Polyethylene laminate and packaging material using same

A polyethylene laminate with a base layer and heat seal layer of varying densities, enhanced by electron beam irradiation, addresses heat resistance and recyclability issues, providing improved heat sealability and recyclability in packaging materials.

JP7591199B2Active Publication Date: 2024-11-28DAI NIPPON PRINTING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023104311
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-11-28
Estimated Expiration
2038-09-28

AI Technical Summary

Technical Problem

Polyethylene films used in packaging materials lack sufficient heat resistance and recyclability due to their composition and processing limitations, making them unsuitable for recycling and prone to deformation or melting during heat processing.

Method used

A polyethylene laminate is created with a base layer and a heat seal layer of different densities, where the base layer is electron beam irradiated to enhance heat resistance, and an optional intermediate layer is included to improve stiffness and shape stability, all made from recyclable polyethylene materials.

Benefits of technology

The laminate achieves high heat resistance while maintaining heat sealability and excellent recyclability, addressing the limitations of conventional polyethylene films by enhancing processing suitability and reducing shrinkage during heat sealing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591199000002
    Figure 0007591199000002
  • Figure 0007591199000003
    Figure 0007591199000003
  • Figure 0007591199000004
    Figure 0007591199000004
Patent Text Reader

Abstract

To provide a polyethylene laminate that has high heat resistance and also has excellent recyclability while keeping heat sealability.SOLUTION: A polyethylene laminate has a base material layer and a heat seal layer. The base material layer comprises polyethylene with a density of 0.930 g / cm3 or more and the heat seal layer comprises polyethylene with a density of less than 0.930 g / cm3. Each of the base material layer and the heat seal layer is formed by co-extrusion molding of the polyethylene with a density of 0.930 g / cm3 or more and the polyethylene with a density of less than 0.930 g / cm3. The base material layer is treated with electron beam irradiation.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene laminate, and more specifically to a polyethylene laminate made of a single material, which comprises a polyethylene base layer to which heat resistance has been imparted and a polyethylene layer having heat sealability, and a packaging material using the same. [Background technology]

[0002] Films made of polyethylene have moderate flexibility, excellent transparency, moisture resistance, chemical resistance, etc., and are inexpensive, and therefore are used in various packaging materials. In particular, polyethylene has a melting point that varies somewhat depending on the type, but is generally around 100 to 140°C, and therefore is generally used as a sealant film in the packaging material field.

[0003] On the other hand, since polyethylene has poor heat resistance as described above, if it is used as a packaging material, it will deform or in some cases melt during heat sheet processing, so a laminate obtained by laminating a base film having excellent heat resistance, such as a polyester film or a nylon film, with a polyethylene film is generally used as a packaging material. For example, a bag is made by laminating a base material such as a polyester film with a polyethylene film, and heat sealing the laminate so that the polyethylene film side is on the inside of the packaging bag (for example, Patent Document 1, etc.).

[0004] In recent years, along with the growing demand for the creation of a recycling-oriented society, attempts have been made to recycle and reuse packaging materials. However, there is a problem that the above-mentioned laminates in which different types of resin films are bonded together are difficult to separate by type of resin, making them unsuitable for recycling.

[0005] In response to the above problems, the applicant conducted studies to realize a packaging material consisting of a single polyethylene film without using a base film having excellent heat resistance, such as a polyester film, and as a result proposed that a packaging material consisting of a polyethylene film can be realized by imparting heat resistance to one side of the polyethylene film that has conventionally been used as a heat seal layer by irradiating one side of the polyethylene film with electrons (Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-104525 A [Patent Document 2] JP 2017-031233 A Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, the polyethylene film proposed in Patent Document 2 has one side that is rendered heat-resistant by electron beam irradiation and therefore functions as a substrate, and the other side has heat-sealing properties, so that the film has both heat resistance and heat-sealing properties despite being a single film, and can be suitably used as a packaging material, and furthermore, is excellent in recyclability as it is composed of a single polyethylene material. However, the present inventors conducted further studies and found that the surface of the polyethylene film that was irradiated with electron beams (i.e., the surface that was rendered heat-resistant) may shrink when heat-sealing processing is performed during bag making, and that there is room for further improvement in heat resistance.

[0008] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a polyethylene laminate which has high heat resistance while maintaining heat sealability, and which also has excellent recyclability. Another object of the present invention is to provide a packaging material using the polyethylene laminate. [Means for solving the problem]

[0009] The present inventors have found that by forming a polyethylene laminate using two types of polyethylene having different densities on the side to be irradiated with an electron beam and the side not to be irradiated with an electron beam, it is possible to significantly improve heat resistance while maintaining recyclability. The present invention is based on this finding.

[0010] The polyethylene laminate according to the present invention comprises: A polyethylene laminate having a base layer and a heat seal layer, The base layer has a density of 0.930 g / cm 3 The polyethylene comprises The heat seal layer has a density of 0.930 g / cm 3 less than 1000 mm of polyethylene, The base layer and the heat seal layer have a density of 0.930 g / cm 3 Polyethylene with density of 0.930g / cm 3 and is formed by co-extrusion with polyethylene of less than The substrate layer is characterized in that it has been subjected to an electron beam irradiation treatment.

[0011] The polyethylene laminate according to the present invention may further comprise an intermediate layer between the base layer and the heat seal layer.

[0012] In addition, in the polyethylene laminate according to the present invention, The intermediate layer has a density of 0.942 g / cm 3 The polyethylene comprises The base layer, the intermediate layer and the heat seal layer have a density of 0.930 g / cm 3 Polyethylene with a density of 0.942g / cm 3 Polyethylene with a density of 0.930g / cm 3 The polymer may be formed by co-extrusion with polyethylene of less than 100 mm.

[0013] The polyethylene laminate according to the present invention may further comprise a printed layer on the surface of the base layer.

[0014] The polyethylene laminate according to the present invention may further comprise a barrier layer on the surface of the base layer.

[0015] A packaging material according to another embodiment of the present invention is made of a polyethylene laminate. Effect of the Invention

[0016] According to the present invention, in a laminate having a base layer and a heat seal layer, the base layer is made of a material having a density of 0.930 g / cm 3 The heat seal layer is made of the above polyethylene and has a density of 0.930 g / cm 3 The heat resistance of the base layer can be further improved by subjecting the base layer side of the laminate of the co-extruded base layer and heat seal layer to electron beam irradiation treatment. As a result, a polyethylene laminate that has high heat resistance and excellent recyclability while maintaining heat sealability can be realized. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional schematic diagram of a polyethylene laminate according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional schematic diagram of a polyethylene laminate according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a perspective view showing one embodiment of a packaging material made using the polyethylene laminate of the present invention. [Figure 4] FIG. 1 is a perspective view showing one embodiment of a packaging material made using the polyethylene laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Polyethylene laminate] The polyethylene laminate according to the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view of a polyethylene laminate 10 according to one embodiment of the present invention. The polyethylene laminate 10 according to the first embodiment includes a base layer 1 and a heat seal layer 2. As described later, the polyethylene laminate of the present invention can be suitably used as a packaging material, and when the polyethylene laminate is used to make a packaging material, the base layer 1 side is used to be located on the outer surface of the packaging material, and the heat seal layer 2 is used to be located on the inner surface of the packaging material. The polyethylene laminate 10 according to another embodiment of the present invention may include an intermediate layer 3 between the base layer 1 and the heat seal layer 2. As described later, by including the intermediate layer 3, it is possible to further impart stiffness and strength to the polyethylene laminate. In addition to the above-mentioned layers, the polyethylene laminate of the present invention may also include a print layer or a barrier layer (not shown) as appropriate so as to be suitable for various uses of the packaging material. Each layer constituting the polyethylene laminate of the present invention will be described below.

[0019] <Base material layer> In the present invention, the base layer has a density of 0.930 g / cm 3 The applicant, as mentioned above, in Patent Document 2, has disclosed a polyethylene having a density of 0.91 g / cm 3 We proposed that a single polyethylene film with a density of 0.91 g / cm can be used as a packaging material by irradiating one side of the film with an electron beam to improve the heat resistance of the irradiated side and maintaining the heat sealability of the other side, which is not irradiated with an electron beam. 3 It is believed that by irradiating the following polyethylene with an electron beam, the polyethylene on the surface irradiated with the electron beam is partially crosslinked, improving the heat resistance. However, the density is 0.91 g / cm 3The following polyethylenes are inferior in processability such as stickiness, and the processability is not improved even by electron beam irradiation. In addition, the crosslink density of the polyethylene differs between the surface irradiated with electron beam and the surface not irradiated with electron beam, and wrinkles may occur in the film due to the difference in the thermal shrinkage rate between the front and back surfaces of the film. In the present invention, as described above, a polyethylene having a density of 0.930 g / cm is used as the base layer disposed on the surface to be irradiated with electron beam. 3 The heat seal layer is made of polyethylene with a density of 0.930g / cm 3 By using less than 100% polyethylene, the heat resistance of the base layer (i.e., the occurrence of stickiness and wrinkles) has been improved, and a polyethylene laminate with excellent recyclability has been achieved while maintaining heat sealability.

[0020] Density 0.930g / cm 3 As the above polyethylene, medium density polyethylene (MDPE) or high density polyethylene (HDPE) can be suitably used. Note that medium density polyethylene is 0.930 g / cm 3 More than 0.942g / cm 3 High density polyethylene refers to polyethylene having a density of less than 0.942 g / cm 3 The density of the polyethylene constituting the base layer is 0.930 g / cm or more. 3 More than 0.950g / cm 3 It is preferable that the content is 0.935 g / cm or less, and more preferable that the content is 0.935 g / cm or less. 3 More than 0.945g / cm 3 The density of polyethylene having such a density can be prepared by mixing the above-mentioned medium-density polyethylene and high-density polyethylene in an appropriate ratio. In addition, the polyethylene is not limited to medium-density polyethylene and high-density polyethylene, and may be prepared by mixing high-density polyethylene with low-density polyethylene (LDPE) or linear low-density polyethylene (LLDPE) in an appropriate ratio so as to fall within the above-mentioned density range. The low-density polyethylene has a density of 0.930 g / cm or less. 3 Polyethylene having a density less than 1000 MPa.

[0021] The polyethylenes having different densities and branches as described above can be obtained by appropriately selecting a polymerization method. For example, it is preferable to use a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst as a polymerization catalyst and carry out the polymerization in one stage or in two or more stages by any of gas phase polymerization, slurry polymerization, solution polymerization, and high pressure ion polymerization.

[0022] The single-site catalyst is a catalyst capable of forming a uniform active species, and is usually prepared by contacting a metallocene transition metal compound or a nonmetallocene transition metal compound with an activating cocatalyst. Compared with a multi-site catalyst, a single-site catalyst is preferred because it has a uniform active site structure and can polymerize a polymer with a high molecular weight and a highly uniform structure. As the single-site catalyst, it is particularly preferred to use a metallocene catalyst. The metallocene catalyst is a catalyst containing each catalyst component of a transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, a cocatalyst, and if necessary, an organometallic compound and a carrier.

[0023] In the above-mentioned transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, the cyclopentadienyl skeleton is a cyclopentadienyl group, a substituted cyclopentadienyl group, etc. The substituted cyclopentadienyl group has at least one substituent selected from a hydrocarbon group having 1 to 30 carbon atoms, a silyl group, a silyl-substituted alkyl group, a silyl-substituted aryl group, a cyano group, a cyanoalkyl group, a cyanoaryl group, a halogen group, a haloalkyl group, a halosilyl group, etc. The substituted cyclopentadienyl group may have two or more substituents, and the substituents may be bonded to each other to form a ring, such as an indenyl ring, a fluorenyl ring, an azulenyl ring, or a hydrogenated product thereof. The rings formed by bonding the substituents to each other may further have substituents.

[0024] In the transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, the transition metal may be zirconium, titanium, hafnium, etc., and zirconium and hafnium are particularly preferred. The transition metal compound usually has two ligands having a cyclopentadienyl skeleton, and each ligand having a cyclopentadienyl skeleton is preferably bonded to each other by a bridging group. The bridging group may be an alkylene group having 1 to 4 carbon atoms, a silylene group, a substituted silylene group such as a dialkylsilylene group or a diarylsilylene group, or a substituted germylene group such as a dialkylgermylene group or a diarylgermylene group. The substituted silylene group is preferred. The above-mentioned transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton may be used as a catalyst component, either alone or in a mixture of two or more kinds.

[0025] The co-catalyst refers to a catalyst that can effectively use the above-mentioned transition metal compound of Group IV of the periodic table as a polymerization catalyst or balance the ionic charge in a catalytically activated state. Examples of the co-catalyst include benzene-soluble aluminoxanes of organoaluminum oxy compounds and benzene-insoluble organoaluminum oxy compounds, ion-exchangeable layered silicates, boron compounds, ionic compounds consisting of cations containing or not containing active hydrogen groups and non-coordinating anions, lanthanoid salts such as lanthanum oxide, tin oxide, and phenoxy compounds containing fluoro groups.

[0026] The transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton may be used by being supported on an inorganic or organic carrier. The carrier is preferably an inorganic or organic porous oxide, and specifically includes ion-exchangeable layered silicates such as montmorillonite, SiO2, Al2O3, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or mixtures thereof. Furthermore, examples of organometallic compounds that may be used as needed include organoaluminum compounds, organomagnesium compounds, and organozinc compounds. Of these, organoaluminum compounds are preferably used.

[0027] Copolymers of ethylene and other monomers can also be used. Examples of ethylene copolymers include copolymers of ethylene and α-olefins having 3 to 20 carbon atoms, and examples of α-olefins having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Copolymers with vinyl acetate, acrylic esters, and the like may also be used as long as they do not impair the object of the present invention.

[0028] In addition, in the present invention, polyethylene made from biomass-derived ethylene as a raw material may be used instead of ethylene obtained from fossil fuels. Since such biomass-derived polyethylene is a carbon-neutral material, it can be used as a packaging material with even less environmental impact. Such biomass-derived polyethylene can be produced, for example, by a method such as that described in JP 2013-177531 A. In addition, commercially available biomass-derived polyethylene (for example, Green PE commercially available from Braskem) may be used.

[0029] The substrate layer may contain a light stabilizer. As described later, in the polyethylene laminate of the present invention, the polyethylene of the substrate layer is treated by electron beam irradiation, and therefore, by containing a light stabilizer in the substrate layer, the deterioration of the polyethylene constituting the substrate layer over time can be prevented. When the polyethylene is subjected to electron beam irradiation treatment, the carbon-hydrogen bond in the polyethylene is broken, and radicals are generated at the broken bond ends. The generated radicals come into contact with other polyethylene molecular chains due to the molecular motion of the molecular chains, and remove hydrogen atoms to bond with carbon atoms in the polyethylene molecular chains. As a result, a crosslinked structure is formed in the polyethylene, but the molecular chains are gradually broken by the remaining radicals, which is thought to lead to the deterioration of the polyethylene. The light stabilizer has the function of trapping these remaining radicals.

[0030] Examples of the light stabilizer include antioxidants such as phenol-based antioxidants, amine-based antioxidants, phosphoric acid-based antioxidants, sulfur-based antioxidants, hindered amine-based antioxidants, and hydroxylamine-based antioxidants, as well as ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, and benzophenone-based ultraviolet absorbers.

[0031] It is preferable to use an antioxidant since it is unlikely to inhibit the crosslinking reaction carried out by irradiating the polyethylene film substrate with an electron beam.

[0032] As the antioxidant, it is preferable to use a primary antioxidant that captures generated radicals in combination with a secondary antioxidant that decomposes hydroperoxides generated from the radicals, and it is also possible to use an antioxidant that has both the functions of a primary antioxidant and a secondary antioxidant.

[0033] Examples of primary antioxidants include phenol-based antioxidants, amine-based antioxidants, and hindered amine-based antioxidants. Examples of secondary antioxidants include phosphorus-based antioxidants and sulfur-based antioxidants. Examples of antioxidants having both the functions of a primary antioxidant and a secondary antioxidant include hydroxylamine-based antioxidants.

[0034] Moreover, hydroxylamine-based antioxidants and phosphorus-based antioxidants are preferred because they can prevent discoloration of the polyethylene film substrate.

[0035] The content of the light stabilizer in the substrate layer is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.1% by mass or more and 10% by mass or less, and even more preferably 0.1% by mass or more and 8% by mass or less.

[0036] The substrate layer may also contain a crosslinking agent. As described below, the substrate layer is subjected to electron beam irradiation treatment, and by containing a crosslinking agent, the degree of crosslinking of the polyethylene can be further improved. As a result, the heat resistance of the substrate layer constituting the polyethylene laminate can be further improved.

[0037] Examples of the crosslinking agent include styrene-based elastomers such as styrene-polyisoprene elastomer, styrene-polybutadiene elastomer, and styrene-polyisoprene-butadiene random copolymer; ethylene-acrylate copolymers such as ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer; and ethylene-acrylic acid ester-glycidyl methacrylate.

[0038] The content of the crosslinking agent in the base layer is preferably 1% by mass or more and 49% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 35% by mass or less.

[0039] The base layer may contain additives within the range that does not impair the characteristics of the present invention. Examples of such additives include fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0040] The thickness of the base layer is arbitrary depending on the application, but is usually about 5 μm or more and about 200 μm or less, preferably about 5 μm or more and about 100 μm or less. The thickness can be appropriately adjusted by the screw rotation speed of the melt extruder and the rotation speed of the cooling roll when co-extrusion molding is performed to obtain a laminate, as described later.

[0041] <Heat seal layer> The polyethylene laminate of the present invention is provided with a heat seal layer. When the polyethylene laminate of the present invention is used to prepare a packaging material, the heat seal layer is used so as to be positioned on the inner surface of the packaging material.

[0042] The heat seal layer has a density of 0.930 g / cm3 By using the same material (polyethylene) as the base layer, but using polyethylene with a lower density than the polyethylene used in the base layer as the heat seal layer, it is possible to obtain a polyethylene laminate that maintains heat sealability and has recyclability.

[0043] For the heat seal layer, low density polyethylene or linear low density polyethylene may be used alone, or the two may be used in a suitable mixture. Also, a mixture of low density polyethylene and medium density polyethylene may be used as long as the density is within the above-mentioned range. From the viewpoint of heat sealability, a density of 0.925 g / cm or less is preferred. 3 Preferably, the density is less than 0.920 g / cm 3 It is more preferable to have a density of less than 100 μm.

[0044] The polyethylene film layer may contain the above-mentioned additives to the extent that the properties of the present invention are not impaired.

[0045] The thickness of the heat seal layer is optional depending on the application, but is usually preferably 15 μm or more and 200 μm or less, more preferably 20 μm or more and 200 μm or less, and even more preferably 25 μm or more and 160 μm or less. This allows the heat sealability of the polyethylene laminate of the present invention to be maintained while improving its processability. The thickness of the heat seal layer can be appropriately adjusted by the screw rotation speed of the melt extruder and the rotation speed of the cooling roll when co-extrusion molding to obtain a laminate, as described later.

[0046] The thickness ratio of the base layer to the heat seal layer is preferably 4:1 to 1:4, and more preferably 2:1 to 1:2. The thickness ratio can be appropriately adjusted by the screw rotation speed of the co-extrusion film-forming machine, as described later.

[0047] <Middle Class> The polyethylene laminate of the present invention may have an intermediate layer between the above-mentioned base layer and the heat seal layer. By providing the intermediate layer, the polyethylene laminate can be made stiffer and have improved shape stability. In addition, by providing the intermediate layer, the polyethylene laminate can be prevented from melting and becoming thin during the heat seal process for bag making.

[0048] From the viewpoint of recyclability, the intermediate layer is preferably made of polyethylene, which is the same material as the material constituting the base layer and the heat seal layer. In that case, the intermediate layer has a density of 0.942 g / cm 3 It is preferable that the polyethylene has a density of 0.950 g / cm or more, and more preferably has a density of 0.950 g / cm 3 More than 0.970g / cm 3 The polyethylene is preferably a high density polyethylene, but a mixture of medium density polyethylene and high density polyethylene in an appropriate blend ratio may also be used as long as the density is within the above range.

[0049] The thickness of the intermediate layer may vary depending on the application, but is usually about 5 μm to 100 μm, preferably about 10 μm to 80 μm, and more preferably about 10 μm to 60 μm.

[0050] The intermediate layer may contain ethylene-vinyl alcohol copolymer (EVOH) in addition to the above-mentioned polyethylene. By containing the ethylene-vinyl alcohol copolymer, the intermediate layer functions as a barrier layer, so that the polyethylene laminate can be endowed with barrier properties.

[0051] The thickness of the intermediate layer may be appropriately adjusted within a range that does not impair the function of the intermediate layer, and for example, the thickness ratio of the base layer to the intermediate layer may be in the range of 2:1 to 1:5, and preferably in the range of 1:1 to 1:3. The thickness ratio of the intermediate layer to the heat seal layer may be in the range of 1:2 to 5:1, and preferably in the range of 3:1 to 1:1. The thickness ratio of each layer may be appropriately adjusted by the screw rotation speed of the coextrusion film-forming machine when forming the polyethylene laminate, as described later.

[0052] <Other layers> The polyethylene laminate according to the present invention may be provided with layers other than the above-mentioned layers as long as the recyclability is not impaired. For example, a printed layer or a barrier layer may be provided on the surface of the base layer. Since the surface of the base layer of the polyethylene laminate according to the present invention is treated by electron beam irradiation, the adhesion between the printed layer or barrier layer and the base layer is excellent even if the base layer is not subjected to a particular surface treatment, but the surface may be subjected to a corona treatment, an ozone treatment, a low-temperature plasma treatment using oxygen gas or nitrogen gas, or the like, a glow discharge treatment, an oxidation treatment using chemicals, or the like, or the like.

[0053] The printing layer is a layer on which any desired printed pattern such as letters, numbers, pictures, figures, symbols, designs, etc. is formed for decoration, display of contents, display of expiration date, display of manufacturer, seller, etc., and for imparting aesthetics. The printing layer may be provided on the entire surface or part of the substrate layer or the barrier layer described below. The printing layer can be formed using conventionally known pigments or dyes.

[0054] The method for forming the printed layer is not particularly limited, and can be, for example, a printing method such as an inkjet method, a gravure printing method, an offset printing method, a flexographic printing method, a thermal transfer method, a transfer method, or a hot stamp (foil stamping).

[0055] The printing layer preferably has a thickness of 0.1 μm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less, and even more preferably 1 μm or more and 3 μm or less.

[0056] As the barrier layer, a metal foil or a vapor-deposited layer of a metal or an inorganic oxide can be suitably used.

[0057] As the metal foil, a conventionally known metal foil can be used. Aluminum foil is preferable in terms of gas barrier properties that prevent the transmission of oxygen gas and water vapor, and light blocking properties that prevent the transmission of visible light and ultraviolet rays. In addition, it is possible to impart metallic luster to the packaging bag, thereby improving the design. The thickness of the metal foil is, for example, 5 μm or more and 15 μm or less.

[0058] The vapor-deposited layer of metal or inorganic oxide is a layer consisting of a vapor-deposited film that can be formed by a conventionally known method. By providing a vapor-deposited layer, it is possible to impart or improve gas barrier properties that prevent the permeation of oxygen gas, water vapor, and the like. The barrier layer may have two or more vapor-deposited layers. When two or more vapor-deposited layers are provided, they may have the same composition or different compositions.

[0059] Examples of the metal deposition film that can be used include aluminum (Al), magnesium (Mg), tin (Sn), sodium (Na), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), gold (Au), chromium (Cr), etc. In particular, for packaging bags, it is preferable to have an aluminum deposition film.

[0060] The thickness of the metal vapor deposition film varies depending on the type of metal used, but it is desirable to select any thickness within the range of, for example, 50 Å to 2000 Å, preferably 100 Å to 1000 Å. More specifically, in the case of an aluminum vapor deposition film, the thickness is desirably 50 Å to 600 Å, more preferably 100 Å to 450 Å.

[0061] Examples of inorganic oxide vapor deposition films that can be used include vapor deposition films of oxides of silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), etc. In particular, for packaging bags, it is preferable to have a vapor deposition film of aluminum oxide or silicon oxide.

[0062] Inorganic oxides are expressed as MOX (wherein M represents an inorganic element, and the value of X varies depending on the inorganic element), such as SiOX and AlOX. The range of X is as follows: silicon (Si) is 0-2, aluminum (Al) is 0-1.5, magnesium (Mg) is 0-1, calcium (Ca) is 0-1, potassium (K) is 0-0.5, tin (Sn) is 0-2, sodium (Na) is 0-0.5, boron (B) is 0-1.5, titanium (Ti) is 0-2, lead (Pb) is 0-2, zirconium (Zr) is 0-2, and yttrium (Y) is 0-1.5. In the above, when X=0, it is a completely inorganic element (pure substance) and is not transparent, and the upper limit of the range of X is the value when it is completely oxidized. Silicon (Si) and aluminum (Al) are preferably used for the packaging material, and silicon (Si) with a value in the range of 1.0 to 2.0 and aluminum (Al) with a value in the range of 0.5 to 1.5 can be used.

[0063] The thickness of the inorganic oxide vapor deposition film varies depending on the type of inorganic oxide used, but it is desirable to select any thickness within the range of, for example, 50 Å to 2000 Å, preferably 100 Å to 1000 Å. For example, in the case of a vapor deposition film of aluminum oxide or silicon oxide, the thickness is desirably 50 Å to 500 Å, more preferably 100 Å to 300 Å.

[0064] The vapor-deposited film can be formed on the base layer etc. by using the following forming methods. Examples of the method for forming the vapor-deposited film include physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.

[0065] If necessary, a gas barrier coating film may be provided on the above-mentioned deposition layer. The gas barrier coating film is a coating film that functions as a layer that suppresses the permeation of oxygen gas, water vapor, etc. The gas barrier coating film is a coating film represented by the general formula R 1 nM(OR 2 )m (wherein, R 1 , R 2 represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M. The gas barrier composition contains at least one alkoxide represented by the formula (I) and a polyvinyl alcohol resin and / or an ethylene-vinyl alcohol copolymer, and is further polycondensed by a sol-gel method in the presence of a sol-gel catalyst, an acid, water, and an organic solvent.

[0066] The above general formula R 1 nM(OR 2 As the alkoxide represented by m, at least one of a partial hydrolyzate of an alkoxide and a condensate of hydrolysis of an alkoxide can be used. In addition, as the partial hydrolyzate of the alkoxide, it is not necessary that all of the alkoxy groups are hydrolyzed, and it may be one in which one or more are hydrolyzed, or a mixture thereof. As the condensate of hydrolysis of an alkoxide, a dimer or more of a partially hydrolyzed alkoxide, specifically, a dimer to hexamer, is used.

[0067] The above general formula R 1 nM(OR 2In the alkoxide represented by m, the metal atom represented by M can be silicon, zirconium, titanium, aluminum, or the like. In this embodiment, preferred metals include silicon and titanium. In the present invention, the alkoxide can be used alone or in the form of a mixture of two or more different metal atoms in the same solution.

[0068] In addition, the above general formula R 1 nM(OR 2 In the alkoxide represented by R 1 Specific examples of the organic group represented by the general formula R include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, t-butyl, n-hexyl, n-octyl, and the like. 1 nM(OR 2 In the alkoxide represented by R 2 Specific examples of the organic group represented by the formula (1) include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, etc. In addition, these alkyl groups may be the same or different in the same molecule.

[0069] When preparing the gas barrier composition, for example, a silane coupling agent may be added. As the silane coupling agent, a known organoalkoxysilane containing an organic reactive group may be used. In this embodiment, in particular, an organoalkoxysilane having an epoxy group is preferably used, and specifically, for example, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc. may be used. The silane coupling agents as described above may be used alone or in combination of two or more.

[0070] The polyethylene laminate according to the present invention is one in which the above-mentioned layers are formed by co-extrusion. That is, a polyethylene laminate having a density of 0.930 g / cm3 and a density of 0.930 g / cm3 constituting the base layer is formed by using an inflation film forming machine for co-extrusion. 3 The above polyethylene and the density of the heat seal layer are 0.930 g / cm 3 and optionally, a polyethylene having a density of 0.942 g / cm 3 The polyethylene laminate of the present invention can be obtained by forming a film by co-extruding the above polyethylenes, etc. In this manner, a polyethylene laminate having a base layer, a heat seal layer, and, if desired, an intermediate layer is formed, and then the above-mentioned printed layer and barrier layer are formed on the surface of the base layer, thereby producing the polyethylene laminate of the present invention.

[0071] Next, the electron beam irradiation treatment will be described. In the polyethylene laminate according to the present invention, the base layer is subjected to electron beam irradiation treatment. It is considered that the base layer is subjected to electron beam irradiation treatment, whereby a part of the polyethylene constituting the base layer is crosslinked, and the heat resistance is improved. The presence or absence of crosslinking (i.e., whether or not the base layer is subjected to electron beam irradiation treatment) can also be examined by taking advantage of the insolubility of the crosslinked portion in a solvent, immersing the polyethylene laminate in an organic solvent such as methyl ethyl ketone, drying the insoluble portion that remains undissolved, measuring the mass, and calculating the gel fraction from the thickness (mass) of the base layer before dissolution and the mass of the insoluble portion after drying, thereby examining the crosslink density. The gel fraction of the polyethylene laminate is preferably 20% or more and 80% or less, calculated as the mass of the base layer.

[0072] It is preferable to appropriately change the irradiation energy of the electron beam depending on the intended use of the package. Usually, the higher the irradiation energy of the electron beam, the more radicals are generated and the easier it is to form a crosslinked structure. However, if the irradiation energy is too high, the molecular chains of the polyethylene are cut too much, and the physical properties of the film such as strength tend to decrease.

[0073] The dose of the electron beam is preferably in the range of 10 to 2000 kGy, more preferably 20 to 1000 kGy, and the acceleration voltage of the electron beam is preferably in the range of 30 to 300 kV, more preferably 50 to 300 kV, and particularly preferably 50 to 250 kV. The irradiation energy of the electron beam is preferably 20 to 750 keV, more preferably 25 to 400 keV, further preferably 30 to 300 keV, and particularly preferably 20 to 200 keV.

[0074] As the electron beam irradiation device, a conventionally known device can be used, and for example, a curtain type electron irradiation device (LB1023, manufactured by I-Electron Beam Co., Ltd.) or a line irradiation type low energy electron beam irradiation device (EB-ENGINE, manufactured by Hamamatsu Photonics Co., Ltd.) can be preferably used. In particular, a line irradiation type low energy electron beam irradiation device (EB-ENGINE, manufactured by Hamamatsu Photonics Co., Ltd.) can be preferably used.

[0075] The oxygen concentration in the electron beam irradiation device is preferably 500 ppm or less, more preferably 100 ppm or less. By performing electron beam irradiation under such conditions, it is possible to suppress the generation of ozone and also to suppress the radicals generated by electron beam irradiation from being deactivated by oxygen in the atmosphere. Such conditions can be achieved, for example, by making the inside of the device an inert gas (nitrogen, argon, etc.) atmosphere.

[0076] Since polyethylene films are prone to thermal shrinkage, it is preferable to irradiate the film with electron beams while simultaneously cooling the film using a cooling drum or the like.

[0077] <Packaging materials> The polyethylene laminate described above can be suitably used as a packaging material. In one embodiment of the present invention, a packaging material 20 using the polyethylene laminate of the present invention has a bag-like shape as shown in FIG.

[0078] In another embodiment, a packaging material 30 using the polyethylene laminate of the present invention has a shape of a stand-up pouch including a body 31 and a bottom 32, as shown in Fig. 4. In this embodiment, only the body may be formed of the polyethylene co-extruded film, only the bottom may be formed of the polyethylene co-extruded film, or both the body and bottom may be formed of the polyethylene co-extruded film.

[0079] The packaging material can be produced by folding the above-mentioned polyethylene laminate in half and overlapping it so that the base layer is on the outside and the heat seal layer is on the inside, and then heat sealing the ends, etc. Alternatively, the packaging material can be produced by overlapping two polyethylene laminates so that the base layer sides face each other, and then heat sealing the ends, etc.

[0080] For example, various types of packaging materials can be manufactured by heat sealing in a heat sealing manner such as side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, grooving seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, gusset type, etc. In addition, for example, a self-supporting packaging bag (standing pouch) etc. can also be manufactured. Heat sealing can be performed by known methods such as bar seal, rotary roll seal, belt seal, impulse seal, high frequency seal, ultrasonic seal, etc.

[0081] Packaging materials made from bags using the polyethylene laminate of the present invention are made of a single material (i.e., polyethylene), and therefore have better recyclability than conventional packaging materials made by combining different materials. In addition, the base layer of the polyethylene laminate contains polyethylene of a specific density that has been irradiated with electron beams, and therefore can satisfy the physical properties required for the outer layer of packaging materials, such as strength, dimensional stability, and printability. Furthermore, the heat seal layer of the polyethylene laminate has a density of 0.930 g / cm 3 Since it contains less than 100% polyethylene, it has heat sealability and can be suitably used as a packaging film. EXAMPLES

[0082] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0083] <Example 1> Medium density polyethylene (density: 0.937g / cm 3 , MFR: 1.8g / 10min, Prime Polymer Co., Ltd., product name: SP4020) High density polyethylene (density: 0.958g / cm 3 , MFR: 1.0g / 10min, manufactured by Prime Polymer Co., Ltd., product name: Hizex3600F) Linear low-density polyethylene (density: 0.916 g / cm 3 A polyethylene laminate was obtained by coextrusion molding of a polyethylene terephthalate resin (product name: SP2020, MFR: 2.3 g / 10 min, manufactured by Prime Polymer Co., Ltd.) in a ratio of 1:3:1. The thickness of the obtained coextruded polyethylene laminate was 60 μm. The density of the obtained coextruded polyethylene laminate was 0.937 g / cm 3 The layer of medium density polyethylene is called the base layer, and has a density of 0.916 g / cm 3 The layer side of the linear low density polyethylene is referred to as the heat seal layer.

[0084] The base layer side of the co-extruded polyethylene laminate obtained as described above was subjected to a corona treatment, and further irradiated with an electron beam using an electron beam irradiation device (line irradiation type irradiation device EZ-CURE, manufactured by Iwasaki Electric Co., Ltd.) under the following conditions, thereby obtaining a co-extruded polyethylene laminate in which the base layer was irradiated with an electron beam. (Electron beam irradiation conditions) Voltage: 100kV Irradiation dose: 280kGy Oxygen concentration inside the device: 100ppm or less Line speed: 25m / min

[0085] Immediately after production, an image was formed on the surface of the substrate layer side of the coextruded polyethylene laminate obtained as described above by gravure printing using a solvent-based gravure ink (manufactured by DIC Graphics Corporation, trade name: XOX-901).

[0086] <Example 2> A coextruded polyethylene laminate was obtained in the same manner as in Example 1, except that the electron beam irradiation conditions were as follows: (Electron beam irradiation conditions) Voltage: 110kV Irradiation dose: 280kGy Oxygen concentration inside the device: 100ppm or less Line speed: 25m / min

[0087] <Example 3> A coextruded polyethylene laminate was obtained in the same manner as in Example 1, except that the thickness of the coextruded polyethylene laminate was 100 μm.

[0088] <Example 4> A coextruded polyethylene laminate was obtained in the same manner as in Example 2, except that the thickness of the coextruded polyethylene laminate was 100 μm.

[0089] <Example 5> A coextruded polyethylene laminate was obtained in the same manner as in Example 1, except that the printing method after irradiating the substrate layer surface with electron beams was changed as follows. (Printing method) First, OP varnish (Showa Ink Industrial Co., Ltd., product name: ALEX peelable OP varnish) was applied to the untreated surface of a PET film (Toyobo Co., Ltd., product name: E5100, 12 μm), and an image was formed by gravure printing using a solvent-based gravure ink (Showa Ink Industrial Co., Ltd., product name: ALEX (NT) pattern ink). The obtained image-formed PET film and the co-extruded polyethylene laminate after electron beam irradiation obtained in the same manner as in Example 1 were dry laminated via a two-liquid curing urethane adhesive (Rock Paint Co., Ltd., product name: RU-40 / curing agent H-4) so ​​that the printed surface of the PET film and the electron beam irradiated surface (base layer surface) faced each other, and a co-extruded polyethylene laminate was obtained. Thereafter, the PET film was peeled off, and the printed layer was transferred onto the surface of the base layer side of the coextruded polyethylene laminate to form an image.

[0090] <Example 6> A coextruded polyethylene laminate was obtained in the same manner as in Example 3, except that the printing method after irradiating the substrate layer surface with electron beams was changed as follows. (Printing method) First, OP varnish (Showa Ink Industrial Co., Ltd., product name: ALEX peelable OP varnish) was applied to the untreated surface of a PET film (Toyobo Co., Ltd., product name: E5100, 12 μm), and an image was formed by gravure printing using a solvent-based gravure ink (Showa Ink Industrial Co., Ltd., product name: ALEX (NT) pattern ink). The obtained image-formed PET film and the co-extruded polyethylene laminate after electron beam irradiation obtained in the same manner as in Example 3 were dry laminated via a two-liquid curing urethane adhesive (Rock Paint Co., Ltd., product name: RU-40 / curing agent H-4) so ​​that the printed surface of the PET film and the electron beam irradiated surface (base layer surface) faced each other, and a co-extruded polyethylene laminate was obtained. Thereafter, the PET film was peeled off, and the printed layer was transferred onto the surface of the base layer side of the coextruded polyethylene laminate to form an image.

[0091] <Comparative Example 1> A coextruded polyethylene laminate was obtained in the same manner as in Example 1, except that electron beam irradiation was not performed.

[0092] <Comparative Example 2> A coextruded polyethylene laminate was obtained in the same manner as in Example 3, except that electron beam irradiation was not performed.

[0093] <Heat resistance evaluation> The coextruded polyethylene laminates obtained in the above examples and comparative examples were cut into 5 cm x 5 cm samples, three at a time. Each sample was heated for 5 seconds in a glycerin solution heated to 140°C. The size of the sample pieces after heating was measured in the machine direction (MD) during inflation molding and in the transverse direction (TD) perpendicular thereto. The average shrinkage rate from the time of cutting was as shown in Table 1 below.

[0094] <Seal strength evaluation> The co-extruded polyethylene laminates obtained in the above examples and comparative examples immediately after production were cut into 10 cm x 10 cm samples, each of which was cut into three pieces. Each sample was cut on the side that had not been irradiated with the electron beam, i.e., the side with a density of 0.916 g / cm. 3 The sheet was folded in half with the polyethylene layer on the inside, and a 1 cm x 10 cm area was heat sealed using a heat seal tester at 180°C, 1 kgf / cm2 pressure, and 1 second.

[0095] The heat-sealed sample pieces were cut into strips 15 mm wide, and both ends that were not heat-sealed were held in a tensile tester to measure the peel strength (N / 15 mm) at a speed of 300 mm / min and a load range of 50 N. Note that the co-extruded polyethylene laminates obtained in Comparative Examples 1 and 2 adhered to the heat seal bar, making it impossible to measure the peel strength, and were therefore marked as "-". The measurement results are shown in Table 1 below.

[0096] <Printability test> The formed images were visually observed, and the printability of the coextruded polyethylene laminates obtained in the above Examples and Comparative Examples was evaluated based on the following evaluation criteria. ◯: The dimensional stability during printing was good, and good images without rubbing, bleeding, etc. could be formed. ×: The film expanded and contracted during printing, causing rubbing and bleeding in the formed image. The evaluation results are shown in Table 1.

[0097] <Liquid pouch manufacturing evaluation> Using a liquid pouch filling machine, liquid pouches measuring 100 mm in length and 80 mm in width were produced from the coextruded polyethylene films obtained in the above Examples and Comparative Examples. The bag-making method was as follows: first, two co-extruded polyethylene laminates were stacked with their heat-sealed layers facing each other, and three sides were heat-sealed with a heat-seal bar at 140° C. Next, the heat-sealed co-extruded polyethylene laminate was cut into a size of 100 mm length × 80 mm width to prepare liquid pouches. The suitability of the liquid pouches for bag making was evaluated based on the following evaluation criteria. ◯: The film was not fused to the heat seal bar, and liquid pouches could be produced using the liquid pouch filling machine. ×: The film was fused to the heat seal bar, and the liquid pouch could not be neatly produced by the liquid pouch filling machine. The evaluation results are shown in Table 1.

[0098] <Stand-up pouch bag making evaluation> Using a bag making machine, stand-up pouches measuring 110 mm in length and 150 mm in width were made from the coextruded polyethylene laminates obtained in the above Examples and Comparative Examples. As a bag making method, first, one test piece of 110 mm length x 60 mm width was prepared from the coextruded polyethylene laminate obtained in the examples and comparative examples, and folded in a V shape (110 mm length x 30 mm width) so that the heat seal layer was on the outside. Next, two coextruded polyethylene laminates were overlapped with the heat seal layers facing each other, and the V-folded test piece obtained above was sandwiched at one end and heat sealed with a heat seal bar at 140°C to form a bottom. Next, two sides adjacent to the bottom were heat sealed in the same manner to form a cylindrical body, and the body was cut to a size of 110 mm length x 150 mm width to prepare a stand pouch. The suitability of the stand-up pouches for bag making was evaluated based on the following evaluation criteria. ◯: The film was not fused to the heat seal bar, and a stand-up pouch could be produced using the bag making machine. ×: The film was fused to the heat seal bar, and a clean stand-up pouch could not be produced using the bag making machine. The evaluation results are shown in Table 1.

[0099] [Table 1]

Claims

1. A polyethylene laminate comprising a base layer, a printing layer provided on a surface of the base layer, and a heat seal layer (excluding a heat shrinkable multilayer film comprising a base layer and at least one heat seal layer laminated on the base layer, the heat shrinkable multilayer film having a heat shrinkage rate of 10% or less at 110°C and 30% or more at 140°C in accordance with ASTM D2732 in the machine direction and in a direction perpendicular to the machine direction of the heat shrinkable multilayer film), The substrate layer has a density of 0.930 g / cm 3 It is made up of polyethylene, the substrate layer comprises high density polyethylene and / or medium density polyethylene, but does not comprise low density polyethylene; The heat seal layer has a density of 0.930 g / cm 3 It is made up of polyethylene less than The base layer and the heat seal layer have a density of 0.930 g / cm 3 The above polyethylene and density 0.930 g / cm 3 and is formed by co-extrusion with polyethylene of less than 13. A polyethylene laminate, wherein the substrate layer has been subjected to an electron beam irradiation treatment.

2. 10. The polyethylene laminate of claim 1 comprising an intermediate layer between said substrate layer and said heat seal layer.

3. The intermediate layer has a density of 0.942 g / cm 3 It is made up of polyethylene, The base layer, the intermediate layer and the heat seal layer have a density of 0.930 g / cm 3 The above polyethylene and density 0.942 g / cm 3 The above polyethylene and density 0.930 g / cm 3 3. The polyethylene laminate of claim 2, which is formed by coextrusion with polyethylene of less than 1000 parts by mass.

4. The polyethylene laminate according to any one of claims 1 to 3, further comprising a barrier layer on a surface of the base layer.

5. A packaging material comprising the polyethylene laminate according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Packaging polyolefin film and preparation method thereof

    CN103085415A

  • Polyethylene film, and craft bag using the same

    JP2005104525A

  • Thermal shrinking multilayer film

    JP2010094967A

  • Thermally-shrinkable multilayer film, and packaging bag obtained by using the same

    JP2015147302A

  • Laminate and package using the same

    JP2017030150A