Packaging laminates

The packaging laminate addresses the issues of low-temperature impact resistance and heat resistance in CPP films by using a polypropylene-based structure with specific viscoelastic properties, ensuring durability and recyclability.

JP7589472B2Active Publication Date: 2024-11-26TOYO SEIKAN GRP HLDG LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020153225
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-11
Publication Date
2024-11-26
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Existing CPP films used for retort pouches lack sufficient low-temperature impact resistance, heat resistance for microwave heating, and recyclability, posing challenges in maintaining structural integrity and environmental sustainability.

Method used

A packaging laminate structure comprising a stretched polypropylene base film, a propylene heat seal film with specific viscoelastic properties, and an adhesive layer, utilizing a blend of impact polypropylene and linear low-density polyethylene, with additional layers for reinforcement and gas barrier properties.

Benefits of technology

The laminate exhibits excellent impact resistance at low temperatures, maintains seal strength during microwave heating, and is highly recyclable due to its predominantly propylene-based composition, ensuring durability and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589472000002
    Figure 0007589472000002
  • Figure 0007589472000003
    Figure 0007589472000003
  • Figure 0007589472000004
    Figure 0007589472000004
Patent Text Reader

Abstract

To provide a packaging layered body excellent in low-temperature impact resistance, suitability to microwave heating, and recyclability.SOLUTION: A packaging layered body 10 has a structure obtained by stacking a base film 1 and a heat seal film 5 with an adhesive layer 3 sandwiched therebetween. A stretched polypropylene film is used as the base film 1. A propylene-based film is used as the heat seal film 5. In the propylene-based film, the loss tangent (tan δ) at 5°C in dynamic viscoelasticity test measurement exceeds 0.0594, and the storage elastic modulus (E') at 110°C exceeds 1 MPa.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging laminate, and more particularly to a packaging laminate with high recyclability that is suitable for producing pouches by attachment through heat sealing. [Background technology]

[0002] CPP film (also called non-oriented polypropylene film or cast PP film) made of polypropylene and having heat sealability has excellent heat resistance and is used to make pouches for storing various foods, etc. In recent years, however, impact polypropylene (hereinafter sometimes referred to as impact PP) has come to be used to make CPP film because of the demand for higher heat resistance and impact resistance for retort sterilization (heated steam sterilization) and the like.

[0003] Impact PP, also known as block PP, impact copolymer, or high impact polypropylene, consists of rubber components such as ethylene-propylene copolymer (EPR) or styrene-butadiene copolymer (SBR) dispersed in a matrix of homopolypropylene or random polypropylene. The dispersion of these rubber components significantly improves impact resistance.

[0004] CPP films used to make pouches for retort sterilization are required to have properties such as heat seal strength and impact resistance, as well as blocking resistance and yuzu peel resistance. That is, it goes without saying that blocking resistance is necessary to prevent blocking when films are stacked together, but when the film is subjected to heated steam sterilization such as retort sterilization, the oil contained in the contents may seep into the film, causing the pouch to deform like yuzu peel, so it is also necessary to prevent such yuzu peel-like deformation. The film formed from the above-mentioned impact PP has poor blocking resistance and yuzu peel resistance, so it needs to be modified.

[0005] Various means for improving the above-mentioned properties have been proposed. For example, Patent Documents 1 and 2 propose a propylene-based resin composition in which a propylene-based impact copolymer (corresponding to impact PP) is blended with linear low-density polyethylene (LLDPE), and disclose that such a resin composition can provide a heat-sealable film having various excellent properties.

[0006] In Patent Documents 1 and 2, the physical properties of a heat-sealable film made of impact PP are improved by blending linear low-density polyethylene with impact PP. For example, a pouch is made using this film, and when the pouch is filled with the contents and stored at a temperature of 5°C, and then a bag drop test is performed from an arbitrary height, the pouch shows good low-temperature impact resistance.

[0007] Incidentally, in recent years, retort pouches are often heated using a microwave oven for convenience. Furthermore, this pouch is provided with a mechanism for releasing steam generated from the contents by heating from inside the pouch. This steam release mechanism suppresses excessive pressure buildup inside the pouch and prevents the pouch from breaking. However, as in Patent Documents 1 and 2, when a CPP film containing a large amount of a rubber dispersion or linear low-density polyethylene, which has lower heat resistance than polypropylene, is used, the seal around the pouch may peel off regardless of the presence or absence of a steam release mechanism, which may lead to the pouch breaking.

[0008] Furthermore, due to the recent growing awareness of environmental conservation and effective use of resources, there is a demand to reconsider the film material of retort pouches. In other words, from the viewpoint of recyclability, pouches made of a single material are more desirable than pouches made of different materials, such as the current combination of PET film, Ny film, aluminum foil, CPP film, etc. As for the material, it is desirable to make the pouch out of polypropylene-based resin because of its properties such as heat sealability and heat resistance. Therefore, in order to improve recyclability, it is necessary to realize the impact resistance, etc. that has been achieved with different materials in polypropylene-based resin.

[0009] When the film material for retort pouches is made of polypropylene resin, the CPP film is required to have low-temperature impact resistance and other properties that are greater than ever before. However, it is difficult to achieve both low-temperature impact resistance and heat resistance. For these reasons, the current situation is that conventional CPP films and film configurations for retort pouches lack either low-temperature impact resistance, heat resistance to withstand microwave heating, or recyclability. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 4844091 [Patent Document 2] WO2017 / 038349 issue Summary of the Invention [Problem to be solved by the invention]

[0011] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a packaging laminate which has excellent recyclability as well as low-temperature impact resistance and suitability for microwave heating. Another object of the present invention is to provide a retort pouch obtained from the above-mentioned packaging laminate. [Means for solving the problem]

[0012] According to the present invention, in a packaging laminate having a structure in which a base film and a heat seal film are laminated with an adhesive layer sandwiched therebetween, A stretched polypropylene film is used as the base film, A propylene-based film is used as the heat seal film, The propylene-based film used as the heat seal film has a loss tangent (tan δ) of more than 0.0594 at 5°C and a storage modulus (E') of more than 1 MPa at 110°C, as measured by a dynamic viscoelasticity test.

[0013] The following aspects are preferably applied to the packaging laminate of the present invention. (1) The propylene-based film is formed from a cast film containing an impact polypropylene component. (2) The cast film contains an impact polypropylene component (A) in which an ethylene-propylene copolymer is dispersed in polypropylene, and a linear low-density polyethylene (B). (3) The cast film contains 8% by mass or more of a xylene soluble fraction derived from an ethylene-propylene copolymer. (4) The cast film contains the linear low-density polyethylene (B) in an amount of 20 mass% or less. (5) The adhesive layer is formed from a dry lamination adhesive. (6) A stretched film containing at least one selected from an olefin resin, a polyamide resin, and an ethylene-vinyl alcohol copolymer is laminated separately from the base film. (7) The olefin-based resin is polypropylene.

[0014] The present invention also provides a pouch comprising the above-mentioned packaging laminate. Effect of the Invention

[0015] The packaging laminate of the present invention has a basic structure in which a base film and a heat seal film are laminated via an adhesive layer, but in addition to this basic structure, the propylene-based film used as the heat seal film has dynamic viscoelastic properties, specifically, an important feature in that the loss tangent (tan δ) at 5° C. exceeds 0.0594 and the storage modulus (E') at 110° C. exceeds 1 MPa in dynamic viscoelasticity test measurements. That is, since the propylene-based film has the above-mentioned viscoelastic properties, the packaging laminate of the present invention not only exhibits excellent impact resistance even when subjected to heat treatment such as retort sterilization, but also has excellent impact resistance even in a low temperature range of about 5° C., and can ensure a seal strength that can withstand microwave heating. For example, as shown in the examples described later, in a pouch made from a laminate having a loss tangent (tan δ) and a storage modulus (E') of a propylene-based film (heat seal film) within the above range, the number of times that the pouch was horizontally broken in an environment of 5°C was at least 19 times (Example 2), and the seal strength at 110°C was at least 15N (Example 1), despite the retort treatment. On the other hand, in Comparative Example 3, in which the loss tangent (tan δ) is 0.059, which is smaller than 0.0594, the number of times that the pouch was horizontally broken in an environment of 5°C was 7 times, which is smaller than Examples 1 and 2, and the impact resistance at low temperatures is poor. In Comparative Example 2, in which the storage modulus E' is less than 1 MPa, the seal strength at 110°C was 4N, which is extremely small compared to Examples 1 and 2, and the seal strength at high temperatures is small, and it cannot be applied to microwave oven heating, for example.

[0016] Another important feature of the present invention is that an oriented polypropylene (OPP) film is used as the base film. That is, by using an OPP film as the base film, most of the main materials used in this packaging laminate are propylene-based materials, and as a result, this packaging laminate has excellent recyclability. [Brief description of the drawings]

[0017] [Figure 1]FIG. 1 is a diagram showing a schematic cross-sectional structure of a packaging laminate of the present invention. [Diagram 2] FIG. 2 is a diagram showing the loss tangent (tan δ) temperature curve (10 Hz) obtained by measuring the dynamic viscoelasticity of the propylene-based films used in the examples and comparative examples. [Diagram 3] FIG. 2 is a graph showing the storage modulus curve (E′) temperature curve (10 Hz) obtained by dynamic viscoelasticity measurement of the propylene-based films used in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] 1, a packaging laminate 10 of the present invention generally designated by 10 has a laminate structure including a base film 1, an adhesive layer 3, and a heat seal film 5. Simply put, the structure has a base film 1 and a heat seal film 5 laminated together with an adhesive.

[0019] <Base film 1> A stretched polypropylene film (hereinafter sometimes referred to as OPP film) is used as the base film 1. This OPP film is a film obtained by stretching a propylene-based resin film produced by a known means such as extrusion molding in a uniaxial or biaxial direction. This ensures the drop strength, puncture strength, and rigidity of the pouch. The stretching ratio may be such that the film does not break due to overstretching, and is usually 2 times or more.

[0020] Furthermore, the propylene-based resin used to form the OPP film is typically polypropylene (a homopolymer of propylene), but may also be a random or block copolymer in which an α-olefin such as ethylene, 1-butene, or 4-methyl-1-pentene or a cyclic olefin is copolymerized, so long as the properties of the polypropylene are not impaired.

[0021] The thickness of the base film 1 formed from the above-mentioned OPP film is appropriately determined depending on the capacity of the pouch to be finally produced, but generally, it is sufficient for the thickness to be 10 μm or more.

[0022] In addition, in order to improve the gas barrier property, the above-mentioned base film 1 may be laminated with a gas barrier resin such as an ethylene-vinyl alcohol copolymer, an inorganic coating may be formed on the surface, or an organic material such as polyvinyl alcohol may be formed. The inorganic coating may be formed by coating or may be a vapor deposition film. Such a gas barrier resin layer is formed by attaching a gas barrier resin film using an adhesive such as dry lamination. In addition, the vapor deposition film is an inorganic vapor deposition film formed by physical vapor deposition such as sputtering, vacuum deposition, and ion plating, or chemical vapor deposition such as plasma CVD, and is formed from various metals or metal oxides such as silicon oxide and aluminum oxide. Such a vapor deposition film is formed from an inorganic material, and therefore exhibits higher oxygen barrier property than gas barrier resins such as ethylene-vinyl alcohol copolymer.

[0023] When the gas barrier resin layer or inorganic coating as described above is formed on a base film 1 made of a propylene-based resin, the heat seal film 5 described later may be attached to the gas barrier resin layer or inorganic coating via the adhesive layer 3, or may be attached to the base film 1 side.

[0024] In addition, the oriented polypropylene film (OPP film) used as the base film 1 may relax its oriented structure due to the effect of heat such as heat sealing, which may lead to a decrease in the drop strength. Therefore, in order to prevent the decrease in strength, it is preferable to provide a stretched film layer containing at least one selected from olefin resins, polyamide resins, and ethylene-vinyl alcohol copolymers as a strength reinforcing layer. Such a strength reinforcing layer is intended to mitigate the loss of orientation due to heat treatment such as heat sealing, and to effectively suppress the decrease in strength.

[0025] Such a strength reinforcing layer is a stretched molded product of a blend or laminate of an olefin resin and a reinforcing resin having a higher melting point than the olefin resin. In particular, a stretched film of a blend of an olefin resin and a polyamide resin or an ethylene-vinyl alcohol copolymer is preferred, and the mass ratio of the olefin resin to the reinforcing resin is usually in the range of about 50:50 to 90:10. That is, if the amount of the reinforcing resin is excessively large, the strength reinforcing effect is excellent but the recyclability is low, and if the amount of the reinforcing resin is small, the strength reinforcing effect of this layer is impaired.

[0026] In addition, as the olefin-based resin used to form the above-mentioned strength reinforcement layer, the same type of resin as the propylene-based resin used to form the stretched polyolefin film used as the above-mentioned base film 1, particularly polypropylene, is optimal for (improving) recyclability. The polyamide resin to be blended with the olefin resin is not particularly limited and various types can be exemplified. In general, nylon 6, nylon 6,6, nylon 11, nylon 12, nylon 13, nylon 6 / nylon 6,6 copolymer, aromatic nylon (e.g., polymetaxylylene adipamide), amorphous nylon (e.g., nylon 6I / nylon 6T), etc. are preferably used.

[0027] The strength reinforcing layer may have a laminated structure in which an olefin resin layer and a reinforcing resin layer are laminated. In such a laminated structure, the thickness ratio of the olefin resin layer to the reinforcing resin layer is usually in the range of about 1 / 1 to 3 / 1. That is, if the thickness of the reinforcing resin is too large, the recyclability of the packaging bag is greatly lost, and if the amount of the reinforcing resin is small, the amount of oriented crystals present in the seal portion is small, and there is a risk that the improvement of the drop strength of the bag will be insufficient.

[0028] The strength reinforcing layer may be formed by co-extrusion of the blend and stretching, or by multi-layer extrusion stretching. The strength reinforcing layer may be formed by stretching in a uniaxial or biaxial direction. In addition, the strength reinforcing layer may be formed by co-extrusion of the blend or multi-layer when forming the base film 1, and stretching the co-extruded film in a uniaxial or biaxial direction.

[0029] The thickness of the strength reinforcing layer is not particularly limited, and may be appropriately set to the thickness of the base film 1, which is set depending on the target pouch capacity, etc. In general, the thickness is preferably 5 μm or more, and is particularly preferably in the range of about 5 to 30 μm.

[0030] The above-mentioned strength reinforcing layer may be provided between the base film 1 and the heat seal film 5, or may be provided on the outer side of the base film 1.

[0031] The adhesive used for laminating the above-mentioned strength reinforcing layer onto the base film 1 or the like is the same type of adhesive as that used for the adhesive layer 3 described below.

[0032] <Adhesive layer 3> The adhesive layer 3 is a layer formed using an adhesive, and the heat seal film 5 is laminated onto the base film 1 using this adhesive.

[0033] As such an adhesive, a known dry lamination adhesive such as a so-called dry lamination adhesive, for example, a urethane-based adhesive or an epoxy-based adhesive, can be used.

[0034] For example, a urethane-based dry lamination adhesive may be one made of a reaction product of isocyanate with a (meth)acrylic compound or polyester polyol. This adhesive usually contains a known curing catalyst such as an amine catalyst, a metal catalyst, or a phosphoric acid-modified compound. The amount of the curing catalyst is set according to the type of curing catalyst so that a dense cured film (adhesive layer) can be formed at a temperature and for a time that does not cause thermal deformation of the underlying resin.

[0035] The epoxy adhesive contains a liquid resin having an epoxy group in its molecule and an epoxy curing agent. Representative liquid resins having epoxy groups in the molecule include those obtained by reacting epichlorohydrin with a phenol compound, an amine compound, or a carboxylic acid, and those obtained by oxidizing an unsaturated compound such as butadiene with an organic peroxide, and any type of resin can be used. Specific examples include bisphenol A or bisphenol F epoxy resins, novolac epoxy resins, cyclic aliphatic epoxy resins, long-chain aliphatic epoxy resins, glycidyl ester epoxy resins, and glycidyl amine epoxy resins. As the epoxy curing agent, known agents such as amines, acid anhydrides, polyamides, etc. can be used, but aromatic polyamines such as metaphenylenediamine are particularly preferred.

[0036] The ratio of the amounts of the epoxy resin and the curing agent may be set according to the epoxy equivalent of the epoxy resin so that a sufficient cured film is formed.

[0037] The above-mentioned urethane-based or epoxy-based dry lamination adhesive is applied to the surface of the above-mentioned propylene resin-based base film 1 in the form of a coating liquid in which it is dissolved or dispersed in a volatile organic solvent such as a hydrocarbon, alcohol, ketone, ester, or ether solvent. The adhesive is then dried to volatilize the organic solvent, after which a heat-sealing film (described below) is attached, and the heat-sealing film can be adhered and fixed by heating and curing. The thickness of the adhesive layer 3 thus formed is usually about 0.1 to 10 μm.

[0038] In the above-mentioned dry laminate adhesive, when a vapor deposition film is formed on the surface of the base film 1 (OPP film), when a heat seal film 5 or the like is attached onto it, an epoxy-based dry laminate adhesive is advantageous in avoiding a decrease in gas barrier properties due to retort treatment. The dry lamination adhesive is also used for forming the multi-layer strength reinforcement described above, that is, for laminating an olefin resin-based stretched film and a polyamide resin-based stretched film.

[0039] <Heat seal film 5> The heat seal film 5 is laminated onto the above-mentioned base film 1 by placing the film 5 on the coating layer of the adhesive and pressing it, and then heating and curing the adhesive in this state. The heat seal film 5 melts easily when heated and immediately solidifies when cooled, and this fact can be utilized to thermally bond (heat seal) the laminates 10 (heat seal films 5) together to produce a pouch.

[0040] In the present invention, the heat seal film 5 is a propylene-based film having dynamic viscoelastic properties, and the loss tangent (tan δ) at 5°C in dynamic viscoelasticity measurement at 10 Hz exceeds 0.0594. That is, by having such viscoelasticity at 5°C, the heat seal film 5 in the packaging laminate 10 exhibits good low-temperature impact resistance in the low-temperature range (around 5°C) and is very difficult to break. In addition, the heat seal film 5 must have a storage modulus (E') at 110°C in dynamic viscoelasticity measurement at 10 Hz of more than 1 MPa. That is, by having such a large value of storage modulus E' at 110°C, the heat seal film 5 exhibits appropriate elasticity in the high-temperature range (around 110°C) and maintains sufficient seal strength to seal a pouch even at high temperatures. Therefore, the pouch obtained from this laminate 10 has high seal strength at high temperatures, effectively prevents seal destruction due to microwave heating, and enables effective microwave heating.

[0041] In the present invention, the heat seal film 5 (propylene-based film) having the above-mentioned viscoelasticity is obtained by using a cast film containing impact polypropylene (impact PP) (hereinafter simply abbreviated as CPP film) and adjusting the composition of the impact PP and the type and amount of the modified resin component used in combination.

[0042] That is, the CPP film having the above-mentioned viscoelasticity is obtained by melt extrusion of a resin composition containing an impact PP component (A) and a modifying resin component (B).

[0043] Impact PP component (A); The impact PP component (A) is made of impact polypropylene (impact PP), and this impact PP has a structure in which ethylene-propylene copolymer (EPR) is dispersed in homo- or random polypropylene. In other words, the dispersion of EPR in polypropylene gives impact resistance to the polypropylene. In addition to EPR, styrene-butadiene copolymer (SBR) and ethylene-propylene-butene copolymer (EPBR) are also known as rubber components dispersed in polypropylene. Although those other than EPR can improve the low-temperature impact resistance (tan δ at 5°C greater than 0.0594) that is the objective of the present invention, EPR is the most suitable.

[0044] From the viewpoint of film formability (extrusion formability) and the like, the above-mentioned impact PP has an MFR (melt flow rate, 230° C.) in the range of about 0.5 to 10 g / 10 min.

[0045] The EPR content in the impact PP can be expressed by the xylene soluble content of the CPP film used to form the heat seal film 5. The xylene soluble content is the proportion of components that do not precipitate when the impact PP resin is completely dissolved in boiling xylene and the xylene solution is cooled to room temperature. It is preferable that the xylene soluble content is 8% by mass or more, particularly in the range of 8 to 20% by mass. That is, if the xylene soluble content is smaller than the above range, the amount of EPR is small, and the impact resistance of the pouch decreases. If the soluble content is excessively high, the heat resistance of the pouch decreases, and further, the pouch may have a poor appearance.

[0046] Furthermore, the intrinsic viscosity (measured using tetralin at 135°C as a solvent) of the xylene soluble fraction (EPR) is preferably in the range of 1.0 to 2.9 dl / g. This intrinsic viscosity is a parameter corresponding to the molecular weight of the EPR in the impact PP. If this value is outside the above range, the impact resistance tends to be unsatisfactory. This is probably because the size of the EPR molecule is larger or smaller than necessary, and therefore the properties of the modifying resin component (B) described below are not fully exhibited.

[0047] Modified resin component (B); This modifying resin component (B) is a component that enhances the compatibility between the polypropylene (PP) and ethylene-propylene copolymer (EPR) in the above-mentioned impact PP, greatly improving the dispersibility of the EPR in the PP, thereby enabling the EPR to fully exert its impact property improving effect.

[0048] In the present invention, linear low density polyethylene (LLDPE) is preferably used as the modifying resin component (B). This LLDPE has a density of 0.860 to 0.925 g / cm 3 It is a linear low-density polyethylene in the range of 0.1 to 1.0 mm, and its density is reduced by copolymerizing a small amount (a few percent) of an α-olefin such as butene-1, hexene-1, or 4-methylpentene-1 with ethylene, and its molecular linearity is extremely high.

[0049] Moreover, since this LLDPE is used by being mixed with impact PP, in order not to impair film formability, one having an MFR (190° C.) of 1.0 to 15 g / 10 min is preferably used.

[0050] Furthermore, it is preferable that the LLDPE has a comonomer α-olefin content of 12 mol% or less and a polystyrene-equivalent number average molecular weight of 10,000 or more as measured by GPC. In other words, if the comonomer α-olefin content is high or if the number average molecular weight is low and a large amount of low molecular weight components are included, the oil resistance and flavor of the contents will be poor when used as a pouch. In addition, a part of the LLDPE may dissolve in xylene, and the xylene-soluble content in the molded film may not correspond to the EPR derived from the impact PP.

[0051] The above-mentioned LLDPE is preferably designed in the film composition so that the amount of LLDPE in the CPP film (corresponding to the amount of LLDPE in the heat-sealable resin layer 5) is 20 mass % or less. In other words, if an excessive amount of LLDPE is contained, the blocking resistance and heat resistance of the film may be impaired.

[0052] The resin composition used to form the CPP film may contain additives that are known per se.

[0053] The CPP film containing the above-mentioned impact PP components is produced by dry blending the components, feeding them into an extruder to melt-knead them, melt-extruding the blend into a film from a T-die, bringing the extruded molten film into contact with a cooling roll to solidify it, and winding it up. There are no particular limitations on the thickness of such a CPP film, but taking into consideration the rigidity, ease of opening, and the like, it is usually suitable to have a thickness in the range of 20 to 100 μm, particularly 50 to 80 μm.

[0054] The packaging laminate 10 of the present invention obtained by laminating the above-mentioned layers or films may have, for example, a printed layer or a transparent protective layer (PET film) laminated on the outer surface side of the base film 1.

[0055] <Use of packaging laminate> The packaging laminate 10 of the present invention described above is made into a bag by attaching it by heat sealing with a heat seal film 5, and is used as a pouch (bag-like container). The bag is made by a known method, for example, by making an empty pouch by sealing three sides of two laminates, filling the pouch with contents from the opening, and finally closing the opening by heat sealing. Alternatively, an empty pouch can be made by folding back one laminate and heat sealing both ends. In this case, it is not necessary to heat seal the bottom. Furthermore, an empty pouch can be made by using a laminate dedicated to the sides or bottom. Such a method is advantageous in increasing the volume of the pouch or imparting standing properties.

[0056] The pouch thus made from the packaging laminate 10 of the present invention and filled with the contents is effectively prevented from losing performance due to retort treatment (sterilization treatment with heated steam at 100 to 130°C), and even after retort treatment, it not only has excellent impact resistance at low temperatures, but also exhibits high seal strength at high temperatures, so it can withstand microwave heating. Therefore, such a pouch is particularly suitable for storing food products. EXAMPLES

[0057] The advantageous effects of the present invention are illustrated in the following examples. The materials and measuring methods used in the following experiments are shown below.

[0058] <Propylene film (CPP film) materials> Impact PP (A): Sunallomer PC480A MFR(230℃):2.0g / 10min EPR content (xylene-soluble content): 17.5 mass% Modified resin component (B) LLDPE (B1); ULTZEX 2022L manufactured by Prime Polymer Co., Ltd. MFR (190 °C): 2.0 g / 10 min Density: 919 kg / m 3 α-olefin species: 4-methylpentene-1 LLDPE (B2); Tafmer A1085S manufactured by Mitsui Chemicals, Inc. MFR (190 °C): 1.2 g / 10 min Density: 885 kg / m 3 α-olefin species: butene-1

[0059] <Commercially available CPP film> As commercially available CPP films, ZK500 and ZK401 (both with a thickness of 70 μm and surface hydrophilized) manufactured by Toray Film Processing Co., Ltd. were used. ZK500; EPR content: 16.9 mass% ZK401; EPR content: 16.6 mass%

[0060] <EPR content (xylene-soluble content)> Impact PP or CPP film was refluxed and dissolved in xylene, allowed to cool, and then subjected to solid-liquid separation. The xylene-soluble component was reprecipitated with methanol, the precipitate was taken out by filtration, dried, and weighed to calculate the EPR content.

[0061] <Dynamic viscoelasticity measurement method> A dynamic viscoelasticity measuring device manufactured by Seiko Instruments Inc. was used. The test conditions are as follows. Test piece film: length 20 mm, width 10 mm Chuck distance 5 mm Temperature range: -70 °C to 150 °C Heating rate: 3 °C / min Frequency: 10 Hz tan δ (loss tangent): Calculated by dividing the loss modulus at 5°C by the storage modulus. E' (storage modulus): Calculated as the value at 110°C.

[0062] <Pouch for horizontal drop bag test> The pouches used for the horizontal bag drop test were made by using an oriented polypropylene film (OPP, thickness 20 μm) as the base layer, and laminating a layer structure of OPP film / CPP film (thickness 70 μm) using a urethane-based adhesive by the dry lamination method to obtain a packaging bag.

[0063] <Pouch for seal strength measurement test> The pouches for the seal strength measurement tests had a layer structure of stretched PET film (OPET, thickness 12 μm) / stretched Ny film (ONy, thickness 15 μm) / aluminum foil (Al, thickness 7 μm) / CPP film (thickness 70 μm) as the base layer, and were laminated by the dry lamination method using a urethane-based adhesive.

[0064] <Pouch manufacturing> The laminated film with the CPP film was cut into two pieces measuring 140 mm (MD) x 180 mm (TD), and filled with 200 g of water to make bags. An impulse sealer manufactured by Fuji Impulse Co., Ltd. was used to make the bags. Pouches for horizontal drop bag test; Sealing conditions: 200℃, 1.4(s), cooling 3.0(s) Seal width: 5mm Test pouches for measuring seal strength; Sealing conditions: 220℃, 1.4(s), cooling 3.0(s) Seal width: 5mm

[0065] <Horizontal drop bag test method> The pouches were retorted at 121℃ for 30 minutes using a shower and cooled overnight in a 5℃ environment. Two of the pouches were then dropped horizontally from a height of 120cm to measure the results. The bottom pouch was the test pouch. The test was performed on three samples, with 20 drops, and the average number of unbroken pouches was measured.

[0066] <Seal strength measurement test method> An autograph (AG-I / 30N-10KN) manufactured by Shimadzu Corporation was used. The test conditions were as follows: Specimen Film: The heat-sealed portion of the pouch was cut at a right angle from the short side (140 mm) to create a 15 mm-wide strip. Six test pieces were created. Ambient temperature: 110℃ Tensile speed: 300mm / min

[0067] <Example 1> A CPP film was produced with a weight ratio of impact PP (A) / LLDPE (B1) = 86 / 14. The CPP film was formed by the following method. The impact PP (A) and LLDPE (B1) were dry-blended in the above composition and fed into the hopper of a single-screw extruder equipped with a T-die. The mixture was melt-kneaded in the extruder set at 230°C and extruded into a film from the T-die. The mixture was solidified by contacting it with a cooling roll at 60°C and wound up to produce a film with a thickness of 70 μm. The obtained film was subjected to a corona discharge treatment to make the surface hydrophilic.

[0068] Dynamic viscoelasticity measurements were performed on this CPP film to determine tan δ at 5° C. and E' at 110° C. The temperature curves of tan δ and E' obtained by this measurement are shown in Figures 2 and 3. Pouches for horizontal drop test and pouches for seal strength measurement were made by laminating the above-mentioned CPP film, and the horizontal drop test and seal strength measurement test were carried out. The results are shown in Table 1.

[0069] <Example 2> A CPP film was produced in the same manner as in Example 1, except that the ratio of the impact PP (A) and the LLDPE (B2) was changed to 95 / 5. The dynamic viscoelasticity measurement, the bag drop test, and the seal strength measurement were also performed in the same manner as in Example 1. The results are shown in Table 1.

[0070] <Comparative Example 1> A sealant film was prepared in the same manner as in Example 1, except that the CPP film was prepared using only impact PP (A). Dynamic viscoelasticity measurement, bag drop test, and seal strength measurement were also performed in the same manner as in Example 1, and the results are shown in Table 1.

[0071] <Comparative Example 2> Except for changing the CPP film to ZK500 manufactured by Toray Advanced Film Co., Ltd., the dynamic viscoelasticity measurement, bag drop test, and seal strength measurement test were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0072] <Comparative Example 3> The dynamic viscoelasticity measurement, bag drop test, and seal strength measurement were carried out in the same manner as in Example 1, except that the CPP film was changed to ZK401 manufactured by Toray Advanced Film Co., Ltd. The results are shown in Table 1.

[0073] [Table 1] [Explanation of symbols]

[0074] 1: Base film 3: Adhesive layer 5: Heat seal film 10: Packaging laminate

Claims

1. A packaging laminate having a structure in which a base film and a heat seal film are laminated with an adhesive layer sandwiched therebetween, A stretched polypropylene film is used as the base film, A propylene-based film is used as the heat seal film, The propylene-based film used as the heat seal film has a loss tangent (tan δ) of more than 0.0594 at 5° C. and a storage modulus (E′) of more than 1 MPa at 110° C. in a dynamic viscoelasticity test measurement, The propylene-based film is formed from a cast film that includes an impact polypropylene component; The cast film contains an impact polypropylene component (A) in which an ethylene-propylene copolymer is dispersed in polypropylene, and a linear low-density polyethylene (B), The cast film contains 8 to 20% by mass of a xylene soluble fraction derived from an ethylene-propylene copolymer, The cast film comprises the linear low-density polyethylene (B) in an amount of 14% by mass or less.

2. 2. The packaging laminate according to claim 1, wherein the adhesive layer is formed from a dry lamination adhesive.

3. 3. The packaging laminate according to claim 1 or 2, further comprising a stretched film comprising at least one selected from an olefin-based resin, a polyamide-based resin, and an ethylene-vinyl alcohol copolymer, laminated separately from the base film.

4. 4. The packaging laminate according to claim 3, wherein the olefin resin is polypropylene.

5. A pouch comprising the packaging laminate according to any one of claims 1 to 4.

6. The pouch according to claim 5, wherein the content of the olefin-based resin in the pouch is 80% by mass or more.

Citation Information

Patent Citations

  • JP1973044091A

  • Propylene resin composition and film made thereof

    JP2006161033A

  • Laminate for heat sterilization treatment, packaging material for heat sterilization treatment and package for heat sterilization treatment

    JP2019177521A

  • Laminate for packaging material and packaging material

    JP2020040259A

  • High interlaminar adhesive gas barrier vapor-deposited film

    JP2020131676A