Improvements on superhydrophobic surfaces

A superhydrophobic film using polymer-coated metal oxide nanoparticles addresses durability and UV resistance issues, ensuring high water repellency and mechanical stability for diverse substrates.

JP7591287B2Active Publication Date: 2024-11-28QUEEN MARY UNIV OF LONDON
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021555096
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-12
Filing Date
2020-03-10
Publication Date
2024-11-28
Estimated Expiration
2040-03-10

AI Technical Summary

Technical Problem

Existing superhydrophobic coatings are limited by high costs, environmental hazards, and poor mechanical durability, and they often degrade under UV exposure due to the use of fluorinated chemicals and complex manufacturing processes.

Method used

A superhydrophobic film is developed using metal oxide nanoparticles, such as SiO2 and TiO2, coated with polymers like PDMS, which are applied through methods like spray coating or dip coating, ensuring a particle-to-coating ratio of 2.5:1 to 20:1, providing a durable and UV-resistant surface.

Benefits of technology

The film maintains high water contact angles and mechanical stability, resisting UV degradation and abrasion, making it suitable for various substrates including glass, metal, and fabric, with improved industrial applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591287000003
    Figure 0007591287000003
  • Figure 0007591287000004
    Figure 0007591287000004
  • Figure 0007591287000005
    Figure 0007591287000005
Patent Text Reader

Abstract

Improvements on superhydrophobic surfaces A superhydrophobic film for coating a substrate is disclosed. The superhydrophobic film comprises a plurality of nanoparticles bonded together to form a continuous film, each nanoparticle having a polymer coating, and the ratio of the average particle size of the nanoparticles to the average thickness of their polymer coating is 2.5:1 to 20:1. The superhydrophobic film suitably provides a durable, UV-resistant coating that maintains a high water contact angle during use. A method for preparing a superhydrophobic film on a substrate is also disclosed, which includes mixing nanoparticles with a polymer to form nanoparticles having a polymer coating, and applying the nanoparticles having the polymer coating to a substrate to form a superhydrophobic film. A formulation for coating an article with such a superhydrophobic film is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to superhydrophobic compositions, such as films, articles comprising such superhydrophobic films, methods of making such superhydrophobic films, and formulations for coating articles with such superhydrophobic films. In particular, the present invention relates to superhydrophobic films comprising nanoparticles having a polymeric coating. [Background technology]

[0002] Self-cleaning technology has great commercial potential and can be implemented in a wide range of fields, for example in antifouling paints, window glass, concrete, and textiles, among others. Currently, self-cleaning functionality can be achieved using two main surface types: superhydrophobic or superhydrophilic. Both surface types allow the removal of surface-bound contaminants such as dirt and bacteria.

[0003] Self-cleaning superhydrophilic surfaces exploit the synergistic effects of light-induced photocatalysis and hydrophilicity. In this mechanism, organic material bound to the surface is decomposed and subsequently removed by the action of water, which spreads evenly across the surface in a phenomenon known as water sheeting. Coatings engineered from inherently hydrophilic photoactive materials can become superhydrophilic when illuminated with UV light due to light-induced oxygen vacancies. However, superhydrophilic self-cleaning is often considered inferior to its superhydrophobic equivalent, as high water repellency and reduced biofilm formation provide a more effective cleaning system.

[0004] Superhydrophobic surfaces are formed by combining surface roughening with low surface energy materials. High water contact angle (WCA), defined as greater than 150°, and low contact angle hysteresis (CAH) are characteristics used to quantify hydrophobicity. Water on such superhydrophobic surfaces forms nearly spherical droplets that minimize surface tension, and such droplets roll off the surface, removing unwanted dirt particles and their associated surface bacteria, in a phenomenon known as the lotus effect. Summary of the Invention

[0005] Superhydrophobic surfaces can be engineered inexpensively from inorganic nanoparticles treated with organic coatings. Selection of the appropriate nanoparticle-organic composite is critical to the durability and visual properties of the coating. With regard to visual properties, titania (TiO2) is a wide band gap semiconductor oxide that is essential for pigment coatings due to its high refractive index and known optical properties, the combination of which allows for maximum scattering of visible light in TiO2 nanomaterials. These factors make titania the brightest white pigment commonly used and important for the paint and coatings industry.

[0006] Known methods of forming superhydrophobic coatings using photoactive nanoparticles (such as TiO2) combined with low surface energy materials can limit the usefulness of the resulting superhydrophobic surfaces, as such known coatings have been shown to lose superhydrophobicity relatively quickly, for example after a few hours of UV exposure. Such superhydrophobic coatings have also been reported to have poor mechanical durability, which further limits the industrial usefulness of these coatings.

[0007] Furthermore, successful production methods typically involve the use of fluorinated chemicals, multi-step modification processes, or the need for specialized equipment, all of which can be expensive and / or environmentally hazardous.

[0008] One object of the present invention is, inter alia, to provide a superhydrophobic film that addresses at least one shortcoming of the prior art, whether specified herein or elsewhere, or to provide an alternative to existing superhydrophobic films. For example, an object of the present invention may be to provide a superhydrophobic film having improved UV resistance and improved mechanical stability.

[0009] It is also an object of the present invention to provide a method for forming such superhydrophobic films on a substrate that is more efficient and cost effective than known methods.

[0010] According to aspects of the present invention there are provided superhydrophobic films, articles, methods and formulations as set out in the accompanying claims. Further features of the invention will become apparent from the dependent claims and the following description. [Brief description of the drawings]

[0011] [Figure 1] Figures 1a and 1b show TEM images of as-received P25 TiO2 (80:20 anatase:rutile) and CeO2 nanoparticles used for coating with measured average diameters of 23 nm and 28 nm. Figure 1c shows the amorphous layer surrounding the particles detected by S-TEM after PDMS coating. Figure d shows the energy dispersive X-ray spectroscopy results of TiO2-PDMS. [Diagram 2] FIG. 2 shows SEM images of the top (FIGS. 2a and 2b, ×1,000 and ×20,000 magnifications, respectively) and side (FIG. 2c, ×1,500 magnification) views of the PDMS-modified TiO2 of Example 1. [Diagram 3] FIG. 3 shows a plot of WCA under UV irradiation over time. [Figure 4] Figure 4 is a graph of the WCA of PE particle coatings on nanoparticles with thicknesses ranging from 1.5 nm to 20 nm. [Figure 5a]Figure 5a shows (a) an SEM image of a superhydrophobic film composed of SiO2 / PE nanocomposite with a 1.5 nm PE coating. [Figure 5b] Figure 5b shows (b) an SEM image of a superhydrophobic film composed of SiO2 / PE nanocomposite with a 2 nm PE coating. [Figure 5c] Figure 5c shows (c) an SEM image of a superhydrophobic film composed of SiO2 / PE nanocomposite with a 3 nm PE coating. [Figure 6] FIG. 6 is a graph showing the relationship between WCA and number of iterations for films made from SiO2 / PE nanocomposites with PE coatings of thicknesses of 1.5 nm, 2 nm, and 3 nm. [Figure 7a] Figure 7a shows (a) an SEM image of SiO2 / PE with a 1.5 nm PE coating made from six iterations. [Figure 7b] Figure 7b shows (b) an SEM image of SiO2 / PE with a 1.5 nm PE coating made from four iterations. [Figure 7c] Figure 7c shows (c) an SEM image of SiO2 / PE with a 1.5 nm PE coating made from two iterations. [Figure 8] FIG. 8 shows a graph illustrating the relationship between WCA and number of iterations for SiO2 / PE nanocomposites with PE coatings of 1.5 nm, 2 nm, and 3 nm thickness (0.2 g PE / 70 mL). [Figure 9a] Figure 9a shows (a) SEM images of SiO2 / PE with 1.5 nm PE coating prepared by four replicates (0.2 g PE / 70 mL). [Figure 9b] FIG. 9b shows (b) an SEM image of SiO2 / PE with a 1.5 nm PE coating prepared by six iterations (0.2 g PE / 70 mL). [Figure 10ab]Figure 10 shows SEM images of the side of a PVC substrate and a SiO2 / PVC film applied to the substrate, (a) and (b) are of the PVC material substrate before coating. [Figure 10cd] Figure 10 shows side-view SEM images of a PVC substrate and a SiO2 / PVC film applied to the substrate, (c) and (d) of the SiO2 / PVC coating made using a 2x concentrated MIBK solution. [Fig. 10ef] Figure 10 shows side-view SEM images of a PVC substrate and a SiO2 / PVC film applied to this substrate, (e) and (f) of the SiO2 / PVC coating made using a twice concentrated toluene / MIBK solution. [Figure 11a] FIG. 11 shows (a) and (b) SEM images of SiO2 / PVC coatings prepared with twice concentrated MIBK. [Figure 11b] FIG. 11 shows (a) and (b) SEM images of SiO2 / PVC coatings prepared with twice concentrated MIBK. [Figure 11c] FIG. 11 shows (c) and (d) SEM images of SiO2 / PVC coatings prepared using a twice concentrated toluene / MIBK solution. [Figure 11d] FIG. 11 shows (c) and (d) SEM images of SiO2 / PVC coatings prepared using a twice concentrated toluene / MIBK solution. [Figure 12] FIG. 12 is a diagram of hot pressing the particles into a plasticized PVC material. [Figure 13a] FIG. 13 shows an SEM image of a side view of a silica-PVC film that was hot pressed onto a plasticized PVC material substrate. [Figure 13b] FIG. 13 shows an SEM image of a side view of a silica-PVC film that was hot pressed onto a plasticized PVC material substrate. [Figure 14] FIG. 14 shows images taken with a Drop Shape Analyzer of a hot pressed silica / PVC sample (Example 9) before (left) and after (right) 25 cycles of physical abrasion. [Figure 15] FIG. 15 shows the change in WCA of Example 9 (40 wt % DIDP in PVC / SiO2) over 25 cycles of abrasion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] According to a first aspect of the present invention, there is provided a superhydrophobic film comprising an aggregate of nanoparticles having a polymer coating, the nanoparticles having a ratio of particle size to average thickness of their polymer coating of between 2.5:1 and 20:1.

[0013] A superhydrophobic film suitably has a high water contact angle (WCA), such as at least 150°, meaning that the film is not easily wetted by water in contact with the film, suitably not wetted at all by water in contact with the film. A superhydrophobic film may be considered to be a superhydrophobic composition comprising nanoparticles with a polymer coating, suitably a relatively thin composition having a thickness, for example, between 2 nm and 150 μm. A superhydrophobic film may also be considered to be a superhydrophobic coating. The film is a coating on a substrate, suitably disposed on the substrate, that is relatively thin compared to the thickness of the substrate. Suitable substrates are glass, metal, masonry and fabrics. A superhydrophobic film has at least one surface that exhibits these superhydrophobic properties, suitably a surface that is exposed to the atmosphere in use, suitably a top surface associated with said substrate. A superhydrophobic film includes a surface that is suitably not exposed to the atmosphere in use, suitably bonded to said substrate.

[0014] The superhydrophobic film comprises nanoparticles having a polymer coating. Nanoparticles having a polymer coating may alternatively or additionally be defined as polymer-coated nanoparticles. Suitably, each nanoparticle comprises a polymer layer completely coating the nanoparticle. The average thickness of the coating on the nanoparticles depends on the average particle size of the nanoparticles, where the ratio of particle size to the average thickness of the polymer coating is 2.5:1 to 20:1, suitably 2.5:1 to 15:1, suitably 2.5:1 to 10:1, suitably 2.5:1 to 6:1, suitably 3:1 to 5:1. Thus, smaller nanoparticles suitably have a thinner polymer coating than the polymer coating on larger nanoparticles. The inventors have found that larger nanoparticles can have a thicker polymer coating than is possible with smaller nanoparticles while still maintaining the superhydrophobicity of the film. The average thickness of the polymer coating is suitably 0.5 to 150 nm, depending on the average particle size of the nanoparticles. For example, where the nanoparticles have an average particle size of 5-50 nm, the average thickness of the polymer coating on the nanoparticles is suitably 0.5-25 nm, suitably 0.5-10 nm, the aforementioned ratio of average particle size to average thickness of their polymer coating being 2.5:1-20:1. Where the nanoparticles have an average particle size of 250-500 nm, the average thickness of the polymer coating on the nanoparticles is suitably 25-150 nm. The actual thickness of the polymer coating on any one particular nanoparticle may suitably vary within the stated ranges.

[0015] The superhydrophobic film comprises an aggregate of these nanoparticles with a polymer coating. The superhydrophobic film can therefore be considered to comprise a plurality of polymer-coated nanoparticles arranged together to form a continuous mass that constitutes the superhydrophobic film. Suitably, the superhydrophobic film is continuous, and no part of the surface of the underlying substrate in the region of the substrate coated by the film is exposed to the atmosphere. Suitably, the aggregate of polymer-coated nanoparticles is provided by a plurality of polymer-coated nanoparticles contacting and bonding with each other through their polymer coating. The aggregate can therefore be considered to be formed through bonding of the polymer coatings of adjacent nanoparticles. Suitably, the polymer coating on the nanoparticles is the same polymer, which allows the polymer coatings of adjacent nanoparticles in the film to be partially intermixed (under suitable forming conditions) to provide bonding and produce the superhydrophobic film.

[0016] This aggregation of nanoparticles suitably provides a film with a highly rough and hierarchical morphological surface, providing superhydrophobicity.

[0017] The inventors have found that the superhydrophobic film according to this first aspect can provide a surface with a high WCA, for example greater than 160°, which can be maintained for a significant period of UV light exposure, for example at least 24 hours, or suitably at least 4 days. The superhydrophobic film can also provide a coating with good mechanical resistance to repeated abrasion and may therefore be suitable for industrial applications involving coated surfaces that are subject to wear during use.

[0018] Suitably, the superhydrophobic film has a WCA of at least 150°, suitably greater than 150°. Suitably, the superhydrophobic film has a WCA of at least 155°, such as at least 160° or at least 165°. Suitably, the superhydrophobic film has a WCA of 150-180°, such as 155-175°.

[0019] Suitably, the nanoparticles of the superhydrophobic film are metal oxide nanoparticles.Suitable metal oxide nanoparticles may be selected from SiO2, TiO2, CeO2, CaO, MgO, ZnO2, Al2O3, BaO or mixtures thereof.Suitably, the metal oxide nanoparticles are selected from SiO2, TiO2, CeO2 or mixtures thereof.

[0020] In some embodiments, the nanoparticles are SiO2 nanoparticles, suitably pre-functionalized SiO2 nanoparticles. The pre-functionalization of nanoparticles can be carried out by treating the SiO2 nanoparticles with a reagent that modifies the functional groups on the surface of the SiO2 nanoparticles before coating with a polymer, for example to improve the binding of the polymer to the nanoparticles. Suitably, the SiO2 nanoparticles are pre-functionalized with hexamethyldisilazane (HMDS).

[0021] In some embodiments, the nanoparticles are provided by a mixture of SiO2 or TiO2 and CeO2. Suitably, the nanoparticles are provided by a mixture of TiO2 and CeO2. CeO2 exhibits limited interaction with water, possibly as a result of the shielding effect of its unfilled 4f orbitals, in addition to exhibiting rapid recombination of charge carriers due to a high concentration of oxygen vacancies acting as recombination centers. As a result, the UV degradation resistance of superhydrophobic films can be improved by using CeO2 in combination with other metal oxide nanoparticles. This can be particularly advantageous when used with TiO2 nanoparticles, which are particularly susceptible to degrading polymer coatings when exposed to UV light, thereby adversely affecting the superhydrophobicity of the film.

[0022] In such an embodiment, the nanoparticles may comprise a mixture of SiO2 or TiO2 and CeO2, in a ratio of SiO2 or TiO2:CeO2 of 1:50 to 1:1, suitably 1:20 to 1:5, for example about 1:10. The inventors have found that a TiO2:CeO2 nanoparticle ratio of 1:10 may provide a superhydrophobic film with particularly good resilience to UV radiation.

[0023] Suitably, the nanoparticles of the superhydrophobic film according to this first aspect have an average particle size of 5-1,000 nm, suitably 5-500 nm, suitably 5-100 nm, suitably 5-75 nm, suitably 10-75 nm, suitably 10-50 nm. In some embodiments, the nanoparticles have an average particle size of 5-50 nm. Suitably, the average particle size of the nanoparticles was measured using an electron microscope from about 50 particles per image of TiO2 and CeO2. The particle size referred to above is for the nanoparticles before the polymer coating is applied and therefore does not include the increase in particle size caused by coating with a polymer.

[0024] The average thickness of the polymer coating on the nanoparticles is suitably from 0.5 to 125 nm, suitably from 0.5 to 50 nm, suitably from 0.5 to 20 nm.

[0025] In some embodiments, the nanoparticles have an average particle size of 5-100 nm, suitably 5-50 nm, and the average thickness of the polymer coating on the nanoparticles is 0.5-25 nm, suitably 0.5-10 nm.

[0026] In some embodiments, the average particle size of the nanoparticles is from 100 to 500 nm, suitably from 250 to 500 nm, and the average thickness of the polymer coating on the nanoparticles is from 25 to 150 nm, suitably from 50 to 100 nm.

[0027] To obtain a desired thickness of polymer coating on the nanoparticles, the amount of polymer used must be varied according to the particle size of the nanoparticles, taking into account that coating larger nanoparticles requires less volume of polymer compared to the volume of the nanoparticles than coating smaller nanoparticles with the same thickness of polymer coating. Suitably, the ratio of the volume of polymer coating to the volume of nanoparticles is 10:1 to 1:10, suitably 3:1 to 1:5, suitably 1:1 to 1:3.

[0028] Suitably the superhydrophobic film of this first aspect comprises an aggregate of nanoparticles having a polymer coating, the polymer coating of the nanoparticles having an average thickness of 0.5-10 nm and the nanoparticles having an average particle size of 5-100 nm. The inventors have found that this combination of particle size and polymer coating thickness is particularly advantageous for providing a superhydrophobic surface on the film with a high WCA.

[0029] The polymer coating on the nanoparticles has an average thickness of 0.5-10 nm. Suitably, the polymer coating on the nanoparticles has an average thickness of 0.5-7 nm, suitably 0.5-5 nm, suitably 1-3 nm. The inventors have found that these ranges of thickness of the polymer coating on the nanoparticles provide the highest WCA values, UV resistance and mechanical durability. As the thickness of the polymer coating is increased beyond these limits, the WCA of the film decreases, presumably because the relatively thick polymer coating reduces the roughness of the film surface.

[0030] The polymer that provides the polymer coating of the nanoparticles can be any suitable polymeric material that is compatible with the particular nanoparticle and the solvent system used to form the polymer-coated nanoparticles. The polymer suitably comprises at least 10 monomer repeat units, suitably at least 20 or at least 30 monomer repeat units. The polymer suitably has a weight average molecular weight of at least 500, suitably at least 750, suitably at least 1,000.

[0031] Suitably, the polymer providing the polymeric coating of the nanoparticles is selected from a siloxane-based polymer, a polyolefin, a polyvinyl chloride, or a mixture thereof.

[0032] Suitably, the polymer providing the polymeric coating of the nanoparticles is selected from polydimethylsiloxane, polyethylene, polypropylene, polyvinyl chloride or mixtures thereof.

[0033] In some embodiments, the polymer coating is a siloxane-based polymer. Suitably, the polymer coating is polydimethylsiloxane. Polydimethylsiloxane (PDMS), also known as dimethylpolysiloxane or dimethicone, has the structure (1): [ka] Here, n is an integer.

[0034] In embodiments in which the polymer of the polymeric coating of the nanoparticles is polyvinyl chloride, the polyvinyl chloride is suitably a high molecular weight polyvinyl chloride.

[0035] In embodiments in which the polymer of the polymeric coating of the nanoparticles is polyethylene, the polyethylene is suitably high density polyethylene.

[0036] In embodiments in which the polymer of the polymeric coating of the nanoparticles is polypropylene, the polypropylene suitably has a molecular weight of from 300,000 to 350,000.

[0037] The superhydrophobic film of this first embodiment suitably has a thickness of from 50 nm to 100 μm, suitably from 200 nm to 50 μm.

[0038] In some embodiments, the superhydrophobic film consists essentially of the nanoparticles and the polymer coating.

[0039] In some embodiments, the superhydrophobic film is comprised of nanoparticles and a polymer coating.

[0040] According to a second aspect of the present invention there is provided an article comprising a superhydrophobic film according to the first aspect. Suitably the superhydrophobic film is bonded to at least a portion of the article to provide a superhydrophobic film thereon.

[0041] The superhydrophobic film may have any of the suitable features and advantages described above in relation to the first embodiment.

[0042] Suitably, at least a part of the article on which the superhydrophobic film is formed is glass, fabric, polymer or metal material. Suitably, the article that comprises the superhydrophobic film is mainly formed from at least one of these materials. The article may be a vehicle component (e.g., the interior component of a vehicle), a fabric (e.g., waterproof clothing), a laminated surface (e.g., a workbench), a furniture article, a glass sheet or glass plate, or any other article that benefits from the resistance to water or dirt that the superhydrophobic film of the present invention can provide.

[0043] According to a third aspect of the present invention, there is provided a method of preparing a superhydrophobic film on a substrate, the method comprising: (a) mixing nanoparticles with a polymer to form nanoparticles having a polymer coating; (b) Applying the nanoparticles with a polymer coating to a substrate to form a superhydrophobic film.

[0044] The nanoparticles, polymers and polymer coatings may have any of the suitable features and advantages described above in relation to the first aspect.

[0045] Suitably, the steps of the above method are carried out in the order: step (a) followed by step (b).

[0046] Suitably, the nanoparticles and polymer are mixed in step (a) as described in relation to the first aspect in a ratio that provides a sufficient amount of polymer to form a polymer coating of desired thickness on the nanoparticles. In some embodiments, the average thickness of the polymer coating on the nanoparticles is 0.5-10 nm, suitably a polymer coating of 0.5-5 nm. As mentioned above, for larger nanoparticles, the relative volume of polymer required to coat the nanoparticles to a certain thickness is less than the volume of polymer required to coat smaller nanoparticles to the same thickness. The amount of polymer required can be calculated by considering the average volume of nanoparticles and the volume of polymer coating around the nanoparticles that provides the required polymer coating thickness. For example, a nanoparticle with a particle size (diameter, assuming spherical) of 20 nm with a polymer coating of 2.5 nm will require a polymer coating of 4,189 nm. 3 Nanoparticle volume and 3,992 nm 3 Thus, a polymer to nanoparticle volume ratio of 0.95:1 provides the desired polymer coating thickness of 2.5 nm.

[0047] Suitably the ratio of the volume of the polymer coating to the volume of the nanoparticles is from 10:1 to 1:10, suitably from 3:1 to 1:5, suitably from 1:1 to 1:3.

[0048] Step (a) comprises allowing sufficient time for the polymer to coat the nanoparticles and form polymer-coated nanoparticles. For example, step (a) may comprise mixing the nanoparticles and the polymer, e.g., in a solvent, for at least 10 minutes, suitably at least 30 minutes, suitably at least 1 hour.

[0049] Steps (a) and (b) may be repeated at least once, suitably two or more times, to provide a thicker superhydrophobic film on the substrate. Steps (a) and (b) may be repeated a sufficient number of times to provide complete coverage of the area of ​​the substrate and to provide a superhydrophobic film having the required mechanical durability.

[0050] In some embodiments, step (a) comprises mixing nanoparticles and a polymer in a solvent, and step (b) comprises applying the nanoparticles in the solvent with the polymer coating to a substrate. In such embodiments, the method of preparing the superhydrophobic film may be a spray coating method or a dip coating method. In such embodiments, the method suitably comprises step (c) of drying the applied nanoparticles with the polymer coating to form a superhydrophobic film.

[0051] In such an embodiment, the solvent may be a mixture of solvents. The solvent or solvent mixture may be selected for compatibility with the particular nanoparticles and polymer used. The nanoparticles may be dissolved / suspended in a first solvent to form a first solution / suspension, and the polymer may be dissolved / suspended in a second solvent to form a second solution / suspension, where the first and second solvents may be the same or different. The first and second solutions / suspensions may then be combined in step (a) to provide a mixture of nanoparticles and polymer to form nanoparticles with a polymer coating. For example, an alcohol solvent such as ethanol may be used to dissolve / suspend TiO2, SiO2 or CeO2 nanoparticles, an alkane solvent such as hexane may be used to dissolve the PDMS polymer, and the two solutions / suspensions may be combined in step (a) to form nanoparticles with a PDMS polymer coating. For other combinations of nanoparticles and polymers, different solvents may have better compatibility. For example, polyolefin polymers can be used with xylene or toluene solvents, and PVC polymers can be used with tetrahydrofuran (THF), methyl isobutyl ketone (MIBK), toluene, or a mixture of MIBK and toluene.

[0052] In step (a), the concentration of the solution / suspension of polymer coated nanoparticles formed in the solvent or solvents may be from 0.01 to 1M, suitably from 0.05 to 0.5M, suitably from 0.05 to 0.3M in terms of nanoparticles.

[0053] In some embodiments, the solution / suspension of polymer-coated nanoparticles formed in step (a) may then be spray-coated onto a substrate in step (b) using suitable spray coating equipment that may be known in the art. The solution / suspension of polymer-coated nanoparticles may then be dried, for example in air or by applying heat to the substrate, to form a superhydrophobic film.

[0054] The substrate may be pretreated with a layer of the polymer, suitably the same polymer, used in step (a) to coat the nanoparticles. For example, in step (b), the substrate may be spray-coated with a solution of the polymer, then partially dried or cured, and then spray-coated with a solution / suspension of the polymer-coated nanoparticles. This pretreatment of the substrate may improve the mechanical durability of the superhydrophobic film on the substrate and / or improve the effectiveness of the spray coating process.

[0055] In some embodiments, the spray coating of step (b) may be repeated to build a thicker superhydrophobic film and / or to improve the mechanical durability of the superhydrophobic film. The spray coating of step (b) may be repeated at least twice, suitably at least four times. Suitably, the dip coating is repeated up to 11 times, suitably up to 9 times. Suitably, the spray coating is repeated 3-9 times, suitably 4-8 times, suitably 5-7 times or 7 times.

[0056] In some embodiments, the solution / suspension of polymer-coated nanoparticles formed in step (a) can be dip-coated onto a substrate in step (b) using a suitable dip-coating device that may be known in the art. The solution / suspension of polymer-coated nanoparticles can then be dried, for example in air or by applying heat to the substrate, to form a superhydrophobic film.

[0057] Suitably, dip coating involves immersing the substrate on which the superhydrophobic film is to be formed in the solution / suspension of polymer-coated nanoparticles formed in step (a) for a set time, then withdrawing the substrate from the solution / suspension of polymer-coated nanoparticles, and then drying the substrate. The substrate may be immersed in the solution / suspension of polymer-coated nanoparticles by using an immersion speed of 1,250-1,750 mm / min, e.g., about 1,530 mm / min, an immersion time of 5-20 seconds, e.g., about 10 seconds, and a withdrawal speed of 500-750 mm / min, e.g., about 760 mm / min. This process may be repeated a sufficient number of times to provide a superhydrophobic film of a thickness suitable for a particular application. The number of repetitions required may depend on the concentration of polymer-coated nanoparticles in the suspension / solution, the temperature of the suspension / solution, the nature of the substrate, and the particular combination of nanoparticles and polymers used.

[0058] Suitably, dip coating is performed at least twice, suitably at least four times. Suitably, dip coating is repeated up to 11 times, suitably up to 9 times. Suitably, dip coating is repeated 3 to 9 times, suitably 4 to 8 times, suitably 5 to 7 times or 7 times.

[0059] The concentration of the polymer-coated nanoparticle solution / suspension used for dip coating is

[0060] The solution / suspension of polymer-coated nanoparticles used for dip-coating may be heated above room temperature to perform dip-coating. The temperature of the solution / suspension of polymer-coated nanoparticles used for dip-coating is suitably 75-100°C, suitably 80-90°C, suitably 85-87°C, particularly when using a polyolefin polymer, such as polyethylene, as the polymer coating.

[0061] Dip coating methods can advantageously provide complete coverage of the substrate and a more controllable process (eg, with respect to the thickness of the superhydrophobic film) than other application methods.

[0062] In some embodiments of the method of this third aspect, step (a) is followed by step (a2) of forming a powder of nanoparticles having a polymer coating, and step (b) comprises hot pressing the powder of nanoparticles having a polymer coating onto a substrate. Suitable hot pressing equipment for use in this method is known in the art.

[0063] In such embodiments, step (a) suitably comprises mixing the nanoparticles and the polymer in a solvent, and step (a2) comprises removing the solvent, for example by evaporation, to provide a solid of polymer-coated nanoparticles. Suitably, step (a2) comprises grinding the solid polymer-coated nanoparticles obtained from removing the solvent to provide a powder of polymer-coated nanoparticles.

[0064] In embodiments where the polymer is PVC, the solvent may be THF, MIBK or butyl acetate.

[0065] In embodiments of the method involving hot pressing, step (b) suitably comprises disposing a powder of the nanoparticles having the polymer coating on a substrate, placing the substrate and powder in a suitable hot pressing apparatus, and then applying heat and pressure to the substrate and powder to form a superhydrophobic film on the substrate.

[0066] The temperature at which the hot pressing of step (b) is carried out is suitably 150-200°C, suitably 160-190°C, suitably 170-190°C, for example about 180°C. Suitably, the hot pressing apparatus comprises an upper plate and a lower plate which are brought together to provide the required pressing. The temperature is suitably that of the upper plate of the hot pressing apparatus which contacts the powder of nanoparticles on the substrate having the polymer coating. Suitably, the lower plate is not heated during the process.

[0067] Suitably, the powder of nanoparticles with the substrate and polymer coating are hot pressed in step (b) for a time sufficient to adhere the powder to the substrate and form a superhydrophobic film comprising aggregates of nanoparticles with polymer coating. Suitably, the powder of nanoparticles with the substrate and polymer coating are hot pressed in step (b) for at least 30 seconds, suitably at least 1 minute. Suitably, the hot pressing is performed for up to 10 minutes, suitably up to 5 minutes, suitably up to 3 minutes. The hot pressing may be performed for 30 seconds to 5 minutes, suitably 1 to 3 minutes, suitably about 2 minutes.

[0068] The hot pressing method of this embodiment is particularly suitable for forming superhydrophobic films on nanoparticles coated with PVC, especially on PVC substrates. Such PVC substrates have been difficult to reliably coat with superhydrophobic films using known methods. The ability of the method of this third aspect of the present invention to coat PVC substrates with superhydrophobic films may enable a wider range of industrial applications, such as, for example, fabrics, vehicle interiors, piping, sheets, electric cable insulation and housings (profiles) and flooring, compared to known methods.

[0069] Formation of superhydrophobic films with PVC-coated nanoparticles using spray or dip coating can result in film cracking during removal of solvent from the film. This can be avoided by using the hot press method. The hot press method can also offer reduced solvent usage, with associated cost and environmental benefits. Although a solvent is used in the preparation of the polymer-coated nanoparticles, this solvent can be captured and recycled as it is removed from the solution / suspension. Solvent capture at this stage is much more technically feasible than capturing evaporated solvent from a substrate coated with a polymer-coated nanoparticle solution / suspension, for example, by dip or spray coating, where excess solvent is likely to evaporate into the atmosphere. Thus, there is an overall potential reduction in solvent usage / waste with the hot press method.

[0070] According to a fourth aspect of the present invention, there is provided a formulation for coating an article with a superhydrophobic film, the formulation comprising nanoparticles having a polymeric coating.

[0071] In some embodiments, the formulation comprises a diluent. Suitably, the diluent is a solvent. Thus, in some embodiments, the formulation is a liquid.

[0072] In such embodiments, the concentration of the formulation with respect to the nanoparticles may be from 0.01 to 1M, suitably from 0.05 to 0.5M, suitably from 0.05 to 0.3M.

[0073] The formulation may have any of the suitable features and advantages of the solution / suspension of nanoparticles with a polymer coating as described in relation to the third aspect. The nanoparticles and polymer may have any of the suitable features and advantages of the nanoparticles and polymer as described in relation to the first, second and third aspects.

[0074] The formulation of this fourth aspect may be a ready-to-use formulation that can be used in a suitable coating method, such as spray coating or dip coating, to form a superhydrophobic film on a substrate. Suitably, the formulation is provided in a sealed container.

[0075] The formulation of this fourth aspect provides a convenient and versatile formulation for forming a durable superhydrophobic film on a variety of substrates, and can provide the substrate with the functional benefits that such a superhydrophobic film provides. Suitably, the nanoparticles, polymer and solvent are selected from the options described herein to provide a stable formulation effective to form a superhydrophobic film when applied to the substrate using a suitable method.

[0076] In some embodiments, the formulation is a solid, suitably a powder, comprising nanoparticles with a polymer coating. Such a formulation may be suitable for use in a hot pressing process to form a superhydrophobic film, as described in relation to the third aspect. EXAMPLES

[0077] material Sylgard-184 (silicone elastomer, PDMS) was purchased from Ellsworth Adhesives. Multipurpose adhesive was purchased from 3M. Titanium dioxide (Aeroxide P25, 24 ± 7 nm), cerium oxide (27 ± 14 nm), triethylamine (>99%) and 1H,1H,2H,2H-perfluorooctyltriethoxysilane (98%) were purchased from Sigma-Aldrich. Hexane (HPLC grade) and ethanol (analytical reagent grade) were purchased from Fisher Scientific.

[0078] Comparative Example 1 - TiO2 / FAS film Comparative Example 1 A superhydrophobic TiO2 / FAS film was prepared as follows: TiO2 nanoparticles (0.5 g) were added to a solution of 1H,1H,2H,2H-perfluorooctyltriethoxysilane (FAS) (0.196 mmol, 0.076 ml) in ethanol (12.5 ml) and mechanically stirred for 1 h. Hexane (2 mL) and multipurpose adhesive (4 mL) were mixed together. One layer of this solution was pipetted onto a glass slide to obtain complete coverage of the film of Comparative Example 1 on the glass slide.

[0079] Comparative Example 2 - CeO2 / FAS film Comparative Example 2 A superhydrophobic CeO2 / FAS film was prepared as above using CeO2 instead of TiO2, with the additional step of adding a catalytic amount of triethylamine (7.94 mmol, 1.1 ml) to the ethanolic solution of FAS and CeO2 to promote the formation of a monolayer.

[0080] Comparative Example 3-1: 10TiO2:CeO2 / FAS film Comparative Example 3 A superhydrophobic 1:10 TiO2:CeO2 / FAS film was prepared using a 1:10 ratio of TiO2:CeO2 instead of CeO2.

[0081] Example 1 - TiO2 / PDMS film Example 1 A superhydrophobic TiO2 / PDMS film was prepared as follows: TiO2 nanoparticles (2.91 mmol, TiO2 0.23 g) were suspended in ethanol (10 ml). A base (Sylgard-184) and a curing agent (containing HSiR3 and Pt catalyst) of silicone elastomer (PDMS) (0.165 g) were dissolved in hexane (10 ml) in a mass ratio of 10:1 and mixed to completely dissolve. The resulting PDMS / hexane solution was added to the nanoparticle sol and mechanically stirred for 3 h.

[0082] Example 2 - CeO2 / PDMS film Example 2 A superhydrophobic CeO2 / PDMS film was prepared as described above, using CeO2 (0.5 g) instead of TiO2.

[0083] Example 3-1: 10TiO2:CeO2 / PDMS film Example 3 A superhydrophobic 1:10 TiO2:CeO2 / PDMS film was prepared as above using a 1:10 ratio of TiO2:CeO2 instead of TiO2.

[0084] Film formation by spray coating Films of Comparative Examples 1-3 and Examples 1-3 were formed by spray coating at 2 bar pressure using a compression pump and artist spray gun, all sprays were performed approximately 4 cm away from the surface of the substrate.

[0085] The nanoparticle sols of Comparative Examples 1 to 3 were spray coated onto a glass surface (3 layers, approximately 4 cm from the slide) and allowed to dry for 15 minutes.

[0086] The films of Examples 1-3 were formed as follows: with the temperature probe set to 50° C., a layer of PDMS (0.22 g) / hexane (10 ml) solution was spray coated onto a hot glass slide and left for 30 minutes to partially cure. The temperature probe was then set to 125° C. and the nanoparticle sol was spray coated onto the hot glass slide (2 layers, approximately 4 cm from the slide) and left for an additional 30 minutes.

[0087] UV degradation test The samples were exposed to UV radiation using a 365 nm wavelength UV lamp positioned 6.8 cm above the coated slide.

[0088] Film characterization The surface morphology of the coatings was analyzed using a scanning electron microscope (SEM) (JEOL JSM-7001F) operating at an accelerating voltage of 20 kV. The instrument had a built-in INCA X-act EDX detector. The samples were vacuum sputter coated in a thin layer of chromium to improve electrical conductivity. A transmission electron microscope (JEOL 2100F) was used at an accelerating voltage of 200 kV in both transmission (TEM) and scanning transmission (S / TEM) modes with a CEOS "CESCOR" aberration correction system. FTIR measurements were performed using a Bruker Optics Vertex70 over the range of 450-4000 cm-1. UV-Vis diffuse reflectance spectra were obtained using a Cary5000 UV-Vis-NIR spectrometer in the range of 200-600 nm. Static WCA measurements were made using a DSA100 Expert Drop Shape Analyzer using the Young-Laplace mode of operation and manual settings to record the WCA; a 6 μl water droplet was used and the WCA was averaged over five regions. The tilt angle was recorded manually by placing a water droplet on the surface, tilting the surface and recording the angle at which the droplet begins to roll; the average was taken over five regions. Water splash videos were recorded using a high speed camera with an average of four videos for each coating. A 6 μl water droplet was dispensed from a 30 gauge dispense tip positioned 20 mm above the substrate surface.

[0089] Film performance For the PDMS films of Examples 1-3, the nanoparticles were blended together and suspended in ethanol before mixing with the thermosetting PDMS polymer, as described above. A suspension was formed that required mixing before use. This resulted in the formation of a range of particle aggregates that promoted a highly rough, hierarchical surface morphology in the resulting coating. These particle aggregates dispersed well in the mixed solvent system of ethanol and hexane, requiring no pretreatment before use.

[0090] During the film preparation method, the substrate was first spray-coated with a semi-cured layer of PDMS, which provided a water-repellent base (cured during the second spray coating) that also encapsulated the functionalized nanoparticles; this approach was aimed at increasing hydrophobicity and durability (Figure 1).

[0091] Unmixed titania and ceria composite coatings were prepared along with coatings composed of various ratios of titania and ceria. A 1:10 ratio of TiO2:CeO2 was found to have the greatest repulsion to UV irradiation (maintaining WCA after 16 hours) and was further investigated. Comparative Examples 1-3 (TiO2-FAS, CeO2-FAS, and 1:10 TiO2:CeO2 / FAS films) were prepared from suspensions of particles in 99% ethanol / 1% FAS solution and placed on pre-treated glass substrates (pre-treated with a hexane / adhesive mix used to strengthen the film) using a spray coating technique.

[0092] The resulting coatings of the Examples and Comparative Examples appeared homogeneous and visually bright white or off-white, depending on whether the nanostructured coating was composed primarily of TiO2 or CeO2. Because ceria has a natural light yellow pigmentation, blending the particles with titania slightly increased the white pigmentation of the coating. UV-Vis diffuse reflectance spectroscopy was used to confirm this.

[0093] Fourier transform infrared (FTIR) was performed to analyze the surface coatings of Examples 1-3, which showed absorption peaks consistent with PDMS; -1 represents the asymmetric CH3 stretch of Si-CH3 at 1258 cm -1 indicates CH3 symmetric deformation of Si-CH3, 1065cm -1 and 1010cm -1 is due to the Si-O-Si stretching vibration, and 790 cm -1is characteristic of the Si-C stretching vibration. Furthermore, FTIR was performed on the particles modified with the self-assembled monolayer of FAS, and all the spectra were consistent with the expectations.

[0094] Figures 1a and 1b show as-received TEM images of P25 TiO2 (80:20 anatase:rutile) and CeO2 nanoparticles used for coating with measured average diameters of 23 nm and 28 nm. The TiO2 particles were primarily uniform in size and shape, whereas the CeO2 nanoparticles had a broad distribution of sizes and were irregular in shape. Initially, both particles appeared without an external coating. However, as seen in Figure 1c, an amorphous layer surrounding the particles was detected by S-TEM after PDMS coating. The external PDMS coating was measured to be approximately 7.1 nm thick. Energy dispersive X-ray spectroscopy of the TiO2-PDMS was used to further investigate the chemical composition of the coating (Figure 1d). EDS mapping was performed showing high densities of titanium, silicon and oxygen in the areas where the TiO2-PDMS particles were present.

[0095] The surface morphology was analyzed by SEM. Figure 2 shows SEM images of the top (Figures 2a and 2b, ×1,000 and ×20,000 magnification, respectively) and side (Figure 2c, ×1,500 magnification) surfaces of the PDMS modified TiO2 of Example 1. Irregular structures can be observed throughout the film, resulting in a substantially hierarchical surface roughness from particle aggregation during the sol-gel / spray-coating process. The coating is formed from a PDMS coating microstructure attached to the glass substrate, and an additional base layer of thermosetting PDMS can be seen on the SEM images. The average film thickness was estimated to be 12-16 μm, including a PDMS base layer of 4 μm and a layer of polymer-coated nanoparticles that was measured to be 8-12 μm. However, microstructures ranging up to 43 μm could be seen distributed throughout the surface, as a result of the spray technique used to coat the substrate. The EDS spectrum of the film was measured, confirming the presence of all expected elements.

[0096] The thickness of the polymer coating surrounding the TiO2 nanoparticles influenced the superhydrophobicity of the resulting films. Insufficient mass of PDMS resulted in a non-uniform coating with varying hydrophobicity due to exposure of the underlying substrate material. However, excess PDMS can cause loss of hydrophobicity due to reduced surface roughness. Thus, an optimal ratio exists between nanoparticles and PDMS, whereby maximum WCA was achieved by ensuring complete particle coverage while maintaining high surface roughness. Various relative masses of PDMS to TiO2 were examined, ranging from 10 to 70 wt% of PDMS in the TiO2 / PDMS mixture, to investigate the relationship between polymer mass and WCA. The critical mass of PDMS was established to be in the range of 30 to 40 wt%. A decrease in WCA was detected past this weight percentage, likely due to excess polymer replacing trapped air between surface protrusions, thus modifying the surface morphology and reducing the overall surface roughness.

[0097] Coating UV durability A plot of WCA under UV irradiation over time showing the change in WCA under UV irradiation is shown in Figure 3. The shape of water droplets on the composite surface after 0 and 96 hours of UV irradiation is shown for (a) Example 1 and Comparative Example 1; (b) Example 2 and Comparative Example 2; and (c) Example 3 and Comparative Example 3; (d) (1) Example 1; (2) Example 2; (3) Example 31; (4) Comparative Example 1 (0 hours and 90 minutes); (5) Comparative Example 2, and (6) Comparative Example 3.

[0098] A UV lamp (wavelength ∼365 nm) was utilized to provide exposure to UV radiation comparable to that which penetrates the Earth's atmosphere the furthest (UVA). This provided an indication of the film's repulsiveness to exposure to solar radiation. The dashed lines show the WCA of the PDMS coated samples (Examples 1-3). Initially, TiO2-PDMS (Example 1) exhibited a WCA of 164.3° (CAH = 1.5°), which showed negligible change after 96 hours of irradiation, decreasing by <1° to 163.5° (CAH = 1.8°). In contrast, Comparative Examples 1-3 (solid lines) showed a decrease in WCA upon UV light exposure, which was most evident for the films containing TiO2 (Comparative Examples 1 and 2). It is known that the primary interaction between TiO2 and PDMS is hydrogen bonding between the surface adsorbed hydroxyl groups of TiO2 and the backbone oxygen atoms of PDMS. Siloxane is a type of polymer with a very flexible backbone, and therefore the combination of high surface coverage and excellent backbone flexibility due to extensive intermolecular interactions may have inhibited the photodegradation of PDMS caused by TiO2 particles. This subsequently resulted in a pigmented coating with extreme UV resistance. The high photocatalytic activity of TiO2 was further investigated by FAS system (Comparative Examples 1-3). The inclusion of CeO2 promoted e-h+ recombination and thus reduced the photocatalytic activity. TiO2 / FAS (Comparative Example 1) underwent a photoinduced transformation from superhydrophobic (161.8°) to superhydrophilic (4.2°) immediately after 90 min of UV irradiation. This transition was also tracked using FTIR, where a decrease in the intensity of the peak representative of FAS could be seen. In contrast, the CeO2 nanostructured film (Comparative Example 2) withstood the entire period of 96 h irradiation without losing superhydrophobicity (from 166.0° to 152.5°) and showed significantly less photocatalytic activity, although an increase in water-surface adhesion was evident.

[0099] Testing a mixed phase system containing 1:10 TiO2:CeO2 / FAS (Comparative Example 3) showed an immediate loss of superhydrophobicity after 48 hours (from 166.8° to 152.5°), followed by a significant decrease in WCA at 72 and 96 hours (87.8° and 69.3°), respectively. To further enhance UV resistance, the effects of PDMS and ceria were combined in Examples 2 and 3. Initially, the films of Examples 3 and 2 exhibited WCAs of 167.6° (CAH=1.7°) and 165.1° (CAH=1.7°), respectively, exceeding that of Example 1 (Figures 3b and 3c). After 96 hours of exposure to UV irradiation, the variation in WCA was minimal, with Example 3 showing a decrease of 3° (CAH=2.5°) and CeO2 / PDMS showing a decrease of 1.5° (CAH=2°). The resulting WCA was found to be very similar to that of Example 1. The additional UV repellency provided by CeO2 was investigated in an extended study where the films were exposed to intense irradiation for up to 250 hours. This resulted in WCAs of 160° and 162° for Examples 1 and 2, respectively. In all PDMS films (Examples 1-3), the water roll-off properties were maintained even after prolonged irradiation, ensuring a functional self-cleaning surface. Furthermore, superhydrophobicity was still observed after the films were left under ambient conditions for 3 months, indicating potential usefulness in real-world applications.

[0100] Water splash The interaction of water with the PDMS composite films (Examples 1-3) was imaged using a high-speed camera (1000 frames / sec). A 6 μl water droplet was dispensed from a 27-gauge dispensing tip placed 20 mm above the substrate surface, as this was pre-determined as the height at which the droplet would carry maximum momentum. The average number of splashes was typically found to be proportional to the CA observed for any given coating, with TiO2 / PDMS (Example 1) showing an average of 11.5 splashes, CeO2 / PDMS (Example 2) showing 12 splashes, and 14 could be seen for the 1:10 TiO2:CeO2 / PDMS (Example 3). This can be explained by a broader distribution of particle sizes from the combination of two inorganic oxides used in Example 3, which resulted in an increased surface roughness leading to an increased number of bounces.

[0101] summary The example films utilize nanoparticles and hydrophobic polymers to provide high surface roughness with the water repellency properties required to provide superhydrophobic films. It includes an optimized polymer:nanoparticle ratio aimed at providing both maximized surface roughness and complete substrate coverage. The robustness of the polymer-encapsulated nanoparticles can be further enhanced by using a surface pretreatment that allows for physical bonding to the underlying substrate.

[0102] As seen in Comparative Examples 1 and 2, the use of titanium dioxide in superhydrophobic films has been limited because the photocatalytic activity of TiO2 degrades organic polymer coatings upon exposure of the surface to UV light (including sunlight). However, the polymer coatings of the examples of the present invention appear to prevent the superhydrophobic films from undergoing such degradation. Examples including CeO2 can also further attenuate this photocatalytic activity.

[0103] Examples 4-7 - Polyolefin Coating material All chemicals were purchased from Sigma-Aldrich: hexamethyldisilazane (≥99.0%), toluene (≥99.98%), xylene (≥99.83%), methylene blue (≥82.0%), high density polyethylene, polypropylene, SiO2 nanoparticles (10–20 nm) and TiO2 nanoparticles (21 nm).

[0104] SiO by HDMS 2 and TiO 2 Nanoparticle functionalization Nanoparticles (5 g) were added into a 500 ml round bottom flask containing toluene (100 ml). In a separate flask, 0.5 ml of HMDS was added to toluene (100 ml). Both mixtures were stirred for 30 minutes to ensure good dispersion. The reaction mixture was mixed to reflux at 160° C. for 24 hours with constant stirring. After the reaction was complete, the particles were isolated using toluene, centrifuged (2000 rpm for 10 minutes), and further washed with ethanol. The precipitate was dried at 100° C. for 24 hours.

[0105] Example 4 - SiO2 / PE film Polyethylene (0.1 g) was weighed into a 100 ml beaker containing xylene (70 ml). The solution was heated to 110° C. with constant stirring for 20 min. Functionalized SiO2 (amount varying according to the desired polymer coating thickness, e.g., for 1.5 nm coating, 0.3472 g SiO2; for 20 nm coating, 0.0052 g SiO2) was added and stirring was continued for 30 min to obtain a polymer coating in the range of 1-20 nm. Substrates were then dip-coated into this suspension.

[0106] Example 5 - TiO2 / PE film Polyethylene (0.1 g) was weighed into a 100 ml beaker containing xylene (70 ml). The solution was heated to 110° C. with constant stirring for 20 minutes. The functionalized TiO2 was added and the solution was kept stirring for 30 minutes. A substrate was then dip coated into the suspension.

[0107] Example 6 - SiO2 / PP film Polypropylene (0.1 g) was weighed into a 100 ml beaker containing xylene (70 ml). The solution was heated to 130° C. with constant stirring for 20 minutes. Functionalized silica (amount varied according to the desired polymer coating thickness, e.g., for 1.5 nm coating, 0.3484 g SiO2; for 2 nm coating, 0.2457 g SiO2; for 3 nm coating, 0.1453 g SiO2). Substrates were then dip-coated into this suspension.

[0108] Example 7 - SiO2 / TiO2 / PE film Polyethylene (0.1 g) was weighed into a 100 ml beaker containing xylene (60 ml). The solution was heated to 110° C. with constant stirring for 20 min. Once the polyethylene was completely dissolved, 5 ml of butanol was added slowly using a syringe. The premixed SiO2 and TiO2 nanoparticles were added to the flask and stirred at 110° C. for 10 min to remove the butanol. An additional 10 ml of xylene was added before dip coating the substrate.

[0109] result Example films 4-7 containing thermoplastic polymer coatings were prepared as described above to further illustrate the invention. In preparing these examples, different deposition techniques were used to deposit the films onto the substrates, as specific temperature ranges are required to ensure complete dissolution of the thermoplastic polymer, which is essential for uniform coverage of the substrate. Unlike thermosetting polymers, which harden upon heating, thermoplastic polymers harden upon cooling and then precipitate out of solution when the temperature drops below a certain range. To optimize the dip-coating process of the particle / thermoplastic nanosuspension, a solution of SiO2 / PE (Example 4) in xylene was used to investigate the immersion and withdrawal speeds, immersion and drying times, number of iterations, and concentration of the colloidal suspension. The optimized dip-coating process was carried out as follows:

[0110] For suspensions containing silica: 1. Thermoplastic polymer was weighed (0.1 g) and added to a 100 mL beaker containing 70 mL of xylene. 2. The solution was stirred and heated to >110°C for PE or >130°C for PP to ensure complete dissolution of the polymer. 3. To ensure solvent / nanoparticle compatibility, the surface chemistry of SiO2 was modified using HMDS (method described in the experimental report) and set up on one side. 4. Once the polymer had completely dissolved and a clear solution was obtained, an exact mass of pre-functionalized silica was added to form a suspension of nanoparticles with a known polymer coating of average thickness x (nm). 5. The suspension was stirred for approximately another 10-20 minutes while the temperature was reduced to the desired range (83-88°C for PE, or 68-70°C for PP). The solvent was marked on the beaker to ensure no evaporation losses during this period and the concentration remained accurate. 6. Optimal settings were set on the dip coater: 75 immersion speed (1530 mm / min), 10 sec immersion time, 50 withdrawal speed (760 mm / min) and 10 sec drying time. 7. The glass slide was mounted in the dip coater and x repetitions were performed. 8. The slides were left for approximately 30 minutes to allow the coating to dry.

[0111] For suspensions containing titania: Pre-functionalization with oleic acid leads to problems with the dispersibility of the particles in solution, therefore, a mixed solvent system was prepared to aid in the suspension of unfunctionalized TiO2 nanoparticles in organic solvents. 1. Thermoplastic was weighed (0.1 g) and added to a 100 mL beaker containing 60 mL of xylene. 2. Same as above. 3. Same as above. 4. Once the polymer was completely dissolved and a clear solution was obtained, 5 mL of butanol was slowly added via syringe, slow enough to ensure that the polymer did not precipitate out of solution. 5. A precise mass of unfunctionalized titania was added to form a suspension of nanoparticles with a known polymer coating of average thickness x (nm). 6. The temperature of the solution was maintained at >100° C. with stirring for approximately 10 minutes to remove most of the butanol (boiling point of butanol; 118° C.). 7. The volume of the solution was slowly increased to 70 mL to achieve the desired concentration while avoiding premature polymer precipitation. 8. Steps 5-8 above.

[0112] For superhydrophobic films based on SiO2 nanoparticles, silica surface-modified with hexamethyldisilazane (HMDS) was used to induce hydrophobic functionality and ensure solvent compatibility of the colloidal suspension. Issues related to the solvent compatibility of oleic acid-functionalized TiO2 nanoparticles were attributed to the use of a mixed solvent system of xylene and butanol (12:1 by volume) with unfunctionalized TiO2. After inducing the coating of the particles, the removal of the butanol by evaporation was carried out. The results of both fabrication methods were the same. After establishing the optimal settings of the dip-coating equipment, the relationship of the ratio between polymer and particles was investigated to achieve the highest degree of superhydrophobicity. To do this, the amount of SiO2 nanoparticles suspended in dissolved polyethylene (PE) (set concentration of 0.1 g in 70 mL of xylene) was varied. Suspensions of the nanocomposite were formulated with PE particle coatings on the nanoparticles with thicknesses ranging from 1.5 nm to 20 nm. The resulting WCA is graphically shown in Figure 4. Figure 5 shows SEM images of superhydrophobic films composed of SiO2 / PE nanocomposite with (a) 1.5 nm PE coating, (b) 2 nm PE coating, and (c) 3 nm PE coating. As shown in Figures 4 and 5, thicker polymer coatings resulted in surface pores filled with excess polymer, thus reducing the surface roughness and limiting the amount of air that can be present between the surface protrusions. This, in turn, reduced the superhydrophobicity and induced the surface attachment of water droplets. The film with 1.5 nm PE coating on the nanoparticles was found to exhibit the highest WCA (162°) due to its very rough surface morphology made from nano- and microstructures and limited area of ​​flat polymer surface.

[0113] As mentioned above, there may be an optimal temperature range for forming an example superhydrophobic film, especially with polyolefins. If the temperature drops below this, the polymer will begin to precipitate out of solution and will no longer be able to coat the particles. If the temperature rises above the desired range, the polymer coating will redissolve from the substrate and the resulting film will no longer be superhydrophobic. The optimal temperature range was determined to be 85-87°C for polyethylene. However, by limiting the extreme temperature jumps, it is possible to achieve a uniform coating between 83-88°C.

[0114] Samples of SiO2 / PE compositions (based on Example 4) with 1.5 nm, 2 nm and 3 nm thick PE coatings on the nanoparticles were used to examine the number of film formation / coating cycles ("iterations") to assess the number of coatings required to produce a superhydrophobic thin film. As seen in FIG. 6, a graph showing the relationship between WCA and number of iterations for films made from SiO2 / PE nanocomposites with 1.5 nm, 2 nm and 3 nm thick PE coatings, 7 iterations appeared to be the optimal number of cycles, resulting in the highest WCA for all films. Further iterations beyond this resulted in a decrease in WCA, likely due to a thicker coating reducing surface roughness.

[0115] FIG. 7 shows SEM images of SiO2 / PE with 1.5 nm PE coating made from (a) 6 repeats, (b) 4 repeats, and (c) 2 repeats.

[0116] Furthermore, the relationship between concentration and number of iterations was investigated to minimize the use of solvents and aid in commercial and industrial viability. This was investigated using a doubly concentrated nanosuspension (0.2 g PE / 70 ml xylene) (see Figure 8). Figure 8 shows a graph depicting the relationship between WCA and number of iterations for SiO2 / PE nanocomposites with PE coatings (0.2 g PE / 70 mL) of thickness 1.5 nm, 2 nm and 3 nm. SEM was used to examine these results. The doubly concentrated nanocomposite suspension resulted in a thick substrate coating, which caused the formation of cracks on the film surface during the drying process. The lowest WCA obtained from the SiO2 / PE (1.5 nm PE) film was after four iterations. Cracks were generated due to excess polymer from the third and fourth iterations, exposing the underlying substrate material (hydrophilic glass) and inducing surface wetting. However, when the fifth and sixth iterations were applied, the surface cracks were filled with polymer and an increased WCA was observed. See Figure 9, which shows SEM images of SiO2 / PE with 1.5 nm PE coating produced by (a) 4 replicates and (b) 6 replicates (0.2 g PE / 70 mL). Thus, changing the suspension concentration and reducing the solvent usage under these conditions resulted in some issues with film formation.

[0117] Further Examples 5-7 were prepared as above. As noted for SiO2 / PE, for both SiO2 / PP (Example 6) and TiO2 / PE (Example 5), the WCA was observed to decrease with increasing polymer content. The polypropylene had to be heated to 130°C and then reduced to 68-70°C to allow complete coating of the glass substrate.

[0118] Example polymer-coated nanoparticles 5 (TiO2 / PE) and 6 (SiO2 / PP) were prepared as described above with polymer coatings having average thicknesses of 1, 2 and 3 nm. The water contact angles of these polymer-coated nanoparticles are shown in Table 1 below. [Table 1]

[0119] These examples demonstrate that a variety of nanoparticle-polymer-solvent systems can be used to create functional superhydrophobic films, provided all three components of the nanoparticle-polymer-solvent are compatible.

[0120] Examples 8 and 9 - PVC Coating Example 8 - Spray-coated SiO2 / PVC film PVC (0.1 g) was added to the solvent (30 ml) in a round bottom flask and stirred until completely dissolved. Silica nanoparticles (0.2353 g) were added to the flask and stirred for an additional 20 min, followed by a final 2 min of sonication to ensure complete mixing. The hotplate on which the substrate was placed was set to the desired temperature and the silica / PVC mixture was spray coated onto the heated substrate until the substrate was completely coated. The hotplate temperatures for the different solvent systems were as follows: MIBK: 80° C., MIBK / toluene: 80° C., THF: 50° C.

[0121] Methyl isobutyl ketone (MIBK) is a well-known solvent used industrially to dissolve PVC in many applications. Therefore, in Example 8, the preparation was carried out using PVC dissolved in MIBK, and deposition was carried out using a spray coating technique since it does not require special conditions (heating, inert atmosphere, etc.). A colloidal suspension of HMDS-functionalized SiO2 coated with about 1.5 nm of PVC and suspended in MIBK (0.1 g / 70 ml) was spray coated onto a glass substrate previously coated with a thin layer of PVC to form the film of Example 8.

[0122] It was found that rapid evaporation of MIBK is necessary to successfully produce a superhydrophobic film from this composition. Spraying onto a cold substrate can cause the MIBK to dissolve the underlying PVC layer, which then mixes with the PVC coating on the SiO2 nanoparticles, preventing the resulting film from being superhydrophobic. Therefore, spraying onto a hot substrate (e.g., at 50°C) was found to be beneficial.

[0123] When SiO2 / PVC in MIBK was spray-coated onto a heated PVC material substrate (50°C), many iterations (~15) were required to show some degree of superhydrophobicity. However, due to MIBK having a boiling point of 116°C and low vapor pressure, using excess MIBK significantly weakened the substrate, as evaporation was still relatively slow even at 50°C.

[0124] To overcome this, we tried (i) using a mixed solvent system of MIBK and toluene, (ii) using a doubly concentrated suspension, and (iii) using a higher deposition temperature. Toluene solubilizes PVC at a much slower rate than MIBK, and therefore it was expected that the underlying substrate would be largely undissolved. Thus, a mixed solvent system (1:2 toluene:MIBK by volume) was used. Doubly concentrated suspensions of SiO2-PVC in MIBK (0.1 g / 30 ml MIBK) and SiO2-PVC in MIBK / toluene (0.1 g / 10 ml MIBK / 20 ml toluene) were prepared to limit the solvent usage and used to coat the PVC material at 80 °C. A higher deposition temperature was used to promote rapid removal of the solvent and thus keep substrate solvation to a minimum.

[0125] The resulting films were largely superhydrophobic, and the coatings appeared to physically adhere to the underlying substrate under both solvent conditions (see FIG. 10). FIG. 10 shows side-view SEM images of a PVC substrate and a SiO2 / PVC film applied to the substrate. (a) and (b) are of the PVC substrate material before coating, (c) and (d) are of the SiO2 / PVC coating made using a two-fold concentrated MIBK solution, and (e) and (f) are of the SiO2 / PVC coating made using a two-fold concentrated toluene / MIBK solution.

[0126] As shown in Figure 11, evaporation of the solvent at high temperatures caused some cracks in the film, increased water adhesion, and impaired the reproducibility of the coating. Figure 11 shows SEM images of (a) and (b) SiO2 / PVC coatings made with twice concentrated MIBK, and (c) and (d) SiO2 / PVC coatings made with twice concentrated toluene / MIBK solutions. Furthermore, the coatings made with the MIBK / toluene solvent system showed reduced robustness to a simple finger wipe test compared to the films made with MIBK alone. This was likely due to a reduction in the physical bond between the coating and the substrate.

[0127] To provide consistent superhydrophobic films, i.e., crack-free films, the MIBK solvent was replaced with tetrahydrofuran (THF), a solvent that readily dissolves PVC and has a lower boiling point and increased vapor pressure compared to MIBK. Deposition of SiO2 / PVC in THF (0.1 g / 30 mL of THF) solution at a low temperature of 40-50 °C provided films with high superhydrophobicity and significantly reduced cracking. A plasticized PVC-coated polyester fabric material (containing 40-50 wt% phthalate ester plasticizer) was also dissolved in THF and used to coat SiO2 nanoparticles. This suspension was then sprayed onto a moderately heated substrate (40-50 °C) of the same material, clearly demonstrating that this fabrication method allows the same PVC material to be used as a hydrophobic coating surrounding the substrate and particles, improving the physical repulsion of the coating.

[0128] Example 9 - Hot-pressed SiO2 / PVC / Plasticizer Film To aid in commercial and industrial viability, a solvent-free fabrication method was used to generate robust superhydrophobic films. The process involves synthesizing silica-PVC nanocomposite particles (described below), grinding them into finer particle aggregates, and hot pressing the particles into plasticized PVC material (described above) at 180 °C, as shown in Figure 12. The plasticized PVC material (here also used as the substrate) was dissolved in tetrahydrofuran (THF) and used to coat the silica particles to promote a strong physical bond between the coating and the substrate. This was intended to increase mechanical robustness. THF was initially used to synthesize the silica-PVC nanocomposite, but more environmentally friendly solvents that are compatible with both components, such as methyl isobutyl ketone (MIBK) and butyl acetate, may work in a similar manner. The solvent can be collected and recycled via evaporation / agglomeration during particle synthesis.

[0129] Plasticized PVC (40 wt% DIDP in PVC) was prepared by thoroughly mixing 0.6 g of PVC and 0.41 mL of DIDP (diisodecyl phthalate) in a crucible (total mass 1 g - individual mass of each component is based on wt%). The hotplate was heated to 180°C and the crucible was placed on the hotplate until the PVC was completely dissolved in the plasticizer to form a viscous clear liquid. The mixture was then left to cool to room temperature to obtain the plasticized PVC.

[0130] Next, PVC-coated SiO2 nanoparticles were prepared as follows: Plasticized PVC (0.1 g) was dissolved in THF (30 ml) and pre-functionalized silica nanoparticles (0.2365 g) were added to the PVC / THF solution and stirred for 30 min followed by sonication for 2 min. The solution was evaporated by heating and the silica-PVC powder was collected. The powder was ground with a pestle and mortar to break up any large agglomerates.

[0131] A hot press film formation method on a PVC substrate was used using the SiO2 / PVC / plasticizer powder composition prepared as described above. The PVC substrate was completely covered with SiO2 / PVC / plasticizer powder and placed between two pieces of foil. This sample of substrate, powder and foil layer was hot pressed at 180°C for 30 seconds using a suitable hot press apparatus. Excess powder was removed and a new layer of SiO2 / PVC / plasticizer powder was placed on the substrate. The sample was then hot pressed as described above and the process was repeated with an additional layer of SiO2 / PVC / plasticizer powder. The sample was then immediately placed in a refrigerator for 30 minutes to cool.

[0132] A scanning electron microscope (SEM) was used to image the cross-section of the applied coating. Figure 13 shows an SEM image of the side of a silica-PVC film hot pressed onto a plasticized PVC material substrate. It can be seen in Figure 13 that no separate layers are evident, and the substrate and coating film appear to be physically fused together.

[0133] Samples of this hot pressed film were subjected to optional robustness tests to evaluate mechanical durability. A weighed sample (100 g) attached to a glass support was placed coating side down and pushed 10 cm across the sandpaper, rotated 90°, and pushed another 10 cm to complete one cycle (standard sandpaper, grit no. P120). Before physical abrasion, a WCA of 156.5 ± 1° was recorded, indicating that these films were superhydrophobic. Initially, no surface adhesion of water droplets to the surface was observed, as trapped air present between the surface protrusions results in minimal contact between the hydrophobic surface and the droplet. A total of 25 cycles were performed. After 25 cycles, a decrease in the WCA was observed (149.9 ± 4°). However, water droplets were seen to bead easily when in contact with the film, even in the most visually damaged areas where the film coating appeared to be completely removed. This is likely due to the action of the underlying PVC-SiO2 / PVC layer, which was hot pressed onto the PVC substrate. Figure 14 shows images taken with a Drop Shape Analyzer of a hot pressed silica / PVC sample (Example 9) before (left) and after (right) 25 cycles of physical abrasion. Figure 15 shows the change in WCA of Example 9 (40 wt% DIDP in PVC / SiO2) over 25 cycles of abrasion.

[0134] In summary, the present invention provides a superhydrophobic film for coating a substrate. The superhydrophobic film comprises a plurality of nanoparticles bonded together to form a continuous film, each nanoparticle having a polymer coating, and the ratio of the average particle size of the nanoparticles to the average thickness of their polymer coating is between 2.5:1 and 20:1. The superhydrophobic film suitably provides a durable UV-resistant coating that maintains a high water contact angle during use. A method of preparing a superhydrophobic film on a substrate is also provided, the method comprising mixing nanoparticles with a polymer to form nanoparticles having a polymer coating, and applying the nanoparticles having the polymer coating to a substrate to form a superhydrophobic film. A formulation for coating an article with such a superhydrophobic film is also provided.

[0135] While several preferred embodiments have been shown and described, it will be understood by those skilled in the art that various changes and modifications can be made therein without departing from the scope of the invention, as defined in the appended claims.

[0136] Throughout this specification, the term "comprising" or "comprises" means including the specified components but not excluding the presence of other components. The term "consisting essentially of" or "consists essentially of" means including the specified components but excluding other components, except for materials present as impurities, unavoidable substances present as a result of the process used to provide the components, and components added for purposes other than achieving the technical effect of the invention. Typically, when referring to a composition, a composition consisting essentially of a set of components contains less than 5% by weight, typically less than 3% by weight, and more typically less than 1% by weight of non-specified components.

[0137] The words "consisting of" or "consists of" mean the inclusion of the specified components but excluding the addition of other components.

[0138] Wherever appropriate, depending on the context, use of the word "comprises" or "comprising" can also be interpreted to include or include the meaning "consists essentially of" or "consisting essentially of", and can also be interpreted to include the meaning "consists of" or "consisting of".

[0139] For the avoidance of doubt, when the amount of a component in a composition is stated in wt%, this means the weight percent of the particular component relative to the total composition referred to.

[0140] Any features described herein may be used individually or in combination with each other, where appropriate, and in particular in the combinations described in the appended claims. Optional features of each aspect or exemplary embodiment of the present invention described herein should be interpreted as applicable to any other aspect or exemplary embodiment of the present invention, where appropriate. In other words, a person skilled in the art reading this specification should consider the optional features of each exemplary embodiment of the present invention as interchangeable and combinable between different exemplary embodiments.

[0141] Attention is directed to all papers and documents relating to this application filed contemporaneously or prior to this application and open to public inspection herewith, and the contents of all such papers and documents are hereby incorporated by reference.

[0142] All of the features disclosed in the specification (including any accompanying claims, and drawings), and / or all of the steps of any method or process so disclosed, may be combined in any combination, except combinations in which at least some of such features and / or steps are mutually exclusive.

[0143] Each feature disclosed in the specification (including any accompanying claims, and drawings), unless expressly stated otherwise, may be replaced by an alternative feature serving the same, equivalent or similar purpose, and thus, unless expressly stated otherwise, each feature disclosed is only an example of a generic series of equivalent or similar features.

[0144] The invention is not limited to the details of the foregoing embodiments. The invention extends to any novel one, or any novel combination, of the features disclosed in this specification (including any accompanying claims and drawings), or to any novel one, or any novel combination of steps of any method or process so disclosed.

Claims

1. 1. A superhydrophobic film comprising an aggregate of nanoparticles having a polymer coating, comprising: The nanoparticles have a ratio of particle size to the average thickness of their polymer coating of 2.5:1 to 20:1; A superhydrophobic film, wherein the nanoparticles having a polymer coating are obtainable by a method comprising mixing the nanoparticles and the polymer in a solvent.

2. 10. The superhydrophobic film of claim 1, wherein the nanoparticles are metal oxide nanoparticles.

3. The metal oxide nanoparticles are SiO 2 , TiO 2 , CeO 2 3. The superhydrophobic film of claim 2, wherein the superhydrophobic film is selected from the group consisting of fluoro, fluorophenyl ...

4. The superhydrophobic film of any one of claims 1 to 3, wherein the nanoparticles have an average particle size of 5 to 500 nm.

5. The superhydrophobic film of any one of claims 1 to 4, wherein the polymer of the polymeric coating is selected from polydimethylsiloxane, polyethylene, polypropylene, polyvinyl chloride and mixtures thereof.

6. The superhydrophobic film of any one of claims 1 to 5, wherein the ratio of the volume of the polymer coating to the volume of the nanoparticles is from 1:1 to 1:

3.

7. The superhydrophobic film of any one of claims 1 to 6, having a water contact angle of at least 150°.

8. The superhydrophobic film of any one of claims 1 to 7, having a thickness of 50 nm to 100 μm.

9. An article comprising the superhydrophobic film according to any one of claims 1 to 8.

10. 1. A method for preparing a superhydrophobic film on a substrate, comprising: (a) mixing nanoparticles and a polymer in a solvent to form nanoparticles having a polymer coating, wherein the nanoparticles have a ratio of particle size to average thickness of their polymer coating of 2.5:1 to 20:1; (b) applying the nanoparticles having a polymer coating to a substrate to form a superhydrophobic film.

11. The method of claim 10, wherein the nanoparticles and the polymer are mixed in a volume ratio of 3:1 to 1:

5.

12. 12. The method of claim 10 or 11, wherein step (b) comprises applying the nanoparticles in a solvent having a polymer coating to a substrate.

13. 12. The method of claim 10 or 11, wherein step (a) is followed by step (a2) of forming a powder of nanoparticles having a polymer coating, and step (b) comprises hot pressing the powder of nanoparticles having a polymer coating onto a substrate.

14. A formulation for coating an article with a superhydrophobic film, comprising nanoparticles having a polymeric coating: wherein the nanoparticles have a ratio of particle size to the average thickness of their polymer coating of from 2.5:1 to 20:1; Said nanoparticles having a polymer coating may be obtained by a method comprising mixing the nanoparticles and the polymer in a solvent.

15. The formulation of claim 14, comprising the solvent.

Citation Information

Patent Citations

  • Water-repellent / oil-repellent coating film and article including the same

    JP2014080465A

  • Bi-spheric block copolymers and their applications

    JP2014513174A

  • Water-repellent coating material, water-repellent laminate material, water-repellent bag-shaped container, and method for forming water-repellent coated film

    JP2018062660A

  • Method for manufacturing high permeable and super water repellent surface on which nanoparticles coated with silicon carbide complex are arranged

    KR101362511B1

  • Durable superhydrophobic coating

    US20070009657A1