Petroleum resin composition, its production method, and rubber composition containing same

A low-viscosity resin composition, modified with a molecular weight regulator and viscosity modifier, addresses compatibility issues in tire tread compositions, enhancing braking, fuel efficiency, and wear resistance by improving processability and dispersion.

JP7590544B2Active Publication Date: 2024-11-26KOLON INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023504053
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2021-10-22
Publication Date
2024-11-26
Estimated Expiration
2041-10-22

Smart Images

  • Figure 0007590544000001
    Figure 0007590544000001
  • Figure 0007590544000002
    Figure 0007590544000002
  • Figure 0007590544000003
    Figure 0007590544000003
Patent Text Reader

Abstract

The present invention relates to a resin composition comprising a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one of both ends of an at least partially hydrogenated or non-hydrogenated petroleum resin, and having a viscosity of 5,000 cps to less than 50,000 cps at 25°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a resin composition, a method for producing the same, and a rubber composition, coating composition, paint composition and tire tread composition containing the same. [Background technology]

[0002] Tires support the load of a vehicle, absorb shocks from the road surface, and transmit the power and braking force of the automobile engine to the road surface, thereby maintaining the movement of the vehicle. There are various required characteristics that vehicle tires must satisfy, such as durability, wear resistance, rolling resistance, fuel economy, handling stability, ride comfort, braking performance, vibration, and noise.

[0003] The tire tread is the outermost part of the tire that comes into direct contact with the road surface and plays an important role in braking, fuel economy, wear, etc. The viscoelastic properties of tire tread rubber are used as an indicator of a tire's fuel economy and braking performance. When the hysteresis caused by contact with the ground and repeated deformation during driving is high, a lot of energy is lost as heat, which is detrimental to fuel economy but favorable to braking performance.

[0004] The performance of a tire tread is greatly influenced by the rubber composition that constitutes it, and in particular, is greatly influenced by the properties of the synthetic resin compounded therewith, in addition to the raw rubber.

[0005] There remains a need in the industry for synthetic resins, such as petroleum resins, that are not only highly compatible with the raw rubbers of tire tread compositions, but also provide improved braking, fuel economy, and wear performance. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a low-viscosity resin composition, a rubber composition containing the same, and uses thereof. [Means for solving the problem]

[0007] According to one embodiment, there is provided a resin composition comprising a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one of both ends of an at least partially hydrogenated or non-hydrogenated petroleum resin, and having a viscosity of 5,000 cps to less than 50,000 cps at 25°C.

[0008] According to another aspect, there is provided a rubber composition comprising raw rubber and the resin composition.

[0009] According to yet another aspect, there is provided a tire tread composition comprising the rubber composition.

[0010] According to yet another aspect, there is provided a method for producing a resin composition, the method comprising the step of adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, and a molecular weight modifier, to carry out a polymerization reaction, and obtaining a polymerization reaction product, The resin composition has a viscosity at 25°C of 5,000 cps to less than 50,000 cps. [Effects of the Invention]

[0011] The rubber composition according to the present invention contains a low-viscosity resin composition having a viscosity of 5,000 cps to less than 50,000 cps at 25°C, and therefore functions similarly to process oil during the raw material blending process, facilitating the dispersion of raw materials and shortening the blending time, which is advantageous from an economical standpoint.

[0012] Furthermore, the resin composition according to the present invention, which contains a petroleum resin or a hydrogenated petroleum resin modified with a molecular weight modifier and a viscosity modifier, has improved processability and, when applied to a tire tread composition, can solve the problems of improving tire braking, fuel economy, and wear resistance. DETAILED DESCRIPTION OF THE INVENTION

[0013] Various aspects and various embodiments of the present invention will be described in more detail below.

[0014] As used herein, "petroleum resin" includes polymers of one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer. For example, the petroleum resin includes homopolymers and copolymers. Examples of the petroleum resin homopolymer include a polymer of a C5 monomer, a polymer of a C5 mixed fraction, a polymer of a C9 monomer, a polymer of a C9 mixed fraction, a polymer of a cyclic diolefin monomer, and a polymer of a linear olefin monomer. Examples of the petroleum resin copolymer include copolymers of two different C5 monomers, copolymers of two different C9 monomers, copolymers of two different cyclic diolefin monomers, copolymers of two different linear olefin monomers, copolymers of a C5 fraction and a C5 monomer, copolymers of a C5 fraction and a C9 monomer, copolymers of a C9 fraction and a C5 monomer, copolymers of a C5 monomer and a C9 monomer, copolymers of a C9 fraction and a C5 monomer, copolymers of a C5 monomer and a C9 monomer, copolymers of a C9 fraction and a C9 monomer, copolymers of a C5 fraction and a linear olefin monomer, copolymers of a C9 fraction and a linear olefin monomer, copolymers of a C5 fraction and a cyclic diolefin monomer, copolymers of a C9 fraction and a cyclic diolefin monomer, copolymers of a C5 monomer and a cyclic diolefin monomer, copolymers of a C9 monomer and a linear olefin monomer, and copolymers of a cyclic diolefin monomer and a linear olefin monomer.

[0015] In this specification, the term "hydrogenated petroleum resin" refers to the above-mentioned petroleum resin in which at least a portion of unsaturated moieties such as ethylene has been modified to saturated hydrocarbons by a hydrogenation reaction.

[0016] As used herein, the term "C5 (mixed) fraction" refers to aliphatic C5 and C6 paraffins, olefins, and diolefins derived from naphtha cracking. For example, the C5 fraction may include, but is not limited to, pentene, isoprene, 2-methyl-2-butene, 2-methyl-2-pentene, cyclopentadiene, and piperylene, and may also include any mixture of two or more of the C5 monomers. The C5 fraction may also be selectively alkylated.

[0017] As used herein, the term "C5 monomer" refers to any one of the components contained in the aforementioned C5 (mixed) fraction.

[0018] As used herein, "C9 (mixed) fraction" refers to a composition derived from petroleum processing, e.g., cracking, that boils at atmospheric pressure and between about 100°C and 300°C, and is generally understood in the art to which the present invention pertains. 10 The C9 fraction may include olefin species, such as, but not limited to, vinyltoluene, α-methylstyrene, styrene, dicyclopentadiene, indene, trans-β-methylstyrene, and methylindene, and may also include mixtures of two or more of the C9 monomers. The C9 fraction may also be selectively alkylated. For example, the C9 fraction of the present invention may include vinyltoluene, indene, styrene, dicyclopentadiene, and alkylated derivatives of these components, such as α-methylstyrene and methylindene.

[0019] As used herein, the term "C9 monomer" refers to any one of the components contained in the aforementioned C9 fraction.

[0020] As used herein, "olefin" includes unsaturated compounds containing at least one ethylenically unsaturated (C=C) bond. For example, the olefin may include, but is not limited to, linear olefins, cyclic olefins, α-olefins, etc.

[0021] As used herein, "cyclic diolefin" includes cyclic unsaturated compounds containing two C=C bonds. For example, the cyclic diolefin can include, but is not limited to, dicyclopentadiene, tricyclopentadiene, and the like.

[0022] One aspect of the present invention relates to a method for producing a resin composition having a viscosity of 5,000 cps to less than 50,000 cps at 25°C, the method comprising the steps of: adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, and a molecular weight regulator, to carry out a polymerization reaction, and obtaining a polymerization reaction product.

[0023] According to an embodiment, the solution may further include a viscosity modifier, which facilitates adjustment of the viscosity of the polymerization reaction product.

[0024] The viscosity modifier does not participate in the formation of the structure of the product polymer, but serves to adjust the viscosity of the reactants and the product. Therefore, according to the present invention, a polymerization reaction is carried out by adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, a molecular weight modifier, and a viscosity modifier, and the resulting polymerization reaction product may be a mixture of a modified polymer and a viscosity modifier.

[0025] According to an embodiment, the method may further include a step of converting the petroleum resin into a hydrogenated petroleum resin by hydrotreating in the presence of a catalyst.

[0026] The catalyst used in the hydrotreating process may be a hydrogenation catalyst well known in the petroleum resin field, such as Pd, Ni, Pt, or a mixture thereof.

[0027] According to one embodiment, the molecular weight modifier may be included in an amount of more than 0 to 16 parts by weight per 100 parts by weight of the total resin composition, and the viscosity modifier may be included in an amount of more than 0 to 44 parts by weight per 100 parts by weight of the total resin composition.

[0028] For example, the molecular weight regulator may be included in an amount of 1 to 10 parts by weight, 1 to 5 parts by weight, 1 to 4 parts by weight, 1 to 2.5 parts by weight, or 1 to 1.5 parts by weight.

[0029] For example, the viscosity modifier may be included in an amount of 5 to 30 parts by weight, 5 to 25 parts by weight, 5 to 20 parts by weight, or 5 to 14.9 parts by weight.

[0030] When the contents of the molecular weight modifier and viscosity modifier satisfy the above ranges, it is possible to produce a low-viscosity petroleum resin that has good compatibility with raw rubber. Without the molecular weight modifier, a high-molecular-weight and high-viscosity petroleum resin is obtained. If the amount exceeds 15 parts by weight, the molecular weight becomes too small, the viscosity becomes too low, or the degree of polymerization becomes low, resulting in a decrease in yield. Furthermore, the viscosity modifier is added to lower the viscosity of the modified petroleum resin and can be added if necessary. However, if the amount exceeds 40 parts by weight, the ratio of aromaticity decreases due to a decrease in the ratio of resin polymerization components, which is undesirable because it reduces compatibility with the raw rubber.

[0031] According to one embodiment, the molecular weight regulator usable in the present invention is a chain transfer agent, and examples thereof include thiols or halocarbons such as carbon tetrachloride.

[0032] For example, the thiols, i.e., organic mercaptan molecular weight regulators containing one or more thiol groups (—SH), are useful, including aliphatic mercaptans, cycloaliphatic mercaptans, or aromatic mercaptans.

[0033] Such mercaptans may contain 1 to 4 thiol groups per molecule, and 1 to 20 carbons, preferably 1 to 15 carbons, per thiol group.

[0034] In addition to the hydrocarbon group and the thiol group, other substituents may be included. Examples of such substituents include a hydroxy group, a carboxylic acid group, an ether group, an ester group, a sulfide group, an amine group, an amide group, and the like.

[0035] In the present invention, the mercaptans useful as molecular weight regulators are not particularly limited as long as they are organic compounds having a thiol group, and specific examples include alkyl mercaptans such as ethyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, and dodecyl mercaptan; thiolphenols such as phenyl mercaptan and benzyl mercaptan; hydroxyl group- or carboxylic acid group-containing mercaptans such as 2-mercaptoethanol, thiol glycolic acid, and 3-mercaptopropionic acid; mercaptans having two or more functional groups such as pentaerythritol tetrakis(3-mercapto)propionate; and mixtures of two or more thereof.

[0036] Specific examples of such mercaptans include, but are not limited to, methyl mercaptan, ethyl mercaptan, butyl mercaptan, octyl mercaptan, lauryl mercaptan, mercaptoethanol, mercaptopropanol, mercaptobutanol, mercaptoacetic acid, mercaptopropionic acid, benzyl mercaptan, phenyl mercaptan, cyclohexyl mercaptan, 1-thioglycerol, 2,2'-dimercaptodiethyl ether, 2,2'-dimercaptodipropyl ether, 2,2'-dimercaptodiisopropyl ether, 3,3'-dimercaptodipropyl ether, 2,2'-dimercaptodiethyl sulfide, 3,3'-dimercaptodipropyl sulfide, bis(β-mercaptoethoxy)methane, bis(β-mercaptoethylthio)methane, trimethylolpropane trithioglycolate, pentaerythritol tetrathioglycolate, and the like.

[0037] According to one embodiment, the molecular weight regulator of the present invention includes ethyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan; phenyl mercaptan, benzyl mercaptan; mercaptoethanol, thiol glycolic acid, mercaptopropionic acid; and pentaerythritol tetrakis(3-mercapto)propionate.

[0038] For example, in the present invention, the effect of molecular weight control can be maximized by using n-dodecyl mercaptan of the following Chemical Formula 1, 2-mercaptoethanol of the following Chemical Formula 2, or a mixture thereof as a molecular weight control agent.

[0039] [ka]

[0040] [ka]

[0041] According to one embodiment, the viscosity modifier may be a low-viscosity liquid resin having a viscosity (25°C) of 20 to 500 cps. However, any liquid resin satisfying the above viscosity may be used as a viscosity modifier for a resin composition according to one embodiment of the present invention without any particular limitation.

[0042] For example, the low viscosity liquid resin may be selected from hydrogenated DCPD-C9 copolymer resin, hydrogenated DCPD resin, and a mixture thereof.

[0043] Here, the hydrogenated dicyclopentadiene (DCPD)-C9 copolymer resin refers to a white thermoplastic resin obtained by polymerization and hydrogenation of dicyclopentadiene (DCPD). As such a hydrogenated dicyclopentadiene (DCPD)-C9 copolymer resin, a commercially available resin such as SUKOREZ (registered trademark) resin can also be used.

[0044] For example, by using a hydrogenated dicyclopentadiene (DCPD)-C9 copolymer resin having the following structure as a viscosity modifier, the effects of viscosity control and improvement of air permeability resistance can be maximized.

[0045] [ka]

[0046] According to an embodiment, the polymerization catalyst may be selected from the group consisting of Lewis acid catalysts, halohydric acids, AlCl3, BF3, and mixtures of two or more thereof.

[0047] Preferably, the polymerization catalyst is a Lewis acid catalyst selected from AlCl3, BF3, SnCl4, TiCl4, AgClO4, I2, and a mixture of two or more thereof.

[0048] According to one embodiment, the application of heat may be performed by raising the temperature to 100°C to 300°C.

[0049] One aspect of the present invention relates to a resin composition comprising, at least a portion of a modified petroleum resin having a structure in which a molecular weight regulator is bound to at least one of both ends of a hydrogenated or non-hydrogenated petroleum resin, and a viscosity modifier, and having a viscosity at 25°C of 5,000 cps to less than 50,000 cps.

[0050] According to one embodiment, the modified petroleum resin is a petroleum resin obtained by polymerizing one or more of the C5 monomer, C5 mixed fraction, C9 monomer, C9 mixed fraction, cyclic diolefin monomer, and linear olefin monomer, and then modifying the at least partially hydrogenated or non-hydrogenated petroleum resin with the molecular weight modifier. By modifying the terminals of the petroleum resin with the molecular weight modifier, not only is it excellent in compatibility and blendability with rubber, but it can also be compatible with the amorphous region of the polymer to form a membrane, further improving processability and air permeability resistance. In contrast, if the terminals are not modified with a molecular weight modifier, the number average molecular weight increases, the glass transition temperature also increases, and compatibility with rubber becomes poor, resulting in poor blending. As a result, processability and final product performance deteriorate.

[0051] According to one embodiment, the modified petroleum resin has a structure in which one or more of the C5 monomer, C5 mixed fraction, C9 monomer, C9 mixed fraction, cyclic diolefin monomer, and linear olefin monomer are polymerized through an addition polymerization reaction or a chain polymerization reaction to obtain an at least partially hydrogenated or non-hydrogenated petroleum resin, and the molecular weight regulator is bound to at least one of both ends of the at least partially hydrogenated or non-hydrogenated petroleum resin.

[0052] For example, the petroleum resin may contain at least one unit structure derived from a C9 mixed fraction, or may be composed of repeating units derived from a C9 mixed fraction.

[0053] According to one embodiment, the unit structure derived from the C9 mixed fraction may include vinyltoluene, α-methylstyrene, styrene, dicyclopentadiene, indene, and methylindene.

[0054] According to one embodiment, the petroleum resin comprises a structure in which repeating units such as those represented by the following formula 4a are bonded: For example, the petroleum resin may comprise the following structure formed by the polymerization of monomers such as styrene, α-methylstyrene, vinyltoluene, indene, methylindene, dicyclopentadiene, and α-methylstyrene or methylindene contained in the C9 mixed fraction, or alkylated derivative monomers of these components.

[0055] [ka]

[0056] The above formula 4a is merely an exemplary representation, and in addition to the structure, repeating units derived from other C5 monomers, C9 monomers, cyclic diolefin monomers, and linear olefin monomers not shown may also be included.

[0057] For example, the petroleum resin is a polymer represented by the above structure, and the polymer means a random polymer, but is not limited thereto, and also includes a block copolymer or an alternating copolymer.

[0058] Although not specifically illustrated, the petroleum resin may include a structure in which at least one of the repeating units represented by Formula 4a is hydrogenated.

[0059] According to another embodiment, the petroleum resin may have a structure in which the following repeating units are bonded: For example, the petroleum resin may have a structure in which at least one of both ends has a double bond, and the structure in which both ends have a double bond is exemplarily represented by the following chemical formula 4b:

[0060] [ka]

[0061] In this way, a molecular weight modifier is bonded to at least one double bond located at the terminal to form a petroleum resin (e.g., a polymer of C9 monomers) modified with the molecular weight modifier. The molecular weight modifier may be bonded to either terminal, or may be bonded to only one terminal, as shown in the following exemplary formula 4c:

[0062] Although not separately illustrated, the petroleum resin may include a structure in which at least one of the repeating units represented by Formula 4b or 4c is hydrogenated.

[0063] [ka]

[0064] According to one embodiment, the resin composition has a number average molecular weight (Mn) of 150 to 300, a weight average molecular weight (Mw) of 300 to 500, and a Z average molecular weight (Mz) of 1,000 to 2,000.

[0065] If the number average molecular weight is lower than 150, when compounded with raw rubber, the rubber hardness becomes too low, resulting in a decrease in tire load performance, while if it is higher than 300, compounding processability may be reduced. In addition, such a low molecular weight range provides excellent processability and allows the compound to be used in rubber compositions for tire treads as a substitute for existing process oils, thereby improving processability, grip, and abrasion resistance.

[0066] According to one embodiment, the resin composition has polar properties, excellent processability, low crystallinity, and can be compatible with the amorphous region of the polymer to form a film, thereby further improving processability and compoundability. Also, in one embodiment of the rubber composition of the present invention, the resin composition has a viscosity of 5,000 to 50,000 cps at 25°C and a glass transition temperature of -40°C to -25°C.

[0067] If the glass transition temperature is lower than -40°C, when compounded with raw rubber, the rubber hardness becomes too low, resulting in a decrease in the tire's load-bearing performance. If the glass transition temperature is higher than -25°C, the rubber hardness becomes too high, resulting in a decrease in the tire's shock-absorbing performance and wet grip.

[0068] According to an embodiment, the resin composition may further include a viscosity modifier.

[0069] According to one embodiment, the viscosity modifier may be included in an amount of more than 0 and less than or equal to 40 parts by weight per 100 parts by weight of the resin composition.

[0070] As described above, according to one embodiment of the present invention, when the modified petroleum resin further contains a viscosity modifier, the modified petroleum resin is obtained by carrying out a polymerization reaction by adding a polymerization catalyst and / or heat to a solution containing one or more of a C5 monomer, a C5 mixed fraction, a C9 monomer, a C9 mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, a molecular weight modifier, and a viscosity modifier. However, the viscosity modifier does not participate in the structure formation of the modified petroleum resin product, but serves to adjust the viscosity of the reactants and the product, so the polymerization reaction product may be a mixture of the modified polymer and the viscosity modifier.

[0071] For details regarding the C5 monomer, C5 mixed fraction, C9 monomer, C9 mixed fraction, cyclic diolefin monomer, and linear olefin monomer, please refer to the above, and various specific examples of the molecular weight modifier, viscosity modifier, etc. are as described above.

[0072] According to one embodiment, the resin composition may have a viscosity of 5,000 to 15,000 cps measured at 25°C and an aromaticity of 15% to 50%, for example, 24% to 47%, or 30% to 40%.

[0073] When the aromaticity range is satisfied, the compound has excellent compatibility with raw rubber, and therefore can be used in tire tread applications that require excellent ground contact and durability, and in paint compositions that require excellent coatability and weather resistance, but is not limited to such applications.

[0074] One aspect of the present invention relates to a rubber composition comprising a raw rubber and a resin composition according to various embodiments of the present invention.

[0075] According to an embodiment, the rubber composition may further include at least one of a raw rubber, a reinforcing agent, a silane coupling agent, a vulcanizing agent, and a vulcanization accelerator, in addition to the modified petroleum resin and the viscosity modifier.

[0076] The raw rubber may include natural rubber, synthetic rubber, or a combination thereof having olefinic double bonds.

[0077] The raw rubber is not particularly limited as long as it has an olefinic double bond (carbon-carbon double bond), and natural rubber, synthetic rubber, or a mixture thereof can be used.

[0078] For example, the raw rubber may include at least one selected from the group consisting of natural rubber, butadiene rubber, nitrile rubber, silicone rubber, isoprene rubber, styrene-butadiene rubber (SBR), isoprene-butadiene rubber, styrene-isoprene-butadiene rubber, acrylonitrile-butadiene rubber (NBR), ethylene-propylene-diene rubber, halogenated butyl rubber, halogenated isoprene rubber, halogenated isobutylene copolymer, chloroprene rubber, butyl rubber, and halogenated isobutylene-p-methylstyrene rubber.

[0079] The reinforcing agent may include carbon black and silica.

[0080] By including carbon black, the rubber composition can obtain effects such as improved abrasion resistance, improved rotation resistance, prevention of cracks and cracks caused by ultraviolet rays (prevention of ultraviolet degradation), etc. The carbon black that can be used in the present invention is not particularly limited, and any carbon black that is commonly used in the technical field can be used.

[0081] According to an embodiment, the carbon black may include furnace black, acetylene black, thermal black, channel black, graphite, or a combination thereof.

[0082] For example, the physical properties of the carbon black, such as particle size, pore volume, and specific surface area, are not particularly limited, and may include various carbon blacks conventionally used in the rubber industry, such as SAF, ISAF, HAF, FEF, GPF, and SRF (all of which are abbreviations for carbon blacks classified in the American ASTM standard D-1765-82a).

[0083] The silica may be any silica used as a reinforcing agent for rubber, without any particular limitation, and examples thereof include dry process white carbon, wet process white carbon, synthetic silicate white carbon, colloidal silica, precipitated silica, etc. The specific surface area of ​​the silica is not particularly limited, but is usually 40 to 600 m 2 / g, e.g., 70 to 300 m 2 / g, and those having a primary particle diameter of 10 to 1,000 nm can be used. They may be used alone or in combination of two or more.

[0084] In addition to the carbon black and silica, the reinforcing agent may be mineral powders such as clay and talc; carbonates such as magnesium carbonate and calcium carbonate; alumina hydrates such as aluminum hydroxide; and the like.

[0085] According to one embodiment, the silane coupling agent is used to incorporate silica, and may be selected from the group consisting of vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, bis(3-(triethoxysilyl)propyl)disulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-(triethoxysilyl)propyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyl The silane may comprise trimethoxysilane, 2-mercaptoethyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzolyl tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, 3-trimethoxysilylpropyl methacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, dimethoxymethylsilylpropyl benzothiazolyl tetrasulfide, or a combination thereof. For example, the silane coupling agent may include bis(3-(triethoxysilyl)propyl)tetrasulfide.

[0086] The crosslinking agent may be any agent that is commonly used for crosslinking rubber, without any particular limitation, and may be appropriately selected depending on the rubber component and the isobutylene polymer.

[0087] According to an embodiment, examples of the crosslinking agent include sulfur crosslinking agents such as sulfur, morpholine disulfide, and alkylphenol disulfide; and organic peroxide crosslinking agents such as cyclohexanone peroxide, methyl acetoacetate peroxide, tert-butyl peroxyisobutyrate, tert-butyl peroxybenzoate, benzoyl peroxide, lauroyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, and 1,3-bis(tert-butylperoxyisopropyl)benzene.

[0088] In addition to the crosslinking agent, the rubber composition for a tire tread according to the present invention may contain a vulcanization accelerator or a vulcanization aid.

[0089] According to an embodiment, the vulcanization accelerator and vulcanization aid are not particularly limited and may be appropriately selected depending on the rubber component, isobutylene polymer, and crosslinking agent contained in the rubber composition. Furthermore, "vulcanization" refers to crosslinking involving at least one sulfur atom.

[0090] Examples of the vulcanization accelerator include thiuram accelerators such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, and tetraethylthiuram disulfide; thiazole accelerators such as 2-mercaptobenzothiazole and dibenzothiazyl disulfide; sulfenamide accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide and N-oxydiethylene-2-benzothiazolylsulfenamide; aldehyde-amine accelerators such as n-butylaldehyde-aniline condensation products and butyraldehyde-monobutylamine condensation products; aldehyde-ammonia accelerators such as hexamethylenetetramine; and thiourea accelerators such as thiocarbanilide. When these vulcanization accelerators are used, one type may be used alone, or two or more types may be used in combination.

[0091] Examples of the vulcanization aid include metal oxides such as zinc oxide (zinc white) and magnesium oxide; metal hydroxides such as potassium hydroxide; metal carbonates such as zinc carbonate and basic zinc carbonate; fatty acids such as stearic acid and oleic acid; aliphatic metal salts such as zinc stearate and magnesium stearate; amines such as n-butylamine and dicyclohexylamine; ethylene dimethacrylate, diallyl phthalate, N,Nm-phenylenedimaleimide, triallyl isocyanurate, trimethylolpropane trimethacrylate, etc. When these vulcanization aids are blended, one type may be used alone, or two or more types may be used in combination.

[0092] Furthermore, the rubber composition according to the present invention may contain, as necessary, one or more of various additives used in the rubber industry, such as antioxidants, vulcanization retarders, peptizers, process oils, plasticizers, etc.

[0093] Additionally, the present invention provides a rubber molded article produced from the rubber composition.

[0094] The rubber molded article according to an embodiment of the present invention may be a tire. For example, the rubber molded article may be a tire tread. The tire tread is manufactured into a tire by selecting an appropriate blending ratio of raw materials in consideration of the use and physical properties of the tire and using a known method.

[0095] According to one embodiment, the rubber composition according to the present invention may be prepared by kneading the above components using a kneading machine such as a plastomill, a Banbury mixer, a roll, an internal mixer, etc. Specifically, it is preferable to knead the above components except for the crosslinking agent and the vulcanization accelerator, and then add the crosslinking agent and the vulcanization accelerator to the resulting kneaded mixture, followed by further kneading.

[0096] The rubber composition produced by the above method can be used as a material for forming the tread portion (and the cap portion including the tread portion) that comes into contact with the road surface. Regarding the production method, the rubber composition is extruded according to the shape of the tire (specifically, the shape of the tread) into which it must be formed, and molded in a tire building machine by a conventional method to produce an uncrosslinked molded body for a tire. This uncrosslinked molded body for a tire is then heated and pressurized, for example, in a vulcanizer to produce a tire tread, and the desired tire can be manufactured by combining this tire tread with other components.

[0097] The tires manufactured in this way have excellent mechanical properties (hardness, tensile strength, modulus, etc.), chip break resistance, and adhesion, which are essential for tires. In particular, they have high grip (wet / dry), excellent driving stability and braking performance, and low rolling resistance, which can realize low fuel consumption.

[0098] Therefore, the rubber composition of the present invention is suitable as a rubber composition for obtaining treads of tires such as fuel-efficient tires and high-performance tires.

[0099] One aspect of the present invention relates to coating compositions that include a base resin and a resin composition according to various embodiments of the present invention.

[0100] According to an embodiment, the coating composition may include a curing agent, a curing accelerator, a pigment, an additive, and a solvent in addition to the base resin and the resin composition.

[0101] The coating composition may be free of plasticizers by using a low viscosity resin composition.

[0102] According to an embodiment, the base resin may include an epoxy resin.

[0103] According to an embodiment, the curing agent may include a known heat-curing agent, a photo-curing agent, or a UV-curing agent, and may be appropriately selected depending on the application.

[0104] According to an embodiment, the curing accelerator is added to adjust the curing speed of the curing agent, and may be appropriately selected from known curing accelerators, including sulfonic acid curing catalysts and carbamate curing catalysts, as needed.

[0105] According to one embodiment, the pigment is added to provide color to the coating composition or to improve whiteness, and may include, but is not limited to, inorganic pigments such as titanium dioxide. Any known pigment may be appropriately selected and used. For example, the resin composition according to one embodiment of the present invention may have a Gardner color scale of 11 or less, e.g., 1 to 11, thereby reducing the amount of pigment added, thereby improving economic efficiency.

[0106] According to one embodiment, the additives may include all components that can be incorporated into paints, excluding curing agents, curing accelerators, pigments, and solvents. For example, the additives may include surface conditioners, light stabilizers, weathering additives, preservatives, appearance control agents, defoamers, leveling agents, or combinations thereof. Such additives may be appropriately selected from known materials.

[0107] According to an embodiment, the solvent may be selected from solvents that have good miscibility with the coating material, for example, an organic solvent may be used.

[0108] The raw materials to be blended into the above-mentioned coating composition can be appropriately blended by a person skilled in the art, taking into consideration the intended use, desired viscosity, hue, etc., and referring to known compositions.

[0109] The present invention will be described in more detail below through examples, etc. However, the following examples should not be construed as narrowing or limiting the scope and content of the present invention. Furthermore, based on the disclosure of the present invention including the following examples, it is clear that a person skilled in the art can easily practice the present invention, even though no specific experimental results have been presented, and it goes without saying that such variations and modifications fall within the scope of the claims.

[0110] Furthermore, the experimental results presented below are only representative experimental results of the examples and comparative examples, and the respective effects of various embodiments of the present invention that are not explicitly presented below will be specifically described in the relevant sections.

[0111] Example 1: Production of resin composition To 83.86 parts by weight of purified C9 fraction (YNCC), 14.80 parts by weight of viscosity modifier LP-A180 (Kolon Industries) and 1.34 parts by weight of molecular weight modifier n-dodecyl mercaptan were added, and then 30.21 parts by weight of polymerization catalyst BF was added and the polymerization reaction was carried out for 2 hours at 180°C. After the polymerization was completed, the polymer was degassed to remove unreacted reactants, and a resin composition was produced.

[0112] Example 2 and Comparative Examples 1 to 3: Preparation of Resin Compositions A resin composition was prepared in the same manner as in Example 1, except that the contents of the purified C9 fraction, viscosity modifier and molecular weight modifier were adjusted as shown in Table 1 below.

[0113] <Evaluation example 1: Viscosity measurement> A Brookfield viscometer was used. Spindle No. 27 was used, and 10.5 g samples of the resin compositions prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were placed in the chamber. After a stabilization time of 30 minutes at 25°C, the RPM value of the stirring shaft was adjusted, and the viscosity values ​​at 50% torque were recorded in Table 1 below.

[0114] <Evaluation Example 2: Gardner Hue Measurement> The color of the resin compositions prepared in Examples 1 and 2 and Comparative Examples 1 to 3 was measured according to ASTM D 1544. Specifically, the resin compositions were placed in a rectangular quartz cell (20 mm wide, 40 mm long, and 10 mm long). The cell was then attached to a PFX 195 colorimeter, which was then operated to measure the Gardner color, and the results were recorded in Table 1 below.

[0115] <Evaluation Example 3: Aromaticity Evaluation> The aromaticity of the resin compositions prepared in Examples 1 and 2 and Comparative Examples 1 to 3 was confirmed by NMR analysis, and the results are shown in Table 1 below.

[0116] [Table 1]

[0117] <Evaluation Example 4: Molecular Weight Evaluation> The polystyrene-equivalent weight-average molecular weight (Mw), number-average molecular weight (Mn), Z-average molecular weight (Mz), and polydispersity (MWD) of the resin compositions prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were determined by gel permeation chromatography (GPC; size exclusion chromatography (SEC)) (Model HP-1100; product of Hewlett-Packard). The polymers to be measured were dissolved in tetrahydrofuran to a concentration of 4,000 ppm, and 100 μL was injected into the GPC. The mobile phase for the GPC was tetrahydrofuran, with a flow rate of 1.0 mL / min. Analysis was performed at 30 °C. Three PIgel (Agilent Technologies) columns (1,000 + 500 + 100 Å) were connected in series. An RI detector (HP-1047A (Hewlett-Packard)) was used as the detector, and measurements were performed at 30 °C. The results are shown in Table 2 below.

[0118] [Table 2]

[0119] As can be seen from Tables 1 and 2 above, it was confirmed that the examples containing the molecular weight regulator easily satisfied the appropriate viscosity range, Gardner color, and molecular weight range.

Claims

1. The present invention includes a modified petroleum resin having a structure in which a molecular weight regulator is bonded to at least one of both ends of an at least partially hydrogenated or non-hydrogenated petroleum resin, A petroleum resin composition having a viscosity at 25°C of 5,000 cps to less than 50,000 cps, The molecular weight regulator comprises a mercaptan compound containing one or more thiol groups, The petroleum resin composition has an aromaticity of 24% to 47%, the aromaticity being a content of aromatic compound monomers contained in the petroleum resin composition.

2. The modified petroleum resin is 9 The petroleum resin composition according to claim 1, comprising at least one unit structure derived from a mixed fraction.

3. Said C 9 The petroleum resin composition according to claim 2, wherein the unit structure derived from the mixed fraction includes vinyltoluene, α-methylstyrene, styrene, dicyclopentadiene, indene, beta-trans-methylstyrene and methylindene.

4. The petroleum resin composition according to claim 1, wherein the modified petroleum resin has a structure in which a molecular weight regulator is bonded to both ends.

5. The petroleum resin composition comprises: The number average molecular weight (Mn) is 150 to 300; The weight average molecular weight (Mw) is 300 to 500; Z-average molecular weight (Mz) is 1,000 to 2,000; The petroleum resin composition according to claim 1, having a glass transition temperature of -40 to -25°C.

6. The petroleum resin composition according to claim 1, wherein the mercaptan compound is selected from the group consisting of ethyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan; phenyl mercaptan, benzyl mercaptan; mercaptoethanol, thiol glycolic acid, mercaptopropionic acid; pentaerythritol tetrakis(3-mercapto)propionate; or any mixture thereof.

7. The petroleum resin composition according to claim 1, further comprising a viscosity modifier.

8. The petroleum resin composition according to claim 7, wherein the viscosity modifier comprises a low-viscosity liquid resin having a viscosity of 20 to 500 cps at 25°C.

9. The low viscosity liquid resin is hydrogenated dicyclopentadiene (DCPD)-C 9 9. The petroleum resin composition of claim 8, wherein the petroleum resin is selected from the group consisting of copolymer resins, hydrogenated dicyclopentadiene (DCPD), and mixtures thereof.

10. The molecular weight regulator is contained in an amount of more than 0 and not more than 15 parts by weight per 100 parts by weight of the total petroleum resin composition, The petroleum resin composition according to claim 7, wherein the viscosity modifier is contained in an amount of more than 0 and not more than 40 parts by weight per 100 parts by weight of the petroleum resin composition.

11. The petroleum resin composition comprises:

2. The petroleum resin composition according to claim 1, having a viscosity measured at 25° C. of 5,000 to 15,000 cps.

12. C 5 Monomer, C 5 Distillate, C 9 Monomer, C 9 A method for producing a petroleum resin composition, comprising the steps of: adding a polymerization catalyst and / or heat to a solution containing a mixed fraction, at least one of a cyclic diolefin monomer and a linear olefin monomer, and a molecular weight regulator to carry out a polymerization reaction, thereby obtaining a polymerization reaction product; The petroleum resin composition has a viscosity at 25°C of 5,000 cps to less than 50,000 cps; The molecular weight regulator comprises a mercaptan compound containing at least one thiol group, The petroleum resin composition has an aromaticity of 24% to 47%, and the aromaticity is a content of aromatic compound monomers contained in the petroleum resin composition.

13. The solution is 9 The C 9 The method for producing a petroleum resin composition according to claim 12, wherein the mixed fraction contains vinyltoluene, α-methylstyrene, styrene, dicyclopentadiene, indene and methylindene.

14. The method for producing a petroleum resin composition according to claim 12, wherein the solution further contains a viscosity modifier.

15. The method for producing a petroleum resin composition according to claim 14, wherein the viscosity modifier comprises a low-viscosity liquid resin having a viscosity of 20 to 500 cps at 25°C.

16. The molecular weight regulator is contained in an amount of more than 0 and not more than 15 parts by weight per 100 parts by weight of the total petroleum resin composition, The method for producing a petroleum resin composition according to claim 14, wherein the viscosity modifier is contained in an amount of more than 0 and not more than 40 parts by weight per 100 parts by weight of the total petroleum resin composition.

17. The polymerization catalyst is AlCl 3 , B.F. 3 , SnCl 4 , TiCl 4 , AgClO 4 , I 2 and a mixture of two or more of them.

18. The method for producing a petroleum resin composition according to claim 12, wherein the heat addition is carried out by raising the temperature to 100°C to 300°C.

19. The polymerization reaction product comprises a mixture of a modified petroleum resin and a viscosity modifier; The modified petroleum resin is converted into the above-mentioned C 5 Monomer, C 5 Mixed fraction, C 9 Monomer, C 9 The method for producing a petroleum resin composition according to claim 14, wherein the molecular weight regulator is bonded to at least one of both ends of a petroleum resin obtained by polymerizing one or more of a mixed fraction, a cyclic diolefin monomer, and a linear olefin monomer, and at least a portion of the petroleum resin is hydrogenated or non-hydrogenated.

20. Raw rubber; A rubber composition comprising the petroleum resin composition according to any one of claims 1 to 11.

21. A tire tread composition comprising the rubber composition of claim 20.

Citation Information

Patent Citations

  • Water soluble C#-[9] petroleum resin terpolymers with scale-inhibiting property and preparation process thereof

    CN1594383A

  • Thermal polymerization of dicyclopentadiene

    JP1996048723A

  • Copolymer and its production

    JP1999130820A

  • Rubber composition and pneumatic tire using the same

    JP2015189873A

  • Resin composition and molded article

    JP2019178190A