Solution containing lithium and niobium, method for producing same, and method for producing active material for lithium secondary battery
A lithium and niobium solution with controlled particle size and concentration is used to coat the positive electrode active material, addressing interfacial resistance issues in all-solid lithium batteries by forming a uniform lithium niobate coating, thus improving battery performance.
Patent Information
- Application Number
- JP2020192199
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-11-19
AI Technical Summary
The increase in interfacial resistance between the positive electrode active material and the solid electrolyte in all-solid lithium batteries due to the presence of fine particles with a particle size exceeding 500 nm and uneven niobium distribution, which impedes effective contact and reduces battery performance.
A solution containing lithium and niobium with a particle size distribution of 500 nm or less, preferably 30 nm or less, and a niobium concentration between 1% to 15% by mass, with a molar ratio of lithium to niobium between 0.9 and 1.4, and optionally including additional elements like Ta, F, La, P, B, Ti, Zr, W, Al, Zn, Si, Ge, and V, is used to coat the positive electrode active material, followed by filtration and heat treatment to form a uniform lithium niobate coating layer.
The solution effectively reduces interfacial resistance by minimizing the presence of fine particles and ensuring uniform niobium distribution, thereby enhancing the performance of lithium secondary batteries.
Smart Images

Figure 0007593792000001 
Figure 0007593792000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a solution containing lithium and niobium, an active material for a lithium secondary battery, and a method for producing the same. [Background technology]
[0002] Lithium-ion secondary batteries have the characteristics of high energy density and the ability to operate at high voltages. Therefore, they are used in information devices such as mobile phones as secondary batteries that are easy to make small and lightweight. In recent years, there has also been an increasing demand for them as secondary batteries for large power sources such as hybrid automobiles.
[0003] In lithium ion secondary batteries, non-aqueous electrolytes in which salts are dissolved in organic solvents are generally used as electrolytes. However, since the non-aqueous electrolytes are flammable, lithium ion secondary batteries need to solve safety problems. In order to ensure the safety, measures such as incorporating safety devices into lithium ion secondary batteries have been implemented. In addition, as a more fundamental solution, a method has been proposed in which the electrolyte is made non-flammable, that is, a solid electrolyte is used as the lithium ion conductor to make an all-solid-state lithium battery.
[0004] Generally, the electrode reaction of a battery occurs at the interface between the electrode active material and the electrolyte. When a liquid electrolyte is used as the electrolyte, the liquid electrolyte penetrates between the active material particles by immersing an electrode containing an electrode active material in the liquid electrolyte, and a reaction interface is formed. On the other hand, when a solid electrolyte is used as the electrolyte, since the solid electrolyte does not have a mechanism for penetrating between the active material particles, it is necessary to mix a powder containing the electrode active material particles with a powder of the solid electrolyte in advance. For this reason, the positive electrode of an all-solid-state lithium battery is usually a mixture of a powder of the positive electrode active material and a solid electrolyte.
[0005] However, in all-solid-state lithium batteries, the resistance that occurs when lithium ions move across the interface between the positive electrode active material and the solid electrolyte (hereinafter, may be referred to as "interface resistance") tends to increase. When the interface resistance increases, the performance of the all-solid-state lithium battery, such as the battery capacity, decreases.
[0006] Here, it has been reported (Non-Patent Document 1) that the increase in the interface resistance is caused by the reaction between the positive electrode active material and the solid electrolyte, resulting in the formation of high resistance sites on the surface of the positive electrode active material. Non-Patent Document 1 discloses a proposal to reduce the interface resistance by covering the surface of lithium cobalt oxide, which is a positive electrode active material, with lithium niobate, which is a lithium ion conductor, thereby improving the performance of all-solid-state lithium batteries.
[0007] As a method for coating a positive electrode active material such as lithium cobalt oxide with lithium niobate, the present applicant has disclosed in Patent Document 1 that a solution containing lithium and a niobium complex is used as a coating solution to coat the positive electrode active material. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2012-74240 A [Non-patent literature]
[0009] [Non-Patent Document 1] Electrochemistry Communications, 9(2007), p.1486-1490 Summary of the Invention [Problem to be solved by the invention]
[0010] On the other hand, there is an increasing demand in the market for further reducing the interfacial resistance between the positive electrode active material and the solid electrolyte. In response to the demands of the market, the present inventors have continued their research and found that, between the positive electrode active material and the solid electrolyte, in a solution containing lithium and niobium that coats the positive electrode active material, there may be fine particles having a 90% cumulative particle size (D90) based on the light scattering intensity standard measured by the dynamic light scattering method of the solution exceeding 500 nm and having a high niobium concentration. When the fine particles having a D90 exceeding 500 nm and a high niobium concentration are present in the coating of lithium niobate that coats the positive electrode active material, a niobium uneven distribution region is generated in a part of the lithium niobate. As a result, it was considered that the value of the interface resistance between the positive electrode active material and the solid electrolyte is increased.
[0011] The present invention has been made based on the above-mentioned findings and considerations, and the problem to be solved by the present invention is to provide a solution containing lithium and niobium, in which the presence of fine particles between a positive electrode active material and a solid electrolyte is reduced, and a method for producing the same. [Means for solving the problem]
[0012] That is, the first invention for solving the above-mentioned problems is: A solution containing lithium and niobium, The solution contains lithium and niobium, and has a D90 of 500 nm or less, which is a light scattering intensity standard measured by a dynamic light scattering method. The second invention is A solution containing lithium and niobium, The solution contains lithium and niobium and has a D90 of 30 nm or less, which is a light scattering intensity standard measured by a dynamic light scattering method. The third invention is In the solution containing lithium and niobium according to the first or second invention, a niobium concentration of the solution containing lithium and niobium is 1% by mass or more and 15% by mass or less. The fourth invention is The solution containing lithium and niobium according to any one of the first to third aspects of the present invention, wherein the molar ratio of lithium to 1 mole of niobium (Li / Nb) in the solution containing lithium and niobium is 0.9 or more and 1.4 or less. The fifth invention is The solution containing lithium and niobium according to any one of the first to fourth aspects of the present invention is added to the solution containing lithium and niobium, and the solution has a loading index value of 0.15 or less, which is obtained by measuring the solution by frequency analysis using a heterodyne method as a dynamic light scattering method. The sixth invention is The solution containing lithium and niobium according to any one of the first to fifth aspects of the present invention is a solution containing lithium and niobium further containing an M element (wherein the M element is one or more elements selected from Ta, F, La, P, B, Ti, Zr, W, Al, Zn, Si, Ge, and V). The seventh invention is The solution containing lithium and niobium according to any one of the first to sixth aspects of the present invention, wherein the niobium is a niobium complex. The eighth invention is The method for producing a solution containing lithium and niobium includes a step of filtering the solution containing lithium and niobium using a filter having a filter pore size of 500 nm or less to obtain a solution containing lithium and niobium having a D90 of 500 nm or less, which is a light scattering intensity standard measured by dynamic light scattering of the solution. The ninth invention is The method for producing a solution containing lithium and niobium includes a step of filtering the solution containing lithium and niobium using a filter having a filter pore size of 30 nm or less to obtain a solution containing lithium and niobium having a D90 of 30 nm or less, which is a light scattering intensity standard measured by dynamic light scattering of the solution. The tenth invention is The method for producing a solution containing lithium and niobium according to the eighth or ninth invention, wherein the filtration is cross-flow filtration. The eleventh invention is The method for producing a solution containing lithium and niobium according to any one of the eighth to tenth aspects of the present invention, wherein the temperature of the solution containing lithium and niobium is maintained at 40° C. or lower during the filtration. The twelfth invention is The method for producing a solution containing lithium and niobium according to any one of the eighth to eleventh aspects of the present invention uses a niobium complex as the niobium. The thirteenth invention is The active material for lithium secondary batteries has a coating layer of lithium niobate on its surface, the active material being formed using a solution containing lithium and niobium according to any one of the first to seventh aspects of the present invention. The fourteenth invention is A step of performing a coating treatment on a surface of an active material for a lithium secondary battery using a solution containing lithium and niobium according to any one of the first to seventh aspects of the present invention; and heat-treating the coated active material for lithium secondary batteries. Effect of the Invention
[0013] According to the present invention, it is possible to provide a solution containing lithium and niobium, which can reduce the presence of fine particles that cause an increase in the interfacial resistance between a positive electrode active material and a solid electrolyte, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In recent years, in the field of lithium ion secondary batteries, research and development of all-solid-state lithium batteries using a solid electrolyte with lithium ion conductivity has been actively conducted on the market. Furthermore, there is an increasing demand from the development sites of the all-solid-state lithium batteries for further reducing the interface resistance between the positive electrode active material and the solid electrolyte.
[0015] In response to this market demand, the inventors have conducted extensive research and discovered that fine particles may be present at the interface between the positive electrode active material and the solid electrolyte. The inventors have continued their research and have concluded that the fine particles prevent contact between the positive electrode active material and the solid electrolyte, thereby increasing the interfacial resistance.
[0016] Based on the above findings and considerations, the present inventors have conducted research into the cause of the generation of fine particles present at the interface between the positive electrode active material and the solid electrolyte. Then, they focused on a solution containing lithium and niobium according to the prior art, which was considered to be a solution in which solids were dissolved, because the appearance was transparent when observed with the naked eye and the absorbance of light at a wavelength of 660 nm using a transmitted light measurement method was low at 0.15 or less. The solution was then measured using DLS (dynamic light scattering). As a result, it was found that fine particles with a particle size exceeding 500 nm existed in the solution when the value of the 90% cumulative particle size based on the light scattering intensity of the DLS measurement was taken as D90.
[0017] In this way, when a positive electrode material is coated with a solution containing lithium and niobium including fine particles having a particle size exceeding 500 nm in D90, the light scattering intensity standard of DLS measurement, the coating layer present at the interface between the positive electrode active material and the solid electrolyte will have thick and thin locations.
[0018] Furthermore, the inventors found that fine particles having a particle size exceeding 500 nm in the D90 may be fine particles having a high niobium concentration. As a result, the inventors found that the presence of fine particles having a particle size exceeding 500 nm in the coating layer at the interface between the positive electrode active material and the solid electrolyte results in the generation of an unevenly distributed region of niobium, which causes an increase in the interface resistance at the contact interface between the positive electrode material and the solid electrolyte.
[0019] As a result of further research based on the findings described above, the inventors came up with a configuration in which the above-mentioned solution containing lithium and niobium is filtered to obtain a solution containing lithium and niobium having a particle size of 500 nm or less in D90, a light scattering intensity standard measured by dynamic light scattering of the solution.The inventors then came up with the idea that the use of a solution containing lithium and niobium that satisfies the above configuration contributes to reducing the interface resistance at the contact interface between the positive electrode material and the solid electrolyte.
[0020] As a result of further research, the inventors have also come to the conclusion that by setting the particle size of the microparticles to 30 nm or less in D90, the light scattering intensity standard of DLS measurement, it is possible to form a uniform film thickness in the positive electrode material regardless of the presence of the microparticles, and to suppress or reduce areas of uneven distribution of niobium.
[0021] Hereinafter, embodiments for carrying out the present invention will be described in the following order: 1. A solution containing lithium and niobium, 2. A method for producing a solution containing lithium and niobium, and 3. An active material for a lithium secondary battery and a method for producing the same.
[0022] 1. Solutions containing lithium and niobium The solution containing lithium and niobium according to the present invention is a solution containing lithium and niobium, and has a particle size D90 based on the light scattering intensity measured by a dynamic light scattering method of 500 nm or less, preferably 200 nm or less, more preferably 30 nm or less, and most preferably 10 nm or less. When a positive electrode material is coated with the solution containing lithium and niobium according to the present invention, no fine particles with a particle size exceeding 500 nm, which would lead to the generation of an unevenly distributed region of niobium, are present at the interface between the positive electrode material and the solid electrolyte, and the cause of an increase in interfacial resistance at the interface between the positive electrode material and the solid electrolyte can be suppressed. The solution containing lithium and niobium according to the present invention has an absorbance of 0.15 or less at a wavelength of 660 nm when measured by a transmitted light measurement method. The light absorbance is an index of the amount of solids remaining without being dissolved. A solution having a light absorbance of 0.15 or less has a small amount of solids remaining without being dissolved, and can be used as a solution for forming lithium niobate as a coating layer on the surface of a positive electrode active material described later.
[0023] In the solution containing lithium and niobium according to the present invention, the niobium concentration is preferably 1% by mass or more and 15% by mass or less. When the niobium concentration is 15% by mass or less, the stability of the niobium compound in the solution containing lithium and the niobium compound is ensured, and the storage stability is also ensured. From this viewpoint, the niobium concentration is more preferably 10% by mass or less. On the other hand, if the niobium concentration is 1 mass% or more, it is advantageous in terms of cost due to reduced transportation / storage costs. From this viewpoint, the niobium concentration is more preferably 2 mass% or more, and further preferably 3 mass% or more. In the present invention, the term "niobium concentration" means "the concentration of niobium element in a solution containing lithium and niobium." The procedure for measuring the niobium concentration will be described in Comparative Example 1 below.
[0024] In the solution containing lithium and niobium according to the present invention, the number of moles of lithium can be set arbitrarily relative to the number of moles of niobium contained in the solution. However, if the amount of lithium is too small relative to the amount of niobium, when lithium niobate represented by LiNbO3 is formed as a coating layer of the positive electrode active material, the lithium conductivity of the coating layer may decrease. Also, if the amount of lithium is too large relative to the amount of niobium, non-conductive lithium hydroxide or lithium nitrite may be mixed into the lithium niobate coating layer, which may decrease the conductivity of the coating layer. Therefore, it is preferable that the molar ratio of lithium to 1 mole of niobium (Li / Nb) in the solution containing lithium and niobium is 0.9 or more and 1.4 or less.
[0025] The solution containing lithium and niobium according to the present invention may further contain an M element (wherein the M element is one or more elements selected from Ta, F, La, P, B, Ti, Zr, W, Al, Zn, Si, Ge, and V). However, the content of the M element in the solution containing lithium and niobium is In terms of molar ratio, Li / (Nb+M)=0.9 or more and 1.4 or less; And, in terms of mass%, M / (Nb+M)=0.01 mass% or more and 10.0 mass% or less By setting the content of the M element in the solution containing lithium and niobium within this range, it may be possible to realize a reduction in the interface resistance and a suppression of an increase in the interface resistance.
[0026] In the solution containing lithium and niobium according to the present invention, when DLS is measured using a DLS measurement device, the loading index value obtained at the same time is preferably 0.15 or less. In the present invention, the "loading index value obtained during DLS measurement" refers to a value calculated simultaneously with the DLS value calculated from the total amount of scattered light when a solution containing lithium and niobium as a sample is irradiated with laser light using a DLS measurement device. In the case of the solution containing lithium and niobium according to the present invention, if the solution contains fine particles, it is considered that the solution scatters laser light. From this viewpoint, if the loading index value obtained in DLS measurement is 0.15 or less, the content of fine particles in the solution is sufficiently low, and the solution containing lithium and niobium according to the present invention can be suitably used.
[0027] 2. Method for producing a solution containing lithium and niobium The solution containing lithium and niobium according to the present invention can be obtained by mixing a solution containing a niobium compound, a lithium compound, and an alkali. The present inventors believe that the solution containing lithium and niobium is produced, for example, as represented by the following formulas 1 and 2. Nb2O5·3H2O+8H2O2+6NH3→2(NH4)3[Nb(O2)4]+8H2O···(Formula 1) 2(NH4)3[Nb(O2)4]+2LiOH+H2O→2Li[Nb(O2)3]·2H2O+6NH3+H2O+O2···(Formula 2)
[0028] The method for producing a solution containing lithium and niobium according to the present invention will be described in the following order: (1) solvent, (2) lithium compound, (3) niobium compound, (4) M element compound, and (5) method for producing a solution containing lithium and niobium.
[0029] (1) Solvent As the solvent, various solvents can be used, however, taking into consideration the raw material cost, environmental load, workability, etc., water is preferred.
[0030] (2) Lithium compounds There are no particular limitations on the lithium compound, so long as it dissolves in the solvent used. Of course, if water is used as the solvent, suitable examples include lithium salts such as lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), lithium carbonate, and lithium nitrite, with lithium hydroxide being preferred from the viewpoint of not introducing impurities into the solution.
[0031] (3) Niobium compounds The niobium compound is not particularly limited as long as it is soluble in the solvent used. However, a niobium complex compound (sometimes referred to as a niobium complex in the present invention) is preferred from the viewpoint of being stably dissolved in various solvents. However, when water is used as the solvent, preferred examples include niobium oxalate and various water-soluble niobium complexes. Among them, the peroxo complex of niobic acid ([Nb(O2)4]) is a water-soluble niobium complex. 3-The peroxo complex of niobic acid is particularly suitable because it does not contain carbon in its chemical structure and therefore no carbon remains in the coating film of lithium niobate that is finally produced.
[0032] (4)M element compound When adding the M element to the solution containing lithium and niobium according to the present invention, there are no particular limitations as long as it is a salt of the M element and is soluble in the solvent used. However, if water is used as the solvent, the preferred salts are the same as those explained in "(2) Lithium Compounds." If there is no suitable water-soluble salt, the M element may be added as a complex as explained in "(3) Niobium Compounds."
[0033] On the other hand, the peroxo complex in a solution containing lithium and niobium can be identified by measuring using the single reflection ATR method of FT-IR with an incident angle to a germanium prism of 45°. As a result of the measurement, 855 cm assigned to the peroxo complex was -1 ±20cm -1 and 1650cm -1 ±10cm -1 If a peak is confirmed at 1000 nm, it is believed that the niobium dissolved in the solution containing lithium and a niobium compound is in the form of a niobium complex (specifically, a peroxo complex).
[0034] (5) A method for producing a solution containing lithium and niobium The method for producing the solution containing lithium and niobium is not particularly limited. As an example of the method, a method for producing an aqueous solution containing lithium and a niobium complex will be described in the order of <1> a niobium dissolving step, <2> a lithium dissolving step, and <3> a filtration step.
[0035] <1> Niobium melting process The niobium dissolution process involves adding niobic acid (Nb2O5·nH2O) to, for example, hydrogen peroxide water and mixing it to form a niobium peroxo complex as a niobium compound.
[0036] When a niobium peroxo complex is used as the niobium complex, the molar ratio of hydrogen peroxide to 1 mole of niobium is preferably 4 moles or more during the above mixing. On the other hand, even if the molar ratio of hydrogen peroxide to 1 mole of niobium exceeds 30 moles, the effect is considered to be saturated. Therefore, the molar ratio of hydrogen peroxide to 1 mole of niobium is preferably 20 moles or less, and more preferably 15 moles or less. Furthermore, when niobic acid is added to and mixed with hydrogen peroxide, the liquid temperature of the hydrogen peroxide is preferably 0° C. or higher and 60° C. or lower in order to avoid decomposition of the hydrogen peroxide. In this mixing, although niobic acid does not dissolve in hydrogen peroxide water, a milky suspension containing niobic acid can be obtained.
[0037] By adding an alkali such as aqueous ammonia to a suspension containing niobic acid and mixing it, a transparent solution containing a peroxo complex of niobium can be obtained. When aqueous ammonia is added as an alkali to a suspension containing niobic acid, it is preferable to add it so that the molar ratio of ammonia to 1 mole of niobium (ammonia / Nb) is 3 or more. On the other hand, it is believed that the effect becomes saturated even if the molar ratio of ammonia to 1 mole of niobium exceeds 8 moles, and therefore it is preferable to set the molar ratio of ammonia to 1 mole of niobium to 6 moles or less. Furthermore, when an alkali such as ammonia water is added to and mixed with the suspension containing niobic acid, the liquid temperature of the ammonia water or the like is preferably 0° C. or higher and 60° C. or lower in order to avoid volatilization of ammonia.
[0038] Furthermore, in addition to the ammonia water, an alkaline aqueous solution can be added. In this case, the amount of the alkaline aqueous solution added is such that the pH value of the aqueous solution after the addition is 10 or more, preferably 11 or more. It is a preferred configuration to add a lithium hydroxide aqueous solution as the alkaline aqueous solution.
[0039] <2> Lithium dissolving process In the lithium dissolving step, a lithium compound is added to the solution containing the niobium complex obtained in the "<1> niobium dissolving step" under an inert gas or air atmosphere, and the solution containing lithium and the niobium complex is obtained by dissolving the lithium compound. The mole number of lithium in the lithium compound to be added can be set arbitrarily with respect to the mole number of niobium in the niobium complex contained in the solution. However, if the amount of lithium is too small relative to the amount of niobium, when lithium niobate represented by LiNbO3 is formed as a coating layer of the positive electrode active material, the lithium conductivity of the coating layer may be reduced. In addition, if the amount of lithium is excessive relative to the amount of niobium, non-conductive lithium hydroxide or lithium nitrite may be mixed into the lithium niobate coating layer, which may reduce the conductivity of the coating layer. Therefore, it is preferable that the molar ratio of lithium to 1 mole of niobium (Li / Nb) is 0.9 or more and 1.4 or less. As the inert gas atmosphere, a nitrogen gas atmosphere is convenient.
[0040] <3> Filtration process This is a process in which an aqueous solution containing lithium and a niobium complex, obtained by carrying out the above-described <1> niobium dissolving step and <2> lithium dissolving step, is filtered to obtain an aqueous solution containing lithium ions and a niobium complex, the aqueous solution having a light scattering intensity standard D90 of 500 nm or less as measured by a dynamic light scattering method.
[0041] The filtration method is not particularly limited, and may be a centrifugation method, a filtration method using various filters, etc., but from the viewpoint of the efficiency of removing fine particles and productivity, pressure filtration using pressure and a filter in combination, or microfiltration or ultrafiltration using pressure and a filter having a fine pore size in combination are preferred. In addition, the filtration method includes dead-end filtration and cross-flow filtration, but cross-flow filtration is preferred because it has a high filtration speed and can process a large amount at one time. The liquid temperature during filtration is preferably 10° C. or higher and 40° C. or lower in terms of filtration productivity and stability of the niobium complex in the solution. If the liquid temperature is 10° C. or higher, the viscosity of the solution decreases and the filtration rate is ensured. If the liquid temperature is 40° C. or lower, the stability of the niobium complex is ensured.
[0042] The pore size of the filter is 500 nm or less from the viewpoints of fine particle removal efficiency and productivity. When a solution containing a lithium and niobium complex having a D90 of 30 nm or less is desired, the pore size is preferably 1 nm or more and 30 nm or less, more preferably 10 nm or more and 25 nm or less. The pressure applied during filtration is preferably 0.05 MPa or more and 0.6 MPa or less, and more preferably 0.1 MPa or more and 0.4 MPa or less, from the viewpoints of fine particle removal efficiency and productivity. When cross-flow filtration is performed, the flow rate of the solution is preferably 0.5 m / s or more and 5 m / s or less, and more preferably 1 m / s or more and 3 m / s or less. When cross-flow filtration is performed under the above favorable conditions, the filtration rate of the solution is 1 kg / m 2 ·hr or more, 100kg / m 2 Approximately 1 / hr or less.
[0043] Furthermore, the solid matter remaining on the filter after filtration was dried and subjected to elemental analysis using ICP. It was found that the solid matter contained lithium and niobium with a Li / Nb molar ratio of about 0.5, and was a solid oxide with an excess of niobium, which was thought to be the cause of the fine particles present between the positive electrode active material and the solid electrolyte.
[0044] On the other hand, when the IR spectrum of the aqueous solution containing the lithium and niobium complex was measured using the single reflection ATR method of FT-IR before and after the filtration step, it was confirmed that there was no change in the IR spectrum before and after filtration.
[0045] 3. Active material for lithium secondary batteries and its manufacturing method The above-described solution containing lithium and niobium is used as a solution for forming a coating layer containing lithium niobate, and a coating treatment is performed on the surface of the active material for lithium secondary batteries.Then, by subjecting the coated active material to a heat treatment, it is possible to manufacture an active material for lithium secondary batteries having a coating layer containing lithium niobate.The thickness of the coating layer that coats the surface of the active material for lithium secondary batteries is preferably 1 nm to 30 nm.
[0046] The method for producing an active material for lithium secondary batteries having a coating layer containing lithium niobate according to the present invention will be described in the following order: (1) the active material for lithium secondary batteries, (2) a coating treatment on the surface of the active material for lithium secondary batteries using a solution containing lithium and niobium, and (3) a heat treatment of the coated active material for lithium secondary batteries.
[0047] (1) Active materials for lithium secondary batteries The active material for lithium secondary batteries is not particularly limited, but lithium cobalt oxide (LiC Lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO4), and active materials in which some of the transition metals in these active materials have been replaced with Al, Ti, Cr, Fe, Zr, Y, W, Ta, or Nb (for example, LiNi 0.95 Al 0.05 O2, etc.), and active materials that combine these active materials (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.5 Mn 1.5 O4, etc., can be preferably used.
[0048] (2) Coating the surface of an active material for a lithium secondary battery using a solution containing lithium and niobium The method for coating the surface of the active material for lithium secondary batteries with the solution containing lithium and niobium according to the present invention is not particularly limited, although a preferred coating method is to spray and coat the solution containing lithium and niobium on the powder of the active material for lithium secondary batteries while heating it to about 100°C to 120°C. There is also a method of coating the active material powder for lithium secondary batteries by immersing it in a solution containing lithium and niobium.
[0049] (3) Heat treatment of the coated active material for lithium secondary batteries When the above-mentioned coated active material for lithium secondary batteries is used as a positive electrode material for a lithium ion battery, in order to avoid adverse effects on the battery characteristics, the coated active material for lithium secondary batteries is subjected to an appropriate heat treatment for the purpose of decomposing and removing components containing elements such as N (nitrogen) present in the coating layer. Specifically, the coated active material for lithium secondary batteries may be heat-treated, for example, in air at 120° C. to 350° C. for 1 hour to 10 hours. The heat treatment can produce the active material for lithium secondary batteries having a coating layer containing lithium niobate according to the present invention. EXAMPLES
[0050] The lithium- and niobium-containing solution according to the present invention and the method for producing the same will be specifically described below with reference to examples.
[0051] Comparative Example 1 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5, content 72.6% by mass)) was added to 74.6 g of hydrogen peroxide solution with a concentration of 30% by mass. After the addition of niobic acid, the temperature of the solution to which niobic acid had been added was adjusted to be within the range of 20°C to 30°C. 12.3 g of ammonia water with a concentration of 28% by mass was added to the temperature-adjusted solution, and the solution was thoroughly stirred to obtain a transparent solution. In the transparent solution, the molar ratio of hydrogen peroxide to 1 mole of niobium (hydrogen peroxide / Nb) was 14, and the molar ratio of ammonia to 1 mole of niobium (ammonia / Nb) was 4.3.
[0052] Next, in a nitrogen gas atmosphere, 1.08 g of lithium hydroxide monohydrate (LiOH·H2O) was added to the obtained transparent solution to obtain a transparent solution containing lithium and a niobium peroxo complex. While stirring the obtained solution containing lithium and a niobium peroxo complex, 2.79 g of a 40% lithium nitrite aqueous solution (LiNO2) was added to obtain a solution containing lithium and niobium according to Comparative Example 1. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 1 described above.
[0053] For the obtained solution containing lithium and niobium according to Comparative Example 1, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2.
[0054] The presence or absence of the niobium complex was determined by the single reflection ATR method of FT-IR. Specifically, the FT-IR device NICOLE T6700 manufactured by Thermo Fisher Scientific and the single reflection ATR accessory Smart OMNI-Sampler (germanium crystal, incident angle 45°) were used, with the number of scans being 16 and the resolution being 4 cm. -1The measurements were performed under the following conditions. In order to remove the low wavenumber peaks of the water solvent, ion-exchanged water with a conductivity of 1 mS / m or less was used for background measurements. The measured peaks were subjected to auto-baseline correction using the analysis software (OMNIC Specta) attached to the NICOLE T6700 FT-IR device, followed by one auto-smoothing step and peak detection at a sensitivity of 50. As a result, the peak at 855 cm assigned to the niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed at 1000 nm, it was determined that the solution contained a niobium complex.
[0055] The particle size distribution was measured by light scattering intensity distribution measurement in accordance with JISZ8828:2019, using frequency analysis with the heterodyne method of dynamic light scattering, and the loading index value was also measured at the same time. Specifically, the Nanotrac WaveII UT151 manufactured by Microtrack Bell Corporation was used, and the measurement was performed under the following measurement conditions. <Measurement conditions> ·time SetZero Time: 60 seconds Measurement time: 120 seconds Number of measurements: 1 Particle conditions Transparency: transparent Particle refractive index: 2.25 Shape: Non-spherical Solvent conditions Solvent Water Solvent refractive index 1.333 Viscosity Viscosity at high temperature 30℃ 0.797cp(0.797mPa·s) Viscosity at low temperature 20℃ 1.002cp(1.002mPa·s) Filter Stand:Norm Sensitivity Standard Nano range correction disabled Mono Disperse Mode Disabled Advanced Filter Disabled For the solutions in this example and the comparative example, the solid matter concentration was low, so the light scattering and reflected light amount were in the low range. Therefore, a Setzero measurement using pure water was performed for each sample measurement, and measurements were performed after confirming that no error message was displayed on the measuring device.
[0056] The 10% particle size based on the light scattering intensity standard was defined as D10, the 50% particle size as D50, and the 90% particle size as D90. When the D10, D50, and D90 values were measured, the results were D10 was 44.1 nm, D50 was 228.7 nm, and D90 was 521.0 nm, indicating that D90 did not satisfy the requirement of 500 nm or less. On the other hand, the loading index value was read as 0.563, which did not satisfy the requirement of 0.15 or less.
[0057] The lithium concentration was measured using ICP-OES. Specifically, 0.1 g of the solution containing lithium and niobium according to Comparative Example 1 was taken, and 5 ml of hydrochloric acid and 15 ml of pure water were added. Then, 2 ml of hydrogen peroxide was added to dissolve the lithium to obtain a solution. Pure water was added to the obtained solution to make the volume constant to 100 ml, and the lithium concentration was measured using an ICP-OES device (ICP-720 manufactured by Agilent Technologies, Inc.), and was found to be 0.37% by mass.
[0058] The niobium concentration was measured using ICP-OES. Specifically, 0.1 g of the solution containing lithium and niobium according to Comparative Example 1 was taken, and 5 ml of hydrochloric acid and 15 ml of pure water were added. Then, 2 ml of hydrogen peroxide was added to dissolve the niobium to obtain a solution. Pure water was added to the obtained solution to make the volume 100 ml, and then pure water was added to dilute it 20 times. The niobium concentration was measured using an ICP-OES device (ICP-720 manufactured by Agilent Technologies, Inc.), and was found to be 4.9 mass%.
[0059] The Li / Nb ratio (molar ratio) was calculated from the lithium concentration and niobium concentration measured as described above. Specifically, the mole numbers of lithium and niobium in the solution containing lithium and niobium according to Comparative Example 1 were calculated from the lithium concentration and niobium concentration measured as described above, and the Li / Nb ratio (molar ratio) was calculated to be 1.00.
[0060] When the absorbance of light at wavelengths of 400 to 700 nm was measured using a UV-visible spectrophotometer (UV-1800, manufactured by SHIMADZU CORPORATION) by the transmitted light measurement method, the absorbance of light at a wavelength of 660 nm was 0.06, which was lower than the 0.15 that is considered to be a solution.
[0061] Example 1 The same procedure as in Comparative Example 1 was carried out to prepare a solution containing lithium and niobium. The prepared solution was placed in a multipurpose tank holder (Advantech: KST-90-UH) equipped with a hydrophilic PTFE type membrane filter (pore size: 0.5 μm) (Advantech: H050A047A) and filtered under a pressure of 0.4 MPa to obtain a solution containing lithium and niobium according to Example 1. The filtration rate was 20 kg / m 2 -hr. The conditions for producing the solution containing lithium and niobium according to the above-described Example 1 are shown in Table 1.
[0062] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Example 1, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm measured by an ultraviolet-visible spectrophotometer are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0063] From the results shown in Table 2, the D90 of the solution containing lithium and niobium according to Example 1 was 361.7 nm, which satisfied the requirement of 500 nm or less. The loading index value displayed was read to be 0.115, which was within the range of 0.15 or less. Then, in the same manner as described in Comparative Example 1, the IR spectrum was measured using the single reflection ATR method of FT-IR, and the 855 cm -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed, it was determined that the solution contained a niobium complex.
[0064] Example 2 The same procedure as in Comparative Example 1 was carried out to prepare a solution containing lithium and niobium. The prepared solution was placed in a multipurpose tank holder (Advantech Co., Ltd.: KST-90-UH) equipped with a hydrophilic cellulose mixed ester membrane filter (pore size: 0.025 μm) (MERCK: MF-Millipore) and filtered under a pressure of 0.4 MPa to prepare a solution containing lithium and niobium according to Example 2. The filtration rate was 1 kg / m 2 -hr. The conditions for producing the solution containing lithium and niobium according to the above-described Example 2 are shown in Table 1.
[0065] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Example 2, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0066] From the results shown in Table 2, the solution containing lithium and niobium according to Example 2 had a D90 of 21.6 nm, which was within the range of 500 nm or less and also within the range of 30 nm or less. The loading index value displayed was read to be 0.052, which was within the range of 0.15 or less.
[0067] The obtained solution containing lithium and niobium according to Example 2 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 1. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed, it was determined that the solution contained a niobium complex.
[0068] Example 3 The same operation as in Comparative Example 1 was repeated several times to prepare about 5 L of a solution containing lithium and niobium. The prepared solution was filtered through an ultrafiltration membrane (nominal pore size: 10 nm, membrane area: 0.016 m 2 Using a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech Corporation) (diameter 30 mm, length 250 mm), ultrafiltration by cross-flow filtration was performed at a liquid circulation flow rate of 3 m / s, average filtration pressure (0.1 MPa; filtrate side open to atmosphere, 0 MPa), and liquid temperature of 25°C. Prior to the ultrafiltration, the 37 holes of φ3 provided in the ultrafiltration membrane were sealed with packing to reduce the number of holes to 7, thereby ensuring a circulation flow rate of 3 m / s.
[0069] Then, when the supplied liquid stopped circulating, the circulation of the liquid was stopped, the filtrate was recovered, and a solution containing lithium and niobium according to Example 3 was prepared. During the filtration operation, filtrate was forced into the filter by air pressure (0.2 MPa) for 2 seconds to perform pulse backwashing. The filtration rate was 80 kg / m 2 -hr. During the filtration operation, the temperature of the solution was controlled to 25° C. using a jacket. Table 1 shows the production conditions for the solution containing lithium and niobium according to the third embodiment described above.
[0070] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Example 3, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0071] From the results shown in Table 2, the solution containing lithium and niobium according to Example 3 had a D90 of 9.3 nm, which satisfied the requirement of 500 nm or less and also satisfied the requirement of 30 nm or less. The loading index value displayed was read to be 0.010, which was within the range of 0.15 or less.
[0072] The obtained solution containing lithium and niobium according to Example 3 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1. It was confirmed that there was no change in the IR spectrum before and after the filtration process according to Example 3. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed, it was determined that the solution contained a niobium complex.
[0073] (Examples 4 and 5) A solution containing lithium and niobium according to Example 4 was prepared by carrying out the same operations as in Example 3, except that the average filtration pressure was changed to 0.2 MPa. Moreover, a solution containing lithium and niobium according to Example 5 was prepared by carrying out the same operations as in Example 3, except that the average filtration pressure was changed to 0.3 MPa. Table 1 shows the conditions for producing the solutions containing lithium and niobium according to the above-described Examples 4 and 5.
[0074] For the obtained solutions containing lithium and niobium according to Examples 4 and 5, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0075] From the results shown in Table 2, the D90 of the solution containing lithium and niobium according to Example 4 was 9.5 nm, and the D90 of the solution containing lithium and niobium according to Example 5 was 9.9 nm, which satisfied the requirement of 500 nm or less and further satisfied the requirement of 30 nm or less. When the loading index values displayed were read, it was 0.011 for Example 4 and 0.013 for Example 5, both of which satisfied the requirement of 0.15 or less.
[0076] The obtained solutions containing lithium and niobium according to Examples 4 and 5 were subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1. It was confirmed that there was no change in the IR spectrum before and after the filtration process according to Examples 4 and 5. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed, it was determined that the solution contained a niobium complex.
[0077] (Examples 6 and 7) A solution containing lithium and niobium according to Example 6 was prepared by carrying out the same operation as in Example 3, except that the circulation flow rate of the liquid was changed to (1 m / s) and the filtration pressure was changed to (0.2 MPa). A solution containing lithium and niobium according to Example 7 was prepared by carrying out the same operation as in Example 3, except that the circulation flow rate of the liquid was changed to (2 m / s) and the filtration pressure was changed to (0.2 MPa). Table 1 shows the production conditions for the solutions containing lithium and niobium according to Examples 6 and 7 described above.
[0078] For the obtained solutions containing lithium and niobium according to Examples 6 and 7, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0079] From the results shown in Table 2, the D90 of the solution containing lithium and niobium according to Example 6 was 9.4 nm, and the D90 of the solution containing lithium and niobium according to Example 7 was 9.5 nm, both of which satisfied the requirement of 500 nm or less. When the loading index values displayed were read, it was 0.012 for Example 6 and 0.012 for Example 7, both of which satisfied the requirement of 0.15 or less.
[0080] The obtained solutions containing lithium and niobium according to Examples 6 and 7 were subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1. It was confirmed that there was no change in the IR spectrum before and after the filtration process according to Examples 6 and 7. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0081] (Examples 8, 9, and 10) The filtration membrane was changed to a filtration membrane having a nominal pore size of 100 nm (Example 8), 200 nm (Example 9), or 500 nm (Example 10) (microfiltration membranes MF-0.1, MF-0.2, and MF-0.5 manufactured by NGK Filtech Corporation), and the same operation as in Example 3 was carried out to prepare solutions containing lithium and niobium according to Examples 8, 9, and 10. The conditions for producing the solutions containing lithium and niobium according to Examples 8, 9 and 10 described above are shown in Table 1.
[0082] For the obtained solutions containing lithium and niobium according to Examples 8, 9, and 10, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0083] From the results shown in Table 2, the D90 of the solution containing lithium and niobium according to Example 8 was 134.6 nm, the D90 of the solution containing lithium and niobium according to Example 9 was 194.7 nm, and the D90 of the solution containing lithium and niobium according to Example 10 was 381.2 nm, which satisfied the requirement of 500 nm or less. The loading index values displayed were read and found to be 0.025 for Example 8, 0.049 for Example 9, and 0.093 for Example 10, all of which were within the range of 0.15 or less.
[0084] The IR spectrum of the obtained solutions containing lithium and niobium according to Examples 8, 9, and 10 was measured using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1. It was confirmed that there was no change in the IR spectrum before and after the filtration process according to Examples 8, 9, and 10. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0085] Comparative Example 2 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 72.6% by mass)) was added to 74.6 g of hydrogen peroxide solution with a concentration of 30% by mass. After the addition of niobic acid, the temperature of the solution to which niobic acid had been added was adjusted to be within the range of 20 to 30°C. 12.3 g of ammonia water with a concentration of 28% by mass was added to the temperature-adjusted solution, and the solution was thoroughly stirred to obtain a transparent solution containing a niobium peroxo complex. In this transparent solution, the molar ratio of ammonia to 1 mole of niobium was 4.3. Next, 2.15 g of lithium hydroxide monohydrate was added to the obtained transparent solution in a nitrogen gas atmosphere to obtain a transparent solution containing lithium and a peroxo complex of niobium. Next, while stirring the solution at 20 to 30° C., ultraviolet light was irradiated from 3 cm above the solution using an ultraviolet lamp (GL4ZH manufactured by Sankyo Electric Co., Ltd.) with irradiation wavelengths of 185 nm and 253.7 nm. The stirring and irradiation were carried out for 10 hours to prepare a solution containing lithium and niobium according to Comparative Example 2. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 2 described above.
[0086] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Comparative Example 2, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0087] From the results shown in Table 2, the solution containing lithium and niobium according to Comparative Example 2 had a D90 of 624.9 nm, which did not satisfy the requirement of 500 nm or less. The loading index value displayed was read as 0.433, which did not meet the requirement of 0.15 or less.
[0088] Next, the obtained solution containing lithium and niobium according to Comparative Example 2 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1, and a peak at 855 cm assigned to a niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0089] Example 11 Comparative Example 2 was carried out multiple times to obtain about 5 L of a solution containing lithium and a niobium complex. This solution was subjected to a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech, and the same operation as in Example 3 was carried out except that the circulation flow rate of the liquid was changed to (3 m / s) and the filtration pressure was changed to (0.2 MPa), to prepare a solution containing lithium and niobium according to Example 11. The conditions for producing the solution containing lithium and niobium according to Example 11 described above are shown in Table 1.
[0090] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Example 11, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0091] From the results shown in Table 2, the solution containing lithium and niobium according to Example 11 had a D90 of 9.1 nm, which satisfied the requirement of 500 nm or less and also satisfied the requirement of 30 nm or less. The loading index value displayed was read to be 0.016, which was within the range of 0.15 or less.
[0092] The obtained solution containing lithium and niobium according to Example 11 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 2. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 11. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0093] Comparative Example 3 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 72.6% by mass)) was added to 74.6 g of hydrogen peroxide solution with a concentration of 30% by mass. After the addition of niobic acid, the temperature of the solution to which niobic acid had been added was adjusted to be within the range of 20 to 30°C. 12.3 g of ammonia water with a concentration of 28% by mass was added to the temperature-adjusted solution, and the solution was thoroughly stirred to obtain a transparent solution containing a niobium peroxo complex. In this transparent solution, the molar ratio of ammonia to 1 mole of niobium was 4.3. Next, 2.06 g of lithium hydroxide monohydrate was added to the obtained transparent solution in a nitrogen gas atmosphere to obtain a transparent solution containing lithium and a peroxo complex of niobium. Next, 10 g of photocatalytic titanium oxide (STS-21 (slurry)) manufactured by Ishihara Sangyo Kaisha, Ltd. was added to the solution.
[0094] Next, while stirring the solution at 20 to 30° C., ultraviolet light was irradiated from 3 cm above the solution using an ultraviolet lamp (GL4ZH manufactured by Sankyo Electric Co., Ltd.) with irradiation wavelengths of 185 nm and 253.7 nm. The stirring and irradiation were carried out for 10 hours, and the added photocatalytic titanium oxide was removed by centrifugal filtration, after which a solution containing lithium and niobium according to Comparative Example 3 was prepared. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 3 described above.
[0095] For the obtained solution containing lithium and niobium according to Comparative Example 3, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0096] From the results shown in Table 2, the solution containing lithium and niobium according to Comparative Example 3 had a D90 of 821.2 nm, which did not satisfy the requirement of 500 nm or less. The loading index value displayed was read as 0.762, which did not meet the requirement of 0.15 or less.
[0097] Next, the obtained solution containing lithium and niobium according to Comparative Example 3 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1, and a peak at 855 cm attributed to a niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since an absorption peak was confirmed, it was determined that the solution contained a niobium complex.
[0098] Example 12 Comparative Example 3 was carried out multiple times to obtain about 5 L of a solution containing lithium and niobium. This solution was subjected to a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech, and the same operation as in Example 3 was carried out except that the circulation flow rate of the liquid was changed to (3 m / s) and the filtration pressure was changed to (0.2 MPa), to prepare a solution containing lithium and niobium according to Example 12. The conditions for producing the solution containing lithium and niobium according to Example 12 described above are shown in Table 1.
[0099] The presence or absence of a niobium complex in the obtained solution containing lithium and niobium according to Example 12, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0100] From the results shown in Table 2, the solution containing lithium and niobium according to Example 12 had a D90 of 9.8 nm, which satisfied the requirement of 500 nm or less and also satisfied the requirement of 30 nm or less. The loading index value displayed was read to be 0.013, which was within the range of 0.15 or less.
[0101] The obtained solution containing lithium and niobium according to Example 12 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 3. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 12. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0102] Comparative Example 4 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 72.6% by mass)) was added to 74.6 g of hydrogen peroxide solution with a concentration of 30% by mass. After the addition of niobic acid, the temperature of the solution to which niobic acid had been added was adjusted to be within the range of 20 to 30°C. 12.3 g of ammonia water with a concentration of 28% by mass was added to the temperature-adjusted solution, and the solution was thoroughly stirred to obtain a transparent solution containing a niobium peroxo complex. In the transparent solution, the molar ratio of hydrogen peroxide to 1 mole of niobium (hydrogen peroxide / Nb) was 14, and the molar ratio of ammonia to 1 mole of niobium was 4.3. Next, 2.15 g of lithium hydroxide monohydrate was added to the obtained transparent solution in a nitrogen gas atmosphere to obtain a transparent solution containing lithium and a peroxo complex of niobium. Next, the solution was heated from 20°C to 60°C over a period of 3 hours while stirring in the air, and then kept at 60°C for 10 hours to prepare a solution containing lithium and niobium according to Comparative Example 4. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 4 described above.
[0103] For the obtained solution containing lithium and niobium according to Comparative Example 4, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0104] From the results shown in Table 2, the solution containing lithium and niobium according to Comparative Example 4 had a D90 of 662.0 nm, which did not satisfy the requirement of 500 nm or less. The loading index value displayed was read as 0.408, which did not meet the requirement of 0.15 or less.
[0105] Next, the obtained solution containing lithium and niobium according to Comparative Example 4 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1, and a peak at 855 cm assigned to a niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0106] Example 13 Comparative Example 4 was carried out multiple times to obtain about 5 L of a solution containing lithium and niobium. This solution was subjected to a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech, and the same operation as in Example 3 was carried out except that the circulation flow rate of the liquid was changed to (3 m / s) and the filtration pressure was changed to (0.2 MPa), to prepare a solution containing lithium and niobium according to Example 13. The conditions for producing the solution containing lithium and niobium according to Example 13 described above are shown in Table 1.
[0107] For the obtained solution containing lithium and niobium according to Example 13, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0108] From the results shown in Table 2, the solution containing lithium and niobium according to Example 13 had a D90 of 8.7 nm, which was within the range of 500 nm or less and also within the range of 30 nm or less. The loading index value displayed was read to be 0.012, which was within the range of 0.15 or less.
[0109] The obtained solution containing lithium and niobium according to Example 13 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 4. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 13. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0110] Comparative Example 5 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 72.6% by mass)) was added to 74.6 g of hydrogen peroxide solution with a concentration of 30% by mass. After the addition of niobic acid, the temperature of the solution to which niobic acid had been added was adjusted to be within the range of 20 to 30°C. 12.3 g of ammonia water with a concentration of 28% by mass was added to the temperature-adjusted solution, and the solution was thoroughly stirred to obtain a transparent solution containing a niobium peroxo complex. In this transparent solution, the molar ratio of ammonia to 1 mole of niobium was 4.3. Next, 2.06 g of lithium hydroxide monohydrate was added to the obtained transparent solution in a nitrogen gas atmosphere to obtain a transparent solution containing lithium and a peroxo complex of niobium. Next, the solution was heated from 20°C to 40°C over 1 hour while stirring in the air. 24.9 g of hydrogen peroxide solution with a concentration of 30 mass% was added to this solution over 1 hour, and the solution was further maintained and stirred at 40°C for 9 hours to prepare a solution containing lithium and niobium according to Comparative Example 5. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 5 described above.
[0111] For the obtained solution containing lithium and niobium according to Comparative Example 5, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0112] From the results shown in Table 2, the solution containing lithium and niobium according to Comparative Example 5 had a D90 of 518.8 nm, which did not satisfy the requirement of 500 nm or less. The loading index value displayed was read as 0.417, which did not meet the requirement of 0.15 or less.
[0113] Next, the obtained solution containing lithium and niobium according to Comparative Example 5 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1, and a peak at 855 cm assigned to a niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0114] Example 14 Comparative Example 5 was carried out multiple times to obtain about 5 L of a solution containing lithium and niobium. This solution was subjected to a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech, and the same operation as in Example 3 was carried out except that the circulation flow rate of the liquid was changed to (3 m / s) and the filtration pressure was changed to (0.2 MPa), to prepare a solution containing lithium and niobium according to Example 14. The conditions for producing the solution containing lithium and niobium according to Example 14 described above are shown in Table 1.
[0115] For the obtained solution containing lithium and niobium according to Example 14, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0116] From the results shown in Table 2, the solution containing lithium and niobium according to Example 14 had a D90 of 9.6 nm, which satisfied the requirement of 500 nm or less and also satisfied the requirement of 30 nm or less. The loading index value displayed was read to be 0.014, which was within the range of 0.15 or less.
[0117] The obtained solution containing lithium and niobium according to Example 14 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 5. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 14. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0118] Comparative Example 6 57.0 g of pure water was added to a container containing 8.58 g of niobic acid (Nb2O5·5.5H2O (Nb2O5 content 72.6% by mass)) and 2.15 g of lithium hydroxide·monohydrate. After stirring for 5 minutes, 8.54 g of 28% by mass ammonia water was added and stirred for a further 5 minutes, after which 21.2 g of 30% by mass hydrogen peroxide water was added and the liquid temperature was adjusted to within the range of 35 to 45°C. After thorough stirring, a slightly cloudy white solution containing a niobium peroxo complex was obtained. In this solution, the molar ratio of ammonia to 1 mole of niobium was 3.0. Next, the solution was heated from 40°C to 60°C over 2 hours while stirring in the air, and then kept at 60°C for 10 hours to prepare a solution containing lithium and niobium according to Comparative Example 6. Table 1 shows the production conditions for the solution containing lithium and niobium according to Comparative Example 6 described above.
[0119] For the obtained solution containing lithium and niobium according to Comparative Example 6, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0120] From the results shown in Table 2, the solution containing lithium and niobium according to Comparative Example 6 had a D90 of 802.1 nm, which did not satisfy the requirement of 500 nm or less. The loading index value displayed was read as 0.921, which did not meet the requirement of 0.15 or less.
[0121] Next, the obtained solution containing lithium and niobium according to Comparative Example 6 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 1, and a peak at 855 cm assigned to a niobium complex was detected. -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0122] Example 15 Comparative Example 6 was carried out multiple times to obtain about 5 L of a solution containing lithium and niobium. This solution was subjected to a benchtop filtration tester equipped with an ultrafiltration membrane (UF-50000) manufactured by NGK Filtech, and the same operation as in Example 3 was carried out except that the circulation flow rate of the liquid was changed to (3 m / s) and the filtration pressure was changed to (0.2 MPa), to prepare a solution containing lithium and niobium according to Example 15. The conditions for producing the solution containing lithium and niobium according to Example 15 described above are shown in Table 1.
[0123] For the obtained solution containing lithium and niobium according to Example 15, the presence or absence of a niobium complex, the particle size distribution measurement results by light scattering intensity distribution measurement, the loading index value, the lithium and niobium contents, the Li / Nb ratio (molar ratio), and the light absorbance value at a wavelength of 660 nm are shown in Table 2. The measurement methods and calculation methods for these values are the same as those described in Comparative Example 1.
[0124] From the results shown in Table 2, the solution containing lithium and niobium according to Example 15 had a D90 of 9.6 nm, which was within the range of 500 nm or less and also within the range of 30 nm or less. The loading index value displayed was read to be 0.014, which was within the range of 0.15 or less.
[0125] The obtained solution containing lithium and niobium according to Example 15 was subjected to IR spectrum measurement using the single reflection ATR method of FT-IR in the same manner as described in Comparative Example 7. It was confirmed that there was no change in the IR spectrum before and after the filtration step according to Example 15. And the 855cm attributed to the niobium complex -1 ±20cm -1 and 1650cm -1 ±10cm -1 Since a peak was confirmed, it was determined that the solution contained a niobium complex.
[0126] [Table 1] [Table 2]
Claims
1. A solution containing lithium and niobium, A solution containing lithium and niobium, the solution having a D90 of 200 nm or less as measured by a dynamic light scattering method based on light scattering intensity.
2. A solution containing lithium and niobium, A solution containing lithium and niobium, the solution having a D90 of 30 nm or less as measured by a dynamic light scattering method based on light scattering intensity.
3. 3. The solution containing lithium and niobium according to claim 1 or 2, wherein the niobium concentration of the solution containing lithium and niobium is 1% by mass or more and 15% by mass or less.
4. The solution containing lithium and niobium according to any one of claims 1 to 3, wherein the molar ratio of lithium to 1 mole of niobium (Li / Nb) in the solution containing lithium and niobium is 0.9 to 1.
4.
5. The solution containing lithium and niobium according to any one of claims 1 to 4, wherein the loading index value obtained by measurement using a frequency analysis using a heterodyne method as a dynamic light scattering method is 0.15 or less. The solution containing lithium and niobium.
6. 6. A solution containing lithium and niobium according to any one of claims 1 to 5, further comprising an M element (wherein the M element is one or more elements selected from Ta, F, La, P, B, Ti, Zr, W, Al, Zn, Si, Ge, and V).
7. 7. The solution containing lithium and niobium according to claim 1, wherein the niobium is a niobium complex.
8. A method for producing a solution containing lithium and niobium, comprising the steps of filtering a solution containing lithium and niobium using a filter having a filter pore size of 200 nm or less to obtain a solution containing lithium and niobium having a D90 of 200 nm or less, based on light scattering intensity, as measured by dynamic light scattering of the solution.
9. A method for producing a solution containing lithium and niobium, comprising the steps of filtering a solution containing lithium and niobium using a filter having a filter pore size of 30 nm or less to obtain a solution containing lithium and niobium having a D90 of 30 nm or less, based on light scattering intensity, as measured by dynamic light scattering of the solution.
10. The method for producing a solution containing lithium and niobium according to claim 8 or 9, wherein the filtration is cross-flow filtration.
11. The method for producing a solution containing lithium and niobium according to any one of claims 8 to 10, wherein the temperature of the solution containing lithium and niobium is maintained at 40°C or lower during the filtration.
12. The method for producing a solution containing lithium and niobium according to any one of claims 8 to 11, wherein a niobium complex is used as the niobium.
13. A step of performing a coating treatment on a surface of an active material for a lithium secondary battery using the solution containing lithium and niobium according to any one of claims 1 to 7; and heat-treating the coated active material for lithium secondary batteries.
Citation Information
Patent Citations
Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery
JP2012074240A
Manufacturing method for high-purity electrode materials
JP2015511366A
Solution, method for producing the same, and method for producing active material for secondary battery
JP2017160081A
Method of manufacturing electrode layer for all-solid battery
JP2020013701A
Inorganic particle dispersion, inorganic particle-containing composition, coating film, plastic substrate with coating film, and display device
JP2020019958A
Cited By
Nb complex aqueous solution, method for manufacturing positive electrode active material for all-solid-state lithium ion battery, method for manufacturing positive electrode for all-solid-state lithium ion battery, and method for manufacturing all-solid-state lithium ion battery
JP7774761B1