Wafer with piezoelectric actuator, method for manufacturing wafer with piezoelectric actuator, method for manufacturing piezoelectric actuator, and method for manufacturing inkjet head
By arranging piezoelectric actuators on a wafer with uniform distance from end faces to the center and optimizing shape, the method ensures consistent piezoelectric properties across actuators, enhancing inkjet head performance.
Patent Information
- Application Number
- JP2020147410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-02
AI Technical Summary
Existing methods for manufacturing piezoelectric actuators result in non-uniform distribution of piezoelectric properties across a wafer, leading to variations in ink ejection characteristics among nozzles of an inkjet head.
The arrangement of piezoelectric actuators on a wafer is optimized such that the distance from the midpoint of both end faces in the longitudinal direction to the center point is approximately the same, with each actuator having a length of 1/3 or more of the wafer diameter, and featuring rounded corners or reverse tapered cross-sections to ensure uniformity.
This approach enables the production of a large number of piezoelectric actuators with consistent piezoelectric properties, reducing variations in ink ejection speed and improving the performance of inkjet heads.
Smart Images

Figure 0007593012000002 
Figure 0007593012000003 
Figure 0007593012000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer with a piezoelectric actuator, a piezoelectric actuator, an inkjet head, and methods for manufacturing the same, and more particularly to a wafer with a piezoelectric actuator that can produce a large number of piezoelectric actuators having good uniformity in piezoelectric characteristics. [Background technology]
[0002] The piezoelectric actuator used in the piezoelectric thin film inkjet head has many piezoelectric actuator units corresponding to the nozzles of the inkjet head, and each piezoelectric actuator unit has its own piezoelectric element and pressure chamber. In order to suppress the variation in the ink discharge characteristics between the nozzles of the inkjet head, it is desirable to make the piezoelectric characteristics between the piezoelectric elements of each piezoelectric actuator unit as uniform as possible.
[0003] One conventional method for manufacturing piezoelectric actuators involves manufacturing a wafer with piezoelectric actuators by forming multiple piezoelectric actuators in a lattice pattern on a single wafer, and then individualizing and producing each piezoelectric actuator as a single product.
[0004] The method for depositing the piezoelectric thin film is to deposit PZT (Pb(Zr,Ti)O 3 Conventionally, films have been formed by sputtering using a target such as lead zirconate titanate (PZT). Piezoelectric thin films formed by sputtering have high piezoelectric properties because heating promotes crystal growth, but the distribution of the piezoelectric properties tends not to be uniform across the entire wafer. The distribution of the piezoelectric properties is affected by the temperature and plasma distribution during sputtering, but in terms of the design of the sputtering device, it is common to control the temperature and plasma distribution so that they are uniform in a concentric pattern.
[0005] For example, (1) inner and outer heaters are arranged concentrically to heat a heat-equalizing plate (susceptor) and the inner and outer heaters are controlled independently, or (2) magnets are arranged concentrically or a mold unit with magnets embedded in it is rotated to uniformly distribute the applied magnetic field and thus the plasma. By using these techniques, it is possible to control the distribution of the piezoelectric properties concentrically, but it is difficult to make the piezoelectric properties uniform over the entire wafer.
[0006] Therefore, in the case of a wafer with piezoelectric actuators in which the piezoelectric actuators are arranged in a lattice pattern, the distribution of piezoelectric characteristics is not taken into consideration, and therefore, among the piezoelectric actuators individualized and made into single products from this wafer with piezoelectric actuators, only a few have good uniformity in the piezoelectric characteristics. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2009-45871 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a wafer with piezoelectric actuators, which can produce a large number of piezoelectric actuators having good uniformity in piezoelectric characteristics. [Means for solving the problem]
[0009] In order to solve the above problems, the inventors investigated the causes of the above problems and discovered that by arranging multiple piezoelectric actuators on a wafer so that the distance from the midpoint of each lower side of both longitudinal end faces of each piezoelectric actuator to the center point of the wafer with piezoelectric actuators is approximately the same, it is possible to obtain a large number of piezoelectric actuators with good uniformity in piezoelectric characteristics from a single wafer with piezoelectric actuators, which led to the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0010] 1. On the wafer 12 or more A wafer having a piezoelectric actuator, the piezoelectric actuator includes at least a piezoelectric element including a first electrode, a piezoelectric thin film, and a second electrode, and a plurality of pressure chambers; and On the wafer The above The arrangement of the piezoelectric actuators is The above The piezoelectric actuators are also arranged such that the distances from the midpoints of the lower sides of both longitudinal end faces to the center point of the piezoelectric actuator-equipped wafer are approximately the same.
[0011] 2. The wafer with piezoelectric actuators according to claim 1, wherein the longitudinal length of each of the piezoelectric actuators is 1 / 3 or more of the diameter of the wafer.
[0012] 3. The longitudinal direction of the piezoelectric actuator is not unidirectional. 3. The wafer with a piezoelectric actuator according to claim 1 or 2,
[0013] 4. The piezoelectric actuator The corners are chamfered. A wafer with a piezoelectric actuator according to any one of claims 1 to 3. .
[0014] 5. The piezoelectric actuator is A pressure chamber member is provided. The cross section of the pressure chamber member when cut along a plane perpendicular to the longitudinal direction of the piezoelectric actuator is an inverse tapered type. A wafer with a piezoelectric actuator according to any one of claims 1 to 4. .
[0016] 6 A method for manufacturing a wafer with piezoelectric actuators having 12 or more piezoelectric actuators on the wafer, comprising the steps of: the piezoelectric actuators are arranged on the wafer such that the distances from the midpoints of the lower sides of both end faces in the longitudinal direction of each of the piezoelectric actuators to the center point of the wafer with the piezoelectric actuators are substantially the same for each of the piezoelectric actuators; forming a piezoelectric element, which is composed of a first electrode, a piezoelectric thin film, and a second electrode, on a wafer by a sputtering method; forming a seed layer; depositing a pressure chamber member by Ni electroforming; and A method for manufacturing a wafer with piezoelectric actuators, wherein the step of depositing the pressure chamber member by Ni electroforming is characterized in that when depositing the pressure chamber member, the pressure chamber member is not deposited around each piezoelectric actuator.
[0017] 7 The method is characterized in that, when the piezoelectric thin film is formed by sputtering, the temperature and plasma distribution are controlled so as to be uniform concentrically on the wafer. 6 Item 1. A method for manufacturing a wafer with a piezoelectric actuator according to item 1.
[0018] 8 The longitudinal direction of the piezoelectric actuator is not in one direction. 6 Section or Article 7 Item 1. A method for manufacturing a wafer with a piezoelectric actuator according to item 1. 9 .No. 6 From item to item 8 A method for manufacturing a piezoelectric actuator using the method for manufacturing a wafer with a piezoelectric actuator according to any one of claims 1 to 5, transferring the piezoelectric actuators from the wafer with the piezoelectric actuators onto another support substrate and removing the wafer; forming a plurality of piezoelectric elements in each piezoelectric actuator by patterning the first electrode and the piezoelectric thin film; and removing the seed layer around each of the piezoelectric actuators to separate each of the piezoelectric actuators.
[0019] 10 The present invention is characterized in that the corners of the piezoelectric actuator are rounded. 9 Item 14. A method for manufacturing the piezoelectric actuator according to item 13.
[0020] 11 The cross section of the pressure chamber member when cut along a plane perpendicular to the longitudinal direction of the piezoelectric actuator is processed to have an inverse tapered shape. 9 Section or Article 10 Item 14. A method for manufacturing the piezoelectric actuator according to item 13.
[0021] 12 .No. 9 From item to item 11 3. A method for manufacturing an inkjet head, comprising the steps of: Effect of the Invention
[0022] According to the above-mentioned means of the present invention, it is possible to provide a wafer with piezoelectric actuators, which is capable of producing a large number of piezoelectric actuators having good uniformity in piezoelectric characteristics.
[0023] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.
[0024] In the case of a wafer with piezoelectric actuators in which the piezoelectric characteristics are uniform concentrically, the piezoelectric characteristics of the piezoelectric thin film at locations that are the same distance from the center point of the wafer will be identical, but the piezoelectric characteristics of the piezoelectric thin film at locations that are different distances from the center point of the wafer will not necessarily be identical. Therefore, when piezoelectric actuators are arranged in a lattice pattern on a wafer as in the conventional method, depending on the location of the actuator, the piezoelectric characteristics of the piezoelectric thin film within each piezoelectric actuator may not be uniform. However, in piezoelectric actuators arranged so that the distance from each midpoint of the lower side of both longitudinal end faces to the center point of the wafer with piezoelectric actuator is approximately the same, the piezoelectric characteristics of the piezoelectric elements at both ends are identical, and there is also no significant difference in the piezoelectric characteristics of the piezoelectric elements on the inside, so that piezoelectric actuators arranged in this manner have good uniformity in their piezoelectric characteristics. Therefore, by arranging all the piezoelectric actuators in this manner, it is possible to obtain only piezoelectric actuators with excellent uniformity in piezoelectric characteristics from a single wafer. This makes it possible to obtain many piezoelectric actuators with excellent uniformity in piezoelectric characteristics suitable for inkjet heads from a single wafer. [Brief description of the drawings]
[0025] [Figure 1] Top view of wafer with piezoelectric actuator [Diagram 2] Diagram showing the arrangement of piezoelectric actuators on a wafer [Diagram 3] A diagram showing an example of an arrangement of piezoelectric actuators of different sizes. [Figure 4] Enlarged plan view of a wafer with a piezoelectric actuator [Diagram 5] Enlarged cross-sectional view of a wafer with a piezoelectric actuator [Figure 6] Plan view of piezoelectric actuator (after individualization, before individualization) [Figure 7] Cross-sectional view of a piezoelectric actuator (after individualization, before individualization) [Figure 8]Cross-sectional view of piezoelectric actuator (after being made into a single product) [Figure 9] Plan view of piezoelectric actuator (after individualization) [Figure 10] 1 is a cross-sectional view showing a process of forming a first electrode and a piezoelectric thin film; [Figure 11] Cross-sectional view showing the process of forming an insulating film [Figure 12] 4 is a cross-sectional view showing a process of forming a second electrode; [Figure 13] Cross-sectional views showing the ink blocking film forming process [Figure 14] 1 is a cross-sectional view showing a seed layer formation process; [Figure 15] Cross-sectional view showing the process of forming the DFR layer [Figure 16] Plan view showing the process of forming the DFR layer [Figure 17] Cross-sectional view showing the process of forming a DFR layer to create an inverse tapered cross section of a piezoelectric actuator [Figure 18] 4 is a cross-sectional view showing a lamination process of the pressure chamber member; [Figure 19] Diagram of electroplating equipment [Figure 20] Cross-sectional view showing the DFR layer removal process [Figure 21] Plan view showing the DFR layer removal process [Figure 22] Cross-sectional view showing the bonding process of the support substrate [Diagram 23] Cross-sectional view showing a wafer removal process [Figure 24] 1 is a cross-sectional view showing a patterning step of a first electrode; [Diagram 25] Cross-sectional view showing the patterning process of the piezoelectric thin film [Figure 26] Cross-sectional view showing the process of forming a protective film [Figure 27] Cross-sectional view showing the individualization process [Figure 28] Plan view of wafer 1 with piezoelectric actuator (present invention) [Figure 29] Plan view of wafer 2 with piezoelectric actuator (comparative example) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The wafer with piezoelectric actuators of the present invention is a wafer with piezoelectric actuators having a plurality of piezoelectric actuators on the wafer, the piezoelectric actuators at least comprising a piezoelectric element consisting of a first electrode, a piezoelectric thin film, and a second electrode, and a plurality of pressure chambers, and the arrangement of the plurality of piezoelectric actuators on the wafer is such that the distances from the respective midpoints of the lower sides of both end faces in the longitudinal direction of each piezoelectric actuator to the center point of the wafer with piezoelectric actuators are substantially the same for each piezoelectric actuator. This feature is a technical feature common to or corresponding to the following embodiments.
[0027] In an embodiment of the wafer with piezoelectric actuator of the present invention, the longitudinal length of any of the piezoelectric actuators is preferably equal to or greater than 1 / 3 of the diameter of the wafer, since this allows many piezoelectric elements to be arranged within one actuator, making it possible to provide a large number of nozzles, and the like, thereby improving the performance of the piezoelectric actuator.
[0028] As an embodiment of the piezoelectric actuator-equipped wafer of the present invention, it is preferable that the wafer has 12 or more piezoelectric actuators, since this allows the production of more piezoelectric actuators within a wafer and reduces costs.
[0029] The piezoelectric actuator of the present invention is a piezoelectric actuator formed using the piezoelectric actuator-equipped wafer of the present invention, and is characterized in that the corners are rounded or the cross section is inversely tapered. The corners are rounded, which is preferable in that it is possible to prevent foreign matter from falling off when the ink flow path member is bonded. The cross section is inversely tapered, which is preferable in that it is possible to reduce the overflow of adhesive when the ink flow path member is bonded.
[0030] The inkjet head of the present invention is characterized by including the piezoelectric actuator of the present invention.
[0031] The method for manufacturing a wafer with piezoelectric actuators of the present invention is a method for manufacturing a wafer with piezoelectric actuators having a plurality of piezoelectric actuators on the wafer, wherein the arrangement of the plurality of piezoelectric actuators on the wafer is such that the distance from the midpoint of each lower side of both longitudinal end faces of each piezoelectric actuator to the center point of the wafer with piezoelectric actuators is approximately the same, and the method includes the steps of depositing a piezoelectric element consisting of a first electrode, a piezoelectric thin film, and a second electrode on the wafer by a sputtering method, forming a seed layer, and depositing a pressure chamber member by a Ni electroforming method, and is characterized in that the pressure chamber member is not deposited around each piezoelectric actuator when depositing the pressure chamber member.
[0032] In an embodiment of the method for manufacturing a wafer with a piezoelectric actuator of the present invention, when the piezoelectric thin film is formed by a sputtering method, it is preferable to control the temperature and plasma distribution so as to be uniform concentrically on the wafer, since this makes it possible to make the piezoelectric characteristics of the piezoelectric thin film uniform on concentric circles.
[0033] The method for manufacturing a piezoelectric actuator of the present invention is a method for manufacturing a piezoelectric actuator using the method for manufacturing a wafer with a piezoelectric actuator of the present invention, and is characterized by comprising the steps of transferring the piezoelectric actuator from the wafer with a piezoelectric actuator to another support substrate and removing the wafer, patterning the first electrode and the piezoelectric thin film to form a plurality of piezoelectric elements in each piezoelectric actuator, and removing the seed layer around each piezoelectric actuator to individualize each piezoelectric actuator.
[0034] As an embodiment of the method for manufacturing a piezoelectric actuator of the present invention, it is preferable to perform R-chamfering on the corners of the piezoelectric actuator, since this makes it possible to manufacture a piezoelectric actuator that can prevent foreign matter from falling off when the ink flow path member is bonded.
[0035] As an embodiment of the method for manufacturing a piezoelectric actuator of the present invention, it is preferable to process the cross section of the piezoelectric actuator into an inverted tapered shape, since this makes it possible to manufacture a piezoelectric actuator that can reduce the overflow of adhesive when bonding an ink flow path member.
[0036] The method for producing an inkjet head of the present invention is characterized by using the method for producing a piezoelectric actuator of the present invention.
[0037] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower limit and upper limit.
[0038] 1. Overview of the wafer with piezoelectric actuator The wafer with piezoelectric actuators of the present invention is a wafer with piezoelectric actuators having a plurality of piezoelectric actuators on the wafer, wherein the piezoelectric actuators at least comprise a piezoelectric element consisting of a first electrode, a piezoelectric thin film, and a second electrode, and a plurality of pressure chambers, and the arrangement of the plurality of piezoelectric actuators on the wafer is such that the distance from each midpoint of each lower side of both longitudinal end faces of each piezoelectric actuator to the center point of the wafer with piezoelectric actuators is approximately the same.
[0039] Furthermore, the wafer with piezoelectric actuators of the present invention exhibits the effects of the present invention particularly when the longitudinal length of each piezoelectric actuator is 1 / 3 or more of the diameter of the wafer. This is because the importance of uniform piezoelectric characteristics increases as the longitudinal length of the piezoelectric actuator increases. Furthermore, in the case of a conventional lattice-like arrangement, when the longitudinal length of the piezoelectric actuators is 1 / 3 or more of the diameter of the wafer, only two rows or one row can be arranged on the wafer, which drastically reduces the number of piezoelectric actuators that can be obtained from one wafer.
[0040] Furthermore, the piezoelectric actuator-equipped wafer of the present invention exhibits the effects of the present invention particularly when it has 12 or more piezoelectric actuators, because in the case of a conventional lattice-like arrangement, the greater the number of piezoelectric actuators, the greater the proportion of piezoelectric actuators with non-uniform piezoelectric characteristics.
[0041] In addition, in the wafer with piezoelectric actuators of the present invention, it is preferable that the corners of each piezoelectric actuator are rounded, since this increases the number of piezoelectric actuators that can be arranged on one wafer. It is also preferable that piezoelectric actuators having rounded corners can be manufactured. Piezoelectric actuators having rounded corners are preferable because they can prevent foreign matter from falling off when the ink flow path member is bonded.
[0042] In addition, in the wafer with piezoelectric actuators of the present invention, it is preferable that the cross section of each piezoelectric actuator is an inverse tapered type, since it is possible to manufacture a piezoelectric actuator having an inverse tapered cross section. A piezoelectric actuator having an inverse tapered cross section is preferable because it is possible to reduce the overflow of adhesive when adhering an ink flow path member.
[0043] In this application, a "piezoelectric actuator" refers to one that has at least a piezoelectric element and a pressure chamber. Even if it is formed on a support substrate (including a wafer), if it has a piezoelectric element and a pressure chamber, that part is called a "piezoelectric actuator." Separating other piezoelectric actuators from components other than the support substrate is called "individualization," and separating it from the support substrate is called "single product."
[0044] The wafer with piezoelectric actuator of the present invention will now be described with reference to the drawings.
[0045] 1 is a plan view of a wafer with a piezoelectric actuator. When viewed from above, the wafer with a piezoelectric actuator is divided into a piezoelectric actuator 101, a through groove portion 102, and other regions. The through groove portion 102 and other regions are regions that do not become piezoelectric actuators. The through groove portion 102 refers to a region in which a pressure chamber member is not formed in order to individualize the piezoelectric actuator, and refers to a region of about 1 mm around the outside of the piezoelectric actuator.
[0046] FIG. 2(a) is a diagram showing the arrangement of the piezoelectric actuators 101 on the wafer 201. For the sake of explanation, only one piezoelectric actuator 101 is arranged. FIG. 2(b) is a perspective view showing the piezoelectric actuator 101 in a simplified rectangular parallelepiped form. The double-headed arrows in FIG. 2(b) indicate the longitudinal direction. In the present application, the longitudinal end faces refer to two faces positioned perpendicular to the longitudinal direction, and are the faces indicated by diagonal lines in FIG. 2(b). In addition, the midpoints of the lower sides of the longitudinal end faces are indicated by two points in FIG. 2(b). The wafer with piezoelectric actuators of the present invention is characterized in that the midpoints of the lower sides of the longitudinal end faces (the two midpoints on each lower side) of each piezoelectric actuator 101 are arranged so that the distances to the center point of the wafer with piezoelectric actuators are approximately the same, as shown in FIG. 2(a).
[0047] The positional relationship between different piezoelectric actuators is not limited as long as the two midpoints of each piezoelectric actuator are disposed so that the distances to the center point of the wafer with piezoelectric actuators are approximately the same.
[0048] The term "approximately the same" means that the difference in distance is within 10%, preferably within 5%, and more preferably within 3%, including "the same." The smaller the difference in distance, the better the uniformity of the piezoelectric characteristics can be.
[0049] FIG. 3 is a diagram showing an example in which piezoelectric actuators of different sizes are arranged. As shown in FIG. 3, the wafer with piezoelectric actuators of the present invention allows piezoelectric actuators of different sizes to be arranged on the same wafer. Although not shown, piezoelectric actuators with different corner shapes can also be arranged on the same wafer. This makes it possible to simultaneously manufacture piezoelectric actuators of different models. In addition, since the area on the wafer can be effectively utilized, the number of piezoelectric actuators that can be arranged on one wafer can be increased.
[0050] 4 is an enlarged plan view of a wafer with a piezoelectric actuator, and is an enlarged view of a portion corresponding to range E in FIG. 1. When viewed from above, the wafer with a piezoelectric actuator of the present invention has portions on which pressure chamber material is deposited and portions on which it is not deposited. Piezoelectric actuator 101 has pressure chamber interior 103 and pressure chamber wall portion 104. No pressure chamber material is deposited in pressure chamber interior 103, and pressure chamber material is deposited on pressure chamber wall portion 104. No pressure chamber material is deposited in through groove portion 102. FIG. 4 shows, as an example, pressure chambers arranged in two rows within each piezoelectric actuator.
[0051] Fig. 5 is an enlarged cross-sectional view of the wafer with piezoelectric actuators, and corresponds to the dashed line FF in Fig. 4. The following description will be given with reference to Fig. 5.
[0052] The piezoelectric actuator 101 of the piezoelectric actuator wafer of the present invention is characterized by having at least a piezoelectric element 106 consisting of a first electrode 202, a piezoelectric thin film 203 and a second electrode 205, and a plurality of pressure chambers 105.
[0053] In the wafer with piezoelectric actuators of the present invention, each piezoelectric actuator 101 has a plurality of pressure chambers 105, but the number and arrangement of the pressure chambers are not particularly limited. For example, there may be 200 per row x 4 rows, totaling 800 pressure chambers.
[0054] Moreover, it is preferable that an insulating film 204 is formed between the piezoelectric thin film 203 and the second electrode 205 by patterning.
[0055] In addition, a seed layer 207 for depositing the pressure chamber member 210 may be formed below the piezoelectric chamber member 210.
[0056] In addition, it is preferable that an ink blocking film 206 is formed between the second electrode 205 and the seed layer 207 by patterning.
[0057] The material, thickness, etc. of each component will be described in detail in the description of the manufacturing method below.
[0058] 2. Overview of Piezoelectric Actuators The piezoelectric actuator of the present invention is a piezoelectric actuator formed using the piezoelectric actuator-equipped wafer of the present invention, and is characterized in that the corners are rounded or the cross section is inversely tapered, or may have both of these characteristics.
[0059] In this application, as described above, the piezoelectric actuator includes a state in which it is fixed to a wafer as shown in FIG. 5, but also a state in which the piezoelectric elements are patterned to correspond to each piezoelectric actuator unit by processing as described below, or a state in which they are individualized or made into individual products.
[0060] FIG. 6 is a plan view of a piezoelectric actuator (after individualization, before being made into a single product).
[0061] 7 is a cross-sectional view of a piezoelectric actuator (after individualization, before being made into a single product). Although it is individualized because members such as the seed layer of the through groove portion 102 have been removed, the piezoelectric actuator is not yet made into a single product because it is fixed to the support substrate 211 via the thermal release sheet 212. The piezoelectric actuator 101 has a plurality of piezoelectric actuator units 107, and each piezoelectric actuator unit 107 has one piezoelectric element 106 and one pressure chamber 105.
[0062] In addition, it is preferable that the surface of the piezoelectric actuator has a protective film 213 .
[0063] 8 is a cross-sectional view of a piezoelectric actuator (after being separated from a supporting substrate) according to an embodiment of the present invention.
[0064] Moreover, the piezoelectric actuator in FIG. 8 represents a piezoelectric actuator having an inverted tapered cross section.
[0065] Figure 9 is a plan view of a piezoelectric actuator (after being made into a single product). Figure 9(a) is a plan view of a piezoelectric actuator without R-surface treatment, and Figure 9(b) is a plan view of a piezoelectric actuator with R-surface treatment on the corners.
[0066] The material and shape of each component will be described in detail in the description of the manufacturing method below.
[0067] 3. Overview of Inkjet Heads The inkjet head of the present invention is characterized by including the piezoelectric actuator of the present invention.
[0068] As long as the piezoelectric actuator of the present invention is included, other members are not particularly limited. For example, the ink flow path member and nozzle plate described in JP-A-2009-45871 can be used.
[0069] 4. Method for manufacturing a wafer with piezoelectric actuators according to the present invention The method for manufacturing a wafer with piezoelectric actuators of the present invention is a method for manufacturing a wafer with piezoelectric actuators having a plurality of piezoelectric actuators on the wafer, wherein the arrangement of the plurality of piezoelectric actuators on the wafer is such that the distance from the midpoint of each lower side of both longitudinal end faces of each piezoelectric actuator to the center point of the wafer with piezoelectric actuators is approximately the same, and the method includes the steps of depositing a piezoelectric element consisting of a first electrode, a piezoelectric thin film, and a second electrode on the wafer by a sputtering method, forming a seed layer, and depositing a pressure chamber member by a Ni electroforming method, and is characterized in that the pressure chamber member is not deposited around each piezoelectric actuator when depositing the pressure chamber member.
[0070] When forming the piezoelectric thin film by sputtering, it is preferable to control the temperature and plasma distribution so as to be uniform and concentric on the wafer.
[0071] Hereinafter, the method for producing a wafer with a piezoelectric actuator according to the present invention will be described with reference to the drawings.
[0072] As shown in FIG. 10, a first electrode 202 and a piezoelectric thin film 203 are formed on the entire surface of a wafer 201 .
[0073] The wafer 201 is preferably a silicon wafer. Although there is no particular limit to the size, the diameter φ is preferably within the range of 6 to 12 inches.
[0074] Although not shown, an adhesive layer may be formed before the first electrode 202 is formed in order to improve the adhesiveness between the wafer 201 and the first electrode 202 .
[0075] The adhesion layer can be obtained, for example, by using a Ti target, applying 500 W of high frequency power while heating the wafer 201 to 400° C., and forming the adhesion layer by sputtering for 1 minute in argon gas with a gas pressure of 1 Pa during sputtering.
[0076] The target is not limited to Ti, but may be tantalum, iron, cobalt, nickel, chromium, or a compound thereof.The thickness of the adhesive layer is preferably within the range of 0.005 to 0.2 μm.
[0077] Next, the first electrode 202 is formed.
[0078] The thickness of the first electrode 202 is preferably within the range of 0.005 to 2 μm.
[0079] The first electrode can be formed by a sputtering method. For example, a Pt target is used, and sputtering is performed for 12 minutes with a high frequency power of 500 W in argon gas with a gas pressure of 1 Pa during sputtering while heating the wafer to 600° C. The target may be any one of platinum, iridium, palladium, and ruthenium, or a compound thereof.
[0080] Next, the piezoelectric thin film 203 is formed by sputtering.
[0081] The thickness of the piezoelectric thin film 203 is preferably within the range of 1 to 10 μm.
[0082] When the piezoelectric thin film 203 is formed by sputtering, it is preferable to control the temperature and plasma distribution so as to be uniform and concentric on the wafer. For example, by arranging inner and outer heaters concentrically to heat a heat equalizing plate (susceptor), and independently controlling the inner and outer heaters, it is possible to control the temperature distribution to be uniform concentrically on the wafer.Also, by arranging magnets in a concentric direction or rotating a mold unit with magnets embedded in it to uniformize the distribution of the applied magnetic field, it is possible to control the plasma distribution to be uniform concentrically on the wafer.
[0083] The target is PZT (Pb(Zr,Ti)O 3It is preferable to use lead zirconate titanate (PZT). When PZT is used, the Zr / Ti composition is preferably Zr / Ti=30 / 70 to 70 / 30. In addition, the target may be a piezoelectric material whose main component is PZT, such as PZT containing additives such as La, Sr, Nb, or Al, or PMN (Pb(Mg,Nb)O 3 : Lead magnesium oxide niobate) and PZN (Pb(Zn,Nb)O 3 : lead zincate niobate) can also be used.
[0084] Next, it is preferable to form an insulating film 204 as shown in FIG. The insulating film 204 can be formed, for example, by applying a photosensitive polyimide resin by a spin coating method. The insulating film 204 is formed in the area where the lead wiring, the electrode pads, etc. are formed, and is mainly used to prevent short circuits.
[0085] A mask pattern that removes the insulator film is transferred by exposure to light in the through groove and the area where the piezoelectric thin film is to be formed between the first and second electrodes, and then developed. After patterning, the film is hardened by baking at 300°C. The exposure device can be a device corresponding to the wafer size, such as the UX-4438SC aligner manufactured by Ushio Inc. (hereinafter, in this application, the same device can be used for exposure).
[0086] In addition, the insulating film 204 is not a coating of photosensitive polyimide resin, but a SiO 2 Alternatively, the insulating layer 11 can be formed by forming a film of an inorganic material such as the above by a sputtering method.
[0087] The arrangement and shape of the region in which the piezoelectric actuator is formed are determined by the patterning of the through groove portion when forming the pressure chamber member described below, but when forming the insulator film 204, the arrangement and shape of the patterning of the insulator film 204 must also correspond to the arrangement and shape of the patterning of the through groove portion.
[0088] In the wafer with piezoelectric actuators of the present invention, each piezoelectric actuator is positioned so that the distance from each midpoint of the lower side of both end faces in the longitudinal direction to the center point of the wafer with piezoelectric actuators is approximately the same, and the patterning of the insulator film also corresponds to this arrangement.
[0089] Furthermore, when each piezoelectric actuator is processed to have rounded corners, the insulating film 204 is also patterned to correspond to this shape.
[0090] Next, the second electrode 205 is formed as shown in FIG.
[0091] The second electrode 205 can be formed by a sputtering method. For example, it can be formed by stacking two kinds of metal films. A Cu film of 1.5 μm can be obtained by forming the second electrode 205 at room temperature with 500 W high frequency power in argon gas with a gas pressure of 1 Pa during sputtering for 170 minutes using a Cu target. A Cr film of 2.0 μm can be obtained by forming the second electrode 205 at room temperature with 500 W high frequency power in argon gas with a gas pressure of 1 Pa during sputtering for 220 minutes using a Cr target.
[0092] The material of the second electrode 205 is not limited to Cu or Cr, but may be nickel, aluminum, tantalum, tungsten, silicon, or oxides or nitrides thereof (for example, silicon dioxide, aluminum oxide, zirconium oxide, silicon nitride), or the like.
[0093] Moreover, the total film thickness of the second electrode 205 is preferably within the range of 1 to 10 μm.
[0094] Furthermore, when two types of metal films are laminated, it is preferable that the metal film provided closer to the piezoelectric thin film 203 is made of a material with a smaller Young's modulus than the other metal film. This reduces stress concentration in the piezoelectric thin film 203 during the fabrication of the laminate, allowing for a stable process. Also, since the displacement surface of the piezoelectric thin film 203 is set farther outward, more efficient energy generation is achieved.
[0095] Next, as shown in FIG. 13, an ink blocking film 206 is formed on the second electrode 205 if necessary.
[0096] The ink blocking film 206 can prevent the penetration of ink and also prevent cracks in the piezoelectric thin film. It also functions as a stress relaxation layer. The thickness of the ink blocking film 206 is preferably within the range of 1.0 to 1.5 μm.
[0097] The ink blocking film 206 can be formed, for example, by applying a photosensitive polyimide resin by spin coating and curing it by baking at 200°C.
[0098] Although not shown, the ink blocking film in the through groove portion may be removed in this process. When removing the ink blocking film in the through groove portion in this process, a mask pattern for removing the through groove portion can be transferred by exposure and developed before the photosensitive polyimide resin is cured.
[0099] Furthermore, when forming the ink blocking film 206, an adhesion layer may be formed on the ink blocking film 206 in order to increase adhesion between the ink blocking film 206 and a seed layer 207 described below. The material of the adhesion layer may be selected in consideration of compatibility with the ink blocking film, and for example, Cr, Ti, Mo, etc. may be used.
[0100] Next, a seed layer is formed as shown in FIG. The seed layer 207 is formed on the entire surface of the wafer, including the through grooves. It can be formed by a sputtering method, and the target used is the same as the material of the pressure chamber member 210 described later. The thickness is preferably about 0.5 μm.
[0101] Next, the pressure chamber member is formed. As a pretreatment, it is preferable to first carry out a degreasing treatment. The degreasing process can be carried out by, for example, using a mixture of a surfactant (L505-B manufactured by World Metals) and pure water in a ratio of 1:5, and treating for 1 minute at a liquid temperature of 40°C. After the degreasing process, it is recommended to rinse and wash with pure water, and then perform an acid wash. The acid wash can be carried out by using 10% hydrochloric acid, treating for 30 seconds at a liquid temperature of 40°C. After the acid wash, rinse and wash with pure water.
[0102] Next, dry film resist layers 208 and 209 are formed as shown in Figures 15 and 16. Figure 16 is an enlarged view of a portion corresponding to the range G in Figure 4. The term "dry film resist" refers to a film-like resist material that is applied to a wiring board to form a circuit when producing a printed wiring board or the like.
[0103] The material of the dry film resist (DFR) layer is not particularly limited, but for example, ORDYL MP108 manufactured by Tokyo Ohka Co., Ltd. can be used. The thickness of the dry film resist layer may be determined according to the height of the pressure chamber.
[0104] To form the dry film resist layer, first a dry film resist is applied to the entire surface, and then a mask pattern for removing the pressure chamber interior 103 and the through groove portion 102 is transferred by exposure and developed. This leaves a dry film resist layer 208 in the area that will become the pressure chamber interior 103 and a dry film resist layer 209 in the area that will become the through groove portion 102.
[0105] At this time, the through grooves 102 are patterned so that the distances from the midpoints of both end faces in the longitudinal direction to the center point of the wafer with piezoelectric actuators are approximately the same in each region in which the piezoelectric actuators are formed.
[0106] Furthermore, by patterning the through groove portion 102 so that the corners of the area in which the piezoelectric actuator is to be formed have a R-chamfered shape, it is possible to produce a wafer with piezoelectric actuators in which the corners of the piezoelectric actuators have a R-chamfered shape.
[0107] By lengthening the exposure time and development time, the shape of the dry film resist layer can be adjusted so that the width becomes narrower toward the bottom, as shown in Fig. 17, and the cross-sectional shapes of the pressure chamber member 210 and the piezoelectric actuator can be adjusted to be inversely tapered. For example, the cross section of the piezoelectric actuator can be processed to be inversely tapered by performing exposure processing at 500 W for 40 seconds using a UX-4438SC aligner manufactured by Ushio Inc., and developing processing in a 0.1% sodium carbonate aqueous solution at 30°C for 1 minute. By changing the exposure and development conditions, when the height of the dry film resist is 160 μm, the difference in width between the top and bottom of the dry film resist layer can be adjusted within the range of 0 to 30 μm.
[0108] By forming the dry film resist layer 208, when the pressure chamber members are deposited by Ni electroforming, the pressure chamber members can be prevented from being deposited inside each pressure chamber.
[0109] By forming the dry film resist layer 209, when the pressure chamber member is deposited by Ni electroforming, the pressure chamber member can be prevented from being deposited in the through groove portion (around each piezoelectric actuator).
[0110] Next, a degreasing treatment is preferably carried out. The degreasing treatment can be carried out in the same manner as described above.
[0111] Next, the pressure chamber member 210 is deposited by Ni electroforming. 18, a pressure chamber member 210 made of Ni is deposited by Ni electroforming in the portion from which the dry film resist has been removed. The pressure chamber member 210 is not deposited in the portion where the dry film resist layer 208 and the dry film resist layer 209 remain without being removed.
[0112] The pressure chamber member 210 made of Ni may contain small amounts of other metals, such as Co, Mo, and Ru.
[0113] From the viewpoint of workability and processing accuracy in the grinding process described below, it is preferable that the hardness of the deposited pressure chamber member 210 is within the range of 400 to 700 Hv. The hardness can be measured by an ultra-microindentation hardness tester ENT110a manufactured by Elionix.
[0114] (Example of Ni electroforming) As an example of a method for depositing the pressure chamber member 210 by Ni electroforming, a method using a Ni electroplating apparatus shown in FIG. 19 will be described.
[0115] 19, a wafer in a process stage on which a dry film resist layer has been formed is fixed at a predetermined position on cathode electrode 403 of the Ni electroplating device, and setting is performed in a state of electrical continuity with cathode electrode 403. Next, cathode electrode 403 is set in plating tank 402, shielding plate 405 is sandwiched in plating solution 412, and a voltage is applied between anode electrode 404 and workpiece 401 by rectifier 406 to pass electricity, thereby performing electroplating.
[0116] The Ni electroplating apparatus shown in FIG. 19 is configured to circulate a plating solution 412 between a plating tank 402 and a reserve tank 407, and a circulation pump 409, a filter 410, and a flowmeter 411 are installed between the plating tank 402 and the reserve tank 407. In the reserve tank 407, the plating solution is heated by a heater 408 to adjust the plating solution 412 to a constant temperature. The plating solution 412 is prepared by adding, for example, 56 L of 60% nickel sulfamate, 1.0 kg of nickel chloride, 3.0 kg of boric acid, 0.3 L of stress relaxation agent (NSF-H-4 manufactured by Nippon Kagaku Sangyo Co., Ltd.), and 1.0 L of pit prevention agent (Pitless S manufactured by Nippon Kagaku Sangyo Co., Ltd.) to a liquid volume of 100 L, and adding pure water to make the total volume 100 L. The ratio of the chemicals in the plating tank 402 and the reserve tank 407 is adjusted to 2:8. In order to adjust the hardness and gloss after electroplating, additives containing small amounts of other metals, such as Co, Mo, Ru, etc., can be added. These metals are contained in small amounts in Ni after deposition.
[0117] Specific conditions for Ni electroplating to form the pressure chamber member 210 are, for example, a distance between the cathode and anode of 85 mm, a circulation flow rate of 5 L / min, a liquid temperature of 40° C., and a pH kept in the range of 4.0 to 4.5, with a current density of 8 A / dm 2 By setting the temperature at 400° C. and performing electroplating for three hours, a pressure chamber material having a thickness of 180 μm can be deposited.
[0118] Next, the upper portion of the pressure chamber member is ground to a predetermined height. In order to make the pressure chamber member 210 have a predetermined height, the upper part of the pressure chamber member 210 is ground together with the dry film resist layers 208 and 209. This height is not particularly limited, and may be set to a height that is preferable as the height of the inside of the pressure chamber. For example, it is about 150 μm.
[0119] The grinding method is not particularly limited, but for example, grinding can be performed using a Disco Corporation grinding machine DAG810 with a resin grindstone #320 at a grindstone rotation speed of 4000 rpm, a table rotation speed of 300 rpm, and a rate of 15 μm / min.
[0120] Next, the dry film resist is removed. As shown in Figures 20 and 21, the dry film resist layers 208 and 209 are removed. Figure 21 is an enlarged view of the area corresponding to range G in Figure 4. The dry film resist layers 208 and 209 can be removed by immersing the substrate in a remover, MP2 manufactured by Tokyo Ohka Kogyo Co., Ltd., at a liquid temperature of 60 to 70°C for 3 hours, and by simultaneously using brush cleaning in between.
[0121] After the dry film resist layers 208 and 209 have been completely removed, the wafer is washed and dried to complete the production of a wafer with piezoelectric actuators.
[0122] In addition, if the dry film resist layer is difficult to remove due to grinding burrs generated by the above grinding, the grinding burrs may be treated by electrolytic polishing or the like before removing the dry film resist layer.
[0123] 5. Manufacturing method of the piezoelectric actuator of the present invention The method for manufacturing a piezoelectric actuator of the present invention is a method for manufacturing a piezoelectric actuator using the method for manufacturing a wafer with a piezoelectric actuator of the present invention, and is characterized by comprising the steps of transferring the piezoelectric actuator from the wafer with a piezoelectric actuator to another support substrate and removing the wafer, patterning the first electrode and the piezoelectric thin film to form a plurality of piezoelectric elements in each piezoelectric actuator, and removing the seed layer around each piezoelectric actuator to individualize each piezoelectric actuator.
[0124] Moreover, the corners of the piezoelectric actuator may be subjected to R-chamfering.
[0125] The cross section of the piezoelectric actuator may be processed to have an inverse tapered shape.
[0126] Hereinafter, a method for manufacturing a piezoelectric actuator of the present invention will be described with reference to FIGS.
[0127] The piezoelectric actuators are transferred from the wafer 201 to a supporting substrate 211 . 22, a support substrate 211 is attached onto a pressure chamber member 210 with a thermal release sheet 212. There is no particular limitation on the material of the support substrate 211, and a glass substrate or the like can be used. There is no particular limitation on the size of the support substrate 211 as long as it is large enough to fix all the piezoelectric actuators formed on the wafer, but it is preferable that the support substrate 211 is approximately the same size as the wafer.
[0128] At least the surface of the thermal release sheet 212 that is bonded to the piezoelectric actuator must be thermally peelable. The thermal release sheet 212 may be bonded to the support substrate 211 using a double-sided thermal release sheet, or may be bonded using an adhesive such as UV resin. The thermal release sheet 212 may be, for example, a product manufactured by Nitto Denko Corporation.
[0129] In addition, in consideration of the process load, a reinforcing adhesive may be applied to the edge of the wafer, etc., as necessary.
[0130] After the support substrate 211 is attached, the wafer 201 is removed as shown in Fig. 23. In Fig. 23, the top and bottom of the piezoelectric actuator are shown in reverse to those in Figs. 22 and 23. The wafer 201 can be removed by dry etching, but it is also possible to remove the wafer by grinding or the like beforehand until the thickness of the wafer is 50 to 100 µm before the dry etching. The etching gas is sulfur hexafluoride (SF 6 ) allows etching to be performed while minimizing the physical effects on the piezoelectric actuator, and the upper electrode acts as an etching stopper.
[0131] If an adhesive layer is formed between the wafer 201 and the first electrode 202, this adhesive layer can be removed in the same manner as the wafer 201, but it is not necessarily required to remove it.
[0132] Next, as shown in FIG. 24, the first electrode 202 is patterned by photolithography.
[0133] The first electrode 202 is separated by patterning so as to correspond to each piezoelectric actuator unit, and at the same time, the first electrode 202 between each actuator is removed.
[0134] Patterning by photolithography can be performed by forming a resist mask, removing it by dry etching, and peeling off the resist mask. The etching gas is argon, oxygen, trifluoromethane (CHF 3 ) may be used.
[0135] The resist mask can be formed by applying a resist, transferring a mask pattern by exposure, and developing. Hereinafter, the resist mask in this application is formed in the same manner unless otherwise specified.
[0136] When the first electrode 202 is patterned, a lead wiring and an electrode pad portion may be formed by extending from the first electrode.
[0137] Next, as shown in FIG. 25, the piezoelectric thin film 203 is patterned by photolithography.
[0138] The piezoelectric thin film 203 is separated into individual piezoelectric actuator units by patterning, and at the same time, the piezoelectric thin film 203 in the through groove portion is removed.
[0139] Patterning by photolithography can be performed by forming a resist mask, removing it by etching, and peeling off the resist mask. Etching can be either dry etching or wet etching. In the case of dry etching, a mixed gas of chlorine and bromine, for example, can be used as the etching gas. In the case of wet etching, a mixed liquid of an aqueous hydrofluoric acid solution and an aqueous nitric acid solution (hydrofluoric nitric acid) can be used as the etching solution.
[0140] Next, if necessary, a protective film 213 is formed as shown in FIG.
[0141] The protective film 213 can be formed by applying a photosensitive polyimide resin by a spin coating method.
[0142] When forming the protective film 213, after coating the entire surface, a mask pattern that removes the protective film from the through groove and electrode pad parts is transferred by exposure and developed. This allows patterning to be done on the parts excluding the electrode pad parts on the piezoelectric actuator. After patterning, it is cured by baking at 100°C.
[0143] Next, as shown in FIG. 27, the seed layer 207 in the through-groove portion, the second electrode 205 and the ink blocking film 206 are removed.
[0144] By removing the seed layer 207, the second electrode 205, and the ink blocking film 206 in the through-groove portion, each piezoelectric actuator is individualized, and the piezoelectric actuator on the support substrate is completed. The seed layer 207, the second electrode 205, and the ink blocking film 206 can be removed by laser processing, which can minimize damage to the piezoelectric actuator.
[0145] In addition, when the ink blocking film 206 is not formed, or when the ink blocking film 206 is formed but the ink blocking film 206 in the through groove portion is removed during formation, the seed layer 207 and the second electrode 205 can be removed by laser processing or by photolithography.
[0146] Removal by laser processing can be achieved by laser scanning the through groove portion using an IR (infrared) laser or UV (ultraviolet) laser.
[0147] Removal by photolithography can be performed by forming a resist mask on the piezoelectric actuator, removing the seed layer and the like in the through groove by etching, and peeling off the resist mask. After peeling off the resist mask, it is preferable to perform rinsing and cleaning.
[0148] When the material of the second electrode 205 is Cr, it can be etched using an etching solution prepared by mixing, for example, 1000 parts by mass of pure water, 200 parts by mass of potassium ferricyanide, and 60 parts by mass of sodium hydroxide. When the material of the second electrode 205 is Cu, it can be etched using an etching solution prepared by mixing, for example, 1000 parts by mass of pure water, 90 parts by mass of ammonium persulfate, and 6 parts by mass of ammonium chloride. Furthermore, when such an alkaline etching solution is used, it is preferable to use an alkaline-resistant rubber-based resist as the resist material, and for example, OMR resist manufactured by Tokyo Ohka Kogyo Co., Ltd. can be used.
[0149] The etching gas used to etch away the seed layer was argon and oxygen, CHF 3 A mixed gas of the above can be used.
[0150] Next, each piezoelectric actuator is removed from the support substrate 211 and separated into individual components. The individualized piezoelectric actuators are attached to the support substrate 211 with a thermal release sheet 212, and can be removed by heating the thermal release sheet to a temperature above the foaming temperature using a hot plate or a heating furnace.
[0151] 6. Method for manufacturing inkjet head of the present invention The method for producing an inkjet head of the present invention is characterized by using the method for producing a piezoelectric actuator of the present invention.
[0152] As long as the method for producing a piezoelectric actuator of the present invention is used, other steps and the like are not particularly limited.
[0153] For example, an inkjet head can be manufactured by transferring an adhesive to the lower end surface of the pressure chamber member of the piezoelectric actuator of the present invention, adjusting the alignment with a separately prepared ink flow path member, and bonding the two together with the adhesive.
[0154] The ink flow path member has a common liquid chamber, a supply port, and an ink flow path formed therein, and can be bonded to a nozzle plate having nozzle holes formed therein. EXAMPLES
[0155] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.
[0156] <Preparation of piezoelectric actuator 1> A wafer 1 with piezoelectric actuators was fabricated on an 8-inch silicon wafer with 20 piezoelectric actuators arranged as shown in Figure 28, and piezoelectric actuators 1 were then separated from the wafer 1 with piezoelectric actuators. The size of the piezoelectric actuator 1 was 68.2 mm on the long side and 12.8 mm on the short side, and each piezoelectric actuator had 200 units / row x 4 rows, for a total of 800 piezoelectric actuator units.
[0157] The above arrangement is such that the distances from the midpoints of the lower sides of both end faces in the longitudinal direction of each piezoelectric actuator to the center point of the wafer with the piezoelectric actuator are substantially the same.
[0158] In each process, a multi-target sputtering device was used for sputtering, and the exposure device used was the UX-4438SC aligner manufactured by Ushio Inc.
[0159] First, a 0.02 μm adhesive layer was formed on an 8-inch silicon wafer by sputtering using a Ti target. The sputtering was performed for 1 minute in argon gas at a temperature of 400° C., high-frequency power of 500 W, and gas pressure of 1 Pa during sputtering.
[0160] Next, a first electrode having a thickness of 0.2 μm was formed by sputtering using a Pt target at a temperature of 600° C., a high-frequency power of 500 W, and an argon gas pressure of 1 Pa during sputtering for 12 minutes.
[0161] Next, a 3 μm piezoelectric thin film was formed by sputtering using PZT. The sputtering was performed in a mixed atmosphere of argon and oxygen (gas volume ratio Ar:O) at a temperature of 580°C, high-frequency power of 500 W, and gas pressure of 0.3 Pa during sputtering. 2 The PZT used was a sintered body with a Pb content greater than the stoichiometric composition (Zr / Ti=53 / 47, Pb in excess of 20 mol%).
[0162] Next, a 1 μm insulator film was formed by applying photosensitive polyimide resin by spin coating and then patterning it. The patterning was performed by transferring a mask pattern that removes the insulator film from the through groove and the area where the piezoelectric element sandwiched between the first and second electrodes is to be formed by exposure, and developing it. After patterning, it was baked at 300°C to harden it.
[0163] Next, a second electrode consisting of a 1.5 μm Cu film and a 2.0 μm Cr film was formed by sputtering. The Cu film was sputtered for 170 minutes at room temperature, with a high-frequency power of 500 W and a gas pressure of 1 Pa in argon gas. The Cr film was sputtered for 120 minutes at room temperature, with a high-frequency power of 500 W and a gas pressure of 1 Pa in argon gas.
[0164] Next, a 1 μm thick ink blocking film was applied by spin coating photosensitive polyimide resin, and then cured by baking at 200°C.
[0165] Next, a 0.5 μm seed layer was formed by sputtering in argon gas at a high frequency power of 500 W and a gas pressure of 1 Pa during sputtering for 15 minutes.
[0166] Next, a 160μm dry film resist layer was formed by laminating two layers of 80μm-thick dry film resist, ORDYL MP108 manufactured by Tokyo Ohka Kogyo Co., Ltd. Next, a mask pattern for removing the inside of the pressure chamber and the through groove was transferred by exposure and developed. Exposure was performed at 500W for 40 seconds. Development was performed by processing in a 0.1% sodium carbonate aqueous solution at 30℃ for 1 minute.
[0167] Next, a pressure chamber member made of Ni was deposited to a thickness of 180 μm by Ni electroforming on the portion where the dry film resist layer had been removed. This pressure chamber member, together with the dry film resist layer, was ground to a height of 150 μm using a Disco Corporation grinding machine DAG810 with a resin grindstone #320 at a grindstone rotation speed of 4000 rpm, a table rotation speed of 300 rpm, and a speed of 15 μm / min.
[0168] Next, using MP2 manufactured by Tokyo Ohka Kogyo Co., Ltd., the substrate was immersed in the liquid at a temperature of 60 to 70°C for 3 hours, and brush cleaning was also used during the process to remove the dry film resist layer. After removal, the substrate was washed and dried.
[0169] Next, an 8-inch glass support substrate was attached onto the pressure chamber member using a double-sided thermal release sheet manufactured by Nitto Denko Corporation. Next, the silicon wafer was ground to a thickness of about 50 μm, and then SF 6 The film was completely removed by dry etching using a fluorine-based etching method.
[0170] Next, a Tokyo Ohka OMR resist was applied onto the first electrode, and a mask pattern that removes the first electrode except for the area that will become the piezoelectric element corresponding to the piezoelectric actuator unit was transferred by exposure and developed to form a resist mask. Next, the first electrode in the area where the resist mask was not formed was covered with argon, oxygen, and CHF 3 The resist mask was removed by dry etching using a mixed gas of the following: After cleaning, the resist mask was stripped using a stripping solution.
[0171] Next, Tokyo Ohka OMR resist was applied, and a mask pattern for removing the piezoelectric thin film except for the area that will become the piezoelectric element was transferred by exposure and developed to form a resist mask. Next, the piezoelectric thin film in the area where the resist mask was not formed was removed by dry etching using a mixed gas of chlorine and bromine. After washing, the resist mask was peeled off using a stripping solution.
[0172] Next, a 1 μm protective film was formed by applying photosensitive polyimide resin by spin coating and then patterning it. The patterning was performed by transferring a mask pattern that removes the protective film in the through groove and electrode pad areas by exposure and developing it. After patterning, it was baked at 100°C to harden it.
[0173] Next, the second electrode in the through groove, the ink blocking film, and the seed layer were removed using an IR laser to separate each piezoelectric actuator.
[0174] Next, the support substrate was heated to a temperature equal to or higher than the foaming temperature of the thermal release sheet to separate each piezoelectric actuator.
[0175] <<Preparation of piezoelectric actuator 2>> A wafer 2 with piezoelectric actuators was fabricated on an 8-inch silicon wafer with 18 piezoelectric actuators arranged as shown in Figure 29, and piezoelectric actuators 2 were then separated from the wafer 2 with piezoelectric actuators. The size of the piezoelectric actuator 2 is the same as that of the piezoelectric actuator 1, with a long side of 68.2 mm and a short side of 12.8 mm.
[0176] Piezoelectric actuator 2 was produced using the same materials and process as in Example A, except that the piezoelectric actuators were arranged in a lattice pattern on the wafer, there were 18 of them on the wafer, no through grooves were provided, and each piezoelectric actuator was individualized by cutting with a dicer.
[0177] Evaluation An ink flow path member and a nozzle plate were attached to 100 piezoelectric actuators 1 made from 5 wafers and 90 piezoelectric actuators 2 made from 5 wafers, respectively, by adhesive to produce 100 inkjet heads 1 and 90 inkjet heads 2. The diameter of the nozzle hole of the nozzle plate used was 20 μm.
[0178] After filling each inkjet head with ink, a predetermined waveform was applied to eject the ink. The ejection speed S [m / s] of the ink was measured using a drop watcher.
[0179] The ink jet speed S [m / s] of the ink jetted from 200 piezoelectric actuator units in one row that is not on either end of the four rows of piezoelectric actuator units in each inkjet head is calculated using the following formula: d [%] was calculated. S d [%]=[(S max -S min ) / S ave ] x 100 S max is the maximum injection speed S in the row S min is the minimum injection speed S in the row S ave is the average injection speed S in the row
[0180] S d The smaller the value of [%], the smaller the speed variation between nozzles, and the more uniform the piezoelectric characteristics of the piezoelectric actuator and inkjet head.
[0181] Each inkjet head is S d The percentages of particles in each level were calculated for inkjet head 1 and inkjet head 2, and are shown in Table I.
[0182] [Table 1]
[0183] As can be seen from Table I, the inkjet head 1 of the present invention has a d There are many inkjet heads with low [%] values. This shows that many piezoelectric actuators with good uniformity in the piezoelectric characteristics can be obtained from a single wafer. [Explanation of symbols]
[0184] 101 Piezoelectric actuator 102 Through groove 103 Inside the pressure chamber 104 Pressure chamber wall 105 Pressure Chamber 106 Piezoelectric element 107 Piezoelectric Actuator Unit 201 Wafer 202 1st electrode 203 Piezoelectric Thin Film 204 Insulating film 205 2nd electrode 206 Ink blocking film 207 Seed Layer 208 DFR layer inside pressure chamber 209 DFR layer of penetration wall 210 Pressure chamber member 211 Support substrate 212 Heat release sheet 213 Protective film 401 Work 402 Plating tank 403 Cathode Electrode 404 Anode Electrode 405 Shielding plate 406 Rectifier 407 Reserve Tank 408 Heater 409 Pump 410 Filter 411 Flowmeter 412 Plating solution
Claims
1. A piezoelectric actuator wafer having 12 or more piezoelectric actuators on the wafer, the piezoelectric actuator includes at least a piezoelectric element including a first electrode, a piezoelectric thin film, and a second electrode, and a plurality of pressure chambers; A wafer with piezoelectric actuators, characterized in that the piezoelectric actuators are arranged on the wafer such that the distance from each midpoint of the lower side of each of the longitudinal end faces of each of the piezoelectric actuators to the center point of the wafer with piezoelectric actuators is approximately the same.
2. 2. The wafer with piezoelectric actuators according to claim 1, wherein the longitudinal length of each of said piezoelectric actuators is equal to or greater than 1 / 3 of the diameter of the wafer.
3. 3. The wafer with piezoelectric actuators according to claim 1, wherein the longitudinal direction of the piezoelectric actuators is not in one direction.
4. A wafer with a piezoelectric actuator described in any one of claims 1 to 3, characterized in that the corners of the piezoelectric actuator are R-chamfered.
5. The piezoelectric actuator has a pressure chamber member, 5. The wafer with piezoelectric actuators according to claim 1, wherein a cross section of the pressure chamber member when cut along a plane perpendicular to a longitudinal direction of the piezoelectric actuator is inversely tapered.
6. A method for manufacturing a wafer with piezoelectric actuators having 12 or more piezoelectric actuators on the wafer, comprising the steps of: the piezoelectric actuators are arranged on the wafer such that the distances from the midpoints of the lower sides of both end faces in the longitudinal direction of each of the piezoelectric actuators to the center point of the wafer with the piezoelectric actuators are substantially the same for each of the piezoelectric actuators; forming a piezoelectric element, which is composed of a first electrode, a piezoelectric thin film, and a second electrode, on a wafer by a sputtering method; forming a seed layer; depositing a pressure chamber member by Ni electroforming; and A method for manufacturing a wafer with piezoelectric actuators, wherein the step of depositing the pressure chamber members by Ni electroforming is characterized in that the pressure chamber members are not deposited around each piezoelectric actuator when depositing the pressure chamber members.
7. 7. The method for producing a wafer with piezoelectric actuators according to claim 6, wherein when the piezoelectric thin film is formed by sputtering, the temperature and plasma distribution are controlled so as to be uniform concentrically on the wafer.
8. 8. The method for manufacturing a wafer with piezoelectric actuators according to claim 6, wherein the longitudinal direction of the piezoelectric actuators is not in one direction.
9. A method for manufacturing a piezoelectric actuator using the method for manufacturing a wafer with a piezoelectric actuator according to any one of claims 6 to 8, transferring the piezoelectric actuators from the wafer with the piezoelectric actuators onto another support substrate and removing the wafer; forming a plurality of piezoelectric elements in each piezoelectric actuator by patterning the first electrode and the piezoelectric thin film; and removing the seed layer around each of the piezoelectric actuators to separate each of the piezoelectric actuators.
10. 10. The method for manufacturing a piezoelectric actuator according to claim 9, further comprising the step of chamfering corners of the piezoelectric actuator.
11. 11. The method for manufacturing a piezoelectric actuator according to claim 9, wherein a cross section of the pressure chamber member when cut along a plane perpendicular to a longitudinal direction of the piezoelectric actuator is machined to have an inverse tapered shape.
12. A method for manufacturing an inkjet head, comprising using the method for manufacturing a piezoelectric actuator according to any one of claims 9 to 11.
Citation Information
Patent Citations
Liquid droplet ejection head, liquid droplet ejector, manufacturing method for liquid droplet ejection head, and manufacturing method for liquid droplet ejector
JP2008265013A
Ink jet head, manufacturing method of ink jet head, and ink jet recorder
JP2009045871A
Electromechanical conversion member, manufacturing method of electromechanical conversion member, droplet discharge head, and image forming apparatus
JP2016162817A
Etching piezoelectric material
US20110117311A1