Resin composition, toner for developing electrostatic images, image forming method, and photosensitive adhesive
A resin composition with an azomethine moiety addresses color reproduction issues in azobenzene derivatives and facilitates easy removal of 3D printer supports through reversible fluidization upon light irradiation, enhancing industrial application efficiency.
Patent Information
- Application Number
- JP2020102757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-15
AI Technical Summary
Existing azobenzene derivatives used in industrial products suffer from color reproduction issues due to strong absorption in the long wavelength region, and 3D printer support materials require easy removal methods that do not cause burrs, which are time-consuming to polish.
A resin composition containing a compound with an azomethine moiety, represented by a specific general formula, that undergoes reversible fluidization/non-fluidization upon isomerization upon light irradiation, allowing for colorless and rapid fixation of electrostatic images and easy removal of 3D printer supports.
The resin composition enables high color reproducibility and easy removal of 3D printer supports without the need for heat or pressure, providing a colorless and efficient image fixing process.
Smart Images

Figure 0007592984000031 
Figure 0007592984000032 
Figure 0007592984000033
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a toner for developing electrostatic images, an image forming method and a photosensitive adhesive, and in particular to a resin composition which is colorless but which induces a reversible fluidification / imfluidification phenomenon upon isomerization and can be rapidly imfluidized. [Background technology]
[0002] Azobenzene derivatives are known to be materials that absorb light and soften from a solid state (photochemical phase transition). This photochemical phase transition is thought to occur when the trans (E) isomer is converted to the cis (Z) isomer, causing the crystal structure to collapse. The azobenzene derivatives described in Patent Document 1 or Patent Document 2 undergo a phase change associated with an isomerization reaction upon irradiation with light. However, these compounds are colored orange due to strong absorption in the long-wavelength region resulting from the n-π* transition, which poses a problem in that the desired color cannot be reproduced when applied to industrial products. In addition, with the recent spread of 3D printers, the molding of laminates by the hot melt extrusion method can be colored, or in addition to filaments made of opaque polylactic acid, ABS resin, polypropylene, etc., transparent filaments such as PET and polycarbonate are also on the market. 3D printers have a process in which a dummy support is made depending on the shape of the object to be molded, and the support is removed after the molding is completed. During this removal, burrs appear at the contact points, which requires time and effort such as polishing. To simplify the manufacturing process of 3D printers, a support that can be easily removed with light is desired, and a composition that softens with light is strongly desired as a filament material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-191078 A [Patent Document 2] JP 2014-191077 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a resin composition that is colorless but induces a reversible fluidization / imfluidization phenomenon upon isomerization and can be rapidly imfluidized. It is also an object of the present invention to provide a toner for developing electrostatic images that can be fixed by light irradiation and has high color reproducibility, and an image forming method using the toner for developing electrostatic images, using the resin composition. It is also an object of the present invention to provide a photosensitive adhesive. [Means for solving the problem]
[0005] In the course of investigating the causes of the above problems in order to solve the above problems, the present inventors discovered that by using a specific compound having an azomethine moiety, it is possible to provide a resin composition which is colorless, can be reversibly fluidized / non-fluidized, and can be rapidly non-fluidized, thereby arriving at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0006] 1. A resin composition comprising a compound having a structure represented by the following general formula (1): [ka] [In the general formula (1), Z1 and Z2 each independently represent N or CH, and Z1 ≠ Z2. A1 and A2 each independently represent a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. L1 and L2 each represent a linking group. n represents 0 or 1. B represents a complementary multiple hydrogen bonding group, and the complementary multiple hydrogen bonding group is selected from the group consisting of adenine, thymine, and 2,6-diacetylaminopyridine. , Me Lamin, cyanuric acid, and 4,6-Diamino-2-pyrimidino Hmm? G is a substituent or a residue of a compound selected from the group consisting of The above phase SupplementaryWhen G is a substituent, n=0.]
[0008] 2 The first method is characterized in that the material is reversibly fluidized and non-fluidized by irradiation with light. In the section The resin composition described above.
[0009] 3 The wavelength of the light irradiation is within the range of 280 to 480 nm. 2 The resin composition according to item 1.
[0010] 4 .Items 1 to 5 3 3. A toner for developing electrostatic images, comprising the resin composition according to claim 1.
[0011] 5 The toner base particles contain a binder resin. 4 2. The toner for developing electrostatic images according to claim 1.
[0012] 6 The binder resin contains at least one resin selected from the group consisting of styrene-acrylic resin and polyester resin. 5 2. The toner for developing electrostatic images according to claim 1.
[0013] 7 The toner base particles contain a colorant. 4 From item to item 6 Item 1. The toner for developing an electrostatic image according to any one of items 1 to 9.
[0014] 8 The toner base particles contain a release agent. 4 From item to item 7 Item 1. The toner for developing an electrostatic image according to any one of items 1 to 9.
[0015] 9 .No. 4 From item to item 8An image forming method using the toner for developing an electrostatic image according to any one of claims 1 to 5, An image forming method comprising: a step of forming a toner image made of the toner for developing an electrostatic image on a recording medium; and a step of irradiating the toner image with light to soften the toner image.
[0016] 10 The wavelength of the light irradiation is within the range of 280 to 480 nm. 9 2. The image forming method according to claim 1 .
[0017] 11 The method further comprises a step of pressing the toner image. 9 Section or Article 10 2. The image forming method according to claim 1 .
[0018] 12 In the step of applying pressure, the toner image is further heated. 11 2. The image forming method according to claim 1 .
[0019] 13. A photosensitive adhesive comprising a compound represented by the following general formula (1): [ka] [In the general formula (1), Z1 and Z2 each independently represent N or CH, and Z1 ≠ Z2. A1 and A2 each independently represent a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. L1 and L2 each represent a linking group. n represents 0 or 1. B represents a complementary multiple hydrogen bonding group, and the complementary multiple hydrogen bonding group is selected from the group consisting of adenine, thymine, and 2,6-diacetylaminopyridine. , Me Lamin, cyanuric acid, and 4,6-Diamino-2-pyrimidino Hmm? G is a substituent or a residue of a compound selected from the group consisting of The above phase Supplementary When G is a substituent, n=0.] Effect of the Invention
[0020] The above-mentioned means of the present invention can provide a resin composition that is colorless but induces a reversible fluid / non-fluid phenomenon upon isomerization and can be rapidly non-fluidized. In addition, by using the resin composition, it is possible to provide a toner for developing electrostatic images that can be fixed by light irradiation and has high color reproducibility, and an image forming method using the toner for developing electrostatic images. Furthermore, it is possible to provide a photosensitive adhesive.
[0021] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. The resin composition of the present invention contains a compound having a structure represented by general formula (1), i.e., a compound having an azomethine moiety (hereinafter also referred to as an "azomethine derivative"). Therefore, it is possible to provide a colorless compound that can be reversibly fluidized or non-fluidized by light irradiation. Azobenzene derivatives are colored orange due to the strong absorption resulting from the n-π* transition, but colorlessness can be achieved by using azomethine derivatives, which have almost no absorption peak.
[0022] In addition, the fluidization that accompanies photoisomerization is thought to be induced by the isomerization of the non-fluid trans form (E) to the cis form (Z) when the non-fluid trans form (E) is irradiated with light, which causes the regular structure of the crystal to collapse and undergoes a phase transition. Therefore, in order to induce the reversible fluid / non-fluid phenomenon, it is thought that many trans forms (E) must be isomerized to the cis form (Z).
[0023] This is thought to occur because, like azobenzene derivatives, the crystal structure collapses due to isomerization from the trans form (E) to the cis form (Z). The mechanism is thought to be as follows. When azomethine derivative crystals are irradiated with light, the azomethine molecules on the crystal surface are isomerized, and the crystal structure is broken down, causing it to become fluid and improving its light transmittance. The surface layer of the crystal becomes fluid, improving its transmittance, allowing light to reach the inside of the crystal, and the inner crystal layer becomes fluid from the outermost layer. This mechanism causes the entire crystal to become fluid.
[0024] The azomethine derivative of the present invention has a slightly twisted structure compared to the planarity of the two benzene rings constituting azobenzene. In addition, compared to a para-substituted azobenzene structure, an azomethine derivative composed of a 5-membered ring and a 6-membered ring has a reduced molecular linearity. As a result, the crystallinity and packing of the molecules are poorer than those of an azobenzene derivative. For these reasons, it is considered that the azomethine derivative is superior to the azobenzene derivative during the photo-induced phase transition (fluidization). On the other hand, when going from a fluidized molten state to a non-fluid state, it is believed that the cis (Z) form isomerizes to the trans (E) form, and then crystallizes, resulting in non-fluidity. At this time, if the molecular packing is weak, crystallization will be slow, so it is expected that azomethine derivatives will be at a disadvantage compared to azobenzene derivatives in terms of molecular structure. In order to achieve rapid and active immobilization, we developed a molecular structure in which complementary multiple hydrogen-bonding groups were introduced to the molecular terminals of the azomethine derivative. Even if the rate of isomerization from cis (Z) to trans (E) is low during immobilization, the structure is designed to form a supramolecular polymer through hydrogen bonds, resulting in immobilization. When a supramolecular polymer is used, the polymer becomes fluid when the azomethine moiety is isomerized by light irradiation, breaking the hydrogen bonds that make up the supramolecular polymer and reducing the number of molecular units. From the above, it is believed that the compound having the structure represented by the above general formula (1) is colorless but induces a reversible fluidization / non-fluidization phenomenon upon isomerization, and is capable of rapid non-fluidization. By introducing this compound into a toner for developing electrostatic images, it is possible to obtain a toner that can be fixed by light irradiation and has high color reproducibility. In the present invention, "flow" refers to a state in which a system is deformed without or with a small external force. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a schematic diagram showing an image forming apparatus used in an image forming method according to an embodiment of the present invention; [Diagram 2] Schematic diagram of an irradiation unit in an image forming apparatus [Diagram 3] Schematic diagram of an apparatus for measuring the change in adhesiveness of the compounds synthesized in the examples and comparative examples upon irradiation with light. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The resin composition of the present invention is characterized by containing a compound having a structure represented by the general formula (1). This feature is a technical feature common to or corresponding to each of the following embodiments.
[0027] In an embodiment of the present invention, the complementary multiple hydrogen bonding group is preferably any one of residues of a compound selected from adenine, thymine, 2,6-diacetylaminopyridine, uracil, melamine, cyanuric acid, 4,6-diamino-2-pyrimidinone and 2-ureido-4-pyrimidinone, in terms of the arrangement and number of donors and acceptors.
[0028] In addition, the compound is preferably reversibly fluidized and non-fluidized by light irradiation, in that by introducing the compound into a toner for developing electrostatic images, a toner that can be fixed by light irradiation and has high color reproducibility can be obtained.
[0029] The wavelength of the light irradiation is preferably within the range of 280 to 480 nm, since the light is absorbed well, resulting in good light melting property and good fixability, and is also preferably in that the material can be fluidized without the application of heat or pressure.
[0030] The resin composition of the present invention is preferably used for a toner for developing an electrostatic image, thereby making it possible to obtain a toner which can be fixed by light irradiation and has high color reproducibility.
[0031] The toner base particles constituting the electrostatic image developing toner preferably contain a binder resin, and it is preferable that the binder resin contains at least one resin selected from the group consisting of a styrene-acrylic resin and a polyester resin, in that the binder resin has a low viscosity when melted and has high sharp melting properties.
[0032] In addition, it is preferable that the toner base particles contain a colorant, since a toner having high color reproducibility of the colorant can be obtained. Furthermore, it is preferable that the toner base particles contain a release agent, since a toner having excellent fixing properties can be obtained.
[0033] The image forming method using the toner for developing electrostatic images of the present invention is characterized by comprising the steps of: forming a toner image made of the toner for developing electrostatic images on a recording medium; and irradiating the toner image with light to soften the toner image.
[0034] The wavelength of the light irradiation is preferably within the range of 280 to 480 nm in terms of improving fixability, and also in terms of fluidization without the application of heat or pressure. It is preferable to further include a step of applying pressure to the toner image, which is preferable in that the toner image can be further heated in the step of applying pressure, thereby softening the toner image further.
[0035] The photosensitive adhesive of the present invention is characterized by containing a structure represented by the above general formula (1), thereby making it possible to obtain an adhesive that can be fixed by irradiation with light.
[0036] The present invention, its components, and embodiments for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as lower and upper limits.
[0037] [Resin composition of the present invention] The resin composition of the present invention is characterized by containing a compound having a structure represented by the following general formula (1) (also referred to as a "compound having an azomethine moiety" or an "azomethine derivative").
[0038] [ka] [In the general formula (1), Z1 and Z2 each independently represent N or CH, and Z1 ≠ Z2. A1 and A2 each independently represent a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. L1 and L2 each represent a linking group. n represents 0 or 1. B represents a complementary multiple hydrogen bonding group. G represents a substituent or a mutual multiple hydrogen bonding group, and when G is a substituent, n=0.]
[0039] In the general formula (1), B and G represent complementary multiple hydrogen bonding groups. The complementary multiple hydrogen bonding group is a group that forms complementary multiple hydrogen bonds as described below, has a plurality of hydrogen bond acceptors and donors in its structure, and forms hydrogen bonds between molecules. Specific structures include residues of nucleic acid bases such as adenine, guanine, pyrimidine derivatives such as cytosine, thymine, and uracil, and derivatives thereof, urea, thiourea, melamine, cyanuric acid, barbituric acid, 2,6-diacylaminopyrimidine, 4,6-diamino-2-pyrimidinone, 2-amino-4,6-pyrimidinedinone, 2,4,6-triaminopyrimidine, phthalimide, 2,6-diamino-1,3,5-triazine, 2-ureido-4-amino-1,3,5-triazine, and 2-ureido-4-pyrimidinone, and derivatives thereof, with adenine, thymine, 2,6-diacetylaminopyridine, uracil, melamine, cyanuric acid, 4,6-diamino-2-pyrimidinone, and 2-ureido-4-pyrimidinone being preferred.
[0040] The substituent G shown when n is 0 includes various groups and is not particularly limited. Representative groups include alkyl, aryl, anilino, acylamino, sulfonamide, alkylthio, arylthio, alkenyl, cycloalkyl, cycloalkenyl, alkynyl, heterocyclic, alkoxy, aryloxy, heterocyclicoxy, siloxy, amino, alkylamino, imido, ureido, sulfamoylamino, alkoxycarbonylamino, aryloxycarbonylamino, alkoxycarbonyl, aryloxycarbonyl, heterocyclicthio, thioureido, hydroxy, and mercapto groups, as well as spiro compound residues, bridged hydrocarbon compound residues, sulfonyl, sulfinyl, sulfonyloxy, sulfamoyl, phosphoryl, carbamoyl, acyl, acyloxy, oxycarbonyl, carboxyl, cyano, nitro, halogen-substituted alkoxy, halogen-substituted aryloxy, pyrrolyl, tetrazolyl, and other groups, and halogen atoms.
[0041] The alkyl group preferably has 1 to 32 carbon atoms and may be linear or branched. The aryl group is preferably a phenyl group. The acylamino group includes an alkylcarbonylamino group and an arylcarbonylamino group; the sulfonamide group includes an alkylsulfonylamino group and an arylsulfonylamino group; and the alkyl and aryl components of the alkylthio and arylthio groups include the above-mentioned alkyl and aryl groups. The alkenyl group preferably has 2 to 32 carbon atoms, the cycloalkyl group preferably has 3 to 12 carbon atoms, particularly preferably 5 to 7 carbon atoms, the alkenyl group may be linear or branched, and the cycloalkenyl group preferably has 3 to 12 carbon atoms, particularly preferably 5 to 7 carbon atoms.
[0042] The ureido group is preferably an alkylureido group, an arylureido group, or the like; the sulfamoylamino group is preferably an alkylsulfamoylamino group, an arylsulfamoylamino group, or the like; the heterocyclic group is preferably one having 5 to 7 members, specifically, a 2-furyl group, a 2-thienyl group, a 2-pyrimidinyl group, a 2-benzothiazolyl group, or the like; the heterocyclic oxy group is preferably one having a 5 to 7 membered heterocycle, specifically, a 3,4,5,6-tetrahydropyranyl-2-oxy group, a 1-phenyltetrazole-5-oxy group, or the like; the heterocyclic thio group is preferably a 5 to 7 membered heterocyclic thio group, specifically, a 2-pyridylthio group, Examples of the siloxy group include a trimethylsiloxy group, a triethylsiloxy group, a dimethylbutylsiloxy group, and the like; examples of the imido group include a succinimido group, a 3-heptadecylsuccinimido group, a phthalimido group, a glutarimido group, and the like; examples of the spiro compound residue include spiro[3.3]heptan-1-yl, and the like; examples of the bridged hydrocarbon compound residue include bicyclo[2.2.1]heptan-1-yl, tricyclo[3.3.1.3.7]decan-1-yl, 7,7-dimethyl-bicyclo[2.2.1]heptan-1-yl, and the like.
[0043] Examples of the sulfonyl group include alkylsulfonyl, arylsulfonyl, halogen-substituted alkylsulfonyl, and halogen-substituted arylsulfonyl; examples of the sulfinyl group include alkylsulfinyl and arylsulfinyl; examples of the sulfonyloxy group include alkylsulfonyloxy and arylsulfonyloxy; examples of the sulfamoyl group include N,N-dialkylsulfamoyl, N-N-diarylsulfamoyl, and N-alkyl-N-arylsulfamoyl; examples of the phosphoryl group include alkoxyphosphoryl, aryloxyphosphoryl, alkylphosphoryl, and arylphosphoryl; and examples of the carbamoyl group include Examples of the acyl group include alkylcarbonyl and arylcarbonyl; the acyloxy group includes alkylcarbonyloxy; the oxycarbonyl group includes alkoxycarbonyl and aryloxycarbonyl; the halogen-substituted alkoxy group includes α-halogen-substituted alkoxy; the halogen-substituted aryloxy group includes tetrafluoroaryloxy and pentafluoroaryloxy; the pyrrolyl group includes 1-pyrrolyl; and the tetrazolyl group includes 1-tetrazolyl. In addition to the above substituents, a trifluoromethyl group, a heptafluoroisopropyl group, a nonylfluoro-t-butyl group, a tetrafluoroaryl group, a pentafluoroaryl group, and the like are also preferably used.
[0044] These groups may further include a substituent such as a non-diffusible group such as a long chain hydrocarbon group or a polymer residue, and these substituents may further be substituted with one or more substituents.
[0045] In the general formula (1), A1 and A2 each independently represent a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. The substituted aromatic hydrocarbon group and the substituted aromatic heterocyclic group may be substituted with the above-mentioned substituents.
[0046] In the general formula (1), L1 and L2 represent a linking group. Examples of the linking group include alkylene groups (e.g., methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene, cyclohexane-1,4-diyl, etc.), alkenylene groups (e.g., ethene-1,2-diyl, butadiene-1,4-diyl, etc.), alkynylene groups (e.g., ethyne-1,2-diyl, butane-1,3-diyne-1,4-diyl, etc.), linking groups derived from compounds containing at least one aromatic group (e.g., substituted or unsubstituted benzene, condensed polycyclic hydrocarbons, aromatic heterocycles, aromatic hydrocarbon ring assemblies, aromatic heterocycle assemblies, etc.), and heteroatom linking groups (oxygen, sulfur, nitrogen, silicon, phosphorus atoms, etc.), but are preferably groups linked by alkylene groups and arylene groups. These linking groups may be further substituted with the above-mentioned substituents, and may be combined to form a composite group.
[0047] Examples of compounds having a structure represented by the general formula (1) include those shown below.
[0048] [ka]
[0049] [ka]
[0050] [ka]
[0051] [ka]
[0052] [ka]
[0053] [ka]
[0054]
change
[0055]
change
[0056]
change
[0057]
change
[0058]
change
[0059]
change
[0060]
change
[0061]
change
[0062]
change
[0063]
change
[0064] [ka]
[0065] (synthesis method) The compound having the structure represented by the general formula (1) may be synthesized by a conventionally known synthesis method. An example of the synthesis method of the exemplary compound is shown below.
[0066] [Synthesis Example 1: Synthesis of Exemplary Compound 1] <Synthesis of Azomethine-2NO2> 4-Nitroaniline (Tokyo Chemical Industry Co., Ltd.) (80.0 g, 0.58 mol), 5-nitro-2-furaldehyde (Kanto Chemical Industry Co., Ltd.) (81.7 g, 0.58 mol) and 1000 ml of ethanol were placed in a 2000 ml four-neck flask equipped with a cooling tube, nitrogen inlet tube and thermometer, and heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was carried out in a mixed solvent of methanol / ethanol to obtain 128.6 g of azomethine-2NO2 (yield 85%). The structure is: 1 The results were confirmed by H-NMR and IR.
[0067] <Synthesis of azomethine-2NH2> The synthesis was carried out with reference to Chemistry of Heterocyclic Compounds, 2004,40(6), 701. A 1000 ml four-neck flask was equipped with two three-way stopcocks, a thermometer, a dropping funnel and a ball stopper, and the inside of the container was decompressed and replaced with nitrogen. This operation was repeated three times. While flowing nitrogen, 400 ml of ethyl acetate, azomethine-2NO2 (100.0 g, 0.38 mol) and allylpalladium (II) chloride dimer (Tokyo Chemical Industry Co., Ltd.) (2.8 g, 8 mmol) were added and stirred at room temperature for 30 minutes. Then, while keeping the liquid temperature below 10 ° C in an ice bath, triethylsilane (Tokyo Chemical Industry Co., Ltd.) (53.4 g, 0.46 mol) was added to the dropping funnel and dropped into the solution over 30 minutes. After dropping, the ice bath was replaced with an oil bath and stirred at 65 ° C for 17 hours. The reaction solution was concentrated with an evaporator, and the obtained solid was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 50.1 g (65% yield) of azomethine-2NH2 was obtained. The structure is: 1 The results were confirmed by H-NMR and IR.
[0068] The following synthesis was carried out with reference to J. Am. Chem. Soc., 2001, 123(25), 5947.
[0069] <Synthesis of Adenine-COOH> 9-(2-carboxyethyl)adenine was synthesized using adenine and β-propiolactone in a similar manner to Chem. Lett., 1973, 967. The structure is: 1 The results were confirmed by H-NMR and IR.
[0070] <Synthesis of adenine CF3-COOPhNO2 (active ester)> In a 5L four-neck flask, 2000ml of pyridine, 9-(2-carboxyethyl)adenine (40.0g, 0.19mol), 4-nitrophenol (Tokyo Chemical Industry Co., Ltd.) (30.0g, 0.22mol), and 4-nitrophenyl trifluoroacetate (Tokyo Chemical Industry Co., Ltd.) (200.0g, 0.85mol) were added and stirred at 50℃ for 2 hours. The solution was then concentrated using a rotary evaporator until it solidified, and the resulting solid was dissolved in CHCl3. Diethyl ether was added to this solution, and the precipitated solid was filtered using a Nutsche filter. This solid was redissolved in CHCl3 and slowly dropped into the same amount of diethyl ether as the vigorously stirred CHCl3, and reprecipitation purification was performed. This solid was filtered using a Nutsche filter and dried in a reduced pressure oven at 50℃ to obtain 63.0g of 4-nitrophenyl-3-(6-trifluoroacetamidopurin-9-yl)propionate (yield 77%). The structure is: 1 The results were confirmed by H-NMR and IR.
[0071] <Synthesis of Thymine-COOH> 1-(2-carboxyethyl)adenine was synthesized using thymine and β-propiolactone in a similar manner to Chem. Lett., 1973, 967. The structure is: 1 The results were confirmed by H-NMR and IR.
[0072] <Synthesis of thymine-COOPhCl5 (active ester)> In a 2L four-neck flask, 1000ml of DMF, 400ml of triethylamine, and pentachlorophenyl trichloroacetate (Tokyo Chemical Industry Co., Ltd.) (200g, 0.49mol) were added, and the mixture was stirred at room temperature to completely dissolve the mixture. 1-(2-carboxyethyl)thymine (50.0g, 0.25mol) was added to the solution, and the mixture was reacted at room temperature for 20h. Then, DMF, triethylamine, etc. were distilled off under reduced pressure until the solution solidified, and the resulting solid was taken out of the flask and washed with cold water on a Nutsche. The solid was dried in a reduced pressure oven at 50°C, and then recrystallized with CHCl3 / MeOH=1 / 1 (v / v) to obtain 40g of pentachlorophenyl 3-(2,4-dihydroxy-5-methylpyrimidin-1-yl)propionate (yield 36%). The structure is as follows: 1It was confirmed by 1H-NMR and IR.
[0073] <Synthesis of Half Amine> Into a 500 ml eggplant flask, 3-(2,4-dihydroxy-5-methylpyrimidin-1-yl)phenyl pentachloropropionate (11.1 g, 0.02 mol), azomethine-2NH2 synthesized in the above <Synthesis of Azomethine-2NH2> (50.0 g, 0.25 mol), and 200 ml of diethyl ether were added and dissolved by stirring at room temperature. Then, after reacting at room temperature for 12 hours, it was concentrated under reduced pressure using a rotary evaporator to obtain a solid. The obtained solid was washed with water and then washed with acetone. The washed solid was purified by column chromatography using a methylene chloride / methanol solvent system. As a result, 2.2 g (yield 23%) of monoamine was obtained. The structure was 1 It was confirmed by 1H-NMR and IR.
[0074] <Synthesis of Exemplary Compound 1 Protected by CF3CO> Into a 500 ml eggplant flask, 4-nitrophenyl 3-(6-trifluoroacetamidopurin-9-yl)propionate (9.4 g, 22.2 mmol), half azomethine synthesized in the above <Synthesis of Half Amine> (2.0 g, 5.2 mmol), and 400 ml of diethyl ether were added and dissolved by stirring at room temperature. Then, after reacting at room temperature for 3 days, it was concentrated under reduced pressure using a rotary evaporator to obtain a solid. The obtained solid was washed with water and then washed with diethyl ether. The washed solid was purified by column chromatography using a methylene chloride / methanol solvent system. As a result, 2.5 g (yield 72%) of exemplary compound 1 protected by CF3CO was obtained. The structure was 1 It was confirmed by 1H-NMR and IR.
[0075] <Synthesis of Exemplary Compound 1 (Deprotection of CF3CO)> To a 100 ml eggplant flask, potassium carbonate (1.0 g, 7.5 mmol) and 10 ml of water were added and dissolved by stirring at room temperature. Then, 10 ml of methanol was added to the solution, and the CF3CO-protected exemplary compound 1 (2.5 g, 3.8 mmol) synthesized in the above <Synthesis of CF3CO-Protected Exemplary Compound 1> was added, and the mixture was stirred at room temperature for 12 hours. It was concentrated under reduced pressure using a rotary evaporator, and the resulting solid was washed with water. The obtained solid was redissolved in ethanol and purified by reprecipitation by slowly dropping it into vigorously stirred water. This solid was dried in a vacuum oven at 50 °C to obtain 1.9 g of the exemplary compound 1 (yield 90%). The structure was 1 confirmed by 1H-NMR and IR.
[0076] [Synthesis Example 2: Synthesis of Exemplary Compound 3] Exemplary compound 3 was synthesized in the same manner except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Inc.) in Synthesis Example 1 was replaced with 1-methyl-5-nitro-1H-pyrrole-2-carboxaldehyde (manufactured by Accel Pharmtec). The structure was 1 confirmed by 1H-NMR and IR.
[0077] [Synthesis Example 3: Synthesis of Exemplary Compound 6] Exemplary compound 6 was synthesized in the same manner except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Inc.) in Synthesis Example 1 were replaced with 5-nitro-2-thiopheneamine (manufactured by Chemieliva Pharmaceutica) and 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure was 1 confirmed by 1H-NMR and IR.
[0078] [Synthesis Example 4: Synthesis of Exemplary Compound 8] Exemplary compound 8 was synthesized in the same manner except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Inc.) in Synthesis Example 1 were replaced with 2,5-dimethoxy-4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure was 1 confirmed by 1H-NMR and IR.
[0079] [Synthesis Example 5: Synthesis of Exemplary Compound 11] Exemplary compound 11 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 1-methyl-5-nitro-1H-pyrrol-2-amine (manufactured by Aurora Fine Chemicals LLC) and 3-fluoro-4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure is: 1 The results were confirmed by H-NMR and IR.
[0080] [Synthesis Example 6: Synthesis of Exemplary Compound 14] Exemplary compound 14 was synthesized in the same manner as in Synthesis Example 1, except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) was replaced with 4-methoxy-5-nitro-2-thiophenecarboxaldehyde (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0081] [Synthesis Example 7: Synthesis of Exemplary Compound 16] Exemplary compound 16 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) were replaced with 3-acetyl-2-amino-5-nitrothiophene (manufactured by Aurora Fine Chemicals LLC) and 4-methyl-5-nitro-2-furancarboxaldehyde (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0082] [Synthesis Example 8: Synthesis of Exemplary Compound 18] Azomethine-2NH2 (100.0 g, 0.5 mol) synthesized by replacing 4-nitroaniline (Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (Kanto Chemical Industry Co., Ltd.) in Synthesis Example 1 with 5-nitro-2-thiophenamine (Chemieliva Pharmaceutica Co., Ltd.) and 4-nitrobenzaldehyde (Tokyo Chemical Industry Co., Ltd.) was dissolved in 500 ml of toluene, triethylamine (112.7 g, 1.1 mol) was added, and the solution temperature was kept below 10°C in an ice bath. 5-Aminopentanoyl chloride (Aurora Fine Chemicals LLC Co., Ltd.) (137.3 g, 1.0 mol) was added dropwise to this solution over 30 minutes, and the reaction was carried out at 50°C for 5 hours. After adding methanol to quench the mixture, the mixture was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The obtained solid was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 86.1 g of azomethine-2NH2(2) was obtained (yield 45%). The structure is 1 The reaction was confirmed by H-NMR and IR. The subsequent process was the same as in Synthesis Example 1 to synthesize Example Compound 18. The structure is: 1 The results were confirmed by H-NMR and IR.
[0083] [Synthesis Example 9: Synthesis of Exemplary Compound 20] Azomethine-2NH2 (100.0 g, 0.46 mol), which was synthesized by replacing 4-nitroaniline (Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 1 with 1-methyl-5-nitro-1H-pyrrol-2-amine (Aurora Fine Chemicals LLC), was dissolved in 200 ml of toluene, and triethylamine (5.6 g, 0.06 mol) was added, and the solution temperature was kept below 10°C in an ice bath. 5-Aminopentanoyl chloride (Aurora Fine Chemicals LLC) (6.2 g, 0.05 mol) was added dropwise to this solution over 30 minutes, and the reaction was carried out at 50°C for 5 hours. After adding methanol to quench the reaction, the mixture was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The obtained solid was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 4.3 g of azomethine-2NH2 (3) was obtained (yield 31%). The structure is as follows:1 The results were confirmed by H-NMR and IR. Azomethine-2NH2 (3) (4.0 g, 13.2 mmol) was dissolved in 30 ml of toluene, and triethylamine (1.8 g, 17.4 mmol) was added, and the solution temperature was kept below 10°C in an ice bath. 3-Amino-5-methylbenzoyl chloride (Chemieliva Pharmaceutical) (2.5 g, 14.5 mmol) was added dropwise to this solution over 30 minutes, and the reaction was carried out at 50°C for 5 hours. After adding methanol to quench the reaction, the mixture was concentrated under reduced pressure using a rotary evaporator, and the resulting solid was washed with water. The resulting solid was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 4.5 g of azomethine-2NH2 (4) was obtained (yield 82%). The structure is as follows: 1 The compound was confirmed by H-NMR and IR. The subsequent process was the same as in Synthesis Example 1 to synthesize Example Compound 20. The structure is: 1 The results were confirmed by H-NMR and IR.
[0084] [Synthesis Example 10: Synthesis of Exemplary Compound 41] Exemplary compound 41 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 3-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiophenecarboxaldehyde (manufactured by Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0085] [Synthesis Example 11: Synthesis of Exemplary Compound 25] Exemplary compound 25 was synthesized in the same manner as in Synthesis Example 1 <Synthesis of half amine>, except that a half amine in which the thymine moiety is bonded to a six-membered ring amine was used. The structure is: 1 The results were confirmed by H-NMR and IR.
[0086] [Synthesis Example 12: Synthesis of Exemplary Compound 27] Exemplary compound 27 was synthesized in the same manner as in Synthesis Example 1, except that 5-nitro-2-furaldehyde (Kanto Chemical) was replaced with 1-methyl-5-nitro-1H-pyrrole-2-carboxaldehyde (Accel Pharmtec). The structure is: 1 The results were confirmed by H-NMR and IR.
[0087] [Synthesis Example 13: Synthesis of Exemplary Compound 22] Exemplary compound 22 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiopheneamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0088] [Synthesis Example 14: Synthesis of Exemplary Compound 24] Exemplary compound 24 was synthesized in the same manner as in Synthesis Example 1, except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) was replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure is: 1 The results were confirmed by H-NMR and IR.
[0089] [Synthesis Example 15: Synthesis of Exemplary Compound 29] Exemplary compound 29 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 3-fluoro-4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furanamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0090] [Synthesis Example 16: Synthesis of Exemplary Compound 35] Exemplary compound 35 was synthesized in the same manner as in Synthesis Example 1, except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) was replaced with 5-nitro-1-phenylmethyl-1H-pyrrole-2-carboxaldehyde (manufactured by Chemieliva Pharmaceutical Co., Ltd.). The structure is: 1 The results were confirmed by H-NMR and IR.
[0091] [Synthesis Example 17: Synthesis of Exemplary Compound 36] Exemplary compound 36 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-methyl-5-nitro-2-furancarboxaldehyde (manufactured by Aurora Fine Chemicals LLC) and 5-nitro-2-furanamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0092] [Synthesis Example 18: Synthesis of Exemplary Compound 37] Exemplary compound 37 was synthesized in the same manner as in Synthesis Example 1, except that 4-nitroaniline (Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furanamine (Aurora Fine Chemicals LLC), and a half amine in which a 5-aminopentenoyl group was introduced into the amine of the furan ring was used as azomethine-2NH2. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0093] [Synthesis Example 19: Synthesis of Exemplary Compound 39] 5-Nitro-2-thiophenamine (manufactured by Chemieliva Pharmaceutica) and 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 8 were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiophenamine (manufactured by Aurora Fine Chemicals LLC), and 5-aminopentanoyl chloride (manufactured by Aurora Fine Chemicals LLC5) was replaced with 4-aminobenzoyl chloride (manufactured by Aurora Fine Chemicals LLC). Exemplary Compound 39 was synthesized in the same manner. The structure was 1 confirmed by 1H-NMR and IR.
[0094] 〔Synthesis Example 20: Synthesis of Exemplary Compound 44〕 Exemplary Compound 44 was synthesized in the same manner except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Inc.) in Synthesis Example 1 were replaced with 3-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 3-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure was 1 confirmed by 1H-NMR and IR.
[0095] 〔Synthesis Example 21: Synthesis of Exemplary Compound 52〕 <Synthesis of Exemplary Compound 52 Protected by CF3CO> Into a 1000 ml eggplant flask, 4-nitrophenyl 3-(6-trifluoroacetamidopurin-9-yl)propionate (23.2 g, 54.7 mmol) synthesized in <Synthesis of Adenine CF3-COOPhNO2 (Active Ester)> of Synthesis Example 1, imidazole (4.2 g, 62.1 mmol), azomethine-2NH2 (5.0 g, 24.8 mmol) synthesized in <Synthesis of Azomethine-2NH2> of Synthesis Example 1, and 500 ml of DMF were added and dissolved by stirring at room temperature. Then, after reacting at room temperature for 3 days, it was concentrated under reduced pressure using a rotary evaporator to obtain a solid content. The obtained solid content was washed with water and then washed with diethyl ether. The washed solid content was purified by column chromatography using a methylene chloride / methanol-based solvent. As a result, 8.1 g (yield 42%) of Exemplary Compound 52 protected by CF3CO was obtained. The structure was 1It was confirmed by 1H-NMR and IR.
[0096] <Synthesis of Exemplary Compound 52 (Deprotection of CF3CO)> To a 200 ml eggplant flask, potassium carbonate (2.0 g, 20.7 mmol) and 30 ml of water were added and dissolved by stirring at room temperature. Then, the CF3CO-protected exemplary compound 52 (8.0 g, 10.4 mmol) synthesized in the above <Synthesis of Exemplary Compound 52 Protected with CF3CO> was added to the solution containing 30 ml of methanol, and the mixture was stirred at room temperature for 12 hours. It was concentrated under reduced pressure using a rotary evaporator, and the obtained solid content was washed with water. The obtained solid was redissolved in ethanol and reprecipitated and purified by slowly dropping it into vigorously stirred water. By drying this solid content in a vacuum oven at 50 °C, 5.5 g of exemplary compound 52 was obtained (yield 91%). The structure was 1 It was confirmed by 1H-NMR and IR.
[0097] 〔Synthesis Example 22: Synthesis of Exemplary Compound 48〕 <Synthesis of Exemplary Compound 48> To a 1000 ml eggplant flask, pentachlorophenyl 3-(2,4-dihydroxy-5-methylpyrimidin-1-yl)propionate (22.2 g, 54.7 mmol) synthesized in <Synthesis of Thymine-COOPhCl5 (Active Ester)> of <Synthesis of Thymine-COOPhCl5 (Active Ester)>, azomethine-2NH2 (5.0 g, 24.8 mmol) synthesized in <Synthesis of Azomethine-2NH2> of Synthesis Example 1, and 300 ml of DMF were added and dissolved by stirring at room temperature. Then, after reacting at room temperature for 12 hours, it was concentrated under reduced pressure using a rotary evaporator to obtain a solid content. The obtained solid content was washed with water and then washed with acetone. The washed solid content was purified by column chromatography using a methylene chloride / methanol-based solvent. As a result, 14.2 g (yield 51%) of the CF3CO-protected exemplary compound 48 was obtained. The structure was 1 It was confirmed by 1H-NMR and IR.
[0098] 〔Synthesis Example 23: Synthesis of Exemplary Compound 55〕 Exemplary compound 55 was synthesized in the same manner as in Synthesis Example 21, except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) was replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure is: 1 The results were confirmed by H-NMR and IR.
[0099] [Synthesis Example 24: Synthesis of Exemplary Compound 51] Exemplary Compound 51 was synthesized in the same manner as in Synthesis Example 22, except that 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) was replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure was confirmed by 1H-NMR and IR.
[0100] [Synthesis Example 25: Synthesis of Exemplary Compound 57] Exemplary compound 57 was synthesized in the same manner as in Synthesis Example 21, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 3-fluoro-4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiophenecarboxaldehyde (manufactured by Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0101] [Synthesis Example 26: Synthesis of Exemplary Compound 58] Exemplary compound 58 was synthesized in the same manner as in Synthesis Example 22, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) was replaced with 5-nitro-2-furanamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0102] [Synthesis Example 27: Synthesis of Exemplary Compound 62] Azomethine-2NH2 was synthesized by replacing 5-nitro-2-furaldehyde (Kanto Chemical) in Synthesis Example 1 with 1-methyl-5-nitro-1H-pyrrole-2-carboxaldehyde (Accel Pharmtec). Azomethine-2NH2 (2) was synthesized by using azomethine-2NH2 and replacing 5-aminopentanoyl chloride (Aurora Fine Chemicals LLC) in Synthesis Example 8 with 3-amino-2-methylpropanoyl chloride (Aurora Fine Chemicals LLC). Then, Exemplary Compound 62 was synthesized in the same manner as in Synthesis Example 21. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0103] [Synthesis Example 28: Synthesis of Exemplary Compound 61] Azomethine-2NH2 was synthesized by replacing 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) in Synthesis Example 1 with 5-nitro-2-thiophenecarboxaldehyde (manufactured by Aldrich Co., Ltd.). Azomethine-2NH2 (2) was synthesized by using azomethine-2NH2 and replacing 5-aminopentanoyl chloride (manufactured by Aurora Fine Chemicals LLC) in Synthesis Example 8 with 3-amino-propanoyl chloride (manufactured by Aurora Fine Chemicals LLC). Then, Exemplary Compound 61 was synthesized in the same manner as in Synthesis Example 22. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0104] [Synthesis Example 29: Synthesis of Exemplary Compound 70] Exemplary compound 70 was synthesized in the same manner as in Synthesis Example 21, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 1-methyl-5-nitro-1H-pyrrol-2-amine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0105] [Synthesis Example 30: Synthesis of Exemplary Compound 66] Exemplary compound 66 was synthesized in the same manner as in Synthesis Example 22, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 1-methyl-5-nitro-1H-pyrrol-2-amine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0106] [Synthesis Example 31: Synthesis of Exemplary Compound 69] Exemplary compound 69 was synthesized in the same manner as in Synthesis Example 21, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiopheneamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0107] [Synthesis Example 32: Synthesis of Exemplary Compound 65] Exemplary compound 65 was synthesized in the same manner as in Synthesis Example 22, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-thiopheneamine (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0108] [Synthesis Example 33: Synthesis of Exemplary Compound 75] Exemplary compound 75 was synthesized in the same manner as in Synthesis Example 21, except that 4-nitroaniline (Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (Kanto Chemical Industry Co., Ltd.) were replaced with 1-methyl-5-nitro-1H-pyrrole-2-carboxaldehyde (Accel Pharmtec Co., Ltd.) and 5-nitro-2-furanamine (Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0109] [Synthesis Example 34: Synthesis of Exemplary Compound 72] Exemplary compound 72 was synthesized in the same manner as in Synthesis Example 22, except that 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Industry Co., Ltd.) were replaced with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 3-methyl-4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure is: 1 The results were confirmed by H-NMR and IR.
[0110] [Synthesis Example 35: Synthesis of Exemplary Compound 79] Azomethine-2NH2 was synthesized by replacing 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Ltd.) in Synthesis Example 1 with 3-fluoro-4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.). Azomethine-2NH2 (2) was synthesized by using azomethine-2NH2 and replacing 5-aminopentanoyl chloride (manufactured by Aurora Fine Chemicals LLC) in Synthesis Example 8 with 4-aminobenzoyl chloride (manufactured by Aurora Fine Chemicals LLC). Then, Exemplary Compound 79 was synthesized in the same manner as in Synthesis Example 21. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0111] [Synthesis Example 36: Synthesis of Exemplary Compound 77] Azomethine-2NH2 was synthesized from 5-nitro-2-furaldehyde (Kanto Chemical) in Synthesis Example 1 and 5-nitro-2-thiophenecarboxaldehyde (Aldrich). Azomethine-2NH2 (2) was synthesized using azomethine-2NH2 in the same manner as in Synthesis Example 8. Then, Exemplary Compound 77 was synthesized in the same manner as in Synthesis Example 22. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0112] [Synthesis Example 37: Synthesis of Exemplary Compound 80] <Synthesis of 2,6-diacetamidopyridine-NO2> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, dropping funnel, and thermometer, 50 ml of CH2Cl2, 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) (5.0 g, 22.4 mmol), and triethylamine (Tokyo Chemical Industry) (4.1 g, 40.3 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature below 10°C. Then, 4-nitrobenzoyl chloride (Sigma-Aldrich) (5.0 g, 26.9 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The washed solid was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 7.0 g (84% yield) of 2,6-diacetamidopyridine-NO2 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0113] <Synthesis of 2,6-diacetamidopyridine-NH2> 2,6-Diacetamidopyridine-NO2 (7.0g, 18.8mmol) and palladium carbon (0.09g, 188mmol) were placed in a 200ml Erlenmeyer flask, 30ml each of ethanol and tetrahydrofuran were added, and the mixture was stirred while hydrogen was sealed in. Palladium carbon was removed from the reaction solution, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 5.9g (yield 84%) of 2,6-diacetamidopyridine-NH2.
[0114] <Synthesis of 5-formyl-2-furancarbonyl chloride> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CHCl, 5-formyl-2-furan carboxylic acid (Sigma-Aldrich) (5.5 g, 39.3 mmol) and a few drops of DMF were added and dissolved at room temperature by stirring. The solution was cooled in an ice bath and the liquid temperature was maintained below 10°C. Then, oxalyl chloride (Tokyo Chemical Industry) (5.5 g, 43.2 mmol) was added dropwise over 30 minutes, and then the ice bath was removed to return the liquid temperature to room temperature and stirred for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and 50 ml of CHCl was added again, followed by concentration under reduced pressure using a rotary evaporator. This operation was repeated three times. As a result, 6.2 g of 5-formyl-2-furan carboxylic acid was obtained (yield 99%).
[0115] <Synthesis of Uracil-CHO> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CHCl, 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical) (5.0 g, 32.0 mmol), and triethylamine (Tokyo Chemical Industry) (4.9 g, 48.0 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature at 10°C or less. Then, 5-formyl-2-furancarbonyl chloride (6.1 g, 38.4 mmol) synthesized above was added dropwise over 30 minutes, and the mixture was stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 8.7 g of uracil-CHO was obtained (yield 81%). The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0116] <Synthesis of Example Compound 80> The diaminopyridine-NH2 (5.0 g, 14.6 mmol) and uracil-CHO (4.1 g, 14.6 mmol) synthesized above and 30 ml of ethanol were placed in a 50 ml four-neck flask equipped with a cooling tube, a nitrogen inlet tube, and a thermometer, and the mixture was heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. The mixture was further purified by column chromatography using a methylene chloride / methanol solvent. As a result, 5.7 g (yield 65%) of exemplary compound 80 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0117] [Synthesis Example 38: Synthesis of Exemplary Compound 85] Exemplary compound 85 was synthesized in the same manner as in Synthesis Example 37, except that 5-formyl-2-furan carboxylic acid (Sigma-Aldrich) was replaced with 5-formyl-2-thiophene carboxylic acid (Sigma-Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0118] [Synthesis Example 39: Synthesis of Exemplary Compound 90] Exemplary compound 90 was synthesized in the same manner as in Synthesis Example 37, except that 4-nitrobenzoyl chloride (Sigma-Aldrich) and 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) were replaced with 3-formyl-5-methylbenzoyl chloride (Aurora Fine Chemicals LLC) and 1-methyl-5-nitro-1H-pyrrole-2-carboxylic acid (Sigma-Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0119] [Synthesis Example 40: Synthesis of Exemplary Compound 95] <Synthesis of 2,6-diacetamidopyridine-NH2> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CH2Cl2, 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) (6.0 g, 26.9 mmol), and triethylamine (Tokyo Chemical Industry) (4.9 g, 48.4 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature at 10°C or less. Then, 4-aminopropanoyl chloride (Aurora Fine Chemicals LLC) (3.5 g, 32.3 mmol) was added dropwise over 30 minutes, and the mixture was stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 7.0 g (88% yield) of 2,6-diacetamidopyridine-NH2 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0120] <Synthesis of 2,6-diacetamidopyridine-NO2> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CH2Cl2, the 2,6-diacetamidopyridine-NH2 (7.0 g, 23.8 mmol) synthesized above, and triethylamine (Tokyo Chemical Industry Co., Ltd.) (4.3 g, 42.8 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath and the liquid temperature was maintained at 10°C or less. Then, 3-nitrobenzoyl chloride (Tokyo Chemical Industry Co., Ltd.) (5.3 g, 28.5 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 8.4 g (80% yield) of 2,6-diacetamidopyridine-NO2 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0121] <Synthesis of 2,6-diacetamidopyridine-NH2(2)> 2,6-Diacetamidopyridine-NO2 (7.0g, 15.8mmol) and palladium carbon (0.07g, 158mmol) were placed in a 200ml Erlenmeyer flask, 30ml each of ethanol and tetrahydrofuran were added, and the mixture was stirred while hydrogen was sealed in. Palladium carbon was removed from the reaction solution, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 5.4g (yield 82%) of 2,6-diacetamidopyridine-NH2 (2).
[0122] <Synthesis of Uracil-NH2> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CHCl, 1-N-methyl-6-(hydroxyethyl)uracil (manufactured by Chemieliva Pharmaceutical) (5.0 g, 32.0 mmol) (6.0 g, 26.9 mmol), and triethylamine (manufactured by Tokyo Kasei Co., Ltd.) (5.8 g, 57.6 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath and the liquid temperature was maintained at 10°C or less. Then, 4-aminopropanoyl chloride (manufactured by Aurora Fine Chemicals LLC) (4.1 g, 38.4 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 5.9 g of uracil-NH2 (yield 81%) was obtained. The structure is: 1 The results were confirmed by H-NMR and IR.
[0123] <Synthesis of Uracil-CHO> Into a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CH2Cl2, the uracil-NH2 (5.0 g, 22.0 mmol) synthesized above, and triethylamine (Tokyo Chemical Industry Co., Ltd.) (3.3 g, 33.0 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath and the liquid temperature was maintained at 10°C or less. Then, 4-formyl-2,5-dimethoxybenzoyl chloride (6.0 g, 26.4 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 8.4 g of uracil-CHO was obtained (yield 76%). The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0124] <Synthesis of Example Compound 95> The diaminopyridine-NH2(2) (5.0 g, 12.1 mmol) and uracil-CHO (5.1 g, 12.1 mmol) synthesized above and 30 ml of ethanol were placed in a 50 ml four-neck flask equipped with a cooling tube, a nitrogen inlet tube, and a thermometer, and the mixture was heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. The mixture was further purified by column chromatography using a methylene chloride / methanol solvent. As a result, 6.1 g (yield 64%) of exemplary compound 95 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0125] [Synthesis Example 41: Synthesis of Exemplary Compound 96] Exemplary compound 96 was synthesized with reference to the method used in Synthesis Example 37. <Synthesis of 2,6-diacetamidopyridine-CHO> 2,6-Diacetamidopyridine-CHO was synthesized in the same manner as in Synthesis Example 37 <Synthesis of Uracil-CHO>, except that 1-N-methyl-6-(hydroxyethyl)uracil (manufactured by Chemieliva Pharmaceutical) was replaced with 2,6-diacetamido-4-hydroxymethylpyridine (manufactured by Apichemical). The structure is: 1The results were confirmed by H-NMR and IR.
[0126] <Synthesis of Exemplary Compound 96> Exemplary compound 96 was synthesized in the same manner as in <Synthesis of exemplary compound 80> in Synthesis Example 37, using 2,6-diacetamidopyridine-CHO synthesized in <Synthesis of 2,6-diacetamidopyridine-CHO> in Synthesis Example 41 and 2,6-diacetamidopyridine-NH2 synthesized in <Synthesis of 2,6-diacetamidopyridine-NH2> in Synthesis Example 37. The structure is: 1 The results were confirmed by H-NMR and IR.
[0127] [Synthesis Example 42: Synthesis of Exemplary Compound 98] Exemplary compound 98 was synthesized by referring to the method used in Synthesis Example 41, except that 4-nitrobenzoyl chloride (Sigma-Aldrich) and 5-formyl-2-furan carboxylic acid (Sigma-Aldrich) were replaced with 4-formylbenzoyl chloride (Sigma-Aldrich) and 5-amino-1-methyl-1H-pyrrole carboxylic acid (Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0128] [Synthesis Example 43: Synthesis of Exemplary Compound 99] Exemplary compound 99 was synthesized by referring to the method used in Synthesis Example 41, except that 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) was replaced with 3-formylbenzoyl chloride (Sigma-Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0129] [Synthesis Example 44: Synthesis of Exemplary Compound 101] The reaction of 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) and 4-aminopropanoyl chloride (Aurora Fine Chemicals LLC) was carried out in the same manner as in Synthesis Example 40 <Synthesis of uracil-NH2>, except that 4-nitrobenzoyl chloride (Sigma-Aldrich) and 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) in Synthesis Example 41 were replaced with 4-formylbenzoyl chloride (Sigma-Aldrich) and 5-nitro-2-thiophenamine (Aurora Fine Chemicals LLC). In addition, the reaction between the compound obtained from 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) and 4-aminopropanoyl chloride (Aurora Fine Chemicals LLC) and 3-formibenzoyl chloride was performed in the same manner as in Synthesis Example 40 <Synthesis of Uracil-CHO>, and the rest was synthesized using the method of Synthesis Example 41 to synthesize Exemplary Compound 101. The structure is: 1 The results were confirmed by H-NMR and IR.
[0130] [Synthesis Example 45: Synthesis of Exemplary Compound 107] Except for replacing 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) with 4-formylbenzoyl chloride (Sigma-Aldrich), and further replacing 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) with 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical), the exemplary compound 107 was synthesized using the method of Synthesis Example 41. The structure is: 1 The results were confirmed by H-NMR and IR.
[0131] [Synthesis Example 46: Synthesis of Exemplary Compound 108] Exemplary compound 108 was synthesized using the method of Synthesis Example 41, except that 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) and 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical) were replaced with 6-(2-aminoethyl)-1-methyl-2,4-pyrimidinedione (Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0132] [Synthesis Example 47: Synthesis of Exemplary Compound 109] Except for replacing 4-nitrobenzoyl chloride (Sigma-Aldrich) and 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) with 4-formylbenzoyl chloride (Sigma-Aldrich) and 5-nitro-2-thiophenamine (Aurora Fine Chemicals LLC), and further replacing 2,6-diacetamido-4-hydroxymethylpyridine (Apichemical) with 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical), exemplary compound 109 was synthesized using the method of Synthesis Example 41. The structure is: 1 The results were confirmed by H-NMR and IR.
[0133] [Synthesis Example 48: Synthesis of Exemplary Compound 111] The reaction of 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical) and 4-aminopropanoyl chloride (Aurora Fine Chemicals LLC) was carried out in the same manner as in Synthesis Example 40 <Synthesis of 2,6-diacetamidopyridine-NH2>, except that 4-nitrobenzoyl chloride (Sigma-Aldrich) and 5-formyl-2-furancarboxylic acid (Sigma-Aldrich) in Synthesis Example 41 were replaced with 3-nitrobenzoyl chloride (Tokyo Chemical Industry Co., Ltd.) and 2-cyano-4-formylbenzoic acid (Aurora Fine Chemicals LLC). In addition, the reaction between the compound obtained from 1-N-methyl-6-(hydroxyethyl)uracil (Chemieliva Pharmaceutical) and 4-aminopropanoyl chloride (Aurora Fine Chemicals LLC) and 3-nitrobenzoyl chloride (Tokyo Chemical Industry Co., Ltd.) was carried out in a similar manner to that of Synthesis Example 40 (Synthesis of 2,6-diacetamidopyridine-NO2), and the rest of the reaction was carried out in the same manner as in Synthesis Example 41 to synthesize Exemplary Compound 111. The structure is: 1 The results were confirmed by H-NMR and IR.
[0134] [Synthesis Example 49: Synthesis of Exemplary Compound 116] <Synthesis of Azomethine-NO2> 5-Nitro-2-furanamine (Aurora Fine Chemicals LLC) (6.0 g, 46.8 mmol), 2,4,6-trimethylbenzaldehyde (Tokyo Kasei Co., Ltd.) (6.9 g, 46.8 mmol), and 50 ml of ethanol were added to a 100 ml four-neck flask equipped with a condenser, nitrogen inlet tube, and thermometer, and the mixture was heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. The product was further purified by column chromatography using a methylene chloride / methanol solvent. As a result, 8.4 g (yield 69%) of azomethine-NO2 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0135] <Synthesis of Azomethine-NH2> A 200ml Erlenmeyer flask was charged with the above synthesized azomethine-NO2 (8.0g, 31.0mmol) and palladium carbon (0.14g, 310mmol), 30ml each of ethanol and tetrahydrofuran, and stirred while sealing in hydrogen. Palladium carbon was removed from the reaction solution, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 6.2g of azomethine-NH2 (yield 87%).
[0136] <Synthesis of azomethine-NH2(2)> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CH2Cl2, the above synthesized azomethine-NH2 (6.0 g, 26.9 mmol), and triethylamine (Tokyo Chemical Industry Co., Ltd.) (4.8 g, 47.3 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature below 10°C. Then, 3-aminopropanoyl chloride (Aurora Fine Chemicals LLC) (3.4 g, 31.5 mmol) was added dropwise over 30 minutes, and the mixture was stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 6.9 g (yield 88%) of azomethine-NH2 (2) was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0137] <Synthesis of Example Compound 116> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 100 ml of DMF, the above synthesized azomethine-NH2 (2) (6.0 g, 20.0 mmol), and sodium bicarbonate (Kanto Chemical Co., Ltd.) (3.0 g, 36.1 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature at 10°C or less. Then, diaminotriazine chloride (Sigma-Aldrich Co., Ltd.) (3.5 g, 24.1 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was poured into water, filtered, and the obtained solid was washed with water. The washed solid was dried and purified by column chromatography using a methylene chloride / methanol solvent. As a result, 6.0 g (73% yield) of the exemplary compound 116 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0138] [Synthesis Example 50: Synthesis of Exemplary Compound 113] Except for replacing 5-nitro-2-furanamine (manufactured by Aurora Fine Chemicals LLC) and 2,4,6-trimethylbenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 49 with 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-butyl-2-thiophenecarboxaldehyde (manufactured by Sigma-Aldrich Co., Ltd.), Exemplary Compound 113 was synthesized using the method of Synthesis Example 41. The structure is: 1 The results were confirmed by H-NMR and IR.
[0139] [Synthesis Example 51: Synthesis of Exemplary Compound 115] Except for replacing 5-nitro-2-furanamine (manufactured by Aurora Fine Chemicals LLC) and 2,4,6-trimethylbenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 49 with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4-dodecylaniline (manufactured by Tokyo Chemical Industry Co., Ltd.), Example Compound 115 was synthesized using the method of Synthesis Example 41. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0140] [Synthesis Example 52: Synthesis of Exemplary Compound 123] <Synthesis of Azomethine-NO2> The above synthesized azomethine-NO2 (8.0 g, 56.7 mmol), 4-decylaniline (Tokyo Chemical Industry Co., Ltd.) (13.2 g, 56.7 mmol), and 100 ml of ethanol were added to a 100 ml four-neck flask equipped with a cooling tube, nitrogen inlet tube, and thermometer, and the mixture was heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. The mixture was further purified by column chromatography using a methylene chloride / methanol solvent. As a result, 14.6 g (72% yield) of azomethine-NO2 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0141] <Synthesis of Azomethine-NH2> A 200 ml Erlenmeyer flask was charged with the above synthesized azomethine-NO2 (14.0 g, 39.3 mmol) and palladium-carbon (0.18 g, 393 mmol), 50 ml each of ethanol and tetrahydrofuran, and the mixture was stirred while hydrogen was sealed in. The palladium-carbon was removed from the reaction solution, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 11.0 g of azomethine-NH2 (yield 87%).
[0142] <Synthesis of Azomethine-NO2(2)> Into a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CH2Cl2, the above synthesized azomethine-NH2 (11.0 g, 33.7 mmol), and triethylamine (Tokyo Chemical Industry Co., Ltd.) (6.1 g, 60.6 mmol) were added, and the mixture was stirred at room temperature to dissolve. The solution was cooled in an ice bath, and the liquid temperature was maintained below 10°C. Then, 4-nitrobenzoyl chloride (Tokyo Chemical Industry Co., Ltd.) (7.5 g, 40.4 mmol) was added dropwise over 30 minutes, and the mixture was stirred at room temperature for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and the obtained solid was washed with water. The solid after washing was purified by column chromatography using a methylene chloride / methanol solvent. As a result, 13.1 g (82% yield) of azomethine-NO2 (2) was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0143] <Synthesis of azomethine-NH2(2)> A 200 ml Erlenmeyer flask was charged with the above synthesized azomethine-NO2 (13.0 g, 27.3 mmol) and palladium carbon (0.13 g, 273 mmol), 30 ml each of ethanol and tetrahydrofuran, and the mixture was stirred while hydrogen was sealed in. The palladium carbon was removed from the reaction solution, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 10.5 g of azomethine-NH2 (2) (yield 87%).
[0144] <Synthesis of Example Compound 123> In a 300 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 100 ml of CH2Cl2, the above synthesized azomethine-NH2 (2) (10.0 g, 22.4 mmol), and triethylamine (Tokyo Chemical Industry Co., Ltd.) (4.1 g, 40.4 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature at 10°C or less. N-chlorocarbonyl isocyanate (Aurora Fine Chemicals LLC) (2.8 g, 26.9 mmol) was then added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was poured into water, filtered, and the obtained solid was washed with water. The washed solid was dried and purified by column chromatography using a methylene chloride / methanol solvent. As a result, 7.3 g (80% yield) of the exemplary compound 123 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0145] [Synthesis Example 53: Synthesis of Exemplary Compound 125] Except for replacing 4-decylaniline (Tokyo Chemical Industry Co., Ltd.) and 4-nitrobenzoyl chloride (Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 52 with 1-methyl-5-nitro-1H-pyrrole-2-carboxaldehyde (Accel Pharmtec) and 4-dodecylaniline (Tokyo Chemical Industry Co., Ltd.), the exemplary compound 125 was synthesized by the method of Synthesis Example 41. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0146] [Synthesis Example 54: Synthesis of Exemplary Compound 122] Except for replacing 4-nitrobenzoyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) in Synthesis Example 52 with 4-nitrobenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.), the method of Synthesis Example 41 was used to synthesize Exemplary Compound 122. The structure is: 1 The results were confirmed by H-NMR and IR.
[0147] [Synthesis Example 55: Synthesis of Exemplary Compound 131] <Synthesis of Azomethine-COOH> 5-Amino-2-thiophenecarboxylic acid (Aurora Fine Chemicals LLC) (15.0 g, 104.8 mmol), 4-isobutylbenzaldehyde (Tokyo Chemical Industry Co., Ltd.) (17.0 g, 104.8 mmol), and 100 ml of ethanol were added to a 200 ml four-neck flask equipped with a condenser, nitrogen inlet tube, and thermometer, and the mixture was heated and stirred at 50°C. The reaction liquid was suction filtered, and the resulting powder was washed with cooled ethanol. The product was further purified by column chromatography using a methylene chloride / methanol solvent. As a result, 21.7 g (72% yield) of azomethine-COOH was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0148] <Synthesis of azomethine-COCl> In a 100 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 50 ml of CHCl2, the azomethine-COOH (20.0 g, 69.6 mmol) synthesized above, and a few drops of DMF were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath, and the liquid temperature was maintained at 10°C or less. Then, oxalyl chloride (Tokyo Chemical Industry Co., Ltd.) (9.2 g, 76.6 mmol) was added dropwise over 30 minutes, and then the ice bath was removed, the liquid temperature was returned to room temperature, and the mixture was stirred for 5 hours. The solution was concentrated under reduced pressure using a rotary evaporator, and 50 ml of CHCl2 was added again, followed by concentration under reduced pressure using a rotary evaporator. This operation was repeated three times. As a result, 21.1 g of azomethine-COCl was obtained (yield 99%).
[0149] <Synthesis of dicarbonitriles> In a 200 ml Erlenmeyer flask, malonitrile (Tokyo Chemical Industry Co., Ltd.) (15.0 g, 0.23 mol), 4-acetoxybenzaldehyde (Sigma-Aldrich Co., Ltd.) (41.0 g, 0.25 mol), palladium carbon (1.1 g, 2.27 mol), and 30 ml of acetic acid were added, and a solution of 0.8 ml of piperidine dissolved in 10 ml of acetic acid was further added. This solution was stirred for 18 hours while sealing hydrogen. The reaction solution was filtered to remove palladium carbon, and the resulting solution was concentrated and then recrystallized from ethanol to obtain 34.0 g of dicarbonitrile (yield 70%).
[0150] <Synthesis of diaminopyrimidine-OAc> A 500ml four-neck flask was equipped with two three-way stopcocks, a thermometer, a dropping funnel and a ball stopper, and the pressure in the container was reduced, followed by nitrogen replacement. This operation was repeated three times. While flowing nitrogen, the dicarbonitrile (30.0g, 0.14mol), sodium ethoxide (9.5g, 0.14mol), thiourea (10.7g, 0.14mol) and 150ml of dehydrated ethanol (Kanto Chemical Co., Ltd.) were added and stirred at 80°C for 5 hours. After the solution was cooled to room temperature, 125ml of water was added while stirring, and the solution was neutralized to near neutrality with hydrochloric acid. The solid matter obtained by filtration was suspended in 375ml of water, to which chloroacetic acid (Tokyo Chemical Co., Ltd.) (33.1g, 0.35mol) was added, and the mixture was stirred at 100°C for 3 hours. After the solution was cooled to room temperature, 40ml of concentrated sulfuric acid was carefully added while stirring. The mixture was then stirred again at 100°C for 3 hours. The solution was cooled to room temperature and the solids were filtered. The solids were placed in a 500ml four-neck flask, and saturated NaHCO3 aqueous solution was added until the solution became neutral, and the solution was stirred at 70°C for 10 hours. The solution was filtered to obtain 28.0g of diaminopyrimidine-OAc (73% yield).
[0151] <Synthesis of diaminopyrimidine-OH> The diaminopyrimidine-OAc (25.0 g, 91.1 mmol) synthesized above and 100 ml of THF were added to a 300 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, and then 6N hydrochloric acid (Kanto Chemical Co., Ltd.) (45.5 g, 45.6 mmol) was added and the mixture was heated to reflux at 70°C for 3 hours. The solution was neutralized to near neutrality with an aqueous sodium hydroxide solution, and the organic layer was separated using a separatory funnel. The organic layer was dried over MgSO4, and the filtered organic layer was concentrated using a rotary evaporator to obtain 20.3 g of diaminopyrimidine-OH (yield 96%).
[0152] <Synthesis of diaminopyrimidine-NH2> In a 200 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 100 ml of CH2Cl2, the diaminopyrimidine-OH (20.0 g, 86.1 mmol) synthesized above, and triethylamine (Tokyo Chemical Industry Co., Ltd.) (12.5 g, 124.0 mmol) were added and stirred at room temperature to dissolve. The solution was cooled in an ice bath to maintain the liquid temperature at 10°C or less. Then, 5-aminopentanoyl chloride (Aurora Fine Chemicals LLC) (14.0 g, 103.3 mmol) was added dropwise over 30 minutes and stirred at room temperature for 5 hours. The solution was poured into water, filtered, and the obtained solid was washed with water. The washed solid was dried and purified by column chromatography using a methylene chloride / methanol solvent. As a result, 10.3 g of diaminopyrimidine-NH2 (yield 36%) was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0153] <Synthesis of Example Compound 131> In a 200 ml 4-neck flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer, 100 ml of CH2Cl2, the diaminopyrimidine-NH2 (10.0 g, 30.2 mmol) synthesized above, and triethylamine (Tokyo Chemical Industry Co., Ltd.) (7.3 g, 72.4 mmol) were added, and the mixture was stirred at room temperature to dissolve. The solution was cooled in an ice bath, and the liquid temperature was maintained at 10°C or less. Then, the azomethine-COCl (18.5 g, 60.4 mmol) synthesized above was added dropwise over 30 minutes, and the mixture was stirred at room temperature for 5 hours. The solution was poured into water, filtered, and the obtained solid was washed with water. The washed solid was dried and purified by column chromatography using a methylene chloride / methanol solvent. As a result, 6.0 g (yield 38%) of the exemplary compound 131 was obtained. The structure is as follows: 1 The results were confirmed by H-NMR and IR.
[0154] [Synthesis Example 56: Synthesis of Exemplary Compound 126] Exemplary compound 126 was synthesized by using the method of Synthesis Example 55, except that 5-amino-2-thiophene carboxylic acid (manufactured by Aurora Fine Chemicals LLC) and 4-isobutylbenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.) were replaced with 4-aminobenzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-pentyl-2-furan carboxaldehyde (manufactured by Aurora Fine Chemicals LLC). The structure is: 1 The results were confirmed by H-NMR and IR.
[0155] [Synthesis Example 57: Synthesis of Exemplary Compound 132] Exemplary compound 132 was synthesized using the method of Synthesis Example 55, except that 5-amino-2-thiophene carboxylic acid (Aurora Fine Chemicals LLC), 4-isobutylbenzaldehyde (Tokyo Chemical Industry Co., Ltd.), and 5-aminopentanoyl chloride (Aurora Fine Chemicals LLC) were replaced with 5-formyl-1-methyl-1H-pyrrole-2-carboxylic acid (Sigma-Aldrich), 4-hexylaniline (Tokyo Chemical Industry Co., Ltd.), and 3-aminopropenoyl chloride (Sigma-Aldrich). The structure is: 1 The results were confirmed by H-NMR and IR.
[0156] [Synthesis Example 58: Synthesis of Exemplary Compound 129] Exemplary Compound 129 was synthesized using the same method as in Synthesis Example 55, except that 5-amino-2-thiophenecarboxylic acid (manufactured by Aurora Fine Chemicals LLC), 4-isobutylbenzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.), and 5-aminopentanoyl chloride (manufactured by Aurora Fine Chemicals LLC) were replaced with 4-formylbenzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 4-hexylaniline (manufactured by Tokyo Chemical Industry Co., Ltd.), and 3-aminobutanoyl chloride (manufactured by Sigma-Aldrich Co., LLC). The structure was confirmed by 1 1H-NMR and IR.
[0157] [Synthesis Example 59: Synthesis of Exemplary Compound 133] [Synthesis of Azomethine-2NO2] In the same manner as in Synthesis Example 1, Azomethine-2NO2 was synthesized from 4-nitroaniline (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5-nitro-2-furaldehyde (manufactured by Kanto Chemical Co., Inc.).
[0158] [Synthesis of Azomethine-2NH2] Azomethine-2NH2 was synthesized by the same method as in Synthesis Example 1.
[0159] [Synthesis of UPy-COOH] N-(1,6-Dihydro-4-methyl-6-oxo-2-pyrimidinyl)-1H-imidazole-1-carboxamide (manufactured by Chemieliva Pharmaceutical Co., Ltd.) (50.0 g, 0.23 mol) and 500 ml of DMF were charged into a 1000 ml four-necked flask equipped with a nitrogen inlet tube, a dropping funnel, and a thermometer. Subsequently, 7-aminoheptanoic acid (manufactured by Sigma-Aldrich Co., LLC) (49.7 g, 0.34 mol) was gradually added, and the mixture was stirred at room temperature for 12 hours. Then, the solution was poured into water, and the solid content was collected by filtration and dried under reduced pressure at 50 °C. This solid content was purified by column chromatography using a methylene chloride / methanol solvent system. As a result, 56.8 g (yield 84%) of UPy-COOH was obtained. The structure was 1It was confirmed by 1H-NMR and IR.
[0160] <Synthesis of UPy-COOPhCl5 (active ester)> To a 2 L four-necked flask, 1000 mL of DMF, 400 mL of triethylamine, and pentachlorophenyl trichloroacetate (138.9 g, 0.34 mol) were added and completely dissolved by stirring at room temperature. UPy-COOH (50.0 g, 0.17 mol) was added to this solution and reacted at room temperature for 20 h. Then, DMF, triethylamine, etc. were distilled off under reduced pressure until the solution solidified. The obtained solid was taken out of the flask and washed with cold water on a Buchner funnel. After drying this solid in a vacuum oven at 50 °C, recrystallization with CHCl3 / MeOH gave 34.9 g of UPy-COOPhCl5 (yield 38%). The structure was 1 It was confirmed by 1H-NMR and IR.
[0161] <Synthesis of Exemplary Compound 133> To a 500 mL eggplant flask, the UPy-COOPhCl5 (29.8 g, 54.7 mmol) synthesized above, the azomethine-2NH2 (5.0 g, 24.8 mmol) synthesized above, and 200 mL of CH2Cl2 were charged and dissolved by stirring at room temperature. Then, after reacting at room temperature for 12 h, it was concentrated under reduced pressure using a rotary evaporator to obtain a solid content. The obtained solid content was washed with water and then washed with acetone. The washed solid content was purified by column chromatography using a methylene chloride / methanol-based solvent. As a result, 12.6 g (yield 67%) of Exemplary Compound 133 was obtained. The structure was 1 It was confirmed by 1H-NMR and IR.
[0162] 〔Synthesis Example 60: Synthesis of Exemplary Compound 134〕 Exemplary Compound 134 was synthesized using the method of Synthesis Example 59, except that the azomethine-2NH2 and 7-aminoheptanoic acid (manufactured by Sigma-Aldrich) in Synthesis Example 59 were replaced with the azomethine-2NH2 and 7-amino-4-methylheptanoic acid (manufactured by Aurora Fine Chemicals LLC) used in Synthesis Example 28. The structure was 1 It was confirmed by 1H-NMR and IR.
[0163] [Synthesis Example 61: Synthesis of Exemplary Compound 135] Except for replacing the azomethine-2NH2, 7-aminoheptanoic acid (Sigma-Aldrich) used in Synthesis Example 59 with the azomethine-2NH2, 7-amino-5-ethylheptanoic acid (Aurora Fine Chemicals LLC) used in Synthesis Example 2, the method of Synthesis Example 59 was used to synthesize Exemplary Compound 135. The structure is: 1 The results were confirmed by H-NMR and IR.
[0164] [Synthesis Example 62: Synthesis of Exemplary Compound 136] Exemplary compound 136 was synthesized by the method of Synthesis Example 59, except that azomethine-2NH2, 7-aminoheptanoic acid (Sigma-Aldrich) was replaced with azomethine-2NH2, 7-aminoundecanoic acid (Aurora Fine Chemicals LLC) used in Synthesis Example 14. The structure is: 1 The results were confirmed by H-NMR and IR.
[0165] Regarding the synthesis of compounds other than those exemplified above, they can be synthesized with reference to the methods shown above, without any particular limitations.
[0166] In the resin composition of the present invention, in order to form a supramolecular polymer consisting of complementary multiple hydrogen bonds, it is preferable to use one or more types of the compound having the structure represented by the general formula (1) depending on the type of the compound.
[0167] <Complementary multiple hydrogen bonds> In the present invention, the complementary multiple hydrogen bonds are known to be pairs of guanine / cytosine and adenine / thymine that form hydrogen bonds between nucleic acid bases, as shown below.
[0168] [ka]
[0169] In guanine, the hydrogen atoms of NH and N-H2 are donors, and the shared electron pair of the carbonyl oxygen is the acceptor, while in its counterpart, cytosine, the hydrogen atom of N-H2 is the donor, the shared electron pair of the nitrogen atom, and the carbonyl oxygen are the acceptors. The donor part of guanine forms multiple complementary hydrogen bonds by hydrogen bonding with the acceptor part of cytosine. For example, when a compound having two guanine units and two cytosine units at the molecular end is dissolved and mixed in a solution, the guanine / cytosine units form complementary multiple hydrogen bonds in the solution, and by repeating this process, a supramolecular polymer is formed. Although the bond energy of each hydrogen bond is small, the formation of multiple multiple hydrogen bonds results in the physical properties of a polymer.
[0170] Examples of sites that form complementary multiple hydrogen bonds include nucleic acid base pairs such as guanine / cytosine, adenine / thymine, adenine / uracil, and guanine / cytosine, barbituric acid / 2,4,6-triaminopyrimidine, 2,6-diacetylaminopyridine / uracil, 2,4-diamino-1,3,5-triazine / 1H-benzo[de]isoquinoline-1,3-dione, melamine / cyanuric acid, melamine / barbituric acid, 4,6-diamino-2-pyrimidinone / 2-amino-4,6-pyrimidinedione, etc. Examples of sites that form complementary multiple hydrogen bonds in one structure include 4,6-diamino-2-pyrimidinone, 2-amino-4,6-pyrimidinedione, 2-amino-4-acylamino-1,3,5-triazine, urea, thiourea, and 2-ureidopyrimidinone. Of these, adenine / thymine, 2,6-diacetylaminopyridine / uracil, melamine / cyanuric acid, 4,6-diaminopyrimidinone, and 2-ureido-4-pyrimidinone are preferred.
[0171] <Ratio of Compound A and Compound B> When two compounds having a structure represented by the general formula (1) of the present invention are used to form complementary multiple hydrogen bonds, if the molar number is different and one of the compounds is in excess, the excess compound will not form a supramolecular compound but will function as a plasticizer for the composition, making it impossible to obtain the desired physical properties. Therefore, when two compounds having a structure represented by the general formula (1) of the present invention are used to form complementary multiple hydrogen bonds, it is preferable to use them in equimolar amounts.
[0172] The resin composition of the present invention also contains a resin.
[0173] <Resin> The resin constituting the resin composition of the present invention is not particularly limited, and examples thereof include polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, styrene-butadiene-acrylonitrile resin (ABS resin), acrylonitrile-styrene resin (AS resin), acrylic resins such as polymethyl methacrylate (PMMA), polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyolefins such as glass fiber reinforced polyethylene terephthalate and polybutylene terephthalate. Although there is no particular limitation as long as the resin is a thermoplastic resin such as a cellulose derivative such as a cellulose ester, a cyclic polyolefin, polyphenylene sulfide, polytetrafluoroethylene, polysulfone, polyethersulfone, amorphous polyarylate, liquid crystal polymer, polyetheretherketone, polyimide, polyamideimide, polylactic acid, or a cellulose ester, or a copolymer thereof, the resin used in the present invention is preferably an acrylic resin such as polymethyl methacrylate (PMMA), a polyester such as polycarbonate, polyethylene terephthalate, or polybutylene terephthalate, a styrene-acrylic copolymer, or a polyester. In addition, for the toner, a styrene-acrylic copolymer or a polyester is preferable, and a styrene-acrylic copolymer is more preferable.
[0174] (styrene-acrylic resin) The styrene-acrylic resin in the present invention is formed by polymerization of at least a styrene monomer and a (meth)acrylic acid ester monomer. Here, the styrene monomer includes not only styrene represented by the structural formula CH2=CH-C6H5, but also those having a structure with a known side chain or functional group in the styrene structure.
[0175] The (meth)acrylic acid ester monomer is a monomer having a functional group with an ester bond in the side chain. Specifically, it includes vinyl ester compounds such as acrylic acid ester monomers represented by CH2=CHCOOR (R is an alkyl group) and methacrylic acid ester monomers represented by CH2=C(CH3)COOR (R is an alkyl group).
[0176] Specific examples of styrene monomers and (meth)acrylic acid ester monomers capable of forming styrene-acrylic resins are shown below, but the examples are not limited to those shown below.
[0177] Examples of the styrene monomer include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pt-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.
[0178] Representative (meth)acrylic acid ester monomers include the acrylic acid ester monomers and methacrylic acid ester monomers shown below, and examples of the acrylic acid ester monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, lauryl acrylate, phenyl acrylate phenyl, etc. Examples of the methacrylic acid ester monomers include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, lauryl methacrylate, phenyl methacrylate, diethylaminoethyl methacrylate, dimethylaminoethyl methacrylate, etc.
[0179] These styrene monomers, acrylic acid ester monomers, and methacrylic acid ester monomers may be used alone or in combination of two or more kinds.
[0180] In addition to the above-mentioned copolymers formed only from styrene monomer and (meth)acrylic acid ester monomer, styrene-acrylic copolymers can also be formed by combining a general vinyl monomer with these styrene monomer and (meth)acrylic acid ester monomer. The following are examples of vinyl monomers that can be used in combination when forming the styrene-acrylic copolymer of the present invention, but the vinyl monomers that can be used in combination are not limited to those shown below.
[0181] (1) Olefins Ethylene, propylene, isobutylene, etc. (2) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (3) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (4) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (5) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (6)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile and acrylamide, and the like.
[0182] It is also possible to prepare a resin having a crosslinked structure by using a polyfunctional vinyl monomer. Furthermore, it is also possible to use a vinyl monomer having an ionic dissociation group in the side chain. Specific examples of the ionic dissociation group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Specific examples of the vinyl monomer having these ionic dissociation groups are shown below.
[0183] Specific examples of vinyl monomers having a carboxyl group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.
[0184] The method for forming the styrene-acrylic resin is not particularly limited, and may be a method of polymerizing monomers using a known oil-soluble or water-soluble polymerization initiator. If necessary, a known chain transfer agent such as n-octyl mercaptan may be used.
[0185] When forming the styrene-acrylic resin used in the present invention, the contents of the styrene monomer and the acrylic ester monomer are not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening temperature and the glass transition temperature of the binder resin. Specifically, the content of the styrene monomer is preferably within a range of 40 to 95% by mass, more preferably within a range of 50 to 80% by mass, based on the total monomers. The content of the acrylic ester monomer is preferably within a range of 5 to 60% by mass, more preferably within a range of 10 to 50% by mass, based on the total monomers.
[0186] The method for forming the styrene-acrylic resin is not particularly limited, and examples thereof include a method of polymerizing monomers using a known oil-soluble or water-soluble polymerization initiator. Specific examples of the oil-soluble polymerization initiator include the azo- or diazo-based polymerization initiators and peroxide-based polymerization initiators shown below.
[0187] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.
[0188] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.
[0189] In addition, when forming styrene-acrylic resin particles by emulsion polymerization, water-soluble radical polymerization initiators can be used. Examples of water-soluble radical polymerization initiators include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.
[0190] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 12 hours.
[0191] Styrene-acrylic resin particles formed by emulsion polymerization can be made to have two or more layers of resins with different compositions. In this case, a multi-stage polymerization method can be used, in which a polymerization initiator and a polymerizable monomer are added to a dispersion of resin particles prepared by a conventional emulsion polymerization process (first-stage polymerization), and the system is polymerized (second-stage polymerization).
[0192] (polyester resin) The polyester resin is a known polyester resin obtained by a polycondensation reaction between a divalent or higher carboxylic acid (a polyvalent carboxylic acid component) and a divalent or higher alcohol (a polyhydric alcohol component). The polyester resin may be amorphous or crystalline.
[0193] The valence of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably 2 to 3, and particularly preferably 2. Therefore, as a particularly preferred embodiment, the case where the valence is 2 (i.e., a dicarboxylic acid component and a diol component) will be described.
[0194] Examples of the dicarboxylic acid component include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; methylenesuccinic acid, Examples of the dicarboxylic acid include unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid; unsaturated aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylenediacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and anthracenedicarboxylic acid; and lower alkyl esters and acid anhydrides of these compounds can also be used. The dicarboxylic acid component can be used alone or in combination of two or more kinds.
[0195] In addition, trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid, anhydrides of the above carboxylic acid compounds, or alkyl esters having 1 to 3 carbon atoms can also be used.
[0196] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentane. Examples of the diol component include saturated aliphatic diols such as ethyl glycol; unsaturated aliphatic diols such as 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, and alkylene oxide adducts of bisphenols such as ethylene oxide adducts and propylene oxide adducts thereof, and derivatives thereof can also be used. The diol component may be used alone or in combination of two or more kinds.
[0197] The method for producing the polyester resin is not particularly limited, and the polyester resin can be produced by polycondensing (esterifying) the polyvalent carboxylic acid component and the polyhydric alcohol component using a known esterification catalyst.
[0198] Examples of catalysts that can be used in the production of polyester resins include alkali metal compounds such as sodium and lithium; compounds containing Group 2 elements such as magnesium and calcium; compounds of metals such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds. Specifically, examples of tin compounds include dibutyltin oxide (dibutyltin oxide), tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-normal-butyl titanate (Ti(On-Bu)4), tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolamine. Examples of germanium compounds include germanium dioxide. Examples of aluminum compounds include polyaluminum hydroxide, aluminum alkoxide, and tributylaluminate. These may be used alone or in combination of two or more.
[0199] The polymerization temperature is not particularly limited, but is preferably 70 to 250° C. The polymerization time is also not particularly limited, but is preferably 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0200] <Other Additives for Resin Composition> In addition to the resins described above, various additives can be used in the resin composition of the present invention as long as they do not impair the effects of the present invention. Examples of applicable additives are shown below.
[0201] (Plasticizer) In the present invention, the addition of a compound known as a plasticizer is preferable from the viewpoint of modifying the resin composition, such as improving mechanical properties, imparting flexibility, imparting water absorption resistance, and reducing moisture permeability. Plasticizers applicable to the present invention include phosphate ester plasticizers, ethylene glycol ester plasticizers, glycerin ester plasticizers, diglycerin ester plasticizers (fatty acid esters), polyhydric alcohol ester plasticizers, dicarboxylate ester plasticizers, polycarboxylate ester plasticizers, and polymer plasticizers. Among these, it is preferable to use either a polyhydric alcohol ester plasticizer (an ester plasticizer made of a polyhydric alcohol and a monovalent carboxylic acid) or a polycarboxylic acid ester plasticizer (an ester plasticizer made of a polyvalent carboxylic acid and a monovalent alcohol), or both.
[0202] As for details of the plasticizer applicable to the resin composition of the present invention, for example, the compounds described in paragraphs
[0102] to
[0162] of Japanese Patent No. 5380840 can be mentioned. The amount of the plasticizer added is preferably within the range of 0.001 to 50 parts by mass, more preferably 0.01 to 30 parts by mass, and even more preferably 0.1 to 15 parts by mass, based on 100 parts by mass of the resin composition of the present invention.
[0203] (Antioxidants) An antioxidant may be added to the resin composition of the present invention in order to prevent the resin from being decomposed by heat or light. Examples of antioxidants applicable to the present invention include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, heat-resistant processing stabilizers, light stabilizers, oxygen scavengers, etc. Among these, phenol-based antioxidants, particularly hindered phenol-based antioxidants having a bulky branched alkyl at the ortho position relative to the hydroxy group of the phenol compound, 2,2,6,6-tetraalkylpiperidine derivatives, and combinations thereof are preferred.
[0204] As for details of the antioxidant applicable to the resin composition of the present invention, for example, the compounds described in paragraphs
[0163] to
[0186] of Japanese Patent No. 5380840 can be mentioned. The amount of antioxidant added is appropriately selected within a range that does not impair the object of the present invention, but is preferably within the range of 0.001 to 5 parts by mass, more preferably 0.01 to 3.0 parts by mass, and even more preferably 0.1 to 1.0 part by mass, per 100 parts by mass of the resin composition of the present invention.
[0205] (acid scavenger, UV absorber) Examples of additives that can be used in the three-dimensional laminate using the resin composition of the present invention include acid scavengers described in paragraphs
[0187] to
[0192] of Japanese Patent No. 5380840, and ultraviolet absorbers described in paragraphs
[0193] to
[0197] of the same.
[0206] (Other additives) In addition, various resin additives that can be used in combination with the resin composition of the present invention include fine particles, release agents, dyes and pigments, flame retardants, antistatic agents, antifogging agents, lubricants and antiblocking agents, flow improvers, dispersants, and antibacterial agents. Various fillers can also be blended. There are no particular limitations on the fillers to be blended as long as they do not reduce the functionality of the composition, and powdery, fibrous, granular, and plate-shaped inorganic fillers, as well as resin-based fillers and natural fillers, can be preferably used. Two or more of these may be used in combination.
[0207] In the resin composition of the present invention, the ratio of the compound having the structure represented by the general formula (1) (compound having an azomethine moiety) to the resin (compound having an azomethine moiety / resin) is such that in an area where the resin is low, the composition is softened by isomerization accompanying light irradiation of the composition, but the composition peels off from the adhesive. In addition, when introduced into the toner, the number of molecules that do not form hydrogen bonds with the compounds having the azomethine moiety of the present invention increases, and the azomethine compounds that do not form supramolecular polymers act as plasticizers to reduce the viscosity. Therefore, in the case of multi-colored compositions, the particles spread after light irradiation, causing color mixing. In an area where the resin is high, the softening of the composition does not progress sufficiently due to isomerization accompanying light irradiation of the composition, causing poor softening of the composition and toner. Therefore, the ratio of the compound having an azomethine moiety to the resin (compound having an azomethine moiety / resin) is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, and even more preferably 20 / 80 to 80 / 20.
[0208] When the resin composition of the present invention is used as a temporary bonding material for bonding two objects, if it is not made non-fluid after peeling from the object by light irradiation, it will adhere to various things in the working environment and pollute the working environment. In addition, it will cause deterioration of the quality of the object, so it is necessary for the resin composition of the present invention to be reversibly fluidized and non-fluidized by light irradiation.
[0209] The wavelength of the light irradiation is within the range of 280 to 480 nm, more preferably within the range of 300 to 420 nm, and particularly preferably within the range of 330 to 420 nm. Within this range, light is absorbed well, so that the light melting property is improved and the fixability is improved. In addition, by irradiating the light having the above wavelength, it is possible to fluidize the toner without applying heat or pressure. Therefore, by introducing the compound having the azomethine moiety into the toner described later, it is possible to fix the toner at the above wavelength and obtain a toner with high color reproducibility. The above wavelength range is the ultraviolet region, but also includes the visible light region close to ultraviolet. This is because the compound having the azomethine moiety can be fluidized under the following irradiation conditions even with the light having the visible light region close to ultraviolet.
[0210] [Toner for developing electrostatic images] The toner for developing electrostatic images (hereinafter, also simply referred to as "toner") of the present invention is characterized by containing the above-mentioned resin composition. The content of the resin in the resin composition contained in the toner, that is, the binder resin and the compound having the structure represented by the general formula (1) (compound having an azomethine moiety) varies depending on the type of compound and the type of resin, but from the viewpoint of fixability and color reproducibility, it is preferable that the compound having an azomethine moiety:binder resin is in the range of 5:95 to 95:5 (mass ratio), more preferably 10:90 to 90:10 (mass ratio), even more preferably 10:90 to 80:20 (mass ratio), particularly preferably 10:90 to 70:30 (mass ratio), and particularly preferably 10:90 to 60:40 (mass ratio). Within this range, the photo-induced phase transition of the compound having an azomethine moiety is easily caused, and the toner has a sufficient softening speed due to light irradiation.
[0211] The toner of the present invention includes toner particles having toner base particles and an external additive attached to the surface of the toner base particles. In this specification, "toner base particles" are those that constitute the base of "toner particles." "Toner base particles" contain at least a binder resin, and may contain other components such as a colorant, a release agent (wax), and a charge control agent, as necessary. "Toner base particles" are called "toner particles" when an external additive is added. "Toner" refers to an aggregate of "toner particles."
[0212] <Binding resin> The toner base particles preferably further contain a binder resin in addition to the compound having the structure represented by the general formula (1). It is generally known that by utilizing an emulsion aggregation method, which will be described later, as a method for producing toner, toner particles having a substantially uniform particle size and shape can be produced. By using the compound having an azomethine moiety in combination with a binder resin, toner particles having a substantially uniform particle size and shape can be produced by salting out in an emulsion aggregation method, and thus the toner containing the compound having an azomethine moiety and the binder resin can be more easily applied to electrophotographic toners.
[0213] Such a binder resin can be any resin generally used as a binder resin constituting a toner without any restrictions. Specific examples include styrene resin, acrylic resin, styrene-acrylic resin, polyester resin, silicone resin, olefin resin, amide resin, and epoxy resin. These binder resins can be used alone or in combination of two or more kinds.
[0214] Among these, from the viewpoint of having a low viscosity when melted and having high sharp melting properties, the binder resin preferably contains at least one selected from the group consisting of a styrene resin, an acrylic resin, a styrene-acrylic resin, and a polyester resin, and more preferably contains at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.
[0215] The styrene-acrylic resin and polyester resin, which are preferred binder resins, are similar to the styrene-acrylic resin and polyester resin contained in the resin composition described above, and therefore a detailed description thereof will be omitted here.
[0216] The toner containing the compound having an azomethine moiety and the binder resin may have a single-layer structure or a core-shell structure. The types of the binder resin used for the core particle and the shell of the core-shell structure are not particularly limited.
[0217] <Coloring agent> The toner base particles preferably further contain a colorant. It is believed that the compound having the azomethine moiety is colorless but can induce reversible fluidization and non-fluidization phenomena upon isomerization. Therefore, by introducing a desired colorant into the toner together with the compound having the azomethine moiety, a toner can be obtained that can be fixed by light irradiation and has high color reproducibility of the added colorant. Generally known dyes and pigments can be used as the colorant.
[0218] Examples of colorants for obtaining black toner include carbon black, magnetic materials, iron-titanium composite oxide black, etc. Examples of carbon black include channel black, furnace black, acetylene black, thermal black, lamp black, etc. Examples of magnetic materials include ferrite, magnetite, etc.
[0219] Colorants for obtaining yellow toners include dyes such as CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; and pigments such as CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185.
[0220] Colorants for obtaining magenta toner include dyes such as CI Solvent Red 1, 49, 52, 58, 63, 111, and 122; and pigments such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.
[0221] Colorants for obtaining cyan toner include dyes such as CI Solvent Blue 25, 36, 60, 70, 93, and 95; and pigments such as CI Pigment Blue 1, 7, 15, 60, 62, 66, and 76.
[0222] The colorants for obtaining the toner of each color may be used alone or in combination of two or more kinds for each color.
[0223] The content of the colorant in the toner base particles is preferably within a range of 0.5 to 20% by mass, and more preferably within a range of 2 to 10% by mass.
[0224] <Release agent> The toner of the present invention preferably further contains a release agent. By introducing a release agent into the toner together with the compound having an azomethine moiety, a toner having better fixing properties can be obtained.
[0225] The release agent used is not particularly limited, and various known waxes can be used. Examples of waxes include polyolefins such as low molecular weight polypropylene, polyethylene, or oxidized low molecular weight polypropylene and polyethylene, paraffin, and synthetic ester waxes. In particular, it is preferable to use synthetic ester waxes because of their low melting point and low viscosity. As the synthetic ester wax, it is particularly preferable to use behenyl behenate, glycerin tribehenate, pentaerythritol tetrabehenate, etc.
[0226] The content of the release agent in the toner base particles is preferably within a range of 1 to 30% by mass, and more preferably within a range of 3 to 15% by mass.
[0227] <Charge control agent> The toner of the present invention may further contain a charge control agent. The charge control agent used is a substance capable of imparting positive or negative charge by frictional charging and is colorless, and is not particularly limited. Any of various known positively chargeable charge control agents and negatively chargeable charge control agents can be used.
[0228] The content of the charge control agent in the toner base particles is preferably within a range of 0.01 to 30% by mass, and more preferably within a range of 0.1 to 10% by mass.
[0229] <External additives> In order to improve the fluidity, chargeability, cleaning properties, etc. of the toner, external additives such as a fluidizing agent, a cleaning aid, etc., which are so-called post-treatment agents, may be added to the toner particles to form the toner of the present invention.
[0230] Examples of the external additive include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate particles and zinc titanate particles. These may be used alone or in combination of two or more kinds.
[0231] These inorganic particles may be surface-treated with a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, or the like in order to improve heat resistance, storage stability, and environmental stability.
[0232] The amount of these external additives added is preferably within a range of 0.05 to 5% by mass, and more preferably within a range of 0.1 to 3% by mass, of the toner base particles.
[0233] <Average particle size of toner> The average particle size of the toner is the volume-based median diameter (D 50 ) is preferably in the range of 4 to 10 μm, and more preferably in the range of 6 to 9 μm. 50 ) in the above range, the transfer efficiency is increased, the image quality of halftones is improved, and the image quality of fine lines, dots, etc. is improved.
[0234] In the present invention, the volume-based median diameter (D 50 ) is measured and calculated using a measuring device consisting of a "Coulter Counter 3" (manufactured by Beckman Coulter, Inc.) connected to a computer system (manufactured by Beckman Coulter, Inc.) equipped with the data processing software "Software V3.51."
[0235] Specifically, 0.02 g of the measurement sample (toner) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing surfactant components 10 times with pure water in order to disperse toner particles) and allowed to mix, after which ultrasonic dispersion is performed for 1 minute to prepare a toner dispersion. This toner dispersion is then pipetted into a beaker containing an "ISOTONII" (manufactured by Beckman Coulter, Inc.) in the sample stand until the concentration indicated on the measuring device reaches 8%.
[0236] By setting the concentration range, it is possible to obtain reproducible measurement values. In the measurement device, the number of particles to be measured is set to 25,000, the aperture diameter is set to 50 μm, the measurement range of 1 to 30 μm is divided into 256 parts, and the frequency value is calculated. The particle diameter of 50% from the largest volume cumulative fraction is determined to be the volume-based median diameter (D 50 ) is said to be
[0237] [Toner manufacturing method] The method for producing the toner of the present invention is not particularly limited. When a toner containing the compound represented by the general formula (1), a binder resin, and additives such as a colorant is produced, a production method utilizing an emulsion aggregation method, which allows easy control of particle size and shape, is preferable.
[0238] Such a manufacturing method is (1A) Binder resin particle dispersion preparation step of preparing a binder resin particle dispersion (1B) A colorant particle dispersion liquid preparation step for preparing a colorant particle dispersion liquid (1C) A step of preparing a dispersion liquid of the compound particles having an azomethine moiety, which prepares a dispersion liquid of the compound particles having an azomethine moiety (2) An association step in which a flocculant is added to an aqueous medium in which binder resin particles, colorant particles, and the compound particles having an azomethine moiety are present, and salting out is promoted while simultaneously flocculation and fusion are carried out to form associated particles. (3) Aging process to form toner base particles by controlling the shape of aggregated particles (4) A filtering and washing process for filtering the toner particles from the aqueous medium and removing surfactants and the like from the toner base particles. (5) A drying process for drying the washed toner base particles. (6) Additive addition step of adding additives to the dried toner base particles It is preferable that the method includes the steps of: Steps (1A) to (1C) are described below.
[0239] (1A) Binder resin particle dispersion preparation process In this process, resin particles are formed by a conventional emulsion polymerization or the like, and the resin particles are aggregated and fused to form binder resin particles. As an example, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and polymerized by a polymerization initiator to prepare a dispersion of binder resin particles.
[0240] Further, as a method for obtaining a binder resin particle dispersion, in addition to the above-mentioned method of polymerizing a polymerizable monomer in an aqueous medium by a polymerization initiator, for example, a method of performing a dispersion treatment in an aqueous medium without using a solvent, or a method of dissolving a binder resin (such as a crystalline resin) in a solvent such as ethyl acetate to prepare a solution, emulsifying and dispersing the solution in an aqueous medium using a disperser, and then performing a solvent removal treatment, can be mentioned.
[0241] In this case, if necessary, a release agent (wax) may be incorporated in advance into the binder resin. For dispersion, it is also preferable to carry out polymerization in the presence of a known surfactant (e.g., an anionic surfactant such as polyoxyethylene (2) sodium dodecyl ether sulfate, sodium dodecyl sulfate, or dodecylbenzenesulfonic acid). A release agent particle dispersion may be prepared separately from the binder resin particle dispersion in the same manner as in the colorant particle dispersion preparation step, and may be present in the aqueous medium in the association step (2) above.
[0242] The volume-based median diameter of the binder resin particles in the dispersion is preferably within a range of 50 to 300 nm. The volume-based median diameter of the binder resin particles in the dispersion can be measured by a dynamic light scattering method using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).
[0243] (1B) Colorant particle dispersion preparation process The colorant particle dispersion preparation step is a step of dispersing a colorant in the form of fine particles in an aqueous medium to prepare a colorant particle dispersion.
[0244] The colorant can be dispersed by utilizing mechanical energy. The median diameter based on the number of colorant particles in the dispersion is preferably within a range of 10 to 300 nm, and more preferably within a range of 50 to 200 nm. The median diameter based on the number of colorant particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0245] (1C) Preparation of a dispersion of compound particles having an azomethine moiety The compound particle dispersion preparation step is a step of dispersing the compound having the azomethine moiety in a fine particle state in an aqueous medium to prepare a dispersion of the compound particles having the azomethine moiety. In preparing the compound particle dispersion, first, an emulsion of the compound having the azomethine moiety is prepared. Examples of a method for preparing an emulsion of the compound include a method in which the compound having an azomethine moiety is dissolved in an organic solvent to obtain a solution of the compound having an azomethine moiety, and then the compound solution is emulsified in an aqueous medium.
[0246] The method for dissolving the compound having an azomethine moiety in an organic solvent is not particularly limited, and for example, there is a method of adding the compound having an azomethine moiety to an organic solvent and stirring and mixing the compound having an azomethine moiety so that the compound is dissolved. The addition ratio of the compound having an azomethine moiety is preferably within a range of 5 to 100 parts by mass, more preferably within a range of 10 to 50 parts by mass, relative to 100 parts by mass of the organic solvent.
[0247] Next, the liquid of the compound having an azomethine moiety is mixed with an aqueous medium and stirred using a known dispersing machine such as a homogenizer, whereby the compound having an azomethine moiety becomes droplets and is emulsified in the aqueous medium, thereby preparing an emulsion of the compound having an azomethine moiety.
[0248] The addition ratio of the compound solution having an azomethine moiety is preferably within a range of 10 to 90 parts by mass, and more preferably within a range of 30 to 70 parts by mass, relative to 100 parts by mass of the aqueous medium.
[0249] Furthermore, the temperatures of the liquid of the compound having an azomethine moiety and the aqueous medium when they are mixed are in a temperature range below the boiling point of the organic solvent, and are preferably in the range of 20 to 80° C., and more preferably in the range of 30 to 75° C. When they are mixed, the temperatures of the liquid of the compound having an azomethine moiety and the aqueous medium may be the same or different, and are preferably the same.
[0250] Regarding the stirring conditions of the dispersing machine, for example, when the capacity is 1 to 3 L, the rotation speed is preferably within the range of 7000 to 20000 rpm, and the stirring time is preferably within the range of 10 to 30 minutes.
[0251] The particle dispersion of the compound having an azomethine moiety is prepared by removing the organic solvent from an emulsion of the compound having an azomethine moiety. Examples of the method for removing the organic solvent from the emulsion of the compound having an azomethine moiety include known methods such as blowing air, heating, reducing pressure, or a combination of these.
[0252] As an example, the emulsion of the compound having an azomethine moiety is heated in an inert gas atmosphere such as nitrogen, preferably within a range of 25 to 90° C., more preferably within a range of 30 to 80° C., until about 80 to 95% by mass of the initial amount of organic solvent is removed, thereby removing the organic solvent. As a result, the organic solvent is removed from the aqueous medium, and a dispersion of the compound having an azomethine moiety in which particles of the compound having an azomethine moiety are dispersed in the aqueous medium is prepared.
[0253] The mass average particle diameter of the compound particles having an azomethine moiety in the dispersion of the compound particles having an azomethine moiety is preferably within the range of 90 to nm. The mass average particle diameter of the compound particles having an azomethine moiety can be set within the above range by appropriately adjusting the viscosity when the compound having an azomethine moiety is mixed with an organic solvent, the mixing ratio of the compound liquid having an azomethine moiety and water, and the stirring speed of the dispersing machine when preparing the emulsion of the compound having an azomethine moiety. The mass average particle diameter of the compound particles having an azomethine moiety in the dispersion of the compound particles having an azomethine moiety can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0254] <Organic solvent> The organic solvent used in this step is not particularly limited as long as it can dissolve the compound having an azomethine moiety of the present invention.Specific examples include esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, diisopropyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, saturated hydrocarbons such as hexane and heptane, and halogenated hydrocarbons such as dichloromethane, dichloroethane, and carbon tetrachloride.
[0255] Such organic solvents can be used alone or in combination of two or more kinds. Among these organic solvents, ketones and halogenated hydrocarbons are preferred, and methyl ethyl ketone and dichloromethane are more preferred.
[0256] <Aqueous medium> The aqueous medium used in this step may be water, or an aqueous medium containing water as the main component and water-soluble solvents such as alcohols and glycols, and optional components such as surfactants and dispersants. The aqueous medium used is preferably a mixture of water and a surfactant.
[0257] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, and hexadecyl trimethyl ammonium bromide. Examples of the anionic surfactant include fatty acid soaps such as sodium stearate and sodium dodecanoate, sodium dodecyl benzene sulfonate, and sodium dodecyl sulfate. Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonyl phenyl ether, polyoxyethylene lauryl ether, polyoxyethylene sorbitan monooleate ether, and monodecanoyl sucrose.
[0258] Such surfactants can be used alone or in combination of two or more. Among the surfactants, anionic surfactants are preferred, and sodium dodecylbenzenesulfonate is more preferred.
[0259] The amount of the surfactant added is preferably within a range of 0.01 to 10 parts by mass, and more preferably within a range of 0.04 to 1 part by mass, relative to 100 parts by mass of the aqueous medium.
[0260] The steps from (2) association step to (6) external additive addition step can be carried out according to various conventionally known methods.
[0261] The flocculant used in the (2) association step is not particularly limited, but is preferably selected from metal salts. Examples of metal salts include monovalent metal salts such as salts of alkali metals such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts because they can promote flocculation with a smaller amount. These can be used alone or in combination of two or more.
[0262] [Developer] The toner of the present invention may be used, for example, as a one-component magnetic toner by incorporating a magnetic material, as a two-component developer by mixing with a so-called carrier, or as a non-magnetic toner alone, and any of these may be suitably used.
[0263] As the magnetic material, for example, magnetite, γ-hematite, or various ferrites can be used.
[0264] As the carrier constituting the two-component developer, magnetic particles made of conventionally known materials such as metals such as iron, steel, nickel, cobalt, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead can be used.
[0265] As the carrier, it is preferable to use a coated carrier in which the surface of magnetic particles is coated with a coating agent such as a resin, or a so-called resin dispersion type carrier in which magnetic powder is dispersed in a binder resin. The resin for coating is not particularly limited, but for example, olefin resin, styrene resin, styrene-acrylic resin, silicone resin, polyester resin, or fluororesin is used. In addition, the resin for constituting the resin dispersion type carrier is not particularly limited, and a known one can be used, for example, acrylic resin, styrene-acrylic resin, polyester resin, fluororesin, phenolic resin, etc. can be used.
[0266] The volume-based median diameter of the carrier is preferably within a range of 20 to 100 μm, and more preferably 25 to 80 μm. The volume-based median diameter of the carrier can be measured typically by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.
[0267] The mixing amount of the toner with respect to the carrier is preferably within a range of 2 to 10% by mass, with the total mass of the toner and carrier being 100% by mass.
[0268] [Image forming method] The toner of the present invention can be used in various known electrophotographic image forming methods. For example, it can be used in monochrome image forming methods and full-color image forming methods. In the full-color image forming method, it can be applied to any image forming method, such as a four-cycle image forming method consisting of four types of color developing devices for yellow, magenta, cyan, and black, and one photoconductor, and a tandem image forming method in which image forming units having color developing devices and photoconductors for each color are installed for each color. An image forming method according to one embodiment of the present invention includes the steps of forming a toner image on a recording medium, the toner image being made of a toner containing a compound having a structure represented by general formula (1), and softening the toner image by irradiating the toner image with light.
[0269] In order to sufficiently fluidize the compound having an azomethine moiety in the toner and quickly soften the toner image, the wavelength of light used when irradiating the toner image is preferably within the range of 280 to 480 nm. From the viewpoint of obtaining a better fixing property, it is preferable to further include a step of pressurizing the toner image. Furthermore, from the viewpoint of obtaining a better fixing property, it is preferable to further heat the toner image in the pressurizing step.
[0270] Fig. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. However, the image forming apparatus used in the present invention is not limited to the following form and illustrated example. Fig. 1 shows an example of a monochrome image forming apparatus 100, but the present invention can also be applied to a color image forming apparatus.
[0271] The image forming apparatus 100 is an apparatus for forming an image on a recording paper S as a recording medium, and is equipped with an image reading device 71 and an automatic document feeder 72, and performs image formation on the recording paper S transported by a paper transport system 7 using an image forming unit 10, an irradiation unit 40, and a pressing unit 9.
[0272] Furthermore, while image forming apparatus 100 uses recording paper S as a recording medium, the medium on which an image is formed may be something other than paper.
[0273] An original d placed on the platen of the automatic document feeder 72 is scanned and exposed by the optical system of the scanning exposure device of the image reading device 71 and read into the image sensor CCD. An analog signal photoelectrically converted by the image sensor CCD is subjected to analog processing, A / D conversion, shading correction, image compression processing, etc. in the image processing unit 20, and then input to the exposure device 3 of the image forming unit 10.
[0274] The paper transport system 7 includes a plurality of trays 16, a plurality of paper feed units 11, transport rollers 12, a transport belt 13, etc. The trays 16 each store recording paper S of a predetermined size, and operate the paper feed unit 11 of the specified tray 16 in response to an instruction from the control unit 90 to supply the recording paper S. The transport rollers 12 transport the recording paper S sent out from the tray 16 by the paper feed unit 11 or the recording paper S brought in from the manual paper feed unit 15 to the image forming unit 10.
[0275] The image forming unit 10 is configured with a charger 2, an exposure unit 3, a developing unit 4, a transfer unit 5, a charge removal unit (not shown), and a cleaning unit 8 arranged in this order around the photoreceptor 1 along the direction of rotation of the photoreceptor 1.
[0276] The photoconductor 1, which is an image carrier, is an image carrier having a photoconductive layer formed on its surface, and is configured to be rotatable in the direction of the arrow in Fig. 1 by a driving device (not shown). A thermo-hygrometer 17 that detects the temperature and humidity inside the image forming apparatus 100 is provided near the photoconductor 1.
[0277] The charger 2 uniformly charges the surface of the photoreceptor 1, thereby uniformly charging the surface of the photoreceptor 1. The exposure unit 3 is equipped with a beam emission source such as a laser diode, and irradiates the charged surface of the photoreceptor 1 with a beam of light, thereby dissipating the charge in the irradiated area and forming an electrostatic latent image on the photoreceptor 1 according to the image data. The development unit 4 supplies the toner contained therein to the photoreceptor 1, and creates a toner image on the surface of the photoreceptor 1 based on the electrostatic latent image.
[0278] The transfer unit 5 faces the photoreceptor 1 via the recording paper S, and transfers the toner image onto the recording paper S. The charge removing unit removes charge from the photoreceptor 1 after the toner image has been transferred. The cleaning unit 8 includes a blade 85. The blade 85 cleans the surface of the photoreceptor 1 to remove any developer remaining on the surface of the photoreceptor 1.
[0279] The recording paper S onto which the toner image has been transferred is transported by a transport belt 13 to a pressing unit 9. The pressing unit 9 may be installed arbitrarily, and performs a fixing process on the recording paper S onto which the toner image has been transferred by applying pressure alone or heat and pressure with pressure members 91 and 92, thereby fixing the image onto the recording paper S. The recording paper S onto which the image has been fixed is transported by transport rollers to a paper discharge unit 14, and is discharged from the paper discharge unit 14 to the outside of the machine.
[0280] In addition, the image forming apparatus 100 is equipped with a paper inversion section 24, so that the recording paper S that has been subjected to the heat fixing process is transported to the paper inversion section 24 just before the paper discharge section 14, and either the recording paper S is inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10, and images can be formed on both sides of the recording paper S.
[0281] <Irradiation unit> FIG. 2 is a schematic diagram of the irradiation unit 40 in the image forming apparatus 100. As shown in FIG.
[0282] The image forming apparatus 100 according to one embodiment of the present invention includes an irradiation unit 40. Examples of devices constituting the irradiation unit 40 include a light emitting diode (LED) and a laser light source.
[0283] The irradiation section 40 melts and fluidizes a compound (a compound having a structure represented by the general formula (1)) contained in the toner of the developer that undergoes a phase transition upon light absorption. The wavelength of the irradiated light may be sufficient to sufficiently fluidize the toner, and light having a wavelength preferably within the range of 280 to 480 nm, more preferably within the range of 300 to 420 nm, and even more preferably within the range of 330 to 420 nm is irradiated. The amount of light irradiated by the irradiation section 40 may also be sufficient to sufficiently fluidize the toner, and is preferably 0.1 to 200 J / cm. 2 within the range of 0.1 to 100 J / cm 2 within the range of 0.1 to 50 J / cm 2 is within the range.
[0284] When a compound having an azomethine moiety is to be made non-fluid (re-solidified), it may be made non-fluid by leaving it at room temperature (within the range of 25±15° C.).
[0285] That is, an image forming method according to one embodiment of the present invention includes the steps of forming a toner image made of the toner of the present invention on a recording medium, irradiating the toner image with light having a wavelength in the range of 280 to 480 nm to soften the toner image, and leaving the softened toner image at room temperature (within the range of 25±15° C.) to solidify the toner image and fix it to the recording medium. Note that the fixing step preferably further includes a step of pressurizing the softened toner image. In the pressurizing step, it is preferable to further heat the softened toner image. This is because heating the toner image can further soften it.
[0286] The heating temperature during the further heating in the pressurizing step is preferably within the range of 30 to 100°C, and more preferably within the range of 40 to 100°C.
[0287] Irradiation unit 40 irradiates light toward a first surface of recording paper S holding a toner image, which is on the photoreceptor side, and is disposed on the photoreceptor side with respect to the surface of recording paper S nipped between photoreceptor 1 and transfer roller 5, which is a transfer unit. Irradiation unit 40 is disposed along the transport direction of recording paper S (paper transport direction).
[0288] The irradiation unit 40 is disposed downstream of the nip position between the photoconductor 1 and the transfer roller 5 in the paper transport direction and upstream of the pressure bonding unit 9 in the paper transport direction.
[0289] According to an image forming method according to an embodiment of the present invention, the photoconductor 1 is charged by applying a uniform potential to it using the charger 2, and then the photoconductor 1 is scanned with a light beam irradiated by the exposure unit 3 based on original image data to form an electrostatic latent image. Next, the developing unit 4 supplies onto the photoconductor 1 a developer having a toner containing a compound that undergoes a phase transition upon light absorption (the compound having the azomethine moiety).
[0290] When the recording paper S is transported from the tray 16 to the image forming unit 10 in time with the rotation of the photoconductor 1 causing the toner image carried on the surface of the photoconductor 1 to reach the position of the transfer roller 5, which is the transfer unit, the toner image on the photoconductor 1 is transferred onto the recording paper S, which is nipped between the transfer roller 5 and the photoconductor 1, by the transfer bias applied to the transfer roller 5.
[0291] In addition, the transfer member 5 also serves as a pressure member, and is capable of transferring the toner image from the photoreceptor 1 to the recording paper S while reliably adhering the compound having an azomethine moiety contained in the toner image to the recording paper S.
[0292] After the toner image is transferred onto the recording paper S, the blade 85 of the cleaning unit 8 removes the developer remaining on the surface of the photoconductor 1 .
[0293] In the process in which the recording paper S onto which the toner image has been transferred is transported by the transport belt 13 to the pressing unit 9, the irradiation unit 40 irradiates the toner image transferred onto the recording paper S with light having a wavelength of 280 to 480 nm. By irradiating the toner image on the first surface of the recording paper S with ultraviolet light by the irradiation unit 40, the toner image can be melted more reliably, and the fixability of the toner image to the recording paper S can be improved.
[0294] When the recording paper S carrying the toner image reaches the pressing unit 9 by the conveyor belt 13, the pressure members 91 and 92 press the toner image onto the first side of the recording paper S. Before the toner image is fixed by the pressing unit 9, the toner image is softened by irradiation with ultraviolet light by the irradiation unit 40, so that energy saving can be achieved in pressing the image onto the recording paper S. It is preferable that the image forming method of the present invention further includes a step of pressing the toner image with the pressure members 91 and 92 while leaving it at room temperature (within a range of 25±15° C.) in the step of solidifying the toner image and fixing it onto the recording medium. By applying pressure with the pressure members 91 and 92, the fixability of the toner image onto the recording paper S is further improved.
[0295] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably in the range of 0.01 to 5.0 MPa, and more preferably in the range of 0.05 to 1.0 MPa. By setting the pressure at 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure at 5.0 MPa or less, shock noise during pressing can be suppressed.
[0296] In the pressurizing step, it is preferable to further heat the toner image. By applying pressure and heat by the pressure members 91 and 92, the fixability of the toner image to the recording paper S is further improved. Specifically, when the recording paper S passes between the pressure members 91 and 92, the toner image softened by light irradiation is pressurized by the pressure member 91 in a state further softened by heating, so that the fixability of the toner image to the recording paper S is further improved.
[0297] Thereafter, the toner image on the recording paper S is solidified in a natural environment (left at room temperature). Specifically, by leaving the recording paper S that has passed between the pressure members 91 and 92 in a natural environment (left at room temperature) until it reaches the paper discharge unit 14, the toner image on the recording paper S can be solidified more reliably, and the fixability of the toner image to the recording paper S can be further improved.
[0298] When forming images on both sides of the recording paper S, the recording paper S that has been subjected to the pressure bonding process is transported to the paper inversion section 24 just before the paper discharge section 14, and either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10.
[0299] [Photosensitive adhesive] The compound having the structure represented by the general formula (1) according to the present invention can be reversibly fluidized or non-fluidized by light irradiation, and therefore can be used to prepare a photosensitive adhesive that can be used repeatedly. For example, it can be applied to various adhesion techniques as a photosensitive adhesive that can be repeatedly attached and detached by light in response to changes in viscosity (friction coefficient).
[0300] The photosensitive adhesive of the present invention can be used for temporary fixing that can be reused repeatedly, and is also suitable for recycling, but is not limited thereto.
[0301] In addition to the compound having a structure represented by general formula (1), the photosensitive adhesive of the present invention may contain additives such as the resins described above in <Resins> and <Other additives to the resin composition>, plasticizers, antioxidants, acid scavengers, and ultraviolet absorbers, but is not limited to these. EXAMPLES
[0302] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0303] Compounds 1 to 62 shown in Tables I to IV below were synthesized by the above-mentioned synthesis method, respectively. Comparative compounds D to F used in the comparative examples were synthesized by the following method.
[0304] [Synthesis of comparative compound D (azobenzene compound D)] An azobenzene compound D was obtained by the same method as "(1-1-1) Synthesis of UV softening material A" described in paragraphs
[0217] to
[0224] of JP2014-191078A. The structure is: 1 1 H-NMR and IR confirmed that the desired compound had been obtained.
[0305] [ka]
[0306] [Synthesis of Comparative Compound E (Azobenzene Compound E)] An azobenzene compound E was obtained in the same manner as in "(1-2-1) Synthesis of UV softening material B" described in paragraphs
[0227] to
[0237] of JP2014-191078A. The structure is:1 1 H-NMR and IR confirmed that the desired compound had been obtained.
[0307] [ka]
[0308] [Synthesis of Comparative Compound F (Azomethine Compound F)] 4-Hydroxy-3-methylbenzaldehyde and iodohexane (CH 13 I) was reacted with potassium carbonate (K2CO3) by heating under reflux, the reaction solution was washed with water, concentrated, and purified by column chromatography to obtain 4-hexyloxy-3-methylbenzaldehyde (see Scheme* below). 4-Hexyloxy-3-methylbenzaldehyde obtained in Scheme 1 and 5-hexylthiophene-2-amine were reacted in ethanol (EtOH) by heating and stirring, the reaction solution was filtered, the resulting powder was washed with cooled ethanol, and recrystallized from methanol / ethanol to obtain the target azomethine compound F (see Scheme 2 below). The structure is 1 1 H-NMR and IR confirmed that the desired compound had been obtained.
[0309] [ka]
[0310] The abbreviations and physical properties (Tg: glass transition temperature) of the resins used below are as follows, and they were prepared based on the literature information for each. PMMA: PolyMethyl Methacrylate, Tg 42℃, Journal of Polymer Science, Part A-2, 4, 199-208 (1966) PBT: Polybutyleneterephthalate, Tg 42℃, Journal of Polymer Science, Polymer Physics Edition, 21, 7, 1091-1101 (1983) PET: Polyethyleneterephtalate, Tg 48℃, Macromolecules, 37, 7, 2532-2537 (2004) PC: Polycarbonate (2,2'-Dimethylbisphenol A polycarbonate), Tg 49℃, Macromolecules, 25, 18, 4588-4596 (1992)
[0311] (1) Example 1 [Preparation of resin composition] <Preparation of Resin Composition 1-1> 5 mg of PMMA and 95 mg of the exemplary compound 1 were placed in a petri dish, and 100 ml of CHCl3 was added. The dish was covered with aluminum foil and left in a draft until the CHCl3 was completely dried. The solvent was then removed by vacuum drying at room temperature using a reduced pressure dryer.
[0312] <Resin Compositions 1-2 to 1-60 and 1-A to 1-F> Compositions 1-2 to 1-60 and Comparative Examples 1-A to 1-F were prepared in the same manner as in <Preparation of Composition 1-1> using the resins and exemplary compounds described in Tables I and II, and the resins and exemplary compounds in the ratios described in Tables I and II. In the case of a composition that was difficult to dissolve, the solution was heated to dissolve it. In addition, in the case of using two kinds of example compounds (example compound A and example compound B), example compound A and example compound B were weighed out so that the number of moles was the same.
[0313] [Photoresponsive adhesion test] The change in adhesiveness of the resin compositions 1-1 to 1-60 and 1-A to 1-F prepared above due to light irradiation was evaluated by the following photoresponsive adhesion test using the device shown in FIG. As shown in FIG. 3, 2 mg of compound was placed on an 18 mm square cover glass 1 within a 6 mm radius from the center of the glass, and a cover glass 2 of the same size was placed at a position shifted by about 4 mm in the parallel direction relative to the cover glass 1. After each of resin compositions 1-1 to 1-60 and 1-A to 1-F was sandwiched between cover glasses, the cover glasses were heated to melt the resin composition and bond cover glass 1 and cover glass 2. Each of the obtained samples was subjected to the following fluidization test (non-fluidity to fluidity test), and then to the following non-fluidization test (fluidity to non-fluidity test).
[0314] <Fluidity test (test to change non-fluidity to fluidity)> Part (A) shown in Figure 3 was fixed to the stand with cellophane tape, and a 30 cm long vinyl string with a 100 g weight attached was fixed to part (C) with cellophane tape. Part (B) was irradiated with light of 365 nm wavelength at a dose of 30 J / cm. 2 It was then confirmed whether cover glass 2 peeled off from cover glass 1, and the peeling was judged according to the following evaluation criteria. In the following evaluation criteria, ○ was deemed to be acceptable. The obtained results are shown in Tables I and II. (Evaluation Criteria) ○: Cover glass 2 was completely peeled off from cover glass 1 △: Cover glass 2 is displaced ×: Cover glass 2 did not move
[0315] <Defluidity test (fluidity to non-fluidity test)> Non-fluidity → 5 minutes after the start of the fluidity test (the 5 minutes were left in a natural environment, i.e., at room temperature (within the range of 25±15°C)), cover glass 3 (same size as cover glasses 1 and 2) was placed over the sample portion (part (B)) of cover glass 1 used in the above test, and it was confirmed whether cover glass 1 and cover glass 3 were adhered, and judged according to the following evaluation criteria. In the following evaluation criteria, ○ was considered to be a pass. The results obtained are shown in Tables I and II.
[0316] (Evaluation Criteria) 〇: Did not adhere (had become non-fluid) △: Partially adhered (partially maintained in a fluid state) ×: Adhered (fluid state was maintained)
[0317] [Table 1]
[0318] [Table 2]
[0319] As shown by the above results, it was confirmed that the resin composition of the present invention induces reversible fluidization / non-fluidization phenomena in the fluidization and non-fluidization tests. In contrast, the resin composition of the comparative example did not induce both fluidization and non-fluidization phenomena. In addition, in the fluidization test for the comparative resin composition 1-A, the cover glass 2 was completely peeled off from the cover glass 1, but the coating film peeled off from the cover glass.
[0320] (2) Example 2 [Production of Toner 2-1] <Preparation of styrene-acrylic resin particle dispersion 1> (First stage polymerization) A solution of 8 parts by mass of sodium dodecyl sulfate dissolved in 3,000 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen inlet device, and the internal temperature was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen stream. After the temperature was raised, a solution of 10 parts by mass of potassium persulfate dissolved in 200 parts by mass of ion-exchanged water was added, and the liquid temperature was again raised to 80° C. A polymerizable monomer solution consisting of 480 parts by mass of styrene, 250 parts by mass of n-butyl acrylate, 68.0 parts by mass of methacrylic acid, and 16.0 parts by mass of n-octyl-3-mercaptopropionate was added dropwise over 1 hour, and the mixture was heated and stirred at 80° C. for 2 hours to polymerize, thereby preparing a styrene-acrylic resin particle dispersion (1A) containing styrene-acrylic resin particles (1a).
[0321] (Second stage polymerization) A solution of 7 parts by mass of sodium polyoxyethylene-2-dodecyl ether sulfate dissolved in 800 parts by mass of ion-exchanged water was charged into a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98°C. After that, a polymerizable monomer solution of 260 parts by mass of the above styrene-acrylic resin particle dispersion (1A), 245 parts by mass of styrene, 120 parts by mass of n-butyl acrylate, 1.5 parts by mass of n-octyl-3-mercaptopropionate, and 67 parts by mass of paraffin wax "HNP-11" (manufactured by Nippon Seiro Co., Ltd.) as a release agent was added at 90°C, and the mixture was mixed and dispersed for 1 hour using a mechanical disperser "CREARMIX" (manufactured by M Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). Next, an initiator solution prepared by dissolving 6 parts by mass of potassium persulfate in 200 parts by mass of ion-exchanged water was added to this dispersion, and the system was heated and stirred at 82°C for 1 hour to carry out polymerization, thereby preparing a styrene-acrylic resin particle dispersion (1B) containing styrene-acrylic resin particles (1b).
[0322] (Third stage polymerization) A solution of 11 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added to the above styrene-acrylic resin particle dispersion (1B), and a polymerizable monomer solution consisting of 435 parts by mass of styrene, 130 parts by mass of n-butyl acrylate, 33 parts by mass of methacrylic acid, and 8 parts by mass of n-octyl-3-mercaptopropionate was added dropwise over 1 hour at a temperature of 82°C. After the dropwise addition, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28°C to obtain styrene-acrylic resin particle dispersion 1 containing styrene-acrylic resin 1. The glass transition temperature Tg of this styrene-acrylic resin 1 was measured and found to be 45°C.
[0323] (Preparation of Polyester Resin Particle Dispersion 1) In a 10-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 524 parts by mass of bisphenol A propylene oxide 2 mole adduct, 105 parts by mass of terephthalic acid, 69 parts by mass of fumaric acid, and 2 parts by mass of tin octylate (esterification catalyst) were added, and a polycondensation reaction was carried out at a temperature of 230°C for 8 hours. The polycondensation reaction was further continued at 8 kPa for 1 hour, and then cooled to 160°C to obtain polyester resin 1. 100 parts by mass of this polyester resin 1 was pulverized with a "Landermill Type: RM" (manufactured by Tokuju Machinery Co., Ltd.), mixed with 638 parts by mass of a 0.26% by mass aqueous solution of sodium lauryl sulfate prepared in advance, and ultrasonically dispersed at V-LEVEL and 300 μA for 30 minutes using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.) while stirring, to obtain polyester resin particle dispersion 1. The glass transition point Tg of this polyester resin 1 was measured and found to be 42°C.
[0324] (Preparation of Cyan Dispersion) 11.5 parts by mass of sodium n-dodecyl sulfate was dissolved in 1,600 parts by mass of pure water, and 25 parts by mass of copper phthalocyanine (CI Pigment Blue 15:3) was gradually added. Then, a cyan dispersion was prepared using "Clearmix (registered trademark) W Motion CLM-0.8 (manufactured by M Technique Co., Ltd.)".
[0325] (Preparation of azomethine moiety-containing compound particle dispersion 1) 80 parts by mass of dichloromethane and 20 parts by mass of exemplary compound 1 were mixed and stirred while heating at 40°C, and compound 1 was dissolved. Then, heating and stirring were stopped, and the mixture was left to stand for 3 hours. Stirring was started again, and a mixture of 99.5 parts by mass of distilled water heated to 50°C and 0.5 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate was added to 100 parts by mass of the liquid. Then, the mixture was emulsified by stirring at 16000 rpm for 20 minutes using a homogenizer (manufactured by Heidolph) equipped with a shaft generator 18F, to obtain an emulsion 1 of a compound having an azomethine moiety. The obtained emulsion 1 of the compound having an azomethine moiety was placed in a separable flask, and heated and stirred at 40°C for 90 minutes while blowing nitrogen into the gas phase to remove the organic solvent, thereby obtaining particle dispersion 1 of the compound having an azomethine moiety.
[0326] (Agglomeration, fusion) The above-prepared styrene-acrylic resin particle dispersion 1 (504 parts by solids), azomethine moiety-containing compound particle dispersion (216 parts by solids), ion-exchanged water (900 parts by solids), and cyan dispersion (70 parts by solids) were charged into a reaction apparatus equipped with a stirrer, a temperature sensor, and a cooling tube. The temperature inside the vessel was kept at 30°C, and a 5 mol / L aqueous solution of sodium hydroxide was added to adjust the pH to 10. Next, an aqueous solution of 2 parts by mass of magnesium chloride hexahydrate dissolved in 1000 parts by mass of ion-exchanged water was added dropwise over 10 minutes while stirring, and then heating was started. The temperature of this system was raised to 70°C over 60 minutes, and the particle growth reaction was continued while maintaining the temperature at 70°C. In this state, the particle size of the associated particles was measured using a "Multisizer 3" (manufactured by Beckman Coulter, Inc.), and the median diameter (D 50 When the particle size reached 6.5 μm, an aqueous solution of 190 parts by weight of sodium chloride dissolved in 760 parts by weight of ion-exchanged water was added to stop particle growth. After stirring at 70°C for 1 hour, the temperature was further increased, and the particles were heated and stirred at 75°C to promote fusion of the particles. The mixture was then cooled to 30°C to obtain a dispersion of toner particles. The dispersion of the toner particles obtained above was subjected to solid-liquid separation using a centrifuge to form a wet cake of the toner particles. The wet cake was washed with ion-exchanged water at 35°C until the electrical conductivity of the filtrate from the centrifuge reached 5μS / cm, and then transferred to a "Flash Jet Dryer (manufactured by Seishin Enterprise Co., Ltd.)" and dried until the moisture content reached 0.5% by mass to produce Toner 2-1.
[0327] [Production of Toners 2-2 to 2-58 and 2-A to 2-F] Toners 2-2 to 2-58 and 2-A to 2-F were produced in the same manner as in the production of toner 2-1, except that the types of resin, example compound and colorant, the mass ratio of resin to example compound, and the presence or absence of wax were appropriately changed as described in III below. When two kinds of exemplary compounds (exemplary compound A and exemplary compound B) were used, exemplary compound A and exemplary compound B were weighed out so that their molar amounts were the same.
[0328] [Preparation of developer] For each of the toners prepared above, ferrite carrier particles with a volume average particle size of 30 μm coated with a copolymer resin of cyclohexane methacrylate and methyl methacrylate (monomer mass ratio 1:1) were mixed so that the toner particle concentration was 6 mass%, to obtain developers 2-1 to 2-58 and 2-A to 2-F. Mixing was performed for 30 minutes using a V-type mixer.
[0329] [Image forming method] Using each of the obtained developers, a toner image was formed on a recording medium, plain paper, to obtain a printed matter. Specifically, one side was the developer and the other side was gloss coated paper (basis weight: 128 g / m 2 The developer was placed between a pair of parallel flat plate (aluminum) electrodes with a magnetic force, and the gap between the electrodes was 0.5 mm. The DC bias and AC bias were used to control the toner adhesion amount to 4 g / m. 2 The toner was developed under the above conditions to form a toner layer on the surface of the plain paper, which was then fixed by a fixing device to obtain a print.
[0330] [evaluation] <Fixation test> The 1 cm square image of the print obtained above was rubbed 10 times with a "JK Wiper (registered trademark)" (manufactured by Nippon Paper Crecia Co., Ltd.) at a pressure of 50 kPa, and the image fixation rate was evaluated. A fixation rate of 80% or more was considered to be acceptable. The evaluation results (fixation rate) of the fixation test obtained are shown in Table III below. The image fixation rate is a value expressed as a percentage obtained by measuring the density of the image after printing and the image after rubbing using a reflection densitometer "RD-918" (manufactured by Sakata Inx Engineering Co., Ltd.) and dividing the reflection density of the solid image after rubbing by the reflection density of the solid image after printing. The fixing devices used were the following three types of devices constructed by appropriately modifying the device shown in FIG. Fixing device No. 1: There is no pressure bonding unit 9 in FIG. 2. The wavelength of the ultraviolet light emitted from the irradiation unit 40 is 365 nm (light source: LED light source with an emission wavelength of 365 nm±10 nm), and the irradiation amount is 10 J / cm 2 The toner softened by the ultraviolet light irradiation was left to solidify (make the compound non-fluid) and be fixed in the natural environment, i.e., at room temperature (20° C.), until it reached the paper discharge section 14 (see FIG. 1). Fixing device No. 2: The fixing device No. 2 has the pressure bonding unit 9 in FIG. 2, the temperature of the pressure member 91 is 20° C., and the pressure when pressing is 0.2 MPa. The light source and the amount of irradiation of the irradiation unit are the same as those of No. 1. The toner softened by the ultraviolet light irradiation is fixed by pressure applied by the pressure member 91, and then solidified (the compound is made non-fluid) by leaving it at room temperature (20° C.) until it reaches the paper discharge unit 14 (see FIG. 1). Fixing device No. 3: It has the pressure bonding unit 9 in FIG. 2, and the temperature of the pressure member 91 is 80° C. The light source and the amount of irradiation of the irradiation unit are the same as those of No. 1. The pressure when pressing by the pressure member 91 is the same as that of No. 2. The toner softened by the ultraviolet light irradiation is further softened and fixed by the pressure and heat of the pressure member 91. Thereafter, it is left at room temperature (20° C.) until it reaches the paper discharge unit 14 (see FIG. 1) and solidifies (the compound is made non-fluid).
[0331] (Evaluation Criteria for Fixation) Pass: 80% or higher Fail: Less than 80%
[0332] <Color reproducibility> The color reproducibility of the example images obtained above was evaluated by visual evaluation by 10 monitors according to the following evaluation criteria. Specifically, as a sample for evaluation comparison, a toner containing only a binder resin was prepared for the toner described in each example, and developed in the same manner as in (Image formation), and fixed using fixing devices No. 1 to 3 shown in Table III. Ten monitors were shown the sample for evaluation and the sample described in the embodiment in turn, and asked whether the colors of the two images were clearly different. The results of the evaluation based on the following color reproducibility evaluation criteria are shown in Table III below. "◎" and "◯" were considered to be acceptable.
[0333] (Evaluation criteria for color reproducibility) ◎: Less than 2 people answered that it was clearly different ○: 3 to 4 people answered that it was clearly different △: 5 to 7 people answered that it was clearly different ×: 8 or more people answered that it was clearly different
[0334] [Table 3]
[0335] [Table 4]
[0336] As shown by the above results, it is recognized that the toner of the present invention has higher fixability and color reproducibility by light irradiation than the toner of the comparative example. [Explanation of symbols]
[0337] 1 photoreceptor 2 Charger 3 Exposure device 4 Development Section 5 Transfer section (transfer roller) 7 Paper transport system 8 Cleaning Section 9 Crimping section 10 Image forming section 11 Paper feed section 12 Transport roller 13 Conveyor belt 14 Paper output section 15 Manual feed section 16 Tray 17 Thermohygrometer 20 Image processing section 24 Paper Reversal Section 40 Irradiation unit 71 Image reading device 72 Automatic document feeder 85 Bree 90 Control section 91, 92 Pressure member 100 Image forming device d Manuscript S Recording Paper
Claims
1. A resin composition comprising a compound having a structure represented by the following general formula (1): [Formula 1] [In general formula (1), Z 1 and Z 2 each independently represents N or CH, and Z 1 ≠Z 2 It is. 1 and A 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. 1 and L 2 represents a linking group; n represents 0 or 1; B represents a complementary multiple hydrogen bonding group, which is any one of residues of a compound selected from adenine, thymine, 2,6-diacetylaminopyridine, melamine, cyanuric acid, and 4,6-diamino-2-pyrimidinone; G represents a substituent or the complementary multiple hydrogen bonding group, and when G is a substituent, n=0.]
2. 2. The resin composition according to claim 1, which is reversibly fluidized and non-fluidized by irradiation with light.
3. 3. The resin composition according to claim 2, wherein the wavelength of the light irradiation is within a range of 280 to 480 nm.
4. A toner for developing electrostatic images, comprising the resin composition according to claim 1 .
5. 5. The toner for developing electrostatic images according to claim 4, wherein the toner base particles contain a binder resin.
6. 6. The toner for developing electrostatic images according to claim 5, wherein the binder resin contains at least one resin selected from the group consisting of styrene-acrylic resins and polyester resins.
7. 7. The toner for developing an electrostatic image according to claim 4, wherein the toner base particles contain a colorant.
8. 8. The toner for developing an electrostatic image according to claim 4, wherein the toner base particles contain a releasing agent.
9. An image forming method using the toner for developing an electrostatic image according to any one of claims 4 to 8, An image forming method comprising: a step of forming a toner image made of the toner for developing an electrostatic image on a recording medium; and a step of irradiating the toner image with light to soften the toner image.
10. 10. The image forming method according to claim 9, wherein the wavelength of the light irradiation is within a range of 280 to 480 nm.
11. 11. The image forming method according to claim 9, further comprising a step of pressing the toner image.
12. 12. The image forming method according to claim 11, wherein in the pressurizing step, the toner image is further heated.
13. A photosensitive adhesive comprising a compound represented by the following general formula (1): [Case 2] [In general formula (1), Z 1 and Z 2 each independently represents N or CH, and Z 1 ≠Z 2 It is. 1 and A 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted aromatic heterocyclic group. 1 and L 2represents a linking group; n represents 0 or 1; B represents a complementary multiple hydrogen bonding group, which is any one of residues of a compound selected from adenine, thymine, 2,6-diacetylaminopyridine, melamine, cyanuric acid, and 4,6-diamino-2-pyrimidinone; G represents a substituent or the complementary multiple hydrogen bonding group, and when G is a substituent, n=0.]
Citation Information
Patent Citations
Electrophotographic toner
JP1993273788A
Image forming apparatus
JP2014191077A
Developer and fixing method
JP2014191078A
Method for forming resist pattern, permanent mask resist and photosensitive resin composition
JP2018156111A
Polyimide and photosensitive resin composition
JP2018203959A