Semiconductor device manufacturing method
By forming controlled grain structures in amorphous films and using low-temperature crystallization, the method stabilizes the ferroelectric layer in ferroelectric memory cells, addressing variations in crystal grain size and orientation to enhance device performance.
Patent Information
- Application Number
- JP2023212917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2038-05-18
AI Technical Summary
The challenge in manufacturing ferroelectric memory cells is the formation of amorphous HfO2 films on semiconductor substrates, which upon high-temperature crystallization transform into paraelectric monoclinic phases, leading to variations in crystal grain size and orientation, affecting the threshold voltage and performance of the semiconductor device.
A method involving the formation of a two-layer or three-layer structure of amorphous films with controlled grain distribution, followed by low-temperature crystallization using microwaves, ensures the ferroelectric films maintain a rectangular crystal phase, aligning grain sizes and orientations for uniformity.
This approach stabilizes the ferroelectric layer, reducing variations in threshold voltage and enhancing the performance of ferroelectric memory cells by improving rewrite durability and retention.
Smart Images

Figure 0007594650000001 
Figure 0007594650000002 
Figure 0007594650000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a semiconductor device, and more particularly to a technique that is effective when applied to a method for manufacturing a semiconductor device used as a memory element using a ferroelectric film. [Background technology]
[0002] In recent years, ferroelectric memory cells using a ferroelectric layer have been developed as semiconductor memory elements that operate at low voltages. Ferroelectric memory cells are non-volatile memory cells that change the write and erase states of information by controlling the direction of polarization of the ferroelectric layer.
[0003] Patent Document 1 discloses a nonvolatile memory cell in which a ferroelectric layer formed above a select transistor is electrically connected to one of the diffusion regions of the select transistor. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] US Patent Application Publication No. 2014 / 0340372 Summary of the Invention [Problem to be solved by the invention]
[0005] In a ferroelectric memory cell using a HfO2 film constituting a ferroelectric layer, the crystal phase of the HfO2 film must be orthorhombic. However, the orthorhombic crystal is a metastable phase, and in the manufacturing process of a semiconductor device, if an amorphous (non-crystalline) HfO2 film is formed on a semiconductor substrate and then heat-treated at a high temperature of, for example, about 700 to 1000°C for crystallization, the crystal phase of the HfO2 film becomes monoclinic, and the HfO2 film becomes a paraelectric rather than a ferroelectric. In a ferroelectric memory cell, the threshold voltage is controlled by applying positive and negative voltages to the gate electrode and controlling the inversion of the polarization domain in the ferroelectric layer. For this reason, there is a problem that the crystal grain size and crystal orientation of the ferroelectric layer vary, resulting in a large variation in the threshold voltage relative to the gate voltage. In other words, the challenge is to align the crystal grain size and crystal orientation of the ferroelectric layer to improve the performance of the semiconductor device.
[0006] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0007] A brief outline of a representative embodiment of the present invention will be described below.
[0008] A method for manufacturing a semiconductor device according to one embodiment includes the steps of: (a) forming a first amorphous film made of a material containing hafnium and oxygen; (b) forming a plurality of grains containing a first element selected from the group consisting of aluminum, carbon, nitrogen, fluorine, and titanium on an upper surface of the first amorphous film so as to cover a portion of an upper surface of the first amorphous film after the step (a) and to expose another portion of the upper surface of the first amorphous film; (c) forming a first amorphous film on the upper surface of the first amorphous film after the step (b) to cover the plurality of grains and to expose another portion of the upper surface of the first amorphous film; (d) forming a second amorphous film made of a material containing hafnium and oxygen on the upper surface of the first amorphous film so as to be in contact with the other portion of the upper surface of the amorphous film that is exposed from the plurality of grains; (d) forming a first metal film on the second amorphous film after the step (c); and (e) crystallizing the first amorphous film by performing a heat treatment after the step (d) to form a first ferroelectric film of an orthorhombic crystal system and to crystallize the second amorphous film to form a second ferroelectric film of an orthorhombic crystal system. Effect of the Invention
[0009] According to one embodiment, the performance of a semiconductor device can be improved. [Brief description of the drawings]
[0010] [Figure 1] 1 is a planar layout diagram of a semiconductor chip which is a semiconductor device according to a first embodiment. [Diagram 2] 1 is a cross-sectional view of a semiconductor device according to a first embodiment. [Diagram 3] 1 is a graph obtained through an experiment conducted by the inventor of the present application. [Figure 4] 1 is a table showing an example of conditions for applying voltages to each portion of a selected memory cell during "writing," "erasing," and "reading." [Diagram 5] 2A to 2C are cross-sectional views showing a manufacturing process of the semiconductor device according to the first embodiment. [Figure 6] 6 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 5. [Figure 7]7A to 7C are cross-sectional views showing the manufacturing process of the semiconductor device following FIG. 6. [Figure 8] 8 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 7. [Figure 9] 9 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 8. [Figure 10] 10 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. [Figure 11] 11 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 10. [Figure 12] 12 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 11. [Figure 13] 13 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 12. [Figure 14] 14 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 13. [Figure 15] 15 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 14. [Figure 16] 16 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 15. [Figure 17] 17 is a cross-sectional view showing a manufacturing process of the semiconductor device subsequent to FIG. 16. [Figure 18] 1 is a graph obtained through an experiment conducted by the inventor of the present application. [Figure 19] 10A to 10C are cross-sectional views showing a manufacturing process of a semiconductor device according to a second embodiment. [Figure 20] 11A to 11C are cross-sectional views showing a manufacturing process of a semiconductor device according to a third embodiment. [Figure 21] FIG. 11 is a cross-sectional view of a semiconductor device according to a fourth embodiment. [Figure 22] FIG. 13 is a perspective view of a semiconductor device according to a fifth embodiment. [Diagram 23] 13A to 13C are cross-sectional views showing a manufacturing process of a semiconductor device according to a fifth embodiment. [Figure 24] 1A to 1C are cross-sectional views showing a manufacturing process of a semiconductor device according to a study example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the following embodiments, when necessary for convenience, the description will be divided into a plurality of sections or embodiments, but unless otherwise specified, they are not unrelated to each other, and one is a partial or complete modification, detail, supplementary explanation, etc. of the other. In addition, in the following embodiments, when the number of elements (including the number, numerical value, amount, range, etc.) is mentioned, it is not limited to the specific number, except when specifically specified or when it is clearly limited to a specific number in principle, and it may be more than or less than the specific number. Furthermore, in the following embodiments, it goes without saying that the components (including element steps, etc.) are not necessarily essential, except when specifically specified or when it is clearly considered to be essential in principle. Similarly, in the following embodiments, when the shape, positional relationship, etc. of the components, etc. are mentioned, it includes those that are substantially similar to or similar to the shape, etc., except when specifically specified or when it is clearly considered not to be essential in principle. This also applies to the above numerical values and ranges.
[0012] Hereinafter, the embodiments will be described in detail with reference to the drawings. In all the drawings for explaining the embodiments, the same reference numerals are used for the members having the same functions, and the repeated explanations are omitted. In the following embodiments, the explanations of the same or similar parts will not be repeated as a rule unless it is particularly necessary.
[0013] Furthermore, in the drawings used in the embodiments, hatching may be omitted in order to make the drawings easier to understand.
[0014] (Embodiment 1) A semiconductor device having a ferroelectric memory cell, which is a nonvolatile memory cell in this embodiment, will be described with reference to the drawings. First, the planar layout configuration of a semiconductor chip CHP, which is a semiconductor device in which a system including a ferroelectric memory cell is formed, will be described with reference to Fig. 1. In Fig. 1, the semiconductor chip CHP has a ferroelectric memory circuit C1, a CPU (Central Processing Unit) circuit C2, a RAM (Random Access Memory) circuit C3, an analog circuit C4, and an I / O (Input / Output) circuit C5.
[0015] The ferroelectric memory circuit C1 has a circuit in which stored information can be electrically rewritten, and is an area in which a plurality of ferroelectric memory cells, which are nonvolatile memory cells, are formed as semiconductor elements.
[0016] The CPU circuit C2 has a logic circuit that operates at a voltage of about 1.5V, and is an area in which low-voltage metal insulator semiconductor field effect transistors (MISFETs), which have a low withstand voltage and operate quickly, are formed as semiconductor elements.
[0017] The RAM circuit C3 has an SRAM (Static RAM), and is an area in which low-voltage MISFETs having substantially the same structure as the CPU circuit C2 are formed as semiconductor elements.
[0018] The analog circuit C4 is a region having an analog circuit, and in which semiconductor elements such as capacitance elements, resistance elements, bipolar transistors, and high-voltage MISFETs that have a higher withstand voltage than low-voltage MISFETs and are driven by a voltage of about 6 V are formed.
[0019] The I / O circuit C5 has input / output circuits, and is a region in which high-voltage MISFETs, similar to those in the analog circuit C4, are formed as semiconductor elements. <Structure of Semiconductor Device>
[0020] The structure of the semiconductor device of this embodiment will be described below with reference to Figures 2 and 3. In this embodiment, as an example of the structure of the semiconductor device, a ferroelectric memory cell MC formed in a ferroelectric memory circuit C1 and a low-voltage MISFET 1Q formed in a CPU circuit C2 will be described.
[0021] As shown in FIG. 2, the semiconductor device of the present embodiment includes a region MR in which a ferroelectric memory cell MC is formed, and a region LR in which a low voltage MISFET 1Q is formed.
[0022] The semiconductor substrate (semiconductor wafer) SB is made of p-type single crystal silicon (Si) having a resistivity of, for example, about 1 to 10 Ωcm. A p-type well region PW1 is formed in the semiconductor substrate SB in the region MR, and a p-type well region PW2 is formed in the semiconductor substrate SB in the region LR. A plurality of element isolation parts STI are formed in the well region PW1 and the well region PW2. The element isolation parts STI are configured by embedding an insulating film such as a silicon oxide film in a trench formed in the semiconductor substrate SB.
[0023] First, the structure of the ferroelectric memory cell MC in the region MR will be described. In this embodiment, as the ferroelectric memory cell MC, a memory cell having a Metal Ferroelectric Insulator Semiconductor (MFIS) structure in which a ferroelectric layer FEL is applied to a transistor structure will be exemplified.
[0024] In the region MR, an insulating film IF1 is formed on the semiconductor substrate SB including the well region PW1. The insulating film IF1 is, for example, a silicon oxide film, and has a thickness of, for example, 1 nm to 3 nm. The insulating film IF1 is a film provided for the purpose of stabilizing the interface between the semiconductor substrate SB and a ferroelectric layer FEL described later, or for the purpose of preventing electrons from entering the ferroelectric layer FEL from the semiconductor substrate SB when a voltage is applied to a gate electrode G1 described later during operation of the ferroelectric memory cell MC. Therefore, if these purposes can be achieved, there are cases in which the insulating film IF1 does not need to be provided.
[0025] The ferroelectric layer FEL is formed on the insulating film IF1. The ferroelectric layer FEL has a ferroelectric film FE1, a ferroelectric film FE2, and a plurality of grains GR formed between the ferroelectric film FE1 and the ferroelectric film FE2.
[0026] Each of the ferroelectric films FE1 and FE2 is made of a metal oxide film and is a high dielectric constant film having a higher dielectric constant than, for example, a silicon nitride film. The thickness of each of the ferroelectric films FE1 and FE2 is, for example, 5 nm. In this case, the thickness of the ferroelectric layer FEL is, for example, 10 nm.
[0027] Moreover, each of the ferroelectric films FE1 and FE2 is an insulating film made of a material in which dielectric polarization occurs when an electric field is applied and the polarization does not become zero even when the electric field is removed, that is, a ferroelectric. In other words, polarization remains in the ferroelectric films FE1 and FE2 even when an electric field is not applied. A ferroelectric is a material in which electric dipoles are aligned even in the absence of an external electric field, and the direction of the dipoles can be changed by an electric field.
[0028] Each of the ferroelectric films FE1 and FE2 must be an orthorhombic crystal. In other words, a film mainly composed of crystals other than an orthorhombic crystal is a paraelectric film. Therefore, in the ferroelectric memory cell MC, in order to increase the remanent polarization of the ferroelectric layer FEL, improve the performance as a ferroelectric, and reduce the driving power of the ferroelectric memory cell MC, it is necessary to form the crystals constituting the ferroelectric films FE1 and FE2 as orthorhombic as possible.
[0029] In this embodiment, each of the ferroelectric films FE1 and FE2 is an insulating film made of a material containing, for example, hafnium (Hf), oxygen (O), and zirconium (Zr) as a first element. The first element may be any of silicon (Si), germanium (Ge), yttrium (Y), lanthanum (La), and ytterbium (Yb) instead of zirconium.
[0030] Between the ferroelectric film FE1 and the ferroelectric film FE2, a plurality of grains GR are formed as a part of the ferroelectric layer FEL. As described later, the plurality of grains GR function as crystal nuclei for forming the ferroelectric film FE1 and the ferroelectric film FE2 into rectangular crystals during the manufacturing process of the ferroelectric layer FEL. Therefore, the plurality of grains GR are composed of a plurality of grains separated from each other. In other words, the plurality of grains GR are not a film formed continuously like the ferroelectric film FE1 and the ferroelectric film FE2, but are formed discontinuously. If the plurality of grains GR were each combined to form a film, the function of the plurality of grains GR as a crystal nucleus would be reduced.
[0031] The plurality of grains GR include a second element different from any of hafnium, oxygen, and the first element. The second element is, for example, aluminum (Al). Instead of aluminum, the second element may be any of carbon (C), nitrogen (N), fluorine (F), and titanium (Ti). In this embodiment, each of the plurality of grains GR is composed of one atom or an aggregate of 2 to 4 atoms.
[0032] In addition, the multiple grains GR may be bonded to substances contained in the ferroelectric film FE1 and the ferroelectric film FE2 near the interface between the ferroelectric film FE1 and the ferroelectric film FE2 during the manufacturing process of the ferroelectric layer FEL. That is, the multiple grains GR are ultimately either aluminum, carbon, nitrogen, fluorine, or titanium, or compounds of these elements bonded to hafnium, oxygen, or the first element.
[0033] Fig. 3 is a graph obtained by an experiment by the inventor of the present application, in which the vertical axis indicates the concentration of the plurality of grains GR, and the horizontal axis indicates the thickness in the film thickness direction in the ferroelectric layer FEL. Also, here, the measurement results are shown when aluminum (Al) is used as the plurality of grains GR. In Fig. 3, the solid line indicates the concentration of aluminum (Al), and the dashed line indicates the concentration of hafnium (Hf). Note that Fig. 3 shows not only the graph of the first embodiment, but also the graph of the second embodiment described later.
[0034] Referring to the graph of the first embodiment in FIG. 3, the aluminum (Al) concentration peak is large in the ferroelectric layer FEL near the interface between the ferroelectric film FE1 and the ferroelectric film FE2. The aluminum (Al) concentration peak is small or does not exist near the lower surface of the ferroelectric film FE1 and near the upper surface of the ferroelectric film FE2. Therefore, it is found that a part of the aluminum exists in the ferroelectric film FE1 and the ferroelectric film FE2, but most of the aluminum exists near the interface between the ferroelectric film FE1 and the ferroelectric film FE2. As described above, aluminum and compounds of aluminum and substances contained in the ferroelectric film FE1 and the ferroelectric film FE2 are present near the interface between the ferroelectric film FE1 and the ferroelectric film FE2. That is, it is found that aluminum or aluminum compounds are not diffused throughout the ferroelectric film FE1 and the ferroelectric film FE2, but remain near the interface between the ferroelectric film FE1 and the ferroelectric film FE2.
[0035] Thus, the concentration peak of the plurality of grains GR is larger at a position close to the interface between the ferroelectric film FE1 and the ferroelectric film FE2 than at a position close to the bottom surface of the ferroelectric film FE1 and a position close to the top surface of the ferroelectric film FE2. Therefore, since the plurality of grains GR are present near the interface between the ferroelectric film FE1 and the ferroelectric film FE2, each of the ferroelectric film FE1 and the ferroelectric film FE2 has a highly uniform crystal grain size, and is easily formed as a rectangular crystal. Therefore, when the ferroelectric layer FEL is applied to the ferroelectric memory cell MC, the problem of the threshold voltage variation increasing due to the polarization reversal of the ferroelectric layer FEL can be suppressed, and the problem of the rewrite resistance of the ferroelectric memory cell MC decreasing or the retention decreasing can be suppressed. That is, the technology of this embodiment can improve the performance of the semiconductor device.
[0036] Moreover, in the ferroelectric layer FEL, when comparing the ratio of hafnium, the ratio of the first element (Zr, etc.), and the ratio of the second element (grains GR), the ratio of the second element is smaller than the ratio of hafnium and the ratio of the first element. Specifically, when the sum of the ratio of hafnium, the ratio of the first element, and the ratio of the second element is 100%, in the ferroelectric layer FEL, the ratio of hafnium is within a range of 30% to 50%, the ratio of the first element is within a range of 30% to 50%, and the ratio of the second element is within a range of 0.5% to 5.0%.
[0037] A metal film MF1 is formed on the ferroelectric layer FEL. The metal film MF1 is a conductive film made of, for example, a titanium nitride film, a tantalum nitride film, or a tungsten film. The thickness of the metal film MF1 is, for example, 10 nm to 20 nm. The metal film MF1 is a cap film provided to apply stress to the ferroelectric film FE1 and the ferroelectric film FE2 during the manufacturing process of the ferroelectric layer FEL and to control the crystal orientation of each of the ferroelectric film FE1 and the ferroelectric film FE2. Therefore, after the formation of the ferroelectric layer FEL, if each of the ferroelectric film FE1 and the ferroelectric film FE2 can exist as a rectangular crystal, the metal film MF1 may be removed. However, since the removal of the metal film MF1 may cause the crystal orientation of each of the ferroelectric film FE1 and the ferroelectric film FE2 to vary, it is more preferable to leave the metal film MF1. In addition, if the metal film MF1 is left, the metal film MF1 also functions as a part of the gate electrode G1 described later.
[0038] A gate electrode G1 is formed on the metal film MF1. The gate electrode G1 is a conductive film made of, for example, a polycrystalline silicon film into which an n-type impurity is introduced. The material constituting the gate electrode G1 may be a metal film such as a titanium nitride film, an aluminum film, or a tungsten film, or a laminated film in which these are appropriately laminated, instead of a polycrystalline silicon film.
[0039] A sidewall spacer SW is formed on the side surface of the gate electrode G1. The sidewall spacer SW is made of, for example, a laminated film of a silicon oxide film and a silicon nitride film.
[0040] In the well region PW1 under the sidewall spacer SW, an extension region EX1 which is a low-concentration n-type impurity region is formed. In addition, in the well region PW1 at a position aligned with the sidewall spacer SW, a diffusion region D1 which is a higher-concentration n-type impurity region than the extension region EX1 is formed. The extension region EX1 and the diffusion region D1 are connected to each other and respectively constitute a part of the source region or a part of the drain region of the ferroelectric memory cell MC.
[0041] A silicide layer SI made of, for example, cobalt silicide (CoSi2), nickel silicide (NiSi) or nickel platinum silicide (NiPtSi) is formed on the gate electrode G1 and the diffusion region D1. The silicide layer SI is formed mainly to reduce the contact resistance with a plug PG described later.
[0042] Next, the structure of the low-voltage MISFET 1Q in the region LR will be described.
[0043] In the region LR, a gate insulating film GF is formed on the semiconductor substrate SB including the well region PW2. The gate insulating film GF is, for example, a silicon oxide film, and has a thickness of, for example, 1 nm to 4 nm.
[0044] A gate electrode G2 is formed on the gate insulating film GF. The gate electrode G2 is a conductive film made of, for example, a polycrystalline silicon film into which an n-type impurity is introduced. The material constituting the gate electrode G2 may be, instead of the polycrystalline silicon film, a metal film such as a titanium nitride film, an aluminum film, or a tungsten film, or a laminated film in which these are appropriately laminated.
[0045] A sidewall spacer SW is formed on the side surface of the gate electrode G2. The sidewall spacer SW is made of, for example, a laminated film of a silicon oxide film and a silicon nitride film.
[0046] In the well region PW2 below the sidewall spacer SW, an extension region EX2 which is a low-concentration n-type impurity region is formed. In addition, in the well region PW2 at a position aligned with the sidewall spacer SW, a diffusion region D2 which is a higher-concentration n-type impurity region than the extension region EX2 is formed. The extension region EX2 and the diffusion region D2 respectively constitute a part of the source region or a part of the drain region of the MISFET 1Q.
[0047] The impurity concentration of the extension region EX1 of the region MR is approximately the same as the impurity concentration of the extension region EX2 of the region LR. The impurity concentration of the diffusion region D1 of the region MR is approximately the same as the impurity concentration of the diffusion region D2 of the region LR.
[0048] A silicide layer SI made of, for example, cobalt silicide (CoSi2), nickel silicide (NiSi) or nickel platinum silicide (NiPtSi) is formed on the gate electrode G2 and the diffusion region D2. The silicide layer SI is formed mainly to reduce the contact resistance with a plug PG described later.
[0049] An interlayer insulating film IL1 is formed on the ferroelectric memory cell MC formed in the region MR and on the MISFET1Q formed in the region LR. The interlayer insulating film IL1 is, for example, a silicon oxide film. A plurality of contact holes are formed in the interlayer insulating film IL1, and a plurality of plugs PG are formed in the plurality of contact holes. The plug PG is, for example, made of a barrier metal film made of a titanium film, a titanium nitride film, or a laminated film of these, and a conductive film mainly made of tungsten. The plug PG is electrically connected to the diffusion region D1 or the diffusion region D2 via a silicide layer SI. Although not shown, the interlayer insulating film IL1 also has a gate electrode G1 and a plug PG electrically connected to the gate electrode G1.
[0050] Although not shown, a plurality of wirings are formed on the plug PG. For example, an interlayer insulating film is formed on the interlayer insulating film IL1, and a groove for wiring is formed in the interlayer insulating film. Then, a conductive film mainly composed of, for example, copper is embedded in the groove for wiring to form a first layer wiring connected to the plug PG.
[0051] <Operation of ferroelectric memory cell MC> Next, an example of the operation of the ferroelectric memory cell MC will be described with reference to FIG.
[0052] Fig. 4 is a table showing an example of voltages applied to each portion of a selected memory cell among ferroelectric memory cells MC during "write", "erase" and "read". The table in Fig. 4 lists the voltage Vd applied to the drain region (one diffusion region D1) of the ferroelectric memory cell MC shown in Fig. 2, the voltage Vg applied to the gate electrode CG1, the voltage Vs applied to the source region (the other diffusion region D1) and the voltage Vb applied to the well region PW1 during each of the "write", "erase" and "read" operations. Note that the table in Fig. 4 shows a preferred example of voltage application conditions, and is not limited thereto, and can be changed in various ways as necessary.
[0053] In this embodiment, the polarization of the ferroelectric layer FEL is directed upward, and the threshold voltage of the ferroelectric memory cell MC is relatively high, which is defined as "writing". The polarization of the ferroelectric layer FEL is directed downward, and the threshold voltage of the ferroelectric memory cell MC is relatively low, which is defined as "erasing".
[0054] The write operation is performed by applying a negative voltage to the gate electrode G1. That is, for example, a voltage as shown in the "write" column of Fig. 4 is applied to each portion of the selected memory cell to be written. This causes the polarization of the ferroelectric layer FEL to be upward, the threshold voltage of the ferroelectric memory cell MC to increase, and the ferroelectric layer FEL enters the write state.
[0055] The erase operation is performed by applying a positive voltage to the gate electrode G1. That is, for example, a voltage as shown in the "Erase" column in Figure 4 is applied to each part of the selected memory cell to be erased. This causes the polarization of the ferroelectric layer FEL to be downward, the threshold voltage of the ferroelectric memory cell MC to decrease, and the ferroelectric layer FEL enters the erased state.
[0056] In the read operation, for example, voltages such as those shown in the "Read" column in Fig. 4 are applied to each portion of the selected memory cell to be read. The written state and the erased state can be distinguished by setting the voltage Vg applied to the gate electrode G1 to a value between the threshold voltage of the ferroelectric layer FEL in the written state and the threshold voltage of the ferroelectric layer FEL in the erased state.
[0057] <Semiconductor device manufacturing process> A method for manufacturing the semiconductor device of the present embodiment will be described below with reference to Figures 5 to 17. Each of Figures 5 to 17 is a cross-sectional view showing a region MR in which a ferroelectric memory cell MC is formed and a region LR in which a low voltage MISFET 1Q is formed.
[0058] FIG. 5 shows a process of forming the element isolation portion STI, the well region PW1, and the well region PW2.
[0059] First, a semiconductor substrate SB made of single crystal silicon doped with p-type impurities is prepared. Next, a groove is formed in the semiconductor substrate SB using photolithography and etching. Next, an insulating film such as a silicon oxide film is formed so as to fill the groove, and then the insulating film outside the groove is removed by CMP (Chemical Mechanical Polishing) to form an element isolation part STI made of the insulating film remaining in the groove.
[0060] Next, impurities are introduced into the semiconductor substrate SB using photolithography and ion implantation to form a p-type well region PW1 in the region MR and a p-type well region PW2 in the region LR.
[0061] FIG. 6 shows a process for forming the gate insulating film GF.
[0062] First, a gate insulating film GF made of, for example, silicon oxide is formed on the semiconductor substrate SB in the regions MR and LR, by performing a heat treatment in an atmosphere containing oxygen on the semiconductor substrate SB including the well region PW1 in the region MR and the well region PW2 in the region LR. The thickness of the gate insulating film GF is, for example, 1 nm to 3 nm. Next, a resist pattern RP1 having an opening in the region MR and a pattern covering the region LR is formed. Next, an etching process is performed using the resist pattern RP1 as a mask, thereby removing the gate insulating film GF in the region MR so that the gate insulating film GF in the region LR is left. Thereafter, the resist pattern RP1 is removed by, for example, an ashing process.
[0063] FIG. 7 shows a process of forming the insulating film IF1.
[0064] The semiconductor substrate SB is subjected to a heat treatment in an atmosphere containing oxygen, for example, to form an insulating film IF1 made of, for example, silicon oxide on the semiconductor substrate SB in the region MR. The insulating film GF has a thickness of, for example, 1 nm to 3 nm. At this time, the gate insulating film GF is formed in the region LR, but the thickness of the gate insulating film GF increases slightly due to the thermal oxidation treatment.
[0065] FIG. 8 shows the process of forming the amorphous film AM1.
[0066] An amorphous film (non-crystalline film) AM1 is formed on the insulating film IF1 in the region MR and on the gate insulating film GF in the region LR by, for example, ALD (Atomic Layer Deposition). The amorphous film AM1 has a thickness of, for example, 5 nm. The amorphous film AM1 is, for example, a film made of a material containing hafnium (Hf), oxygen (O), and zirconium (Zr) as a first element. The first element may be any of silicon (Si), germanium (Ge), yttrium (Y), lanthanum (La), and ytterbium (Yb) instead of zirconium.
[0067] FIG. 9 shows the process of forming a plurality of grains GR.
[0068] The semiconductor wafer is transferred from the ALD apparatus used in the amorphous film AM1 formation process of FIG. 8 to another apparatus, and the process of FIG. 9 is carried out. In this embodiment, a plurality of grains GR are formed on the amorphous film AM1 in the regions MR and LR by a sputtering method. The plurality of grains GR are separated from each other. In other words, the plurality of grains GR are not a film formed continuously like the amorphous film AM1, but are formed discontinuously. That is, the plurality of grains GR do not cover the entire amorphous film AM1, but are scattered on the amorphous film AM1. Therefore, a part of the amorphous film AM1 is covered by the plurality of grains GR, and the other part of the amorphous film AM1 is exposed from the plurality of grains GR. In addition, a part of the plurality of grains GR is deposited on the upper surface of the amorphous film AM1, but there are also a plurality of grains GR introduced near the upper surface in the amorphous film AM1. For this reason, the plurality of grains GR can function as crystal nuclei in the process of crystallizing the amorphous film AM1, etc., which will be described later.
[0069] Moreover, the plurality of grains GR contain a second element different from any of hafnium, oxygen, and the first element. The second element is, for example, aluminum (Al). The second element may be any of carbon (C), nitrogen (N), fluorine (F), and titanium (Ti) instead of aluminum. In this embodiment, the case where the second element is aluminum will be described as a representative example.
[0070] The grains GR may be formed by a CVD (Chemical Vapor Deposition) method instead of the sputtering method. However, as described above, it is preferable to form the grains GR so as to be separated from each other. Therefore, it is preferable to form the grains GR by the sputtering method. The surface density of the grains GR on the upper surface of the amorphous film AM1 is 5×10 12 / cm 2 ~5×10 14 / cm 2This allows the radius of the crystal grain size of the multiple grains GR to be precisely controlled within a range of, for example, 0.1 nm to 1 nm.
[0071] Moreover, in order to prevent the plurality of grains GR from diffusing excessively in the amorphous film AM1, the above-mentioned sputtering method is preferably carried out at a temperature in the range of 1° C. or more and 150° C. or less.
[0072] As described above, the second element constituting the plurality of grains GR may be other elements instead of aluminum. In such a case, the method of forming the plurality of grains GR may be performed by using an ion implantation method instead of a sputtering method. When using an ion implantation method, the dose amount of the plurality of grains GR is set to 5×10 12 / cm 2 ~5×10 14 / cm 2 Within the range.
[0073] FIG. 10 shows the process of forming the amorphous film AM2.
[0074] In the region MR and the region LR, an amorphous film (non-crystalline film) AM2 is formed on the plurality of grains GR and the amorphous film AM1 by, for example, the ALD method. Through this process, the plurality of grains GR are covered with the amorphous film AM2. The thickness of the amorphous film AM2 is, for example, 5 nm. The amorphous film AM2 is made of the same material as the amorphous film AM1, and is, for example, a film made of a material containing hafnium (Hf), oxygen (O), and zirconium (Zr) as a first element. The first element may be any one of silicon (Si), germanium (Ge), yttrium (Y), lanthanum (La), and ytterbium (Yb) instead of zirconium.
[0075] FIG. 11 shows the process of forming the metal film MF1.
[0076] In the regions MR and LR, a metal film MF1 made of, for example, titanium nitride, tantalum nitride, or tungsten is formed on the amorphous film AM2 by, for example, CVD or sputtering. The thickness of the metal film MF1 is, for example, 10 nm to 20 nm. The metal film MF1 is provided mainly to apply stress to the amorphous films AM1 and AM2.
[0077] FIG. 12 shows the process of forming the ferroelectric film FE1, the ferroelectric film FE2, and the ferroelectric layer FEL.
[0078] In the region MR and the region LR, with the metal film MF1 formed on the amorphous film AM2, a heat treatment is performed to crystallize the amorphous film AM1 to form a ferroelectric film FE1 which is a rectangular crystal, and to crystallize the amorphous film AM2 to form a ferroelectric film FE2 which is a rectangular crystal.
[0079] This heat treatment can be performed at a temperature of 600°C or less by RTA (Rapid Thermal Annealing), but is preferably performed using microwaves with a frequency of 1 GHz to 10 GHz as electromagnetic waves, and more preferably microwaves with a frequency of 2.45 GHz. Heat treatment using microwaves allows crystallization at a lower temperature, and can be performed at a temperature of, for example, 400°C or less.
[0080] In this microwave heat treatment, microwaves are irradiated so that the vibration direction of the electric field is 90 degrees (perpendicular) to the top surface of the metal film MF1 or the top surface of the semiconductor substrate SB. Such electromagnetic waves such as microwaves have the property that the energy is absorbed by polarization crystals, so that the ferroelectric films FE1 and FE2, which are polarization crystals, are easily formed. Therefore, as described above, it becomes easy to perform the heat treatment for crystallization at a low temperature of 400°C or less.
[0081] For example, if the heat treatment for crystallization is performed at a high temperature of about 700 to 1000° C., the crystal phase of the ferroelectric film FE1 and the ferroelectric film FE2 is likely to be monoclinic, and the ferroelectric film FE1 and the ferroelectric film FE2 will become paraelectric films rather than ferroelectric films. By performing the heat treatment at a low temperature of 400° C. or less as in this embodiment, it becomes easy to form the ferroelectric film FE1 and the ferroelectric film FE2 as rectangular crystals.
[0082] In addition, in this crystallization process, the orientation of each of the ferroelectric films FE1 and FE2 is controlled by the stress from the metal film MF1. That is, when the amorphous films AM1 and AM2 are crystallized into the ferroelectric films FE1 and FE2, the metal film MF1 has a function of orienting the crystal phase of each of the ferroelectric films FE1 and FE2 into a rectangular crystal.
[0083] In this embodiment, a plurality of grains GR are formed between the amorphous film AM1 and the amorphous film AM2. These grains function as crystal nuclei in the crystallization process. Through the heat treatment, some of the grains GR are combined with the substances contained in the amorphous film AM1 and the amorphous film AM2 to form compounds. That is, the grains GR after the heat treatment are either aluminum, carbon, nitrogen, fluorine, or titanium, or compounds of these combined with hafnium, oxygen, or the first element.
[0084] As an example of the crystallization process, a case where the second element constituting the plurality of grains GR is aluminum will be described below. Most of the plurality of aluminum grains, which are the plurality of grains GR, are bonded with oxygen contained in the amorphous film AM1 and the amorphous film AM2 to become a plurality of aluminum oxide grains. The amorphous film AM1 and the amorphous film AM2 are crystallized using the plurality of aluminum oxide grains as crystal nuclei to become the ferroelectric film FE1 and the ferroelectric film FE2. Here, the radius of the crystal grain size of the plurality of aluminum grains is precisely controlled within a range of, for example, 0.1 nm to 1 nm. That is, the crystal grain size of each of the ferroelectric film FE1 and the ferroelectric film FE2 is made uniform according to the crystal grain size of the plurality of aluminum oxide grains, and therefore the uniformity of the crystal grain size in the ferroelectric layer FEL is improved.
[0085] In this way, the uniformity of the crystal grain size can be improved and the crystal orientation can be aligned to a rectangular crystal in the ferroelectric layer FEL. Therefore, when the ferroelectric layer FEL is applied to a ferroelectric memory cell MC, the film quality of the ferroelectric layer FEL deteriorates due to polarization inversion of the ferroelectric layer FEL, and the crystal grain size and crystal orientation of the ferroelectric layer FEL vary, which can suppress the problem of increasing the variation in threshold voltage. Therefore, the problem of the write endurance of the ferroelectric memory cell MC decreasing or the retention decreasing can be suppressed. That is, the technology of this embodiment can improve the performance of the semiconductor device.
[0086] FIG. 13 shows the manufacturing process of the semiconductor device subsequent to FIG. 12, and illustrates the step of removing the metal film MF1 and the ferroelectric layer FEL.
[0087] First, a resist pattern RP2 having a pattern that opens the region LR and covers the region MR is formed. Next, an etching process is performed using the resist pattern RP2 as a mask to remove the metal film MF1 and the ferroelectric layer FEL formed in the region LR so that the metal film MF1 and the ferroelectric layer FEL formed in the region MR are left. After that, the resist pattern RP2 is removed by, for example, an ashing process.
[0088] FIG. 14 shows the process of forming the conductive film FG.
[0089] A conductive film FG made of, for example, polycrystalline silicon doped with n-type impurities is formed by, for example, the CVD method on the metal film MF1 in the region MR and on the gate insulating film GF in the region LR.
[0090] As described above, if the ferroelectric layer FEL can be sufficiently maintained as a rectangular crystal, the metal film MF1 may be removed before the conductive film FG is formed.
[0091] FIG. 15 shows a process for forming the gate electrodes G1 and G2.
[0092] The conductive film FG in the region MR and the region LR is patterned by photolithography and etching. As a result, the gate electrode G1 is formed in the region MR, and the gate electrode G2 is formed in the region LR. Then, by performing etching, the metal film MF1, the ferroelectric layer FEL, and the insulating film IF1 that are not covered by the gate electrode G1 in the region MR are removed, and the gate insulating film GF that is not covered by the gate electrode G2 in the region LR is removed.
[0093] In addition, in the present embodiment, the case where the metal film MF1 is left under the gate electrode G1 (under the conductive film FG) is exemplified, so that the metal film MF1 functions as a part of the gate electrode G1.
[0094] FIG. 16 shows a process for forming the extension regions EX1 and EX2.
[0095] By photolithography and ion implantation, an extension region EX1 which is an n-type impurity region is formed in the well region PW1 at a position aligned with the gate electrode G1 in the region MR, and an extension region EX2 which is an n-type impurity region is formed in the well region PW2 at a position aligned with the gate electrode G2 in the region LR. The extension region EX1 constitutes a part of the source region or a part of the drain region of the ferroelectric memory cell MC, and the extension region EX2 constitutes a part of the source region or a part of the drain region of the MISFET1Q.
[0096] FIG. 17 shows a process of forming the sidewall spacers SW, the diffusion regions D1, D2 and the silicide layer SI.
[0097] First, for example, a silicon oxide film and a silicon nitride film are sequentially formed by, for example, a CVD method so as to cover the gate electrodes G1 and G2. Next, the silicon nitride film is processed by anisotropic etching. After that, the silicon oxide film formed on the upper surface of the gate electrode G1 and the upper surface of the gate electrode G2 is removed. As a result, a sidewall spacer SW made of a laminated film of a silicon oxide film and a silicon nitride film is formed on the side surface of the gate electrode G1 and the side surface of the gate electrode G2.
[0098] Next, by photolithography and ion implantation, a diffusion region D1 which is an n-type impurity region is formed in the well region PW1 at a position aligned with the sidewall spacer SW in the region MR, and a diffusion region D1 which is an n-type impurity region is formed in the well region PW2 at a position aligned with the sidewall spacer SW in the region LR.
[0099] In the region MR, the diffusion region D1 has a higher impurity concentration than the extension region EX1, is connected to the extension region EX1, and forms part of the source region or part of the drain region of the ferroelectric memory cell MC.
[0100] In the region LR, the diffusion region D2 has a higher impurity concentration than the extension region EX2, is connected to the extension region EX2, and constitutes a part of the source region or a part of the drain region of the MISFET1Q.
[0101] Next, a low-resistance silicide layer SI is formed on the upper surfaces of the diffusion region D1, the diffusion region D2, the gate electrode G1 and the gate electrode G2 by a salicide (Self Aligned Silicide) technique.
[0102] Specifically, the silicide layer SI can be formed as follows. First, a metal film for forming the silicide layer SI is formed so as to cover the regions MR and LR. This metal film is made of, for example, cobalt, nickel, or a nickel-platinum alloy. Next, the semiconductor substrate SB is subjected to a first heat treatment at about 300 to 400°C, and then a second heat treatment at about 600 to 700°C, thereby reacting the materials contained in the diffusion region D1, the diffusion region D2, the gate electrode G1, and the gate electrode G2 with the metal film. As a result, the silicide layer SI made of cobalt silicide (CoSi2), nickel silicide (NiSi), or nickel platinum silicide (NiPtSi) is formed on the upper surfaces of the diffusion region D1, the diffusion region D2, the gate electrode G1, and the gate electrode G2. Then, the unreacted metal film is removed.
[0103] Furthermore, when a metal film such as a titanium nitride film, an aluminum film or a tungsten film, or a laminated film obtained by appropriately stacking these films is used as the material constituting the gate electrode G1, after the step of FIG. 17, the polycrystalline silicon film which is the material of the gate electrode G1 can be replaced with the metal film or the laminated film by using a so-called gate last process.
[0104] As a result of the above, a ferroelectric memory cell MC having an MFIS structure is formed in the region MR, and a MISFET 1Q is formed in the region LR.
[0105] After that, the structure shown in FIG. 2 is obtained through the following steps.
[0106] First, an interlayer insulating film IL1 made of, for example, silicon oxide is formed by, for example, a CVD method so as to cover the ferroelectric memory cell MC formed in the region MR and the MISFET1Q formed in the region LR. Next, a plurality of contact holes are formed in the interlayer insulating film IL1 by using a photolithography method and an etching process. Next, a barrier metal film made of, for example, a titanium film, a titanium nitride film, or a laminated film of these is formed in the plurality of contact holes, and a conductive film mainly made of tungsten is formed on the barrier metal film. Next, a plug PG is formed in the contact hole by removing the barrier metal film and the conductive film outside the contact hole by, for example, a CMP method. The plug PG is electrically connected to the diffusion region D1 or the diffusion region D2 via the silicide layer SI. Although not shown, a gate electrode G1 and a plug PG electrically connected to the gate electrode G1 also exist.
[0107] <Comparison between the study example and this embodiment> Fig. 24 shows a semiconductor device of an example studied by the present inventors, and shows a cross-sectional view during a manufacturing process corresponding to Fig. 12 of the present embodiment. That is, Fig. 24 shows a state in which a ferroelectric film FE4 is formed by subjecting an amorphous film to be the ferroelectric layer FEL to a heat treatment for crystallization.
[0108] In the study example, as in the present embodiment, a ferroelectric memory cell MC having a ferroelectric layer FEL is provided, but the ferroelectric layer FEL in the study example is made of a single layer of a ferroelectric film FE4, not a laminated film of a ferroelectric film FE1 and a ferroelectric film FE2 as in the present embodiment, and does not have a plurality of grains GR. In addition, the ferroelectric film FE4 has a first element consisting of hafnium (Hf), oxygen (O), and zirconium (Zr).
[0109] For example, in the case of a hafnium oxide film (HfO2 film), if an amorphous film is deposited by the ALD method or the like and then heat-treated at a high temperature of about 700 to 1000°C, the crystal phase of the HfO2 film becomes monoclinic, and the HfO2 film becomes a paraelectric rather than a ferroelectric. Therefore, by adding a first element made of zirconium (Zr) to the HfO2 film, the ferroelectric film FE4 is easily formed as a rectangular crystal. In addition, by forming a metal film MF1 such as titanium nitride on the amorphous film, the orientation of the ferroelectric film FE4 is easily controlled.
[0110] In the ferroelectric memory cell MC, the threshold voltage is controlled by controlling the reversal of the polarization domain in the ferroelectric layer FEL by applying positive and negative voltages to the gate electrode. Therefore, the threshold voltage variation in the ferroelectric memory cell MC depends greatly on the variation in the crystal grain size and the variation in the crystal orientation of the ferroelectric film FE4. When the number of rewrites of the ferroelectric memory cell MC increases, the film quality in the ferroelectric layer FEL deteriorates, and the magnitude of the variation in the crystal grain size and the variation in the crystal orientation significantly affects the variation in the threshold voltage.
[0111] According to the research of the present inventors, it was found that in the studied example, the variation in crystal grain size and the variation in crystal orientation of the ferroelectric film FE4 were not sufficiently suppressed, and the variation in threshold voltage became larger as the number of times the ferroelectric memory cell MC was rewritten increased.
[0112] In contrast, in the present embodiment, a laminated structure of an amorphous film AM1 and an amorphous film AM2 is adopted when forming the ferroelectric layer FEL, and further, a plurality of grains GR are provided between the amorphous film AM1 and the amorphous film AM2. The radius of the crystal grain size of each of the plurality of grains GR is precisely controlled within a range of, for example, 0.1 nm to 1 nm. Then, in a state in which the metal film MF1 is formed on the amorphous film AM2, the amorphous film AM1, the amorphous film AM2, and the plurality of grains GR are subjected to a heat treatment for crystallization, so that the crystal grain size of each of the ferroelectric film FE1 and the ferroelectric film FE2 is made uniform according to the crystal grain size of the plurality of grains GR. Therefore, the uniformity of the crystal grain size in the ferroelectric layer FEL is improved. In this way, the uniformity of the crystal grain size in the ferroelectric layer FEL can be improved and the crystal orientation can be made uniform to a rectangular crystal.
[0113] When the ferroelectric layer FEL including the ferroelectric film FE1, the ferroelectric film FE2, and the plurality of grains GR thus formed is applied to the ferroelectric memory cell MC, the above-mentioned problem of the large variation in threshold voltage can be suppressed. Therefore, the problem of the decrease in the rewrite resistance of the ferroelectric memory cell MC or the decrease in retention can be suppressed. That is, the technology of this embodiment can improve the performance of the semiconductor device.
[0114] In addition, in this embodiment, electromagnetic waves such as microwaves are used for the heat treatment for crystallization. Heat treatment using microwaves allows crystallization at a lower temperature, for example, at a temperature of 400° C. or less. This makes it easy to form the crystal phase of the ferroelectric film FE1 and the ferroelectric film FE2 as orthorhombic crystals, and makes it easy to form the ferroelectric film FE1 and the ferroelectric film FE2 as ferroelectrics rather than paraelectrics.
[0115] (Modification) A semiconductor device according to a modification of the first embodiment will be described below with reference to Fig. 18. In the following description, differences from the first embodiment will be mainly described.
[0116] Fig. 18 is a graph obtained by an experiment by the inventor of the present application, showing a comparison of temperatures when multiple grains GR are formed by a sputtering method in the process of Fig. 9 of the first embodiment. Here, an example is shown in which aluminum is used as the second element constituting the multiple grains GR. In Fig. 18, the vertical axis shows the diffusion length D of aluminum diffusing into the amorphous film AM1, and the horizontal axis shows the reciprocal (1 / T) of the Kelvin temperature T [K] during the sputtering process.
[0117] In the first embodiment, the temperature when the plurality of grains GR are formed by the sputtering method is set to 300° C. or less, thereby suppressing the diffusion of aluminum, which is the plurality of grains GR, into the amorphous film AM1. Aluminum becomes a crystal nucleus when the amorphous film AM1 and the amorphous film AM2 are crystallized into the ferroelectric film FE1 and the ferroelectric film FE2. Therefore, it is preferable that more crystal nuclei are present near the upper surface of the amorphous film AM1, that is, near the interface between the amorphous film AM1 and the amorphous film AM2. In other words, it is preferable that the aluminum, which is the plurality of grains GR, does not diffuse too much into the amorphous film AM1 when the plurality of grains GR are formed by the sputtering method.
[0118] As can be seen from the graph in Fig. 18, as the formation temperature of the plurality of grains GR decreases, the diffusion length D of the plurality of grains GR decreases. From this graph, the formation temperature of the plurality of grains GR is performed at 1°C or higher, preferably 150°C or lower, more preferably 100°C or lower, and most preferably 27°C (room temperature) or lower.
[0119] In this way, by forming the plurality of grains GR at a lower temperature, the uniformity of the crystal grain size in the ferroelectric layer FEL is further improved, and the crystal orientation can be easily aligned to a rectangular crystal.
[0120] (Embodiment 2) The semiconductor device of the second embodiment will be described below with reference to Fig. 19. In the following description, differences from the first embodiment will be mainly described. Fig. 19 shows a cross-sectional view during the manufacturing process corresponding to Fig. 12 of the first embodiment.
[0121] In the first embodiment, the two-layer structure of the ferroelectric film FE1 and the ferroelectric film FE2 is applied as the ferroelectric layer FEL. In the second embodiment, the three-layer structure of the ferroelectric film FE1, the ferroelectric film FE2, and the ferroelectric film FE3 is applied as the ferroelectric layer FEL.
[0122] FIG. 19 shows a state after heat treatment for crystallization using microwaves or the like, similar to FIG. 12 of the first embodiment.
[0123] First, in the same manner as in the manufacturing process described with reference to FIGS. 8 to 10 in the first embodiment, the amorphous film AM1, the plurality of grains GR, and the amorphous film AM2 are successively formed on the insulating film IF1 in the region MR and the region LR.
[0124] 19, a plurality of grains GR are again formed on the amorphous film AM2 by a sputtering method. Next, an amorphous film (non-crystalline film) AM3 is formed on the plurality of grains GR and the amorphous film AM2 by, for example, an ALD method. The material constituting the amorphous film AM3 is the same as that of the amorphous film AM1 and the amorphous film AM2.
[0125] In the second embodiment, the amorphous film AM1 has a thickness of about 2.5 nm, the amorphous film AM2 has a thickness of about 5 nm, and the amorphous film AM3 has a thickness of about 2.5 nm. That is, the thicknesses of the amorphous films AM1 and AM3 in the second embodiment are each thinner than the thickness of the amorphous film AM1 in the first embodiment, which is 5 nm.
[0126] Next, in the same manner as in the manufacturing process described with reference to FIG. 11 in the first embodiment, a metal film MF1 is formed on the amorphous film AM3.
[0127] Next, in a state where the metal film MF1 is formed on the amorphous film AM3, the amorphous films AM1 to AM3 are crystallized by heat treatment to form the ferroelectric films FE1 to FE3, which are orthorhombic crystals. This forms the ferroelectric layer FEL including the ferroelectric films FE1 to FE3 and the multiple grains GR. This heat treatment can be performed by the RTA method at a temperature of 600°C or less as in the first embodiment, but is preferably performed by microwaves at a temperature of 400°C or less.
[0128] In this way, in the second embodiment, a plurality of grains GR are formed between the amorphous film AM1 and the amorphous film AM2, and between the amorphous film AM2 and the amorphous film AM3. Therefore, in the second embodiment, the number of grains GR that become crystal nuclei is greater than in the first embodiment. Furthermore, since the thicknesses of the amorphous films AM1 and AM3 are thin, the crystal grain sizes of the amorphous films AM1 and AM3 are easily grown in accordance with the crystal grain sizes of the plurality of grains GR. Therefore, in the second embodiment, the uniformity of the crystal grain sizes of the ferroelectric films FE1 to FE3 can be further improved compared to the first embodiment.
[0129] 3, the concentration peaks of aluminum (Al) grains GR are large near the interface between the ferroelectric film FE1 and the ferroelectric film FE2 and near the interface between the ferroelectric film FE2 and the ferroelectric film FE3 in the ferroelectric layer FEL.Then, the concentration peaks of aluminum (Al) are small or absent near the bottom surface of the ferroelectric film FE1, near the center of the ferroelectric film FE2, and near the top surface of the ferroelectric film FE3.
[0130] Thus, the concentration peak of the multiple grains GR is larger at a position close to the first interface between the ferroelectric film FE1 and the ferroelectric film FE2 and at a position close to the second interface between the ferroelectric film FE2 and the ferroelectric film FE3 than at a position close to the bottom surface of the ferroelectric film FE1, at the center of the ferroelectric film FE2, and at a position close to the top surface of the ferroelectric film FE3. Therefore, since the multiple grains GR are present near the first interface between the ferroelectric film FE1 and the ferroelectric film FE2 and at the second interface between the ferroelectric film FE2 and the ferroelectric film FE3, each of the ferroelectric films FE1 to FE3 has a highly uniform crystal grain size and is easily formed as a rectangular crystal.
[0131] Therefore, when the ferroelectric layer FEL is applied to the ferroelectric memory cell MC, the problem of the threshold voltage variation increasing due to the polarization inversion of the ferroelectric layer FEL can be further suppressed, and the problem of the rewrite endurance of the ferroelectric memory cell MC decreasing or the retention decreasing can be further suppressed. That is, the technology of the second embodiment can further improve the performance of the semiconductor device.
[0132] Also in the second embodiment, similarly to the first embodiment, when comparing the ratio of hafnium, the ratio of the first element (Zr, etc.), and the ratio of the second element constituting the plurality of grains GR in the ferroelectric layer FEL, the ratio of the second element is smaller than the ratio of hafnium and the ratio of the first element. Specifically, when the sum of the ratio of hafnium, the ratio of the first element, and the ratio of the second element is taken as 100%, in the ferroelectric layer FEL, the ratio of hafnium is within a range of 30% to 50%, the ratio of the first element is within a range of 30% to 50%, and the ratio of the second element is within a range of 0.5% to 5.0%.
[0133] In the second embodiment, the ferroelectric layer FEL has a three-layer structure consisting of the ferroelectric films FE1 to FE3, but it is also possible to form three or more layers of ferroelectric films and form a plurality of grains GR between the respective ferroelectric films. In this case, it is possible to further improve the uniformity of the crystal grain size in the ferroelectric layer FEL.
[0134] (Embodiment 3) The semiconductor device of the third embodiment will be described below with reference to Fig. 20. In the following description, differences from the first embodiment will be mainly described.
[0135] In the first embodiment, a ferroelectric memory cell MC having an MFIS structure is exemplified, but in the third embodiment, a memory cell having a MFMIS (Metal Ferroelectric Metal Insulator Semiconductor) structure in which a ferroelectric layer FEL is applied to a transistor structure is exemplified as the ferroelectric memory cell MC.
[0136] FIG. 20 is a cross-sectional view corresponding to the time when the step of FIG. 12 in the first embodiment is completed.
[0137] As shown in FIG. 20, in the ferroelectric memory cell MC of the third embodiment, a metal film MF2 is formed between the ferroelectric layer FEL and the insulating film IF1. The metal film MF2 can be formed between the process of FIG. 7 and the process of FIG. 8 of the first embodiment. That is, after the insulating film IF1 is formed in the region MR in FIG. 7, the metal film MF2 is formed on the insulating film IF1 in the region MR and on the gate insulating film GF in the region LR. Thereafter, an amorphous film AM1 is formed on the metal film MF2 in the regions MR and LR by a method similar to the manufacturing method described in FIG. 8. The metal film MF2 is made of the same material as the metal film MF1, and can be formed by the same manufacturing method as the metal film MF1.
[0138] Similarly to the metal film MF1, the metal film MF2 has a function of orienting the crystal phase of each of the ferroelectric films FE1 and FE2 to a rectangular crystal when the amorphous films AM1 and AM2 are crystallized into the ferroelectric films FE1 and FE2. Therefore, the orientation of each of the ferroelectric films FE1 and FE2 is controlled not only by the stress from the metal film MF1 but also by the stress from the metal film MF2. Therefore, in the third embodiment, the stress for controlling the crystal phase of each of the ferroelectric films FE1 and FE2 is large compared to the first embodiment, so that each of the ferroelectric films FE1 and FE2 can be more reliably made into a rectangular crystal.
[0139] Moreover, the technique disclosed in the second embodiment can be applied to the technique disclosed in the third embodiment.
[0140] (Embodiment 4) The semiconductor device of the fourth embodiment will be described below with reference to Fig. 21. In the following description, differences from the third embodiment will be mainly described.
[0141] In the third embodiment, a ferroelectric memory cell MC having an MFMIS structure in which the ferroelectric layer FEL is applied to a transistor structure is exemplified, but in the fourth embodiment, a ferroelectric memory cell MC is configured by forming the ferroelectric layer FEL in a wiring layer and electrically connecting the ferroelectric layer FEL to a MISFET2Q formed on a semiconductor substrate SB.
[0142] Fig. 21 shows only a region MR in which a ferroelectric memory cell MC is formed. As shown in Fig. 21, a MISFET2Q is formed on a semiconductor substrate SB. The MISFET2Q has the same structure as the MISFET1Q of the first embodiment, for example, and is formed by the same manufacturing method as the MISFET1Q.
[0143] A diffusion region D2 which becomes a drain region of the MISFET 2Q is connected to a metal film MF2 via a plug PG. A ferroelectric layer FEL is formed on the metal film MF2, and a metal film MF1 is formed on the ferroelectric layer FEL.
[0144] The polarization inversion of the ferroelectric layer FEL is performed by a voltage supplied from a diffusion region D2 which becomes the drain region of the MISFET 2Q. That is, the MISFET 2Q constitutes the selection transistor of the ferroelectric memory cell MC.
[0145] The ferroelectric layer FEL of such a ferroelectric memory cell MC does not need to be formed on the semiconductor substrate SB, but is formed in the wiring layer, so that the device area of the semiconductor substrate SB can be reduced. Therefore, the ferroelectric memory cell MC of the fourth embodiment is advantageous for miniaturization of the semiconductor chip CHP.
[0146] (Embodiment 5) A semiconductor device according to the fifth embodiment will be described below with reference to Fig. 22 and Fig. 23. In the following description, differences from the first embodiment will be mainly described. Fig. 22 is a perspective view of a ferroelectric memory cell MC according to the fifth embodiment, and Fig. 23 is a cross-sectional view taken along line AA shown in Fig. 22 during the manufacturing process.
[0147] In the first embodiment, the ferroelectric memory cell MC having the MFIS structure, which is a planar transistor, is illustrated on the semiconductor substrate SB, but in the fifth embodiment, a case in which the ferroelectric memory cell MC having the MFIS structure is applied to a fin transistor is illustrated.
[0148] FIG. 22 shows only the region MR in which the ferroelectric memory cells MC are formed, and illustrates a case in which two ferroelectric memory cells MC are formed in a fin FA.
[0149] In a plan view, a fin FA extending in the X direction is formed on the semiconductor substrate SB. Although not shown in the figure, a plurality of such fins FA are formed, and the plurality of fins FA are arranged at equal intervals in the Y direction. The X direction and the Y direction are directions along the main surface of the semiconductor substrate SB, and the X direction is perpendicular to the Y direction. The length of the fin FA in the X direction is longer than the length of the fin FA in the Y direction. In other words, the X direction is the long side direction of the fin FA, and the Y direction is the short side direction of the fin FA. The fin FA is a part of the semiconductor substrate SB, and is a rectangular parallelepiped protruding portion (convex portion) selectively protruding from the upper surface of the semiconductor substrate SB.
[0150] Element isolation parts STI are formed in the semiconductor substrate SB between the multiple fins FA. The position of the upper surface of the element isolation parts STI is lower than the position of the upper surface of the fins FA. In other words, a part of the fin FA protrudes from the element isolation parts STI, and the other part of the fin FA is positioned so as to be sandwiched between the element isolation parts STI in the Y direction. In this way, the upper part of each fin FA is insulated and isolated by the element isolation parts STI.
[0151] The portions of the fins FA that protrude beyond the element isolation parts STI are mainly active regions for forming the ferroelectric memory cells MC. That is, the regions of the semiconductor substrate SB that are partitioned by the element isolation parts STI are the active regions.
[0152] The insulating film IF1 is formed on the upper surface and the side surface of the fin FA, the ferroelectric layer FEL is formed on the insulating film IF1 and the element isolation part STI, and the metal film MF1 is formed on the ferroelectric layer FEL. The gate electrode G1 is formed on the upper surface and the side surface of the fin FA via the metal film MF1, the ferroelectric layer FEL, and the insulating film IF1, and extends in the Y direction.
[0153] A p-type well PW1 is formed in the entire fin FA and in a part of the semiconductor substrate SB. An n-type diffusion region D1 is formed in the fin FA as a drain region and a source region of the ferroelectric memory cell MC. The fin FA sandwiched between two diffusion regions D1 and covered with a gate electrode G1 constitutes a channel region of the ferroelectric memory cell MC. These diffusion regions D1 are regions formed by substantially the same method as the diffusion region D1 of the first embodiment. Here, a case is illustrated in which two ferroelectric memory cells MC adjacent to each other in the X direction share the diffusion region D1.
[0154] In this way, in the fifth embodiment, the ferroelectric memory cells MC are formed by utilizing the upper surface and the side surface of the fin FA. Therefore, the area in which the ferroelectric layer FEL is polarized can be increased in the film thickness direction compared to the ferroelectric memory cells MC of the planar transistor of the first embodiment. Therefore, when the memory capacity of the fifth embodiment is approximately the same as that of the first embodiment, the area occupied by the ferroelectric memory cells MC in the semiconductor substrate SB can be reduced. That is, the semiconductor device can be miniaturized.
[0155] FIG. 23 shows a manufacturing process for a plurality of grains GR in the fifth embodiment, which corresponds to FIG. 9 in the first embodiment.
[0156] 23 indicates the formation of a plurality of grains GR by an ion implantation method. In the fifth embodiment, since the fin FA is applied, it is difficult to form a plurality of grains GR on the amorphous film AM1 formed on the side surface of the fin FA by a sputtering method.
[0157] Therefore, in the fifth embodiment, a plurality of grains GR are introduced into the amorphous film AM1 by oblique ion implantation from the direction along the Y direction in FIG. 22 (the gate width direction of the ferroelectric memory cell MC). This ion implantation is performed, for example, at an angle θ from a perpendicular line to the upper surface of the semiconductor substrate SB. This angle θ is, for example, in the range of 15 degrees or more and 45 degrees or less. In this manner, a plurality of grains GR can be formed on the amorphous film AM1 formed on the upper surface and side surface of the fin FA. Note that the second element constituting the plurality of grains GR, the concentration of the plurality of grains GR, and the like are the same as those in the first embodiment.
[0158] The manufacturing process thereafter is almost the same as in the first embodiment, and therefore a description thereof will be omitted.
[0159] Moreover, the techniques disclosed in the second and third embodiments can also be applied to the technique disclosed in the fifth embodiment.
[0160] The invention made by the inventor of the present application has been specifically described above based on an embodiment, but the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. [Explanation of symbols]
[0161] 1Q MISFET AM1~AM3 Amorphous film C1~C5 circuit D Diffusion length D1, D2 diffusion area EX1, EX2 extension area FA Fin FE1~FE4 Ferroelectric film FEL Ferroelectric layer FG conductive film G1, G2 gate electrodes GF Gate insulating film GR grain IF1 insulating film IL1 Interlayer insulating film LR area MC memory cell MF1, MF2 Metal film MR area PG plug PR1, PR2 resist pattern PW1, PW2 well area SB Semiconductor Substrate SI silicide layer STI element isolation section SW Sidewall spacer T temperature
Claims
1. (a) forming a first amorphous film made of a material including hafnium and oxygen; (b) after the step (a), forming a plurality of grains including a first element selected from the group consisting of aluminum, carbon, nitrogen, fluorine, and titanium on the upper surface of the first amorphous film so as to cover a portion of the upper surface of the first amorphous film and to expose another portion of the upper surface of the first amorphous film; (c) after the step (b), forming a second amorphous film made of a material containing hafnium and oxygen on the upper surface of the first amorphous film so as to cover the plurality of grains and to be in contact with the other part of the upper surface of the first amorphous film that is exposed from the plurality of grains; (d) after the step (c), forming a first metal film on the second amorphous film; (e) after the step (d), a step of performing a heat treatment to crystallize the first amorphous film to form a first ferroelectric film having an orthorhombic crystal structure and to crystallize the second amorphous film to form a second ferroelectric film having an orthorhombic crystal structure; A manufacturing method of a semiconductor device comprising:
2. 2. The method of manufacturing a semiconductor device according to claim 1, each of the first amorphous film and the second amorphous film contains a second element; The second element is one of zirconium, silicon, germanium, yttrium, lanthanum, and ytterbium.
3. 3. The method of manufacturing a semiconductor device according to claim 2, The method for manufacturing a semiconductor device, wherein in the step (e), the heat treatment is performed by a rapid thermal annealing (RTA) method.
4. 3. The method of manufacturing a semiconductor device according to claim 2, In the step (b), the plurality of grains are formed separately from one another, In the step (e), the plurality of grains function as crystal nuclei for the first ferroelectric film and the second ferroelectric film.
5. 4. The method of manufacturing a semiconductor device according to claim 3, In the step (b), the plurality of grains are formed as a plurality of aluminum grains, the step (e) converts the aluminum grains into aluminum oxide grains by the heat treatment, and the aluminum oxide grains function as crystal nuclei of the first ferroelectric film and the second ferroelectric film.
6. 4. The method of manufacturing a semiconductor device according to claim 3, a first metal film that is formed on the first ferroelectric film and a second ferroelectric film that is formed on the second ferroelectric film;
7. 3. The method of manufacturing a semiconductor device according to claim 2, The method for manufacturing a semiconductor device, wherein the step (b) is performed by a sputtering method.
8. 7. The method of manufacturing a semiconductor device according to claim 6, The method for manufacturing a semiconductor device, wherein the step (b) is carried out at a temperature of 1° C. or more and 27° C. or less.
9. 3. The method of manufacturing a semiconductor device according to claim 2, The method for manufacturing a semiconductor device, wherein the step (b) is performed by an ion implantation method.
10. 3. The method of manufacturing a semiconductor device according to claim 2, In the step (b), the surface density of the plurality of grains on the upper surface of the first amorphous film is 5×10 12 / cm 2 ~5×10 14 / cm 2 2. A method for manufacturing a semiconductor device, the method comprising the steps of:
11. 3. The method of manufacturing a semiconductor device according to claim 2, A method for manufacturing a semiconductor device, wherein in the step (e), the heat treatment is performed using microwaves such that an electric field of the microwaves oscillates in a direction perpendicular to an upper surface of the first metal film.
Citation Information
Patent Citations
Ferroelectric film and manufacturing method thereof, ferroelectric capacitor, ferroelectric memory, and manufacturing method thereof
JP2008028197A
Semiconductor memory, and method of manufacturing the same
JP2009212448A
Semiconductor device and dielectric film
JP2015065251A
Insulating film and storage device
JP2017054903A
User interface devices
US20140340372A1