additives, it is known in the art to use modified grid designs, such as glass fiber mats soaked in sulfuric acid electrolyte in valve-regulated lead-acid batteries (VRLABs), and / or otherwise modified electrolyte compositions to improve conventional starting, lighting, ignition (SLI) lead-acid batteries and make them useful for operating modes at lower states of charge (SOC) (see, for example, D. Pavlov, Lead-Acid Batteries-Science and Technology, Elsevier 2011, Chapter 7). The battery characteristics obtained in these advanced lead-acid batteries in shallow, high-rate discharge operation make them suitable candidates for micro- and mild-hybrid electric vehicles.

[0006] The addition of graphite, expanded graphite, activated carbon and carbon black to the negative electrode has been shown to result in improved cycle life of lead-acid batteries, primarily due to a reduction in the sulfation effect.

[0007] Several hypotheses have been proposed to explain the mechanism of carbon effect in the negative electrode. Surveys of the broad spectrum of carbon influences have been summarized in the literature (PT Moseley, Journal of Power Sources 191 (2010) 134-138 and DP Boden, DV Loosemore, MA Spence, TD Wojcinski et al., Journal of Power Sources 195 (2010) 4470-4493). Recently, it has been shown that carbon should have a high affinity for lead to allow the formation of a carbon-lead framework in the negative electrode during lead plating during electrode formation at the first charge of a new freshly assembled cell (D. Pavlov, P. Nikolov, T. Rogachev et al., Journal of Power Sources 196 (2011) 5155-5167). The carbon-lead framework increases the surface area, and in addition, the carbon provides an additional supercapacitive effect in the electrode, both of which provide possible explanations for the increased charge acceptance.

[0008] In addition to the electrical conductivity properties, conductive additives also have an effect on the structure and porosity of the electrode. For example, the electrolyte penetration of the electrode can be affected by the surface and porosity of the electrode, which has an effect on the ionic resistance of the electrode (see, for example, MESpahr's Lithium-ion Batteries-Science and Technology, edited by M. Yoshio, RJ Brodd, A. Kozawa et al., Springer, New York, 2009, Chapter 5).

[0009] The positive electrode of a lithium-sulfur battery contains sulfur mixed with a binder material and one or more carbon components. The carbon provides electrical conductivity and is also believed to ensure dimensional stability of the electrode during cell discharge when the sulfur content of the positive electrode decreases due to the formation of discharge products (see, for example, Xiong, Shizhao; Hong, Xiaobin; Xie, Kai; Rong, Lixia et al., Huagong Jinzhan (2011), 30(5), 991-996; Yao, Zhen-Dong; Wei, Wei; Wang, Jiu-Lin; Yang, Jun; Nuli, Yan-Na et al., Wuli Huaxue Xuebao (2011), 27(5), 1005-1016).

[0010] Additionally, electrochemical cells having an air electrode contained in a fuel cell stack or metal-air battery may require a carbonaceous material in the positive air electrode, which is believed to act as a support for the metal or metal oxide catalyst and also provide a structure to the electrode that provides dimensional stability. For use in air electrodes, carbon supports are required to exhibit high corrosion resistance to air or oxygen, and failure to exhibit such corrosion resistance limits cell durability (see, e.g., S. Sarangapani, P. Lessner, L. Swette, J. Giner et al., Proceedings-Electrochemical Society (1992), 92-11 (Proc. Workshop Struct. Eff. Electrocatal. Oxygen Electrochem., 1992), 510-22; S. Muller, F. Holzer, H. Aral, O. Haas et al., Journal of New Materials for Electrochemical Systems (1999), 2(4), 227-232; and F. Maillard, P. Simonov, E. Savinova et al., Carbon Materials for Catalysis (2009), 429-480).

[0011] As noted above, natural or synthetic graphite, expanded graphite, activated carbon and carbon black have all been used as conductive additives.

[0012] Graphite is a crystalline carbon. The electrical conductivity of graphite is based on the crystalline graphite structure, which consists of stacked layers of six-membered carbon rings with delocalized electrons conjugated to p-orbitals parallel to the graphite layers. The electrical conductivity parallel to the stacked planes is about three orders of magnitude higher than the electrical conductivity perpendicular to the planes. This results in the well-known anisotropic behavior of electrical conductivity (A.W. Hull, Phys. Rev. 10 (1917) 661 and W. Primak, L.H. Fuchs et al., Phys. Rev. 95 (1) (1954) 22).

[0013] For example, the use of graphite as a conductive additive may result in an improvement in the electrode density of the cell due to properties such as its high compressibility. It has also been demonstrated that the carbon conductive additive can significantly improve the cycling stability of the electrode and the charge / discharge performance at low temperatures.

[0014] Typically, high surface area graphite is obtained by reducing the particle size of graphite in a grinding process. To avoid oxidation of the graphite product during grinding, grinding may be performed in an inert gas atmosphere (see, for example, NJ Welham, JS Williams et al. Carbon 36(9) (1998) 1309-1315; TS Ong, H. Yang et al. Carbon 38 (2000) 2077-2085; and Y. Kuga, M. Shirahige, Y. Ohira, K. Ando et al. Carbon 40 (2002) 695-701). Under these conditions, the downsized graphite particles tend to form loosely bound aggregates. A typical grinding process is performed in an air atmosphere, and under these conditions, grinding of graphite results in downsizing of the graphite particles. A drawback of the conventional grinding process is that the obtained graphite material may contain a relatively large amount of trace metals due to wear of the metal-based grinding equipment. Metallic trace elements act as electrocatalysts that interfere with the desired electrochemical processes and cause parasitic chemical or electrochemical side reactions, thus reducing the cycling stability and decreasing the cell life.

[0015] Carbon black is an amorphous form of carbon. Typically, the carbon black structure is composed of spherical amorphous or quasicrystalline primary particles that are bound together by covalent bonds to form larger aggregates. Typically, conductive carbon black consists of primary particles with sizes between 10 and 50 nm, with larger composite aggregates often larger than 100 nm in diameter. Further agglomeration due to electrostatic forces contributes to the structure of carbon black as well. Conductive carbon black aggregates form conductive networks in porous electrodes, thus reducing electrical resistance beyond the percolation threshold observed at a critical carbon concentration (JB Donnet, RP Bansal, MJ Wang et al., Carbon Black Science and Technology, 2nd ed., Marcel Dekker Inc., New York, 1993). The large internal and inter-aggregate void volume of conductive carbon black, created by the structure of carbon black, results in a high oil absorption number. Typically, conductive carbon black has an oil absorption of greater than 150 mL / 100 g (measured by ASTM D2414-01, see method described below).

[0016] Another type of carbonaceous material is activated carbon. Activated carbon consists of amorphous, high surface area carbon powders derived from natural organic products, such as coconut shells, wood products or polymers. These precursors are carbonized at temperatures between 700 and 1600 °C under an inert atmosphere. Following carbonization, the material undergoes an activation process using steam, CO2 or aqueous zinc chloride solutions at elevated temperatures, which increases the BET surface area of ​​the carbonized material. The activation process forms so-called "micropores" as well as mesopores, which are believed to be responsible for the observed increase in surface area (see, for example, H. Marsh, F. Rodriguez-Reinoso et al., Activated Carbon, Elsevier, 2006).

[0017] For example, the use of carbon black as a conductive additive may be due to properties such as high liquid absorption, which is believed to result in higher electrolyte penetration in the electrode. Furthermore, it has been observed that the addition of high surface area carbon components to the negative electrodes of lead-acid batteries results in a significant increase in charge acceptance due to the increased electrochemically available internal electrode area, which is believed to be the result of a more "open" structure of the electrode. A further explanation for the positive effect of carbon black additives is that the charging of the added carbon surface (supercapacitor effect) can result in increased electrochemical capacity, a desirable property in, for example, negative electrodes of lead-acid batteries and supercapacitors.

[0018] However, despite the use of high surface area carbon as a carbon additive, some adverse results regarding cycle life, performance at high rates and low temperature discharge have been observed in lead-acid batteries. The observed effects are related to electrochemical and chemical side reactions occurring at the increased electrode surface. A further problem associated with high surface area carbon components is high water uptake during the formation of electrode pastes, which can negatively impact the manufacture of electrodes containing such additives.

[0019] Furthermore, the decomposition of the aqueous electrolyte, which occurs as a parasitic side reaction during charging in lead-acid batteries, leads to hydrogen formation at the negative electrode. The rate of electrolyte decomposition has been found to be accelerated by the high surface area of ​​carbon and in the presence of typical metallic impurities. The oxygen formed in this reaction at the positive electrode may also be responsible for oxidative carbon corrosion, which is believed to occur especially with high surface area amorphous carbon. The decomposition of the electrolyte to the point of drying out the battery is considered a severe safety issue.

[0020] From the properties described above, it can be seen that the conductive carbon additive is believed to have a significant impact on electrode engineering, its properties, and the manufacturing process of the electrode.

[0021] As explained above, graphite and conductive carbon black are considered to have many complementary properties when considering their use as conductive additives in electrodes. Since both low surface area and high surface area carbons (graphite and amorphous / non-graphitic carbon powders) have different drawbacks but positive effects in the intended applications, attempts to use mixtures of the two have been described in the following literature (see, for example, M. Fernandez, Batteries & Energy Storage (BEST) Spring 2011, 81-93 and M. Fernandez, N, Munoz, R. Nuno, F. Trinidad et al., Proceedings of the 8th International Conference on Lead Acid Batteries, Extended Abstract #6, Lead Acid Battery Department of the Bulgarian Academy of Science, Sofia, Bulgaria, June 7th-10th, 2011, p.23-28). However, these mixtures are associated with problems. For example, in the manufacturing process of the negative electrode, the required uniform mixing of two carbon components, one of which has a very low volume density in the lead oxide paste formulation, can be problematic.

[0022] Efforts to overcome such problems have been described in the prior art, for example WO 2013 / 174536 of Imerys Graphite & Carbon Switzerland describes a process in which graphite is first ground under inert conditions and then the surface of the ground graphite particles is functionalized by controlled oxidation, i.e. exposure to an oxygen-containing atmosphere under defined conditions. Summary of the Invention [Problem to be solved by the invention]

[0023] It is therefore an object of the present invention to provide yet another advantageous carbon material, which can be reliably produced, is easy to handle and has excellent physicochemical and electrochemical properties, particularly when used as a carbon component in electrodes, as well as a method for its preparation. [Means for solving the problem]

[0024] The present disclosure provides novel surface-functionalized carbonaceous particles containing a non-graphitic core, methods for their production and uses for said particles, which exhibit favorable mechanical and electrochemical properties, for example when used as a carbon additive or component in electrode materials.

[0025] Thus, the present disclosure relates in a first aspect to a method for preparing surface-functionalized carbon particles, the method comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed container; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Includes.

[0026] One example for applying mechanical force includes, but is not limited to, grinding to reduce and homogenize the size of the starting particles to a desired size. In some cases, activation of the surface of the particles during grinding leads to agglomeration of the fine carbon particles and increased reactivity to oxidizing reactants. Typically, the functionalization step b) is achieved by exposing the particles obtained from step a) to an oxygen-containing atmosphere until the particles (optionally in agglomerated form) have the desired properties.

[0027] Optionally, the method may also include the preparation of a non-agglomerated product by dispersing the surface-functionalized agglomerate particles obtained from the functionalization step in a liquid (typically water or a water / alcohol mixture) in the presence of a stabilizing amount of a dispersant, or in a polymer, mainly by applying shear forces.

[0028] Thus, further aspects of the present disclosure include crystallographic L of less than about 14 nm, less than about 12 nm, or less than about 10 nm. c and an oxygen content of greater than about 0.6 wt%, greater than about 0.8 wt%, or greater than about 1 wt%. As described above, optionally, such particles may represent agglomerates of finer primary carbon particles. Surface-functionalized carbonaceous particles can be obtained, for example, by the processes described above and further described herein below.

[0029] Dispersions of surface-functionalized carbonaceous particles in non-agglomerated form are a further relevant aspect of the present disclosure. Another aspect of the present disclosure relates to the use of dispersions of surface-functionalized carbonaceous particles as conductive or lubricious coatings.

[0030] Yet another aspect of the invention relates to polymeric compounds filled with the surface-functionalized carbon particles of the invention, as well as battery electrodes comprising the surface-functionalized carbon particles of the invention as conductive additives, and optionally other compounds as functionalizing additives, such as barium sulfate and / or lignosulfates.

[0031] A further aspect of the present invention is directed to providing a conductive additive comprising surface-functionalized carbonaceous particles, which can be used in a variety of applications, such as in lead acid batteries, lithium sulfur batteries, electrochemical double layer capacitors, catalyst supports, and others. [Brief description of the drawings]

[0032] [Figure 1] FIG. 1 shows scanning electron microscope (SEM) pictures (at two different resolutions) of untreated precursor material for surface-functionalized carbon particle material numbers 1, 6 and 7. [Diagram 2] FIG. 1 shows SEM pictures (at two different resolutions) of untreated precursor material for surface-functionalized carbon particles material numbers 2 and 3. [Diagram 3]FIG. 1 shows SEM pictures (at two different resolutions) of untreated precursor material for surface-functionalized carbon particles material numbers 4 and 5. [Figure 4] 1 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 1 obtained according to example 1. [Diagram 5] 2 shows SEM pictures (at two different resolutions) of the surface-functionalized carbon particles material number 2 obtained according to example 1. [Figure 6] 3 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 3 obtained according to example 1. [Figure 7] 3 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 4 obtained according to example 1. [Figure 8] 4 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 5 obtained according to example 1. [Figure 9] 4 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 6 obtained according to example 2. [Figure 10] 4 shows SEM pictures (at two different resolutions) of surface-functionalized carbon particles material number 7 obtained according to example 2. [Figure 11] 1 a) to c) show scanning transmission electron microscope (STEM) images of precursor materials for surface-functionalized carbon particle materials 1 to 7 used in the methods described in Examples 1 and 2. [Figure 12] a) to g) show STEM micrographs of surface-functionalized carbon particles material numbers 1 to 7 obtained by the methods described in Examples 1 and 2, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The present disclosure relates to a method for producing novel surface-functionalized carbon particles, comprising the steps of applying mechanical forces (e.g., grinding) to a non-graphitic carbonaceous particulate material, followed by a step of functionalizing the surface of the modified or newly formed particles by controlled oxidation, as well as novel surface-functionalized carbon particles obtainable by said method. Downstream products and methods using the novel surface-functionalized carbon particles of the present disclosure are also included herein.

[0034] Method for producing novel surface-functionalized carbonaceous particles - Patents.com In a first aspect, the present disclosure relates to a method for preparing surface-functionalized carbon particles, the method comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed container; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Includes.

[0035] In this context, "applying mechanical force" means that mechanical energy is transferred to the non-graphitic carbonaceous starting material to create particles with altered particle morphology, typically including changing their particle size distribution. Mechanical force includes, but is not limited to, impact, grinding and shear forces. One well-known example of how mechanical force is applied includes "grinding", which should be interpreted broadly in this context. It therefore includes not only "classical" grinding using well-known mechanical tools such as ball mills, rotor mills, grinding mills and the like, but also other types of equipment that can transfer mechanical force to particles to generate particles with different morphology (e.g. smaller size), such as jet mills or fluidized bed mills / reactors. Such fluidized bed reactors can accelerate particles to an extent that results in size modification, or can break them up upon collision with other particles or the walls of the equipment.

[0036] It is not necessary to start with a non-graphitic carbonaceous material in particulate form, since the term "applying mechanical force" includes, but is not limited to, the grinding of the carbonaceous material. Thus, non-particulate materials (e.g., sheets or other three-dimensional objects made from non-graphitic carbonaceous materials) can also be converted into particles with the desired size distribution before the subsequent functionalization step by controlled oxidation. However, it is clear that the most convenient starting material is still a non-graphitic carbonaceous material in crystalline form, which may already be close to the desired particle size distribution typically envisaged in the present method.

[0037] As used herein, "controlled oxidation" is a deliberate and deliberate process in which the particles resulting from the first step of the process are exposed to an oxygen-containing atmosphere under controlled conditions, thereby resulting in oxidation of the surface of the carbon particles. Thus, the controlled oxidation in the functionalization step b) results in carbonaceous particles that are functionalized (i.e. modified) at the surface of the carbonaceous particles.

[0038] Controlled conditions in the present context means that the particles obtained from step a) are subjected to such oxygen-containing conditions at a defined, i.e. controlled, temperature and for a defined time (either predetermined by some routine experimentation or until a desired level of oxidation of the particles is achieved).

[0039] Typically, the controlled oxidation can be carried out in the presence of air, moisture, oxygen, another oxidizing gas and / or an oxidizing liquid. Examples of such oxidizing gases are NO x , ozone or carbon dioxide, while oxidizing liquids may include, for example, hydrogen peroxide or nitric acid.

[0040] For example, the controlled oxidation step can be carried out in an atmosphere of oxygen diluted by nitrogen or another inert gas, typically with an oxygen content of 1-50 vol%, preferably 5-30 vol%, more preferably 10-20 vol%. Typically, the upper limit for the oxygen concentration is dependent on the reactivity of the carbon obtained from the first step (which is typically related to the processing time for step a), i.e., carbon particles with a more reactive carbon surface require a lower oxygen content to avoid excessive heat generation and burn-off of the carbonaceous material. Optionally, the controlled oxidation includes moving the carbonaceous particles in a suitable container (e.g. mixer, rotary kiln or fluidized bed reactor) to achieve a uniform functionalization of the particles by contacting the particles with the reactant gas in an ideal manner. Thus, the controlled oxidation of the functionalization step b) is different from simply storing the material from step a) under atmospheric conditions.

[0041] In certain embodiments of the present disclosure, the controlled oxidation is carried out by stirring the materials in a mixer. The mixer may be a powerful batch mixer, which is useful for mixing the materials together in a fast, uniform, and reproducible manner. The mixer may also be, for example, a paddle batch mixer or a dual shaft paddle batch mixer, which allows for a high degree of fluidization of the solid particles and promotes sufficient contact of the carbonaceous particles with the reaction gas (or liquid).

[0042] The exposure time for step b) can generally vary widely depending on the oxygen-containing gas or liquid selected and the temperature in the container. However, suitable exposure times can be easily determined by those skilled in the art depending on the desired parameters of the product, as explained above. Some suitable examples of oxidizing gases and reaction conditions for step b) are outlined herein below and in the examples.

[0043] The functionalization step b) is, for example, any oxidation reaction, typically an exothermic reaction, i.e. the temperature in the reactor / container increases during the contact with oxygen in step b). Thus, the temperature in the reactor may increase to a level that may eventually cause burn-off of the carbonaceous material (e.g. even carbon monoxide or carbon dioxide), especially in an atmosphere containing a large amount of oxygen (e.g. air with about 21 vol% oxygen). The burn-off effect is also influenced by the surface area of ​​the carbonaceous material, a larger surface area resulting in a more exothermic oxidation reaction in step b). Thus, it may be necessary to cool or keep the reactor at least at a temperature low enough to avoid significant burn-off, especially causing loss of carbonaceous material.

[0044] Alternatively or additionally, it is useful and therefore expedient to use a gas with a lower oxygen content in step b).Thus, in some embodiments, the functionalization step b) comprises exposing the particles obtained from process step a) to an atmosphere containing less than 20 vol.%, less than 15 vol.%, less than 10 vol.%, less than 8 vol.%, or less than 6 vol.% oxygen and / or other oxygen-containing gases.As described above, the reduction in oxygen content relative to a "normal" air atmosphere results in less violent oxidation reactions, thereby resulting in less temperature increase during the functionalization step b), which can limit the burn-off of the carbonaceous material under such conditions.

[0045] Thus, the functionalization step b), i.e. the controlled oxidation, is in some embodiments carried out or at least initiated at temperatures below 400° C., below 300° C., below 200° C., below 100° C., below 50° C. or below 30° C. Thereby, no or very limited burn-off of the carbonaceous material is observed, whereas in others, burn-off is observed in the surface modification process at temperatures higher than 400-500° C. Nevertheless, as briefly described above, due to the exothermic reaction of the oxygen-containing gas with the (activated) surface of the carbon particles occurring in step a), an increase in temperature (e.g. to about 150° C. or higher) is often observed in the mixer, even if no external heating is applied to the mixture, because of the exothermic reaction of the oxygen-containing gas with the (activated) surface of the carbon particles occurring in step a).

[0046] In the case of a liquid functionalization process, after completion of the functionalization step b), the product obtained can subsequently be filtered from the liquid and dried.

[0047] It has been found that the oxidation of the non-graphitic carbonaceous particles obtained from step a) can be achieved even at ambient temperature, under the exclusion of air or moisture (e.g., by milling the carbonaceous material in a ball or attritor mill in a closed (airtight) reactor, possibly but not necessarily under reduced pressure or in an inert atmosphere), due to the mechanical activation of the carbon surface. During the mechanical activation step, the morphology of the carbon starting material changes to a mesoporous amorphous morphology. Particles with such a morphology tolerate an increased amount of surface oxides, in some instances even more than about 1 wt% of the material, when exposed to an oxidizing reactant after mechanical activation.

[0048] When carbon black is used as the starting material, it has been observed that the typical carbon black structure disappears after the starting material is subjected to the method described herein. Typically, mechanical activation and the formation of mesoporosity are linked to an increase in the BET SSA of the carbonaceous material (see Tables 1 and 2 below). If a high BET SSA of the resulting carbonaceous material is desired, the use of a carbon precursor with a high BET SSA can reduce the required milling time. The reduced milling time can reduce the cost of materials as well as the cost of potential decontamination by trace impurities during the milling process.

[0049] It has further been discovered that the subsequent functionalization process is believed to effect the desired surface "oxidation" chemistry as well as saturate the activated carbon surface of the carbonaceous particles described herein.

[0050] Generally, the process including steps a) and b) is carried out until the resulting product has the desired product properties and the functionalization reaction with the oxidizing reactant is complete (and the surface is saturated with chemically absorbed oxygen).For example, in certain embodiments, the process, and in particular the functionalization step b), is carried out until the oxygen content of the resulting particles is greater than about 0.6 wt%, greater than about 0.8 wt%, greater than about 1 wt%, or greater than about 1.2 wt% (as determined by instrumental gas analysis (IGA)).

[0051] Alternatively or additionally, the process is carried out until the pH of the aqueous dispersion comprising the particles resulting from the process is below 5.5, below 5.3, below 5.1 or below 5.0 and / or until the pH of the aqueous dispersion comprising the obtained particles is reduced by at least 0.4 pH, at least 0.6 pH units or at least 0.8 pH units compared to the starting material used in step a) of the process.

[0052] In some embodiments, alternatively or additionally, the process comprises providing a particle having a BET SSA of about 100 m 2 / g~about 500m 2 / g, the BET SSA value is particularly important when the starting material already has a very high BET SSA (e.g., certain carbon blacks, both the starting material and the final modified material have a BET SSA of about 500 m 2 / g) may sometimes be outside these values.

[0053] Alternatively or additionally, the process may provide for the xylene density of the resulting particles to be about 1.65 g / cm 3 ~Approx. 2.1g / cm 3 ; approx. 1.85g / cm 3 ~Approx. 2.00g / cm 3 ; approx. 1.90g / cm 3 ~Approx. 2.00g / cm 3 or about 1.95 g / cm 3 ~Approx. 2.00g / cm 3 In certain embodiments, the process can also (alternatively or additionally) be carried out until the resulting particles have an oil absorption (OA) of 70-300 mL / 100 g and / or the material exhibits a mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature below about 580° C. or below about 570° C.

[0054] In certain embodiments, especially in those in which a ball mill or other mill with metal grinding equipment is used during step a), the process can be carried out until the lead incorporation exceeds a certain threshold, for example a lead content of more than 1000 ppm or more than 2000 ppm.On the other hand, in many embodiments, the lead incorporation should also not exceed a certain upper threshold, for example 50000 ppm.Thus, in some embodiments, the process can be carried out until the lead incorporation of the obtained particles is such that the final lead content of the particles is about 2500 ppm to 40000 ppm.However, the lead incorporation can be lower, especially when non-metal grinding equipment and reactor lining are used.

[0055] As described hereinbefore, typically the application of mechanical force in step a) can be achieved by "comminuted". For convenience, step a) can therefore also be referred to as the "comminuted step", although it is not strictly limited to comminution and includes all techniques capable of changing the size and morphology of non-graphitic carbonaceous materials by mechanical energy.

[0056] Examples of suitable types of equipment for step a) described herein include, but are not limited to, sealed (i.e. airtight) vibratory mills, rocker mills, swing mills, planetary ball mills, drum or tumbling mills, ball mills, grinders or grinding mills (horizontal and vertical), pearl and bead mills, and others. In some embodiments of the present invention, the sealed reactor used is a grinding mill or ball mill, such as a rotary mill, tumbling mill or vibratory mill. The grinding media can vary in terms of shape (e.g. spheres, cylinders, cylpebs, rods, etc.), size and material (e.g. steel, iron, ceramics, ZrO2, Al2O3, etc.), depending on the particular plant or reactor used.

[0057] For example, in a vibratory mill, impact forces are generated by the collision of balls when the drum container vibrates. Vibratory mills are known to work effectively because impact forces can be generated effectively even at a filling level of more than 90%. This is a gentler method compared to, for example, grinding with a rotating ball mill, which generally applies higher impact and shear forces (depending on the rotation speed and filling level) to the material to be ground. Thus, in a vibratory mill, the desired product is formed faster, while foreign particle contamination remains less due to less wear of the balls and the inner walls of the grinding compartment. Thus, contamination with metallic impurities is kept low, but of course can be completely eliminated by using non-metallic based balls and linings.

[0058] Thus, according to one embodiment of the invention, the grinding media used in the mill may be made from a non-metallic material, such as ZrO2, Al2O3 or ceramic. Optionally, the mill may be provided with an internal non-metallic lining to prevent further metallic contamination of the particles.

[0059] Additionally, in many embodiments of this aspect of the invention, the grinding step a) is carried out for at least 5 h, at least 10 h, or at least 15 h, and typically for up to 150 h, up to 96 h, up to 84 h, up to 72 h, or up to 60 h, although of course other grinding times (depending on the specific equipment used) can also achieve suitable results. A typical grinding process involves the mechanical treatment of non-graphitic carbonaceous material, ideally having a high purity, in a hermetically sealed ball mill or vibratory mill.

[0060] In certain embodiments, the filling level of the ball mill should be less than 75% or less than 80%, and the rotational speed of the mill should be high enough to ensure that the balls are carried to the top of the drum cylinder and drop into the graphite / ball mass at the bottom of the drum, maximizing the impact of shear forces on the particles being processed.

[0061] Overall, those skilled in the art will understand that the main grinding parameters may have to be readjusted to achieve high surface area or other desired product specifications targeted within industrially "acceptable" time limits, i.e., to reduce grinding time, the carbon material batch size, grinding media type, size and shape, mill packing factor or mass ratio (of carbon to grinding media) will need to be optimized for each specific type of equipment selected, if necessary by performing some routine experimentation.

[0062] In any event, in some embodiments, the milling step is carried out so that the resulting particles are i) D of 1.0 μm to 8.0 μm, preferably 1.0 μm to 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of 12 μm to 70 μm, preferably 15 μm to 40 μm 90 Particle size distribution (PSD) with values; iii) D of 0.4 μm to 1.5 μm, preferably 0.5 μm to 1.2 μm 10 Particle size distribution (PSD) with values; iv) a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or v) a ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32 This is carried out until the feature is achieved.

[0063] All particle size (PSD) values ​​above were determined by laser diffraction using the dry dispersion method described in more detail in the Methods section below. 10 / D 50 / D 90 The value can relate to the agglomerated morphology of the finer primary particles.

[0064] The treatment time in step a) clearly depends on the equipment and is mainly governed by the desired properties of the resulting particles. However, when mechanical force is applied in step a) by grinding, in certain embodiments, suitable grinding times may typically be from about 10 h to about 60 h or from about 15 h to about 50 h.

[0065] In certain embodiments, the grinding step is carried out until the particle size of the non-graphitic starting material is reduced such that the fine particles begin to (re)agglomerate due to their activated (i.e. energy-rich) surface to larger, typically more spherical agglomerates. Thus, in effect, process step a) can serve to create new synthetic carbonaceous (non-graphitic) particles in agglomerated form. These particles are then functionalized in step b) of controlled oxidation. Thus, in some embodiments, the carbonaceous starting material is converted into a new carbonaceous material with mesoporous amorphous morphology having an increased amount of surface oxides of more than about 0.6 wt%, more than about 0.8 wt%, or even more than about 1 wt%. When carbon black is used as the starting material, it has been found that the typical carbon black structure disappears after undergoing the method of the present disclosure.

[0066] Since step a) is carried out in an airtight container, it is typically not necessary to either evacuate the container / reactor (e.g., mill) or even purge it with an inert gas, especially since any remaining oxygen in the reactor is quickly consumed by the carbonaceous material. Typically, the gas quickly adheres to the surface of the particles, but chemical reactions, especially with the oxygen, can also take place (often forming carbon monoxide) at the higher temperatures that arise during the influence of mechanical energy and / or external heating. In some embodiments, the amount of oxygen in the reactor / mill is less than 0.5 wt%, less than 0.2 wt%, or less than 0.05 wt% relative to the total mass of the carbonaceous material.

[0067] Sometimes it may be advantageous to hold the carbonaceous particles obtained in step a) in a hermetically sealed reactor for at least 15 min, at least 30 min, or at least 45 min before carrying out step b), which may serve to complete the agglomeration of the comminuted finer carbonaceous particles having a high surface energy, believed to be due to the activation of the surface upon application of mechanical force during step a).

[0068] As used herein, generally, the term "non-graphitic carbonaceous material" refers to a material having the properties and structure of graphite, e.g., a L of less than about 10 nm. c value, a c / 2 value greater than about 0.3365 nm and / or about 2.2 g / cm 3 Carbonaceous materials that lack the lower xylene density.

[0069] In any event, the methods described herein can be carried out with any non-graphitic starting material, such as carbon black, petroleum coke, calcined petroleum coke, needle coke, coal tar based coke, anthracite, calcined anthracite, polymer derived charcoal, biomass, pyrolytic carbon and mixtures thereof.

[0070] The method described herein is primarily useful for non-graphitic starting materials, such as those listed in the previous paragraph, although, optionally, the method can also be carried out with carbonaceous materials that include some amount of graphitic material mixed with the non-graphitic starting material. Suitable graphitic materials to be mixed with the non-graphitic starting material include, but are not limited to, natural graphite, synthetic graphite, graphitized coke, graphitized anthracite, or mixtures thereof.

[0071] Thus, in certain embodiments, the methods described herein can be carried out using a carbonaceous starting material composition in which a non-graphitic carbonaceous material is mixed with about 10 wt % to about 90 wt %, about 20 wt % to about 80 wt %, or about 10 wt % to about 50 wt % of a graphitic carbon material prior to the grinding performed in step a) or prior to the functionalization step b), see for example the materials prepared in Examples 1 and 2 (properties listed in Tables 1 and 2).

[0072] It has been found that the surface-functionalized (e.g., surface-oxidized) carbonaceous particles obtainable by the method described herein exhibit very good affinity for lead and support the electrochemical deposition of lead. It has been found that the amount of lead uptake typically correlates with the surface oxide content of the particles, i.e., the higher the surface oxide concentration, the higher the amount of lead uptake. The novel carbon particles can be incorporated into the lead structure of the negative plate of a lead-acid battery, where they contribute to the reversible formation of lead sulfate.

[0073] Thus, the particles can be used as an additive that can improve the cycle stability of advanced lead-acid batteries operated in the high current part of the charging operation mode of the advanced lead-acid batteries used to support start / stop functions in vehicles. The particles can also improve the charge acceptance of the advanced lead-acid batteries, which is necessary for the storage of electricity generated from braking operations.

[0074] The carbonaceous particles obtained from the methods described herein may be primarily, but not exclusively, agglomerated or non-agglomerated particles, depending on the primary particle size after step a), where primary particles smaller than a certain size tend to form agglomerated, typically fairly isotropic particles, due to the high surface energy arising in the grinding step a).

[0075] The carbonaceous particles resulting from step b) (functionalization by controlled oxidation) are typically obtained in dry form (unless a liquid oxidant is used, in which case the material can be dried). The dry particles can then be used in a number of downstream applications, as described in more detail herein below.

[0076] In some embodiments, however, the method includes an additional step, where the particles from step b) are then dispersed in a liquid, such as water, alcohol, or a mixture thereof (for environmental reasons, water or a water-ethanol mixture is preferred). Optionally, the suspension may further include one or more dispersants, such as a PEO-PPO-PEO block copolymer, such as Pluronic PE 6800®, available from BASF AG. Alternative dispersants are ionic dispersants such as sulfonic acids, e.g. Morwet EFW® from AkzoNobel, non-ionic dispersants such as alcohol polyethoxylates, e.g. Emuldac AS 25® from Sasol, alkyl polyethers, e.g. Tergitol 15-S-9® from Dow Chemical, n-alkyl polyethylene oxides, polyethylene glycols, iso-alkyl polyethylene oxides or polyethylene glycols or any other dispersants known to a person skilled in the art in the field of pigment dispersions, and / or one or more polymeric binder compounds, e.g. polyacrylates, polyurethanes, styrene butadiene rubbers, acrylic butadiene rubbers, polyvinyl acetates or polyvinyl chlorides.

[0077] Novel surface-functionalized carbonaceous particles Further embodiments of the present disclosure include crystallographic L of less than about 14 nm, less than about 12 nm, or less than about 10 nm. c value; and for surface-functionalized carbon particles having an oxygen content of greater than about 0.6 wt%, greater than about 0.8 wt%, or greater than about 1 wt%.

[0078] As previously described in the method description, the novel carbonaceous particles have a limited crystallite size L cHowever, in certain embodiments, the novel carbonaceous material may also include materials resulting from the blending of non-graphitic and graphitic particles prior to step a) or step b). In these cases, in certain instances, especially for materials made from blends containing a large amount of graphitic particles, the crystallographic L c Preferably, however, such materials have an overall crystallographic L of less than 14 nm, or less than 12 nm, or less than 10 nm, as set forth in the preceding paragraphs. c The values ​​are similarly characterized.

[0079] In some embodiments, surface-functionalized carbon particles according to the present invention can be obtained by the methods described in this disclosure.

[0080] As described above, surface-functionalized carbonaceous particles are generally characterized by an increased concentration of oxygen groups chemisorbed on the carbon surface, and therefore may be referred to herein as "surface oxides". Thus, the oxygen content of the surface-functionalized carbonaceous particles is at least about 0.60 wt%, at least 0.70 wt%, at least about 0.80 wt%, at least about 0.85 wt%, at least about 0.90 wt%, at least about 1.0 wt%, or at least about 1.20 wt%, and typically is about 5 wt% or less or 4 wt% or less, as measured according to the method presented below in the Methods section. As can be seen from Table 1 in the Examples section, all starting materials had an oxygen content (often well below) of 0.60 wt%. Since some of the oxygen groups on the surface of the particles are effectively carboxyl groups, it is not surprising that in many embodiments, the surface-functionalized carbonaceous particles have an acidic pH, i.e., a pH below 7.0, and often even below about 5.5.

[0081] Without wishing to be bound by theory, it is believed that the concentration of the "surface oxide" is particularly related to the affinity of the particle for lead. This is particularly important when using surface-functionalized carbonaceous particles as a conductive additive, for example, in the negative electrode of a lead-acid battery. Furthermore, it is believed that the combination of a specific carbon morphology and a high concentration of the "surface oxide" results in superior lead plate properties.

[0082] In some examples, the surface-functionalized carbonaceous particles according to the present disclosure may be characterized by the following parameters: i) About 100m 2 / g or greater than about 110m 2 / g or greater than about 120m 2 BET surface area greater than 100 m / g, optionally about 100 m 2 / g~about 500m 2 / g, about 110m 2 / g~about 400m 2 / g or about 120m 2 / g ~ approx. 350m 2 BET SSA in / g; ii) an intragranular pore volume less than about 2 mL / g, or less than about 1.8 mL / g; iii) a total pore volume less than about 3 mL / g, or less than about 2.5 mL / g; iv) lead incorporation greater than about 1000 ppm, greater than about 2000 ppm, greater than about 2500 ppm, or greater than about 2800 ppm; v) a pH of the aqueous dispersion containing the particles less than about 5.5, less than about 5.3, less than about 5.1, or less than about 5.0; vi) a mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature of less than about 580° C. or less than about 570° C.; and / or vii) an oil absorption of less than about 500 mL / 100 g, less than about 400 mL / 100 g, less than about 300 mL / 100 g, less than about 250 mL / 100 g, about 70 to about 300 mL / 100 g, or about 70 to about 260 mL / 100 g (OA, Marcol) Any of the following (alone or in any combination) may be further featured:

[0083] Due to the unique morphology of the surface-functionalized carbonaceous materials, the oil absorption is typically significantly lower than other carbon materials, such as carbon black, coke, or activated carbon, with comparable pore volumes and BET SSA.

[0084] In some embodiments, the surface-functionalized carbonaceous particles may alternatively or additionally comprise: i) D of about 1.0 μm to about 8.0 μm, optionally about 1.0 μm to about 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of about 12 μm to about 70 μm, optionally about 15 μm to about 40 μm 90 and / or a particle size distribution (PSD) having a value; iii) D of about 0.4 μm to about 1.5 μm, optionally about 0.5 μm to about 1.2 μm 10 Particle size distribution (PSD) with values; The particle size distribution (PSD, measured by laser diffraction using the dry dispersion method) of the .alpha.-to-.alpha.

[0085] Further, in some instances, the surface-functionalized carbonaceous particles may comprise: a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or A ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32. The method may further comprise:

[0086] It is understood that any of the above additional parameters may be used alone or in combination with another one or more of those parameters to define the novel surface-functionalized carbonaceous particles described herein.

[0087] In certain embodiments, the novel surface-functionalized carbonaceous particles are present in agglomerate form, where submicron non-agglomerated particles are attached together to form agglomerate microstructures. These agglomerates (microstructures) have been found to act as "hosts" with good mechanical stability, for example for use in sulfur cathodes in lithium-sulfur batteries.

[0088] Since the grinding step a) often results in the formation of agglomerated, fairly isotropic particles, it is not surprising that in many instances the Scott density of the novel surface-functionalized carbonaceous materials is typically quite high. Thus, in many embodiments, the Scott density of the carbonaceous materials is between 0.15 and 0.5 g / cm. 3 or 0.20~0.45g / cm 3 and the density is typically much higher compared to the (unmodified) starting material.

[0089] For some embodiments, the surface-functionalized carbonaceous particles may be further characterized by an iron (Fe) content value of less than 500 ppm, less than 400 ppm, less than 300 ppm, less than 200 ppm, or less than 160 ppm. In some embodiments, particularly those in which non-metallic grinding media, such as grinding media made from ZrO2, Al2O3, or ceramic materials, are used in the grinding process, the surface-functionalized carbonaceous particles may be further characterized by an Fe content value of less than 50 ppm, less than 10 ppm, or less than 5 ppm.

[0090] With respect to crystal structure, in certain embodiments, the surface-functionalized carbonaceous particles have a crystallite size L of 1 to 10 nm, 3 to 8 nm, or 4 to 6 nm (as measured by Raman spectroscopy). a has.

[0091] The crystallographic c / 2 values ​​of the surface-functionalized carbonaceous particles were found to be relatively unaffected by the process (i.e., the milling and functionalization steps). Thus, the c / 2 value is largely determined by the c / 2 value of the starting material, although it has been observed that the c / 2 value upon undergoing the processing steps described herein typically increases slightly compared to the starting material (see Table 1 below). Typically, because the particles are made starting from non-graphitic materials, the c / 2 values ​​are mostly greater than 0.3400 nm, greater than 0.3450 nm, or even greater than 0.3500 nm.

[0092] Polymeric compounds filled with surface-functionalized carbonaceous particles The polymeric compounds filled with surface-functionalized carbon particles described herein are another aspect of the present invention, and show good mechanical properties as well as excellent electrical and thermal conductivity. Examples of polymers may be, but are not limited to, polypropylene, polyethylene, polystyrene, polyamide, polyimide, polyphenylene sulfide, polyethyl ether ketone, and elastomers, such as synthetic or natural rubber. It has been found that in many cases, surface-functionalized carbonaceous particles can be used directly, i.e., as agglomerates, to prepare filled polymeric compounds, since it has been observed that typical extrusion processes apply sufficient shear stress to disperse the agglomerates into primary (or at least finer) particles that are then stabilized in the polymer.

[0093] Use of surface-functionalized carbonaceous particles as additives in battery electrodes Because the surface-functionalized carbonaceous particles described herein exhibit superior electrochemical properties, battery electrodes comprising surface-functionalized carbon particles as conductive additives represent a further aspect of the present invention. Due to the submicron particle size of the primary particles, the carbon particles of the present invention exhibit favorable properties, especially in electrodes containing submicron sized electrode materials.

[0094] In some embodiments, the battery electrode material may additionally include barium sulfate, which is known to inhibit the deposition of lead sulfate as a thin non-conductive film on the surface of the electrode material by acting as a (chemically inert) site for the precipitation of lead sulfate itself. Typically, barium sulfate is used with an average particle size of about 1 μm, although particle sizes slightly larger than 1 μm can also work.

[0095] In such an embodiment, barium sulfate is added in an amount of about 0.2 to about 2 wt %, preferably 0.5 to 1.5 wt % or 0.7 to 1.3 wt %, and most preferably about 1 wt % of the total mass of the electrode (see, e.g., Boden, J. Power Sources 73 (1998), pp. 89-92).

[0096] Additionally or alternatively, such battery electrodes may contain, in addition to the surface-functionalized carbonaceous particles and optionally barium sulfate, as further additives. Lignosulfonate may also contain. Lignosulfonate are complex aromatic polyethers that are known to prevent flocculation of lead particles due to their amphiphilic nature, with large hydrophobic organic moieties adsorbing to the surface of the lead particles, while the hydrophilic non-organic components come into contact with the aqueous electrolyte layer, thereby preventing the particles from coalescing or further precipitating (see again, e.g., Boden, J. Power Sources 73 (1998), pp. 89-92).

[0097] In such an embodiment, typically Lignosulfonate is added in an amount of about 0.1 to about 1.5 wt %, preferably 0.3 to 1.0 wt %, and most preferably about 0.75 wt % of the total mass of the electrode.

[0098] Generally, carbon, barium sulfate, and lignosulfate are used as additives and are collectively referred to as "weighting agents." Accordingly, a further embodiment of the present invention is to provide a surface-functionalized carbonaceous particle comprising one or more Lignosulfonateand / or with barium sulfate. Such mixtures can be used, for example, as additives for the negative electrodes of lead-acid batteries.

[0099] The use of battery electrodes containing surface-functionalized carbonaceous particles and, optionally, barium sulfate and / or lignosulfate in lead-acid batteries is yet another aspect of the present invention. The surface-functionalized carbonaceous particles described herein are suitable for plating lead, which is believed to be due to the high mesopore content of the surface-functionalized carbonaceous particles and the chemical reaction of the surface "oxide" groups. Furthermore, better resistance to oxidative corrosion and electrolyte decomposition in lead-acid batteries has also been observed for the carbonaceous particles described herein compared to other carbons with similar surface areas. In addition, the increased concentration of surface oxide surface groups results in a more polar carbon surface, thereby increasing the hydrophilicity of the carbon. This improved wettability of the carbonaceous surface in aqueous media provides an advantage in the manufacturing process of the negative electrode mass, since the carbonaceous mixes more easily into an aqueous paste of lead oxide and other negative electrode components compared to typical graphite or carbon black.

[0100] In a further embodiment of this aspect, a battery electrode containing the surface-functionalized carbonaceous particles can be used as a positive electrode in a lithium-sulfur battery. Due to the microstructure of the surface-functionalized carbonaceous particles, the surface-functionalized carbonaceous particles can act as a host for sulfur, which acts as the electrochemically active component in the positive electrode. It has been found that the positive electrode containing sulfur absorbed in the microstructure of the surface-functionalized carbonaceous particles exhibits excellent mechanical stability and resistance to oxidative corrosion.

[0101] In yet another embodiment of the invention, the battery electrodes described herein can be used as electrochemical double layer capacitors. In some embodiments, the electrochemical double layer capacitors have an average capacitance greater than 7 F / g, greater than 6 F / g, or greater than 5.5 F / g.

[0102] Use of surface-functionalized carbonaceous particles as catalyst supports. The use of surface-functionalized carbon particles as defined herein as carbon supports represents another aspect of the present invention. When used as a scaffold or carbon support in air electrodes used in, for example, fuel cells and metal-air batteries, metal catalysts or metal oxide catalysts may be finely dispersed on the amorphous carbon surface. The surface oxides and pores are believed to act as anchor points to stabilize the finely dispersed catalyst on the carbon surface, which is believed to suppress any separation effects during preparation and operation. A high degree of uniform dispersion of metal catalysts cannot be achieved in typical graphite powders, which is believed to be due, at least in part, to the lack of the previously described surface morphology exhibited by the carbonaceous particles described herein.

[0103] Dispersions of surface-functionalized carbonaceous particles Dispersions of the surface-functionalized carbon particles described herein in a liquid, optionally in the presence of a dispersing agent that aids in the formation of colloidal carbon dispersions, represent another aspect of the invention. These dispersions can be obtained by a process that includes a step of disrupting the (typically agglomerated) particles resulting from the functionalization step by applying energy, mainly in the form of shear forces, and a step of stabilizing the primary particles by using a dispersing agent in a liquid polar medium, for example water, alcohol (methanol, ethanol, propanol) or mixtures thereof.

[0104] Thus, the dispersion process represents a further embodiment of this aspect of the invention. For example, the dispersion process is carried out in an attritor mill. It is clear that the polar surface morphology of the carbonaceous particles facilitates the wetting process with water or polar solvents, aiding in the preparation of colloidal carbon dispersions. Therefore, another related aspect relates to the use of the surface-functionalized carbon particles described herein to form a dispersion in a liquid in the presence of a dispersing agent by applying shear forces to deagglomerate the particles. Examples of suitable dispersing agents that can be used include, but are not limited to, those already referenced above.

[0105] For example, the dispersions described herein above can be used as a base for a conductive coating.

[0106] Measurement method Percentage (%) values ​​specified herein are by weight unless specifically stated otherwise.

[0107] Specific BET surface area, DFT micropore and mesopore volumes and areas The method is based on the expression of the absorption isotherm of liquid nitrogen in the range of p / p0 = 0.04-0.30 at 77 K. Nitrogen gas adsorption is carried out in a Micromeritics Tristar apparatus. According to the instructions proposed by Brunauer, Emmet and Teller (Adsorption of Gases in Multimolecular Layers, J. Am. Chem. Soc., 1938, 60, 309-319), the monolayer volume can be determined. Based on the cross-sectional area of ​​the nitrogen molecule, the monolayer volume and mass of the sample and then the specific surface can be calculated. At 77 K, p / p0 10 -5 The isotherms measured at a pressure of -1 (performed using a Micromeritics ASAP2020 instrument) were determined and processed by DFT calculations to evaluate the pore size distribution, the volume and area of ​​the micro- and micropores. References: Ravikovitch, P., Vishnyakov, A., Russo, R., Neimark, A., Langmuir 16 (2000) 2311~2320; Jagiello, J., Thommes, M, Carbon 42 (2004) 1227~1232

[0108] Particle Size Distribution (PSD) The presence of particles in a coherent beam of light causes diffraction. The broadening of the diffraction pattern is related to particle size. A parallel beam from a low power laser illuminates a cell containing the sample suspended in water. The beam leaving the cell is focused by an optical system. The distribution of light energy in the focal plane of the system is then analyzed. The electrical signal provided by the optical detector is converted by a computer into a particle size distribution. The method yields the ratio of the total volume of particles to the number of distinct size classes, which ratio forms the volumetric particle size distribution (PSD). Typically, a particle size distribution is calculated using a value D 10 , D 50 and D. 90 where 10 vol% of the particle number is D 10 The particle size is smaller than the value, and 50 vol% of the particle number is D 50 The particle size is smaller than the value, and 90 vol% of the particle number is D 90 The measurements were carried out on a Sympatec Helos system using a dry measuring cell.

[0109] The particle size distribution of the coarse graphite is determined by sieve analysis using a vibrating sieve or an air jet sieve, the particle size distribution being determined by the amount of material having a particle size larger than the mesh size of the sieve applied.

[0110] Thermal mass spectrometry (TGA) The determination of the mass loss rate of any carbonaceous material is carried out by using a conventional thermogravimetric analyzer (TGA). Approximately 20-30 mg of sample was used for the measurement. The atmosphere in the thermogravimetric analyzer was air with a flow rate of 10 mL / min and was brought to 1200°C with a heating rate of 10°C / min.

[0111] oxygen content The oxygen mass fraction in solid samples is evaluated using the principle of inert gas fusion or solid carrier gas thermal extraction (IGA). The sample is placed in a graphite crucible and inserted into an electrode furnace. The crucible is held between the upper and lower electrodes of an impulse furnace. After purging with inert gas (H or Ar) and increasing the temperature (above 2500°C), a high current is passed through the crucible. The gases evolved in the furnace are released into a flowing inert gas stream. The gas stream is then sent to a suitable infrared detector (O as CO by non-dispersive infrared (NDIR)) or thermal conductivity detector (N and H by thermal conductivity detector (TCD)) for measurement. The calibration of the instrument is performed using known reference materials.

[0112] pH value A 1.5 g sample of carbon is dispersed in 50 mL of distilled water with a few drops of acetone and sonication. A calibrated pH meter electrode is placed in the slurry. After a stabilization period of 2 min, the slurry is stirred and the pH value is recorded to the nearest 0.05 unit. Reference: ASTM D1512-95(method B))

[0113] Xylene Density The xylene density is obtained by displacement of xylene. Approximately 2.5 g (accurate to 0.1 mg) of powder is weighed in a pycnometer. Xylene is added under vacuum. After a residence time of several hours at normal pressure, the pycnometer is filled, conditioned and weighed. The density represents the ratio between the mass of graphite and the volume of displaced xylene. The value is in g / cm 3 It is written as: reference ISO 8004 Carbonaceous materials for the production of aluminum-calcined coke and calcined carbon products.Determination of the density in xylene by a pyknometric method ISO 9088 Carbonaceous materials used for the production of aluminum-Cathode blocks and prebaked anodes-Determination of the density in xylene by a pyknometric method DIN 51901 (“Prufung von Kohlenstoffmaterialien-Bestimmung der Dichte nach dem Xylolverfahren”) ASTM D5004 (Standard Test Method for Real Density of Calcined Petroleum Coke by Xylene Displacement)

[0114] Tap Density 100 g of dry graphite powder is carefully poured into a graduated cylinder. The cylinder is then secured to an off-center shaft-based tapping machine and 1500 strokes are made. The volume is read and the tapped density is calculated. Reference: DIN-ISO 787-11

[0115] Scott Density The dry carbon powder was passed through a Scott volumetric meter and then 3 (1in 3 The Scott density is calculated from the ratio of mass to volume. Reference: ASTM B 329-98(2003)

[0116] Oil absorption amount The oil absorption test is a technique to determine the general behavior of graphite and graphite-type materials in terms of absorption of liquids. A slow filter paper is placed in a centrifuge metal tube with an inner diameter of 13.5 nm and a sieve (18 mesh) at the bottom. 0.5 g of paraffin oil is filled into the tube to wet the filter paper, and 521 g (1 g = 9.81 m / s) is added. 2 Centrifuge for 30 min at 521 g (corresponding to 1500 rpm in a Sigma 6-10 centrifuge). After the wetting procedure, the tube is defrosted and 0.5 g of graphite powder is added. Cover the graphite with 1.5 g of paraffin oil and centrifuge for 90 min at 521 g. After centrifugation, the tube is weighed. The oil absorption per 100 g of graphite powder is calculated based on the mass gain.

[0117] Metal concentrations (iron and lead in carbon samples) The analysis is carried out by a SDAR OES simultaneous emission spectrometer. Carbon powder milled to a maximum particle size of 80 μm using a vibratory mill is packed into tablets. The sample is placed in the excitation stand under an argon atmosphere of the spectrometer. The fully automated analysis can then be started. Reference: (i) K.Slickers Automatic Emission Spectroscopy Bruhl Druck und Presshaus Giessen (D) (1992), (ii) M.Wissler und P.Gebhardt Protokoll der29.Sitzung des Unterausschusses Feststoffe im Arbeitskreis Kohlenstoff der Deutschen Keramischen Gesellschaft(12. / 13.Dez 1984)

[0118] Crystallite size L a Crystallite size L a is the expression: L a [Angstrom (Å)] = C × (I G / I D) where the constant C has values ​​of 44 [Å] and 58 [Å] for lasers with wavelengths of 514.5 nm and 632.8 nm, respectively, and I G and I D are 1580cm -1 and 1320cm -1 are the intensities of the Raman absorption peaks of the G- and D-bands at 100 nm.

[0119] Raman analysis was performed using a HORIBA Scientific LabRAM-ARAMIS Micro-Raman Spectrometer with a 632.8 nm HeNe LASER.

[0120] Crystallite size L c Crystallite size L c is determined by analysis of the (002) and (004) X-ray diffraction profiles. For the present invention, the method proposed by Iwashita (N. Iwashita, C. Rae Park, H. Fujimoto, M. Shiraishi and M. Inagaki, Carbon 42, 701-714 (2004)) is used. The algorithm proposed by Iwashita is developed specifically for carbon materials. The width of the line profile at half maximum of the sample and the reference is measured. By means of a correction function, the width of the pure diffraction profile can be determined. The crystallite size is then calculated by applying the Scherrer formula (P. Scherrer, Göttinger-Nachrichten 2 (1918) p. 98).

[0121] Layer spacing c / 2 The interlayer spacing c / 2 is determined by X-ray diffraction. The angular position of the peak maximum in the (002) diffraction profile is determined and the interlayer spacing is calculated by applying the Bragg equation. The carbon sample is mixed with a silicon standard. A mixture of polyglycol and ethanol is added to obtain a very high viscosity slurry. A thin layer of about 150 μm is then applied to a glass plate and allowed to dry. A Cu Kα X-ray beam is used. Reference: Klug and Alexander, X-Ray Diffraction Procedures John Wiley and Sons Inc., New York London (1967)

[0122] Lead intake A 10 wt% dispersion of carbonaceous material in 1 M aqueous Pb(NO3)2 is stirred for 24 h. It is then filtered and the residual carbon is washed repeatedly with distilled water and then dried. The BET surface area and Pb content are measured on the dried carbon by the methods described above.

[0123] SEM image Scanning electron microscope (Zeiss Sigma) images were taken at 10,000x and 50,000x (reference Polaroid 545) with an accelerating voltage of 1 kV and a working distance of 2-3 mm using an in-lens detector, and at 100,000x (reference Polaroid 545) with an accelerating voltage of 30 kV and a working distance of 5.5-6 mm using a STEM detector.

[0124] Mercury intrusion porosimetry The method is based on the measurement of the amount of mercury versus the pressure applied to a sample immersed in mercury. Based on the applied pressure, the surface tension of the mercury, the contact angle between the mercury and the solid surface and the pore size can be calculated. Experiments were performed on samples (approximately 0.1-0.3 g) over pressures of 0.5-4000 bar using a Micromeritics Autopore V machine. For data processing, a contact angle of 130° and a pore size of 485×10 -3 Surface tension in N / m was used.

[0125] Conductivity, compressibility and work of compression of powders A powder sample is pressed in a die while a current is passed through the sample by the die piston and anvil. The body of the die is insulating. While the sample is compressed, the pressure, force, sample thickness and voltage are measured. The resistivity is calculated as follows:

number

number

number

[0126] Mixture powder conductivity The resistance of the mixture of carbon and another material is measured by the above method. 4.5kNcm for different mixtures -2 The resistance at a pressure of 100 MPa is plotted as a function of carbon concentration.

[0127] The invention can also be described with reference to the following numbered items: Item 1. A method for preparing surface-functionalized carbon particles, comprising: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; The method includes: Item 2. The process is i) the oxygen content (IGA) of the resulting particles is greater than about 0.8 wt%, preferably greater than about 1 wt%; ii) the pH of the resulting aqueous dispersion containing the particles is less than 5.5, less than 5.3, or less than 5.0; and / or iii) the pH of the resulting aqueous dispersion containing the particles is reduced by at least 0.4 pH, at least 0.6 pH units, or at least 0.8 pH units. The method according to item 1, wherein Item 3. The process is such that the BET SSA of the resulting particles is about 100m 2 / g~about 500m 2 3. The method according to item 1 or 2, wherein the concentration of 1 / g is 1 / g. Item 4. The process is i) The xylene density of the resulting particles is about 1.65 g / cm 3 ~Approx. 2.1g / cm 3 , about 1.85g / cm 3 ~Approx. 2.00g / cm 3 or about 1.95 g / cm 3 ~Approx. 2.00g / cm 3 Or will it be; ii) Whether the oil absorption (OA) of the obtained particles is between 70 and 300 mL / 100 g; iii) the lead incorporation in the resulting particles is between 2,500 ppm and 40,000 ppm; and / or iv) the resulting particles exhibit a mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature of less than about 580° C. or less than about 570° C. The method according to any one of Items 1 to 3, Item 5. The resulting particles are i) D of 1.0 μm to 8.0 μm, preferably 1.0 μm to 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of 12 μm to 70 μm, preferably 15 μm to 40 μm 90 Particle size distribution (PSD) with values; iii) D of 0.4 μm to 1.5 μm, preferably 0.5 μm to 1.2 μm 10Particle size distribution (PSD) with values; iv) a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or v) a ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32 5. The method according to any one of items 1 to 4, Item 6. The method according to any one of Items 1 to 5, wherein the treatment time in step a) is about 10 hours to 60 hours or about 15 hours to about 50 hours. Item 7. The method according to any one of Items 1 to 6, wherein the product from step a) is held in a hermetically sealed reactor for at least 15 min, at least 30 min, or at least 45 min before carrying out step b). Item 8. Controlled oxidation is carried out in the presence of air, moisture, oxygen, another oxidizing gas and / or an oxidizing liquid, and the oxidizing gas produces NO x 8. The method according to any one of items 1 to 7, wherein the oxidizing liquid is hydrogen peroxide or nitric acid. Item 9. The method according to any one of items 1 to 8, wherein the functionalization step b) comprises exposing the particles obtained from step a) to an atmosphere containing less than 20 vol.%, less than 15 vol.%, or less than 10 vol.% oxygen and / or oxygen-containing gas. Item 10. The method according to any one of items 1 to 9, wherein the non-graphitic carbonaceous material used in step a) is selected from carbon black, petroleum coke, calcined petroleum coke, needle coke, coal tar-based coke, anthracite, calcined anthracite, charcoal derived from polymers, biomass, pyrolytic carbon, and mixtures thereof. Item 11. The method according to any one of items 1 to 10, wherein the non-graphitic carbonaceous material is mixed with about 10 wt% to about 90 wt% or about 20 wt% to about 80 wt% of the graphitic carbon material prior to the application of mechanical force in step a). Item 12. The graphitic carbon material is selected from natural graphite, synthetic graphite, graphitized coke, or graphitized anthracite, and optionally, the graphitic carbon material has a diameter of less than about 1 mm. 50 Item 12. The method according to item 11, characterized by a particle size having: Item 13. The method according to any one of items 1 to 12, wherein the particles obtained from step b) are dispersed in a liquid, optionally in the presence of a dispersant or a polymeric compound. Item 14. Surface-functionalized carbonaceous particles obtainable by the method according to any one of items 1 to 13. Item 15. A crystallographic L of less than about 14 nm, less than about 12 nm, or less than about 10 nm. c value; and An oxygen content of greater than about 0.6 wt%, greater than about 0.8 wt%, or greater than about 1 wt%. Surface-functionalized carbonaceous particles having Item 16. i) About 100m 2 / g larger BET surface area; ii) an oil absorption (OA) of less than about 500 mL / 100 g, less than about 400 mL / 100 g, or less than about 300 mL / 100 g; iii) an intragranular pore volume less than about 2 mL / g, or less than about 1.8 mL / g; iv) a total pore volume of less than about 3 mL / g or less than about 2.5 mL / g; and / or v) Lead incorporation greater than about 2800 ppm 16. The surface-functionalized carbonaceous particles according to item 15, further characterized by: Item 17. i) an oxygen content (IGA) of greater than about 0.6 wt.%, or greater than about 0.8 wt.%, preferably greater than about 1 wt.%; ii) a pH of the resulting aqueous dispersion containing the particles less than 5.5, less than 5.3, less than 5.1, or less than 5.0; and / or iii) About 100m 2 / g~about 500m 2 / g BET SSA 17. The surface-functionalized carbonaceous particles according to item 15 or 16, further characterized by: Item 18. i) Approx. 1.65g / cm 3 ~Approx. 2.1g / cm 3 , about 1.85g / cm 3 ~Approx. 2.00g / cm 3 or about 1.95 g / cm 3 ~Approx. 2.00g / cm 3 density of xylene; ii) Oil absorption (OA) of about 70~300mL / 100g; iii) a lead incorporation of about 2,500 ppm to about 40,000 ppm; and / or iv) A mass loss of 5 wt.% by thermogravimetric analysis (TGA) at an onset temperature of less than about 580° C. or less than about 570° C. 18. The surface-functionalized carbonaceous particles according to any one of items 15 to 17, further characterized by: Item 19. i) D of 1.0 μm to 8.0 μm, optionally 1.0 μm to 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of 12 μm to 70 μm, optionally 15 μm to 40 μm 90 Particle size distribution (PSD) with values; iii) D of 0.4 μm to 1.5 μm, optionally 0.5 μm to 1.2 μm 10 Particle size distribution (PSD) with values; iv) a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or v) a ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32 19. The surface-functionalized carbonaceous particles according to any one of items 15 to 18, further characterized by: Item 20. A surface-functionalized carbonaceous particle as defined in any one of items 15 to 19, and at least one Lignosulfonate and / or barium sulfate. Item 21. Use of the surface-functionalized carbonaceous particles as defined in any one of items 15 to 19 or the composition according to item 20 as a conductive additive in a lead-acid battery, in a lithium-sulfur battery, as a catalyst support, as an additive in a battery, as an additive in a polymer, as a filtration aid, as a capacitive deionization aid, or in an electrochemical double layer capacitor, optionally having an average capacitance of more than 5.5 F / g, more than 6 F / g, more than 6.5 F / g, or more than 7.0 F / g. Item 22. A battery electrode comprising the surface-functionalized carbonaceous particles defined in any one of items 15 to 19 or the composition defined in item 20 as a conductive additive. Item 23. The electrode further comprises barium sulfate in an amount of about 0.2 to about 2 wt% of the total mass of the electrode, and / or at least one Lignosulfonate 23. The battery electrode of item 22, further comprising: Item 24. Use of the battery electrode according to item 22 or 23 in a lead-acid battery or a lithium-sulfur battery. Item 25. A polymeric compound filled with surface-functionalized carbonaceous particles as defined in any one of items 15 to 19 or with the composition as defined in item 20. Item 26. A dispersion of surface-functionalized carbonaceous particles as defined in any one of items 15 to 19 or the composition as defined in item 20 in a liquid, optionally in the presence of a dispersant and / or a polymer.

[0128] While various aspects of the invention have been described in general terms above, it will be apparent to those skilled in the art that many modifications and slight variations are possible without departing from the spirit and scope of the invention. Certain embodiments will now be described, by way of illustration, in connection with the following examples. EXAMPLES

[0129] Example 1: Method for the preparation of surface-functionalized carbonaceous particles A carbonaceous material (precursor) with the characteristics shown in Table 1 below was loaded into a drum mill with a chamber volume of 40-50 L, filled to about 25% volume with steel balls with a diameter of about 30 mm and a total mass of 50 kg. The amount of carbonaceous material loaded corresponds to a grinding media / carbonaceous material mass ratio of about 25. The drum mill was filled with nitrogen and hermetically sealed. The (dry) grinding process was then carried out in the airtight grinding chamber of the drum mill.

[0130] After the grinding process was completed, the ground material was placed in a sealed (airtight) grinding chamber for at least about 0.5 h and then transferred into a powerful batch mixer (Eirich, Germany, batch size of 8 L) for the functionalization process. The material was gently stirred in contact with air for a minimum of 1 h without heating (i.e. starting from room temperature, but the mixture warming up due to the exothermic reaction), resulting in surface-functionalized carbon particles with the characteristics in Table 1. Table 1 - Physical characteristics of carbonaceous starting materials and surface-functionalized carbonaceous particles prepared according to Example 1 [Table 1-1] [Table 1-2]

[0131] Example 2: Method for the preparation of carbon / graphite mixed surface-functionalized carbonaceous particles Carbon black material with the characteristics shown in Table 2 below was mixed with synthetic graphite, TIMREX® KS 500 (graphite / carbon black mass ratios of 60 / 40 (material 7) and 80 / 20 (material 8) respectively) and loaded into a drum mill with a chamber volume of 40-50 L, filled to about 25% volume with steel balls with a diameter of about 30 mm and a total mass of 50 kg. Typical values ​​for the synthetic graphite are shown in Table 2A below. The amount of carbonaceous material loaded corresponds to a grinding media / carbonaceous material mass ratio of about 25. The drum mill was filled with nitrogen and hermetically sealed. The (dry) grinding process was then carried out in the airtight grinding chamber of the drum mill.

[0132] After the grinding process was completed, the ground material was placed in a sealed (airtight) grinding chamber for at least about 0.5 h and then transferred into a powerful batch mixer (Eirich, Germany, batch size of 8 L) for the functionalization process. The material was gently stirred in contact with air for a minimum of 1 h without heating (i.e. starting from room temperature, but the mixture warming up due to the exothermic reaction), resulting in surface-functionalized carbon particles with the characteristics in Table 2. Table 2A - Physical characteristics of precursor graphite material TIMREX KS 500 precursor for material numbers 6 and 7 [Table 2] Table 2B - Physical characteristics of carbonaceous starting materials and surface-functionalized carbonaceous particles prepared according to Example 2 [Table 3-1] [Table 3-2]

[0133] Example 3: Additional characteristics of carbonaceous materials (resistance and compressibility) The carbonaceous materials prepared as described in Examples 1 and 2 were further characterized with respect to their electrical resistivity and their compressibility. The results are summarized in Table 3 below. Table 3 - Resistance and compressibility of carbonaceous starting material and surface-functionalized carbonaceous particles prepared according to Examples 1 and 2 [Table 4]

[0134] As shown in Table 1 above, in particular, the BET SSA for material 1 is only 64m 2 From the BET SSA of the precursor carbon black material (CB1) at 291 m / g, 2 / g; lead incorporation increased from 700 ppm to 6000 ppm; and IGA oxygen content (wt%) increased significantly from 0.085% to 2.8%.

[0135] For materials 2 and 3, in particular, the BET SSA is only 3m 2 / g of the precursor coke material; lead uptake was also significantly increased compared to 25 ppm of the precursor coke; and IGA oxygen content (wt%) was significantly increased compared to 0.028% of the precursor coke.

[0136] For materials 4 and 5, notably, the BET SSA was similar to that for the precursor carbon black (CB2) material; however, the IGA oxygen content (wt%) was increased versus 0.53% for the precursor carbon black (CB2); and the internal pore volume (<12 μm) was significantly lower than the 3.04 mL / g of the precursor CB2 material.

[0137] As shown in Table 2B above, specifically for materials 6 and 7 (starting materials being a mixture of carbon black and graphite), the BET SSA is significantly lower than that of the precursor carbon black material (CB1), which is only 64m 2 / g) and BET SSA (1.6m 2 / g); lead uptake was significantly increased from 700 ppm for precursor CB1; and IGA oxygen % was also significantly increased from that of precursor CB1.

[0138] As shown in Table 3 above, especially for material 1, 4 and 20 kN / cm 2 The resistance at 0.052 and 0.019 increased slightly relative to the resistance for the precursor carbon black material (CB1), respectively.

[0139] Furthermore, for materials 2 and 3, 4 and 20 kN / cm 2 The resistance at increased slightly relative to the resistance for the precursor coke material of only 0.045 and 0.023, respectively.

[0140] Furthermore, for materials 6 and 7, 20 kN / cm 2 The resistance at increased slightly relative to the resistance for the precursor CB1 material of only 0.019.

[0141] In addition, 4kN / cm 2 The density at these compression pressures increased slightly for the carbon black derived material but decreased slightly for the coke derived material.

[0142] Because the treatment appears to destroy or modify the original carbon black structure, the compressibility of materials derived from treated carbon black was increased compared to the carbon black precursor, as seen by the density measured at 100 kg cm mechanical work in Table 3.

[0143] The increased content of oxygen-containing groups at the surface of materials 1-7 relative to the precursor materials (as suggested by their increased IGA oxygen %) is believed to be responsible for the observed high affinity for lead, which is expected to result in enhanced electrochemical deposition of lead.

[0144] Thus, carbon materials, such as materials 1-7, can be effectively incorporated into the lead structure, especially in the negative plate of a lead-acid battery. As an additive, these carbon materials can improve the cycle stability of lead-acid batteries, especially when operated in the high current part of the charging operation mode of advanced lead-acid batteries used to support start / stop functions in automobiles, as well as in other industrial lead-acid battery applications. In addition, carbons with increased BET surface area, such as materials 1-7, also improve the charge acceptance of advanced lead-acid batteries, which is necessary for the storage of electricity generated by braking operations. The present invention can be embodied in the following manner. (Appendix 1) 1. A method for preparing surface-functionalized carbon particles, comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; and optionally, the process i) the oxygen content (IGA) of the resulting particles is greater than about 0.8 wt%, preferably greater than about 1 wt%; ii) the pH of the resulting aqueous dispersion containing the particles is below 5.5, below 5.3 or below 5.0; and / or iii) the pH of the resulting aqueous dispersion containing the particles is reduced by at least 0.4 pH, at least 0.6 pH units, or at least 0.8 pH units. The method used to (Appendix 2) The process is i) The BET specific surface area (BET SSA) of the obtained particles is approximately 100 m 2 / g~about 500m 2 / g or; ii) The xylene density of the resulting particles is about 1.65 g / cm 3 ~Approx. 2.1g / cm 3 , about 1.85g / cm 3 ~Approx. 2.00g / cm 3 or about 1.95 g / cm 3 ~Approx. 2.00g / cm 3 Or will it be; iii) Whether the oil absorption capacity (OA) of the obtained particles is 70-300 mL / 100 g; iv) the lead uptake of the resulting particles is between 2,500 ppm and 40,000 ppm; and / or v) the resulting particles exhibit a mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature of less than about 580° C. or less than about 570° C. The method according to claim 1, (Appendix 3) The resulting particles are i) D of 1.0 μm to 8.0 μm, preferably 1.0 μm to 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of 12 μm to 70 μm, preferably 15 μm to 40 μm 90 Particle size distribution (PSD) with values; iii) D of 0.4 μm to 1.5 μm, preferably 0.5 μm to 1.2 μm 10 Particle size distribution (PSD) with values; iv) a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or v) a ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32 3. The method according to claim 1 or 2, (Appendix 4) i) the treatment time in step a) is about 10 hours to 60 hours or about 15 hours to about 50 hours; ii) the product from step a) is held in a hermetically sealed reactor for at least 15 min, at least 30 min or at least 45 min before carrying out step b); and / or iii) the functionalization step b) comprises exposing the particles obtained from step a) to an atmosphere containing less than 20 vol.%, less than 15 vol.%, or less than 10 vol.% oxygen and / or an oxygen-containing gas, optionally the controlled oxidation in step b) is carried out in the presence of air, moisture, oxygen, another oxidizing gas and / or an oxidizing liquid, the oxidizing gas being NO x 4. The method according to any one of claims 1 to 3, wherein the oxidizing liquid is ozone or carbon dioxide, and the oxidizing liquid is hydrogen peroxide or nitric acid. (Appendix 5) 5. The method according to any one of claims 1 to 4, wherein the non-graphitic carbonaceous material used in step a) is selected from carbon black, petroleum coke, calcined petroleum coke, needle coke, coal tar based coke, anthracite, calcined anthracite, charcoal derived from polymers, biomass, pyrolytic carbon and mixtures thereof. (Appendix 6) The non-graphitic carbonaceous material is mixed with about 10 wt % to about 90 wt % or about 20 wt % to about 80 wt % of a graphitic carbon material prior to the application of mechanical force in step a); optionally, the graphitic carbon material is selected from natural graphite, synthetic graphite, graphitized coke, or graphitized anthracite, and optionally, the graphitic carbon material has a diameter of less than about 1 mm D. 50 11. The method according to any one of claims 1 to 10, characterized by a particle size having: (Appendix 7) 7. The method according to any one of claims 1 to 6, wherein the particles obtained from step b) are dispersed in a liquid, optionally in the presence of a dispersant or a polymeric compound. (Appendix 8) Surface-functionalized carbonaceous particles obtainable by the method according to any one of claims 1 to 7. (Appendix 9) A crystallographic L of less than about 14 nm, less than about 12 nm, or less than about 10 nm. c value; and An oxygen content of greater than about 0.6 wt%, greater than about 0.8 wt%, or greater than about 1 wt%. and optionally having i) About 100m 2 / g larger BET surface area; ii) an oil absorption (OA) of less than about 500 mL / 100 g, less than about 400 mL / 100 g, or less than about 300 mL / 100 g; iii) an intragranular pore volume less than about 2 mL / g, or less than about 1.8 mL / g; iv) a total pore volume of less than about 3 mL / g or less than about 2.5 mL / g; and / or v) Lead incorporation greater than about 2800 ppm The surface-functionalized carbonaceous particles further characterized by: (Appendix 10) i) an oxygen content (IGA) of greater than about 0.6 wt.%, or greater than about 0.8 wt.%, preferably greater than about 1 wt.%; ii) a pH of the resulting aqueous dispersion containing the particles less than 5.5, less than 5.3, less than 5.1, or less than 5.0; iii) About 100m2 / g~500m 2 BET SSA in / g; iv) Approx. 1.65g / cm 3 ~Approx. 2.1g / cm 3 , about 1.85g / cm 3 ~Approx. 2.00g / cm 3 or about 1.95 g / cm 3 ~Approx. 2.00g / cm 3 density of xylene; v) Oil absorption (OA) of about 70~300mL / 100g; vi) a lead incorporation level of about 2,500 ppm to about 40,000 ppm; and / or vii) A mass loss of 5 wt. % by thermogravimetric analysis (TGA) at an onset temperature of less than about 580° C. or less than about 570° C. 10. The surface-functionalized carbonaceous particles of claim 9, further characterized by: (Appendix 11) i) D of 1.0 μm to 8.0 μm, optionally 1.0 μm to 5.0 μm 50 Particle size distribution (PSD) with values; ii) D of 12 μm to 70 μm, optionally 15 μm to 40 μm 90 Particle size distribution (PSD) with values; iii) D of 0.4 μm to 1.5 μm, optionally 0.5 μm to 1.2 μm 10 Particle size distribution (PSD) with values; iv) a ratio of DFT mesopore area / BET SSA less than about 0.15, less than about 0.12, or less than about 0.10; and / or v) a ratio of DFT micropore area / BET SSA greater than about 0.25, greater than about 0.30, or greater than about 0.32 11. The surface-functionalized carbonaceous particles of claim 9 or 10, further characterized by a particle size distribution (PSD) of: (Appendix 12) A composition comprising the surface-functionalized carbonaceous particles according to any one of claims 8 to 11 and at least one lignosulfonic acid and / or barium sulfate. (Appendix 13) Use of the surface-functionalized carbonaceous particles according to any one of claims 8 to 11 or the composition according to claim 12 as a conductive additive in a lead-acid battery, in a lithium-sulfur battery, as a catalyst support, as an additive in a battery, as an additive in a polymer, as a filtration aid, as a capacitive deionization aid, or in an electrochemical double layer capacitor, optionally having an average capacitance greater than 5.5 F / g, greater than 6 F / g, greater than 6.5 F / g, or greater than 7.0 F / g. (Appendix 14) 13. A battery electrode comprising the surface-functionalized carbonaceous particles according to any one of claims 8 to 11 or the composition according to claim 12 as a conductive additive, and optionally further comprising barium sulfate in an amount of about 0.2 to about 2 wt % of the total mass of the electrode, and / or at least one lignosulfonic acid in an amount of about 0.1 to about 1.5 wt % of the total mass of the electrode. (Appendix 15) 13. A polymeric compound filled with the surface-functionalized carbonaceous particles according to any one of claims 8 to 11, or the composition according to claim 12, or a dispersion of the surface-functionalized carbonaceous particles according to any one of claims 8 to 11, or the composition according to claim 12, in a liquid, optionally in the presence of a dispersing agent and / or a polymer.

Claims

1. A method for preparing surface-oxidized carbon particles, comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Including, The process is i) The BET specific surface area (BET SSA) of the resulting particles is 100 m 2 / g to 500m 2 / g; and / or ii) The xylene density of the resulting particles is 1.65 g / cm 3 ~2.1 g / cm 3 and / or iii) the oil absorption (OA) of the resulting particles is between 70 and 300 mL / 100 g; and / or iv) the resulting particles have a lead incorporation of between 2500 ppm and 40,000 ppm; and / or v) the resulting particles exhibit a mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature below 580° C. A method that is carried out until 2. A method for preparing surface-oxidized carbon particles, comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Including, The resulting particles are i) D of 1.0 μm to 8.0 μm 50 and / or a particle size distribution (PSD) having a value; ii) D of 12 μm to 70 μm 90 and / or a particle size distribution (PSD) having a value; iii) D of 0.4 μm to 1.5 μm 10 and / or a particle size distribution (PSD) having a value; iv) a ratio of DFT mesopore area / BET SSA lower than 0.15; and / or v) a ratio of DFT micropore area / BET SSA greater than 0.25 A method comprising:

3. A method for preparing surface-oxidized carbon particles, comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Including, A method wherein the non-graphitic carbonaceous material is mixed with 10 wt % to 90 wt % graphitic carbon material prior to the application of mechanical force in step a).

4. A method for preparing surface-oxidized carbon particles, comprising the steps of: a) applying a mechanical force to a non-graphitic carbonaceous material in a hermetically sealed reactor; and b) functionalizing the resulting modified carbon particles by controlled oxidation; Including, The process wherein the particles obtained from step b) are dispersed in a liquid.

5. i) the treatment time in step a) is 10 h to 60 h; and / or ii) the product from step a) is held in a hermetically sealed reactor for at least 15 min before carrying out step b); and / or 3. The method according to claim 1, wherein the functionalization step b) comprises exposing the particles obtained from step a) to an atmosphere containing less than 20 vol.% oxygen and / or oxygen-containing gas.

6. 6. The method according to any one of claims 1 to 5, wherein the non-graphitic carbonaceous material used in step a) is selected from carbon black, petroleum coke, calcined petroleum coke, needle coke, coal tar based coke, anthracite, calcined anthracite, charcoal derived from polymers, biomass, pyrolytic carbon and mixtures thereof.

7. Crystallographic L smaller than 14 nm c value; and Oxygen content greater than 0.6 wt% The non-graphitic, surface oxidized carbonaceous particles have a

8. i) an oxygen content (IGA) greater than 0.6 wt%; and / or ii) a pH of the resulting aqueous dispersion containing the particles that is less than 5.5; and / or iii) 100m 2 / g to 500m 2 / g BET SSA; and / or iv) 1.65g / cm 3 ~2.1 g / cm 3 and / or the xylene density v) an oil absorption (OA) of 70 to 300 mL / 100 g; and / or vi) lead incorporation between 2500 ppm and 40000 ppm; and / or vii) A mass loss of 5 wt % by thermogravimetric analysis (TGA) at an onset temperature of less than 580° C.

8. The surface oxidized carbonaceous particle of claim 7, further characterized by:

9. i) D of 1.0 μm to 8.0 μm 50 and / or a particle size distribution (PSD) having a value; ii) D of 12 μm to 70 μm 90 and / or a particle size distribution (PSD) having a value; iii) D of 0.4 μm to 1.5 μm 10 and / or a particle size distribution (PSD) having a value; iv) a ratio of DFT mesopore area / BET SSA lower than 0.15; and / or v) a ratio of DFT micropore area / BET SSA greater than 0.25 9. The surface oxidized carbonaceous particles of claim 7 or 8, further characterized by a particle size distribution (PSD) of:

10. A composition comprising the surface-oxidized carbonaceous particles according to any one of claims 7 to 9 and at least one lignosulfonate and / or barium sulfate.

11. Use of the surface-oxidized carbonaceous particles according to any one of claims 7 to 9 or the composition according to claim 10 as a conductive additive in a lead-acid battery, in a lithium-sulfur battery, as a catalyst support, as an additive in a battery, as an additive in a polymer, as a filtration aid, as a capacitive deionization aid, or in an electrochemical double layer capacitor.

12. A battery electrode comprising the surface-oxidized carbonaceous particles according to any one of claims 7 to 9 or the composition according to claim 10 as a conductive additive.

13. A polymer compound filled with the surface-oxidized carbonaceous particles according to any one of claims 7 to 9 or the composition according to claim 10, or a dispersion in a liquid of the surface-oxidized carbonaceous particles according to any one of claims 7 to 9 or the composition according to claim 10.

Citation Information

Patent Citations

  • Production process of large isotropic and isostatic high purity graphite with fine particles

    CN102502603A

  • JP1975151902A

  • Aqueous dispersion of carbon black and water-based ink using the same

    JP1999349314A

  • Oxidized carbon colloid and plant growth agent made of the same

    JP2001180921A

  • Activated carbon and its manufacturing method

    JP2006104002A