Charge transporting polymer, charge transporting material, ink composition, organic layer, organic electronics element, organic electroluminescence element, lighting device, display element, and display device
A charge transporting polymer with triarylamine, arylcarbazole, and fluoroalkyl groups addresses filter passability issues in the coating process, ensuring high-quality organic layers for organic EL devices by reducing fine particle content and improving solubility and solvent resistance.
Patent Information
- Application Number
- JP2020163720
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-29
AI Technical Summary
In the coating process for organic electroluminescent (EL) devices, insoluble fine particles can lead to variations in product characteristics and yield, necessitating fine-pore filtration which poses challenges in filter passability.
Development of a charge transporting polymer with specific structural units, including triarylamine, arylcarbazole, and fluoroalkyl groups, which enhances filter permeability and reduces fine particle content, allowing for improved solubility and solvent resistance.
The polymer enables effective filtration through 0.2 μm membranes, reduces fine particle content, and facilitates the formation of high-quality organic layers with enhanced characteristics in organic electronic devices.
Smart Images

Figure 0007593032000022 
Figure 0007593032000001 
Figure 0007593032000002
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present invention relates to charge transporting polymers, charge transporting materials, ink compositions, organic layers, organic electronic devices, organic electroluminescent devices (also referred to as "organic EL devices"), lighting devices, display devices, and display devices. [Background technology]
[0002] Organic EL elements have been attracting attention as large-area solid-state light sources, for example, as replacements for incandescent lamps, gas-filled lamps, etc. They are also attracting attention as the most promising self-luminous display to replace liquid crystal displays (LCDs) in the field of flat panel displays (FPDs), and commercialization of these devices is progressing.
[0003] Organic EL elements are broadly divided into two types based on the organic materials used: low molecular weight organic EL elements using low molecular weight compounds, and polymeric organic EL elements using polymeric compounds. Manufacturing methods for organic EL elements are broadly divided into two types: dry processes in which films are formed mainly in a vacuum system, and coating processes in which films are formed by plate printing such as letterpress printing and intaglio printing, or plateless printing such as inkjet printing. Because the coating process allows for simple film formation, it is expected to be an essential method for future large-screen organic EL displays. For example, Patent Document 1 discloses an organic electronics material containing a polymer or oligomer having a structure branched in three directions.
[0004] In order to improve the efficiency and / or life of organic EL elements, attempts have been made to form multiple organic layers and separate the functions of each layer. For example, Patent Document 2 discusses a method of using a compound having at least one polymerizable group to form multiple organic layers. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2010 / 140553 [Patent Document 2] JP 2006-279007 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the coating process, insoluble fine particles may exist in the solution containing the charge transporting polymer, etc., and when an organic layer formed by coating a material containing such insoluble matter is used in an organic EL element, etc., this may affect the characteristics such as the variation in product characteristics and the yield in mass production. Therefore, filtration using a filter is performed to remove these fine particles. The finer the pores of the filter, the greater the effect of removing fine particles, so the quality of the filter passing through the fine pores becomes an issue.
[0007] In view of the above, an object of an embodiment of the present invention is to provide a charge transport polymer and a charge transport material that are suitable for coating processes, have good filter passability, and suppress the inclusion of fine particles. Another object of the present invention is to provide an ink composition using the charge transport material. Another object of the present invention is to provide an organic layer that is suitable for improving the properties of an organic electronic element. Another object of the present invention is to provide an organic electronic element, an organic EL element, a display element, a lighting device, and a display device that have excellent properties. [Means for solving the problem]
[0008] Examples of embodiments of the present invention are listed below. The present invention is not limited to the following embodiments.
[0009] (1) A charge transporting polymer containing a divalent structural unit having a triarylamine structure containing an electron-withdrawing group, a trivalent or higher structural unit having an arylcarbazole structure, and a monovalent structural unit having an aryl group substituted with a fluoroalkyl group.
[0010] (2) The charge transporting polymer according to (1), further comprising a monovalent structural unit having a polymerizable substituent.
[0011] (3) The charge transporting polymer according to (2), wherein the polymerizable substituent includes at least one group selected from the group consisting of a group having a carbon-carbon unsaturated bond, a cycloalkyl group, a cycloalkenyl group, a condensed ring group, a cyclic ether group, and a group having a heterocycle.
[0012] (4) The charge transporting polymer according to (2) or (3), wherein the monovalent structural unit having a polymerizable substituent comprises the following structure:
[0013] [ka]
[0014] * represents a bonding site to another structure, and X represents a group containing the above polymerizable substituent.
[0015] (5) A charge transporting material comprising the charge transporting polymer according to any one of (1) to (4).
[0016] (6) An ink composition comprising the charge transporting polymer according to any one of (1) to (4) or the charge transporting material according to (5) and a solvent.
[0017] (7) An organic layer formed using the charge transporting polymer according to any one of (1) to (4), the charge transporting material according to (5), or the ink composition according to (6).
[0018] (8) An organic electronic device comprising at least one organic layer according to (7).
[0019] (9) An organic electroluminescence device comprising at least one organic layer according to (7).
[0020] (10) The organic electroluminescence element according to (9), further comprising a flexible substrate.
[0021] (11) The organic electroluminescence element according to (9), further comprising a resin film substrate.
[0022] (12) A display device comprising the organic electroluminescence device according to any one of (9) to (11).
[0023] (13) A lighting device comprising the organic electroluminescence element according to any one of (9) to (11).
[0024] (14) A display device comprising the organic electroluminescence element according to any one of (9) to (11).
[0025] (15) A display device comprising the display device according to (14) and a liquid crystal element as a display means. Effect of the Invention
[0026] According to an embodiment of the present invention, it is possible to provide a charge transport polymer and a charge transport material that are suitable for a coating process, have good filter passing properties, and suppress the inclusion of fine particles. According to another embodiment of the present invention, it is possible to provide an ink composition using the charge transport material. According to another embodiment of the present invention, it is possible to provide an organic layer that is suitable for improving the properties of an organic electronic device. According to another embodiment of the present invention, it is possible to provide an organic electronic device, an organic EL device, a display device, a lighting device, and a display device having excellent properties. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of an organic EL element according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0029] <Charge transport polymer> The charge transporting polymer will now be described. A charge-transporting polymer has the ability to transport charges. The term "polymer" includes so-called "oligomers" that have a small number of repeating structural units.
[0030] The charge transporting polymer contains at least a divalent structural unit having a triarylamine structure containing an electron-withdrawing group (hereinafter also referred to as "structural unit (1)"), a trivalent or higher structural unit having an arylcarbazole structure (hereinafter also referred to as "structural unit (2)"), and a monovalent structural unit having an aryl group substituted with a fluoroalkyl group (hereinafter also referred to as "structural unit (3)").
[0031] Structural unit (1) The charge transporting polymer contains a structural unit (1). The structural unit (1) is a divalent structural unit having a triarylamine structure containing an electron-withdrawing group and having two bonding sites with other structures. The charge transporting polymer may contain only one type of structural unit (1), or may contain two or more types of structural units (1).
[0032] [ka]
[0033] In the structural unit (1), * denotes a bonding site to other structures, and each Ar independently represents a substituted or unsubstituted aryl group or arylene group. At least one Ar is an aryl group or arylene group having an electron-withdrawing group.
[0034] An aryl group is an atomic group obtained by removing one hydrogen atom from an aromatic hydrocarbon. An arylene group is an atomic group obtained by removing two hydrogen atoms from an aromatic hydrocarbon. Examples of aromatic hydrocarbons include benzene, naphthalene, anthracene, tetracene, fluorene, and phenanthrene. Examples of electron-withdrawing groups include a cyano group, a nitro group, a carboxy group, an ester group, an aldehyde group, a carbonylamino group, an alkylsulfonyl group (e.g., a methylsulfonyl group), an arylsulfonyl group (e.g., a phenylsulfonyl group), a halogen atom, a halogenated alkyl group, and a halogenated sulfanyl group.
[0035] Each Ar is preferably a substituted or unsubstituted phenyl group or phenylene group, a substituted or unsubstituted naphthyl group or naphthylene group, or a substituted or unsubstituted anthracenyl group or anthrylene group, and more preferably a substituted or unsubstituted phenyl group or phenylene group, or a substituted or unsubstituted naphthyl group or naphthylene group. The electron-withdrawing group preferably contains a halogen atom, and more preferably is a fluoro group or a fluoroalkyl group.
[0036] The above structural unit (1) is preferably, for example, the following structural unit (1a).
[0037] [ka]
[0038] In the structural unit (1a), * represents a bonding site with other structures, and R represents a hydrogen atom or a substituent. At least one R has the above-mentioned electron-withdrawing group as a substituent. The substituents in R are each independently -R 1 , -OR 2 , -SR 3 , -OCOR 4 , -COOR 5 , -SiR 6 R 7 R 8 and halogen atoms. 1 ~R8 are each independently a hydrogen atom or at least one selected from the group consisting of linear, cyclic or branched alkyl groups, alkenyl groups, alkynyl groups, and alkoxy groups having 1 to 22 carbon atoms, and aryl groups and heteroaryl groups having 2 to 30 carbon atoms. The heteroaryl group refers to an atomic group obtained by removing one hydrogen atom from an aromatic heterocycle. The aryl group and heteroaryl group may further have a substituent. The substituent is preferably a linear, cyclic or branched alkyl group having 1 to 22 carbon atoms, or a heteroaryl group having 2 to 30 carbon atoms.
[0039] Specific examples of aromatic hydrocarbons contained in the aryl group include benzene, naphthalene, anthracene, tetracene, fluorene, and phenanthrene, etc. Specific examples of aromatic heterocycles include pyridine, pyrazine, quinoline, isoquinoline, acridine, phenanthroline, furan, pyrrole, thiophene, carbazole, oxazole, oxadiazole, thiadiazole, triazole, benzoxazole, benzoxadiazole, benzothiadiazole, benzotriazole, and benzothiophene, etc.
[0040] In the structural unit (1a), a1 represents an integer of 0 to 5, and a2 and a3 each independently represent an integer of 0 to 4. However, all of a1 to a3 are not 0. From the viewpoint of ease of bonding with other structures, a2 and a3 are preferably 0.
[0041] In addition, in the structural unit (1a), a1 is preferably 1 or more, and R preferably contains an electron-withdrawing group, for example, a fluoro group or a fluoroalkyl group, which is an electron-withdrawing group.Furthermore, it is preferably at least one structural unit selected from the group consisting of the following structural units (1b) to (1e) containing a fluoro group or a perfluoromethyl group.
[0042] [ka]
[0043] Structural unit (2) The charge transporting polymer contains a structural unit (2). The structural unit (2) is a trivalent or higher structural unit (2) that has an arylcarbazole structure and has three or more bonding sites with other structures. By containing the structural unit (2), the charge transporting polymer becomes a branched polymer, and becomes a polymer having three or more terminals in one molecule. The branched polymer can easily have a large molecular weight and tends to exhibit good solubility. The charge transporting polymer may contain only one type of the structural unit, or two or more types.
[0044] The arylcarbazole structure is a carbazole structure substituted with one or more aryl groups or arylene groups. As the aryl group or arylene group, for example, the aryl group or arylene group exemplified in the structural unit (1) can be used. In the carbazole structure, it is preferable that an aryl group or arylene group is substituted on the nitrogen atom at the 9th position. The number of aryl groups or arylene groups substituted on the carbazole structure is preferably 1 to 7, and more preferably 1.
[0045] The structural unit (2) is preferably, for example, the following structural unit (2a).
[0046] [ka]
[0047] In the structural unit (2a), * denotes a bonding site to other structures, Ar denotes a substituted or unsubstituted arylene group, and R denotes a hydrogen atom or a substituent, each of which independently represents the above-mentioned -R 1 , -OR 2 , -SR 3 , -OCOR 4 , -COOR 5 , -SiR 6 R 7 R 8and a halogen atom. The arylene group has 2 to 30 carbon atoms, and for example, the arylene groups exemplified in the structural unit (1) can be used.
[0048] In the structural unit (2a), b5 and b6 each independently represent an integer of 0 to 3. From the viewpoint of ease of bonding with other structures, b5 and b6 are preferably 0.
[0049] The structural unit (2a) is preferably, for example, the following structural unit (2b).
[0050] [ka]
[0051] In the structural unit (2b), * represents a bonding site to other structures, and R represents a hydrogen atom or a substituent, and each of the substituents independently represents the above-mentioned -R 1 , -OR 2 , -SR 3 , -OCOR 4 , -COOR 5 , -SiR 6 R 7 R 8 and halogen atoms.
[0052] In the structural unit (2b), b4 represents an integer of 0 to 4, and b5 and b6 each independently represent an integer of 0 to 3. From the viewpoint of ease of bonding with other structures, b4 to b6 are preferably 0.
[0053] The structural unit (2b) is preferably, for example, the following structural unit (2c).
[0054] [ka]
[0055] Structural unit (3) The charge transporting polymer contains a structural unit (3). The structural unit (3) is a monovalent structural unit having an aryl group substituted with a fluoroalkyl group and having one bonding site with another structure. The structural unit (3) is contained at the end of the polymer chain of the charge transporting polymer. The inclusion of the structural unit (3) can improve the solubility of the charge transporting polymer, which is believed to reduce the viscosity of the charge transporting polymer solution obtained by dissolving the charge transporting polymer in an organic solvent, improving filter passability. The charge transporting polymer may contain only one type of structural unit (3), or two or more types.
[0056] The number of carbon atoms in the fluoroalkyl group is preferably 1 to 4, and more preferably 1 or 2. The fluoroalkyl group is preferably a perfluoroalkyl group.
[0057] The aryl group has 2 to 30 carbon atoms, and for example, the aryl groups exemplified for the structural unit (1) can be used.
[0058] The structural unit (3) is preferably, for example, the following structural unit (3a).
[0059] [ka]
[0060] In the structural unit (3a), * represents a bonding site with other structures, and each R independently represents a fluoro group or a fluoroalkyl group. The number of carbon atoms in the fluoroalkyl group is preferably 1 to 4, and more preferably 1 or 2. The fluoroalkyl group is preferably a perfluoroalkyl group.
[0061] The two R's may be the same or different, and are preferably the same. Each R is more preferably a fluoroalkyl group, and more preferably a perfluoroalkyl group having 1 to 4 carbon atoms.
[0062] The structural unit (3a) is preferably, for example, the following structural unit (3b).
[0063] [ka]
[0064] In the structural unit (3b), m and n each independently represent an integer of 1 to 4. m and n may be the same or different, and are preferably the same.
[0065] The structural unit (3b) is particularly preferably the following structural unit (3c).
[0066] [ka]
[0067] The charge transporting polymer of this embodiment may contain at least the structural units (1) to (3). By adopting such a constitution, it is possible to reduce the viscosity of the charge transporting polymer solution obtained by dissolving the charge transporting polymer in an organic solvent such as toluene, which is used when forming an organic layer, and as a result, for example, the charge transporting polymer solution can pass through a membrane filter having a pore size of 0.2 μm. This makes it possible to obtain a charge transporting polymer solution that does not contain particles having a pore size larger than 0.2 μm, and to obtain an organic electronics element having good characteristics. In addition, the charge transporting polymer of this embodiment makes it possible to obtain an organic layer having excellent solvent resistance, and it is possible to easily introduce multiple organic layers into an organic electronics element.
[0068] [any structural unit] The charge transporting polymer may further contain any structural unit other than the above structural units (1) to (3) (hereinafter referred to as "any structural unit").
[0069] (Monovalent structural unit having a polymerizable substituent) The charge transport polymer may further include a monovalent structural unit having a polymerizable substituent (hereinafter also referred to as "structural unit (4)") as a monovalent structural unit other than the structural unit (3). The polymerizable substituent has the ability to be cured by a polymerization reaction and to change the solubility in a solvent. The "polymerizable substituent" refers to a functional group that can form bonds with each other within a molecule and / or between molecules by applying heat and / or light.
[0070] Examples of the polymerizable substituent include groups having a carbon-carbon unsaturated bond (e.g., vinyl group, allyl group, butenyl group, ethynyl group, acryloyl group, acryloyloxy group, acryloylamino group, methacryloyl group, methacryloyloxy group, methacryloylamino group, vinyloxy group, vinylamino group, etc.), groups having a small ring (e.g., cycloalkyl groups such as cyclopropyl group, cyclobutyl group, cyclopentyl group, etc.; cycloalkenyl groups such as cyclopropenyl group, cyclobutenyl group, etc.; condensed ring groups such as benzocyclobutenyl group, etc.; cyclic ether groups such as epoxy group (oxiranyl group), oxetanyl group, etc.; diketene group; episulfide group; lactone group; lactam group, etc.), and groups having a heterocycle having a heteroatom (e.g., furan-yl group, pyrrol-yl group, thiophen-yl group, silol-yl group). As the polymerizable substituent, in particular, ethynyl group, vinyl group, acryloyl group, methacryloyl group, cyclobutenyl group, epoxy group, and oxetanyl group are preferred, and from the viewpoint of transparency and characteristics of organic electronics element, vinyl group, cyclobutenyl group, epoxy group, or oxetanyl group are more preferred, and from the viewpoint of reactivity, epoxy group or oxetanyl group are even more preferred. In addition, the above-mentioned group having a carbon-carbon unsaturated bond, group having a small ring, and group having a heterocycle having a hetero atom may have a substituent, and for example, it is preferred to have an alkyl group.
[0071] From the viewpoint of increasing the degree of freedom of the polymerizable substituent and facilitating the polymerization reaction, the main skeleton of the charge transporting polymer and the polymerizable substituent may be linked by an alkylene chain. In addition, for example, when forming an organic layer on an electrode described later, from the viewpoint of improving affinity with a hydrophilic electrode such as ITO (indium oxide-tin oxide), the main skeleton and the polymerizable substituent may be linked by a hydrophilic chain such as an ethylene glycol chain or a diethylene glycol chain. Furthermore, from the viewpoint of facilitating the preparation of a monomer used for introducing a polymerizable substituent, the charge transporting polymer may have an ether bond or an ester bond at the terminal of the alkylene chain and / or the hydrophilic chain, that is, at the linking portion between these chains and the polymerizable substituent, and / or at the linking portion between these chains and the skeleton of the charge transporting polymer.
[0072] By introducing a polymerizable substituent into the terminal portion of the charge transporting polymer, it is possible to achieve both the curability and the charge transportability of the charge transporting polymer.
[0073] Specific examples of the structural unit (4) include the following structural unit (4a), but the group containing a polymerizable substituent is not limited thereto.
[0074] *-Ar-X (4a)
[0075] In the structural unit (4a), * represents a bonding site with other structures, Ar represents a substituted or unsubstituted arylene group, and X represents a polymerizable substituent. Specific examples of aromatic hydrocarbons contained in the arylene group include benzene, naphthalene, anthracene, tetracene, fluorene, and phenanthrene. The arylene group is preferably a phenylene group or a naphthylene group, and more preferably a phenylene group. Examples of the polymerizable substituent include the above-mentioned group having a carbon-carbon unsaturated bond, a group having a small ring, and a group having a heterocycle.
[0076] From the viewpoint of improving the solvent resistance of the organic layer, the structural unit (4a) is preferably, for example, a structural unit (4b) as shown in the following structural formula.
[0077] [ka]
[0078] In the structural unit (4b), * represents a bonding site with other structures, and X represents a group containing a polymerizable substituent. Examples of the polymerizable substituent include the above-mentioned group having a carbon-carbon unsaturated bond, a group having a small ring, and a group having a heterocycle. The group containing a polymerizable substituent refers to the polymerizable substituent itself, or a group combining a polymerizable substituent with an alkylene chain or the like. As the group containing a polymerizable substituent, for example, the groups exemplified in WO 2010 / 140553 can be suitably used.
[0079] A specific example of the group containing a polymerizable substituent in the structural unit (4b) is the following structure (4b-1), but the polymerizable substituent is not limited thereto.
[0080] -(CH2) n -CH=CH2(4b-1)
[0081] In the above structure (4b-1), n is an integer of 0 to 20. From the viewpoint of improving life characteristics, n is preferably 0 to 8, more preferably 0 to 6, even more preferably 0 to 3, and particularly preferably 0 or 1. From the viewpoint of improving solubility, n is preferably 4 to 20, more preferably 4 to 16, even more preferably 4 to 12, and particularly preferably 4 to 8.
[0082] The structure (4b-1) has excellent reactivity, and therefore the curing reaction of the charge transporting polymer can be efficiently promoted. In addition, since the charge transporting polymer contains a polymerizable substituent that contributes to the curing reaction, an ink composition having excellent storage stability, as described below, can be obtained. In the structure (4b-1), it is preferable that the value of n is small in order to obtain an organic electronic element that exhibits better life characteristics. On the other hand, it is preferable that the value of n is large in order to obtain excellent solubility.
[0083] The structural unit (4b) preferably has a structure as shown below, for example.
[0084] [ka]
[0085] The charge transporting polymer may contain only one type or two or more types of monovalent structural units having a polymerizable substituent.
[0086] (Any other structural unit) Other optional structural units include, for example, a substituted or unsubstituted aromatic amine structure, a substituted or unsubstituted carbazole structure, a substituted or unsubstituted thiophene structure, a substituted or unsubstituted fluorene structure, a substituted or unsubstituted benzene structure, a substituted or unsubstituted biphenyl structure, a substituted or unsubstituted terphenyl structure, a substituted or unsubstituted naphthalene structure, a substituted or unsubstituted anthracene structure, a substituted or unsubstituted tetracene structure, a substituted or unsubstituted phenanthrene structure, a substituted or unsubstituted dihydrophenanthrene structure, a substituted or unsubstituted pyridine structure, a substituted or unsubstituted pyrazine structure, a substituted or unsubstituted quinoline structure, a substituted or unsubstituted isoquinoline structure, a substituted or unsubstituted quinoline structure, a substituted or unsubstituted phenyl ... The aryl group is selected from a substituted or unsubstituted xaline structure, a substituted or unsubstituted acridine structure, a substituted or unsubstituted diazaphenanthrene structure, a substituted or unsubstituted furan structure, a substituted or unsubstituted pyrrole structure, a substituted or unsubstituted oxazole structure, a substituted or unsubstituted oxadiazole structure, a substituted or unsubstituted thiazole structure, a substituted or unsubstituted thiadiazole structure, a substituted or unsubstituted triazole structure, a substituted or unsubstituted benzothiophene structure, a substituted or unsubstituted benzoxazole structure, a substituted or unsubstituted benzoxadiazole structure, a substituted or unsubstituted benzothiazole structure, a substituted or unsubstituted benzothiadiazole structure, a substituted or unsubstituted benzotriazole structure, and structures containing one or more of these.
[0087] The other optional structural units may be monovalent or higher, preferably monovalent to hexavalent, and more preferably monovalent to tetravalent.
[0088] The explanation of the substituents in the structural unit (1a) above can be applied to the substituents contained in any other structural unit.
[0089] [Content of each structural unit] The charge transporting polymer may contain a divalent structural unit other than the structural unit (1). From the viewpoint of adjusting the energy level, the content of the structural unit (1) is preferably 50 mol% or more, more preferably 75 mol% or more, and even more preferably 90 mol% or more, based on the total amount of the divalent structural units. The upper limit of the content of the structural unit (1) is 100 mol%.
[0090] The content of the divalent structural unit contained in the charge transporting polymer is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more based on the total structural units from the viewpoint of obtaining sufficient charge transportability. In addition, the content of the divalent structural unit is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 85 mol% or less, taking into consideration the monovalent structural unit and the trivalent or higher structural unit.
[0091] The charge transporting polymer may contain a trivalent or higher structural unit other than the structural unit (2). From the viewpoint of obtaining good charge transporting properties, the content of the structural unit (2) is preferably 50 mol% or more, more preferably 75 mol% or more, and even more preferably 90 mol% or more, based on the total amount of the trivalent or higher structural units. The upper limit of the content of the structural unit (2) is 100 mol%.
[0092] The content of the trivalent or higher structural unit contained in the charge transporting polymer is preferably 1 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more based on the total structural units from the viewpoint of obtaining an organic layer with excellent solvent resistance. Also, the content of the trivalent or higher structural unit is preferably 50 mol% or less, more preferably 40 mol% or less, even more preferably 30 mol% or less, and particularly preferably 20 mol% or less from the viewpoint of suppressing an increase in viscosity and favorably synthesizing the charge transporting polymer, or from the viewpoint of obtaining sufficient charge transportability.
[0093] The charge transporting polymer may contain a monovalent structural unit other than the structural unit (3), for example, the structural unit (4), or may contain a monovalent structural unit other than the structural units (3) and (4). From the viewpoint of obtaining good storage stability of the liquid composition, the content of the structural unit (3) is preferably 85 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more, based on the total amount of the monovalent structural units. The upper limit of the content of the structural unit (3) is 100 mol%.
[0094] The content of the monovalent structural unit contained in the charge transporting polymer is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more based on the total structural units from the viewpoint of curability and solubility of the charge transporting polymer and from the viewpoint of improving the properties of the organic electronics element. Also, the content of the monovalent structural unit is preferably 60 mol% or less, more preferably 55 mol% or less, and even more preferably 50 mol% or less from the viewpoint of obtaining sufficient charge transportability.
[0095] The charge transporting polymer may contain an optional structural unit. From the viewpoint of obtaining sufficient effects of the structural units (1) to (3), the content of the optional structural unit is preferably 50 mol % or less, more preferably 30 mol % or less, even more preferably 20 mol % or less, and particularly preferably 10 mol % or less or 5 mol % or less, based on the total structural units. The lower limit of the content of the optional structural unit is 0 mol %. That is, the charge transporting polymer may not contain any optional structural unit.
[0096] The content of the structural unit (4) is preferably 1 to 99 mol % based on the total amount of monovalent structural units forming the terminal portion of the polymer chain. From the viewpoint of improving the solvent resistance of the organic layer, the content of the structural unit is preferably 2 mol % or more, more preferably 3 mol % or more, even more preferably 5 mol % or more, and particularly preferably 10 mol % or more. From the viewpoint of maintaining charge transportability, the content of the structural unit is preferably 95 mol % or less, more preferably 90 mol % or less, and even more preferably 80 mol % or less. To obtain high charge transportability, the content may be 75 mol % or less, or may be 50 mol % or less.
[0097] The proportion of the polymerizable substituent contained in the structural unit (4) is preferably 0.1 mol% or more, more preferably 1 mol% or more, and even more preferably 3 mol% or more, based on all structural units, from the viewpoint of efficiently curing the charge transporting polymer. Also, the proportion of the polymerizable substituent is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 50 mol% or less, based on all structural units, from the viewpoint of obtaining good charge transporting properties. Here, the "proportion of the polymerizable substituent" refers to the proportion of structural units having a polymerizable substituent.
[0098] From the viewpoint of contributing to the change in solubility, it is preferable that the polymerizable substituent is contained in a large amount in the charge transport polymer. On the other hand, from the viewpoint of not hindering the charge transport property, it is preferable that the amount of the polymerizable substituent contained in the charge transport polymer is small. The content of the polymerizable substituent can be appropriately set in consideration of these.
[0099] For example, the number of polymerizable substituents per molecule of the charge transporting polymer is preferably 2 or more, more preferably 3 or more, from the viewpoint of obtaining a sufficient change in solubility, and is preferably 1,000 or less, more preferably 500 or less, from the viewpoint of maintaining the charge transporting property.
[0100] The number of polymerizable substituents per molecule of the charge transporting polymer can be determined as an average value using the amount of polymerizable substituents (e.g., the amount of monomer having a polymerizable substituent) used to synthesize the charge transporting polymer, the amount of monomer corresponding to each structural unit, the weight average molecular weight of the charge transporting polymer, etc. 1 It can be calculated as an average value using the ratio of the integral value of the signal derived from the polymerizable substituent in the H NMR (nuclear magnetic resonance) spectrum to the integral value of the entire spectrum, the weight average molecular weight of the charge transport polymer, etc. When the amount of the charge is clear, it is preferable to use the value calculated using the amount of the charge, because it is simple.
[0101] The ratio (molar ratio) of the contents of the divalent structural units, trivalent or higher valent structural units, and monovalent structural units contained in the charge transporting polymer is preferably divalent structural units:trivalent or higher valent structural units:monovalent structural units=100:5 to 70:50 to 150, more preferably 100:10 to 60:60 to 135, and even more preferably 100:15 to 50:80 to 120, in consideration of the balance of the effects of each structural unit.
[0102] [Structural example of charge transport polymer] The charge transporting polymer contains at least a divalent structural unit containing the structural unit (1), a trivalent or higher structural unit containing the structural unit (2), and a monovalent structural unit containing the structural unit (3). The trivalent or higher structural units form the branched portions of the charge transporting polymer, and the monovalent structural units form the terminal portions of the charge transporting polymer.
[0103] Examples of partial structures contained in the charge transporting polymer include the following. The charge transporting polymer is not limited to polymers having the following partial structures. In the partial structures, "L" represents a divalent structural unit L, "T" represents a monovalent structural unit T, and "B" represents a trivalent or higher structural unit B. In the partial structures contained in the charge transporting polymer shown below, "*" in the formula represents a bonding site with other structural units. In the partial structures below, multiple Ls may be the same structural unit or different structural units. The same applies to T and B.
[0104] [ka]
[0105] [Number average molecular weight] The number average molecular weight of the charge transporting polymer can be appropriately adjusted in consideration of solubility in a solvent, film-forming property, etc. From the viewpoint of excellent charge transportability, the number average molecular weight is preferably 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more. In addition, from the viewpoint of maintaining good solubility in a solvent and facilitating preparation of an ink composition, the number average molecular weight is preferably 1,000,000 or less, more preferably 100,000 or less, and even more preferably 50,000 or less.
[0106] [Weight average molecular weight] The weight average molecular weight of the charge transporting polymer can be appropriately adjusted in consideration of solubility in a solvent, film-forming property, etc. From the viewpoint of excellent charge transportability, the weight average molecular weight is preferably 1,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. In addition, from the viewpoint of maintaining good solubility in a solvent and facilitating preparation of an ink composition, the weight average molecular weight is preferably 1,000,000 or less, more preferably 700,000 or less, and even more preferably 400,000 or less.
[0107] The number average molecular weight and the weight average molecular weight can be measured by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene.
[0108] [Method of manufacturing charge transport polymer] Charge transporting polymers can be produced by various synthesis methods, and are not particularly limited. For example, known coupling reactions such as Suzuki coupling, Negishi coupling, Sonogashira coupling, Stille coupling, and Buchwald-Hartwig coupling can be used. Suzuki coupling is a cross-coupling reaction between an aromatic boronic acid derivative and an aromatic halide using a Pd catalyst. According to Suzuki coupling, a charge transporting polymer can be easily produced by bonding desired aromatic rings together.
[0109] In the coupling reaction, for example, Pd(0) compound, Pd(II) compound, Ni compound, etc. are used as catalyst. In addition, a catalyst species generated by mixing a precursor such as tris(dibenzylideneacetone)dipalladium(0) or palladium(II) acetate with a phosphine ligand can also be used. For the synthesis method of the charge transporting polymer, for example, the description in International Publication No. 2010 / 140553 can be used.
[0110] <Charge transport material> The charge transporting material according to the embodiment of the present invention contains one or more of the charge transporting polymers described above. The charge transporting material may further contain an optional component.
[0111] [Optional components] Additives such as polymerization initiators, antioxidants, anti-yellowing agents, ultraviolet absorbers, visible light absorbers, colorants, plasticizers, stabilizers, and fillers may be added within a range that does not adversely affect the characteristics of the organic electronics element. In addition, an ionic compound may be mixed with the charge transport material for the purpose of improving the luminous efficiency and life of the organic EL element. By mixing and using an ionic compound, the electrical conductivity of the organic EL element can be improved, and the stability and life of the organic EL element can be increased.
[0112] (ionic compounds) Here, in the present specification and the like, the term "ionic compound" refers to a compound consisting of a cation and an anion. From the viewpoint of electrical conductivity and stability, it is preferable that the anion contains an electron-withdrawing organic substituent, and examples thereof include halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms, alkylsulfonyl groups substituted with alkyls such as cyano groups, thiocyano groups, nitro groups, and mesyl groups, arylsulfonyl groups substituted with aryls such as tosyl groups and mesityl groups, acyl groups having a carbon number of usually 1 to 12, preferably 6 or less, such as formyl groups, acetyl groups, and benzoyl groups, alkoxycarbonyl groups having a carbon number of usually 2 to 10, preferably 7 or less, such as methoxycarbonyl groups and ethoxycarbonyl groups, and alkoxycarbonyl groups having a carbon number of usually 2 to 10, preferably 7 or less, such as phenoxycarbonyl groups and pyridyloxycarbonyl groups. Examples of such groups include an aryloxycarbonyl group having an aromatic hydrocarbon group or an aromatic heterocyclic group which usually has 3 or more, preferably 4 or more and 25 or less, and preferably 15 or less; an acyloxy group having a carbon number of usually 2 to 20, such as acetoxy; a haloalkyl, haloalkenyl, haloalkynyl group, a pentafluorophenyl group, and the like, which are linear, branched, or cyclic alkyl, alkenyl, or alkynyl groups each having a carbon number of usually 1 to 10, preferably 6 or less, substituted with a halogen atom such as a fluorine atom or a chlorine atom.
[0113] The cation in the ionic compound is not particularly limited, but is preferably a monovalent cation from the viewpoint of reactivity and handling. The cation in the ionic compound is more preferably iodonium, sulfonium, phosphonium, carbenium (trityl), anilinium, bismuthonium, ammonium, selenium, pyridinium, imidazolium, oxonium, quinolinium, pyrrolidinium, aminium, immonium, tropylium, morpholinium, piperidinium, quinolium, isoquinolium, thiazonium, acridium, etc.
[0114] The cation may be contained in the charge transporting polymer.
[0115] The ionic compound is preferably an onium salt from the viewpoint of improving charge transportability. The onium salt refers to a compound consisting of a cation such as a sulfonium ion, an iodonium ion, a selenium ion, an ammonium ion, a phosphonium ion, an oxonium ion, or a bismuthonium ion and a counter anion. Examples of the anion include F - , Cl - , Br - , I - Halogen ions such as OH - ;ClO4 - ;FSO3 - , ClSO3 - , CH3SO3 - , C6H5SO3 - , CF3SO3 - Sulfonic acid ions such as HSO4 - , SO4 2- Sulfate ions such as HCO3 - , CO3 2- Carbonate ions such as H2PO4 - , HPO4 2- , PO4 3- Phosphate ions such as PF6 - , PF5OH - Fluorophosphate ions such as BF4 - , B(C6F5)4 - , B(C6H4CF3)4 - Boric acid ions such as AlCl4 - ;BiF6 - ;SbF6 - , SbF5OH - Fluoroantimonate ions such as AsF6 - , AsF5OH - and fluoroarsenate ions such as those mentioned above.
[0116] The ionic compounds may be used alone or in combination of two or more.
[0117] (Polymerization initiator) The ionic compound can be used as a polymerization initiator to promote the curing of the charge transport polymer. The trigger for initiating polymerization is not particularly limited as long as it is capable of polymerizing a polymerizable substituent by application of heat, light, microwaves, radiation, electron beams, etc., but is preferably one that initiates polymerization by light irradiation and / or heating, and most preferably one that initiates polymerization by heating.
[0118] The condition for using the polymerization initiator is 0.1 to 50% by mass, more preferably 0.1 to 25% by mass, and even more preferably 0.1 to 20% by mass, based on the charge transporting material. If the ratio of the polymerization initiator mixed is less than this, the polymerization does not proceed efficiently and the solubility cannot be changed sufficiently. If the ratio is more than this, a large amount of polymerization initiator and / or decomposition products remain, reducing the effect of washing. In addition, a sensitizer for improving photosensitivity and / or heat sensitivity may be included.
[0119] <Ink composition> The ink composition of the present embodiment is characterized by containing the above-mentioned charge transporting polymer or charge transporting material and a solvent, and may contain other additives such as a polymerization inhibitor, a stabilizer, a thickener, a gelling agent, a flame retardant, an antioxidant, a reduction inhibitor, an oxidizing agent, a reducing agent, a surface modifier, an emulsifier, an antifoaming agent, a dispersing agent, a surfactant, etc. Examples of the solvent include water; alcohols such as methanol, ethanol, and isopropyl alcohol; alkanes such as pentane, hexane, and octane; cyclic alkanes such as cyclohexane; aromatic solvents such as benzene, toluene, xylene, mesitylene, tetralin, and diphenylmethane; aliphatic ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol-1-monomethyl ether acetate; 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, anisole, phenetole, 2-methoxytoluene, 3-methoxytoluene, 4-methoxytoluene, 2,3-dimethyltoluene, dimethyl ether ... Examples of the solvent include aromatic ethers such as ethyl anisole and 2,4-dimethyl anisole; aliphatic esters such as ethyl acetate, n-butyl acetate, ethyl lactate and n-butyl lactate; aromatic esters such as phenyl acetate, phenyl propionate, methyl benzoate, ethyl benzoate, propyl benzoate and n-butyl benzoate; amide solvents such as N,N-dimethylformamide and N,N-dimethylacetamide; and other solvents such as dimethyl sulfoxide, tetrahydrofuran, acetone, chloroform and methylene chloride. However, aromatic solvents, aliphatic esters, aromatic esters, aliphatic ethers and aromatic ethers are preferably used.
[0120] In the ink composition, the content of the charge transporting polymer relative to the solvent is preferably 0.1 to 50% by mass from the viewpoint of application to various coating processes. From the viewpoint of reducing the remaining solvent during film formation, the content of the charge transporting polymer is more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. Moreover, from the viewpoint of uniformly dissolving the charge transporting material, the content is more preferably 40% by mass or less, and even more preferably 30% by mass or less.
[0121] <Organic layer> The organic layer of the present embodiment is a layer formed using a charge transporting polymer, a charge transporting material, or an ink composition. It is preferable to form the organic layer by a coating method using a charge transporting polymer, a charge transporting material, or an ink composition. Examples of the coating method include known methods such as spin coating; casting; immersion; plate printing methods such as letterpress printing, intaglio printing, offset printing, lithographic printing, letterpress reverse offset printing, screen printing, and gravure printing; and plateless printing methods such as inkjet printing. When forming an organic layer by a coating method, the organic layer (coated layer) obtained after coating may be dried using a hot plate or an oven to remove the solvent.
[0122] When the charge transporting polymer contains a polymerizable substituent, the polymerization reaction can be promoted by light irradiation, heat treatment, etc., and the solubility of the organic layer can be changed. In the charge transporting material, the ionic compound can function as a polymerization initiator. By stacking organic layers with changed solubility, it becomes possible to easily achieve multi-layering of organic electronics elements. For the method of forming the organic layer, for example, the description in International Publication No. 2010 / 140553 can be cited.
[0123] For example, after forming a thin film from an ink composition containing the above-mentioned charge transporting polymer, polymerization initiator, and solvent, the organic layer can be formed by heating in vacuum, air, or an inert gas atmosphere such as nitrogen or argon. The heating temperature and time are not particularly limited as long as the polymerization reaction can be sufficiently promoted, but the temperature is preferably 300° C. or less, more preferably 200° C. or less, and even more preferably 150° C. or less, since various substrates can be applied. The time is preferably 8 hours or less, more preferably 2 hours or less, and even more preferably 1 hour or less, from the viewpoint of increasing productivity.
[0124] The thickness of the organic layer after drying or curing is preferably 0.1 nm or more, more preferably 1 nm or more, and even more preferably 3 nm or more, from the viewpoint of improving the efficiency of charge transport, and is preferably 300 nm or less, more preferably 200 nm or less, and even more preferably 100 nm or less, from the viewpoint of reducing the electrical resistance.
[0125] The organic layer of this embodiment can be used in organic electronics elements and organic EL elements described below, and can form organic electronics elements and organic EL elements that have a lower driving voltage and a longer light emission life than conventional elements.
[0126] <Organic electronics elements> The organic electronics element of the present embodiment includes at least one of the organic layers. Examples of the organic electronics element include an organic EL element such as an organic light-emitting diode (OLED), an organic photoelectric conversion element, and an organic transistor. The organic electronics element preferably has a structure in which an organic layer is disposed between at least a pair of electrodes. The organic electronics element of the present embodiment is not particularly limited as long as it includes a light-emitting layer, an organic layer, an anode, a cathode, and a substrate. The organic layer can be used as a hole injection layer, an electron injection layer, a hole transport layer, or an electron transport layer.
[0127] <Organic EL element> The organic EL device of the present embodiment includes at least one of the organic layers. The organic EL device of the present embodiment is not particularly limited as long as it includes a light-emitting layer, an organic layer, an anode, a cathode, and a substrate. The organic layer can be used as a hole injection layer, an electron injection layer, a hole transport layer, or an electron transport layer. It is preferable to apply the organic layer of the present embodiment to the hole injection layer or the hole transport layer.
[0128] Fig. 1 is a cross-sectional schematic diagram showing one embodiment of an organic EL element. The organic EL element shown in Fig. 1 has a multi-layer structure in which a substrate 8, an anode 2, a hole injection layer 3, a hole transport layer 6, a light-emitting layer 1, an electron transport layer 7, an electron injection layer 5, and a cathode 4 are laminated in this order. Each layer will be described in detail below.
[0129] (Light Emitting Layer) The material used for the light-emitting layer may be a low molecular weight compound or a polymer, and dendrimers and the like can also be used. Examples of low molecular weight compounds that utilize fluorescent emission include perylene, coumarin, rubrene, quinacridone, dyes for dye lasers (e.g., rhodamine, DCM1, etc.), aluminum complexes (e.g., Tris(8-hydroxyquinolinato)aluminum(III)(Alq3)), stilbene, and derivatives thereof. Examples of polymers that utilize fluorescent emission include polyfluorene, polyphenylene, polyphenylenevinylene (PPV), polyvinylcarbazole (PVK), fluorene-benzothiadiazole copolymers, fluorene-triphenylamine copolymers, and derivatives and mixtures thereof.
[0130] On the other hand, in recent years, in order to improve the efficiency of organic EL elements, phosphorescent organic EL elements have been actively developed. In phosphorescent organic EL elements, it is possible to utilize not only singlet state energy but also triplet state energy, and the internal quantum yield can be increased to 100% in principle. In phosphorescent organic EL elements, phosphorescence is extracted by doping a metal complex phosphorescent material containing heavy metals such as platinum and iridium as a phosphorescent dopant into a host material (see MA Baldo et al., Nature, Vol. 395, p. 151 (1998), MA Baldo et al., Apllied Physics Letters, Vol. 75, p. 4 (1999), MA Baldo et al., Nature, Vol. 403, p. 750 (2000)).
[0131] In the organic EL device of this embodiment, it is also preferable to use a phosphorescent material in the light-emitting layer from the viewpoint of high efficiency. As the phosphorescent material, a metal complex containing a central metal such as Ir or Pt can be suitably used. Specifically, as the Ir complex, for example, FIr(pic) [iridium(III)bis[(4,6-difluorophenyl)-pyridinate-N,C 2 ]picolinate], Ir(ppy)3 [fatty tris(2-phenylpyridine)iridium] which emits green light (see MA Baldo et al., Nature, Vol. 403, p. 750 (2000) above), or (btp)2Ir(acac){bis[2-(2'-benzo[4,5-α]thienyl)pyridinato-N,C]pyridinate ... 3 ]iridium(acetylacetonate)}, Ir(piq)3 [tris(1-phenylisoquinoline)iridium] (see Adachi et al., Appl. Phys. Lett., 78, no. 11, 2001, 1622, supra).
[0132] An example of a Pt complex is 2,3,7,8,12,13,17,18-octaethyl-21H,23H-phorphine platinum (PtOEP), which emits red light. The phosphorescent materials may be small molecule or dendritic species, such as iridium core dendrimers, and derivatives thereof may also be suitably used.
[0133] When the light-emitting layer contains a phosphorescent material, it is preferable that the light-emitting layer contains a host material in addition to the phosphorescent material. The host material may be a low molecular weight compound or a high molecular weight compound, and a dendrimer or the like may also be used.
[0134] Examples of low molecular weight compounds that can be used include CBP (4,4'-Bis(Carbazol-9-yl)-biphenyl), mCP (1,3-bis(9-carbazolyl)benzene), and CDBP (4,4'-Bis(Carbazol-9-yl)-2,2'-dimethylbiphenyl). Examples of high molecular weight compounds that can be used include polyvinylcarbazole, polyphenylene, and polyfluorene, and derivatives of these compounds can also be used.
[0135] The light-emitting layer may be formed by a deposition method or a coating method. When the light-emitting layer is formed by a coating method, it is more preferable because the organic EL element can be manufactured at low cost. To form the light-emitting layer by a coating method, a solution containing a phosphorescent material and, if necessary, a host material is coated on a desired substrate by a known method such as a printing method such as an inkjet method, a casting method, a dipping method, letterpress printing, intaglio printing, offset printing, lithographic printing, letterpress reverse offset printing, screen printing, gravure printing, or a spin coating method.
[0136] (cathode) The cathode material is preferably a metal or a metal alloy such as Li, Ca, Mg, Al, In, Cs, Ba, Mg-Ag, LiF, or CsF.
[0137] (anode) The anode can also be made of a metal (e.g., Au) or other material with metallic conductivity, such as an oxide (e.g., ITO), or a conductive polymer (e.g., a polythiophene-polystyrene sulfonate mixture (PEDOT:PSS)).
[0138] (Hole transport layer, hole injection layer) It is preferable to use the organic layer described above as at least one of a hole transport layer and a hole injection layer. As described above, by using an organic layer containing an organic electronic material, these layers can be easily formed. In addition, for example, when an organic EL element has the organic layer described above as a hole transport layer and further has a hole injection layer, a known material may be used for the hole injection layer. In addition, when an organic EL element has the organic layer described above as a hole injection layer and further has a hole transport layer, a known material may be used for the hole transport layer. In addition, an organic EL element may have the organic layer described above as a hole transport layer and a hole injection layer.
[0139] When a material containing a triphenylamine structure is used for the hole injection layer, it is preferable to use the above-mentioned organic layer for the hole transport layer from the viewpoint of the energy level for the movement of holes. In this case, the polymerization initiator may be contained in the organic layer that is the hole transport layer, or in the organic layer below the hole transport layer.
[0140] (electron transport layer, electron injection layer) Examples of the electron transport layer and the electron injection layer include phenanthroline derivatives (e.g., 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP)), bipyridine derivatives, nitro-substituted fluorene derivatives, diphenylquinone derivatives, thiopyran dioxide derivatives, heterocyclic tetracarboxylic anhydrides such as naphthalene perylene, carbodiimides, fluorenylidene methane derivatives, anthraquinodimethane and anthrone derivatives, oxadiazole derivatives (2-(4-biphenylyl)-5-(4-tert-butylphenyl-1,3,4-oxadiazole) (PBD)), aluminum complexes (e.g., Tris(8-hydroxyquinolinato)aluminum(III)(Alq3)), and the like. In addition, thiadiazole derivatives in which the oxygen atom of the oxadiazole ring is replaced with a sulfur atom in the above oxadiazole derivatives, and quinoxaline derivatives having a quinoxaline ring known as an electron-withdrawing group can also be used.
[0141] (substrate) The substrate usable for the organic EL element of the present embodiment is not particularly limited in type, such as glass or plastic, and is not particularly limited as long as it is transparent, but glass, quartz, a light-transmitting resin film, etc. are preferably used. When a resin film is used, it is particularly preferable because it can impart flexibility to the organic EL element and function as a flexible substrate.
[0142] Examples of resin films include films made of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethersulfone (PES), polyetherimide, polyetheretherketone, polyphenylene sulfide, polyarylate, polyimide, polycarbonate (PC), cellulose triacetate (TAC), cellulose acetate propionate (CAP), and the like.
[0143] When a resin film is used, the resin film may be coated with an inorganic material such as silicon oxide or silicon nitride in order to suppress the transmission of water vapor, oxygen, and the like.
[0144] (Emitting color) The color of light emitted by the organic EL element of this embodiment is not particularly limited, but a white light emitting element is preferred because it can be used in various lighting fixtures such as home lighting, car lighting, clocks, and liquid crystal backlights.
[0145] As for a method for forming a white light emitting element, since it is currently difficult to emit white light from a single material, multiple luminescent materials are used to simultaneously emit multiple luminescent colors and mix them to obtain white light. The combination of multiple luminescent colors is not particularly limited, but includes those containing three maximum emission wavelengths of blue, green, and red, and those containing two maximum emission wavelengths that utilize the relationship of complementary colors such as blue and yellow, or yellow-green and orange. The emission color can be controlled by adjusting the type and amount of phosphorescent material.
[0146] <Element, lighting device, display device> The display element of this embodiment is characterized by including the organic EL element. For example, by using an organic EL element as an element corresponding to each pixel of red, green, and blue (RGB), a color display element can be obtained. In the method of forming an image, there are a simple matrix type that directly drives each organic EL element arranged on a panel with electrodes arranged in a matrix, and an active matrix type that arranges a thin film transistor for each element and drives it. The former has a simple structure but has a limit in the number of vertical pixels, so it is used for displaying characters and the like. The latter has a low driving voltage, requires less current, and can obtain a bright and high-definition image, so it is used for high-quality displays.
[0147] Further, the lighting device of this embodiment is characterized by including the organic EL element. Furthermore, the display device of this embodiment is characterized by including a lighting device and a liquid crystal element as a display means. A display device using the above-described lighting device as a backlight (white light source) and a liquid crystal element as a display means, that is, a liquid crystal display device, may be used. This configuration is a configuration in which only the backlight in a known liquid crystal display device is replaced with the above-described lighting device, and the liquid crystal element portion can use known techniques.
Example
[0148] Hereinafter, this embodiment will be described in more detail with reference to examples, but this embodiment is not limited to the following examples.
[0149] Hereinafter, a synthesis example of the charge transporting material used in this example will be shown.
[0150] <Preparation of Pd catalyst> In a glove box under a nitrogen atmosphere, at room temperature, a fluororesin-coated ceramic stirrer was placed in a glass sample vial, 73.2 mg (80 μmol) of tris(dibenzylideneacetone)dipalladium was weighed out, 15 mL of toluene was added, and the mixture was stirred for 30 minutes. Similarly, a fluororesin-coated ceramic stirrer was placed in a glass sample vial, 129.6 mg (640 μmol) of tris(t-butyl)phosphine was weighed out, 5 mL of toluene was added, and the mixture was stirred for 5 minutes. These solutions were mixed and stirred at 80°C for 2 hours, and the resulting solution was used as a catalyst after removing insoluble matter using a membrane filter with a pore size of 0.2 μm. All solvents were degassed by nitrogen bubbling for more than 30 minutes before use.
[0151] <Synthesis of charge transport materials> (Synthesis of charge transporting polymer 1) In a 100mL three-necked round-bottom glass flask, 2.34g (4.6mmol) of the following monomer 1, 0.87g (1.8mmol) of the following monomer 2, 0.91g (3.1mmol) of the following monomer 3, 0.08g (0.3mmol) of the following monomer 4, 0.09g (0.3mmol) of the following monomer 5, and 17.7mL of toluene were added, and 3.9mL of a 1% by mass toluene solution of trioctylmethylammonium chloride and 7.2mL of a 3M aqueous potassium hydroxide solution were added. All solvents were used after being degassed by nitrogen bubbling for 30 minutes or more. A reflux condenser and a nitrogen gas flow tube were attached to the flask containing the reaction solution, and the flask was immersed in an oil bath heated to 60°C and stirred for 30 minutes to dissolve the monomer. Subsequently, 1.0mL of the above-prepared Pd catalyst solution was added, and the temperature of the oil bath was set to 120°C to carry out the reaction. The reaction solution was heated and refluxed for 2 hours. All reactions were carried out under a nitrogen stream.
[0152] [ka]
[0153] After the reaction was completed, the organic layer was washed with water and poured into a methanol-water (9:1) mixed solution. The resulting precipitate was filtered off and washed with methanol. The precipitate was washed with ethyl acetate, and the eluted solid was vacuum dried. The dried solid was dissolved in toluene, and a metal adsorbent ("Triphenylphosphine, polymer-bound on styrene-divinylbenzene copolymer" manufactured by Strem Chemicals, 200 mg per 100 mg of precipitate) was added and stirred at 40°C for 2 hours. After stirring, the solution was filtered through a membrane filter with a pore size of 0.2 μm to remove the metal adsorbent and solid impurities, and the solution was poured into methanol. The precipitate was suction filtered and washed with methanol, and then the solid was vacuum dried to obtain charge transport polymer 1.
[0154] (Synthesis of charge transporting polymer 2) The charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using the following monomer 6 instead of monomer 5 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 3.1 mmol, monomer 4: 0.3 mmol, monomer 6: 0.3 mmol).
[0155] [ka]
[0156] (Synthesis of charge transporting polymer 3) The charge transport polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using the following monomer 7 instead of monomer 4 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 3.1 mmol, monomer 5: 0.3 mmol, monomer 7: 0.3 mmol).
[0157] [ka]
[0158] (Synthesis of charge transporting polymer 4) The charge transport polymer 3 was synthesized in the same manner as above, except that the reaction was carried out using monomer 6 instead of monomer 5 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 3.1 mmol, monomer 6: 0.3 mmol, monomer 7: 0.3 mmol).
[0159] (Synthesis of charge transporting polymer 5) Charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using monomer 4 instead of monomer 5 (total amount of monomer 4: 0.6 mmol).
[0160] (Synthesis of charge transporting polymer 6) Charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using monomer 5 instead of monomer 4 (total amount of monomer 5: 0.6 mmol).
[0161] (Synthesis of charge transporting polymer 7) Charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using monomer 6 instead of monomer 4 and monomer 5 (total amount of monomer 6: 0.6 mmol).
[0162] (Synthesis of charge transporting polymer 8) Charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using monomer 7 instead of monomer 4 and monomer 5 (total amount of monomer 7: 0.6 mmol).
[0163] (Synthesis of charge transporting polymer 9) The charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using 0.75 g (2.6 mmol) of monomer 3, 0.15 g (0.6 mmol) of monomer 4, and 0.19 g (0.6 mmol) of monomer 5 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 4: 0.6 mmol, monomer 5: 0.6 mmol).
[0164] (Synthesis of charge transporting polymer 10) The charge transporting polymer 9 was synthesized in the same manner as above, except that the reaction was carried out using monomer 7 instead of monomer 4 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 5: 0.6 mmol, monomer 7: 0.6 mmol).
[0165] (Synthesis of charge transporting polymer 11) The charge transporting polymer 9 was synthesized in the same manner as above, except that the reaction was carried out using the following monomer 8 instead of monomer 4 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 5: 0.6 mmol, monomer 8: 0.6 mmol).
[0166] [ka]
[0167] (Synthesis of charge transporting polymer 12) Charge transport polymer 11 was synthesized in the same manner as above, except that monomer 6 was used instead of monomer 5 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 6: 0.6 mmol, monomer 8: 0.6 mmol).
[0168] (Synthesis of charge transporting polymer 13) The charge transporting polymer 3 was synthesized in the same manner as in the synthesis of the above charge transporting polymer 3, except that the reaction was carried out using 0.75 g (2.6 mmol) of monomer 3, 0.28 g (0.9 mmol) of monomer 5, and 0.05 g (0.3 mmol) of monomer 7 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 5: 0.9 mmol, monomer 7: 0.3 mmol).
[0169] (Synthesis of charge transporting polymer 14) The charge transport polymer 13 was synthesized in the same manner as above, except that the reaction was carried out using monomer 6 instead of monomer 5 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 6: 0.9 mmol, monomer 7: 0.3 mmol).
[0170] (Synthesis of charge transporting polymer 15) Charge transport polymer 13 was synthesized in the same manner as above, except that monomer 8 was used instead of monomer 7 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 3: 2.6 mmol, monomer 5: 0.9 mmol, monomer 8: 0.3 mmol).
[0171] (Synthesis of charge transporting polymer 16) The charge transporting polymer 1 was synthesized in the same manner as above, except that the reaction was carried out using the following monomer 9 instead of monomer 3 (monomer 1: 4.6 mmol, monomer 2: 1.8 mmol, monomer 4: 0.3 mmol, monomer 5: 0.3 mmol, monomer 9: 3.1 mmol).
[0172] [ka]
[0173] (Evaluation of filter permeability) The charge transport polymer (10.0 mg) was dissolved in 0.9 mL of toluene to prepare a charge transport polymer solution. The charge transport polymer solution was placed in a 3 mL disposable syringe, a membrane filter with a pore size of 0.2 μm was attached to the tip, and the charge transport polymer solution was dropped into a glass sample tube. The solution that was able to be dropped in its entirety was evaluated as "passed" and the solution that did not come out was evaluated as "not passed."
[0174] (Evaluation of Solvent Resistance) An organic layer was formed using a charge transport polymer, and the solvent resistance was evaluated by measuring the remaining film ratio as follows. That is, an organic layer was formed in the process shown below, and the quartz plate with the formed organic layer was immersed in 10 mL of toluene under air and room temperature, and left to stand for 10 minutes. The remaining film ratio (%) of the organic layer was calculated using the following formula from the ratio of absorbance (Abs) at the absorption maximum (λmax) in the visible ultraviolet spectroscopy (UV-vis) spectrum before and after immersing the organic layer in toluene. The higher the remaining film ratio, the better the solvent resistance.
[0175] Residual film rate (%) = (absorbance of organic layer after immersion in toluene / absorbance of organic layer before immersion in toluene) × 100
[0176] Example 1 The charge transport polymer 1 (10.0 mg) was weighed into a glass sample tube and dissolved in 0.9 mL of toluene to prepare a charge transport polymer solution. The filter passability of the charge transport polymer solution was evaluated. In addition, the charge transport polymer solution was spin-coated on a quartz plate at 3,000 rpm in air. Next, the spin-coated quartz plate was placed in a nitrogen atmosphere glove box and heated on a nitrogen atmosphere hot plate at 230°C for 30 minutes to carry out a curing reaction, forming an organic layer, and the remaining film rate (%) of the organic layer was calculated.
[0177] (Examples 2 to 16) The same procedure as in Example 1 was carried out except that any one of charge transporting polymers 2 to 16 was used instead of charge transporting polymer 1, and the filter passability of the charge transporting polymer solution was evaluated and the residual film rate was measured.
[0178] Comparative Example 1 The filter passability of the charge transporting polymer solution was evaluated in the same manner as in Example 1, except that charge transporting polymer 17 was used instead of charge transporting polymer 1. The charge transporting polymer of Comparative Example 1 did not pass through the filter, and therefore could not be formed into a film, and the remaining film rate could not be measured.
[0179] The results of Examples 1 to 16 and Comparative Example 1 are shown in Table 1 below.
[0180] [Table 1]
[0181] It is seen from Examples 1 to 16 that the charge transporting polymer containing monomer 3 has better filterability than Comparative Example 1 which does not contain monomer 3. It is also seen that Examples 11, 12, and 15 which contain monomer 8 have improved film remaining rates compared to Examples 10, 13, and 14 which contain monomer 7.
[0182] As described above, by containing at least the monomers 1 to 3 in the charge transporting polymer, good filterability can be obtained, and it is possible to obtain a good laminate of organic layers by using the charge transporting polymer in which the inclusion of fine particles is suppressed. [Explanation of symbols]
[0183] 1. Light-emitting layer 2 Anode 3. Hole injection layer 4 cathode 5 Electron injection layer 6. Hole transport layer 7 Electron transport layer 8 Substrate
Claims
1. a divalent structural unit having a triarylamine structure containing an electron-withdrawing group; a trivalent or higher structural unit having an arylcarbazole structure; a monovalent structural unit having an aryl group substituted with a fluoroalkyl group; At least one of a structural unit derived from the following monomer 5 and a structural unit derived from the following monomer 6, [Formula 1] A charge transporting polymer comprising the structure: [chemical 2] * represents a bonding site to other structures, and X represents a group having a carbon-carbon unsaturated bond.
2. A charge transporting material comprising the charge transporting polymer of claim 1 .
3. An ink composition comprising the charge transporting polymer according to claim 1 or the charge transporting material according to claim 2 and a solvent.
4. An organic layer formed by using the charge transporting polymer according to claim 1, the charge transporting material according to claim 2, or the ink composition according to claim 3.
5. An organic electronic device comprising at least one organic layer according to claim 4.
6. An organic electroluminescence device comprising at least one organic layer according to claim 4.
7. The organic electroluminescent device according to claim 6 , further comprising a flexible substrate.
8. The organic electroluminescence device according to claim 6 , further comprising a resin film substrate.
9. A display device comprising the organic electroluminescence device according to any one of claims 6 to 8.
10. A lighting device comprising the organic electroluminescence element according to any one of claims 6 to 8.
11. A display device comprising the organic electroluminescence element according to any one of claims 6 to 8.
12. A display device comprising the lighting device according to claim 10 and a liquid crystal element as a display means.
Citation Information
Patent Citations
Organic electroluminescent element, display device, and lighting device
JP2006279007A
Organic electronics material, organic electronic element, and organic electroluminescent element
JP2017123438A
Electronic device
JP2019008200A
Charge transporting material and organic electronic device
JP2019083259A
Display
JP2020144160A