Electrode active material, its manufacturing method, and secondary battery
Surface modification of electrode active materials with phosphoric acid derivatives addresses issues of ion diffusion and electrolyte reactivity, enhancing battery performance by preventing side reactions and improving cycle stability and efficiency.
Patent Information
- Application Number
- JP2020120011
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-13
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-07-13
AI Technical Summary
Electrode active materials in batteries face issues such as slow diffusion of ions, agglomeration during slurry preparation, and side reactions with electrolytes, leading to poor cycle characteristics and low Coulombic efficiency, particularly in magnesium and lithium secondary batteries.
Surface modification of electrode active materials with phosphoric acid or phosphoric acid derivatives forms a thin, dense, and uniform coating that suppresses side reactions and improves adhesion to electrode metal foils, using methods like coprecipitation and heat treatment to enhance uniformity and stability.
The coating prevents side reactions, enhances ion diffusion, and improves charging and discharging characteristics, resulting in better cycle stability and Coulombic efficiency, while maintaining smoothness and adhesion in the electrode structure.
Smart Images

Figure 0007594754000001 
Figure 0007594754000002 
Figure 0007594754000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode active material, a method for producing the same, and a secondary battery. [Background technology]
[0002] One of the ways to improve the electrochemical properties of electrode active materials is surface modification. It is expected that surface modification can suppress side reactions such as oxidative and reductive decomposition of the electrolyte that occur at the active sites on the electrode surface, and improve the Coulombic efficiency, which is the ratio of the discharge capacity to the charge capacity.
[0003] It is known that the cycle characteristics and rate characteristics of the positive electrode active materials of lithium ion secondary batteries and all-solid-state lithium batteries can be improved and surface side reactions suppressed by coating them with various oxides (Non-Patent Documents 1 and 2). It has also been reported that the charge / discharge characteristics and cycle characteristics of positive electrode active materials that have a charge / discharge range of 4.5 V or higher relative to lithium metal can be improved by surface modification using a coupling agent containing a fluoroalkyl group (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2012 / 081348 [Non-patent literature]
[0005] [Non-Patent Document 1] N. Ohta, K. Takada, I. Sakaguchi, L. Zhang, R. Ma, K. Fukuda, M. Osada, T. Sasaki, Electrochem. Commun. 9, 1486 (2007) [Non-Patent Document 2] Z. Chen, Y. Qin, K. Amine, Y.-K. Sun, J. Mater. Chem. 20, 7606 (2010); P. Guan, L. Zhou, Z. Yu, Y. Sun, Y. Liu, F. Wu, Y. Jiang, D. Chu, J. Energy. Chem. 43, 220 (2020) [Non-Patent Document 3] S. Yagi, Y. Ichikawa, I. Yamada, T. Doi, T. Ichitsubo, E. Matsubara, Jpn. J. Appl. Phys. 53, 119201 (2014) [Non-Patent Document 4] K. Ishii, S. Doi, R. Ise, T. Mandai, Y. Oaki, S. Yagi, H. Imai, J. Alloy Compound. 816, 152556 (2020) Summary of the Invention [Problem to be solved by the invention]
[0006] Electrode active materials are the constituent materials of batteries, and many active materials are known that use the insertion and removal of mobile ions to charge and discharge. In the positive electrode active material of magnesium secondary batteries, insertion and removal of magnesium ions occurs. Since magnesium ions diffuse slowly within the active material, in order to improve its properties, it is necessary to nanoparticle the constituent material of the electrode active material and shorten the diffusion distance of the magnesium ions within the particles. On the other hand, when the constituent material of the electrode active material is nanoparticled, water adsorption on the surface becomes significant, which causes aggregation and separation of the slurry when preparing the slurry for producing the coated electrode, making it difficult to apply uniformly. The same problem applies to lithium secondary batteries, and in order to make coating easier, efforts have been made to intentionally aggregate nanoparticles to granulate large particles.
[0007] When materials that are highly reactive to electrolytes, such as manganese or cobalt, are used as the transition metal elements that make up the electrode active material, in addition to the insertion and removal of mobile ions, side reactions such as oxidative and reductive decomposition of the electrolyte, which consists of solvents, supporting salts, additives, etc., become prominent during charging and discharging, making it difficult to charge up to the theoretical capacity and causing problems such as low cycle characteristics and low Coulombic efficiency.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide an electrode active material that can prevent side reactions during charge and discharge and suppress deterioration of charge and discharge characteristics by surface modification of the electrode active material, and to provide a coated electrode that promotes mixing of a slurry containing an electrode active material and has excellent uniformity, smoothness, and binding ability to an electrode metal foil. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention employs the following means.
[0010] (1) An electrode active material according to one embodiment of the present invention comprises, as a main component, a surface-modified active material having reactive properties toward an electrolyte solution and including active material particles made of a compound of a transition metal element, and a first coating covering the surfaces of the active material particles and made of phosphoric acid or a phosphoric acid derivative.
[0011] (2) In the electrode active material described in (1) above, it is preferable that the first coating film is made of a phosphate compound produced by reacting at least one of phosphoric acid, polyphosphoric acid, and derivatives thereof with a part of the transition metal element.
[0012] (3) In the electrode active material according to either of (1) or (2) above, the first coating is a phosphonic acid RPO(OH)2 containing an organic group R, a phosphinic acid R containing organic groups R1 and R2, 1 R 2 It is preferable that the phosphoric acid compound is formed by reacting at least one of PO(OH) and derivatives thereof with a part of the transition metal element.
[0013] (4) In the electrode active material described in (3) above, the phosphonic acid RPO(OH)2 and the phosphinic acid R 1 R 2 It is preferred that PO(OH) and at least one of said derivatives thereof have a hydrocarbon group.
[0014] (5) In the electrode active material described in (4) above, the phosphonic acid RPO(OH)2 and the phosphinic acid R 1 R 2 At least one of PO(OH) and the derivatives thereof preferably contains at least one of a phenyl group, a methyl group, an ethyl group, a propyl group, and a butyl group.
[0015] (6) In the electrode active material according to any one of (1) to (5) above, the surface-modified active material may further include a second coating film covering a surface of the first coating film and made of a compound that is non-reactive with an electrolyte solution.
[0016] (7) In the electrode active material according to any one of the above (1) to (6), the compound of the transition metal element may be capable of inserting and desorbing lithium or magnesium.
[0017] (8) In a secondary battery according to one aspect of the present invention, at least one of a positive electrode active material and a negative electrode active material is the electrode active material according to any one of the above (1) to (7).
[0018] (9) A method for producing an electrode active material according to one embodiment of the present invention is the method for producing an electrode active material described in (7) above, and includes a first step of surface-modifying a powder of a compound of a transition metal element in a solution of a salt of phosphoric acid, phosphonic acid, phosphinic acid, or a derivative thereof, and a second step of recovering the surface-modified powder after washing and drying it.
[0019] (10) The method for producing an electrode active material according to (9) above may further include a third step of heating the dried powder.
[0020] (11) In the method for producing an electrode active material according to either (9) or (10) above, the first step and the second step, or the first step, the second step, and the third step may be repeated in that order. Effect of the Invention
[0021] The electrode active material of the present invention comprises a compound of a transition metal element reactive to an electrolyte as an active material particle, the surface of which is covered with a first coating of phosphoric acid or a phosphoric acid derivative. Therefore, when the electrode active material of the present invention is used as a positive electrode active material or a negative electrode active material of a secondary electrode, it is possible to suppress side reactions during charging and discharging caused by contact of the transition metal element with an electrolyte, and to suppress deterioration of charge and discharge characteristics. In addition, the electrode active material of the present invention controls the surface physical properties by coating the surface with phosphoric acid and its derivatives. Since the binding force between phosphoric acid and transition metal ions is strong and the rate of condensation polymerization between phosphoric acids is slow, dense, thin and uniform surface modification is possible. [Brief description of the drawings]
[0022] [Figure 1] 1 is a cyclic voltammogram of a composite electrode of surface-unmodified active material particles according to Comparative Example 1. [Diagram 2] 4 shows charge / discharge curves of a composite electrode of surface-unmodified active material particles according to Comparative Example 1. [Diagram 3] 1 shows Fourier transform infrared spectra of surface-unmodified active material particles according to Comparative Example 1 and surface-modified active material particles according to Examples 1 and 2. [Figure 4] 4 is a cyclic voltammogram of a composite electrode of the surface-modified active material particles according to Example 1. [Diagram 5] 4 is a cyclic voltammogram of a composite electrode of surface-modified active material particles according to Example 2. [Figure 6] 13 is a cyclic voltammogram of a composite electrode of surface-modified active material particles according to Example 3. [Figure 7] 13 is a cyclic voltammogram of a composite electrode of surface-modified active material particles according to Example 4. [Figure 8] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 3. [Figure 9] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 4. [Figure 10] 13 shows charge / discharge curves of a composite electrode of surface-unmodified active material particles according to Comparative Example 2. [Figure 11] 1(a) and 1(b) are Fourier transform infrared spectra of a powder of surface-unmodified active material particles according to Comparative Example 2 and a powder of surface-modified active material particles according to Examples 5 to 9. [Figure 12] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 5. [Figure 13] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 7. [Figure 14] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 8. [Figure 15] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 9. [Figure 16] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 10. [Figure 17] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 11. [Figure 18] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 12. [Figure 19] 13 shows charge / discharge curves of a composite electrode of surface-modified active material particles according to Example 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, the electrode active material, the secondary battery and the manufacturing method thereof according to the embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. In addition, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and can be appropriately modified and implemented within the scope of the present invention.
[0024] First Embodiment The electrode active material according to the first embodiment of the present invention mainly contains, as a main component, a plurality of surface-modified active material particles each including an active material particle and a first coating covering the surface of the active material particle.
[0025] The active material particles are compounds that contain transition metal elements such as Sc, Ti, V, Cr, Mn, Co, Ni, and Cu, and that can insert and release mobile ions and are reactive to the electrolyte. Examples of mobile ions include lithium ions and magnesium ions. In the electrode active material, a plurality of active material particles are distributed in the form of aggregated porous secondary particles.
[0026] The first coating is made of a phosphoric acid compound produced by reacting at least one of phosphoric acid (H3PO4), polyphosphoric acid, or a derivative thereof with a part of a transition metal element. Examples of phosphoric acid derivatives include phosphate esters.
[0027] Phosphoric acid has the property of strongly bonding with transition metal elements, but the polycondensation between phosphoric acids is slow. Therefore, when phosphoric acid or a phosphoric acid derivative is reacted with a transition metal element, the phosphoric acid quickly bonds to the exposed surface of the transition metal element, but bonds slowly to the phosphoric acid already bonded to the transition metal element. As a result, a thin, dense, and uniform first coating made of phosphoric acid or a phosphoric acid derivative is formed around the active material particles in the secondary particle state.
[0028] The electrode active material can be mainly manufactured through the following steps: First, a powder of a transition metal element compound (e.g., MgCo2O4, MgMn2O4, ZnMn2O4, LiCoO2, LiMn2O4, etc.) prepared by a coprecipitation method or the like is added to a solution of a phosphate source (e.g., diammonium hydrogen phosphate (NH4)2HPO4, triammonium phosphate (NH4)3PO4, etc.) and stirred to perform surface modification (first step).
[0029] Next, the surface-modified powder is washed, recovered, and dried to obtain a surface-modified active material in which the surfaces of the active material particles are modified with phosphoric acid or a phosphoric acid compound (second step). The first step and the second step are sequentially performed once or multiple times to obtain an electrode active material.
[0030] If necessary, the dried sample may be heat-treated (third step). In this case, the first step, the second step, and the third step may be performed once or multiple times in that order to obtain an electrode active material.
[0031] The surface-modified active material may further include a second coating film covering the surface of the first coating film and made of a metal or a compound (oxide) thereof that is non-reactive with the electrolyte. The metal that constitutes the second coating film strongly bonds with the phosphoric acid that constitutes the first coating film, and can also reduce the gap between the phosphoric acid that is bonded to the transition metal element that constitutes the active material particle, thereby improving the coverage of the active material particle. Examples of compounds that are non-reactive with the electrolyte include compounds of iron and aluminum. If necessary, it is also possible to form any number of layers, alternating between phosphoric acid or phosphoric acid compound layers and compound layers, outside the second coating film.
[0032] As described above, the electrode active material according to the present embodiment includes a compound of a transition metal element having reactivity with an electrolyte as an active material particle, and the surface of the active material is covered with a thin, dense, and uniform first coating made of phosphoric acid or a phosphoric acid compound. Therefore, when the electrode active material according to the present embodiment is used as a positive electrode active material or a negative electrode active material of a secondary electrode, it is possible to prevent side reactions during charging and discharging caused by contact of the transition metal element with the electrolyte, and to suppress deterioration of the charge and discharge characteristics.
[0033] Second Embodiment The electrode active material according to the second embodiment of the present invention is similar to the electrode active material according to the first embodiment in that it mainly comprises a plurality of surface-modified active material particles having active material particles and a first coating covering the surfaces of the active material particles, but the first coating is a phosphonic acid RPO(OH)2 containing one organic group R, a phosphinic acid R containing two organic groups R1 and R2, and 1 R 2 It is different in that it is composed of a phosphoric acid compound produced by reacting at least one of PO(OH) and its derivatives with a part of a transition metal element. Examples of the organic groups R, R1, and R2 include an alkyl group, an aryl group, a cycloalkyl group, a haloalkyl group, a vinyl group, an allyl group, and a polyoxyethylene group. The organic groups R1 and R2 may be the same or different from each other.
[0034] At least one of the phosphonic acid, phosphinic acid, and derivatives thereof constituting the first coating preferably has a hydrocarbon group, such as phenyl, methyl, ethyl, propyl, and butyl groups, such as phenylphosphonic acid, diphenylphosphonic acid, methylphosphonic acid, ethylphosphonic acid, propylphosphonic acid, and butylphosphonic acid.
[0035] Even when phosphonic acid, phosphinic acid, or a derivative thereof is used as the phosphate compound, a thin, dense, and uniform first coating can be formed. By covering the surfaces of the active material particles with this first coating, side reactions during charging can be suppressed and deterioration of the charge-discharge characteristics can be suppressed, as in the first embodiment.
[0036] Furthermore, according to this embodiment, the problem of water being adsorbed on the surface of an electrode active material (e.g., MgMn2O4, etc.) produced using a complex polymerization method and agglomerating in the slurry can be solved. That is, according to this embodiment, even if the active material particles have water adsorbed on the surface, such as MgMn2O4, the surface can be made hydrophobic by forming a first coating film made of an organic phosphonic acid, and the adsorption of water molecules can be suppressed. This is because the phenyl group, methyl group, ethyl group, propyl group, and butyl group contained in phosphonic acid and phosphinic acid are all hydrophobic. Therefore, according to this embodiment, a coated electrode excellent in uniformity, smoothness, and binding to an electrode metal foil can be provided. EXAMPLES
[0037] The effects of the present invention will be more clearly understood by using the following comparative examples and examples. Note that the present invention is not limited to the following examples, and can be appropriately modified and implemented without departing from the spirit and scope of the present invention.
[0038] Comparative Example 1 Using MgCo2O4 powder prepared by coprecipitation according to the procedure of Non-Patent Document 3, a composite electrode was prepared by a dry method in the following procedure. 30 mg of active material powder, acetylene black, and polytetrafluoroethylene (PTFE) were weighed out in a weight ratio of 60:30:10, and kneaded in an agate mortar. The obtained mixture was pressed in a state where about 2 mg was supported on a Pt mesh (80 mesh) to prepare a working electrode of the composite electrode.
[0039] The counter electrode was magnesium, the reference electrode was a silver wire immersed in a 0.01M silver nitrate and 0.1M Mg(TFSA)2 solution of triglyme (G3), and the electrolyte was a tetraglyme (G4)-based solvated ionic liquid (0.3M [Mg(G4)(TFSA)2] / Pyr13TFSA). Cyclic voltammetry and charge / discharge measurements were performed at 100°C. The sweep rate of cyclic voltammetry was 0.1mVs. -1 The first sweep was started from the open circuit potential (OCV) toward the negative potential. The charge / discharge measurement was started from the discharge side in constant current mode, with a current value of 10.4 mAg. -1 It was decided.
[0040] Figures 1 and 2 show the cyclic voltammogram and charge / discharge curve of unmodified MgCo2O4. In the cyclic voltammogram in Figure 1, the charge / discharge curve is 3.5V vs. Mg / Mg 2+ An increase in current was observed that was thought to be due to the oxidative decomposition of the electrolyte. In addition, from the charge / discharge curves in Figure 2, it was found that the ratio of the discharge capacity to the charge capacity (Coulomb efficiency) was ~0.5, which is considerably smaller than 1. This is thought to be because part of the charging current was consumed by the decomposition of the electrolyte.
[0041] (Examples 1 and 2) After dissolving 3.8 mmol of (NH4)2HPO4 in 192 mmol of water, 3.8 mmol of MgCo2O4 powder prepared by coprecipitation was added and stirred for 24 hours while heating to 60°C. The resulting suspension was centrifuged, and the precipitate was washed with water and centrifuged five times. The precipitate was then suspended in water, collected, and dried at 100°C for 24 hours.
[0042] After drying, the mixture was crushed in an agate mortar and placed in an alumina boat, and then saturation with simulated air (nitrogen 80 mL min -1 , oxygen 20mL min -1 ) in a tubular atmosphere furnace for 200°C·h -1 After heating to 600°C, the sample was held for 1 hour to obtain the phosphoric acid-modified sample (r P / MCO This procedure was repeated again to obtain the phosphate-modified sample of Example 2 (r P / MCO= 1, × 2) was obtained. Here, r P / MCO is MgC in solution. O2 The molar ratio of P to O4 is shown.
[0043] Figure 3 shows the Fourier transform infrared (ATR-FT-IR) spectra of unmodified MgCo2O4 and phosphoric acid-modified MgCo2O4. The phosphoric acid-modified sample had a peak at 850–1200 cm -1 The absorption band assigned to the PO stretching vibration (ν(PO)) was observed in the phosphate group. The intensity of the PO stretching vibration increased with repeated phosphate modification.
[0044] The results of cyclic voltammetry performed on the phosphoric acid-modified MgCo2O4 of Examples 1 and 2 in the same manner as in Comparative Example 1 are shown in Figures 4 and 5. In both Examples 1 and 2, the phosphoric acid modification resulted in a 3.5 V vs. Mg / Mg 2+ The increase in current was suppressed. Comparing Examples 1 and 2, it can be seen that the inhibitory effect was enhanced by repeating the phosphate modification twice.
[0045] (Examples 3 and 4) After dissolving 2.4 mmol of (NH4)2HPO4 in 555 mmol of water, 2.4 mmol of MgCo2O4 powder prepared by coprecipitation was added and stirred for 24 hours while heating to 60°C. The resulting suspension was centrifuged, and the precipitate was washed with water and centrifuged five times, after which it was suspended in water and collected.
[0046] Next, an aqueous solution of 2.4 mmol of iron nitrate nonahydrate dissolved in 555 mmol of water was added, and the mixture was stirred for 24 hours while being heated to 60°C. The resulting suspension was centrifuged, and the precipitate was washed with water and centrifuged five times. The precipitate was then suspended in water and collected, and dried at 100°C for 24 hours. After drying, the mixture was crushed in an agate mortar and placed in an alumina boat, and sieved in simulated air (nitrogen 80 mL min -1 , oxygen 20mL min -1 ) in a tubular atmosphere furnace at 200°C for -1 The temperature was raised to 600°C and then held for 1 hour to obtain the phosphate-iron composite modified sample (r P-Fe / MCOIn addition, a phosphate-iron composite modified sample (r = 1) of Example 4 was obtained by the same procedure, except that an aqueous solution of 4.8 mmol of (NH4)2HPO4 was added to 555 mmol of water, and then 4.8 mmol of iron nitrate nonahydrate was dissolved in 555 mmol of water. P-Fe / MCO =2).
[0047] The results of cyclic voltammetry performed on the phosphate-iron composite-modified MgCo2O4 of Examples 3 and 4 in the same manner as in Comparative Example 1 are shown in Figures 6 and 7. The results of charge-discharge measurements performed on the MgCo2O4 of Examples 3 and 4 in the same manner as in Comparative Example 1 are shown in Figures 8 and 9. From these results, it is clear that in both Examples 3 and 4, the phosphate-iron composite modification reduces the 3.5V vs. Mg / Mg charge due to the oxidative decomposition of the electrolyte during charging. 2+ It can be seen that the increase in current is suppressed and the coulomb efficiency is improved.
[0048] Comparative Example 2 Charge and discharge measurements were performed on a composite electrode made of unmodified porous MgMn2O4 powder prepared by a dry process using a complex polymerization method according to the procedure in Non-Patent Document 4. The current value for the charge and discharge measurements was 10 mA g -1 The charging time was 270 mA g, which is the theoretical capacity of MgMn2O4. -1 Half of that, 135mA g -1 The other conditions were the same as those in Comparative Example 1.
[0049] Figure 10 shows the charge / discharge curves of unmodified MgMn2O4. During charging, the charge / discharge curve shows a drop of 3.1 to 3.2 V vs. Mg / Mg, which is believed to be due to the oxidative decomposition of the electrolyte. 2+ In addition, it can be seen that in the cycle where the plateau was observed, the coulomb efficiency was significantly smaller than 1 (approximately 0.6).
[0050] A coated electrode was made using acetylene black as a conductive additive and polyvinylidene fluoride (PVDF) as a binder in the following procedure. Acetylene black and N-methylpyrrolidone (NMP) were added to the porous MgMn2O4 powder in that order, and each time they were added, they were kneaded for 10 minutes at 2000 rpm using a planetary mixer. A PVDF NMP solution (PVDF weight fraction 12%) was added to this and kneaded for 10 minutes in the same manner.
[0051] The amount of NMP added was 600μL, the total weight of MgMn2O4, acetylene black, and PVDF was 500mg, and the weight ratio was 80:10:10. The obtained slurry was applied to an aluminum foil at a thickness of 4mil (101.6μm). This was vacuum dried overnight at 80°C using a vacuum dryer to obtain a coated electrode. The coated electrode had poor smoothness, with aggregates observed here and there. In addition, the adhesion to the aluminum foil was weak, and it was easy to peel off.
[0052] (Examples 5 to 9) Porous MgMn2O4 with a surface modified with phosphonic acid or phosphinic acid was prepared. In Examples 5 to 8, the modifying phosphonic acid was methylphosphonic acid (MePA), ethylphosphonic acid (EtPA), n-butylphosphonic acid (BuPA), and phenylphosphonic acid (PhPA), respectively, and in Example 9, the modifying phosphinic acid was diphenylphosphinic acid (Ph2PA).
[0053] After dissolving 1 mmol of phosphonic or phosphinic acid in 1 g of water, 1.5 mmol (Ph2PA) or 2.5 mmol (MePA, EtPA, BuPA, PhPA) of ammonia was added as 10% aqueous ammonia, and the resulting clear solution was dried at 80 °C for 3 h to obtain diammonium phosphonate or ammonium phosphinate.
[0054] The ammonium salt was dissolved in 300 mmol of methanol, and then 2.5 mmol of the porous MgMn2O4 powder prepared by the complex polymerization method was added and stirred for 3 hours. The resulting suspension was centrifuged, and the precipitate was washed with methanol and centrifuged twice, after which the precipitate was suspended in ethanol and collected. The suspension was dried overnight at 60°C to obtain a surface-modified active material powder.
[0055] Figure 11 (a) and (b) show the ATR-FT-IR spectra of unmodified MgMn2O4 and MgMn2O4 modified with phosphonic acid, respectively. In the phosphonic acid modified sample, the absorption band assigned to the PO stretching vibration (ν(PO)) is in the range of 950–1150 cm -1 This indicates that a phosphonic acid layer was formed on the surface of the sample by the surface modification treatment. The absorption intensity of the PO stretching vibration in the diphenylphosphonic acid modified sample was smaller than that of the other samples. In addition, the absorption intensity of the PO stretching vibration in the 3000-3500 cm -1 The broad peak at approximately 3500 cm, which is attributable to the OH stretching vibration (ν(OH)) of adsorbed water, was reduced by the phosphonic acid modification treatment. -1 A peak due to isolated OH groups on the surface appeared at the 100 nm region. These results indicate that the surface of the porous MgMn2O4 was hydrophobized by the organic phosphonic acid modification, and the amount of adsorbed water was reduced.
[0056] 12 to 15 show the results of charge / discharge measurements performed according to the procedure of Comparative Example 2 for porous MgMn2O4 powder modified with methylphosphonic acid (MePA), n-butylphosphonic acid (BuPA), phenylphosphonic acid (PhPA), and diphenylphosphinic acid (Ph2PA), respectively.
[0057] 3.1-3.2V vs. Mg / Mg, which is thought to be due to oxidative decomposition of the electrolyte 2+ The plateau of the β-amino acid modification was shorter than that of the unmodified sample and almost disappeared in the butylphosphonic acid and phenylphosphonic acid modified samples. The coulombic efficiency of the β-amino acid and phenylphosphonic acid modified samples was almost 1.
[0058] When a coated electrode was prepared for the phenylphosphonic acid modified sample according to the procedure of Comparative Example 2, the surface was smooth, no aggregates were observed, and the adhesion to the aluminum foil was good.
[0059] (Examples 10 to 12) In addition, a coated electrode was prepared using carbon nanotubes (CNT) as a conductive additive and polyvinylidene fluoride (PVDF) as a binder, as follows: NMP and a CNT NMP dispersion (CNT weight fraction 4%) were added to the phenylphosphonic acid-modified porous MgMn2O4 powder in that order, and after each addition, the mixture was kneaded for 10 minutes at 2000 rpm using a planetary centrifugal mixer. A PVDF NMP solution (PVDF weight fraction 12%) was added to this and kneaded for 10 minutes in the same manner.
[0060] The amount of NMP added was 300 μL, the total weight of MgMn2O4, CNT, and PVDF was 150 mg, and the weight ratio was 98-w CNT :w CNT :2(w CNT = 0.5, 1.0, 2.0). CNT The cases where the ratio was 0.5, 1.0, and 2.0 were designated Examples 10 to 12. All of the coated electrodes were smooth, no aggregates were observed, and the adhesion to the aluminum foil was also good.
[0061] About 2 mg of the obtained slurry was supported on a Pt mesh (80 mesh), vacuum dried overnight at 80°C, and pressed to prepare a composite electrode. Using this composite electrode as the working electrode, charge / discharge measurements were performed according to the procedure of Comparative Example 2. The results are shown in Figures 16 to 18. CNT The composite electrode with wCNT = 2.0% had a charge / discharge capacity comparable to that of the acetylene black composite electrode (Figure 13). On the other hand, the capacity of the composite electrode with wCNT ≦ 1% was small, but this is thought to be due to the low CNT content and insufficient current collection. These results show that CNT can be used as a conductive additive in the surface-modified MgMn2O4, and that the weight fraction of the positive electrode active material in the positive electrode can be increased to 96%.
[0062] (Example 13) A coated electrode of phenylphosphonic acid-modified porous MgMn2O4 powder was prepared in the same manner as in Examples 10 to 12. The amount of NMP added was 800 μL, the total weight of CNT and PVDF was 400 mg, and the weight ratio was 92:4:4. The obtained coated electrode was smooth, no aggregates were observed, and the adhesion to the aluminum foil was good.
[0063] A 2032-type coin cell was fabricated consisting of a coated electrode positive electrode, an AZ31 alloy negative electrode, a glass fiber separator, and a 0.3M Mg[B(HFIP)4]2 / G3 electrolyte, and a current value of 10 mAg was applied. -1 A constant current charge / discharge test was performed at 25°C. The charge / discharge curve is shown in Figure 19. The initial discharge capacity was 70mAhg. -1 No significant capacity degradation was observed even after four charge / discharge cycles.
[0064] Comparative Example 3 190mg (2mmol) of anhydrous magnesium chloride was dissolved in a mixed solvent of 25mL of methanol and 25mL of ethylene glycol dimethyl ether, and 723mg (2mmol) of tetrabutylammonium permanganate was added. After stirring for 30 minutes, water was added, centrifuged, washed, and dried to synthesize MgMn2O4 powder. The molar ratio of Mg:Mn in MgMn2O4 obtained by SEM-EDX analysis was 28.0:72.0.
[0065] The resulting MgMn2O4 powder (30 mg) was mixed with acetylene black and polytetrafluoroethylene (PTFE) in a weight ratio of 60:30:10 to obtain a composite electrode (4 mg). The electrode was pressed onto an Al mesh (10 mmφ, 100 mesh) to prepare a positive electrode. The electrode was vacuum dried overnight at 120°C and then placed in a glove box. A 2032-type coin cell was prepared consisting of an AZ31 alloy negative electrode, a glass fiber separator, and a 0.3M Mg[B(HFIP)4]2 / G3 electrolyte, and a current value of 10 mAg was measured. -1 A constant current discharge test was performed at 25°C with a discharge end potential of 0.1 V. The initial discharge capacity was 25 mAhg -1 It was.
[0066] Example 14 To 7 g (10 mmol) of tetrabutylammonium hydroxide (37% methanol solution), 790 mg (5 mmol) of phenylphosphonic acid was added and stirred for 1 hour, and then the solvent was removed by evaporation to obtain 3 g of ditetrabutylammonium phenylphosphonate.
[0067] 190 mg (2 mmol) of anhydrous magnesium chloride was dissolved in a mixed solvent of 25 mL of methanol and 25 mL of ethylene glycol dimethyl ether, and 723 mg (2 mmol) of tetrabutylammonium permanganate was added. After stirring for 30 minutes, 135 mg (0.2 mmol) of ditetrabutylammonium phenylphosphonate was added and stirred for another 30 minutes. Water was added to the reaction solution, which was then centrifuged, washed, and dried to synthesize phenylphosphonic acid-modified MgMn2O4 powder.
[0068] The molar ratio of Mg:Mn:P of the phenylphosphonic acid modified MgMn2O4 obtained by SEM-EDX analysis was 28.7:64.9:6.3. As in Comparative Example 3, the charge-discharge measurement of the phenylphosphonic acid modified MgMn2O4 was performed. The initial discharge capacity was 29 mAhg -1 It was.
Claims
1. active material particles having a reactivity with an electrolyte and made of a compound of a transition metal element; The active material includes, as a main component, a surface-modified active material having a first coating film made of phosphoric acid or a phosphoric acid derivative, the first coating film covering the surfaces of the active material particles, The electrode active material is characterized in that the first coating comprises a phosphoric acid compound produced by reacting at least one of a phosphonic acid RPO(OH)2 containing an organic group R, a phosphinic acid R1R2PO(OH) containing organic groups R1 and R2, and a derivative thereof with a portion of the transition metal element.
2. The phosphonic acid RPO(OH) 2 , the phosphinic acid R 1 R 2 2. The electrode active material according to claim 1, wherein PO(OH) and at least one of the derivatives thereof have a hydrocarbon group.
3. The phosphonic acid RPO(OH) 2 , the phosphinic acid R 1 R 2 3. The electrode active material according to claim 2, wherein PO(OH) and at least one of the derivatives thereof contain at least one of a phenyl group, a methyl group, an ethyl group, a propyl group, and a butyl group.
4. The electrode active material according to any one of claims 1 to 3, characterized in that the surface-modified active material further comprises a second coating film covering a surface of the first coating film and made of a compound having non-reactivity with an electrolyte.
5. 5. The electrode active material according to claim 1, wherein the compound of the transition metal element is capable of inserting and desorbing lithium or magnesium.
6. A secondary battery, characterized in that at least one of a positive electrode active material and a negative electrode active material is the electrode active material according to any one of claims 1 to 5.
7. A method for producing an electrode active material according to claim 5, A first step of surface-modifying a powder of a compound of a transition metal element in a solution of a salt of phosphoric acid, phosphonic acid, phosphinic acid, or a derivative thereof; and a second step of washing the surface-modified powder, recovering it, and drying it.
8. 8. The method for producing an electrode active material according to claim 7, further comprising a third step of heating the dried powder.
9. The method for producing an electrode active material according to claim 8, characterized in that the first step and the second step, or the first step, the second step, and the third step are sequentially repeated.
Citation Information
Patent Citations
Composite material for electrode and method for producing the same, and lithium ion battery employing the composite material for electrode
JP2012084506A
Positive electrode active material for lithium secondary cell, positive electrode for lithium secondary cell, lithium secondary cell, and method for manufacturing them
JP2017010923A
Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2019003801A
Positive electrode active material for secondary cells
WO2012081348A1
Active material with excellent high-voltage properties
WO2014115559A1