Electrochemical production of uranium nitride.

An electrochemical method simplifies uranium nitride production by reducing UF6 to UN in a nitrogen-containing salt, addressing the complexity and temperature issues of current methods, enabling higher uranium-235 enrichment and improved reactor performance.

JP7592073B2Active Publication Date: 2024-11-29WESTINGHOUSE ELECTRIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022515776
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-10
Filing Date
2020-09-04
Publication Date
2024-11-29
Estimated Expiration
2040-09-04

AI Technical Summary

Technical Problem

Uranium nitride is difficult to manufacture, and the current production process is slow and complex, involving multiple steps and high temperatures.

Method used

A method involving an electrochemical process where uranium hexafluoride gas is reduced to uranium nitride in a nitrogen-containing salt at the cathode, using a porous membrane electrode, in up to two steps: UF6 → UxNy → UN, with the reaction occurring at the cathode or anode surface, and optionally in a separate chamber at elevated temperatures.

Benefits of technology

Simplifies the production process, allows higher uranium-235 enrichment, and reduces the complexity and temperature requirements, enabling higher burn-up in nuclear reactors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592073000001
    Figure 0007592073000001
  • Figure 0007592073000002
    Figure 0007592073000002
  • Figure 0007592073000003
    Figure 0007592073000003
Patent Text Reader

Abstract

This paper describes a method for producing UN from UF6 in at most two steps, including UF6 → intermediate → UN. The principle of this reaction is that in the first step, UF 6 U x N y where x is an integer selected from 1 to 3 and y is an integer selected from 1 and 2. The reduction occurs at or near the surface of a gaseous membrane electrode, which is also in contact with a nitrogen-containing salt. In the second step, U x N y The N2O2 gas and N3O4 can be separated into two separate reactors, either in the same reactor as the first step or after being transferred to a separate unit for further processing. 2 It breaks down into gas.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit of application 62 / 898,083, entitled “ELECTROCHEMICAL DIURANIZATION NITRIDE PRODUCTION,” filed on September 10, 2019, the contents of which are incorporated herein by reference.

[0002] This invention was made with Government support under Contract No. NE-0008824 awarded by the Department of Energy. The United States Government has certain rights in this invention.

[0003] This application relates to a method for producing fuel for nuclear reactors, and more particularly to a method for producing uranium nitride. [Background technology]

[0004] Uranium nitride has a higher uranium density than uranium dioxide and therefore may be a good choice as an alternative to uranium dioxide as fuel for use in nuclear reactors. The higher uranium density of uranium nitride allows a higher uranium-235-density to be achieved in the fuel compared to similarly enriched uranium dioxide, thereby allowing a higher burnup (MW-days / kgU) for a given enrichment. Uranium nitride also has higher heat conductivity and has potential as an accident tolerant fuel due to its very low residual heat content during reactor operation, preventing the expansion and rupture of fuel rods during any operating transients. Summary of the Invention [Problem to be solved by the invention]

[0005] Unfortunately, uranium nitride is difficult to produce, and the manufacturing process is time-consuming and complex, often involving multiple steps and high temperatures. Current methods follow the following product chain: UF6 → UO2 → UC → UN. [Means for solving the problem]

[0006] The following summary is provided to facilitate understanding of some of the unique and innovative features of the disclosed embodiments and is not intended to be a complete description. Various aspects of the embodiments can be obtained by taking the entire specification, claims, abstract, and drawings into account.

[0007] A method for producing uranium nitride fuel is described in which UF gas is exposed to a nitrogen-containing salt at or near the cathode to reduce uranium hexafluoride. x N y (wherein x is an integer of 1 or 2, and y is an integer of 1 to 3) is spontaneously generated in the salt or on the surface of the cathode or anode. x N y is converted to UN and nitrogen gas. x N y Whether is produced in the salt or at one of the electrodes depends on how the electrodes and salt solution are managed. For example, if multiple three-electrode configurations are placed in the salt, one set of electrodes can be tuned to produce a specific uranium fluoride product, and another set of electrodes can be tuned to produce a specific U product. x N y can be adjusted to generate

[0008] The method may be further described as including a reaction generally represented by the following steps: (1) xUF6+yN 3- →U x N y +6xF - and (2) U x Ny→xUN+(yx) / 2N2; In the formula, x is an integer selected from 1 or 2, and y is an integer selected from 1 to 3. The method reduces the reaction to produce UN to at most two steps: UF6 → intermediate → UN. The UF6 → intermediate reaction is carried out on a porous UF6 membrane electrode in contact with a nitrogen-containing salt. The intermediate → UN reaction occurs at the same porous UF6 membrane electrode or anode, or in the salt.

[0009] The nitrogen source may be an alkali or alkaline group nitride salt, or a transition metal nitride salt, for example, the salt may be any one or mixture of NaCN, KCN, NaCNO, KCNO, K2CO3, KCl, LiCl-KCl-Li3N, and LiF-NaF-KF-Li3N.

[0010] Alternatively or additionally, the nitrogen source may be by introduction of nitrogen gas into a salt, such as a neutral salt, or another solvent.

[0011] At least the first step of the present invention is carried out in an electrochemical reaction chamber comprised of a cathode and an anode, each having an end immersed in a nitrogen-containing salt. UF6 gas is introduced into the salt through the cathode, and in certain embodiments, nitrogen gas may be introduced into the salt through the anode. The salt itself may be a nitrogen salt.

[0012] The method can be carried out in a batch process or a continuous process. The second step of the method is carried out in the electrochemical reaction chamber or in a separate chamber, the separate chamber being at a temperature higher than that of the electrochemical reaction chamber and at a temperature lower than that of the U x N y is heated to a temperature high enough to decompose it into UN.

[0013] The features and advantages of the present disclosure may be better understood with reference to the accompanying figures. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram of features that may be used in an exemplary electrochemical reactor for a batch process for UxNy production.

[0015] [Diagram 2] FIG. 1 is a schematic diagram of features that may be used in an exemplary electrochemical reactor for a continuous process of UxNy production.

[0016] [Diagram 3] FIG. 1 is a schematic diagram of features that may be used in an exemplary alternative electrochemical reactor for a continuous process of UxNy production.

[0017] [Figure 4] 1 is a table showing the electromotive forces for the oxidation / reduction couples uranium(III) / uranium(0) and uranium(IV) / uranium(0) in eutectic LiCl-KCl at 450° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] As used herein, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates otherwise.

[0019] Directional terms used herein, such as, but not limited to, top, bottom, left, right, lower, upper, front, rear, and variations thereof, relate to the orientation of the elements illustrated in the accompanying figures and do not limit the scope of the claims, unless expressly stated to the contrary.

[0020] In this application, including the claims, unless otherwise indicated, all numerical values ​​expressing quantities, values, or characteristics shall be understood to be modified in all instances by the term "about". Thus, numerical values ​​may be read as if preceded by the word "about", even if the term "about" does not explicitly appear with a number. Accordingly, unless indicated to the contrary, all numerical parameters set forth in the following description may vary depending on the desired properties sought to be obtained in the compositions and methods according to the present disclosure. At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter set forth in this description should be construed, at the very least, in light of the number of reported significant digits and by applying conventional rounding techniques.

[0021] All numerical ranges recited herein are intended to include all subranges subsumed therein, for example, a range of "1 to 10" is intended to include all subranges between (and including) the recited minimum value of 1 and the recited maximum value of 10, i.e., having a minimum value of 1 or more and a maximum value of 10 or less.

[0022] A method for producing UN from UF6 in a maximum of two steps including UF6 → intermediate → UN is described herein. The reaction principle is that in the first step, UF6 converts to U x N y where x may be an integer selected from 1 and 2, and y is an integer selected from 1, 2, and 3. The reduction occurs at or near the surface of a gaseous membrane electrode that is also in contact with a nitrogen-containing salt. The UF6 → intermediate reaction is carried out on a porous UF6 membrane electrode that is in contact with a nitrogen-containing salt. A voltage is applied to the electrode, whereby UF6 is reduced to U x N y The reaction intermediate → UN occurs at the same porous UF6 membrane electrode or anode, or in a nitrogen-containing salt. In certain embodiments, the nitrogen-containing salt can contain a small amount of one or both of UF4 and UF3 sufficient to initiate the reaction, at least at the beginning of the reaction.

[0023] As used herein, "nitrogen-containing salt" shall mean (1) a salt that contains at least one nitrogen molecule bonded (covalently or ionically) to at least one other molecule in the salt composition, e.g., NaCN, KCN, NaCNO, KCNO, or (2) a salt that is not bonded (covalently or ionically) to a nitrogen molecule, but contains an unbound nitrogen molecule, e.g., N2, mixed with or dispersed within a quantity of the salt. In certain embodiments, at least at the beginning of the method, the nitrogen-containing salt may contain a small amount of one or both of UF4 and UF3 sufficient to initiate the reaction. The addition of UF4 and UF3 to the nitrogen-containing salt may be accomplished by using two sets of electrodes to measure the concentration of UF4 in the salt and the concentration of UF3 in the salt. x N y This is required in embodiments where production occurs at a second set of anodes and reduction of UF6 to UF4, UF3 and / or U-metal occurs at another set.

[0024] In various embodiments, U x N y can be one or any combination of UN2 (x is 1 and y is 2), U2N3 (x is 2 and y is 3), and UN (both x and y are 1). In various embodiments, the nitrogen used in the methods described herein is at least 95% by weight N 15 which is about 99.6% by mass N 14 It is separated prior to use in the present process by isotope separation from the naturally occurring nitrogen gas, which is

[0025] The nitrogen source may be an alkali or alkaline nitride salt, or a transition metal nitride salt. Alternatively or additionally, the nitrogen source may be by introduction of nitrogen gas into a salt, which may be a neutral salt, or into another solvent.

[0026] Exemplary alkali metals for use in the nitrogen-containing salts may be selected from Group 1 of the Periodic Table of Elements and may include Li, Na, K, Rb, Cs, and Fr. Li, Na, and K are preferred. Exemplary transition metals for use in the nitrogen-containing salts may be selected from Groups 3-12 of the Periodic Table of Elements. Many commercially available nitrogen-containing salts are known and available for use in liquid nitriding processes. For example, mixtures of NaCN, KCN, NaCNO, KCNO, K2CO3, KCl, etc. may be used. These mixtures usually have relatively low melting points, and current nitriding processes operate at about 500-600°C. Other salt mixtures such as LiCl-KCl-Li3N or LiF-NaF-KF-Li3N are also possible, which avoid cyanides. For example, LiCl-KCl melts at about 352°C. FLiNaK melts at about 454°C. The nitride component in the salt may be reconstituted by the addition of an extra nitride or another porous electrode.

[0027] In the second step, U x N y is decomposed into UN and N2 gases in the same reactor as the first step or after transfer to a separate unit for further processing.

[0028] The method may be further described as comprising reactions generally represented in the following steps: (1) xUF6+yN 3- →U x N y +6xF - and (2) U x Ny→xUN+(yx) / 2N2; In the formula, x is an integer selected from 1 or 2, and y is an integer selected from 1 to 3.

[0029] In its simplest form, the overall reaction is: UF6+2N 3- →UN2+6F - As an example, assuming FLiNaK with LiN is used as the nitrogen-containing salt, the overall exemplary reaction can be as follows: UF6+2Li3N → UN2+6LiF

[0030] Similar reactions occur with a wide variety of salts, and this disclosure is intended to cover any nitrogen-containing salt using a porous UF6 membrane electrode.

[0031] Fluoride is thermodynamically stable and therefore not suitable for direct conversion of fluoride to nitrogen. Also, for the exchange reaction to occur, the reaction taking place at the electrode / salt / UF6 gas interface must be, for example, x N y Before the formation of UF6, we first convert it to the lower state U 4+、3+、0 For example, the direct conversion of UF6 to UN requires at least 6+ →U 3+ This requires a change in the state of the cathode to produce the following electrode reaction: U 6+ +3e - →U 3+

[0032] This means that, at a minimum, the potential of the UF6 gaseous membrane electrode is 3+ 4 indicates that the electrode must be kept cathodic enough to induce the formation of UF6. In practice, however, a boundary layer tends to form on the electrode, which requires the application of a voltage greater than the theoretical minimum to overcome the boundary layer. Thus, with this usual need for overpotential, the electrode may need to be kept even more cathodic in various embodiments. In practice, the actual cathodic potential of the electrode can vary anywhere between the potential required to induce the initial reduction of UF6 (and so negative that metal film electrodes must be galvanically protected) to a cathodic potential that is not so negative that the major salt solvent constituents precipitate. The table in FIG. 4 shows that the U 0 U in eutectic LiCl-KCl salt for conversion to 3+and U 4+ The electromotive force for U 4+ From U 0 To obtain the required voltage, at least 2 volts must be applied under the conditions stated in the table. 6+ Lower state U 4+、3+、0 To convert this to 1 V, the voltage required is much higher, such as 3 volts or more.

[0033] If UF6 is not converted directly to UN, then U is added to keep the nitrogen chemically present in the salt. x N y It is desirable for the conversion of UF6 to UN to occur in the salt, which should reduce the complexity of the system required to recapture the expensive component, concentrated nitrogen-15. It may be possible to convert UF6 to UN2, which would require less overpotential since U would remain in the +6 state, but it would still be ideal for the UN2→UN conversion to occur in the same salt in the same electrochemical reactor. This can be done by increasing the temperature to above about 975°C. See Silva GW et al., INORGANIC CHEMISTRY, Reaction sequence and kinetics of uranium nitride decomposition, Nov 16,2009;48(22):10635-42.doi:10.1021 / ic901165j.

[0034] Compared to other production methods, the process described herein adds simplification and reduction of unit steps for generating UN from a uranium hexafluoride supply. The ability to use uranium nitride rather than uranium oxide allows for higher uranium-235 enrichment at lower enrichments, thereby allowing nuclear reactors to achieve higher burnups using current enrichment limits.

[0035] The methods currently used to produce UN are time consuming and multi-step in use. In various aspects, the methods described herein can generate UN directly from UF6 in molten salt. This process makes the enriched nitrogen-15 easier to store because it remains chemically bound as UN or in the salt. This process can occur at relatively low temperatures, for example up to about 400°C for some salts, or below 600°C for other salts. In addition, the process should minimize oxidation contaminants in the product.

[0036] Referring now to the figures, exemplary electrochemical reactors 10, 100, and 200 are shown. x N y 1 shows a reactor 10 in which a batch process for the production of U can occur. The reactor 10 includes a chamber 16 containing a cathode 12, an anode 14, and a molten salt 20 held in a salt container 30 in a bottom portion of the chamber 16. The cathode and anode each have a first end 24 extending out from the top of the reactor chamber 16 and a second end 26 immersed in the molten salt 20. The second end 26 of the cathode 12 terminates in a bubbler 18 that is also immersed in the salt 20. A gas outlet conduit 22 opens into a space 28 above the salt 20 in the chamber 16. One set of electrodes is shown in the figure. However, in certain aspects, a second set of electrodes (not shown) may be used. In embodiments in which two sets of electrodes are used in the salt, U x N y The formation occurs at the anode of the second set of electrodes and the reduction of UF6 to UF4, UF3 and / or U metal occurs at the first set of electrodes.

[0037] In various embodiments, the cathode 12 may be in the form of a solid-walled tube through which UF6 gas flows from a first end 24 to a second end 26 into a bubbler 18, which injects the UF6 into the molten salt 20. A suitable voltage is applied to the cathode and electricity flows between the cathode and the anode by electrical connections (not shown) from any suitable external source. If the salt is a nitride salt, UF6 is converted into UF6 gas by a current of 1000 volts. x N y The conversion to U typically occurs by reaction with a salt at or near the cathode. Alternatively, the salt may be neutral or another type of solvent, and the nitrogen source may enter chamber 16 through anode 14. Nitrogen gas in the form of N2, NH4, or NF3 may enter first end 24 of anode 14 and exit second end 26 of anode 14 into salt 20, where when an appropriate voltage is applied to cathode 12, the nitrogen gas reacts to produce U. x N y Alternatively, UF can be reduced at the cathode surface to produce U x N y The generation of can occur at or adjacent to the anode surface 14. Although only one nitrogen source is required, nitrogen may enter the salt 20 from two sources. Thus, nitrogen can be introduced into the reactor 10 from either or both of the nitride salts 20, or from nitrogen gas injected through the anode 14.

[0038] Excess or unreacted UF6 blown through the salt 20 to the space 28 above the salt may be withdrawn through an outlet conduit 22 for eventual reuse. In a typical recycling process, UF6 gas may be withdrawn from the space 28 of the chamber 16 and passed to a condenser. The condensate is then evaporated, returning the UF6 to its gaseous state, and may be stored or passed back through the cathode 12 for reuse.

[0039] U generated in reactor 10 x N ymay be separated from the salt 20 after reaction by boiling the salt. This reaction may also convert UN2 to U2N3 and then to UN if the boiling point is above 975°C, depending on the salt and its boiling point. As noted above, the reaction in reactor 10 may directly produce UN. However, if one or both of UN2 and U2N3 are produced, the reaction product removed from chamber 16 may be advanced to a second chamber or unit for further processing to produce UN. If separated, UN2 and U2N3 may be heated to temperatures of about 975°C to 1300°C to decompose UN2 and / or U2N3 to UN. Temperatures above 1700°C may be used to evaporate the remaining salt, which may be recycled back into the reactor.

[0040] Referring to Figure 2, U x N y A continuous process for the production of UF6 may be carried out in an electrochemical reactor 100. The reactor 100 includes a cathode 112, an anode 114, a chamber 116, a bubbler 118, a molten salt vessel 130, a salt distillation condenser 132, a separator member 134, and a conveying device 136. A recycle or UF6 gas outlet conduit 122 is also provided for withdrawing excess or unreacted UF6 gas from the space 128 above the salt vessel 130. An appropriate voltage is applied to the cathode 112 by an electrical connection (not shown) from any suitable external source, and electricity flows between the cathode and the anode.

[0041] The chamber 116 has an upper portion 142 and a lower portion 144. The upper portion 142 is maintained at a lower temperature than that of the lower portion 144. For example, in various embodiments, depending on the salt used in the method, the upper portion 142 may be between 500-1600°C, a temperature range that allows the salt to flow through the distillation condenser but below the volatilization temperature of the salt. In other embodiments, the upper portion 142 may be between 300-400°C, again depending on the salt used. The lower portion 144 of the chamber 116 may be kept at about 1200°C or higher but below the melting point of UN (about 2500°C-2600°C) in various embodiments. In this temperature range, the salt is distilled and the UN is solid.

[0042] In the reactor 100, UF6 gas is introduced into the chamber 116 through the cathode 112. The interior end 126 of the cathode 112 enters a bubbler 118 located along the bottom or floor of a salt vessel 130. The salt vessel 130 holds a molten salt 20, which, like the salt in the reactor 10, may be a nitrogen source such as an alkali or transition metal nitride salt. Alternatively or additionally, nitrogen may be introduced into the salt as N2 or NF3 gas through the anode 114. UF6 is converted into U x N y The reaction converting U to U occurs at or near the cathode surface in the manner described above, thereby producing one or more of U2N3, UN2, and UN, which flow through the bubbler 118 to form solid U x N y The liquid salt enters a filter or sieve or other element 134 to separate the salt from the salt inlet. The pressure difference between the salt container and the membrane cathode causes U x N y is forced through the membrane and into the separation member 134. The pressure can be applied by a salt head or by pressurizing the reaction vessel.

[0043] The temperature in the lower portion of the chamber 116 is maintained above 1200° C. Salts are distilled at higher temperatures, but U x N yThe salt distillate rises to the upper portion 142 of the chamber 116 where the temperature is cooler and the salt distillate condenses to a liquid in the distillation condenser 132 where the liquid is poured back into the salt vessel 130 as molten salt 20.

[0044] The separator member 134 may be, for example, a U-shaped filter or sieve to facilitate passage therethrough. x N y The member 134 may be a vibrating surface to break up the solid pieces of U into smaller particles. The member 134 may be heated to temperatures above 1200° C. to 1700° C. or higher to aid in the distillation of the salt 20 and convert any U2N3 and UN2 present into UN and N2 gas. At temperatures above 1700° C., pure UN may be produced. x N y The reaction products (U2N3, UN2, and / or UN) are passed from the separator member 134 to or from the conveying system 136 for transport to further unit processes as required. The nitrogen gas produced is N 15 which is captured, for example as nitrogen gas, introduced through anode 114 for reintroduction into the process.

[0045] An alternative electrochemical reactor 200 for use in a process for batch or continuous production of UF6 is shown in FIG. 3. The reactor 200 includes two chambers 216 and 217. The chamber 216 includes a cathode 212 for the introduction of UF6 gas, an anode 214, a salt container 230, and a bubbler 218, each of which is similar to the cathode 12, anode 14, salt container 30, and bubbler 18 in the reactor 10. The salt container 230 can hold a molten nitrogen-containing salt, such as an alkali or transition metal salt as described above, or a neutral salt or other solvent, in the case where the nitrogen source is nitrogen gas introduced through the anode 214. As in the reactors 10 and 100, an outlet conduit 122 is provided to withdraw the UF6 gas for recycling. The chamber 216 of the reactor 200 includes a salt distillation condenser 232, which functions in the same manner as the distillation condenser 132 in the reactor 100. An appropriate voltage is applied to the cathode 212 by an electrical connection (not shown) from any suitable outside source, causing electricity to flow between the cathode and the anode.

[0046] Chamber 217 may be a separate chamber spaced apart from chamber 216 but connected to chamber 216 by two conduits 248 and 250. Alternatively, chambers 216 and 217 may be two adjacent sections of a single chamber, fluidly connected by conduits 248 and 250. If chambers 216 and 217 are adjacent sections of a single chamber, the sections are preferably insulated to maintain a temperature differential between the two sections.

[0047] Chamber 216 is maintained at a lower temperature than chamber 217. For example, in various embodiments, depending on the salt used in the method, chamber 216 may be between 500° C.-600° C., a temperature range that allows the salt to flow through distillation condenser 232, but below the volatilization temperature of the salt. Chamber 217, in various embodiments, may be kept at or above about 1200° C., high enough to distill the salt, but below the melting point of UN (about 2500° C.-2600° C.).

[0048] The chamber 217 includes a separator member 234 similar to member 134 in the reactor 100. A conduit 248 is provided for the molten salt and U. x N y Reaction products (e.g. U2N3, UN 2、 and / or UN) from a salt container 230 in chamber 216 to a higher temperature chamber 217, which is now emptied onto a separator member 234. The separator member 234, such as member 134, may be, for example, a separator member that is emptied of U to facilitate passage through a filter or sieve. x N y The member 234 may be a vibrating surface to break up the solid pieces of U into smaller particles. The member 234 may be heated to a temperature in excess of 1200° C., up to 1700° C. or higher to aid in the distillation of the salt 20 and convert any U2N3 and UN2 present into UN and N2 gas. x N y Reaction product (U2N 3、 The U2N3 and UN2 are pumped from the separator member 234 into or out of the transport system 236 for transport to further unit processes, if necessary. When all of the U2N3 and UN2 have been successfully converted to UN from the heated separator member 234 and / or the heated chamber 217, the transport system 236 transports the final UN, for example to a storage facility. The nitrogen gas produced in this step of the method is N 15 which is captured, for example, as nitrogen gas introduced through anode 114 for reintroduction into the process.

[0049] The salt 20 distilled from the separator member 234 in chamber 217 rises to the upper portion of chamber 217 and passes through conduit 250 back to chamber 216 where it is at a lower temperature and the salt distillate is condensed to a liquid in distillation condenser 232 where it is poured back into the salt vessel 230 as molten salt 20.

[0050] Both the UF6 and the molten salt used in the reactor 10 / 100 / 200 are corrosive. Therefore, the cathode 12 / 112 / 212 and anode 14 / 114 / 214 of the reactor 10 / 100 / 200 are made of conductive, corrosion-resistant materials such as high Ni alloys, platinum, tungsten, or carbon. Those skilled in the art will understand that other corrosion-resistant materials may be used as electrodes in the electrochemical reactor 10 / 100 / 200 described herein.

[0051] Although exemplary embodiments of electrochemical reactors capable of carrying out the methods described herein have been described, those skilled in the art will recognize that modifications and additions can be made to the basic components. Features of the electrochemical reactors of this method include good gas / salt contact, and corrosion resistant cathodes and anodes. Additionally, the reactors are designed to be able to withstand the U while maintaining the temperature differentials required for salt distillation and salt condensation at the appropriate stages of the reaction. x N y The reaction products are kept in a solid state and, in various aspects, x N y A means for converting the intermediate to UN should be included. 15 Due to the scarcity and cost of reactants such as UF6, the ability to recapture and recycle is desirable.

[0052] All patents, patent applications, publications, or other disclosure materials mentioned herein are incorporated herein by reference in their entirety, as if each individual reference were expressly incorporated by reference. All references and any materials or portions thereof that are said to be incorporated herein by reference are incorporated herein only to the extent that the incorporated materials do not contradict existing definitions, statements, or other disclosed materials set forth in this disclosure. Thus, to the extent necessary, the disclosure set forth herein supersedes any conflicting materials incorporated herein by reference, and the disclosure set forth in this application controls.

[0053] The present invention has been described with reference to various exemplary and illustrative embodiments. The embodiments described herein are understood to provide exemplary features of various details of various embodiments of the disclosed invention. Thus, unless otherwise specified, it should be understood that one or more features, elements, components, ingredients, components, structures, modules, and / or aspects of the disclosed embodiments can be combined and separated. Replaced and / or rearranged with one or more other features, elements, components, ingredients, components, structures, modules, and / or aspects of the disclosed embodiments without departing from the scope of the disclosed invention. Thus, it will be recognized by those skilled in the art that various substitutions, modifications, or combinations of any of the exemplary embodiments can be made without departing from the scope of the invention. Moreover, those skilled in the art will recognize, or be able to ascertain using no more than routine experimentation, many equivalents to the various embodiments of the invention described herein upon review of this specification. Thus, the present invention is not limited by the description of the various embodiments, but rather by the scope of the claims. The following items are elements that are claimed in the international application: [1] A method for producing uranium nitride fuel, comprising the steps of: UF 6 The gas is exposed to a nitrogen-containing salt at or near the cathode to produce U x N y wherein x is an integer of 1 or 2 and y is an integer of 1 to 3; U x N y converting the nitrogen gas into UN; The method includes a reaction represented by: [2] The method according to [1], wherein the method is carried out in a batch process in a single reaction chamber. [3] The method according to [1], wherein the method is carried out in a continuous process in a single reaction chamber. [4] The method according to [1], wherein the method is carried out in a continuous process in two separate chambers. [5] The method according to [1], wherein the nitrogen-containing salt is a nitride salt. [6] The method according to [5], wherein the nitride salt is selected from the group consisting of alkali nitrides, alkali metal nitrides and transition metal nitrides. [7] The method according to [5], further comprising the step of introducing nitrogen gas into the nitride salt. [8] The nitrogen-containing salt is NaCN, KCN, NaCNO, KCNO, K 2 CO 3 , KCl and mixtures thereof. [9] The nitrogen-containing salt is LiCl-KCl-Li 3 N, LiF-NaF-KF-Li 3 The method according to [5], wherein the moiety is selected from the group consisting of N and mixtures thereof.

[10] The method according to [1], wherein the nitrogen-containing salt is produced by introducing nitrogen gas into a neutral salt or solvent.

[11] The nitrogen is N 15 The method according to claim 1,

[12] The method of [1], further comprising the step of reconstituting the nitrogen-containing salt by adding a nitride to the salt.

[13] The method of [1], wherein a voltage of 2 volts or greater is applied to the cathode.

[14] A method for producing uranium nitride fuel, comprising the steps of: Follow these steps: (1)xUF 6 +yN 3- →U x N y +6xF - and (2)U x Ny→xUN+(yx) / 2N 2 ; The reaction includes a reaction represented by In the formula, x is an integer of 1 or 2, and y is an integer of 1 to 3. The reaction is carried out on the porous UF of the first set of electrodes in contact with a nitrogen-containing salt. 6 The method is carried out on a membrane electrode.

[15] The method according to

[14] , wherein the nitrogen-containing salt is selected from the group consisting of alkali nitrides, alkali metal nitrides and transition metal nitrides.

[16] The nitrogen-containing salt is UF 4 and U.F. 3 One or both of the following are included: The method of claim 14, wherein step (2) is carried out at the anode of the second set of electrodes in contact with the nitrogen-containing salt.

[17] The nitrogen-containing salt is NaCN, KCN, NaCNO, KCNO, K 2 CO 3 , KCl and mixtures thereof.

[18] The nitrogen-containing salt is LiCl-KCl-Li 3 N, LiF-NaF-KF-Li 3 The method according to

[14] , wherein the moiety is selected from the group consisting of N and mixtures thereof.

[19] wherein step (1) of the reaction is UF 6 +2Li 3 N→UN 2 +6LiF The method according to

[18] , represented by:

[20] The method of

[14] , carried out at a temperature in the range of 350°C to 600°C.

[21] The method of

[14] , further comprising the step of rearranging the reaction by the addition of a nitriding component.

[22] Furthermore, the porous UF of the first set of electrodes 6 14. The method of claim 13, further comprising the step of reconstituting the reaction by replacing the membrane electrode or adding a second set of electrodes having a second porous UF6 membrane electrode.

[23] Furthermore, the salt is volatilized, and the U x N y 3. The method of claim 1, further comprising the steps of: removing said U from said salt by distilling said salt at a temperature sufficient to maintain said U as a solid; x N y The method according to

[14] , comprising the step of separating

[24] Furthermore, the solid U x N y is heated to a temperature between 975°C and less than 2500°C to obtain U x N y The method of

[23] , comprising the step of converting

[25] Furthermore, condensing the distilled salt; adding the condensed salt to the nitrogen-containing salt; adding nitride to the condensed salt; The method according to claim 23, comprising:

[26] The method according to

[23] , wherein the temperature for volatilizing the salt is about 1200°C.

Claims

1. 1. A method for producing uranium nitride fuel, comprising: UF 6 The gas is exposed to a nitrogen-containing salt at or near the cathode to produce U x N y wherein x is an integer of 1 or 2 and y is an integer of 1 to 3; U x N y converting the nitrogen gas into UN and nitrogen gas; The method includes a reaction represented by:

2. The method of claim 1 , wherein the method is carried out in a batch process in a single reaction chamber.

3. The method of claim 1 , wherein the method is carried out in a continuous process in a single reaction chamber.

4. The method of claim 1 , wherein the method is carried out in a continuous process in two separate chambers.

5. The method of claim 1 , wherein the nitrogen-containing salt is a nitride salt.

6. 6. The method of claim 5, wherein the nitride salt is selected from the group consisting of alkali nitrides, alkali metal nitrides and transition metal nitrides.

7. The method of claim 5 , wherein the method further comprises the step of introducing nitrogen gas into the nitride salt.

8. 6. The method of claim 5, wherein the nitrogen-containing salt is selected from the group consisting of NaCN, KCN, NaCNO, KCNO, and mixtures thereof.

9. The nitrogen-containing salt is LiCl-KCl-Li 3 N, LiF-NaF-KF-Li 3 6. The method of claim 5, wherein the alkyl group is selected from the group consisting of N and mixtures thereof.

10. 2. The method of claim 1, wherein the nitrogen-containing salt is generated by introducing nitrogen gas into a neutral salt or solvent.

11. The nitrogen is N 15 The method of claim 1, wherein

12. The method of claim 1 further comprising the step of reconstituting the nitrogen-containing salt by adding a nitride to the salt.

13. The method of claim 1 , wherein a voltage of 2 volts or greater is applied to the cathode.

14. 1. A method for producing uranium nitride fuel, comprising: Steps below: (1) xUF 6 +yN 3- →U x N y +6xF - and (2)U x Ny→xUN+(y-x) / 2N 2 ; The reaction includes a reaction represented by In the formula, x is an integer of 1 or 2, and y is an integer of 1 to 3, The reaction is carried out by the porous UF of the first set of electrodes in contact with a nitrogen-containing salt. 6 The method is carried out on a membrane electrode.

15. 15. The method of claim 14, wherein the nitrogen-containing salt is selected from the group consisting of alkali nitrides, alkali metal nitrides, and transition metal nitrides.

16. The nitrogen-containing salt is 4 and U.F. 3 One or both of the following are included:

15. The method of claim 14, wherein step (2) occurs at the anode of the second set of electrodes in contact with the nitrogen-containing salt.

17. 15. The method of claim 14, wherein the nitrogen-containing salt is selected from the group consisting of NaCN, KCN, NaCNO, KCNO, and mixtures thereof.

18. The nitrogen-containing salt is LiCl-KCl-Li 3 N, LiF-NaF-KF-Li 3 15. The method of claim 14, wherein said alkyl group is selected from the group consisting of N and mixtures thereof.

19. The reaction step (1) is <h2 style=";text-align:left;direction:ltr">5F<h2 style=";text-align:left;direction:ltr"> 6 <h2 style=";text-align:left;direction:ltr"> 22Li<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> N→UN<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +6LiF 20. The method of claim 18, wherein the

20. 15. The method of claim 14 carried out at a temperature in the range of 350°C to 600°C.

21. The method of claim 14 further comprising the step of reconstituting the reaction by the addition of a nitriding component.

22. Further, the porous UF of the first set of electrodes 6 15. The method of claim 14, comprising the step of reconstituting the reaction by replacing the membrane electrode or adding a second set of electrodes having a second porous UF6 membrane electrode.

23. Furthermore, the salt is volatilized, and the U x N y The U is removed from the salt by distilling the salt at a temperature sufficient to maintain the salt as a solid. x N y The method of claim 14 , further comprising the step of:

24. Furthermore, the solid U x N y to a temperature between 975° C. and less than 2500° C. to obtain U x N y 24. The method of claim 23, further comprising converting:

25. moreover, condensing the distilled salt; adding the condensed salt to the nitrogen-containing salt; adding nitride to the condensed salt; 24. The method of claim 23, comprising:

26. 24. The method of claim 23, wherein the temperature for volatilizing the salt is about 1200°C.

Citation Information

Patent Citations

  • Device and method for preparing fuel salt of molten salt reactor

    CN108109710A

  • Nuclear fuel cycle

    JP1995120580A

  • Reprocessing method for nuclear fuel

    JP1998010285A

  • Method for preparing uranium mononitride