Silicon composite oxide for negative electrode material of lithium secondary batteries and its manufacturing method

A silicon composite oxide with a core-shell structure and carbon coating addresses the volume change issue in silicon-based electrodes, enhancing capacity and retention rates in lithium secondary batteries.

JP7594790B2Active Publication Date: 2024-12-05DAEJOO ELECTRONICS MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021564129
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-29
Filing Date
2020-04-29
Publication Date
2024-12-05
Estimated Expiration
2040-04-29

AI Technical Summary

Technical Problem

Existing silicon-based negative electrode materials for lithium secondary batteries suffer from high volume change during charging and discharging, leading to capacity retention issues and instability due to irreversible reactions, which limits their performance and efficiency.

Method used

A silicon composite oxide is formed with a core-shell structure containing Si clusters and Mg silicate (MgSiO4 and MgSiO3) around the Si clusters, achieved by reacting silicon, silicon oxide, and magnesium in a gaseous state, followed by a carbon coating to enhance stability and capacity retention.

Benefits of technology

The silicon composite oxide exhibits higher capacity and significantly improved capacity retention rates compared to conventional materials, with reduced volume changes and increased initial charge/discharge efficiency, making it suitable for advanced lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594790000004
    Figure 0007594790000004
  • Figure 0007594790000005
    Figure 0007594790000005
  • Figure 0007594790000006
    Figure 0007594790000006
Patent Text Reader

Abstract

The present invention relates to a silicon composite oxide for use as an anode material in lithium secondary batteries and a method for producing the same, and more particularly to a silicon composite oxide for use as an anode material in lithium secondary batteries, which contains Si clusters and MgSiOy (0≦x≦3, 0≦y≦5) formed around the Si clusters, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silicon composite oxide for a negative electrode material of a lithium secondary battery and a method for producing the same, and more particularly, to Si clusters in particles and Mg formed in the peripheral portion of the Si clusters x SiO y (0 < x ≦ 3, 0 < y ≦ 5), and a method for producing the same.

Background Art

[0002] In miniaturization and high performance of portable devices, and further in electric vehicles and large-capacity energy storage industries, the need for secondary batteries is increasing, and the demand for improving the performance of lithium secondary batteries is also increasing. In order to increase the energy density, research and development are being carried out, such as increasing the capacity of the positive and negative electrode active materials, increasing the density of the electrode plate, thinning the separator membrane, and increasing the charge and discharge voltage.

[0003] However, thinning the separator membrane, increasing the density of the electrode plate, and increasing the charge and discharge voltage may cause fatal problems in the stability of the secondary battery, and since the current technical limit has been reached, the research and development direction is towards increasing the capacity of the positive and negative electrode active materials.

[0004] As the negative electrode active material, materials that can exhibit a capacity several times or more higher than the theoretical capacity (372 mAh / g) of existing graphite-based materials have been reported. Conventionally, as the negative electrode active material of lithium secondary batteries, carbon-based, silicon-based, tin-based, transition metal oxides, etc. have been mainly studied and developed. However, the negative electrode active materials developed so far have not reached a satisfactory level in terms of capacity, initial charge and discharge efficiency, expansion rate, and life characteristics, so there is still room for improvement.

[0005] In particular, materials such as Si, Ge, and Sn have attracted attention as new anode materials due to their high theoretical capacity. Among them, silicon has a high capacity performance of 4,200mAh / g, and is attracting attention as a next-generation alternative to carbon-based anode materials. However, in the case of silicon, 44 lithium atoms are required per silicon, which forms an alloy and shows high capacity, but this brings about a volume change of about 300% or more. This volume change causes pulverization of the anode active material due to repeated charging and discharging, and causes the anode active material to be electrically detached from the current collector. This electrical detachment significantly reduces the capacity retention rate of the battery.

[0006] To solve the above problems, a technology has been proposed in which silicon is combined with carbon by mechanical milling and the surface of the silicon particles is coated with a carbon layer by chemical vapor deposition (CVD) (Patent Document 1). However, this technology has limitations in terms of suppressing the expansion and contraction of the volume during charging and discharging. x Although its capacity is smaller than that of silicon, it has a capacity (approximately 1,500 mAh / g) that is several times higher than the capacity of carbon-based anodes (approximately 350 mAh / g). Because it has a structure in which silicon nanocrystals are uniformly dispersed in a silicon dioxide matrix, it is in the spotlight as a material with dramatically improved volume expansion rate and lifespan (capacity retention rate) characteristics compared to other silicon-based materials.

[0007] Silicon oxide, which has excellent capacity and life characteristics, reacts with lithium during initial charging to produce lithium oxide (including lithium oxide and lithium silicate), but the lithium oxide produced cannot reversibly return to the positive electrode during discharge. This irreversible reaction causes lithium to be lost, and the initial charge-discharge efficiency (ICE) drops to 75% or less, requiring an excessive positive electrode capacity when designing a secondary battery. This causes a problem in that the capacity per unit mass of the negative electrode is offset in actual batteries. Silicon oxide (SiO x As a method for improving the initial charge-discharge efficiency of xis reacted with metallic lithium powder to obtain Si-SiO x However, this method has the problem that, although it improves the initial efficiency, it reduces the battery capacity, the stability of the paste during electrode production is reduced, and handling is difficult, making industrial production difficult.

[0008] In order to improve the stability during electrode fabrication, SiO x A method has been proposed in which a silicon-silicon oxide composite is mixed with a magnesium compound and heated to improve the initial charge-discharge efficiency. x A Si-SiO2-Mg2-SiO4-carbon composite was produced by reacting SiOx with magnesium nitrate (Mg(NO3)2), but the discharge capacity was low at 900mAh / g and the initial charge / discharge efficiency was low at 73%. This is because magnesium nitrate was used as the magnesium precursor, and the reaction with SiOx produced a large amount of amorphous SiO2 and MgO, which meant that the irreversible reaction was not suppressed and the charge / discharge capacity did not reach the expected level.

[0009] In addition, SiO x In order to reduce the irreversible capacity of x A method for producing a magnesium- or calcium-containing silicon-silicon oxide composite by reacting a powder with magnesium hydride (MgH2) or calcium hydride (CaH2) has been reported (Patent Document 4). x During the reaction of the powder with MgH2 or CaH2, the amount of oxygen mixed in is reduced, but the size of the silicon crystals grows rapidly due to a localized exothermic reaction, and Mg or Ca is distributed unevenly, resulting in the formation of SiO x It was shown that the capacity retention rate decreased with increasing the temperature. Summary of the Invention [Problem to be solved by the invention]

[0010] In order to solve the above-mentioned problems of the conventional technology, the present invention provides a Si / SiO xBy evaporating a mixture of a / SiO2 raw material powder and magnesium and reacting them in a gaseous state, Si clusters are formed inside the particles during the particle formation process, and Mg is formed at the periphery of the Si clusters. x SiO y An object of the present invention is to provide a silicon composite oxide for a negative electrode material of a lithium secondary battery having a new structure that exhibits a high capacity and has a high capacity retention rate by including (0 < x ≤ 3, 0 < y ≤ 5).

[0011] Another object of the present invention is to provide a method for producing a silicon composite oxide for a negative electrode material of a lithium secondary battery according to the present invention.

Means for Solving the Problems

[0012] In order to solve the above problems, the present invention provides Si clusters and Mg formed at the periphery of the Si clusters. x SiO y A silicon composite oxide for a negative electrode material of a lithium secondary battery containing a magnesium silicate represented by (0.5 ≤ x ≤ 2, 2.5 ≤ y ≤ 4) is provided.

[0013] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the Si clusters and Mg formed at the periphery of the Si clusters. x SiO y (0.5 ≤ x ≤ 2, 2.5 ≤ y ≤ 4) can form a core-shell structure.

[0014] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the domain size of Si(220) of the Si clusters can be 12 nm or less.

[0015] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention may exhibit a peak attributed to Si crystals in the range of diffraction angle 28° < 2θ < 29° and a peak attributed to MgSiO3 crystals in the range of diffraction angle 30.5° < 2θ < 31.5° during X-ray diffraction pattern analysis.

[0016] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, when analyzing the X-ray diffraction pattern, the full width at half maximum (FWHM (deg)) of Si(111) due to the above Si clusters can be 0.7 to 1.5 (deg).

[0017] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention contains Mg2SiO4 (forsterite) crystals, and the content of the above Mg2SiO4 (forsterite) crystals can be less than the content of MgSiO3 (orthoenstatite) crystals.

[0018] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the peak intensity ratio I Mg2SiO4 / I MgSiO3 between the Mg2SiO4 (forsterite) crystal phase and the MgSiO3 (orthoenstatite) crystal phase of the above silicon composite oxide can be 0 to 0.5 or less.

[0019] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention can contain Mg in a proportion of 2 to 15 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight in total.

[0020] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention can include a carbon coating on the surface.

[0021] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the average thickness of the above carbon coating can be 5 to 100 nm.

[0022] The present invention also provides a step of mixing silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture; the above Si / SiO x / SiO2 raw material powder mixture and metallic magnesium are each evaporated, reacted, and then deposited to form a composite oxide; a step of cooling the formed silicon composite oxide; and The step of pulverizing the above-mentioned cooled silicon composite oxide; Provided is a method for producing a silicon composite oxide for a secondary battery negative electrode material according to the present invention, which includes the above steps.

[0023] The method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention may further include the step of coating the surface of the pulverized silicon composite oxide with carbon.

[0024] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, the above silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder are mixed to form Si / SiO x / SiO2 raw material powder mixture, in the step of preparing the Si / SiO x / SiO2 raw material powder mixture, the molar ratio of O / Si may be 0.9 to 1.1.

[0025] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, the above silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder are mixed to form Si / SiO x / SiO2 raw material powder mixture, in the step of preparing the Si / SiO 2 / SiO2 raw material powder mixture, the average particle size and specific surface area of the silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder mixed as the above raw materials may be 10 nm to 100 μm, 5 to 500 m

[0026] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, after the step of mixing silicon powder, silicon oxide (SiO x , 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture is performed, the step of heat-treating the Si / SiO x / SiO2 raw material powder mixture at 800 to 1100 °C and normal pressure for 1 to 3 hours may further be included.

[0027] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and reacting the Si / SiO raw material powder mixture and metallic magnesium, the Si / SiO x The / SiO2 raw powder mixture and metallic magnesium can be vaporized in separate reactors and reacted in a gaseous state.

[0028] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and reacting the Si / SiO raw material powder mixture and metallic magnesium, the Si / SiO x The / SiO2 raw powder mixture can be evaporated at 1000-1600°C under a pressure of 0.001-5 torr.

[0029] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and depositing the / SiO2 raw material powder mixture and metallic magnesium, the metallic magnesium can be evaporated at 700 to 1000° C. under a pressure of 0.001 torr to 2 torr.

[0030] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, in the step of coating the surface with carbon, the silicon composite oxide can be reacted in a gaseous state with at least one carbon precursor selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene at 600 to 1200°C.

[0031] The present invention also provides a negative electrode for a lithium secondary battery, comprising the silicon composite oxide for use in a negative electrode material for a secondary battery according to the present invention.

[0032] The present invention also provides a lithium secondary battery including a negative electrode for a lithium secondary battery comprising the silicon composite oxide for use in a negative electrode material for a secondary battery according to the present invention.

[0033] In a lithium secondary battery including a negative electrode for a lithium secondary battery comprising the silicon composite oxide for use as a negative electrode material for secondary batteries of the present invention, the peak intensity at about 0.45 V in the dQ / dV curve is greater than the peak intensity at 0.25 V after two charge cycles.

[0034] The lithium secondary battery including the negative electrode for lithium secondary batteries of the present invention is discharged twice, and then Mg x SiO y It is possible that no XRD peaks originating from Effect of the Invention

[0035] The silicon composite oxide for secondary battery negative electrode material of the present invention forms Si clusters within the particles and also forms Mg around the Si clusters. x SiO y This is a silicon composite oxide for use as a negative electrode material in lithium secondary batteries, which has a new structure containing (0≦x≦3, 0≦y≦5), and which exhibits higher capacity than conventional silicon-based negative electrode materials for secondary batteries and also has an extremely high capacity retention rate. [Brief description of the drawings]

[0036] [Figure 1] 3 shows the results of TEM-EDX analysis of a cut specimen of a silicon composite oxide for a negative electrode material of a lithium secondary battery produced in one embodiment of the present invention. [Diagram 2] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Diagram 3] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 4] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Diagram 5] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 6] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 7] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 8] 1 shows the results of XRD analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 9] 1 shows the results of XPS analysis of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in examples and comparative examples of the present invention. [Figure 10] FIG. 1 shows a schematic diagram of components on a cross section of silicon composite oxide for anode materials of lithium secondary batteries produced in an example of the present invention and a comparative example. [Figure 11] 1 shows the results of measuring the electrochemical characteristics of batteries including negative electrode materials of an example of the present invention and Comparative Example 3. [Figure 12] 1 shows the results of measuring the electrochemical characteristics of batteries including negative electrode materials of an example of the present invention and Comparative Example 3. [Figure 13] 1 shows the results of Ex-Situ XRD measurement of electrodes after charging and discharging of batteries including negative electrode materials according to an embodiment of the present invention and a comparative example. [Figure 14] 1 shows the results of XRD measurement after 100 cycles for silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in an example of the present invention and a comparative example. [Figure 15] 1 shows the results of STEM measurement of silicon composite oxides for use as negative electrode materials for lithium secondary batteries produced in an example of the present invention and a comparative example. [Figure 16] 1 shows the results of TEM, STEM-HAADF, and STEM-EDS measurements before and after charging and discharging batteries including negative electrode materials of an example of the present invention and Comparative Example 3. [Figure 17] FIG. 2 is a schematic diagram showing the structural change before and after charging and discharging the batteries including the negative electrode materials of an example of the present invention and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] The present invention will be described in detail below with reference to examples. The following examples are merely illustrative of the present invention, and the scope of the present invention is not limited to these examples.

[0038] As used herein, terms such as "comprises" should be understood as open-ended terms that include the possibility of including other embodiments, unless otherwise stated in the phrase or sentence in which the term contains the term.

[0039] As used herein, the words "preferred" and "preferably" refer to embodiments of the invention that may offer certain advantages, under particular circumstances. However, other embodiments may also be preferred, under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.

[0040] The silicon composite oxide for use as a negative electrode material for lithium secondary batteries according to the present invention will be described in detail below.

[0041] The present invention relates to a Si cluster and Mg x SiO y The present invention provides a silicon composite oxide for use as a negative electrode material for lithium secondary batteries, which contains magnesium silicate represented by (0.5≦x≦2, 2.5≦y≦4).

[0042] A cross section of the silicon composite oxide for use as a negative electrode material for lithium secondary batteries according to the present invention is shown in Fig. 1. As shown in Fig. 1, the silicon composite oxide for use as a negative electrode material for lithium secondary batteries according to the present invention contains clusters in which the concentration of Si is non-uniformly aggregated within the particles, and magnesium silicate Mg x SiO y It can be confirmed that (0.5≦x≦2, 2.5≦y≦4) is included.

[0043] The silicon composite oxide for use as a negative electrode material for lithium secondary batteries of the present invention is the above-mentioned Si / SiO x The mixture of raw SiO2 powder and metallic magnesium is evaporated to react in a gaseous state. The raw materials are melted at high temperature and evaporated in a solid solution state by reducing pressure. When the raw materials are cooled after reacting in a gaseous state, phase separation between the products proceeds, and the Si clusters and the surrounding Mg x SiO y An interface may be formed where (0.5≦x≦2, 2.5≦y≦4).

[0044] Therefore, the silicon composite oxide for lithium secondary battery negative electrode material of the present invention is a magnesium silicate formed in the Si clusters and the periphery of the Si clusters, which is not formed at all by the conventional technique of doping magnesium after forming a silicon composite. x SiO y (0.5≦x≦2, 2.5≦y≦4).

[0045] The silicon composite oxide for use as a negative electrode material for lithium secondary batteries of the present invention is a material that is formed by combining the above-mentioned Si clusters and the Mg x SiO y (0.5≦x≦2, 2.5≦y≦4) can form a core-shell structure.

[0046] In the silicon composite oxide for use as a negative electrode material for lithium secondary batteries of the present invention, the domain size of the Si(220) of the Si cluster may be 12 nm or less.

[0047] Furthermore, in the X-ray diffraction pattern analysis of the silicon composite oxide for use as a negative electrode material for lithium secondary batteries of the present invention, a peak attributable to Si crystals appears in the diffraction angle range of 28°<2θ<29°, and a peak attributable to MgSiO3 crystals may appear in the diffraction angle range of 30.5°<2θ<31.5°.

[0048] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, when performing X-ray diffraction pattern analysis, the full width at half maximum (FWHM (deg)) of Si(111) by the above Si clusters can be 0.7 to 1.5 (deg).

[0049] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention contains Mg2SiO4 (forsterite) crystals, and the content of the above Mg2SiO4 (forsterite) crystals can be less than the content of MgSiO3 (orthoenstatite) crystals. In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the peak intensity ratio I Mg2SiO4 / I MgSiO3 of the Mg2SiO4 (forsterite) crystal phase and the MgSiO3 (orthoenstatite) crystal phase of the above silicon composite oxide can be 0 to 0.5 or less.

[0050] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention can contain Mg in a proportion of 2 to 15 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight in total.

[0051] The silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention can include a carbon coating on the surface.

[0052] In the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention, the average thickness of the above carbon coating can be 5 to 100 nm.

[0053] Hereinafter, the manufacturing method of the silicon composite oxide for a negative electrode material of a lithium secondary battery of the present invention will be described in detail.

[0054] The present invention mixes silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture; evaporates and reacts the above Si / SiO x / SiO2 raw material powder mixture and metallic magnesium respectively, and then deposits them to form a composite oxide. The step of cooling the formed silicon composite oxide; and The step of pulverizing the cooled silicon composite oxide; A method for producing a silicon composite oxide for a secondary battery negative electrode material according to the present invention, which includes the above steps is provided.

[0055] The method for producing a silicon composite oxide for a secondary battery negative electrode material according to the present invention may further include a step of coating the surface of the pulverized silicon composite oxide with carbon.

[0056] In the method for producing a silicon composite oxide for a secondary battery negative electrode material according to the present invention, in the step of mixing the silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture, the Si / SiO x / SiO2 raw material powder mixture can be dry-mixed and stirred.

[0057] In the method for producing a silicon composite oxide for a secondary battery negative electrode material according to the present invention, in the step of mixing the silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture, the molar ratio of O / Si in the Si / SiO x / SiO2 raw material powder mixture can be 0.9 to 1.1. When the molar ratio of O / Si in the Si / SiO x / SiO2 raw material powder mixture is 0.9 or less, or 1.1 or more, the yield of the silicon composite oxide may be significantly reduced.

[0058] Also, the surface of the silicon powder may be in an oxidized state. The surface of the silicon powder may be oxidized by oxygen in the air during the manufacturing process, and the oxygen content of the silicon powder is not limited. If the oxygen content is 50% by weight or less based on the entire silicon powder, it is easier to adjust the O / Si molar ratio, and more preferably, it is 30% by weight or less.

[0059] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, in the Si / SiO x / SiO2 raw material powder mixture, the silicon oxide powder can be contained in an amount of 30% by weight or more, preferably 50% or more, more preferably 70% by weight or more, based on the total amount of the raw material powder mixture.

[0060] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, by including SiO x even when the raw materials are dry-mixed in a powder state and used, it is possible to adjust the reaction rate and produce a product of uniform quality. If the content of the silicon oxide powder is 30% by weight or less, when the raw material powder mixture is evaporated under heating and reduced pressure and reacted with magnesium vapor, it is difficult to adjust the evaporation rate of silicon oxide depending on the reaction time, so a uniform quality cannot be obtained, and the yield of the reaction product may decrease. Also, in order to increase the evaporation rate of the raw material powder mixture, there is a disadvantage that a higher evaporation temperature is required.

[0061] Also, the average particle size and specific surface area of the silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder mixed as the above raw materials are not particularly limited, and are preferably 10 nm to 100 μm, 5 to 500 m 2 / g.

[0062] In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, after performing the step of mixing silicon powder, silicon oxide (SiOx, 0.9 < x < 1.1) powder, and silicon dioxide powder to prepare a Si / SiO x / SiO2 raw material powder mixture, the method may further include the step of heat-treating the Si / SiO x / SiO2 raw material powder mixture. In the method for producing a silicon composite oxide for a secondary battery negative electrode material of the present invention, in the step of heat-treating the Si / SiO x / SiO2 raw material powder mixture, by performing heat treatment on the raw material powder mixture at 800 to 1100 °C and normal pressure for 1 to 3 hours, the compositional uniformity of the raw material powder mixture can be enhanced.

[0063] The heat treatment is preferably carried out in an atmosphere of an inert gas such as argon, nitrogen, or helium, or a reducing gas such as hydrogen. In an oxidizing gas atmosphere, the silicon powder and silicon oxide powder may be oxidized, resulting in a decrease in yield.

[0064] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and reacting the Si / SiO raw material powder mixture and metallic magnesium, the Si / SiO x The Si / SiO2 raw material powder mixture and metallic magnesium are vaporized in separate reactors, and reacted in a gaseous state. x The mixture of the raw material powder of SiO2 and metallic magnesium is heated and evaporated in separate reactors, and then reacted in a gaseous state to form the silicon composite oxide for the secondary battery anode material, which is composed of Si clusters and Mg formed around the Si clusters. x SiO y It may have a structure containing magnesium silicate represented by (0.5≦x2, 2.5≦y≦4).

[0065] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x The evaporation of the / SiO2 raw powder mixture and metallic magnesium can be carried out at 800 to 1600°C under a pressure of 0.001 to 2 torr.

[0066] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and depositing the Si / SiO raw material powder mixture and metallic magnesium, x The / SiO2 raw powder mixture can be performed at 1000-1600° C. under a pressure of 0.001-2 torr.

[0067] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, the Si / SiO x In the step of forming a composite oxide by evaporating and depositing the SiO2 / SiO2 raw material powder mixture and metallic magnesium, the metallic magnesium may be evaporated and deposited at a temperature of 800 to 1000° C. under a pressure of 0.001 torr to 2 torr.

[0068] In the method for producing a silicon composite oxide for use as a secondary battery negative electrode material of the present invention, in the step of coating the surface with carbon, the silicon composite oxide can be reacted in a gaseous state with at least one carbon precursor selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene at 600 to 1200°C.

[0069] The present invention also provides a negative electrode for a lithium secondary battery, comprising the silicon composite oxide for use in a negative electrode material for a secondary battery according to the present invention.

[0070] The present invention further provides a lithium secondary battery including a negative electrode for a lithium secondary battery comprising the silicon composite oxide for use in a negative electrode material for a secondary battery according to the present invention.

[0071] In a lithium secondary battery including a negative electrode for a lithium secondary battery comprising the silicon composite oxide for use as a negative electrode material for secondary batteries of the present invention, the peak intensity at about 0.45 V in the dQdV curve is greater than the peak intensity at 0.25 V after two charge cycles.

[0072] The lithium secondary battery including the negative electrode for lithium secondary batteries of the present invention is discharged twice, and then Mg x SiO y XRD peaks due to may not appear.

[0073] The present invention will be described in detail below based on examples, but the present invention is not limited to these.

[0074] [Example] <Example 1> Production of silicon composite oxide-carbon composite powder Mg8-SiOx / C 20 kg of silicon powder with an average particle size of 20 μm, 50 kg of silicon dioxide powder with an average particle size of 20 nm, and 130 kg of silicon oxide (SiOx, x=1.03) powder with an average particle size of 200 μm were stirred in a Henschel mixer for 2 hours to uniformly mix them to form a raw material powder mixture. The raw material powder mixture was heat-treated at 1000° C. for 2 hours under an argon atmosphere at normal pressure.

[0075] The heat-treated raw powder mixture and 16 kg of metallic magnesium were placed in crucible-A and crucible-B of a vacuum reactor, respectively, and the pressure was reduced to 0.1 torr, followed by heating. The crucible-A containing the raw powder mixture was heated to 1450°C for evaporation, and the crucible-B containing metallic magnesium was heated to 850°C for evaporation, and then reacted in a vapor state for 5 hours. The silicon composite oxide mass that was reacted in the high-temperature gas phase and deposited on the substrate in the reactor was quickly cooled to room temperature using a water-cooled substrate.

[0076] The silicon composite oxide lumps were mechanically pulverized to control the particle size so that the average particle size became 6 μm.

[0077] 50 g of the pulverized silicon composite oxide powder was placed in a tube-type electric furnace, and maintained at 1000°C for 1 hour while flowing Ar and methane gas at 1 L / min each, to produce a silicon composite oxide-carbon composite powder Mg-SiO / C whose surface was coated with carbon.

[0078] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Example 1, ICP-MS analysis was carried out, and the Mg content was measured to be 8 wt %.

[0079] <Example 2> Preparation of silicon composite oxide-carbon composite powder Mg6-SiOx / C A silicon composite oxide-carbon composite powder Mg6-SiOx / C was produced in the same manner as in Example 1 above, except that the content of metallic magnesium in Example 1 was changed to 12 kg.

[0080] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Example 2, ICP-MS analysis was carried out, and the Mg content was measured to be 6 wt %.

[0081] <Example 3> Preparation of silicon composite oxide-carbon composite powder Mg3-SiOx / C A silicon composite oxide-carbon composite powder Mg3-SiOx / C was produced in the same manner as in Example 1 above, except that the content of metallic magnesium in Example 1 was changed to 6 kg.

[0082] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Example 3, ICP-MS analysis was carried out, and the Mg content was measured to be 3 wt %.

[0083] <Example 4> Preparation of silicon composite oxide-carbon composite powder Mg12-SiOx / C A silicon composite oxide-carbon composite powder Mg12-SiOx / C was produced in the same manner as in Example 1 above, except that the content of metallic magnesium in Example 1 was changed to 24 kg.

[0084] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Example 4, ICP-MS analysis was carried out, and the Mg content was measured to be 12 wt %.

[0085] <Comparative Example 1> Production of silicon composite oxide-carbon composite powder 20 kg of silicon powder with an average particle size of 20 μm and 50 kg of silicon dioxide powder with an average particle size of 20 nm were added to water, stirred for 12 hours to mix uniformly, and then dried at 1200°C (or 200°C, temperature confirmation required) for 2 hours to form a raw powder mixture.

[0086] The raw material powder mixture and 11 kg of metallic magnesium were placed in crucible-A and crucible-B of a vacuum reactor, respectively, and the pressure was reduced to 0.1 torr. After that, the mixture was heated. Crucible-A containing the raw material powder mixture was heated to 1600°C for evaporation, and crucible-B containing the metallic magnesium was heated to 900°C for evaporation. The vapor from crucible-A and the vapor from crucible-B were reacted for 3 hours, and then the silicon composite oxide-carbon composite powder of Comparative Example 1 was produced by the same cooling, pulverization and carbon coating steps as in Example 1.

[0087] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Comparative Example 1, ICP-MS analysis was carried out, and the Mg content was measured to be 13 wt %.

[0088] <Comparative Example 2> Production of silicon composite oxide-carbon composite powder A silicon composite oxide-carbon composite powder of Comparative Example 2 was produced in the same manner as in Comparative Example 1, except that the amount of metallic magnesium added was changed to 13 kg.

[0089] In order to measure the Mg content in the silicon composite oxide-carbon composite powder produced in Comparative Example 2, ICP-MS analysis was carried out, and the Mg content was measured to be 16 wt %.

[0090] <Comparative Example 3> Production of silicon composite oxide-carbon composite powder SiOx / C 20 kg of silicon powder with an average particle size of 20 μm and 50 kg of silicon dioxide powder with an average particle size of 20 nm were added to water, stirred for 12 hours to mix uniformly, and then dried at 1200°C (or 200°C, temperature confirmation required) for 2 hours to form a raw material powder mixture.

[0091] The raw material powder mixture was put into crucible-A and crucible-B, and the pressure was reduced to 1 torr, followed by heating. The crucible-A containing the raw material powder mixture was heated to 1600°C, and evaporated on a cooling plate for 3 hours. The same cooling, crushing and carbon coating steps as in Example 1 were then carried out to produce a silicon oxide-carbon composite powder SiOx / C of Comparative Example 3, to which no magnesium was added.

[0092] <Experimental example>TEM-EDX measurement For the silicon composite oxide-carbon composite powder Mg-SiO / C measurement sample produced in Example 1 above, FIB processing was performed using an FIB from the surface (porous layer surface) of the measurement sample in the depth direction (direction toward the inside of the measurement sample) to produce a processed surface (cross section).

[0093] The processed surface was subjected to TEM-EDX measurement (backscattered electron image) at an accelerating voltage of 2.1 kV and a magnification of 6500 times. The results are shown in FIG.

[0094] As shown in FIG. 1, the silicon composite oxide-carbon composite powder Mg-SiO / C produced in Example 1 is composed of Si clusters and Mg x SiO y It was confirmed that the material contains magnesium silicate represented by the formula (0.5≦x≦2, 2.5≦y≦4).

[0095] TEM-EDX measurements were performed on the products produced in Examples 2 to 4 in a similar manner. As a result, it was confirmed that the silicon composite oxide-carbon composite powders produced in Examples 2 to 4 also contained Si clusters and magnesium silicate formed in the periphery of the Si clusters.

[0096] <Experimental Example> XRD Measurement XRD data was measured for the products produced in the above Examples 1 to 4 and Comparative Examples 1 to 3, and the results are shown in FIGS. 2 to 8. In addition, the intensity of each peak was measured, and the results are shown in Table 1 below. [Table 1]

[0097] In FIG. 8, which shows the results of XRD measurement of Comparative Example 3, which is not doped with magnesium, it was confirmed that peaks due to amorphous silicon oxide (a-SiO2) appeared in the range of 20° to 40°, and peaks due to crystalline silicon oxide appeared with the highest intensity at 28° and 45°.

[0098] In Example 1, as shown in Fig. 2, only a peak due to the MgSiO3 crystal phase appears, whereas in Comparative Examples 1 and 2, a peak due to the forsterite crystal phase of Mg2SiO4 appears. As a result, in the case of the Example, the ratio I Mg2SiO4 / I MgSiO3 However, it was confirmed that it was less than 0.5.

[0099] <Experimental Example> Measurement of domain size From the results of the XRD measurement, the Si crystal size in the silicon composite oxide can be measured as follows.

[0100] In the X-ray diffraction pattern, the domain size was measured based on the full width at half maximum (FWHM) of the peak assigned to Si(111) using the Scherrer equation shown in the following general formula (1). The results are shown in Table 1 above. CS[nm]=K.λ / B.cosθ···General formula (1) (In the formula, K=0.9, λ=0.154nm, half width (FWHM, rad), θ: peak position (angle))

[0101] In Table 1 above, it was confirmed that the domain size of the crystalline silicon particles Si(220) increases in proportion to the Mg content in the particles.

[0102] <Experimental Example> XPS Measurement The particles produced in the above Example and Comparative Example 3 were subjected to XPS measurement, and the results are shown in FIG.

[0103] As shown in FIG. 9, in the examples of the present invention, when the Mg content in the particles was 8 wt%, no peak due to Mg2SiO4 appeared, but a peak due to MgSiO3 appeared, whereas in the comparative examples of the present invention, when the Mg content in the particles was 13 wt%, a peak due to Mg2SiO4 appeared.

[0104] In addition, as shown in FIG. 9, as the Mg content in the particles increases, the binding energy of SiO corresponding to 98 to 99 eV and Si corresponding to MgxSiOy increases. 3+ It was confirmed that the peak intensity due to

[0105] This is because the reaction from SiOx to Si decreases as the Mg content in the particles increases, and Mg is converted to MgxSiOy.

[0106] <Experimental example> STEM-EDX measurement The particles produced in the above examples were subjected to STEM-EDX measurement, and the results are shown in Figure 15. It was found from Figure 15 that the surface of the silicon composite oxide produced above was covered with a carbon layer of several tens of nanometers having the shape of carbon nanofibers and graphene, etc. It was also confirmed from Figure 15 that magnesium was uniformly distributed in the silicon composite oxide powder produced by the present invention.

[0107] <Manufacturing example> Manufacturing of lithium secondary batteries using silicon composite oxide The silicon composite oxide powders prepared in Examples 1 and 2 and Comparative Example 3 were mixed with natural graphite in a weight ratio of 73:27 to prepare an electrode active material, and a negative electrode for a lithium secondary battery and a battery (coin cell) were manufactured using the mixture.

[0108] The mixed active material, carboxymethyl cellulose (CMC) as a binder, and styrene butadiene rubber (SBR) were mixed with water in a weight ratio of 97:1.5:1.5 to prepare a negative electrode slurry.

[0109] The composition was applied to a copper foil having a thickness of 18 μm and dried to prepare an electrode having a thickness of 70 μm. The copper foil to which the electrode was applied was punched into a circle having a diameter of 14 mm to prepare a negative electrode for a coin cell, and a metallic lithium foil having a thickness of 0.3 mm was used as the opposite electrode.

[0110] A 0.1 mm thick porous polyethylene sheet was used as the separator, and a 1M LiPF6 solution was dissolved in a 1:1 volumetric mixture of ethylene carbonate (EC) and diethylene carbonate (DEC) to form the electrolyte. Using the above components, a coin cell (battery) with a thickness of 2 mm and a diameter of 32 mm (the so-called 2032 type) was fabricated.

[0111] <Experimental Example> Evaluation of electrochemical properties The coin cells produced from each sample in the above manufacturing examples were charged at a constant current of 0.1 C until the voltage reached 0.005 V, and then discharged at a constant current of 0.1 C until the voltage reached 2.0 V, and the charge capacity (mAh / g), discharge capacity (mAh / g), and initial charge / discharge efficiency (%) were determined.

[0112] In addition, the coin cells produced from each sample in the above manufacturing examples were charged and discharged once, and then in the second charge and discharge, they were charged at a constant current of 0.5 C until the voltage reached 0.005 V, and then discharged at a constant current of 0.5 C until the voltage reached 2.0 V, and the cycle characteristics (capacity retention rate) were determined.

[0113] The results of the analysis of the charge / discharge capacity, the initial charge / discharge efficiency, and the capacity retention rate are shown in Table 2. [Table 2]

[0114] In Table 2 above, the initial discharge capacity was 1382 mAh / g in Example 1, which was lower than 1647 mAh / g in Comparative Example 3. However, the initial charge / discharge efficiency was higher in Example 1 than in Comparative Example 3, and the initial discharge capacity of Comparative Example 2 was the lowest at 1143 mAh / g.

[0115] MgxSiOy, which is generated by the reaction of magnesium with silicon oxide, is known to be electrochemically inactive. It is considered that the higher the Mg content in Comparative Example 1, the more the electrochemically inactive MgxSiOy is generated, and the lower the charge / discharge capacity is, as compared to Example 1.

[0116] In FIG. 12, it was confirmed that the voltage during charging was below 0.1 V, but the overvoltage increased as the magnesium content increased.

[0117] Using the batteries manufactured in the above examples of the present invention and comparative examples, dQ / dV was measured after two charge / discharge cycles and 100 charge / discharge cycles, and the results are shown in FIG.

[0118] As shown in FIG. 11, in the embodiment of the present invention, it was confirmed that the peak near 0.45 V in the dQ / dV curve was larger than the peak at 0.25 V after two charging operations.

[0119] <Experimental Example> Measurement of volume change due to charging and discharging The battery manufactured in the above manufacturing example was subjected to 100 charge / discharge cycles, and then the electrodes were subjected to SEM analysis and the particles were subjected to XRD analysis. The results are shown in Table 3 below. [Table 3]

[0120] As shown in Table 3 above, in Example 1, the electrode thickness before charging and discharging was 23 um, but the electrode thickness after 100 charging and discharging cycles changed to 33 um, and in Comparative Example 1, the electrode thickness before charging and discharging was 18 um, but the electrode thickness after 100 charging and discharging cycles changed to 40 um. It was confirmed that the volume change of the silicon composite oxide in Example 1 was reduced compared to Comparative Example 1.

[0121] <Experimental Example> Ex-situ XRD measurement before and after charging and discharging For the batteries containing the silicon composite particles of Example 1 and Comparative Example 1, ex-situ XRD measurements were performed after one charge / discharge and after 100 charge / discharge cycles, and the results are shown in FIG.

[0122] In FIG. 13, in Example 1, after one charge / discharge cycle, no peaks appear other than those due to MgSiO3 and the copper used as the current collector, and after 100 charge / discharge cycles, peaks due to lithium hydroxide and lithium oxide are observed. In contrast, in Comparative Example 1, as shown in FIG. 13, after one charge / discharge cycle, no peaks are observed other than those due to Mg2SiO4, as in Example 1, but after 100 charge / discharge cycles, peaks similar to those in the case of the initial particles appear.

[0123] As can be seen from FIG. 13, in the embodiment of the present invention, after two discharges, Mg x SiO y It was confirmed that no XRD peaks due to

[0124] The results of XRD in Example 1, Comparative Example 1, and Comparative Example 3 after 100 charge / discharge cycles are shown in Fig. 14. It was confirmed from Fig. 14 that LiOH was detected only in Comparative Example 3 and Example 1.

[0125] <Experimental example> TEM, STEM-HAADF, STEM-EDX measurements The particles of Example 1, Example 2, and Comparative Example 3 were subjected to TEM, STEM-HAADF, and STEM-EDX measurements, and the results are shown in FIG.

[0126] In FIG. 15, in Comparative Example 3 in which Mg was not mixed, ring patterns corresponding to Si(111) and Si(220) were formed.

[0127] Unlike Comparative Example 3, Example 1 has a wider crystal structure than Comparative Example 3, and MgSiO3 spots appear. On the other hand, in Comparative Example 1, the amorphous portion is narrower than Comparative Example 3 and Example 1, and most of the portion is observed to be crystalline. As shown in FIG. 15(c), it was confirmed that the grain boundary between Si and Mg2SiO4 appears clearly.

[0128] In Example 1, as shown in Figs. 15(e) and 15(h), SiOx is formed around Si in a core-shell structure, whereas in Comparative Example 1, as shown in Figs. 15(f) and 15(i), the portions where Si and MgxSiOy are present are clearly separated, and it was found that the crystal structures of Example 1 and Comparative Example 1 are completely different.

[0129] Based on the above analysis results, FIG. 10 shows a schematic diagram of the cross-sectional components of the produced particles.

[0130] Carbon components are shown in black, silicon oxide in orange, silicon components in green, and magnesium silicate in blue.

[0131] <Experimental Example> Measurement of EDS images before and after charging and discharging For the batteries containing the particles of Example 1, Example 2, and Comparative Example 3, EDX measurements were performed after one charge / discharge and after 100 charge / discharge cycles, and the results are shown in FIG.

[0132] In Example 1, in which the Mg content is 8%, after one charge / discharge cycle, MgxSiOy aggregates around the Si core as shown in Figs. 16(a) to 16(d), but after 100 charge / discharge cycles, MgxSiOy spreads uniformly within the particles and becomes stable. In Comparative Example 1, in which the Mg content is 13%, large MgxSiOy and Si domains are formed from the beginning as shown in Figs. 16(e) to 16(h), and a structural change occurs to align the stable form, which causes a volume change associated with charge / discharge and deteriorates the life characteristics.

[0133] The structural changes described above are shown diagrammatically in FIG.

[0134] Although specific parts of the present invention have been described in detail above, it is clear to those skilled in the art to which the present invention pertains that such specific descriptions are merely preferred embodiments and are not intended to limit the scope of the present invention. Therefore, the substantial scope of the present invention is defined by the claims and their equivalents.

Claims

1. Si clusters; and The Mg formed around the Si cluster x SiO y (0.5≦x≦2, 2.5≦y≦4) magnesium silicate; Including, The silicon cluster forms a core of a core-shell structure, and the magnesium silicate forms a shell of the core-shell structure.

2. 2. The silicon composite oxide for use as a negative electrode material for lithium secondary batteries according to claim 1, wherein the domain size of Si(111) due to the Si clusters is 12 nm or less.

3. In the X-ray diffraction pattern analysis, a peak attributed to Si crystal appears in the diffraction angle range of 28°<2θ<29°. MgSiO in the diffraction angle range of 30.5° < 2θ < 31.5° 3 2. The silicon composite oxide for use as a secondary battery negative electrode material according to claim 1, which exhibits a peak attributable to crystals.

4. 2. The silicon composite oxide for lithium secondary battery negative electrode material according to claim 1, wherein the full width at half maximum (FWHM (deg)) of Si (111) due to the Si clusters is 0.7 to 1.5 (deg) in XRD analysis.

5. The silicon composite oxide is Mg 2 SiO 4 (forsterite) crystals, The Mg 2 SiO 4 The content of (forsterite) crystals is MgSiO 3 2. The silicon composite oxide for use as a secondary battery negative electrode material according to claim 1, wherein the content of (enstatite) crystals is less than that of the silicon composite oxide.

6. The silicon composite oxide Mg 2 SiO 4 Forsterite crystal phase and MgSiO 3 Peak intensity ratio I to crystalline phase Mg2SiO4 / I MgSiO3 The silicon composite oxide for secondary battery negative electrode material according to claim 1, wherein is 0 to 0.5 or less.

7. 2. The silicon composite oxide for use as a secondary battery negative electrode material according to claim 1, wherein the silicon composite oxide contains 2 to 15 parts by weight of Mg per 100 parts by weight of the total.

8. 2. The silicon composite oxide for use as a secondary battery negative electrode material according to claim 1, wherein the silicon composite oxide includes a carbon coating on a surface thereof.

9. 9. The silicon composite oxide for use as a secondary battery negative electrode material according to claim 8, wherein the carbon coating has an average thickness of 5 to 100 nm.

10. Silicon powder, silicon oxide (SiO x , 0.9<x<1.1) powder and silicon dioxide powder were mixed to obtain Si / SiO x / SiO 2 Preparing a raw powder mixture; The Si / SiO x / SiO 2 a step of evaporating the raw material powder mixture and metallic magnesium, respectively, reacting them, and then depositing them to form a composite oxide; Cooling the formed silicon composite oxide; and pulverizing the cooled silicon composite oxide; The method for producing the silicon composite oxide for use as a secondary battery negative electrode material according to claim 1, comprising:

11. The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, further comprising a step of coating a surface of the pulverized silicon composite oxide with carbon.

12. The silicon powder and the silicon oxide (SiO x , 0.9<x<1.1) powder, and the silicon dioxide powder are mixed to obtain the Si / SiO x / SiO 2 In the step of preparing a raw material powder mixture, the Si / SiO x / SiO 2 The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, wherein the O / Si molar ratio in the raw material powder mixture is 0.9 to 1.

1.

13. The silicon powder and the silicon oxide (SiO x , 0.9<x<1.1) powder, and the silicon dioxide powder are mixed to obtain the Si / SiO x / SiO 2 In the step of preparing a raw material powder mixture, the silicon powder, the silicon oxide (SiO x , 0.9<x<1.1) powder, and the average particle size and specific surface area of ​​the silicon dioxide powder are 10 nm to 100 μm and 5 to 500 m 2 The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, wherein the silicon composite oxide has a molecular weight of 1000 to 15000 kPa (1 / g).

14. The silicon powder and the silicon oxide (SiO x , 0.9<x<1.1) powder, and the silicon dioxide powder are mixed to obtain the Si / SiO x / SiO 2 After the step of preparing the raw material powder mixture is performed, the Si / SiO x / SiO 2 The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, further comprising a step of heat treating the raw material powder mixture at 800 to 1100° C. and normal pressure for 1 to 3 hours.

15. The Si / SiO x / SiO 2 In the step of forming the composite oxide by vapor deposition after evaporating the raw material powder mixture and the metallic magnesium, the Si / SiO x / SiO 2 11. The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, wherein the raw material powder mixture and the metallic magnesium are evaporated in separate reactors and reacted in a gaseous state.

16. The Si / SiO x / SiO 2 In the step of forming the composite oxide by vapor deposition after evaporating the raw material powder mixture and the metallic magnesium, the Si / SiO x / SiO 2 The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, wherein the raw material powder mixture is evaporated at 1000 to 1600° C. under a pressure of 0.001 to 5 torr.

17. The Si / SiO x / SiO 2 11. The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 10, wherein in the step of evaporating the raw material powder mixture and the metallic magnesium, respectively, reacting them, and then depositing them to form the composite oxide, the metallic magnesium is evaporated at a pressure of 0.001 to 2 torr and at a temperature of 700 to 1000° C.

18. The method for producing a silicon composite oxide for a secondary battery negative electrode material according to claim 11, wherein in the step of coating with carbon, the silicon composite oxide is reacted in a gaseous state with any one or more carbon precursors selected from the group consisting of methane, propane, butane, acetylene, benzene, and toluene at 600 to 1200° C.

19. A negative electrode for a lithium secondary battery comprising the silicon composite oxide for use as a negative electrode material for secondary batteries according to claim 1 .

20. A lithium secondary battery comprising the negative electrode for lithium secondary batteries according to claim 19.

Citation Information

Patent Citations

  • Negative electrode material for secondary battery, and its manufacturing method

    JP2010170943A

  • Silicon composite oxide for lithium secondary battery negative electrode material and production method thereof

    JP2018156922A

  • Negative electrode material for non-aqueous electrolyte secondary battery, method for producing the same, and non-aqueous electrolyte secondary battery including the same

    JP2018519648A

  • Negative electrode active material for non-aqueous electrolyte cell, negative electrode for non-aqueous electrolyte secondary cell, non-aqueous electrolyte secondary cell, and cell pack

    WO2015145521A1

  • Negative electrode active material, negative electrode comprising negative electrode active material, and secondary battery comprising negative electrode

    WO2018208111A1