Conductive composition and molded body or coating film containing said conductive composition
A conductive composition combining carbon nanofibers with scaly graphite or spherical carbon particles enhances dispersibility and conductivity, addressing the limitations of single dispersion and achieving high electrical conductivity suitable for various applications.
Patent Information
- Application Number
- JP2021011607
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Current technologies face challenges in achieving high electrical conductivity and stable dispersion of carbon nanofibers with large aspect ratios, leading to limited utility in applications requiring good dispersibility and conductivity.
A conductive composition is developed by combining carbon nanofibers with specific shapes and sizes, along with scaly graphite or spherical carbon particles, to enhance dispersibility and conductivity, using a combination of dry and wet pulverization methods to achieve a dispersed state.
The composition exhibits significantly improved electrical conductivity compared to single dispersion, with volume resistivity reduced to 7×10^-4 Ω·cm or less, suitable for applications requiring high conductivity and dispersibility.
Smart Images

Figure 0007590880000006 
Figure 0007590880000007 
Figure 0007590880000008
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrically conductive composition comprising a base material and a carbonaceous material dispersed therein, and more particularly to an electrically conductive composition having increased electrical conductivity by using a group of carbonaceous materials of different shapes in combination, and a molded body or coating film containing the electrically conductive composition, or a paint for forming the electrically conductive composition. [Background technology]
[0002] Carbon fiber and carbon fiber reinforced plastics (CFRP) are lightweight and combine strength and flexibility, and are therefore widely used as substitutes for metals in a variety of molded products. The shortest carbon fibers are also called milled fibers, and generally have an average fiber length of 70 μm to 200 μm and an average fiber diameter of approximately 3 μm to 20 μm (3,000 nm to 20,000 nm). Because of their small shape (size), they are often used as abrasives, reinforcing agents, auxiliary agents, etc.
[0003] Chopped fiber and long fiber, which have a longer average fiber length than milled fiber, are primarily used in molded products such as prepregs and forged products. In addition, fine CFRP made by further crushing milled fibers to shorten the fiber length is used, for example, as a concrete reinforcing material. However, the shorter the particle diameter, the more difficult it becomes to process the particles, and the particles are more likely to aggregate after being pulverized. Therefore, at present, the particles are of little value in fields where good dispersion is required.
[0004] If we define carbon fibers simply based on their shape (size), without considering the actual dispersion of carbon fibers (the presence of each individual fiber) or the utility of the carbon fibers, the currently known general definitions are "carbon fibers defined as having a diameter of 3 μm to 10 μm and a length of 500 μm to 10,000 μm," "carbon nanofibers with a diameter of 50 nm to 1,000 nm and a length of 0.2 μm to 200 μm," and "carbon nanotubes with a diameter of 0.4 nm to 100 nm and a length of 50 nm to 20,000 nm."
[0005] Although there are documents that describe the diameter and aspect ratio of carbon fibers (for example, Patent Documents 1 and 2), at present, there are almost no carbon nanofiber groups like the "(1) carbon nanofiber group" in the present invention, which are actually small in shape (size), have a particularly large aspect ratio, and are in a state that allows them to be isolated (separated) approximately one by one, or that allow them to be (stably) dispersed approximately one by one in a dispersion medium, etc. At present, there are almost no carbon nanofiber groups that have the shape (size) defined above and that can be easily separated and dispersed. In addition, the utilization rate of carbon fibers of the carbon nanofiber size is extremely low due to poor dispersibility or redispersibility, etc.
[0006] Furthermore, nano-sized carbon fibers with large aspect ratios that are dispersed or in a dispersible state do not exist on the market (at least commercially). The reason for this is thought to be that when the raw carbon fibers are crushed, they are specifically and neatly split vertically, in other words, the raw filaments cannot be suitably peeled off from the filaments. Therefore, there is no known composition, molded body, coating film, dispersion liquid, or paint in which “carbon fibers such as carbon nanofibers” having a large aspect ratio, such as the “(1) carbon nanofiber group” in the present invention, are stably and well dispersed. In other words, carbon nanofibers, which have a large aspect ratio, are dispersible, and have dispersion stability, are expected to have a wide range of demands (applications), but good ones have not been realized so far.
[0007] On the other hand, it is known to use a mixture of carbonaceous materials having different shapes. Patent Document 3 describes a "carbon material for the negative electrode of a secondary battery" that contains scaly graphite particles (A) and carbonaceous particles (B). The carbonaceous particles (B) in this case have characteristic surface shape and surface properties, and are not carbon nanofibers in the first place, but are on the order of μm in size.
[0008] Patent Document 4 describes a resin composition for sliding members containing an amorphous resin, flake graphite, and carbon fibers, but the purpose is to improve physical properties, and the carbon fibers in this composition have a number average fiber diameter of 5 μm to 20 μm and are not carbon nanofibers in the first place.
[0009] There is a strong demand for carbonaceous material-containing compositions with excellent electrical performance, and for molded bodies, coating films, and paints containing the same, but excellent compositions have not yet been realized, and there is room for development. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2012-188790 A [Patent Document 2] JP 2017-066546 A [Patent Document 3] JP 2014-165018 A [Patent Document 4] JP 2015-067726 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made in view of the above-mentioned background art, and an object of the present invention is to provide an "electrically conductive composition containing a group of multiple types of carbonaceous materials having different shapes" having high electrical conductivity, and a molded body, coating film, or paint containing the electrically conductive composition. [Means for solving the problem]
[0012] The present inventors have conducted extensive research to solve the above problems and have found that a specific group of carbon nanofibers can be dispersed in a base material in an unprecedentedly favorable manner. Furthermore, they have found that by using (1) the carbon nanofibers having a specific size and shape range in combination with "(2a) the flake graphite group or (2b) the roughly spherical carbon particles," they are suitably dispersed in the base material, resulting in extremely good electrical conductivity. The present inventors also found that the combined use of at least two of these carbonaceous materials improves electrical conductivity compared to the use of either one alone, and thus completed the present invention.
[0013] That is, the present invention provides an electrically conductive composition characterized by containing the following carbonaceous material group (1) and "(2a) or (2b)" in a dispersed state in a base material. (1) A group of carbon nanofibers obtained by crushing carbon fibers, in which 50% or more of the total number of carbon nanofibers are distributed in the range of "diameter 30 nm to 1000 nm and length 0.2 μm to 70 μm" (2a) A group of flake graphite in which, when the number average value of the maximum diameter length of the basal plane of the flake graphite is D1 and the number average value of the minimum diameter length is D2, both D1 and D2 are 1 μm or more and 300 μm or less, D1 / D2 is 3 or less, and when the number average thickness of the flake graphite is d, the number average aspect ratio [(D1+D2) / 2] / d is 10 or more. (2b) A group of approximately spherical carbon particles in which L1 / L2 is 3 or less, where L1 is the number average value of the maximum diameter of the approximately spherical carbon particles and L2 is the number average value of the minimum diameter of the approximately spherical carbon particles.
[0014] In addition, the present invention provides a method for producing a conductive composition comprising the steps of: (1) carbon nanofiber group [A×r] mass % and (2a) flake graphite group and / or (2b) substantially spherical carbon particle group “B×(1-r)” mass % (r is a real number greater than 0 and less than 1) co-dispersing the (1) carbon nanofiber group [A×r] mass % and (2a) flake graphite group and / or (2b) substantially spherical carbon particle group “B×(1-r)” mass % (r is a real number greater than 0 and less than 1) in the base material, (1) The electrical conductivity is made higher than that of a composition in which only the carbon nanofiber group is dispersed in an amount of A% by mass, and The present invention provides an electrically conductive composition having a higher electrical conductivity than a composition in which only "the (2a) flake graphite group and / or the (2b) approximately spherical carbon particle group" are dispersed in an amount of B mass %.
[0015] The present invention also provides the aforementioned conductive composition, wherein the carbon nanofibers contained in the carbon nanofiber group have a number average aspect ratio of 3 or more and 200 or less.
[0016] The present invention also provides the conductive composition, wherein the (1) carbon nanofiber group is obtained by dry-pulverizing carbon fibers until the number average length becomes 100 μm or less, and then wet-pulverizing the carbon fibers.
[0017] The present invention also provides the aforementioned conductive composition, wherein the raw material for the carbon nanofiber group (1) is mesophase pitch carbon fiber.
[0018] The present invention also provides the conductive composition, wherein the (1) carbon nanofiber group is obtained by dry grinding followed by wet grinding, and the wet grinding is bead mill grinding or ball mill grinding carried out in an aqueous medium in the presence of a surfactant.
[0019] The present invention also provides a carbon nanofiber group having a volume resistivity of 7×10 -4 The present invention provides the above conductive composition having a resistivity of Ω·cm or less.
[0020] The present invention also provides the conductive composition, which contains the (2a) flake graphite group or the (2b) approximately spherical carbon particle group in an amount of 5 mass % or more and 70 mass % or less with respect to the entire carbonaceous material group.
[0021] The present invention also provides a molded article comprising the above-mentioned conductive composition.
[0022] The present invention also provides a coating film comprising the above-mentioned conductive composition.
[0023] The present invention also provides a coating material comprising the above-mentioned conductive composition and a liquid dispersion medium. Effect of the Invention
[0024] The conductive composition of the present invention solves the above problems and issues, and when (1) carbon nanofibers having a specific shape and a large aspect ratio, such as a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less, are contained approximately one by one in a base material, they can be made to be in a good dispersed state, and when the dispersion is mixed and dispersed with a specific (2a) flake graphite group or a specific (2b) roughly spherical carbon particle group to standardize the content so that it can be compared, it is surprisingly possible to increase the conductivity compared to when they are dispersed alone.
[0025] Here, "the conductivity is increased by the combined dispersion compared to the single dispersion" is defined as follows. In the following, "the conductivity is increased" can be read as "the volume conductivity is increased" or "the volume resistivity is decreased", etc.
[0026] The vertical axis represents the volume conductivity or logarithm of the volume resistivity of the conductive composition, and the horizontal axis represents the mixture ratio of "(1) carbon nanofiber group" and "(2a) flake graphite group or (2b) approximately spherical carbon particle group," "conductive compositions each having 100 mass % of the total carbonaceous material dispersed in a base material," and the measured values of the volume conductivity (logarithm) are plotted (see FIG. 10 of Example 1 and FIG. 11 of Example 2).
[0027] The left end of the horizontal axis represents "100 mass% of (1) carbon nanofiber group relative to the entire carbonaceous material," and the right end of the horizontal axis represents "100 mass% of (2a) flake graphite or 100 mass% of (2b) approximately spherical carbon particle group relative to the entire carbonaceous material," or "100 mass% as the total amount of (2a) flake graphite and (2b) approximately spherical carbon particle group." In other words, the left and right ends of the horizontal axis represent conductive compositions that contain only either (1) or "(2a) or (2b)." The left and right ends may be reversed.
[0028] Here, the content ratio of the carbonaceous material group in the base material is arbitrary for both the left and right ends. Usually, an appropriate content is set in consideration of mechanical strength, thermal properties, electrical properties, dispersibility, dispersion stability, etc., when used alone. The concentration of (1) carbon nanofibers in the conductive composition at the left end and the concentration of (2a) flake graphite and / or (2b) roughly spherical carbon particles in the conductive composition at the right end may be the same or different, so long as the above-mentioned physical properties (when used alone) are satisfactory. At both the left and right ends, the content ratio of the carbonaceous material group in the conductive composition containing the base material (concentration of the single carbonaceous material in the conductive composition) is arbitrary, so even if the concentration relative to the base material at the left or right end (i.e., the content concentration in the conductive composition) is a single point, it is said that "conductivity increases when used in combination" as long as the conditions below are met.
[0029] Also, as shown in Example 4, Table 3, and FIG. 12, the "total amount of carbonaceous materials (total carbon amount) relative to the entire conductive composition" is kept constant (constant at 40 mass% in Example 4), and within that, "(1) carbon nanofiber group" and "(2a) scaly graphite and / or (2b) approximately spherical carbon particle group" are allocated and contained, and the volume resistivity and electrical conductivity are measured to see whether, for example, the minimum value (minimum value) of volume resistivity is present in a mixture portion that is neither at the left nor the right end.
[0030] Under the above conditions, "the electrical conductivity is increased by using them in combination compared to when they are used individually" means that there is a maximum value of volume conductivity (or a minimum value of volume resistivity) in the above plot for the mixed portion (combined portion) where the "carbonaceous material on the left end" is not 100% volume conductivity by mass and the "carbonaceous material on the right end" is not 100% volume conductivity by mass. "Conductivity increases when used in combination" means that even when the vertical axis is the logarithm of the volume resistivity (of the conductive composition), the minimum value is in the plot for the above combination (the middle part, not the left end or the right end).
[0031] The (1) carbon nanofiber group in the present invention exhibits superior thermal, mechanical, and electrical effects compared to other carbon nanofiber groups, even when used alone as a dispersed component in a base material. Generally, the more carbonaceous materials are contained in a base material, the higher the electrical conductivity becomes, but this usually leads to deterioration in physical properties such as mechanical strength, dispersibility, dispersion stability, cost, etc. According to the present invention, it is possible to overcome this contradictory relationship, and further, by using the specific (2a) flake graphite group or the specific (2b) substantially spherical carbon particle group in combination, the electrical properties are further improved.
[0032] Generally, when a base material with an overwhelmingly low electrical conductivity is mixed with multiple types of fine particles (carbonaceous material groups) with different electrical conductivities, the electrical conductivity of the resulting composition (molded body), when compared at the same content level, will be at most the electrical conductivity when the fine particle group (carbonaceous material group) with the higher electrical conductivity is contained alone. However, in the present invention, when a comparison was made at the same content level (when the content was made so that the electrical conductivity could be compared), the dispersion of a specific plurality of types of carbonaceous materials in a base material was able to increase the electrical conductivity more than that of either of the materials dispersed alone.
[0033] In particular, with regard to (1) carbon nanofiber group, by using specific raw carbon fibers, a specific crushing method, a crushing method while performing a specific surface treatment, or by performing a specific treatment, it was possible to obtain (1) carbon nanofiber group having an unprecedentedly high dispersibility in the base material. Furthermore, by using such (1) carbon nanofibers and mixing and dispersing them with "(2a) flake graphite groups or (2b) roughly spherical carbon particle groups," it is possible to increase the electrical conductivity (particularly the volume electrical conductivity) compared to using them alone.
[0034] In the first place, the carbon nanofiber group (1) according to the present invention, in which 50% or more by number of all carbon nanofibers are distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less," has not existed in the past. Even if the above numerical values (ranges) existed (were known) as the definition of "carbon nanofiber," they would actually be non-dispersible or lacking dispersion stability. Therefore, if we limit the scope to carbon nanofibers that have dispersibility, etc., the above "(1) carbon nanofiber group" is novel.
[0035] Carbon nanofibers are generally known as carbon fibers in the broad sense, with multiple fibers tightly bound to the surroundings to form a single unit. Conventionally, it has not been possible to produce carbon nanofibers by separating or peeling them while maintaining a high aspect ratio. In other words, conventional techniques have not been able to produce carbon nanofibers by pulverization or other methods while maintaining a high aspect ratio, and to make them reproducibly and stably separable or dispersible without causing agglomeration. As described above, the improvement in electrical conductivity compared to the case of a single dispersion is due to the good dispersibility of the (1) carbon nanofiber group.
[0036] The (1) carbon nanofiber group in the present invention has extremely good dispersibility in the base resin, so that each carbon nanofiber can come into contact with and be entangled with the flake graphite or approximately spherical carbon particles. In particular, by connecting flake graphite or approximately spherical carbon particles that are not in direct contact with each other, and ensuring electrical conductivity, the electrical conductivity is increased synergistically (resistivity is reduced).
[0037] Since the electrical conductivity increases when these are used in combination, the electrically conductive composition of the present invention and molded bodies and coating films containing the electrically conductive composition of the present invention can achieve higher electrical conductivity even when the total content of carbonaceous materials, such as (1) carbon nanofibers, (2) flake graphite, and (3) approximately spherical carbon particles, in the base material is less or the same. Therefore, the electrically conductive composition of the present invention can be particularly suitably used for molded bodies and coating films that require high electrical conductivity, high electromagnetic wave absorption, etc., or for types of molded bodies and coating films in which it is desired to reduce the content of carbonaceous materials. [Brief description of the drawings]
[0038] [Figure 1] (1) Scanning electron microscope (SEM) photographs of the cross section of pitch-based carbon fiber, the raw material before grinding used to produce carbon nanofibers. (Left) Radial mesophase pitch-based carbon fiber (middle) Random mesophase pitch-based carbon fiber (right) Onion mesophase pitch-based carbon fiber [Diagram 2] (1) Schematic diagrams of the cross sections of pitch-based carbon fibers, which are raw materials before being pulverized in the production of carbon nanofibers. (a) (a') Random mesophase pitch-based carbon fibers (b) Radial mesophase pitch-based carbon fibers (c) Onion mesophase pitch-based carbon fibers [Diagram 3] (1) A scanning electron microscope (SEM) photograph of the cross section of a single random mesophase pitch-based carbon fiber, which is preferably used as a raw material for carbon nanofibers. [Figure 4] (1) Scanning electron microscope (SEM) photographs of random mesophase pitch-based carbon fibers (before grinding), which are preferably used as a raw material for carbon nanofibers. (a) 400x (b) 1300x. [Diagram 5] (1) Scanning electron microscope (SEM) images of carbon fibers after dry grinding in the production of carbon nanofibers. (a) 600x magnification (b) 1500x magnification [Figure 6] (1) This is a 700x optical microscope (biological microscope) photograph of the wet grinding process in the production of carbon nanofibers (reference image). [Figure 7] (1) Scanning electron microscope (SEM) photographs of carbon nanofibers after wet grinding. (a) 1500x magnification (b) 6500x magnification [Figure 8] FIG. 1 is a schematic diagram showing a process for producing filaments of (random type) mesophase pitch-based carbon fibers that are preferably used as a raw material for carbon nanofibers. [Figure 9] FIG. 1(1) is a schematic diagram showing an example of an apparatus used for dry pulverization in producing carbon nanofiber groups. [Figure 10] 1 is a graph of Example 1, showing the change in volume resistivity [Ω·cm] (vertical axis) when the horizontal axis represents the mixture ratio of "(1) the inclusion of carbon nanofiber groups and polyimide" and "(2a) the inclusion of flake graphite (graphene) and polyimide." (a) The vertical axis (volume resistivity) is on a logarithmic scale. (b) The vertical axis (volume resistivity) is on a linear scale. [Figure 11] 1 is a graph of Example 2, showing the change in volume resistivity [Ω·cm] (vertical axis) when the horizontal axis represents the mixture ratio of "(1) a material containing carbon nanofibers and polyimide" and "(2b) a material containing approximately spherical carbon particles (Ketjen black) and polyimide." (a) Vertical axis (volume resistivity) is on a logarithmic scale (b) Vertical axis (volume resistivity) is on a linear scale [Figure 12]13 is a graph showing the measurement results of the volume resistivity of Example 4 (a mixture of (1) carbon nanofiber groups and (2b) approximately spherical carbon particle groups, the base material being polyester). [Figure 13] 1 is a graph showing the measurement results of the volume resistivity of Comparative Example 1 ((1) a mixture of carbon nanofiber groups and (2a') flake graphite having a small aspect ratio, with the base material being polyester). [Figure 14] 1 is a graph showing the measurement results of volume resistivity in Example 5 and Comparative Example 2. [Figure 15] 1 is a scanning electron microscope (SEM) photograph of the (2a) flake graphite used in Examples 1 and 2 taken at 1200 times. [Figure 16] 1 is a scanning electron microscope (SEM) photograph of the (2a) flake graphite used in Examples 1 and 2 at a magnification of 5,000 times. [Figure 17] 1 is a 600x scanning electron microscope (SEM) photograph of (2a') (spherical) flake graphite used in Comparative Example 1. [Figure 18] 1 is a scanning electron microscope (SEM) photograph of (2a') (spherical) flake graphite used in Comparative Example 1 at 4,000 times magnification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The present invention will be described below, however, the present invention is not limited to the specific embodiments below and can be modified as desired within the scope of the technical concept.
[0040] The conductive composition of the present invention is characterized in that it contains the following carbonaceous material group (1) and (2a) or (2b) in a dispersed state in a base material. (1) A group of carbon nanofibers obtained by crushing carbon fibers, in which 50% or more of the total number of carbon nanofibers are distributed in the range of "diameter 30 nm to 1000 nm and length 0.2 μm to 70 μm" (2a) A group of flake graphite in which, when the number average value of the maximum diameter length of the basal plane of the flake graphite is D1 and the number average value of the minimum diameter length is D2, both D1 and D2 are 1 μm or more and 300 μm or less, D1 / D2 is 3 or less, and when the number average thickness of the flake graphite is d, the number average aspect ratio [(D1+D2) / 2] / d is 10 or more. (2b) A group of nearly spherical carbon particles in which L1 / L2 is 3 or less, where L1 is the number average value of the maximum diameter of the nearly spherical carbon particles and L2 is the number average value of the minimum diameter of the nearly spherical carbon particles.
[0041] The length and diameter of the carbon nanofibers in the present invention; the length and diameter of the carbon nanofibers during production; (1) the number average diameter and number average length of the carbon nanofiber groups in the present invention; (2a) the number average value of the maximum and minimum diameter lengths on the basal plane of the scaly graphite groups in the present invention; and (2b) the number average value of the maximum and minimum diameters of the approximately spherical carbon particle groups in the present invention; etc., the length and average length are measured and calculated by randomly selecting 100 nanofibers with a scanning electron microscope (SEM), measuring the diameter and length of each nanofiber, and taking the arithmetic mean.
[0042] In the present invention, the sizes and average sizes such as diameter, length, aspect ratio, etc. are defined as those measured and calculated as described above. Since the carbon nanofibers in the present invention have a large aspect ratio, the diameter and length of each fiber are measured using a microscope rather than using a particle size distribution meter. Since the diameter and length cannot be suitably measured using an automatic particle size distribution meter, the above method is the only option.
[0043] [(1) Carbon nanofibers] As described above, the (1) carbon nanofiber (group) in the present invention is essentially one obtained by pulverizing carbon fibers, in which 50% or more of the total carbon nanofibers are distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less"
[0044] In the present invention, the term "carbon fiber" refers to any long and thin carbonaceous material (carbon material) having a graphene structure, and includes carbon fiber, carbon nanofiber, and carbonaceous materials (carbon materials) of similar size to these, etc. Furthermore, the term "carbon fiber" includes a filament 10 of a carbonaceous material (carbon material) having a graphene structure, the elementary filaments 20 that constitute the filament 10, and a strand in which the filaments 10 are arranged vertically in parallel, etc.
[0045] The carbon nanofiber group in the present invention has a diameter of 30 nm or more and 1000 nm or less, and a length of 0.2 μm or more and 70 μm or less, with 50% or more of the total number of the carbon nanofiber group being distributed in that range. It is essential that 50% or more of the total is distributed within the above range, but preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, particularly preferably 95% or more, and most preferably 98% or more. According to the present invention, since it is possible to produce particles having the above-mentioned percentage or more, the sharper the distribution, the better in terms of dispersibility and the properties of the molded body and coating material containing the particles, but a broader distribution is acceptable in terms of productivity, etc.
[0046] The diameter of the "carbon nanofibers in which 50% or more by number is distributed" is 30 nm to 1000 nm, preferably 50 nm to 850 nm, and more preferably 100 nm to 700 nm. According to the present invention, carbon nanofibers having a diameter in the above range can be produced with good yield. If the diameter is too small, it may be difficult to manufacture, or the length may be too short, resulting in a small aspect ratio, etc. On the other hand, if the diameter is too large, the performance at the intended use may be poor, or the applications of the carbon nanofiber group may be limited.
[0047] The length of the "carbon nanofibers in which 50% or more by number is distributed" is 0.2 μm to 70 μm, more preferably 1 μm to 50 μm, even more preferably 2 μm to 30 μm, and particularly preferably 5 μm to 20 μm. According to the present invention, carbon nanofibers having a length in the above range can be produced with good yield. If the length is too short, the aspect ratio may become small, the performance may be poor in the application (e.g., molded body, paint, etc.), the applications of the carbon nanofibers may be limited, it may be difficult to prevent aggregation, etc. On the other hand, if the length is too long, the applications of the carbon nanofibers may be limited, and it may be difficult to manufacture while maintaining a large aspect ratio, etc.
[0048] The above size distribution is determined based on the diameter and length ranges in which many (e.g., 50% or more by number, 70% or more by number, etc.) carbon nanofibers are distributed within the carbon nanofiber group, but when specified on average, it is preferable that the number average diameter is 30 nm or more and 1000 nm or less, and the number average length is 0.2 μm or more and 70 μm or less. In other words, in the conductive composition of the present invention, (1) it is preferable that the number average diameter of the carbon nanofibers contained in the carbon nanofiber group is 30 nm or more and 1000 nm or less, and that the number average length is 0.2 μm or more and 70 μm or less.
[0049] The number average diameter is more preferably from 50 nm to 850 nm, particularly preferably from 100 nm to 700 nm. The number average length is more preferably from 1 μm to 50 μm, further preferably from 2 μm to 30 μm, and particularly preferably from 5 μm to 20 μm.
[0050] The isolable and dispersible carbon nanofibers of the present invention have a diameter and length within the above ranges (preferably within the above ranges), and therefore one of their characteristics is that they have a large aspect ratio. The number average aspect ratio of the carbon nanofibers is preferably 3 or more and 200 or less, more preferably 5 or more and 160 or less, even more preferably 7 or more and 130 or less, particularly preferably 15 or more and 100 or less, and most preferably 20 or more and 70 or less.
[0051] If the aspect ratio is too small, it may not be possible to suitably increase the electrical conductivity when used in combination with the flake graphite group (2a) or the approximately spherical carbon particle group (2b), and the performance of, for example, conductive compositions, molded bodies, coating films, paints, etc., in which the carbon nanofiber group is contained may be inferior or applications may be limited. On the other hand, if the aspect ratio is too large, manufacturing may become difficult or the part may be wasted.
[0052] If pitch-based carbon fibers are used as the raw material and dry-milled and then wet-milled, the raw carbon fibers are specifically and neatly split vertically during milling; in other words, the raw filaments 20 can be suitably peeled off from the filaments 10 without shortening their length too much. In the present invention, this resulted in the production of carbon nanofibers that were previously not possible and have a suitable aspect ratio, and it is presumed that the large aspect ratio and the suitable size and shape of the carbon nanofibers improved the physical properties of the molded bodies, coating films, and paints in which the obtained carbon nanofibers are dispersed. In addition, the electrical conductivity could be suitably increased by using the carbon nanofibers in combination with flake graphite groups (2a) or approximately spherical carbon particle groups (2b).
[0053] When the carbon nanofibers are contained or dispersed in the base material, they may be contained in a solid (powder) state or may be contained first as a dispersion liquid. When it exists in a solid (powder) form, for example, as shown in FIG. 7, it is in a state where each carbon nanofiber can be isolated or dispersed individually.
[0054] When present in a dispersion (paint), molded body, or coating, the carbon nanofibers are substantially dispersed individually. Although it is not necessarily possible to separate the carbon nanofibers into individual filaments as described below, it is sufficient if the carbon nanofibers can be dispersed individually. "Substantially dispersed individually" means "dispersed approximately individually," and refers to a state in which the carbon nanofibers are not strongly aggregated in parallel, and the base material is embedded between the carbon nanofibers. The (1) carbon nanofiber group in the present invention can be made to have the above-mentioned dispersibility and dispersed state.
[0055] <(1) Production of carbon nanofiber(s)> In the present invention, the carbon nanofibers having the above-mentioned shape (diameter and length) and the carbon nanofiber group having the above-mentioned distribution are obtained by at least dry pulverization and then wet pulverization. Furthermore, by specifying the carbon fibers as the raw material, the (re)dispersible carbon nanofiber group having the above-mentioned shape and distribution can be obtained. It is also preferable to add other treatments (operations) as necessary before the dry grinding, between or during the above two types of grinding, or after the wet grinding. Moreover, the above dry grinding and the above wet grinding may each be carried out in one stage or two or more stages.
[0056] In particular, "carbon nanofibers obtained by dry-pulverizing pitch-based carbon fibers and then wet-pulverizing them" can be suitably dispersed in a base material, and the molded body, coating film, or paint in which they are dispersed has excellent physical properties as described below, and can be suitably used in combination with (2a) flake graphite or (2b) approximately spherical carbon particles to increase electrical conductivity.
[0057] A "particularly preferred manufacturing process" for the (1) carbon nanofiber group of the present invention is shown below, but the (1) carbon nanofiber group of the present invention is not limited to only those actually manufactured by the "preferred manufacturing process" described below. However, the (1) carbon nanofiber group in the present invention can be produced by changing the production conditions, such as the raw material carbon fiber (carbon material), the grinding method and conditions, the types of dispersants and surfactants used, and the types of treatments, as specified in the "preferred production method" described below.
[0058] Regarding the manufacturing process, when the following processes are carried out, it is particularly preferable to carry out them in the following order, but other processes may be interposed between them. That is, preparation of raw carbon fiber, pre-grinding, dry grinding, heat treatment, moistening treatment, wet grinding, anti-agglomeration treatment, and water removal treatment.
[0059] Of the above, at least preparing specific raw carbon fibers, dry grinding, and wet grinding are particularly important for obtaining the (1) carbon nanofiber group of the present invention, and by doing so, the conductive composition of the present invention, and a molded body or coating film or paint containing the same can be suitably produced. Of the above, pre-grinding, heat treatment, wetting treatment, aggregation prevention treatment, and water removal treatment are not essential, but for good production, it is preferable to carry out some or all of them as necessary. In particular, heat treatment is preferable when the raw material contains a resin such as a sizing material, but may not be carried out when the raw material has not been subjected to sizing treatment or the like. Each processing step will be described below in the order of preferred processing.
[0060] <<Raw carbon fiber>> In the present invention, the carbon fiber before grinding (raw carbon fiber) is not particularly limited, but it is preferable to use pitch-based carbon fiber, more preferable to use mesophase pitch-based carbon fiber, and particularly preferable to use random mesophase pitch-based carbon fiber (see FIG. 4). With PAN-based carbon fibers, no matter what grinding method is used, it is difficult to obtain a group of carbon nanofibers having a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less, and having the high number average aspect ratio as described above.
[0061] Furthermore, even if the pitch-based carbon fiber is an isotropic pitch-based carbon fiber, it may be difficult to obtain carbon nanofibers having the above size, shape, and distribution.
[0062] On the other hand, mesophase pitch-based carbon fibers are classified at least into radial type (Figure 1 (left), Figure 2 (b)), random type (Figure 1 (center), Figure 2 (a) (a'), Figure 3), and onion type (Figure 1 (right), Figure 2 (c)) based on their cross-sectional shape (i.e., internal shape). A "random type" is one in which the fiber cross section is random. For this reason, it was named random type.
[0063] In the present invention, even if the mesophase pitch-based carbon fiber is a radial type mesophase pitch-based carbon fiber or an onion type mesophase pitch-based carbon fiber, it may be somewhat difficult to obtain a carbon nanofiber group having the above size, shape, and distribution. If a radial type or an onion type is used as the raw carbon fiber, it may not be possible to preferably obtain the above shape, form, and distribution, and in particular, it may not be possible to preferably obtain a carbon nanofiber group having a large number average aspect ratio (for example, only those with an aspect ratio of less than 3 may be obtained).
[0064] The "filaments constituting the random mesophase pitch carbon fiber" are made up of smaller rod-shaped or plate-shaped (sheet-shaped) filaments. For example, in Figure 3, plate-shaped (sheet-shaped) filaments are vertically assembled. In this specification, the “smaller rod-shaped or plate-shaped (sheet-shaped) object” constituting the filament 10 is abbreviated as “bare filament” 20. It is thought that within one elementary filament, graphene structures in which benzene rings are condensed are stacked together facing in the same direction to form a single unit, or one or more carbon nanotubes are bundled together facing in the same direction to form a single unit.
[0065] In the present invention, the carbon fiber raw material has a number average thickness or number average thickness of the filaments 20 constituting the filament 10 of preferably 10 nm or more and 200 nm or less, more preferably 15 nm or more and 150 nm or less, even more preferably 20 nm or more and 100 nm or less, and particularly preferably 30 nm or more and 70 nm or less. When the size of the raw carbon fiber filaments is equal to or larger than the lower limit, a synergistic effect is achieved when used in combination with the flake graphite group (2a) or the approximately spherical carbon particle group (2b), thereby making it possible to suitably increase the electrical conductivity (reduce the resistance value). On the other hand, when it is equal to or less than the above upper limit, it is easy to prepare "filaments 10 or carbon fibers" containing such raw filaments 20 as a raw material.
[0066] Fig. 8 shows an outline of the manufacturing process of mesophase pitch carbon fiber filament 10. Random mesophase pitch carbon fiber can also be obtained by adjusting the spinning viscosity, nozzle shape, flow state of the raw material pitch, etc. in Fig. 8. The manufacturing process of mesophase pitch-based carbon fiber does not include a drawing process. The microstructure controlled in the spinning process becomes the crystal structure of the filament 10 almost as it is, and boundaries of different crystal structure orientations are created, resulting in the appearance (existence) of the raw filament 20.
[0067] In FIG. 8, the thickness of the raw material filament 10 is usually 4000 nm to 20000 nm, and often 5000 nm to 12000 nm. On the other hand, the number average thickness or number average thickness of the raw filaments 20 in the raw material carbon fiber filament 10 in the present invention is preferably 10 nm or more and 200 nm or less, and more preferably 15 nm or more and 100 nm or less. Therefore, in the raw material carbon fiber, one filament 10 typically contains 40 to 700 raw filaments 20, and in most cases 60 to 400 raw filaments 20. When one elementary filament 20 is divided (defined) at a boundary where the orientation of the crystal structure is different, the above number of elementary filaments 20 are bundled together to form one filament 10. Note that in Fig. 8, for ease of viewing, it is depicted as if one filament were made up of three elementary filaments when viewed from the front.
[0068] In the present invention, when random mesophase pitch carbon fibers are used as the raw material, the above-mentioned embodiment is particularly preferred, although there are no limitations thereon. The shape, distribution, etc. of the (1) carbon nanofiber group in the present invention, as well as whether or not such (1) carbon nanofiber group can be formed in the first place, depend on the type of carbon fiber that is the raw material.
[0069] <<<Relationship between the carbon nanofiber of the present invention and the raw filament>>> The carbon nanofibers of the present invention are preferably configured by gathering together 2 to 20 "prime filaments constituting the raw filament," more preferably 3 to 16, and particularly preferably 4 to 12. The number of the prime filaments is the average value for each carbon nanofiber in the (1) carbon nanofiber group. When producing carbon nanofibers, the crystallinity and external shape of the filaments may be slightly deformed, but this is also included in the above-mentioned "number of filaments." Even if the filaments are originally plate-shaped, they become elongated after being crushed, and are therefore referred to as the "number of filaments" as above.
[0070] <<Pre-grinding>> The carbon fibers used as raw materials may be in the form of chopped fibers or milled fibers, but are preferably in the form of chopped fibers. In the case of milled fibers, many short fibers with lengths of about 1 μm are mixed in, so chopped fibers are preferred in order to obtain carbon nanofibers with a large aspect ratio. In the case of milled fibers, even if the average length is said (publicly announced) to be, for example, 70 μm, many short fibers with lengths of about 1 μm may be mixed in.
[0071] Although not limited, the carbon fiber raw material in the pre-pulverization is preferably 1 mm to 15 mm on average, more preferably 2 mm to 10 mm, and particularly preferably 5 mm to 8 mm. For example, in the case of a long fiber bobbin type, pre-pulverization may be necessary. If the size is within the above range from the beginning, it is also preferable not to perform pre-pulverization.
[0072] The grinding method for the pre-grinding is not particularly limited, and any commercially available dry grinding machine can be used, for example, a cutter mill or the like can be used as the device.
[0073] <<Dry grinding>> In the present invention, "dry grinding" is not particularly limited, but is preferably airflow grinding, cutter grinding, or "grinding in which both airflow grinding and cutter grinding are performed simultaneously." "Grounding in which both airflow grinding and cutter grinding are performed simultaneously" means "grinding that has both an airflow grinding mechanism and function and a cutter grinding mechanism and function at the same time."
[0074] <<<Airflow grinding>>> Examples of the airflow pulverization include pulverization using an airflow pulverizer such as a cyclone mill, and a jet mill. Airflow pulverization using a cyclone mill produces an airflow by rotating an impeller (rotating blade) and pulverizes the object thrown into the airflow in a dry state to produce fine particles, while airflow pulverization using a jet mill produces fine particles by colliding the object with a collision plate in a dry state to pulverize the object. In order to obtain (1) carbon nanofibers of a predetermined shape by wet grinding, an airflow grinder having a rotating body such as an impeller, rotor, blade, or rotary blade (such as a jet mill) or a grinder described later in <<Grinding performing both airflow grinding and cutter grinding simultaneously>>> is preferable as the "dry grinding before wet grinding".
[0075] As the cyclone mill, commercially available devices can also be suitably used, such as the Cyclone Mill manufactured by Shizuoka Plant Co., Ltd., the Cyclone Mill manufactured by Shizuoka Seiki Co., Ltd., the Super Powder Mill manufactured by Nishimura Machinery Works Co., Ltd., the Tornado Mill manufactured by Sansho Industry Co., Ltd., and the Dream Mill manufactured by Furukawa Industrial Machinery Systems Co., Ltd.
[0076] The structure of the cyclone mill is not particularly limited, but it is particularly preferred that the cyclone mill has one or more impellers and crushes the materials to be crushed by mainly colliding them with each other using a swirling air current generated by the impeller, because this makes it easier to achieve the effects of using the air current crusher, there is very little metal contamination, etc.
[0077] As the jet mill, commercially available devices can be suitably used, for example, from Seishin Enterprise Co., Ltd., Hosokawa Micron Corporation, Nippon Pneumatic Co., Ltd., and Nisshin Engineering Inc.
[0078] <<<Cutter-type crushing>>> Examples of cutter-type pulverization include pulverization using a crusher mill, a pin mill, a cutter mill, a hammer mill, an axial flow mill, and the like.
[0079] <<<Simultaneous airflow and cutter grinding>>> As the dry pulverization in the present invention, pulverization in which both airflow pulverization and cutter pulverization are carried out simultaneously is particularly preferred. In particular, the dry grinding in the present invention is preferably carried out using a dry grinder having a blade and capable of applying shear and impact, or is preferably carried out using a dry grinder that applies "shear and impact by a blade". A schematic diagram of an example of such a dry grinding mill is shown in FIG.
[0080] In the case of "full airflow mills that do not use impellers for pulverization" such as jet mills, cyclone mills, tornado mills, Dream Mills (registered trademark), etc., depending on the raw material, the diameter may become too small in the dry pulverization stage, which may result in an aspect ratio that is too small (resulting in a round shape) in the subsequent wet pulverization. Therefore, although not limited thereto, they may not be very suitable for pulverization prior to wet pulverization.
[0081] The ambient temperature or set temperature in dry grinding is not particularly limited and may be in accordance with the method of use of the device used, but is preferably 0°C or higher and 50°C or lower, and particularly preferably 5°C or higher and 35°C or lower. The impeller rotation speed may also be determined in accordance with the method of use of the device used, but is preferably 4,000 rpm or more and 20,000 rpm or less, and particularly preferably 8,000 rpm or more and 15,000 rpm or less.
[0082] It is preferable to use the above-mentioned apparatus and the above-mentioned pulverizing method to dry-pulverize the material until the number average length reaches 100 μm or less, and then to provide the material for the next step. By dry-pulverizing the carbon nanofibers to a particle size of 100 μm or less and then wet-pulverizing the same, the diameter, length, aspect ratio, shape distribution, etc. of the carbon nanofibers tend to fall within the above-mentioned essential or preferred ranges.
[0083] It is preferable to adjust the number average length by dry grinding to 100 μm or less, more preferably 5 μm to 70 μm, even more preferably 7 μm to 50 μm, and particularly preferably 10 μm to 40 μm. If the number average length after dry grinding is too long, it may be difficult to achieve a final diameter and length of the carbon nanofiber within the above-mentioned range in the subsequent wet grinding step, even if the conditions for the wet grinding are adjusted. On the other hand, if the length after dry pulverization is too short, the length of the carbon nanofibers after wet pulverization cannot be longer than that, and therefore it may be difficult for the final length and number-average aspect ratio of the carbon nanofibers to fall within the above-mentioned preferred ranges, etc. In particular, the aspect ratio of the final carbon nanofibers may be too small.
[0084] Regarding the number average diameter after dry milling, it is difficult to make it small by dry milling alone, that is, it is difficult to mill so as to increase the aspect ratio. Furthermore, if the diameter is forcibly reduced by dry milling, the length also becomes shorter, and it becomes difficult to keep the final aspect ratio after wet milling within a suitable range. The diameter after dry pulverization is preferably 3000 nm or more, more preferably 5000 nm to 15000 nm, and particularly preferably 7000 nm to 12000 nm. It is desirable to carry out dry pulverization so that the diameter falls within this range.
[0085] The number average aspect ratio after dry grinding is not particularly limited, but is preferably 10 or less, more preferably 1.2 or more and 7 or less, and particularly preferably 1.5 or more and 5 or less. By dry grinding, it is difficult to increase the average aspect ratio above the upper limit in the first place, i.e., it is difficult to reduce the average fiber diameter to a degree that allows the average aspect ratio to be increased above the upper limit. In the present invention, it has been found that by performing dry pulverization, the number average length is preferably set to 100 μm or less, and a relatively large diameter and a relatively small number average aspect ratio are achieved, or by performing wet pulverization in this manner, a group of carbon nanofibers having the above-mentioned suitable "diameter, length, and large number average aspect ratio" can be finally obtained.
[0086] <<Heat treatment>> In the electrically conductive composition of the present invention, the (1) carbon nanofiber group is preferably substantially free of any resin that is mixed in the raw carbon fibers before pulverization. Here, the case where a mixed resin is included includes, for example, a case where a sizing agent or the like is contained in the carbon fiber as a raw material. That is, the mixed resin is not limited, but includes, for example, a sizing agent or the like.
[0087] In the present invention, when a resin is present in the dry-ground product, it is preferable to remove the resin by carrying out a heat treatment. In other words, the conductive composition of the present invention contains the (1) carbon nanofiber group obtained by dry grinding and then wet grinding, and it is preferable that a heat treatment is performed between the dry grinding and the wet grinding to remove any resins present in the raw materials. In addition, when no resin such as a sizing agent is mixed in, the heat treatment can be omitted.
[0088] The conditions for the heat treatment are not limited, but for example, the material is heated in a furnace at a temperature of 320°C to 480°C for 5 to 15 minutes, and the resin content is reduced to preferably 0.1 mass% or less, and particularly preferably 0.01 mass% or less. The term "substantially free of mixed resins" refers to a state in which the resin content is reduced to the above-mentioned level (by the above-mentioned heat treatment, etc.). By carrying out the heat treatment, preferably after dry grinding and before wet grinding, the grinding and dispersion effects of the wetting agent or surfactant used in the subsequent wet treatment or wet grinding step (if wet treatment is carried out) are improved.
[0089] <<Wet processing>> Although not limited thereto, it is preferable to further carry out a moistening treatment, and it is particularly preferable to carry out the moistening treatment after the dry grinding or heat treatment. The wet treatment is preferably carried out by immersing the product obtained above in an aqueous solution containing an anionic surfactant, a cationic surfactant, or an amphoteric surfactant, which can also be suitably used in the subsequent wet grinding.
[0090] The anionic surfactant is preferably a polymeric anionic surfactant ("polymer" also includes oligomers), and more preferably an alkali metal salt, ammonium salt, alkylammonium salt, alkylolammonium salt, or the like, of a (co)polymer having an acid group. The above-mentioned anionic surfactants may be used alone or in combination of two or more kinds.
[0091] The above-mentioned "(co)polymer having an acid group" is particularly preferably at least one (co)polymer selected from the group consisting of (co)polymers of (meth)acrylic acid, (co)polymers of (anhydride) phthalic acid, (co)polymers of vinylbenzenesulfonic acid, and (co)condensates of naphthalenesulfonic acid. Here, the terms "(co)", "(meth)", and "(anhydride)" include both the presence and absence of parentheses. In the case of copolymers, the copolymerizing monomer is not particularly limited, and examples thereof include (meth)acrylic acid alkyl esters, (meth)acrylic acid hydroxyalkyl esters, styrene, vinyl acetate, and the like. The (co)condensation product of naphthalenesulfonic acid includes a product in which the ring is bonded with an aldehyde such as formaldehyde. In the case of the co-condensation product, the co-condensation monomer includes phenol, cresol, naphthol, etc.
[0092] In addition, the cationic surfactant is preferably a surfactant in which a quaternary ammonium is a hydrophilic group, and the "N" of the quaternary ammonium is + The substituent on " is not particularly limited, but preferable are alkyl groups (which may have a substituent) such as stearyl group, palmityl group, dodecyl group, methyl group, benzyl group, butyl group, etc. Furthermore, long-chain alkyl groups having 12 or more carbon atoms are more preferable. The counter anion is not particularly limited, but a halogen ion such as a chloride ion or a bromide ion is particularly preferred.
[0093] Examples of amphoteric surfactants include alkyl betaine type, fatty acid amidopropyl betaine type, alkyl imidazole type, amino acid type, and amine oxide type.
[0094] Among these, it is preferable to use an anionic surfactant or an amphoteric surfactant. The surfactant content and the carbon fiber content (after dry grinding) in the aqueous dispersion medium are in the same range as the numerical range for <wet grinding> described below.
[0095] The use of a surfactant, and in particular the use of the preferred anionic or amphoteric surfactants described above, has the effect of unraveling the carbon fibers vertically, allowing the diameter to be reduced while maintaining a long length, resulting in carbon nanofiber(s) with a large average aspect ratio.
[0096] <<Wet grinding>> In the present invention, the (1) carbon nanofiber group production method preferably includes dry pulverization followed by wet pulverization. The wet pulverization is not particularly limited, but is preferably bead mill pulverization or ball mill pulverization. Bead mill pulverization or ball mill pulverization in an aqueous medium in the presence of a surfactant is particularly preferable. Between the dry milling and the wet milling, the above-mentioned "other treatments" such as heat treatment and wet treatment may be performed. The "other treatments" further include premixing, preliminarily preparing a solution, and the like.
[0097] The surfactant may be any of those described in the <Wetting Treatment> section above, whether the wetting treatment has been performed or not. The same surfactants are also preferred. That is, as described above in the section on <Wet Treatment>, anionic surfactants, cationic surfactants, or amphoteric surfactants are preferred. The surfactant used in the wet treatment may be used as is in the wet grinding, or a new surfactant may be added or a different surfactant from that used in the wet treatment may be added during the wet grinding.
[0098] The amount of the surfactant used is not particularly limited, but is preferably 0 parts by mass or more and 100 parts by mass or less, more preferably 0 parts by mass or more and 50 parts by mass or less, and particularly preferably 0 parts by mass or more and 10 parts by mass or less (when two or more types of surfactants are used in combination, the total amount) relative to 100 parts by mass of the carbon fibers (carbon nanofibers in the process of being ground) to be ground and dispersed. If too much surfactant is used, the carbon fibers may aggregate as they are unraveling vertically. As a result, the carbon nanofibers will be in an aggregated state in the dispersion, which may affect the physical properties of the resulting product when applied to an object.
[0099] When the above-mentioned wetting treatment is carried out, a new surfactant may be added in wet pulverization, or the surfactant that was mixed in the wetting treatment may be used as it is. When a surfactant is added during wet grinding, the surfactant may be the same as or different from the surfactant used in the wet treatment.
[0100] <<<Wet grinding method, equipment and conditions>>> By carrying out wet pulverization, it is possible to produce (1) carbon nanofibers that have the specific shape (diameter, length, aspect ratio) and particle size distribution as described above and are also well-dispersed. The conditions of the wet pulverization are adjusted so as to obtain carbon nanofiber(s) having the above-mentioned specific shape (diameter, length, aspect ratio) of the present invention.
[0101] Preferred materials for the grinding media used in wet grinding include glass, alumina, zircon (zirconia-silica ceramics), zirconia, metal (steel), and the like.
[0102] Taking a bead mill as an example, the diameter of the beads used is preferably 0.1 mm or more and 3 mm or less, more preferably 0.2 mm or more and 2 mm or less, and particularly preferably 0.3 mm or more and 1 mm or less. If the bead diameter is too large, the number of beads in the bead mill container will decrease, which will reduce the number of contact points, making it impossible to crush and disperse properly, or the diameter will not be small enough to crush the beads, etc. On the other hand, if the bead diameter is too small, it may not be possible to crush and disperse properly, or crushing may take too long, etc.
[0103] The bead filling rate used in the bead mill is preferably from 45% to 90%, more preferably from 55% to 87%, and particularly preferably from 65% to 85%. If the bead filling rate is too low, the carbon fibers are less likely to split vertically, and it may be difficult to produce carbon nanofibers with a large aspect ratio, etc. On the other hand, if the bead filling rate is too high, it may be difficult for the stirring blades of the bead mill to rotate, etc.
[0104] The carbon fiber content after dry pulverization is preferably 1% by mass to 20% by mass, more preferably 3% by mass to 15% by mass, and particularly preferably 5% by mass to 10% by mass, based on the entire slurry to be treated by the bead mill.
[0105] The shape of the stirring blade used in the bead mill treatment is not particularly limited. The rotation speed of the stirring blade (agitator) depends on the span length of the stirring blade and the capacity of the bead mill, but in terms of a 2 L capacity, it is preferably 600 rpm or more and 4500 rpm or less, more preferably 800 rpm or more and 4000 rpm or less, and particularly preferably 1000 rpm or more and 3500 rpm or less. The peripheral speed of the tip of the stirring blade (agitator) depends on the span length of the stirring blade, but is preferably within the range that can be calculated from the above rotation speed assuming a diameter of 20 cm. Specifically, it is preferably 5 m / s to 40 m / s, more preferably 7 m / s to 30 m / s, and particularly preferably 9 m / s to 20 m / s.
[0106] The operation method of the bead mill for grinding and dispersing may be either a circulation type or a batch type, but the circulation type is preferred. In the case of the circulation type, the material is not transferred to a container as in the batch type, so that aggregation does not progress. When using a circulation system, the degree of pulverization varies depending on the number of passes. For example, when the residence time per pass is increased, the particle size distribution becomes sharper because there is no short pass of the processed material, but the aspect ratio of the carbon nanofibers also becomes smaller. Therefore, for example, when converted to 4L, the bead mill treatment is performed by circulation for preferably 70 minutes or more and 270 minutes or less, more preferably 80 minutes or more and 230 minutes or less, and particularly preferably 90 minutes or more and 180 minutes or less.
[0107] The temperature in the wet treatment is preferably from 0° C. to 50° C., particularly preferably from 5° C. to 35° C. The bead mill may be of either a vertical or horizontal type. In addition, a commercially available bead mill can be used, such as the Dyno Mill by Willy & Bachofen (WAB) and the Bead Mill by Netsch (USA).
[0108] The time per pass (continuous operation time), the number of passes, and the total time may depend on the equipment structure, slurry concentration, grinding and dispersion conditions, the type of surfactant, etc., so it is preferable to take out the material after each pass or during the wet grinding and observe it one by one with a particle size distribution measuring device, an optical microscope, a scanning electron microscope (SEM), etc., and adjust it appropriately.
[0109] By using the above-mentioned "production method using both dry and wet grinding" and appropriately adjusting the grinding conditions within the above-mentioned ranges, it is possible to obtain carbon nanofibers (group) having a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less.
[0110] Also, a carbon nanofiber group (1) is obtained in which the carbon nanofibers are in a state in which they can be isolated one by one, or in a state in which they are substantially dispersed one by one in a base material described below. Here, "a state in which they are substantially dispersed one by one" means "a state in which they are dispersed almost one by one" and refers to a state in which the carbon nanofibers are not in close contact with each other in parallel, and the base material is inserted between the carbon nanofibers.
[0111] Furthermore, by using the above-mentioned "production method using both dry and wet grinding" and appropriately adjusting the grinding conditions within the above-mentioned range, it is possible to obtain carbon nanofibers (group) having a number average aspect ratio of 3 or more and 200 or less.
[0112] <<Anti-aggregation treatment>> After the wet grinding, it is particularly preferable to carry out an anti-aggregation treatment, although this is not limited thereto. The anti-aggregation treatment is preferably carried out by blending an anti-aggregation agent such as a (composite) metal chelate compound, fine particles of a (composite) metal oxide, a wax containing a metal, or water containing a (composite) metal ion, or a surfactant, although this is not limited thereto. The aggregation prevention treatment may be carried out immediately after the above-mentioned wet pulverization, or after the water removal treatment described below, or may be carried out at both stages.
[0113] The anti-aggregation agent used in the anti-aggregation treatment is preferably a metal-containing anti-aggregation agent as described above, more preferably a (composite) metal chelate compound, and even more preferably a metal salt such as HEDTA, EDTA, PDTA, NTA, ethylenediamine, bipyridine, phenanthroline, or porphyrin. Among these, metal salts of acetic acid derivatives such as HEDTA (hydroxyethyl ethylene diamine triacetic acid), EDTA (ethylenediaminetetraacetic acid), PDTA (1,3-propanediamine tetraacetic acid), and NTA (nitrilo triacetic acid) are particularly preferred.
[0114] As the surfactant used in the anti-aggregation treatment, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant is preferably mentioned, and an anionic surfactant or an amphoteric surfactant is more preferably mentioned. Although not limited thereto, particularly preferred specific surfactants include those similar to those described in the above sections of <Wet treatment> and <Wet grinding>.
[0115] The types of anti-aggregation agents such as metal-containing anti-aggregation agents and surfactants are determined taking into consideration the surface condition of the object to be prevented from agglomeration immediately before the anti-aggregation treatment. When the types of the aggregation preventing agent and surfactant are as described above, aggregation is unlikely to occur during the process of removing the dispersion medium (water) and over time thereafter, and storage stability is improved.
[0116] The amount of the anti-aggregation agent such as a (composite) metal chelate compound to be used is not particularly limited, but is preferably added in an amount of 0.01% by mass or more and 1% by mass or less, and particularly preferably 0.03% by mass or more and 0.3% by mass or less, based on the total amount of the slurry after wet pulverization. It is also preferable to add 0.01 to 5 parts by mass, and particularly preferably 0.1 to 1 part by mass, per 100 parts by mass of the object to be prevented from agglomerating, such as carbon nanofiber groups.
[0117] In addition, the amount of surfactant used in the anti-aggregation treatment is not particularly limited, but when two or more types of surfactants are used in combination, the total amount is preferably 0 parts by mass or more and 10 parts by mass or less, more preferably 0 parts by mass or more and 5 parts by mass or less, and particularly preferably 0 parts by mass or more and 1 part by mass or less, per 100 parts by mass of the object to be prevented from aggregation.
[0118] When the amount of the anti-aggregating agent or surfactant used is within the above range, aggregation is unlikely to occur during the removal treatment step of the dispersion medium (water) and over time thereafter, and storage stability is improved.
[0119] The stirring during the aggregation prevention treatment is not particularly limited, but examples thereof include stirring with a hand mixer, etc. The stirring speed is not particularly limited, but is preferably 300 to 1200 rpm, and particularly preferably 500 to 1000 rpm. The temperature for the aggregation prevention treatment is not particularly limited, but is preferably from 20°C to 100°C, more preferably from 40°C to 90°C, and particularly preferably from 60°C to 80°C.
[0120] <<Water removal treatment>> (1) In order to obtain carbon nanofibers in powder form, a water removal process is carried out. However, the (1) carbon nanofibers dispersed in the base material may be carbon nanofibers contained in the slurry after wet milling, may be carbon nanofibers contained in the slurry after the above-mentioned anti-agglomeration treatment, or may be powdered carbon nanofibers after water is removed from the slurry. Regardless of whether the (1) carbon nanofibers are in any of the above states, they can be used in combination with (2a) flake graphite or (2b) approximately spherical carbon particles as an electrically conductive composition for various applications.
[0121] The method for the water removal treatment is not particularly limited, and can be performed by reducing pressure and / or increasing temperature. It is particularly preferable to semi-dry up the material by a cyclone separation and recovery method, and then remove (dry) water by reducing pressure and / or increasing temperature in an oven. The temperature for the water removal treatment is not particularly limited, but is preferably from 40°C to 160°C, and particularly preferably from 70°C to 130°C.
[0122] Furthermore, it is also preferable to perform baking at about 400° C. in order to remove the surfactant. The carbon nanofibers constituting the carbon nanofiber group produced by the production method of the present invention have good dispersibility themselves, so it is also preferable that no dispersant or surfactant is attached to the surface of the carbon nanofibers.
[0123] It is also preferable to carry out the above-mentioned anti-agglomeration treatment after the above-mentioned water removal treatment. That is, it is also preferable to mix the above-mentioned anti-agglomeration agent and surfactant into the concentrated slurry or powder after the above-mentioned water removal treatment.
[0124] The (1) carbon nanofiber group has a volume resistivity of 2×10 -3 It is preferable that the resistivity is less than 7×10 -4 It is more preferable that the resistivity is less than 4×10 -4 It is particularly preferable that the resistivity is Ω·cm or less. Here, the volume resistivity is measured in accordance with JIS R 7222, a method for measuring physical properties of graphite materials, and is defined as the volume resistivity measured in this manner.
[0125] According to the above-mentioned manufacturing method, it is possible to manufacture a material having the above-mentioned volume resistivity (electrical conductivity). The (1) carbon nanofiber group having the above volume resistivity, when used in combination with the (2a) flake graphite group or the (2b) substantially spherical carbon particle group described below, synergistically increases the electrical conductivity (particularly the volume electrical conductivity) and makes it easier to achieve the above-mentioned effects. In other words, the resistivity (particularly the volume resistivity) can be lowered, making it easier to achieve the above-mentioned effects.
[0126] The powdered (1) carbon nanofiber group produced by the above-mentioned production method, even if it is solidified, can be easily dispersed in the base material itself such as resin emulsion or resin, and can be diffused without agglomeration to obtain a conductive composition. Figure 7 shows an SEM photograph of the final (1) carbon nanofiber group. The resin may be a thermoplastic resin or a thermosetting resin, and in the case of a two-component thermosetting resin, it disperses well in both the base resin and the curing agent.
[0127] [(2a) Flake-like graphite group] The conductive composition of the present invention is characterized in that it contains the following carbonaceous material group (1) and (2a) or (2b) in a dispersed state in a base material. (1) Carbon nanofiber group (2a) Scaly graphite group as described below (2b) Nearly spherical carbon particles (described later)
[0128] Here, in the (2a) scaly graphite group, when the number average value of the maximum diameter length on the basal plane of the scaly graphite is D1 and the number average value of the minimum diameter length is D2, it is essential that both D1 and D2 are 1 μm or more and 300 μm or less, D1 / D2 is 3 or less, and when the number average thickness of the scaly graphite is d, the number average aspect ratio [(D1+D2) / 2] / d is 10 or more.
[0129] Here, the above-mentioned "minimum diameter length" refers to the minimum diameter length on the basal surface, provided that it passes through the midpoint of the line segment that gives the above-mentioned "maximum diameter length". Both D1 and D2 must be 1 μm or more and 300 μm or less, but D1 is preferably 2 μm or more and 300 μm or less, more preferably 3 μm or more and 100 μm or less, and particularly preferably 4 μm or more and 30 μm or less. Moreover, D2 is preferably 1 μm or more and 100 μm or less, more preferably 1.5 μm or more and 50 μm or less, and particularly preferably 2 μm or more and 30 μm or less.
[0130] D1 / D2 must be 3 or less, but is preferably 2 or less, more preferably 1.7 or less, and particularly preferably 1.4 or less.
[0131] There is no particular limitation on d as long as the number average aspect ratio [(D1+D2) / 2] / d satisfies the range described below, but d is preferably 3 nm or more and 1000 nm or less, more preferably 5 nm or more and 500 nm or less, and particularly preferably 7 nm or more and 300 nm or less.
[0132] The number average aspect ratio [(D1+D2) / 2] / d must be 10 or more, but is preferably 50 or more, more preferably 100 or more, further preferably 300 or more, and particularly preferably 700 or more.
[0133] If D1, D2, D1 / D2, d, and [(D1+D2) / 2] / d are within the above ranges, the combined use with the carbon nanofiber group (1) above can synergistically increase the electrical conductivity (particularly the volume electrical conductivity) and facilitate the above-mentioned effects. In other words, the resistivity (particularly the volume resistivity) can be lowered, and the above-mentioned effects can be facilitated. Specifically, within the above range, each carbon nanofiber in the carbon nanofiber group (1) mentioned above contacts the basal surface to ensure electrical conductivity, and when these carbon nanofibers overlap and connect together, they come into contact with each other overall and are electrically conductive, making it possible to synergistically increase electrical conductivity (reduce resistivity). The lower limit of d and the upper limit of [(D1+D2) / 2] / d are also limited by factors such as ease of production, availability, and stability.
[0134] Flake graphite may be natural or crushed natural flake graphite, synthetic, or naturally processed (semi-synthetic). The origin of natural graphite is not particularly limited, and may be China, India, Brazil, Ukraine, Japan, etc. Highly crystalline graphite is preferable, and graphite with large anisotropy in physical properties such as electrical conductivity in the directions parallel and perpendicular to the basal plane is preferable.
[0135] (2a) Examples of the flake graphite include natural graphite, artificial graphite, and graphene, and particularly preferred examples include artificial graphite and graphene. In addition, commercially available products can also be used as long as they meet the above requirements.
[0136] (2a) The flake graphite group has a volume resistivity of 1×10 -3 It is preferable that the resistivity is less than 5×10 -4 It is more preferable that the resistivity is less than 1.5×10 -4 It is particularly preferable that the volume resistivity of the flake graphite group (2a) is Ω·cm or less. The above "volume resistivity of the flake graphite group" is a value measured on the basal plane (AB plane). Here, the volume resistivity is measured according to the method described in the section "(1) Carbon nanofiber group" above, and is defined as the volume resistivity thus measured.
[0137] The flake graphite group (2a) having the above volume resistivity, when used in combination with the carbon nanofiber group (1), synergistically increases the electrical conductivity (particularly the volume electrical conductivity) and makes it easier to achieve the above-mentioned effects. In other words, the resistivity (particularly the volume resistivity) can be lowered, making it easier to achieve the above-mentioned effects.
[0138] [(2b) Nearly spherical carbon particles] The conductive composition of the present invention is characterized in that it contains the following carbonaceous material group (1) and (2a) or (2b) in a dispersed state in a base material. (1) Carbon nanofiber group The above-mentioned (2a) flake graphite group (2b) Nearly spherical carbon particles
[0139] Here, (2b) the substantially spherical carbon particle group must have an L1 / L2 ratio of 3 or less, where L1 is the number average maximum diameter of the substantially spherical carbon particles and L2 is the number average minimum diameter.
[0140] Here, the "minimum diameter" refers to the smallest diameter (diameter length) that passes through the midpoint of the line segment that gives the "maximum diameter" mentioned above.
[0141] L1 is more preferably from 5 nm to 200 nm, and particularly preferably from 10 nm to 100 nm. L2 is preferably 5 nm or more and 100 nm or less, more preferably 10 nm or more and 70 nm or less, and particularly preferably 20 nm or more and 50 nm or less.
[0142] L1 / L2 must be 3 or less, but is preferably 2 or less, more preferably 1.7 or less, and particularly preferably 1.4 or less.
[0143] If L1, L2, and L1 / L2 are within the above ranges, the combined use with the carbon nanofiber group (1) described above can synergistically increase the electrical conductivity (particularly the volume electrical conductivity) and facilitate the above-mentioned effects. In other words, the resistivity (particularly the volume resistivity) can be lowered, and the above-mentioned effects can be easily achieved. Specifically, within the above range, the carbon nanofibers in the carbon nanofiber group as described above (1) are in contact with each other via the approximately spherical carbon particles, and the carbon nanofibers in the carbon nanofiber group that are not in direct contact are connected to ensure conductivity, and the carbon nanofibers are connected in a series, thereby synergistically increasing the electrical conductivity (reducing the resistivity).
[0144] The roughly spherical carbon particles may be natural or synthetic, or may be natural particles that have been crushed and physically or chemically processed (semi-synthetic products) if necessary. Also, flake graphite may be physically or chemically spheroidized. In the case of naturally derived particles, there are no particular limitations on the place of origin, etc.
[0145] (2b) Examples of the roughly spherical carbon particles include furnace black, channel black, acetylene black, thermal black, and ketjen black, and particularly preferred are ketjen black and acetylene black. In addition, commercially available products can be used as long as they satisfy the above requirements. As commercially available products, those commercially available as (highly) conductive carbon black and the like are preferable, and specifically, for example, Ketjen Black and the like can be mentioned.
[0146] The (2b) substantially spherical carbon particles having the above volume resistivity, when used in combination with the (1) carbon nanofibers, synergistically increase the electrical conductivity (particularly the volume electrical conductivity) and facilitate the above-mentioned effects. In other words, the resistivity (particularly the volume resistivity) can be lowered, and the above-mentioned effects can be facilitated.
[0147] [Base material] In the conductive composition of the present invention, the base material is not particularly limited, and specific examples thereof include organic materials such as resins; and inorganic materials such as glass, ceramics, metals, and alloys; and the like. <Base resin> A particularly preferred base material is a resin, and the resin may be a thermoplastic resin or a thermosetting resin.
[0148] The thermoplastic resin is particularly preferably one or more thermoplastic resins selected from the group consisting of polyethylene, polypropylene, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl acetate, thermoplastic polyurethane, polytetrafluoroethylene, acrylonitrile butadiene styrene resin, acrylonitrile styrene resin, (meth)acrylic resin, polyamide, polyacetal, polycarbonate, (modified) polyphenylene ether, polyester, cyclic polyolefin, polyphenylene sulfide, polytetrafluoroethylene, polysulfone, polyether sulfone, polyarylate, polyether ether ketone, thermoplastic polyimide, and polyamide imide.
[0149] When the resin is in the form of a resin emulsion, the resin is not limited, but examples thereof include (meth)acrylic resins, styrene-maleic anhydride resins, and urethane resins, which have particularly good dispersibility of carbonaceous materials.
[0150] The carbon nanofiber(s) of the present invention is suitably dispersed in a thermoplastic resin and exhibits superior thermal, mechanical and electrical effects as described above, compared to other carbon nanofiber(s). In particular, when used in combination with (2a) flake graphite or (2b) roughly spherical carbon particles, it is possible to obtain an electrically conductive composition that exhibits synergistically high electrical conductivity.
[0151] The thermosetting resin is particularly preferably one or more thermosetting resins selected from the group consisting of phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, thermosetting polyurethanes, and thermosetting polyimides.
[0152] The (1) carbon nanofiber(s) of the present invention is suitably dispersed in the base material (containing unreacted resin having functional groups) of the thermosetting resin and / or the curing agent (which crosslinks, reacts, and polymerizes the functional groups) and exhibits superior thermal, mechanical, and electrical effects as described above compared to other carbon nanofiber(s).In particular, when used in combination with (2a) flake graphite or (2b) roughly spherical carbon particles, a conductive composition having high electrical conductivity can be obtained.
[0153] <Other ingredients> The conductive composition of the present invention, a molded body or coating film comprising "the conductive composition of the present invention," or a coating material for forming the conductive composition may contain "other components" as necessary within the range in which the effects of the present invention can be obtained.
[0154] Examples of the "other components" include colorants such as inorganic pigments and organic dyes; antioxidants; crystallization regulators such as nucleating agents; release agents such as wax; lubricants; antistatic agents; light stabilizers; ultraviolet absorbers; particles such as inorganic fillers and organic fillers; processing aids for each base material; flame retardants; plasticizers, etc. These "other components" may be used alone or in combination of two or more. The content thereof may be appropriately determined.
[0155] [Concentration of each carbonaceous material group in the conductive composition containing the base material and the mixing ratio of each carbonaceous material group] (1) Carbon nanofiber group, and (2a) scaly graphite group or (2b) approximately spherical carbon particle group are contained in a base material to form an electrically conductive composition, but the concentration of each carbonaceous material group relative to the entire electrically conductive composition is not particularly limited as long as the conductivity is increased synergistically. That is, it depends on whether the base material is an organic or inorganic material, and if the organic material is a resin, it also depends on the type of the resin. It also depends on whether the product containing the conductive composition is a molded body or a coating film, and on whether the important conductivity is volume conductivity (volume resistivity) or surface conductivity (surface resistance).
[0156] However, in any case, the following ranges are preferred. The total carbon content (total amount of carbonaceous materials) is preferably 6 mass% or more and 90 mass% or less, more preferably 10 mass% or more and 85 mass% or less, still more preferably 15 mass% or more and 65 mass% or less, and particularly preferably 20 mass% or more and 55 mass% or less, based on the entire conductive composition, the entire molded body, or the entire coating film.
[0157] (1) The carbon nanofiber group preferably accounts for 6 mass % or more and 90 mass % or less, more preferably 10 mass % or more and 85 mass % or less, and particularly preferably 14 mass % or more and 65 mass % or less, of the entire conductive composition, the entire molded body, or the entire coating film. When (2b) roughly spherical carbon particle groups are not used, (2a) flake graphite groups are preferably 5 mass% or more and 60 mass% or less, more preferably 10 mass% or more and 50 mass% or less, and particularly preferably 15 mass% or more and 40 mass% or less, of the entire conductive composition. When (2a) flake graphite groups are not used, (2b) approximately spherical carbon particle groups are preferably 3 mass% or more and 20 mass% or less, more preferably 4 mass% or more and 15 mass% or less, and particularly preferably 5 mass% or more and 10 mass% or less, of the entire conductive composition. When the (2a) flake graphite group and the (2b) approximately spherical carbon particle group are used together in combination with the (1) carbon nanofiber group, the total mass of the (2a) flake graphite group and the (2b) approximately spherical carbon particle group is preferably 3 mass% or more and 40 mass% or less, more preferably 4 mass% or more and 20 mass% or less, and particularly preferably 5 mass% or more and 15 mass% or less, of the entire conductive composition.
[0158] The mixing ratio of each carbonaceous material group is preferably as follows: That is, the (2a) flake graphite group or the (2b) approximately spherical carbon particle group is preferably contained in an amount of 3 mass % or more and 50 mass % or less, more preferably 5 mass % or more and 45 mass % or less, still more preferably 10 mass % or more and 40 mass % or less, and particularly preferably 15 mass % or more and 35 mass % or less, based on the entire (total carbon amount) of "(1) carbonaceous material group including carbon nanofiber group."
[0159] The conductive composition of the present invention is not particularly limited, but is preferably one produced without applying an external orientation treatment to the carbonaceous material contained therein, such as (1) carbon nanofibers. In the present invention, the volume resistivity can be reduced by mixing (to a minimum value) without applying an orientation treatment for the purpose of orientation. That is, (1) carbon nanofibers, (2a) flake graphite, and (2b) approximately spherical carbon particles may be naturally oriented and dispersed in the conductive composition of the present invention, or may be randomly dispersed. Carbonaceous materials may be oriented by coating, kneading, etc., without being subjected to an external treatment for the purpose of orientation, and such orientation is included as a preferred embodiment of the present invention.
[0160] [Increase in electrical conductivity of conductive compositions and the absolute value of electrical conductivity (volume resistivity) when used in combination] The conductive composition of the present invention is prepared by mixing and dispersing two or more types of carbonaceous materials (combined dispersion) in a base resin. The phrase "the conductivity is improved by the combined dispersion compared to the single dispersion" is defined as described in the "Effects of the Invention" above.
[0161] In a preferred embodiment of the present invention, the (1) carbon nanofiber group [A×r] mass % and "the (2a) scaly graphite group and / or the (2b) substantially spherical carbon particle group" "B×(1-r)" mass % (r is a real number greater than 0 and less than 1) are co-dispersed in the base material, with respect to the entire base material, (1) The electrical conductivity is made higher than that of a composition in which only the carbon nanofiber group is dispersed in an amount of A% by mass, and The conductive composition has a higher electrical conductivity than a composition in which only "the (2a) flake graphite group and / or the (2b) approximately spherical carbon particle group" are dispersed at B mass %.
[0162] The above "r" is preferably from 0.30 to 0.98, more preferably from 0.40 to 0.94, even more preferably from 0.50 to 0.90, and particularly preferably from 0.60 to 0.86. If the content falls within this range, the effect described in the "Effects of the Invention" above is easily achieved. Alternatively, if the content falls within this range, the "maximum value of electrical conductivity (minimum value of volume resistivity) due to mixing" described in the "Effects of the Invention" is achieved.
[0163] In addition to satisfying the above-mentioned "preferred embodiment", a composition that satisfies the above-mentioned concentrations of each carbonaceous material group in the "conductive composition containing a base material" and / or the mixing ratios of each carbonaceous material group is preferred.
[0164] Taking various physical properties into consideration, the volume resistivity of the conductive composition (solid) obtained by dispersing the optimal amount of "(1) carbon nanofibers and (2a) flake graphite or (2b) roughly spherical carbon particles" in a suitable base resin, which is an insulator, is 0.01 to 100 [Ω·cm]. By further optimization, it can be made 0.1 to 10 [Ω·cm], and by further optimization, it can be made 0.5 to 1 [Ω·cm].
[0165] The conductive composition of the present invention is most characterized by the (1) carbon nanofiber group contained therein. The unique properties of the (1) carbon nanofiber group synergistically increase the electrical conductivity of the "conductive composition having carbonaceous material mixed and dispersed therein." However, in terms of electrical conductivity alone, the (2a) flake graphite group or the (2b) roughly spherical carbon particle group may be higher than the (1) carbon nanofiber group.
[0166] [Paint for forming molded body, coating film, or conductive composition] The conductive composition of the present invention can be incorporated into a molded article or coating film, and the molded article or coating film also has synergistically improved electrical conductivity compared to when a carbonaceous material is used alone (contains the carbonaceous material). Furthermore, when a coating film is formed using a paint containing the conductive composition of the present invention and a liquid dispersion medium, the coating film has synergistically improved electrical conductivity compared to the coating film that uses (contains) a carbonaceous material alone.
[0167] The manufacturing method of the above molded body or coating film is not particularly limited, and examples thereof include injection molding, extrusion molding, blow (air) molding, vacuum molding, compressed air molding, roll molding, cast molding, compression molding, coating and drying of paint, impregnation into paint, etc. If necessary, the composition can be kneaded with a kneader, mixer, etc. before molding.
[0168] The method for producing the paint is not particularly limited, but the paint can be obtained by placing the conductive composition ((1) carbon nanofibers; (2a) flake graphite or (2b) approximately spherical carbon particles; base material; and "other components"), a liquid dispersion medium, and, if necessary, paint additives, etc., in a container and mixing, stirring, and dispersing them in the liquid dispersion medium with a stirrer or the like.
[0169] [Application] The conductive composition of the present invention can be suitably used as a molded body, coating film, or paint, and further, the conductive composition of the present invention can also be used in the form of a molded body called fiber reinforced plastics (FRP) by impregnating or penetrating the mesh of a woven or knitted cloth (sheet) made of carbon fiber, glass fiber, organic fiber, etc. In other words, the conductive composition of the present invention can also be suitably used as a matrix resin for fiber reinforced plastics (FRP).
[0170] Molded bodies, coating films, paints, fiber-reinforced plastics (FRP), and the like, which contain the conductive composition of the present invention, are suitably used in a variety of applications and fields, such as applications and fields requiring electrical conductivity; and various applications and fields requiring electromagnetic wave absorption due to high electrical conductivity.
[0171] [Operation / principle] In the present invention, the mechanism by which the combined use of carbonaceous materials synergistically increases the electrical conductivity (or synergistically decreases the volume resistivity) of the conductive composition (or its molded body or coating film) containing them is not particularly clear, but is thought to be as follows. That is, it is believed that the (1) carbon nanofiber group in the present invention has extremely good dispersibility despite its large aspect ratio, and therefore the carbon nanofibers are broken down into individual fibers in the base material, come into contact with the (basal surface of) flake graphite or the (surface of) approximately spherical carbon particles, and are then entangled to obtain conductivity. In other words, it is believed that the large aspect ratio and highly dispersible carbon nanofibers connect flake graphite particles and roughly spherical carbon particles that are not in direct contact with each other, ensuring electrical conductivity and linking them together, thereby synergistically increasing electrical conductivity (reducing resistivity). EXAMPLES
[0172] The present invention will be explained in more detail below by giving Production Examples, Examples and Comparative Examples, but the present invention is not limited to these as long as it does not depart from the gist of the present invention.
[0173] Manufacturing Example 1 [(1) Carbon fiber, the raw material for carbon nanofibers] <Dry grinding> "Chopped fibers of approximately 6 mm," which are random mesophase pitch-based carbon fibers that have not been subjected to sizing treatment, were dry-ground at 30°C for 10 minutes using a "shear and impact grinder with blades" as shown in Figure 9, so that 90% of the total particles were in the diameter 10 μm and length range of 10 μm to 40 μm.
[0174] <Wet processing> A slurry was obtained by mixing and stirring 100 parts by mass of dry-milled carbon fiber (e.g., FIG. 5(a)(b)) that had not been subjected to a heat treatment, 1 part by mass of a wetting agent (surfactant), and 1,500 parts by mass of purified water. Here, the wetting agent (surfactant) was an ammonium salt of a compound having an acid group.
[0175] The above slurry was subjected to a wetting treatment by stirring at 800 rpm with a hand mixer at 30° C. for 10 minutes.
[0176] <Wet grinding> Using a bead mill with a volume of 0.6 L, beads with a diameter of 0.3 mm, a bead filling rate of 60%, a vessel motor rotation speed of 1500 rpm, and a tubular circulation pump with a transfer rate of 500 mL per minute, 4 L of the slurry obtained above was circulated for 90 minutes or more.
[0177] <Anti-aggregation treatment> Only 3500 mL of the obtained slurry was transferred from the container of the bead mill to a separate container, and then 0.01% by mass of a coblock polymer was added as an anti-aggregation agent with respect to the entire slurry (3500 mL). After the addition, the mixture was stirred at room temperature (15 to 25° C.) at 800 rpm for 5 minutes using a hand mixer to carry out an anti-aggregation treatment.
[0178] <Water removal treatment> After applying heat and reducing pressure, the semi-dried material was collected using a cyclone separation and recovery method, and heated in an oven at 120°C for 240 minutes to remove the water, producing solid carbon nanofibers.
[0179] <Evaluation of the carbon nanofiber group obtained in Production Example 1> The obtained solid (1) carbon nanofiber group and the carbon nanofiber group in the dispersion liquid (slurry) before the water removal treatment were observed with an optical microscope and a scanning electron microscope and measured as described above. As a result, the obtained (1) carbon nanofiber group had a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less, with 90% by number of the total carbon nanofibers distributed within the above range.
[0180] The carbon nanofibers contained in the carbon nanofiber group (1) obtained as described above had a number average diameter of 700 nm, a number average length of 5 μm, and a number average aspect ratio of 7.
[0181] The obtained solid (1) carbon nanofiber group was added to an aqueous emulsion of acrylic resin, an aqueous emulsion of styrene-maleic anhydride resin, and an aqueous emulsion of polyurethane resin, and by stirring normally, the carbon nanofibers were suitably dispersed in water approximately one by one from the solid (1) carbon nanofiber group. The carbon nanofibers did not aggregate during dispersion, and did not aggregate over time.
[0182] In addition, when the obtained solid carbon nanofibers were dispersed in a matrix resin made of any general-purpose thermoplastic resin using a conventional kneader, the fibers were dispersed favorably in the matrix resin, approximately one by one.
[0183] Furthermore, when the obtained solid carbon nanofibers were dispersed in the curing agent of any general-purpose thermosetting resin using a conventional stirrer, the fibers were dispersed favorably in the curing agent approximately one by one. When the curing agent in which the carbon nanofibers were dispersed was mixed with a base resin containing either an epoxy resin or a urethane resin, the dispersion was maintained in either case without agglomeration, and the resin could be suitably used as a thermosetting resin.
[0184] Carbon nanofiber groups were prepared in the same manner as in Production Example 1, except that isotropic pitch-based carbon fiber, radial mesophase pitch-based carbon fiber, and onion mesophase pitch-based carbon fiber were used as raw materials instead of random mesophase pitch-based carbon fiber.
[0185] The ease of production of "carbon nanofibers having a diameter of 30 nm or more and 1000 nm or less, a length of 0.2 μm or more and 70 μm or less, and preferably a number average aspect ratio of 3 or more" was as follows. In addition, the higher (left) you go, the more superior the item is. The degree of superiority is also indicated by ">>", ">", and ">>". Random mesophase pitch carbon fiber >>Radial type mesophase pitch carbon fiber ≒ Onion-type mesophase pitch carbon fiber >>PAN-based carbon fiber
[0186] The order of superiority was also roughly the same for dispersibility, dispersion stability, high-concentration dispersibility, thermal properties, mechanical properties, and electrical properties. The order of superiority also seemed to be the same as above, with the order being ">>", ">", and ≒.
[0187] Manufacturing Example 2 (1) Carbon nanofiber group was obtained in the same manner as in Production Example 1, except that in Production Example 1, milled fibers having a diameter of 10 μm and a length of 70 μm were used as the raw material instead of the chopped fibers.
[0188] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm, a number average length of 5 μm, and a number average aspect ratio of 7.
[0189] Since there were many short fibers with lengths of approximately 1 μm, the number average aspect ratio tended to be small, but a good group of carbon nanofibers was obtained and the dispersibility and other aspects were also evaluated as good.
[0190] Production Example 3 Instead of the "6 mm chopped fiber" in Production Example 1, a long fiber bobbin type was used as the raw material.
[0191] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0192] Although pre-pulverization with a cutter mill was necessary, (1) carbon nanofiber groups were obtained satisfactorily in the same manner as in Production Example 1, and the dispersibility and other properties were also evaluated to be good.
[0193] Production Example 4 The same treatment as in Production Example 1 was carried out except that in the dry grinding step of Production Example 1, a full airflow type grinder that does not use impellers, blades, etc. (or does not use impellers, etc.), such as a jet mill, cyclone mill, tornado mill, or dream mill, was used instead of the "mill using shear and impact with blades."
[0194] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0195] (1) Carbon nanofibers were obtained satisfactorily, and the evaluation of dispersibility, etc. was also favorable. However, there was a tendency for the number average aspect ratio to become slightly smaller during the dry grinding stage, and even after the subsequent wet grinding, this tendency for the number average aspect ratio to become slightly smaller remained.
[0196] Production Example 5 In Production Example 1, a group of carbon nanofibers was obtained in the same manner as in Production Example 1, except that sized random mesophase pitch carbon fibers were used as the raw material instead of the random mesophase pitch carbon fibers that had not been sized, and that heat treatment was performed after dry grinding. The heat treatment was performed in an electric furnace at a temperature of 400° C. for 10 minutes.
[0197] The epoxy resin contained in the raw materials was reduced to 0.01% by mass or less. As a result, the surfactant (wetting agent) was effectively absorbed into the filaments (in the gaps between the filaments), resulting in the creation of carbon nanofibers with a large number-average aspect ratio.
[0198] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0199] Production Example 6 In Production Example 1, the wetting treatment was not carried out. Instead, the same wetting agent (surfactant) as that used in the wetting treatment in Production Example 1 was blended as a surfactant in the wet grinding. Other than that, the same procedure as in Production Example 1 was carried out to obtain carbon nanofiber groups.
[0200] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0201] Although the effect of the wetting agent (surfactant) was slightly less than in Production Example 1 and the number average aspect ratio tended to be smaller, good carbon nanofiber groups were obtained and the dispersibility and other properties were also evaluated as good.
[0202] Production Example 7 A plurality of types of carbon nanofiber groups were obtained in the same manner as in Production Example 6, except that a carbobetaine type, imidazoline type, amidobetaine type, amidosulfobetaine type, or amidoamine oxide type amphoteric surfactant was used instead of the surfactant used in Production Example 6 (the wetting agent (surfactant) used in the wetting treatment in Production Example 1). Those using amphoteric surfactants showed good high foaming properties in hard water and over a wide pH range. As the carbobetaine type amphoteric surfactant, Softazoline (manufactured by Kawaken FinChemical Co., Ltd.) was used.
[0203] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0204] As in Production Examples 1 and 6, carbon nanofibers were obtained satisfactorily, and the evaluation of dispersibility and the like was also favorable.
[0205] Production Example 8 Carbon nanofiber groups were obtained in the same manner as in Production Examples 1 and 5, except that the raw material in Production Example 5 was used and the aggregation prevention treatment in Production Example 1 was not carried out.
[0206] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0207] In all cases, (1) carbon nanofiber groups were obtained well, and the evaluation of dispersibility, etc. was also good. However, the obtained carbon nanofiber dispersion tended to aggregate slightly over time compared to the dispersion obtained in Production Example 1, but it was not at a level that was problematic.
[0208] Production Example 9 A carbon nanofiber dispersion was obtained without performing the water removal treatment in Production Example 1. The dispersion had excellent dispersibility and could be used for the next application as it was.
[0209] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0210] Manufacturing Example 10 In the aggregation prevention treatment of Production Example 1, highly condensed sodium naphthalenesulfonate, which is an anionic surfactant, was added in an amount of 5 mass% to the entire slurry (3500 mL) instead of the composite metal chelate used in Production Example 1. That is, 50 mass parts were added to 100 mass parts of the target. Carbon nanofiber groups were obtained in the same manner as Production Example 1 except for the above.
[0211] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0212] (1) Carbon nanofibers were obtained satisfactorily, and the evaluations of dispersibility and dispersion stability were also good.
[0213] Manufacturing Example 11 In Production Examples 1 and 10, the order of the anti-agglomeration treatment and the water removal treatment was reversed, and the target material that had been subjected to the water removal treatment to turn into a thick slurry or powder was mixed with the "surfactant that is an anionic surfactant" in Production Example 10 or the "composite metal chelate that is an anti-agglomeration agent" in Production Example 1. Carbon nanofiber groups were obtained in the same manner as in Production Examples 1 and 10, except that the order of the anti-agglomeration treatment and the water removal treatment was reversed, and the target material that had been subjected to the water removal treatment to turn into a thick slurry or powder was mixed with the "surfactant that is an anionic surfactant" in Production Example 10 or the "composite metal chelate that is an anti-agglomeration agent" in Production Example 1.
[0214] In the (1) carbon nanofiber group obtained as described above, 90% of the total carbon nanofibers were distributed in the range of "diameter 30 nm or more and 1000 nm or less, and length 0.2 μm or more and 70 μm or less." The carbon nanofibers contained therein had a number average diameter of 700 nm and a number average length of 5 μm.
[0215] (1) Carbon nanofibers were obtained satisfactorily, and the evaluations of dispersibility and dispersion stability were also good.
[0216] Manufacturing Example 12 In Production Example 1, an attempt was made to obtain carbon nanofibers by dry grinding alone, without wet grinding, but it was difficult to obtain a group of carbon nanofibers in which 50% or more of the total carbon nanofibers were distributed within the above ranges, with a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less. The carbon nanofibers contained therein had a number average diameter of 7000 nm and a number average length of 150 μm.
[0217] Manufacturing Example 13 In Production Example 1, an attempt was made to obtain carbon nanofibers by wet grinding only, without performing dry grinding, but the grinding did not progress well, and it was difficult to obtain a group of carbon nanofibers in which 50% or more of the total carbon nanofibers were distributed within the above range, with a diameter of 30 nm or more and 1000 nm or less and a length of 0.2 μm or more and 70 μm or less.
[0218] Example 1 <[(1)+(2a)] / Polyimide> A thermosetting polyimide varnish (U-Varnish-A (registered trademark) manufactured by Ube Industries, Ltd.) was prepared in an amount equivalent to 70 parts by mass in terms of polyimide. To the above amount of polyimide varnish (containing 70 parts by mass of polyimide), 30 parts by mass of the (1) carbon nanofiber group obtained in Production Example 2 was added as a solid, and NMP (N-methylpyrrolidone) was further added as a dispersion medium. The mixture was stirred at room temperature using a planetary stirrer to disperse the (1) carbon nanofiber group. The resultant is abbreviated as "CNF30%".
[0219] On the other hand, the above-mentioned polyimide varnish was prepared in an amount equivalent to 90 parts by mass in terms of polyimide. To the above amount of polyimide varnish (containing 90 parts by mass of polyimide), 10 parts by mass of the (2a) flake graphite group sold as "flake graphite" (SEM photographs are shown in Figures 15 and 16) was added as a solid and dispersed in the same manner. The result is abbreviated as "GRF10%."
[0220] In the "flake graphite" used here, when the number average value of the maximum diameter length on the basal surface was D1 and the number average value of the minimum diameter length was D2, both D1 and D2 were 10 μm, and D1 / D2 was 1. In other words, when the basal surface was viewed, there was no distortion (vertical or horizontal directionality) and it was a nearly perfect circle. In addition, when the number average thickness was d, d was 13 nm, and therefore the number average aspect ratio [(D1+D2) / 2] / d was 770.
[0221] The paint was prepared by gradually varying the mixture ratio of "CNF 30%" and "GRF 10%" from 0 parts by mass / 1 part by mass to 1 part by mass / 0 parts by mass, as shown on the horizontal axis of Figure 10(a) and (b). The obtained coating material was applied to a glass substrate using a bar coater so as to give a dry film thickness of 50 μm for measuring the volume resistivity, and then the coating film was formed by heating and drying at 200° C. The coating film is both the “conductive composition” and the “molded body” in the present invention.
[0222] The volume resistivity of the resulting coating film (conductive composition) was measured in accordance with JIS·K·7194 "Test method for resistivity of conductive plastics by four-probe method".
[0223] The results are shown in Table 1 and Figures 10(a) and (b). In this specification and drawings, the total mass% of the carbonaceous material contained in the entire coating film (conductive composition) may be referred to as "total carbon amount [mass%]". In Figures 10(a) and (b), "CNF30%" / "GRF10%" = 0 part by mass / 1 part by mass is shown at the left end of the horizontal axis, and "CNF30%" / "GRF10%" = 1 part by mass / 0 part by mass is shown at the right end of the horizontal axis.
[0224] [Table 1]
[0225] As can be seen from Table 1 and FIGS. 10(a) and 10(b), the volume resistivity of the coating film prepared by mixing “CNF30%” / “GRF10%” at 0.5 part by mass / 0.5 part by mass was lower than that of the coating film (left end) prepared by mixing “CNF30%” / “GRF10%” at 0 part by mass / 1 part by mass, and was also lower than that of the coating film (right end) prepared by mixing “CNF30%” / “GRF10%” at 1 part by mass / 0 part by mass. That is, by using the mixture (the combined use of two carbonaceous substances), the volume resistivity became lower than that of any of the single uses. In other words, there was a minimum value of the volume resistivity near the above-mentioned content ratio. In other words, there was a minimum value of the volume resistivity at the point where 0 < r < 1.
[0226] Example 2 <[(1)+(2b)] / Polyimide> Using the same (1) carbon nanofiber group as in Example 1, “CNF30%” was prepared in the same manner as in Example 1.
[0227] On the other hand, the same polyimide varnish as in Example 1 was prepared in an amount of 90 parts by mass as the polyimide. To the above amount of polyimide varnish (the amount containing 90 parts by mass of polyimide), 10 parts by mass of commercially available (2b) substantially spherical carbon particle groups as “Ketjen black” were added as a solid and dispersed with a disper and a roll mill. The obtained product was abbreviated as “KTJ10%”.
[0228] The above-mentioned “Ketjen black” used here was a substantially spherical carbon particle group with an average number value of the maximum diameter of L1 and an average number value of the minimum diameter of L2, both of which were 30 nm and L1 / L2 was 1.
[0229] “CNF30%” and “KTJ10%” were used to prepare a paint by gradually changing the mixing ratio shown in FIGS. 11(a) and 11(b) from 0 part by mass / 1 part by mass to 1 part by mass / 0 part by mass. The obtained coating material was applied to a substrate using a bar coater so as to have a dry film thickness of 50 μm for measuring the volume resistivity, and then dried to form a coating film. The coating film is also the "conductive composition" and the "molded body" in the present invention.
[0230] The volume resistivity of the obtained coating film (conductive composition) was measured in accordance with JIS K7194. The results are shown in Table 2 and FIGS. 11(a) and (b). In FIGS. 11(a) and (b), "CNF30%" / "KTJ10%" = 0 parts by mass / 1 part by mass is taken at the left end of the horizontal axis, and "CNF30%" / "KTJ10%" = 1 part by mass / 0 part by mass is taken at the right end of the horizontal axis.
[0231]
Table 2
[0232] As can be seen from Table 2 and FIGS. 11(a) and (b), the volume resistivity of the coating film prepared by mixing "CNF30%" / "KTJ10%" at 0.75 parts by mass / 0.25 parts by mass is smaller than the volume resistivity of the coating film (left end) prepared by mixing "CNF30%" / "KTJ10%" at 0 parts by mass / 1 part by mass, and is also smaller than the volume resistivity of the coating film (right end) prepared by mixing "CNF30%" / "KTJ10%" at 1 part by mass / 0 part by mass. That is, by using a mixture (using two kinds of carbonaceous materials in combination), the volume resistivity became lower than that of any single use. In other words, the minimum value of the volume resistivity existed at the point where 0 < r < 1.
[0233] Example 3 <[(1)+(2a)] / Polyimide> A conductive composition was prepared and a coating film for measuring the volume resistivity was formed in the same manner as in Examples 1 and 2, except that the "(1) carbon nanofiber group obtained in Production Example 2" used in Examples 1 and 2 was replaced with the "(1) carbon nanofiber group obtained in Production Examples 1, 3 to 11".
[0234] As in Examples 1 and 2, the mixing ratio of the carbonaceous material was varied and the volume resistivity was measured in the same manner as in Examples 1 and 2. The minimum value of the volume resistivity was found in the mixed portion. When the (1) carbon nanofiber group obtained in Production Examples 1, 3 to 11 was used, a significant reduction in volume resistivity (synergistic effect) was observed when used in combination with (2a) flake graphite or (2b) approximately spherical carbon particles, as in Examples 1 and 2 in which the (1) carbon nanofiber group obtained in Production Example 2 was used, in both combinations of (2a) and (2b).
[0235] Example 4 <[(1)+(2b)] / Polyester> A commercially available polyester-based varnish (FS-7733 (solid content: 28 mass%) manufactured by Arakawa Paint Co., Ltd.) was mixed with the total amount (total amount of carbonaceous material, total carbon amount) of "(1) carbon nanofiber group obtained in Production Example 2" used in Examples 1 and 2 and "(2b) roughly spherical carbon particle group sold as 'Ketjen black'" at a constant amount of 40 mass% relative to the total solid content of the coating film, and the ratio of (1) to (2b) was varied. In other words, 60 mass% of resin was mixed with 40 mass% of the total amount of carbonaceous material (total carbon amount).
[0236] (1) Carbon nanofiber groups were varied in amounts of 40.0 to 27.5 mass% relative to the total solid content of the coating film, and (2b) approximately spherical carbon particle groups were varied in amounts of 0 to 12.5 mass% relative to the total solid content of the coating film, and the paint was prepared by diluting with a solvent (toluene / butyl acetate = 7 / 3) to obtain an appropriate viscosity.
[0237] The "Ketjen Black" used here was a group of approximately spherical carbon particles with a number average maximum diameter L1 and a number average minimum diameter L2, both of which were 30 nm, and an L1 / L2 ratio of 1.
[0238] The coating material prepared as described above was applied to a dry film thickness of 30 μm in the same manner as in Examples 1 and 2, and the volume resistivity of the resulting coating film was measured in the same manner. The coating film is both the "conductive composition" and the "molded body" in the present invention. The measurement results are shown in Table 3 below and FIG.
[0239] [Table 3]
[0240] As can be seen from Table 3 and FIG. 12, even though the total carbon amount (total amount of carbonaceous material) is the same, there are points where the volume resistivity decreases (minimum point), demonstrating the synergistic effect of the two types of carbonaceous material.
[0241] The conductive composition (coating) is obtained by co-dispersing (1) carbon nanofiber(s) [40×r] mass % and (2b) approximately spherical carbon particle(s) “40×(1-r)” mass % (r is a real number greater than 0 and less than 1) in the base material relative to the entire conductive composition (coating in Example 4). That is, for the above A and B, A=B=40.
[0242] As is clear from Table 3 and Fig. 12, (1) for the carbon nanofiber (group), there is a minimum value near 40 x r = 35. Therefore, r = 35 / 40 = 0.88. On the other hand, although it is the same thing, as is clear from Table 3 and FIG. 12, (2b) the approximately spherical carbon particle (group) has a minimum value in the vicinity of 40×(1−r)=5. Therefore, 1-r=5 / 40, r=1-5 / 40=35 / 40=0.88.
[0243] The volume resistivity in the above-mentioned "r=0.88 blend (carbonaceous material content)" was lower (higher electrical conductivity) than (1) a blend in which only carbon nanofiber groups were dispersed at 40 mass%, and was also lower (higher electrical conductivity) than (2b) a blend in which only roughly spherical carbon particle groups were dispersed at 40 mass%.
[0244] Comparative Example 1 <[(1)+(2a') (Spherical) flake graphite group with number-average aspect ratio of 4] / Polyester> Instead of the (2a) flake graphite group, a paint was prepared using the (2a') (spherical) flake graphite group with a number-average aspect ratio [(D1+D2) / 2] / d of 4 (SEM photographs are shown in Figures 17 and 18).
[0245] A paint was prepared by mixing a commercially available polyester varnish (FS-7733, solid content 28 mass%, manufactured by Arakawa Paint Co., Ltd.) with the total amount (total amount of carbonaceous materials, total carbon amount) of "(1) Carbon nanofiber group obtained in Production Example 2 used in Examples 1 and 2" and "(2a') (spherical) flake graphite (highly purified natural graphite from Mozambique, D50 = 9 μm, manufactured by NSC Corporation)" at a constant 40 mass% relative to the entire solid content of the coating film, with the "(1) Carbon nanofiber group" varying from 40 to 30 mass% relative to the entire solid content of the coating film and the "(2a') (spherical) flake graphite" varying from 0 to 10 mass% relative to the entire solid content of the coating film, and diluting with a solvent (toluene / butyl acetate = 7 / 3) to obtain an appropriate viscosity.
[0246] The coating material prepared as described above was applied in the same manner as in Examples 1 and 2 so as to give a dry film thickness of 30 μm, and the volume resistivity of the resulting coating film was measured in the same manner. The measurement results are shown in Table 4 below and in FIG.
[0247] [Table 4]
[0248] As shown in Table 4 and FIG. 13, unlike Example 4, (1) the volume resistivity of the coating film containing only carbon nanofiber groups was the lowest, and there was no point where the volume resistivity decreased (minimum point) due to mixing, and no synergistic effect of the two types of carbonaceous materials was observed.
[0249] Example 5, Comparative Example 2 <[(1)+(2b)] / Polyester> A commercially available polyester-based varnish (FS-7733 manufactured by Arakawa Paint Co., Ltd., solid content 28 mass %) was mixed with the "(1) carbon nanofiber group obtained in Production Example 2" used in Examples 1 and 2 in the content [mass %] shown in "Example 5" in Table 5, and 5.0 mass % of "(2b) roughly spherical carbon particle group" sold as "Ketjen black". In addition, as shown in "Example 5" in Table 5, 27.5% by mass to 32.5% by mass of (1) carbon nanofiber group was blended and diluted with a solvent (toluene / butyl acetate = 7 / 3) to obtain an appropriate viscosity to prepare a paint.
[0250] The coating material was applied in the same manner as in Examples 1 and 2 so as to give a dry film thickness of 30 μm, and the volume resistivity of the resulting coating film was measured in the same manner.
[0251] As Comparative Example 2, in the above Example 5, (1) only the carbon nanofiber group was blended so that the total carbon amount (amount of carbonaceous matter) in the coating film was 30 mass% to 50 mass%, and a paint was prepared by diluting with a solvent (toluene / butyl acetate = 7 / 3) to obtain an appropriate viscosity (see Table 5).
[0252] The coating material was applied in the same manner as in Examples 1 and 2 so as to give a dry film thickness of 30 μm, and the volume resistivity of the resulting coating film was measured in the same manner.
[0253] As a result, the coating film in which (2b) approximately spherical carbon particles were added to (1) carbon nanofibers at a concentration of 5 mass% (Example 5) had a lower volume resistivity than the coating film in which (1) carbon nanofibers were used alone (Comparative Example 2) when compared at the same total carbon amount (see FIG. 14).
[0254] [Table 5]
[0255] Example 6 An electrically conductive composition was prepared in the same manner as in Example 2, except that the base material in Example 2 was changed to a thermoplastic resin, polycarbonate (manufactured by Mitsubishi Engineering Plastics Corporation, Iupilon (registered trademark)), and a coating film for measuring volume resistivity was formed.
[0256] When evaluated in the same manner as in Example 2, the minimum volume resistivity was found in the mixture of the two types of carbonaceous materials.
[0257] Example 7 In Example 2, the base material was replaced with a thermosetting epoxy resin for evaluation. That is, the base material was made by mixing an epoxy resin base agent (jER828 (registered trademark) manufactured by Mitsubishi Chemical Corporation) and a dedicated epoxy resin hardener (jER Cure ST14 (registered trademark) manufactured by the same company) in the ratio specified in the instructions. Except for the above, an electrically conductive composition was prepared in the same manner as in Example 2, and a coating film for measuring the volume resistivity was formed.
[0258] When evaluated in the same manner as in Example 2, the minimum volume resistivity was found in the mixture of the two types of carbonaceous materials. [Industrial Applicability]
[0259] The conductive composition of the present invention contains (1) carbon nanofibers that have excellent shape, size, distribution, etc., and a surface state with good dispersibility. In addition, the carbon nanofibers are a collection of individual carbon nanofibers and have good dispersibility in base materials and dispersion media, so that the composition can be widely used in various fields requiring various performances, such as electrically conductive objects and electromagnetic wave absorption, in the form of dispersions, molded bodies, coating films, paints, films, paints, layers (membranes), circuits, powders, etc. [Explanation of symbols]
[0260] 10... Filament 20 Plain filament
Claims
1. 1. An electrically conductive composition comprising the following carbonaceous material group (1) and (2a) or (2b) dispersed in a base material: (1) A group of carbon nanofibers obtained by pulverizing carbon fibers, in which 50% or more of the total number of carbon nanofibers are distributed in the range of "diameter 30 nm or more and 1000 nm or less and length 0.2 μm or more and 70 μm or less." (2a) A group of flake graphite particles in which, when the number average value of the maximum diameter length of the basal plane of the flake graphite is D1 and the number average value of the minimum diameter length is D2, both D1 and D2 are 1 μm or more and 300 μm or less, D1 / D2 is 3 or less, and when the number average thickness of the flake graphite is d, the number average aspect ratio [(D1+D2) / 2] / d is 10 or more. (2b) A group of approximately spherical carbon particles in which L1 / L2 is 3 or less, where L1 is the number average value of the maximum diameter of the approximately spherical carbon particles and L2 is the number average value of the minimum diameter of the approximately spherical carbon particles.
2. By co-dispersing the (1) carbon nanofiber group [A×r] mass % and “the (2a) scaly graphite group and / or the (2b) substantially spherical carbon particle group” “B×(1−r)” mass % (r is a real number greater than 0 and less than 1) in the base material with respect to the entire conductive composition, (1) The electrical conductivity is higher than that of a composition in which only carbon nanofiber groups are dispersed in an amount of A mass %, and 2. The conductive composition according to claim 1, which has a higher electrical conductivity than a composition in which only "the (2a) flake graphite group and / or the (2b) approximately spherical carbon particle group" are dispersed in an amount of B mass %.
3. 3. The electrically conductive composition according to claim 1, wherein the number-average aspect ratio of the carbon nanofibers contained in the carbon nanofiber group (1) is 3 or more and 200 or less.
4. The conductive composition according to any one of claims 1 to 3, wherein the number average diameter of the carbon nanofibers contained in the (1) carbon nanofiber group is 30 nm or more and 1000 nm or less, and the number average length is 0.2 μm or more and 70 μm or less.
5. The conductive composition according to any one of claims 1 to 4, wherein the (1) carbon nanofiber group is obtained by dry-pulverizing carbon fibers until the number average length is 100 μm or less, and then wet-pulverizing the carbon fibers.
6. 6. The conductive composition according to claim 1, wherein the carbon nanofiber groups (1) are dispersed substantially individually in the base material.
7. The conductive composition according to any one of claims 1 to 6, wherein the (1) carbon nanofiber group is obtained by dry-pulverizing pitch-based carbon fibers and then wet-pulverizing them.
8. The conductive composition according to claim 7, wherein the number average thickness or number average diameter of the elementary filaments constituting "the filaments possessed by the pitch-based carbon fiber that is the raw material for the (1) carbon nanofiber group" is 10 nm or more and 200 nm or less.
9. 9. The conductive composition according to claim 7 or 8, wherein the carbon nanofibers of the carbon nanofiber group are constituted by an aggregation of 2 to 20 individual filaments constituting "the filaments possessed by the pitch-based carbon fiber that is the raw material for the (1) carbon nanofiber group."
10. 10. The electrically conductive composition according to claim 7, wherein the pitch-based carbon fiber, which is a raw material for the carbon nanofiber group (1), is a mesophase pitch-based carbon fiber.
11. 11. The conductive composition according to claim 10, wherein the mesophase pitch-based carbon fiber is a random mesophase pitch-based carbon fiber.
12. The conductive composition according to any one of claims 1 to 11, wherein the (1) carbon nanofiber group is substantially free of mixed resins present in the raw material carbon fibers before pulverization.
13. The conductive composition according to any one of claims 1 to 12, wherein the (1) carbon nanofiber group is obtained by dry pulverization followed by wet pulverization, and a heat treatment is performed between the dry pulverization and the wet pulverization to remove any resin mixed in the raw material.
14. The conductive composition according to any one of claims 1 to 13, wherein the (1) carbon nanofiber group is obtained by dry pulverization followed by wet pulverization, and the wet pulverization is bead mill pulverization or ball mill pulverization carried out in an aqueous medium in the presence of a surfactant.
15. (1) The carbon nanofiber group has a volume resistivity of 7×10 -4 15. The conductive composition according to claim 1, which has a resistivity of Ω·cm or less.
16. 16. The electrically conductive composition according to claim 1, wherein the number average thickness d of the flake graphite groups (2a) is 3 nm or more and 1000 nm or less.
17. 17. The electrically conductive composition according to claim 1, wherein the (2a) flake graphite group or the (2b) substantially spherical carbon particle group is contained in an amount of 5% by mass or more and 70% by mass or less with respect to the entire carbonaceous material group.
18. 18. The electrically conductive composition according to claim 1, wherein the (2a) flake graphite group or the (2b) substantially spherical carbon particle group is contained in an amount of 10% by mass or more and 50% by mass or less with respect to the entire carbonaceous material group.
19. 19. The conductive composition according to claim 1, wherein the base material is one or more thermoplastic resins selected from the group consisting of polyethylene, polypropylene, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl acetate, thermoplastic polyurethane, polytetrafluoroethylene, acrylonitrile butadiene styrene resin, acrylonitrile styrene resin, (meth)acrylic resin, polyamide, polyacetal, polycarbonate, (modified) polyphenylene ether, polyester, cyclic polyolefin, polyphenylene sulfide, polytetrafluoroethylene, polysulfone, polyethersulfone, polyarylate, polyetheretherketone, thermoplastic polyimide, and polyamideimide; or one or more thermosetting resins selected from the group consisting of phenolic resin, epoxy resin, melamine resin, urea resin, unsaturated polyester resin, alkyd resin, thermosetting polyurethane, and thermosetting polyimide.
20. A molded body comprising the conductive composition according to any one of claims 1 to 19.
21. A coating film comprising the conductive composition according to any one of claims 1 to 19.
22. A paint comprising the electrically conductive composition according to any one of claims 1 to 19 and a liquid dispersion medium.
Citation Information
Patent Citations
Electroconductive resin film
JP2010018685A
Ultrafine carbon fiber and method for manufacturing the same
JP2012188790A
Carbon material for nonaqueous secondary battery negative electrode, negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery
JP2014165018A
Resin composition for sliding member
JP2015067726A
Si / C electroactive material composition
JP2015510666A