Method for manufacturing a defective bonded structure test block
The method of controlled adhesive curing and defect simulation in test blocks addresses the challenge of manufacturing test blocks with predefined defects, enabling accurate simulation and detection of structural weaknesses in bonded structures.
Patent Information
- Application Number
- JP2021562900
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-05
- Filing Date
- 2020-12-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Manufacturing test blocks with controlled defects such as kissing bonds and weak adhesion to detect internal defects in bonded structures is difficult.
A method involving the controlled application and curing of adhesive layers on plates to create test blocks with predefined defects, using a pre-curing device to heat specific areas and adjusting curing temperatures based on rheological properties to simulate actual defects.
Enables the production of test blocks that accurately simulate defects like weak adhesion and kissing bonds, facilitating effective mechanical detection and evaluation of structural integrity.
Smart Images

Figure 0007590342000001 
Figure 0007590342000002 
Figure 0007590342000003
Abstract
Description
[Technical field]
[0001] Related Applications This application is based on and claims priority from Chinese Patent Application No. 202010507968.9, filed on June 5, 2020, the entire contents of which are incorporated herein by reference. [Background technology]
[0002] Technical Field The present disclosure relates to the field of non-destructive detection, and more particularly, to a method for manufacturing a bonded structural test block having defects.
[0003] background With the rapid development of civil aviation, there is a demand for aircraft structural materials to be developed with low density, high strength, high toughness, high temperature resistance, and corrosion resistance. In traditional civil aviation structures, some parts must be formed by connecting parts with a large number of rivets. Small aircraft usually contain tens of thousands of rivets, which inevitably increases the weight of the aircraft. Although bonded structures are being widely applied in civil aircraft structures instead of riveting, various defects such as cracks, voids / holes, peeling, and weak bonds are inevitably generated in the manufacturing process of bonded structures.
[0004] Kissing bonds are a type of defect in bonded structures where two surfaces are in intimate contact, i.e., the two surfaces are not bonded together; kissing bonds lead to reduced structural load-bearing capacity. A similar defect to kissing bonds is weak bonds, i.e., two surfaces are incompletely bonded together. Weak bonds can be more difficult to evaluate due to some structural continuity. Kissing and weak bond defects can occur in monolithic, sandwiched, bonded or repaired composites, which may occur during the manufacturing process or due to inadequate damage or repair. It is particularly important to detect and evaluate the defect type as the structural strength is reduced under in-service loading conditions and defects can potentially grow (i.e., from weak bonds / kissing bonds to delamination). Summary of the Invention [Problem to be solved by the invention]
[0005] To check for defects, a comparison test block with defects must first be made. However, because manufacturing test blocks is difficult, it is very important to controllably manufacture test blocks with kissing bonds and weak bonds to detect internal defects. [Means for solving the problem]
[0006] overview The present disclosure provides a method for manufacturing a defective bonded structure test block, comprising: providing a first plate and a second plate; applying an adhesive to a top surface of the first plate to form an adhesive layer; A step of first heat-curing at least a portion of the adhesive layer; placing a second plate on the adhesive layer; and heat curing the adhesive layer a second time to form an adhesive structure test block.
[0007] In some embodiments, at least some of the regions include a plurality of pre-defined area blocks spaced apart and distributed on the adhesive layer, and the step of heat-curing at least some of the regions of the adhesive layer a first time includes heat-curing the plurality of pre-defined area blocks of the adhesive layer individually.
[0008] In some embodiments, the method further includes determining positions and areas of the plurality of pre-defined area blocks according to the pre-defined positions and the pre-defined area of the defect prior to the step of independently heat-curing the plurality of pre-defined area blocks of the adhesive layer.
[0009] In some embodiments, the step of independently heating and curing the multiple pre-set area blocks of the adhesive layer is performed by a pre-curing device, the pre-curing device including a heating plate and multiple heating columns movably disposed on the heating plate, and the positions of the multiple heating columns are adjusted to correspond to the multiple pre-set area blocks on the adhesive layer.
[0010] In some embodiments, applying adhesive to the top surface of the first plate to form an adhesive layer includes applying adhesive to an area near an edge of the top surface of the first plate and overlapping the second plate over the edge of the first plate.
[0011] In some embodiments, the method further includes the steps of performing a temperature-elevated rheological property test on the adhesive to obtain a rheological curve of the adhesive, and selecting a temperature for the first heat-curing step and a temperature for the second heat-curing step according to the rheological curve.
[0012] In some embodiments, the step of applying adhesive to the upper surface of the first plate to form an adhesive layer includes applying adhesive to the entire area of the upper surface of the first plate to cover the upper surface of the first plate with adhesive. The at least some area includes the entire area of the adhesive layer. The above manufacturing method further includes a step of attaching a second plate onto the adhesive layer and then heat-curing the adhesive layer for the first time before the step of heat-curing the entire area of the adhesive layer for the first time, and a step of separating the first plate and the second plate from the center of the adhesive layer, overlapping the separated first plate and the second plate, and heat-curing the adhesive layer for the second time after the step of heat-curing the entire area of the adhesive layer for the first time.
[0013] In some embodiments, the step of heat-curing the adhesive layer for the first time and the step of heat-curing the adhesive layer for the second time are both performed by autoclave, the temperature of the step of heat-curing the adhesive layer for the first time and the step of heat-curing the adhesive layer for the second time is the same, and the heating time of the step of heat-curing the adhesive layer (3) for the first time and the step of heat-curing the adhesive layer for the second time is different.
[0014] In some embodiments, the method further comprises the step of cracking the adhesive layer.
[0015] In some embodiments, the adhesive is an adhesive film that is coated onto the top surface of the first plate to form an adhesive layer.
[0016] In some embodiments, a first plate and a second plate are provided that are made of a composite material, the composite material of the first plate and the composite material of the second plate being the same or different.
[0017] In some embodiments, after the test block is obtained, the test block is ultrasonically scanned to determine defect information.
[0018] Based on the technical solution provided by the present disclosure, a manufacturing method for a bonded structure test block having defects includes the steps of providing a first plate and a second plate, applying an adhesive on the upper surface of the first plate to form an adhesive layer, heat-curing at least a portion of the adhesive layer for a first time, placing a second plate on the adhesive layer, and heat-curing the adhesive layer for a second time to form a bonded structure test block. According to the present disclosure, at least a portion of the adhesive layer is heat-cured for a first time to cause a chemical reaction, which results in at least a portion of the adhesive layer forming a defect, and the controllable manufacturing of the defect is realized. A mechanical detection is performed on the test block having defects to simulate an actual defective product. Furthermore, according to the method provided by the present disclosure, weak adhesion defects and kissing bond defects with different adhesive strengths are simulated by controlling the proportion of at least a portion of the adhesive layer in the total area.
[0019] Other features and advantages of the present disclosure will become apparent from the following detailed description of illustrative embodiments thereof, which proceeds with reference to the accompanying drawings.
[0020] In order to more clearly describe the embodiments of the present disclosure or the technical solutions in the prior art, the accompanying drawings necessary for describing the embodiments or the prior art are briefly described below. It is clear that the accompanying drawings in the accompanying drawings described below show some embodiments recorded in the present disclosure, and those skilled in the art can still derive other drawings from these accompanying drawings. [Brief description of the drawings]
[0021] [Figure 1] 1A-1D are schematic diagrams of steps in a method for manufacturing a defective bonded structure test block according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a rheology curve of an adhesive film according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a structural schematic diagram of a pre-curing device used according to one embodiment of the present disclosure. [Figure 4] FIG. 2 is a schematic diagram of the processing steps of a test block having weak adhesion defects manufactured according to one embodiment of the present disclosure, showing the step of performing a first heat curing on the adhesive layer by a pre-curing device. [Diagram 5] FIG. 1 is a schematic diagram of the processing steps of a test block having weak adhesion defects manufactured according to one embodiment of the present disclosure, showing the step of overlapping a second plate onto a first plate. [Figure 6] FIG. 6 is a schematic diagram of the processing steps of a test block having a weak adhesion defect manufactured according to an embodiment of the present disclosure, and is an enlarged structural view of the adhesive layer of FIG. 5 . [Figure 7] FIG. 1 is a schematic diagram of the processing steps of a test block having a weak adhesion defect manufactured according to one embodiment of the present disclosure; and FIG. 2 is a structural schematic diagram of a test block having a defect formed after a second heat curing. [Figure 8] FIG. 1 is a schematic diagram of processing steps for a test block having kissing bond defects manufactured according to one embodiment of the present disclosure, showing the steps of overlapping a first plate, an adhesive layer, and a second plate. [Figure 9] FIG. 13 is a schematic diagram of the processing steps of a test block having kissing bond defects manufactured according to one embodiment of the present disclosure, showing the step of separating the first and second plates of an intermediate bonded structure subjected to a first heat curing. [Figure 10] FIG. 1 is a schematic diagram of the processing steps of a test block having a kissing bond defect manufactured according to one embodiment of the present disclosure; and FIG. 2 is a structural schematic diagram of a test block having the defect formed after a second heat curing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Detailed Description In order to make the objectives, technical solutions and advantages of the present disclosure clearer, the manufacturing method of the bonded structure defect test block provided by the present disclosure will be further described in detail below through embodiments with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only for illustrating the present disclosure, not for limiting the present disclosure.
[0023] As shown in FIG. 1, a method for manufacturing a defective bonded structure test block according to an embodiment of the present disclosure includes: Step 101: Providing a first plate 1 and a second plate 2; Step 102: Applying adhesive to the top surface of the first plate 1 to form an adhesive layer 3; Step 103: A step of first heat-curing at least a part of the adhesive layer 3; Step 104: placing a second plate 2 on the adhesive layer 3; Step 105: Heat curing the adhesive layer 3 for a second time to form an adhesive structure test block.
[0024] According to the embodiment of the present disclosure, at least a part of the area of the adhesive layer 3 is heated and cured once to cause a chemical reaction, which results in the formation of defects in at least a part of the area, and the controllable manufacture of the defects is realized. A mechanical detection is performed on the test block having the defects to simulate an actual defective product. Furthermore, according to the manufacturing method provided by the present disclosure, the proportion of at least a part of the area in the total area of the adhesive layer is controlled to simulate weak adhesive defects with different adhesive strengths.
[0025] It should be noted that other steps may be performed between the above steps. Referring to FIG. 6, FIG. 6 is a structural diagram of the adhesive layer 3 after the first heat curing, where 31 is a non-cured area and 32 is a cured area. Before manufacturing the bonded structure defect test block, first determine the preset position and preset area of the defect of the test block having the defect to be manufactured. The method of this embodiment further includes a step of determining the position and area of the multiple preset area blocks according to the preset position and preset area of the defect before the step of independently heating the multiple preset area blocks of the adhesive layer. That is, the preset area blocks are cured areas.
[0026] In one embodiment, the present disclosure provides a method for manufacturing a weak adhesion defect test block. As shown in FIG. 4, the at least some region of the present embodiment includes a plurality of pre-set area blocks spaced apart from each other and distributed on the adhesive layer 3, and the step of heat-curing the at least some region of the adhesive layer 3 for the first time includes independently heating the plurality of pre-set area blocks of the adhesive layer 3.
[0027] Specifically, in this embodiment, multiple pre-set regions on the adhesive layer 3 are independently heated by a pre-curing device 5 shown in Fig. 3. The pre-curing device 5 includes a heating plate 51 and multiple heating columns 52 movably disposed on the heating plate 51, and the positions of the multiple heating columns 52 are adjusted to correspond to the multiple pre-set regions on the adhesive layer 3.
[0028] In order to be suitable for manufacturing test blocks having various defect sizes and positions, the pre-curing device 5 of this embodiment further includes a positioning groove 53, and the heating columns 52 are disposed in the positioning groove 53, and the position of each heating column 52 is changed by adjusting the position of the positioning groove 53.
[0029] As shown in FIG. 4, multiple heating columns 52 contact the adhesive layer 3 to heat-cure multiple pre-set areas of the adhesive layer 3 for the first time, and the adhesive layer 3 after the first heat-cure is shown in FIG. 6.
[0030] As shown in FIG. 7 , the step of applying adhesive to the top surface of the first plate 1 to form an adhesive layer 3 includes the step of forming an adhesive layer 3 in an area near the edge of the top surface of the first plate 1 and overlapping a second plate 2 onto the first plate.
[0031] As shown in FIG. 2, the method of this embodiment further includes a step of performing a temperature-elevated rheological property test on the adhesive to obtain a rheological curve of the adhesive, and a step of selecting a temperature for the first heat-curing step and a temperature for the second heat-curing step according to the rheological curve.
[0032] Specifically, the temperature in the first heat-curing step is lower than the temperature in the second heat-curing step.
[0033] The manufacturing method of the test block having weak adhesion defects is described in detail below with reference to specific embodiments.
[0034] First, select the materials of the first plate 1, the second plate 2, and the adhesive film. In this embodiment, the composite material of the first plate 1 and the composite material of the second plate 2 are the same, which is CYCOM X850, and the material of the adhesive film is PL7000.
[0035] The adhesive film is subjected to a temperature-elevated rheological property test using a rheometer. In this test, the adhesive film is pressed into a wafer of 25 mm diameter at room temperature using a parallel plate clamp, and three adhesive films are stacked and compressed to prepare a test sample, and the rheological curve of the adhesive film is obtained as shown in Figure 2.
[0036] As shown in FIG. 4, the first plate 1 is attached, and an adhesive film is attached to the surface of the first plate 1 .
[0037] The heating columns 51 of the pre-curing device 5 are adjusted according to the preset position and preset area of the designed weak adhesion defect, and connected to the upper surface of the adhesive film. Specifically, in this embodiment, 50 needle-shaped heating columns are arranged, and each heating column 51 is a circle with a diameter of 0.2 mm.
[0038] The adhesive film is partially pre-cured by the pre-curing device 5, the heating rate of the adhesive film in contact with the heating column 51 on the adhesive film is 2-3°C / min, the curing temperature is 100°C±10°C, and the curing time is 30 minutes.
[0039] As shown in FIG. 5, the pre-cure device 5 is removed and the second plate 2 is completed to cover the adhesive film, resulting in a single overlap bonded structure.
[0040] On the pasted single overlap bonded structure, peelable cloth, insulating film, breathable felt, and pressure equalizing plate auxiliary material are arranged in sequence, and the test block is packaged in a vacuum bag and placed in an autoclave for curing. The curing temperature is 180°C, the heat retention is 120 minutes, and the curing pressure is 0.7Mpa.
[0041] Demolding results in a single overlap test block with partial weak adhesion as shown in FIG.
[0042] The test block is ultrasonically scanned to obtain defect signals, and machined to obtain a single overlap test block that meets specifications.
[0043] Mechanical property tests are performed on single overlap test blocks. In another embodiment, the present disclosure provides a method for manufacturing a test block having a kissing bond defect. As shown in FIG. 8, the adhesive layer 3 covers the top surface of the first plate 1. The at least some area includes the entire area of the adhesive layer 3. The manufacturing method further includes a step of attaching the second plate 2 to the adhesive layer 3 and then heat-curing the adhesive layer 3 for the first time before the step of heat-curing the entire area of the adhesive layer 3 for the first time, and a step of separating the first plate 1 and the second plate 2 from the center of the adhesive layer 3, overlapping the separated first bond 1 and the second plate 2 as shown in FIG. 9 (FIG. 10 shows that the separated first plate 1 and the second plate 2 are overlapped), and heat-curing the entire bonded structure to heat-cur the adhesive layer 3 for the second time after the step of heat-curing the entire area of the adhesive layer 3 for the first time.
[0044] As shown in Figure 9, the first plate 1 and the second plate 2 are separated from the center of the adhesive layer 3, and at this time, an adhesive layer divider 3a is arranged on the upper surface of the first plate 1, and an adhesive layer divider 3b is arranged on the lower surface of the second plate 2.
[0045] In this embodiment, an autoclave is used for both the first heat curing and the second heat curing, and the first heat curing and the second heat curing have the same temperature but different heating times.
[0046] In the above embodiment, cracks may be pre-set in the adhesive layer 3 according to the defect setting requirements.
[0047] To facilitate the formation of the adhesive layer 3 , the adhesive in this embodiment is an adhesive film, which is applied to the top surface of the first plate to form the adhesive layer 3 .
[0048] The manufacturing method of this embodiment provides a first plate 1 and a second plate 2 made of a composite material, and the composite material of the first plate 1 and the composite material of the second plate 2 are the same or different.
[0049] After the test block is obtained, the test block is ultrasonically scanned to determine defect information. The manufacturing method of the test block having kissing bond defects will be described in detail below with reference to a specific embodiment.
[0050] First, prepare a first plate 1, a second plate 2, and an adhesive film. In this embodiment, the composite material of the first plate 1 and the composite material of the second plate 2 are the same, which is CYCOM 970 / PWC T300 3K ST(CCF), and the material of the adhesive film is PL7000.
[0051] As shown in Figure 8, the adhesive film is pre-set with a crack 33, the first plate 1, the adhesive film, and the second plate 2 are sequentially attached to form an intermediate bond structure, and the peelable cloth, the insulating film, the breathable felt, and the pressure-equalizing plate auxiliary material are sequentially arranged on the intermediate bond structure, and the intermediate bond structure is packaged in a vacuum bag and placed in an autoclave for the first heat curing. The curing temperature is 177°C±10°C, the heat retention is 120 minutes, and the curing pressure is 0.7Mpa.
[0052] As shown in FIG. 9, the first plate 1 and the second plate 2 are separated by an external force, and the first plate 1 and the second plate 2 are separated from the center of the adhesive layer 3 .
[0053] As shown in Figure 10 (Figure 10 does not show the adhesive layer but includes the adhesive layer), the separated first plate 1 and second plate 2 are stacked and heat cured for the second time. The curing temperature is 177°C ± 10°C, the temperature is kept for 60 minutes, and the curing pressure is 0.7Mpa. Then, the mold is released to obtain a test block containing pre-cracks and kissing bond defects.
[0054] It should be noted that when a component is said to be "fixed" to another component, the component may be placed directly on the other component, or there may be intermediate components present. When a component is said to be "connected" to another component, the component may be directly connected to the other component, or there may be intermediate components present at the same time. Conversely, when a component is said to be "directly on" another component, there is no intermediate component. The terms "vertical," "horizontal," "left," and "right," and similar expressions, as used herein, are for illustrative purposes only.
[0055] In describing the present disclosure, the terms "first" and "second" are merely a matter of convenience and should not be understood to denote or imply any relative importance.
[0056] Meanwhile, the words "upper", "lower", "left", "right", "middle", and "one" cited in this specification are merely for convenience of clarifying the description, and are not used to limit the scope of the present disclosure. Any change or adjustment of the relative relationship should be considered as the scope of the present disclosure in which the technical content is not substantially changed.
[0057] The above embodiments merely illustrate some embodiments of the present disclosure, and the description is more specific and detailed, but should not be interpreted as limiting the patent scope of the present disclosure.It is pointed out that some variations and improvements can be made by those skilled in the art without departing from the concept of the present disclosure, and such variations and improvements should be included in the protection scope of the present disclosure.Therefore, the protection scope of the patent of the present disclosure shall be determined by the attached claims.
Claims
1. 1. A method for manufacturing a defective bonded structure test block, comprising the steps of: Providing a first plate (1) and a second plate (2); applying an adhesive to the upper surface of the first plate (1) to form an adhesive layer (3); A step of first heat-curing at least a portion of the adhesive layer (3); placing the second plate (2) on top of the adhesive layer (3); and heat curing the adhesive layer (3) a second time to form an adhesive structure test block.
2. 2. The method for manufacturing a defective adhesive structure test block according to claim 1, wherein the at least some area comprises a plurality of pre-set area blocks (32) spaced apart and distributed on the adhesive layer (3), and the step of heat-curing at least some area of the adhesive layer (3) once comprises a step of heat-curing the plurality of pre-set area blocks (32) of the adhesive layer (3) separately.
3. 3. The method for manufacturing an adhesive structure test block having a defect according to claim 2, further comprising a step of determining positions and areas of the plurality of pre-set area blocks (32) according to a pre-set position and a pre-set area of a defect before a step of independently heat-curing the plurality of pre-set area blocks (32) of the adhesive layer (3).
4. 3. The method for manufacturing a defective adhesive structure test block according to claim 2, wherein the step of independently heating and curing the plurality of pre-set area blocks (32) of the adhesive layer (3) is performed by a pre-curing device (5), the pre-curing device (5) comprising a heating plate (51) and a plurality of heating columns (52) movably arranged on the heating plate (51), and the positions of the plurality of heating columns (52) are adjusted to correspond to the positions of the plurality of pre-set area blocks (32) on the adhesive layer (3).
5. 2. The method for manufacturing a defective adhesive structure test block as described in claim 1, wherein the step of applying adhesive to the upper surface of the first plate (1) to form an adhesive layer includes a step of applying the adhesive to an area near an edge of the upper surface of the first plate (1) and overlapping the second plate (2) on the edge of the first plate (1).
6. 2. The method for manufacturing a defective adhesive structure test block according to claim 1, further comprising the steps of: performing a temperature-elevated rheological property test on the adhesive to obtain a rheological curve of the adhesive; and selecting a temperature for the first heat-curing step and a temperature for the second heat-curing step according to the rheological curve.
7. 2. The method for manufacturing a defective adhesive structure test block according to claim 1, wherein the step of applying adhesive to the upper surface of the first plate (1) comprises a step of applying the adhesive to an entire area of the upper surface of the first plate (1) to cover the upper surface of the first plate (1) with the adhesive layer (3), the at least a portion of the area comprising the entire area of the adhesive layer (3), and the manufacturing method further comprises a step of attaching the second plate (2) on top of the adhesive layer (3) and then heat-curing the adhesive layer (3) for a first time before the step of heat-curing the entire area of the adhesive layer (3) for a first time, and a step of separating the first plate (1) and the second plate (2) from the center of the adhesive layer (3), overlapping the separated first plate (1) and the second plate (2) and then heat-curing the adhesive layer (3) for a second time after the step of heat-curing the entire area of the adhesive layer (3) for a first time.
8. 8. The method for manufacturing a defective adhesive structure test block according to claim 7, wherein the steps of heat-curing the adhesive layer (3) for the first time and heat-curing the adhesive layer (3) for the second time are both performed by autoclave, the temperatures of the steps of heat-curing the adhesive layer (3) for the first time and heat-curing the adhesive layer (3) for the second time are the same, and the heating times of the steps of heat-curing the adhesive layer (3) for the first time and heat-curing the adhesive layer (3) for the second time are different.
9. The method for manufacturing a defective bonded structure test block according to claim 1, further comprising the step of generating a crack (33) in the adhesive layer (3).
10. 2. The method for manufacturing a defective adhesive structure test block according to claim 1, wherein the adhesive is an adhesive film, and the adhesive film is applied to the top surface of the first plate (1) to form the adhesive layer (3).
11. 2. A method for manufacturing a defective bonded structure test block as described in claim 1, wherein the first plate (1) and the second plate (2) are made of a composite material, and the composite material of the first plate (1) and the composite material of the second plate (2) are the same or different.
12. The method for manufacturing a defective bonded structure test block according to claim 1 , further comprising the step of: after obtaining the test block having defects, ultrasonically scanning the test block to obtain defect information.
Citation Information
Patent Citations
Detection structure and detection method for bonding quality
CN111208195A
An artificially defective cured laminate.
EP2769834A1
Composite articles with artificial defects and methods for making them
US20070028661A1
Magnet, magnet lamination, method for producing lamination magnet, and production system for lamination magnet
US20160059518A1