Long resin film with knurling
Optimized knurling of resin film ends addresses static charge and curling issues, ensuring stable unwinding and uniform coating on films with different surface compositions, enhancing film flatness and coating quality.
Patent Information
- Application Number
- JP2022511948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-22
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Existing resin films wound into rolls experience issues with static charge accumulation at the core, leading to coating disruptions, curling, and wrinkles, especially when surfaces have different compositions, affecting coating uniformity and film flatness.
A long resin film with controlled knurling at both ends, where the knurl heights and uniformity are optimized to minimize static charge, ensuring stable unwinding and maintaining film flatness, even after storage and transportation.
The solution results in reduced static charge during unwinding, preventing coating repellency and ensuring uniform coating thickness, while minimizing curling and wrinkles, thus maintaining film flatness and surface integrity.
Smart Images

Figure 0007593396000001 
Figure 0007593396000002 
Figure 0007593396000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a long resin film wound into a roll. More specifically, the present invention relates to a long resin film that has been subjected to knurling and wound into a roll. [Background technology]
[0002] Conventionally, a technique has been known in which a resin film is knurled (thickened) at both ends to enable stable winding of the resin film and prevent misalignment and damage to the resin film. However, even when a resin film is wound after knurling, the knurls are crushed at the core of the roll, and the above-mentioned effects cannot be fully achieved. For this reason, various knurling techniques have been proposed, such as a method of controlling the size of the knurl convex portion (see, for example, Patent Document 1), a method of providing a reinforcing portion at the concave portion (see, for example, Patent Document 2), and a method of providing a knurl by a non-contact method (see, for example, Patent Document 3).
[0003] On the other hand, resin films are often coated with a coating layer on the surface, but when the resin film has a high charge amount, there are problems such as repelling of the coating film during coating, unevenness in the thickness of the coating film becomes large, and alignment is disturbed when an alignment film of a liquid crystal compound is provided. The charge of the resin film during coating has been controlled by removing electricity when the resin film is wound or unwound, but this has not been sufficient for coating of coating films that require high accuracy in recent years. In response to this problem, there has been a proposal to perform knurling to suppress the relative movement of the wound resin film and suppress the charge amount of the wound resin film (see, for example, Patent Document 4), but this was not sufficient to control it. In particular, even with a resin film that has been knurled, the charge amount increases as it approaches the roll core, causing a problem of disturbance of the coating film. In particular, in the case of a resin film with different compositions on both surfaces, the charge amount increases when it is unwound, and due to the above problem, stable coating cannot be performed to the end of the resin film wound into a roll, resulting in large losses. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] WO11 / 030684 [Patent Document 2] JP 2013-166317 A [Patent Document 3] WO10 / 001752 [Patent Document 4] Japanese Patent Application Publication No. 63-74850 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made against the background of the problems of the conventional technology. That is, a main object of the present invention is to provide a long resin film wound into a roll in which the charge generation at the time of unwinding is suppressed up to the core part. A further object of the present invention is to provide a long resin film in which the occurrence of winding slippage and wrinkles after storage and transportation is suppressed and high flatness is maintained. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to achieve the above object, and as a result have completed the present invention. Section 1. A long resin film wound into a roll, Both ends of the film width are knurled. When the observer faces the roll and unwinds the film from the top of the roll toward the observer, The knurl at the right end is the right knurl, The knurl at the left end is the left knurl, The height of the knurl at the core of the right knurl is Hnbr, The height of the left knurl at the core is Hnbl. The height of the surface of the right knurl is Hner, The height of the surface layer of the left knurl is Hnel, In this case, A long resin film that satisfies the following conditions (1) and (2). (1) Both Hnbr and Hnbl are 0.5-4 μm (2) Both Hnbr / Hner and Hnbl / Hnel are 0.3-0.9. Section 2. Item 2. The long resin film according to item 1, wherein both Hner and Hnel are 1.2 to 6 μm. Section 3. Item 3. The long resin film according to item 1 or 2, wherein the absolute value of the uniformity of the knurl height on the left and right sides of the core portion, calculated by |(Hnbr-Hnbl) / [(Hnbr+Hnbl) / 2]|, is 0.3 or less. Section 4. 4. The long resin film according to any one of items 1 to 3, wherein when the outer surface of the long resin film is surface A and the inner surface of the long resin film is surface B, surface A and surface B have different compositions. Section 5. 5. The long resin film according to any one of items 1 to 4, wherein when the outer surface of the long resin film is surface A and the inner surface of the long resin film is surface B, at least one of surface A and surface B is the surface of the first coating layer. Section 6. 6. The long resin film according to any one of items 1 to 5, which is a stretched polyester film. Section 7. 7. A laminated film comprising the long resin film according to any one of items 1 to 6, and a second coating layer provided on at least one surface of the long resin film. Section 8. Item 8. The laminate film according to item 7, wherein the second coating layer is a hard coating layer, an antiglare layer, an antireflection layer, a low reflection layer, an alignment layer, or a retardation layer. Section 9. Item 9. The laminate film according to item 7 or 8, which is a polarizer protective film or a thin film layer transfer film. Section 10. A method for producing a laminated film, comprising: (A) unwinding the long resin film according to any one of items 1 to 6; and (B) applying a coating liquid for a second coating layer to at least one surface of the unwound long resin film. Section 11. Item 11. The method for producing a laminate film according to item 10, wherein the laminate film is a polarizer protective film. Section 12. Item 11. The method for producing a laminated film according to item 10, wherein the laminated film is a thin film layer transfer film. Effect of the Invention
[0007] The long resin film of the present invention wound into a roll has a small amount of electrostatic charge when the film is unwound all the way to the core, and when the film is coated, for example, the coating film has little repelling and can be provided with a coating film having excellent thickness accuracy all the way to the end of the film. Furthermore, the long resin film of the present invention is inhibited from slipping during winding or wrinkling after storage or transportation, has no scratches on the film surface, and has excellent flatness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] (Long resin film) The long resin film of the present invention is wound into a roll. The resin constituting the long resin film (when the long resin film has a base film and a coating layer (a first coating layer described later) provided on at least one side of the base film, the resin constituting the base film) is not particularly limited, and any resin can be used. As the resin, polyester, polycycloolefin, triacetyl cellulose, acrylic, polycarbonate, polyamide, polyimide, and polypropylene are preferable, polyester, polycycloolefin, and triacetyl cellulose are more preferable, and polyester is even more preferable. In the case of polyester, polyethylene terephthalate and polyethylene naphthalate are preferable.
[0009] The long resin film may be an unstretched film or a stretched film (uniaxially or biaxially stretched film). The long resin film is preferably a stretched film, and particularly preferably a stretched polyester film. In this specification, the term "stretched polyester film" is used to include a film obtained by laminating a first coating layer described below on at least one side of a base film made of a polyester film and stretching the film.
[0010] The lower limit of the width of the long resin film is preferably 500 mm, more preferably 800 mm, even more preferably 1000 mm, and particularly preferably 1200 mm. The upper limit of the width of the long resin film is preferably 4000 mm, more preferably 3500 mm, even more preferably 3000 mm, particularly preferably 2700 mm, and most preferably 2500 mm.
[0011] The lower limit of the length of the long resin film is preferably 1000 m, more preferably 1500 m, and even more preferably 2000 m. The upper limit of the length of the long resin film is preferably 20000 m, more preferably 15000 m, even more preferably 10000 m, and particularly preferably 7000 m.
[0012] The lower limit of the thickness of the long resin film is preferably 25 μm, more preferably 30 μm, even more preferably 35 μm, particularly preferably 40 μm, and most preferably 45 μm. By making it equal to or greater than the lower limit, it is possible to effectively prevent wrinkles and winding slippage. The upper limit of the thickness of the long resin film is preferably 200 μm, more preferably 150 μm, even more preferably 100 μm, particularly preferably 90 μm, and most preferably 80 μm. By making it equal to or less than the upper limit, it becomes easier to handle.
[0013] In the case of a long resin film, when the outer surface of the film is called side A and the inner surface of the film is called side B, the compositions of sides A and B may be the same or different. If the compositions of sides A and B are different, the film is likely to become highly charged when unwound. The present invention is preferably applied to such a long resin film having different compositions on sides A and B.
[0014] Examples of cases where the composition is different between the A side and the B side include cases where different kinds of raw resins are laminated by coextrusion, cases where a coating layer (first coating layer) is provided only on the A side or the B side (when one of the A side and the B side is the surface of the first coating layer and the other is the surface of the base film), and cases where coating layers with different compositions (referred to as the first coating layer A and the first coating layer B, respectively) are provided on both the A side and the B side (when the A side is the surface of the first coating layer A and the B side is the surface of the first coating layer B). In any case, the present invention is suitably applied. In particular, the present invention is preferably applied to a long-sized resin film in which the resin compositions of the layers constituting the A side and the B side are different. In addition, the present invention is preferably applied to a long-sized resin film in which at least one of the A side and the B side is the surface of the first coating layer.
[0015] (First Coat Layer) Preferred examples of the first coating layer include an easy-adhesion layer, an easy-slip layer, a smoothing layer, a hard coating layer, and an orientation control layer. The first coating layer may be a single layer or a multilayer of two or more layers. The first coating layer may be provided in-line during film formation, or may be provided offline after film formation. When the first coating layer is provided, the long resin film having the knurl of the present invention includes the first coating layer.
[0016] Preferred examples of the resin used in the first coating layer include polyester, acrylic, polyurethane (polyester polyurethane, polycarbonate polyurethane, polyether polyurethane, etc.), ethylene vinyl acetate copolymer, polyamide, styrene acrylic copolymer, polyvinyl alcohol, etc. In addition, when the first coating layer is a hard coating layer, etc., the resin used in the first coating layer may be a photocurable resin, or a monomer or oligomer of a double bond-containing compound.
[0017] It is also preferable that the resin used in the first coating layer contains a crosslinking agent. Preferred examples of the crosslinking agent include isocyanate, amino resin such as melamine, oxazoline compound, and epoxy resin. In the case of a photocurable resin, the crosslinking agent may be a compound (monomer or oligomer) containing multiple double bonds, such as trimethylolpropane triacrylate, pentaerythritol tetraacrylate, acrylic-modified polyurethane, and acrylic-modified epoxy resin.
[0018] The first coating layer may contain additives, such as particles, surfactants, leveling agents, antistatic agents, catalysts, and combinations thereof.
[0019] The lower limit of the thickness of the first coating layer is preferably 0.001 μm, more preferably 0.005 μm, even more preferably 0.01 μm, and particularly preferably 0.02 μm. The upper limit of the thickness of the first coating layer is preferably 10 μm, more preferably 5 μm, even more preferably 3 μm, particularly preferably 2 μm, and most preferably 1 μm.
[0020] (Knurl processing) The long resin film is preferably one that has been knurled at both ends of the film width (one that has knurled parts), and is preferably one that has been wound into a roll after knurling. The method of knurling is not particularly limited, and examples thereof include a method of pressing the film against a knurl to deform the film, a method of irradiating laser light to create a bulge around a hole, and a method of providing dots of ultraviolet curing resin or hot melt resin using a method such as inkjet printing. These methods can provide dot-like protrusions on the film surface.
[0021] "Both ends of the film width" refers to a region within 50 mm (or within 10% of the total width when the total width is less than 500 mm) from each end in the film width direction. The lower limit of the distance between the end of the film width direction and the knurl position (the edge of the film end side of the knurl processed part) is preferably 0.5 mm, more preferably 1 mm, on both the right and left sides. The upper limit of the distance between the end of the film width direction and the knurl position is preferably 20 mm, more preferably 15 mm, and even more preferably 10 mm, on both the right and left sides. By setting it in the above range, stable knurl processing can be performed on both ends of the film width direction and the effective width of the film can be secured.
[0022] The lower limit of the width of the knurl processed portion is preferably 3 mm, more preferably 5 mm, and even more preferably 7 mm. By making it equal to or greater than the lower limit, the knurl can be made less likely to be crushed. The upper limit of the width of the knurl processed portion is preferably 30 mm, more preferably 25 mm, and even more preferably 20 mm. By making it equal to or less than the upper limit, the degree of knurl crushing can be optimized and the effective width of the film can be secured.
[0023] The lower limit of the spacing between the convex portions of the knurled portion (for example, the spacing in the width direction or length direction) is preferably 0.5 mm, more preferably 0.6 mm, and even more preferably 0.7 mm. The upper limit of the spacing between the convex portions of the knurled portion is preferably 3 mm, more preferably 2.5 mm, even more preferably 2 mm, and particularly preferably 1.5 mm. The spacing between the convex portions of the knurled portion is the spacing between the center points of the convex portions. In the case of hot knurling described later, a bulge is formed around the protrusion according to the shape of the knurled protrusion, and for example, the spacing between the centers of the rectangular bulges is the spacing between the convex portions.
[0024] The lower limit of the density of the protrusions of the knurled part is preferably 10 pieces / cm 2 and more preferably 15 / cm 2 and more preferably 25 particles / cm 2 and particularly preferably 40 particles / cm 2 and most preferably 60 particles / cm 2 The upper limit of the density of the protrusions of the knurled portion is preferably 400 pieces / cm 2 and more preferably 300 particles / cm 2 and more preferably 250 particles / cm 2 The crushability of the knurl can be adjusted by the density of the protrusions of the knurl processed portion, but by setting the density within the above range, it becomes easy to adjust the crushability by relatively simple knurl processing.
[0025] The arrangement of the convex portions of the knurled portion may be, for example, aligned vertically and horizontally, a staggered arrangement in which adjacent concave-convex arrays are shifted by half a period, or a diagonal arrangement in which adjacent concave-convex arrays are shifted by 1 / 3 or 1 / 4.
[0026] (Knurling) As an example of knurling, a commonly used method of deforming a film by pressing the film against a knurl will be described in detail, but the present invention is not limited to this method.
[0027] The material of the knurl is preferably a metal. Examples of metals include SUS, stainless steel, aluminum, titanium, hard chrome, etc. The surface of the knurl may be plated.
[0028] The lower limit of the diameter of the knurl is preferably 3 cm, more preferably 5 cm. The upper limit of the diameter of the knurl is preferably 30 cm, more preferably 25 cm, and even more preferably 20 cm. By setting the diameter within the above range, a knurling device of appropriate size can be obtained.
[0029] The lower limit of the knurling thickness is preferably 3 mm, more preferably 5 mm, and even more preferably 7 mm. The upper limit of the knurling thickness is preferably 50 mm, more preferably 40 mm, and even more preferably 30 mm.
[0030] The outer periphery of the knurling is provided with protrusions in accordance with the arrangement of the convex portions to be applied. The lower limit of the height of the protrusions is preferably 0.05 mm, more preferably 0.1 mm, even more preferably 0.15 mm, and particularly preferably 0.2 mm. The upper limit of the height of the protrusions is preferably 3 mm, more preferably 2.5 mm, even more preferably 2 mm, and particularly preferably 1.5 mm.
[0031] The shape of the protrusions, as viewed from above, may be a circle, an ellipse, a triangle, a square, a rectangle, a rhombus, a trapezoid, a pentagon, a hexagon, or a polygon with more sides, among which a square, a rectangle, or a rhombus is preferable. The three-dimensional shape may be a pyramid such as a cone or a polygonal pyramid, or a truncated pyramid such as a truncated cone or a polygonal pyramid, but knurls provided in a truncated pyramid shape tend to be less likely to be crushed.
[0032] When the protrusions are frustum-shaped, the total area of the flat parts on the upper surfaces of the protrusions is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more, of the area of the knurled outer periphery on which the protrusions are provided. This total area is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less, of the area of the knurled outer periphery on which the protrusions are provided. By setting the area within the above range, the effect of the frustum shape can be more reliably exhibited.
[0033] (Knurl processing conditions) The knurling may be performed, for example, on both sides of a film by sandwiching the film between two knurls. In this case, the two knurls may be a pair of knurls that engage with each other's unevenness, or may be a pair of knurls that perform knurling independently without engaging with each other. In addition, the knurling may be performed only on one side of a film by sandwiching the film between a knurl and a smooth roll.
[0034] The knurling is preferably performed by pressing the film against the knurl. The height of the knurl can be adjusted by this pressing force. The lower limit of the pressing force is preferably 20N, more preferably 40N, and even more preferably 50N. The upper limit of the pressing force is preferably 2000N, more preferably 1500N, and even more preferably 1000N. By setting the pressing force within the above range, the knurling can be performed without using excessive equipment. In addition, the pressing may be performed by moving either the pair of knurls, or the knurl and the smooth roll, or by moving both of them.
[0035] The knurling process using knurling may be performed either without heating the knurl (cold knurling method) or by heating the knurling to a temperature above the softening temperature of the film (e.g., the glass transition temperature (Tg)) (hot knurling method), but the knurl tends to be less likely to be crushed when using the hot knurling method.
[0036] The surface temperature of the knurl is preferably 10°C or higher, more preferably 20°C or higher. In the case of the hot knurl method, the surface temperature of the knurl is preferably the Tg of the film or higher, more preferably (Tg+20°C) or higher, and even more preferably (Tg+50°C) or higher. The surface temperature of the knurl is preferably below the melting point of the film, more preferably (melting point-10°C) or lower, and even more preferably (melting point-20°C) or lower. By keeping it within the above range, efficient knurl processing is possible, and it is possible to suppress the resin from melting at the knurl-processed portion to generate whiskers, and the film from becoming wavy at the knurl-processed portion.
[0037] Specifically, in the case of a polyethylene terephthalate film (including a film having a first coating layer provided on at least one side of a base film made of a polyethylene terephthalate film, and films obtained by stretching these), the surface temperature of the knurling is preferably 80 to 250°C, more preferably 100 to 240°C, and even more preferably 120 to 230°C.
[0038] Methods for increasing the surface temperature of the knurl include, for example, a method of flowing a heated fluid such as oil inside the knurl, induction heating, infrared heating, hot air, etc. Also, the portion of the film to be knurled (the edge of the film) may be preheated with infrared rays, hot air, etc.
[0039] The lower limit of the knurling speed is preferably 20 m / min, more preferably 30 m / min, and even more preferably 50 m / min. The upper limit of the knurling speed is preferably 800 m / min, more preferably 600 m / min, and even more preferably 500 m / min. By setting the speed in the above range, highly productive knurling is possible, and stable knurling can be performed under appropriate conditions. The knurling speed is limited by the processing speed of processes accompanied by knurling, such as slitting and coating.
[0040] The knurl height can be adjusted by adjusting the pressing pressure of the knurl, the temperature of the knurl surface, the knurl processing speed, and the like.
[0041] (Initial knurl height) The lower limit of the knurl height (initial knurl height) immediately after the knurl processing is preferably 1.5 μm, more preferably 2 μm, and even more preferably 2.5 μm. The upper limit of the knurl height immediately after the knurl processing is preferably 15 μm, more preferably 12 μm, even more preferably 10 μm, particularly preferably 7 μm, and most preferably 6 μm.
[0042] The knurl immediately after knurling has a portion that is easily crushed when wound into a roll. The reason for this is thought to be that in the case of the cold knurling method, the film is pushed out to the opposite side of the knurl by the knurling projections to form a knurl, but the pushed-out knurl has a portion that is easily depressed by pressure, and in the case of the hot knurling method, the resin is raised around the knurling projections, but this is not a uniform height but is of uneven height, so the raised portion is easily crushed even with low pressure.
[0043] Therefore, the initial knurl height is measured on the film taken from the outermost layer immediately after being wound into a roll. Taking the above into consideration, it is preferable to adjust the initial knurl height so that the knurl heights of the surface layer and the core are within the range described below.
[0044] (winding) The long resin film is preferably wound into a roll around a cylindrical core. The lower limit of the winding tension is preferably 50 N / m, more preferably 60 N / m, even more preferably 70 N / m, particularly preferably 80 N / m, and most preferably 90 N / m. The upper limit of the winding tension is preferably 330 N / m, more preferably 300 N / m, even more preferably 270 N / m, particularly preferably 250 N / m, and most preferably 230 N / m. By setting it within the above range, the degree of knurl crushing can be optimized, and it is possible to prevent winding slippage, wrinkles, deterioration of flatness, etc. during storage.
[0045] During winding, it is preferable to press the touch roll against the film and wind the film while removing the entrained air. In this case, the lower limit of the winding contact pressure of the touch roll is preferably 30 N / m, more preferably 40 N / m, even more preferably 50 N / m, and particularly preferably 60 N / m. The upper limit of the winding contact pressure is preferably 600 N / m, more preferably 500 N / m, even more preferably 400 N / m, and particularly preferably 300 N / m. By setting the pressure within the above range, the degree of knurl crushing can be adjusted, and winding slippage, wrinkles, deterioration of flatness, etc. during storage can be prevented.
[0046] (Knurl height of long resin film wound into a roll) In this specification, the right side, the left side, the surface layer portion, and the winding core portion are defined as follows. Right side: The right end when an observer faces the roll and unwinds the film from the top of the roll toward the viewer. Left side: The left end when an observer faces the roll and unwinds the film from the top of the roll toward the viewer. Surface layer: 100±1m from the end of a roll of film (or approximately 10% of the total length of the film if the total length is less than 1000m). Core: The part 100±1m from the beginning of the film wound into a roll (or about 10% of the total length of the film if the total length is less than 1000m).
[0047] The abbreviations for the knurl heights at each location are as follows: Surface right side knurl height: Hner Surface left side knurl height: Hnel Note that Hne represents the height of the knurl at the surface layer without being limited to the left or right. Height of right side of core: Hnbr Height of left side knurl of core: Hnbl It should be noted that Hnb represents the knurl height of the core portion without being limited to the left or right.
[0048] The lower limit of the knurl height (both Hnbr and Hnbl) of the core is preferably 0.5 μm, more preferably 0.7 μm, even more preferably 0.9 μm, particularly preferably 1 μm, and most preferably 1.1 μm. The upper limit of the knurl height (both Hnbr and Hnbl) of the core is preferably 4 μm, more preferably 3.5 μm, even more preferably 3.2 μm, and particularly preferably 3 μm.
[0049] The lower limit of the knurl height (both Hner and Hnel) of the surface layer is preferably 1.2 μm, more preferably 1.3 μm, even more preferably 1.4 μm, particularly preferably 1.5 μm, and most preferably 1.6 μm. The upper limit of the knurl height (both Hner and Hnel) of the surface layer is preferably 6 μm, more preferably 5 μm, even more preferably 4 μm, particularly preferably 3.7 μm, and most preferably 3.5 μm.
[0050] The knurl collapse reaches a steady state about one month after winding into a roll. Therefore, it is preferable to measure the knurl height of the core and surface layer one month after winding into a roll. The knurl height of the core and surface layer can be set within the above range depending on the type of knurl, initial knurl height, knurl shape, knurl width, winding tension, winding contact pressure, winding length, etc.
[0051] The lower limit of the knurl residual ratio (Hnb / Hne) [both the right knurl residual ratio (Hnbr / Hner) and the left knurl residual ratio (Hnbl / Hnel)] is preferably 0.3, more preferably 0.35, even more preferably 0.4, and particularly preferably 0.45. The upper limit of the knurl residual ratio (Hnb / Hne) [both Hnbr / Hner and Hnbl / Hnel] is preferably 0.9, more preferably 0.85, even more preferably 0.8, particularly preferably 0.75, and most preferably 0.7. The knurl residual ratio can be set within the above range depending on the knurl type, initial knurl height, knurl shape, knurl width, knurl height uniformity, winding tension, winding length, etc.
[0052] The lower limit of the knurl reduction amount (Hne-Hnb) [both the right knurl reduction amount (Hner-Hnbr) and the left knurl reduction amount (Hnel-Hnbl)] is preferably 0.2 μm, more preferably 0.23 μm, even more preferably 0.25 μm, particularly preferably 0.28 μm, and most preferably 0.3 μm. The upper limit of the knurl reduction amount (Hne-Hnb) [both Hner-Hnbr and Hnel-Hnbl] is preferably 3 μm, more preferably 2.7 μm, even more preferably 2.5 μm, particularly preferably 2.2 μm, and most preferably 2 μm. The knurl reduction amount can be set within the above range depending on the knurl type, initial knurl height, knurl shape, knurl width, knurl height uniformity, winding tension, winding length, etc.
[0053] By setting the knurl height, knurl residual rate, knurl reduction amount, etc. of the core portion within the above ranges, the unwinding charge amount can be reduced, scratches on the film surface can be prevented, and winding slippage and wrinkles can be prevented, ensuring flatness. These effects can be further improved in a more preferable direction by setting the knurl height, knurl residual rate, knurl reduction amount, etc. of the surface layer portion within the above ranges.
[0054] The lower limit of the absolute value of the knard height uniformity on the left and right sides of the winding core (|(Hnbr-Hnbl) / [(Hnbr+Hnbl) / 2]|) is preferably 0, more preferably 0.01, and the upper limit is preferably 0.3, more preferably 0.25, even more preferably 0.2, and particularly preferably 0.15.
[0055] The lower limit of the absolute value of the knurl height uniformity (|(Hner-Hnel) / [(Hner+Hnel) / 2]|) on the left and right sides of the surface layer is preferably 0, more preferably 0.01, and the upper limit is preferably 0.3, more preferably 0.25, even more preferably 0.2, and particularly preferably 0.15.
[0056] By keeping the uniformity of the knurl height on the left and right sides of the core and surface layer within the above range, the amount of charge at unwinding can be reduced, scratches, winding slippage, and wrinkles on the film surface can be prevented, and flatness can be ensured, while also preventing meandering and sagging when the film is unwound from the roll and processed.
[0057] The knurl height tends to vary between the left and right sides due to differences in the film's length across the width, differences in physical properties such as elastic modulus, and differences in tension across the width when the film is wound up. The absolute value of the uniformity of the knurl height can be reduced by precisely controlling the parallelism of the transport rolls before the film is wound up, and by controlling the temperature so that differences in physical properties do not occur during film formation such as stretching and heat setting.
[0058] The long resin film of the present invention wound into a roll has a low charge amount when unwound all the way to the core of the roll. Therefore, for example, when the film is unwound and processed, such as for example, coating, the coating liquid is less likely to repel or have uneven thickness, and a defect-free coating film can be obtained.
[0059] (unwinding charge amount) The upper limit of the unwinding charge amount at the core is, in absolute value, preferably 25 kV, more preferably 20 kV, further preferably 15 kV, and particularly preferably 12 kV. The lower limit of the unwinding charge amount at the core is, in absolute value, preferably 0.1 kV, more preferably 0.5 kV. The unwinding charge amount refers to the charge amount at the center in the width direction of the film immediately after unwinding at 100 m / min.
[0060] (Laminated film) The long resin film of the present invention is preferably used as a base film for providing each functional layer, and processed into a laminate film. The laminated film of the present invention preferably has a long resin film and a second coating layer (a coating film formed by applying a coating liquid and laminating it) provided on at least one side of the long resin film. The manufacturing method of the laminated film preferably includes a step (A) of unwinding the long resin film, and a step (B) of applying a coating liquid for the second coating layer to at least one side of the unwound long resin film. The laminated film may be one in which the second coating layer is laminated on at least one side of the long resin film and then wound into a roll, or one in which the second coating layer is laminated (without being wound into a roll) and then cut to a predetermined size.
[0061] Resins used in the coating liquid for the second coating layer are preferably polyester, acrylic resin, polyurethane (e.g., polyester polyurethane, polycarbonate polyurethane, polyether polyurethane), ethylene vinyl acetate copolymer, polyamide, styrene acrylic copolymer, polyvinyl alcohol, etc., and if a radiation-curable coating film is to be formed, preferably used are acrylic monomers, acrylic oligomers, polymerizable liquid crystal compounds, etc. Among them, acrylic monomers, acrylic oligomers, and polymerizable liquid crystal compounds are preferably used.
[0062] As the solvent for the coating liquid for the second coat layer, aromatic hydrocarbons such as toluene, alcohols, ketones, and esters are preferable, but if the coating liquid is radiation-curable, it may be solvent-free.
[0063] The lower limit of the thickness of the second coating layer (thickness of the resulting coating film after drying) is preferably 0.001 μm, more preferably 0.005 μm, even more preferably 0.01 μm, and particularly preferably 0.02 μm. The upper limit of the thickness of the coating layer is preferably 20 μm, more preferably 15 μm, even more preferably 10 μm, particularly preferably 7 μm, and most preferably 5 μm.
[0064] The second coating layer (obtained coating film) is preferably an optically functional layer such as a hard coating layer, an antiglare layer, an antireflection layer, a low reflection layer, an alignment layer (e.g., a photoalignment layer), or a retardation layer (e.g., a λ / 4 retardation layer, a λ / 2 retardation layer). The second coating layer may be, for example, an adhesive or a pressure-sensitive adhesive. The second coating layer may be a single layer or a multilayer of two or more layers (e.g., an alignment layer and a retardation layer).
[0065] The surface of the second coating layer does not necessarily have to have the same characteristics as the surface of the long resin film of the present invention. In addition, the laminated film may be one in which both ends (knurled portions) of the film width are cut. Even if the long resin film itself does not have a first coating layer, the coating layer laminated on the long resin film is called the second coating layer.
[0066] Preferred applications of the laminate film include antiglare films, low reflection films, antireflection films, transparent conductive film substrates, polarizer protective films, retardation films having a retardation layer made of a liquid crystal compound, and thin film layer transfer films for transferring these functional layers. EXAMPLES
[0067] (1) Naar height A digital micrometer (Sony Manufacturing Systems Corporation μ-mate M-30) was used. The central part of the width of the knurl was measured at 10 points along the MD (also called the flow direction, longitudinal direction, vertical direction, etc.) at intervals of approximately 5 cm, and the average value was recorded as the "knurl thickness." The knurl-processed part was measured at 10 points along the MD at intervals of approximately 5 cm about 1 cm inside from the edge of the central side of the film, and the average value was recorded as the "film thickness," and "knurl thickness - film thickness" was recorded as the knurl height. The film was wound into a roll, stored at room temperature for one month, and then unwound, and measurements were taken at a total of four points on the surface layer and core of the right and left sides of the film.
[0068] The right side, left side, surface layer, and core are as follows: Right side: The right end when an observer faces the roll and unwinds the film from the top of the roll toward the viewer. Left side: The left end when an observer faces the roll and unwinds the film from the top of the roll toward the viewer. Surface layer: The area 100m from the end of a roll of film. Core section: The section 100m from the beginning of a roll of film.
[0069] The abbreviations for the knurl heights at each location are as follows: Surface right side knurl height: Hner Surface left side knurl height: Hnel Height of right side of core: Hnbr Height of left side knurl of core: Hnbl
[0070] (2) Nale Residual Rate It is as follows. Right side nar survival rate: Hnbr / Hner Left nale survival rate: Hnbl / Hnel
[0071] (3) Amount of reduction in nar It is as follows. Right side narl reduction: Hner-Hnbr Left narl reduction: Hnel-Hnbl
[0072] (4) Uniformity of knurl height It is as follows. Uniformity of knurl height on left and right sides of core: Absolute value of (Hnbr-Hnbl) / [(Hnbr+Hnbl) / 2] Uniformity of surface knurl height on both sides: absolute value of (Hner-Hnel) / 〔(Hner+Hnel) / 2〕 (5) Unwinding charge After storage at room temperature for one month, the rolled film was unwound from the surface at a speed of 100 m / min, and the amount of electrostatic charge in the center of the film core was measured. The measurement was performed using a KSD-0103 made by Kasuga Electric Co., Ltd., and the part of the film immediately after peeling from the roll was measured. (6) Winding Misalignment After storage at room temperature for one month, the end surface of the rolled film was observed. ⊚: No difference from the state immediately after winding, no unevenness. ◯: A slight increase in unevenness or a bamboo shoot-like deformation was observed. Δ: An increase in unevenness or a bamboo-shoot-like deformation was observed, but the level was not problematic for practical use. ×: Increase in unevenness or bamboo-shoot-like deformation to a level that makes practical use impossible was observed.
[0073] (7) Wrinkles After storage at room temperature for one month, the rolled film was unwound and the wrinkles along its entire length were observed. : No wrinkles at all. ○: Slight wrinkles were observed along a portion of the entire length. △: Weak wrinkles were observed in some areas along the entire length, but were not significant. ×: Wrinkles were observed in part of the entire length to such an extent that practical use was not possible. (8) Film flatness After storing at room temperature for one month, the rolled film was unwound, and a 3m length was cut from the film 80-90m from the surface, which was placed on a table with a flat, matte black top, and flatness was evaluated based on the shape of the fluorescent light on the ceiling reflected on the film. The flatness was also evaluated by comparing it with the flatness of the film immediately after it was unwound. : No difference from the sample immediately after winding. ○: Planarity was slightly deteriorated. Δ: Planarity was deteriorated, but not at a problem-free level. ×: Planarity was deteriorated to a level that was not practically usable.
[0074] (Production of Easy-Adhesion Layer Component for First Coat Layer) (Polymerization of polyester resin) A stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser was charged with 194.2 parts by mass of dimethyl terephthalate, 184.5 parts by mass of dimethyl isophthalate, 14.8 parts by mass of dimethyl-5-sodium sulfoisophthalate, 233.5 parts by mass of diethylene glycol, 136.6 parts by mass of ethylene glycol, and 0.2 parts by mass of tetra-n-butyl titanate, and the transesterification reaction was carried out at a temperature of 160°C to 220°C for 4 hours. The mixture was then heated to 255°C, the reaction system was gradually depressurized, and the mixture was reacted for 1 hour and 30 minutes under a reduced pressure of 30 Pa to obtain a copolymer polyester resin. The obtained copolymer polyester resin was pale yellow and transparent. The reduced viscosity of the copolymer polyester resin was measured and found to be 0.70 dl / g. The glass transition temperature measured by DSC was 40°C.
[0075] (Preparation of Polyester Water Dispersion) 30 parts by mass of polyester resin and 15 parts by mass of ethylene glycol n-butyl ether were placed in a reactor equipped with a stirrer, a thermometer, and a reflux device, and the resin was dissolved by stirring while heating at 110°C. After the resin was completely dissolved, 55 parts by mass of water was gradually added while stirring the polyester solution. After the addition was completed, the mixture was cooled to room temperature while stirring to obtain a milky white polyester water dispersion with a solid content of 30% by mass.
[0076] (Preparation of aqueous polyvinyl alcohol solution) 90 parts by mass of water was placed in a vessel equipped with a stirrer and a thermometer, and 10 parts by mass of polyvinyl alcohol resin (manufactured by Kuraray, polymerization degree 500 and saponification degree 74%) was gradually added while stirring. After the addition was completed, the mixture was heated to 95°C while stirring to dissolve the resin. After the resin was dissolved, the mixture was cooled to room temperature while stirring to obtain an aqueous polyvinyl alcohol solution with a solid content of 10% by mass.
[0077] (Preparation of blocked polyisocyanate crosslinking agent used in adhesive layer P1) In a flask equipped with a stirrer, a thermometer and a reflux condenser, 100 parts by mass of a polyisocyanate compound having an isocyanurate structure made from hexamethylene diisocyanate (Asahi Kasei Chemicals, Duranate TPA), 55 parts by mass of propylene glycol monomethyl ether acetate, and 30 parts by mass of polyethylene glycol monomethyl ether (average molecular weight 750) were charged and kept at 70°C for 4 hours under a nitrogen atmosphere. Thereafter, the temperature of the reaction liquid was lowered to 50°C, and 47 parts by mass of methyl ethyl ketoxime were added dropwise. The infrared spectrum of the reaction liquid was measured to confirm that the absorption of the isocyanate group had disappeared, and water was further added to obtain a blocked polyisocyanate aqueous dispersion with a solid content of 40% by mass.
[0078] (Preparation of Coating Solution for Adhesion Layer P1) The following raw materials were mixed to prepare a coating solution for P1. Water 40.61% by mass Isopropanol 30.00% by mass Polyester water dispersion 11.67% by mass Polyvinyl alcohol aqueous solution 15.00% by mass Blocked isocyanate crosslinking agent (aqueous solution) 0.67% by mass Particles (silica sol with an average particle size of 100 nm, solid content concentration of 40% by mass) 1.25% by mass Catalyst (organotin compound, solid concentration 14% by mass) 0.3% by mass Surfactant (silicon-based, solids concentration 10% by mass) 0.5% by mass
[0079] (Preparation of polyurethane resin used in adhesive layer P2) A polyurethane resin containing an aliphatic polycarbonate polyol as a constituent component was prepared by the following procedure. 43.75 parts by mass of 4,4-diphenylmethane diisocyanate, 12.85 parts by mass of dimethylol butanoic acid, 153.41 parts by mass of polyhexamethylene carbonate diol having a number average molecular weight of 2000, 0.03 parts by mass of dibutyltin dilaurate, and 84.00 parts by mass of acetone as a solvent were added to a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, and the mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and it was confirmed that the reaction liquid reached a predetermined amine equivalent. Next, the temperature of this reaction liquid was lowered to 40°C, and then 8.77 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 450 g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C. The water was stirred for 2000 min. -1 The polyurethane prepolymer solution was added and dispersed while stirring and mixing at 40°C. Then, acetone and a part of the water were removed from the mixed solution under reduced pressure to prepare a water-soluble polyurethane resin (polyurethane resin aqueous solution) with a solid content of 35%. The glass transition temperature of the obtained polyurethane resin containing an aliphatic polycarbonate polyol as a constituent component was -30°C.
[0080] (Preparation of oxazoline-based crosslinking agent used in adhesive layer P2) A mixture of 58 parts by mass of ion-exchanged water and 58 parts by mass of isopropanol as an aqueous medium, and 4 parts by mass of a polymerization initiator (2,2'-azobis(2-amidinopropane) dihydrochloride) were placed in a flask equipped with a thermometer, a nitrogen gas inlet tube, a reflux condenser, a dropping funnel, and a stirrer. Meanwhile, a mixture of 16 parts by mass of 2-isopropenyl-2-oxazoline as a polymerizable unsaturated monomer having an oxazoline group, 32 parts by mass of methoxypolyethylene glycol acrylate (average number of moles of ethylene glycol added: 9 moles, Shin-Nakamura Chemical Co., Ltd.), and 32 parts by mass of methyl methacrylate were placed in the dropping funnel, and added dropwise at 70°C for 1 hour under a nitrogen atmosphere. After the dropwise addition was completed, the reaction solution was stirred for 9 hours and cooled to obtain a water-soluble resin having an oxazoline group (oxazoline-based crosslinking agent aqueous solution) with a solid content of 40% by mass.
[0081] (Preparation of Coating Solution for Adhesion Layer P2) The following raw materials were mixed to prepare a coating solution for P2 for forming a coating layer with excellent adhesion to the functional layer. Water 55.62% by mass Isopropanol 30.00% by mass Polyurethane resin aqueous solution 11.29% by mass Oxazoline crosslinker aqueous solution 2.26% by mass Particles (silica sol with an average particle size of 40 nm, solid content concentration of 40% by mass) 0.71% by mass Particles (silica sol with an average particle size of 450 nm, solid content concentration of 40% by mass) 0.07% by mass Surfactant (silicon-based, solids concentration 100% by mass) 0.05% by mass
[0082] (Manufacture of polyester resin for base film) The esterification reactor was heated, and when it reached 200°C, 86.4 parts by mass of terephthalic acid and 64.6 parts by mass of ethylene glycol were charged, and 0.017 parts by mass of antimony trioxide, 0.064 parts by mass of magnesium acetate tetrahydrate, and 0.16 parts by mass of triethylamine were charged as catalysts while stirring. Next, the temperature was increased under pressure, and a pressurized esterification reaction was carried out under conditions of a gauge pressure of 0.34 MPa and 240°C, after which the esterification reactor was returned to normal pressure and 0.014 parts by mass of phosphoric acid was added. Further, the temperature was increased to 260°C over 15 minutes, and 0.012 parts by mass of trimethyl phosphate was added. Next, after 15 minutes, a dispersion treatment was carried out using a high-pressure disperser, and after 15 minutes, the obtained esterification reaction product was transferred to a polycondensation reactor, and a polycondensation reaction was carried out under reduced pressure at 280°C.
[0083] After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cut diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets. The intrinsic viscosity of the resulting polyethylene terephthalate resin was 0.68 dL / g, and it contained substantially no inert particles or internally precipitated particles (hereinafter abbreviated as PET). The intrinsic viscosity was measured in a phenol / tetrachloroethane = 60 / 40 (mass ratio) solution, assuming that the Huggins constant was 0.38.
[0084] (Production of Film A) As the film raw material, PET pellets were dried under reduced pressure (1 Torr) at 135°C for 6 hours, then fed into an extruder and melted at 285°C. The molten polymer was filtered through a sintered stainless steel filter medium (nominal filtration accuracy of 10μm particles, 95% cut), extruded from a die into a sheet, and then wrapped around a casting drum with a surface temperature of 30°C using an electrostatic casting method, cooled and solidified to produce an unstretched film.
[0085] Next, the P1 coating solution was applied to one side of the unstretched PET film, and the P2 coating solution was applied to the other side, both in a coating amount of 0.12 g / m2 after drying. 2 After coating so that the coating was applied, the coating was introduced into a dryer and dried at 80° C. for 20 seconds.
[0086] The unstretched film with the coating layer formed thereon was introduced into a tenter stretching machine, and while the ends of the film were held with clips, the film was introduced into a hot air zone at a temperature of 135°C and stretched 4.0 times in the width direction. Next, while maintaining the width stretched in the width direction, the film was treated at a temperature of 225°C for 30 seconds, and then cooled to 130°C. Both ends of the film were cut with a shear blade and stretched at 0.5 kg / mm 2 The edges were cut off under a tension of 0.01 mm and then wound up to obtain uniaxially oriented PET film A with a film thickness of 70 μm. The intrinsic viscosity of the entire film was 0.65 dL / g. The obtained film A was slit into a width of 1300 mm, knurled on both ends, and wound up with the knurled surface facing outward to obtain a roll with a length of 3500 m. The roll was placed in a polyethylene bag, the opening tied with rubber, and side plates larger than the outer diameter of the roll were fitted to both ends of the core, and stored at 25°C.
[0087] (Production of Film B) Film B was produced in the same manner as Film A, except that the P1 coating liquid was not applied (the P2 coating liquid was applied to one side) and the thickness was 50 μm. Film B was then slit and knurled in the same manner to obtain a roll.
[0088] (Knurl processing) The knurling process was performed by passing both ends of the slit film between a knurled upper roll and a mirror-finished lower roll, and the height of the knurled part was adjusted by adjusting the pressure of the upper roll. The width of the knurling process was adjusted by changing the thickness of the lower roll. The knurling was heated by induction heating. Distance between the knurled part and the end of the film: 3 mm Knurling speed: 185m / min
[0089] (Knurling) The knurling is a disk 20 mm thick and 100 mm in diameter, with the following 10 protrusions arranged on the outer surface at a 45 degree angle over a length of 10 mm (10 x 10 protrusions for a 10 mm x 10 mm area).
[0090] Knurled protrusion shape Square pyramid type A: Base length 1000μm×1000μm, height 900μm Square pyramid type B: Base length 1000μm×1000μm, height 330μm Square pyramid type: Square pyramid type A polished to a height of 600 μm
[0091] Examples 1 to 11, Comparative Examples 1 to 7 The results of knurling under various conditions using film A and film B are shown in Tables 1 and 2 as examples and comparative examples. Film A and film B were coated as follows. Two rolls of film were prepared under the same conditions, one of which was used to measure the knurl height and unwinding charge amount, and to evaluate the roll winding state, and the other was used to evaluate the coating of the coating liquid. The winding tension in Tables 1 and 2 is the tension when the film is wound into a roll around a cylindrical core after knurling on both ends of the film. The winding contact pressure is the winding contact pressure of the touch roll, which was pressed against the film during winding.
[0092] The roll of film A was unwound, and a coating solution for an antiglare layer having the following composition was applied to the surface of the easy-adhesion layer P2 using a gravure coater. The coating was then dried in an oven at 90°C, and then irradiated with ultraviolet light to harden the coating, thereby providing an antiglare layer as a second coating layer. (Composition of coating solution for antiglare layer) KAYARAD PET-30 (manufactured by Nippon Kayaku Co., Ltd.) 38.7 parts by weight Viscoat #360 Osaka Organic Chemical Industry Co., Ltd. 9.7 parts by weight Eposter MA1006, manufactured by Nippon Shokubai Co., Ltd. 0.1 parts by weight Irgacure 184 1.5 parts by weight Methyl isobutyl ketone 30.0 parts by mass Methyl ethyl ketone 20.0 parts by mass Fluorosurfactant 0.02 parts by mass
[0093] (Coating uniformity evaluation of film A) The state of the antiglare layer in a portion of Film A that was 100 m to 150 m from the beginning of winding was observed to evaluate the coating uniformity. ◎: There were no irregularities and it was uniform within 50m. ○: There were several places within 50m that appeared to have slight unevenness or craters. △: There were several places within 50m where unevenness or cratering was clearly observed. ×: Frequent unevenness or cissing was observed within 50 m.
[0094] The roll of film B was unwound, and a coating solution for a photo-alignment layer having the following composition was applied to the surface not provided with an easy-adhesion layer using a gravure coater, and after drying at 80°C, a coating film with a thickness of 150 nm was formed. Subsequently, polarized UV light was irradiated to obtain film B having a photo-alignment layer laminated thereon as a second coating layer. The polarization direction of the UV light was set at 45 degrees to the longitudinal direction of film B. (Coating liquid for photo alignment layer) Based on the descriptions in Examples 1, 2, and 3 of JP2013-33248A, a 5% by mass solution of a polymer represented by the following formula (1) in cyclopentanone was prepared.
[0095] 5 parts by mass of polymer represented by formula (1) [ka] Surfactant 0.1 parts by weight Cyclopentanone 95 parts by mass
[0096] (Forming of alignment layer of alignment liquid crystal compound) Subsequently, a coating solution for forming an aligned liquid crystal compound layer having the following composition was applied to the photoalignment layer surface by a bar coating method, dried at 110°C for 3 minutes, and cured by irradiating with ultraviolet light to form an aligned liquid crystal compound layer (λ / 4 retardation layer) as a second coating layer on the film. (Coating solution for forming alignment liquid crystal compound layer) Rod-shaped liquid crystal compound (BASF LC242) 95 parts by weight Trimethylolpropane triacrylate 5 parts by weight Irgacure 379 3 parts by weight Surfactant 0.1 parts by weight Methyl ethyl ketone 250 parts by mass
[0097] (Coating uniformity evaluation of film B) The state of the λ / 4 retardation layer was observed in a section 100m to 150m from the beginning of the roll of Film B. The observation was carried out in a room where a fluorescent LED was installed on the ceiling as a lighting fixture, Film B with the λ / 4 retardation layer laminated thereon was placed on an aluminum plate with a mirror surface so that the λ / 4 retardation layer surface was facing down, and a polarizing plate was placed on top of it so that the longitudinal direction of Film B was parallel to the extinction axis direction (absorption axis direction) of the polarizing plate, and the uniformity of the anti-reflection as a circular polarizing plate was observed from above to evaluate the coating uniformity. ◎: There were no irregularities within 50m, and the anti-reflection condition was uniform. ○: There were several places within 50m where the anti-reflection condition was slightly deteriorated. △: There were several places within 50m where the anti-reflection condition was clearly degraded. ×: There were frequent locations within 50 m where the anti-reflection condition was degraded.
[0098] [Table 1]
[0099] [Table 2] [Industrial Applicability]
[0100] The long film of the present invention wound into a roll has a small amount of electrostatic charge when the film is unwound all the way to the core, and when the film is coated, for example, the coating film has little repelling and can be provided with a coating film with excellent thickness accuracy all the way to the end of the film. Furthermore, the long resin film of the present invention is suppressed from shifting during winding and wrinkling after storage or transportation, has no scratches on the film surface, and has excellent flatness.
Claims
1. A long resin film wound into a roll, Both ends of the film width are knurled. When the observer faces the roll and unwinds the film from the top of the roll toward the observer, The knurl at the right end is the right knurl, The knurl at the left end is the left knurl, The height of the knurl at the core of the right knurl is Hnbr, The height of the left knurl at the core is Hnbl, The height of the surface of the right knurl is Hner, The height of the surface layer of the left knurl is Hnel, The core portion is a portion 100 m from the start of winding of the film wound into a roll, and the surface portion is a portion 100 m from the end of winding of the film wound into a roll, A long resin film that satisfies the following conditions (1) to (3). (1) Both Hnbr and Hnbl are 0.5 to 4 μm. (2) Both Hnbr / Hner and Hnbl / Hnel are 0.3 to 0.9 (3) Both Hner and Hnel are 1.2 to 6 μm.
2. 2. The long resin film according to claim 1, wherein the absolute value of the uniformity of the knurl heights on the left and right sides of the core portion, calculated by |(Hnbr-Hnbl) / [(Hnbr+Hnbl) / 2]|, is 0.3 or less.
3. 3. The long resin film according to claim 1, wherein the outer surface of the long resin film is surface A and the inner surface of the long resin film is surface B, and the compositions of surface A and surface B are different.
4. A long resin film according to any one of claims 1 to 3, wherein when the outer surface of the long resin film is surface A and the inner surface of the long resin film is surface B, at least one of surface A and surface B is the surface of the first coating layer.
5. The long resin film according to any one of claims 1 to 4, which is a stretched polyester film.
6. A laminated film comprising the long resin film according to any one of claims 1 to 5 and a second coating layer provided on at least one surface of the long resin film.
7. The laminate film according to claim 6 , wherein the second coating layer is a hard coating layer, an antiglare layer, an antireflection layer, a low reflection layer, an alignment layer, or a retardation layer.
8. The laminate film according to claim 6 or 7, which is a polarizer protective film or a thin film layer transfer film.
9. A method for producing a laminated film, comprising: a step (A) of unwinding a long resin film according to any one of claims 1 to 5; and a step (B) of applying a coating liquid for a second coating layer to at least one side of the unwound long resin film.
10. The method for producing a laminated film according to claim 9 , wherein the laminated film is a polarizer protective film.
11. The method for producing a laminated film according to claim 9, wherein the laminated film is a film for thin film layer transfer.
Citation Information
Patent Citations
Method of winding up film
JP1988074850A
Cellulose acylate film and solution film forming method
JP2005104148A
Knurling roller, apparatus, method of manufacturing film roll, and optical film
JP2013166317A
Wound body of thermoplastic resin film and method for manufacturing the same
JP2014108849A
Method for manufacturing taken-up body of optical film
JP2014126822A