Warp knitted fabric for clothing
A warp-knitted fabric with specific yarn combinations and structures addresses the issues of stretchability, hygroscopicity, and durability in cellulose-based fabrics, ensuring comfort and aesthetic appeal in work and dress clothing.
Patent Information
- Application Number
- JP2022050036
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-03-25
AI Technical Summary
Existing warp-knitted fabrics containing cellulose fibers suffer from low stretchability, poor hygroscopicity, and durability issues, leading to discomfort and aesthetic problems, especially in work clothes and dress shirts, due to the use of polyurethane elastic fibers that degrade over time and require ironing to remove wrinkles.
A warp-knitted fabric using three reeds with specific yarn types and structures, including a front reed of polyester fiber with white metal oxide, a middle reed of twisted cellulose and highly crimped polyester yarn, and a back reed of polyester fiber, achieving a moisture content of 1.0 to 7.0%, elongation rate of 25 to 65%, and transparency resistance of 85 to 98%, with improved wash durability and appearance.
The fabric provides excellent stretchability, moisture absorption, and shape retention, maintaining a beautiful appearance and comfort even after multiple washes, suitable for frequently worn clothing.
Smart Images

Figure 0007592041000002 
Figure 0007592041000003 
Figure 0007592041000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a cellulose-containing warp knitted fabric which is excellent in moisture absorption, lightweight and has appropriate stretchability, while also exhibiting anti-see-through properties and shape stability. [Background technology]
[0002] In work clothes and sportswear, highly elastic knit fabrics are used so that they can move with the wearer's movements, while in dress shirts, work clothes, lab coats, etc., it is preferred to mix cellulose fibers such as cotton for comfort.
[0003] However, woven and knitted fabrics containing cellulose fibers have low stretchability, and in order to obtain high stretchability and stretch-back properties, core spun yarns or covering yarns with spandex in the core are often used, or spandex is interwoven. For example, Patent Document 1 proposes a knitted fabric in which a yarn made of cellulose long fibers is used as the ground yarn, a yarn made of hydrophobic fibers is used as the face yarn, and a yarn made of elastic yarn, hydrophobic fiber, plant fiber, or functional fiber is used as the inlay yarn, and these face yarns and ground yarns are plated together.
[0004] However, when polyurethane-based elastic fibers having high stretchability are mixed in, there is a problem that the knitted fabric is easily deteriorated due to deterioration over time such as photo-yellowing and hydrolysis of polyurethane, making it difficult to use in applications such as dress blouses, work clothes, and white coats, which are often used while being washed repeatedly. In addition, woven and knitted fabrics containing cellulose fibers are difficult to remove wrinkles when washed, so ironing is essential.
[0005] To solve the above problems, Patent Document 2 proposes a warp knitted fabric using a side-by-side or eccentric sheath-core type composite polyester fiber, one of which is mainly composed of polyethylene terephthalate and the other of which is mainly composed of polytrimethylene terephthalate. Patent Document 3 also proposes a warp knitted fabric in which the back yarn and front yarn are polyester fiber, and the middle yarn is made of polyester fiber composed of two or more types of polymers and conductive fiber to form an insertion knit.
[0006] The knitted fabrics in Patent Documents 2 and 3 do not use polyurethane elastic fibers, so they can provide warp knitted fabrics with stretchability at a low cost and have excellent washing durability. However, because they are made only of polyester fibers, they have poor moisture absorption properties, tend to become stuffy during work, and are inferior in comfort when worn as work clothes. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-199678 A [Patent Document 2] JP 2004-44069 A [Patent Document 3] Patent Publication No. 2022-11744 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been devised to overcome the above-mentioned problems of the conventional technology, and has as its technical object to provide a warp knitted fabric for clothing which has appropriate moisture absorption and stretchability required for uniform use, while also having excellent shape retention with excellent washing durability, and further having a good appearance quality. [Means for solving the problem]
[0009] As a result of intensive research into solving the above-mentioned problems, the inventors have discovered that the above-mentioned problems can be solved by appropriately selecting the type of yarn used and the knitting structure in a warp knitted fabric knitted with three or more reeds, and producing a warp knitted fabric that satisfies the characteristic values of weight per unit area, moisture content, weft elongation rate, and anti-see-through properties, and have thus completed the present invention.
[0010] That is, the present invention relates to the following (1) to (7). (1) A warp knitted fabric for clothing knitted with three or more reeds including a front reed, a middle reed, and a back reed, the front reed and the back reed using yarn made of polyester fiber containing 0.8 to 3.5% by mass of white metal oxide, the middle reed using a double-twisted yarn of a spun yarn containing cellulose fiber and a polyester highly crimped yarn having an elastic stretchability of 20% to 80% after hot water treatment at 90°C, the middle reed knitting an insertion weave, and the warp knitted fabric for clothing characterized in that it satisfies all of the following conditions (i) to (iv): (i) Weight per unit area is 90 to 230 g / m 2 That is, (ii) In an environment of 20°C and 85% RH, the moisture content of the knitted fabric is 1.0% to 7.0% according to JIS-L1096:2010 8.10; (iii) The elongation rate in the weft direction measured by JIS-L1096 elongation rate method B (load 14.7 N) is 25 to 65%; (iv) The anti-see-through property according to JIS-L1923:2017B method is 85 to 98%. (2) The warp knitted fabric for clothing according to (1), characterized in that a yarn obtained by twisting together a spun yarn containing cotton having a British cotton count of 40 to 120 and the polyester highly crimped yarn having no interlace entanglement and a total fineness of 33 to 90 decitex with a twist number of 10 to 300 T / m is used for a middle reed. (3) A warp knitted fabric for clothing according to (1) or (2), characterized in that the front and back reeds are of a single-needle or double-needle construction, and the underlap directions of the front and back reeds are opposite to each other. (4) A warp knitted fabric for clothing according to any one of (1) to (3), characterized in that the middle reed has an insertion structure with one or two needles. (5) A warp knitted fabric for clothing according to any one of (1) to (4), characterized in that the wash and wear property after 10 washings and tumble drying according to the JIS-L1096-C4M method is 3.0 or higher. (6) The warp knitted fabric for clothing according to any one of (1) to (5), characterized in that the frictional charging voltage on the back surface measured according to JIS-L1094:2014 7.2B method is 0 to 2500 V according to JIS-L1096-C4M method after 10 washes. (7) A garment made of the warp knitted fabric for clothing according to any one of (1) to (6), the garment being selected from the group consisting of a blouse, a dress shirt, a uniform shirt, a white coat, uniform pants, and a uniform jacket. Effect of the Invention
[0011] The warp knitted fabric for clothing of the present invention has excellent stretchability and moisture absorption properties and is comfortable to wear, while also having a beautiful appearance and excellent shape retention with excellent washing durability, and therefore can be suitably used for clothing that is washed frequently, such as uniform clothing. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is an example of a knitting structure diagram showing one embodiment of the knitting structure of a back reed, a front reed and a middle reed of the warp knitted fabric of the present invention. [Diagram 2] FIG. 2 is a knitting structure diagram showing one embodiment of the knitting structure of the back reed, front reed and middle reed of the warp knitted fabric of the embodiment. [Diagram 3] FIG. 3 is a woven fabric diagram showing the plain weave of Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The warp knitted fabric for clothing of the present invention will be described in detail below. The warp knitted fabric for clothing of the present invention is a warp knitted fabric knitted with three or more reeds including a front reed, a middle reed, and a back reed, in which yarn made of polyester fiber is used for the front and back reeds, and a twisted yarn of a spun yarn containing cellulose fiber and a polyester highly crimped yarn is used for the middle reed, and the middle reed is a warp knitted fabric formed by knitting an insertion weave.
[0014] First, a twisted yarn of spun yarn containing cellulose fiber and polyester highly crimped yarn used in the middle reed constituting the warp knitted fabric for clothing of the present invention will be described. Spun yarn containing cellulose fiber has the effect of improving comfort when worn due to the moisture absorption of cellulose, and the cellulose fiber on the back side improves the feel against the skin. Cellulose fiber is a fiber having a polymer structure of a cellulose skeleton, and examples of such fibers include natural cellulose fibers such as cotton and hemp, regenerated cellulose (including solvent-spun cellulose) such as lyocell, viscose rayon, polynosic, and high wet modulus, and semi-synthetic fibers such as cuprammonium rayon, diacetate, and triacetate. Of these, cotton is particularly preferred.
[0015] The spun yarn is made of cellulose fibers alone or is a spun yarn mainly made of cellulose fibers. Other fibers can be used in combination as long as the moisture absorption of the knitted fabric is not impaired. Here, the range in which the moisture absorption of the knitted fabric is not impaired is a range in which the moisture content of the knitted fabric does not fall below 1% in an environment of 20°C and 85% RH (relative humidity), and fibers other than cellulose fibers can be mixed in this range. Specifically, the blending ratio of cellulose fibers in the spun yarn is preferably 50 to 100% by mass, more preferably 60 to 100% by mass, and even more preferably 80 to 100% by mass. If the blending ratio of cellulose fibers is less than the above range, the moisture absorption of the entire knitted fabric decreases, making it difficult to obtain comfortable wear. In addition, from the viewpoints of moisture absorption and texture, the blending ratio of cellulose fibers in the entire knitted fabric is preferably 3 to 30% by mass, more preferably 5 to 25% by mass.
[0016] The total fineness of the spun yarn is preferably 40 to 120 English count, more preferably 50 to 100 English count, and even more preferably 55 to 85 English count. If the count is less than the above range, the yarn is too thick, and the knitted fabric using the spun yarn is heavy, making it difficult to obtain a thin and light knitted fabric. If the count exceeds the above range, the blend ratio of cellulose fiber in the knitted fabric decreases, and the wearing comfort is likely to decrease.
[0017] When the cellulose fiber is cotton, the effective fiber length of the spun yarn is preferably 30 to 45 mm. More preferably, it is 37 to 43 mm. The effective fiber length of the spun yarn can be adjusted by using extra-long staple cotton such as Supima cotton, GIZA45, GIZA92, GIZA96, Supima cotton, Xinjiang cotton, and Sea Island cotton, which has a fiber length of 35 mm or more, or by blending the extra-long staple cotton with medium-fiber cotton such as Upland cotton and Australian cotton. If the effective fiber length is less than the above range, the surface fluff of the spun yarn increases, and the fiber fluff is likely to come out on the surface of the knitted fabric after repeated washing. In addition, when the cellulose is regenerated cellulose, the cut length of the fiber is preferably 30 to 55 mm. More preferably, the cut length is 35 to 48 mm. If it is within this range, it is easy to produce the spun yarn using general cotton spinning equipment.
[0018] Examples of methods for spinning spun yarn include various methods such as ring spinning, open-end spinning, and bundling spinning (e.g., Murata Vortex Spinner). Among these, ring spinning is preferred because it is easy to produce fine spun yarn and the texture is good. Combed yarn is more preferred. In addition, before the spun yarn is spun by the various methods described above, it can be subjected to various treatments such as blending, carding, combing, drawing, and roving by general methods. When using the above cellulose fibers, first, the fiber mass of the raw cellulose fiber is opened and large impurities are removed from the raw cotton in the carding process, the fibers are separated into individual strands, impurities and short fibers are removed, and the remaining long fibers are bundled as parallel as possible to form a string (carded sliver) in the carding process, the short fibers are thoroughly removed and the remaining long fibers are bundled and formed into a string (combed sliver) in the fine carding process, the combed sliver is stretched to straighten the fibers and eliminate unevenness in thickness in the length direction, and a drawing process is performed to form a string (drawn sliver). The resulting drawn sliver is twisted to prevent the fibers from slipping off each other, and then passed through a roving process in which it is wound onto a bobbin to form a roving yarn. When using fibers other than cellulose fibers, it is preferable to add them in the carding process or the drawing process. The resulting roving yarn is spun in a spinning machine to finally produce a spun yarn (combed yarn).
[0019] The twist coefficient of the spun yarn is preferably 2.8 to 5.0. More preferably, it is 3.0 to 4.5. When the twist coefficient is in the above range, the yarn can be made to have a soft texture, relatively little fuzz, and high strength. When the twist coefficient is below the above range, the strength of the yarn is low, the productivity of the knitted fabric is reduced, and the strength of the knitted fabric may not be suitable for the intended use. When the twist coefficient exceeds the above range, the texture of the knitted fabric is likely to become hard, and there is a concern that the knitting property of the knitted fabric may be reduced. The twist coefficient K is calculated based on the following formula from the number of twists obtained according to JIS-L1095-9.15.1 A method. Twist factor K=[T] / [NE] 1 / 2 In the above formula, [T] is the number of twists (twists / 2.54 cm), and [NE] is the English cotton count.
[0020] In the present invention, the polyester highly crimped yarn to be plied with the cellulose spun yarn is a polyester-based long fiber, and is a highly crimped yarn having a stretching extension rate of 20 to 80% after hot water treatment at 90°C. If the stretching extension rate is less than the lower limit of the above range, sufficient stretchability cannot be imparted to the plied yarn with the cellulose spun yarn having low elongation. The lower limit of the stretching extension rate is preferably 25% or more, more preferably 30% or more. On the other hand, if the stretching extension rate exceeds the upper limit of the above range, poor quality and reduced productivity occur. The upper limit of the stretching extension rate is preferably 75% or less, more preferably 70% or less. The stretching extension rate can be measured based on JIS-L1013:2010 8.11 Elasticity A method. The stretching extension rate of the polyester highly crimped yarn is preferably 10% or more higher than the stretching extension rate of the polyester fiber used in the front yarn and the back yarn, and more preferably 15% or more higher. The stretch recovery rate of the highly crimped polyester yarn is 30 to 65%, and more preferably 35 to 60%. If the stretch recovery rate is below the above range, the kickback property of the yarn ply / twisted with the cellulose spun yarn is likely to deteriorate. If it exceeds the above range, the yarn quality such as fluff is likely to deteriorate. The stretch extension rate of the highly crimped polyester yarn in the warp knitted fabric for clothing of the present invention is preferably 15 to 55%, and more preferably 20 to 50%.
[0021] Highly crimped polyester yarn is obtained by subjecting polyester filaments to high crimping. The preferred crimping method is false twisting. Examples of false twisting methods include spindle false twisting, friction disk false twisting, and belt false twisting. In order to achieve high crimping, it is preferred to use spindle false twisting, which can be processed at low speed, or low-speed friction disk false twisting.
[0022] For example, when a highly crimped polyester yarn is subjected to a highly crimped process by a spindle false twist method, it is produced as follows. A highly oriented polyester yarn or an intermediately oriented yarn is set in a one-stage or two-stage false twisting machine equipped with a twisting heater and an untwisting heater, and a one-stage false twisted yarn is obtained by false twisting at a predetermined draw ratio determined by the spinning speed, a heater temperature of 180°C to 220°C, a false twist number of 2800 to 10000 T / M, and a yarn speed of 80 to 250 m / min. In order to obtain a highly crimped yarn, the false twist number, heater temperature, and yarn speed must be high enough to avoid problems such as unreleased flames, fluff, and yarn breakage during production. A suitable false twist number is 3000 to 5500 T / m, and more preferably 3500 to 4500 T / m. The heater temperature is 180°C to 230°C, and more preferably 190 to 210°C. If the false twist number and heater temperature are lower than these conditions, a highly crimped false twisted yarn cannot be obtained, and if they are higher, yarn breakage and incomplete deflagration occur, resulting in extremely poor operability. Although a deflagration heater can be used to improve knitting properties, it is better not to use a deflagration heater or to limit the treatment to a low temperature of 170°C or less in order to maintain high crimp.
[0023] In the case of friction disk false twisting, it is preferable to process the yarn under similar conditions by slowing the yarn speed to the same as spindle false twisting. The method of adjusting the false twist number in the case of friction disk false twisting includes selecting the disk configuration of the twisting body, adjusting the ratio of the disk peripheral speed to the yarn speed (so-called D / Y), and adjusting the draw ratio. Depending on the type and amount of oil applied to the highly oriented undrawn yarn, it is sufficient to appropriately adjust the yarn speed at 250 to 700 m / min and D / Y: 1.5 to 2.3 times while checking the crimp state of the finished yarn. The twist tension is 0.15 to 0.5 g / processed yarn fineness dtex, and when using an intermediate oriented yarn, it is preferable to appropriately take a draw ratio of 1.3 to 1.8 times. If the twist tension and the untwist tension are almost equal, an almost preferable false twist number can be obtained. The number of false twists can be checked by grabbing the running yarn in the twisting zone, untwisting it with a twist detector, and calculating the number of false twists per meter based on the untwisted length. The direction of the false twist may be either the S direction or the Z direction, but it is preferable to match the direction of the false twist yarn with the direction of the twist of the cellulose spun yarn.
[0024] It is preferable that polyester highly crimped yarn does not have any interlacing such as interlacing. If it does have any interlacing, it is better to keep the degree of interlacing below 50 pieces / m. If there is no interlacing, the highly crimped yarn can maintain a high stretchability. It also improves the covering of the spun yarn, and has the effect of suppressing the protrusion of the cotton yarn on the back side and fuzzing.
[0025] The polyester highly crimped yarn is preferably made of homopolymers or blend polymers such as polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, or copolymers mainly made of these. For example, polybutylene terephthalate fibers have a larger bending of the molecular chain than polyethylene terephthalate fibers, which results in excellent elasticity and flexibility. Therefore, false twist yarns made of polybutylene terephthalate fibers are preferred because they have high crimpability. In addition to polybutylene terephthalate fibers, false twist yarns made of conjugate fibers of polybutylene terephthalate and polyethylene terephthalate are also preferred. This conjugate fiber has latent crimping due to the uneven distribution of polybutylene terephthalate in the cross section of the fiber, and has crimping properties equal to or higher than those of false twist yarns made of polybutylene terephthalate fibers alone. Here, the conjugate fiber of polybutylene terephthalate and polyethylene terephthalate is a composite fiber having a cross section, for example, a side-by-side structure using both components, an eccentric core-sheath structure, etc. In this case, the cross section may be a known cross section such as a round cross section, a triangular cross section, a hollow cross section, etc. In addition, the filament crimped yarn may contain, as necessary, a matting agent such as titanium oxide, a stabilizer such as phosphoric acid, an ultraviolet absorber such as a hydroxybenzophenone derivative, a crystallization nucleating agent such as talc, a lubricant such as aerosil, an antioxidant such as a hindered phenol derivative, and other flame retardants, antistatic agents, pigments, fluorescent whitening agents, infrared absorbing agents, defoamers, etc.
[0026] The total fineness of the highly crimped polyester yarn is not particularly limited, but is preferably 15 to 120 dtex. When the fineness of the elastic fiber is within the above range, the effect of preventing the cotton yarn from protruding and the effect of increasing the stretchability are improved. On the other hand, if it is lower than 15 dtex, it is difficult to obtain sufficient stretchability. Also, if it is higher than 120 dtex, the cellulose blend ratio decreases and the wearing comfort is likely to decrease. Also, the single fiber fineness of the highly crimped polyester yarn is preferably 0.5 to 3.5 dtex.
[0027] When the polyester highly crimped yarn and the cellulose spun yarn are twisted together, the twisting direction is preferably opposite to the false twisting direction of the highly crimped yarn. More preferably, the twisting direction of the cellulose spun yarn and the false twisting direction of the highly crimped false twisted yarn are the same, and the twisting direction is opposite to those directions. The false twist textured yarn has a crimped form that is false twisted in a nearly untwisted state, but by twisting together, a twist in the opposite direction to the false twisted crimped form of the filament crimped yarn is added, so that a repulsive action of crimp occurs between the filament single yarns, and the filament easily covers the spun yarn. This has the effect of making it difficult for the spun yarn to protrude to the back side when the knitted fabric is shrunk during dyeing processing. In addition, stretchability and abrasion resistance can be improved. The number of twists in the twisting is preferably 20 to 600 T / m, more preferably 25 to 300 T / m. If the number of twists is less than the above range, there is a concern that the cotton yarn may easily protrude into the back cotton, whereas if it is more than the above range, the binding force of the highly crimped yarn becomes too strong, and the stretchability of the knitted fabric may easily decrease.
[0028] In the warp knitted fabric for clothing of the present invention, the cellulose fibers are used in the middle reed for knitting the insertion structure, so that the cellulose fibers are not easily exposed on the surface of the knitted fabric, resulting in a good appearance and improved wear resistance. As the insertion method, 00 / 11 / / , 00 / 22 / / , 00 / 33 / / , or their reverse structure is preferable. More preferably, 00 / 11 / / , 11 / 00 / / , or their reverse structure is preferable, and further, the yarn used in the middle reed is reversed to the yarn used in the front reed. This can prevent the cotton yarn from protruding to the back surface. In addition, the yarn used in the middle reed may be arranged in a full set in the middle reed, but since the purpose is to achieve a thin and lightweight fabric, it is easier to keep the basis weight within the range specified in the present invention by using 1in1out or 1in2out, etc.
[0029] The warp knitted fabric of the present invention has excellent antistatic properties because it contains cellulose fibers with a high moisture content, but antistatic yarns may be used to further enhance the antistatic function. When using antistatic yarns, it is preferable to twist the antistatic yarn with the yarn used for the middle reed. In the present invention, a composite yarn obtained by twisting a spun yarn containing cellulose fibers and a polyester highly crimped yarn is used for the middle reed, so this composite yarn may be further twisted with an antistatic yarn. However, it is preferable in terms of cost to twist the antistatic yarn at the same time as twisting the spun yarn containing cellulose fibers and the polyester highly crimped yarn. In addition, in order to impart sufficient antistatic performance to the warp knitted fabric of the present invention, it is preferable to arrange the yarn containing the antistatic yarn at a rate of 1 thread / inch or more in the wale direction. It is preferable that the antistatic yarn is one in which conductive fine particles are kneaded into the fiber, and specifically, it may be either a conductive fiber (single component system) formed of a fiber-forming resin such as polyester resin or polyamide resin (conductive resin) kneaded with a conductive material, or a conductive fiber (composite component system) formed of a conductive resin and a non-conductive resin. Examples of conductive materials include conductive carbon black; metal elements such as silver, nickel, copper, iron, and tin; and metal compounds such as copper sulfide, zinc sulfide, and copper iodide. In order to achieve excellent antistatic performance both initially and after washing, the electrical resistance of the conductive yarn is preferably 100 to 1000 Ω / cm. Examples of conductive yarns that can be used include "Curacarbo" manufactured by Kuraray Trading Co., Ltd., "Belltron" manufactured by KB Seiren Co., Ltd., "Luana" manufactured by Toray Industries, Inc., and "Emina White" manufactured by Toyobo Co., Ltd.
[0030] Next, the yarn made of polyester fiber used in the front reed and the back reed constituting the warp knitted fabric for clothing of the present invention will be described. As the yarn made of polyester fiber, yarn made of polyester fiber such as polyethylene terephthalate fiber, polybutylene terephthalate fiber, polytrimethylene terephthalate fiber, polylactic acid fiber, etc. can be used. The form of the yarn may be either filament yarn or spun yarn, but filament yarn is preferable. By using filament yarn, the flexibility and shape stability of the knitted fabric can be further improved. As the filament yarn, flat yarn (raw silk), false twisted yarn, air intertwined yarn, etc. can be used. In view of abrasion resistance, moderate stretchability, and washing durability, false twisted yarn is preferable. This false twisted yarn may be the same high crimp yarn as the yarn used in the middle reed, but it may be a false twisted yarn with a normal stretching and elongation rate. The stretching and elongation rate of this false twisted yarn is preferably 5% to 40%, more preferably 8% to 30%. If the stretching extension rate is less than the lower limit of the above range, the effect of covering the stitches by the false twist yarn is less likely to be exhibited, and it is difficult to obtain anti-see-through properties, and if it exceeds the upper limit, not only is it difficult to prevent the cellulose fibers from protruding, but the entire knitted fabric is likely to shrink significantly during dyeing and become heavy. The stretching extension rate can be measured based on JIS-L1013:2010 8.11 Elasticity Method A. Methods of false twisting include spindle false twisting, friction disk false twisting, and belt false twisting.
[0031] The fineness of the false twisted yarn is preferably 30 to 180 dtex, more preferably 50 to 110 dtex. Yarns with different finenesses within the above range may be interwoven. If the fiber fineness of the yarn used is thinner than the above range, the knitted fabric tends to have a strong sense of transparency. If it is thicker than the above range, the knitted fabric tends to be thick and bulky. In particular, the false twisted yarn has a single fiber fineness of 0.8 to 3.5 dtex and a total fineness of 30 to 110 dtex.
[0032] The polyester fiber used for the front and back reeds is added with a white metal oxide such as titanium oxide to prevent see-through. The amount added is in the range of 0.8 to 3.5% by mass. It is preferably 1.0 to 3.0% by mass, and more preferably 1.3 to 2.8% by mass. For lab coats, office blouses, dress shirts, gym clothes, etc., which are often used in white or light colors, if the amount added is less than the above range, the see-through feeling is likely to be strong, and if the amount added is more than the above range, the spinnability is extremely poor and the yarn quality such as fluff is likely to be poor. In addition, the polyester fiber may contain, as necessary, a matting agent, a stabilizer such as phosphoric acid, an ultraviolet absorber such as a hydroxybenzophenone derivative, a crystallization nucleating agent such as talc, a lubricant such as aerosil, an antioxidant such as a hindered phenol derivative, and other flame retardants, antistatic agents, pigments, fluorescent whitening agents, infrared absorbing agents, defoaming agents, etc.
[0033] The warp knitted fabric for clothing of the present invention has a basis weight of 90 to 230 g / m 2 It is necessary that the thickness is 100 to 200 g / m 2 , and more preferably 100 to 180 g / m 2 If the basis weight is less than the above range, the fabric tends to be too see-through and difficult to use for applications such as white coats and office shirts. If the basis weight exceeds the above range, the fabric becomes too heavy and comfort is likely to decrease. The warp knitted fabric for clothing of the present invention preferably has a thickness of 0.3 to 1.2 mm, more preferably 0.5 to 1.0 mm. If the thickness exceeds the above range, the fabric becomes too thick and is likely to be less suitable for applications such as uniform shirts and white coats. If the thickness is less than the above range, it is difficult to obtain anti-see-through properties.
[0034] Next, the warp knitted fabric for clothing of the present invention having the above-mentioned configuration and characteristic values is preferably configured as described below. The warp knitted fabric for clothing of the present invention is knitted by a warp knitting machine such as a tricot machine. The needle density of the machine is preferably 22 to 32 gauge / inch, more preferably 28 to 32 gauge / inch. If the needle density does not satisfy the above range, the fabric becomes highly transparent or too thick, making it difficult to use for thin uniforms.
[0035] The warp knitted fabric for clothing of the present invention is knitted with at least three reeds, a front reed, a middle reed, and a back reed. The front reed and the back reed are preferably made of a single-needle or double-needle structure. From the viewpoint of the strength and durability of the knitted fabric, it is preferable that the knit loops are mainly used as closed loops. It is particularly preferable that all the knit loops are closed loops. For example, it is preferable that either the front reed or the back reed is made of a closed loop denby, and the other is made of a closed loop plain cord. It is also preferable that the underlap directions of the front reed and the back reed are reversed. By making them reversed, the knit loops on the surface face the wale direction, so that the loop shape is regular and stable, and the surface is beautiful and the fluff of the spun yarn can be suppressed from coming to the surface. In addition, the transparency is reduced and durability against abrasion is improved.
[0036] In the present invention, the middle reed is for combining an insertion structure as an intermediate layer with the warp knitted fabric of the front reed and back reed as described above. The insertion structure is a structure that does not have loops. Since it does not have loops, cellulose fibers do not appear on the surface, and the fabric surface on the front side looks beautiful. The middle reed is preferably an insertion structure with one or two needles.
[0037] An example of a knitting structure diagram showing one embodiment of the knitting structure of the back reed, front reed, and middle reed of the warp knitted fabric of the present invention is shown in Figure 1. In Figure 1, the front reed shows a knitted structure of 1-2 / 1-0 / / . The middle reed shows a knitted structure of 0-0 / 1-1 / / . The back reed shows a knitted structure of 1-0 / 2-3. Although not shown in the figure, the yarn arrangement in the middle reed is 1 in 1 out.
[0038] That is, in Fig. 1, the middle reed knits an insertion structure, and the front and back reeds knit a knit structure. The insertion structure formed by the middle reed forms a loop structure in which the yarn used for the front reed and the yarn used for the back reed overlap each other in the knit loop, and the structure is maintained by knitting so that the yarn used for the front reed and the yarn used for the back reed sandwich the yarn used for the middle reed. In this way, by forming loops in which the yarn used for the front reed and the yarn used for the back reed overlap each other in all knit loops that make up the knitted fabric, the yarn used for the front reed and the yarn used for the back reed firmly sandwich the yarn used for the middle reed, so that the elasticity of the yarn used for the middle reed greatly contributes to the elasticity of the knitted fabric.
[0039] When obtaining the warp knitted fabric for clothing of the present invention, it is preferable to scour and dry the grey fabric knitted in the above-mentioned structure to remove excess oil and impurities, and to preset it at 170 to 190°C to stabilize the shape. Furthermore, depending on the application, fluorescent bleaching and dyeing are performed using a conventional polyester dyeing method, and the knitted fabric is shrunk and exhibits elasticity by being dyed at high temperature while being softened. Thereafter, in the finishing and final setting, it is preferable to perform finishing under conditions in which the course and wale density after finishing does not decrease by 3% or more from the wale density after dyeing. In the warp knitted fabric produced as described above, the stretching extension rate of the highly crimped yarn in the middle yarn is preferably 20 to 80%. If the stretching extension rate of the highly crimped yarn is within this range, the weft direction extension rate of the knitted fabric (JIS-L1096 extension rate method B (load 14.7N)) can be set to 25 to 65%.
[0040] The warp knitted fabric of the present invention has a moisture content of 1.0 to 7.0% in an environment of 20°C and 85% RH, and is hygroscopic, so that it can regulate the humidity inside the garment to a comfortable range even during high activity work when the humidity inside the garment is likely to become high due to insensible perspiration. If the moisture content is less than 1.0%, the hygroscopicity is low and the humidity regulation function inside the garment is likely to decrease, and if it exceeds 7.0%, fuzz will appear on the surface appearance and the appearance of the dyed product will be prone to flickering.
[0041] The warp knitted fabric of the present invention has a suitable stretchability, without causing the spun cellulose yarn to protrude or the cellulose fluff to appear on the surface, even though it uses spun yarn of cellulose fiber with low extensibility. Specifically, the extensibility in the weft direction of the warp knitted fabric of the present invention can be realized to be 25 to 65%, preferably 30% to 65%, and more preferably 35% to 65%, as measured by the JIS-L1096B method (load 14.7N). The extensibility in the warp direction is preferably smaller than that in the weft direction, and is easily tailored when it is kept at about half that in the weft direction. If the extensibility exceeds the above range, the spun cellulose yarn will easily protrude on the back surface, and the cellulose fluff will easily appear on the surface.
[0042] The warp knitted fabric of the present invention has almost no cellulose fibers on the surface and has a beautiful appearance of polyester long fibers, and is therefore suitable for clothing such as blouses, dress shirts, uniform shirts, lab coats, uniform pants, uniform jackets, etc. In addition, since no fluff of cellulose short fibers appears on the fabric surface, the fabric can be suitably used in applications where dust and the like are undesirable, such as uniforms in clean rooms and the food industry.
[0043] The warp knitted fabric of the present invention contains cellulose fibers, but is resistant to wrinkles caused by washing, and even after 10 washings according to the JIS-L1096-C4M method and tumble drying, the fabric has a wash-and-wear property (W&W property) of 3.0 or higher, preferably 3.5 or higher, and more preferably 4.0 or higher. This is believed to be because the cellulose fibers do not form knitted loops in the knitted structure, and therefore the wrinkle fixation of the cellulose fibers is unlikely to appear in the knitted fabric.
[0044] The warp knitted fabric of the present invention can achieve a frictional charging voltage on the back surface measured according to JIS-L1094:2014 7.2B method, after 10 washes according to JIS-L1096-C4M method of 2500 V or less, preferably 2000 V or less. As a result, when the warp knitted fabric of the present invention is used as clothing, static electricity generation during wearing is suppressed, making it comfortable to wear.
[0045] The warp knitted fabric of the present invention has an optimized white metal oxide content in the polyester fiber used in the front and back reeds and a optimized basis weight of the knitted fabric, and therefore meets the requirements for anti-see-through properties according to the JIS-L1923:2017B method. 8 It is possible to achieve 7~98%. EXAMPLES
[0046] The present invention will now be described in detail using examples and comparative examples, but the present invention is not limited to these examples. Modifications in these examples are within the technical scope of the present invention as long as they do not deviate from the gist of the present invention. The measurement methods for the characteristic values used in the present invention are as follows.
[0047] <Stretching and elongation rate> The elasticity was measured according to JIS-L1013:2010 8.11 Elasticity Method A. The samples were pretreated in hot water at 90°C for 20 minutes.
[0048] <Stretch recovery rate> The measurement was performed according to the method of JIS-L1013:2010 8.12. The sample was pretreated in hot water at 90°C for 20 minutes.
[0049] <Stretching and elongation rate of highly crimped yarn in knitted fabric> The warp knitted fabric was carefully disassembled along the wale, 50 cm of the ply-twisted yarn was pulled out, and 10 highly crimped yarns were taken out by untwisting them. These were measured according to JIS-L1013:2010 8.11 Elasticity Method A. The arithmetic average of the measurements of the 10 yarns was taken as the elasticity extension rate of the highly crimped yarn in the knitted fabric.
[0050] <Effective fiber length of cotton fibers> Measurement was performed in accordance with JIS-L-1019:2006 7.2.1 Fiber Length Method A (double sorter method).
[0051] <Total fineness> The apparent cotton count (English count) was measured according to the method of JIS-L1095:2010 9.4.2.
[0052] <Twist coefficient> The number of twists was measured according to JIS-L1095:2010 9.15.1 Method A, and the twist coefficient (K) was calculated using the following formula. Twist factor (K) = twists per inch (T) / √ count ('s)
[0053] <Intertwining degree> Measured according to JIS-L1013:2010 8.15.
[0054] <Thickness of knitted fabric> Measurements were performed according to the test method of JIS-L 1096:2010 8.4 A method.
[0055] <Weight of knitted fabric> Measurements were performed in accordance with the test method of JIS-L 1096:2010 8.3.
[0056] <Extension rate> The weft elongation of knitted and woven fabrics was measured using JIS-L 1096:2010 8.16.1 B method (constant load method) with a load of 14.7N.
[0057] <Moisture percentage> The moisture content of knitted or woven fabrics was measured according to JIS-L 1096:2010 8.10. The moisture content was measured under environmental conditions of 20°C and 85% RH.
[0058] <Stuffiness> Uniform shirts were made using the knitted or woven fabrics of the Examples and Comparative Examples on the front and back of the shirts, and were worn by men in their 20s. The feeling of stuffiness inside the garment was evaluated immediately after walking for 20 minutes at a speed of 800 m / min in an indoor environment of 30°C and 85% RH. If stuffiness was felt, it was rated as ×, if only a little stuffiness was felt, it was rated as △, and if no stuffiness was felt and it was comfortable, it was rated as ◯.
[0059] <Frictional charging voltage> The knitted or woven fabric was washed 10 times according to the JIS-L1096-C4M method and then dried, and the measurement was performed according to JIS-L1094:2014 7.2B method (friction charging voltage measurement method). However, the friction surface was the technical back (front reed side).
[0060] <Anti-see-through property> Evaluated according to JIS-L1923:2017 B method (instrument method).
[0061] <Surface appearance> In the JIS-L1096-C4M method, in the center of a knitted or woven fabric after 10 washes, if 20 or more cellulose fluff particles were visible on the surface of the fabric in any 2.54 cm x 2.54 cm area, the fabric was rated as "X", if one or more fluff particles were found, the fabric was rated as "△", and if no fluff was found, the fabric was rated as "O".
[0062] <Shape retention> The fabric was washed 10 times using the JIS-L1096-C4M method, then tumble dried, and the smoothness of the knitted or woven fabric appearance after washing was evaluated according to JIS-L1924:2017 8.2 a). A replica of AATCC TM124 was used to rank the fabric from 1 to 5. Three test samples were graded, and the average value was used.
[0063] <Backside protrusion> The backside of the finished knitted fabric (sinker loop side) was checked to see if the yarn used for the middle reed was protruding in a loop on the backside within an arbitrary 2.54cm x 2.54cm area, and if it was protruding, the state of protrusion was checked. A four-level evaluation was given: ◎ if it was not protruding at all, 〇 if it was slightly floating on the backside but not protruding, △ if it was protruding on the backside but not to the point of feeling uncomfortable against the skin, and × if it was protruding on the backside and felt against the skin. ◎ and 〇 were considered to be acceptable.
[0064] (Manufacture of polyester highly crimped yarns a, b, c, and d) Manufacture of polyester highly crimped yarn a Polyethylene terephthalate polymer (intrinsic viscosity 0.63 m) containing 0.5% by weight of titanium oxide (white metal oxide) 31 / kg) was melted at 295°C, and the polyester fiber was melt-extruded from a spinneret device (36 holes) with a circular cross section. After cooling and solidifying, a spinning oil was added and the yarn was wound up to obtain a highly oriented undrawn yarn of 90 decitex and 36 filaments. Then, using a low-speed friction disk type friction false twisting machine with 5 mm thick urethane disks and the number of disks was set to 1-7-1, the highly oriented undrawn yarn was false twisted under the conditions of a draw ratio of 1.58, a yarn speed of 300 m / min, a D / Y ratio of 1.8, a heater surface temperature of 200°C, and a twisting direction of Z, and the yarn was wound up without air entanglement to obtain a highly crimped yarn a of 56 decitex and 36 filaments. The stretch elongation rate of this highly crimped yarn a was 62.8%, and the stretch recovery rate was 51.3%. This highly crimped yarn a had a false twist number of 4150 T / m when measured on the machine, and did not impair handleability.
[0065] Manufacture of polyester highly crimped yarn b A drawn yarn of 84 decitex 36 filament polyethylene terephthalate long fiber with a round cross section and titanium oxide (white metal oxide) content of 0.5% by weight was prepared. The finished yarn was fed from a feed roller using a spindle false twisting machine (manufactured by Mitsubishi Heavy Industries), and false twisted at a processing speed of 100 m / min, heater temperature of 200°C, twist direction Z, and false twist number of 3900. The yarn was then wound up without interlacing to obtain highly crimped yarn b. The stretch extension rate of this highly crimped yarn b was 46.9%, and the stretch recovery rate was 38.5%.
[0066] Manufacture of polyester highly crimped yarn c A drawn yarn (elongation 30.5%) of 56 dtex 36 filament side-by-side composite fiber of polybutylene terephthalate and polyethylene terephthalate (weight ratio 50 / 50) was prepared. This drawn yarn was fed from the feed roller using a spindle false twisting machine (Mitsubishi Heavy Industries LS6) and false twisted in the twisting direction Z at a processing speed of 100 m / min, heater temperature of 190°C, and false twist number of 3800. Thereafter, it was wound up without interlacing to obtain highly crimped yarn c. The stretch elongation rate of this highly crimped yarn c was 65.4%, and the stretch recovery rate was 49.1%.
[0067] Manufacture of polyester highly crimped yarn Polyethylene terephthalate polymer (intrinsic viscosity 0.63 m) containing 0.5% by weight of titanium oxide (white metal oxide) 3 1 / kg) was melted at 295°C, and the polyester fiber was melt-extruded from a spinneret device (36 holes) with a circular cross section. After cooling and solidifying, a spinning oil was added and wound up to obtain a highly oriented undrawn yarn of 90 decitex and 36 filaments. Then, using a low-speed friction disk type friction false twisting machine with 5 mm thick urethane disks and the number of disks was set to 1-7-1, the highly oriented undrawn yarn was false twisted under the conditions of a draw ratio of 1.58, a yarn speed of 300 m / min, a D / Y ratio of 1.8, a heater surface temperature of 200°C, and a twisting direction of Z, and then air entanglement was performed and wound up to obtain a highly crimped yarn d of 56 decitex and 36 filaments. The stretch elongation rate of this highly crimped yarn d was 33.9%, and the stretch recovery rate was 38.5%. The interlace number (degree of entanglement) of this highly crimped yarn d was 55 pieces / m, and the false twist number measured on the machine was 4150 T / m.
[0068] (Manufacture of cellulose spun yarns a, b, c, and d) Manufacture of cellulose spun yarn a American Supima cotton and GIZA92 cotton were mixed in a weight ratio of 50:50 and mixed using an OHARA cotton blending machine, after which carded slivers were made using an Ishikawa Seisakusho carding machine. After being combed, the mixture was passed through a Hara Loom Works drawing frame twice to make a 210 grain / 6 yd sliver. It was then passed through a Toyota Automatic Loom Works roving frame to make a 80 grain / 15 yd roving. This roving was then subjected to a draft of approximately 40 times using a ring spinning frame to make 100% cotton spun yarn A (twist factor 3.5, Z twist, effective fiber length 38 mm) with a British cotton count of 60 (60 / 1).
[0069] Manufacture of cellulose spun yarn b A roving yarn of 50 grains / 15 yards was produced at the roving frame, and 80 / 1 spun yarn b (twist factor 3.8, Z twist, effective fiber length 38 mm) was produced in the same manner as spun yarn a, except that the draft was 32 times during fine spinning.
[0070] Manufacture of cellulose spun yarn c Ring spinning was carried out in the same manner as for spun yarn a, except that Lenzing's "Modal (registered trademark), 1.0 dtex, cut length 39 mm) was used instead of Supima cotton and GIZA92 cotton, to produce 100% rayon spun yarn c (twist coefficient 3.5, Z twist) at 60 / 1.
[0071] Manufacture of cellulose spun yarn A combed sliver was produced in the same manner as for spun yarn a, except that Australian cotton was used instead of Supima cotton and GIZA92 cotton, and a 300 grain / 6 yd sliver was made by passing it through a drawing frame twice. A 125 grain / 15 yd roving was produced at the roving frame, and a draft of 40 times was used for fine spinning to produce spun yarn d with an English count of 40 / 1 (twist factor 3.5, Z twist, effective fiber length 29 mm).
[0072] (Manufacturing of twisted yarns A, B, C, D, E, and F) Manufacturing of twisted yarn A The cellulose spun yarn a and the highly crimped yarn a were put into a plying and twisting machine and plyed at 100 T / m using an S twist to produce ply-twisted yarn A.
[0073] Manufacturing of ply-twisted yarn B Highly crimped yarn b was used instead of highly crimped yarn a, and plied with cellulose spun yarn a using an S twist at 30 T / m to produce plied yarn B.
[0074] Manufacturing of ply-twisted yarn C Cellulose spun yarn b was used instead of cellulose spun yarn a, and combined with highly crimped yarn a and twisted at 30 T / m using an S twist to produce ply-twisted yarn C.
[0075] Manufacturing of twisted yarn D The cellulose spun yarn c and the highly crimped yarn c were put into a plying and twisting machine and plyed at 100 T / m using an S twist to produce ply-twisted yarn D.
[0076] Manufacturing of twisted yarn E Highly crimped yarn d was used instead of highly crimped yarn a, and plied with cellulose spun yarn a using an S twist at 100 T / m to produce plied yarn E.
[0077] Manufacturing of ply-twisted yarn F When producing the ply-twisted yarn A, the cellulose spun yarn a, the highly crimped yarn a, and an antistatic yarn (Beltron 22T6-B31 manufactured by Kuraray) were ply-twisted at 100 T / m using an S-twist to produce the ply-twisted yarn F.
[0078] Example 1 A 28-gauge tricot knitting machine (Karl MAYER KE type) was used with three reeds to knit the following yarns in the knitting pattern shown in Figure 2, to obtain a warp-knitted fabric. Front reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 84 dtex, 72 filaments, stretch elongation rate 10.1%, stretch recovery rate 28.5%) Structure: 1-2 / 1-0 / / Middle reed: Ply-twisted yarn A Structure: 0-0 / 1-1 / / (1in1out) Back reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 56 dtex, 36 filaments, stretch elongation rate 11.1%, stretch recovery rate 29.5%) Structure: 1-0 / 2-3 / /
[0079] Next, the obtained warp knitted fabric was passed through a pre-wetter as a normal tricot dyeing process, and then refined and dried to remove excess oil and impurities, and pre-set at 180°C in width in a tenter. Furthermore, using a high-pressure dyeing machine (Circular NS manufactured by Hisaka Senshoku), it was dyed at high pressure at 130°C with fluorescent dye Hakkol STR (manufactured by Showa Chemical Industry Co., Ltd.) 1% owf), dehydrated and spread, and softener was added, and the fabric was finished by final setting at 170°C in a tenter. The density of the completed warp knitted fabric was 39 wales / inch and 62 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric of Example 1 and the evaluation results of the knitted fabric physical properties are shown in Table 1.
[0080] <Example 2> A warp knitted fabric was obtained in the same manner as in Example 1, except that the yarn usage was changed as follows. The density of the finished warp knitted fabric was 37 wales / inch and 61 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 2 and the evaluation results of the knitted fabric properties are shown in Table 1. Front reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 84 dtex, 72 filaments, stretch elongation rate 10.1%, stretch recovery rate 28.5%) Structure: 1-2 / 1-0 / / Middle reed: Double twisted yarn B Structure: 0-0 / 1-1 / / (1in1out) Back reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 84 dtex, 72 filaments, stretch elongation rate 10.1%, stretch recovery rate 28.5%) Structure: 1-0 / 2-3 / /
[0081] <Example 3> A white warp knitted fabric was obtained in the same manner as in Example 1, except that the yarn usage was changed as follows. The density of the finished warp knitted fabric was 36 wales / inch and 60 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 3 and the evaluation results of the knitted fabric physical properties are shown in Table 1. Front reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 56 dtex, 36 filaments, stretch elongation rate 11.1%, stretch recovery rate 29.5%) Structure: 1-2 / 1-0 / / Middle reed: Ply-twisted yarn C Structure: 0-0 / 1-1 / / (1in1out) Back reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 56 dtex, 36 filaments, stretch elongation rate 11.1%, stretch recovery rate 29.5%) Structure: 1-0 / 2-3 / /
[0082] <Example 4> A warp knitted fabric was obtained in the same manner as in Example 1, except that the yarn usage was changed as follows. The density of the finished warp knitted fabric was 42 wales / inch and 62 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 4 and the evaluation results of the knitted fabric properties are shown in Table 1. Front reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 56 dtex, 36 filaments, stretch elongation rate 11.1%, stretch recovery rate 29.5%) Structure: 1-0 / 2-3 / / Middle reed: Ply-twisted yarn A Structure: 0-0 / 1-1 / / (1in1out) Back reed: Commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 56 dtex, 36 filaments, stretch elongation rate 11.1%, stretch recovery rate 29.5%) Structure: 1-2 / 1-0 / /
[0083] <Example 5> A warp knitted fabric was obtained in the same manner as in Example 1, except that the middle reed was changed from double-twisted yarn A to double-twisted yarn D. The density of the finished warp knitted fabric was 41 wales / inch and 61 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 5 and the evaluation results of the knitted fabric properties are shown in Table 1.
[0084] <Example 6> A warp knitted fabric was obtained in the same manner as in Example 1, except that the middle reed was changed from double-twisted yarn A to double-twisted yarn E. The density of the finished warp knitted fabric was 36 wales / inch and 60 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 6 and the evaluation results of the knitted fabric properties are shown in Table 1.
[0085] <Example 7> A warp knitted fabric was obtained in the same manner as in Example 1, except that the yarn usage for the middle reed was changed as follows. The density of the finished warp knitted fabric was 39 wales / inch and 62 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric in Example 7 and the evaluation results of the knitted fabric properties are shown in Table 1. Middle reed: Yarn usage: Ply-twisted yarn A: Ply-twisted yarn F=11:1 Structure: 0-0 / 1-1 / / (1in1out)
[0086] Comparative Example 1 A warp knitted fabric was obtained in the same manner as in Example 2, except that the middle reed was changed from doubled and twisted yarn a to cellulose spun yarn d. The density of the resulting warp knitted fabric was 29 wales / inch and 58 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric of Comparative Example 1 and the evaluation results of the knitted fabric properties are shown in Table 1.
[0087] Comparative Example 2 A warp knitted fabric was obtained in the same manner as in Example 2, except that the middle reed was changed from the twisted yarn a to the same commercially available full-dull false twist textured yarn (friction disc 2 heater, titanium oxide (white metal oxide) content 1.5% by weight, round cross section, 84 dtex, 72 filaments, stretch elongation rate 10.1%, stretch recovery rate 28.5%) as the front and back reeds. The density of the finished warp knitted fabric was 31 wales / inch and 60 courses / inch. Details of the knitted fabric configuration of the warp knitted fabric of Comparative Example 2 and the evaluation results of the knitted fabric properties are shown in Table 1.
[0088] Comparative Example 3 A commercially available full-dull false twist yarn (friction disc 2 heater, titanium oxide (white metal oxide) 1.5% by weight content, round cross section, 84 dtex, 72 filaments, stretch elongation rate 10.1%, stretch recovery rate 28.5%) was used for the warp yarn, and a double-twisted yarn B was used for the weft yarn. A plain weave with a warp density of 100 / 2.54 cm and a weft density of 68 / 2.54 cm was woven using a Tsudakoma Industrial Co., Ltd. water jet loom. The fabric was scoured using a continuous scourer in the usual manner, cylinder dried, and then pre-set to the width using a tenter (190°C x 30 seconds), and dyed at high pressure at 130°C with a disperse dye (DIANIX Blue UN-SE 3% owf) using a high-pressure dyeing machine (Circular NS manufactured by Hisaka Sensho Co., Ltd.), dehydrated and spread, softener was added, and the final setting was performed at 170°C using a tenter to finish. The finished density was 123 warp threads / 2.54 cm and 74 weft threads / 2.54 cm. Table 1 shows the details of the fabric construction of the fabric of Comparative Example 3 and the evaluation results of the fabric properties.
[0089] [Table 1]
[0090] As can be seen from Table 1, all of Examples 1 to 7, which satisfy the requirements of the present invention, are excellent in moisture absorption (steaminess), stretchability (weft elongation), shape retention (W&W property), and appearance quality (surface appearance, back surface protrusion). Moreover, Example 6 shows that when the degree of entanglement of the highly crimped polyester yarn is high, the stretch elongation rate of the highly crimped polyester yarn decreases. Moreover, Example 7 shows that the use of an antistatic yarn (ply-twisted yarn F) in the middle reed improves antistatic properties (frictional charging voltage).
[0091] In contrast, in Comparative Example 1, the yarn used for the middle reed is made of only cellulose fiber and does not contain highly crimped polyester yarn, so it is inferior in stretchability (weft elongation rate), shape retention (W&W property), and appearance quality (surface appearance, back surface protrusion). In Comparative Example 2, the yarn used for the middle reed is made of the same polyester fiber as the front and back reeds, so it is inferior in moisture absorption (stuffiness) and stretchability (weft elongation rate). Comparative Example 3 is a woven fabric rather than a knitted fabric, so it is inferior in stretchability (weft elongation rate), shape retention (W&W property), and appearance quality (surface appearance). [Industrial Applicability]
[0092] The warp knitted fabric for clothing of the present invention has excellent stretchability and moisture absorption properties and is comfortable to wear, while also having a beautiful appearance and excellent shape retention with excellent washing durability, making it useful for clothing that is washed frequently, such as uniforms.
Claims
1. A warp knitted fabric for clothing is knitted with three or more reeds including a front reed, a middle reed, and a back reed, the front reed and the back reed using yarn made of polyester fiber containing 0.8 to 3.5% by mass of white metal oxide, the middle reed using a combined and twisted yarn of a spun yarn containing cellulose fiber and a polyester highly crimped yarn having a stretching elongation rate of 20% to 80% after hot water treatment at 90°C, the middle reed knitting an insertion weave, and the warp knitted fabric for clothing is characterized in that it satisfies all of the following conditions (i) to (iv): (i) basis weight is 90 to 230 g / m 2 That is, (ii) In an environment of 20°C and 85% RH, the moisture regain of the knitted fabric is 1.0 to 7.0% according to JIS-L1096:2010 8.10; (iii) The elongation rate in the weft direction measured by the elongation rate method B (load 14.7 N) of JIS-L1096 is 25 to 65%; (iv) The anti-see-through property according to JIS-L1923:2017B method is 87 to 98%.
2. The warp knitted fabric for clothing according to claim 1, characterized in that a yarn obtained by twisting together a spun yarn containing cotton and having a British cotton count of 40 to 120 and the polyester highly crimped yarn having no interlace entanglement and a total fineness of 33 to 90 decitex with a twist number of 10 to 300 T / m is used for the middle reed.
3. 3. The warp knitted fabric for clothing according to claim 1, wherein the front and back reeds are of a single-needle or double-needle structure, and the underlap directions of the front and back reeds are opposite to each other.
4. 4. The warp knitted fabric for clothing according to claim 1, wherein the middle reed has an insertion structure of one or two needles.
5. 5. The warp knitted fabric for clothing according to claim 1, characterized in that the wash and wear property after 10 washings and tumble drying according to JIS-L1096-C4M method is 3.0 or higher.
6. The warp knitted fabric for clothing according to any one of claims 1 to 5, characterized in that the frictional charging voltage on the back surface measured according to JIS-L1094:2014 7.2B method is 0 to 2500 V after 10 washes according to JIS-L1096-C4M method.
7. 7. An article of clothing made of the warp knitted fabric for clothing according to any one of claims 1 to 6, the article of clothing being selected from the group consisting of blouses, dress shirts, uniform shirts, white coats, uniform pants, and uniform jackets.
Citation Information
Patent Citations
Composite yarn
JP1980107534A
Warp knitted fabric and method for producing the same
JP2004044069A
Antistatic warp knit
JP2007113157A
Plied yarn
JP2009120991A
Polyester-based warp-knitted fabric and method of producing the same
JP2014034748A