Mineral wool binders and curing resins

A curable formaldehyde-free resin with reducing sugar, polycarboxylic acid, polyol, and epoxy silane addresses mechanical weaknesses in existing resins, providing enhanced adhesion and weather resistance in mineral wool products.

JP7587596B2Active Publication Date: 2024-11-20URSA INSULATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022562148
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-16
Filing Date
2021-04-13
Publication Date
2024-11-20
Estimated Expiration
2041-04-13

AI Technical Summary

Technical Problem

Existing formaldehyde-free resins for mineral wool products suffer from poor mechanical properties, especially under humid conditions, and issues such as low solubility in cold water, instability of dispersions, and high manufacturing costs.

Method used

A curable formaldehyde-free resin comprising reducing sugar, polycarboxylic acid, polyol, and epoxy silane, with specific weight ratios, that forms an aqueous dispersion and cures at elevated temperatures, enhancing adhesion and mechanical properties through esterification and crosslinking reactions.

Benefits of technology

The resin achieves improved mechanical properties under both dry and humid conditions, with enhanced weather resistance and reduced manufacturing costs, while being environmentally friendly due to the use of renewable components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587596000001
    Figure 0007587596000001
  • Figure 0007587596000002
    Figure 0007587596000002
  • Figure 0007587596000003
    Figure 0007587596000003
Patent Text Reader

Abstract

Provided herein are embodiments of a curable formaldehyde-free resin and a method for producing the curable formaldehyde-free resin. The curable formaldehyde-free resin is provided in the form of an aqueous dispersion. The curable formaldehyde-free resin includes component (a) a reducing sugar, component (b) a polycarboxylic acid, component (c) one or more polyols having a molecular weight of less than 1000 g / mol, and component (d) an epoxy silane. The total amount of component (c) in the curable formaldehyde-free resin is 0.5 to 10 wt % based on the sum of components (a) and (b). The amount of component (d) is 0.1 to 2 wt % based on the sum of components (a) and (b). Additionally, a method for producing a curable formaldehyde-free resin according to one of the embodiments of the present disclosure is provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY OF THE DISCLOSURE The presently described embodiments relate to curable formaldehyde-free resins in the form of aqueous dispersions and methods for making the curable formaldehyde-free resins. [Background technology]

[0002] Mineral wool products are widely used for fire protection as well as thermal and sound insulation of various parts of buildings, vehicles and other equipment. Mineral wool materials are primarily randomly entangled masses of mineral fibers of various lengths, usually bound together by a resin-based binder. Three types of mineral materials are most commonly used: glass, stone or slag. Mineral wool is formed by a complex network of fibers that can be bound at their crossings by various means, for example, using a hardening binder. Methods for producing mineral wool products are well known in the art and typically include melting the mineral material to a suitable temperature, fiberizing the molten mixture into fine fibers, applying (e.g., spraying) a binder composition to the individual fibers, collecting the fibers and forming a primary fleece on a perforated conveyor, densifying the fleece, and curing the binder at high temperatures. The hardened mat is then cut to the desired size using cross trimmers and edge trimmers and optionally rolled up before being packaged for transportation.

[0003] The type and amount of binder used to bind the fibers in the mineral wool plays an important role in the final properties of the mineral wool produced. Although various binder systems have been described in the art, including binders based on melamine urea formaldehyde resins, furan-based resins, etc., phenol-formaldehyde resin-based binders have been preferred for a very long time due to their good performance and attractive low cost.

[0004] However, due to environmental and toxicological concerns regarding formaldehyde emitted from products made with phenol-formaldehyde resin-based binders, there is a movement in the mineral wool industry to reduce or completely eliminate the use of such resins, or to reduce the amount of excess formaldehyde they contain.

[0005] In this regard, various formaldehyde-free resins are described in the art, which claim to reduce formaldehyde emission to zero.Some illustrative examples of these alternative resins are (a) resins based on esterification reaction between carboxylated polymers (e.g., acrylic copolymers) and low molecular weight polyfunctional alcohols, (B) resins using renewable carbohydrate materials reacted with low molecular weight polyacids as crosslinking agents, and (c) resins based on the Maillard reaction between reducing sugars, acid precursors and nitrogen sources; (d) starch and its derivatives are also explored as renewable components of formaldehyde-free resin-based binder compositions, due to their low cost availability.

[0006] For example, binders are known from WO 2015 / 132518 A1, WO 2015 / 144843 A1, EP 3148951 A1, WO 2009 / 080938 A2, and WO 2013 / 021112 A1.

[0007] Formaldehyde-free resins previously described in the art have various drawbacks. Many formaldehyde-free resins have poor mechanical properties (i.e., poor resistance to degradation), especially under wet conditions. For the purpose of using formaldehyde-free resins in insulation products, weatherability and good aging properties are very important factors. Further drawbacks of some conventional formaldehyde-free resins include low solubility in cold water, instability of their dispersions, undesirably high viscosity of the solutions obtained after solubilization (e.g., after gelatinization, hydrolysis, etc.), and high production costs. Summary of the Invention

[0008] Detailed Description of the Invention and Preferred Embodiments Briefly, a curable formaldehyde-free resin and a method for producing the curable formaldehyde-free resin are provided to overcome at least some of the above-mentioned limitations of prior art formaldehyde-free resins. This object is achieved by the resin according to claim 1 and the method for producing the resin according to claim 13.

[0009] According to one embodiment, a curable formaldehyde-free resin in the form of an aqueous dispersion is provided. The curable formaldehyde-free resin comprises component (a) a reducing sugar, component (b) a polycarboxylic acid, component (c) one or more polyols having a molecular weight of less than 1000 g / mol, and component (d) an epoxy silane. The total amount of component (c) in the curable formaldehyde-free resin is 0.5 to 10% by weight based on the sum of components (a) and (b). The amount of component (d) is 0.1% by weight to 2% by weight based on the sum of components (a) and (b).

[0010] The resins according to the present disclosure are "curable" and therefore cure when subjected to high heating temperatures. For example, the resins of the present invention can be cured at temperatures above 100°C in a curing oven. The curing step is contemplated so that the curable formaldehyde-free resin acts as a binder for the mineral wool. Without intending to be bound by theory, it is believed that an esterification reaction between the reducing sugar of component (a) and the polycarboxylic acid of component (b) occurs during curing. In addition, it is also believed that the resins of the present invention may also cure by a crosslinking reaction between the multiple carboxyl groups of the polycarboxylic acid (component (b)) and the multiple hydroxyl groups in the reducing sugar (component (a)) and / or in one or more polyols (component (c)). Additionally and / or alternatively, other curing mechanisms may occur based on chemical or physical interactions between the components.

[0011] "Formaldehyde-free" according to the present disclosure is to be understood as meaning that the resin does not contain or is essentially free of formaldehyde, and that no formaldehyde is released or is essentially free of formaldehyde from the resin or from the binder or mineral wool product containing the resin by curing the resin. "Essentially free of formaldehyde" means that the formaldehyde concentration in the formaldehyde-free resin is less than 0.1% by weight, more preferably less than 0.01% by weight, or even less than the detectable limit of formaldehyde, and even more preferably zero, based on the sum of the weights of the resin components (a), (b), (c) and (d).

[0012] Components (a), (b), (c) and (d) of the curable formaldehyde-free resin according to the present disclosure comprise all such components in the resin, i.e., all of the reducing sugars contained in the resin are contained in component (a), all of the polycarboxylic acids contained in the resin are contained in component (b), all of the polyols contained in the resin are contained in component (c), and all of the epoxy silanes contained in the resin are contained in component (d).

[0013] Component (a) may be selected from monosaccharides, oligosaccharides, polysaccharides and mixtures thereof. Typically, component (a) is a mixture of different saccharides, in particular a mixture of monosaccharides, oligosaccharides and polysaccharides. According to one embodiment, component (a) is a dextrin, preferably a maltodextrin. The dextrose equivalent (DE) of component (a) may be between 11 and 21, preferably between 12 and 20, more preferably between 14 and 19, even more preferably between 15 and 17. In a preferred embodiment, the dextrose equivalent is between 17 and 21. In another preferred embodiment, the dextrose equivalent is between 11 and 15. In a more preferred embodiment, the dextrose equivalent is about 12 or 19.

[0014] Suitable methods for determining dextrose equivalent are well known in the art. In particular, all dextrose equivalent values ​​referred to in this disclosure were measured according to ISO standard 5377-1994, which specifies the Lane-Eynon titration method for determining reducing power and dextrose equivalent in starch hydrolysis products.

[0015] In a particular embodiment, component (a) is a maltodextrin having a DE of 11-21, preferably a DE of 11-15 or 17-19.

[0016] Typically, the curable formaldehyde-free resin comprises component (a), in particular maltodextrin, in the range of 50-80 wt. %. According to one embodiment, the curable formaldehyde-free resin comprises component (a), in particular maltodextrin, in the range of 60-70 wt. %.

[0017] The weight percentages disclosed herein are given as relative ratios by weight % unless otherwise stated. In some embodiments, the sum of all components may be greater than 100%. In many examples, the relative weight percentages are specified so that the sum of components (a) and (b) corresponds to 100% for ease of comparison. Throughout this specification and claims, the weight percentages given for components (a)-(d) and any other components are given for the compounds in their pure form, excluding any impurities, e.g., water or solvents, that may be contained in their commercial form.

[0018] Typically, component (b) is a saturated aliphatic polycarboxylic acid or anhydride or salt thereof. Exemplarily, component (b) may be a monomeric polycarboxylic acid. The monomeric polycarboxylic acid may be a dicarboxylic acid or a tricarboxylic acid. In certain embodiments, the polycarboxylic acid is a C3-C10 polycarboxylic acid comprising at least two carboxyl groups separated by at least one carbon atom. Suitable acids include maleic acid, malonic acid, fumaric acid, malic acid, ascorbic acid, succinic acid, adipic acid, glutaric acid, tartaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, citric acid, anhydrides and salts thereof, and combinations thereof. In certain embodiments, component (b) may be selected from citric acid, succinic acid, tartaric acid, adipic acid, anhydrides and salts thereof. Component (b) may also be any combination of citric acid, succinic acid, tartaric acid, adipic acid, anhydrides and salts thereof. According to one embodiment, the polycarboxylic acid is citric acid.

[0019] In one particular embodiment, the curable formaldehyde-free resin is characterized in that component (a) is maltodextrin and component (b) is citric acid. Preferably, the curable formaldehyde-free resin is characterized in that component (a) is maltodextrin having a DE of 17-19 or having a DE of 11-15 and component (b) is citric acid.

[0020] According to one embodiment, the curable formaldehyde-free resin comprises component (b), in particular citric acid, in the range of 20% to 50% by weight, optionally in the range of 25% to 40% by weight.

[0021] In a particular embodiment, the curable formaldehyde-free resin comprises 50-80% by weight maltodextrin and 20-50% by weight citric acid, preferably 60-70% by weight maltodextrin and 25-40% by weight citric acid.

[0022] The polyol described herein is an organic compound that contains at least two hydroxyl groups. Sugars, especially reduced sugars, are not polyols in the present disclosure (although they contain multiple hydroxyl groups), as is common knowledge to those skilled in the art. On the other hand, sugar alcohols (or hydrogenated sugars), which are generally derived from sugars, such as sorbitol, can be considered as polyols in the present disclosure. It is believed that the polyol in the formaldehyde-free resin of the present application acts as an agent for improving the degree of crosslinking.

[0023] In a preferred embodiment, the polyol has few hydroxyl groups and limited carbon chain length. Each of the one or more polyols has a molecular weight of less than 1000 g / mol, preferably less than 500 g / mol, and even more preferably less than 300 g / mol. In one embodiment, the one or more polyols contain 5 or less hydroxyl groups, preferably 4 or less hydroxyl groups, and more preferably 3 hydroxyl groups. In another embodiment, the one or more polyols contain exactly 2 hydroxyl groups.

[0024] In a particular embodiment, the polyol in the formaldehyde-free resin of the present invention, i.e., component (c), is an alkylene glycol. In the context of the present invention, an alkylene glycol is understood as an organic diol having two hydroxyl groups on two different carbon atoms. Preferably, the carbon atoms having the hydroxyl groups are adjacent. They can also be described as alcohols derived from ethylene glycol. The term alkylene glycol, as used herein, also includes diols obtained by condensation of ethylene glycol, in which the hydroxyl groups are located on non-adjacent carbon atoms. Preferred alkylene glycols are ethylene glycol, propylene glycol, trimethylene glycol (1,3-propanediol), neopentyl glycol, diethylene glycol, triethylene glycol and polyethylene glycol. More preferably, the alkylene glycol is selected from ethylene glycol, propylene glycol and mixtures thereof. Even more preferably, the alkylene glycol is ethylene glycol.

[0025] In a preferred embodiment, the polyol in the formaldehyde-free resin of the present invention, i.e., component (c), is selected from ethylene glycol, tetraethylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerol, diglycerol, triglycerol, triethanolamine, diethanolamine, trimethylolpropane, propylene glycol, poly(ethylene) glycol, and combinations thereof. Suitable poly(ethylene glycols) according to the present invention are those having a molecular weight of less than 1000 g / mol, such as PEG-200, PEG-300, PEG-400, PEG-600, etc. More preferably, the polyol is selected from ethylene glycol, tetraethylene glycol, 1,4-butanediol, glycerol, triglycerol, triethanolamine, trimethylolpropane, propylene glycol, poly(ethylene) glycol, and combinations thereof. In one embodiment, the one or more polyols are ethylene glycol.

[0026] The total amount of component (c) in the curable formaldehyde-free resin is 0.5-10% by weight based on the sum of components (a) and (b). Surprisingly, the inventors have found that when the total amount of polyols exceeds 10% by weight based on the sum of components (a) and (b), the mechanical properties of the curable formaldehyde-free resin, such as the maximum load value, i.e., the maximum mechanical bond strength or the maximum slope value of the strain-stress curve, are dramatically reduced. Therefore, the total amount of polyols in the curable formaldehyde-free resin should be 10% by weight or less based on the sum of components (a) and (b).

[0027] In one embodiment, the total amount of component (c) in the curable formaldehyde-free resin is 1 to 6% by weight, preferably 2 to 5% by weight, more preferably 3 to 4% by weight, based on the total of components (a) and (b). Alternatively, the total amount of component (c) in the curable formaldehyde-free resin is 1 to 2% by weight, based on the total of components (a) and (b). The range of 1 to 2% shows particularly high weather resistance and good aging resistance.

[0028] In a preferred embodiment, the epoxy silane is an alkoxy-epoxy-silane, in particular an alkoxy-epoxy-silane selected from tri-methoxy-epoxy-silane, tri-ethoxy-epoxy-silane, isopropoxy-epoxy-silane, tert-butoxy-epoxy-silane, di-methoxy-epoxy-silane or di-ethoxy-epoxy-silane. Illustratively, component (d) may be 3-glycidoxypropyltrimethoxysilane, 3-glycidoxyethyltrimethoxysilane, 3-glycidoxymethyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxyethyltriethoxysilane, 3-glycidoxymethyltriethoxysilane, or a combination thereof.

[0029] The amount of component (d) is 0.1% by weight to 2% by weight based on the total of components (a) and (b). Preferably, the amount of component (d) is 0.1% by weight or more and less than 2% by weight based on the total of components (a) and (b). In a more preferred embodiment, the amount of component (d) is 0.2% by weight to 1.9% by weight, or 0.3% by weight to 1.8% by weight based on the total of components (a) and (b). In another preferred embodiment, the amount of component (d) is 0.2% by weight to 1.5% by weight, or 0.4% by weight to 1% by weight, or more preferably 0.5% by weight to 0.8% by weight based on the total of components (a) and (b). Typically, the amount of component (d) is 0.4% by weight to 1.7% by weight, or 0.6% by weight to 1.3% by weight, or more preferably 0.7% by weight to 1.1% by weight, or 0.8% by weight to 1% by weight based on the total of components (a) and (b). Alternatively, the amount of component (d) may be 0.2% to 0.5% by weight based on the total of components (a) and (b). The 0.2% to 0.5% by weight range may be advantageous for applications requiring particularly high mechanical strength of the curable resin under dry conditions.

[0030] The epoxy groups of the epoxy silane (component (d)) open in an aqueous environment, resulting in a silane containing a hydroxyl group that can act as a crosslinker in the resin. Furthermore, when component (d) is an alkoxy-epoxy-silane, the alkoxy groups of the alkoxy-epoxy-silane are hydrolyzed in contact with an aqueous medium to hydroxyl groups that can react with the functional groups of the mineral wool, e.g., the silanol groups of glass fibers.

[0031] Epoxy silanes improve adhesion between organic resins and inorganic mineral wool during the curing process, i.e. act as "coupling agents". Although it is known in the art to provide such coupling agents, prior art resins are primarily based on aminosilanes. Aminosilanes are fairly inexpensive components, exhibit good chemical stability, and have been shown to improve adhesion of the cured resin compared to the complete absence of coupling agents in the curable resin. The inventors have discovered that resins containing epoxysilanes exhibit significantly better mechanical properties compared to resins containing aminosilanes. However, epoxysilanes are a fairly expensive component. Resins containing 2.5 wt%, 3 wt% or higher amounts of epoxysilanes improve mechanical properties, but result in products of little commercial interest, which led the inventors to consider other options.

[0032] The present invention is based on the surprising discovery that by providing a curable resin comprising an epoxy silane and a polyol, the mechanical properties can exceed those of a curable resin containing only an epoxy silane, particularly as a "coupling agent" or "adhesion promoter", when the amount of epoxy silane is limited to less than 2% by weight relative to the sum of components (a) and (b). Without intending to be bound by theory, it is believed that the polyol acts as a coupling agent between the inorganic mineral wool and the organic components of the resin, in addition to the epoxy silane. It is believed that the low concentration of epoxy silane acts as an adhesion promoter between the fiber and the resin, while the polyol acts as a crosslinker within the resin. The small size of the polyol considered in the composition (having a molecular weight of less than 1000 g / mol) may allow the polyol to act as a crosslinker between the components of the resin. On the other hand, the presence of the amount of polyol according to the present disclosure results in an improvement of the mechanical properties of the resin. A higher amount of polyol may result in very high crosslinking, but high crosslinking may result in a hard resin that is difficult to handle. As mentioned above, another surprising finding of the present invention is that when polyol is provided in high amounts, at a certain point, the mechanical properties deteriorate dramatically, especially under wet conditions. These findings are in stark contrast to the disclosure of WO 2015 / 144843 A1, which teaches the use of large amounts of epoxy silane and large amounts of polyol (hydrogenated sugar). Furthermore, the presence of the amount of polyol and epoxy silane according to the present disclosure facilitates processing of the curable resin. The low solubility of epoxy silane hinders processing with increasing weight percentage, even requiring pre-reaction in water. In addition, the reactivity of epoxy silane can result in undesirable reactions that are difficult to control. Thus, the curable resin according to the present disclosure with a moderate amount of epoxy silane minimizes the aforementioned disadvantages associated with the use of epoxy silane.

[0033] The advantageous mechanical properties mentioned above relate both to the post-manufacturing situation and to the post-aging situation under environmental humid conditions, i.e. the resins of the present invention show enhanced resistance to the effects of weathering. The mechanical properties of the resin are properties of the resin after the curing step, which is a direct result of the composition of the curable resin itself. The curing step can be carried out by conventional methods known to those skilled in the art.

[0034] Yet another advantage of the present invention is the use of components that are of natural origin and / or derived from renewable resources, thus enhancing the recyclability of the resin. For example, component (a) (reducing sugars) and many of the preferred polycarboxylic acids (component (b)), such as citric acid, are of natural origin, while many of the preferred polyols, such as ethylene glycol, glycerol, 1,4-butanediol, 1,3-butanediol, etc., can be derived from renewable resources.

[0035] The curable formaldehyde-free resin may further contain a catalyst. The catalyst can promote and / or accelerate the subsequent curing step. Typical examples of useful catalysts are phosphorus-containing esterification catalysts, such as alkali metal hypophosphites, alkali metal phosphites, and alkali metal polyphosphates. A preferred catalyst is sodium hypophosphite. The concentration of the catalyst in the formaldehyde-free resin of the present invention is preferably greater than 0.1% and / or less than 5% by weight, based on the sum of the weights of components (a) and (b) of the resin, and more preferably, the concentration of the catalyst is about 3% by weight. In a particular embodiment, the curable formaldehyde-free resin of the present invention contains sodium hypophosphite in an amount greater than 0.1% and less than 5% by weight, based on the sum of the weights of components (a) and (b) of the resin, and preferably in an amount of about 3% by weight.

[0036] The curable formaldehyde-free resin may further contain optional additives. Non-limiting examples of such additives are, among others, hydrophobizing agents such as silicone and fluorocarbon polymers, dust removers such as paraffin and mineral oil, fabric softeners, preservatives, dyes and / or corrosion inhibitors. The amount of these optional additives in the curable formaldehyde-free resin does not exceed 20% by weight, preferably does not exceed 10% by weight, of the total non-aqueous content of the curable formaldehyde-free resin.

[0037] The curable formaldehyde-free resin is in the form of an aqueous dispersion and the solids content may be in the range of 10 to 60% by weight, preferably in the range of 15 to 35% by weight.

[0038] The following summarizes some preferred embodiments of the present invention: (1) A curable formaldehyde-free resin according to any embodiment disclosed herein, comprising component (a) maltodextrin in the range of 60-70% by weight, component (b) citric acid in the range of 25-40% by weight, component (c) ethylene glycol, and component (d) epoxy silane. The amount of ethylene glycol, i.e., the total amount of polyols, is 0.5-2% by weight based on the total of maltodextrin and citric acid, and the amount of epoxy silane is 0.5% or more and less than 2% by weight based on the total of maltodextrin and citric acid. Preferably, the maltodextrin has a DE of 17-19. (2) A curable formaldehyde-free resin according to any embodiment disclosed herein, comprising component (a) maltodextrin in the range of 60-70% by weight, component (b) citric acid in the range of 25-40% by weight, component (c) one or more polyols having a molecular weight less than 1000 g / mol and having exactly two hydroxyl groups, and component (d) an epoxy silane. The total amount of the one or more polyols is 0.5-2% by weight based on the total of the maltodextrin and the citric acid, and the amount of the epoxy silane is 0.5% or more and less than 2% by weight based on the total of the maltodextrin and the citric acid. Preferably, the maltodextrin has a DE of 17-19. (3) A curable formaldehyde-free resin according to any embodiment disclosed herein, comprising component (a) maltodextrin in the range of 60-70% by weight, component (b) citric acid in the range of 25-40% by weight, component (c) ethylene glycol, and component (d) epoxy silane. The amount of ethylene glycol, i.e., the total amount of polyol, is 0.5-2% by weight based on the total of maltodextrin and citric acid, and the amount of epoxy silane is 0.1%-0.5% by weight based on the total of maltodextrin and citric acid. Preferably, the maltodextrin has a DE of 17-19. (4) A curable formaldehyde-free resin according to any embodiment disclosed herein, comprising component (a) maltodextrin in the range of 60-70% by weight, component (b) citric acid in the range of 25-40% by weight, component (c) one or more polyols having a molecular weight less than 1000 g / mol and having exactly two hydroxyl groups, and component (d) epoxy silane. The total amount of the one or more polyols is 0.5-2% by weight based on the total of the maltodextrin and citric acid, and the amount of the epoxy silane is 0.1%-0.5% by weight based on the total of the maltodextrin and citric acid. Preferably, the maltodextrin has a DE of 17-19.

[0039] In one aspect, a binder for mineral wool is provided that includes a curable formaldehyde-free resin according to the present disclosure. The binder includes a curable formaldehyde-free resin according to any of the embodiments of the present disclosure. Thus, the binder that includes the curable formaldehyde-free resin of the present invention can be cured at a temperature above 100°C. The binder of the present invention may be a formaldehyde-free aqueous binder. Typically, the binder contains the resin in a diluted form, i.e., the resin and additional water.

[0040] In a preferred embodiment, in addition to the resin, other additives described in the art can be incorporated for the preparation of the binder of the present invention. These additives are intended to aid in the manufacture of mineral wool products or to improve the properties of the manufactured products. Non-limiting examples of such additives are, among others, hydrophobizing agents such as silicone and fluorocarbon polymers, dedusting agents such as paraffin and mineral oil, fabric softeners, preservatives, dyes and / or corrosion inhibitors. The amount of these optional additives in the binder of the present invention does not exceed 20% by weight, preferably 10% by weight, of the total non-aqueous content of the binder. In a preferred embodiment, the binder composition of the present invention may contain at least one filler or resin extender, such as urea, sugars, molasses, lignosulfonates or tannins. Resin extenders are compounds added to the resin composition to "extend" the resin, thereby reducing the amount of resin used, reducing the total resin cost and, up to a certain concentration, not unacceptably deteriorating the final resin properties. The amount of optional fillers and / or resin extenders in the binder of the present invention does not exceed 20% by weight, preferably does not exceed 10% by weight, of the total non-aqueous content of the binder. The time between the contact of the binder additive with the resin and the application of the binder to the mineral fibers is usually in the range of 1 to 5 minutes. According to one embodiment, these additives may already be incorporated in the hardenable resin before the binder is prepared, as long as this does not impair stability. It is also preferred that the total amount of optional additives plus fillers or resin extenders in the binder of the present invention is not more than 30% by weight, even more preferably not more than 20% by weight, of the total non-aqueous content of the binder.

[0041] Based on the curable resins of the present disclosure, binders are obtained that have properties suitable for use in mineral wool products, in particular, the viscosity of the binders described above is sufficiently reduced to make them suitable for application to mineral wool.

[0042] Another aspect of the present invention relates to a mineral wool product comprising mineral fibers and a hardened binder, the hardened binder being obtained by curing the binder according to any of the embodiments of the present disclosure at a temperature above 100°C.

[0043] The mineral wool products of the present invention can be used, for example, in the thermal and acoustic insulation of buildings, vehicles or equipment, or for fire protection, as well as for other non-insulating applications.

[0044] One aspect of the present invention relates to a method for producing a curable formaldehyde-free resin according to one of the embodiments of the present disclosure. The method includes a step in which component (c) and component (d) are premixed. In a preferred embodiment, polycarboxylic acid (component (b)) is added to water under mechanical agitation. The premixed components (c) and (d) are then added to the aqueous mixture with continuous agitation. Subsequently, reducing sugar (component (a)) may be added to the aqueous mixture, and agitation is continued until the components are dissolved.

[0045] The process for producing the curable formaldehyde-free resin according to the present invention is preferably carried out at room temperature, ie, 20-25°C, preferably 25°C.

[0046] The present disclosure relates to the use of a curable formaldehyde-free resin according to any of the embodiments of the present disclosure for the manufacture of mineral wool products.

[0047] Mineral wool products can be produced by applying the binder of the invention to individual mineral fibers after fiberization while the fibers still retain some residual heat. Preferably, the binder is applied to the mineral fibers by spraying. The impregnated fibers are then collected on a perforated conveyor in a forming chamber, where the primary uncured mat is formed. Most of the water contained in the binder evaporates at this stage. Due to the specific composition of the resin of the invention, the viscosity of the resin and binder of the invention is particularly low. This allows, firstly, a more uniform distribution of the binder on the fibers and, secondly, a more efficient flow of the binder to the intersections of the fibers in the mat before curing. This produces mineral wool products with better properties.

[0048] The binder is applied in an amount that produces a solid binder content in the final product after drying and curing, preferably between 3 and 12% by weight based on the weight of the mineral wool product. This amount of cured binder is measured as LOI (loss on ignition) according to ISO 29771:2008.

[0049] After the fibers have been impregnated and the primary mat formed, the binder of the present invention is cured at a temperature above 100°C, preferably at a temperature between 140 and 180°C. The curing time is preferably in the range of 3 to 5 minutes. The cured mineral wool mat is then trimmed and formed to its final dimensions, and optionally rolled and packaged. Additional exterior layers such as paper, aluminum, glass veil or mixtures thereof may also be applied to the mineral wool depending on its intended use.

[0050] It is to be understood that other embodiments may be utilized and structural or logical changes may be made without departing from the scope of the present invention. Therefore, the specification is not to be construed in a limiting sense, and the scope of the present invention is defined by the appended claims. The described embodiments use specific language that should not be construed as limiting the scope of the appended claims. EXAMPLES

[0051] Different resin examples of the invention and comparative examples are described in this section and included in Tables 1 through 12. These examples are included to help explain the invention, but are not intended to be limiting.

[0052] The mechanical properties disclosed herein are measured on the resin after curing. However, the advantageous properties of the cured resins shown herein are a direct result of the composition of the curable resin itself. The curing process is carried out by conventional methods known to those skilled in the art.

[0053] In Tables 1, 4, 7 and 10, the amounts are given as relative ratios in weight percent. For ease of comparison, the relative weights are given such that the sum of component (a) and component (b) equals 100.

[0054] The raw materials used in the examples are as follows: - component (a): maltodextrin supplied by Roquette and having a DE of 19; - Component (b): Citric Acid supplied by Citrique Belge; - Component (c): Ethylene glycol (2 primary OH groups), tetraethylene glycol (2 primary OH groups), 1,4-butanediol (2 primary OH groups), glycerol (2 primary and 1 secondary OH groups), triglycerol (2 primary and 3 secondary OH groups), triethanolamine (3 primary OH groups), trimethylpropane (3 primary OH groups), poly(ethylene) glycol PEG-200 (2 primary OH groups), all supplied by Sigma-Aldrich. - Component (d): The "epoxy silane" used was (3-glycidyloxypropyl)trimethoxysilane (CAS number: 2530-83-8) supplied by OniChem Europe. - Added Ingredients: Sodium hypophosphite supplied by SMC Global.

[0055] Experiments were also carried out with aminosilane, component (d). The mechanical properties obtained by applying aminosilane-based fibres to a material and then curing were very poor compared to resins containing epoxysilanes.

[0056] Following this general procedure, different curable resins are prepared at room temperature. Citric acid is added to water under mechanical stirring. After this step, premixed epoxy silane and polyol are added to the aqueous mixture under continuous stirring. Subsequently, reducing sugar is incorporated into the aqueous mixture and stirring is continued until the ingredients are dissolved. The curable resin obtained by this method is in the form of a transparent, low-viscosity aqueous dispersion.

[0057] The curable resin is obtained with a solids content of approximately: - Examples 1-8 (Table 1), Examples 18-21 (Table 7), Examples 22-23 (Table 10): solids content 25%; - Examples 9 to 17 (Table 4): 20% solids.

[0058] A curable resin is then applied to the material and subsequently cured. The materials, details of the application of the binder to the material, and curing parameters are given in separate sections dedicated to the examples of Tables 1, 4, 7 and 10.

[0059] The following mechanical properties are measured experimentally: maximum load (given in units of N), Young's modulus (N / mm 2 The mechanical properties are evaluated in terms of the maximum slope (given in units of N / mm), the maximum slip (given in units of N / mm), and the maximum hardness (given in units of N / mm). The details of the experimental procedure for evaluating the mechanical properties are given in a separate section dedicated to the examples in tables 1, 4, 7 and 10. For all the examples presented herein, the mechanical properties were measured under two different experimental conditions, namely "dry conditions", immediately after the preparation of the samples, and "wet conditions", where the samples were exposed for one week in a climatic chamber at a temperature of 50° C. and a relative humidity of 95%. The measurements under "wet conditions" allow the evaluation of the product's ability to withstand weathering effects, i.e. the evaluation of the deterioration of the mechanical properties during ageing in environmental wet conditions.

[0060] Examples 1~9 The curable resins of Examples 1-8 were applied to glass microspheres. This type of experiment is a particularly difficult test of the mechanical properties of the curable resins, as the mechanical properties decrease dramatically when the glass microspheres are not integrated and have poor cohesion.

[0061] Mix 300 g of glass microspheres with an average diameter of 100-200 µm supplied by Abrasivos y Maquinaria SA with 60 g of hardenable resin (with a solids content of approximately 25%).

[0062] The mixture is then poured into a stainless steel mold to produce test specimens with dimensions 81 mm x 22 mm x 7 mm. The specimens are cured at 200°C for 25 minutes in a ventilated oven (Matis oven: Lab-dryer / coater type LTE / H-(TSM)). Half of the specimens are used to study the mechanical properties under "dry conditions" and the other half for "wet conditions".

[0063] The mechanical properties of the samples are examined by a tensile meter Instron 3367 by gradually applying a tensile force to each sample at a constant tensile speed of 5 mm / min. The resulting deformation of each sample subjected to stretching and the applied tensile force are both recorded. Strain-stress curves are obtained from the recorded deformations and applied forces. Examples 1-8 are characterized by determining the maximum load value of the strain-stress curve (maximum mechanical bond strength) and the maximum slope of the stress-strain curve.

[0064] Examples 1 and 2 are comparative examples lacking one of the essential components according to an embodiment of the present invention or having a weight ratio outside the range of the embodiment. Examples 3-8 are curable resins according to an embodiment of the present disclosure. Examples 2-8 were prepared using ethylene glycol as component (c).

[0065] The ingredients and their relative weight ratios for Examples 1-8 are shown in Table 1. Table 2 summarizes the maximum load values ​​obtained for Examples 1-8 under both "dry" and "wet" conditions. Table 3 summarizes the maximum tilt values ​​obtained for Examples 1-8 under both "dry" and "wet" conditions. Table 1: [Table 1]

[0066] In the following, reference is made to the maximum load values ​​given in Table 2. Examples 3 to 8 all result in high maximum load values ​​under dry conditions. Comparative Example 1 results in slightly inferior maximum load values ​​under dry conditions compared to Examples 3 to 8, while Comparative Example 2 results in maximum load values ​​under dry conditions comparable to some of Examples 3 to 8. The best results under dry conditions are obtained for Examples 3 and 4, both of which contain an amount of epoxy silane of 0.5 wt. % or less relative to the sum of components (a) and (b).

[0067] The difference between Examples 3-8 and the Comparative Example is noticeable under wet conditions. Comparative Example 1, which does not contain any epoxy silane, shows very low maximum load values, i.e. the mechanical properties are significantly worse in the absence of epoxy silane and therefore no aggregation of glass microspheres occurs. Epoxy silane has a clear positive effect in maintaining adhesion under accelerated humidity and temperature aging conditions. Comparative Example 2 also shows significantly poorer maximum load values ​​under "wet conditions". All maximum load values ​​of Examples 3-8 exceed the maximum load value of Comparative Example 2 by more than 50%. The best results under "wet conditions" are obtained for Examples 7 and 8, both of which contain an amount of component (c) of 2 wt. % or less relative to the sum of components (a) and (b). Table 2: [Table 2]

[0068] In the following, reference is made to the maximum slope values ​​shown in Table 3. Examples 3-8 all provide high maximum slope values ​​under dry conditions. Comparative Example 1 provides slightly inferior maximum load values ​​under dry conditions compared to Examples 3-8, while Comparative Example 2 provides maximum load values ​​under dry conditions comparable to some of Examples 3-8.

[0069] Under wet conditions, the differences between Examples 3-8 and the Comparative Examples are again striking. Comparative Example 1, which does not contain epoxysilane, shows a very low maximum slope value, i.e., the mechanical properties are dramatically deteriorated in the absence of epoxysilane and therefore no adhesion of the glass microspheres occurs. Comparative Example 2 also shows a significantly poorer maximum slope value under "wet conditions". Table 3: [Table 3]

[0070] Examples 9~17 The curable resins of Examples 9-17 were applied to glass paper on a laboratory scale.

[0071] A 21 x 14.85 cm piece of borosilicate GF / A filter paper (20.3 x 25.4 cm, Catalogue No. 1820 866, Whatman International, Maidstone, UK) is immersed for 1 minute in 100 g of hardenable resin (with a solids content of about 20%). The impregnated glass paper is then passed through a calendar roller (2.5 bar pressure between the rollers and a roller speed of 2.5 m / min). The sample is then dried on leaving the calendar roller and cured for 3 minutes at 170 °C in a ventilated oven. The sample is then divided into 12 pieces of 25 mm x 75 mm. Six of these pieces are used to investigate the mechanical properties under "dry conditions" and the other six are used to test under "wet conditions".

[0072] The mechanical properties of the samples are examined by a tensile meter Instron 3367 by gradually applying a tensile force to each sample at a constant tensile speed of 10 mm / min. The resulting deformation of each sample subjected to stretching and the applied tensile force are both recorded. The strain-stress curve of each individual sample is obtained from the recorded deformation and applied force. Examples 10-16 are characterized by determining the maximum load value (maximum mechanical bond strength) of the strain-stress curve and the Young's modulus of the stress-strain curve.

[0073] Example 9 is a comparative example lacking components (c) and (d). Example 10 is a comparative example lacking component (c). Examples 11-17 all correspond to inventive embodiments of a curable resin. The relative weight ratios are the same in all of Examples 11-17, but each of Examples 11-17 contains a different component (c).

[0074] The ingredients and their relative weight ratios for Examples 9-17 are shown in Table 4. Table 5 summarizes the maximum load values ​​obtained for Examples 9-17 under both "dry" and "wet" conditions. Table 6 summarizes the Young's modulus values ​​obtained for Examples 9-17 under both "dry" and "wet" conditions. Table 4: [Table 4]

[0075] In the following, reference is made to the maximum load values ​​given in Table 5. The maximum load values ​​are significantly improved for Examples 11-17 of the invention compared to Comparative Example 9 under both "dry" and "wet" conditions. Furthermore, the examples of the invention show an increase in the maximum load under dry conditions with respect to the comparable Example 10, i.e. an improvement over a curable resin without polyol and a large amount of epoxy silane. The highest maximum load values ​​are obtained for Examples 11-13. In Examples 11-13 a polyol containing two OH groups is used, whereas Examples 14-17 contain a polyol with more than two OH groups. Table 5: [Table 5]

[0076] Reference is made below to the Young's Modulus values ​​shown in Table 6. The inventive examples also show increased Young's Modulus compared to non-inventive Example 10, i.e., an improvement over a curable resin that does not contain a polyol and a large amount of epoxy silane. Table 6: [Table 6]

[0077] Examples 18~21 The curable resins of Examples 18 to 21 were applied to glass microspheres. The experimental details, i.e., preparation of the microspheres, fabrication of test specimens, curing, and testing of mechanical properties, were carried out in the same manner as described above in connection with Examples 1 to 8.

[0078] Example 18 is a comparative example lacking components (c) and (d). Examples 19-21 all correspond to inventive embodiments of a curable resin. Although the relative weight ratios are the same in all of Examples 19-21, each of Examples 19-21 contains a different component (c).

[0079] The ingredients and their relative weight ratios for Examples 18-21 are shown in Table 7. Table 8 summarizes the maximum load values ​​obtained for Examples 18-21 under both "dry" and "wet" conditions. Table 9 summarizes the maximum tilt values ​​obtained for Examples 18-21 under both "dry" and "wet" conditions. Table 7: [Table 7]

[0080] In the following, reference is made to the maximum load values ​​shown in Table 8. Examples 19-21 all provide high maximum load values ​​under "dry conditions" and "wet conditions". Comparative Example 18 has a poorer maximum load value under dry conditions compared to the examples of the present invention, which is even more pronounced under "wet conditions". Table 8: [Table 8]

[0081] In the following, reference is made to the maximum slope values ​​given in Table 9. All of the inventive examples 19-21 result in high maximum slope values ​​under dry conditions. Comparative example 18 results in maximum slope values ​​comparable to some of the examples 19-21 under dry conditions. The difference between the inventive examples and the comparative examples is noticeable under wet conditions. Comparative example 18, which does not contain any epoxy silane, shows a very low maximum slope value under wet conditions, i.e. the mechanical properties are significantly worse in the absence of epoxy silane and therefore no adhesion of the glass microspheres occurs. The epoxy silane has a clear positive effect in maintaining the adhesion under accelerated humidity and temperature aging conditions. The best results under "wet conditions" are obtained when component (c) is ethylene glycol (example 19). Table 9: [Table 9]

[0082] Example 22~23 The curable resins of Examples 22-23 were applied to glass microspheres. This type of experiment is a particularly difficult test of the mechanical properties of the curable resin because the mechanical properties decrease dramatically when the glass microspheres are not integrated and have poor cohesion.

[0083] Mix 300 g of glass microspheres with an average diameter of 100-200 µm supplied by Abrasivos y Maquinaria SA with 60 g of hardenable resin (with a solids content of approximately 25%).

[0084] The mixture is then poured into a stainless steel mold to produce test specimens with dimensions 81 mm x 22 mm x 7 mm. The specimens are cured at 200°C for 25 minutes in a ventilated oven (Matis oven: Lab-dryer / coater type LTE / H-(TSM)). Half of the specimens are used to study the mechanical properties under "dry conditions" and the other half for "wet conditions".

[0085] The mechanical properties of the samples are examined by a tensile meter Instron 3367 by gradually applying a tensile force to each sample at a constant tensile speed of 5 mm / min. The resulting deformation of each sample subjected to stretching and the applied tensile force are both recorded. A strain-stress curve is obtained from the recorded deformation and applied force. Examples 22 and 23 are characterized by determining the maximum load value of the strain-stress curve (maximum mechanical bond strength) and the maximum slope of the stress-strain curve.

[0086] Example 22 is a comparative example lacking component (c) (polyol) and including an epoxy silane with a weight ratio outside the range of embodiments of the present disclosure. Example 23 is a curable resin according to embodiments of the present disclosure. Example 23 was prepared using component (c) of poly(ethylene) glycol (PEG-200).

[0087] The ingredients and their respective relative weight ratios for Examples 22 and 23 are shown in Table 10. Table 11 summarizes the maximum load values ​​obtained for Examples 22 and 23 under both "dry" and "wet" conditions. Table 12 summarizes the maximum tilt values ​​obtained for Examples 22 and 23 under both "dry" and "wet" conditions. Table 10: [Table 10]

[0088] See the maximum load values ​​shown in Table 11. Comparative Example 22 *shows lower maximum load values ​​under "wet conditions" compared to Example 23. Table 11: [Table 11]

[0089] See the maximum slope values ​​shown in Table 12. Comparative Example 22 * exhibited a lower maximum slope value under "wet conditions" compared to Example 23, i.e., Comparative Example 22 * The mechanical properties of deteriorate under wet conditions and therefore the adhesion of glass microspheres is poor. Table 12: [Table 12]

Claims

1. A curable formaldehyde-free resin comprising the following components in the form of an aqueous dispersion: Component (a) maltodextrin having a DE of 11 to 21; Component (b) polycarboxylic acid, Component (c) one or more polyols having a molecular weight of less than 1000 g / mol (excluding reducing sugars); and Component (d) epoxy silane, Here, the total amount of component (c) in the curable formaldehyde-free resin is 0.5 to 10% by weight based on the total of components (a) and (b), and the amount of component (d) is 0.1 to 2% by weight based on the total of components (a) and (b).

2. 2. The curable formaldehyde-free resin of claim 1, wherein component (b) is selected from citric acid, succinic acid, tartaric acid, adipic acid, anhydrides and salts thereof, and combinations thereof.

3. The curable formaldehyde-free resin of any one of claims 1 to 2, wherein component (b) is citric acid.

4. 4. The curable formaldehyde-free resin of claim 1, wherein component (a) is a maltodextrin having a DE of 17-19 and component (b) is citric acid.

5. 5. The curable formaldehyde-free resin of any one of claims 1 to 4, comprising 50 to 80% by weight of maltodextrin and 20 to 50% by weight of citric acid.

6. 6. The curable formaldehyde-free resin of claim 1, comprising 60-70% by weight of maltodextrin and 25-40% by weight of citric acid.

7. 7. The curable formaldehyde-free resin of any one of claims 1 to 6, wherein component (c) is selected from ethylene glycol, tetraethylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerol, diglycerol, triglycerol, triethanolamine, diethanolamine, trimethylolpropane, propylene glycol, poly(ethylene) glycol, and combinations thereof.

8. The curable formaldehyde-free resin of any one of claims 1 to 7, wherein component (c) is ethylene glycol.

9. 9. The curable formaldehyde-free resin according to claim 1, wherein the total amount of component (c) in the curable formaldehyde-free resin is 1 to 6 wt. %, based on the sum of components (a) and (b).

10. 10. The curable formaldehyde-free resin according to claim 1, wherein the total amount of component (c) in the curable formaldehyde-free resin is 2 to 5 wt. % relative to the sum of components (a) and (b).

11. 11. The curable formaldehyde-free resin according to claim 1, wherein the total amount of component (c) in the curable formaldehyde-free resin is 3 to 4 wt. % relative to the sum of components (a) and (b).

12. 10. The curable formaldehyde-free resin according to claim 1, wherein the total amount of component (c) in the curable formaldehyde-free resin is 1 to 2 wt. % relative to the sum of components (a) and (b).

13. 13. The curable formaldehyde-free resin according to claim 1, wherein the amount of component (d) is 0.1% by weight or more and less than 2% by weight, based on the sum of components (a) and (b).

14. 14. The curable formaldehyde-free resin according to any one of claims 1 to 13, wherein the amount of component (d) is from 0.2% to 1.5% by weight, based on the sum of components (a) and (b).

15. 15. The curable formaldehyde-free resin according to any one of claims 1 to 14, wherein the amount of component (d) is from 0.4% to 1% by weight, based on the sum of components (a) and (b).

16. 16. The curable formaldehyde-free resin according to any one of claims 1 to 15, wherein the amount of component (d) is from 0.5% to 0.8% by weight, based on the sum of components (a) and (b).

17. 15. The curable formaldehyde-free resin according to any one of claims 1 to 14, wherein the amount of component (d) is 0.2 to 0.5 wt. %, based on the sum of components (a) and (b).

18. 2. The curable formaldehyde-free resin of claim 1, wherein the resin comprises the following components: Component (a) 60-70% by weight of maltodextrin having a DE of 17-19; Component (b) 25 to 40% by weight of citric acid; Component (c) ethylene glycol, and Component (d) epoxy silane, Here, the amount of ethylene glycol is 0.5 to 2% by weight based on the total weight of the maltodextrin and citric acid, and the amount of epoxy silane is 0.5% by weight or more and less than 2% by weight based on the total weight of the maltodextrin and citric acid.

19. A method for producing the curable formaldehyde-free resin of any one of claims 1 to 18, comprising the step of premixing component (c) and component (d).

20. A binder for mineral wool comprising the curable formaldehyde-free resin according to any one of claims 1 to 18.

21. 21. A mineral wool product comprising mineral fibers and a cured binder, the cured binder being obtained by curing the binder of claim 20 at a temperature above 100°C.

Citation Information

Patent Citations

  • Binders and materials made therewith

    AU2015202521A1

  • Formaldehyde-free binders and mineral wool insulation products

    JP2015527431A

  • Binder composition for mineral wool

    JP2017508898A

  • Sizing composition based on non-reducing and hydrogenated sugars and resulting insulation product

    JP2017514029A