Photosensitive composition, cured product, and organic electroluminescent display device
A photosensitive composition with controlled volatile organic compounds and oxygen levels, combined with a specific manufacturing process, addresses the handling and reliability issues of organic EL devices by minimizing environmental impact and improving sealing effectiveness.
Patent Information
- Application Number
- JP2022512121
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-26
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Existing compositions for sealing organic electroluminescent (EL) devices are not industrially easy to handle and do not adequately enhance the reliability of the devices due to issues such as environmental pollution and moisture/oxygen ingress, leading to degradation.
A photosensitive composition comprising a polymerizable compound and a photopolymerization initiator, with controlled water and toluene concentrations, and a manufacturing process involving devolatilization, dehydration, and deoxidation to minimize volatile organic compounds and oxygen, ensuring the composition is easy to handle and effective in sealing organic EL elements.
The composition improves the reliability of organic EL devices by reducing environmental pollution and minimizing moisture and oxygen ingress, thereby enhancing the durability and performance of the devices.
Smart Images

Figure 0007591563000001 
Figure 0007591563000002
Abstract
Description
[Technical field]
[0001] The present invention relates to, for example, a photosensitive composition, a cured product, an organic electroluminescent display device, and a method for producing the photosensitive composition. More specifically, the present invention relates to a photosensitive composition, a cured product thereof, an organic electroluminescence display device in which an organic electroluminescence element is encapsulated with the cured product, and a method for producing the photosensitive composition for encapsulating an organic electroluminescence element. [Background technology]
[0002] Organic electroluminescence elements (hereinafter referred to as organic EL elements) have been attracting attention as elements capable of emitting light with high brightness. However, organic EL elements have the problem that they deteriorate due to oxygen and moisture, resulting in a decrease in their light-emitting properties. To solve this problem, technology to seal organic EL elements and prevent deterioration is being considered.
[0003] Patent Document 1 describes a sealant for an organic electroluminescence display element, which contains a polymerizable compound and a polymerization initiator, has a viscosity of 5 to 50 mPa s at 25°C, a surface tension of 15 to 35 mN / m at 25°C, and has a water content of 1000 ppm or less at 25°C after being left to stand for 24 hours in an environment of 25°C and 50% RH.
[0004] Patent Document 2 describes a resin composition suitable for use as an encapsulant for organic EL devices, which contains a (meth)acrylate compound (A) having an aromatic hydrocarbon skeleton, a cyclic (meth)acrylate compound (B) and a polymerization initiator (C). Here, the cyclic (meth)acrylate compound (B) is at least one (meth)acrylate compound selected from the group consisting of (meth)acrylate compounds having an aromatic hydrocarbon skeleton, which are (meth)acrylate compounds different from compound (A), (meth)acrylate compounds having an alicyclic hydrocarbon skeleton, and (meth)acrylate compounds having a heterocyclic skeleton.
[0005] Patent Document 3 describes a sealant for organic electroluminescence display elements that contains (A) an alkanediol di(meth)acrylate having 4 to 20 carbon atoms and (B) a photopolymerization initiator, and in which the amount of hydrophilic functional groups per (meth)acrylate is in the range of 4.80 to 7.60 mmol / g. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-040872 A [Patent Document 2] JP 2014-193970 A [Patent Document 3] International Publication No. 2019 / 203071 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, various compositions for encapsulating organic EL elements have been proposed so far. However, according to the findings of the present inventors, there is still room for improvement in the compositions for encapsulating organic EL elements. For example, it is preferable that a composition for sealing an organic EL device is easy to handle industrially. It would also be desirable to improve the reliability of organic EL devices by improving the compositions for encapsulating the organic EL devices.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a composition for encapsulating an organic EL element, which is easy to handle industrially and capable of improving the reliability of the organic EL element. [Means for solving the problem]
[0009] The present inventors have completed the invention provided below and have solved the above problems.
[0010] According to the present invention, A photosensitive composition comprising a polymerizable compound and a photopolymerization initiator, The water concentration in the composition is 1 ppm or more and 50 ppm or less, The toluene concentration in the composition is a, The composition was exposed to 1500 mJ / cm of light with a wavelength of 395 nm emitted from an LED lamp. 2 When the toluene concentration in the cured film obtained by irradiation is b, A photosensitive composition having ab of 50 ppm or less. is provided.
[0011] Further, according to the present invention, A cured product of the above photosensitive composition is provided.
[0012] Further, according to the present invention, An organic electroluminescence display device in which an organic electroluminescence element is sealed with the above cured product. is provided.
[0013] Further, according to the present invention, A method for producing the photosensitive composition, comprising the steps of: The method for producing a photosensitive composition includes a volatilization step of subjecting the polymerizable compound to a reduced pressure of 1000 Pa or less at 10 to 100° C. for 10 minutes or more. is provided. Effect of the Invention
[0014] According to the present invention, for example, there is provided a composition for encapsulating an organic EL device, which is industrially easy to handle and capable of increasing the reliability of the organic EL device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail.
[0016] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass."
[0017] In the description of groups (atomic groups) in this specification, when a description is made without specifying whether the group is substituted or unsubstituted, the description includes both groups having no substituents and groups having a substituent. For example, an "alkyl group" includes not only an alkyl group having no substituents (unsubstituted alkyl group) but also an alkyl group having a substituent (substituted alkyl group). In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate." In this specification, the term "polyfunctional (meth)acrylate" refers to a compound having two or more (meth)acryloyl groups in one molecule, and the term "monofunctional (meth)acrylate" refers to a compound having only one (meth)acryloyl group in one molecule. In this specification, the term "organic group" means an atomic group obtained by removing one or more hydrogen atoms from an organic compound, unless otherwise specified. For example, a "monovalent organic group" refers to an atomic group obtained by removing one hydrogen atom from any organic compound. As used herein, the term "PET" refers to polyethylene terephthalate, unless otherwise specified.
[0018] <Photosensitive composition> The photosensitive composition of the present embodiment contains a polymerizable compound and a photopolymerization initiator. The photosensitive composition of the present embodiment is preferably used for encapsulating an organic electroluminescence element, that is, the photosensitive composition of the present embodiment is preferably used for encapsulating an organic EL element to produce an organic EL display device. The dissolved oxygen concentration in the photosensitive composition of the present embodiment is preferably 0.1 mg / L or more and 20 mg / L or less. The water concentration in the photosensitive composition of this embodiment is 1 ppm or more and 50 ppm or less. The toluene concentration in the photosensitive composition of this embodiment is set to a, and the composition is exposed to light of 395 nm wavelength emitted from an LED lamp at 1500 mJ / cm 2 When the toluene concentration in the cured film obtained by irradiation is b, ab is 50 ppm or less.
[0019] The photosensitive composition of the present embodiment is less likely to pollute the environment due to its small ab. For example, in today's world where reducing VOC emissions is important, the photosensitive composition of the present embodiment, which has a small ab, can be easily handled industrially. In addition, a small ab, that is, when the composition is made into a film, a small amount of toluene is released outside the film, which means that a small amount of toluene is released during the manufacturing process of the organic EL display device, and therefore the toluene is less likely to corrode the organic EL device. In other words, by sealing an organic EL device using the photosensitive composition of the present embodiment having a small ab, the reliability of the organic EL display device can be improved. Additionally, the composition of this embodiment is a "photosensitive composition." In other words, the photosensitive composition of this embodiment is cured by irradiation with light. By sealing the organic EL element (curing the composition) with light rather than heat, it is possible to further reduce the release of toluene and other components. In other words, the composition of this embodiment is "photosensitive" and does not necessarily need to be heated for curing, which is thought to lead to less environmental pollution and improved reliability of organic EL display devices.
[0020] In the photosensitive composition of this embodiment, the moisture concentration is 1 ppm or more and 50 ppm or less, and preferably the dissolved oxygen concentration is 0.1 mg / L or more and 20 mg / L or less, which are believed to also lead to improved reliability of the organic EL display device. In the structure of an organic EL display device, an inorganic protective film with a thickness of about 1 μm is usually provided between the organic EL element and the sealing material (cured product). If a pinhole occurs in this inorganic protective film, water or oxygen may enter the organic EL element through the pinhole, which may reduce the reliability of the organic EL element. Therefore, by sealing the organic EL element with a photosensitive composition having a moisture concentration of 1 ppm or more and 50 ppm or less (preferably, a dissolved oxygen concentration of 0.1 mg / L or more and 20 mg / L or less), the reliability of the organic EL element is less likely to be impaired even if a pinhole occurs in the inorganic protective film (since there is little water or oxygen entering the organic EL element through the pinhole in the first place).
[0021] The photosensitive composition of the present embodiment is produced by selecting appropriate materials and appropriate production conditions. Examples of "appropriate materials" include (i) using a polymerizable compound with low volatility, and (ii) preparing the photosensitive composition substantially without solvent. Examples of "appropriate production conditions" include (i) separately devolatilizing the raw polymerizable compound and photopolymerization initiator, (ii) dehydrating with a molecular sieve, and (iii) deoxidizing by reducing pressure and bubbling with nitrogen gas. Details of these will be described later.
[0022] The photosensitive composition of the present embodiment will now be described in detail.
[0023] (polymerizable compound) The polymerizable compound is not particularly limited as long as it is a compound that can be polymerized by active species generated from a photopolymerization initiator described below. In the present embodiment, the polymerizable compound preferably contains a (meth)acrylate compound. The (meth)acrylate compound will be described below.
[0024] The polymerizable compound preferably contains a polyfunctional (meth)acrylate compound. By using a polyfunctional (meth)acrylate compound, the photocurability tends to be improved. The polyfunctional (meth)acrylate compound may include, for example, a difunctional to hexafunctional, specifically a difunctional to tetrafunctional (meth)acrylate compound. In terms of the balance of various performances, the polyfunctional (meth)acrylate compound preferably includes a difunctional (meth)acrylate compound, that is, a di(meth)acrylate compound.
[0025] The polymerizable compound preferably contains a polyfunctional (meth)acrylate and a monofunctional (meth)acrylate. By using the polyfunctional (meth)acrylate and the monofunctional (meth)acrylate in combination, it becomes possible to adjust the polymerization property and the physical properties of the cured film. In terms of balance of various performances, when a polyfunctional (meth)acrylate and a monofunctional (meth)acrylate are used in combination, preferably 40% by mass or more of the total polymerizable compounds, more preferably 50% by mass or more of the total polymerizable compounds are polyfunctional (meth)acrylate. Preferably 70% by mass or more of the total polymerizable compounds, more preferably 80% by mass or more of the total polymerizable compounds, most preferably 90% by mass or more of the total polymerizable compounds are polyfunctional (meth)acrylate. Preferably 100% by mass or less of the total polymerizable compounds, more preferably 95% by mass or less of the total polymerizable compounds are polyfunctional (meth)acrylate. Just to be clear, the polymerizable compound may contain only a monofunctional (meth)acrylate, so long as good performance is achieved.
[0026] Specific examples of the polyfunctional (meth)acrylate compound include the following.
[0027] The following bifunctional (meth)acrylates: bis(1-(meth)acryloxy-2-hydroxypropyl)phthalate, bis(2-(meth)acryloxyethyl)phosphate, bis((meth)acryloxy-2-hydroxypropyloxy)diethylene glycol, bisphenol A di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, bisphenol A di-(3-(meth)acryloxyethyl)ether, bisphenol A di-(3-(meth)acryloxy-2-hydroxypropyl)ether, 1,3-butanediol di(meth) Acrylate, 1,4-butanediol di-(3-(meth)acryloxy-2-hydroxypropyl) ether, 1,4-butanediol di(meth)acrylate, 1,3-butanediol bis((meth)acryloxypropionate), 1,4-butanediol bis((meth)acryloxypropionate), 2-butene-1,4-diol di(meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, diethylene glycol di(meth)acryl acrylate, 2,2-dimethyl-1,3-propanediol di(meth)acrylate, dipentaerythritol ether di(meth)acrylate, diphenolic acid di-(3-(meth)acryloxy-2-hydroxypropyl)ether, dipropylene glycol di(meth)acrylate, 7,7,9-trimethyl-3,13-dioxo-3,14-dioxa-5,12-diazahexadecane-1,16-diol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,2-ethanediol di(meth)acrylate meth)acrylate, 1,2-ethanediol bis((meth)acryloxypropionate), 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,4-phenylenedi(meth)acrylate, 1-phenyl-1,2-ethanediol di(meth)acrylate, polyoxyethyl-2,2-di(p-hydroxyphenyl)propane di(meth)acrylate, 1,2-propanediol di(meth)acrylate, 1,3-Propanediol di(meth)acrylate, propoxylated bisphenol A di(meth)acrylate, tetrabromobisphenol A di-(3-(meth)acryloxy-2-hydroxypropyl)ether, tetrachlorobisphenol A di-(3-(meth)acryloxy-2-hydroxypropyl)ether, tetraethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 2,2,4-trimethyl-1,3-pentanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate.
[0028] The following trifunctional (meth)acrylates: 1,2,4-butanetriol tri(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, polyoxypropyl trimethylolpropane tri(meth)acrylate, silicone tri(meth)acrylate, 1,3,5-tri(meth)acryloylhexahydro-s-triazine, trimethylolethane tri(meth)acrylate, 1,1,1-trimethylolpropane tri(meth)acrylate, 1,2,3-trimethylolpropane tri(meth)acrylate, 1,1,1-trimethylolpropane tris((meth)acryloxypropionate), 1,2,3-trimethylolpropane tris((meth)acryloxypropionate), tris-(2-(meth)acryloxyethyl)isocyanurate.
[0029] The following tetrafunctional (meth)acrylates: Pentaerythritol tetra(meth)acrylate, pentaerythritol tetrakis((meth)acryloxypropionate).
[0030] Specific examples of the monofunctional (meth)acrylate compound include the following.
[0031] Methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, benzyl (meth)acrylate, glycidyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, n-octyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, methoxytetraethylene glycol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(o-phenylphenoxy)ethyl (meth)acrylate.
[0032] In the volatilization step described below, from the viewpoint of leaving the polymerizable compound (not volatilizing) while sufficiently volatilizing toluene, the polymerizable compound preferably contains one that is difficult to volatilize. Specifically, the polymerizable compound preferably contains one having a molecular weight of 210 or more and 2000 or less, more preferably one having a molecular weight of 300 or more and 2000 or less, even more preferably one having a molecular weight of 300 or more and 1000 or less, and particularly preferably one having a molecular weight of 300 or more and 600 or less. That is, the photosensitive composition of this embodiment preferably contains one that fits the above molecular weight from among the above-listed (meth)acrylate compounds (particularly polyfunctional (meth)acrylates). More specifically, the photosensitive composition of this embodiment preferably contains 50% by mass or more of the polymerizable compound that fits the above molecular weight in the total polymerizable compounds. Just to be clear, even if a polymerizable compound does not fall within the above molecular weight range, its use is not excluded in this embodiment.
[0033] (Photopolymerization initiator) The photopolymerization initiator is not particularly limited as long as it is capable of polymerizing the above-mentioned polymerizable compound. The photopolymerization initiator preferably contains a photoradical polymerization initiator. Examples of the photoradical polymerization initiator include benzophenone and its derivatives, benzil and its derivatives, anthraquinone and its derivatives, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isobutyl ether, benzoin derivatives such as benzil dimethyl ketal, diethoxyacetophenone, acetophenone derivatives such as 4-tert-butyltrichloroacetophenone, 2-dimethylaminoethyl benzoate, p-dimethylaminoethyl benzoate, etc. diphenyl disulfide, thioxanthone and its derivatives, camphorquinone, 7,7-dimethyl-2,3-dioxobicyclo[2.2.1]heptane-1-carboxylic acid, 7,7-dimethyl-2,3-dioxobicyclo[2.2.1]heptane-1-carboxy-2-bromoethyl ester, 7,7-dimethyl-2,3-dioxobicyclo[2.2.1]heptane-1-carboxy-2-methyl ester, 7,7-dimethyl-2,3-dioxobicyclo[2.2.1]heptane-1-carboxylic acid chloro camphorquinone derivatives such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, α-aminoalkylphenone derivatives such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, benzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, benzoyldiethoxyphosphine oxide, 2,4,6-trimethylbenzoyldimethoxyphenylphosphine oxide, acylphosphine oxide derivatives such as 2,4,6-trimethylbenzoyldiethoxyphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; phenyl-glyoxylic acid-methyl ester; oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]-ethyl ester; and oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]-ethyl ester.
[0034] The photopolymerization initiators can be used alone or in combination of two or more. As the photopolymerization initiator, an acylphosphine oxide derivative is preferred because it can be cured only by visible light of 390 nm or more and can be cured without damaging the organic EL display element. Among the acylphosphine oxide derivatives, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide is the most preferred because it can be cured only by light of 395 nm or more without reducing the transmittance of visible light when used in an organic EL display device. Examples of 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide include "Omnirad TPO" manufactured by IGM Resins.
[0035] The content of the photopolymerization initiator is preferably 0.05 parts by mass or more and 10 parts by mass or less, more preferably 0.5 parts by mass or more and 8 parts by mass or less, still more preferably 1 part by mass or more and 5 parts by mass or less, and particularly preferably 2 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the polymerizable compound. By using an appropriate amount of the photopolymerization initiator, it is easy to ensure sufficient transparency of the encapsulant while obtaining sufficient sensitivity / curing speed.
[0036] (Other optional ingredients) The photosensitive composition of the present embodiment may or may not contain other components for adjusting performance, in addition to the polymerizable compound and the photopolymerization initiator. Other components include antioxidants, surfactants, sensitizers, etc.
[0037] It is not excluded that the photosensitive composition of this embodiment contains an organic solvent. However, from the viewpoint of making ab 50 ppm or less, it is preferable that the photosensitive composition of this embodiment does not substantially contain an organic solvent, or if it does contain an organic solvent, it contains only a small amount. Specifically, the amount of the organic solvent is preferably 5 mass % or less, more preferably 3 mass % or less, further preferably 1 mass % or less, and particularly preferably 0.1 mass % or less in the entire photosensitive composition. Ideally, the photosensitive composition of this embodiment does not substantially contain an organic solvent. Many of the organic solvents that are easily used industrially often contain toluene as an impurity, and therefore, by preparing a photosensitive composition substantially without using an organic solvent, it is easy to prepare a photosensitive composition having an ab of 50 ppm or less.
[0038] (Additional and supplementary explanations regarding various values) As described above, ab may be 50 ppm or less, but ab is preferably 30 ppm or less, and more preferably 15 ppm or less. Ideally, ab is zero, but in reality, ab is, for example, 1 ppm or more, specifically 3 ppm or more.
[0039] The value of the toluene concentration a itself is preferably 1 ppm or more and 100 ppm or less, more preferably 1 ppm or more and 80 ppm or less, and even more preferably 1 ppm or more and 50 ppm or less. The value of the toluene concentration b itself is also preferably about the same. By having the toluene concentrations a and / or b within the above numerical ranges, for example, corrosion of the organic EL element by toluene can be further suppressed, and the reliability of the organic EL display device can be further improved. For details on the method for measuring the toluene concentration a and the toluene concentration b, see the Examples given later.
[0040] As described above, the dissolved oxygen concentration in the photosensitive composition of the present embodiment is preferably 0.1 mg / L or more and 20 mg / L or less, more preferably 0.1 mg / L or more and 10 mg / L or less, and particularly preferably 0.1 mg / L or more and 5 mg / L or less. For the method of measuring the dissolved oxygen concentration, see the description in the Examples section below.
[0041] The viscosity of the photosensitive composition of the present embodiment is preferably from 3 mPa·s to 50 mPa·s, more preferably from 5 mPa·s to 30 mPa·s. This level of viscosity improves the ease of ejection when applying an inkjet method, the ease of film formation, and the like.
[0042] The change in viscosity of the photosensitive composition of this embodiment when aged at 80°C for 16 hours is preferably less than 3 mPa·s, more preferably 2 mPa·s or less, and even more preferably 1 mPa·s or less. Designing the photosensitive composition in this manner improves the storage stability of the photosensitive composition, i.e., makes it easier to handle industrially. In addition, forming a film under constant conditions makes it easier to obtain a cured film with constant properties, which is effective in improving the yield of organic EL display devices. Incidentally, the inventors have found that by mainly using methacrylate, which has lower reactivity than acrylate, as the polymerizable compound, it is easy to design the viscosity change after aging at 80°C for 16 hours to be within the above range.
[0043] The viscosity can be measured, for example, using a cone-plate viscometer (manufactured by Eiko Seiki Co., Ltd., product number: HB DV3T, etc.) under conditions of 25° C. and 200 to 250 rpm (preferably 250 rpm).
[0044] When the photosensitive composition of the present embodiment is allowed to stand at 23° C. for 16 hours, the mass loss is preferably 10% or less, more preferably 7% or less, and even more preferably 5% or less. Here, the mass loss is determined by forming a film of the photosensitive composition on alkali-free glass using an inkjet device, leaving the film at 23°C for 16 hours, and calculating based on the formula {(mass before leaving - mass after leaving) / mass before leaving} x 100 (%). The mass before leaving and the mass after leaving are determined by subtracting the mass of the alkali-free glass from the mass of "alkali-free glass + photosensitive composition with film formed thereon." For details of the measurement conditions, see the examples below.
[0045] <Method for producing photosensitive composition> The photosensitive composition of the present embodiment can be produced by using the above-mentioned components and employing an appropriate production method. Specifically, the photosensitive composition of the present embodiment can be produced through the steps of (1) devolatilization of the materials, (2) mixing of the materials, (3) dehydration, (4) deoxidation, and (5) filtration. These steps will be described below.
[0046] (1) Material devolatilization process It is preferable to thoroughly remove volatile components from some or all of the materials before mixing. By carrying out this process, it becomes easier to produce a photosensitive composition having an ab of 50 ppm or less. It is particularly preferable to remove volatile components from polymerizable compounds that are used in large amounts. The temperature during devolatilization is preferably about 10°C or higher and 100°C or lower, and more preferably about 30°C or higher and 80°C or lower. The devolatilization time is preferably 10 minutes or more, and more preferably 10 minutes or more and 60 minutes or less. The pressure during volatilization can be preferably 1000 Pa or less, and more preferably 1 Pa or more and 1000 Pa or less.
[0047] In a laboratory scale, the devolatilization treatment can be carried out, for example, by placing a stirrer in a flask, connecting a vacuum pump and a vacuum gauge, and reducing the pressure. When attempting to volatilize the volatile matter more actively by heating, it is preferable to use an oil bath. Incidentally, air bubbling (blowing air into the liquid) may be used to maintain an appropriate degree of vacuum. This is because if the concentration of oxygen, which deactivates the polymerization active species, becomes too low, the polymerizable compound may polymerize. When the devolatilization treatment is carried out on a large scale, it can be carried out, for example, in a stainless steel pressure vessel equipped with a stirrer. (2) Material mixing process The materials volatilized in the above (1) are mixed in appropriate amounts to obtain a mixture. The mixing method is not particularly limited, and the materials can be stirred using a known stirrer.
[0048] (3) Dehydration process The mixture obtained in (2) above is subjected to as much water removal as possible. The method for reducing the water content is not particularly limited, but examples thereof include the following methods. (i) A desiccant is used. The desiccant is separated by decantation or filtration after removing the moisture. The desiccant is not particularly limited as long as it does not affect the composition. Examples of the desiccant include polymer adsorbents (molecular sieves, synthetic zeolite, alumina, silica gel, etc.), inorganic salts (calcium chloride, anhydrous magnesium sulfate, quicklime, anhydrous sodium sulfate, anhydrous calcium sulfate, etc.), solid alkalis (sodium hydroxide, potassium hydroxide, etc.), etc. (ii) Heating under reduced pressure. (iii) Purifying by distillation under reduced pressure. (iv) An inert gas such as dry nitrogen or dry argon gas is blown through each component. (v) Freeze-drying.
[0049] As a method for reducing moisture, a method using a molecular sieve is preferred from the viewpoints of simplicity and suppression of deterioration of the components.
[0050] (4) Deoxidation process The deoxygenation step can reduce the amount of dissolved oxygen in the mixture. The method for reducing dissolved oxygen is not particularly limited, and examples thereof include the following methods. (i) Exposing the mixture to reduced pressure conditions. (ii) An inert gas such as dry nitrogen or dry argon gas is bubbled through the mixture. (iii) Exposure to low oxygen concentrations.
[0051] Incidentally, the amount of dissolved oxygen may be reduced by combining two or more of the above methods. For example, the method of combining (i) and (ii) may be used, that is, the amount of dissolved oxygen in the mixture may be reduced by blowing an inert gas such as dry nitrogen or dry argon gas into the mixture under reduced pressure conditions.
[0052] (5) Filtration process The mixture obtained through the above steps (1) to (4) is filtered using an appropriate filter. This allows the photosensitive composition of the present embodiment to be obtained. Although there are no particular limitations on the filter that can be used, it is preferable to use a filter with a pore size of 1 μm or less in order to obtain a photosensitive composition that meets the specifications required for sealing an organic EL device.
[0053] <Cured product, organic EL display device>
[0054] A cured product can be obtained by irradiating the photosensitive composition of the present embodiment with light. In addition, an organic EL display device can be manufactured by sealing an organic EL element with the photosensitive composition of the present embodiment.
[0055] The light source for curing the photosensitive composition is not particularly limited, and examples thereof include a halogen lamp, a metal halide lamp, a high-power metal halide lamp (containing indium, etc.), a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a xenon excimer lamp, a xenon flash lamp, and an LED.
[0056] Examples of methods for producing an organic EL display device include (i) forming a film (uncured film) of the photosensitive composition of this embodiment on the surface of a substrate on which an organic EL element is provided, and (ii) irradiating the film with light. In this way, the organic EL element can be sealed with the cured product of the photosensitive composition of this embodiment. As described above, by sealing the organic EL element with the cured product of the photosensitive composition of this embodiment, the reliability of the finally obtained organic EL display device can be improved. Incidentally, after the above (ii), an inorganic protective film such as SiN may be further provided on the surface of the cured product.
[0057] The above-mentioned film formation (i) is preferably performed by an inkjet method. In the manufacture of an organic EL display device, it is preferable to form a film by an inkjet method since it is necessary to uniformly form a film on a large-area substrate on which a plurality of organic EL elements are provided. In the film formation of (i) above, the film thickness is, for example, 1 μm to 10 μm, preferably 3 μm to 9 μm. By forming and curing a film having a thickness of 1 μm or more, it is easy to obtain a sufficient sealing ability as a sealing material. In addition, a film thickness of 10 μm or less leads to miniaturization of an organic EL display device and reduction in manufacturing costs.
[0058] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. A photosensitive composition comprising a polymerizable compound and a photopolymerization initiator, The water concentration in the composition is 1 ppm or more and 50 ppm or less, The toluene concentration in the composition is a, The composition was exposed to 1500 mJ / cm of light with a wavelength of 395 nm emitted from an LED lamp. 2 When the toluene concentration in the cured film obtained by irradiation is b, A photosensitive composition having ab of 50 ppm or less. 2. 1. The photosensitive composition according to claim 1, A photosensitive composition having a dissolved oxygen concentration of 0.1 mg / L or more and 20 mg / L or less. 3. 1. The photosensitive composition according to 1. or 2., A photosensitive composition, the change in viscosity of which when aged at 80°C for 16 hours is less than 3 mPa·s. 4. The photosensitive composition according to any one of 1. to 3., A photosensitive composition having a viscosity of 3 mPa·s or more and 50 mPa·s or less. 5. The photosensitive composition according to any one of 1. to 4., The photosensitive composition has a mass loss of 10% or less when allowed to stand at 23°C for 16 hours. 6. The photosensitive composition according to any one of 1. to 5., The toluene concentration a is 1 ppm or more and 100 ppm or less, The photosensitive composition, wherein the toluene concentration b is 1 ppm or more and 100 ppm or less. 7. The photosensitive composition according to any one of 1. to 6., The photosensitive composition contains a polymerizable compound having a molecular weight of 300 or more and 2,000 or less. 8. The photosensitive composition according to any one of 1. to 7., The photosensitive composition, wherein the polymerizable compound includes a (meth)acrylate compound. 9. The photosensitive composition according to any one of 1. to 8., A photosensitive composition for encapsulating an organic electroluminescence element. 10. A cured product of the photosensitive composition according to any one of 1. to 9. 11. 10. An organic electroluminescence display device, comprising an organic electroluminescence element encapsulated with the cured product according to claim 10. 12. A method for producing the photosensitive composition according to any one of 1. to 9., A method for producing a photosensitive composition, comprising a volatilization step of subjecting the polymerizable compound to a reduced pressure of 1,000 Pa or less at 10 to 100° C. for 10 minutes or more. EXAMPLES
[0059] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.
[0060] <Production of Photosensitive Composition> (Examples 1 to 8) Using the polymerizable compounds and photopolymerization initiators shown in the table below, photosensitive compositions of Examples 1 to 8 were produced according to the following specific procedures.
[0061] (1) Devolatilization process The polymerizable compound was subjected to devolatilization treatment under conditions of 23° C. or higher, 15 minutes or longer, and 1000 Pa or lower. (2)Mixing process The volatile polymerizable compound and photopolymerization initiator were weighed out in the amounts (unit: parts by mass) shown in the table, and stirred at 200 rpm and 23° C. for 3 hours using a stirrer (Three-One Motor), to obtain a mixture. (3) Dehydration process A dehydrating agent (molecular sieve 5A) was added in an amount of 10 mass % to the mixture obtained in (2) above, and the mixture was allowed to stand at 23° C. for 16 hours. (4) Deoxidation process The mixture that had been subjected to the above dehydration step (3) was subjected to nitrogen gas bubbling under conditions of 1000 Pa or less for 30 minutes or more. (5) Filtration process The mixture that had been subjected to the above-mentioned deoxidation step (4) was filtered through a filter having a pore size of 1 μm or less to remove foreign matter. In this manner, a photosensitive composition was produced.
[0062] Comparative Example 1 (1) A photosensitive composition was produced in the same manner as in Example 2, except that the devolatilization step was not carried out.
[0063] Comparative Example 2 (3) A photosensitive composition was produced in the same manner as in Example 1, except that the dehydration step was not carried out.
[0064] Comparative Example 3 Photosensitive compositions were produced in the same manner as in Examples 1 to 8, except that the type and amount of the polymerizable compound were changed as shown in the table.
[0065] For reference, the sources of the polymerizable compounds and initiators used here are listed below. SR262 (1,12-dodecanediol dimethacrylate, molecular weight 338): Arkema BPE200 (ethoxylated bisphenol A dimethacrylate (m+n=4 in the chemical formula below), molecular weight 540): Shin-Nakamura Chemical Co., Ltd.
[0066] [ka]
[0067] A-LEN-10 (ethoxylated o-phenylphenol acrylate (2-(o-phenylphenoxy)ethyl acrylate), molecular weight 268): Shin-Nakamura Chemical Co., Ltd. TMPTA (trimethylolpropane triacrylate, molecular weight 296): Osaka Organic Chemical Industry Co., Ltd. DCP (Dimethylol-tricyclodecane dimethacrylate, molecular weight 332): Shin-Nakamura Chemical Co., Ltd. ·LA (Lauryl acrylate, molecular weight 240): Osaka Organic Chemical Industry Co., Ltd. EHMA (2-ethylhexyl methacrylate, molecular weight 198): Mitsubishi Gas Chemical Company · TPO (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide): IGM Resins
[0068] <Various measurements / evaluations> (Toluene concentration in composition a) 0.200 g of the photosensitive composition was weighed out in a 20 mL measuring flask, and acetone was added up to the target mark. The flask was then shaken well to prepare a measurement sample. The measurement sample was then subjected to gas chromatography to quantify the toluene concentration. The details of the gas chromatography are as follows. ·Equipment: Agilent 7890B Col.: HP-5MS 60m x φ0.25mm x film thickness 0.25μm Col.Temp.: 40℃ for 1 min, then increase temperature to 180℃ at 20℃ / min, then increase temperature to 300℃ at 10℃ / min, and hold for 50 min. Inj.Temp.:300℃ Det.Temp.:300℃ Flow: 1mL / min x 22min, then 0.1mL / min, then 2mL / min, split 1 / 20 Inj: 1μL
[0069] (Toluene concentration in cured film b) The toluene concentration b was determined using the following procedure. (1) A photosensitive composition was applied (dropped) onto a first PET film with a 100 μm-thick spacer tape attached, and a second PET film was attached from above, thereby obtaining a sample in which the uncured photosensitive composition was sandwiched between the first PET film and the second PET film. (2) 395 nm light emitted from an LED lamp is applied to the front and back of the sample at 750 mJ / cm 2 (total 1500mJ / cm2 ) was irradiated. As a result, a cured film of the photosensitive composition was obtained. (3) The cured film was carefully peeled off from the first PET film and the second PET film. (4) 0.5 g of the cured film was cut into pieces of 5 mm square or less, placed in a screw-cap bottle, 5 mL of acetone was poured in, and ultrasonic waves were applied for 30 minutes. After that, it was left overnight and filtered through a membrane filter with a pore size of 0.45 μm to obtain a filtrate. The filtrate was subjected to gas chromatography to quantify the toluene concentration (the gas chromatography conditions were the same as those described above (Measurement of toluene concentration a in the composition)).
[0070] (Dissolved oxygen concentration) The dissolved oxygen concentration in the photosensitive composition was measured at 23° C. with stirring using a dissolved oxygen meter, DO meter B-506S (diaphragm type galvanic cell type) manufactured by Iijima Electronics Co., Ltd.
[0071] (Moisture concentration (moisture content)) Aquamicron AX (manufactured by Mitsubishi Chemical Corporation) was used as the Karl Fischer solution, and the measurement was performed using a trace moisture analyzer CA-06 (manufactured by Mitsubishi Chemical Corporation).
[0072] (Mass loss (volatile)) A film of the photosensitive composition was formed on the alkali-free glass using an inkjet device, and the glass was allowed to stand at 23° C. for 16 hours. The mass loss was calculated based on the formula {(mass before standing - mass after standing) / mass before standing} x 100 (%). The mass before and mass after standing in the formula were calculated by subtracting the mass of the alkali-free glass from the mass of "alkali-free glass + photosensitive composition with film formed thereon." The details are supplemented below. Inkjet device: Fujifilm, DMP2850 Inkjet conditions: Droplets were fired to a thickness of 10 μm on a 35 mm square area at 23°C. Storage conditions: Open system (atmosphere), clean room (class 1000), under yellow lamp, humidity about 40%
[0073] (Viscosity and its change over time (heat stability)) The viscosity of the photosensitive composition was measured using a cone-plate type viscometer (manufactured by Eiko Seiki Co., Ltd., HB DV3T, cone plate: CPA-40Z) at 25° C. and 250 rpm. The viscosity of the photosensitive composition was measured in the same manner after aging at 80°C for 16 hours, and the heat stability was evaluated. The evaluation criteria were as follows: a viscosity change of less than 3 mPa s was rated as ◯ (no change), and a viscosity change of 3 mPa s or more was rated as × (increased viscosity).
[0074] (Reliability evaluation of organic electroluminescence display devices (organic electroluminescence reliability)) - Fabrication of OLED display elements for evaluation A 30 mm square glass substrate (700 μm thick) with an ITO electrode was washed with acetone and then isopropanol. The following compounds were then deposited in order to form thin films by vacuum deposition to obtain a substrate with a 2 mm square organic EL element consisting of an anode, hole injection layer, hole transport layer, light emitting layer, hole blocking layer, electron transport layer, electron injection layer, and cathode. The composition of each layer is as follows: Anode (ITO): 150nm / polymer Hole injection layer (polymer HIL): 60 nm Hole transport layer (α-NPD): 30nm Emitting layer (Ir(ppy)3+CBP[6%]): 30nm Hole blocking layer (BAlq): 10 nm Electron transport layer (Alq3): 30nm Electron injection layer (LiF): 0.8nm Cathode (MgAg / IZO): 10nm / 100nm
[0075] Next, the photosensitive composition was sprayed in a nitrogen atmosphere using an inkjet device (model number: DMP2850) manufactured by Fujifilm Corporation so as to cover an organic EL element of 2 mm x 2 mm, to obtain a photosensitive resin film of 10 μm in thickness. After that, in an N2 environment, an LED lamp (UV-LED LIGHT SOURCE H-4MLH200-V1 manufactured by HOYA Corporation) emitting light with a wavelength of 395 nm was used to apply an integrated light amount of 1,500 mJ / cm2 at a wavelength of 395 nm to the photosensitive film. 2 The coating was irradiated with light under the following conditions: As a result, a cured film was obtained. A mask (cover) with an opening of 10 mm x 10 mm was placed so as to cover the entire cured film obtained, and a SiN film was formed by plasma CVD. The thickness of the formed SiN (inorganic film) was about 1 μm. In this way, an organic EL device was obtained.
[0076] The obtained organic EL element was attached to a non-alkali glass (Corning Eagle XG) of 30 mm x 30 mm x 0.7 mmt using a transparent substrate-less double-sided tape of 30 mm x 30 mm x 25 μmt. In this way, an organic EL display device for evaluation was produced.
[0077] Reliability testing The organic EL display device for evaluation obtained as described above was placed in a high-temperature, high-humidity environment of 85°C and 85% RH for 500 hours. Before and after this high-temperature, high-humidity treatment, a current was passed through the organic EL display device for evaluation, and the light-emitting surface was photographed. The photographed images (before and after the high-temperature, high-humidity treatment) were analyzed using Innotek's image analysis software "Quick Grain" to determine the light-emitting area. The reduction rate (%) of the light-emitting area before and after the high-temperature, high-humidity treatment was then calculated.
[0078] Information regarding the examples and comparative examples is summarized in the table below.
[0079] [Table 1]
[0080] As shown in the above table, the ab of the photosensitive compositions of Examples 1 to 8 was 1 ppm or more and 50 ppm or less. In other words, it can be said that the photosensitive compositions of Examples 1 to 8 are less likely to pollute the environment and are easy to handle industrially. Moreover, it can be seen from the evaluation results of the rate of decrease in the light-emitting area that the reliability of the organic EL display devices produced using the photosensitive compositions of Examples 1 to 8 was better than that of the comparative example. Incidentally, a comparison of Examples 1 to 7 with Example 8 shows that there is a tendency for the reliability of the organic EL display device to be further improved by reducing the dissolved oxygen concentration in the photosensitive composition.
[0081] For reference, a comparative example will be added. Comparative Example 1: It is believed that the reliability of the organic EL display device was reduced because the photosensitive composition had a large ab (that is, because a large amount of toluene was released during sealing of the organic EL element). Comparative Example 2: It is believed that the reliability of the organic EL display device was reduced because the moisture concentration of the photosensitive composition was high. Comparative Example 3: The ab of the photosensitive composition was large. Incidentally, in Comparative Example 3, the polymerizable compound TMPTA was thickened during the volatilization treatment in the production of the photosensitive composition, so it was not possible to produce a photosensitive composition with a viscosity that could be used for inkjet printing.
[0082] This application claims priority based on Japanese Patent Application No. 2020-063227, filed on March 31, 2020, the disclosure of which is incorporated herein in its entirety.
Claims
1. A photosensitive composition comprising a polymerizable compound and a photopolymerization initiator, The moisture concentration in the composition is 1 ppm or more and 50 ppm or less, The toluene concentration in the composition is a, The composition was exposed to light of 395 nm wavelength emitted from an LED lamp at 1500 mJ / cm 2 When the toluene concentration in the cured film obtained by irradiation is b, a-b is 50 ppm or less, For sealing organic electroluminescence elements. The photosensitive composition, wherein 70% by mass or more of the total polymerizable compounds is a polyfunctional (meth)acrylate.
2. 2. The photosensitive composition of claim 1, A photosensitive composition having a dissolved oxygen concentration of 0.1 mg / L or more and 20 mg / L or less.
3. The photosensitive composition according to claim 1 or 2, A photosensitive composition, the change in viscosity of which when aged at 80° C. for 16 hours is less than 3 mPa·s.
4. The photosensitive composition according to any one of claims 1 to 3, A photosensitive composition having a viscosity of 3 mPa·s or more and 50 mPa·s or less.
5. The photosensitive composition according to any one of claims 1 to 4, The photosensitive composition has a mass loss of 10% or less when allowed to stand at 23° C. for 16 hours.
6. The photosensitive composition according to any one of claims 1 to 5, The toluene concentration a is 1 ppm or more and 100 ppm or less, The photosensitive composition, wherein the toluene concentration b is 1 ppm or more and 100 ppm or less.
7. The photosensitive composition according to any one of claims 1 to 6, The photosensitive composition contains the polymerizable compound having a molecular weight of 300 or more and 2,000 or less.
8. A cured product of the photosensitive composition according to any one of claims 1 to 7.
9. An organic electroluminescence display device, comprising an organic electroluminescence element encapsulated with the cured product according to claim 8.
Citation Information
Patent Citations
Method for producing condensed dehydration product
JP2002173465A
Sealant composition for liquid crystal display cell
JP2007219039A
Energy ray-curable resin composition and cured product of the same
JP2014193970A
Sealing agent for organic el display element and method for manufacturing the same
JP2019040872A
Composition, curable composition, production method therefor, and cured product