Lead acid battery
The lead-acid battery design with a balanced negative electrode mixture and sodium ions addresses charge acceptance and water loss issues, enhancing performance and durability.
Patent Information
- Application Number
- JP2021038820
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-03-11
AI Technical Summary
Lead-acid batteries face challenges in maintaining high charge acceptance and water loss resistance while ensuring startability, particularly in vehicles with idling stop systems and tropical climates, where electrolyte evaporation and stratification lead to reduced performance and shortened lifespan.
A lead-acid battery design with a negative electrode mixture that includes specific surface area ratios and sodium ions within a defined range, balancing conductivity and water loss resistance, using carbon materials and sodium ions to enhance charge acceptance.
The battery achieves improved charge acceptance and resistance to water loss, maintaining startability and extending lifespan.
Smart Images

Figure 0007590226000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a lead-acid battery. [Background technology]
[0002] In recent years, in order to reduce the burden on the environment, vehicles have come to be equipped as standard with control systems that reduce gasoline consumption, such as charging control systems and idling stop systems. Due to the control system described above, lead-acid batteries are often operated in a partial state of charge (hereinafter, also referred to as "PSOC", an acronym for Partial State of Charge). In PSOC, gas generation due to electrolysis of the electrolyte and the resulting stirring of the electrolyte are difficult to occur. As a result, stratification of the electrolyte cannot be sufficiently suppressed, and lead-acid batteries are prone to having a short life. As degradation processes caused by stratification, for example, in the positive plate, the active material at the bottom of the plate softens and falls off, and grid corrosion occurs, and in the negative plate, sulfation occurs in which passive lead sulfate crystals grow at the bottom of the plate, resulting in a decrease in discharge capacity. As such degradation progresses, the internal resistance of the lead-acid battery increases, making it difficult to draw the large current required for starting the engine, resulting in a decrease in starting ability.
[0003] As a lead-acid battery that exhibits excellent performance even under PSOC operation, the applicant has proposed a lead-acid battery in which aluminum ions are added to the electrolyte, as disclosed in Patent Document 1. A lead-acid battery in which aluminum ions are added to the electrolyte has excellent charge acceptance and is also excellent in starting performance because stratification and sulfation are suppressed. However, in recent years, the demand for reducing environmental impact is increasing. When a vehicle's control system regulates gasoline consumption by frequently stopping the engine, lead-acid batteries that are charged by an alternator connected to the engine tend to operate at a lower PSOC, and higher charging acceptance is required.
[0004] Patent Document 2 proposes a lead-acid battery in which two types of carbon materials with different particle sizes and powder resistance are contained in the negative electrode in order to improve PSOC life performance without impairing low-temperature high-rate performance (i.e., engine startability at low temperatures) and charge acceptance performance.
[0005] On the other hand, vehicles equipped with charge control systems and idling stop systems are becoming more common in tropical regions such as Thailand and India. In such tropical regions, the engine compartment in which the lead-acid battery is installed is prone to high temperatures, which makes it easier for the water in the electrolyte to evaporate, and the amount of electrolyte loss (also known as "water loss") tends to increase. The progression of water loss accelerates the shortening of the lifespan of lead-acid batteries. For example, as the specific gravity of the electrolyte increases, the active material at the bottom of the positive plate becomes more susceptible to softening and falling off, and grid corrosion occurs more easily. Meanwhile, the progression of sulfation becomes more pronounced in the negative plate. To prevent such deterioration, users are forced to frequently replenish the electrolyte (also known as "water refilling").
[0006] Therefore, in order to extend the life of lead-acid batteries and improve user convenience by making them maintenance-free, high resistance to water loss is necessary. However, the above-mentioned resistance to water loss is in a trade-off relationship with charge acceptance. In other words, lead-acid batteries to which carbon with a high specific surface area that improves charge acceptance has been added have the drawback that water loss is likely to progress due to electrolysis. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 4799560 [Patent Document 2] WO2018 / 199124 publication Summary of the Invention [Problem to be solved by the invention]
[0008] As a result of the inventors' investigations, it was found that simply incorporating two types of carbon materials having different particle sizes or powder resistance into the negative electrode, as in the lead-acid battery described in Patent Document 2, can achieve both starting performance and charge acceptance, but does not provide sufficient resistance to water reduction. In view of the above circumstances, an object of the present invention is to provide a lead-acid battery that has higher charge acceptance and resistance to water reduction while ensuring starting performance. [Means for solving the problem]
[0009] In order to solve the above problems, the lead-acid battery of the present invention is a lead-acid battery having a negative electrode plate including a negative electrode active material, a carbon material, and a negative electrode mixture containing sodium ions, and the specific surface area S (m 2 / g) of the specific surface area C (m 2 The product CF of the carbon material content (wt. / g) and the ratio F (mass%) of the amount of carbon material added to the negative electrode mixture satisfies the following formula (1), and the amount of sodium ions in the negative electrode mixture is 20 ppm or more and 220 ppm or less. 0.3 ≦ CF / S ≦ 5.0 (1) Effect of the Invention
[0010] According to the present invention, there is provided a lead-acid battery which has higher charge acceptance and resistance to water reduction while ensuring starting performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A lead-acid battery according to one embodiment of the present invention will be described in detail below. However, the present invention is not limited to this embodiment. [Negative electrode mixture] The negative electrode mixture contains a negative electrode active material, a carbon material, an additive, and a reinforcing material and a shrinkage inhibitor that are added as necessary. The negative electrode mixture has a specific surface area S (m 2 / g). The negative electrode active material is a substance used in charge and discharge reactions, and is mainly composed of spongy metallic lead when the lead-acid battery is in a fully charged state.
[0012] The carbon material can be selected from carbon black, graphite, activated carbon, vapor-grown carbon fiber, carbon nanotubes, fullerenes, and other known carbon materials. The carbon material can be selected according to the type, particle shape, particle size, specific surface area C(m 2 The effect on battery performance, such as the conductivity of the negative electrode plate after addition and the capacitor capacity, varies depending on various parameters such as the surface functional group, the amount of carbon material added, and the like. In addition, the carbon material also affects the hardness and fluidity of the negative electrode mixture paste during production, and if an excessive amount is added, it may reduce the fluidity of the negative electrode mixture paste, resulting in a significant deterioration in manufacturability. The addition ratio of such carbon material is quantified by the ratio F (mass%) of the amount of carbon material added to the negative electrode active material.
[0013] The reinforcing material refers to short fibers or the like added mainly for the purpose of maintaining the shape of the negative electrode mixture, and for example, short fibers made of acrylic or polypropylene are suitable. The shrinkage inhibitor refers to an additive that is added to suppress the shrinkage of the negative electrode mixture and to prevent the deterioration of low-temperature starting performance. For example, barium sulfate, sodium lignin sulfonate (also called "lignin"), synthetic shrinkage inhibitors, etc. are suitable. The negative electrode mixture used in the negative electrode plate of the present invention satisfies the condition of the following formula (1) after chemical formation. 0.3 ≦ CF / S ≦ 5.0 (1)
[0014] The inventors of the present application have determined the specific surface area S (m 2 / g) of the specific surface area C (m 2 It has been found that when the value of the ratio CF / S of the product CF of the carbonaceous material content (wt%) relative to the negative electrode active material (wt%) is within the above range, starting performance is not impaired even when the battery is operated at a low PSOC, and a lead-acid battery having an excellent balance between charge acceptance and water reduction resistance is provided. When the CF / S is less than 0.3, the water reduction resistance is relatively high, but the conductivity of the negative electrode active material is insufficient, resulting in low charge acceptance. On the other hand, when the CF / S exceeds 5.0, the charge acceptance is high, but the water reduction resistance is reduced.
[0015] As a result of further research by the inventor, it was found that in a lead-acid battery having a negative electrode mixture satisfying formula (1), when the amount of sodium ions in the negative electrode mixture is 20 ppm or more and 220 ppm or less, better water reduction resistance is obtained. When the amount of sodium ions in the negative electrode mixture is less than 20 ppm, the effect of suppressing water reduction resistance is low. When the amount of sodium ions exceeds 220 ppm, not only the effect of suppressing water reduction resistance is saturated, but also the charge acceptance is reduced. Although the reason is unclear, it is thought that the sodium ions added to the negative electrode mixture increase the hydrogen overvoltage of the negative plate during charging and discharging, suppressing hydrogen generation, and thereby suppressing the excessive progress of electrolysis. For example, it is known that sodium ions in the electrolyte reduce charge acceptance (GS Yuasa Technical Report, p. 22-28, Vol. 8, No. 2, 2011), and it is speculated that sodium ions in the negative electrode mixture may also reduce charge acceptance depending on the amount.
[0016] Two or more types of carbon materials may be selected in combination. In that case, CF / S is the sum of each carbon. For example, when two types of carbon materials, carbon material A and carbon material B, are selected, the following condition of formula (2) is satisfied. 0.3 ≦ (C A ×F A +C B ×F B ) / S ≦ 5.0 (2) In the above formula (2), the meanings of the respective symbols are as follows: C A : Specific surface area of carbon material A (m 2 / g) C B : Specific surface area of carbon material B (m 2 / g) F A : Proportion of the amount of carbon material A added to the negative electrode active material (mass%) F B : Proportion of the amount of carbon material B added to the negative electrode active material (mass%) S: specific surface area of negative electrode mixture S (m 2 / g)
[0017] The specific surface area S of the negative electrode mixture and the specific surface area C of the carbon material are the BET specific surface areas. The BET specific surface area is a specific surface area measured by the BET method, which is a method in which an inert gas (e.g., nitrogen gas) with a known molecular size is adsorbed on the surface of a measurement sample, and the surface area is calculated from the amount of adsorption and the area occupied by the inert gas, and is a general measurement method for specific surface area. The specific surface area S of the negative electrode mixture is measured according to the procedure specified in JIS Z 8830:2013. The specific surface area C of the carbon material is measured according to the procedure specified in JIS K 6217-7:2013.
[0018] The amount of sodium ions in the negative electrode mixture was measured by ICP emission spectrometry. ICP emission spectrometry is a general analytical method in which the amount of light emitted from a component element excited by applying plasma energy is measured to determine the content of the component element. In the present invention, the amount of sodium ions in the negative electrode mixture is measured according to the procedure specified in JIS K 0116:2014. As a method for introducing sodium ions into the negative electrode mixture, a method of adding a sodium compound such as sodium sulfate or sodium lignin sulfonate as a sodium ion source to the negative electrode paste, or a method of adding a sodium compound to dilute sulfuric acid injected as an electrolyte can be considered. EXAMPLES
[0019] The present invention will be described in more detail below with reference to examples and comparative examples. Procedures and configurations not mentioned may be arbitrarily selected from conventionally known techniques. <Examples 1 to 3 and Comparative Examples 1 and 2> First, the method of producing the lead-acid battery of Example 1 will be described in order from the production of the positive plate. The positive plate has a positive electrode current collector and a positive electrode mixture, and the positive electrode mixture is held by the positive electrode current collector. The positive electrode current collector has a plate-shaped grid body and an ear made of a lead alloy, and is produced by gravity casting or the like. In Example 1, the plate-shaped grid body, which is approximately rectangular in plan view, is formed with a frame bone forming the four sides of the rectangle and a plurality of inner bones surrounded by the frame bone. Then, an ear is formed on the frame bone forming one side of the rectangle so as to protrude outward in the surface direction. For convenience of explanation, the frame bone having the ear is called the upper frame bone, the frame bone parallel to the upper frame bone is called the lower frame bone, and the frame bones parallel to each other that connect the left and right ends of the upper frame bone and the lower frame bone are called the left frame bone and the right frame bone. The inner bone is formed with a vertical bar connecting the upper frame bone and the lower frame bone, and a horizontal bar connecting the left frame bone and the right frame bone. A plurality of openings are formed in the plate-like grid by the frame and inner frame.
[0020] The positive electrode mixture contains lead dioxide as a positive electrode active material in a charged state after chemical formation. The paste of the positive electrode mixture before chemical formation (hereinafter referred to as positive electrode paste) was prepared by mixing lead powder mainly composed of lead monoxide with red lead, cut polyester fiber as a reinforcing material, and compound particles containing bismuth oxide (hereinafter referred to as dry mixing), then adding water and kneading (hereinafter referred to as water kneading), and then adding dilute sulfuric acid and kneading again (hereinafter referred to as acid kneading). The obtained positive electrode paste was filled into a positive electrode current collector (about 50 g / sheet, thickness about 1.3 mm) prepared by gravity casting for JIS-B size, and dilute sulfuric acid was sprayed uniformly on the surface of the electrode plate at a predetermined pressure, and then passed through a preheating drying furnace. Then, aging and drying were performed under predetermined conditions to obtain a positive electrode aged plate.
[0021] The negative electrode plate has a negative electrode current collector and a negative electrode mixture, and the negative electrode mixture is held by the negative electrode current collector. The negative electrode current collector has a plate-shaped lattice having a frame and an inner frame, and an ear, similar to the positive electrode current collector, and is manufactured by a continuous casting method or the like. The negative electrode mixture contains metallic lead (such as sponge-like lead) as a negative electrode active material in a charged state after chemical formation. The paste of the negative electrode mixture before chemical formation (hereinafter referred to as negative electrode paste) was prepared by dry mixing lead powder mainly composed of lead monoxide, cut fiber of polyester fiber as a reinforcing material, barium sulfate and lignin (sodium lignin sulfonate) as shrinkage inhibitors, Ketjen black as a carbon material serving as a conductive material, and sodium sulfate as an additive, followed by water kneading and then acid kneading. The obtained negative electrode paste was continuously filled into a continuous casting substrate for JIS-B size (about 40 g / sheet, thickness about 1.0 mm) and passed through a preheating drying furnace. Thereafter, aging and drying were carried out under predetermined conditions to obtain a negative electrode aged plate.
[0022] In Example 1, sodium sulfate and lignin were added as sodium ion sources to the negative electrode mixture, so that the total amount of sodium ions in the negative electrode mixture in the lead-acid battery after formation was 25 ppm. In addition, the specific surface area C (BET specific surface area (m 2 / g)) is 1000m 2 / g, and the amount added was 0.2 wt % relative to the amount of the negative electrode active material. If the ratio F (mass %) of the amount of the carbon material added to the negative electrode active material changes during the manufacturing process due to leakage into the electrolyte, etc., the value after chemical formation is used.
[0023] Next, the negative electrode aged plates were respectively stored in polyethylene separators formed into a bag shape by gear seal, and five positive electrode aged plates and six negative electrode aged plates were alternately stacked and combined, and the plates of the same polarity were welded to each other by the COS method (cast-on-strap method) to form a positive electrode strap and a negative electrode strap to form an electrode plate group. The positive electrode strap and the negative electrode strap have a positive electrode intermediate pole and a negative electrode intermediate pole as conventionally known, and a positive electrode pole and a negative electrode pole as external terminals. Six of these electrode plate groups were stored one by one in a cell chamber of a monoblock type battery case made of PP (polypropylene) with an opening at the top. Adjacent cell chambers were separated by a partition wall, but a communication port was formed at the top of the partition wall, and the intermediate poles were resistance-welded to each other at the communication port so that all the electrode plate groups were electrically connected in series. When storing in the cell chamber, the pressure on the electrode plate group was 10 kPa. Next, a lid with a bushing insert molded into it is placed over the opening of the battery case and heat sealed. A liquid inlet of the lid is poured into the battery case, with a specific gravity of 1.22 g / cm. 3 The battery was then sealed with a plug containing diluted sulfuric acid to obtain a B20 type unformed lead-acid battery. Finally, the battery was formed by a conventional method, and the specific gravity after formation was adjusted to 1.285 (20°C conversion value) to obtain the lead-acid battery of Example 1.
[0024] In the present invention, six lead-acid batteries were prepared under the same preparation conditions, three of which were subjected to a battery performance test, and the remaining three were disassembled after formation, and the specific surface area was measured and the composition was analyzed. In each test, measurement, and analysis, the average value of the three lead-acid batteries was used. It was also assumed that the test cells obtained under the same preparation conditions had the same battery performance and configuration. In this specification, the positive electrode aged plate in which the lead oxide has been converted to a positive electrode active material through chemical formation is called a positive electrode plate, and the negative electrode aged plate in which the lead oxide has been converted to a negative electrode active material is called a negative electrode plate. The chemical composition of the active material and the mechanical structure such as the specific surface area of the mixture change depending on the charging state, but unless otherwise specified, they refer to the composition and structure in the fully charged state after chemical formation.
[0025] The lead-acid batteries of Examples 2 to 3 and Comparative Example 2 are the same as the lead-acid battery of Example 1, except that sodium sulfate and lignin are added as sodium ion sources to the negative electrode mixture, and the total amount of sodium ions in the negative electrode mixture after the chemical formation is 105 ppm, 185 ppm, and 230 ppm. In addition, in the lead-acid battery of Comparative Example 1, only lignin is added as an ion source for introducing sodium ions into the negative electrode mixture, and sodium sulfate is not added. In the lead-acid battery of Comparative Example 1, the amount of lignin added is adjusted so that the amount of sodium ions in the negative electrode mixture after the chemical formation is 15 ppm. Except for the amount of sodium ions in the negative electrode mixture after the chemical formation, the lead-acid battery of Comparative Example 1 is the same as the lead-acid battery of Example 1. For Examples 1 to 3 and Comparative Examples 1 and 2, the specific surface area S (BET specific surface area (m 2 / g) is 0.8m 2 / g and the CF / S value was 2.5.
[0026] <Comparative Examples 3 to 7> The carbon material in the negative electrode mixture has a specific surface area C of 1177.5 m 2 A lead-acid battery was fabricated in the same manner as in Comparative Example 1 for Comparative Example 3, in Example 1 for Comparative Example 4, in Example 2 for Comparative Example 5, in Example 3 for Comparative Example 6, and in Comparative Example 2 for Comparative Example 7, except that carbon black with a high specific surface area of 0.1 μm / g was used and the amount of addition F was 0.35% by weight relative to the amount of the negative electrode active material. For Comparative Examples 3 to 7, the specific surface area S (BET specific surface area (m 2 / g) is 0.8m 2 / g and the CF / S value was 5.2.
[0027] <Comparative Examples 8 to 12> The carbon material in the negative electrode mixture has a specific surface area C of 75.4 m 2 / g and acetylene black with a specific surface area C of 1.03 m 2A lead-acid battery was fabricated in the same manner as in Comparative Example 1 for Comparative Example 8, in Comparative Example 9, in Comparative Example 10, in Comparative Example 2, in Comparative Example 11, in Comparative Example 3, and in Comparative Example 12, in Comparative Example 2, except that graphite having a molecular weight of 0.2 wt % or 1.0 wt % was used and the additive amount F was set to 0.2 wt % or 1.0 wt % relative to the amount of the negative electrode active material. For Comparative Examples 8 to 12, the specific surface area S (BET specific surface area (m 2 / g) is 0.8m 2 / g and the CF / S value was 0.2.
[0028] <Examples 4 to 6 and Comparative Examples 13 and 14> The carbon material in the negative electrode mixture has a specific surface area C of 75.4 m 2 / g and acetylene black with a specific surface area C of 1.03 m 2 A lead-acid battery was fabricated in the same manner as in Comparative Example 13, in Example 4, in Example 1, in Example 5, in Example 2, in Example 6, in Example 3, and in Comparative Example 14, in Comparative Example 2, except that graphite having a molecular weight of 0.3 wt % or 1.5 wt % was used and the additive amount F was set to 0.3 wt % or 1.5 wt % relative to the amount of the negative electrode active material. For Examples 4 to 6 and Comparative Examples 13 and 14, the specific surface area S (BET specific surface area (m 2 / g) is 0.8m 2 / g and the CF / S value was 0.3.
[0029] <Examples 7 to 9 and Comparative Examples 15 and 16> The carbon material in the negative electrode active material paste has a specific surface area C of 1177.5 m 2 / g, and carbon black with a specific surface area C of 1.03 m 2 A lead-acid battery was fabricated in the same manner as in Comparative Example 15, Example 1, Example 7, Example 8, Example 2, Example 9, Example 3, and Comparative Example 16, except that graphite having a molecular weight of 0.1 wt % or 0.2 wt % was used, and the additive amount F was set to 0.3 wt % and 1.5 wt % relative to the amount of the negative electrode active material, respectively. For Examples 7 to 9 and Comparative Examples 15 and 16, the specific surface area S (BET specific surface area (m 2 / g) is 0.8m 2 / g and the CF / S value was 4.4.
[0030] As a test for evaluating the charge acceptance performance, the "7.3 Dynamic Charge acceptance test (DCA)" specified in BS EN 50342-6:2015 of the European standard (EN standard) was carried out. Also, as a test for evaluating the water resistance reduction performance, the "6.9 Water consumption test" specified in BS EN 50342-1:2015 was carried out. Note that for DCA, water resistance reduction, and comprehensive judgment, with the performance of Comparative Example 8 taken as 100%, the judgments were made as follows respectively.
[0031] DCA: X (%) X < 90: × (insufficient) 90 ≤ X < 110: △ (ordinary) 110 ≤ X < 120: ○ (good) 120 ≤ X: ◎ (excellent)
[0032] Water resistance reduction: Y (%) 100 < Y: × (insufficient) 90 ≤ Y ≤ 100: △ (ordinary) 75 ≤ Y < 90: ○ (good) Y < 75: ◎ (excellent)
[0033] Comprehensive judgment When both the DCA judgment and the water reduction judgment are ◎, or one is ◎ and the other is ○: ◎ When both the DCA judgment and the water reduction judgment are ○: ○ When both the DCA judgment and the water reduction judgment are △: △ When at least one of the DCA judgment and the water reduction judgment is ×: ×
[0034] The test results and evaluation are shown in Table 1. In Table 1, Carbon A is Ketjen black, Carbon B is acetylene black, Carbon C is carbon black with a high specific surface area, and Carbon D is graphite. In Table 1, NAM is an abbreviation for Negative Active Material, which directly means the negative electrode active material, but in Table 1 it refers to the negative electrode mixture. Also, Na+ refers to sodium ions, and therefore the same column in Table 1 refers to the content of sodium ions in the negative electrode mixture. The following became clear from Table 1.
[0035] The lead-acid batteries of Examples 1 to 9 have a CF / S in the range of 0.3 or more and 5.0 or less, and a sodium ion content in the negative electrode mixture in the range of 20 ppm or more and 220 ppm or less, and thus achieve a high level of both charge acceptance and water reduction resistance. The lead acid batteries of Comparative Examples 3 to 7 have a CF / S of more than 5.0, and therefore have high charge acceptance but low resistance to water reduction. The lead-acid batteries of Comparative Examples 1, 3, 8, 13, and 15 had a sodium ion content in the negative electrode mixture of less than 20 ppm, and thus had a low water reduction suppression effect. The lead-acid batteries of Comparative Examples 2, 7, 12, 14, and 16 had a sodium ion content in the negative electrode mixture exceeding 220 ppm, and thus had a significantly reduced charge acceptance and a saturated water reduction resistance suppressing effect.
[0036] [Table 1]
Claims
1. A lead-acid battery having a negative electrode plate including a negative electrode mixture containing a negative electrode active material, a carbon material, and sodium ions, The specific surface area S (m 2 / g) of the specific surface area C (m 2 / g) and the ratio F (mass%) of the amount of the carbon material added to the negative electrode active material satisfies the relationship of the following formula (1), 0.3 ≦ CF / S ≦ 5.0 (1) and wherein the amount of sodium ions in the negative electrode mixture is 20 ppm or more and 220 ppm or less.
2. 2. The lead-acid battery according to claim 1, wherein the negative electrode active material contains two or more kinds of carbon materials.
Citation Information
Patent Citations
Lead-acid battery and its manufacture
JP2001035486A
Lead battery with miniature control valve
JP2001332264A
Lead acid storage battery
JP2008243489A
Lead storage battery
JP2017016971A
Lead storage battery
JP2020115424A