Magnetic Recording Media

The magnetic recording medium with ε iron oxide particles and additives addresses the challenge of balancing coercive force and magnetization, enhancing both electromagnetic conversion and long-term reliability.

JP7590738B2Active Publication Date: 2024-11-27SONY GROUP CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021572760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-21
Filing Date
2021-01-20
Publication Date
2024-11-27
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

Existing tape-shaped magnetic recording media face challenges in achieving both high electromagnetic conversion characteristics and long-term reliability, particularly due to the trade-off between coercive force and mass magnetization of ε iron oxide particles.

Method used

A magnetic recording medium with a magnetic layer containing ε iron oxide particles, where the ratio of residual magnetic force to perpendicular coercive force (Hrp/Hc) is less than 2.0 and saturation magnetization per unit area is 4.5 mA or more, optimized with additives like cobalt and zirconium to enhance coercive force and mass magnetization.

Benefits of technology

The solution achieves improved electromagnetic conversion characteristics and high long-term reliability by maintaining a balanced Hrp/Hc ratio and enhancing magnetic properties, ensuring stable signal retention over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590738000002
    Figure 0007590738000002
  • Figure 0007590738000003
    Figure 0007590738000003
  • Figure 0007590738000004
    Figure 0007590738000004
Patent Text Reader

Abstract

Provided is a magnetic recording medium capable of balancing improving electromagnetic conversion properties and ensuring high long-term reliability. This magnetic recording medium has a magnetic layer and a substrate. The magnetic layer has a magnetic powder which contains ε-iron oxide. The ratio (Hrp / Hc) of the remanent coercivity (Hrp), which is measured in a direction perpendicular to the magnetic recording medium by using a pulse magnetic field, to the perpendicular coercivity (Hc) of the magnetic recording medium is no more than 2.0. The saturation magnetization (Mst) per unit area of the magnetic recording medium is at least 4.5mA.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to magnetic recording media. [Background technology]

[0002] Tape-type magnetic recording media are widely used for storing electronic data. For example, Patent Document 1 proposes a magnetic recording medium that has excellent electromagnetic conversion characteristics in a high-temperature environment. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 203468 Summary of the Invention

[0004] Incidentally, such tape-type magnetic recording media are expected to have improved electromagnetic conversion characteristics and high long-term reliability.

[0005] Therefore, there is a demand for a magnetic recording medium that can simultaneously improve electromagnetic conversion characteristics and ensure high long-term reliability.

[0006] A magnetic recording medium according to an embodiment of the present disclosure includes a magnetic layer and a substrate. The magnetic layer includes magnetic powder containing ε-iron oxide. The ratio (Hrp / Hc) of the remanent coercivity (Hrp) measured using a pulsed magnetic field to the perpendicular coercivity (Hc) of the magnetic recording medium is 2.0 or less, and the saturation magnetization (Mst) per unit area of ​​the magnetic recording medium is 4.5 mA or more.

[0007] Since the magnetic recording medium according to an embodiment of the present disclosure has the above-mentioned configuration, it is possible to achieve both improved electromagnetic conversion characteristics and improved thermal stability. [Brief description of the drawings]

[0008] [Figure 1]1 is a cross-sectional view of a magnetic recording medium according to an embodiment of the present disclosure. [Diagram 2] 2 is a schematic diagram showing an example of a diffraction pattern measured by in-plane X-ray diffraction (Cu tube) in the magnetic layer shown in FIG. 1. [Figure 3A] 2 shows an example of a magnetization curve (MH loop) in the magnetic layer shown in FIG. [Figure 3B] 1 shows an example of a magnetization curve (MH loop) in a magnetic layer as a reference example. [Figure 4] FIG. 2 is a cross-sectional view that typically illustrates the cross-sectional structure of an ε iron oxide particle contained in the magnetic layer shown in FIG. [Diagram 5] 2 is a characteristic diagram showing an example of a remanent magnetization curve for measuring the remanent coercivity of the magnetic recording medium shown in FIG. [Figure 6] FIG. 11 is a cross-sectional view that typically illustrates a cross-sectional structure of an ε-iron oxide particle as a modified example. [Figure 7] FIG. 11 is a cross-sectional view of a magnetic recording medium as another modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The description will be made in the following order. 1. Background 2. One embodiment 2-1. Structure of magnetic recording media 2-2. Manufacturing method of magnetic recording media 2-3.Effects 3. Variations

[0010] <1. Background> First, the background to the creation of the technology of the present disclosure will be described. Up to now, the use of ε iron oxide as a magnetic powder constituting the magnetic layer of a magnetic recording medium has been considered. To achieve high density recording in a magnetic recording medium, it is desirable to make the magnetic powder finer, and this ε iron oxide has a high coercive force even when made finer. However, since the mass magnetization of ε iron oxide is small, the output and thermal stability of the magnetic recording medium are insufficient. The decrease in thermal stability can be avoided by setting the ratio Hrp / Hc to 2.0 or less, which will be described later. Furthermore, if the ratio Hrp / Hc is 2.0 or less, the signal attenuation rate after 10 years, which will be described later, is improved, and long-term reliability can be ensured. Therefore, the present disclosure proposes a magnetic recording medium that employs a magnetic layer containing, for example, ε iron oxide, and simultaneously improves the electromagnetic conversion characteristics and thermal stability, i.e., ensures long-term reliability.

[0011] <2. One embodiment> [2-1 Configuration of the magnetic recording medium 10] FIG. 1 shows an example of a cross-sectional configuration of a magnetic recording medium 10 according to an embodiment of the present disclosure. As shown in FIG. 1, the magnetic recording medium 10 has a laminated structure in which multiple layers are laminated. Specifically, the magnetic recording medium 10 includes a long tape-shaped substrate 11, an underlayer 12 provided on one main surface 11A of the substrate 11, a magnetic layer 13 provided on the underlayer 12, and a back layer 14 provided on the other main surface 11B of the substrate 11. A surface 13S of the magnetic layer 13 is the surface against which the magnetic head will run while contacting it. The underlayer 12 and the back layer 14 are provided as necessary and may not be required. The average thickness of the magnetic recording medium 10 may be, for example, 5.6 μm or less.

[0012] The magnetic recording medium 10 is in the form of a long tape, and runs along its own longitudinal direction during recording and reproducing operations. The magnetic recording medium 10 is preferably used in a recording and reproducing device equipped with a ring-type head as a recording head, for example.

[0013] (Base 11) The substrate 11 is a non-magnetic support that supports the underlayer 12 and the magnetic layer 13. The substrate 11 is in the form of a long film. The upper limit of the average thickness of the substrate 11 is preferably 4.2 μm or less, and more preferably 4.0 μm or less. When the thickness is 3 μm or less, the recording capacity that can be recorded in one data cartridge can be made higher than that of a general magnetic recording medium. The lower limit of the average thickness of the substrate 11 is preferably 3 μm or more, and more preferably 3.2 μm or more. When the lower limit of the average thickness of the substrate 11 is 3 μm or more, a decrease in the strength of the substrate 11 can be suppressed.

[0014] The average thickness of the substrate 11 is obtained as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, layers other than the substrate 11 of the sample, i.e., the underlayer 12, the magnetic layer 13, and the back layer 14, are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample substrate 11 is measured at five or more positions using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device. Then, the measured values ​​are simply averaged (arithmetic average) to calculate the average thickness of the substrate 11. Note that the measurement positions are selected randomly from the sample.

[0015] The base 11 contains, for example, polyesters as a main component. Alternatively, the base 11 may contain PEEK (polyether ether ketone) as a main component. In addition to polyesters or PEEK, the base 11 may contain at least one of polyolefins, cellulose derivatives, vinyl resins, and other polymer resins. When the base 11 contains two or more of the above materials, the two or more materials may be mixed, copolymerized, or laminated.

[0016] The polyesters contained in the base 11 include, for example, at least one of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate.

[0017] The polyolefins contained in the base 11 include, for example, at least one of PE (polyethylene) and PP (polypropylene). The cellulose derivatives include, for example, at least one of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate) and CAP (cellulose acetate propionate). The vinyl resins include, for example, at least one of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).

[0018] Other polymer resins contained in the base 11 include, for example, at least one of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, such as Zylon (registered trademark)), polyether, PEK (polyetherketone), polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).

[0019] (Magnetic layer 13) The magnetic layer 13 is a recording layer for recording signals, and contains, for example, iron oxide containing an ε-iron oxide phase. The magnetic layer 13 contains, for example, magnetic powder, a binder, and a lubricant. The magnetic layer 13 may further contain additives such as conductive particles, an abrasive, and an anti-rust agent, as necessary.

[0020] As the magnetic layer 13 contains the ε iron oxide phase, the magnetic recording medium 10 exhibits a first peak PK1 at 32.9° and a second peak PK2 at 36.6° in a diffraction pattern by in-plane X-ray diffraction (Cu tube), as illustrated in FIG. 2. FIG. 2 is a schematic diagram of an example of a diffraction pattern of the magnetic recording medium 10 measured by in-plane X-ray diffraction (Cu tube). The peak positions of the diffraction pattern shown in FIG. 2 are determined using any analysis software attached to the X-ray diffraction (XRD) device. At this time, certain processing required for analysis, such as averaging the obtained diffraction pattern, may be performed. Thus, the fact that the first peak PK1 at 32.9° and the second peak PK2 at 36.6° are detected in the diffraction pattern by in-plane X-ray diffraction (Cu tube) of the magnetic layer 13 indicates that the magnetic layer 13 contains the ε iron oxide phase. By including ε iron oxide as magnetic powder, the magnetic layer 13 has a high perpendicular coercive force Hc. The in-plane XRD measurement is carried out as follows. The measurement sample is prepared by cutting out any data area from the magnetic tape wound inside the cartridge. The cut-out size is, for example, 12.65 mm x 60 mm. The cut-out sample is attached to an amorphous glass substrate, and the glass substrate is fixed to the XRD measurement stage using grease. The alignment adjustment and other necessary measurement procedures are performed before in-plane XRD measurement. The measurement conditions are as follows: Device name: Rigaku ATX-G Tube (X-ray source): Cu Kα Tube power: 50 kV, 200 mA Step (2θ): 0.05 degree Step speed: 1.5 degree / sec

[0021] In addition, the saturation magnetization Mst per unit area of ​​the magnetic recording medium 10 is preferably 4.5 mA or more. By making the saturation magnetization Mst per unit area of ​​the magnetic recording medium 10 4.5 mA or more, the output of the magnetic recording medium 10 can be further improved, and as a result, a good SNR (Signal-to-Noise Ratio) can be realized. This is because the larger the saturation magnetization Mst per unit area of ​​the magnetic layer 13, the more the output of the magnetic recording medium 10 improves, and the influence of the system noise of the magnetic head itself becomes relatively small. In addition, the saturation magnetization Mst per unit area of ​​the magnetic layer 13 can be adjusted by adjusting the filling amount and composition of the magnetic powder contained in the magnetic layer 13. For example, the saturation magnetization Mst per unit area of ​​the magnetic layer 13 can be increased by reducing non-magnetic components such as binders contained in the magnetic layer 13. In addition, by adjusting the composition of the magnetic powder, for example by replacing part of the iron (Fe) in the ε iron oxide particles with an additive element such as cobalt (Co), or by adjusting the synthesis conditions of the magnetic powder (such as the firing temperature), the mass magnetization of the magnetic powder can be increased, and the saturation magnetization Mst per unit area of ​​the magnetic layer 13 can be increased.

[0022] The saturation magnetization Mst per unit area of ​​the magnetic layer 13 is found as follows. First, three magnetic recording media 10 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to create a measurement sample. At this time, markings are made with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic recording medium 10 can be identified. Then, the MH loop of the measurement sample (entire magnetic recording medium 10) corresponding to the perpendicular direction (thickness direction) of the magnetic recording medium 10 is measured using a vibrating sample magnetometer (VSM).

[0023] Next, the coating film, i.e., the undercoat layer 12, the magnetic layer 13, and the back layer 14, are wiped off with acetone or ethanol, leaving only the substrate 11. Three of the obtained substrates 11 are then stacked together with double-sided tape, and punched out with a φ6.39 mm punch to obtain a sample for background correction (hereinafter simply referred to as a correction sample). Then, the MH loop of the correction sample (substrate 11) corresponding to the perpendicular direction of the substrate 11 (perpendicular direction of the magnetic recording medium 10) is measured using a VSM.

[0024] The MH loop of the measurement sample (whole magnetic recording medium 10) and the MH loop of the correction sample (substrate 11) are measured using, for example, a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Kogyo Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.

[0025] After the two MH loops are obtained, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 10), and the MH loop after background correction is obtained. The measurement and analysis program attached to the "VSMP7-15" is used for the calculation of this background correction.

[0026] The saturation magnetization Ms (emu) of the MH loop after background correction and the area (cm 2 ) the saturation magnetization per unit area Mst is calculated using the following formula: Mst(mA)=Ms(emu) / area(cm 2 ) x 10000

[0027] The area of ​​the sample is calculated according to the following formula: Area (cm 2 )=3.14×(0.639 / 2) 2 ×3

[0028] It should be noted that all of the above MH loop measurements are performed at 25° C. Furthermore, when the MH loop is measured in the perpendicular direction to the magnetic recording medium 10, no “demagnetization field correction” is performed.

[0029] The magnetic layer 13 has, for example, a surface 13S on which a large number of recesses are provided. A lubricant is stored in these recesses. It is preferable that the large number of recesses extend in a direction perpendicular to the surface of the magnetic layer 13. This is because this can improve the supply of the lubricant to the surface 13S of the magnetic layer 13. Note that some of the large number of recesses may extend in the vertical direction.

[0030] The upper limit of the average thickness of the magnetic layer 13 is preferably 90 nm or less, particularly preferably 80 nm or less, more preferably 70 nm or less, and even more preferably 50 nm or less. When the upper limit of the average thickness of the magnetic layer 13 is 90 nm or less, when a ring-type head is used as the recording head, magnetization can be recorded uniformly in the thickness direction of the magnetic layer 13, thereby improving the electromagnetic conversion characteristics.

[0031] The lower limit of the average thickness of the magnetic layer 13 is preferably 35 nm or more. If the upper limit of the average thickness of the magnetic layer 13 is 35 nm or more, output can be ensured when an MR head is used as the reproducing head, and therefore the electromagnetic conversion characteristics can be improved.

[0032] The average thickness of the magnetic layer 13 is determined as follows. First, a carbon film is formed by vapor deposition on the surface 13S of the magnetic layer 13 and the surface 14S of the back layer 14 of the magnetic recording medium 10, and then a tungsten thin film is further formed by vapor deposition on the carbon film covering the surface 13S of the magnetic layer 13. These carbon and tungsten films protect the sample during the thinning process described below.

[0033] Next, the magnetic recording medium 10 is processed by a FIB (Focused Ion Beam) method or the like to be sliced. When the FIB method is used, a carbon film and a tungsten thin film are formed as protective films as a pretreatment for observing a TEM image of the cross section described later. The carbon film is formed on the magnetic layer side surface and the back layer side surface of the magnetic recording medium 10 by a vapor deposition method, and the tungsten thin film is further formed on the magnetic layer side surface by a vapor deposition method or a sputtering method. The slice is performed along the length direction (longitudinal direction) of the magnetic recording medium 10. That is, the slice forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic recording medium 10. The cross section of the obtained sliced ​​sample is observed under the following conditions by a transmission electron microscope (TEM) to obtain a TEM image. The magnification and acceleration voltage may be appropriately adjusted depending on the type of device. Equipment: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000x

[0034] Next, using the obtained TEM image, the thickness of the magnetic layer 13 is measured at at least 10 positions in the longitudinal direction of the magnetic recording medium 10. The obtained measurements are simply averaged (arithmetic average) to obtain the average thickness of the magnetic layer 13. The positions at which the measurement is performed are selected randomly from the test piece.

[0035] As shown in FIG. 3A, the magnetization curve (MH loop) showing the relationship between the magnetization M and the magnetic field H in the magnetic layer 13 is preferably closed in the range of the magnetic field H exceeding -15 kOe and less than +15 kOe. This is because better electromagnetic conversion characteristics can be obtained. The MH loop being "closed" here means that there is an overlapping portion of the MH loop in the magnetic field H range of -15 kOe or more and +15 kOe or less, as shown in FIG. 3A. In the example of FIG. 3A, there is an overlapping portion of the MH loop in both the end region MH- where the magnetic field H is in the vicinity of -15 kOe, and the end region MH+ where the magnetic field H is in the vicinity of +15 kOe. In contrast, the MH loop being "not closed" means that there is no overlapping portion of the MH loop in the magnetic field H range of -15 kOe or more and +15 kOe or less, as shown in FIG. 3B. In the example of FIG. 3B, there is no overlapping portion of the MH loop in both the end region MH- and the end region MH+. FIG. 3B shows an example of a magnetization curve (MH loop) that shows the relationship between the magnetization M and the magnetic field H in the magnetic layer as a reference example. If the MH loop is "not closed," it means that the perpendicular coercive force Hc is excessively high or that the perpendicular coercive force Hc is distributed over a wide range of the magnetic field H. This makes it difficult to achieve saturation recording with the magnetic recording head. As a result, it is considered difficult to obtain good electromagnetic conversion characteristics.

[0036] (magnetic powder) The magnetic powder contained in the magnetic layer 13 may have a mass magnetization σs of, for example, 30 emu / g or more and 60 emu / g or less. When the mass magnetization σs of the magnetic powder is 30 emu / g or more, an improvement in the output of the magnetic recording medium 10 can be expected.

[0037] The magnetic powder contains a plurality of magnetic particles having an average particle diameter of, for example, 20 nm or less. Specifically, the magnetic powder contains, for example, a powder of nanoparticles containing ε-iron oxide (hereinafter referred to as "ε-iron oxide particles"). Even fine particles of ε-iron oxide particles can obtain high coercivity. It is preferable that the ε-iron oxide contained in the magnetic layer 13 has a preferential crystal orientation in the thickness direction (perpendicular direction) of the magnetic recording medium 10.

[0038] Fig. 4 is a cross-sectional view showing a schematic example of the cross-sectional structure of the ε iron oxide particles 20 contained in the magnetic layer 13. As shown in Fig. 4, the ε iron oxide particles 20 are spherical or nearly spherical, or cubic or nearly cubic. Since the ε iron oxide particles 20 have the above-mentioned shapes, when the ε iron oxide particles 20 are used as the magnetic particles, the contact area between the particles per unit volume in the thickness direction of the magnetic recording medium 10 can be reduced and the aggregation between the particles can be suppressed, compared to when hexagonal plate-shaped magnetic particles such as hexagonal ferrite are used as the magnetic particles. Therefore, the dispersibility of the magnetic powder can be improved, and a better SNR can be obtained.

[0039] The ε iron oxide particle 20 may have, for example, a core-shell structure. Specifically, as shown in Fig. 4, the ε iron oxide particle 20 includes a core portion 21 and a shell portion 22 having a two-layer structure provided around the core portion 21. The shell portion 22 having a two-layer structure includes a first shell portion 22a provided on the core portion 21 and a second shell portion 22b provided on the first shell portion 22a. As described later, the ε iron oxide particle 20 desirably contains both cobalt (Co) and zirconium (Zr) as additive elements.

[0040] The ε-iron oxide particles 20 are formed, for example, as follows. First, a silicon compound is added to a solution containing a first compound containing an iron element and a second compound containing the additive element to generate a silica xerogel containing the iron element and the additive element in silica. Next, the generated silica xerogel is heat-treated at a temperature of 850 to 1300°C for 4 to 6 hours. In this manner, the ε-iron oxide particles 20 containing the ε-iron oxide and the additive element are formed. Note that the amount of the additive element in the ε-iron oxide particles 20 in the present disclosure refers to the abundance ratio (atomic %, at %) of the additive element when the total atomic % of Fe and the additive element is taken as 100.

[0041] The content of the above-mentioned additive element in the ε iron oxide particles 20 is measured, for example, as follows. First, a carbon film is formed on the surface 13S of the magnetic layer 13 and the surface 14S of the back layer 14 of the magnetic recording medium 10 by a vapor deposition method, and then a tungsten thin film is further formed on the carbon film covering the surface 13S of the magnetic layer 13 by a vapor deposition method. These carbon films and tungsten films protect the sample in the flaking process described below. Next, the magnetic recording medium 10 is processed by a FIB (Focused Ion Beam) method or the like to be flaked. When the FIB method is used, a carbon film and a tungsten thin film are formed as protective films as a pretreatment for observing a TEM image of the cross section described below. The carbon film is formed on the magnetic layer side surface and the back layer side surface of the magnetic recording medium 10 by a vapor deposition method, and the tungsten thin film is further formed on the magnetic layer side surface by a vapor deposition method or a sputtering method. The flaking is performed along the length direction (longitudinal direction) of the magnetic recording medium 10. That is, this flaking forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic recording medium 10. The cross section of the obtained flaked sample is observed under the following conditions using a scanning electron microscope (SEM) to obtain an SEM image. Note that the magnification and acceleration voltage may be appropriately adjusted depending on the type of device. After obtaining the SEM image, elemental analysis is performed on the recording layer under the following conditions. <Elemental analysis (area analysis)> Analysis method: Energy dispersive X-ray spectroscopy (EDS) Scanning transmission electron microscope: JEOL JEM-ARM200F Accelerating voltage: 200kV Beam diameter: approx. 0.2 nmφ Elemental analyzer: JED-2300T X-ray detector: Si drift detector Energy resolution: Approximately 140 eV X-ray extraction angle: 21.9° Solid angle: 0.98sr Number of captured pixels: 256 x 256 Next, the atomic percentage of the additive element relative to the atomic percentage of Fe is calculated from the obtained elemental analysis results. Note that the position where the content of the additive element in the ε-iron oxide particle 20 is measured is selected at random from the test piece.

[0042] The core portion 21 of the ε-iron oxide particle 20 contains ε-iron oxide. The ε-iron oxide contained in the core portion 21 is ε-Fe 2 O 3 The crystals are preferred as the main phase, and the single-phase ε-Fe 2 O 3 It is more preferable that the core portion 21 is made of the ε-iron oxide. To achieve high density recording in the magnetic recording medium 10, it is desirable that the ε-iron oxide contained in the core portion 21 is microparticulated. However, although the microparticulated ε-iron oxide exhibits high coercivity, its mass magnetization σs tends to be small. A decrease in the mass magnetization σs of the magnetic powder is undesirable because it may lead to a decrease in the output and thermal stability of the magnetic recording medium 10. Therefore, Co (cobalt) is added to the core portion 21. This is because the inclusion of Co in the ε-iron oxide is expected to improve the mass magnetization σs of the ε-iron oxide particles 20.

[0043] However, single-phase ε-Fe 2 O 3 Adding only Co (cobalt) to the core portion 21 causes distortion in a part of the MH loop. In order to eliminate such a phenomenon, in the present disclosure, the core portion 21 further contains Zr (zirconium) in addition to Co. The core portion 21 is made of ε-Fe 2O 3 On the other hand, by using a material that contains both Co and Zr as additive elements, the distortion of the MH loop is alleviated, and sub-peaks are less likely to occur in the SFD (Switching Field Distribution) curve of the magnetic recording medium 10. It is believed that by adding Zr, a tetravalent element, together with Co, a divalent element, the average valence can be made trivalent, which has the effect of making it easier to introduce the Co element. Therefore, it is believed that the divalent element Co can be distributed more uniformly in the ε-iron oxide containing Fe, a trivalent element, and the distortion of the MH loop can be eliminated or reduced. As a result, the occurrence of sub-peaks in the SFD curve of the magnetic recording medium 10 is suppressed, and the area that can contribute to magnetic recording in the magnetic layer 13 can be secured more widely. Therefore, the magnetic recording medium 10 is advantageous for high-density recording. The amount of Co added in the core portion 21 is preferably 3 atomic % or more and 20 atomic % or less, when the atomic % of Fe and Co combined is taken as 100. Furthermore, in this case, the amount of Zr added in core region 21 is preferably 1 atomic % or more and 8 atomic % or less, when the total atomic % of Fe, Co, and Zr is taken as 100. By setting the amount of Co added and the amount of Zr added in core region 21 within the above ranges, the perpendicular coercive force Hc can be increased while the distortion of the MH loop can be sufficiently reduced, resulting in a magnetic recording medium 10 that is more advantageous for high density recording.

[0044] The core portion 21 may further contain a metal element such as Hf (hafnium) as an additional element.

[0045] The first shell portion 22a covers at least a part of the periphery of the core portion 21. Specifically, the first shell portion 22a may cover a part of the periphery of the core portion 21, or may cover the entire periphery of the core portion 21. From the viewpoint of ensuring sufficient exchange coupling between the core portion 21 and the first shell portion 22a and improving magnetic characteristics, it is preferable that the entire surface of the core portion 21 is covered.

[0046] The first shell portion 22a is a so-called soft magnetic layer, and is made of, for example, α-Fe, Ni-Fe alloy, CoOFe2 O 3 Alternatively, it includes a soft magnetic material such as an Fe—Si—Al alloy. The α-Fe may be obtained by reducing ε iron oxide contained in the core portion 21.

[0047] The second shell portion 22b is an oxide coating as an oxidation prevention layer. The second shell portion 22b includes α-iron oxide, aluminum oxide, or silicon oxide. The α-iron oxide is, for example, Fe 3 O 4 , Fe 2 O 3 and FeO. In the case where first shell portion 22a contains α-Fe (soft magnetic material), the α-iron oxide may be obtained by oxidizing the α-Fe contained in first shell portion 22a.

[0048] By having the first shell portion 22a as described above, the coercive force Hc of the core portion 21 alone can be kept large to ensure thermal stability, while the coercive force Hc of the entire ε-iron oxide particle (core-shell particle) 20 can be adjusted to a coercive force Hc suitable for recording. Furthermore, by having the second shell portion 22b as described above, the ε-iron oxide particle 20 can be prevented from deteriorating in the properties of the ε-iron oxide particle 20 due to rust or the like occurring on the particle surface caused by exposure of the ε-iron oxide particle 20 to air during and before the manufacturing process of the magnetic recording medium 10. Therefore, by covering the first shell portion 22a with the second shell portion 22b, deterioration in the properties of the magnetic recording medium 10 can be prevented.

[0049] The average particle size (average maximum particle size) of the magnetic powder is preferably 20 nm or less, more preferably 8 nm to 16 nm, and even more preferably 8 nm to 13 nm. In the magnetic recording medium 10, the region having a size of 1 / 2 the recording wavelength becomes the actual magnetized region. Therefore, by setting the average particle size of the magnetic powder to half the shortest recording wavelength or less, a good SNR can be obtained. Therefore, when the average particle size of the magnetic powder is 20 nm or less, good electromagnetic conversion characteristics (e.g., SNR) can be obtained in a high recording density magnetic recording medium 10 (e.g., a magnetic recording medium 10 configured to be able to record signals at the shortest recording wavelength of 50 nm or less). On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., SNR) can be obtained.

[0050] The average aspect ratio of the magnetic powder is preferably 1 or more and 3.0 or less, more preferably 1 or more and 2.8 or less, and even more preferably 1 or more and 1.8 or less. When the average aspect ratio of the magnetic powder is within the range of 1 or more and 3.0 or less, aggregation of the magnetic powder can be suppressed, and the resistance applied to the magnetic powder when the magnetic powder is vertically oriented in the process of forming the magnetic layer 13 can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved.

[0051] The average particle size and average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic recording medium 10 to be measured is processed and thinned by FIB (Focused Ion Beam) method or the like. The thinning is performed along the length direction (longitudinal direction) of the magnetic tape. That is, this thinning forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic recording medium 10. The obtained thin sample is observed by a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times so that the entire magnetic layer 13 is included in the thickness direction of the magnetic layer 13, and a TEM photograph is taken. Next, 50 particles are randomly selected from the TEM photograph, and the long axis length DL and short axis length DS of each particle are measured. Here, the long axis length DL means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the contour of each particle (so-called maximum Feret diameter). On the other hand, the minor axis length DS means the maximum length of the particle in a direction perpendicular to the major axis length DL of the particle.

[0052] Next, the long axis lengths DL of the 50 measured particles are simply averaged (arithmetic mean) to determine the average long axis length DLave. The average long axis length DLave thus determined is the average particle size of the magnetic powder. The short axis lengths DS of the 50 measured particles are also simply averaged (arithmetic mean) to determine the average short axis length DSave. The average aspect ratio of the particles (DLave / DSave) is then calculated from the average long axis length DLave and the average short axis length DSave.

[0053] The average particle volume of the magnetic powder is preferably 5500 nm 3 Less than or equal to 270 nm, more preferably 3 More than 5500nm 3 Less than or equal to 900 nm, and even more preferably 3 More than 5500nm 3 The average particle volume of the magnetic powder is 5500 nm or less. 3 When the average particle size of the magnetic powder is 22 nm or less, the same effect as when the average particle volume of the magnetic powder is 270 nm or less can be obtained. 3If the average particle size of the magnetic powder is 8 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 8 nm or more can be obtained.

[0054] When the ε iron oxide particles 20 are spherical or nearly spherical, the average particle volume of the magnetic powder is calculated as follows. First, the average major axis length DLave is calculated in the same manner as in the above-mentioned method for calculating the average particle size of the magnetic powder. Next, the average volume V of the magnetic powder is calculated by the following formula. V = (π / 6) × (DLave) 3

[0055] (Binding agent) As the binder, a resin having a structure in which a crosslinking reaction is given to a polyurethane resin, a vinyl chloride resin, or the like is preferable. However, the binder is not limited to these, and other resins may be appropriately blended depending on the physical properties required for the magnetic recording medium 10. There is no particular limitation on the resin to be blended, so long as it is a resin that is generally used in coating-type magnetic recording media 10.

[0056] Examples of the polymer include polyvinyl chloride, polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinyl chloride copolymer, methacrylic acid ester-ethylene copolymer, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymer, acrylonitrile-butadiene copolymer, polyamide resin, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymer, polyester resin, amino resin, and synthetic rubber.

[0057] Examples of the thermosetting resin or reactive resin include phenol resin, epoxy resin, urea resin, melamine resin, alkyd resin, silicone resin, polyamine resin, and urea formaldehyde resin.

[0058] In addition, in order to improve the dispersibility of the magnetic powder, -SO 3 M, -OSO 3 M, -COOM, P=O(OM) 2 In the above chemical formula, M is a hydrogen atom or an alkali metal such as lithium, potassium, or sodium.

[0059] Furthermore, the polar functional groups include -NR1R2, -NR1R2R3 + X - Side chain type with terminal group of >NR1R2 + X - In the above formula, R1, R2, and R3 are hydrogen atoms or hydrocarbon groups, and X - is a halogen element ion such as fluorine, chlorine, bromine, or iodine, or an inorganic or organic ion. Examples of the polar functional group include -OH, -SH, -CN, and an epoxy group.

[0060] (Lubricant) The lubricant contained in the magnetic layer 13 contains, for example, a fatty acid and a fatty acid ester. The fatty acid contained in the lubricant is, for example, a compound represented by the following general formula: <1> and compounds represented by the general formula <2> In addition, the fatty acid ester contained in the lubricant preferably contains at least one of the compounds represented by the following general formula: <3> and compounds represented by the general formula <4> It is preferred that the lubricant contains at least one of the compounds represented by the general formula: <1> and compounds represented by the general formula <3> By including two kinds of compounds represented by the general formula <2> and compounds represented by the general formula <3> By including two kinds of compounds represented by the general formula <1> and compounds represented by the general formula <4> By including two kinds of compounds represented by the general formula <2> and compounds represented by the general formula <4> By including two kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> and compounds represented by the general formula <3> By including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> and compounds represented by the general formula <4> By including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <3> and compounds represented by the general formula <4> By including three kinds of compounds represented by the general formula <2> Compounds represented by the general formula <3> and compounds represented by the general formula <4> or by including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> Compounds represented by the general formula <3> and compounds represented by the general formula <4> By containing these four compounds, it is possible to suppress an increase in the dynamic friction coefficient due to repeated recording or reproduction on the magnetic recording medium 10. As a result, the running properties of the magnetic recording medium 10 can be further improved. CH 3 (CH 2 ) k COOH... <1> (However, the general formula <1> In the formula, k is an integer selected from the range of 14 to 22, more preferably from the range of 14 to 18. CH 3 (CH 2 )n CH=CH(CH 2 ) m COOH... <2> (However, the general formula <2> In the formula, the sum of n and m is an integer selected from the range of 12 to 20, more preferably from the range of 14 to 18. CH 3 (CH 2 ) p COO(CH 2 ) q CH 3 ... <3> (However, the general formula <3> In the formula, p is an integer selected from the range of 14 to 22, more preferably from 14 to 18, and q is an integer selected from the range of 2 to 5, more preferably from 2 to 4. CH 3 (CH 2 ) p COO-(CH 2 ) q CH(CH 3 ) 2 … <4> (However, the above general formula <4> In the formula, p is an integer selected from the range of 14 to 22, and q is an integer selected from the range of 1 to 3.

[0061] (Additives) The magnetic layer 13 may further contain non-magnetic reinforcing particles such as aluminum oxide (α, β or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase titanium oxide), etc.

[0062] (base layer 12) The underlayer 12 is a non-magnetic layer containing a non-magnetic powder and a binder. The underlayer 12 may further contain at least one additive selected from the group consisting of a lubricant, conductive particles, a hardener, and an anti-rust agent, as necessary. The underlayer 12 may have a multi-layer structure in which a plurality of layers are laminated. The average thickness of the underlayer 12 is preferably 0.5 μm or more and 0.9 μm or less, more preferably 0.6 μm or more and 0.7 μm or less. By reducing the average thickness of the underlayer 12 to 0.9 μm or less, the Young's modulus of the entire magnetic recording medium 10 is effectively reduced compared to the case where the thickness of the base 11 is reduced. This makes it easier to control the tension of the magnetic recording medium 10. In addition, by making the average thickness of the underlayer 12 0.5 μm or more, the adhesive force between the base 11 and the underlayer 12 is ensured. In addition, the variation in thickness of the underlayer 12 can be suppressed, and the roughness of the surface 13S of the magnetic layer 13 can be prevented from increasing.

[0063] The average thickness of the underlayer 12 can be obtained, for example, as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared, and cut into a length of 250 mm to prepare a sample. Next, the underlayer 12 and the magnetic layer 13 are peeled off from the substrate 11 for the sample magnetic recording medium 10. Next, a Mitutoyo Laser Hologram (LGH-110C) is used as a measuring device to measure the thickness of the laminate of the underlayer 12 and the magnetic layer 13 peeled off from the substrate 11 at five or more positions. After that, the measured values ​​are simply averaged (arithmetic averaged) to calculate the average thickness of the laminate of the underlayer 12 and the magnetic layer 13. The measurement positions are selected randomly from the sample. Finally, the average thickness of the underlayer 12 is obtained by subtracting the average thickness of the magnetic layer 13 measured using the TEM as described above from the average thickness of the laminate.

[0064] The underlayer 12 may have pores, that is, the underlayer 12 may have a large number of pores. The pores of the underlayer 12 may be formed, for example, by forming pores (depressions) in the magnetic layer 13, and in particular, may be formed by pressing a large number of protrusions provided on the surface 14S of the back layer 14 of the magnetic recording medium 10 against the surface of the magnetic layer side. That is, pores may be formed in the magnetic layer 13 and the underlayer 12 by forming depressions corresponding to the shape of the protrusions on the surface 13S of the magnetic layer 13. In addition, the pores may be formed by volatilization of the solvent in the drying process of the paint for forming the magnetic layer. In addition, when the paint for forming the magnetic layer is applied to the surface of the underlayer 12 to form the magnetic layer 13, the solvent in the paint for forming the magnetic layer may pass through the pores of the underlayer 12 formed when the underlayer is applied and dried, and penetrate into the underlayer 12. Thereafter, when the solvent that has penetrated into the underlayer 12 volatilizes during the drying process of the magnetic layer 13, the solvent that has penetrated into the underlayer 12 may move from the underlayer 12 to the surface 13S of the magnetic layer 13, thereby forming pores. The pores thus formed may, for example, communicate with the magnetic layer 13 and the underlayer 12. The average diameter of the pores can be adjusted by changing the solid content or type of solvent of the paint for forming the magnetic layer and / or the drying conditions of the paint for forming the magnetic layer. By forming pores in both the magnetic layer 13 and the underlayer 12, a particularly suitable amount of lubricant for good running stability appears on the magnetic layer side surface, and the increase in the dynamic friction coefficient due to repeated recording or reproduction can be further suppressed.

[0065] From the viewpoint of suppressing a decrease in the dynamic friction coefficient after repeated recording or reproduction, it is preferable that the pores of the underlayer 12 are connected to the recesses of the magnetic layer 13. Here, the pores of the underlayer 12 being connected to the recesses of the magnetic layer 13 includes a state in which some of the many pores of the underlayer 12 are connected to some of the many recesses of the magnetic layer 13.

[0066] From the viewpoint of improving the supply of lubricant to the surface 13S of the magnetic layer 13, it is preferable that the numerous recesses include those extending in a direction perpendicular to the surface 13S of the magnetic layer 13. Also, from the viewpoint of improving the supply of lubricant to the surface 13S of the magnetic layer 13, it is preferable that the pores of the underlayer 12 extending in a direction perpendicular to the surface 13S of the magnetic layer 13 and the recesses of the magnetic layer 13 extending in a direction perpendicular to the surface 13S of the magnetic layer 13 are connected to each other.

[0067] (Non-magnetic powder in underlayer 12) The non-magnetic powder includes at least one of inorganic particle powder and organic particle powder. The non-magnetic powder may also include carbon powder such as carbon black. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles include, for example, metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, or metal sulfides. The shape of the non-magnetic powder may be, for example, various shapes such as needle-like, spherical, cubic, and plate-like, but is not limited thereto.

[0068] (Binding agent for base layer 12) The binder in the underlayer 12 is the same as that in the magnetic layer 13 described above.

[0069] (Back layer 14) The back layer 14 contains, for example, a binder and a nonmagnetic powder. The back layer 14 may further contain at least one additive selected from the group consisting of a lubricant, a hardener, and an antistatic agent, as necessary. The binder and nonmagnetic powder in the back layer 14 are the same as those in the underlayer 12 described above.

[0070] The average particle size of the non-magnetic powder in the back layer 14 is preferably 10 nm or more and 150 nm or less, more preferably 15 nm or more and 110 nm or less. The average particle size of the non-magnetic powder in the back layer 14 is determined in the same manner as the average particle size of the magnetic powder in the magnetic layer 13. The non-magnetic powder may include powder having two or more particle size distributions.

[0071] The upper limit of the average thickness of the back layer 14 is preferably 0.6 μm or less, and particularly preferably 0.5 μm or less. If the upper limit of the average thickness of the back layer 14 is 0.6 μm or less, the thickness of the underlayer 12 and the base 11 can be kept thick even when the average thickness of the magnetic recording medium 10 is 5.6 μm or less, so that the running stability of the magnetic recording medium 10 in a recording and reproducing device can be maintained. The lower limit of the average thickness of the back layer 14 is not particularly limited, but is, for example, 0.2 μm or more, and particularly preferably 0.3 μm or more.

[0072] The average thickness of the back layer 14 is obtained as follows. First, a magnetic recording medium 10 having a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, the thickness of the sample magnetic recording medium 10 is measured at five or more points using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, and the measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t T [μm] is calculated. Note that the measurement positions are selected randomly from the sample. Next, the back layer 14 is removed from the sample magnetic recording medium 10 with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. After that, the above-mentioned laser hologram is used again to measure the thickness of the sample from which the back layer 14 has been removed from the magnetic recording medium 10 at five or more points, and these measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t B [μm] is calculated. The measurement positions are selected randomly from the sample. Finally, the average thickness t of the back layer 14 is calculated from the following formula: b Calculate [μm]. t b [μm]=t T [μm]-t B [μm]

[0073] (Average thickness of magnetic recording medium 10) The upper limit of the average thickness (average total thickness) of the magnetic recording medium 10 is preferably 5.6 μm or less, more preferably 5.0 μm or less, particularly preferably 4.6 μm or less, and even more preferably 4.4 μm or less. When the average thickness of the magnetic recording medium 10 is 5.6 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic recording medium. The lower limit of the average thickness of the magnetic recording medium 10 is not particularly limited, but is, for example, 3.5 μm or more.

[0074] The average thickness tT of the magnetic recording medium 10 is found as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared, and then cut into a length of 250 mm to prepare a sample. Next, using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, the thickness of the sample is measured at five or more positions, and the measured values ​​are simply averaged (arithmetic mean) to calculate the average value tT [μm]. Note that the measurement positions are selected randomly from the sample.

[0075] (ratio Hrp / Hc) Furthermore, the ratio Hrp / Hc of the remanent coercivity Hrp (see FIG. 3A) measured in a direction perpendicular to the film surface of the magnetic recording medium 10 using a pulsed magnetic field to the perpendicular coercivity Hc (see FIG. 3A) in a direction perpendicular to the film surface of the magnetic recording medium 10 is preferably 2.0 or less. By keeping the ratio Hrp / Hc within a predetermined range, the amount of signal attenuation can be improved. That is, the thermal stability of the magnetic recording medium 10 in which the difference between the remanent coercivity Hrp and the perpendicular coercivity Hc is small and the ratio Hrp / Hc is close to 1 is high. On the other hand, the thermal stability of the magnetic recording medium 10 in which the difference between the remanent coercivity Hrp and the perpendicular coercivity Hc is large and the value of the ratio Hrp / Hc is significantly greater than 1 (for example, to the extent of exceeding 2) is low. By setting the ratio Hrp / Hc to 2.0 or less, it is possible to avoid a decrease in thermal stability and ensure ease of writing magnetization signals. By avoiding the decrease in thermal stability, it is possible to prevent the magnetic recording medium 10 from becoming unstable and susceptible to the influence of the surrounding temperature, and to improve the data storage properties (long-term reliability of the magnetic recording medium 10). In order to make the ratio Hrp / Hc 2.0 or less, for example, it is preferable to form the magnetic layer 13 using a magnetic powder having a mass magnetization σs of 30 emu / g or more and 60 emu / g or less. Since the ε-iron oxide of the present disclosure has a high mass magnetization σs as described above and a high perpendicular coercive force Hc, which is an inherent characteristic of ε-iron oxide, it is possible to have high thermal stability even in the form of fine particles. At the same time, since the mass magnetization σs is high, a high Mst (saturation magnetization per unit area) can be ensured, and a high recording and reproducing output can be maintained. That is, as described above, it is possible to achieve both high thermal stability, i.e., long-term reliability, and high electromagnetic conversion characteristics. In addition, the perpendicular coercive force Hc is preferably 2000 Oe or more and 6000 Oe or less, and more preferably 2500 Oe or more and 4500 Oe or less.

[0076] When measuring the perpendicular coercivity Hc, the magnetic field is swept at a low speed, so that the mass magnetization σ of the magnetic layer 13 fluctuates even during the measurement due to the influence of the surrounding heat. On the other hand, when measuring the remanent coercivity Hrp, a pulsed magnetic field is applied and the measurement is performed in an instant. Therefore, the influence of the surrounding heat is small, and it is considered that the remanent coercivity Hrp is large. If the magnetic recording medium has high thermal stability, the decrease in the perpendicular coercivity Hc due to heat is small, and therefore it is considered that the ratio Hrp / Hc is small. On the other hand, in the case of a magnetic recording medium with low thermal stability, the opposite phenomenon occurs, and the decrease in the perpendicular coercivity Hc due to heat is large, and it is considered that the ratio Hrp / Hc is large.

[0077] The perpendicular coercive force Hc is obtained as follows. First, three magnetic recording media 10 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to create a measurement sample. At this time, markings are made with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic recording medium 10 can be identified. Then, the MH loop of the measurement sample (entire magnetic recording medium 10) corresponding to the perpendicular direction (thickness direction) of the magnetic recording medium 10 is measured using a VSM.

[0078] Next, the coating film, i.e., the undercoat layer 12, the magnetic layer 13, and the back layer 14, are wiped off with acetone or ethanol, leaving only the substrate 11. Three of the obtained substrates 11 are then stacked together with double-sided tape, and punched out with a φ6.39 mm punch to obtain a sample for background correction (hereinafter simply referred to as a correction sample). Then, the MH loop of the correction sample (substrate 11) corresponding to the perpendicular direction of the substrate 11 (perpendicular direction of the magnetic recording medium 10) is measured using a VSM.

[0079] The MH loop of the measurement sample (whole magnetic recording medium 10) and the MH loop of the correction sample (substrate 11) are measured using, for example, a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Kogyo Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.

[0080] After the two MH loops are obtained, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 10), and the MH loop after background correction is obtained. The measurement and analysis program attached to the "VSMP7-15" is used for the calculation of this background correction.

[0081] The perpendicular coercivity Hc is obtained from the obtained MH loop after background correction. Note that all of the above MH loop measurements are performed at 25°C. Also, no "demagnetization field correction" is performed when measuring the MH loop in the perpendicular direction of the magnetic recording medium 10. Note that the measurement and analysis program included with the "VSM-P7-15" is used for this calculation.

[0082] The remanent coercivity Hrp is calculated as follows: For the measurement sample, the same sample as that used to calculate the perpendicular coercivity Hc described above is used to measure the remanent magnetization curve in the direction perpendicular to the film surface using a high speed response characteristic evaluation device HR-PVSM20 manufactured by Hayama Corporation.

[0083] First, a vertical magnetic field of about -3980 kA / m (about -15 kOe) is applied to the entire sample, and the magnetic field is returned to zero to create a residual magnetization state. After that, a magnetic field of about 40.2 kA / m (about 505 Oe) is applied in the opposite direction, and the magnetic field is returned to zero again to measure the residual magnetization. The applied magnetic field has a pulse width of 10 -8The magnetic field is a pulse magnetic field of 1000 s. Thereafter, a similar measurement is repeated in which a magnetic field approximately 40.2 kA / m larger than the previous magnetic field is applied and returned to zero, and the residual magnetization is plotted against the applied magnetic field to measure the DCD curve. The measurement magnetic field is up to approximately 20 kOe. No background correction or demagnetizing field correction is performed. The magnitude of the magnetic field applied to the sample is changed by changing the applied voltage. The step voltage is 17.5 V (equivalent to a magnetic field of approximately 505 Oe). The main measurement conditions are as follows. Initial magnetization voltage: 220V (equivalent to -3980kA / m) Measurement start voltage: 0V (equivalent to 0 Oe) Step voltage: 17.5V (equivalent to approximately 505Oe) Maximum voltage: 350V (equivalent to 20kOe) Lock-in amplifier waiting time: 10 seconds A residual magnetization curve can be obtained by performing phase correction on the data stored after measurement (Figure 5). In Figure 5, a line is drawn between two points on either side of the X-axis (points P1 and P2), and the point where the line intersects with the X-axis is calculated as the residual coercivity Hrp. Although the unit of magnetization is originally emu, in the above-mentioned high-speed response characteristic evaluation device, the magnetization amount in each applied magnetic field is output as a voltage V, and the magnetization amount (voltage V) in each applied magnetic field is output as a positive value regardless of whether it is positive or negative. Therefore, correction according to the phase in each applied magnetic field is necessary. For this correction, phase information data included in the output result by the above-mentioned high-speed response characteristic evaluation device is used. The phase information data is also output for each applied magnetic field together with the magnetization amount (voltage V) in each applied magnetic field. If the phase information data of the magnetization amount (voltage V) measured for a certain magnetic field is a negative value, the measured magnetization amount (voltage V) needs to be multiplied by "-1", and the value obtained by multiplying the measured magnetization amount (voltage V) by "-1" is used to obtain the residual magnetization curve. The process of multiplying by "-1" is the above-mentioned phase correction. On the other hand, if the phase information data of the magnetization amount (voltage V) measured for a certain magnetic field is a positive value, there is no need to multiply the measured magnetization amount (voltage V) by "-1", and the measured magnetization amount (voltage V) is used as it is to obtain the remanent magnetization curve. By plotting the phase-corrected magnetization amount obtained as described above (multiplied by "-1") and the measured magnetization amount (not multiplied by "-1") against the magnetic field, the remanent magnetization curve shown in the figure is obtained.

[0084] [2-2 Manufacturing method of magnetic recording medium 10] Next, a method for manufacturing the magnetic recording medium 10 having the above-mentioned configuration will be described. First, a paint for forming the undercoat layer is prepared by kneading and dispersing non-magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming the magnetic layer is prepared by kneading and dispersing magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming the back layer is prepared by kneading and dispersing binder, non-magnetic powder, etc. in a solvent. For example, the following solvents, dispersing devices, and kneading devices can be used to prepare the paint for forming the magnetic layer, the paint for forming the undercoat layer, and the paint for forming the back layer.

[0085] Examples of the solvent used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol-based solvents such as methanol, ethanol, and propanol, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate, ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane, aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene, and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. These may be used alone or in appropriate mixture.

[0086] Examples of the kneading device used in the preparation of the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of diluting in multiple stages, a kneader, a pressure kneader, a roll kneader, etc. Examples of the dispersing device used in the preparation of the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (for example, "DCP Mill" manufactured by Eirich Co., Ltd.), a homogenizer, an ultrasonic dispersing machine, etc.

[0087] Next, the underlayer forming paint is applied to one main surface 11A of the substrate 11 and dried to form the underlayer 12. Next, the magnetic layer forming paint is applied to the underlayer 12 and dried to form the magnetic layer 13 on the underlayer 12. During drying, it is preferable to magnetically orient the magnetic powder in the thickness direction of the substrate 11, for example, by a solenoid coil. Also, during drying, the magnetic powder may be magnetically oriented in the running direction (longitudinal direction) of the substrate 11, and then magnetically oriented in the thickness direction of the substrate 11, for example, by a solenoid coil. By performing such magnetic field orientation treatment, the degree of vertical orientation (i.e., squareness ratio S1) of the magnetic powder can be improved. After the magnetic layer 13 is formed, the back layer forming paint is applied to the other main surface 11B of the substrate 11 and dried to form the back layer 14. This results in a magnetic recording medium 10.

[0088] The obtained magnetic recording medium 10 is then subjected to a calendaring process to smooth the surface 13S of the magnetic layer 13. Next, the calendared magnetic recording medium 10 is wound into a roll, and in this state, the magnetic recording medium 10 is subjected to a heat treatment to transfer the numerous protrusions on the surface 14S of the back layer 14 to the surface 13S of the magnetic layer 13. As a result, numerous recesses are formed on the surface 13S of the magnetic layer 13.

[0089] The heat treatment temperature is preferably 50° C. or higher and 80° C. or lower. When the heat treatment temperature is 50° C. or higher, good transferability can be obtained. On the other hand, when the heat treatment temperature is 80° C. or lower, the amount of pores becomes too large, and there is a risk of an excess of lubricant on the surface 13S of the magnetic layer 13. Here, the heat treatment temperature is the temperature of the atmosphere in which the magnetic recording medium 10 is held.

[0090] The heat treatment time is preferably 15 hours or more and 40 hours or less. When the heat treatment time is 15 hours or more, good transferability can be obtained. On the other hand, when the heat treatment time is 40 hours or less, a decrease in productivity can be suppressed.

[0091] The pressure applied to the magnetic recording medium 10 during the heat treatment should preferably be in the range of 150 kg / cm to 400 kg / cm.

[0092] Finally, the magnetic recording medium 10 is cut to a predetermined width (for example, 1 / 2 inch width). In this way, the desired magnetic recording medium 10 is obtained.

[0093] [2-3 Effects] As described above, the magnetic recording medium 10 of the present embodiment is a tape-shaped member in which the substrate 11, the underlayer 12, the magnetic layer 13, and the back layer 14 are laminated in this order. <1> from <3> It is designed to satisfy each of the above constituent requirements. <1> The magnetic layer 13 contains magnetic powder containing ε iron oxide. <2> The ratio (Hrp / Hc) of the residual coercivity (Hrp) measured in the perpendicular direction of the magnetic recording medium 10 using a pulsed magnetic field to the perpendicular coercivity (Hc) in the direction perpendicular to the film surface is 2.0 or less. <3> It has a magnetic layer with a saturation magnetization per unit area (Mst) of 4.5 mA or more.

[0094] The magnetic recording medium 10 of the present embodiment has such a configuration, and therefore can achieve excellent electromagnetic conversion characteristics and high long-term reliability even when the recording density is increased. The magnetic recording medium 10 satisfies the above-mentioned configuration requirements, for example, by having the magnetic layer 13 have magnetic powder containing ε-iron oxide to which Co and Zr have been added. The magnetic powder containing ε-iron oxide to which Co and Zr have been added has high perpendicular coercive force Hc and mass magnetization σs. Therefore, the magnetic recording medium 10 using such magnetic powder can achieve both excellent electromagnetic conversion characteristics and high long-term reliability.

[0095] <3. Modifications> (Variation 1) In the above embodiment, the ε-iron oxide particles 20 ( FIG. 4 ) having the shell portion 22 with a two-layer structure have been described as an example, but the magnetic recording medium of the present technology may include the ε-iron oxide particles 20A having the shell portion 23 with a single-layer structure, as shown in FIG. 6 . The shell portion 23 in the ε-iron oxide particles 20A has a similar configuration to the first shell portion 22a, for example. However, from the viewpoint of suppressing deterioration of characteristics, the ε-iron oxide particles 20 having the shell portion 22 with a two-layer structure described in the above embodiment are more preferable than the ε-iron oxide particles 20A of Modification 1.

[0096] (Variation 2) The magnetic recording medium 10 may further include a barrier layer 15 provided on at least one surface of the substrate 11, as shown in FIG. 7. The barrier layer 15 is a layer for suppressing dimensional changes of the substrate 11 depending on the environment. For example, one example of a cause of the dimensional changes is the hygroscopicity of the substrate 11, and the provision of the barrier layer 15 can reduce the rate at which moisture penetrates into the substrate 11. The barrier layer 15 includes, for example, a metal or a metal oxide. The metal referred to here may be, for example, at least one of Al, Cu, Co, Mg, Si, Ti, V, Cr, Mn, Fe, Ni, Zn, Ga, Ge, Y, Zr, Mo, Ru, Pd, Ag, Ba, Pt, Au, and Ta. The metal oxide may be, for example, a metal oxide containing one or more of the above metals. More specifically, for example, Al 2 O 3 , CuO, CoO, SiO 2 , Cr 2 O 3 , TiO 2 , Ta 2 O 5 and ZrO 2 At least one of the following can be used. The rear layer 15 is made of diamond-like carbon (DLC) or diamond. It may also include the above.

[0097] The average thickness of the barrier layer 15 is preferably 20 nm or more and 1000 nm or less, more preferably 50 nm or more and 1000 nm or less. The average thickness of the barrier layer 15 is determined in the same manner as the average thickness of the magnetic layer 13. However, the magnification of the TEM image is appropriately adjusted according to the thickness of the barrier layer 15. EXAMPLES

[0098] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to the following examples.

[0099] In the following examples and comparative examples, the saturation magnetization Mst per unit area of ​​the magnetic layer 13, the MH loop, the perpendicular coercivity Hc, the mass magnetization σs of the magnetic layer 13, the average thickness of the magnetic layer 13, the average particle size of the magnetic powder, the remanent coercivity Hrp, and the positions of the first and second peaks in the diffraction pattern measured by in-plane X-ray diffraction (Cu tube) in the magnetic layer 13 are values ​​determined by the measurement method described in the above-mentioned embodiment.

[0100] [Example 1] The magnetic recording medium of Example 1 was obtained as follows.

[0101] <Preparation process of paint for forming magnetic layer> The magnetic layer-forming paint was prepared as follows. First, the first composition having the following composition was kneaded with an extruder. Next, the kneaded first composition and the second composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further sand mill mixing was performed and filtering was performed to prepare the magnetic layer-forming paint.

[0102] (First composition) The components and their weights in the first composition are as follows: ε Iron oxide particle powder (Co[at%] / Fe[at%]=0.14, Zr[at%] / Fe[at%]=0.05, spherical, average aspect ratio 1.1, average particle size 16 nm, particle volume 2150 nm 3 , mass magnetization σs is 39emu / g): 100 parts by mass Vinyl chloride resin: 42 parts by weight (including solvent) (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) (Degree of polymerization: 300, Mn=10,000, polar group: OSO 3 Contains K=0.07mmol / g and secondary OH=0.3mmol / g. Aluminum oxide powder: 5 parts by weight (α-Al 2 O 3 , average particle size 0.1μm) Carbon black (manufactured by Tokai Carbon Co., Ltd., product name: Seast TA): 2 parts by weight

[0103] (Second composition) The components and their weights in the second composition are as follows: Vinyl chloride resin: 3 parts by weight (including solution) (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) n-Butyl stearate as fatty acid ester: 2 parts by weight Methyl ethyl ketone: 121.3 parts by weight Toluene: 121.3 parts by weight Cyclohexanone: 60.7 parts by weight

[0104] To the magnetic layer-forming coating material prepared as described above, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Tosoh Corporation) as a curing agent and 2 parts by mass of stearic acid as a fatty acid were added.

[0105] <Preparation process of paint for forming base layer> The paint for forming the undercoat layer was prepared as follows. First, the third composition having the following composition was kneaded with an extruder. Next, the kneaded third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further mixing was performed with a sand mill and filtering was performed to prepare the paint for forming the undercoat layer.

[0106] (Third composition) The components and their weights in the third composition are as follows: Acicular iron oxide powder (α-Fe 2 O 3 , average major axis length 0.15 μm): 100 parts by mass Vinyl chloride resin (resin solution: resin content 30% by mass, cyclohexanone 70% by mass): 60.6 parts by mass (including solution) Carbon black (average particle size 20 nm): 10 parts by weight

[0107] (4th composition) The components and their weights in the fourth composition are as follows. Polyurethane resin UR8200 (manufactured by Toyobo): 18.5 parts by weight n-Butyl stearate as fatty acid ester: 2 parts by weight Methyl ethyl ketone: 108.2 parts by weight Toluene: 108.2 parts by mass Cyclohexanone: 18.5 parts by weight

[0108] To the coating material for forming an undercoat layer prepared as described above, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Tosoh Corporation) as a curing agent and 2 parts by mass of stearic acid as a fatty acid were added.

[0109] <Preparation process of paint for forming back layer> The paint for forming the back layer was prepared as follows. The following raw materials were mixed in a stirring tank equipped with a disperser, and filtered to prepare the paint for forming the back layer. Small particle size carbon black powder (average particle size (D50) 20 nm): 90 parts by mass Large particle size carbon black powder (average particle size (D50) 270 nm): 10 parts by weight Polyester polyurethane (manufactured by Tosoh Corporation, product name: N-2304): 100 parts by weight Methyl ethyl ketone: 500 parts by weight Toluene: 400 parts by weight Cyclohexanone: 100 parts by weight

[0110] <Coating process> Using the magnetic layer forming paint and the undercoat layer forming paint prepared as described above, a base layer with an average thickness of 0.6 μm and a magnetic layer with an average thickness of 80 nm were formed on one main surface of a long polyester film with an average thickness of 4.0 μm, which is a non-magnetic support, as follows. First, the undercoat layer was formed by applying the undercoat layer forming paint on one main surface of the polyester film and drying it. Next, the magnetic layer was formed by applying the magnetic layer forming paint on the undercoat layer and drying it. During drying of the magnetic layer forming paint, the magnetic powder was magnetically oriented in the thickness direction of the film by a solenoid coil. In addition, the drying conditions (drying temperature and drying time) of the magnetic layer forming paint were adjusted, and the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium was set to the value shown in Table 1. Next, the back layer forming paint was applied on the other main surface of the polyester film and dried to form a back layer with an average thickness of 0.3 μm.

[0111] <Calendar process and transfer process> Then, a calendaring process was performed to smooth the surface of the magnetic layer. Next, the magnetic recording medium with the smoothed surface of the magnetic layer was wound into a roll, and the magnetic recording medium was subjected to a heat treatment at 60°C for 10 hours in this state. Then, the magnetic recording medium was rewound into a roll so that the end located on the inner circumference side was reversed to the outer circumference side, and the magnetic recording medium was subjected to a heat treatment at 60°C for 10 hours in this state again. As a result, many protrusions on the surface of the back layer were transferred to the surface of the magnetic layer, and many recesses were formed on the surface of the magnetic layer.

[0112] <Cutting process> The magnetic recording medium obtained as described above was cut into a width of 1 / 2 inch (12.65 mm), thereby obtaining the desired long magnetic recording medium (average thickness 5.6 μm).

[0113] In the magnetic recording medium as Example 1 obtained as described above, the saturation magnetization Mst per unit area in the magnetic layer was 6.1 mA, and the ratio Hrp / Hc was 1.67.

[0114] [Example 2] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 13 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.15. As a result, the mass magnetization σs of the ε iron oxide particles was set to 40 emu / g. In addition, in the coating process, the drying conditions were adjusted, and the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field were set to the values ​​shown in Table 1. Except for these, a magnetic recording medium as Example 2 was obtained in the same manner as in Example 1 above.

[0115] [Example 3] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 19 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.15. As a result, the mass magnetization σs of the ε iron oxide particles was set to 40 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, a magnetic recording medium as Example 3 was obtained in the same manner as in Example 1 above.

[0116] [Example 4] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. In the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. In addition, in the coating process, the average thickness of the magnetic layer was set to 60 nm. Except for these, the magnetic recording medium of Example 4 was obtained in the same manner as in Example 1 above. In the magnetic recording medium of Example 4 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 4.5 mA.

[0117] [Example 5] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.08. As a result, the mass magnetization σs of the ε iron oxide particles was set to 25 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 5 was obtained in the same manner as in Example 1 above. In addition, in the magnetic recording medium of Example 5 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 4.7 mA.

[0118] [Example 6] In the preparation process of the coating material for forming the magnetic layer, the molar ratio of Co to Fe in the ε iron oxide particles was Co[at%] / Fe[at%]=0.20. As a result, the mass magnetization σs of the ε iron oxide particles was set to 50 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 6 was obtained in the same manner as in Example 1 above. In addition, in the magnetic recording medium of Example 6 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 7.8 mA.

[0119] [Example 7] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.20. As a result, the mass magnetization σs of the ε iron oxide particles was set to 25 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 7 was obtained in the same manner as in Example 1 above. In addition, in the magnetic recording medium of Example 7 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 7.8 mA.

[0120] [Example 8] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.2 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.16. As a result, the mass magnetization σs of the ε iron oxide particles was set to 41 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 8 was obtained in the same manner as in Example 1 above. In addition, in the magnetic recording medium of Example 8 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 6.4 mA.

[0121] [Example 9] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. The molar ratio of Co to Fe in the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.20. As a result, the mass magnetization σs of the ε iron oxide particles was set to 50 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 9 was obtained in the same manner as in Example 1 above. In addition, in the magnetic recording medium of Example 9 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 7.8 mA.

[0122] [Example 10] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. The molar ratio of Co to Fe in the powder of the ε iron oxide particles was set to Co [at%] / Fe [at%] = 0.20. As a result, the mass magnetization σs of the ε iron oxide particles was set to 50 emu / g. In addition, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 10 was obtained in the same manner as in Example 1 above. In the magnetic recording medium of Example 10 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 5.8 mA.

[0123] [Example 11] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 16.2 nm. In the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium of Example 11 was obtained in the same manner as in Example 1 above. In the magnetic recording medium of Example 11 obtained in this manner, the saturation magnetization Mst per unit area of ​​the magnetic layer was 6.1 mA.

[0124] [Comparative Example 1] In the preparation process of the coating material for forming the magnetic layer, Zr was not added to the ε iron oxide particles. As a result, the mass magnetization σs of the ε iron oxide particles was set to 15 emu / g. In the step, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium was obtained as Comparative Example 1 in the same manner as in Example 1 above. In the magnetic recording medium thus obtained as Comparative Example 1, the saturation magnetization Mst per unit area of ​​the magnetic layer was 2.3 mA.

[0125] [Comparative Example 2] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. In addition, Zr was not added to the ε iron oxide particles. As a result, the mass magnetization σs of the ε iron oxide particles was set to 16 emu / g. Furthermore, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, a magnetic recording medium was obtained as Comparative Example 2 in the same manner as in Example 1 above. In the magnetic recording medium thus obtained as Comparative Example 2, the saturation magnetization Mst per unit area of ​​the magnetic layer was 2.5 mA.

[0126] [Comparative Example 3] In the preparation process of the coating material for forming the magnetic layer, the average particle size of the ε iron oxide particles was set to 15.5 nm. In addition, Zr was not added to the ε iron oxide particles. As a result, the mass magnetization σs of the ε iron oxide particles was set to 16 emu / g. Furthermore, in the coating process, the drying conditions were adjusted to set the coercive force Hc in the thickness direction (perpendicular direction) of the magnetic recording medium and the residual coercive force Hrp measured using a pulsed magnetic field to the values ​​shown in Table 1. Except for these, the magnetic recording medium was obtained as Comparative Example 3 in the same manner as in Example 1 above. In the magnetic recording medium thus obtained as Comparative Example 3, the saturation magnetization Mst per unit area of ​​the magnetic layer was 4.7 mA.

[0127] [evaluation] The magnetic recording media of Examples 1 to 11 and Comparative Examples 1 to 3 obtained as described above were evaluated as follows.

[0128] (Loop occlusion) We checked whether the MH loop was blocked in the range of -15 kOe to +15 kOe. In Table 1, if the MH loop was blocked in the range of -15 kOe to +15 kOe, it was displayed as OK, and if the MH loop was not blocked in the range of -15 kOe to +15 kOe, it was displayed as NG.

[0129] (In-plane XRD peak detection) In the diffraction pattern by in-plane X-ray diffraction (Cu tube), it was confirmed whether the first peak appeared at the position of 32.9° and the second peak appeared at the position of 36.6°. In Table 1, if the first peak appeared at the position of 32.9° and if the second peak appeared at the position of 36.6°, respectively, it is displayed as OK.

[0130] (SNR) The SNR (electromagnetic conversion characteristics) of the magnetic recording medium was measured in a 25°C environment using a 1 / 2 inch tape transport device (MTS Transport, manufactured by Mountain Engineering II) equipped with a recording / playback head and a recording / playback amplifier. A ring head with a gap length of 0.2 μm was used as the recording head, and a GMR head with a shield-to-shield distance of 0.1 μm was used as the playback head. The relative speed was 6 m / s, the recording clock frequency was 160 MHz, and the recording track width was 2.0 μm. The SNR was calculated based on the method described in the following document. The results are shown in Table 1 as relative values ​​with the SNR of Comparative Example 3 taken as 0 dB. Y. Okazaki: “An Error Rate Emulation System.”, IEEE Trans. Man., 31, pp.3093-3095(1995)

[0131] (Signal attenuation after 10 years) The signal attenuation after 10 years was determined for each of the samples of the examples and comparative examples as follows. Specifically, a "Tape Head Tester (hereinafter referred to as THT)" manufactured by Micro Physics was used. The recording and reproducing head was the same as that mounted on an IBM tape drive "TS1140". In the measurement, a magnetic tape was cut to a length of 90 cm as a magnetic recording medium, and made into a ring shape with the recording layer of the magnetic tape facing backward, and then both ends of the magnetic tape were joined together on the back side of the magnetic tape with adhesive tape. In addition, a silver tape for detecting the tape rotation position was attached adjacent to the joint. The ring-shaped magnetic tape was attached to the THT and rotated at a speed of 2 m / sec.

[0132] Next, a 10MHz signal generated using a Tektronix signal generator "ARBITRARY WAVEFORM GENERATOR AWG2021" was recorded on the magnetic tape using the optimal recording current for one full revolution of the tape. Following the recording, the signal recorded on the tape was played back continuously from the next revolution, and the playback output was measured with a Hewlett Packard spectrum analyzer "8591E". The spectrum analyzer settings were RBW: 1MHz, VBW: 1MHz, SWP: 500msec, point: 400, zero span mode. The measurement was performed for 0.4 seconds during the "recording section" only, excluding the "near the tape joint" where sufficient recording was not performed, and the average value Y of the playback output during this period was calculated. The measurement was performed for each revolution of the tape, and the average value Y of the playback output for each revolution was taken as the average playback output Y(t) during the elapsed time from the end of signal recording (t=0). Measurements were taken up to t = 100 sec, and the data was sent to a connected computer at appropriate times and recorded.

[0133] The above measurement flow was performed four times using the same magnetic tape, and the Y(t) values ​​obtained from each measurement were averaged for each elapsed time t to obtain the Yave(t) sequence. The obtained Yave(t) was plotted on a graph with the Y axis and the elapsed time t on the X axis, and an approximation curve was created from this graph using logarithmic approximation. The signal attenuation after 10 years was calculated using the obtained approximation curve.

[0134] Table 1 shows the configurations and evaluation results of the magnetic recording media in each of the examples and comparative examples.

[0135] [Table 1]

[0136] As shown in Table 1, in Examples 1 to 11, the magnetic layer had a first peak at 32.9° and a second peak at 36.6° in the diffraction pattern by in-plane X-ray diffraction (Cu tube), a ratio Hrp / Hc of 2.0 or less, contained iron oxide, and had a saturation magnetization Mst per unit area of ​​4.5 mA or more. Therefore, in Examples 1 to 11, good results were obtained in both SNR and signal attenuation.

[0137] In particular, in Example 9, extremely good results were obtained in both SNR and signal attenuation. In Example 9, in addition to the high saturation magnetization Mst per unit area, the remanence Hrp measured using a pulsed magnetic field was also kept low. For this reason, it is easy to write a recording magnetic field to the magnetic layer 13, and a steep magnetization reversal can be formed in the magnetic layer 13, so it is believed that a good SNR is obtained.

[0138] In Example 2, the magnetic particles were made small, and thus a better SNR was obtained, whereas in Example 3, relatively large magnetic particles were used, and thus good results were obtained in terms of the amount of signal attenuation.

[0139] In Comparative Example 1, the saturation magnetization Mst per unit area was less than 4.5 mA, and therefore degradation of the SNR was observed.

[0140] In Comparative Example 2, the saturation magnetization per unit area Mst was less than 4.5 mA and the ratio Hrp / Hc exceeded 2.0, resulting in insufficient SNR. In addition, degradation in the amount of signal attenuation after 10 years was also observed.

[0141] In Comparative Example 3, the ratio Hrp / Hc exceeded 2.0, and the average thickness of the magnetic layer was also relatively thick, resulting in insufficient SNR. In addition, degradation was observed in the amount of signal attenuation after 10 years.

[0142] While the present disclosure has been specifically described above by giving embodiments and modifications thereof, the present disclosure is not limited to the above-described embodiments, and various modifications are possible.

[0143] For example, the configurations, methods, steps, shapes, materials, and values ​​given in the above-mentioned embodiments and their modified examples are merely examples, and different configurations, methods, steps, shapes, materials, and values ​​may be used as necessary. Specifically, the magnetic recording medium of the present disclosure may include components other than the substrate, underlayer, magnetic layer, back layer, and barrier layer. In addition, the chemical formulas of compounds, etc. are representative, and are not limited to the valences, etc. given as long as they are general names of the same compounds.

[0144] Furthermore, the configurations, methods, steps, shapes, materials, numerical values, and the like of the above-described embodiments and their modified examples can be combined with each other without departing from the spirit of this disclosure.

[0145] In addition, in the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range may be replaced with the upper limit or lower limit of another numerical range. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more.

[0146] As described above, according to the magnetic recording medium as an embodiment of the present disclosure, it is possible to achieve both improved electromagnetic conversion characteristics and high long-term reliability. Note that the effects of the present disclosure are not limited to the above, and may be any of the effects described in this specification. In addition, the present technology may have the following configurations. (1) A magnetic recording medium having a magnetic layer and a substrate, the magnetic layer comprises a magnetic powder containing ε iron oxide, the ratio (Hrp / Hc) of the residual coercivity (Hrp) measured in the perpendicular direction of the magnetic recording medium using a pulsed magnetic field to the perpendicular coercivity (Hc) of the magnetic recording medium is 2.0 or less; The saturation magnetization (Mst) per unit area of ​​the magnetic recording medium is 4.5 mA or more. Magnetic recording media. (2) The diffraction pattern by in-plane X-ray diffraction (Cu tube) shows the first peak at 32.9° and the second peak at 36.6°. The magnetic recording medium according to (1) above. (3) The average thickness of the magnetic layer is 80 nm or less. The magnetic recording medium according to (1) above. (4) The perpendicular coercive force is 2000 Oe or more and 6000 Oe or less. The magnetic recording medium according to any one of (1) to (3) above. (5) The perpendicular coercive force is 2500 Oe or more and 4500 Oe or less. The magnetic recording medium according to any one of (1) to (3) above. (6) The mass magnetization of the magnetic powder is 30 emu / g or more and 60 emu / g or less. The magnetic recording medium according to any one of (1) to (5) above. (7) The average particle size of the magnetic powder is 20 nm or less. The magnetic recording medium according to any one of (1) to (6) above. (8) The ε iron oxide contains zirconium (Zr) and cobalt (Co). The magnetic recording medium according to any one of (1) to (7) above. (9) The magnetization curve (MH loop) that represents the relationship between magnetization and magnetic field in the magnetic layer is closed in the range of -15 kOe to +15 kOe. The magnetic recording medium according to any one of (1) to (8) above. (10) The molar ratio of cobalt in the ε-iron oxide is 3 atomic % or more and 20 atomic % or less when the total atomic % of iron (Fe) and cobalt in the ε-iron oxide is 100. The magnetic recording medium according to (8) above. (11) The molar ratio of zirconium is 1 atomic % or more and 8 atomic % or less when the total atomic % of iron (Fe) and zirconium in the ε-iron oxide is 100. The magnetic recording medium according to (8) above.

[0147] This application claims priority based on Japanese Patent Application No. 2020-007832, filed on January 21, 2020 in the Japan Patent Office, the entire contents of which are incorporated herein by reference.

[0148] Those skilled in the art will recognize that various modifications, combinations, subcombinations, and variations may occur to those skilled in the art depending on design requirements and other factors, and that such modifications are within the scope of the appended claims and their equivalents.

Claims

1. A magnetic recording medium having a magnetic layer and a substrate, the magnetic layer comprises a magnetic powder containing ε iron oxide, a ratio (Hrp / Hc) of a remanent coercivity (Hrp) measured in a perpendicular direction of the magnetic recording medium using a pulsed magnetic field to a perpendicular coercivity (Hc) of the magnetic recording medium is 2.0 or less; The saturation magnetization (Mst) per unit area of ​​the magnetic recording medium is 4.5 mA or more. Magnetic recording media.

2. The magnetic recording medium exhibits a first peak at 32.9° and a second peak at 36.6° in a diffraction pattern obtained by in-plane X-ray diffraction (Cu tube).

2. The magnetic recording medium according to claim 1.

3. The average thickness of the magnetic layer is 80 nm or less.

2. The magnetic recording medium according to claim 1.

4. The perpendicular coercive force is 2000 Oe or more and 6000 Oe or less. The magnetic recording medium according to any one of claims 1 to 3.

5. The perpendicular coercive force is 2500 Oe or more and 4500 Oe or less. The magnetic recording medium according to any one of claims 1 to 3.

6. The mass magnetization of the magnetic powder is 30 emu / g or more and 60 emu / g or less. The magnetic recording medium according to any one of claims 1 to 5.

7. The average particle size of the magnetic powder is 20 nm or less. The magnetic recording medium according to any one of claims 1 to 6.

8. The ε iron oxide contains zirconium (Zr) and cobalt (Co). The magnetic recording medium according to any one of claims 1 to 7.

9. The magnetization curve (M-H loop) showing the relationship between the magnetization and the magnetic field in the magnetic layer is closed in the range of -15 kOe to +15 kOe. The magnetic recording medium according to any one of claims 1 to 8.

10. The molar ratio of cobalt in the ε-iron oxide is 3 atomic % or more and 20 atomic % or less when the total atomic % of iron (Fe) and cobalt is 100.

9. The magnetic recording medium according to claim 8.

11. The molar ratio of zirconium in the ε-iron oxide is 1 atomic % or more and 8 atomic % or less when the total atomic % of iron (Fe) and zirconium is 100.

9. The magnetic recording medium according to claim 8.

Citation Information

Patent Citations

  • Co-Fe-BASED ALLOY SPUTTERING TARGET MATERIAL AND METHOD FOR PRODUCING THE SAME

    JP2008189996A

  • Magnetic recording medium

    JP2019023950A

  • Magnetic recording medium, method for producing particles of epsilon-type iron oxide system compound, and method for producing magnetic recording medium

    JP2019175532A

  • JPP6624332B

  • Magnetic recording medium

    WO2018203468A1